Skip to Content
CivilEngCivilEng
  • Article
  • Open Access

1 October 2026

12 Pages

The Preparation of the Engineered Geopolymer Composites and Their Tensile Strain Capacity Research

,
and
1
School of Architecture and Civil Engineering, Huangshan University, 39 Xihai Road, Huangshan 245041, China
2
Department of Engineering Geology, Technical University of Berlin, Ernst-Reuter-Platz 1, 10587 Berlin, Germany
*
Author to whom correspondence should be addressed.

Abstract

This study optimized the mix proportions of ultra-high-toughness fly ash-based geopolymer composites (EGC) and investigated the effects of sub-elevated temperature curing on its tensile properties using dumbbell-shaped tensile tests, microstructural analysis, and Digital Image Correlation (DIC). The results indicate that fiber incorporation significantly mitigates matrix brittleness, enabling EGC to achieve an ultimate tensile strain of up to 4.5%. Under ambient curing, both tensile strength and strain capacity improved with age. Sub-elevated temperature curing markedly enhanced early-age mechanical properties; at later ages, tensile strength further increased while strain capacity slightly declined. Microstructural analysis revealed that sub-elevated temperature curing accelerated geopolymerization, resulting in a denser matrix, with DIC confirming that EGC’s high ductility stems from multiple micro-cracking propagation. By adopting the Menetrey–Willam damage model, numerical simulations successfully captured the stress concentration and damage redistribution process, mechanically confirming the pseudo-plasticity and multiple damage evolution of EGC.

1. Introduction

Engineered cementitious composites (ECC) have gained widespread attention in structural engineering due to their high damage tolerance, ultra-high tensile strain capacity, and unique pseudo-strain-hardening behavior accompanied by saturation multiple cracking. However, traditional ECC formulations rely heavily on high volumes of Ordinary Portland Cement (OPC), leading to substantial carbon emissions, high embodied energy, and adverse environmental impacts during raw material extraction and clinker calcination. To foster green and low-carbon development within the construction sector, using fly ash-based alkali-activated geopolymers as a complete replacement for the OPC matrix to synthesize Engineered Geopolymer Composites (EGC) has emerged as a highly promising direction [1,2,3,4,5]. Geopolymers utilize industrial solid wastes through alkaline activation to build three-dimensional silico-aluminate inorganic polymer networks, offering lower carbon footprints, superior fire resistance, and excellent chemical durability compared to conventional cementitious matrices.
Nevertheless, the mechanical performance and strain-hardening behavior of EGC are highly sensitive to precursor mix proportions, liquid-to-solid ratios, and the chemical composition of the fly ash matrix. Furthermore, in real-world structural applications, prefabricated elements, or specialized industrial environments, these materials are frequently subjected to thermal curing regimes or sub-high temperature exposure during early hydration stages. While elevated temperatures can accelerate the geopolymerization process and modify matrix porosity, their exact influences on the fiber-matrix interfacial bond, microstructural evolution, and long-term uniaxial tensile ductility under sub-high temperatures remain inadequately understood. Unbalanced matrix strength or damaged fiber-matrix interfaces under thermal conditions can easily lead to localized premature rupture rather than desirable multiple cracking.
To address these critical knowledge gaps, this study optimizes the precursor mix proportion to prepare ultra-high-ductility EGC specimens and systematically investigates the effects of sub-high temperature baking duration on their tensile strength, crack spacing, and strain capacity. Additionally, high-resolution Digital Image Correlation (DIC) is employed to track crack initiation, multi-crack propagation, and surface strain field evolution during uniaxial tension in real time, aiming to elucidate the physical mechanism of thermal-induced tensile performance variation and provide a technical foundation for structural design, numerical modeling, and practical application under specific thermal environments [6,7,8,9,10,11].

2. Experiment

2.1. Raw Materials and Mix Proportions

The main raw materials used in this study included low-calcium fly ash (LFA) produced by Shandong Tianyan Mining Co., Ltd. (Rizhao, China), high-calcium fly ash (HFA) produced by Jiangsu Sobute New Materials Co., Ltd. (Nanjing, China), sodium hydroxide (NaOH) produced by Linyi Lvsente (Linyi, China), water glass produced by Dongyue Group (Zibo, China), Kuralon-II REC-15 PVA fibers produced by Kuraray Co., Ltd. (Tokyo, Japan), fine aggregate (sand), and tap water. The chemical compositions of the fly ash used in the experiment are listed in Table 1, and the physical and mechanical properties of the PVA fibers are shown in Table 2.
Table 1. Chemical compositions of fly ash wt. %.
Table 2. Physical and mechanical characteristics of PVA fiber.
In the preparation of Engineered Geopolymer Composites (EGC), using LFA alone leads to an excessively long setting time of the binder and low demolding strength. Conversely, using HFA alone causes rapid setting, which adversely affects specimen molding [12]. Therefore, this study employed a blend of HFA and LFA as the aluminosilicate precursor raw materials for EGC. As shown in Table 1, the CaO contents of HFA and LFA are 13.22% and 3.49%, respectively. According to the Chinese standard GB/T 1596—2017 (fly ash used for cement and concrete), they can be classified as Class C (high-calcium) and Class F (low-calcium) fly ash, respectively. Combined with preliminary exploratory orthogonal tests, the final mix proportions of EGC are presented in Table 3.
Table 3. Mix design proportion by weight for EGC wt. %.

2.2. Specimen Preparation

According to the mix proportions given in Table 3, LFA, HFA, and sand were weighed in sequence and poured into a 5 L mortar mixer, followed by slow dry mixing for 2–4 min until homogeneous. Subsequently, the pre-prepared alkaline activator solution (prepared by mixing sodium hydroxide, water, and water glass in proportion) was poured in, and fast wet mixing was performed for 3–5 min. Once the binder slurry reached the desired fluidity (uniform, clump-free, and exhibiting good flow behavior), the PVA fibers were added gradually and evenly. Fast mixing was continued for another 5–8 min until the fibers were fully dispersed in the mortar without any agglomeration or balling. After mixing was completed, the fresh mixture was cast into dog-bone (dumbbell-shaped) molds for shaping (as shown in Figure 1).
Figure 1. Dimensions of the dumbbell type mold unit: mm.

2.3. Experimental Design

2.3.1. Curing Regimes

After vibration compaction and initial surface smoothing, all specimens in their molds were sealed with plastic film to prevent moisture evaporation. After 24 h of initial setting, the specimens were demolded and cured according to their predefined curing regimes. To investigate the effect of thermal curing duration at a constant elevated temperature on tensile performance, the specimens were divided into four groups (the detailed curing schemes are illustrated in Figure 2):
Figure 2. Specimen conservation system.
Standard Curing Group (R): Specimens were kept demolded and cured in a standard laboratory environment at an ambient temperature of 20 ± 2 °C and a relative humidity (RH) of 60 ± 5% until tensile testing at curing ages of 3, 7, and 28 days.
Thermal Curing Groups (T60-2, T60-4, and T60-6): After demolding, specimens were placed in an electric thermostatic oven at 60 ± 1 °C for thermal treatment lasting 2, 4, and 6 h, respectively. Upon completion of thermal curing, the specimens were removed from the oven and subsequently stored under the same ambient indoor conditions (20 ± 2 °C and 60 ± 5% RH) until tested at 3, 7, and 28 days.

2.3.2. Direct Uniaxial Tensile Test

After curing under different regimes and to specified ages, the specimens were subjected to direct uniaxial tensile tests using an electronic universal testing machine (Jinan Chuanbai Instrument Equipment Co., Ltd., Jinan, China), as shown in Figure 3. The test was conducted under displacement control at a loading rate of 0.3 mm/min. Two linear variable displacement transducers (LVDTs) were mounted on the specimen to measure the displacement over a gauge length of 80 mm.
Figure 3. Setup of uniaxial direct tensile test.

2.3.3. Microscopic Analysis

The changes in the macroscopic physical and mechanical properties of the EGC subjected to sub-high temperatures are fundamentally attributed to the evolution of its internal microstructure. In this study, a research-grade intelligent stereomicroscope was utilized to observe the surfaces of the EGC specimens after various treatments. Images of the surface micromorphology and crack characteristics were captured at a magnification of 30×.

2.3.4. Crack Morphology and Strain Field Analysis

Digital Image Correlation (DIC, as shown in Figure 4), a non-contact optical measurement technique, was employed to analyze the crack morphology and surface strain fields of the specimens. DIC tracks and compares the grayscale intensity distributions within local subsets between undeformed and deformed digital images to determine spatial strain. Prior to testing, a random black-and-white speckle pattern was sprayed onto the specimen surface (Figure 5) to ensure a unique intensity profile for each subset. To capture these surface speckles with high spatial fidelity, digital images were acquired at a maximum resolution of 6000 × 4000 pixels (24.2 megapixels) under uniform LED illumination. During the uniaxial tensile test, a digital camera mounted on a tripod was positioned adjacent to the testing frame, capturing images at an interval of 20 s via remote control. In this study, the commercial software Vic-2D was utilized for two-dimensional image post-processing to quantify the in-plane deformations. Given that the thickness of the specimen was small relative to its other dimensions, out-of-plane displacement was assumed to be negligible during uniaxial tension.
Figure 4. Digital Image Correlation instruments.
Figure 5. Inkjet processing of the specimen.

3. Results and Discussion

3.1. Effect on Uniaxial Tensile Performance

The processed experimental data from the uniaxial tensile tests are summarized in detail in Table 4, Table 5 and Table 6.
Table 4. Tensile properties of R, 60-2, T60-4 and T60-6 at the age of 3 days.
Table 5. Tensile properties of R, 60-2, T60-4 and T60-6 at the age of 7 days.
Table 6. Tensile properties of R, 60-2, T60-4 and T60-6 at the age of 28 days.
As shown in Table 4, at 3 days of curing, both the tensile strength and tensile strain of the EGC increased significantly with the duration of sub-high temperature exposure. Compared with the ambient-cured control group (R), the average tensile strength of the T60-2, T60-4, and T60-6 groups increased by 30%, 155%, and 285%, respectively, while their average tensile strains increased by 30%, 25%, and 50%, respectively. Notably, the T60-6 group exhibited superior overall performance, achieving an average tensile strength of 3.62 MPa and an average strain of 4.19%, indicating simultaneous enhancements in stiffness and toughness.
As indicated in Table 5, at 7 days of curing, the tensile properties fluctuated with thermal curing duration. Compared to the R group, the average tensile strength of the T60-2 group decreased slightly by 2%, whereas those of the T60-4 and T60-6 groups increased by 43% and 75%, respectively. Regarding deformability, the average strain of the T60-2, T60-4, and T60-6 groups decreased by 1%, 12%, and 5%, respectively, relative to the R group. Among them, the R group exhibited excellent strain capacity (average strain of 4.11%), whereas the T60-6 group maintained high tensile strength (average strength of 4.13 MPa).
As presented in Table 6, at 28 days of curing, the average tensile strength of the T60-2 group was comparable to that of the R group, while the T60-4 and T60-6 groups exhibited increases of 23% and 35%, respectively. Conversely, the average strains of the T60-2, T60-4, and T60-6 groups decreased by 19%, 17%, and 11%, respectively, compared with the R group.
In summary, appropriate sub-high temperature treatment significantly improves both the tensile strength and strain capacity of EGCs at early ages (3 d). For long-term curing (28 d), thermal treatment continues to enhance tensile strength, albeit with a slight reduction in ultimate strain capacity. These results indicate that the influence of thermal curing duration on EGC ductility is non-monotonic and non-linear, highlighting the importance of an optimized sub-high temperature regime for enhancing the overall tensile performance.
The tensile stress–strain curves of the R, T60-2, T60-4, and T60-6 specimens are presented in Figure 6, Figure 7, Figure 8 and Figure 9, respectively. Under uniaxial tension, the failure process of EGC can be characterized by three distinct stages: the elastic stage, the multiple cracking stage (strain-hardening stage), and the failure stage. In the elastic stage, the specimen exhibits a rapid increase in stiffness with minimal strain variation and no crack formation, demonstrating linear elastic behavior similar to that of conventional concrete. In the multiple cracking stage, as the load increases, the first microcrack emerges, accompanied by a slight drop in stress. Subsequently, the fibers bridging the crack transfer the tensile stress, causing the stress to rise again. As the number of tensile microcracks increases, the stress–strain curve exhibits a characteristic serrated fluctuation. In the failure stage, as crack development progresses, one of the cracks localizes and widens into a major crack, eventually leading to the fracture of the specimen. During this process, numerous fine and uniformly distributed microcracks can be observed parallel to the main crack within the effective gauge length of the specimen (as shown in Figure 10).
Figure 6. Stress–strain diagram of R specimens at 3 d, 7 d and 28 d.
Figure 7. Stress–strain diagram of T60-2 specimens at 3 d, 7 d and 28 d.
Figure 8. Stress–strain diagram of T60-4 specimens at 3 d, 7 d and 28 d.
Figure 9. Stress–strain diagram of T60-6 specimens at 3 d, 7 d and 28 d.
Figure 10. Stretched specimen.
From 3 days to 28 days of curing, both the tensile strength and strain capacity of the R specimens improved substantially. Among the thermally treated groups, the T60-2 specimens exhibited a significant increase in tensile strength but little change in strain. The T60-4 specimens showed a marginal improvement in the tensile strength with negligible variation in strain, while the T60-6 specimens demonstrated no obvious changes in either strength or strain over time. According to the micromechanics theory proposed by Prof. Victor C. Li from the University of Michigan [13], the fiber bridging effect at the crack interfaces governs the composite’s cracking behavior, and the ultimate tensile strength is determined by this fiber bridging capacity. Specimens with higher bridging stress are more prone to developing saturated multiple cracking. Based on the tensile strength and crack distribution characteristics of the fly ash-based geopolymers observed in this study, the sub-high temperature treatment effectively enhanced the fiber-matrix bridging stress in EGCs. Consequently, the thermally treated specimens exhibited superior strain-hardening characteristics compared to the ambient-cured specimens.

3.2. Effect of Sub-High Temperature Treatment on EGC Surface Morphology

Following the sub-high temperature treatment, the EGC matrix exhibited negligible volumetric change, and the surface color remained largely unchanged, presenting a grayish-white appearance. The surfaces of the specimens remained intact, with no evidence of spalling or cracking. Qualitative physical evaluation revealed that the surfaces of the R and T60-2 specimens were rougher than those of the T60-4 and T60-6 specimens. Microscopic observation of the 7-day specimen surfaces under a stereomicroscope at 30× magnification (as shown in Figure 11) indicated that the R specimens possessed significantly more surface pores compared to the other three groups. The T60-2 specimens exhibited only a minor number of pores, whereas the T60-4 and T60-6 specimens displayed a much more compact inter-crystalline structure on their surfaces.
Figure 11. Surface morphology of EGC specimens under different curing conditions at 7 days.

3.3. Crack Morphology Analysis via DIC

By observing the DIC strain contour maps, the initiation of the first microcrack can be clearly captured, thereby accurately determining the first-cracking stress. Figure 12 illustrates the surface strain field distributions of the T60-4 specimen at 28 days under various tensile strain levels. As the tensile stress increases, the number of surface microcracks multiplies continuously until the specimen fractures at an ultimate tensile strain of approximately 4.0%. According to the analytical results presented in Table 7, as the strain level increases from 1.0% to 4.0%, the maximum crack width increases by 42%, while the number of cracks surges by approximately 320% (from 11 to 42). This demonstrates that the macroscopic ductility of EGC is primarily derived from the proliferation of multiple microcracks rather than the widening of individual cracks. Furthermore, throughout the strain progression from 1.0% to 4.0%, the average crack width is consistently maintained at a stable level of approximately 45 μm. This engineered fly ash-based geopolymer composite exhibits superior crack-control performance compared to traditional cementitious engineered cementitious composites (ECC). Consequently, owing to this stringent restriction on crack widths, the fly ash-based EGC is highly likely to possess better long-term durability than conventional cement-based ECC. Further experimental investigations are warranted to systematically verify the durability performance of these fly ash-based geopolymers.
Figure 12. T60-4 specimen cloud change map at 28 days.
Table 7. Statistics of cracks in the specimen after tension at 28 days.

3.4. Finite Element Stress Field Analysis

A 1:1 full-scale 3D finite element model matching the specimen geometry was constructed, resulting in a mesh total of 23,002 elements. The fly ash-based geopolymer matrix was modeled using an isotropic elasticity formulation (E = 20,000 MPa, ν = 0.2) coupled with the Menetrey–Willam constitutive criteria, configured with a uniaxial compressive strength of 35 MPa, uniaxial tensile strength of 3 MPa, biaxial compressive strength of 40 MPa, a dilatancy angle of 0.52 rad, and a plastic strain at peak compressive strength of 0.0015. Meanwhile, the PVA fiber properties were defined with a density of 1.3 × 10−6 kg/mm3, a Young’s modulus of 42,800 MPa, a Poisson’s ratio of 0.35, and a tensile yield strength of 1600 MPa. The boundary conditions of the numerical model were specified to closely match the experimental setup. Transverse and normal displacements (Uz = Uy = 0) were constrained at the clamped ends, while a displacement-controlled load was applied along the longitudinal axis (X-axis) of the specimen until ultimate structural failure occurred. The specimen was discretized using 3D 10-node tetrahedral solid elements (SOLID187) under an automated meshing method in ANSYS Workbench. An adaptive default mesh sizing scheme (Resolution level 2) was applied, generating a refined tetrahedral mesh that effectively conforms to the complex dog-bone geometry and curved transitional shoulders.
Figure 13 illustrates the contour plot of the first principal stress (or equivalent stress) distribution for the dumbbell-shaped ECC specimen under uniaxial tensile loading. As can be observed, the maximum stress during the loading process reaches 3.22 MPa, which exceeds the initial cracking tensile strength of the fly ash matrix (3.0 MPa). This indicates that the specimen has entered the stage of matrix cracking and fiber bridging stress transfer.
Figure 13. Equivalent stress distribution contour of specimen during tensile failure process.
Regarding the spatial stress distribution characteristics, the gauge section (parallel section) of the specimen exhibits excellent stress redistribution, with the stress in the main body maintained at a high level of 1.80 MPa to 2.51 MPa. This demonstrates that the Menetrey–Willam constitutive model, combined with the tension softening criterion, successfully simulates the stress transfer process following matrix cracking.
It is worth noting that the maximum stress of 3.22 MPa occurs at the transition arc of the varying cross-section, which aligns with the stress concentration effect in continuum mechanics. This suggests that in the geometrically discontinuous region, the matrix reaches its tensile limit first and initiates microcracks. Subsequently, through the bridging effect of the PVA fibers, the tensile stress is transferred to the central gauge section and its surroundings. This mechanism effectively prevents early brittle fracture of the specimen, fully demonstrating the typical multiple cracking and pseudo strain-hardening (or pseudo-plastic deformation) characteristics of ECC materials.

4. Conclusions

Based on the present study, the following main conclusions can be drawn: (1) EGC combines the advantages of traditional engineered cementitious composites (ECC) and geopolymers, exhibiting distinct multiple cracking characteristics and strain-hardening behavior, with a maximum tensile strain reaching up to 4.5%. (2) Under ambient temperature curing conditions, both the tensile stress and strain capacity of EGC increase with the extension of curing age. (3) Following sub-high temperature treatment, both the stress and strain of EGC are significantly enhanced at an early age. At later ages, the stress continues to improve, whereas the strain capacity experiences a slight reduction. (4) Microstructural analysis indicates that appropriate thermal treatment in a 60 °C oven densifies the EGC matrix. Digital Image Correlation (DIC) analysis further reveals that the enhanced ductility of EGC is primarily attributed to the proliferation of multiple microcracks. (5) The established numerical model can effectively simulate the stress distribution and the evolution process of multiple cracking in EGC under tensile loading.

Author Contributions

Conceptualization, C.X.; methodology, C.X.; software, C.X.; validation, Q.W.; formal analysis, Q.W. and D.Y.; investigation, Q.W.; resources, C.X.; data curation, C.X.; writing—original draft preparation, C.X.; writing—review and editing, Q.W.; visualization, C.X.; supervision, Q.W.; funding acquisition, Q.W. All authors have read and agreed to the published version of the manuscript.

Funding

Scientific Research Start-up Project of Huangshan University: Grant No. 2025xkjq013; Technology Development Project of Huangshan University: Grant No. hxkt2026098; Science and Technology Project of Huangshan Municipal Bureau of Science and Technology: Grant No. 2025-Z18; General Research Project of Huangshan University: Grant No. KJHS2021B13.

Institutional Review Board Statement

Not applicable.

Data Availability Statement

The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding author.

Conflicts of Interest

The authors declare no conflicts of interest.

References

  1. Kan, L.L.; Shi, H.S. Investigation of self-healing behavior of Engineered Cementitious Composites (ECC) materials. Constr. Build. Mater. 2012, 29, 348–356. [Google Scholar] [CrossRef] [Scilit]
  2. Kan, L.; Qiao, H.Z.; Wang, F. Combination of Slag and Fly Ash to Prepare Engineered Cementitious Composite: A Study on Mechanical Properties and Gas Permeability. J. Mater. Civ. Eng. 2023, 35, 04023064. [Google Scholar] [CrossRef] [Scilit]
  3. Lin, J.; Yu, J.; Li, V.C. Mechanical properties of PVA fiber reinforeed engineered cementhious composites after thermal treatment. Acta Mater. Compos. Sin. 2016, 33, 116–122. (In Chinese) [Google Scholar]
  4. Kim, J.K.; Kim, J.S.; Ha, G.J.; Kim, Y.Y. Tensile and fiber dispersion performance of ECC (engineered cementitious composites) produced with ground granulated blast furnace slag. Cem. Concr. Res. 2007, 37, 1096–1105. [Google Scholar] [CrossRef] [Scilit]
  5. Li, V.C. Monotonic and fatigue performance in bending of fiber-reinforced engineered cementitious composite in overlay system. Cem. Concr. Res. 2002, 32, 415–423. [Google Scholar] [CrossRef] [Scilit]
  6. Davidovits, J. Geopolymer Chemistry and Applications; Geopolymer Institute: Saint-Quentin, France, 2008. [Google Scholar]
  7. Fernández-Jiménez, A.; Palomo, A.; Criado, M. Microstructure development of alkali activated fly ash cement: A descriptive model. Cem. Concr. Res. 2005, 35, 1024–1029. [Google Scholar] [CrossRef] [Scilit]
  8. Kan, L.; Wang, F.; Zhang, Z.; Wilson, K.; Zhao, Y. Mechanical properties and microstructural characteristics of fly ash based PVA fiber reinforced Engineered Geopolymer Composites. Constr. Build. Mater. 2021, 298, 123880. [Google Scholar]
  9. Saha, S.; Rajasekaran, C. Enhancement of the properties of fly ash based geopolymer paste by incorporating ground granulated blast furnace slag. Constr. Build. Mater. 2017, 146, 615–620. [Google Scholar] [CrossRef] [Scilit]
  10. Lee, B.Y.; Cho, C.G.; Lim, H.J.; Song, J.K.; Yang, K.H.; Li, V.C. Strain hardening fiber reinforced alkali-activated mortar—A feasibility study. Constr. Build. Mater. 2012, 37, 15–20. [Google Scholar] [CrossRef] [Scilit]
  11. Scrivener, K.L.; Kirkpatrick, R.J. Innovation in use and research on cementitious material. Cem. Concr. Res. 2008, 38, 128–136. [Google Scholar] [CrossRef] [Scilit]
  12. Ohno, M.; Li, V.C. A feasibility study of strain hardening fiber reinforced fly ash-based geopolymer composites. Constr. Build. Mater. 2014, 57, 163–168. [Google Scholar] [CrossRef] [Scilit]
  13. Li, V.C.; Wu, H.C.; Maalej, M.; Mishra, D.K.; Hashida, T. Tensile behavior of cement-based composites with random discontinuous steel fibers. J. Am. Ceram. Soc. 2010, 79, 74–78. [Google Scholar]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.