Abstract
In this work, the effect of mechanical activation (MA) on the double complex salt (DCS) [Co(NH3)6][Fe(C2O4)3]·3H2O and its thermolysis is investigated. Mechanical activation is a promising “green chemistry” method that allows improving the physicochemical properties of the DCS [Co(NH3)6][Fe(C2O4)3]·3H2O and the products of its thermal decomposition in an argon atmosphere. The conditions of the MA process and the effect of MA and passivation on the process and kinetics of DCS thermal degradation were investigated. It was shown that due to the removal of outer-sphere coordinated water and carbonation of the DCS during MA, the number of thermal degradation stages changes. It was established that passivation at 450 °C for MA times of 0 and 10 min prevents spontaneous “combustion” of the thermal degradation products of the DCS. Optimal conditions for DCS processing were determined to be 5 min of MA and heat treatment at 450 °C without passivation. Under these conditions, the yield of the CoFe intermetallic compound reaches 82.6 wt%. This optimal combination of sample production conditions allows for a reduction in MA time and the elimination of the passivation process, making the process more cost-effective and creating conditions for optimizing the production of functional materials.
1. Introduction
Mechanical activation (MA) and mechanochemical synthesis (MCS) offer a number of advantages and are promising green chemistry approaches to the preparation of inorganic and coordination compounds in the solid phase with minimal or no solvent use [1,2]. In the context of coordination chemistry, MA is used to prepare a wide range of compounds: from discrete coordination complexes to metal–organic frameworks (MOFs) and coordination polymers [3]. A large body of data on the MA of catalysts and supports was summarized in [4]. In this work, it was noted that the use of MA in various apparatuses (ball mill, bead mill, ultrasonic disintegrator, vibratory mill, and planetary mill) made it possible to synthesize a large number of new catalysts, including in the form of individual chemical compounds. A positive effect of the use of MA on the conditions for the preparation of many catalysts—on the catalytic properties, reactivity, and selectivity of both metal and oxide catalysts—was revealed. In [5], the influence of MA on the production of inverse spinel nanoparticles of a cubic lattice with the general formula AB2O4 based on Al and Ni compounds was investigated. This approach is also fundamentally applicable to Fe-Co systems.
Iwasaki et al. proposed an original mechanochemical method for the mechanical alloying of crystalline layered double hydroxide (LDH) Co2+–Fe2+–Fe3+ with intercalated chloride ions. In this method, an acidic solution of cobalt chloride is milled in a ball mill with steel balls for 6 h at room temperature. The source of iron ions is the steel balls, which are gradually eluted during milling, and the electrons generated during collisions decompose water molecules to form hydroxide ions, which ensures automatic pH control. The resulting LDH had the morphology of nanoplatelet aggregates 100–200 nm long and high crystallinity [6]. Kaczmarek described a new mechanochemical method for the preparation of highly coercive particles of berthalide compounds (CoxFe1−x)3O4. The method is based on reactive milling followed by annealing. It was shown that the MA of α-Fe2O3 in an aqueous medium in the absence of oxygen leads to the complete reduction of hematite to magnetite already at room temperature. The introduction of cobalt allows the production of substituted cobalt ferrites with a controlled Co content (3.7–38.0 at%) and high coercive force values [7]. Lemoine et al. reported the MCS of a mixed cobalt–copper fluorophosphate Co2−xCuxPO4F, which exhibits multifunctional electrochemical activity. The synthesis was carried out in a planetary ball mill, and the obtained material showed activity in the oxygen evolution reaction. This work demonstrates the applicability of the mechanochemical approach to the production of mixed 3d-metal-containing phosphates with a controlled metal ratio [8]. Ordered intermetallic M-Co (M = Pt, etc.) alloys show promise as next-generation low-Pt catalysts for the oxygen reduction reaction in proton exchange membrane fuel cells due to their high activity and excellent long-term stability. In a study by Xu, a high-Pt ordered PtCo alloy with a size of about 3 nm was prepared and exhibited high catalytic activity, achieving an impressive performance of 1.4 W/cm2 at 0.6 V in a hydrogen–air fuel cell and a mass activity of 0.62 A/mg(Pt) at 0.9 V in an H2-O2 fuel cell [9]. Liu et al. reported a method of preparing the intermetallic compound PtCo via controlled direct pyrolysis of the heteronuclear inorganic molecule [Co(NH3)5Cl][Pt(Cl)4]. The obtained Pt1Co1-IMC/C catalyst not only exhibited high mass activity (0.43 A/mg(Pt) at 0.9 V) towards oxygen reduction reaction but also demonstrated a peak power density of 1.06 W/cm2 when used in a hydrogen–air fuel cell [10]. Bai et al. reported the synthesis of a Co–Fe double atom catalyst for oxygen evolution reaction. Although the synthesis was not mechanochemical, this work demonstrates the synergistic effect of the combined presence of Fe and Co in one catalytic system. In double-atom catalysts, the Co–Fe bonding via oxygen/nitrogen bridges provides unique electronic properties, which can also be achieved through mechanochemical treatment of precursors (e.g., double complex salts (DCSs)) [11]. Kahani and Shahrokh [12] investigated the preparation of Cu–Co alloy nanoparticles from the binary complex salts [Co(NH3)6]2[Cu(C2O4)2]3, [Co(NH3)5Cl][Cu(C2O4)2], and [Co(en)3]2[Cu(C2O4)2]3 via chemical reduction with hydrazine. Although MCS was not used in this study, the concept of using DCSs as precursors for the preparation of bimetallic nanoparticles is key. The authors showed that the choice of the initial DCS determines the morphology and magnetic properties of the final nanoparticles; the ferromagnetic behavior was due to the presence of Co in the alloy. For the case of Fe-Co systems, of fundamental interest are the DCSs of the type [Fe(L)x]a[Co(L′)γ]s·nH2O and [Co(L)x]a[Fe(L′)γ]s·nH2O, where L and L′ are different ligands (NH3, en, C2O42−, CN−, etc.). It is precisely these salts that can serve as “pre-organized” precursors for MCS: mechanical activation promotes the solid-phase exchange of ligands or reductive decomposition with the formation of bimetallic phases [12]. Such DCSs attract considerable attention from researchers as single-source precursors for the production of bimetallic oxide, metallic and composite materials with a controlled composition and structure [13], and the use of MA to DCSs containing both Fe and Co ions in cationic and anionic complexes is of great interest for the purpose of producing bimetallic nanomaterials, oxide phases with a spinel structure, catalysts and magnetic materials, as well as nanocrystalline intermetallic compounds [11,14]. The usage of MA to DCSs is also due to the possible change in the coordination environment of the central metal ions, which in turn can lead to processes of disproportionation and recombination of ligands, as well as a decrease in the temperature and energy barriers of subsequent thermal decomposition and softening of the conditions for obtaining functional materials based on Co–Fe.
Previously, we investigated the effect of MA on the properties and thermolysis products of DCS [Co(NH3)6][Fe(CN)6] in [15], which demonstrated the possibility of controlling the properties of functional materials (intermetallic carbon) by combining synthesis using DCS and MA. It was noted that the use of MA contributes to a change in the coordination of ammonia ligands and a decrease in the thermal stability of mechanically treated DCS. The result of thermolysis of mechanically treated DCS at 650 °C in argon for 10 min was the intermetallic compound Co0.5Fe0.5 in a nanocrystalline form with a structure of porous filiform tubes with a specific surface area doubled, in comparison with heat-treated DCS without MA. The thermolysis process of the initial DCS [Co(NH3)6][Fe(CN)6], as well as similar DCSs, is described in detail in [16,17,18,19,20]. A study of solid-phase transformations of [Co(NH3)6][Fe(CN)6] using thermal analysis showed that the decomposition occurs in several stages: topotactic dehydration followed by redistribution of ligands with the formation of cyanide bridges. A similar mechanism of solid-phase transformations was described for the related DCS [Co(NH3)6][Fe(C2O4)3]·3H2O in [13,21]. Based on the general principles of mechanochemistry of coordination compounds and data on the thermal decomposition of [Co(NH3)6][Fe(C2O4)3], the following hypothetical effects of mechanical activation of this DCS can be distinguished: the destruction of hydrogen bonds between ammonia ligands and oxalate groups, which stabilize the crystal structure of the hydrate; the deformation and partial rupture of the Co–NH3 and Fe–O (oxalate) bonds with the possible formation of coordinatively unsaturated centers, which can act as active centers of catalysis; the facilitation of intramolecular electron transfer Co(III) → Fe(III), which can change the thermolysis mechanism; the possible formation of spinel phase nuclei, which will reduce the formation temperature; and increased reactivity with respect to gaseous reagents (CO, H2, O2) due to the accumulation of defects and an increase in the specific surface area [12,17,18,21,22,23]. From a practical point of view, the use of DCSs based on the cyanide anion is more predictable, since such DCSs always have one chiral structure [24], and their areas of application have been studied in more detail [25,26]. DCSs based on both cyanide and oxalate anions can have different structures due to the ability to create one-, two-, and three-dimensional network structures [27,28,29,30], respectively. However, only complexes with oxalate anions can form enantiomers [30]. On the other hand, the possibility of forming DCSs based on oxalate anion with different denticity and coordination significantly expands the range of functional properties [31]. An important advantage of the oxalate anion is the chelating effect, which ensures greater thermodynamic stability, low toxicity, biocompatibility, and safety during synthesis (the principle of “green chemistry”). However, since the multifunctional materials under study are precisely the thermolysis products of Co–Fe DCS, the choice of ligand is critically important, since the process of thermolysis of Co–Fe DCS with different ligands occurs with a different number of stages; for example, the end of the thermal destruction process (the thermogravimetric curve reaching a plateau) occurs in a different temperature range, which leads to the formation of mono- or heterophase functional materials with different physicochemical characteristics (particle size, morphology, specific surface area, catalytic activity, content of gas phases, etc.) [13,17,31,32,33,34]. The thermokinetic properties of the initial DCS [Co(NH3)6][Fe(C2O4)3]·xH2O are described in detail in [35].
The aim of this work is to use and investigate for the first time the influence of MA on the DCS [Co(NH3)6][Fe(C2O4)3]·3H2O, thermolysis products and their properties.
2. Materials and Methods
All experiments were performed at least three times; the data presented in this article are averaged.
The starting binary compound [Co(NH3)6][Fe(C2O4)3]·3H2O (hereinafter referred to as DCS) was obtained in quantitative yield by mixing aqueous solutions of cationic and anionic complexes. Chemicals [Co(NH3)6]Cl3 and K3[Fe(C2O4)3] (Vecton Ltd., Saint Petersburg, Russia) were used. Powder X-ray diffraction (XRD), infrared (IR) spectroscopy, differential thermal analysis (DTA), crystal structure and elemental analysis for DCS are the same as described in [21,36].
After merging the cationic [Co(NH3)6]Cl3 and anionic K3[Fe(C2O4)3] complexes, the target [Co(NH3)6][Fe(C2O4)3]·3H2O DCS precipitates, while KCl remains in the mother liquor. The DCS is filtered off under vacuum, and the wet residue is washed with ice-cold water. The quality of washing from the mother liquor (from chloride ions) was controlled by the cessation of the reaction of the mother liquor with the silver nitrate. The DCS is then washed with ethanol.
The MA conditions were chosen similarly to those in [15]. MA was carried out in a laboratory centrifugal-planetary mill AGO-2 (NPO NOVIC, Novosibirsk, Russia, 2013) in an air atmosphere using steel vials and balls with a diameter of 8 mm for 5 min at a centrifugal factor of 40 g. The ball-to-load ratio was 20:1. To ensure macrohomogeneity of the powders, the mill was turned off after every 60 s of MA and the contents of the vials were mixed with a metal spatula [37]. Before the MA, lining of vials and balls was carried out with a smaller amount of composition.
XRD was carried out at room temperature in the 2θ range of 10–90° using a powder diffractometer XRD 6000 (Shimadzu, Kyoto, Japan, 2008) with a Cu-Kα source (λ = 1.5418 Å) and a graphite monochromator. XRD patterns of products calcined in argon at 200–450 °C were obtained on a powder diffractometer MiniFlex 600 (RIGAKU, Tokyo, Japan, 2021) with a Cu-Kα source (λ = 1.5418 Å), Kβ filter, D/teX Ultra detector, Bragg–Brentano geometry and a graphite monochromator in the 2θ range 10–90°. The crystal lattice parameters were refined using the Rietveld refinement and the fundamental parameters method. The method error was generally 5%. The decoding was pe rformed using a database JCPDS-ICDD PDF 4+ (International Center for Diffraction Data, Philadelphia, PA, USA, 2020). Some data were processed using Jana2006 (v2006) and Jana2020 (v2020) [38,39]. XRD patterns of a single-phase samples were refined by the Le Bail method [40].
Infrared (IR) spectra were recorded on a spectrometer Nicolet 6700 FT-IR (Thermo Fisher Scientific Inc., Hillsboro, OR, USA, 2010) in KBr tablets, with a recording interval of 400–4000 cm−1, 16 scans, resolution 4.
The porous structure of the samples was determined by the method of low-temperature nitrogen sorption on the Tristar 3020 instrument (Norcross, GA, USA, 2009). The measurement error was 5%.
Synchronous thermal analysis (STA) with IR-spectroscopic analysis of exhaust gases (STA-IR) was performed on an HQT-4 device (Beijing Hengjiu HENVEN Experimental Equipment Co., Ltd., Beijing, China, 2022) in argon flow in open Al2O3 lids. The flow rate was 71 mL/min, sample mass was 15 mg, heating rate was 10 °C/min, and temperature range was 40–900 °C. STA in our case included obtaining simultaneous results with thermogravimetry (TG) and differential scanning calorimetry (DSC) analyses. The IR spectroscopic analysis of the evolved gases was performed using an SC-8000 device (Beijing Hengjiu Experimental Equipment Co., Ltd., Beijing, China, 2022) in a flow of dried air. The spectra were continuously registered in the 400–4000 cm−1 wavelength and 40–900 °C temperature ranges in 16 scans. The temperature of the Pike chamber and pipeline was 200 °C. Qualitative analysis was performed using HR Nicolet TGA Vapor Phase, HR Aldrich Vapor, and other libraries. The method for processing STA-IR analysis data and the method for identifying gaseous products of thermal decomposition (GPTD) are presented in [35].
Table 1 presents the multiplication parameters for determining the kinetics of gas-phase removal during STA-IR of samples MA-0, MA-5 and MA-10.
Table 1.
Multiplication parameters for determining the kinetics of gas-phase removal during STA-IR of samples MA-0, MA-5 and MA-10.
Thermolysis at 300 and 450 °C was carried out under isothermal conditions in a tubular furnace Nabertherm RT 50-250/11 (Nabertherm GmbH, Lilienthal, Germany, 2013) in an argon flow of 15 L/min with a heating rate of 10 °C/min in a quartz bed with a sample weight of ~0.5 g. Argon of 99.99% purity was used with additional purification of oxygen impurities by passing through a manganese suspension and drying from traces of water by passing through concentrated H2SO4. Thermolysis time was 1 h.
A scanning electron microscope (SEM), SEM LEO 420 (Carl Zeiss, Oberkochen, Germany, 1998), was also used in some cases.
CHNS elemental analysis was performed on a EuroVector EA3000 (Pavia, Italy, 2008) elemental analyzer at a temperature of up to 1000 °C. Standard deviation of the random component of measurement error is 0.01 wt% [41].
3. Results and Discussion
3.1. Characterization of Samples Before Thermolysis
After the MA, the DCS samples were analyzed using elemental analysis, XRD, and IR spectrometry. We will designate these samples as MA-X, where X is the MA time in minutes.
3.1.1. XRD Analysis
XRD analysis (Figure 1) shows a change in structure (partial disappearance of peaks of the untreated complex (trihydrate DCS) and the appearance of new peaks (anhydrous DCS phase)) after just the first minute of MA. After 10 min of MA, the formation of X-ray completely amorphous material is not observed; less than half of the peaks of the original untreated DCS remain.
Figure 1.
XRD patterns of the initial complex [Co(NH3)6][Fe(C2O4)3]·3H2O (sample MA-0) and the MA complex from 1 min to 10 min (samples MA-1–MA-10).
Figure 2 indicates that the initial DCS is definitely a single-phase [Co(NH3)6][Fe(C2O4)3]·3H2O. According to the XRD analysis of the samples after mechanical activation (Figure 3), it was established that an increase in the treatment time leads to a change in the intensity of reflections and the formation of an impurity phase—anhydrous complex [Co(NH3)6][Fe(C2O4)3] [42] (Figure 2). The content of this phase increases with the duration of mechanical activation. These data are confirmed by the Le Bail refinement (Figure 4 and Figure 5) [40]. Even after 10 min of mechanical activation, the formation of a completely single-phase anhydrous product does not occur (Figure 3). The obtained results suggest that prolonged mechanical action initiates a phase transition with dehydration, which results in the transformation of the crystalline structure. For greater clarity and readability of some images, Figure 2 and Figure 3 are also provided in the Supplementary Materials in scalable form (Figures S1 and S2).
Figure 2.
Comparison of theoretical and experimental XRD patterns for the initial [Co(NH3)6][Fe(C2O4)3]·3H2O (MA-0).
Figure 3.
XRD patterns of MA-0, MA-5 and MA-10.
Figure 4.
XRD pattern of the two-phase sample MA-5, refined according to Le Bail.
Figure 5.
XRD pattern of the two-phase sample MA-10, refined according to Le Bail.
3.1.2. IR Analysis
Here, and in later designations near the band frequencies, ν = stretching, δ = bending, r = rocking, v = very, st = strong, m = medium, w = weak, sym = symmetric, as = antisymmetric, and sh = shoulder.
IR spectra were collected on a Nicolet 6700 FT-IR spectrometer in KBr tablets. Characteristic absorption maxima in the IR spectrum (Figure 6), cm−1: 3548m, 3480w, 3431w ν(OH); 3297st, 3237st ν(NH); 1711v st, 1677 ν as (C = O); also 1677 v st may refer to δ(OH) (Figure 6 is marked with a dotted line); 1397st ν sym(C-O) + ν (C-C); 1328m, 883w, 859w ν sym (C-O) + δ (O-C = O); 1257m, 1255m – ν (C-O); 791m r (OH2); 596vw, 536w ν (M-O) + ν (C-C); 485w δ cyclo + δ (O-C = O). The IR spectrum matches the spectra given in [43], decoding was carried out using [13,44,45,46,47].
Figure 6.
IR spectra of the initial complex [Co(NH3)6][Fe(C2O4)3]·3H2O (sample MA-0) and the MA complex from 1 min to 10 min (samples MA-1–MA-10).
No significant changes are observed in the IR spectra with increasing MA time (Figure 6). However, the intensity of the bands in the 3400–3550 cm−1 range decreases slightly.
3.1.3. Elemental Analysis
The results of CHN analysis (Table 1) show that nitrogen contents remain virtually unchanged, while the carbon content increases by approximately ~3.7 mol% and the hydrogen content decreases by approximately ~4.2 mol%, which is consistent with the dehydration process. The calculation of the change in the quantitative content of carbon and hydrogen (using carbon as an example) was performed as follows (Equation (1)):
which corresponds to ~1.1 water molecules remaining in the DCS structure. This indicates a decrease in the amount of outer-sphere water of crystallization. However, it should be noted that water removal does not occur simultaneously throughout the entire sample. Therefore, Figure 4 and Figure 5 simultaneously show both the anhydrous and trihydrate phases. Table 1 shows that the cationic portion of the DCS undergoes virtually no changes during the MA process.
According to elemental analysis, with increasing MA time, partial carbonization (an increase in carbon content) (Table 2) of the DCS occurs due to interaction with atmospheric CO2 and air moisture during MA, as evidenced by a shift in the CO and CO2 removal temperatures toward higher temperatures (Figure 7 and Figure 8). This process also causes changes in the temperatures of the endo- and exo-effects for samples MA-5 and MA-10 (Table 3).
Figure 7.
STA curves of samples MA-0, MA-5, and MA-10: (a) TG, (b) DTG, (c) DSC, (d) dDSC.
Figure 8.
STA-IR of samples: (a) MA-0, (b) MA-5, (c) MA-10.
Table 2.
Results of elemental analysis of samples.
Table 3.
DSC details for samples MA-0, MA-5 and MA-10.
3.1.4. Synchronous Thermal Analysis
The TG curves do not change significantly with increasing MA time (Figure 7). The TG curve for the untreated complex exhibits six distinct steps. One of the main differences is the TG curve for MA-0 up to 100 °C, which corresponds to a dehydration process that is largely absent in MA-10. At 100 °C, the mass loss is 4.4% by weight, corresponding to the removal of ~1.3 water molecules. Increasing the temperature to 130 °C results in complete dehydration. When heating the untreated DCS to 130 °C, a plateau of 130–200 °C is observed, indicating the presence of a stable dehydrated phase. For the MA-5 sample, this plateau becomes quite diffuse, while for MA-10, the stable dehydrated phase stage is completely absent. To better visualize the observed difference, the temperature derivative of the TG curve—the differential thermogravimetry (DTG) curve—was taken. This is confirmed by DTG and differential scanning calorimetry (DSC) data. The minimum temperature on the DTG for MA-0 is 100 °C, while for MA-5 and MA-10 it is 120 °C; an intense endothermic effect is observed on the DSC curve for MA-0. Using Equation (1), it was determined that 1.9 molecules of coordinated water are removed after 10 min of MA. Consequently, no more than 1.1 molecules of water remain in the total DCS powder after 10 min of MA. This explains the decrease in the mass loss rate upon heating to 130 °C from 10.2 wt% (MA-0) to 2.7 wt% (MA-10). As the MA time increases, this endoeffect becomes less pronounced (the effect is practically invisible on the MA-10 DSC), but the minimum temperature changes only slightly and is approximately 120 °C for MA-0 and 130 °C for MA-5 and MA-10. This is confirmed by the first derivative curve with respect to differential scanning calorimetry (dDSC)—the range of OY values. When heated to 300 °C, no fundamental difference is observed in the presented thermal analysis curves.
A significant difference in the thermal behavior of the MCA-0 and MCA-10 samples is observed at temperatures above 300 °C. As the MA time increases, the inflection in the TG curve increases in the range of 250–350 °C. On the MA-0 TG curve, it is practically invisible, but for MA-10, it is a clearly discernible degree of mass loss (~2.5–3.0 wt%). The DTG curves also show a near-plateau in the 290–340 °C range. For MA-5, a clearly visible mass loss effect is observed, peaking at 355 °C. For MA-10, the effect is even more intense, reaching 365 °C. These changes are reflected in the DSC curves: the exothermic effect is observed at 320 °C for all samples, but while for MA-0 this is a clearly defined peak, for MA-10 it is less intense. These changes are more clearly visible in the DSC curves: the peak for MA-0 at 340 °C is the deepest, while the peaks for MA-5 and MA-10 are shifted toward higher temperatures by ~10 °C and are noticeably less intense.
The end of mass loss according to the TG curve occurs at approximately the same temperature of 430 °C for all samples. The difference in the DTG curve is more significant: 435 °C for MA-0, 470 °C for MA-5, and 490 °C for MA-10. Heat release ends before 500 °C for all samples.
Table 3 summarizes the temperatures and types of thermal effects for samples MA-0, MA-5, and MA-10.
Summarizing the data presented in this article and in [15], it is evident that the influence of the MA process is most pronounced upon heating to 200 °C. After only 5 min of MA, neither the plateau of existence of a stable complex for the [Co(NH3)6][Fe(CN)6] DCS nor the stable anhydrous complex for the [Co(NH3)6][Fe(C2O4)3]·3H2O DCS is observed.
In [15], upon heating above 200 °C, changing the MA time from 0 to 10 min does not significantly affect the course of the thermal decomposition curves. Only a slight change in the temperature of the last stage of mass loss is observed, from 625 °C for MA = 0 to 615 °C for MA = 10. In this study, in the case of DCS [Co(NH3)6][Fe(C2O4)3]·3H2O, a low-intensity stage of mass loss is observed along the TG curve in the region of 300 °C for samples MA-5 and MA-10. This is more clearly demonstrated by the “hole” in the region of 290–365 °C on the DTG.
3.1.5. Synchronous Thermal Analysis with Infrared Spectroscopy of the Exhaust Gas Phase
In [35], the following GPTDs were recorded: H2O, CO, CO2, NH3, and N2O. In this study, the same products were detected, but the release of N2O, as in [35], was extremely insignificant; therefore, in this study, the release of N2O will not be considered separately (Figure 8).
After just 5 min of MA (sample MA-5) and especially after 10 min of MA (sample MA-10), no peak of water release is observed in the IR curves upon heating to 150 °C. Upon heating above 190 °C, three distinct stages of GPTD release are observed. The first stage is reported at 190–300 °C, with a shift in the release minima in the IR spectra, which corresponds to the most intense gas release, from 240 °C for MA-0, 230 °C for MA-5 to 220 °C for MA-10. The second stage also differs in temperature range: 300–330 °C for MA-0 and MA-5 and 300–350 °C for MA-10, with the intensity of CO2 and NH3 release changing symbatically with the MA time. The temperature at the end of the third stage also increases with the MA time: 430 °C for MA-0, 450 °C for MA-5, and 465 °C for MA-10. The temperature of the most intense gas evolution in the third stage is 415 °C for MA-0, 430 °C for MA-5, and 445 °C for MA-10. Moreover, the amounts of CO2 and CO removed from the gas phases also change symbatically with the MA time.
3.2. Characterization of Samples After Thermolysis
The samples in this section are designated MA-X-Y, where X is the MA time in min and Y is the thermolysis temperature.
3.2.1. Elemental Analysis
Heat treatment of the DCS was carried out in a tubular furnace under an argon flow. After an hour-long soak, the quartz tube containing the boat with the DCS sample was removed from the furnace and cooled in air. Argon flow was maintained within the tube until the tube containing the calcined sample had completely cooled. Upon cooling to room temperature, the argon flow was stopped, and the boat was removed into air.
It was noted that at 300 °C, the sample did not undergo any visible changes during the boat-removal process. MA had no significant effect on the change in H and N contents at 300 °C.
The carbon content of the solid products of thermal decomposition (SPTD) at 300 °C remained virtually unchanged (Table 4).
Table 4.
Results of the elemental analysis of samples.
In turn, when the boat was removed from the argon tube and exposed to air after thermolysis at 450 °C, “combustion” of the sample was observed. Specifically, smoldering was visually observed on the sample's surface (initially black, upon exposure to atmospheric oxygen, a self-propagating flame “runs” across the sample, turning gray). The sample after thermolysis at 450 °C without passivation—MA-10-450—is considered pyrolytic. A similar situation was observed in [13].
Therefore, a second method for cooling the SPTD—passivation—was used. After cooling the tube containing the sample to room temperature, the ground sections were left in place, and special clamps were placed on the gas duct hoses to prevent oxygen from the air from rapidly entering the tube. This arrangement was left to allow for uniform, slow mixing of the argon atmosphere in which thermolysis was performed and the ambient air atmosphere for at least 12 h. After the passivation time, the boat was removed from the tube and no additional effects were observed.
Samples after thermolysis with passivation will be designated as MA-X-Y-p, where X is the MA time in min, Y is the thermolysis temperature and p is passivation.
The sample after thermolysis at 450 °C with passivation—MA-10-450-p—is considered stable in air.
MA does not significantly affect the change in H and N contents at 450 °C, regardless of the presence of passivation. The carbon content at 450 °C, regardless of the presence of passivation, increases slightly with increasing MA time (Table 4).
3.2.2. XRD Analysis
The observed phenomena are confirmed by the XRD data (Figure 9). According to Figure 9a, thermolysis at 300 °C leads to the formation of a mixture of FeC2O4 (*) (PDF 00-014-0807) and Co3O4 (●) (PDF 04-007-8056). Increasing the thermolysis temperature to 450 °C without passivation for MA-0-450 and MA-10-450 leads to the formation of samples based on the intermetallic compounds CoFe (°) (PDF 00-049-1568) (cubic space group, Pm3m) and Fe2.38Co0.62O4 (⧫) (PDF 01-08-2152) (cubic space group, Fd3m) in approximately equal proportions, with the exception of sample MA-5, in which the content of the CoFe phase reaches 82.6 wt.%. The use of passivation allows the increasing of the content of the intermetallic compound CoFe to 83.9–85.9 wt.% for all samples, including the sample without the use of MA (Figure 9d) for samples MA-0-450-p, MA-5-450-p and MA-10-450-p. Obtaining a single-phase sample using this combination of processing methods (MA + thermolysis + passivation) is not possible.
Figure 9.
(a) XRD patterns of thermolysis products in argon at 300 °C, (b) XRD patterns of thermolysis products in argon at 450 °C without passivation, (c) XRD patterns of thermolysis products in argon at 450 °C with passivation, (d) histogram of the phase composition of the samples.
Elemental analysis of the DCS after thermolysis (Table 4) shows that MA has virtually no effect on the composition of the resulting samples at the same temperatures. Importantly, thermolysis at 300 °C results in the destruction of the amino group, while increasing the thermolysis temperature from 300 °C to 450 °C results in the destruction of the oxalate group, facilitating the interaction of Co and Fe ions to form the intermetallic compound CoFe (Figure 9b,c).
Comparing the data in Table 1 and Table 4, it is worth noting that heating to 300 °C primarily results in the destruction of the cationic portion of the DCS—a sharp order-of-magnitude decrease in the amounts of H and N. Meanwhile, the carbon content, which indicates the presence of the oxalate ion, even increases slightly.
3.2.3. XRD Analysis
The IR spectra of SPTDs at 300 °C (samples MA-0-300, MA-5-300, and MA-10-300) are completely identical to each other, regardless of the MA time (Figure 10). Comparison of the spectra of uncalcined DCS (MA-0) and SPTD at 300 °C reveals that outer-sphere coordinated water is almost completely removed. The ν water bands in the 3431–3548 cm−1 region are no longer recorded in the intense, clearly distinguishable form they were in DCS before heat treatment (MA-0). The δ water band at 1677 cm−1 is not recorded as a narrow single peak, but transforms into a broad peak with a shoulder in the 1630–1700 cm−1 range. This broad peak is a superposition of several modes simultaneously: bending vibrations of NH3 (δ as (HNH)) and/or some stretching vibrations of C2O42- (ν a (C-O)) and/or water δ a (H-O-H). A low-intensity mode with a minimum at 3401 cm−1 may indicate the presence of a small amount of water sorbed from the air by the samples during storage and sample preparation for physicochemical analysis.
Figure 10.
IR spectra of DCS after heat treatment at 300 and 450 °C with/without passivation at different MA times, min.
The strongest band at 1670 cm−1 is assigned to asymmetric ν(C–O), and bands at 1358 and 1313 cm−1 are characteristic of symmetric ν(C–O) stretching modes, which indicate the presence of bridging oxalates, with all four oxygen atoms coordinated to the metal atoms [48,49]. The asymmetric δ(O–C–O) band is observed at 798 cm−1, while the band at 502 cm−1 is assigned to ν(M–Ox) (predominantly to Co) [50] and symmetric δ(C–C–O). These bands are typical absorption bands of metal oxalate.
A very small symmetrical bending mode of the NH3 groups is observed at 1473 cm−1 [22]. Given the low intensity of this peak, it can be assumed that coordinated ammonia is present in extremely small quantities [51].
Increasing the thermal destruction temperature in argon to 450 °C significantly simplifies the IR spectra (Figure 10), regardless of the presence of passivation. All six samples exhibit a single peak with a minimum at 560–569 cm−1, which indicates a stretching mode, the lattice vibration of the metal–oxygen bond in the spinel structure. The authors [52,53,54,55] attribute this to the Fe-O mode.
3.2.4. Morphology and Porosity Structure
SEM Analysis
According to the SEM image shown in Figure 11, one can judge the characteristic changes in the microstructure due to the effect of MA, namely, the destruction of the “needle-like” structure of the original DCS with the formation of larger agglomerates of various shapes due to heat treatment.
Figure 11.
SEM images of DCS samples under different conditions of MA and thermolysis.
Description of Pore Size Distribution
Table 5 presents the specific surface area (Ssp), pore volume (Vpore), and residues after heat treatment for all samples.
Table 5.
Porous structure of the samples.
For samples without heat treatment, the specific surface area is approximately the same, but sample MA-5 stands out due to the presence of pores in two diameter ranges with comparable ratios (Figure 12a): pores of 3–4 nm and pores with diameters greater than 10 nm. Samples MA-0 and MA-10 are characterized by the presence of pores with diameters greater than 10 nm.
Figure 12.
Description of pore size distribution of samples: (a) MA-0–MA-10, (b) MA-0-300–MA-10-300, (c) MA-0-450–MA-10-450, (d) MA-0-450-p–MA-10-450-p.
Samples MA-0-300–MA-10-300 (Figure 12b) have a small number of pores with diameters up to 4 nm and the overwhelming majority of pores have diameters from 4 to 15 nm, practically regardless of the MA time.
For samples MA-0-450 and MA-10-450, two distribution regions of pores with diameters of 3–4 nm and greater than 10 nm are observed (Figure 12c), which, based on XRD data (Figure 9b), can be attributed to the oxide phase region. Accordingly, the presence of a higher intermetallic content in samples MA-5-450, MA-0-450-p, MA-5-450-p, and MA-10-450-p and the absence of a region of small pore diameters (Figure 9c) confirms the hypothesis of a relationship between the presence of an oxide phase, which likely contains micropores. This same assumption explains the relatively high specific surface area values in samples MA-5-450, MA-0-450-p, MA-5-450-p, and MA-10-450-p. The lower values (approximately 1.5 times) for MA-10-450 and MA-0-450 are due to the agglomeration of oxide particles during combustion.
The data on the calcination residues (Table 5) are interpreted as follows. At 300 °C, the residue after the calcination of sample MA-10-300 has the highest mass, as this sample partially decomposed during the MA process. The logical decrease in the mass of the calcination residue for samples MA-0-300 and MA-5-300 is caused by a decrease in the degree of destruction of the DCS during the MA process.
At 450 °C without passivation, the ignition residue is greater than with passivation. This is explained by the presence of oxygen in the oxide phases of the unpassivated samples. Sample MA-5-450 stands out for its lower ignition residue (24.8 wt%), presumably due to its lower oxide content and higher intermetallic content, respectively. This is consistent with the XRD data for this sample (Figure 9b).
Based on the data presented in Table 5, we believe that 5 min is the optimal MA time. In samples without passivation at 450 °C (samples MA-0-450–MA-10-450), oxide combustion occurs, which leads to a decrease in the surface area compared to samples processed at 300 °C (samples MA-0-300–MA-10-300). However, even when burned at 450 °C without passivation, 5 min MA (sample MA-5-450) is better, since the surface and pore volume are 1.5-2 times larger. With passivation, the pore volume and specific surface area values are equalized (samples MA-0-450-p–MA-10-450-p) due to the fact that at 450 °C, passivation reduces the amount of oxide phase, regardless of the MA time.
When comparing the results obtained in this article and in [14], it is important to note the different heating rates: 10 °C and 5 °C/min, respectively. The main difference in the obtained data from [13] is the use of a completely different format of heat treatment occurring in a tubular furnace (in this work, the argon feed rate is clearly fixed, while in [13] the flow rate is not specified in any way); the difference is also due to the different mass of the load—in our work the mass of the load = 2.5–3.0 g, in [13] the mass of the load varied from 20 to 60 g. This can explain the discrepancy in the values of the specific surface. For example, the specific surface area parameter during thermolysis at 300 °C: 13.84 m2/g in this work and 29 m2/g in [13]; at 400–450 °C for pyrolytic samples: 6.76 m2/g in this work and 17 m2/g in [13]; and at 450 °C for stable samples: 13.42 m2/g in this work and 14.5 m2/g in [13].
A significant factor influencing the specific surface area and pore volume is the heating rate. The influence of heating rate on the TG and DSC curves is clearly described in [35]. In a specific case, reducing the heating rate from 10 °C/min to 1 °C/min leads to a decrease in the end temperature of thermal degradation (the TG curve plateauing) by almost 50 °C. A similar difference is observed in [13], when reducing the heating rate from 10 °C/min to 3 °C/min.
4. Conclusions
- MA of 3d-3d DCS with oxalate ligands was performed for the first time.
- During MA, partial removal of outer-sphere coordinated water and partial carbonation of DCS occur due to interaction with CO2 and moisture from the air. However, even after 10 min of MA, a single-phase anhydrous phase was not obtained.
- MA changed the number of stages and the kinetics of the thermal destruction process, which led to changes in the temperature ranges for the removal of gas products and their ratios.
- The effect of passivation (slow oxidation of calcined products) on the phase and chemical composition was studied. The use of passivation reduces the amount of oxides (Fe2.38Co0.62O4) from ~58 wt% to ~15 wt% (at 300 °C for MA-0, MA-5, MA-10 and 450 °C for MA-0 and MA-10, respectively).
- When comparing the obtained results with the data for DCS [Co(NH3)6][Fe(CN)6] [15], it was found that a similar MA time of 10 min is excessive for obtaining a degradation product with the most suitable production conditions/properties ratio. It was found that 5 min of MA without passivation and any MA time with passivation resulted in a nearly “single-phase” sample with a CoFe intermetallic yield of at least 82 wt%.
- It was found that 5 min of MA and heat treatment at 450 °C without passivation were optimal conditions for processing [Co(NH3)6][Fe(C2O4)3]·3H2O. The sample obtained under these conditions (MA-5-450) was similar in phase and elemental composition, as well as surface area (~15 m2/g), to the samples with passivation. The samples with passivation and sample MA-5-450 were mesoporous, with pore diameters exceeding 10 nm and smaller pores were absent.
- The optimal combination of conditions for obtaining this sample (MA-5-450) reduced the MA time and eliminated the passivation process, which is cost-effective.
Supplementary Materials
The following supporting information can be downloaded at: https://www.mdpi.com/article/10.3390/thermo6030065/s1, Figure S1: Version of the Comparison of theoretical and experimental XRD patterns for the initial [Co(NH3)6][Fe(C2O4)3]·3H2O (MA-0) cropped along the YO-axis; Figure S2: Version of the XRD patterns of MA-0, MA-5 and MA-10 cropped along the YO-axis.
Author Contributions
Conceptualization, A.G.; methodology, A.G., V.V., E.F., M.I. and V.E.K.; validation, A.G., V.V. and O.S.; investigation, A.G., V.V. and O.S.; resources, A.G. and M.I.; data curation, A.G., V.V. and O.S.; writing—original draft preparation, A.G. and V.V.; writing—review and editing, A.G., V.V., V.E.K., A.K. and S.A.; visualization, V.V., O.S., M.I. and V.E.K.; supervision, A.G. and V.V.; project administration, A.G.; funding acquisition, A.G. and M.I. All authors have read and agreed to the published version of the manuscript.
Funding
This research was carried out within the framework of the state assignment of the Tananaev Institute of Chemistry—Subdivision of the Federal Research Centre «Kola Science Centre of the Russian Academy of Sciences» (project FMEZ-2025-0058).
Data Availability Statement
The raw data required to reproduce these findings are available from the authors on reasonable request.
Acknowledgments
The CHNS-analysis of the composition of the materials (E.V. Fatushina) obtained was carried out using the equipment of the Joint Research Centers for the Physical Methods of Research of Kurnakov Institute of General and Inorganic Chemistry of the Russian Academy of Sciences (JRC PMR IGIC RAS). The authors thank Kirill Yakovlev from Tananaev Institute of Chemistry of Kola Science Centre of the Russian Academy of Sciences (ICT KSC RAS) for help with obtaining XRD data.
Conflicts of Interest
The authors declare no conflicts of interest.
Abbreviations
The following abbreviations are used in this manuscript:
| MA | mechanical activation |
| MCS | mechanochemical synthesis |
| MOF | metal–organic framework |
| LDH | layered double hydroxide |
| SEM | Scanning electron microscopy |
| XRD | X-ray diffraction |
| IR | Infrared |
| STA | Synchronous thermal analysis |
| STA-IR | Synchronous thermal analysis with infrared spectroscopy of the exhaust gas phase |
| TG | thermogravimetry |
| DSC | differential scanning calorimetry |
| DTG | differential thermogravimetry |
| dDSC | first derivative with respect to differential scanning calorimetry |
| GPTD | gaseous products of thermal decomposition |
| SPTD | solid products of thermal decomposition |
References
- James, S.L.; Adams, C.J.; Bolm, C.; Braga, D.; Collier, P.; Friščić, T.; Grepioni, F.; Harris, K.D.M.; Hyett, G.; Jones, W.; et al. Mechanochemistry: Opportunities for new and cleaner synthesis. Chem. Soc. Rev. 2012, 41, 413–447. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Yuan, W.; O’Connor, J.; James, S.L. Mechanochemical synthesis of homo- and hetero-rare-earth(iii) metal–organic frameworks by ball milling. CrystEngComm 2010, 12, 3515–3517. [Google Scholar] [CrossRef] [Scilit]
- Dolganov, A.V.; Belov, A.S.; Novikov, V.V.; Vologzhanina, A.V.; Romanenko, G.V.; Budnikova, Y.G.; Zelinskii, G.E.; Buzin, M.I.; Voloshin, Y.Z. First iron and cobalt(II) hexabromoclathrochelates: Structural, magnetic, redox, and electrocatalytic behavior. Dalton Trans. 2015, 44, 2476–2482. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Molchanov, V.V.; Buyanov, R.A. Mechanochemistry of catalysts. Russ. Chem. Rev. 2000, 69, 435–450. [Google Scholar] [CrossRef] [Scilit]
- Filatova, N.V.; Kosenko, N.F.; Denisova, O.P. The Regulation of Spinel Precursors Reactivity by Means of a Mechanical and a Microwave Treatment. Russ. J. Phys. Chem. 2022, 96, 1148–1155. [Google Scholar] [CrossRef] [Scilit]
- Iwasaki, T.; Shimizu, K.; Nakamura, H.; Watano, S. Novel mechanochemical process for facile and rapid synthesis of a Co–Fe layered double hydroxide. Mater. Lett. 2012, 68, 406–408. [Google Scholar] [CrossRef] [Scilit]
- Kaczmarek, W.A. Structural and magnetic properties of cobalt-doped iron oxide particles prepared by novel mechanochemical method. J. Magn. Magn. Mater. 1996, 157–158, 264–265. [Google Scholar] [CrossRef] [Scilit]
- Lemoine, K.; Inaguma, Y.; Heidary, N.; Kornienko, N. Mechanochemical synthesis of cobalt/copper fluorophosphate generates a multifunctional electrocatalyst. Chem. Commun. 2020, 56, 9276–9279. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Xu, W.-C.; Zhang, Z.-M.; Yang, C.-H.; Zhao, K.-M.; Wang, Y.; Tian, N.; Zhou, Z.-Y.; Sun, S.-G. Promotion mechanism of PtCo intermetallic ordered alloys in oxygen reduction reaction and its application in fuel cells. Electrochem. Commun. 2023, 152, 107516–107522. [Google Scholar] [CrossRef] [Scilit]
- Lui, B.; Chen, Y.; Zhu, Y.; Zhao, H.; Gui, S.; Yue, Z.; Cheng, Q.; Yang, H. Heteronuclear inorganic molecule enables the direct synthesis of PtCo intermetallic compounds for proton exchange membrane fuel cells. J. Mater. Chem. A 2025, 13, 3295–3301. [Google Scholar] [CrossRef] [Scilit]
- Bai, L.; Hsu, C.-S.; Alexander, D.T.L.; Chen, H.M.; Hu, X. A Cobalt–Iron Double-Atom Catalyst for the Oxygen Evolution Reaction. J. Am. Chem. Soc. 2019, 141, 14190–14199. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Kahani, S.A.; Shahrokh, M. Preparation and characterization of Cu–Co alloy nanoparticles from double complex salts by chemical reduction. New J. Chem. 2015, 39, 7916–7922. [Google Scholar] [CrossRef] [Scilit]
- Domonov, D.P.; Pechenyuk, S.I.; Semushina, Y.P.; Yusenko, K.V. Solid-State Transformations in Inner Coordination Sphere of [Co(NH3)6][Fe(C2O4)3]·3H2O as a Route to Access Catalytically Active Co-Fe Materials. Materials 2019, 12, 221. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Culita, D.C.; Patron, L.; Teodorescu, V.S.; Balint, I. Synthesis and characterization of spinelic ferrites obtained from coordination compounds as precursors. J. Alloys Compd. 2007, 432, 211–216. [Google Scholar] [CrossRef] [Scilit]
- Gosteva, A.; Kalinkin, A.M.; Vinogradov, V.; Manukovskaya, D.; Nikolaev, V.; Semushin, V.; Teplonogova, M. The Influence of Mechanochemical Activation on the Properties of a Double Complex Salt [Co(NH3)6][Fe(CN)6] and Its Thermolysis Products. Thermo 2026, 6, 7. [Google Scholar] [CrossRef] [Scilit]
- Matiková Maľarová, M.; Černák, J.; Matik, M.; Briančin, J.; Varret, F. Thermal properties of four Co/Fe complexes based on amine-type and cyanido ligands. J. Therm. Anal. Calorim. 2019, 136, 703–715. [Google Scholar] [CrossRef] [Scilit]
- Gosteva, A.N.; Kulikova, M.V.; Semushina, Y.P.; Chudakova, M.V.; Tsvetov, N.S.; Semushin, V.V. Catalytic Activity of Thermolyzed [Co(NH3)6][Fe(CN)6] in CO Hydrogenation Reaction. Molecules 2021, 26, 3782. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Trávníček, Z.; Zbořil, R.; Matiková-Maľarová, M.; Drahoš, B.; Černák, J. Thermal decomposition of [Co(en)3][Fe(CN)6]·2H2O: Topotactic dehydration process, valence and spin exchange mechanism elucidation. Chem. Cent. J. 2013, 7, 28–45. [Google Scholar] [CrossRef] [Scilit] [PubMed][Green Version]
- Pechenyuk, S.I.; Domonov, D.P.; Shimkin, A.A.; Semushina, Y.P.; Ivanov, Y.V. Thermal Behavior of Binary Complex Compounds Containing the Hexacyanoferrate Anion. Russ. J. General. Chem. 2017, 87, 2212–2223. [Google Scholar] [CrossRef] [Scilit]
- Pechenyuk, S.I.; Domonov, D.P.; Semushina, Y.P.; Tsvetov, N.S.; Kadyrova, G.I.; Belyaevskii, A.T. Metal-carbon compositions as thermolysis products of complex compounds [Co(A)6]x[Fe(CN)6]y•nH2O (A = NH3, en/2). Thermochim. Acta 2021, 703, 179009–179017. [Google Scholar] [CrossRef] [Scilit]
- Semushina, Y.P.; Plyusnin, P.E.; Shubin, Y.V.; Pechenyuk, S.I.; Ivanov, Y.V. Thermal Decomposition of [Co(NH3)6][Fe(C2O4)3]·3H2O in Inert and Reductive Atmospheres. Russ. Chem. Bull. 2015, 64, 1963–1966. [Google Scholar] [CrossRef] [Scilit]
- Ingier-Stocka, E.; Maciejewski, M. Thermal decomposition of [Co(NH3)6]2(C2O4)3·4H2O: I. Identification of the solid products. Thermochim. Acta 2000, 354, 45–57. [Google Scholar] [CrossRef] [Scilit]
- Salehirad, A.; Latifi, S.M.; Miroliaee, A. Ion-pair complex precursor route for fabrication of high temperature shift Fe–Cr nanocatalyst. Mater. Res. Bull. 2014, 59, 104–110. [Google Scholar] [CrossRef] [Scilit]
- Seitz, K.; Peschel, S.; Babel, D. On the Crystal of the Cyano Complexes [Co(NH3)6][Fe(CN)6], [Co(NH3)6]2[Ni(CN)4]3·2H2O, and [Cu(en)2][Ni(CN)4]. Z. Fur Anorg. Und Allg. Chem. 2001, 627, 929–934. (In German) [Google Scholar] [CrossRef]
- Khalil, L.H.; Mousssa, N.A.; Mikhail, S. Thermal, Structural and Textural Studies on the Double Complex Salt [Co(NH3)6][Fe(CN)6] and on its Silica-Supported Catalysts. J. Mater. Sci. 1992, 27, 557–568. [Google Scholar] [CrossRef] [Scilit]
- Khassin, A.A.; Pechenyuk, S.I.; Domonov, D.P.; Minyukova, T.P.; Chermashentseva, G.K.; Kustova, G.N.; Plysova, L.M. Catalytic properties of bimetallic catalysts based on binary complexes of transition metals in Fischer-Tropsch synthesis. Chem. Sustain. Dev. 2007, 15, 673–683. [Google Scholar]
- Zhang, D.; Si, W.; Wang, P.; Chen, X.; Jiang, J. 1D to 3D Heterobimetallic Complexes Tuned by Cyanide Precursors: Synthesis, Crystal Structures, and Magnetic Properties. Inorg. Chem. 2014, 53, 3494–3502. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Wang, J.-H.; Javed, M.K.; Li, J.-X.; Zhang, Y.-Q.; Li, Z.-Y.; Yamashita, M. Ferromagnetically coupled single-chain magnets exhibiting a magnetic hysteresis of 0.42 Tesla in cyano-bridged FeIII2MII (M = Ni, Fe) coordination polymers. Dalton Trans. 2023, 52, 15510–15517. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Huang, H.-Y.; Li, H.; Cai, X.; Chan, S.; Zheng, S.; Li, L.; Cen, P.; Chen, L. Syntheses, crystal structures, and magnetic properties of cyanido-bridged one- and two-dimensional Ln(III)-Fe(III) coordination polymers. Inorganica Chim. Acta 2025, 581, 122621–122636. [Google Scholar] [CrossRef] [Scilit]
- Saritha, A.; Raju, B.; Ramachary, M.; Raghavaiah, P.; Hussain, K.A. Synthesis, crystal structure and characterization of chiral, three-dimensional anhydrous potassium tris(oxalato)ferrate(III). Phys. B Condens. Matter 2012, 407, 4208–4213. [Google Scholar] [CrossRef] [Scilit]
- Rao, C.N.R.; Natarajan, S.; Vaidhyanathan, R. Metal Carboxylates with Open Architectures. Angew. Chem. Int. Ed. 2004, 43, 1466–1496. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Gosteva, A.N.; Kulikova, M.V.; Svidersky, S.A.; Grabchak, A.A.; Lapuk, S.E.; Gerasimov, A.V. CO2 hydrogenation on catalysts based on Fe–Co double complex salts. Mendeleev Commun. 2026, 36, 101–103. [Google Scholar] [CrossRef] [Scilit]
- Gosteva, A.N.; Kulikova, M.V.; Ivantsov, M.I.; Grabchak, A.A.; Semushina, Y.P.; Lapuk, S.E.; Gerasimov, A.V.; Tsvetov, N.S. CO2 Hydrogenation over Fe-Co Bimetallic Catalyst Derived from the Thermolysis of [Co(NH3)6][Fe(CN)6]. Catalysts 2023, 13, 1475. [Google Scholar] [CrossRef] [Scilit]
- Domonov, D.; Pechenyuk, S. Thermolysis Products of Double Complex Compounds as Precursors of Metal-Carbon Composites. J. Mater. Sci. Appl. 2024, 8, 1–10. [Google Scholar] [CrossRef] [Scilit]
- Gosteva, A.; Lapuk, S.; Gerasimov, A. Kinetics of Complex Double Salts [Co(A)3][Fe(C2O4)3]·xH2O (A=2NH3, En (Ethylenediamine)). Thermo 2025, 5, 50. [Google Scholar] [CrossRef] [Scilit]
- Yusenko, K.V.; Pechenyuk, S.I.; Vikulova, E.S.; Semushina, Y.P.; Baidina, I.A.; Filatov, E.Y. Isostructurality and Thermal Properties in the Series of Double Complex Salts [M1(NH3)6][M2(C2O4)3]·3H2O (M1 = Co, Ir, M2 = Fe, Cr). J. Struct. Chem. 2019, 60, 1062–1071. [Google Scholar] [CrossRef] [Scilit]
- Zyryanov, V.V. Mechanochemical Synthesis of Complex Oxides. Russ. Chem. Rev. 2008, 77, 105–135. [Google Scholar] [CrossRef] [Scilit]
- Petříček, V.; Dušek, M.; Palatinus, L. Crystallographic computing system JANA2006: General features. Z. Krist. Cryst. Mater. 2014, 229, 345–352. [Google Scholar] [CrossRef] [Scilit]
- Petříček, V.; Palatinus, L.; Plášil, J.; Dušek, M. Jana 2020—A new version of the crystallographic computing system Jana. Z. Krist. Cryst. Mater. 2023, 238, 271–282. [Google Scholar] [CrossRef] [Scilit]
- Le Bail, A. Whole powder pattern decomposition methods and applications: A retrospection. Powder Diffr. 2005, 20, 316–326. [Google Scholar] [CrossRef] [Scilit]
- Eksperiandova, L.P.; Fedorov, O.I.; Stepanenko, N.A. Estimation of metrological characteristics of the element analyzer EuroVector EA-3000 and its potential in the single-reactor CHNS mode. Microchem. J. 2011, 99, 235–238. [Google Scholar] [CrossRef] [Scilit]
- Kristian, N. Synthesis and Structural Characterization of Complex Salts [Co(NH3)6][Fe(C2O4)3] and [CoC2O4(NH3)4][Fe(C2O4)2(OH2)2]. Master’s Thesis, University of Zagreb, Zagreb, Croatia, October 2017. [Google Scholar]
- Pechenyuk, S.I.; Semushina, Y.P.; Mikhalkova, N.L.; Ivanov, Y.V. Binary complexes [Co(a)6][M(C2O4)3] (a = NH3, 1/2C2H8n2, M = Fe, Cr): Synthesis, properties, and thermal decomposition. Russ. J. Coord. Chem. 2015, 41, 175–181. [Google Scholar] [CrossRef] [Scilit]
- Ndong, P.; Signé, M.; Kenfack, P.; Mbiangué, Y.; Bebga, G.; Wenger, E. A Novel Chromium(III) Hybrid Salt, Triethylammonium Trans-Diaquabis(Oxalato-κ2O1,O2) Chromate(III), (C6H16N)[Cr(C2O4)2(H2O)2]: Synthesis, Spectroscopic Studies, Thermal Behavior and Crystal Structure. Open J. Inorg. Chem. 2020, 10, 39–51. [Google Scholar] [CrossRef]
- Abraham, S.; Aruldhas, G. Infrared and polarized Raman spectra of M(HCOO)2·2(NH2)2CO [M = Cd, Mn]. Spectrochim. Acta 1995, 51, 79–88. [Google Scholar] [CrossRef] [Scilit]
- Sacconi, L.; Sabatini, A. The Infra-red spectra of metal(II)-hydrazine complexes. J. Inorg. Nucl. Chem. 1963, 25, 1389–1393. [Google Scholar] [CrossRef] [Scilit]
- Teleb, S.M. Preparation, spectroscopic and thermal studies on the new solid complex Co2(NH2)2(H2O)2(SO4)2. Thermochim. Acta 1993, 228, 131–136. [Google Scholar] [CrossRef] [Scilit]
- Gabal, M.A.; El-Bellihi, A.A.; Ata-Allah, S.S. Effect of Calcination Temperature on Co(II) Oxalate Dihydrate–Iron(II) Oxalate Dihydrate Mixture. Mater. Chem. Phys. 2003, 81, 84–92. [Google Scholar] [CrossRef] [Scilit]
- Feng, Y.; Hu, T.; Pu, Z.; Wu, M.; Mi, J. Non-Isothermal Decomposition Kinetics of FeC2O4·2H2O Prepared by Solid-State Method Aiming at the Formation of Fe2O3. J. Therm. Anal. Calorim. 2015, 122, 947–953. [Google Scholar] [CrossRef] [Scilit]
- Farhadi, S.; Pourzare, K.; Sadeghinejad, S. Simple preparation of ferromagnetic Co3O4 nanoparticles by thermal dissociation of the [CoII(NH3)6](NO3)2 complex at low temperature. J. Nanostructure Chem. 2013, 3, 16–22. [Google Scholar] [CrossRef] [Scilit]
- Nakagawa, I. Far infrared and raman spectra of K3[Co(CN)6] and [Co(NH3)6][Co(CN)6]. Bull. Chem. Soc. Jpn. 1973, 46, 3690–3693. [Google Scholar] [CrossRef] [Scilit]
- Lobo, S.L.; Kalainathan, S.; Kumar, A.R. Investigation of electrical studies of spinel FeCo2O4 synthesized by sol–gel method. Superlattices Microstruct. 2015, 88, 116–126. [Google Scholar] [CrossRef] [Scilit]
- Rao, V.S.; Prasad, V.; Rao, A.R.; Kumar, K.A.; Mohan, T.M. Effect of Zn2+ substitution on DC electrical resistivity and magnetic properties of Mg0.5−xZnxCo0.5Fe2O4 nano ferrite. J. Mater. Sci. Mater. Electron. 2024, 35, 1398–1410. [Google Scholar] [CrossRef] [Scilit]
- Balamurugan, S.; Giribha, N.; Ashika, S.A. Octahedron-Shaped Nano FeCo2O4 Phase Materials: Wet Chemical Synthesis and Characterization Studies. Curr. Nanomater. 2023, 8, 69–76. [Google Scholar] [CrossRef] [Scilit]
- Bereczki, L.; Petruševski, V.M.; Franguelli, F.P.; Béres, K.A.; Farkas, A.; Holló, B.B.; Czégény, Z.; Szilágyi, I.M.; Kótai, L. [Hexaamminecobalt(III)] Dichloride Permanganate–Structural Features and Heat-Induced Transformations into (CoII,MnII)(CoIII,MnIII)2O4 Spinels. Inorganics 2022, 10, 252. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.