Abstract
To address the problems of high residual stress, high cracking susceptibility, and deformation in argon arc repair welding of casting defects in WE43A rare-earth magnesium alloy aero-engine casing castings, a thermo-mechanical coupled finite element model considering the high-temperature properties of the material was established. A double ellipsoid heat source was used to simulate the heat input of argon arc welding, and the effects of the repair welding path, preheating before welding, post-weld heat treatment, and number of repair holes on the residual stress and deformation of repaired components were systematically investigated. The results show that the repair welding path significantly affects residual stress. The peak von Mises equivalent residual stress under a parallel repair welding path reaches 248 MPa, suggesting a relatively high potential cracking risk based on an empirical reference threshold. Under a circular repair welding path, the peak stress decreases to 199.4 MPa, effectively alleviating stress concentration. Increasing the preheating temperature can simultaneously reduce residual stress and welding warpage deformation. Compared with the 150 °C condition, preheating at 350 °C reduces warpage deformation by up to 45%. The residual stress release effect of post-weld heat treatment is enhanced with increasing temperature. Post-weld heat treatment at 450 °C for 1 h can reduce the peak residual stress by nearly half, but low- and medium-temperature post-weld heat treatments have a limited inhibiting effect on the macroscopic deformation of the component. Under the condition of side-hole repair welding on the curved surface of the casing, double-hole repair welding slightly reduces the peak stress and deformation compared with single-hole repair welding, but expands the stress influence range. This study provides a numerical theoretical reference for process optimization of low-stress, small-deformation argon-arc repair welding of WE43A magnesium-alloy casing castings, while it should be noted that mechanical-field outputs have not been independently validated by experimental measurements.
1. Introduction
Magnesium alloys represent an important class of lightweight alloys. Owing to their low density, high specific strength, and excellent damping capacity, they are widely used in aerospace, weaponry, new-energy vehicles, and other industrial sectors [1,2,3,4]. The WE43A magnesium alloy is extensively adopted for fabricating thin-walled aerospace castings with complex geometries [2,5]. However, its high rare-earth content leads to poor fluidity, which makes gravity-cast thin-walled components prone to casting defects such as porosity and shrinkage porosity [5]. In addition, WE43A has a wide solidification temperature range and large solidification shrinkage, increasing susceptibility to hot tearing during casting. Collectively, these drawbacks lead to a low casting yield for magnesium alloy castings. Compared with component remanufacturing, welding repair can substantially reduce material consumption and costs while maximizing the service life of components. Therefore, research on repair technologies for WE43A magnesium alloy carries important practical value.
Several works have focused on repair techniques for magnesium alloy castings. Gas tungsten arc welding (GTAW) is the dominant repair method [6,7,8], and cold metal transfer (CMT) welding is also adopted for such repair tasks [9,10]. However, welding repair introduces substantial residual stress [11,12,13,14,15,16,17], which raises the cracking risk in the repaired region and heat-affected zone (HAZ) and triggers casting distortion. Meng et al. [13] used laser remelting to optimize GTAW joints of AZ31B magnesium alloy, reporting a maximum measured residual stress of 136 MPa. Lobanov et al. [15,16] performed GTAW repair on ML10 magnesium alloy aero-engine casings and obtained a maximum residual stress of 120 MPa, a value comparable to the yield strength of the ML10 alloy. Zhou et al. conducted numerical simulations on GTAW of 2 mm-thick ZW61 magnesium alloy sheets, showing that residual stress is concentrated primarily within the fusion zone and HAZ; the peak longitudinal tensile residual stress was approximately 82 MPa and the peak transverse tensile residual stress reached 104 MPa [17]. Moreover, high tensile residual stress significantly degrades the fatigue performance of weld-repaired components [11,12,13,14,15,16,17,18]. Lobanov [16] applied electrodynamic treatment to AMg6 magnesium alloy welds, converting the initial ~120 MPa tensile residual stress into −75 MPa compressive residual stress and tripling the symmetric bending fatigue life.
Because residual stress generated by repair seriously threatens the fatigue performance and service safety of magnesium alloy castings, effective strategies to control and mitigate welding residual stress are highly desirable. Preheating [19,20,21] and post-weld heat treatment (PWHT) [21,22,23,24] are widely applied in engineering practice and research to reduce residual stress and thereby mitigate its detrimental effects. Chen et al. [19] numerically investigated the influence of preheating temperature on residual stress in laser-arc hybrid welded 5083/6063 dissimilar aluminum alloy joints. Their simulation results showed that HAZ residual stress drops rapidly with preheating temperatures of 100–200 °C; the HAZ residual stress on the 5083 side decreases by more than 30%, and the maximum stress reduction in the weld zone is nearly 40 MPa. Building on this work, Chen et al. [21] further investigated the effect of post-weld annealing on residual stress: annealing at 230 °C for 600 s reduces weld residual stress by 40%, offering a greater stress-reduction benefit than preheating. Goka et al. [23] subjected wire-arc additive-manufactured AZ31 magnesium alloy samples to heat treatment at 320 °C for 24 h and achieved nearly complete residual stress relief. Nevertheless, prolonged high-temperature heat treatment may induce abnormal grain growth in magnesium alloy welded joints and degrade mechanical properties. When TIG-repaired joints of sand-cast Mg-4Y-3RE-0.5Zr alloy underwent conventional T4 solution treatment at 520 °C for 8 h, abnormal grain coarsening occurred in the fusion zone, with grain sizes up to ~800 μm, and the joint elongation was only 1.8% [25].
This work targets WE43A magnesium alloy castings and establishes a coupled thermo-mechanical numerical model for their GTAW repair, aiming to avoid distortion, secondary cracking, repeated repair, and scrap risk induced by residual stress, and to guarantee the fatigue performance of repaired castings. Given the high tendency for stress concentration during GTAW repair of WE43A castings [26,27,28], the effectiveness of repair path planning, preheating, and post-weld heat treatment in reducing residual stress is systematically investigated, with the aim of developing a low-stress, low-distortion GTAW repair process for WE43A castings. Considering real engineering conditions where a single WE43A casting contains multiple shrinkage defects and cracks, sequential multi-spot welding and cooling may induce residual stress accumulation, severe stress concentration, and increased cracking risk, which is numerically investigated in this work.
2. Finite Element Simulation Model
2.1. Simulation of Repair Welding for Magnesium Alloy Plate Specimens
Figure 1a shows the flat simulated specimen for GTAW repair welding of magnesium alloy. Both the base material and repair filler wire are WE43A magnesium alloy, and their chemical compositions are listed in Table 1. The finite element model of this magnesium alloy flat specimen is established according to the diameter of the repair hole and weld width (Figure 1b). The dimensions of the plate are 50 mm × 50 mm × 10 mm, and the repair zone has a diameter of 30 mm. To reduce the computational cost, the specimen is partitioned into three regions: repair welding zone, transition zone, and base material zone. The brown area in Figure 1b represents the mesh of the repair welding zone, discretized with refined hexahedral elements of approximately 0.8 mm × 0.8 mm × 0.8 mm. The areas bounded by the two yellow circles are defined as the transition zone, with an element size of roughly 1 mm × 1 mm × 1 mm. A high temperature gradient develops within this zone during repair welding; therefore, high-quality hexahedral meshes are still employed here. The yellow meshes outside the yellow circles correspond to the base material zone far from the high-temperature molten pool, where relatively coarse hexahedral elements of 2 mm × 2 mm × 2 mm are adopted. The model is sectioned along the dashed line A–A in Figure 1b, and the resulting cross-section is presented in Figure 1c, in which the repair welding zone is filled by two welding layers.
Figure 1.
Repair welding of magnesium alloy equivalent specimen: (a) photograph of the equivalent specimen; (b) mesh model of the equivalent specimen; (c) mesh cross-section of the equivalent specimen.
Table 1.
Chemical composition of WE43A.
To investigate the effects of repair welding path, preheating temperature, and post-weld heat treatment temperature on the residual stress and deformation of magnesium alloy repaired components, three simulation cases were established, as shown in Figure 2. The model in Figure 2a takes the repair welding path as the variable and compares the influences of parallel and annular paths on the residual stress level of the magnesium alloy. The model in Figure 2b regards preheating temperature as the variable. The whole process involves three stages: preheating, repair welding, and cooling. Preheating temperatures of 150 °C, 250 °C, and 350 °C were adopted to explore the effectiveness of preheating in controlling residual stress and deformation. The model in Figure 2c targets post-weld heat treatment temperature as the variable. The entire process includes four stages: repair welding, cooling, heat treatment, and re-cooling. Post-weld heat treatment temperatures of 250 °C, 350 °C, and 450 °C were set to study the stress-relieving effect.
Figure 2.
Schematic diagrams of thermal cycle curves for magnesium alloy repair welding: (a) repair welding path; (b) preheating temperature; (c) post-weld heat treatment temperature.
Mesh convergence and time-step sensitivity analyses were not conducted in this work. Owing to the steep thermal and stress gradients in the fusion zone and HAZ, the reported peak stress values should be interpreted with caution. A systematic convergence study will be implemented in future work.
2.2. Simulation of Repair Welding for Magnesium Alloy Casing
Given the differences in thermophysical conditions and structural features between magnesium alloy castings and simulated flat plates, the residual stress distributions induced by GTAW repair welding vary correspondingly. To evaluate the deformation and cracking risk during repair welding of magnesium alloy castings, a side-hole repair welding model, as shown in Figure 3, was established based on the three-dimensional model of the magnesium alloy casing. According to the practical multi-site repair welding conditions of magnesium alloy castings, two comparative cases, i.e., single-side hole repair welding (Figure 3a) and double-side hole repair welding (Figure 3b), were developed to investigate the effect of residual stress accumulation induced by multi-site repair welding on the deformation and cracking risk of repaired components.
Figure 3.
Mesh generation for repair welding of the magnesium alloy casing: (a) single side-hole repair welding; (b) double side-hole repair welding; (c) enlarged view of the mesh in the repair welding hole region.
The mesh discretization of the repair zone for the side-hole repair welding is shown in Figure 3c. The brown region represents the mesh of the repair welding zone, discretized with refined hexahedral elements of approximately 0.8 mm × 0.8 mm × 0.8 mm. The blue region denotes the transition zone mesh with an element size of roughly 1 mm × 1 mm × 1 mm. A high temperature gradient develops within this zone during repair welding; therefore, high-quality hexahedral meshes are still employed here. The yellow meshes outside the yellow circles correspond to the base material of the casing, which is distant from the high-temperature molten pool. Relatively coarse tetrahedral meshes are adopted here.
2.3. Material Parameters and Boundary Conditions
Given that the thermophysical and mechanical properties of metal vary significantly with temperature during argon arc repair welding, it is unreasonable to define the material using constant average thermophysical and mechanical property parameters. Therefore, the temperature-dependent property relationships of WE43A shown in Figure 4 were incorporated into the model for calculation. In addition, Equation (1) was introduced to describe the plastic hardening behavior of WE43A magnesium alloy, where σ denotes the true stress, ε denotes the true strain, K is the strength coefficient, and n is the work-hardening exponent. Based on preliminary material tests, K is set to 580 MPa, and n is set to 0.14. Experiments reported by Wang L [29], Hu H [30], and others indicated that the ultimate tensile strength of as-cast WE43A alloy is approximately 200 MPa. In this work, a von Mises equivalent residual stress of 200 MPa is adopted as the empirical reference threshold for cracking risk in the simulation. It should be emphasized that, within the tensile residual stress field of repair welding, the elevated stress triaxiality means that cracking may occur in the casting even when the von Mises stress is below 200 MPa. It should be noted that this threshold is not a rigorous physical cracking criterion. Von Mises equivalent stress cannot directly quantify the susceptibility to tensile cracking, as tensile cracking is predominantly governed by the maximum principal tensile stress; cracking risk is also influenced by local plastic strain, microstructure, and service environment. In addition, in the PWHT simulation, only temperature-dependent rate-independent elastoplastic constitutive behavior is adopted. Creep, viscoplasticity, and time-dependent stress relaxation mechanisms are not included
σ = Kεn
Figure 4.
Material property parameters of WE43A magnesium alloy: (a) density and coefficient of thermal expansion; (b) thermal conductivity and specific heat capacity; (c) Young’s modulus and yield strength.
The initial temperature of the model is set to 20 °C. Only combined convective and radiative heat transfer between the workpiece and ambient air is considered, and an overall surface heat transfer coefficient of 60 W·m−2·K−1 is adopted. Other heat-loss mechanisms, including molten pool flow, chemical reactions, evaporative heat loss, and heat conduction through the workbench, are neglected in this coupled temperature–stress model. To reproduce the actual restraint conditions for repair welding of magnesium alloy castings, rigid displacement constraints are imposed in the x, y, and z directions. Specifically, constraints are applied to the four corner nodes on the bottom surface of the flat specimen, as well as four evenly distributed nodes on the bottom surface of the magnesium alloy casting.
In this paper, a double-ellipsoid heat source model is adopted to describe the argon arc heat source. The double-ellipsoid heat source is divided into front and rear parts by the heat source center, and these two parts are described by two quarter-ellipsoids, respectively. In the model, the energy in the x, y, and z directions attenuates in the form of Gaussian curves, as shown in Figure 5. The double-ellipsoid heat source can well represent the characteristic of a short head and a long tail of the molten pool and can also reflect the energy distribution of the heat source in the penetration depth direction. Different expressions are used for the front and rear parts of the double-ellipsoid heat source, respectively [31,32]:
where: P is the arc power (W); η is the thermal efficiency. Based on literature and preliminary computational experience, the thermal efficiency of the GTAW arc heat source is set to 77%. f1 and f2 are the energy distribution coefficients for the front and rear halves of the molten pool, which are taken as 0.6 and 0.4, respectively. To achieve a good agreement with the experimental results, the semi-axis parameters of the ellipsoidal heat source geometry a1, a2, b, and c are assigned values of 5 mm, 10 mm, 10 mm, and 3.5 mm.
Figure 5.
Schematic diagram of the double-ellipsoid heat source model.
All reported residual-stress data refer to von Mises equivalent stress, and deformation results correspond to the Z-direction displacement component. Both stress and displacement values are extracted after the model has fully cooled down to ambient temperature. Mechanical displacement constraints remain fixed throughout all simulation cases, and no constraint release is performed. The stress-influence range is defined as the spatial region where the von Mises equivalent residual stress exceeds 10 MPa. Sampling paths for curve extraction are marked in corresponding cloud-plot figures, from which coordinate information can be read.
2.4. Experimental Validation of Magnesium Alloy Repair Welding
To verify the accuracy of the coupled temperature–stress field model, GTAW repair welding experiments were performed on flat magnesium alloy simulated specimens. The WE43 filler wire with a diameter of 1.2 mm was adopted in this work. The experimental system included a Fronius welding power source, wire feeder, and a KUKA six-axis robotic arm. The repair welding parameters were set as follows: welding voltage of 17 V, base current of 60 A, peak current of 120 A, frequency of 4 Hz, welding speed of 200 mm/min, and wire feeding speed of 400 mm/min. Figure 1a shows the macroscopic morphology of the repaired specimen. After welding, cross-sectional samples of the repair-welded joint were cut by wire electrical discharge machining (WEDM). After grinding and polishing, optical microscopy was used to acquire metallographic images of the single-pass weld. The molten pool dimensions were measured from these metallographs using ImageJ software (ImageJ 1.54p) for comparison with simulated results.
It should be emphasized that the present experimental validation is limited to thermal field features via molten pool profile comparison. No independent experimental measurements of residual stress or welding deformation are available to validate the mechanical response of the thermo-mechanical model. This is an important limitation of the current numerical study. All stress and deformation results reported hereinafter are numerical predictions rather than experimentally verified quantities.
3. Results and Analysis
3.1. Verification of Temperature Field Accuracy for Magnesium Alloy Repair Welding
To validate the accuracy of the present GTAW repair welding model for magnesium alloy, a temperature-field simulation of single-pass GTAW cladding on magnesium alloy was performed. The simulated molten pool profile was compared with the cross-sectional morphology acquired from cladding experiments. Figure 6a shows the overall temperature field distribution of single-pass cladding, where the molten pool is roughly circular. The region within the yellow box marks the molten pool for sampling, and the magnified temperature field of this zone is displayed in Figure 6b. The simulated molten pool geometry agrees well with the experimental cross-sectional profile; this comparison only validates the thermal-field prediction of the present GTAW repair welding model via molten-pool geometry matching. Independent experimental measurements of residual stress and welding deformation are not available in the current work; therefore, the mechanical outputs (residual-stress and deformation fields) from the thermo-mechanical simulation remain without direct experimental validation. The simulated stress and deformation results should be interpreted as numerical predictions rather than quantitatively verified experimental values.
Figure 6.
Comparison and verification of the temperature field and weld seam formation for single-pass repair welding: (a) temperature field distribution of single-pass repair welding; (b) comparison and verification of the repair welding molten pool temperature field and weld seam formation.
3.2. Effect of GTAW Welding Path on Residual Stress in Magnesium Alloy Plate Specimens
The repair welding path is a critical process factor that controls the delivery of welding heat input and the distribution of post-weld residual stress, and it notably affects the forming quality and structural stability of welded joints. To reveal its underlying mechanism and optimize the repair welding procedure, simulation models with parallel and annular repair paths were developed in this work, and the regulatory effect of path geometry on residual stress was examined via comparative simulations. The two repair schemes use the same deposited filler volume and identical individual welding parameters. However, the total heat input differs between the two paths because of their different total welding lengths. Figure 7 presents the evolution of the welding temperature field for the two-layer, eight-pass weld adopting the parallel repair path. As multi-pass welding progresses, welding heat accumulates gradually, producing an evident thermal build-up in the base material around the repair zone. The temperature within the transition zone rises continuously with successive weld passes. Specifically, no preheating effect occurs during the first deposition pass, and the transition zone remains at the initial ambient temperature of 25 °C. By the fourth pass, accumulated heat raises the transition zone temperature to 130 °C. Upon completion of the eighth pass, the transition zone temperature exceeds 300 °C. Owing to the high thermal conductivity of magnesium alloy, heat dissipation pathways around the molten pool expand continuously during welding, which alleviates thermal accumulation. Accordingly, the peak molten pool temperature generally tends to decrease, and the molten pool size shrinks gradually. The peak molten pool temperatures for the eight passes are 700.8 °C, 700.4 °C, 713.9 °C, 656.1 °C, 673.0 °C, 672.3 °C, 656.7 °C and 664.6 °C, respectively.
Figure 7.
Temperature field distribution in parallel-path argon arc repair welding.
Figure 8 shows the contour plot of the post-weld residual stress field for the component under the parallel repair welding path, which illustrates the residual stress distribution pattern and concentration features produced by this welding route. As shown in the figure, the high-stress region formed after parallel-path repair is roughly circular, with pronounced stress concentration; an annular peak-stress band forms within the heat-affected zone near the transition zone. The maximum von Mises equivalent residual stress appears at the welding start position, reaching 248 MPa. This value exceeds the empirical reference threshold derived from the ultimate tensile strength of WE43A magnesium alloy, which indicates an elevated cracking risk when judged purely from the magnitude of residual stress. This finding, however, is not direct experimental evidence that cracks will definitely initiate. Accordingly, the parallel repair path is deemed undesirable from the residual-stress perspective.
Figure 8.
Stress field of parallel-path repair welding: (a) upper surface; (b) internal cross-section; (c) lower surface.
Further analysis of the stress-concentration mechanism reveals that the high stress concentrated in the heat-affected zone originates mainly from the thermal-input characteristics at the welding start. During the initial deposition of the parallel repair path, the arc heat source covers only a limited area, and the subsequent heat-affected zone receives little preheating and remains near the initial ambient temperature. Once the high-temperature molten pool forms and contacts the surrounding base material, an extremely steep instantaneous temperature gradient develops between the molten pool and the heat-affected zone, inducing severe non-uniform thermal expansion and contraction. Meanwhile, the surrounding base material imposes rigid restraint on the locally heated region, restricting free thermal expansion and cooling shrinkage. Under the combined action of thermal strain and mechanical constraint, plastic deformation and work hardening take place in the heat-affected zone, and the associated internal stress cannot be relieved by free deformation. Stress therefore accumulates to form high residual stress, rendering this zone a mechanically vulnerable location of the repaired component.
Figure 9 presents the contour plot of the welding temperature field for the two-layer, four-pass annular repair path, showing the evolution of molten pool temperature and morphology during this annular welding procedure. Compared with the parallel repair path, the welding sequence of the annular path produces distinctive thermal accumulation and preheating behaviors, which exert a notable influence on molten pool morphology and temperature variation. Throughout welding, the heat input from the first and third passes provides sufficient preheating for the regions to be deposited subsequently and improves local temperature uniformity in the component. By contrast, the second and fourth passes cover a relatively narrow zone; heat is confined within a small local region with restricted heat dissipation, leading to pronounced local thermal accumulation and a marked increase in molten pool size at these stages. The peak molten pool temperatures of the four passes show fluctuating trends. The peak values for Passes 1 to 4 are 777.5 °C, 753.4 °C, 689.8 °C, and 788.5 °C, respectively.
Figure 9.
Temperature field distribution in circular-path argon arc repair welding.
The residual stress field distribution characteristics of the magnesium alloy component corresponding to the circular repair welding path are shown in Figure 10. Its stress distribution pattern differs significantly from that of the parallel repair welding path, and the overall stress level is effectively improved. As can be seen from the stress contours, the maximum residual stress of the component is 199.4 MPa. The high-stress region is concentrated in the annular heat-affected zone approximately 3 mm outside the repair zone, corresponding to the yellow region in the figure, which is the stress-weak region of the entire repair-welded structure. Compared with the high-stress state of the heat-affected zone, the overall stress level in the repair welding zone is significantly lower, appearing as a light red distribution in the contour map, among which the residual stress at the center of the upper surface of the weld spot is only 90.4 MPa.
Figure 10.
Residual stress distribution in circular-path argon arc repair welding: (a) upper surface; (b) internal cross-section; (c) lower surface; (d) cross-section along line a–a; (e) cross-section along line b–b.
By comparing with the simulation results of the parallel repair welding path presented above, the maximum residual stress of the parallel path reaches 248 MPa, which is much higher than the peak stress of the annular repair welding path. The annular path achieves a substantial reduction in both the overall peak residual stress and the residual stress within the repair welding zone. It should be noted that tensile cracking susceptibility is mainly governed by maximum principal tensile stress, local plastic strain, metallurgical state, and pre-existing defects, rather than von Mises equivalent stress alone. In the current work, the maximum principal tensile stress data were not extracted in post-processing. Therefore, the von Mises stress is only used as a reference index. The annular repair path reduces the numerically predicted residual stress level and hence may reduce cracking susceptibility. The simulation results show that the annular repair welding path can effectively reduce the peak von Mises residual stress and optimize residual-stress distribution of magnesium alloy repair-welded components, which makes it a promising candidate process scheme based on numerical predictions. Nevertheless, without preheating and post-weld heat treatment, the residual-stress level under the annular-path repair still approaches the material tensile strength, which may degrade the service fatigue performance of the casting. Relying only on repair-path adjustment cannot fully satisfy engineering requirements for residual-stress mitigation.
3.3. Effect of Preheating Temperature on Residual Stress and Deformation of Magnesium Alloy Plate Specimens
To investigate the regulatory effect of preheating temperature on residual stress for annular-path repair welding of magnesium alloy, three preheating levels of 150 °C, 250 °C and 350 °C were adopted for simulation analysis in this work. The residual stress distributions of the component after repair welding under different preheating conditions are shown in Figure 11. As illustrated in the residual stress contour plots in Figure 11a–c, preheating temperature exerts a notable regulatory effect on the magnitude of residual stress within the repaired zone and heat-affected zone. Elevating the preheating temperature can effectively reduce welding residual stress and mitigate stress concentration. Under the preheating condition of 150 °C, the component exhibits a maximum residual stress peak of 188.46 MPa. When the preheating temperature increases to 250 °C, the peak residual stress decreases to 181.26 MPa. With a further rise to 350 °C, the peak stress falls to 171.18 MPa, demonstrating a continuous downward trend of peak stress with increasing preheating temperature.
Figure 11.
Effect of pre-weld preheating temperature on residual stress distribution in argon arc repair welding: (a) 150 °C; (b) 250 °C; (c) 350 °C; (d) residual stress distribution sampled along the dashed line.
For a more detailed examination of stress distribution characteristics, data were extracted along the midline on the top surface of the model. The sampling path is indicated by the yellow dashed line in Figure 11a, and the corresponding residual stress distribution profiles are plotted in Figure 11d. The curve data reveal that raising the preheating temperature produces a favorable modification of the overall stress field of the component. While the reduction in peak residual stress is moderate, the residual stress at the center of the repaired zone is substantially relieved and lowered. At the low preheating temperature of 150 °C, the average residual stress at the center of the repaired zone remains approximately 160 MPa. When the preheating temperature is increased to 250 °C and 350 °C, the average residual stress in this region fluctuates steadily around 135 MPa. This indicates that preheating effectively narrows the temperature differential during welding and alleviates heterogeneous thermal deformation, thereby substantially optimizing the stress distribution within the core repaired zone. In numerical predictions, preheating helps lower residual stress and thus may mitigate the susceptibility to stress-driven cracking for magnesium alloy components after repair welding.
Figure 12 shows the contour plots of welding deformation distribution for the component under the annular repair welding path at preheating temperatures of 150 °C, 250 °C, and 350 °C. As illustrated in Figure 12a–c, preheating temperature exerts a notable suppressing effect on welding warpage of the magnesium alloy repaired workpiece. The overall deformation of the component decreases progressively with increasing preheating temperature, and this trend agrees well with the downward trend of residual stress. At the preheating temperature of 150 °C, warpage of the repaired plate is the most pronounced, with a maximum displacement of 1.923 mm. When the preheating temperature rises to 250 °C, the maximum deformation displacement falls to 1.828 mm. At 350 °C, the maximum warpage displacement of the component is only 1.058 mm, representing a 45% reduction relative to the 150 °C preheating case and demonstrating a prominent effect on deformation suppression.
Figure 12.
Effect of pre-weld preheating temperature on deformation distribution in argon arc repair welding: (a) 150 °C; (b) 250 °C; (c) 350 °C; (d) deformation distribution sampled along the dashed line.
To further analyze the deformation discrepancy, deformation data were extracted along the yellow dashed midline on the top surface of the model, yielding the deformation distribution profiles shown in Figure 12d. The results reveal that both ends of the plate warp upward to varying degrees after repair welding. Elevating the preheating temperature can effectively mitigate the deformation originating from non-uniform contraction. Among the examined conditions, high-temperature preheating at 350 °C delivers the most pronounced reduction in component warpage and favorably improves the dimensional accuracy of the repaired part.
3.4. Effect of Post-Weld Heat Treatment Temperature on Residual Stress and Deformation of Magnesium Alloy Plate Specimens
Figure 13 presents the cloud maps of residual stress distribution in magnesium alloy repaired components under different post-weld heat treatment temperatures, which directly show how heat treatment temperature controls the release and redistribution of welding residual stress. Three working conditions of 250 °C, 350 °C, and 450 °C were set for comparative analysis in this study to systematically investigate the optimization effect of graded heat treatment temperature on the stress field of repaired structures. The simulation results indicate that the reduction of residual stress in magnesium alloy repaired welds shows obvious graded differences with post-weld heat treatment temperature. As the heat treatment temperature increases, the peak residual stress of the component gradually decreases step by step, and the stress release effect keeps improving.
Figure 13.
Effect of post-weld heat treatment temperature on stress distribution in magnesium alloy: (a) 250 °C; (b) 350 °C; (c) 450 °C; (d) residual stress distribution sampled along the dashed line.
At the heat treatment temperature of 250 °C, the maximum residual stress is 186.1 MPa. The stress reduction is very small compared with the untreated condition, which means low-temperature heat treatment has a limited effect on residual stress release. When the temperature rises to 350 °C, the peak stress drops to 175.9 MPa. The stress release effect starts to appear, and local stress concentration is slightly relieved. When the heat treatment temperature increases to 450 °C, the residual stress decreases greatly, and the peak stress is only 103.62 MPa, nearly half of that in the room-temperature control group, showing an extremely remarkable stress release effect. This is because the yield strength of the material drops rapidly within the temperature range of 300–400 °C. A higher post-weld heat treatment temperature can effectively increase the atomic activity of the magnesium alloy matrix, promote temperature-driven plastic redistribution in the welded zone, greatly release the residual stress accumulated during welding, and improve the uniformity of the overall stress distribution of the component in numerical predictions, which may lower the susceptibility to cracking-related failure of repaired components.
Figure 14 intuitively shows the distribution characteristics and numerical variation of welding deformation of magnesium alloy repaired components under different post-weld heat treatment temperatures. To systematically study the effect of post-weld heat treatment on the forming accuracy and deformation behavior of repaired components, three graded heat treatment conditions of 250 °C, 350 °C, and 450 °C were designed for comparative simulation tests, and the evolution trend of component deformation at different temperatures was analyzed. The results reveal that the regulation trend of post-weld heat treatment temperature on the deformation of magnesium alloy repaired components is obviously different from that of residual stress. Heat treatment in the low-temperature range has a weak improvement effect on welding deformation, and the overall deformation fluctuates slightly.
Figure 14.
Effect of post-weld heat treatment temperature on deformation distribution in magnesium alloy: (a) 250 °C; (b) 350 °C; (c) 450 °C; (d) deformation distribution sampled along the dashed line.
When low-temperature post-weld heat treatment at 250 °C is applied, the maximum deformation of the component slightly decreases to 1.828 mm. When the temperature rises to 350 °C, the deformation is further slightly reduced to 1.824 mm. It can be seen that low- and medium-temperature heat treatment can only slightly relieve the warpage deformation of the component, and the optimization effect is not significant. When the heat treatment temperature increases to 450 °C, the maximum deformation of the component drops markedly to 1.08 mm. Comprehensive data analysis shows that the differences in the maximum deformation values among the first three conditions are very small, and there is no obvious trend of sharp deformation reduction with increasing temperature. This indicates that compared with the preheating process, post-weld heat treatment has a limited inhibitory effect on the macroscopic welding deformation of magnesium alloy repaired components. Low- and medium-temperature heat treatment cannot effectively improve the forming deformation, while high-temperature heat treatment can further optimize the deformation state.
3.5. Effect of the Number of Repair-Welded Side Holes on Residual Stress and Deformation of Magnesium Alloy Casings
Figure 15 shows the cloud maps of the residual stress field distribution of a magnesium alloy casting with side-hole defects repaired by annular repair welding. These maps fully demonstrate the stress concentration locations, affected range, and distribution differences between the outer and inner stress fields of this curved side-hole repair structure. The simulation results show that the overall peak residual stress of the side-hole repaired component can reach 192.8 MPa, and obvious welding stress concentration is observed.
Figure 15.
Stress field distribution of single side-hole repair welding in magnesium alloy casing: (a) outer surface contour; (b) distribution along A–A; (c) distribution along B–B.
Figure 15a displays the stress field distribution on the outer side of the casting. The diameter of the region where residual stress exceeds 10 MPa reaches 245 mm. The high-stress area is mainly concentrated in the heat-affected zone of the repair weld. Meanwhile, an obvious stress rise appears at the arc-starting and arc-stopping positions of the repair weld because of discontinuous heat input and abrupt temperature gradient, making these positions the weak parts of the outer structure. Figure 15b and Figure 15c present the stress distribution on the A–A and B–B cross-sections, respectively. The cross-section results further prove that both the repair zone and heat-affected zone are under high stress. The stress field shows an overall conical distribution feature: the affected range is larger on the outer side and smaller on the inner side, which is highly consistent with the inherent conical geometry of the side-hole defect.
To further quantify the magnitude and distribution of residual stress in the side-hole repair structure and accurately compare the stress difference between the outer and inner surfaces, sampling paths were arranged along the A–A and B–B characteristic cross-sections. Data were extracted along the outer surface path a-a and inner surface path b-b to obtain residual stress distribution curves. The data indicate that the maximum residual stress on both the outer and inner surfaces is about 180 MPa. Clear stress plateaus exist on the stress curves, meaning a wide area works under high stress during service. For the outer surface path a-a, the maximum stress occurs in the heat-affected zone; the stress drops in the repair zone but rises again at the weld overlap position. In comparison, the inner surface path b-b shows a generally high stress level within the repair zone with more uniform stress distribution.
This distribution trend is obviously different from the results of the previous flat-plate repair welding model. The reason is that the side wall of the casting is a curved structure, which has different restraint conditions from the flat plate. The curved structure changes the restraint state of the substrate and the coordination mechanism of thermal deformation, and finally produces this unique differential residual stress distribution between the inner and outer sides of the repaired side-hole casting.
Figure 16 shows the overall deformation cloud maps of the magnesium alloy casting after side-hole repair welding, which directly reflect the deformation magnitude and distribution of the curved repaired structure. The simulation results indicate that the maximum welding deformation of the side-hole repaired component reaches 2.1 mm, and the overall deformation is considerable.
Figure 16.
Deformation distribution of single side-hole repair welding in magnesium alloy casing: (a) outer surface contour; (b) distribution along A–A; (c) distribution along B–B.
Figure 16a shows the deformation distribution on the outer side of the casting. Combined with the deformation cloud maps of the A–A and B–B cross-sections, it can be found that the welding deformation of the component is obviously concentrated in local regions. The deformation is mainly concentrated in the side-hole repair zone, while the deformation at the far end of the substrate is small.
To further quantify the deformation amplitude and distribution of the side-hole repair structure and accurately reveal the deformation difference between the inner and outer surfaces, sampling paths were set along the typical A–A and B–B cross-sections, and deformation data were extracted. The deformation distribution curves are shown in Figure 16b,c. The quantitative results show that the deformation peaks on both the inner and outer surfaces of the casting are located in the repair zone, and the deformation decreases sharply in the substrate regions far away from the weld bead. This deformation feature mainly comes from the localized concentrated heat input during repair welding, which induces uneven thermal contraction in the repair zone. Together with the inherent restraint characteristics of the curved casting, it finally forms a concentrated deformation distribution centered on the repair zone.
Figure 17 presents the overall cloud maps of the residual stress field of the magnesium alloy casting after double-hole repair welding, which systematically show the stress concentration level, affected range, and spatial distribution of the inner and outer surfaces and cross-sections under the symmetric double-hole repair welding process. It can provide direct evidence for studying the stress characteristics of multi-spot repair welded structures.
Figure 17.
Stress distribution of double side-hole repair welding in magnesium alloy casing: (a) outer surface contour; (b) distribution along A–A; (c) distribution along B–B; (d) distribution along C–C.
The simulation results show that the peak residual stress of the magnesium alloy casting under the double-hole repair welding process is 186.9 MPa. The peak stress is slightly lower than that of the single side-hole repair welding case, and the structural stress state is better. Figure 17a shows the stress field distribution on the outer side of the casting. The diameter of the region where residual stress exceeds 10 MPa expands to 455 mm, meaning a wider stress coverage area. The high-stress bands are mainly distributed in the heat-affected zones around the two weld beads, which are the main load-bearing and stress-concentrated regions on the outer side.
To further observe the spatial pattern of the stress field, sectional analysis was carried out along typical cross-sections A–A, B–B, and C–C. The corresponding cross-sectional stress cloud maps are shown in Figure 17b–d. The results demonstrate that both the repair zones and heat-affected zones remain at a high stress level. The stress field generally shows a conical spatial distribution: the diffusion range is larger on the outer side while the restrained range is smaller on the inner side. This distribution agrees well with the conical geometry and thickness restraint conditions of the side holes on the casting.
To quantitatively characterize the stress magnitude, distribution uniformity, and regional stress features of the double-hole repair welded structure, multiple sampling paths were arranged on the characteristic cross-sections A–A, B–B, and C–C, and residual stress distribution curves were obtained. The curve data indicate that a stable and continuous stress plateau is formed within the repair zones and heat-affected zones of the double-hole repair welded structure. The plateau stress stays at approximately 180 MPa without abrupt stress spikes.
Figure 18 shows the overall deformation distribution contours of the magnesium alloy side-hole component after double-weld-point repair welding, intuitively presenting the macroscopic deformation amplitude, the deformation differences between the inner and outer surfaces, and the cross-sectional deformation evolution laws of the double-hole repair-welded component. The simulation results show that the maximum deformation peak of the side-hole double-weld-point model after repair welding is 1.76 mm, which is slightly lower than that of the single-hole repair-welded component, indicating better overall forming accuracy. Figure 18a presents the overall deformation distribution morphology of the casting, from which the significant regional concentration characteristic of component deformation can be clearly observed. To further investigate the spatial distribution characteristics of internal deformation in the component, sectional analyses were carried out along three typical characteristic cross-sections, A–A, B–B, and C–C, and the cross-sectional deformation distributions are shown in Figure 18b–d. The cross-sectional contours further verify that the repair welding zone is the core deformation region of the entire component. Owing to the localized heat input during welding and the non-uniform thermal shrinkage, the deformation in this region is the most significant. To quantitatively analyze the deformation amplitude and distribution differences of the double-weld-point repair-welded structure and accurately compare the deformation laws of the inner and outer surfaces, sampling paths were set at cross-sections A–A, B–B, and C–C in this paper, and deformation data were extracted to obtain deformation distribution curves. The curve results show that there are obvious differences in the surface deformation degree at different positions of the component, among which the overall deformation along the outer surface a–a is significantly larger than that along the inner surface b–b. This phenomenon mainly originates from the fact that the repair welding heat source is concentrated on the outer side of the component. The outer side experiences a larger temperature gradient and weaker constraints on free deformation, while the inner base metal exerts a stronger constraint effect, effectively inhibiting shrinkage deformation. This ultimately forms a differentiated deformation distribution law of large deformation on the outer side and small deformation on the inner side.
Figure 18.
Deformation distribution of double side-hole repair welding in magnesium alloy casing: (a) outer surface contour; (b) distribution along A–A; (c) distribution along B–B; (d) distribution along C–C.
4. Conclusions
This study investigates the effects of repair welding path and preheating temperature on residual stress and deformation in argon arc repair welding of a simulated magnesium alloy casing. A thermal-stress field model was built for the argon arc repair process of WE43A magnesium alloy casing, and the main conclusions are as follows.
(1) The repair welding path significantly affects the von Mises equivalent residual-stress field of magnesium alloy argon-arc repair welds. According to numerical predictions, the parallel welding path produces a peak residual stress of ~248 MPa, exceeding the empirical reference threshold and implying high potential cracking risk from a residual-stress perspective. Annular welding lowers the peak stress below 200 MPa, showing an improved stress state in simulation and serving as a promising repair-process candidate.
(2) For residual stress, the peak value decreases by approximately 20 MPa when the preheating temperature rises from 150 °C to 350 °C. For warpage, the maximum displacement is reduced by around 45%. Preheating is therefore an effective strategy to mitigate welding-induced residual stress and suppress severe distortion of the GTAW-repaired WE43 alloy casting.
(3) Post-weld heat treatment is effective for reducing residual stress in magnesium alloy repair welds. Under the post-weld heat treatment condition of 450 °C for 1 h, the peak residual stress is nearly halved compared with the untreated case.
(4) The number of side repair holes has a minor influence on the peak residual stress. Double-hole repair shows slightly lower peak stress and deformation than single-hole repair. However, the affected range of residual stress becomes larger.
Author Contributions
Conceptualization, F.S., Z.Z., X.Z., L.Z., K.Z. and Y.H.; Methodology, F.S., Z.Z., X.Z., L.Z., K.Z. and Y.H.; Software, F.S., X.Z., L.Z., K.Z. and Y.H.; Validation, F.S., X.Z., L.Z., K.Z. and Y.H.; Formal analysis, X.Z., L.Z., K.Z. and Y.H.; Investigation, F.S., Z.Z., X.Z., L.Z., K.Z. and Y.H.; Resources, F.S., X.Z., L.Z., K.Z. and Y.H.; Data curation, F.S. and Z.Z.; Writing—original draft, F.S., Z.Z., X.Z., K.Z. and Y.H.; Writing—review & editing, F.S., Z.Z. and L.Z.; Visualization, Z.Z.; Supervision, X.Z., L.Z., K.Z. and Y.H.; Project administration, X.Z., L.Z., K.Z. and Y.H.; Funding acquisition, X.Z., L.Z., K.Z. and Y.H. All authors have read and agreed to the published version of the manuscript.
Funding
This research received no external funding.
Data Availability Statement
The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding author.
Conflicts of Interest
Author Faming Shen, Xin Zheng, Liyan Zhang, Kai Zhou and Yonghua Han were employed by the company AECC Harbin Dongan Engine Co., Ltd. The remaining authors declare that the research was conducted in the absence of any commercial or financial relationships that could be construed as a potential conflict of interest.
References
- Tong, X.; Wang, Q.; Wu, G.; Zou, W.; Zhang, L.; Wang, L.; Wang, Y.; Ding, W. Recent progress and perspectives in fusion welding of Mg-RE alloys: From weldability fundamentals to process-microstructure correlation. J. Magnes. Alloys 2025, 14, 101933. [Google Scholar] [CrossRef] [Scilit]
- Sharma, S.K.; Grewal, H.S.; Saxena, K.K.; Mohammed, K.A.; Prakash, C.; Davim, J.P.; Buddhi, D.; Raju, R.; Mohan, D.G.; Tomków, J. Advancements in the additive manufacturing of magnesium and aluminum alloys through laser-based approach. Materials 2022, 15, 8122. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Yang, J.; Zhu, Z.; Han, S.; Gu, Y.; Zhu, Z.; Zhang, H. Evolution, limitations, advantages, and future challenges of magnesium alloys as materials for aerospace applications. J. Alloys Compd. 2024, 1008, 176707. [Google Scholar] [CrossRef] [Scilit]
- Zhu, Z.; Ayoub, I.; He, J.; Yang, J.; Zhang, H.; Zhu, Z.; Hao, Q.; Cai, Z.; Ola, O.; Tiwari, S.K. Magnesium alloys with rare-earth elements: Research trends applications, and future prospect. J. Magnes. Alloys 2025, 13, 3524–3563. [Google Scholar] [CrossRef] [Scilit]
- Yang, L.X.; Huang, Y.D.; Hou, Z.Q.; Xiao, L.; Xu, Y.; Dong, X.; Li, F.; Kurz, G.; Sun, B.; Li, Z.; et al. Microstructure, Mechanical Properties and Fracture Behaviors of Large-Scale Sand-Cast Mg-3Y-2Gd-1Nd-0.4Zr Alloy. J. Magnes. Alloys 2023, 11, 2763–2775. [Google Scholar] [CrossRef] [Scilit]
- Chen, Z.; Dong, B.; Cai, X.; Chen, Q.; Fan, Y.; Lin, S. Microstructural Evolution and Hardness of As-Cast ZM6 Magnesium Alloy Welded by Ultrasonic-Frequency Pulsed TIG. Weld. World 2026, 1–16. [Google Scholar] [CrossRef] [Scilit]
- Li, C.; Cheng, B.; Xia, Y.; Lin, S.; Song, X.; Chen, Y. Microstructural Modification and Strengthening Mechanisms in a ZM6 Magnesium Alloy Joint Processed by Ultrasonic-Assisted TIG Welding with Pre-Weld Heat Treatment. Crystals 2026, 16, 646. [Google Scholar] [CrossRef] [Scilit]
- Shen, F.; Chen, Z.; Che, M.; Chang, Z.; Qiao, X.; Li, Y.; Li, G.; Zhao, M.; Xia, Y.; Lin, S. Microstructure and Mechanical Properties of ZM6 Cast Magnesium Alloy with Through-Hole Defects Repaired by Ultrasonic-Assisted TIG Welding. J. Cryst. 2026, 16, 182. [Google Scholar] [CrossRef] [Scilit]
- Cai, Z.; Shen, F.; Chen, Q.; Chen, Z.; Cui, Y.; Shao, T.; Dong, B.; Lin, S.; Cai, X. Effect of Cold Metal Transfer Welding Repair Parameters on the Forming for the Repair of Surface Defects of Cast Magnesium Alloy. Crystals 2024, 14, 679. [Google Scholar] [CrossRef] [Scilit]
- Chen, Q.; Chen, Z.; Dong, B.; Lin, S.; Fan, Y.; Cai, X.; Shen, F.; Wang, M.; Nie, L. Achieving Defect-Free Repair in ZM6 Magnesium Alloy through Cold Metal Transfer Welding Combined with Preheating. J. Mater. Res. Technol. 2026, 42, 189–209. [Google Scholar] [CrossRef] [Scilit]
- Sano, T.; Eimura, T.; Hirose, A.; Kawahito, Y.; Katayama, S.; Arakawa, K.; Masaki, K.; Shiro, A.; Shobu, T.; Sano, Y. Improving Fatigue Performance of Laser-Welded 2024-T3 Aluminum Alloy Using Dry Laser Peening. Metals 2019, 9, 1192. [Google Scholar] [CrossRef] [Scilit]
- Manjhi, S.K.; Bontha, S.; Balan, A.S.S. Enhancing Fatigue Performance of AZ31 Magnesium Alloy Components Fabricated by Cold Metal Transfer-Based Wire Arc Directed Energy Deposition through LPB. J. Magnes. Alloys 2024, 12, 1638–1662. [Google Scholar] [CrossRef] [Scilit]
- Meng, C.; Jiang, Y.H.; Yang, J.T.; Zhang, Z.; Qiu, X.; Wu, C.; Li, M.; Ren, X. The effect of combined laser bionic and ultrasonic impact on the microstructure and fatigue properties of AZ31B magnesium alloy TIG welded joints. Int. J. Fatigue 2023, 176, 107881. [Google Scholar] [CrossRef] [Scilit]
- Pan, X.; Zhou, L.; Wang, C.; Yu, K.; Zhu, Y.; Yi, M.; Wang, L.; Wen, S.; He, W.; Liang, X. Microstructure and Residual Stress Modulation of 7075 Aluminum Alloy for Improving Fatigue Performance by Laser Shock Peening. Int. J. Mach. Tools Manuf. 2023, 184, 103979. [Google Scholar] [CrossRef] [Scilit]
- Lobanov, L.; Pashchin, N. Electrodynamic Treatment by Electric Current Pulses as Effective Method of Control of Stress-Strain States and Improvement of Life of Welded Structures. Procedia Struct. Integr. 2019, 16, 27–34. [Google Scholar] [CrossRef] [Scilit]
- Lobanov, L.M.; Pashchin, N.A.; Mikhodui, O.L.; Khokhlova, J. Investigation of Residual Stresses in Welded Joints of Heat-Resistant Magnesium Alloy ML10 after Electrodynamic Treatment. J. Magnes. Alloys 2016, 4, 77–82. [Google Scholar] [CrossRef] [Scilit]
- Zhou, W.; Le, Q.; Shi, Y.; Liao, Q.; Yin, Z.; Jiang, Y. Numerical Simulation of Gas Tungsten Arc Welding for ZW61 Magnesium Alloy Thin Plates. Mater. Chem. Phys. 2025, 329, 130130. [Google Scholar] [CrossRef] [Scilit]
- Liu, B.; Zhang, H.; Li, S.; Luhovskyi, Y.; Nong, Z. A Review of Fatigue Performance Research on Aluminum Alloy Forming, Heat Treatment, Additive Manufacturing and Surface Modification Technologies. Crystals 2026, 16, 559. [Google Scholar] [CrossRef] [Scilit]
- Chen, X.; Tang, S.; Xie, W.; Zhang, M.; Song, H.; Ran, Q.; Zhang, D. Study on the Effect of Preheating Temperature on Residual Stress in Laser Arc Composite Welding of Dissimilar Aluminum Alloys. JOM 2024, 76, 3832–3839. [Google Scholar] [CrossRef] [Scilit]
- Liu, H.; Li, Z.; Li, W.; Zhang, W.; Wang, T.; Liu, W. Influence of arc preheating on stress and strain of additive manufactured components. J. Mater. Eng. Perform. 2023, 32, 6550–6563. [Google Scholar] [CrossRef] [Scilit]
- Chen, X.; Tang, S.; Xie, W.; Zhang, D. Numerical simulation study of laser-arc hybrid welding of 6063/5083 aluminum alloy. J. Mater. Eng. Perform. 2025, 34, 9342–9351. [Google Scholar] [CrossRef] [Scilit]
- Laleh, M.; Sadeghi, E.; Revilla, R.I.; Chao, Q.; Haghdadi, N.; Hughes, A.E.; Xu, W.; De Graeve, I.; Qian, M.; Gibson, I.; et al. Heat treatment for metal additive manufacturing. Prog. Mater. Sci. 2023, 133, 101051. [Google Scholar] [CrossRef] [Scilit]
- Goka, S.; M, M.; Davidson, M.J. Effects of Post-Weld Heat Treatments on the Microstructure and Residual Stresses of Wire Arc Additive Manufactured Magnesium Alloy. Mater. Werkst. 2025, 56, 1445–1454. [Google Scholar] [CrossRef] [Scilit]
- Azzeddine, H.; Khalfallah, A.; Yusof, F.; Baudin, T.; Brisset, F.; Barrallier, L.; Kawasaki, M. Microstructural and Residual Stress Evolution in an AZ31 Alloy through Friction Stir Welding and Post-weld Heat Treatment. J. Mater. Eng. Perform. 2026. [Google Scholar] [CrossRef] [Scilit]
- Zhang, G.; Tong, X.; Wu, G.; Zhang, L.; Sui, H.; Zhang, X. Research on the post-weld heat treatment of TIG repair welded joint of sand-cast Mg-Y-RE-Zr alloy. Mater. Sci. Eng. A 2021, 821, 141577. [Google Scholar] [CrossRef] [Scilit]
- Yi, J.; Zhang, J.; Cao, S.; Guo, P. Effect of welding sequence on residual stress and deformation of 6061-T6 aluminium alloy automobile component. Trans. Nonferrous Met. Soc. China 2019, 29, 287–295. [Google Scholar] [CrossRef] [Scilit]
- He, P.; Wu, Y.; Zhang, T.; Chen, S.; Zhang, C. Residual stresses in linear friction welding of TC17 titanium alloy considering phase fraction. Trans. Nonferrous Met. Soc. China 2024, 34, 184–193. [Google Scholar] [CrossRef] [Scilit]
- Charitidis, C.A.; Dragatogiannis, D.A.; Koumoulos, E.P.; Kartsonakis, I.A. Residual stress and deformation mechanism of friction stir welded aluminum alloys by nanoindentation. Mater. Sci. Eng. A 2012, 540, 226–234. [Google Scholar] [CrossRef] [Scilit]
- Wang, L.; Hu, J.; Guo, E.; Li, Y.; Kang, H.; Feng, Y. Microstructure and Mechanical Properties of Thick-Walled WE43A Alloy Fabricated by Wire Arc Additive Manufacturing. J. Mater. Eng. Perform. 2025, 34, 16133–16144. [Google Scholar] [CrossRef] [Scilit]
- Hu, H.; Wang, Z.; Guo, Z.; Wu, Y.; Zheng, H. Finite element analysis and experimental investigation of residual stress in WE43 magnesium alloy by Nd:YAG laser shock peening. J. Alloys Compd. 2025, 1038, 182791. [Google Scholar] [CrossRef] [Scilit]
- Xu, Y.; Zheng, P.; Liu, Z.; Zhang, Z.; Shi, L.; Zhang, H.; Du, L. An Integrated Experimental-Numerical Study on the Thermal History-Graded Microstructure and Properties in Laser-Clad Carburized Gear Steels. Coatings 2025, 15, 1467. [Google Scholar] [CrossRef] [Scilit]
- Goldak, J.; Chakravarti, A.; Bibby, M. A new finite element model for welding heat sources. Metall. Trans. B 1984, 15, 299–305. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.