Skip to Content
CoatingsCoatings
  • Article
  • Open Access

29 August 2026

18 Pages

KH550-Modified Nano-ATO/Carbon Black Hybrid-Filled Epoxy Coatings with Enhanced Corona Inception Voltage and Thermal-Cycling Stability

,
,
,
,
and
1
School of Materials Science and Engineering, Xihua University, Chengdu 610039, China
2
Energy and Power College, Xingxin Vocational and Technical College of Xinjiang Production and Construction Corps Tiemenshi, Xinjiang Production and Construction Corps, Tiemenguan City 841007, China
3
Dongfang Electric Corporation Dongfang Electric Machinery Co., Ltd., Deyang 618000, China
4
The Laboratory of Advanced Energetic Materials and Devices, Xihua University, Chengdu 610039, China

Highlights

What are the main findings?
  • The ATO/carbon black ratio non-monotonically regulated surface resistance and CIV.
  • A3C7 achieved a surface resistance of 1.17×104Ω and the highest CIV of 2.58 kV.
  • A3C7 increased CIV by 40.1% relative to A0C10 and limited resistance drift to 12.62% after 50 thermal cycles.
What are the implications of the main findings?
  • Partial replacement of carbon black with KH550-modified ATO provides a favorable balance between low resistance and corona inception performance.
  • Optimizing the hybrid-filler composition is more important than simply minimizing surface resistance.
  • The A3C7 formulation exhibits improved macroscopic electrical stability during repeated thermal cycling.

Abstract

Conventional carbon-black-based low-resistance anti-corona coatings can exhibit electrical properties that are sensitive to filler dispersion, particle spacing, interfacial conditions, and temperature-induced structural rearrangement. In this study, nano antimony-doped tin oxide (ATO) was surface-modified with γ-aminopropyltriethoxysilane (KH550) and used to partially replace carbon black in an E-51 epoxy matrix. The total hybrid-filler loading was fixed at 10 wt% relative to the mass of E-51 epoxy resin, while the ATO/carbon black mass ratio was varied from 0:10 to 10:0. Fourier transform infrared spectroscopy was used to examine the introduction of KH550-derived organosilane species onto ATO, and the coating formulations were screened by measuring surface resistance and corona inception voltage (CIV) under a needle–plate electrode configuration. The selected A3C7 coating was further compared with a commercial carbon-black-based low-resistance anti-corona coating through scanning electron microscopy and thermal cycling between 25 and 150 °C. A3C7 exhibited a surface resistance of (1.17 ± 0.07) × 104 Ω and the highest CIV of 2.58 ± 0.04 kV, representing a 40.1% increase relative to the carbon-black-only A0C10 coating. Relatively uniform circular or elliptical micron-scale features were observed on the A3C7 surface; however, their chemical origin could not be determined by conventional SEM. After 50 thermal cycles, the relative resistance change in A3C7 was 12.62% ± 1.19%, markedly lower than the 63.95% ± 6.76% obtained for the commercial coating. The corresponding CIV retentions were 91.86% and 82.40%, respectively. These results demonstrate that partial replacement of carbon black with KH550-modified ATO can provide a favorable balance among low surface resistance, increased CIV, and improved thermal-cycling electrical stability. The microscopic origin of this behavior remains to be clarified by direct characterization of filler distribution and conductive pathways.

1. Introduction

High-voltage rotating machines rely on stator-bar insulation systems that operate under combined electrical, thermal, and mechanical stresses. Partial discharge and corona activity are important manifestations of insulation defects and degradation in generator stator bars and windings [1]. Local defects in the slot and end regions can distort the electric-field distribution and produce distinct discharge patterns [2]. Discharge behavior is also affected by the surrounding medium and operating temperature [3,4]. Sustained discharge may promote surface erosion, localized heating, and interfacial deterioration, thereby reducing the reliability and service life of the winding insulation.
In practical stator-bar insulation systems, corona protection is designed according to regional electric-field conditions. The semiconductive layer over the slot portion maintains electrical contact between the main-insulation surface and the grounded stator core, thereby reducing the potential difference across local air gaps and suppressing surface discharge [5]. By contrast, materials extending beyond the slot exit are used for gradual potential or stress grading because abrupt termination of the grounded slot coating can produce a high tangential electric field [6,7]. Accordingly, a slot-region low-resistance coating must provide a sufficiently low, uniform, and stable surface resistance rather than strong nonlinear field-grading behavior. The present study therefore focuses on the low-resistance slot coating and examines whether the partial replacement of carbon black with modified ATO can improve electrical stability without sacrificing surface-charge dissipation capability.
Carbon nanoparticles are widely used to impart electrical conductivity to epoxy matrices because continuous conductive pathways can be established at relatively low filler loadings [8]. In carbon black/epoxy systems, conductivity is strongly affected by curing-induced aggregation, filler content, dispersion state, and the resulting percolation structure [9,10]. Filler composition and particle morphology further regulate the continuity and efficiency of conductive pathways [11]. At the microscopic scale, electrical transport can involve direct particle contacts together with short-range transport across narrow polymer-rich gaps [12]. These network features make the resistance sensitive to structural rearrangement and temperature-dependent changes in particle spacing [13,14,15]. Consequently, a conductive network dominated by carbon black may exhibit resistance drift during repeated thermal cycling, which can limit the long-term stability of conventional low-resistance anti-corona coatings.
Antimony-doped tin oxide (ATO) is an n-type conductive oxide whose electrical behavior is associated with Sb-doped SnO2 structures [16,17]. Its electrical and mechanical characteristics have supported its use in functional coatings and polymer-based nanocomposites [18,19,20]. However, the high surface energy of nano-ATO promotes secondary agglomeration and may restrict conductive-network continuity. More specifically, several studies have explored ATO/carbon hybrid systems for improving electrical performance. Yang et al. [21] incorporated ATO and graphene nanosheets into an epoxy coating and reported enhanced electrostatic conductivity together with improved corrosion resistance. Wu et al. [22] prepared CNT/ATO composite films and showed that the introduction of modified CNTs markedly decreased the sheet resistance of the ATO-based films. Ren et al. [23] further demonstrated that combining ATO with reduced graphene oxide enhanced charge transport in ATO–RGO nanocomposites. Wang et al. [24] introduced ATO together with a silica@graphene hybrid into waterborne epoxy coatings and obtained improved antistatic performance. These studies demonstrate the potential of combining ATO with carbonaceous conductive components; however, their applications mainly concern antistatic, electrothermal, electrochemical, or anticorrosive systems rather than low-resistance anti-corona coatings for stator-slot insulation. In addition, amino-silane treatment has been used to improve the surface compatibility of inorganic particles with epoxy or related organic matrices [25,26,27,28]. These considerations suggest that KH550-modified ATO may serve as a thermally stable auxiliary semiconducting component while carbon black maintains the principal low-resistance pathways.
Existing studies have primarily addressed SiC-based stress-grading materials, carbon black/epoxy percolation, ATO-containing functional coatings, or silane-modified oxide/epoxy interfaces [7,9,15,25]. However, the partial replacement of carbon black with silane-modified ATO in low-resistance epoxy anti-corona coatings remains insufficiently understood. In particular, the relationships among the ATO/carbon black ratio, surface resistance, corona inception voltage, coating morphology, and thermal-cycling stability remain unclear. In this study, the total hybrid-filler loading was fixed at 10 wt%, while the ATO/carbon black mass ratio was varied from 0:10 to 10:0. Surface resistance and CIV were used to screen the formulations, and the selected A3C7 coating was compared with a commercial low-resistance coating through SEM observation and thermal cycling between 25 and 150 °C. The composition-dependent electrical behavior and possible roles of the two fillers were subsequently discussed based on the experimental results and relevant literature.

2. Materials and Methods

2.1. Raw Materials

Bisphenol A epoxy resin E-51 and its matched curing agent were supplied by Kunshan Jiulimei Electronic Materials Co., Ltd. (Kunshan, China). The epoxy equivalent weight of E-51 was 196 g/eq, and the recommended mass ratio of E-51 to the curing agent was 3:1. Nano antimony-doped tin oxide (ATO), with an average particle size of 20 nm and an Sb doping content of 10 wt%, was purchased from Shanghai Muheng New Materials Co., Ltd. (Shanghai, China). Conductive carbon black NCT-TY5 was supplied by Changzhou Tanbo New Materials Technology Co., Ltd. (Changzhou, China), with an average particle size of 100 nm and a specific surface area of 238 m2/g. γ-Aminopropyltriethoxysilane (KH550), absolute ethanol, and glacial acetic acid were obtained from Chengdu Kelong Chemical Co., Ltd. (Chengdu, China). A commercial room-temperature-curable low-resistance anti-corona coating, DECJ1344, was provided by Dongfang Electric Machinery Co., Ltd. (Deyang, China). All materials were used as received unless otherwise specified.

2.2. Surface Modification of Nano-ATO with KH550

Nano-ATO was surface-modified with KH550 through hydrolysis and condensation reactions [25,26]. First, 10.0 g of nano-ATO powder was dispersed in 200 mL of an ethanol/deionized-water mixture with a volume ratio of 9:1. The suspension was ultrasonicated for 30 min to reduce particle agglomeration and improve dispersion stability. The pH of the suspension was then adjusted to 4–5 using glacial acetic acid. Separately, 0.50 g of KH550 was added to a small amount of the same ethanol/deionized-water mixture and pre-hydrolyzed at pH 4–5 for 30 min. The hydrolyzed KH550 solution was subsequently added dropwise to the ATO suspension under continuous mechanical stirring. After the addition was completed, the mixture was maintained in a thermostatic water bath at 60 °C for 4 h to promote the interaction between the hydrolyzed silane molecules and the hydroxyl groups on the ATO surface. The reaction temperature of 60 °C was selected based on reported KH550 surface-treatment conditions and was not independently optimized in the present study. This moderate temperature was used to facilitate the hydrolysis/condensation reactions of the silane while avoiding excessively rapid self-condensation at higher temperatures. After the reaction, the suspension was cooled to room temperature and centrifuged to collect the solid product. The obtained powder was washed three times with absolute ethanol to remove unreacted or physically adsorbed silane species. The product was then dried in a vacuum oven at 80 °C for 12 h, ground, and passed through a 200-mesh sieve. The resulting KH550-modified nano-ATO was denoted as m-ATO. For comparison, unmodified ATO was subjected to the same dispersion, centrifugation, washing, drying, and sieving procedures without the addition of KH550 and was denoted as u-ATO. The preparation procedure of KH550-modified nano-ATO is schematically illustrated in Figure 1.
Figure 1. Preparation procedure of KH550-modified nano-ATO.

2.3. Preparation of ATO/Carbon Black/Epoxy Composite Coatings

The total loading of the m-ATO/carbon black hybrid filler was fixed at 10 wt% relative to the mass of E-51 epoxy resin. Accordingly, 10 parts by mass of the hybrid filler were added per 100 parts by mass of E-51. The m-ATO/carbon black mass ratios were designed as 0:10, 1:9, 2:8, 3:7, 4:6, 5:5, 6:4, 7:3, 8:2, 9:1, and 10:0. The corresponding samples were denoted as A0C10, A1C9, A2C8, A3C7, A4C6, A5C5, A6C4, A7C3, A8C2, A9C1, and A10C0, respectively. The detailed formulations are summarized in Table 1. Before mixing, m-ATO and carbon black were separately dried in a vacuum oven at 80 °C for 6 h to remove adsorbed moisture. The fillers were then weighed according to the designed mass ratios and manually ground together for 5 min. E-51 epoxy resin was preheated at 60 °C for 30 min to reduce its viscosity and improve filler wetting. The hybrid filler was divided into four portions and gradually introduced into the epoxy resin under stirring at 500 r/min. After complete addition, the mixture was further mechanically stirred at 600 r/min for 15 min while the temperature was maintained at approximately 60 °C. When the filled epoxy mixture had cooled to 35–40 °C, the curing agent was added at an E-51/curing-agent mass ratio of 3:1. The mixture was stirred at 400 r/min for 10 min. Before coating, the laminate substrates were lightly abraded with sandpaper, wiped with absolute ethanol to remove surface dust and contaminants, and then allowed to dry at room temperature before use. The same substrate-preparation procedure was applied to all specimens. The mixture was then uniformly coated onto the surfaces of the prepared laminate substrates. The coatings were cured at room temperature for 24 h to obtain the ATO/carbon black/E-51 composite anti-corona coatings. The dry coating thickness was determined using an electronic blade micrometer by subtracting the substrate thickness before coating from the total thickness after coating and curing at the corresponding positions. Measurements were performed at five positions, giving an average dry coating thickness of 39.6 ± 2.3 μm. The degree of cure was not independently quantified by residual-heat DSC or spectroscopic conversion analysis; therefore, the present study does not claim complete curing, and the term “cured coating” refers to specimens after the specified 24 h curing treatment. The commercial coating was prepared according to the manufacturer-recommended procedure. The preparation route of the hybrid-filled epoxy coatings, including filler drying, proportioning, mechanical mixing, curing-agent addition, substrate coating, and room-temperature curing, is presented in Figure 2.
Table 1. Formulations of the ATO/carbon black-filled E-51 epoxy coatings.
Figure 2. Preparation procedure of the ATO/carbon black hybrid-filled E-51 epoxy anti-corona coatings.

2.4. Characterization and Testing

2.4.1. Fourier Transform Infrared Spectroscopy

The surface chemical structures of u-ATO and m-ATO were characterized using a Vector 22 Fourier transform infrared spectrometer (Bruker Optik GmbH, Ettlingen, Germany). The samples were analyzed using the KBr pellet method over a wavenumber range of 4000–400 cm−1. The obtained spectra were normalized and vertically offset to facilitate comparison of the characteristic absorption bands.
FTIR was used to determine whether KH550-derived organic silane structures had been introduced onto the ATO surface. The resulting spectra and characteristic absorption bands are presented and discussed in Figure 3.
Figure 3. FTIR spectra of unmodified ATO (u-ATO) and KH550-modified ATO (m-ATO). The spectra were normalized and vertically offset for clarity; the band near 2350 cm−1 originated from atmospheric CO2.

2.4.2. Surface-Resistance Measurement

The surface resistance of the cured coatings was measured using a DEM21 digital multimeter (Delixi Electric Co., Ltd., Yueqing, China) and two parallel copper-strip electrodes. The effective electrode length was 40 mm, and the distance between the two electrodes was 10 mm. The resistance value was recorded after the reading had remained stable for at least 5 s. All surface-resistance measurements were performed under ambient laboratory conditions at room temperature. The relative humidity was not actively controlled during the measurements.
Three independently prepared specimens were tested for each formulation. The directly measured resistance between the two parallel strip electrodes, R, was recorded in ohms. To facilitate comparison with other conductive coatings, the corresponding sheet resistance, Rsh, was calculated by correcting for the electrode geometry according to Rsh = R(W/L), where W is the effective electrode length (40 mm) and L is the electrode spacing (10 mm). Therefore, Rsh = 4R for the present electrode configuration. Both the directly measured resistance and the calculated sheet resistance are reported. The effects of the ATO/carbon black mass ratio on the individual measurements and mean surface resistance are presented in Figure 4a and Table 2.
Figure 4. Effects of the ATO/carbon black mass ratio on (a) surface resistance and (b) corona inception voltage. Open symbols represent individual measurements, whereas filled symbols and error bars represent the mean ± sample standard deviation (n = 3).
Table 2. Measured resistance, sheet resistance, and corona inception voltage of the coatings with different ATO/carbon black ratios.
The same electrode geometry, measurement procedure, and ambient laboratory conditions were used for all specimens to ensure consistent comparative evaluation. The measurement was used as a comparative laboratory method rather than as a standardized surface-resistivity qualification test.

2.4.3. Corona Inception Voltage

Corona inception voltage was measured using a ZQTC-60 kVA power-frequency withstand-voltage testing system (Wuhan Zhuoqi Electric Co., Ltd., Wuhan, China) under a needle–plate electrode configuration. The needle electrode was made of copper and had a tip radius of approximately 0.5 mm. A circular copper plate with a diameter of 50 mm was used as the grounded plate electrode. The vertical distance between the needle tip and the coating surface was maintained at 1.5 ± 0.1 mm.
The applied voltage had a frequency of 50 Hz and was increased at a rate of 0.2 kV/s. All CIV measurements were performed under the same ambient laboratory conditions at room temperature; the relative humidity was not actively controlled. During testing in a darkened environment, CIV was defined as the voltage at which a continuous and reproducible faint blue glow first appeared near the needle tip and persisted for at least 3 s without developing into a complete arc.
Three independently prepared specimens were tested for each formulation. The individual CIV measurements, mean values, and sample standard deviations are presented in Figure 4b and Table 2.
The same electrode geometry, voltage-rising rate, visual inception criterion, and ambient laboratory conditions were applied to all specimens. The needle–plate configuration was used as a comparative laboratory protocol rather than as a standardized machine-insulation qualification test.

2.4.4. Scanning Electron Microscopy

The surface morphologies of the selected A3C7 coating and the commercial low-resistance coating were examined using an SU8600 field-emission scanning electron microscope (Hitachi High-Tech Corporation, Tokyo, Japan). Before observation, the specimens were sputter-coated with gold for 60 s. SEM imaging was performed at an accelerating voltage of 3.0 kV and a working distance of 7.5–7.8 mm.
Images were collected at magnifications of 1.00 k, 2.50 k, and 5.00 k. At least three different surface regions were examined for each coating to assess the reproducibility of the observed morphology. The analysis focused on surface continuity, the size and spatial distribution of circular or elliptical microdomains, and localized filler-rich structures.
The sizes of the circular or elliptical surface domains observed in A3C7 were quantified from the 2.50 k SEM image using ImageJ version 1.54P (National Institutes of Health, Bethesda, MD, USA). Fifty clearly distinguishable domains that did not intersect the image boundary were analyzed, and their equivalent circular diameters were calculated from the measured projected areas. The comparative SEM images of the commercial coating and A3C7 at the three magnifications are presented in Figure 5.
Figure 5. Surface SEM images of the commercial coating (a,c,e) and A3C7 (b,d,f) at magnifications of 1.00 k, 2.50 k, and 5.00 k, respectively; (g) equivalent-diameter distribution of the circular or elliptical surface domains observed in A3C7.

2.4.5. Thermal-Cycling Test

Three independently prepared specimens of A3C7 and the commercial coating were subjected to thermal cycling between 25 and 150 °C. Each specimen was first maintained at 25 ± 2 °C for 60 min and then transferred within 5 min to an oven maintained at 150 ± 2 °C. After holding at 150 °C for 60 min, the specimen was returned within 5 min to an environment at 25 ± 2 °C and held for another 60 min. This complete heating and cooling sequence was defined as one thermal cycle.
A total of 50 cycles were performed. Surface resistance was measured after 0, 10, 20, 30, 40, and 50 cycles. CIV was measured before thermal cycling and after completion of the 50th cycle. All electrical measurements after thermal cycling were conducted after the specimens had returned to room temperature under the same ambient laboratory conditions used for the initial measurements.
The relative resistance change in each specimen after n thermal cycles was calculated using Equation (1):
△ R n = R n − R 0 R 0 × 100 %
where R0 is the initial surface resistance of the specimen and Rn is the surface resistance of the same specimen after n thermal cycles.
The CIV retention after 50 thermal cycles was calculated using Equation (2):
η C I V = U 50 U 0 × 100 %
where U0 and U50 are the CIV values before thermal cycling and after 50 cycles, respectively.
The evolution of surface resistance, relative resistance change, and CIV during thermal cycling is presented in Figure 6 and Table 3.
Figure 6. Thermal-cycling performance of A3C7 and the commercial coating: (a) surface resistance, (b) relative resistance change, and (c) corona inception voltage before and after 50 cycles. Error bars represent the sample standard deviation (n = 3).
Table 3. Surface-resistance evolution during thermal cycling.

2.4.6. Statistical Analysis

All quantitative results are expressed as the mean ± sample standard deviation of three independently prepared specimens. Surface-resistance data were log10-transformed before statistical analysis. The effects of coating formulation on log10(Rs) and CIV were evaluated separately using one-way analysis of variance, followed by Tukey’s honestly significant difference test. A value of p < 0.05 was considered statistically significant. Statistical analyses were performed using OriginPro 2022 (OriginLab Corporation, Northampton, MA, USA).

3. Results and Discussion

3.1. FTIR Analysis of KH550-Treated Nano-ATO

The FTIR spectra of u-ATO and m-ATO are compared in Figure 3. Both samples exhibited a broad metal–oxygen lattice-vibration region between approximately 700 and 500 cm−1, indicating that the principal inorganic structure of ATO was retained after KH550 treatment. Compared with u-ATO, m-ATO exhibited additional absorption features near 1518 and 1144 cm−1. The band near 1518 cm−1 was assigned to the deformation vibration of amino groups introduced by the aminopropyl structure of KH550, whereas the band near 1144 cm−1 was associated with Si–O-related vibrations [25,26].
The spectra were normalized and vertically offset to facilitate comparison, as shown in Figure 3. The sharp band near 2350 cm−1 was attributed to atmospheric CO2 and was therefore not considered evidence of surface modification. The additional N–H- and Si–O-related absorption features in m-ATO indicate that KH550-derived organosilane structures were introduced onto the ATO surface [27,28]. However, because Si–O-related vibrations may overlap with the metal–oxygen lattice region of ATO, the FTIR results alone do not permit an unambiguous assignment of a specific ATO–O–Si bonding configuration. Moreover, the present FTIR results only confirm the introduction of KH550-derived organosilane structures and do not directly demonstrate improved ATO dispersion, stronger interfacial adhesion, or enhanced compatibility with the epoxy matrix. Therefore, the present FTIR results are interpreted as evidence for the presence of KH550-derived organosilane species on the treated ATO rather than definitive proof of covalent silane grafting.

3.2. Effects of the ATO/Carbon Black Ratio on Electrical Performance

The effects of the ATO/carbon black mass ratio on surface resistance and corona inception voltage are summarized in Figure 4 and Table 2. Individual measurements are included in Figure 4 to show the data distribution, whereas the filled symbols and error bars represent the mean values and sample standard deviations, respectively.

3.2.1. Surface Resistance

As shown in Figure 4a, the surface resistance exhibited a pronounced non-monotonic dependence on the ATO/carbon black ratio at a constant total filler loading of 10 wt%. A0C10 showed a surface resistance of (1.28 ± 0.17) × 104 Ω, indicating that A0C10 exhibited a low surface resistance of (1.28 ± 0.17) × 104 Ω, confirming the effective low-resistance behavior of the carbon-black-filled coating at the investigated filler loading. When 1 wt% carbon black was replaced with m-ATO, the resistance increased markedly to (4.43 ± 0.57) × 104 Ω for A1C9. This unusually high resistance may be associated with several factors, including an unfavorable local filler distribution, filler agglomeration or insufficient dispersion at this particular composition, and the resulting change in the macroscopic electrical connectivity of the coating. Experimental variability may also contribute to the observed increase. However, because no direct dispersion or compositional characterization was performed specifically for A1C9, the exact origin of this behavior cannot be conclusively determined from the present data [9,10,11].
With further increases in the ATO content, the surface resistance decreased to (1.74 ± 0.12) × 104 Ω for A2C8 and reached its lowest mean value of (1.17 ± 0.07) × 104 Ω for A3C7. No significant difference was observed between A3C7 and A0C10 (p = 0.985), indicating that the replacement of 3 wt% carbon black with m-ATO did not compromise the overall low-resistance level.
When the ATO/carbon black ratio increased from 4:6 to 8:2, the surface resistance remained within a relatively narrow range of 1.78 × 104–1.92 × 104 Ω. In contrast, A10C0 exhibited a resistance of (1.23 ± 0.22) × 105 Ω, approximately 10.5 times that of A3C7. This result confirms that, at the investigated total filler loading, carbon black remained the principal component responsible for the low-resistance behavior of the coating.
The non-monotonic variation suggests that the electrical response was governed not only by the individual conductivities of ATO and carbon black but also by changes in filler dispersion and network connectivity. Comparable composition-dependent behavior has been reported for epoxy or polymer composites containing carbon black with a second conductive or semiconductive component [14,21,22,23,24].
The commercial coating exhibited a significantly lower surface resistance of (9.26 ± 1.17) × 102 Ω than all laboratory-prepared coatings (p < 0.001). However, a lower surface resistance alone does not necessarily indicate better overall anti-corona performance, because CIV and resistance stability must also be considered.

3.2.2. Corona Inception Voltage and Formulation Selection

As shown in Figure 4b, CIV initially increased and then decreased with increasing ATO content, followed by a partial recovery for the ATO-only formulation. The CIV of A0C10 was 1.84 ± 0.07 kV. After the introduction of m-ATO, the CIV progressively increased to 2.04 ± 0.10, 2.36 ± 0.07, and 2.58 ± 0.04 kV for A1C9, A2C8, and A3C7, respectively.
A3C7 exhibited the highest mean CIV, representing an increase of 40.1% relative to A0C10 and 49.9% relative to the commercial coating. When the ATO/carbon black ratio increased further from 4:6 to 8:2, CIV generally decreased from 2.34 to approximately 1.87–1.88 kV, although the surface resistances of these formulations remained within a similar range. This result indicates that average surface resistance alone did not determine corona inception behavior.
A10C0 exhibited a CIV of 2.22 ± 0.11 kV despite having the highest surface resistance among the investigated formulations. Therefore, neither continuously decreasing resistance nor continuously increasing ATO content produced the highest CIV. Instead, corona inception was likely affected by the combined influences of charge dissipation, local conductive-domain distribution, and interfacial heterogeneity. Surface conductivity can influence surface-charge accumulation and the resulting local electric-field distribution [29], while temperature-dependent surface-potential decay and flashover behavior have been reported for epoxy-based composites [30]. These studies provide mechanistic context rather than a direct quantitative comparison with the present AC needle–plate CIV test.
One-way analysis of variance confirmed a significant formulation effect on CIV (p < 0.001). Tukey’s test showed that the CIV of A3C7 was significantly higher than those of A0C10 and the commercial coating (both p < 0.001). However, the differences between A3C7 and A2C8 or A4C6 were not statistically significant (p > 0.05). Accordingly, A3C7 was selected as the representative formulation for subsequent comparison because it simultaneously exhibited the lowest mean surface resistance and the highest mean CIV among the investigated formulations. This selection was based on the combined electrical-performance criteria rather than on a statistically unique superiority in CIV.

3.3. Surface Morphology of A3C7 and the Commercial Coating

The surface morphologies of the commercial coating and A3C7 are compared in Figure 5 at magnifications of 1.00 k, 2.50 k, and 5.00 k. The images in the left column correspond to the commercial coating, whereas those in the right column correspond to A3C7. As shown in Figure 5a,c,e, the commercial coating exhibited a relatively uniform surface with only a small number of irregular flake-like or block-like features. In comparison, numerous circular or elliptical microdomains with different sizes were distributed over the A3C7 surface, as shown in Figure 5b,d,f.
The A3C7 coating appeared macroscopically smooth. Therefore, the circular or elliptical features observed in Figure 5 should not be interpreted directly as open pores or macroscopic surface defects. The primary particle sizes of ATO and carbon black were approximately 20 and 100 nm, respectively, whereas the observed domains were on the micrometre scale and were therefore substantially larger than individual filler particles. To provide a quantitative description of these SEM-visible morphological features, the equivalent diameters of 50 clearly distinguishable circular or elliptical surface domains were analyzed. As shown in Figure 5g, the equivalent diameters ranged from approximately 1.11 to 5.58 μm, with an average value of 2.88 ± 1.30 μm (n = 50). This distribution describes only the dimensions of the SEM-visible surface domains and should not be interpreted as the particle-size distribution of ATO or carbon black.
Numerous circular or elliptical contrast features were observed on the A3C7 surface, as shown in Figure 5b,d,f. These features were substantially larger than the nominal primary particle sizes of both ATO and carbon black. However, because conventional SEM does not provide chemical identification of these regions, their origin cannot be conclusively determined from the present images. They may arise from secondary filler agglomeration, resin-rich or filler-rich regions, surface depressions, or other local morphological heterogeneities. Therefore, Figure 5 is used only to demonstrate the distinct surface morphology of A3C7 relative to the commercial coating. The SEM observations do not establish the spatial distribution of ATO and carbon black separately and do not provide direct evidence for electrical contacts or conductive pathways between the two fillers. Elemental mapping or higher-resolution compositional characterization would be required to resolve these features.

3.4. Thermal-Cycling Stability

The thermal-cycling performance of A3C7 and the commercial coating is compared in Figure 6 and Table 3. Figure 6a presents the evolution of surface resistance, Figure 6b shows the corresponding relative resistance changes, and Figure 6c compares the CIV values before and after 50 thermal cycles.

3.4.1. Surface-Resistance Stability

As shown in Figure 6a, the surface resistance of both coatings increased progressively with the number of thermal cycles. However, the magnitude of the resistance increase differed substantially between A3C7 and the commercial coating.
The mean surface resistance of A3C7 increased from (1.17 ± 0.07) × 104 Ω before cycling to (1.31 ± 0.07) × 104 Ω after 50 cycles. The corresponding relative resistance change was only 12.62% ± 1.19%, as shown in Figure 6b and Table 3.
In contrast, the resistance of the commercial coating increased from (9.26 ± 1.17) × 102 to (1.52 ± 0.25) × 103 Ω. Its relative resistance change reached 63.95% ± 6.76%, approximately 5.1 times that of A3C7.
Although the commercial coating retained a lower absolute resistance after cycling, its substantially larger relative change indicates poorer resistance stability. Therefore, the electrical stability of a low-resistance coating should not be evaluated solely from its initial resistance value.
No high voltage was continuously applied during the thermal-cycling procedure. Consequently, the resistance variations observed in Figure 6a,b reflect the macroscopic electrical response of the coatings to thermal cycling rather than degradation caused directly by corona oxidation. Temperature-dependent conductivity and resistance changes in carbon-filled epoxy systems have been associated with thermal expansion and rearrangement of conductive contacts [13,15,31,32]. The smaller resistance drift of A3C7 therefore demonstrates that its macroscopic electrical response was less sensitive to the imposed thermal-cycling conditions.

3.4.2. CIV Retention

The CIV values measured before and after thermal cycling are compared in Figure 6c. The CIV of A3C7 decreased from 2.58 kV before cycling to 2.37 kV after 50 cycles, corresponding to a retention of 91.86% and a decrease of 8.14%.
For the commercial coating, CIV decreased from 1.72 ± 0.09 to 1.42 ± 0.06 kV, corresponding to a retention of 82.40%. After 50 cycles, the CIV of A3C7 remained approximately 66.9% higher than that of the commercial coating.
The CIV results are consistent with the resistance-stability results shown in Figure 6a and b. A3C7 exhibited both a smaller resistance drift and a higher CIV retention, indicating greater electrical stability under the specified 25–150 °C thermal-cycling conditions.
These results further support the selection of A3C7 as the representative formulation for subsequent evaluation. Although the commercial coating showed the lowest initial surface resistance, A3C7 achieved a more favorable balance between low-resistance charge dissipation, corona inception performance, and resistance to thermal-cycling-induced electrical changes.

3.5. Possible Interpretation of the Composition-Dependent Electrical Behavior

A conceptual interpretation of the composition-dependent electrical behavior and thermal-cycling response is illustrated in Figure 7. This conceptual interpretation was developed based on the FTIR, surface-resistance, CIV, SEM, and thermal-cycling results rather than from any single characterization method.
Figure 7. Conceptual illustration of (a) KH550 modification of nano-ATO; (b) hypothetical conductive structures of the carbon-black-only and ATO/carbon black hybrid systems; and (c) schematic thermal-cycling responses of the conventional carbon-black/epoxy coating and A3C7. The filler configurations and conductive pathways shown are hypothetical and are not directly resolved by the present SEM observations. Gray spheres represent m-ATO, black spheres represent carbon black, and light-blue lines represent the epoxy matrix. Red and blue dashed lines correspond to the schematic conductive-contact/network features indicated in the figure. These schematic connections are hypothetical.
As illustrated in Figure 7a, hydrolyzed KH550 introduces silanol groups that interact with hydroxylated sites on the ATO surface. Previous studies have reported that amino-silane treatment can improve the compatibility and wetting of inorganic particles in epoxy-related matrices [25,26,27,28]. However, the present FTIR results do not directly verify such improvements for the ATO/epoxy interface. This interpretation is consistent with the additional N–H- and Si–O-related absorption bands observed for m-ATO in Figure 3.
Figure 7b schematically compares the conductive structures of the carbon-black-only and ATO/carbon black hybrid systems. For carbon-black-filled polymer composites, particle-contact and short-range transport mechanisms have been widely discussed in previous studies [9,10,12,13]. These literature-based mechanisms provide possible context for the low-resistance behavior observed here. However, because the total filler loading was fixed at 10 wt% in the present study, no percolation threshold, critical exponent, or conductive transition was determined, and the specific microscopic conduction mechanism cannot be established from the present data. Consequently, disruption of a limited number of critical contacts may noticeably affect the overall resistance. In A3C7, carbon black remains the principal component responsible for the low-resistance behavior, as indicated by the substantially higher resistance of the carbon-black-free A10C0 formulation.
The introduction of 3 wt% m-ATO did not simply dilute the carbon black network. Instead, the combined electrical and morphological results suggest that replacing part of the carbon black with m-ATO altered the macroscopic electrical response of the coating; however, the present measurements do not identify the corresponding microscopic conductive configuration. As shown in Figure 4, the dependence of surface resistance and CIV on ATO/carbon black ratio was non-monotonic, indicating that the electrical behavior cannot be described simply by the nominal content of either filler. The incorporation of a second conductive or semiconductive component can regulate network topology and filler-domain distribution [21,22,23,24,33,34,35]. As shown in Figure 5, relatively uniformly distributed micron-scale domains are present on the A3C7 surface. However, conventional SEM cannot directly identify nanoscale ATO–carbon black contacts.
This composition-dependent interpretation is consistent with the non-monotonic electrical behavior shown in Figure 4. A3C7 retained a surface resistance comparable to that of A0C10 while exhibiting a 40.1% higher CIV. Therefore, the observed electrical performance cannot be explained solely by the intrinsic conductivity of either filler. Instead, it likely results from an appropriate balance among filler composition, local filler distribution, and interfacial structure.
The proposed response to thermal cycling is shown in Figure 7c. Repeated expansion and contraction of the epoxy matrix can change the contact distance between conductive particles and reorganize carbon black aggregate chains [13,15,34,35].
Accordingly, A3C7 exhibited a relative resistance change of only 12.62% ± 1.19% after 50 cycles, compared with 63.95% ± 6.76% for the commercial coating, while its CIV retention remained 91.86%. These results are consistent with the conceptual interpretation shown in Figure 7, in which carbon black is considered the principal low-resistance component, while the smaller resistance drift of A3C7 demonstrates improved macroscopic electrical stability; however, the present results do not establish that ATO directly stabilizes carbon-black contacts or forms specific semiconducting nodes.
It should be emphasized that the present thermal-cycling test was performed without continuous corona exposure. Therefore, the results directly demonstrate improved resistance stability under the specified thermal-cycling conditions, but they do not independently establish long-term resistance to corona oxidation. The potential role of ATO under combined electrical, thermal, and oxidative stresses requires further verification through prolonged corona-aging or multi-stress aging experiments.
Broadband dielectric characterization was not included in the present study because the investigated coating was designed as a low-resistance semiconductive layer rather than a bulk insulating dielectric; such characterization using independently prepared coating films will be considered in future work.

4. Conclusions

KH550-modified nano-ATO was combined with carbon black to prepare low-resistance epoxy anti-corona coatings with a fixed total hybrid-filler loading of 10 wt%. FTIR analysis showed additional N–H- and Si–O-related absorption features near 1518 and 1144 cm−1 for m-ATO, indicating the introduction of KH550-derived organosilane structures onto the ATO surface. Because of overlapping absorption regions, FTIR alone was not used to assign a specific ATO–O–Si bonding configuration. The ATO/carbon black ratio produced non-monotonic changes in both surface resistance and CIV. Among the investigated formulations, A3C7 exhibited a surface resistance of (1.17 ± 0.07) × 104 Ω and the highest mean CIV of 2.58 ± 0.04 kV, representing a 40.1% increase relative to the carbon-black-only A0C10 formulation. SEM revealed distinct circular or elliptical micron-scale surface features in A3C7; however, their chemical origin could not be determined from conventional SEM, and no direct conclusion regarding ATO/carbon black conductive contacts was drawn from these observations. After 50 thermal cycles between 25 and 150 °C, the relative resistance change in A3C7 was 12.62% ± 1.19%, substantially lower than the 63.95% ± 6.76% measured for the commercial coating, while the corresponding CIV retentions were 91.86% and 82.40%, respectively. Overall, partial replacement of carbon black with KH550-modified ATO enabled A3C7 to achieve a favorable combination of low surface resistance, increased CIV, and reduced resistance drift during thermal cycling. Nevertheless, the microscopic mechanism responsible for this behavior cannot be established from the present SEM and electrical measurements and requires further investigation using direct compositional and local-conductivity characterization. The specific effect of KH550 treatment also requires verification using unmodified-ATO coating controls, while long-term corona-aging and partial-discharge-resistance tests are needed to evaluate durability under more realistic electrical stresses.

Author Contributions

Conceptualization, Q.G., D.C., T.L. and S.M.; Methodology, S.L., Q.G. and D.C.; Software, Q.G., D.C. and T.L.; Validation, S.L., T.L. and S.M.; Formal analysis, Q.G., T.L., Y.Z. and S.M.; Investigation, S.L., Q.G., D.C., T.L. and Y.Z.; Resources, S.M.; Data curation, Q.G. and Y.Z.; Writing—original draft, S.L. and S.M.; Writing—review & editing, S.L., Y.Z. and S.M.; Visualization, S.M.; Supervision, Y.Z. and S.M.; Project administration, Y.Z. and S.M.; Funding acquisition, Y.Z. and S.M. All authors have read and agreed to the published version of the manuscript.

Funding

This work was funded by the Laboratory of Advanced Energetic Materials and Devices.

Institutional Review Board Statement

Not applicable.

Data Availability Statement

The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding authors.

Conflicts of Interest

Author Yue Zhang was employed by the Dongfang Electric Corporation Dongfang Electric Machinery Co., Ltd. The remaining authors declare that the research was conducted in the absence of any commercial or financial relationships that could be construed as a potential conflict of interest.

References

  1. Emery, F.T. Partial discharge, dissipation factor, and corona aspects for high voltage electric generator stator bars and windings. IEEE Trans. Dielectr. Electr. Insul. 2005, 12, 347–361. [Google Scholar] [CrossRef] [Scilit]
  2. Li, C.; Peng, X.; Wang, H.; Chen, Y.; Ling, P.; Liu, T.; Zhang, Y.; Zhou, J. Dynamic partial discharge characteristics of generator stator bar with four typical defects. IEEE Trans. Dielectr. Electr. Insul. 2025, 32, 494–503. [Google Scholar] [CrossRef] [Scilit]
  3. Li, C.; Song, J.; Lin, L.; Lei, Z.; Su, W.; Bi, X. Effects of vapor with different chemical properties on corona partial discharges of stator windings. IEEE Trans. Dielectr. Electr. Insul. 2014, 21, 964–972. [Google Scholar] [CrossRef] [Scilit]
  4. Nakamura, S.; Kuraishi, T.; Kanegami, M.; Miyazaki, S. Impact of temperature on partial discharge in generator stator windings. IEEE Trans. Dielectr. Electr. Insul. 2026. early access. [Google Scholar] [CrossRef] [Scilit]
  5. Kurimský, J.; Kolcunová, I.; Cimbala, R. Understanding surface partial discharges in HV coils and the role of semi-conductive protection. Electr. Eng. 2010, 92, 283–289. [Google Scholar] [CrossRef] [Scilit]
  6. Zohdi, T.I.; Abali, B.E. Modeling of power transmission and stress grading for corona protection. Comput. Mech. 2018, 62, 411–420. [Google Scholar] [CrossRef] [Scilit]
  7. Bai, X.; Li, M.; Shang, G.; Li, Z.; Niu, B.; Guo, J.; Liu, X. The dielectric characteristics of SiC/PEEK for outer corona protection in large generator. J. Appl. Polym. Sci. 2026, 143, e57998. [Google Scholar] [CrossRef] [Scilit]
  8. Martin-Gallego, M.; Yuste-Sanchez, V.; Sanchez-Hidalgo, R.; Verdejo, R.; Lopez-Manchado, M.A. Epoxy nanocomposites filled with carbon nanoparticles. Chem. Rec. 2018, 18, 928–939. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  9. Wu, T.H.; Foyet, A.; Kodentsov, A.; van der Ven, L.G.J.; van Benthem, R.A.T.M.; de With, G. Curing and percolation for carbon black-epoxy-amine nanocomposites. Compos. Sci. Technol. 2019, 181, 107672. [Google Scholar] [CrossRef] [Scilit]
  10. Schueler, R.; Petermann, J.; Schulte, K.; Wentzel, H.-P. Agglomeration and electrical percolation behavior of carbon black dispersed in epoxy resin. J. Appl. Polym. Sci. 1997, 63, 1741–1746. [Google Scholar] [CrossRef]
  11. Kim, D.; Jeong, J.W.; Lee, S.; Lee, D.Y.; Jeon, Y.J.; Seong, D.G. Tailoring electrical conductivity of epoxy composites through strategic filler composition and morphology of graphite and carbon black. Funct. Compos. Struct. 2025, 7, 035006. [Google Scholar] [CrossRef] [Scilit]
  12. Zhang, Q.; Xu, Y.; Yang, Y.; Li, L.; Song, C.; Su, X. Conductive mechanism of carbon black/polyimide composite films. J. Polym. Eng. 2018, 38, 147–156. [Google Scholar] [CrossRef] [Scilit]
  13. El-Tantawy, F.; Kamada, K.; Ohnabe, H. Electrical properties and stability of epoxy reinforced carbon black composites. Mater. Lett. 2002, 57, 242–251. [Google Scholar] [CrossRef] [Scilit]
  14. Jia, W.; Tchoudakov, R.; Joseph, R.; Narkis, M.; Siegmann, A. The conductivity behavior of multi-component epoxy, metal particle, carbon black, carbon fibril composites. J. Appl. Polym. Sci. 2002, 85, 1706–1713. [Google Scholar] [CrossRef] [Scilit]
  15. Abdel-Aal, N.; El-Tantawy, F.; Al-Hajry, A.; Bououdina, M. Epoxy resin/plasticized carbon black composites. Part I. Electrical and thermal properties and their applications. Polym. Compos. 2008, 29, 511–517. [Google Scholar] [CrossRef] [Scilit]
  16. Sun, H.; Liu, X.; Liu, B.; Yin, Z. Preparation and properties of antimony doped tin oxide nanopowders and their conductivity. Mater. Res. Bull. 2016, 83, 354–359. [Google Scholar] [CrossRef] [Scilit]
  17. Liu, J.; Coleman, J.P.; Madhukar, P. Synthesis and characterization of tin oxide nanoparticles heavily doped with antimony. Microsc. Microanal. 1997, 3, 433–434. [Google Scholar] [CrossRef] [Scilit]
  18. Castro, M.R.S.; Oliveira, P.W.; Schmidt, H.K. Enhanced mechanical and electrical properties of antimony-doped tin oxide coatings. Semicond. Sci. Technol. 2008, 23, 035013. [Google Scholar] [CrossRef] [Scilit]
  19. Zhou, H.; Wang, H.; Tian, X.; Zheng, K.; Cheng, Q. Preparation and properties of waterborne polyurethane/antimony doped tin oxide nanocomposite coatings via sol-gel reactions. Polym. Compos. 2014, 35, 1169–1175. [Google Scholar] [CrossRef] [Scilit]
  20. Wang, L.; Hang, J.; Shi, L.; Sun, X.; Xu, F. Preparation and characterization of NIR cutoff antimony doped tin oxide/hybrid silica coatings. Mater. Lett. 2012, 87, 35–38. [Google Scholar] [CrossRef] [Scilit]
  21. Yang, M.; Liu, B.; Xia, J.; Liu, Y.; Shi, Z.; Lv, X. Study on the properties of a novel electrostatic conductive and anti-corrosive composite coating improved by graphene nanosheets. Prog. Org. Coat. 2019, 136, 105244. [Google Scholar] [CrossRef] [Scilit]
  22. Wu, Q.; Tong, W.; Chen, Q.; Gu, B.; Hou, H.; He, S. Electrothermal performance of CNTs/ATO composite film. J. Alloys Compd. 2019, 789, 282–287. [Google Scholar] [CrossRef] [Scilit]
  23. Ren, L.; Xu, B.; Wang, G.; Yin, X.; Liu, Y.; Yang, W.; Chen, Y. Fabrication of an antimony doped tin oxide–graphene nanocomposite for highly effective capacitive deionization of saline water. RSC Adv. 2020, 10, 39130–39136. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  24. Wang, T.; Ge, H.; Zhang, K. A novel core-shell silica@graphene straticulate structured antistatic anticorrosion composite coating. J. Alloys Compd. 2018, 745, 705–715. [Google Scholar] [CrossRef] [Scilit]
  25. Wu, J.; Ji, G.; Wu, Q. Preparation of epoxy/ZrO2 composite coating on the Q235 surface by electrostatic spraying and its corrosion resistance in 3.5% NaCl solution. RSC Adv. 2022, 12, 10625–10633. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  26. Li, Y.; Chen, H.; Wu, J.; He, Q.; Li, Y.; Yang, W.; Zhou, Y. Preparation and characterization of APTES modified magnetic MMT capable of using as anisotropic nanoparticles. Appl. Surf. Sci. 2018, 447, 393–400. [Google Scholar] [CrossRef] [Scilit]
  27. Atta, A.M.; Ezzat, A.O.; El-Saeed, A.M.; Tawfeek, A.M.; Sabeela, N.I. Self-healing of chemically bonded hybrid silica/epoxy for steel coating. Prog. Org. Coat. 2020, 141, 105549. [Google Scholar] [CrossRef] [Scilit]
  28. Baghdadi, Y.N.; Youssef, L.; Bouhadir, K.; Harb, M.; Mustapha, S.; Patra, D.; Tehrani-Bagha, A.R. The effects of modified zinc oxide nanoparticles on the mechanical/thermal properties of epoxy resin. J. Appl. Polym. Sci. 2020, 137, 49330. [Google Scholar] [CrossRef] [Scilit]
  29. Wang, Q.; Liang, X.; Chen, K.; Wu, C.; Liu, S. Surface charge properties of epoxy composites under DC voltage affected by surface and bulk conductivity. Energies 2021, 14, 370. [Google Scholar] [CrossRef] [Scilit]
  30. Du, B.X.; Liang, H.C.; Li, J.; Zhang, C. Temperature dependent surface potential decay and flashover characteristics of epoxy/SiC composites. IEEE Trans. Dielectr. Electr. Insul. 2018, 25, 631–638. [Google Scholar] [CrossRef] [Scilit]
  31. Babu, M.S.; Sarathi, R.; Vasa, N.J.; Imai, T. Understanding the influence of nano micro filler on electrical and mechanical behaviour of epoxy nanocomposites. IEEE Trans. Dielectr. Electr. Insul. 2019, 26, 1098–1106. [Google Scholar] [CrossRef]
  32. Wu, J.; Ye, Z.; Ge, H.; Chen, J.; Liu, W.; Liu, Z. Modified carbon fiber/magnetic graphene/epoxy composites with synergistic effect for electromagnetic interference shielding over broad frequency band. J. Colloid Interface Sci. 2017, 506, 217–226. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  33. Rahnamol, A.M.; Gopalakrishnan, J. Improved dielectric and dynamic mechanical properties of epoxy/polyaniline nanorod/in situ reduced graphene oxide hybrid nanocomposites. Polym. Compos. 2020, 41, 2998–3013. [Google Scholar] [CrossRef] [Scilit]
  34. Reis, J.M.L.; Martins, S.A.; da Costa Mattos, H.S. Combination of temperature and electrical conductivity on semiconductor graphite/epoxy composites. J. Braz. Soc. Mech. Sci. Eng. 2020, 42, 404. [Google Scholar] [CrossRef] [Scilit]
  35. Wang, W.; Wang, C.; Yue, X.; Zhang, C.; Zhou, C.; Wu, W.; Zhu, H. Raman spectroscopy and resistance-temperature studies of functionalized multiwalled carbon nanotubes/epoxy resin composite film. Microelectron. Eng. 2019, 214, 50–54. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.