Abstract
This study examines how pulsed-energy timing and spacing are associated with weld geometry, tensile response, and modelled thermal history in 2-mm-thick 4J50 butt joints. Four conditions were welded at a nominal average power of 227.5 W and compared with a three-dimensional transient thermal model. The A–B and C–D pairs hold nominal frequency and pulse duration fixed while changing travel speed; these changes also alter line energy and pulse spacing. Cases A and D share a nominal peak power of about 3.79 kW and a line energy of 22.75 J/mm, yet the measured penetration depth in D is 2.33 times that in A. Across the four calibration conditions, the mean absolute differences between the simulated segment means and the measured values were 0.050 mm for penetration depth and 0.064 mm for weld width. With one tensile specimen tested per condition, peak nominal stress followed the same rank order as measured penetration depth. These results highlight the coupled roles of pulse energy, duration, spacing, and off-time in weld formation.
1. Introduction
4J50 is an iron-nickel controlled-expansion precision alloy, which is a type of Invar alloy. Between 20 °C and °C, its average linear expansion coefficient is approximately °C−1. This value matches well with soft glasses and alumina ceramics [1,2]. After the sealed part is cooled down, the alloy and the glass shrink at almost the same rate, so the internal stress is small. The sealing can even reach a leak rate of [3]. Because of this special property, 4J50 is used in many places. For example, it is used for the lead wires and the housings of electron vacuum devices, such as traveling wave tubes, magnetrons, and vacuum capacitors [3]. Therefore, the welding quality directly determines the hermeticity, mechanical strength, and service life of the package.
Welding of 4J50 presents a specific thermal difficulty. The alloy has an abnormally low thermal conductivity for a metal, so laser energy deposited in a small volume dissipates slowly [4], thermal stress concentrates in the heated region, and hot cracking and distortion become the dominant failure modes [3,5,6,7,8]. Fusion welding of Invar-type alloys is nevertheless well established: TIG, laser, and electron-beam processes have all been applied [9], and process windows have been reported in which moderate heat input, high-purity argon shielding, and post-weld stress relief (for example, 750–800 °C slow cooling or 250–300 °C low-temperature ageing) suppress heat-affected-zone (HAZ) cracking and restore dimensional accuracy [3,9]. Among the fusion processes, laser welding offers the lowest and most localized heat input, and reduced residual stress and improved fatigue life have been reported for laser-welded Invar-type components [5,9]. The parameter sensitivity, however, is severe: small changes in process variables can compromise joint reliability, and a quantitative, mechanism-level understanding of how welding energy is deposited and redistributed is required for robust process design [10,11,12]. Pulsed laser welding is attractive for such precision joints because its energy input can be controlled at the level of individual milliseconds-scale pulses, giving a narrow HAZ and a controllable thermal cycle [13,14,15]. However, the same average power can be delivered by infinitely many combinations of pulse energy, pulse duration, repetition rate, and welding speed, and these combinations are not equivalent [16,17,18]. These observations point to one question: which feature of the pulse energy per pulse, irradiation duration, the interval between successive pulses, or the spatial offset between their footprints—actually controls the shape of the fusion zone? Average power and line energy, the customary process-descriptors, cannot distinguish between these features by construction [18].
Previous pulsed-laser studies show that weld geometry depends on pulse energy, pulse duration, repetition rate, and the time available for cooling. In Ni-base thin-sheet welding at fixed average heat input, Chai et al. reported changes in fusion-zone area and bead geometry with pulse duty ratio, together with changes in weld microstructure [16]. Invar studies have also examined how beam oscillation and heat accumulation relate to weld microstructure and mechanical response, while multiparameter pulsed-laser optimization studies have coupled process maps with melt-pool predictions and joint testing. These studies establish the sensitivity of weld formation to spatiotemporal energy delivery, but their materials, joint configurations, and process designs differ from the present autogenous 4J50 butt welds [3,15].
The contribution of this work is a four-condition comparison for 2-mm 4J50 butt joints at the same nominal average power, including a pair with the same line energy and nominal peak power but different pulse timing and spacing. Pulse-resolved thermal histories, historical temperature fields, and modelled melting-count distributions are examined alongside cross-sectional geometry and tensile response. This will give process theory support to the aerospace and electronic packaging fields, where high hermeticity and dimensional stability are needed. It also has academic value and engineering meaning for the development of the precision welding technology of controlled-expansion alloys.
2. Experimental
2.1. Materials
The material was annealed 4J50 alloy (Shanghai Dimmco Special Alloy Co., Ltd., Shanghai, China). Plates measuring 60 by 35 by 2 mm were joined as butt joints using a pulsed Nd:YAG laser (JK Lasers, Rugby, UK). Before welding, the plates were pickled ultrasonically in 5 percent HCl for 10 s and cleaned ultrasonically in ethanol for 10 min. A pronged fixture held the plate edges in tight butt contact, with no gap between them throughout the welding experiments. No filler metal was used.
2.2. Pulsed Laser Welding
The experiments were performed with a JK2003SM pulsed Nd:YAG laser. Pure argon was supplied through a nozzle at 20 L/min for shielding. The beam was delivered through an optical fibre and quartz lens to a five-axis laser workstation. A closed-circuit television system was used to monitor beam positioning over the joint. The plates remained tightly butted in the pronged fixture throughout welding, as shown in Figure 1. The welding parameters for cases A–D are listed in Table 1.
Figure 1.
Material characterization and schematic sketch of the experimental steps of pulsed laser welding: (a) material characterization and XRD testing; (b) Schematic sketch for the pulsed laser experiment.
Table 1.
The parameters used in the pulsed laser welding experiment.
The nominal average laser power was 227.5 W for all four conditions. Cases A and B share a frequency of 15 Hz and a duration of 4 ms, while cases C and D share 10 Hz and 6 ms. A–B and C–D therefore compare total changes within fixed nominal pulse families. Because changing speed also changes line energy and pulse spacing, these comparisons do not isolate a speed-only mechanism. Frequency and duration change together between the pulse families and cannot be evaluated as independent factors in this design.
2.3. Tensile Testing
Tensile specimens were prepared from the welded joints to the dimensions shown in Figure 2. The specimen had an overall length of 80 mm, a gauge length of 30 mm, a gauge width of 10 mm, a grip width of 15 mm, a grip-section length of 15.43 mm, and a transition radius of R20; the plate thickness was 2 mm. Specimen preparation and room-temperature tensile testing followed GB/T 2651-2008 [19] and GB/T 228.1-2010 [20], respectively. Tests were performed on a SANS universal testing machine with a capacity of 10 kN at a crosshead speed of 1 mm/min. One tensile specimen was tested for each of the four welding conditions.
Figure 2.
Dimensions of the tensile specimen used for the welded-joint tensile test.
The nominal tensile stress was calculated by dividing the recorded force by the nominal original gauge-section area of . The strain of each sample is the displacement recorded by the testing machine, divided by the nominal 30 mm gauge length and expressed as a percentage. The recorded displacement increased at approximately 1 mm/min during steady loading, consistent with the prescribed crosshead speed. The resulting values were apparent strain because the recorded displacement can include deformation of the load train and movement at the grips. Peak nominal stress is the maximum recorded force divided by the nominal area.
3. Finite Element Analysis of the Temperature Field in Pulsed Laser Welding of 4J50 Alloy
3.1. Geometry and Initial Condition
The three-dimensional half-domain was used to describe heat transfer during pulsed laser welding. The schematic representation of the heat transfer process during pulsed laser welding of the 4J50 alloy is depicted in Figure 3. Assuming symmetrical conditions for heat transfer with respect to the welding line, the representative volume element for the numerical analysis is a half-plate of length = 35 mm, width = 60 mm and thickness H = 2 mm. The half-plate is discretised with a graded hexahedral mesh with 0.08 mm spacing near the welding line and 0.05 mm spacing through the thickness. The in-plane element size of graded hexahedral mesh grows from = 0.08 mm at the symmetry plane to 1.50 mm at the far edge through four successive refinement zones (0.08/0.20/0.40/1.50 mm), while the through-thickness size is kept constant at = 0.050 mm over 40 layers.
Figure 3.
Computational domain and boundary conditions of the half-plate weld model.
The initial temperature of the 4J50 half-plate is assumed to be 293 K (single-phase fcc, solid). On the application of the incident pulsed laser beam of spot radius = 0.5 mm, the temperature of the medium starts to rise. The input heat flux to the workpiece is from the laser, whereas conduction is the only heat transfer mode retained inside the metal; radiative and convective losses to the environment are represented by a single Robin condition on the outer surfaces. The initial velocity of the solid workpiece is set as 0, and the alloy is treated as homogeneous. For the thermodynamic calculation, the measured composition (Table 2) was approximated by a binary Fe–Ni model with mass fractions of 50 wt.% for each element, neglecting the minor alloying elements. This approximation differs slightly from the measured 50.5 wt.% Ni. The resulting Ni mole fraction is , calculated using Equation (1):
with = 55.847 g mol−1 and = 58.69 g mol−1, giving a mean atomic mass of the alloy = 57.2332 g mol−1 that is used below to convert molar quantities into mass-specific ones.
Table 2.
Chemical composition of 4J50 Invar alloy (mass fraction, wt.%).
3.2. Theory and Calculation
The partial differential equation (PDE) for phase-change-based heat transfer in the computational domain of the 4J50 half-plate undergoing pulsed laser welding (Figure 3) is given as follows:
Here, T is temperature and t is time. The apparent heat capacity combines sensible heat capacity and the regularized latent-heat contribution around melting. The model solves heat transfer without an explicit liquid-velocity field; thus .
Marangoni-driven convection is not resolved as fluid flow. Its possible effect on lateral heat transport is represented approximately by the increased in-plane conductivity assigned to the liquid, while the through-thickness conductivity is unchanged. This reduced thermal closure does not predict flow direction, free-surface deformation, recoil pressure, or keyhole dynamics [4,21,22].
3.2.1. Heat Source Model of Pulsed Laser Welding
The volumetric heat source of the pulsed laser is expressed as the product of a radial distribution, an in-depth attenuation and a temporal gate:
where is the depth below the irradiated surface, is the radial distance from the instantaneous beam axis, is the position of the moving spot, the absorptance, the peak power and the effective absorption depth. A super–Gaussian radial profile with = 20 is used instead of the usual Gaussian ( = 2), because the measured beam of a fibre-delivered pulsed source has a flat top with a sharp edge [23]; Figure 4a compares the two radial distributions at the irradiated surface. The normalisation volume follows from the separation of variables, with = 2.78861 ( = for the classical Gaussian).
Figure 4.
Space–time structure of the volumetric heat source : (a) radial distribution at the irradiated surface, comparing the classical Gaussian with the super-Gaussian profile ( = 20) used here; (b) Laser pulse waveforms for cases A–D.
The measured weld profiles informed the selection of the effective heat-source attenuation length, which was set to 0.10 mm for A/B and 0.42 mm for C/D. These lengths describe the depth distribution prescribed by the heat-source model. The quantitative comparison in Section 4.1 uses the same four welding conditions and therefore assesses the calibration fit. Independent validation would require measurements excluded from source-parameter selection and predictions made with the calibrated parameters fixed.
The effective normalisation volume and the radial normalisation coefficient are given by Equation (5).
The temporal gate describes the pulse train, where f is the pulse repetition rate, the pulse duration and the duty cycle. For the four welding conditions considered here the duty cycle is identical, = 0.060, so that the pulse train differs between the cases only through the pulse spacing (Table 3). The laser pulse waveforms used in the pulsed laser welding experiments for Cases A–D are shown in Figure 4b.
Table 3.
Process parameters of the four welding conditions (experimental values, kept fixed throughout the calibration).
3.2.2. Boundary Conditions
The initial temperature of the 4J50 half-plate was set to 293 K. A zero normal heat flux was imposed on the symmetry plane. On the exposed surfaces, convection and radiation were included through the following nonlinear heat-flux boundary condition:
where is the outward unit normal, is the thermal conductivity tensor, and is the local surface temperature. The convective heat transfer coefficient was set to , and the ambient temperature was set to 293 K for both convection and radiation. Radiative heat loss was calculated using the Stefan–Boltzmann law, consistent with prior pulsed-laser welding simulations [24]. Elmer’s idealized radiation option was used. A constant surface emissivity of was assumed for the exposed 4J50 surfaces, following the pulsed-laser seam-welding model [25]. The Stefan–Boltzmann constant was . The laser energy was supplied separately as a moving volumetric heat source.
3.2.3. Calculation of Enthalpy
In order to obtain numerical values of the effective heat capacity material property in Equation (2), it is necessary to compute the thermodynamic property, that is, the temperature-dependent enthalpy of the 4J50 alloy for the solid, the liquid and the phase-transition period. Thermodynamically, the enthalpy of a phase is defined as Equation (8):
In the present work, all the terms appearing in Equation (8) are evaluated numerically with pycalphad, an open-source CALPHAD implementation [26]. A dedicated, compact binary Fe–Ni thermodynamic database was compiled for this work and is listed in Table 4.
Table 4.
Thermodynamic quantities of 4J50 obtained with pycalphad and the corresponding values adopted in the finite-element model.
The baseline Elmer model uses a regularised melting interval from to . These temperatures are numerical endpoints, rather than independently measured phase boundaries. Within this interval, the melting fraction is defined by Equations (9) and (10).
The baseline values are K, kg m−3 from the density curve, and kJ kg−1 from Table 4. The volumetric latent-heat increment is therefore J m−3. Sensible heat is supplied separately through the heat-capacity table. The value 7750 kg m−3 is the room-temperature density at 293 K, not the density at melting. The solver implementation and constitutive relation are described in the Elmer documentation [27].
3.2.4. Temperature-Dependent Density and Thermal Conductivity
The thermal conductivity of the alloy is implemented as an orthotropic tensor with = 41 W m−1 K−1 and N = 4.6, i.e., the in-plane conductivity of the liquid is increased by a factor 4.6 relative to the solid, while the through-thickness conductivity is unchanged (Figure 5a). The density is tabulated from 293 to 6000 K, decreasing linearly from 7750 kg m−3 at 293 K to 7300 kg m−3 at 6000 K. Interpolation gives a density of approximately 7638 kg per cubic metre at 1719 K; this is the value used for the volumetric latent-heat conversion.
Figure 5.
Temperature-dependent material properties of 4J50 as implemented in the finite-element model: (a) temperature-dependent anisotropic thermal conductivity; (b) specific heat and density.
4. Results
4.1. Weld Morphology and Cross-Sectional Geometry
Figure 6 compares the experimental cross-sections and the modelled thermal fusion envelopes for the conditions used to select the heat-source settings. The simulated fusion envelope comprises points where the maximum temperature over the saved history reached the numerical liquidus of 1725 K. It represents the region that reached this threshold at some time in that window. As shown in Table 5 and Figure 7, the experimental penetration ordering is C > D > A > B. The fusion zones of cases A and B are broad and shallow, whereas C and D penetrate more deeply. Case C has the greatest depth, 0.9994 mm, and a width of 1.630 mm. Case B has the smallest depth, 0.265 mm, and a width of 1.400 mm. The shape factor is .
Figure 6.
Experimental cross-sections (left) and numerical fusion envelopes (right) for the calibration conditions (a) A, (b) B, (c) C, and (d) D. In the numerical panels, the colours represent simulated temperature, increasing from blue to red. The yellow–green contour marks the adopted numerical liquidus boundary at 1725 K.
Table 5.
Experimental weld dimensions and geometrical descriptors. Penetration depths are the means of multiple measurements for each condition; the count of readings and their dispersion were not reported. Widths and visible fusion-zone areas were traced from the retained transverse sections.
Figure 7.
Experimental weld geometry: (a) penetration depth, (b) weld width, (c) weld shape factor , and (d) visible fusion-zone area.
For A/B, increasing speed from 600 to 900 mm/min changes the measured depth from 0.340 to 0.265 mm (22.1% lower) and width from 1.404 to 1.400 mm (0.3% lower). For C/D, changing speed from 600 to 300 mm/min changes depth from 0.793 to 0.9994 mm (26.0% higher) and width from 1.560 to 1.630 mm (4.5% higher). These are paired condition comparisons at fixed nominal pulse settings, not isolated speed effects: speed changes line energy and pulse spacing at the same time. Cases A and D share an average power of 227.5 W, a speed of 600 mm/min, and a line energy of 22.75 J/mm, yet the measured depth in D is 2.33 times that in A. The width in D is 11.1 percent larger. The A–D comparison changes frequency, duration, pulse energy, off-time, and pulse spacing together; it demonstrates that line energy alone is insufficient, but it does not identify an independent frequency or duration effect.
The penetration depth and weld width were extracted from transverse sections of the historical fusion envelope. The numerical width at the plate surface equalled the maximum transverse width at all sampled sections to the output precision. This common value was used for the width comparison. The differences between the experimental and simulated weld dimensions were shown in Table 6. Table 6 gives mean absolute differences across the four conditions of 0.050 mm for penetration depth and 0.064 mm for weld width. The largest relative depth difference was +21.2% in B. The largest absolute depth difference was 0.091 mm in C, where the measured depth exceeded the maximum in the sampled numerical segment. The largest width difference by magnitude was in D, where the numerical mean was 0.127 mm below the measured width, a difference of 8.1%. The measured widths fell within the corresponding sampled numerical ranges.
Table 6.
Comparison of measured and simulated penetration depth and weld width for the four calibration conditions. Numerical ranges give the minimum and maximum over each sampled weld segment.
4.2. Local Temperature Fields at Pulse Centers and Inter-Pulse Midpoints
To compare the local thermal responses during the pulsed laser welding, Figure 8 compares selected local temperature fields at two longitudinal positions: the center of a pulse footprint (Figure 8a–d) and the midpoint between adjacent pulse centers (Figure 8e–h). At the pulse-centre sections, cases A and B exhibit a hot region concentrated near the surface, whereas C and D develop a deeper high-temperature region despite less intense surface colours. This difference demonstrates that a higher local surface temperature does not necessarily correspond to greater penetration. Penetration depends on the temperature reached below the surface and on the duration and spatial extent of melting.
Figure 8.
Selected temperature cross sections at pulse-center positions for (a) A, (b) B, (c) C, and (d) D, and at inter-pulse midpoints for (e) A, (f) B, (g) C, and (h) D. The colours represent temperature in kelvin, as indicated by the colour bar. The green contour marks the adopted numerical liquidus isotherm at 1725 K.
4.3. Evolution of Historical High-Temperature Regions over Successive Pulses
For the analysis of the relation between penetration and the duration of melting during the pulsed laser welding. Figure 9 and Figure 10 show the historical maximum temperature after one, two, and three selected pulses, at the surface and at a depth of 0.2 mm, respectively. This temperature field records the highest temperature attained within the duration of three selected pulses for different cases.
Figure 9.
Surface historical maximum-temperature distributions after one (a1–d1), two (a2–d2), and three (a3–d3) selected pulses.
Figure 10.
Historical maximum-temperature distributions at 0.2 mm below the original surface after one (a1–d1), two (a2–d2), and three (a3–d3) selected pulses. The case order, pulse alignment, temperature scale, and historical liquidus criterion are the same as in Figure 9.
From Figure 9 and Figure 10, at the surface, the directly irradiated cores of cases A and B are hotter than those of cases C and D in the present model. As additional pulses are included, the neighboring high-temperature footprints interact. With the accumulation of successive pulses, the neighbouring footprints merge: case C develops the most extensive merged high-temperature region, the lobes of B and D remain more distinct, and A is intermediate. In Figure 10, the comparison changes at 0.2 mm below the surface. At this depth, cases C and D retain stronger high-temperature regions than cases A and B. Case C develops a broad connected historical region as the second and third pulses are included. Case D also produces pronounced subsurface heating, but cooler necks remain between its thermal lobes. The surface–subsurface contrast is consistent with the measured penetration ordering (C > D > A > B) and illustrates how the calibrated depth distribution of the heat source changes the relationship between surface and subsurface temperatures in this model.
4.4. Local Thermal Cycles and Instantaneous Molten-Region Evolution
Figure 11 presents the local thermal cycles at transverse offsets of 0, 0.5, and 1.0 mm from the weld centerline. Near the centerline, each case shows rapid heating during the reference pulse followed by cooling during the off-time. The reference-pulse peaks of cases A and B are higher than those of cases C and D, consistent with the selected near-surface temperature fields. Case C shows strong reheating before and after the reference pulse and retains a comparatively high temperature between the principal peaks. At the 0.5 mm offset, its neighboring excursions reach the adopted melting-temperature range, whereas those of the other cases are substantially weaker. At the 1.0 mm offset, the plotted cycles remain below the adopted melting range. The thermal response therefore changes from repeated melting near the central heated region to predominantly solid-state reheating farther from the weld centerline.
Figure 11.
Local thermal cycles at transverse offsets of 0, 0.5, and 1.0 mm, shown from top to bottom. The horizontal dashed lines indicate the lower and upper thresholds of the numerical melting interval. The vertical line at time zero marks the start of the reference pulse. The light-grey gridlines aid reading.
The instantaneous molten-region measures in Figure 12, cases C and D have markedly greater peak depth and volume than cases A and B, whereas the peak widths are more similar. Within the extracted region and the adopted molten-region criterion, the pool is therefore transient rather than continuously maintained until the next pulse. This observation is compatible with a connected historical fusion zone: a subsequent pulse can remelt previously heated and solidified material. It does not require the same material to remain fully liquid throughout the off-time.
Figure 12.
Instantaneous molten-region depth (a), width (b), and volume (c) as functions of normalized pulse phase.
4.5. Distribution of Repeated-Melting Counts
To characterize the melting behavior of the molten pool during pulsed laser welding, the number of melting events was counted within the weld-region domain for the different cases considered. Figure 13 shows the number of melting events identified in the selected saved-time windows. Cases A and B develop shallow counted regions, consistent with the limited penetration of individual pulses, whereas cases C and D reach markedly greater depths. In case C, the extensive two-melt region surrounding a central three-melt core indicates that each pulse substantially remelts the solidified footprint of its predecessor, while in case D the deep but separated lobes show that the pulses interact strongly within each footprint yet only weakly across neighboring ones. The surface melting-count maps and weld photographs are compared in Figure 14. Their periodic features are consistent with a seam assembled from successive pulse footprints. Such repeated remelting of previously solidified material is an inherent feature of pulsed laser seam welding: each pulse reheats and partially remelts a fraction of the preceding spot, and the extent of this interaction is conventionally described by the overlapping factor [28]. Previous studies have shown that increasing the overlap factor enlarges the remelted volume, which in turn affects defect escape, grain growth, and the uniformity of the fusion-zone microstructure [28,29,30].
Figure 13.
Sectional distributions of the melting count for (a) A, (b) B, (c) C, and (d) D over the saved analysis window. Blue, orange, and red denote one, two, and three melting events, respectively. Light grey denotes zero counted melting events.
Figure 14.
Surface melting-count distributions (left in each panel) and experimental weld-surface photographs (right in each panel) for (a) A, (b) B, (c) C, and (d) D. Light grey, blue, orange, and red denote zero, one, two, and three counted melting events, respectively.
4.6. Mechanical Properties of the Welded Joints
Figure 15 shows the measured tensile curve for the single specimen tested under each welding condition. Table 7 reports the individual peak values. Estimating within-condition variability and the sample standard deviation would require replicate tests. The peak nominal stress of the four specimens increases in the order B, A, D, C, which matches the order of increasing measured penetration depth.
Figure 15.
Measured tensile curves for cases A–D, with one specimen tested per condition. The horizontal coordinate is the recorded machine displacement divided by the 30 mm nominal gauge length. The inset shows the welded tensile specimens.
Table 7.
Tensile results for cases A–D, with one specimen tested per condition. Apparent strain is the recorded machine displacement divided by the 30 mm nominal gauge length.
5. Discussion
5.1. Weld Formation
The four conditions do not form a factorial design. For nominal rectangular pulses, pulse energy, peak power, pulse spacing, off-time, and line energy are calculated as follows:
Here, v is expressed in mm/s for the spacing and line-energy calculations. The duty fraction is 0.060 in every case, giving a nominal peak power of approximately 3.79 kW. The parameters and derived quantities are listed in Table 8.
Table 8.
Nominal rectangular-pulse parameters and derived quantities.
A–B compare the total effect of speed changing from 10 to 15 mm/s while frequency and duration remain 15 Hz and 4 ms; line energy decreases from 22.75 to 15.17 J/mm and spacing increases from 0.667 to 1.000 mm. C–D compare speed changing from 5 to 10 mm/s while frequency and duration remain 10 Hz and 6 ms; line energy decreases from 45.50 to 22.75 J/mm and spacing increases from 0.500 to 1.000 mm. Neither pair separates speed from the accompanying line-energy and spacing changes.
A and D have the same line energy and nominal peak power but differ in pulse timing and spatial delivery: D has 50 percent greater pulse energy, a 50 percent longer pulse duration, a longer off-time, and a larger center-to-center spacing. The measured depth differs by a factor of 2.33. This is evidence that equal global energy descriptors need not produce equal geometry, but the A–D pair cannot attribute that difference to frequency or duration separately.
Earlier work at fixed total heat input likewise reports changes in fusion area and bead geometry as pulse duty ratio changes, while Invar oscillation studies address spatial energy redistribution and heat accumulation. The present 4J50 results add a matched-line-energy comparison and pulse-resolved thermal post-processing, with the limitation that the four conditions do not isolate all process factors [3,15,16].
The relationships among the pulse waveforms, incident-fluence distributions, and weld-section geometry are summarized in Figure 16.
Figure 16.
Schematic diagram for the relationship among the nominal laser pulse waveforms (left column), prescribed incident-fluence distributions (middle column), and weld-section geometry (right column) for A–D, arranged from top to bottom. The waveform and weld-section colours identify A (red), B (blue), C (orange), and D (green). The surface colours in the middle column indicate incident fluence, increasing from blue to red.
Equal average power and nominal peak power do not guarantee equal weld geometry. The present comparisons show that pulse energy, duration, off-time, spacing, and line energy change in coupled ways and are associated with different penetration depths. The four-condition design does not establish an independent ranking of these factors or a universal process optimum. Optimization requires a controlled design that separates these variables and verifies weld stability and performance.
5.2. Tensile Response of Partially Penetrated Welds
All four joints showed partial penetration of the 2 mm plate. The measured penetration was 17.0% of the thickness for A, 13.25% for B, 49.97% for C, and 39.65% for D. During transverse tension, the force crosses the joint through the fused ligament. For a gauge width b and uniform penetration D, the nominal bonded area at the joint plane would be approximately . Nominal tensile stress uses the full original area for plate thickness t. A shallower fused ligament therefore carries the load through a smaller area. The unfused root can also act as a crack-like notch and concentrate stress under transverse tension [31]. Both effects can reduce the peak nominal stress of a partially penetrated joint.
This geometric interpretation is consistent with the observed ranking of peak nominal stress for the four specimens. Assessing the repeatability of this ranking requires tests of independently welded replicate specimens. Variation of penetration along the weld can change the area of the ligament crossing each specimen. The bonded area, fracture location, and fracture initiation site of each tensile specimen were unavailable, so the magnitude of the area effect and the role of root-initiated fracture remain unresolved.
6. Conclusions
The experimental weld geometry, tensile records, and available temperature-field results were combined to examine pulsed laser seam formation in 4J50 alloy. The following conclusions are drawn:
- For the four tested conditions, measured penetration ranged from 0.265 to 0.999 mm and width from 1.400 to 1.630 mm. Cases A and D shared nominal average power, nominal peak power, and line energy, while case D had 2.33 times the measured depth of A.
- With one specimen tested per condition, the rank order of peak nominal stress matched that of measured penetration depth. The four joints had partial penetration, with the fused depth spanning approximately 13–50% of the original plate thickness.
- The thermal model predicts stronger subsurface heating and larger fusion envelopes for C/D than A/B, alongside higher surface temperatures in A/B. This interpretation is conditional on the geometry-informed source-depth parameters and effective-conductivity closure.
- A connected historical fusion region can be produced by repeated melting of previously heated material and does not require a liquid bridge throughout the off-time. Successive pulses reheated and remelted earlier weld spots. Case C showed regions melted two or three times at 0.5 mm pulse spacing.
Author Contributions
Conceptualization, S.S., W.L. and Y.W.; Methodology, S.S., N.Z. and H.M.; Software, J.T.; Validation, J.T., X.H. and H.M.; Formal analysis, S.S., J.T. and L.S.; Investigation, J.T., N.Z., X.H. and L.S.; Resources, J.T. and X.H.; Data curation, N.Z. and L.S.; Writing—original draft, S.S.; Writing—review and editing, H.M., W.L. and Y.W.; Visualization, X.H. and L.S.; Supervision, W.L. and Y.W.; Project administration, H.M., W.L. and Y.W.; Funding acquisition, S.S. and N.Z. All authors have read and agreed to the published version of the manuscript.
Funding
This work was supported by the Guizhou Province Science and Technology Planning Project (Qianke He Jichu ZK [2023] Yiban 134), Guizhou Province Science and Technology Planning Project (Qianke He Zhicheng ZK [2024] Yiban182, Qianke He Pingtai JSZK [2025] 015), Major Science and Technology Special Project of Guizhou Province (Qiankehe Rencai XKBF [2025] 008).
Data Availability Statement
The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding authors.
Conflicts of Interest
Authors Jiaxin Tian, Xuedong He, Lei Shi, and Wenhai Lin were employed by Guizhou Zhenhua Qunying Electric Appliance Co., Ltd. The remaining authors declare that the research was conducted in the absence of any commercial or financial relationships that could be construed as a potential conflict of interest.
References
- Akgul, B.; Kul, M.; Erden, F. The puzzling thermal expansion behavior of invar alloys: A review on process-structure-property relationship. Crit. Rev. Solid State Mater. Sci. 2024, 49, 254–307. [Google Scholar] [CrossRef] [Scilit]
- Shiga, M. Invar alloys. Curr. Opin. Solid State Mater. Sci. 1996, 1, 340–348. [Google Scholar] [CrossRef] [Scilit]
- Zhao, J.; Wang, J.; Kang, X.; Wang, X.; Zhan, X. Effect of beam oscillation and oscillating frequency induced heat accumulation on microstructure and mechanical property in laser welding of Invar alloy. Opt. Laser Technol. 2023, 158, 108831. [Google Scholar] [CrossRef] [Scilit]
- DebRoy, T.; David, S.A. Physical processes in fusion welding. Rev. Mod. Phys. 1995, 67, 85–112. [Google Scholar] [CrossRef] [Scilit]
- Norrman, S.; Torstensson, P.A. Hermetic sealing of Kovar hybrid packages by laser welding. Hybrid Circuits 1985, 1, 21–23. [Google Scholar] [CrossRef] [Scilit]
- Guan, X.; Wang, L.; Hu, Z.; Ji, J.; Duan, Y.; Bu, H.; Tian, F.; Zhan, X. A new cracking criterion for additive manufacturing and repair of Ni-based superalloys via laser directed energy deposition. Acta Mater. 2026, 315, 122400. [Google Scholar] [CrossRef] [Scilit]
- Liu, Z.; Wang, J.; Xu, Z.; Li, Y.; Sun, Q.; Zhan, X. Unraveling microstructure evolution induced mechanical responses in coaxial fiber-diode laser hybrid welded Fe–36Ni Invar alloy. Mater. Sci. Eng. A 2024, 908, 146778. [Google Scholar] [CrossRef] [Scilit]
- Zhou, Y.; Cheng, L.; Li, Y.; Wang, J.; Zhan, X. Interfacial microstructure evolution and mechanical properties in laser welded Invar alloy/TC4 dissimilar joints. Intermetallics 2024, 166, 108171. [Google Scholar] [CrossRef] [Scilit]
- El-Batahgy, A.M.M.; Gumenyuk, A.; Gook, S.; Rethmeier, M. Comparison between GTA and laser beam welding of 9%Ni steel for critical cryogenic applications. J. Mater. Process. Technol. 2018, 261, 193–201. [Google Scholar] [CrossRef] [Scilit]
- Fu, J.; van Slingerland, J.; Brouwer, H.; Bliznuk, V.; Richardson, I.; Hermans, M. Applicability Study of Pulsed Laser Beam Welding on Ferritic–Martensitic ODS Eurofer Steel. Metals 2020, 10, 736. [Google Scholar] [CrossRef] [Scilit]
- Liu, J.; Nie, Y.; Feng, Q.; Liang, X.; Lei, H.; Niu, S.; Lou, M. Influence of Welding Speed on the Microstructure and Mechanical Properties of Laser-Welded Joints in 316L Stainless Steel Sheets. Metals 2025, 15, 624. [Google Scholar] [CrossRef] [Scilit]
- Bologna, O.; Cecchel, S.; Ferraresi, R.; Cornacchia, G. From Microstructure to Mechanical Performance: Characterization of Similar and Dissimilar Welds in Cast, Wrought, and LPBF Aluminum Alloys. Metals 2026, 16, 1046. [Google Scholar] [CrossRef] [Scilit]
- Chludzinski, M.; dos Santos, R.E.; Churiaque, C.; Ortega-Iguña, M.; Sánchez-Amaya, J.M. Pulsed Laser Welding Applied to Metallic Materials—A Material Approach. Metals 2021, 11, 640. [Google Scholar] [CrossRef] [Scilit]
- Lawrence, J.; Katayama, S. Understanding and Improving Process Control in Pulsed and Continuous Wave Laser Welding. In Advances in Laser Materials Processing, 2nd ed.; Woodhead Publishing/Elsevier: Cambridge, UK, 2018; pp. 153–183. [Google Scholar] [CrossRef] [Scilit]
- Tien, N.T.; Lo, Y.L.; Raza, M.M.; Chen, C.Y.; Chiu, C.P. Optimization of processing parameters for pulsed laser welding of dissimilar metal interconnects. Opt. Laser Technol. 2023, 159, 109022. [Google Scholar] [CrossRef] [Scilit]
- Chai, D.; Wu, D.; Ma, G.; Zhou, S.; Jin, Z.; Wu, D. The Effects of Pulse Parameters on Weld Geometry and Microstructure of a Pulsed Laser Welding Ni-Base Alloy Thin Sheet with Filler Wire. Metals 2016, 6, 237. [Google Scholar] [CrossRef] [Scilit]
- Kuo, T.Y.; Lin, Y.D. Effects of Different Shielding Gases and Power Waveforms on Penetration Characteristics and Porosity Formation in Laser Welding of Inconel 690 Alloy. Mater. Trans. 2007, 48, 219–226. [Google Scholar] [CrossRef] [Scilit]
- Suder, W.J.; Williams, S.W. Investigation of the effects of basic laser material interaction parameters in laser welding. J. Laser Appl. 2012, 24, 032009. [Google Scholar] [CrossRef] [Scilit]
- GB/T 2651-2008; Tensile Test Method on Welded Joints. China Standards Press: Beijing, China, 2008.
- GB/T 228.1-2010; Metallic Materials—Tensile Testing—Part 1: Method of Test at Room Temperature. China Standards Press: Beijing, China, 2010.
- Akbari, M.; Saedodin, S.; Toghraie, D.; Shoja-Razavi, R.; Kowsari, F. Experimental and numerical investigation of temperature distribution and melt pool geometry during pulsed laser welding of Ti6Al4V alloy. Opt. Laser Technol. 2014, 59, 52–59. [Google Scholar] [CrossRef] [Scilit]
- Bruyère, V.; Touvrey, C.; Namy, P.; Authier, N. Multiphysics modeling of pulsed laser welding. J. Laser Appl. 2017, 29, 022403. [Google Scholar] [CrossRef] [Scilit]
- Parent, A.; Morin, M.; Lavigne, P. Propagation of super-Gaussian field distributions. Opt. Quantum Electron. 1992, 24, 1071–1079. [Google Scholar] [CrossRef] [Scilit]
- Kholoud, M.J.; Akbari, M. Numerical investigation of molten pool dimension, temperature field and melting flow during pulsed laser welding of Ti-6Al-4V alloy sheets with different thicknesses. J. Laser Appl. 2021, 33, 032012. [Google Scholar] [CrossRef] [Scilit]
- Sabbaghzadeh, J.; Azizi, M.; Torkamany, M.J. Numerical and experimental investigation of seam welding with a pulsed laser. Opt. Laser Technol. 2008, 40, 289–296. [Google Scholar] [CrossRef] [Scilit]
- Otis, R.A.; Liu, Z.K. pycalphad: Open-source software for phase diagram material model construction and thermodynamic assessment. J. Open Res. Softw. 2017, 5, 1. [Google Scholar] [CrossRef] [Scilit]
- Ruokolainen, J.; Malinen, M.; Råback, P.; Zwinger, T.; Pursula, A.; Byckling, M. Elmer Finite Element Solver Tutorial. Technical report, CSC—IT Center for Science, Espoo, Finland, 2022. Elmer Open-Source Finite Element Software. Available online: https://www.elmerfem.org (accessed on 10 June 2026).
- Lu, H.; Zhang, X.; Zhao, P.; Bian, S. Effect of pulse overlap rate on the microstructure and mechanical properties of laser welds of thin AZ31 magnesium alloy. Mater. Res. Express 2022, 9, 116502. [Google Scholar] [CrossRef] [Scilit]
- Zhou, J.; Tsai, H.L. Transport Phenomena and Keyhole Dynamics During Pulsed Laser Welding. J. Heat Transf. 2006, 128, 680–690. [Google Scholar] [CrossRef] [Scilit]
- Wen, X.; Wu, D.; Zhang, P.; Liu, S.; Luo, Z.; Jia, Z.; Ye, X.; Shi, H.; Yu, Z. Influence mechanism of the keyhole behavior on penetration depth by in-situ monitoring in pulsed laser welding of aluminum alloy. Optik 2021, 246, 167812. [Google Scholar] [CrossRef] [Scilit]
- Matsuura, H.; Kaji, A. Evaluation of Tensile Strength of Partial Penetration Butt Welded Joints by Ultrasonic Testing. JSME Int. J. Ser. A Solid Mech. Mater. Eng. 2001, 44, 514–519. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.