Abstract
Cement-stabilized coral aggregate (CSCA) contains porous particles and heterogeneous cementitious contacts whose deformation can alter the internal void network. This study combines mineralogical analysis, scanning electron microscopy with energy-dispersive spectroscopy, nanoindentation and staged in situ X-ray computed tomography to examine local heterogeneity and pore-network changes during loading. Microscopic measurements were made on beam-derived coupons, whereas CT tracked two separately prepared, fine-graded cylinders containing 7% cement, with one specimen tested at each confining pressure of 0 and 100 kPa. Local indentation moduli ranged approximately from 5 to 95 GPa. Peak deviator stresses were approximately 5.8 and 6.2 MPa, respectively, and the 100 kPa record exhibited more gradual post-peak softening. Changes in the resolved void structure were greater between the near-peak and final scans than between the initial and near-peak scans. Final mean pore volumes were approximately 0.52 and 0.34 mm3, while maximum slice void fractions approached 0.45–0.50 and 0.30–0.35. Extracted throat counts increased in both records, demonstrating that connection abundance and opening-related dimensions describe different aspects of network evolution. These observations characterize the tested loading histories. Different terminal strains and the absence of replicate specimens prevent the differences from being attributed exclusively to confinement; microscopy provides complementary, rather than directly registered, evidence.
1. Introduction
Cement-stabilized coral aggregate (CSCA) is a candidate material for bonded granular layers and engineered fills in island construction, where transporting conventional aggregates can constrain material selection. Its performance depends on the interaction between a compacted particle skeleton and a relatively small cementitious fraction. Coral-derived particles differ from conventional mineral aggregates in their pore structure, irregular geometry and susceptibility to breakage [1]. Research on dense CSCA and coral sand–cement mortar has established the importance of aggregate packing and the aggregate–binder connection [2,3]. Similar links between mixture composition, microscopic structure and strength have been investigated for cement-stabilized aeolian sand, recycled-aggregate macadam and sand-rich stabilized bases [4,5,6]. These studies motivate a structural question for CSCA: how does a porous cemented skeleton lose continuity when it is loaded under lateral restraint?
Earlier investigations of CSCA provide a starting point. Liu et al. [7] used acoustic emission during four-point bending to distinguish stages of damage and showed that CSCA fracture involved both interfaces and aggregate particles. Liu et al. [8] subsequently used distributed fibre-optic measurements and numerical analysis to relate strain localization to the development and position of bending cracks. Together, these studies establish that fracture cannot be represented solely by the strength of a uniform cement matrix. Their principal observations concern bending response, surface or embedded-line deformation, and post-fracture morphology. The evolution of the internal three-dimensional void structure under confined loading remains a separate issue. Resolving this issue is relevant to granular construction layers because surrounding material restricts lateral deformation and changes the way that cemented contacts separate.
In a bonded base layer, overburden and adjacent material restrict lateral deformation while applied loads generate deviatoric stresses. Triaxial compression is therefore useful for examining axial deformation and localized failure under controlled lateral pressure. Here, 0 and 100 kPa provide two laboratory boundary conditions; 100 kPa is not assigned to a particular field depth or traffic load. The objective is to observe internal structural changes, not to derive a shear-strength envelope from two unreplicated tests.
A mechanistic interpretation requires local structure and mechanical properties to be considered together. The interfacial transition zone (ITZ) in concrete is commonly described through changes in packing, hydration products, porosity and stiffness near an aggregate surface [9,10]. Coral-aggregate concrete studies have specifically examined its mechanical and microstructural characteristics and their long-term development [11,12]. Coupled X-ray computed tomography (CT) and digital volume correlation (DVC) provide a further route to characterize mechanical bonding between cement paste and porous aggregates [13]. Reviews of lightweight-aggregate and recycled-aggregate concrete also show why the ITZ depends on aggregate texture and preparation history [14,15]. For compacted CSCA, these findings raise two connected possibilities: local pore filling can strengthen parts of a particle–matrix connection, while pores within the particle or adjacent matrix can still provide sites for damage. A single interface thickness or a fixed aggregate–matrix stiffness ranking may therefore be inadequate.
Nanoindentation offers access to local stiffness and hardness, whereas CT resolves larger-scale spatial arrangements of particles and voids. Indentation studies of cement hydrates and high-performance concrete have demonstrated the value of separating local mechanical populations [16,17]; multiscale work on stabilized macadam has extended this approach to cracking in granular cementitious materials [18]. CT and image-processing studies establish how internal structure can be reconstructed and quantified [19,20,21]. Applications to cement-paste microstructure and tortuosity further demonstrate that three-dimensional information contains features that are absent from a single section [22,23]. In Buildings, a methodological review has connected CT imaging with damage modelling of cementitious materials [24], while in situ CT experiments on carbon-reinforced concrete have combined internal crack assessment with deformation measurements [25]. These developments support the use of complementary measurements, provided that local indentation results and CT-scale structural descriptors retain their distinct physical meanings.
The interpretation of CT changes also depends on the loading condition and on the descriptor being measured. Concrete studies have investigated damage under in situ compression and the three-dimensional strain distribution under passive confinement [26,27]. CT observations under compressive loading of sand, porous carbonate rock and soil–rock mixtures demonstrate the relevance of spatial localization and constituent heterogeneity [28,29,30]. Pore-space models of concrete and CT-based analyses of marine carbonates provide additional foundations for studying damage and pore–throat topology [31,32]. However, the number of extracted connections, their dimensions and the spatial concentration of voids describe different aspects of a network. More connections do not necessarily imply wider cracks or a larger hydraulic conductance. This distinction is especially relevant when specimens differ in their initial pore populations or when image segmentation repartitions a growing connected void.
The present study examines local heterogeneity and three-dimensional void reorganization using complementary specimen groups. Mineralogical analysis, microscopy and nanoindentation characterize composition, contact morphology and local mechanical contrasts in beam-derived material. Staged in situ CT follows two separately prepared fine-graded cylinders, one tested at 0 kPa and one at 100 kPa confinement. Pore dimensions, slice void fractions, coordination distributions and throat characteristics are compared within each loading history and then between the two records. This design distinguishes opening-related geometry from connection abundance, while treating confinement as one possible contributor to the observed differences rather than an independently isolated material effect.
2. Materials and Methods
2.1. Material Provenance and Experimental Design
Coral aggregate from the Xisha Islands in the South China Sea was used in the underlying CSCA experimental programme. Two specimen groups served different purposes. The microscopy and nanoindentation coupons were obtained from representative fractured regions of compacted CSCA beams. The parent beam mixture contained a nominal cement content of 7%, used M32.5 cement, and was prepared with prewetted aggregate followed by cement addition, mixing and static compaction. Its compaction characterization gave an optimum water content of 13% and a maximum dry density of 1.97 g/cm3. These values characterize the parent mixture; they are not measurements of the miniature CT specimens. The preparation and bending behaviour of this material family have been described previously [7,8]. In the cement designation M32.5, M denotes masonry cement and 32.5 denotes its strength grade; the designation follows the nomenclature of GB/T 3183-2017, Masonry Cement [33]. It does not denote the cement content of the mixture.
The in situ CT group used particles smaller than 2 mm and a nominal 7% content of P.O.42.5 Portland cement. The mixture was statically compacted into cylinders 20 mm in diameter and 40 mm in height. Restricting the particle size enabled loading and scanning within the miniature triaxial cell. Accordingly, this group represents a fine-graded cemented coral skeleton rather than the complete grading of a field base course. Table 1 summarizes the distinction between the specimen groups. Microscopy and indentation provide complementary material evidence; they are not spatially registered observations of the cylinders used for CT. The height-to-diameter ratio is 2. Because the maximum particle size is smaller than 2 mm, the diameter-to-maximum-particle-size and height-to-maximum-particle-size ratios exceed 10 and 20, respectively. These geometric ratios do not establish a representative elementary volume or reproduce the packing and fracture paths of a full-graded base-course mixture.
Table 1.
Specimen groups and the scope of the reported preparation parameters.
Static compaction defines the preparation route used here. The CT group is not assumed to reproduce a vibrated field base. Wang et al. [34] found that static and vibration compaction produced different mechanical responses and void distributions in cement-stabilized macadam. This evidence makes compaction a relevant limitation on extrapolation, rather than a basis for correcting the present measurements. The full sieve curves and achieved CT-specimen density are not available in the reported preparation record; the upper particle-size limit alone does not specify a grading curve.
The nominal 7% cement content was held fixed in the existing experimental programme, so cement dosage was not an investigated variable. Research on dense CSCA demonstrates that mixture design depends on aggregate packing and cement content [2]. Work on cement-stabilized aggregate further links shrinkage-crack resistance to grading, cement content and compaction [35]. Accordingly, 7% is treated as the tested formulation, not a recommended optimum. No shrinkage or cement-content comparison is available to establish its suitability for a field base. The M32.5 and P.O.42.5 groups are retained as distinct material groups; their common nominal dosage does not make their binders or hydration histories equivalent.
The experimental arrangement and the relationship between measurements are shown in Figure 1. One CT specimen was tested at each nominal confining pressure, 0 and 100 kPa. Each record contains three scan states: A, initial; B, close to peak load; and C, final post-peak. Thus, there are two independent loading records, not replicated datasets at either pressure. The scans document changes between stages; they do not resolve individual crack velocities. Because the final axial strains differ, states carrying the same letter identify comparable loading stages rather than equal-deformation states.
Figure 1.
Specimen preparation and the complementary measurement framework. Photographs show (a) cylinder end faces; (b) cylinder side views; (c) a mounted specimen and (d) the pressure cell. Microscopy and indentation coupons are separate from the in situ CT specimens. A, B and C denote initial, near-peak and final post-peak scan states.
2.2. Mineralogical and Microscopic Characterization
X-ray diffraction (XRD) and X-ray fluorescence (XRF) characterize the beam-derived material group identified in Table 1. The composition results in Section 3.1 therefore provide context for the microscopy and nanoindentation observations; they are not separate compositional measurements of the CT cylinders. XRD phase fractions and XRF oxide-equivalent composition were interpreted separately. In particular, the CaO-equivalent XRF result was not treated as a measurement of free lime. Minor hydration-phase assignments require caution because reflections can overlap and conventional XRD has limited sensitivity to poorly crystalline products.
For scanning electron microscopy (SEM), naturally separated fracture surfaces containing particles and adjacent cementitious material were selected and cut at low speed. The specimens were dried for 24 h and sputter-coated with gold. The fracture-surface images presented here were acquired at 20 kV, with working distances of approximately 11.6–12.3 mm. The higher-magnification interface image series records an accelerating voltage of 10 kV and working distances of approximately 7.7–8.2 mm. These settings refer to the respective image series. Surface topography, compositional contrast and preparation effects were considered when interpreting the images; quantitative phase segmentation from electron images requires its own controlled imaging procedure [36].
Energy-dispersive X-ray spectroscopy (EDS) included a line crossing a selected particle–matrix boundary, elemental maps of the surrounding region, and a spectrum with selected-element quantification. Ca, Si, C, Mg, Al, S and Cl were examined. The line-scan coordinate was used to locate a compositional transition. It was not interpreted directly as the thickness of an ITZ. The reported composition is normalized over the listed elements and does not include oxygen; it therefore serves as a local chemical signature rather than a complete stoichiometric analysis of hydration products.
2.3. Nanoindentation and Local Mechanical Interpretation
Representative coupons were embedded in resin and progressively ground and polished. A Berkovich diamond indenter with an elastic modulus of 1141 GPa, a Poisson ratio of 0.07 and a nominal tip radius of 20 nm was used. Loading, holding and unloading responses were recorded at multiple positions in selected particle and matrix/interface regions. Local properties were interpreted using the Oliver–Pharr framework [37,38].
The contact stiffness S is the initial unloading slope, P is the indentation load, h is the penetration depth, and hmax denotes the maximum depth. The contact depth is
where Pmax is the maximum load and ε is the indenter-geometry coefficient. Hardness and reduced modulus are expressed as
where Ac is the calibrated projected contact area and β is the geometric correction factor. The contribution of indenter deformation is removed through
where E and ν are the specimen elastic modulus and Poisson ratio, and Ei and νi are the corresponding indenter properties. The reported local modulus and hardness distributions are used to examine spatial heterogeneity. Absolute moduli depend on the area-function calibration, the unloading analysis and the adopted specimen Poisson ratio. A high indentation modulus represents the local solid sampled beneath the tip and does not directly measure the strength of an entire porous coral particle. The selected measurements are interpreted descriptively: the available record does not establish the number of independent interfaces, a population distribution or confidence intervals. Indentation count and spacing, load–hold–unload settings, the adopted specimen Poisson ratio and calibration details are needed to reproduce the absolute values. Published studies show that surface preparation and sampling choices affect cement-paste nanoindentation results [39]; their settings cannot be assigned retrospectively to the present tests.
2.4. CT Loading and Image Analysis
The in situ tests were conducted using a nanoVoxel-3000 CT system with a triaxial loading attachment at Badao Engineering Hospital in Henan, China. The two confinement conditions were compared through deviator stress q and axial strain εa, defined as
where σ1 and σ3 denote axial and confining stresses, and L0 and L are the initial and current specimen heights. Compression is positive. The 0 kPa test represents unconfined axial compression; the 100 kPa test introduces a low level of lateral restraint. The stress–strain response and the three CT states were interpreted together.
Spatial void variation was assessed using the section-wise area fraction
where Avoid(z) and AROI(z) are the resolved void area and the specimen-region area in the section at height z. This dimensionless quantity is distinct from whole-specimen volumetric porosity. Pore radius and volume are arithmetic means over the extracted pore objects. Coordination number is the number of connections associated with a pore. Throat count and mean throat radius, length and volume describe the extracted network, while the pore–throat ratio relates the associated pore and throat diameters. Means of radius, length and volume are separate statistics; a mean volume cannot generally be obtained by applying a single-object formula to mean dimensions.
Numerical values read from plotted summaries are reported approximately. Comparisons emphasize change within each record; no replicate variance, confidence interval or statistical significance is inferred. Initial normalization is used only where the initial and final values refer to the same descriptor. CT voxel size, effective resolution, acquisition settings, reconstruction details, segmentation thresholds and boundary treatment are not recoverable from these summaries. These factors can affect both the resolved pore population and its extracted connections [20,21,40], so the measurements are interpreted at the level supported by the available images and descriptors.
Multi-panel figures contain images from different fields or loading stages, not continuous stitched fields. Original measured image fields, traces and scale bars are retained. The CT summaries support stage-wise comparisons, but do not supply full pore-size distributions or independently registered trajectories of individual pores.
3. Results
3.1. Composition and Porous Fracture Morphology
The XRD pattern of the beam-derived characterization group is shown in Figure 2. Its composition is carbonate-rich, with a strong calcite-related reflection near 2θ = 29.4° and a quartz contribution near 26.6°. The retained labels for portlandite and ettringite indicate proposed minor-phase assignments. They should not be used to quantify hydration or to establish the abundance of calcium silicate hydrate from this pattern alone.
Figure 2.
XRD pattern of the beam-derived CSCA characterization group. Q, quartz; Cc, calcite; CH, portlandite; AFt, ettringite. Minor hydration-phase labels are retained as provisional assignments; the pattern does not quantify poorly crystalline C–S–H.
The mineralogical summary in Table 2 contains 53.6% calcite and 27.3% aragonite, giving a combined reported carbonate fraction of 80.9%. Quartz accounts for 14.5%, while amphibole, clay minerals and gypsum together contribute 4.6%. The listed phase fractions sum to 100%; they describe the reported mineralogical normalization rather than a separately quantified total amorphous fraction. The presence of quartz is relevant when interpreting individual Si-rich particles in the subsequent EDS observations.
Table 2.
Reported mineralogical composition of the beam-derived CSCA characterization group.
Table 3 gives the XRF composition on the reported oxide-equivalent basis. CaO equivalent is 77.880%, followed by SiO2 at 11.367% and Al2O3 at 3.809%. Fe2O3, SrO and MgO are also above 1%. The high Ca signal is compatible with the carbonate-dominated mineralogy. XRF and XRD quantify different representations of composition, so the CaO-equivalent result cannot be substituted for a carbonate mineral fraction or a free-CaO content.
Table 3.
Reported XRF oxide-equivalent composition of the beam-derived CSCA characterization group.
The selected fracture-surface views in Figure 3 show irregular voids, exposed pore walls and solid material remaining within some openings. Yellow circles identify prominent pores; red circles identify selected solid remnants or filling regions. The images document the coexistence of voids and solid ligaments in these fields. Morphology alone does not determine whether each remnant is a coral fragment, cementitious filling or a combination of both, nor does a fractured surface establish the original contact geometry. The observations are compatible with the pore-filling morphology and mixed interface/particle participation reported previously for CSCA [7].
Figure 3.
Selected CSCA fracture surfaces at (a) 100× and (b) 350×, displayed separately at enlarged size. Yellow circles identify prominent pores; red circles identify selected solid remnants or filling regions. The original image intensities and scale bars are retained. The panels are separate fields, and morphology alone does not identify the retained solids.
3.2. Particle–Matrix Morphology and Elemental Contrast
The higher-magnification fields in Figure 4 show a comparatively smooth or layered particle surface adjacent to a rougher matrix. Some boundary segments appear closely joined, whereas recesses and gaps are visible elsewhere in the selected fields. These observations describe local variations in contact morphology. Because the surfaces were exposed during specimen preparation or fracture, they do not quantify the prevalence of such contacts in intact CSCA or establish the strength of individual interfaces. In combination with Figure 3, they support a local description of porous and heterogeneous structure.
Figure 4.
Particle–matrix interface morphology in separate fields at (a,b) 500×, (c,d) 1000× and (e,f) 2000×. The red arrow in (d) indicates the EDS line-scan direction. The original scale bars and image-acquisition metadata are retained.
The EDS line in Figure 5 crosses the boundary visible in Figure 4d. On the particle side, Si intensity is high, generally around 250–300 counts per second. A marked decrease in Si and increase in Ca occur near a line coordinate of 38–40 µm. The matrix-side Ca signal is generally around 50–80 counts per second. These observations identify a Si-rich particle adjoining a more Ca-rich matrix. They do not independently identify that particle as carbonate coral; the quartz fraction in the bulk mineralogical summary provides a possible alternative assignment. The approximately 38–40 µm coordinate locates the transition along the scan, rather than measuring an ITZ thickness.
Figure 5.
EDS line-scan intensities across the selected particle–matrix boundary: (a) Ca, Si and C; (b) S, Al, Cl and Mg. The transition near 38–40 µm denotes a line coordinate rather than a measured ITZ thickness.
The elemental maps in Figure 6 reinforce this distinction. Si is concentrated within the selected particle, while the adjacent region has a stronger Ca contribution. The remaining elements are less sharply partitioned at the displayed intensity scales. Elemental maps provide spatial information, but a visually abrupt boundary does not establish that the bond is exclusively physical or that a chemically modified transition region is absent.
Figure 6.
Electron image and EDS maps of the selected interface field. Panels are arranged from left to right and top to bottom: electron image, C, Mg, Al, Si, S, Cl, Ca and elemental overlay. Colour intensities are qualitative and are not directly comparable between elements.
The spectrum and selected-element quantification are presented in Figure 7 and Table 4. Si, Ca and C dominate the listed normalized composition, with Si and Ca contributing 37.87 and 34.14 wt%, respectively. The reported atomic fractions give a Ca/Si ratio of approximately 0.63. This is a mixed-region analytical ratio, not the Ca/Si ratio of an isolated hydrate. Oxygen is absent from the tabulated element set, and the carbon contribution can be affected by the substrate and preparation. Consequently, these results cannot establish a unique hydration-product assemblage. Work on cement-paste microstructure and concrete ITZ transport similarly emphasizes that local chemistry, phase arrangement and pore structure address different aspects of material behaviour [41,42].
Figure 7.
EDS spectrum of the selected region. The spectrum and the selected-element normalization in Table 4 characterize a mixed region; they are not phase-specific chemical analyses.
Table 4.
Selected-element EDS quantification for the analysed region.
3.3. Local Modulus and Hardness Distributions
Figure 8a shows a broad contrast between the higher-modulus particle regions and the lower-modulus matrix/interface regions. The high-modulus group lies approximately within 60–90 GPa, with hardness around 4.5–5 GPa. The lower group spans a much broader relative range, including moduli below 20 GPa and values extending to approximately 40 GPa. Its hardness is predominantly below about 1.8 GPa. The overlap within the lower group prevents a mechanical assignment of every point to either matrix or ITZ.
Figure 8.
Local mechanical heterogeneity: (a) modulus–hardness distribution and (b) modulus along a selected CSCA traverse. Region labels reflect the local assignments associated with the measurements. The triangular markers represent individual nanoindentation measurements of the elastic modulus along the selected traverse. The red double-headed arrows indicate the approximate spatial extents of the three identified regions: the matrix/interface region, the particle region, and the adjacent matrix/interface region. The dashed vertical lines indicate the approximate boundaries between these regions.The traverse is not registered to the CT specimens or to the EDS line in Figure 5.
The selected traverse in Figure 8b spans approximately 300 µm and contains local moduli of about 5–95 GPa. Modulus rises within the assigned central particle region, although substantial fluctuations also occur there. Alternating lower and higher values occur in the adjacent matrix/interface regions. A continuous layer of uniformly low modulus is not resolved along this traverse. This is an observation of local variability, not evidence that weak interfaces are absent throughout CSCA. Cementitious-composite and stabilized-macadam studies provide context for such heterogeneity [16,17,18], while systematic nanoindentation work demonstrates why preparation, calibration and independent sampling are necessary for quantitative population comparisons [39].
3.4. Initial Structure and the Two Recorded Loading Responses
Figure 9 illustrates the separation of CT images into particle, matrix and void representations and the associated three-dimensional models. The separated particle regions form a closely packed skeleton with matrix material occupying portions of the interparticle space. Resolved voids occur both between particles and within porous regions. For the initial structure, the reported particle area fraction varies approximately from 65% to 80% along the specimen height. This is a section-wise measure and is not used as an independently measured global aggregate volume fraction.
Figure 9.
Illustration of CT phase separation and three-dimensional representation: (a) CT section; (b) particle mask; (c) void mask; (d) matrix mask; (e) extracted pore network; and (f–h) particle, void and matrix renderings. The illustrated renderings demonstrate the representation procedure and are not all identified as initial-state models.
Figure 10 links the loading curves to the selected CT sections. Under 0 kPa confinement, the measured deviator stress reaches approximately 5.8 MPa at an axial strain of about 2%. The curve then softens steeply, followed by a lower-stress post-peak branch. The initial section contains dispersed voids. Changes near the peak are more limited than those between the peak and the final state, where a prominent inclined region of separation is visible across the heterogeneous skeleton.
Figure 10.
Deviator stress–axial strain records and selected CT sections for one specimen at each confinement: (a) 0 kPa and (b) 100 kPa. The right-hand columns show initial (A), near-peak (B) and final post-peak (C) states, with rows identifying particle, matrix and void representations. Insets show the corresponding three-dimensional specimen forms. The final states occur at different axial strains. The solid curves represent the measured deviator stress–axial strain responses under the two confining conditions. The labels A, B, and C indicate three representative loading stages: the initial state, the near-peak state, and the final post-peak state, respectively. The arrows connecting the stress–strain curves to the corresponding three-dimensional specimen renderings identify the locations of these selected scanning stages.
At 100 kPa confinement, the peak deviator stress is approximately 6.2 MPa at an axial strain of roughly 2–3%. The subsequent decrease is more gradual than in the 0 kPa record, and loading extends beyond 10% axial strain. Localized damage is visible in the final sections, with less extensive resolved openings than in the unconfined final section. The peak stresses differ by approximately 0.4 MPa. With one specimen per pressure and different terminal strains, neither this difference nor the post-peak contrast isolates the contribution of confinement from specimen variability and loading history.
3.5. Pore Enlargement and Spatial Localization
Figure 11 combines three-dimensional void renderings with mean pore dimensions. Changes between A and B are comparatively small in the displayed summaries, whereas larger and more connected void regions are visible between B and C in both records. The unconfined final state contains a more extensive concentration of open void space than the confined final state. This comparison concerns the recorded endpoints, which are not matched in axial strain.
Figure 11.
Pore-structure changes between the recorded states: (a–c) 0 kPa at A, B and C; (d–f) 100 kPa at A, B and C; (g) mean pore radius; and (h) mean pore volume. Values are means over the extracted pore objects. Blue and purple bars denote 0 and 100 kPa, respectively.
The plotted initial mean pore radii are approximately 150–165 µm. At C, they reach approximately 180 µm under 0 kPa and 175 µm under 100 kPa. The difference is more pronounced in mean pore volume: initial values of approximately 0.21–0.23 mm3 change only slightly near the peak and reach approximately 0.52 and 0.34 mm3 at C. Thus, the mean pore volume rises to roughly 2.5 and 1.5 times its respective initial value. The change in a mean object volume reflects both pore enlargement and object merging; it is not a direct measurement of total specimen void volume. In the absence of individual-object distributions, these means cannot distinguish widespread enlargement from the development of a small number of large voids or cracks. A specimen-wide resolved void volume would require integration over the segmented three-dimensional region of interest, not multiplication of a plotted mean by an unknown pore count.
Figure 12 shows how the void area fraction varies with height. At A, most sections lie within approximately 0.10–0.18, with somewhat different profiles in the two specimens. The B profiles show comparatively small changes. At C, the unconfined specimen develops a strong height-dependent increase, with an upper-region maximum approaching 0.45–0.50. The confined record reaches approximately 0.30–0.35 and exhibits a less extreme concentration. These distributions identify spatially uneven damage more clearly than a single mean pore size. They are consistent with the importance of local void changes demonstrated in CT studies of strain localization [28]. Pore-sensitive studies using acoustic emission and low-field nuclear magnetic resonance likewise provide a complementary context for relating pore structure to cracking [43]. The height profiles describe each scanned configuration; equal plotted heights are not assumed to identify the same material points across deformed states.
Figure 12.
Slice void area fraction along the specimen height at A, B and C under (a) 0 kPa and (b) 100 kPa confinement. The horizontal scale is a dimensionless area fraction, not a percentage or a bulk volumetric porosity.
3.6. Coordination and Throat-Network Reorganization
The coordination histograms in Figure 13 are dominated by low-degree pores in the initial and near-peak states. The initial distributions are concentrated around coordination numbers of 0–3. At C, the distributions broaden, with more pores connected to several neighbours and a tail extending above a coordination number of 10. The high-degree tail is more extended in the unconfined record, although both specimens undergo substantial reorganization. Because the ordinate is pore count, these histograms contain information about both population size and connectivity; the height of an individual bar is not a normalized probability.
Figure 13.
Pore coordination-number histograms under (a) 0 kPa and (b) 100 kPa confinement. A, B and C denote the three scan states. The ordinate gives counts, so differences in total pore populations must be considered when comparing bar heights.
The throat descriptors in Figure 14 reveal a different aspect of the comparison. Throat counts increase from approximately 1.6 × 103 to 7.6 × 103 under 0 kPa and from approximately 2.1 × 103 to 9.0 × 103 under 100 kPa. The confined specimen therefore has more extracted throats in absolute terms at both A and C. Using each initial count as its own baseline gives approximate increases to 4.8 and 4.3 times the initial count. Baseline normalization makes the relative changes explicit, but it does not remove the effects of unequal terminal strains, initial structure or segmentation.
Figure 14.
Extracted throat-network statistics at A, B and C: (a) throat count; (b) mean radius; (c) mean length; and (d) mean volume. One unit on the volume scale, 106 µm3, equals 0.001 mm3. The statistics describe separate aspects of the extracted network.
Throat dimensions provide the complementary evidence. Initial and near-peak mean throat radii are approximately 70–80 µm. At C, the mean radius approaches 100 µm under 0 kPa and 90 µm under 100 kPa. Mean throat lengths similarly increase from approximately 230–260 µm to about 295 and 265 µm, respectively. At the recorded final states, the unconfined network has larger mean radii and lengths despite its lower throat count. Meanwhile, mean throat volumes decrease from approximately 0.032 to 0.019 mm3 under 0 kPa and from approximately 0.028 to 0.017 mm3 under 100 kPa. The simultaneous increase in count and decrease in mean throat volume is compatible with a more finely partitioned extracted network. It does not, by itself, identify how individual physical channels grow.
The three-dimensional network representations in Figure 15 show the spatial redistribution accompanying these changes. Connections become more numerous in the late-stage networks, and their distribution follows the deformed and damaged specimen geometry. The renderings are used to identify spatial organization; their colours are not treated as a shared quantitative scale between specimens. Table 5 consolidates the approximate initial-to-final comparisons and separates geometric enlargement from connection abundance.
Figure 15.
Pore-network renderings under (a–c) 0 kPa and (d–f) 100 kPa confinement, ordered A, B and C. Balls and connecting segments represent pore bodies and throats. Colours are retained for visualization and do not define a common quantitative scale between conditions.
Table 5.
Approximate initial-to-final pore and throat descriptors for the two loading histories. Final states occur at different axial strains; entries are descriptive comparisons, not isolated confinement effects.
Figure 16 shows the pore–throat ratio distributions and the reported grouped percentages. Under 0 kPa, the fraction in the 0–2 class decreases from 57% at A to 43% at C, while the 3–6 class rises from 37% to 53%. Under 100 kPa, the corresponding changes are 52% to 40% and 42% to 55%. The highest class decreases to about 4% in both final states. The two specimens therefore exhibit qualitatively similar redistribution, with a slightly larger change in the unconfined record. Some grouped totals differ from 100% by one percentage point because the reported values are rounded. These ratio distributions support a change in relative pore–throat geometry but do not establish a percolation threshold or a crack-growth rate.
Figure 16.
Pore–throat ratio distributions and grouped percentages: (a,b) 0 kPa and (c,d) 100 kPa. Histograms retain the recorded counts, and the grouped charts retain the reported ratio classes. Rounded class percentages may sum to 99% or 101%; they have not been silently renormalized.
4. Discussion
4.1. Heterogeneous Contacts and the Participation of Porous Particles
The composition, microscopy and indentation results provide complementary constraints on a damage mechanism. Carbonate minerals dominate the reported bulk composition, while quartz and other constituents remain present. The selected EDS field contains a Si-rich particle, and its identity cannot be inferred solely from the overall coral origin of the aggregate. This distinction matters because a compositional boundary in one microscopic field cannot be generalized into a universal coral–paste interface. Likewise, the indentation traverse records stiffness variations within a small region rather than a specimen-wide constitutive distribution.
The selected observations are compatible with locally stiff solids adjacent to pores and spatially variable cementitious contacts. A stiff indentation site can occur within a mechanically vulnerable particle because indentation samples a small solid volume, whereas particle fracture also depends on pore walls, flaws and geometry. Close contact at one location need not prevent damage in an adjacent porous region. Earlier bending observations of both interface separation and particle fracture in CSCA support this interpretation [7,8]. However, the microscopy and CT groups differ in grading, cement and specimen history, so these local observations do not identify where damage initiated in either CT cylinder.
Coral-concrete ITZ investigations [11,12] and coupled XCT–DVC measurements of paste–porous aggregate bonds [13] offer material analogies, but their binder contents, fabrication routes and local testing procedures differ from compacted CSCA. The present results therefore support a heterogeneous contact description rather than a claim that CSCA universally lacks a weak ITZ. Similar caution applies when selecting modification strategies from lightweight-aggregate or recycled-aggregate concrete [14,15]. Improving contact continuity and preserving the particle skeleton are related objectives, and neither is represented fully by an average interface modulus.
4.2. Interpretation of the Two Loading Histories
The 100 kPa record combines more gradual post-peak softening with a smaller final mean pore volume, lower maximum slice void fraction and smaller final mean throat radius and length than the 0 kPa record. Lateral restraint of separation and dilation is a plausible contributor to this combination. However, one specimen at each pressure cannot distinguish this contribution from specimen-to-specimen variability, and the different terminal strains further confound the endpoint comparison. The continued increase in extracted connections shows that smaller mean opening-related dimensions do not imply an unchanged internal network.
CT/DVC observations of passively confined concrete [27] provide a mechanical analogy for the interaction between restraint and localized deformation. CT studies of sand and porous carbonate rock also demonstrate spatially concentrated changes under compressive loading [28,29]. These studies involve different materials and stress ranges. They support the plausibility of a restraint-related mechanism but do not validate its magnitude in CSCA or replace replicated tests. The two present records therefore motivate a hypothesis about lateral restraint and post-peak opening rather than establish a general confinement law.
In both records, the larger changes between B and C are consistent with deformation concentrating in damaged regions after the peak: separation, sliding and void coalescence can produce conspicuous openings while the macroscopic load decreases. Limited changes between A and B do not establish an absence of earlier damage, because sub-resolution cracking and changes between scans may remain undetected. With three scans, the observations quantify differences between selected stages rather than the onset or rate of cracking. Normalizing deviator stress by its peak value would identify a loading stage but would not make strain histories identical. Likewise, normalizing each descriptor by its initial value accounts for its baseline only. CT geometry at an unscanned common strain cannot be obtained reliably by interpolating the three available states.
4.3. Why Connection Counts and Pore Dimensions Must Be Separated
An extracted pore network is a representation of a segmented void geometry. Its nodes and edges depend on how that geometry is partitioned into pore bodies and throats. Pore-network extraction studies and marine-carbonate applications make this dependence explicit [32,44,45]. During fracture, the opening or merging of a void can change both the geometry and its topological decomposition. A high throat count can therefore coexist with smaller mean throats, as observed in the confined specimen.
The reported throat radius, length and volume trends should also be interpreted jointly rather than forced into a single cylindrical-channel model. Even for ideal cylinders, the mean of radius squared times length is generally different from the product of the squared mean radius and mean length. In a segmented irregular network, additional differences arise from the definitions of pore bodies, constrictions and throat volume. Consequently, the observed decline in mean throat volume does not contradict the numerical increase in mean radius or length without further information on the joint distribution and the extraction definitions. Nor can it be used alone to demonstrate physical refinement of every channel.
The pore–throat ratio describes relative geometry, while coordination describes local adjacency. Neither determines global hydraulic connectivity without spatial continuity, boundary conditions and a transport model. Tortuosity measurements in cement pastes [23] illustrate a further structural quantity relevant to transport. The present tests did not measure permeability; a predicted increase in seepage or chloride transport would therefore require additional verification. Their direct contribution is the separation of opening-related damage from the abundance and organization of extracted connections.
4.4. Implications for Construction Layers and Study Limitations
For construction layers made from cemented coral particles, maintaining a connected solid skeleton requires attention to initial packing, contact continuity and restraint during service. The observed local heterogeneity suggests that mixture development should examine where the binder is placed and how porous particles participate in fracture, in addition to measuring a bulk compressive strength. The value of combining microscopic and macroscopic evaluations has also been demonstrated for cement-stabilized aeolian sand and sand-rich granular bases [4,6]. Work on void-structure deterioration in stabilized macadam further supports including structural descriptors when assessing material integrity [46]. These comparisons motivate future testing of CSCA mixtures rather than establish a design optimum from the present specimens. The fine-graded CT cylinders omit the larger particles and broader size distribution used in practical CSCA. Changes in grading can alter packing, binder distribution, intraparticle porosity and the relative participation of particle breakage and interface separation [1,2]. Therefore, the observations indicate processes worth examining at field-relevant grading rather than directly transferable pore sizes or strength values.
The main limitations are the single specimen at each of two pressures, unequal final strains and incomplete documentation of CT and indentation processing. The two material groups also differ in cement designation, grading, loading history and sampled volume. No registered relationship between a local indentation value and a CT damage site is established. The available pore-object means cannot replace full size distributions, medians, percentiles or total resolved void volume. Effective CT resolution and segmentation choices affect both object dimensions and connectivity [20,21,40]; without the underlying volumes and processing settings, their sensitivity cannot be quantified here. These limitations restrict the findings to an exploratory comparison of the recorded specimens.
Replicated tests at common strain states and additional pressures would be needed to separate specimen variability from a confinement trend. Registered CT/DVC and local measurements could then test the proposed connection between contact heterogeneity and damage localization [13,25]. Full-graded specimens prepared under field-relevant compaction, together with documented imaging and segmentation sensitivity, would be needed before deriving construction-layer design parameters. These are requirements for further validation, not tests completed in the present study.
5. Conclusions
This study combined local characterization of beam-derived CSCA with staged CT of two separately prepared fine-graded cylinders, one tested at 0 kPa and one at 100 kPa confinement. The following conclusions apply to these observations.
(1) The reported mineralogical composition of the beam-derived group contains 80.9% calcite and aragonite combined. Selected SEM fields show voids, solid ligaments and locally variable particle–matrix contact. The EDS boundary separates a Si-rich particle from a more Ca-rich region; its line coordinate does not establish a universal coral ITZ thickness or a specific bonding chemistry.
(2) Local indentation moduli range approximately from 5 to 95 GPa along the selected measurements. The traverse shows spatial variability without resolving a uniformly soft continuous interface layer. It does not establish the population distribution of interface properties or the absence of weak interfaces elsewhere.
(3) Peak deviator stresses are approximately 5.8 MPa in the 0 kPa record and 6.2 MPa in the 100 kPa record. The latter has more gradual post-peak softening. In both records, the displayed structural changes are greater between the near-peak and final scans than between the initial and near-peak scans.
(4) Final mean pore volumes are approximately 0.52 and 0.34 mm3 for the 0 and 100 kPa records, respectively; maximum slice void fractions approach 0.45–0.50 and 0.30–0.35. These differences characterize endpoints reached at different axial strains. Together with the lack of replication, this prevents their attribution exclusively to confinement.
(5) Extracted throat counts increase in both specimens and are higher in the 100 kPa record at both the initial and final states, whereas final mean throat radii and lengths are larger in the 0 kPa record. Connection abundance and opening-related dimensions therefore require separate interpretation. The combined descriptors document network reorganization within the tested histories without establishing a permeability change or a general material law.
Author Contributions
Conceptualization, J.H., D.C. and Z.L.; methodology, Y.Z. and Z.L.; software, D.C. and Z.L.; validation, J.H.; writing—original draft preparation, Z.L., D.C. and J.H.; investigation, J.H. and Y.Z.; writing—review and editing, J.H. and D.C.; funding acquisition, D.C. All authors have read and agreed to the published version of the manuscript.
Funding
This research was funded by National Natural Science Foundation of China, grant number 42377150.
Data Availability Statement
The data supporting the findings of this study are not publicly available at present because they form part of an ongoing research project. These data are available from the corresponding author upon reasonable request for academic research. Requests should specify the data required and the intended research use.
Conflicts of Interest
Jinfang Hou and Yansheng Zhuang are employed by Tianjin Port Engineering Institute Co., Ltd. of CCCC First Harbor Engineering Co., Ltd. and Key Laboratory of Coastal Engineering Hydrodynamics, China Communications Construction Company, Ltd. The remaining authors declare that the research was conducted in the absence of any commercial or financial relationships that could be construed as a potential conflict of interest.
Abbreviations
The following abbreviations are used in this manuscript:
| CSCA | Cement-stabilized coral aggregate |
| CT | Computed tomography |
| DVC | Digital volume correlation |
| EDS | Energy-dispersive X-ray spectroscopy |
| ITZ | Interfacial transition zone |
| ROI | Region of interest |
| SEM | Scanning electron microscopy |
| XRD | X-ray diffraction |
| XRF | X-ray fluorescence |
| C–S–H | Calcium silicate hydrate |
References
- Wang, X.Z.; Jiao, Y.Y.; Wang, R.; Hu, M.J.; Meng, Q.S.; Tan, F.Y. Engineering characteristics of the calcareous sand in Nansha Islands, South China Sea. Eng. Geol. 2011, 120, 40–47. [Google Scholar] [CrossRef] [Scilit]
- Zeng, Z.; Miao, C.; Shi, M.; Zhang, R.; Xu, Y. Study on the dense structure and properties of cement-stabilized coral aggregates. Constr. Build. Mater. 2022, 359, 129465. [Google Scholar] [CrossRef] [Scilit]
- Wang, L.; Mei, J.; Wu, J.; He, X.; Li, H.; Ding, Q. Mechanical Properties and Microscopic Mechanism of Coral Sand-Cement Mortar. Adv. Mater. Sci. Eng. 2020, 2020, 4854892. [Google Scholar] [CrossRef] [Scilit]
- Cui, Q.; Liu, G.; Zhang, Z.; Fang, Y.; Gu, X. Experimental Investigation on the Strength and Microscopic Properties of Cement-Stabilized Aeolian Sand. Buildings 2023, 13, 395. [Google Scholar] [CrossRef] [Scilit]
- Xiang, X.; Chen, W.; Huang, Y.; Wang, P.; Wang, G.; Wu, J.; Tian, W. Application of recycled concrete aggregates in continuous-graded cement stabilized macadam. Case Stud. Constr. Mater. 2024, 21, e03918. [Google Scholar] [CrossRef] [Scilit]
- Wu, B.; Zheng, P.; Wang, B.; Pu, C.; Zhu, S.; Liu, J. Study on Mix Proportion Optimization and Multi-Scale Mechanism of High-Volume Aeolian Sand Cement-Fly Ash Stabilized Gravel Base. Buildings 2026, 16, 590. [Google Scholar] [CrossRef] [Scilit]
- Liu, Z.; Han, Z.; Qin, L.; Cao, D.; Guo, C.; Wang, F.; Ma, B.; Wu, J. Identification of bending fracture characteristics of cement-stabilized coral aggregate in four-point bending tests based on acoustic emission. Constr. Build. Mater. 2023, 402, 132999. [Google Scholar] [CrossRef] [Scilit]
- Liu, Z.; Cao, D.; Guo, C.; Wang, F.; Ma, B.; Wu, J.; Wang, D.; Liang, X. A new insight to investigate the strain distribution, evolution, and crack development of cement-stabilized coral aggregate. Constr. Build. Mater. 2024, 438, 137263. [Google Scholar] [CrossRef] [Scilit]
- Scrivener, K.L.; Crumbie, A.K.; Laugesen, P. The Interfacial Transition Zone (ITZ) Between Cement Paste and Aggregate in Concrete. Interface Sci. 2004, 12, 411–421. [Google Scholar] [CrossRef] [Scilit]
- Chen, Q.; Zhang, J.; Wang, Z.; Zhao, T.; Wang, Z. A review of the interfacial transition zones in concrete: Identification, physical characteristics, and mechanical properties. Eng. Fract. Mech. 2024, 300, 109979. [Google Scholar] [CrossRef] [Scilit]
- Ma, H.; Tu, Y.; Yu, H.; Diao, Y.; Han, W.; Zhang, M. Mechanical properties and microstructural characteristics of coral-aggregate-concrete ITZ: Experimental study. J. Build. Eng. 2023, 72, 106647. [Google Scholar] [CrossRef] [Scilit]
- Tu, Y.; Yu, H.; Ma, H.; Liu, J.; Li, L.; Han, W. Long-term study on the mechanical properties of the ITZ in coral aggregate concrete and its impact on material durability. Constr. Build. Mater. 2024, 449, 138255. [Google Scholar] [CrossRef] [Scilit]
- Fan, S.; Ren, H.; Hong, S.; Xing, F.; Hou, D.; Dong, B. Interfacial mechanical bond characterization between cement pastes and porous aggregates through a coupled XCT and DVC technique. Cem. Concr. Compos. 2023, 142, 105158. [Google Scholar] [CrossRef] [Scilit]
- Zhou, J.; Dong, Y.; Qiu, T.; Lv, J.; Guo, P.; Liu, X. The Microstructure and Modification of the Interfacial Transition Zone in Lightweight Aggregate Concrete: A Review. Buildings 2025, 15, 2784. [Google Scholar] [CrossRef] [Scilit]
- Memon, S.A.; Bekzhanova, Z.; Murzakarimova, A. A Review of Improvement of Interfacial Transition Zone and Adherent Mortar in Recycled Concrete Aggregate. Buildings 2022, 12, 1600. [Google Scholar] [CrossRef] [Scilit]
- Constantinides, G.; Ulm, F.J. The effect of two types of C-S-H on the elasticity of cement-based materials: Results from nanoindentation and micromechanical modeling. Cem. Concr. Res. 2004, 34, 67–80. [Google Scholar] [CrossRef] [Scilit]
- Sorelli, L.; Constantinides, G.; Ulm, F.J.; Toutlemonde, F. The nano-mechanical signature of Ultra High Performance Concrete by statistical nanoindentation techniques. Cem. Concr. Res. 2008, 38, 1447–1456. [Google Scholar] [CrossRef] [Scilit]
- Shi, S.; Wang, N.; Chen, C.; Ma, T.; Chen, F.; Gu, G. Multiscale study of the effect of fly ash geopolymer on the fatigue cracking of cement stabilized macadam. Constr. Build. Mater. 2023, 369, 130464. [Google Scholar] [CrossRef] [Scilit]
- Landis, E.N.; Keane, D.T. X-ray microtomography. Mater. Charact. 2010, 61, 1305–1316. [Google Scholar] [CrossRef] [Scilit]
- Wildenschild, D.; Sheppard, A.P. X-ray imaging and analysis techniques for quantifying pore-scale structure and processes in subsurface porous medium systems. Adv. Water Resour. 2013, 51, 217–246. [Google Scholar] [CrossRef] [Scilit]
- Schlüter, S.; Sheppard, A.; Brown, K.; Wildenschild, D. Image processing of multiphase images obtained via X-ray microtomography: A review. Water Resour. Res. 2014, 50, 3615–3639. [Google Scholar] [CrossRef] [Scilit]
- Gallucci, E.; Scrivener, K.; Groso, A.; Stampanoni, M.; Margaritondo, G. 3D experimental investigation of the microstructure of cement pastes using synchrotron X-ray microtomography (μCT). Cem. Concr. Res. 2007, 37, 360–368. [Google Scholar] [CrossRef] [Scilit]
- Promentilla, M.A.B.; Sugiyama, T.; Hitomi, T.; Takeda, N. Quantification of tortuosity in hardened cement pastes using synchrotron-based X-ray computed microtomography. Cem. Concr. Res. 2009, 39, 548–557. [Google Scholar] [CrossRef] [Scilit]
- Kaczmarczyk, G.P.; Cała, M. Possible Application of Computed Tomography for Numerical Simulation of the Damage Mechanism of Cementitious Materials—A Method Review. Buildings 2023, 13, 587. [Google Scholar] [CrossRef] [Scilit]
- Liebold, F.; Wagner, F.; Giese, J.; Grzesiak, S.; de Sousa, C.; Beckmann, B.; Pahn, M.; Marx, S.; Curbach, M.; Maas, H.G. Damage Analysis and Quality Control of Carbon-Reinforced Concrete Beams Based on In Situ Computed Tomography Tests. Buildings 2023, 13, 2669. [Google Scholar] [CrossRef] [Scilit]
- Li, N.; Zhao, Y.; Xing, Y.; He, X.; Li, H. Meso-damage analysis of concrete based on X-ray CT in-situ compression and using deep learning method. Case Stud. Constr. Mater. 2023, 18, e02118. [Google Scholar] [CrossRef] [Scilit]
- Li, P.D.; Wu, Y.F. Damage evolution and full-field 3D strain distribution in passively confined concrete. Cem. Concr. Compos. 2023, 138, 104979. [Google Scholar] [CrossRef] [Scilit]
- Desrues, J.; Chambon, R.; Mokni, M.; Mazerolle, F. Void ratio evolution inside shear bands in triaxial sand specimens studied by computed tomography. Géotechnique 1996, 46, 529–546. [Google Scholar] [CrossRef] [Scilit]
- Abdallah, Y.; Sulem, J.; Bornert, M.; Ghabezloo, S.; Stefanou, I. Compaction Banding in High-Porosity Carbonate Rocks: 1. Experimental Observations. J. Geophys. Res. Solid Earth 2021, 126, e2020JB020538. [Google Scholar] [CrossRef] [Scilit]
- Sun, X.; Li, X.; Mao, T.; Zheng, B.; Wu, Y.; Li, G. Fracture evolution analysis of soil-rock mixture in contrast with soil by CT scanning under uniaxial compressive conditions. Sci. China Technol. Sci. 2021, 64, 2771–2780. [Google Scholar] [CrossRef] [Scilit]
- Jivkov, A.P.; Engelberg, D.L.; Stein, R.; Petkovski, M. Pore space and brittle damage evolution in concrete. Eng. Fract. Mech. 2013, 110, 378–395. [Google Scholar] [CrossRef] [Scilit]
- Liu, H.; Ma, C.; Zhu, C. X-ray Micro CT Based Characterization of Pore-Throat Network for Marine Carbonates from South China Sea. Appl. Sci. 2022, 12, 2611. [Google Scholar] [CrossRef] [Scilit]
- GB/T 3183-2017; Masonry Cement. Standards Press of China: Beijing, China, 2017.
- Wang, F.; Pang, W.; Fang, Y.; Jiang, Y.; Han, L.; Li, Y. Comparative Research on Mechanical Properties and Void Distribution of Cement Stabilized Macadam Based on Static Pressure and Vibration Compaction. Appl. Sci. 2020, 10, 8830. [Google Scholar] [CrossRef] [Scilit]
- Zhang, J.; Ma, T.; Chen, S.; Gu, G. Evaluation of the shrinkage crack resistance of cement-stabilized aggregate by predicting the crack spacing. Road Mater. Pavement Des. 2024, 25, 291–307. [Google Scholar] [CrossRef] [Scilit]
- Scrivener, K.L. Backscattered electron imaging of cementitious microstructures: Understanding and quantification. Cem. Concr. Compos. 2004, 26, 935–945. [Google Scholar] [CrossRef] [Scilit]
- Oliver, W.C.; Pharr, G.M. An improved technique for determining hardness and elastic modulus using load and displacement sensing indentation experiments. J. Mater. Res. 1992, 7, 1564–1583. [Google Scholar] [CrossRef] [Scilit]
- Oliver, W.C.; Pharr, G.M. Measurement of hardness and elastic modulus by instrumented indentation: Advances in understanding and refinements to methodology. J. Mater. Res. 2004, 19, 3–20. [Google Scholar] [CrossRef]
- Raupach, K.; Bogner, A.; Vogel, M.; Kotan, E.; Dehn, F. Systematic Experimental Investigation into the Determination of Micromechanical Properties of Hardened Cement Paste Using Nanoindentation—Opportunities and Limitations. Materials 2023, 16, 1420. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Vicente, M.A.; Mena, Á.; Mínguez, J.; González, D.C. Use of Computed Tomography Scan Technology to Explore the Porosity of Concrete: Scientific Possibilities and Technological Limitations. Appl. Sci. 2021, 11, 8699. [Google Scholar] [CrossRef] [Scilit]
- Shah, V.; Scrivener, K.; Bhattacharjee, B.; Bishnoi, S. Changes in microstructure characteristics of cement paste on carbonation. Cem. Concr. Res. 2018, 109, 184–197. [Google Scholar] [CrossRef] [Scilit]
- Wu, K.; Han, H.; Li, H.; Dong, B.; Liu, T.; De Schutter, G. Experimental study on concurrent factors influencing the ITZ effect on mass transport in concrete. Cem. Concr. Compos. 2021, 123, 104215. [Google Scholar] [CrossRef] [Scilit]
- Li, Y.; Ma, H.; Wen, L.; Yuan, J.; Zhang, Y.; Li, Y.; Zhou, H.; Chen, J. Influence of pore size distribution on concrete cracking with different AEA content and curing age using acoustic emission and low-field NMR. J. Build. Eng. 2022, 58, 105059. [Google Scholar] [CrossRef] [Scilit]
- Gostick, J.T. Versatile and efficient pore network extraction method using marker-based watershed segmentation. Phys. Rev. E 2017, 96, 023307. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Gostick, J.; Khan, Z.; Tranter, T.; Kok, M.; Agnaou, M.; Sadeghi, M.; Jervis, R. PoreSpy: A Python Toolkit for Quantitative Analysis of Porous Media Images. J. Open Source Softw. 2019, 4, 1296. [Google Scholar] [CrossRef] [Scilit]
- Liu, H.; Qian, J.; Jin, C.; Qian, X. Investigation of mechanical performance and voids structure of cement-stabilised macadam under freeze-thaw actions. Int. J. Pavement Eng. 2023, 24, 2225120. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.