  • Article
  • Open Access

22 November 2026

26 Pages

Microstructural Evolution and Mechanical Property Changes of Al/Mg/Al Laminated Composites Under Different Annealing Temperatures

,
,
,
,
and
1
School of Materials Science and Engineering, Taiyuan University of Science and Technology, Taiyuan 030024, China
2
Shanxi Technology Innovation Center of Flange Basic Component Forming, Taiyuan 030024, China
3
Shanxi Yinguang Huasheng Magnesium Co., Ltd., Wenxi 043800, China
*
Author to whom correspondence should be addressed.
This article belongs to the Section Metal Casting, Forming and Heat Treatment

Abstract

To investigate the effect of annealing temperature on interface evolution, microstructure and the mechanical properties of Al/Mg/Al laminated composites (LMCs), LMCs fabricated by flat rolling at 400 °C were annealed at 200, 250, 300, 325, 350 and 375 °C for 60 min. Scanning electron microscopy (SEM), energy-dispersive spectroscopy (EDS), X-ray diffraction (XRD), electron back-scatter diffraction (EBSD), transmission electron microscopy (TEM), as well as tensile, cupping, peeling and hardness tests were employed to characterize their interfacial structure, microstructure and mechanical properties. With increasing annealing temperature, the interface gradually transforms from mechanical interlocking to metallurgical bonding, and the intermetallic compound (IMC) layer thickens continuously. Excessive elemental interdiffusion causes interfacial embrittlement at 375 °C. The Mg layer undergoes recovery, recrystallization, and grain growth, accompanied by changes in crystallographic texture. In contrast, the Al layer possesses a higher recrystallization temperature; it maintains a deformed microstructure at low temperatures and exhibits prominent recrystallization only at 350 °C. The dislocation density of both layers decreases first and then increases, reaching the minimum value at 350 °C. In terms of mechanical properties, the yield strength (YS) decreases monotonically with rising annealing temperature, and the yield-to-tensile ratio (ratio of yield strength to ultimate tensile strength, σs/σb) declines correspondingly. The work-hardening exponent reaches a peak value of 0.291 at 350 °C. Elongation (EL) increases first and then fluctuates at a high level (10.2% at 350 °C). The peeling strength varies in a non-monotonic trend: it presents the maximum value of 12.3 N/mm at 200 °C, drops to the minimum of 1.1 N/mm at 325 °C, and rebounds to 4.1 N/mm at 350 °C and 8.1 N/mm at 375 °C. For stamping formability, the Erichsen cupping index (IE) is the lowest (2.12 mm) at 200 °C and stabilizes within the range of 3.15–3.31 mm above 250 °C. In summary, favorable comprehensive performance is obtained under the annealing condition of 350 °C/60 min, with σs/σb of 0.733, an IE of 3.27 mm and a peeling strength of 4.1 N/mm. This condition exhibits good comprehensive formability and provides an experimental basis for the annealing-process design of LMCs.

1. Introduction

Lightweight design has become an irreversible trend in the manufacturing of high-end equipment such as automobiles, aerospace, rail transit, and 3C electronics, serving as a core approach to achieve energy conservation and emission reduction, and to enhance transportation efficiency and structural properties [1,2,3]. Among various lightweight structural materials, Mg alloys are hailed as “green engineering materials for the 21st century” due to their ultra-low density, high specific strength, and excellent damping properties [4,5]. However, Mg alloys exhibit poor formability at room temperature, weak corrosion resistance, and high chemical reactivity, making it difficult for them to withstand complex loads and harsh service environments alone [6,7]. On the other hand, Al alloys possess excellent plasticity, workability, and chemical stability. The combination of the two can provide reliable protection for Mg alloys [8,9]. Accordingly, LMCs, which are manufactured by sandwiching Mg alloy between two Al alloy claddings, are employed in this work. They not only fully exploit the lightweight advantage of Mg alloys but also significantly enhance the overall plasticity, corrosion resistance, and deformation stability of the material. They are an ideal choice for lightweight structural components [10,11,12] and hold broad application prospects in areas such as vehicle body panels, battery cases, and thin-walled structural components [13,14,15].
At present, hot rolling bonding serves as the most feasible fabrication process for the large-scale industrial manufacturing of Al/Mg/Al LMCs [16]. Flat-roll hot rolling achieves high production efficiency, stable structural morphology, and homogeneous mechanical properties, outperforming conventional techniques including explosive welding, diffusion bonding, and accumulative rolling [17,18,19]. In this study, Al/Mg/Al laminated composites were prepared using a 400 °C flat rolling process, with an initial thickness ratio of 0.5 mm (Al)/1 mm (Mg)/0.5 mm (Al), and were finally rolled to a total thickness of 1 mm. Nevertheless, heavy-reduction hot rolling exhibits inferior deformation compatibility, attributed to stark structural differences between face-centered cubic (FCC) Al and hexagonal close-packed (HCP) Mg. Massive residual stress, tangled dislocations, deformation textures and shear bands emerge in finished sheets [20]. Meanwhile, the interface is dominated by mechanical interlocking, and the diffusion reaction is insufficient, which can easily result in defects such as micro-voids and insufficient bonding [21,22]. These drawbacks result in pronounced anisotropy, limited ductility and poor formability of hot-rolled Al/Mg/Al laminates. Cracking and delamination frequently occur in subsequent stamping and deep drawing, which renders the composites unqualified for industrial production. Therefore, optimizing the microstructure, eliminating residual stress, regulating the interface structure, and enhancing formability through post-rolling annealing have become key to breaking through the bottleneck of industrialization [6,23].
Annealing is the optimal approach for improving the microstructure and ductility of metallic composite materials [24,25]. During the annealing process, the deformed matrix undergoes recovery and recrystallization, with grains transforming into an equiaxed state, deformation texture weakening, and residual stress being eliminated, significantly enhancing the material’s plastic deformation capability [26,27,28]. However, for Al/Mg/Al laminated composites, the annealing temperature has a dual regulatory effect: increasing the temperature facilitates sufficient recrystallization, grain refinement, and plasticity enhancement of the Al and Mg matrices; but excessively high temperatures will substantially speed up the mutual diffusion of Al and Mg atoms at the interface, leading to the formation of a large number of brittle IMCs such as Mg2Al3 and Mg17Al12 at the interfaces [11,29,30]. These hard and brittle phases significantly reduce the interfacial bonding strength and induce stress concentration and crack initiation, resulting in a sharp deterioration in the plasticity and formability of the LMCs [17]. Therefore, obtaining the optimal annealing temperature that can both ensure sufficient softening of the matrix and inhibit the excessive growth of brittle phases at the interface, in turn balancing the contradiction between matrix softening and interfacial embrittlement, is the core to achieving excellent formability.
Over recent decades, many scholars have deeply investigated the annealing characteristics of Mg/Al and Al/Mg/Al laminated composites, confirming that annealing temperature significantly affects interfacial phase transformation, grain structure, and mechanical properties. Mihara-Narita et al. [6] conducted a study on the annealing characteristics of explosively bonded Mg/Al laminated composites and found that rising annealing temperature promotes the interfacial transformation from a single Mg17Al12 layer to a Mg17Al12 dual-layer structure. Li et al. [31] explored the annealing behaviors of ripple-interface Mg/Al laminated composites and found that within 200–350 °C, elevated temperatures contribute to the continuous thickening of interfacial IMC layers, while monotonically reducing the interfacial shear strength. Yin et al. [32] demonstrated that annealing enhances the interfacial integrity and high-temperature creep resistance of Al/Mg/Al laminated composites. Zhu et al. [33] found that annealing temperatures at or below 200 °C induce interfacial atomic diffusion and further promote interfacial metallurgical bonding. However, continuous IMC layers are generated at the interface when the annealing temperature exceeds 250 °C.
Despite existing research confirming the important role of annealing, there are still three major key deficiencies: Firstly, research has mostly focused on discrete temperature points at 200, 250, 300, and 350 °C, with large temperature intervals and sparse distribution of points in the key medium-temperature range, making it difficult to comprehensively capture the continuous trend of microstructure and mechanical properties with temperature changes. Secondly, most research uses tensile and shear properties as evaluation indicators, and the stamping and forming properties that directly determine industrial applications have not been systematically characterized. Thirdly, the stable and industrially applicable annealing process parameter range for LMCs of this material is still unclear, making it difficult to directly guide actual production.
To meet the demands of industrial production, this study, based on previous research conducted by our team, focuses on LMCs produced by flat rolling at 400 °C. Six sets of annealing temperatures, namely 200, 250, 300, 325, 350, and 375 °C, are designed, with a uniform holding time of 60 min. To resolve the competitive interplay between matrix recrystallization softening and brittle intermetallic-phase growth within the critical 300–350 °C range, an intermediate 325 °C condition was added which captures the transitional microstructural evolution that would be concealed under coarse temperature intervals. This extra sampling point enables us to trace how progressive Mg-layer recrystallization competes against the onset of accelerated intermetallic-phase thickening. Extending experiments to 375 °C further allows us to probe the upper bound of the beneficial annealing window. It reveals how excessive intermetallic growth and interface degradation eventually override the benefits from sufficient matrix recrystallization and deteriorate stamping formability. By combining densified sampling with a broader temperature range, this study systematically reveals the synergistic evolution patterns of recrystallization behavior, interface diffusion, dislocation density, and stamping formability. It clarifies the regulatory mechanisms of intermetallic compounds at the interface, crystal texture, and Schmid factors on formability, providing experimental evidence for the selection of annealing conditions for the investigated Al/Mg/Al laminates.

2. Materials and Methods

2.1. Experimental Materials

The Mg alloy used in this work was AZ31B, and the Al alloy was a 3003 alloy in the annealed temper, supplied by Shanxi Yinguang Huasheng Magnesium Co., Ltd., Wenxi, Shanxi, China. Their chemical compositions are shown in Table 1.
Table 1. Main chemical components of raw materials (mass%).

2.2. Experimental Procedure

Mg plates with dimensions of 500 mm × 300 mm × 1 mm and Al plates with dimensions of 500 mm × 300 mm × 0.5 mm were prepared. As illustrated in Figure 1, before rolling, the surfaces of Mg and Al plates were polished and cleaned to expose the pure metal matrix. The polished and cleaned metal plates were stacked and assembled into blanks. These slabs were heated to a pre-set temperature of 400 °C within a vacuum furnace for 30 min, and the heating was conducted under the safeguard of an inert gas (argon). The transfer time from furnace to rolling mill was approximately 15 s. Two-pass flat hot rolling was implemented at a rolling speed of 0.5 m/s. The nominal reduction of the first pass was 25%, calculated relative to the initial slab thickness of 2.0 mm, yielding a sheet thickness of 1.5 mm after pass 1. No reheating was performed between passes; the interpass time between the first and second rolling pass was kept at 20 s. The second pass was conducted to achieve the final sheet thickness of 1.0 mm. Both the per-pass nominal reduction and the overall thickness reduction of 50% were calculated relative to the initial slab thickness of 2.0 mm. Subsequent to rolling, the processed samples were transferred to an annealing furnace for thermal treatment. The heating rate for annealing was set to 200 °C per hour. The annealing duration remained constant at 60 min, while only the annealing temperature was altered (200 °C, 250 °C, 300 °C, 325 °C, 350 °C, 375 °C). After annealing, all specimens were subjected to furnace cooling inside the furnace to room temperature. All annealing treatments were performed under ambient air atmosphere.
Figure 1. Diagrammatic sketch of rolling and annealing process.

2.3. Microstructure and Mechanical Properties Tests

In this work, the interfacial microstructure was comprehensively characterized on cross-sections defined by the rolling direction (RD) and the normal direction (ND). Sigma 300 SEM (Zeiss, Oberkochen, Germany), together with the Oxford EDS system (Oxford Instruments, Abingdon, UK) and EBSD detector (Oxford Instruments, Abingdon, UK), was employed to characterize the Mg/Al interfacial structure. For SEM analysis, the secondary electron mode was adopted, operating at a voltage ranging from 15 to 20 kV and a working distance between 10 and 15 mm. For EDS measurements, an accelerating voltage of 20 kV and a detector take-off angle of 35° were adopted. EBSD measurements were performed at a scanning voltage of 20 kV, a beam current of 18 nA, a tilt angle of 70°, and a working distance of 15 mm. EBSD mapping was acquired with a step size of 0.5 μm. For each annealing condition, multiple regions were analyzed, and representative EBSD maps were selected for subsequent quantitative statistics. The scan area covered the Mg layer, the Al layer, and the adjacent Mg/Al interfacial zone across the RD-ND cross-section. Grains were classified as recrystallized (GOS < 2°), substructured (2° ≤ GOS ≤ 15°), and deformed (GOS > 15°) based on the grain orientation spread (GOS), defined as the average misorientation between all pixels within a grain. The average recrystallized-grain size was calculated as the arithmetic mean of the equivalent circle diameters only for recrystallized grains (GOS < 2°), and substructured and deformed grains were excluded from this size calculation. Grains intersecting the map boundary were excluded because their complete areas could not be measured. Consequently, the reported mean sizes describe fully contained recrystallized grains within the analyzed fields of view. Kernel average misorientation (KAM) maps were calculated using the default calculation settings in AZtec software (Version 2.1, Oxford Instruments, Abingdon, UK). For an in-depth investigation of interfacial phase evolution after annealing at 350 °C for 60 min, a JEOL-F200 TEM (JEOL, Tokyo, Japan) was utilized for phase characterization.
Schematic illustrations of peeling and tensile test specimens are presented in Figure 2. At room temperature, an AGS-X universal tensile testing machine (Shimadzu, Kyoto, Japan) was employed to carry out the tensile test on the annealed samples. Tensile specimens possessed a thickness of 1 mm. The stretching speed was 0.5 mm/min. The displacements were measured using a Shimadzu non-contact digital video extensometer (Shimadzu, Kyoto, Japan). For the test, specimens in the shape of dog-bones were accurately cut from the LMCs. Wire cutting was performed along the RD, 45° diagonal direction, and transverse direction (TD). The final specimens were machined with a gauge length of 9.525 mm and a width of 2 mm. To evaluate the interfacial bonding properties, peeling specimens were sliced along the RD, which corresponds to the horizontal direction in Figure 2a. Interfacial bonding strength was determined as the ratio of the maximum experimental load to the specimen width. Peeling tests were conducted at room temperature using a universal tensile tester with a loading velocity of 5 mm/min. To ensure the reliability of mechanical properties data, each set of tensile and peeling tests was repeated three times. Regarding the stamping formability, a GBW-60Z cupping machine equipped with a hemispherical punch having a diameter of 20 ± 0.05 mm was utilized to gauge the stamping formability of LMCs. The room-temperature Erichsen cupping test specimen is a 60 mm × 100 mm LMC specimen, with a blank holder force of 10 kN, and each cupping test was repeated 3 times. The microhardness of the Al layer, Mg layer and interfacial diffusion layer on the RD-ND cross-section was measured using an HVT-1000 Vickers microhardness tester (Huayin, Laizhou, China). A force of 100 g was applied and maintained for 10 s during the test. Five testing points were selected at each position to ensure experimental accuracy, and their average value was adopted as the final hardness value.
Figure 2. (a) Schematic diagram of peeling sample; (b) schematic diagram of tensile sample; (c) tensile sample.
YS was determined using the 0.2% offset-strain criterion. The strain-hardening exponent n was fitted over the uniform plastic deformation regime (approximately 1.2–6% true strain), up to the onset of necking. All mechanical properties results are expressed as mean ± standard deviation (SD), and error bars in the related figures represent SD. The differences in mechanical properties between annealing conditions are discussed by comparing the change in mean values with their corresponding SD ranges.

3. Results and Discussion

3.1. Interface SEM Morphology

SEM and EDS in Figure 3 characterize the Al/Mg interface of LMCs at different annealing temperatures, and the corresponding XRD patterns are shown in Figure 4. In this work, the interface diffusion layer is uniformly defined as the transition zone of the Mg/Al interface composition gradient. The IMCs nucleate and grow within the transition zone of the composition gradient, and the thickness of this zone is determined by the range of composition transformation obtained by EDS. When annealed at 200–250 °C, only an extremely narrow interfacial transition zone can be detected. EDS surface-scan results show negligible elemental overlap between Al and Mg, and the line-scan curve on the interface is steep, which indicates limited atomic interdiffusion within this temperature range; interfacial bonding remains dominated by mechanical interlocking inherited from the rolling process. When the annealing temperature rises to 300 °C, EDS line-scan reveals a diffusion-transition layer with a thickness of approximately 2–3 μm. EDS line-scan curves form a gentle compositional plateau within the interfacial region, and the overlapping area of Al and Mg in EDS surface scan expands clearly, pointing to pronounced enhancement of mutual atomic interdiffusion and the initiation of interfacial metallurgical reaction. Combined with the SEM interfacial micrographs in Figure 3, a diffusion-transition layer can be detected via EDS line-scan. As annealing temperature further increases to 325–375 °C, the thickness of the diffusion reaction layer keeps increasing. When the annealing temperature is 350 °C, the diffusion reaction layer thickens to about 12 μm. EDS line-scan results present continuously widened compositional plateaus, reflecting progressive thickening of the intermetallic reaction layer driven by intensified atomic interdiffusion. Meanwhile, referring to the standard-reference positions of Mg17Al12 and Mg2Al3 in Figure 4, weak diffraction signals corresponding to these two intermetallic phases are detectable from 325 °C onward [34]. When annealed at 375 °C, the interdiffusion of the elements is further intensified; the total thickness of the interface reaction layer increases. In addition, due to the difference in diffusion coefficients between the Mg and Al atoms, the Kirkendall effect occurs in the diffusion zone during high-temperature annealing. Figure 5 shows a schematic diagram of the evolution trend of vacancy aggregation and pore band formation based on diffusion theory. As shown in Figure 5, the increase in annealing temperature accelerates the interdiffusion of Mg and Al atoms, promoting the nucleation and growth of Mg-side Mg17Al12 and Al-side Mg2Al3. These intermetallic compounds continue to increase in thickness with increasing annealing temperature. However, excessively thick brittle intermetallic compound layers can easily induce crack initiation under external loading, and the cracks propagate along the brittle intermetallic phases, reducing the effective bearing area of the interface and ultimately damaging the interfacial bonding properties [35,36].
Figure 3. SEM images and EDS spectra of Mg/Al interfaces in LMCs at different annealing temperatures: (a,c) interface morphology and EDS line analysis and (b,d) EDS area analysis.
Figure 4. XRD patterns at different annealing temperatures.
Figure 5. Schematic diagram of element diffusion at different annealing temperatures.

3.2. Mechanical Properties

3.2.1. Microhardness

Figure 6 shows the microhardness distribution of LMCs at different annealing temperatures. Figure 6a shows the micro-indentation morphology, and Figure 6b shows the hardness statistical bar chart, which intuitively reflects the difference in hardness between the matrix and the interface region and its variation with annealing temperature. The micrograph in Figure 6a shows the Mg layer, Al/Mg interface region, and Al layer from top to bottom. As shown in Figure 6a, the Vickers hardness indentation size of the Mg layer is much smaller than that of the Al layer, and the indentation size intuitively reflects the hardness. A smaller indentation size corresponds to higher hardness, whereas a larger indentation size indicates lower hardness. It can be inferred that the hardness of the Mg matrix is higher than that of the Al matrix. As shown in Figure 6b, the microhardness of the Al alloy matrix continues to decrease with increasing annealing temperature, gradually decreasing from about 45 HV at 200 °C to about 28 HV at 375 °C. As the annealing temperature increases, recovery and recrystallization in the Al layer reduce the work hardening introduced by rolling through dislocation rearrangement and annihilation and the formation of recrystallized grains with lower dislocation densities. With further increases in temperature, the growth of recrystallized grains increases the distance over which dislocations can move before encountering grain boundaries, thereby reducing the resistance provided by these boundaries to plastic deformation. Therefore, as the annealing temperature increases, the hardness of the Al alloy matrix gradually decreases. As shown in Figure 6b, as the annealing temperature increases, the microhardness of the Mg alloy matrix gradually decreases, but the decrease is smaller than that of the Al alloy, slowly decreasing from about 71 HV at 200 °C to about 62 HV at 375 °C. The reason is that, on the one hand, as the annealing temperature increases, the Mg alloy undergoes recovery and recrystallization, and the hardness gradually decreases. On the other hand, due to the dense hexagonal crystal structure and recovery and recrystallization characteristics of Mg alloys, the softening process dominated by basal slip is relatively slow, and some work hardening effects are still retained during annealing in the range of 200–375 °C. Therefore, the decrease in microhardness of the Mg alloy matrix is smaller than that of the Al alloy. The hardness change in the Al/Mg interface region exhibits significant non-monotonic characteristics. The hardness slowly increases from about 56 HV to 64 HV in the range of 200–300 °C. When the annealing temperature exceeds 300 °C, the hardness sharply increases, reaching a peak of about 110 HV at 350 °C. At 375 °C, there is a slight decrease, but it still remained at a high level close to 100 HV. This phenomenon is due to the intensified diffusion of Al and Mg elements at the interface as the annealing temperature increases, forming high-hardness intermetallic compound layers such as Mg2Al3 and Mg17Al12. When the annealing temperature is between 200 °C and 300 °C, these intermetallic compounds are generated less, so their hardness increases slowly. When the annealing temperature is between 300 °C and 350 °C, these intermetallic compounds accumulate in large quantities, causing a sudden increase in interfacial hardness. However, when the annealing temperature rises to 375 °C, the difference in diffusion rate between the Al and Mg atoms triggers the Kirkendall effect, resulting in a small number of microporous defects at the interface junction. Holes will reduce the resistance to compression deformation, resulting in a slight decrease in the average hardness at the interface, but the main body at the interface is still a high-hardness intermetallic compound, so the hardness remains at a high level. Overall, the interfacial hardness of the Al/Mg LMCs increases gradually at lower annealing temperatures, rises markedly between 300 and 350 °C, and then decreases slightly at 375 °C. At 350–375 °C, the interfacial hardness is higher than that of both the Al and Mg matrices.
Figure 6. The Vickers hardness test: (a) the micro-indentations and (b) the Vickers hardness at different layers of LMCs.

3.2.2. Tensile Properties

Figure 7 shows the evolution of the mechanical properties of Al/Mg/Al laminated composites along different rolling directions (RD, 45°, TD) after annealing at different temperatures. Figure 7a–c show the engineering stress–strain curves for different rolling directions, and Figure 7d shows the bar charts of average YS, ultimate tensile strength (UTS), and EL of the composite plate. The bar-chart data presented in Figure 7d correspond to arithmetic means calculated from tensile measurements along RD, 45°, and TD directions. Table 2 lists the YS, UTS, EL, σs/σb and n values of LMCs in different rolling directions.
Figure 7. Tensile properties of LMCs at different annealing temperatures: (a–c) engineering stress–strain curves and mechanical properties of LMCs along the RD, 45°, TD directions; (d) arithmetic-mean yield strength, ultimate tensile strength and elongation obtained from RD, 45°, and TD direction tensile tests.
Table 2. Tensile properties of LMCs annealed at different temperatures along RD, 45°, and TD, together with their directional averages.
As shown in Figure 7a–c, with the increase in annealing temperature from 200 °C to 375 °C, the stress–strain curves in all directions show an overall evolution pattern of gradually decreasing peak stress and shifting necking position backwards. After yielding at 200 °C, the stress of the sample rapidly rises to its peak and then fractures quickly. The uniform plastic deformation segment is the shortest and necking occurs earliest. This is because, at this time, the matrix still retains a high dislocation density and rolling deformation structure, and the space for dislocation propagation after yielding is limited, resulting in insufficient reserve for work hardening. At 250 °C, the uniform section is slightly elongated, but the work hardening reserve is still limited. When the temperature continues to rise to 300 °C, recrystallization advances further, and the initial dislocation density of the matrix significantly decreases. After yielding, dislocations can continue to proliferate, and the uniform plastic deformation segment reaches its longest. After 325 °C, the grains begin to coarsen and the uniform section is shortened. At 350 °C, the work hardening ability is further enhanced, and the uniform section slightly recovers. At 375 °C, excessive recovery weakens the work hardening ability, further reduces the peak stress, and there is little change in the uniform section compared to 350 °C. Comparing the three directions, it can be seen that the peak stress in the TD direction is always the highest, and the work hardening section is the steepest, which originates from the plastic anisotropy of the laminated composite. The tensile curves obtained along RD, 45° and TD directions display different mechanical responses, reflecting the plastic anisotropy intrinsic to the Al/Mg/Al laminated composite. The earliest unstable fracture in the RD direction is due to the elongation of grains along the rolling direction, which makes deformation easily concentrated in a few favorably oriented grains, and stress concentration at grain boundaries occurs earlier.
As shown in Figure 7d, YS continuously monotonically decreases from 213.6 MPa at 200 °C to 130.2 MPa at 375 °C with increasing annealing temperature. This is because the recovery and recrystallization gradually eliminate the rolling deformation structure and dislocation strengthening, the initial dislocation density of the matrix continuously decreases, and the resistance to dislocation movement inside the grain continues to decrease. The change in UTS is different: after a significant decrease at 200–250 °C, it rises to 198.1 MPa at 300 °C, at 325 °C it decreases to 185.4 MPa, at 350 °C it slightly rebounds to 187.2 MPa, and at 375 °C it decreases further to 181.3 MPa, showing an overall fluctuating decline. This is because UTS consists of two parts: YS and incremental work hardening after yielding. At lower annealing temperatures, incomplete recrystallization results in limited recovery of work hardening ability, and the decrease in YS directly lowers UTS. With the increase in annealing temperature, the degree of recrystallization increases, the initial dislocation density of the matrix decreases, the space for dislocation proliferation increases after yielding, and the increase in work hardening partially compensates for the decrease in YS. As a result, UTS shows two small increases at 300 °C and 350 °C. Excessive recovery at 375 °C weakens the work hardening ability, leading to a further decrease in UTS. EL slowly increases between 200 °C and 300 °C, reaching a peak of 12.3% in the full temperature range at 300 °C, and then fluctuates between 9.6% and 10.2% thereafter. At 300 °C, recrystallization is already sufficient and the grains are still small, with good deformation coordination, resulting in the highest elongation rate. After 325 °C, the grains gradually coarsen, and dislocations accumulate more at the grain boundaries. Stress concentration is more likely to occur near the grain boundaries, so the EL drops to 9.6%. The improvement of work hardening at 350 °C raised the EL to 10.2%, but it was not enough to offset the adverse effects of grain coarsening. At 375 °C, excessive recovery weakens the work hardening ability and reduces the ability for uniform deformation. At the same time, further coarsening of the grains exacerbates the stress concentration at grain boundaries, resulting in a further decrease in EL to 9.6%.
From Table 2, it can be seen that the average σs/σb continuously decreases from 0.942 at 200 °C to 0.718 at 375 °C, with 0.863 at 250 °C, 0.814 at 300 °C, 0.760 at 325 °C, and 0.733 at 350 °C, showing a monotonic downward trend overall. The continuous decrease in σs/σb indicates that the rate of decrease of YS is faster than that of UTS, and the ability of the material to resist local concentrated deformation continues to increase after yielding. At 200 °C, the material still retains the rolled work-hardened state, with a high initial dislocation density. After yielding, the space available for dislocation propagation is limited, and necking occurs when the material approaches the maximum bearing stress. Therefore, YS is close to UTS, and the σs/σb is as high as 0.942. As the annealing temperature increases, static recrystallization continuously reduces the initial dislocation density, and YS significantly decreases. At the same time, dislocations continuously proliferate and interact, enlarging the gap between UTS and YS and leading to a monotonic reduction in σs/σb. At 350 °C, σs/σb falls to 0.733, a considerable reduction compared with the value obtained at 200 °C, indicating full softening of the matrix. After yielding, the slope of the stress–strain curve is larger, and the material’s ability to resist local concentrated deformation is significantly enhanced. At 375 °C, the σs/σb further decreases to the lowest point of 0.718 in the entire temperature range, and there is a large space for the material to continue deformation after yielding, which is conducive to the uniform distribution of strain in the subsequent forming process.
As shown in Table 2, the evolution trend of the strain-hardening index n with annealing temperature is that its average value continuously increases from 0.125 at 200 °C, reaches a peak of 0.291 at 350 °C, and falls back to 0.272 at 375 °C. This indicates that in the temperature range of 200–350 °C, static recrystallization significantly reduces the initial dislocation density and softens the matrix, resulting in a decrease in YS. At the same time, the continuous proliferation of dislocations during the deformation process allows the material to continue hardening even after yielding, and the n value increases accordingly. At 375 °C, excessive static recovery weakens the matrix’s ability to retain dislocations, the work hardening effect weakens, and the n value decreases instead of increasing.
Figure 8 shows SEM images of the fracture surface of Al/Mg/Al laminated composites after tensile fracture at different annealing temperatures. As shown in Figure 8, the interface bonding state and fracture behavior undergo significant changes with the variation of annealing temperature. At an annealing temperature of 200 °C, the bonding surface of the sample was well bonded (without obvious cracks or separation areas), and the Al layer had significant necking. The fracture surfaces of both Al and Mg layers had abundant toughness dimples. It can be inferred that the interfacial bonding strength is good at an annealing temperature of 200 °C. At 300 °C, the interface remains well bonded without obvious interfacial debonding, while the Al and Mg matrices still maintain their typical toughness and dimple morphology. At an annealing temperature of 350 °C, enhanced interfacial atomic diffusion promotes the formation of dense metallurgical bonds at the Al/Mg interface. At this temperature, the interlayer bonding strength is improved, and the interface necking characteristics are widely distributed, effectively suppressing early delamination cracking and interface debonding failure during tensile deformation. At the same time, high-temperature annealing promotes the full static recovery and recrystallization of the Mg layer, supplemented by texture softening effect, which improves the plasticity of the matrix. Moreover, at this temperature, the dimples in the Mg layer become more clearly developed and relatively uniform in size, indicating a more ductile fracture morphology. After further annealing at a high temperature of 375 °C, although the matrix continues to soften and the plastic reserve of the Mg layer is still sufficient, excessively high temperatures can easily lead to excessive diffusion of interface elements and coarsening of interface structures, resulting in reduced interlayer bonding stability. Small cracks and weak bonding phenomena begin to appear locally at the interface, and the uniformity of fracture toughness dimples deteriorates. Therefore, the over-annealing at 375 °C has the disadvantage of damaging the interface structure.
Figure 8. Scanning electron microscopy (SEM) images of tensile fracture surfaces of LMCs in the RD-ND plane at different annealing temperatures after tensile testing along the TD.

3.3. Stamping Formability

Figure 9a shows the Erichsen cupping specimen and crack morphology, Figure 9b shows the Erichsen values (IE, maximum punch travel when fracture initiates on the specimen) at different annealing temperatures, and Figure 10 shows the SEM cross-sectional morphology of the specimen after cupping fracture at different annealing temperatures. As shown in Figure 9a, the composite plate forms a typical arch structure during the cupping deformation process, and the crack direction is perpendicular to the rolling direction. From the IE in Figure 9b, it can be seen that the IE of the 200 °C annealed sample is only 2.12 mm, which is the lowest value in the entire measured temperature range. This is due to the low degree of metallurgical bonding at the interface, insufficient interlayer coordinated deformation ability after low-temperature annealing, and the mainly mechanical interlocking at the interface. Stress concentration is prone to occur during cup-shaped loading, promoting early crack initiation and ultimately limiting formability. With the increase in annealing temperature, the IE value significantly increased from 2.12 mm at 200 °C to 3.25 mm at 250 °C. This is partly due to the fact that recovery and partial recrystallization at 250 °C eliminated most of the rolling hardening, resulting in a significant decrease in YS. The σs/σb decreased from 0.942 to 0.863, and the plate changed from “difficult to form” to “formable”. On the other hand, annealing promotes the initial diffusion of interface elements, and the interlayer bonding transitions from mechanical interlocking to metallurgical bonding, improving the coordinated deformation ability. After further increasing the annealing temperature to the range of 300–375 °C, IE stabilized at a relatively high level of 3.15 mm–3.31 mm without significant fluctuations in value. This is because the cupping test is subjected to bidirectional tensile stress, and the forming limit is mainly constrained by the intrinsic plasticity of the Mg layer and the coordination of interface deformation. After 250 °C, rolling hardening has been basically eliminated, and although recrystallization continues to advance, it further increases the work hardening index. However, there is limited room for improvement in cupping forming, and the maximum deformation that the sheet can form is close to the intrinsic upper limit of the composite plate system.
Figure 9. (a) Erichsen cupping specimen and crack morphology and (b) IE value.
Figure 10. Fracture morphology of cupped specimens at different annealing temperatures.
From Figure 10, it can be seen that at the four temperatures measured, the main cracks of the sample propagate along the interface at a diagonal angle of 45°, exhibiting shear fracture characteristics. In the sample annealed at 200 °C, the Mg/Al interface was mainly mechanically interlocked, with weak element diffusion and insufficient metallurgical bonding. Passivation effect can be observed at the crack tip. Under the annealing condition of 300 °C, a clear diffusion layer is formed at the interface, achieving preliminary metallurgical bonding. However, the thickness of the diffusion layer is relatively thin, and the interface bonding strength is still low. Although IE is at a relatively high level, the deformation matching between the matrix and the interface is poor, and the deformation uniformity and stability are not as good as those of the 350 °C sample. When annealed at 350 °C, Al and Mg elements undergo sufficient mutual diffusion, and the interface metallurgical bonding quality is good. Under the action of shear load, cracks propagate along the 45° direction inside the Mg matrix, and there is no debonding or delamination at the interface. The IE remains stable at 3.27 mm. When the annealing temperature rises to 375 °C, the interface elements excessively diffuse, and the brittle intermetallic compound layer significantly thickens. Although the main crack still propagates along the 45° direction, delamination defects appear at the interface position, and cracks extend and propagate along the brittle interface layer. The fracture mode changes from matrix-dominated shear fracture to interface brittle separation fracture, which is the main reason for the deterioration of the formability of composite plates.

3.4. Combined Properties

Figure 11 shows the variation of peeling strength at different annealing temperatures. Figure 11a shows the peeling strength–distance curve obtained from the peeling test. Figure 11b shows the average peeling strength bar chart, and Figure 12 shows the SEM morphology, EDS surface scan, and point analysis results of the Al layer surface after peeling. The micrograph enclosed by the red dashed frame in the upper right corner of Figure 12 is a magnified view taken from this peeling surface, showing the detailed fracture microstructure. According to Figure 11, the average peeling strength of the sample annealed at 200 °C is the highest, about 12.3 N/mm, and the peeling curve oscillates significantly between 10 N/mm and 18 N/mm. This is because the interface after hot rolling mainly relies on mechanical interlocking, with limited element diffusion. During the peeling process, cracks repeatedly bypass the concave–convex structure of the interface, and strength peaks appear every time they cross an interlocking point. When the annealing temperature rises to 250 °C, the average peeling strength drops sharply to about 5.5 N/mm, and the overall curve shifts downward with reduced fluctuations, indicating that recovery and partial recrystallization have released rolling residual stresses, and the interface interlocking structure begins to weaken, while metallurgical bonding has not yet been fully established. When the temperature continued to rise to 300 °C, the peeling strength slightly increased to about 6.3 N/mm, indicating that the metallurgical bonding caused by the initial diffusion of elements began to compensate for the weakening of the interlocking effect. At 325 °C, the peeling strength drops to the lowest value in the entire group, only about 1.1 N/mm, and the curve runs almost to the bottom. At this point, the interface interlocking effect has basically disappeared, and the metallurgical bonding is still in a weak stage, with the weakest bonding between the two layers. At 350 °C, the interdiffusion of Mg and Al elements is significantly enhanced, the metallurgical bonding at the interface is improved, and the peeling strength is restored to about 4.1 N/mm. At 375 °C, the peeling strength further increased to about 8.1 N/mm. Based on Figure 12 analysis, the Al surface is relatively flat after peeling at 250 °C, and Mg (red) is sporadically distributed in stripes in EDS surface scan. The Al content at point A is as high as 89.8%, while Mg is only 6.9%, indicating that the cracks mainly propagate along the interface with little Mg residue. At 325 °C, the peeled surface became significantly rougher, and the residual area of Mg in EDS surface scan increased significantly. At 375 °C, a large number of matrix tears and wrinkles can be seen on the peeled surface, with long cracks penetrating the surface. The Mg content at point C significantly increases to 36.8%, and Al and Mg coexist, indicating that Al and Mg diffuse deeper into each other at the interface at high temperatures. During peeling, they no longer separate cleanly along a single interface, but tear off a layer of matrix material on both sides, increasing the actual tearing area and the required peeling force. In summary, the peeling strength of composite panels varies non-monotonically with annealing temperature. This is the result of the combined effects of interface mechanical interlocking, metallurgical bonding, reaction-layer thickness, and crack-propagation path.
Figure 11. (a) Interface delamination curves at different annealing temperatures and (b) average peeling strength at different annealing temperatures.
Figure 12. Peel off surface SEM image and EDS scan.

4. Effects of Microstructure on the Properties of Al/Mg/Al Laminated Composites

Figure 13 shows the microstructure distribution, grain-state fractions, and average recrystallized grain size of recrystallized (blue), substructured (yellow), and deformed (red) grains in LMCs prepared at various temperatures. The grain state is classified based on EBSD grain orientation spread (GOS): GOS < 2° is determined as recrystallized grains, 2–15° is substructured grains, and GOS > 15° is deformed grains. As shown in the figure, the recrystallization response of the Mg layer and the Al layer to annealing temperature exhibits significant differences, and the evolution patterns of the two layers are significantly different. When annealed at 200 °C, the Mg layer is mainly composed of deformed grains and substructured grains, with a recrystallization fraction of about 40% and an average recrystallized grain size of about 3.4 μm. The Al layer is almost entirely composed of deformed grains, with a recrystallization fraction of less than 5% and a recrystallized grain size of only about 2.2 μm. After the annealing temperature was raised to 250 °C, the proportion of substructured grains in the Mg layer significantly increased, and the number of recrystallized grains continued to increase, with an average size of 4.5 μm. The deformation structure of the Al layer did not show significant recovery, and the recrystallized grain size was only about 2.4 μm, indicating no obvious recrystallization evolution. When the annealing temperature rises to 300 °C, recrystallized grains become dominant in the Mg layer, with a mean equivalent circle diameter of approximately 5.0 μm, while a residual fraction of substructured grains remains. The Al layer only shows a small number of substructured grains in the near interface region, with a recrystallized grain size of about 2.3 μm, and the deformation structure still dominates. When the temperature further rises to 325–350 °C, the recrystallized grain size of the Mg layer slowly increases to 5.1 μm–5.6 μm, and the uniformity of the microstructure is further improved. At the same time, the proportion of Al layer recrystallization significantly increased from 4% to 76%, and recrystallization preferentially nucleated in the near interface region. The grain size increased from 3.6 μm to 6.3 μm. The Al layer below 350 °C requires a higher thermal activation temperature to undergo recrystallization, and the recrystallized grains are always relatively small. When the annealing temperature rises to 350 °C, the energy conditions required for Al layer recrystallization are met, and the high dislocation density and lattice distortion introduced by rolling are significantly eliminated, accompanied by the nucleation and growth of new recrystallized grains. The recrystallized crystal nuclei formed at the interface rapidly expand towards the Al layer matrix, significantly enlarging the recrystallized region of the Al layer [37]. At this point, the Mg layer has completely recrystallized, the internal stress has been completely released, and the squeezing effect on the Al layer at the interface has weakened, which is also conducive to the occurrence of Al layer recrystallization. After the annealing temperature was raised to 375 °C, the Mg layer was predominantly recrystallized, with the mean equivalent circle diameter of recrystallized grains increasing to approximately 7.6 μm. The corresponding mean diameter in the Al layer increased to approximately 10.7 μm. Recrystallized, substructured, and deformed regions coexisted near the interface, indicating a heterogeneous microstructure. Compared with 350 °C, the recrystallized fraction of the Al layer decreased despite the increase in the mean size of recrystallized grains, indicating that grain size and recrystallized fraction exhibited different temperature dependences. Comparing the evolution trends of the two layers, the Mg layer exhibited a higher recrystallized fraction than the Al layer at each investigated annealing temperature. However, the mean equivalent circle diameter of recrystallized grains is larger in the Mg layer at 200–325 °C, whereas the Al layer exhibits larger mean values at 350–375 °C, indicating different recrystallization behaviors in the two layers. These differences may be associated with the combined effects of the intrinsic properties, stored deformation energy, and local interfacial stress conditions of Mg and Al.
Figure 13. Recrystallization, substructure, and deformation microstructure, recrystallization fractions, and average recrystallized grain size of LMCs at different annealing temperatures.
Figure 14 shows the IPF orientation maps of the Mg and Al layers and the {0001}, {10–10} and {11–20} pole figures of the Mg layer after annealing at 200–375 °C. Together with the grain-state maps and statistics in Figure 13, these results describe the evolution of grain morphology, recrystallization and crystallographic texture with annealing temperature.
Figure 14. IPF and PF maps of the Mg layer in LMCs along the RD-ND plane at different annealing temperatures.
In the low-temperature annealing range of 200–250 °C, the overall microstructure is still dominated by deformation, with obvious deformation areas and internal grain orientation gradients, and the grain boundary contours are blurred. At this stage, only dislocation recovery and substructure adjustment occurred, without triggering sufficient recrystallization. The corresponding {0001} basal pole figure shows strong basal texture, with a concentrated pole density close to the ND direction, indicating that the genetic orientation of rolling is basically preserved under low-temperature annealing. The prismatic texture also exhibits obvious orientation aggregation, which is consistent with the stability law of low-temperature annealing texture in Mg alloys reported in the literature.
When the annealing temperature increases to 300–325 °C, static recrystallization occurs and leads to grain refinement. From the IPF maps, the original coarse deformed grains are gradually replaced by fine and uniform equiaxed recrystallized grains, and the microstructure uniformity is improved. With further increase in annealing temperature, the recrystallized grains grow gradually.
When the annealing temperature is further increased to 350–375 °C, grain coarsening is observed in the IPF maps, together with a heterogeneous grain size distribution and some relatively large grains. The {0001} basal and prismatic pole figures show changes in texture intensity and orientation distribution; however, the basal texture does not exhibit a monotonic weakening trend over the investigated temperature range. Grain coarsening may reduce the contribution of grain boundary strengthening and thus contribute to the decrease in strength at higher annealing temperatures.
Overall, annealing temperature plays a dominant role in regulating the microstructure and texture of Mg alloys: recovery prevails at low temperatures with stable texture; recrystallization dominates at medium temperatures and achieves grain refinement together with texture weakening; grain growth becomes predominant at high temperatures, bringing further texture homogenization accompanied by grain coarsening.
KAM is defined as the average orientation difference between a measurement point inside a grain and its neighboring measurement points within a set kernel range, used to characterize local lattice distortion. Due to the fact that local orientation distortion directly reflects the accumulation state of dislocation structures, KAM can be used to describe the distribution of geometrically necessary dislocations (GND) and changes in local strain fields: generally speaking, the higher the KAM value, the more severe the corresponding plastic deformation and the higher the density of lattice defects. On this basis [38], the geometrically necessary dislocation density (ρGND) can be estimated from the average KAM value, and its calculation expression is:
ρ G N D = 2 KAM ave μ b
In this equation, ρGND is the geometrically necessary dislocation density, KAMave is the average KAM value, μ is a fixed step size of 0.5 μm, and b is the Burgers vector length (0.312 nm for Mg and 0.286 nm for Al). A positive correlation exists between ρGND and KAMave, where increasing KAM values correspond to elevated ρGND values.
Figure 15 shows the KAM distribution of Mg and Al layers in composite plates at different annealing temperatures. At all annealing temperatures, the KAMave and ρGND of the Al layer were significantly higher than those of the Mg layer, which is due to the greater plastic deformation and higher deformation energy stored in the Al layer during the rolling process. This corresponds perfectly to the results of EDS characterization showing a more uniform distribution of elements in the Al layer and more significant grain deformation in the IPF graph. When annealed at low temperatures (200–250 °C), the KAMave of the Mg layer is 0.78–0.81°, corresponding to a ρGND of 2.23 × 1014–2.28 × 1014 m−2; the KAMave of the Al layer is 1.27–1.69°, corresponding to a ρGND of 4.10 × 1014–4.69 × 1014 m−2. As shown in the figure, both the Mg layer and the Al layer exhibit yellow-green high-orientation-difference regions during low-temperature annealing, with the Al layer having a larger area and higher orientation difference, which indicates severe lattice distortion and higher geometrically necessary dislocation density within its grains. At this stage, recovery is the main focus, with only limited dislocation slip, climb, and annihilation occurring, and deformation storage energy has not yet been fully released. When the annealing temperature is increased from 300 °C to 325 °C, compared with the low-temperature range, the KAMave of the Mg layer decreases to 0.51–0.58°, and the ρGND decreases to 1.37 × 1014–1.55 × 1014 m−2; the KAMave of the Al layer decreases to 1.31–1.56°, and the ρGND decreases to 3.93 × 1014–4.39 × 1014 m−2. At this time, the proportion of high-orientation-difference regions in the Mg layer and Al layer decreases, and the proportion of low distortion blue regions increases, indicating that recovery and recrystallization occur synchronously, and a large number of dislocations are affected. Instances of annihilation and lattice distortion gradually decrease, which is consistent with the trend of increasing the proportion of equiaxed crystals in the IPF diagram and decreasing the texture strength in the PF diagram [39].
Figure 15. KAM distribution map of Mg and Al layers in LMCs prepared at different annealing temperatures.
When the annealing temperature rises to 350 °C, the KAMave and ρGND of the composite plate reach the lowest values within the testing temperature range: the KAMave of the Mg layer is only 0.30°, and the ρGND drops to 0.61 × 1014 m−2; the KAMave of the Al layer is 0.62°, and the ρGND drops to 1.67 × 1014 m−2. Both the Mg layer and the Al layer are dominated by large areas of blue low orientation difference, with only a small amount of weak deformation near the interface. This is because 350 °C is within the effective range of the recrystallization temperature for both layers of the alloy: this temperature is higher than the recrystallization temperature of Mg alloy (250–300 °C), allowing the Mg layer to achieve complete recrystallization and basic elimination of intragranular dislocations. It is also located in the core range of Al alloy recrystallization temperature (300–400 °C), which significantly expands the recrystallization area of the Al layer, causes a large number of dislocations to annihilate, and minimizes lattice distortion [38]. At the same time, the mutual diffusion of interface elements at this temperature is relatively sufficient but not excessive: although intermetallic compounds have intermittently precipitated at the interface, thick and continuous layers have not yet been formed, and no obvious lattice mismatch or stress concentration has been introduced at the interface. This is also one of the reasons why KAMave reaches its lowest value at 350 °C.
When the annealing temperature rises to 375 °C, the KAMave of the Mg layer increases to 0.37° and the ρGND increases to 0.78 × 1014 m−2; the KAMave of the Al layer increases to 1.02° and the ρGND increases to 2.87 × 1014 m−2. It is worth noting that the yellow-green high-orientation-difference area in the interface region increases, which is due to the intensified diffusion of interface elements at high temperatures, forming a large number of intermetallic compounds along the interface. Meanwhile, during the growth process of recrystallized grains, grain boundary migration is accompanied by dislocation proliferation, resulting in lattice distortion and increased dislocation density [38].
Figure 16 shows the Schmid factor (SF) distribution of {0001} <11–20> basal, {1–100} <11–20> prismatic, and {11–22} <11–23> conical slip systems in magnesium alloys at different annealing temperatures. Figure 17 presents the corresponding SF statistical histograms. As shown in Figure 17, the basal texture of the Mg layer is very strong during annealing at 200 °C, and the average SF of basal slip is only 0.21. Most grains are hard-oriented, which is not conducive to the initiation of basal slip. Although the average SF value of basal slip does not change significantly, it shows an overall upward trend with the increase in annealing temperature: it remains at about 0.22 at 250–325 °C, rises to 0.24 at 350 °C annealing temperature, and further increases to 0.25 at 375 °C annealing temperature. In contrast, the average SF of prismatic slip and conical slip remained at a high level of 0.41–0.44 throughout the entire temperature range, without showing a significant temperature correlation. Although the SF of slip between prismatic and conical surfaces is relatively high, due to the dense hexagonal structure of Mg, the basal plane {0001} is the most densely arranged crystal plane, and the lattice resistance that dislocations need to overcome to slip along the densest plane is the smallest. Therefore, the critical shear stress (CRSS) of basal plane slip is the lowest, making it the most easily initiated deformation mode at room temperature. Although the slip between prismatic and conical surfaces has a higher SF, their atomic arrangement is sparse and the resistance to dislocation slip is greater. Therefore, higher stress is often required to activate them at room temperature. Therefore, when the basal slip is limited and the stress concentration at the grain boundary is large enough, prismatic slip, conical <c+a> slip, and tensile twinning will serve as supplementary deformation mechanisms to participate in coordinated deformation. Among them, the cone surface c+a slip and tensile twinning can provide strain components in the c-axis direction, which is a key mechanism for coordinating c-axis deformation and compensating for the shortcomings of basal and prismatic slip that only provide a-direction slip. At the same time, the overall increase in the SF for basal slip with annealing temperature may be associated with changes in crystallographic orientation during recrystallization. The microscopic mechanism can be confirmed by Figure 16: the high SF region is mainly composed of small equiaxed crystals formed by static recrystallization, indicating that recrystallization disperses the grain distribution originally concentrated in basal orientation through the nucleation and growth of new grains, thereby weakening the strong basal texture formed by rolling and causing more grains to shift to an orientation conducive to basal slip. At the same time, recrystallization also enhances the strain coordination deformation ability of grain boundaries by refining grains and increasing the proportion of large-angle grain boundaries, making adjacent grains more prone to slip without cracking. Therefore, recrystallization improves the plastic deformation ability of the magnesium layer by improving the slip geometry conditions of the basal plane, forming a recrystallized structure, and enhancing the coordinated deformation ability of grain boundaries, providing important micro mechanism support for the improvement of the elongation and cupping formability of composite plates.
Figure 16. SF plots of different slip systems in Mg layers of LMCs at different annealing temperatures.
Figure 17. Histogram of SF distribution in different slip systems of Mg layer in LMCs prepared at different annealing temperatures.
From the above analysis, it can be seen that the composite plate has good comprehensive mechanical and formability properties when annealed at 350 °C: n reaches a peak value of 0.291, ρGND is the lowest, EL is 10.2%, UTS is 187.2 MPa, σ s ∕ σ b ¯ ratio is 0.733, IE is stable at 3.27 mm, and peeling strength is about 4.1 N/mm. To elucidate the interface microstructure behind these properties, TEM observations were conducted on the sample at this annealing temperature along the RD-ND direction. Figure 18 shows the bright field image, element plane distribution, and selected area electron diffraction (SAED) results. The yellow dashed line represents the boundary between the Al matrix and the Mg-Al diffusion reaction layer. From the bright field image, it can be seen that the Al/Mg interface is continuous, and no resolvable pores, microcracks, or unbonded areas are observed within the measured field of view. The EDS surface scanning results indicate that the concentration of Al element gradually decreases from the Al layer to the Mg layer, while the concentration gradient of Mg element is opposite. The two form a continuous transition zone at the interface, rather than a steep abrupt interface, confirming that Al and Mg atoms undergo sufficient mutual diffusion during annealing. The SAED results show that the diffraction spots on the Al side (red dashed box) are sharp and symmetrical, without discernible elongation, indicating good crystallinity within the probed Al region. On the Mg side (blue dashed box, crystal band axis [−311]), polycrystalline spots are arranged in a regular pattern, with clear and non-splitting spots, indicating good crystallinity of Mg grains in this area. The above results demonstrate that a continuous and well-bonded diffusion interface forms at the observed region under 350 °C annealing, and both matrix layers show good crystallinity. This is the microstructure reason why the composite plate has good comprehensive mechanical and formability properties at this annealing temperature.
Figure 18. TEM morphology of newly bonded interface in LMCs annealed at 350 °C for 60 min.

5. Conclusions

This article investigates the effects of annealing temperature (200–375 °C, holding for 60 min) on the interface structure, microstructure evolution, dislocations, texture, mechanical properties, and stamping formability of LMCs fabricated by flat rolling at 400 °C. The main conclusions are as follows:
  • As the annealing temperature increases, the mechanical interlocking brought by rolling at the Al/Mg interface gradually transforms into metallurgical bonding driven by elemental interdiffusion, and intermetallic compound layers of Mg17Al12 and Mg2Al3 continue to thicken. Under low-temperature annealing at 200–250 °C, the degree of atomic diffusion is limited, with only a narrow interface transition zone present. After the temperature exceeds 300 °C, intermetallic compounds begin to form noticeably at the interface. At a high temperature of 375 °C, excessive elemental interdiffusion forms a thick and continuous brittle intermetallic compound layer, which can easily induce crack initiation and degrade the reliability of interface bonding.
  • There is a significant difference in the recrystallization behavior between Mg and Al layers. As the annealing temperature increases, Mg alloys undergo recovery, static recrystallization, and grain growth. The Mg layer is basically recrystallized at 300–325 °C, and obvious grain coarsening occurs at 350–375 °C. The Al layer remains predominantly deformed at annealing temperatures up to 325 °C, whereas its recrystallized fraction increases markedly at 350 °C. The geometrically necessary dislocation density of both the Mg layer and the Al layer shows a trend of first decreasing and then increasing, reaching its minimum value at 350 °C. Weakening the basal texture of magnesium alloys increases the average SF of basal slip and improves the coordinated deformation ability of the Mg matrix.
  • YS decreases monotonically with increasing annealing temperature, from 213.6 MPa at 200 °C to 130.2 MPa at 375 °C; UTS shows a fluctuating downward trend; EL reaches a peak of 12.3% at 300 °C and fluctuates within the range of 9.6–10.2% at higher temperatures. σs/σb continues to decrease, while n reaches its maximum value of 0.291 at 350 °C. The microhardness of aluminum and magnesium substrates gradually decreases with increasing temperature. Affected by the formation of hard and brittle intermetallic compounds, the interfacial hardness sharply increases over the range of 300–350 °C. The peeling strength exhibits a non-monotonic variation: reaching a maximum value of 12.3 N/mm at 200 °C, dropping to a minimum of 1.1 N/mm at 325 °C, and then recovering at 350 °C and 375 °C. This is the result of the combined effects of mechanical interlocking, metallurgical bonding, and the thickness of the IMC layer.
  • The metallurgical bonding at the interface of the annealed sample at 200 °C is insufficient, with an IE of only 2.12 mm. After 250 °C, the IE stabilizes at 3.15 mm–3.31 mm. At 375 °C, the brittle intermetallic compound layer is too thick, and interface delamination occurs during cupping deformation, which damages the formability. By comprehensively comparing the interface state, microstructure, tensile mechanical indicators, peeling strength, and cupping ability at different annealing temperatures, it was found that under the present experimental conditions, after annealing at 350 °C for 60 min, a continuous diffusion bonding layer with sound interfacial bonding was formed in the characterized region at the interface of the composite material, with a σs/σb of 0.733, IE of 3.27 mm, peeling strength of 4.1 N/mm, and good work hardening ability. This process achieves a balance between matrix softening and interface embrittlement, yielding favorable comprehensive formability of the material, which can provide an experimental basis for the actual annealing process of rolling Al/Mg/Al composite plates.

Author Contributions

Methodology, X.D.; validation, X.D.; formal analysis, B.F.; investigation, Y.H.; resources, Z.G., Z.W. and H.L.; data curation, Y.H., Z.G., Z.W. and H.L.; writing—original draft preparation, Y.H.; writing—review and editing, X.D. and B.F. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Data Availability Statement

The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding author.

Conflicts of Interest

Authors Zhuowu Guo, Zhiyong Wang, and Huanxin Liu were employed by the company “Shanxi Yinguang Huasheng Magnesium Co., Ltd”. The remaining authors declare that the research was conducted in the absence of any commercial or financial relationships that could be construed as a potential conflict of interest.

References

  1. Yang, Y.; Xiong, X.; Chen, J.; Peng, X.; Chen, D.; Pan, F. Research advances of magnesium and magnesium alloys worldwide in 2022. J. Magnes. Alloys 2023, 11, 2611–2654. [Google Scholar] [CrossRef] [Scilit]
  2. Azadehranjbar, S.; Wei, B.; Xie, D.; Ming, K.; Wang, J.; Shield, J.E. Strength and plasticity of lamellar vs. fibrous eutectic Mg-Al nanocomposites: An in-situ microcompression study. Acta Mater. 2021, 206, 116624. [Google Scholar] [CrossRef] [Scilit]
  3. Mordike, B.; Ebert, T. Magnesium: Properties—Applications—Potential. Mater. Sci. Eng. A 2001, 302, 37–45. [Google Scholar] [CrossRef] [Scilit]
  4. Cai, B.; Fan, J.; Shi, R.; Gao, P.; Yang, D.; Wang, L.; Peng, Y.; Wang, K. Recent progress and perspectives in additive manufacturing of magnesium alloys and composites: A review. J. Magnes. Alloys 2025, 13, 5267–5312. [Google Scholar] [CrossRef] [Scilit]
  5. Kurzynowski, T.; Pawlak, A.; Smolina, I. The potential of SLM technology for processing magnesium alloys in aerospace industry. Arch. Civ. Mech. Eng. 2020, 20, 23. [Google Scholar] [CrossRef] [Scilit]
  6. Mihara-Narita, M.; Chino, Y.; Bian, M.; Sato, H.; Watanabe, Y. Effects of post-welded hot rolling on the properties of explosively welded Mg alloy/Al alloy cladding plates. J. Mater. Res. Technol. 2025, 37, 4457–4465. [Google Scholar] [CrossRef] [Scilit]
  7. Zhang, Z.; Zhang, J.; Wang, W.; Liu, S.; Sun, B.; Xie, J.; Xiao, T. Unveiling the deformation mechanism of highly deformable magnesium alloy with heterogeneous grains. Scr. Mater. 2022, 221, 114963. [Google Scholar] [CrossRef] [Scilit]
  8. Liu, C.; Wang, Q.; Jia, Y.; Jing, R.; Zhang, B.; Ma, M.; Liu, R. Microstructures and mechanical properties of Mg/Mg and Mg/Al/Mg laminated composites prepared via warm roll bonding. Mater. Sci. Eng. A 2012, 556, 1–8. [Google Scholar] [CrossRef] [Scilit]
  9. Wang, H.W.; Wang, C.J.; Deng, K.K.; Nie, K.B.; Liang, W. Microstructure and mechanical properties of Al/Mg/Al composite sheets containing trapezoidal shaped intermediate layer. Mater. Sci. Eng. A 2021, 811, 140989. [Google Scholar] [CrossRef] [Scilit]
  10. Tang, J.; Chen, L.; Zhao, G.; Zhang, C.; Sun, L. Achieving three-layered Al/Mg/Al sheet via combining porthole die co-extrusion and hot forging. J. Magnes. Alloys 2020, 8, 654–666. [Google Scholar] [CrossRef] [Scilit]
  11. Chen, Z.; Wang, D.; Cao, X.; Yang, W.; Wang, W. Influence of multi-pass rolling and subsequent annealing on the interface microstructure and mechanical properties of the explosive welding Mg/Al composite plates. Mater. Sci. Eng. A 2018, 723, 97–108. [Google Scholar] [CrossRef] [Scilit]
  12. Wu, K.; Chang, H.; Maawad, E.; Gan, W.; Brokmeier, H.; Zheng, M. Microstructure and mechanical properties of the Mg/Al laminated composite fabricated by accumulative roll bonding (ARB). Mater. Sci. Eng. A 2010, 527, 3073–3078. [Google Scholar] [CrossRef] [Scilit]
  13. Liu, N.; Chen, L.; Fu, Y.; Zhang, Y.; Tan, T.; Yin, F.; Liang, C. Interfacial characteristic of multi-pass caliber-rolled Mg/Al compound castings. J. Mater. Process. Technol. 2019, 267, 196–204. [Google Scholar] [CrossRef] [Scilit]
  14. Jia, H.Y.; Jiang, S.Y.; Han, J.C.; Cao, S.Z.; Wang, T.; Huang, Q.X. Dual increases in plasticity and strength of AZ31B/5052 clad plates subjected to one-pass hot rolling based on microstructural evolution. Mater. Sci. Eng. A 2023, 870, 144903. [Google Scholar] [CrossRef] [Scilit]
  15. Lei, J.; Ma, L.; Cai, Z.; Jia, W.; Zhi, C.; Yuan, Y.; Pan, H.; Xie, H. Interfacial fracture characteristics of Mg/Al composite plates with different thickness ratios by asymmetrical rolling with differential temperature rolls. Mater. Sci. Eng. A 2023, 869, 144764. [Google Scholar] [CrossRef] [Scilit]
  16. Chang, H.; Zheng, M.; Xu, C.; Fan, G.; Brokmeier, H.; Wu, K. Microstructure and mechanical properties of the Mg/Al multilayer fabricated by accumulative roll bonding (ARB) at ambient temperature. Mater. Sci. Eng. A 2012, 543, 249–256. [Google Scholar] [CrossRef] [Scilit]
  17. Kim, J.S.; Lee, K.S.; Kwon, Y.N.; Lee, B.J.; Chang, Y.W.; Lee, S. Improvement of interfacial bonding strength in roll-bonded Mg/Al clad sheets through annealing and secondary rolling process. Mater. Sci. Eng. A 2015, 628, 1–10. [Google Scholar] [CrossRef] [Scilit]
  18. Macwan, A.; Jiang, X.Q.; Li, C.; Chen, D.L. Effect of annealing on interface microstructures and tensile properties of rolled Al/Mg/Al tri-layer clad sheets. Mater. Sci. Eng. A 2013, 587, 344–351. [Google Scholar] [CrossRef] [Scilit]
  19. Chaudhari, G.P.; Acoff, V. Cold roll bonding of multi-layered bi-metal laminate composites. Compos. Sci. Technol. 2009, 69, 1667–1675. [Google Scholar] [CrossRef] [Scilit]
  20. Zhu, C.C.; Sun, L.Q.; Gao, W.L.; Li, G.Y.; Cui, J.J. The effect of temperature on microstructure and mechanical properties of Al/Mg lap joints manufactured by magnetic pulse welding. J. Mater. Res. Technol. 2019, 8, 3270–3280. [Google Scholar] [CrossRef] [Scilit]
  21. Xu, J.J.; Fu, J.Y.; Li, S.J.; Xu, G.M.; Li, Y.; Wang, Z.D. Effect of annealing and cold rolling on interface microstructure and properties of Ti/Al/Cu clad sheet fabricated by horizontal twin-roll casting. J. Mater. Res. Technol. 2022, 16, 530–543. [Google Scholar] [CrossRef] [Scilit]
  22. Song, L.L.; Peng, X.Y.; Gao, H.T.; Wang, Z.Y.; Cui, H.J.; Foul, A.; Kong, C.; Yu, H.L. Investigation on the microstructural evolution and mechanical properties of Ti/Al/Ti clad sheets via cryorolling and annealing. Adv. Eng. Mater. 2025, 27, 2402211. [Google Scholar] [CrossRef] [Scilit]
  23. Bian, Q.; Liao, J.; Shi, J.; Liu, W.; Pan, H.; Cao, F. Study on the effect of electrolytic surface roughening of a stainless steel plate on the interfacial bonding strength of the stainless steel/aluminum clad plates by the cold roll bonding. Surf. Coat. Technol. 2025, 516, 132703. [Google Scholar] [CrossRef] [Scilit]
  24. Nie, H.H.; Liang, W.; Chen, H.S.; Zheng, L.; Chi, C.; Li, X. Effect of annealing on the microstructures and mechanical properties of Al/Mg/Al laminates. Mater. Sci. Eng. A 2018, 732, 6–13. [Google Scholar] [CrossRef] [Scilit]
  25. Zheng, H.; Yang, J.; Wu, R.; Wang, T.; Ma, X.; Hou, L.; Zhang, M.; Betsofen, S.; Krit, B. Influence of annealing temperature on the microstructure and mechanical properties of Al/Mg/Al composite sheets fabricated by roll bonding. Adv. Eng. Mater. 2016, 18, 1792–1798. [Google Scholar] [CrossRef] [Scilit]
  26. Li, Z.; Gu, H.; Luo, K.; Kong, C.; Yu, H. Achieving high strength and tensile ductility in pure nickel by cryorolling with subsequent low-temperature short-time annealing. Engineering 2024, 33, 190–203. [Google Scholar] [CrossRef] [Scilit]
  27. Zeng, M.; Yang, Y.; Tan, Y.; Zhang, W.; Xiang, S.; Ma, M.; Zhao, F. Recrystallization behavior and texture evolution of cryo-rolled GH159 superalloy with an ultra-high strength. Mater. Charact. 2023, 197, 112656. [Google Scholar] [CrossRef] [Scilit]
  28. Sahoo, B.K.; Srivastava, V.C.; Mahato, B.; Chowdhury, S.G. Microstructure-mechanical property evaluation and deformation mechanism in Al added medium Mn steel processed through intercritical rolling and annealing. Mater. Sci. Eng. A 2021, 799, 140100. [Google Scholar] [CrossRef] [Scilit]
  29. Li, Y.; Yang, D.; Yang, W.; Wu, Z.; Liu, C. Effect of annealing temperature on microstructure and properties of Al/Mg magnetic pulse welding joints. Materials 2022, 15, 5519. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  30. Lee, K.S.; Yoon, D.H.; Kim, H.K.; Kwon, Y.N.; Lee, Y.S. Effect of annealing on the interface microstructure and mechanical properties of a STS–Al–Mg 3-ply clad sheet. Mater. Sci. Eng. A 2012, 556, 319–330. [Google Scholar] [CrossRef] [Scilit]
  31. Li, S.; Li, G.Y.; Wang, H.; Gui, H.L.; Chu, Z.B.; Han, J.C.; Wang, T. Unraveling the link between annealing system and microstructure-mechanical properties of Mg/Al clad plate with corrugated interface. Surf. Interfaces 2025, 69, 106735. [Google Scholar] [CrossRef] [Scilit]
  32. Yin, G.M.; Feng, Z.Y.; Zhao, Z.L.; Cao, Y.-X.; Huang, X.-Z.; Li, L. Microstructure and creep properties of Al/Mg/Al composite clad plates. J. Cent. South Univ. 2023, 30, 2867–2877. [Google Scholar] [CrossRef] [Scilit]
  33. Zhu, Z.; Shi, R.; Klarner, A.D.; Luo, A.A.; Chen, Y. Predicting and controlling interfacial microstructure of magnesium/aluminum bimetallic structures for improved interfacial bonding. J. Magnes. Alloys 2020, 8, 578–586. [Google Scholar] [CrossRef] [Scilit]
  34. Sanamar, S.; Brokmeier, H.G.; Schell, N. Formation of the intermetallic phases Al12Mg17 and Al3Mg2 during heating of elemental Al-Mg composites studied by high-energy X-ray diffraction. J. Alloys Compd. 2022, 911, 165114. [Google Scholar] [CrossRef] [Scilit]
  35. Funamizu, Y.; Watanabe, K. Interdiffusion in the Al–Mg System. Trans. Jpn. Inst. Met. 1972, 13, 278–283. [Google Scholar] [CrossRef] [Scilit]
  36. Liu, T.; Song, B.; Huang, G.; Jiang, X.; Guo, S.; Zheng, K.; Pan, F. Preparation, structure and properties of Mg/Al laminated metal composites fabricated by roll-bonding, a review. J. Magnes. Alloys 2022, 10, 2062–2093. [Google Scholar] [CrossRef] [Scilit]
  37. Zhang, J.; Ma, L.F.; Cai, Z.H.; Zhao, G.; Jia, W.; Liu, P. Effect of annealing on the microstructure and mechanical anisotropy of Mg/Al composite plate. J. Magnes. Alloys 2024, 12, 5164–5178. [Google Scholar] [CrossRef] [Scilit]
  38. Song, K.; Liu, X.; Ji, Y.; Wei, Y.; Luo, J.; Liu, F.; Liu, D.; Zhong, Z. Intermetallic Compounds (IMCs) formation in Al/Mg dissimilar alloy solid state joining: Experimental study and phase field modeling. Met. Mater. Int. 2023, 29, 1165–1180. [Google Scholar] [CrossRef] [Scilit]
  39. Peng, P.; Jiang, S.; Jia, Y.; Han, C.; You, P.; Zhang, J.; Li, Y.; Lu, Z. Orientation and strain dependence of dislocations in aluminum layer of Al/Mg/Al laminates: High-resolution EBSD analysis. J. Alloys Compd. 2025, 1026, 180483. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.