Abstract
Polycarbonate (PC) waste is a valuable source of carbon and aromatic compounds, but conventional recycling methods are limited by material degradation and the low recovery of molecular building blocks. This study investigated the hydrothermal decomposition of PC in subcritical water, focusing on the effects of temperature and reaction time on phase distribution, product composition, and degradation kinetics. Experiments were performed in a high-pressure batch reactor at 250–350 °C, and the resulting solid, aqueous, diethyl ether (DEE)-soluble, and gas phases were characterized. Increasing temperature substantially accelerated PC decomposition, with near-complete conversion achieved at 300–325 °C within 15 min. BPA was the principal product under milder conditions, whereas increasing temperature and reaction time promoted its conversion to phenol and other alkylphenols. At higher reaction temperatures and longer reaction times, gas formation increased, indicating enhanced secondary cracking. A simplified lumped first-order kinetic model successfully described the principal concentration trends and showed increasing apparent rate coefficients for the major degradation pathways with temperature. The results demonstrate that subcritical water can effectively decompose PC and provide control over the distribution of recoverable products.
1. Introduction
The rapid increase in the production and consumption of plastic materials has created significant environmental and resource challenges. Among engineering plastics, polycarbonate (PC) holds an important position due to its excellent mechanical strength, optical transparency, thermal stability, and impact resistance [1]. These properties have enabled its widespread use in electronic devices, optical media, automotive components, construction materials, and consumer products [2]. Global demand for polycarbonate has continued to rise in recent decades, resulting in a corresponding increase in post-consumer PC waste. Polycarbonate is a condensation polymer synthesised primarily from bisphenol A (BPA) and phosgene or carbonate precursors [3]. Conventional disposal methods, such as landfilling and incineration, are increasingly restricted due to environmental concerns, the loss of valuable carbon resources, and the potential release of hazardous emissions. Consequently, the development of efficient and sustainable plastic recycling technologies has become a topic of growing scientific and industrial interest [4].
Mechanical recycling of polycarbonate is currently conducted on an industrial scale; however, it has inherent limitations, including polymer chain scission, contamination, discoloration, and deterioration of mechanical properties after multiple processing cycles [5]. These drawbacks have prompted the exploration of chemical recycling routes that enable recovery of the material at the molecular level.
Several strategies have been reported for the chemical recycling of polycarbonate, including solvolysis in alcohols and glycols, pyrolysis, and catalytic depolymerization [6,7,8]. Alcoholysis and glycolysis can achieve relatively high yields of BPA at moderate temperatures but require large amounts of organic solvent and often rely on homogeneous or heterogeneous catalysts, which complicates downstream separation and increases operating costs [7,9,10,11]. Pyrolysis, by contrast, is typically performed at high temperatures without solvents, leading to a broad distribution of aromatic and phenolic products. Although pyrolysis can process mixed plastic waste streams, it is energy-intensive and provides limited selectivity for valuable monomers such as BPA [12,13].
Hydrothermal decomposition involves treating polymeric materials in water at elevated temperatures and pressures, typically under subcritical or supercritical conditions [14]. Under these conditions, water exhibits unique physicochemical properties that differ markedly from those at room temperature. These changes enhance water’s ability to penetrate polymer matrices, dissolve organic compounds, and promote hydrolytic reactions without the need for additional organic solvents or catalysts [15]. Subcritical water provides a highly reactive medium that acts as both solvent and reactant. Recovering monomers from plastic waste reduces dependence on fossil-derived raw materials and mitigates the environmental impact associated with plastic disposal [16]. In addition, hydrothermal technologies are inherently compatible with wet and contaminated waste streams, reducing the need for extensive pretreatment [17]. This characteristic is particularly important for real-world plastic waste, which often contains additives, fillers, and impurities that complicate conventional recycling processes.
In recent years, increasing attention has been paid to elucidating the degradation pathways of polycarbonate in subcritical and supercritical water. Experimental studies have shown that temperature is a key parameter that strongly influences depolymerisation rates, product distribution, and phase yields. Numerous studies have shown that water plays a crucial dual role as both solvent and reactant, with negligible decomposition occurring below 230 °C, while rapid depolymerisation is observed above 240 °C and is significantly enhanced under supercritical conditions [18,19]. The primary mechanism involves hydrolytic cleavage of the polymer backbone to yield BPA as the dominant intermediate, which subsequently undergoes secondary cracking to form phenol and other alkylphenol components [18,20]. Product distributions are strongly dependent on reaction severity: lower temperatures (250–300 °C) favour high BPA yields (up to 90%), whereas higher temperatures promote further degradation into phenolic compounds [19,21]. Kinetic studies indicate that PC decomposition proceeds via an initial induction period followed by a rapid reaction stage, with models often approximated using lumped or fractional-order kinetics, highlighting the role of BPA as a key intermediate [22]. In addition, the use of catalysts such as alkali salts or ammonia has been shown to significantly accelerate hydrolysis and enhance monomer recovery [22,23].
This study examines the hydrothermal decomposition of polycarbonate plastic under subcritical water conditions. By systematically investigating the effects of temperature and reaction time on phase yield and product composition, this work aims to provide insight into the degradation behaviour of polycarbonate and the transformation pathways of its primary monomer BPA. The findings contribute to a more comprehensive understanding of hydrothermal recycling of polymers and support the development of efficient, environmentally friendly strategies for the chemical processing of polycarbonate waste.
2. Materials and Methods
2.1. Materials and Chemicals
Commercially available PC pellets (3 mm nominal granule size; melt flow index: 6.5 g/10 min; additives: heat stabilizer only—type undisclosed by manufacturer) supplied by Goodfellow (Hamburg, Germany) were used in this study. Bisphenol A, 4-isopropylphenol, and phenol were obtained from Merck (Darmstadt, Germany). Additional phenolic standards, 4-tert-pentylphenol, 4-tert-butylphenol, 4-ethylphenol, and 4-methylphenol, were supplied by Kefo (Ljubljana, Slovenia). Diethyl ether (DEE) was purchased from Sigma Aldrich (St. Louis, MO, USA). Helium (99.999%) and nitrogen (99.5%) were provided by Messer (Ruše, Slovenia).
2.2. Reaction Procedure and Product Recovery
Hydrothermal degradation experiments were conducted in a 75 mL high-pressure batch reactor (Parr Instruments GmbH, Frankfurt am Main, Germany)—shown in Figure 1 (generated by ChatGPT 5.6 Luna/OpenAI from an original 2D scheme)—using 5 g of sample and 25 mL of water, corresponding to a material-to-water ratio of 1 g/5 mL. The required amounts of material, deionised water, and a magnetic stir bar were placed in the reactor, which was then sealed and purged three times with nitrogen to establish an inert atmosphere. The initial pressure in the reactor was set so that, after heating, the pressure was 50 bar at 250 °C, 70 bar at 275 °C, 95 bar at 300 °C, 130 bar at 325 °C and 175 bar at 350 °C (10 bar above the saturation pressure of water at the given reaction temperature). The reactor was heated to the desired temperature at approximately 20 °C/min. The reaction time (t = 0 min) was defined as the moment when the target temperature was reached, and the predetermined reaction time was measured from this point onward. Thus, the heating period was excluded from the reported reaction time. After completion, the reactor was rapidly cooled by immersion in cold water. Once at room temperature, the gas phase was collected in sampling bags for subsequent analysis. The remaining reaction mixture was subjected to liquid–liquid extraction with DEE, followed by vacuum filtration to recover the solid fraction. Both the reactor and filter paper were thoroughly rinsed with DEE to minimise losses, and the rinse was added to the extract. The filter paper was dried overnight at 70 °C and weighed to determine the recovered solid phase. The DEE and aqueous phases were separated in a separatory funnel. DEE was removed from the DEE-soluble phase under vacuum using a rotary evaporator R-300 (Büchi Labortechnik AG, Flawil, Switzerland) to isolate the DEE-soluble fraction; the aqueous phase was evaporated similarly to obtain the water-soluble fraction.
Figure 1.
High-pressure high-temperature system. 1–gas tank, 2–inlet valve, 3–pressure indicator, 4–thermocouple, 5–batch reactor, 6–heating wire, 7–magnetic stir bar, 8–temperature controller, 9–electromagnetic mixer, 10–safety valve, 11–outlet valve (generated by ChatGPT 5.6 Luna/OpenAI from an original 2D scheme).
Phase yields were calculated using the following Equations (1)–(4):
where γ(DEE), γ(aq), γ(s) and γ(g) are the yields of the DEE-soluble, aqueous, solid and gas phases, respectively; m(DEE), m(aq) and m(s) are the weights of the DEE-soluble, aqueous and solid phases, respectively; and m(PC) is the weight of the PC introduced into the reactor. The γ(g) was estimated by difference, based on the recovered solid, aqueous and DEE-soluble fractions. Therefore, it represents an approximate value rather than a direct measurement of gas production. Potential uncertainties associated with material losses and incomplete recovery of the liquid and solid fractions may affect the accuracy of the estimated gas yield. All experiments were conducted in triplicate, and results are reported as mean values ± standard deviation.
γ(DEE) = m(DEE) ⁄ m(PC) × 100%
γ(aq) = m(aq) ⁄ m(PC) × 100%
γ(s) = m(s) ⁄ m(PC) × 100%
γ(g) = 100% − γ(DEE) − γ(aq) − γ(s)
2.3. Material and Product Analysis
The elemental analysis of the PC was performed using a Perkin Elmer 2400 Series II System Analyzer (Waltham, MA, USA) and the content of carbon, hydrogen, nitrogen and sulphur was determined. A Mettler Toledo TGA/DSC 1 STAR (Columbus, OH, USA) apparatus was used to determine the concentration of moisture, ash and volatile matter (proximate analysis) by a method previously described [24]. The ash content was calculated by adding these three values and subtracting the result from 100%. The thermal behavior of PC was examined by thermogravimetry (TGA) and differential scanning calorimetry (DSC) performed on the same apparatus. A small amount of PC (approx. 15 mg) was placed into the aluminum pans. The analyses were performed in a temperature range from 20 to 600 °C at a heating rate of 10 °C/ min in a nitrogen atmosphere and by simultaneous recording of TGA and DSC signals.
The DEE-soluble and gas phases were analysed using gas chromatography with flame ionisation detection (GC-FID) on a GC-2010 system (Shimadzu Corporation, Kyoto, Japan).
For DEE-soluble products, an HP-5MS (Agilent Technologies, Santa Carla, CA, USA) capillary column (30 m × 0.25 mm i.d., 25 µm film thickness) was used with helium as the carrier gas (1.2 mL/min). Samples were injected in split mode (1:20) at 250 °C. The oven programme was as follows: 50 °C for 5 min; ramp at 10 °C/min to 100 °C (hold for 1 min); ramp at 5 °C/min to 280 °C (hold for 5 min) [25]. The detector temperature was 300 °C. Quantification was performed using external calibration curves for BPA, 4-isopropylphenol (4-IPP), 4-tert-pentylphenol, 4-tert-butylphenol, 4-ethylphenol, p-cresol, and phenol. As a 4-isopropenylphenol (4-IPENP) standard was not commercially available, it was quantified using the calibration curve of 4-IPP, consistent with previous work [26]. The presence of 4-IPENP was confirmed by GC-MS QP 2010 Ultra system (Shimadzu Corporation, Kyoto, Japan). The identified compounds accounted for more than 75% of the relative peak area recorded by GC-FID. The mass fraction of the component was calculated according to Equation (5):
where w(c) is the mass fraction of the individual component, m(c) is the weight of the component, and m(PC) is the weight of the PC introduced into the reactor.
w(c) = m(c) ⁄ m(PC) × 100%
Gas-phase components were analysed using an HP-PLOT Q (Agilent Technologies, Santa Carla, CA, USA) column (30 m × 0.32 mm i.d., 20 µm film thickness) with helium as the carrier gas (0.87 mL/min). Samples were injected in split mode (1:100) at 250 °C. The oven programme was: 35 °C for 5 min; 10 °C/min to 80 °C (hold 1 min); 5 °C/min to 200 °C (hold 5 min) [27]. The FID was maintained at 250 °C. Identification was based on external standards, including CO2, methane, ethane, ethylene, propane, propylene, butane, 1-butene, pentane, 1-pentene, hexane, 1-hexene, and acetone. Results are presented as the percentage of the normalized relative peak area.
Total carbon (TC) content in the aqueous phase was measured using a TOC-L analyser (Shimadzu Corporation, Kyoto, Japan). TC concentrations were quantified using a calibration curve prepared from sodium hydrogen phthalate. Corrections were applied to account for the partial solubility of diethyl ether in water [24].
All analytical measurements were performed in triplicate, and results are reported as mean ± standard deviation.
The PC polymer and solid residues obtained after hydrothermal degradation were characterized using a Shimadzu IR-Affinity-1 FTIR spectrophotometer (Kyoto, Japan) equipped with an attenuated total reflectance (ATR) accessory. FTIR spectra were recorded over the wavenumber range of 4000–400 cm−1, using air as the background. Measurements were performed at a spectral resolution of 16 cm−1, with 20 scans accumulated for each spectrum to improve the signal-to-noise ratio. The acquired spectra were subsequently processed and evaluated using apparatus software.
3. Results and Discussion
3.1. Material Characterization
The results of the proximate and ultimate analyses of PC are presented in Table 1. Proximate analysis provides insight into the material’s composition and offers valuable information for understanding its thermal decomposition behavior. The high volatile matter content suggests a substantial potential for decomposition and the release of volatile products upon heating, whereas the relatively low ash content indicates a minor proportion of inorganic matter, which can form because of the possible presence of phosphite thermal stabilizers [28]. In addition, ultimate analysis provides information on the elemental composition of the material.
Table 1.
Ultimate, proximate, TGA and DSC analysis of PC.
The thermostability of PC was characterized by TGA/DSC. TGA, DTG and DSC curves are shown in Figure A1 in Appendix A. The detailed parameters used to evaluate the degradation are listed in Table 1. The onset degradation temperature (Tonset) is usually defined as the temperature at 5% weight loss in the TGA curve (Figure A1a) [29], the maximum degradation temperature (Tmax) and the corresponding maximum mass loss rate (Vmax) are obtained from the peak in the DTG curve (Figure A1a). A relatively broad range of Tonset (436–506 °C) and Tmax (504–549 °C) values has been reported for PC in the literature [29,30], and the results obtained in the present study are within these ranges. The DSC curve (Figure A1b) can be used to determine the glass transition temperature (Tg) of the material. Standard PC is an amorphous thermoplastic polymer; therefore, it does not exhibit a distinct melting point.
3.2. Yield of the Obtained Products
The distribution of product phases (Figure 2) clearly demonstrates the strong influence of reaction conditions on the hydrothermal decomposition of polycarbonate. The yield of the DEE-soluble phase may exceed the theoretical maximum mass yield of BPA due to the possible presence of carbon-containing intermediates and higher-molecular-weight oligomeric compounds in the organic phase, which cannot be detected using the GC-FID method applied in this study because of their limited volatility. Furthermore, water does not act solely as a reaction medium and catalyst during hydrothermal treatment but also participates as a reactant in hydrolysis and other chemical transformations, contributing to the formation of additional degradation products. At 250 °C, the decomposition process is limited, as shown by the high yield of the solid fraction (between 94.5 ± 1.9% and 59.7 ± 1.2%), which represents the undegraded polymer, and the relatively low yield of DEE-soluble products, even after 120 min. Increasing the temperature to 275 °C leads to faster decomposition, with nearly complete conversion of the solid phase and maximum yields of the DEE-soluble phase (95.6 ± 2.9%) achieved after 60 min. At temperatures of 300 and 325 °C, the decomposition process is rapid, reaching near-complete conversion after 15 min (γ(s) < 3.8 ± 0.1%); however, extended reaction times cause a gradual decrease in γ(DEE) and a corresponding increase in γ(g), indicating secondary cracking reactions. This trend is even more pronounced at 350 °C, where long reaction times (>30 min) promote gas formation (from 11.0 ± 0.3% after 30 min to 24.0 ± 0.6% after 120 min) and a decrease in γ(DEE) is observed (from 87.1 ± 2.6% after 30 min to 75.1 ± 2.3% after 120 min) [31]. The aqueous phase yield remains low (<1.2 ± 0.1%) under all conditions investigated, suggesting that almost all compounds are extracted into the DEE phase.
Figure 2.
Yield of DEE-soluble γ(DEE), water-soluble γ(aq), solid γ(s) and gas γ(g) phases after hydrothermal decomposition of PC.
3.3. DEE Phase Composition
Figure 3 shows that at 250 °C, BPA is the dominant product and increases over time, indicating that primary depolymerisation via carbonate bond cleavage is the main reaction pathway [32]. At 275 °C, BPA initially accumulates (reaching a maximum of 27.36 ± 0.82% at 60 min) but then declines, accompanied by a marked increase in the contents of 4-IPENP and phenol, demonstrating the onset of secondary transformations. This becomes even more evident at 300 °C, where the BPA content reaches a maximum of 36.27 ± 1.09% at a short residence time (15 min) and then decreases steadily to only 4.46 ± 0.13% after 120 min, while the amount of phenol continuously increases from 1.17 ± 0.02% (5 min) to 33.51 ± 0.67% (120 min). The intermediate species 4-IPENP and 4-IPP show transient behaviour, first accumulating and then converting further, consistent with their role as intermediates between BPA and phenol [33].
Figure 3.
Composition of DEE phase after hydrothermal decomposition of PC. BPA—bisphenol A, 4-IPENP—4-isopropenylphenol, 4-IPP—4-isopropylphenol.
At 325 and 350 °C, the BPA content rapidly drops even at short reaction times, and phenol becomes the dominant product, reaching its highest content at prolonged residence times (43.68 ± 0.87% at 350 °C and 120 min). Simultaneously, 4-IPP increases significantly at higher temperatures and longer times, indicating enhanced fragmentation and rearrangement reactions. The appearance of the “other” fraction, which includes detected p-cresol and 4-ethylphenol under the most severe conditions, further suggests the formation of minor secondary cracking products. One possible major product previously reported could also be acetone [34], which was detected in the gas phase in the present study. However, its presence in the DEE-soluble phase could not be confirmed using the GC-FID method applied in this study.
3.4. Gas Phase Distribution
The evolution of gas-phase distribution, presented as the percentage of the normalized relative peak area in Table 2, further supports the temperature-dependent shift from a depolymerisation-dominated process to extensive secondary cracking. As chromatographic signal for CO2 was detected, its relative abundance could not be reliably confirmed using the FID detector employed in this study, due to its relative insensitivity to CO2. CO2 formation during hydrothermal degradation of polycarbonate is possible, as decarboxylation reactions have been reported previously [31]. At 250 °C, the gas phase is dominated by hexane, indicating limited fragmentation and suggesting that minor side-chain cleavage is the main gas-forming pathway under mild conditions [35]. At 275 °C, acetone, pentane and hexane dominate the gas-phase composition. The substantial presence of acetone (up to 52.56%) indicates cleavage of isopropylidene linkages from BPA-derived intermediates [26]. The simultaneous formation of C5–C6 hydrocarbons suggests β-scission and side-chain cracking reactions [36]. This trend intensifies at 300 °C, where pentane and acetone are the principal gaseous products at short residence times, while prolonged reaction leads to the emergence of light olefins (ethylene, propylene) and methane, indicating progressive fragmentation. At 325 °C, and especially at 350 °C, a clear transition towards lighter hydrocarbons is observed. Methane content increases significantly with time (reaching 23.39% at 350 °C and 120 min), accompanied by rising fractions of ethylene, propylene, ethane and propane. Concurrently, the contents of heavier species such as hexane and pentane decline. The growing abundance of unsaturated hydrocarbons confirms secondary thermal fragmentation of phenolic intermediates and aromatic side chains [37].
Table 2.
Gas-phase composition after hydrothermal decomposition of PC (% of normalized peak area).
3.5. Total Carbon Content in Aqueous Phase
The total carbon (TC) content in the aqueous phase after hydrothermal degradation of PC at different temperatures and reaction times is presented in Figure 4. At the lowest investigated temperature, 250 °C, the TC concentration increased markedly with reaction time, from 1.256 ± 0.100 g/L at 60 min to a maximum of 5.132 ± 0.411 g/L at 120 min, indicating continuous formation of water-soluble organic compounds. A similar trend was observed at 275 °C, where the TC content increased from 1.741 ± 0.091 g/L at 15 min to 4.168 ± 0.217 g/L at 60 min, followed by a slight decrease to 3.472 ± 0.181 g/L at 120 min. At 300 °C, the TC concentration gradually increased with reaction time, reaching a maximum of 2.856 ± 0.171 g/L at 60 min before decreasing to 1.476 ± 0.089 g/L at 120 min. The highest TC concentration of all investigated conditions, 5.213 ± 0.250 g/L, was obtained at 325 °C after 30 min of reaction, while a comparable value of 4.916 ± 0.197 g/L was measured at 350 °C after 15 min. At both 325 and 350 °C, the TC content decreased rapidly with prolonged reaction time, reaching only 0.992 ± 0.048 and 0.692 ± 0.028 g/L, respectively, after 120 min. The initial increase in TC with increasing temperature and reaction time can be attributed to the formation of water-soluble degradation products during polycarbonate depolymerization [38]. However, under more severe reaction conditions, these compounds undergo further degradation into gaseous products and low-molecular-weight volatile compounds, resulting in a substantial decrease in the TC concentration of the aqueous phase. These observations are consistent with the increase in gas yield and the changes in the composition of the liquid products at higher temperatures and longer reaction times, indicating that secondary degradation reactions become dominant under severe hydrothermal conditions.
Figure 4.
TC content in aqueous phase after hydrothermal decomposition of PC.
3.6. FTIR of Solid Phase Residues
The FTIR spectra of the original PC granules (black lines) in Figure 5 show several characteristic absorption bands associated with the chemical structure of polycarbonate. The main absorption bands include C–H stretching vibrations at approximately 3000 cm−1, the C=O stretching vibration of the carbonate group at around 1770 cm−1, aromatic C=C stretching vibrations at approximately 1500 cm−1, and C–O–C stretching vibrations associated with the carbonate linkages in the 1250–1000 cm−1 region [29].
Figure 5.
FTIR spectra of solid phase after hydrothermal degradation of PC at different temperatures: (a) 250 and 275 °C, (b) 300 °C, (c) 325 °C and (d) 350 °C.
Figure 5 shows the FTIR spectra of the recovered solid residues after hydrothermal treatment at different temperatures and reaction times. At 250 °C, the characteristic absorption bands of PC remain clearly visible even after 60 and 120 min, indicating that a considerable proportion of the polymer structure is preserved under these conditions. At 275 °C, the intensity of the characteristic PC bands progressively decreases with increasing reaction time. A similar temperature- and time-dependent evolution is observed at 300 °C. After 5 and 15 min, the characteristic absorption bands of PC are still clearly identifiable, indicating the presence of undecomposed polymer. After 30 and 60 min, these bands become considerably less pronounced, and after 120 min, most of the characteristic PC absorption bands are no longer distinguishable. At 325 °C, the characteristic bands are still evident after 5 min but become progressively weaker with increasing reaction time, almost disappearing after 30 min. At 350 °C, the characteristic absorption bands of PC are already largely absent after 5 min, and no distinct PC-related bands are observed at longer reaction times. These results show good agreement with the yield of the solid phase γ(s) and demonstrate the strong influence of temperature on the degradation of the PC structure.
The changes observed in the FTIR spectra can be attributed to hydrolytic cleavage of carbonate linkages in the PC backbone under hydrothermal conditions. This process leads to the formation of lower-molecular-weight degradation products. The persistence of some PC-related absorption bands in the recovered solid residues, particularly at lower temperatures and shorter reaction times, suggests that degradation is incomplete and that polymer-derived fragments may remain in the solid phase, which can also be concluded from γ(s). Importantly, the recovered solid fraction does not necessarily consist exclusively of undegraded PC, as partially degraded oligomers or other polymer-derived products may also remain in this fraction depending on their solubility in the extraction solvent.
3.7. Decomposition Pathway and Kinetics
The reaction pathway presented in Figure 6 was proposed in which hydrothermal treatment initially promotes cleavage of the carbonate linkages in the PC backbone, producing BPA. This depolymerisation stage occurs predominantly in the early period of the reaction and represents the primary breakdown of the polymer structure. Because BPA is unstable under hydrothermal conditions [39], it acts as a transient intermediate rather than a final product. As the reaction temperature or residence time increases, BPA undergoes further decomposition, yielding phenol and several alkyl-substituted phenolic compounds. Among the detected intermediates, 4-IPENP appears to play an important role in the reaction sequence. Its formation before 4-IPP suggests that it is generated directly during BPA decomposition. The subsequent decrease in 4-IPENP concentration, accompanied by an increase in 4-IPP, is consistent with conversion of the unsaturated side chain into a saturated isopropyl group. Under more severe hydrothermal conditions, 4-IPP and related alkylphenols undergo further transformations, including dealkylation and side-chain cracking. These reactions contribute to the formation of phenol and smaller alkylphenols, such as p-cresol and 4-ethylphenol. The progressive accumulation of phenol indicates that it is both a major final product and a central intermediate within the degradation network. Its formation may occur through several parallel routes, including direct BPA decomposition and secondary degradation of 4-IPENP, 4-IPP, and other phenolic products.
Figure 6.
Proposed PC degradation pathway in subcritical water.
Based on the proposed hydrothermal degradation pathway of polycarbonate, a simplified lumped-parameter kinetic model was developed to evaluate the adequacy of the reaction network and to estimate the rate constants of the individual reaction steps. In the model, PC was expressed in terms of its repeating units, and the identified products were grouped into BPA, 4-IPENP, 4-IPP, phenol, other products obtained in the liquid phase (4-ethylphenol, p-cresol), and gaseous products. All concentrations used in the kinetic model were calculated based on the initial volume of water measured under ambient conditions. The proposed reaction network comprised the conversion of PC to BPA, the equimolar formation of 4-IPENF and phenol from BPA [34], the subsequent conversion of 4-IPENP to either phenol or 4-IPP, the conversion of 4-IPP to phenol or other products, the further degradation of the other products to phenol, and the conversion of phenol to gaseous products.
All reactions were assumed to be irreversible and first order [38] with respect to the corresponding component. The rate of an individual reaction can therefore be expressed as Equation (6):
where r is the rate of reaction, ki is the corresponding reaction rate constant, and cj is the concentration of the component participating in that reaction. Because water was present in large excess compared with the amount of organic material, its concentration was assumed to remain approximately constant throughout the reaction. Consequently, reactions were treated as pseudo-first-order reactions, and the water concentration was incorporated into an apparent rate constant. Therefore, the kinetic parameters determined in this study should be interpreted as apparent first-order constants under the applied hydrothermal conditions. The reaction network was intentionally simplified to describe the overall evolution of the experimentally identified species rather than individual elementary reaction mechanisms. The resulting system of differential equations (Equations (7)–(13)) can be expressed as follows:
r = ki × cj
dcPC/dt = −k1 × cPC
dcBPA/dt = k1 × cPC − k2 × cBPA
dc4-IPENP/dt = k2 × cBPA − k3 × c4-IPENP − k4 × c4-IPENP
dc4-IPP/dt = k4 × c4-IPENP − k5 × c4-IPP − k6 × c4-IPP
dcother/dt = k6 × c4-IPP − k7 × cother
dcphenol/dt = k2 × cBPA + k3 × c4-IPENP + k5 × c4-IPP + k7 × cother − k8 × cphenol
dcgas/dt = k8 × cphenol
Because the objective of the model was to provide a simple and practical description of the experimentally observed degradation behavior, explicit stoichiometric coefficients were not introduced as separate model parameters. Instead, the effective stoichiometric contributions of the individual pathways were incorporated into the fitted kinetic coefficients. Consequently, the fitted (ki) values should be interpreted as apparent lumped kinetic coefficients, rather than as elementary reaction rate constants. This approach reduced the number of adjustable parameters and avoided over-parameterization of the model while retaining the principal features of the experimentally observed reaction network. Because the extent of PC decomposition at 250 °C was relatively low and only two reaction times (60 and 120 min) were investigated, the available experimental data were considered insufficient for reliable kinetic parameter estimation. Therefore, an independent kinetic model was not developed for this temperature. The gas-phase concentration was calculated as a model-predicted value and is presented only as a predicted profile.
The kinetic parameters for the decomposition of PC at 275, 300, 325, 350 °C were estimated using a genetic algorithm by minimizing the sum of squared normalized residuals between the experimental and calculated concentrations using MATLAB R2024a (v24.1.0.2653294). The kinetic model parameters were fitted independently for each temperature investigated, without imposing an Arrhenius constraint during optimization. Subsequently, the temperature dependence of the estimated rate constants was evaluated using the Arrhenius equation to determine the corresponding activation energies. The heating period was not explicitly included in the kinetic model. The kinetic analysis was performed under the assumption that the reaction time started only after the reactor reached the target temperature. Consequently, the heating stage was not considered in the determination of kinetic parameters. We acknowledge that some degradation may occur during heating; however, this contribution was not investigated separately. Normalization by the experimental concentration range was applied to ensure that high-concentration species did not dominate the objective function and to provide comparable weighting among the different product groups. The resulting model provides a simplified phenomenological description of the hydrothermal degradation process. The resulting apparent kinetic coefficients are consequently specific to the investigated reaction conditions and the model formulation.
The estimated kinetic coefficients, with their activation energy (Ea), and the pre-exponential factor (A), according to the Arrhenius equation for the proposed reaction network, are presented in Table 3. In general, the values of most kinetic coefficients increased with reaction temperature, indicating an acceleration of the corresponding degradation and transformation pathways. The most pronounced temperature dependence was observed for k1 and k2, which correspond to the conversion of PC to BPA and the subsequent transformation of BPA, respectively. This marked increase with reaction temperature indicates that both the initial PC degradation and the subsequent BPA conversion are strongly promoted at higher temperatures.
Table 3.
Rate constants determined by the proposed kinetic model and calculated Arrhenius parameters.
The coefficient k3, associated with the conversion of 4-IPENP to phenol, also increased with temperature, although to a lesser extent. Similarly, k4, representing the conversion of 4-IPENP to 4-IPP, increased by more than one order of magnitude. This indicates that the pathway leading to 4-IPP becomes increasingly important at higher temperatures. In contrast, k5, corresponding to the conversion of 4-IPP to phenol, remained relatively small; this behaviour suggests that this pathway is relatively slow in the proposed reaction network.
The coefficients k6 and k7, associated with the formation and subsequent conversion of the coupled product “other”, were estimated to be zero at 275 and 300 °C. Small non-zero values were obtained at 325 °C, which increased further at 350 °C. This behaviour is consistent with the experimental observation that the formation of these products becomes more significant at higher temperatures. Finally, k8 represents the conversion of phenol to gaseous products. The significant increase in this coefficient indicates an increasing rate of secondary phenol transformation at elevated temperatures.
The calculated concentration profiles obtained using the proposed kinetic coupling model are compared with the experimental data in Figure 7. The model reproduces the general evolution of the main reaction products over the investigated temperature range, although the quality of the fit varies between individual components and reaction temperatures. At 275 °C, the limited extent of PC degradation results in a less satisfactory description of the PC concentration profile, especially at longer reaction times. At higher temperatures, the model generally captures the rapid disappearance of PC and the formation of the main degradation products more accurately. The largest deviations are observed for some intermediate and secondary products. This behaviour is expected for a simplified reaction coupling network, since the multiple parallel and sequential transformations occurring during hydrothermal degradation are represented by a limited number of apparent kinetic pathways. Despite these deviations, the model reproduces the main trends in the concentration profiles, including the rapid degradation of PC with increasing temperature, the transient formation of BPA and 4-IPENF, and the subsequent formation of phenolic products. The fitted kinetic coefficients further indicate that increasing the temperature generally accelerates the main degradation pathways. The quantitative goodness of fit, expressed as the coefficient of determination (R2), is summarised for each modelled component and temperature in Table A1 in Appendix A. The significant deviations between the experimental and model-predicted concentrations of the primary and secondary products can be attributed to the formation of unidentified degradation products. The R2 values demonstrate that the simplified lumped kinetic model adequately captures the principal trends in PC degradation and the formation of the major identified degradation products. The deviations observed for some components, particularly phenol at higher temperatures, highlight the limitations of representing the complex hydrothermal degradation network using a limited number of lumped first-order pathways. The model should therefore be considered a phenomenological representation of the overall degradation behavior.
Figure 7.
Experimental (symbols) and model-predicted (lines) concentration profiles of polycarbonate and its degradation products with time at temperatures of (a) 275 °C, (b) 300 °C, (c) 325 °C, and (d) 350 °C.
4. Conclusions
This study demonstrated the potential of subcritical water for the hydrothermal decomposition of polycarbonate and clarified the influence of temperature and reaction time on phase distribution and product evolution. At 250 °C, decomposition proceeded relatively slowly, whereas increasing the temperature to 275–325 °C substantially accelerated PC conversion. Near-complete disappearance of the solid PC fraction was achieved at 300 and 325 °C within 15 min. The highest DEE-soluble phase yield, 95.6 ± 2.9%, was obtained at 275 °C after 60 min.
BPA was identified as the principal product during the early stages of decomposition, confirming its role as a key intermediate in the degradation pathway. Increasing the reaction temperature and residence time promoted the subsequent transformation of BPA via 4-IPENP and 4-IPP, with phenol becoming the dominant identified product under more severe conditions. The increasing gas yield and formation of lighter hydrocarbons at elevated temperatures and prolonged reaction times further demonstrated that excessive reaction severity promotes secondary cracking. The aqueous phase remained comparatively small in terms of overall mass yield, although measurable total carbon concentrations indicated the formation of water-soluble degradation products.
The proposed lumped first-order kinetic model provided a useful phenomenological description of the main degradation trends between 275 and 350 °C. The fitted apparent kinetic coefficients generally increased with temperature, particularly for PC conversion and BPA transformation, confirming the strong temperature dependence of the principal reaction pathways. Although deviations were observed for some intermediate and secondary products, the model reproduced the major features of PC disappearance, transient BPA and 4-IPENP formation, and subsequent phenolic product generation.
The results indicate that subcritical water treatment offers an effective route for converting polycarbonate into recoverable aromatic products, with reaction temperature and residence time providing important means of controlling product distribution.
Author Contributions
M.I.: Conceptualization, Investigation, Formal analysis, Visualization, Data curation, Software, Writing—original draft. M.Č.: Conceptualization, Investigation, Formal analysis, Writing—review & editing. M.Š.: Conceptualization, Writing—review & editing, Supervision. All authors have read and agreed to the published version of the manuscript.
Funding
This work was supported by the Slovenian Research and Innovation Agency research program no. P2-0421, project no. GC-0007 and a young researcher fellowship awarded to M.I. The authors also acknowledge the funding within the project “Upgrading National Research Infrastructures—RIUM”, which was co-financed by the Republic of Slovenia; the Ministry of Higher Education, Science and Innovation; and the European Union from the European Regional Development Fund.
Data Availability Statement
The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding author.
Acknowledgments
Special thanks to the Laboratory for Separation Processes and Product Design, Faculty of Chemistry and Chemical Engineering, University of Maribor, for all the technical support. During the preparation of this work, the authors used [ChatGPT 5.6 Luna/OpenAI] to convert Figure 1 into a 3D image from an original 2D scheme and to assist with writing the MATLAB code. After using this tool/service, the authors reviewed and edited the content as needed and take full responsibility for the content of the published article.
Conflicts of Interest
The authors declare no conflicts of interest.
Abbreviations
The following abbreviations are used in this manuscript:
| 4-IPENP | 4-isopropenylphenol |
| 4-IPP | 4-isopropylphenol |
| BPA | Bisphenol A |
| DEE | Diethyl ether |
| PC | Polycarbonate |
| TC | Total carbon |
Appendix A
Table A1.
Coefficient of determination (R2) for proposed model for each component at different temperatures.
Figure A1.
TGA, DTG (a) and DSC (b) curves of PC.
References
- Antonakou, E.V.; Achilias, D.S. Recent Advances in Polycarbonate Recycling: A Review of Degradation Methods and Their Mechanisms. Waste Biomass Valorization 2013, 4, 9–21. [Google Scholar] [CrossRef] [Scilit]
- Yu, Z.; Jian, X.; Wang, J.; Zhang, X.; Zhai, S. Advantages and Research Progress of Polycarbonates in Flexible Electronic Devices. Macromol. Rapid Commun. 2025, e00705. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Le Grand, D.G.; Bendler, J.T. (Eds.) Handbook of Polycarbonate Science and Technology; Plastics Engineering; Marcel Dekker, Inc.: New York, NY, USA, 2000. [Google Scholar]
- Martínez-Narro, G.; Hassan, S.; Phan, A.N. Chemical Recycling of Plastic Waste for Sustainable Polymer Manufacturing—A Critical Review. J. Environ. Chem. Eng. 2024, 12, 112323. [Google Scholar] [CrossRef] [Scilit]
- Clark, R.A.; Shaver, M.P. Depolymerization within a Circular Plastics System. Chem. Rev. 2024, 124, 2617–2650. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Kim, J.G. Chemical Recycling of Poly(Bisphenol A Carbonate). Polym. Chem. 2020, 11, 4830–4849. [Google Scholar] [CrossRef] [Scilit]
- Markandeya, N.; Jadhav, M.; Gopale, P.; Ramalingam, K.; Kamble, S. Solvent-Assisted Chemical Recycling of Polycarbonate Using Glycerol as a Renewable Chemical: Mechanistic Insights and Statistical Optimization. Process Saf. Environ. Prot. 2026, 209, 108592. [Google Scholar] [CrossRef] [Scilit]
- Rigo, D.; Lamparelli, D.H.; Buonerba, A.; Capacchione, C.; Kleij, A.W. Depolymerization and Reuse of Polycarbonates: Emerging Classes, Mechanisms and Challenges. Angew. Chem. Int. Ed. 2026, 65, e00003. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Alavi Nikje, M.M.; Askarzadeh, M. Chemical Recycling of Polycarbonate Wastes into Bisphenol A by Using Green Solvent Composition. Polimery 2013, 58, 292–294. [Google Scholar] [CrossRef] [Scilit]
- Huang, J.; Huang, K.; Zhou, Q.; Chen, L.; Wu, Y.; Zhu, Z. Study on Depolymerization of Polycarbonate in Supercritical Ethanol. Polym. Degrad. Stab. 2006, 91, 2307–2314. [Google Scholar] [CrossRef] [Scilit]
- Quaranta, E.; Sgherza, D.; Tartaro, G. Depolymerization of Poly(Bisphenol A Carbonate) under Mild Conditions by Solvent-Free Alcoholysis Catalyzed by 1,8-Diazabicyclo[5.4.0]Undec-7-Ene as a Recyclable Organocatalyst: A Route to Chemical Recycling of Waste Polycarbonate. Green Chem. 2017, 19, 5422–5434. [Google Scholar] [CrossRef] [Scilit]
- Siddiqui, M.N.; Redhwi, H.H.; Antonakou, E.V.; Achilias, D.S. Pyrolysis Mechanism and Thermal Degradation Kinetics of Poly(Bisphenol A Carbonate)-Based Polymers Originating in Waste Electric and Electronic Equipment. J. Anal. Appl. Pyrolysis 2018, 132, 123–133. [Google Scholar] [CrossRef] [Scilit]
- Antonakou, E.V.; Kalogiannis, K.G.; Stefanidis, S.D.; Karakoulia, S.A.; Triantafyllidis, K.S.; Lappas, A.A.; Achilias, D.S. Catalytic and Thermal Pyrolysis of Polycarbonate in a Fixed-Bed Reactor: The Effect of Catalysts on Products Yields and Composition. Polym. Degrad. Stab. 2014, 110, 482–491. [Google Scholar] [CrossRef] [Scilit]
- Goto, M. Supercritical Water Process for the Chemical Recycling of Waste Plastics. AIP Conf. Proc. 2010, 1251, 169–172. [Google Scholar] [CrossRef] [Scilit]
- Queiroz, A.; Pedroso, G.B.; Kuriyama, S.N.; Fidalgo-Neto, A.A. Subcritical and Supercritical Water for Chemical Recycling of Plastic Waste. Curr. Opin. Green Sustain. Chem. 2020, 25, 100364. [Google Scholar] [CrossRef] [Scilit]
- Vanaraj, R.; Suresh Kumar, S.M.; Kim, S.C.; Santhamoorthy, M. A Review on Sustainable Upcycling of Plastic Waste Through Depolymerization into High-Value Monomer. Processes 2025, 13, 2431. [Google Scholar] [CrossRef] [Scilit]
- Che, C.A.; Heynderickx, P.M. Hydrothermal Carbonization of Plastic Waste: A Review of Its Potential in Alternative Energy Applications. Fuel Commun. 2024, 18, 100103. [Google Scholar] [CrossRef] [Scilit]
- Tagaya, H.; Katoh, K.; Kadokawa, J.; Chiba, K. Decomposition of Polycarbonate in Subcritical and Supercritical Water. Polym. Degrad. Stab. 1999, 64, 289–292. [Google Scholar] [CrossRef] [Scilit]
- Seshasayee, M.S.; Savage, P.E. Oil from Plastic via Hydrothermal Liquefaction: Production and Characterization. Appl. Energy 2020, 278, 115673. [Google Scholar] [CrossRef] [Scilit]
- Jin, H.; Bai, B.; Wei, W.; Chen, Y.; Ge, Z.; Shi, J. Hydrothermal Liquefaction of Polycarbonate (PC) Plastics in Sub-/Supercritical Water and Reaction Pathway Exploration. ACS Sustain. Chem. Eng. 2020, 8, 7039–7050. [Google Scholar] [CrossRef] [Scilit]
- Helmer Pedersen, T.; Conti, F. Improving the Circular Economy via Hydrothermal Processing of High-Density Waste Plastics. Waste Manag. 2017, 68, 24–31. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Arai, R.; Zenda, K.; Hatakeyama, K.; Yui, K.; Funazukuri, T. Reaction Kinetics of Hydrothermal Depolymerization of Poly(Ethylene Naphthalate), Poly(Ethylene Terephthalate), and Polycarbonate with Aqueous Ammonia Solution. Chem. Eng. Sci. 2010, 65, 36–41. [Google Scholar] [CrossRef] [Scilit]
- Ikeda, A.; Katoh, K.; Tagaya, H. Monomer Recovery of Waste Plastics by Liquid Phase Decomposition and Polymer Synthesis. J. Mater. Sci. 2008, 43, 2437–2441. [Google Scholar] [CrossRef] [Scilit]
- Irgolič, M.; Čolnik, M.; Škerget, M. Chemical Recycling of Compact Discs (CDs) with High Temperature High Pressure Water. Heliyon 2026, 12, e45225. [Google Scholar] [CrossRef] [Scilit]
- Zhao, X.; Zhan, L.; Xie, B.; Gao, B. Products Derived from Waste Plastics (PC, HIPS, ABS, PP and PA6) via Hydrothermal Treatment: Characterization and Potential Applications. Chemosphere 2018, 207, 742–752. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Hunter, S.E.; Felczak, C.A.; Savage, P.E. Synthesis of P-Isopropenylphenol in High-Temperature Water. Green Chem. 2004, 6, 222–226. [Google Scholar] [CrossRef] [Scilit]
- Kotnik, P.; Čolnik, M.; Finšgar, M.; Knez, Ž.; Škerget, M. Determination of C1–C6 Hydrocarbons in Gaseous Plastic Degradation Products by GC–MS Method. Polym. Degrad. Stab. 2020, 182, 109386. [Google Scholar] [CrossRef] [Scilit]
- Seo, J.S.; Shin, S.Y. A Study on the Physical Properties of Polycarbonate/Acrylonitrile-Butadiene-Styrene Blends with Various Thermal Stabilizers to Secure the Safety of Automobile Passengers. J. Macromol. Sci. Part B 2021, 60, 402–415. [Google Scholar] [CrossRef] [Scilit]
- Feng, Y.; Wang, B.; Wang, F.; Zhao, Y.; Liu, C.; Chen, J.; Shen, C. Thermal Degradation Mechanism and Kinetics of Polycarbonate/Silica Nanocomposites. Polym. Degrad. Stab. 2014, 107, 129–138. [Google Scholar] [CrossRef] [Scilit]
- Cai, B.; Jiang, Q.; Xu, W.; Wang, L.; Luo, Z.; Wang, B. A Nitrogen-rich DOPO -based Phosphoramide for Improving the Fire Resistance of Polycarbonate with Comparable Mechanical Property. J. Appl. Polym. Sci. 2023, 140, e54513. [Google Scholar] [CrossRef] [Scilit]
- Bai, B.; Liu, Y.; Meng, X.; Liu, C.; Zhang, H.; Zhang, W.; Jin, H. Experimental Investigation on Gasification Characteristics of Polycarbonate (PC) Microplastics in Supercritical Water. J. Energy Inst. 2020, 93, 624–633. [Google Scholar] [CrossRef] [Scilit]
- Grause, G.; Kärrbrant, R.; Kameda, T.; Yoshioka, T. Steam Hydrolysis of Poly(Bisphenol A Carbonate) in a Fluidized Bed Reactor. Ind. Eng. Chem. Res. 2014, 53, 4215–4223. [Google Scholar] [CrossRef] [Scilit]
- Harisankar, S.; Biller, P. Kinetics and Recovery of Bisphenol-A from Fiber-Reinforced Polycarbonate Using Subcritical Water. React. Chem. Eng. 2025, 10, 2835–2848. [Google Scholar] [CrossRef] [Scilit]
- Hunter, S.E.; Savage, P.E. Kinetics and Mechanism of P-Isopropenylphenol Synthesis via Hydrothermal Cleavage of Bisphenol A. J. Org. Chem. 2004, 69, 4724–4731. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Bai, B.; Liu, Y.; Wang, Q.; Zou, J.; Zhang, H.; Jin, H.; Li, X. Experimental Investigation on Gasification Characteristics of Plastic Wastes in Supercritical Water. Renew. Energy 2019, 135, 32–40. [Google Scholar] [CrossRef] [Scilit]
- Čolnik, M.; Kotnik, P.; Knez, Ž.; Škerget, M. Hydrothermal Decomposition of Polyethylene Waste to Hydrocarbons Rich Oil. J. Supercrit. Fluids 2021, 169, 105136. [Google Scholar] [CrossRef] [Scilit]
- Satou, S.; Goshima, O.; Hashimoto, T.; Ishihara, A. Hydrothermal Gasification of Phenol with Ru Added Carbon-Metal Oxide Composite-Supported Ni Catalysts Prepared by Sol-Gel Method. J. Supercrit. Fluids 2022, 188, 105694. [Google Scholar] [CrossRef] [Scilit]
- Irgolič, M.; Čolnik, M.; Škerget, M. Decomposition Behavior of Bisphenol A Under Subcritical Water Conditions: A Response Surface Methodology Approach. Processes 2026, 14, 53. [Google Scholar] [CrossRef] [Scilit]
- Pan, Z.; Liu, Y.; Wang, M.; Fang, Y. Stability of BPA in Near Critical Water. In Proceedings of the 2010 4th International Conference on Bioinformatics and Biomedical Engineering, Chengdu, China, 18–20 June 2010; IEEE: Piscataway, NJ, USA, 2010; pp. 1–4. [Google Scholar]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.