Skip to Content
MicromachinesMicromachines
  • Article
  • Open Access

26 November 2026

15 Pages

Comparison of Repetitive ESD-Induced Vth Degradation Between HBM and TLP in RF GaN HEMTs with a Matching Network

,
,
,
,
,
,
and
1
National ASIC System Engineering Research Center, School of Integrated Circuits, Southeast University, Nanjing 210096, China
2
Nanjing Electronic Devices Institute, Nanjing 210016, China
*
Author to whom correspondence should be addressed.

Abstract

Package-integrated matching networks (MNs) are widely used in RF GaN HEMTs; however, it remains unclear whether human body model (HBM) and transmission line pulse (TLP) stresses produce distinguishable degradation in devices with MNs. This work investigates repetitive gate-ESD-induced pinch-off voltage (Vth) degradation in packaged RF GaN HEMTs with and without MNs under HBM and TLP stress. Under positive HBM and TLP stress, the Schottky gate is forward-biased, and high current density at the Schottky interface causes damage and Vth degradation. Because the DUT resistance is much smaller than the stress source resistance, the MN has a negligible effect on the gate voltage, and the Vth degradation trends are similar for DUTs with and without MN. Under negative HBM stress, the reverse-blocked Schottky gate and high electric field at the gate edge induce defects and Vth degradation. The MN can suppress the gate voltage and alleviate degradation in the DUT with an MN. The difference becomes more pronounced as the negative HBM voltage increases. In contrast, under negative TLP stress, the standardized 50 Ω source impedance keeps the gate-voltage difference small, so no obvious Vth degradation difference is observed between DUTs with and without MN. Simplified analytical models and TCAD simulations consistently explain these trends, clarifying why RF GaN HEMTs with an MN and without an MN exhibit distinguishable Vth degradation under negative HBM stress but not under negative TLP stress.

1. Introduction

Radio-frequency (RF) GaN high-electron-mobility transistors (HEMTs) have become the technology of choice for power amplifiers in 5G massive-MIMO base stations, radar, and satellite communication systems, owing to their high power density, wide bandwidth, and superior efficiency [1,2,3,4]. For RF GaN HEMTs used in practical power amplifiers, input/output matching networks (MNs) are employed to optimize impedance and bandwidth. Conventionally, GaN dies are packaged as discrete devices and paired with external PCB-based matching networks built from passive components. In contrast, advanced package-integrated matching network configurations, in which transistor dies and matching elements are co-packaged within a compact package, offer superior performance metrics, including higher linearity, improved power-added efficiency, and wider bandwidth [5,6,7,8]. Thus, this package-integrated approach is widely used in RF GaN devices.
With the mass deployment of RF GaN HEMT applications, electrostatic discharge (ESD) reliability has emerged as a concern because of internal defects in GaN materials [9]. Unlike catastrophic ESD failure, which has been extensively studied in standalone devices, the cumulative effect of repeated non-destructive ESD events during assembly, testing, and operation can induce gradual parameter drift that may compromise RF performance before any hard failure occurs. Two standard stress tests, including the human body model (HBM) and the transmission line pulse (TLP), are usually used to evaluate the ESD robustness of devices. Recently, many reports have focused on the differences between HBM and TLP stresses in GaN HEMTs and have shown that conventional HBM–TLP correlation can yield misleading estimates for GaN HEMTs because the breakdown mechanism of GaN contradicts the physical basis of this correlation [10,11,12]. Meanwhile, repetitive non-destructive HBM-ESD stress can still produce measurable pinch-off voltage (Vth) degradation in GaN devices, creating mismatch risks in bare-die evaluations in our previous work [13]. However, it remains unclear whether these two stress modalities produce distinguishable Vth degradation in RF GaN devices with matching networks.
In this work, to address this question, TLP- and HBM-induced Vth degradation in packaged RF GaN HEMTs with and without matching networks is compared and investigated under repetitive stress. Some HBM experiments and device samples are adopted from our prior work, together with the previously reported Vth-shift trends under repetitive HBM stress for devices with and without matching networks. In addition, all repetitive TLP measurements, transient waveform characterization, corresponding circuit analysis, and the direct comparison between repetitive HBM and repetitive TLP degradation behaviors are newly developed. The results show that under repetitive ESD stress, for both HBM and TLP stresses, the Schottky gate is damaged by the high forward current density and large reverse electric field, which in turn induces Vth degradation. Moreover, the Vth degradation trends do not differ between GaN HEMTs with and without matching networks under repetitive positive HBM and TLP stress. However, the Vth degradation trends differ between GaN HEMTs with and without matching networks under repetitive negative HBM stress, whereas no such difference is observed under repetitive negative TLP stress. On the basis of simulations and simplified analytical models, the underlying mechanism is discussed.

2. Devices and Experiments

Figure 1a shows the top view of the commercial GaN device (A3G26D055N, NXP Semiconductors N.V., Eindhoven, The Netherlands) used in the ESD experiments. After decapping the external package, the GaN HEMT is connected to the matching network via bonding wires at the package level. The equivalent circuit shown in Figure 1b demonstrates that the matching network consists of two bonding-wire inductors (Lm1, Lm2) and a metal-insulator-metal capacitor (Cm) connected in parallel with the gate. The measured value of Cm is approximately 10 pF. The parasitic inductance of the two bonding-wire inductors is difficult to measure directly because no suitable test contact points are available. Instead, the parasitic inductance can be calculated using the analytical models reported in [14,15]. The values of Lm1 and Lm2 are approximately 0.63 nH and 1.04 nH, respectively. As shown in Figure 1c, the GaN device is fabricated on the GaN-on-SiC substrate with the AlGaN/GaN heterojunction. Scanning electron microscopy (SEM) manufactured by Hitachi (Hitachi Ltd., Tokyo, Japan) confirms the formation of a T-shaped Schottky gate structure and a source plate configuration. The gate-to-source length (LGS) is 1.4 μm, the gate-to-drain length (LGD) is 3.4 μm, and the channel length (LCH) is 0.5 μm.
Figure 1. (a) Decapsulated view of the pre-matched GaN HEMT at the package level. (b) Schematic diagram of the DUT and gate-ESD test configuration. (c) Cross-section and SEM picture of the GaN HEMT device.
Considering the direct connection between the MN and the GaN HEMT gate electrode, our investigation focuses on the gate-ESD scenario. Two types of devices under test (DUTs) are prepared to clarify the influence of the MN: a GaN transistor with an MN (w/i MN), which uses the commercial HEMT. A GaN transistor without an MN (w/o MN) uses the same commercial HEMT, but the connection between the matching network and the transistor die is removed, and the gate pad is connected to an external pad with a new bonding wire after de-capping. The initial DC characteristics of the DUTs with and without MN are measured, as shown in Figure 2. No significant difference is observed between them. A commercial HBM ESD generator manufactured by EVERFINE (EVERFINE Corp., Hangzhou, China) and a TLP system manufactured by Hanwa (Hanwa Electronic Ind. Co., Ltd., Wakayama, Japan) are used to measure the DUTs, respectively, and their equivalent test circuits are shown in Figure 3a and Figure 3b, respectively. For HBM testing, a voltage (VHBM) is pre-set on the equivalent human-body capacitor (CHBM), and then VHBM is discharged to the gate of the DUT while the other electrodes remain grounded [16]. For TLP testing, a voltage (VTLP) is pre-charged onto a 50 Ω transmission line (TL1), and VTLP is then discharged to the gate of the DUT through another 50 Ω transmission line (TL2) [17]. Before the repetitive stresses, the gate-ESD robustness of DUTs is determined. Then, non-destructive ESD stresses, including HBM and TLP, are applied repetitively to the gate electrodes. For each stress type, three independent DUTs are measured to ensure data repeatability and stability. The transfer characteristics are monitored using Agilent B1500A (Agilent Technologies Inc., Santa Clara, CA, USA) before and after the ESD stresses, and the Vth values are extracted using the maximum transconductance method. It should be noted that trapping effects can result in a recoverable Vth degradation, which has been widely reported [18,19,20,21]. After negative gate stress, electrons in the channel can be captured by surface traps near the gate region through the gate leakage current [19]. To exclude the trapping-induced Vth shift, a de-trapping process with VGS = 1 V and VDS = 1 V is applied during the experiments [20]. The detailed experiment is described as follows: first, the transfer curve of the fresh DUT is measured. Then, a series of pulse stresses are applied to the gate of the DUTs, with a pulse spacing of 0.1 s for both HBM and TLP stresses. When the number of stress pulses reaches a certain value (e.g., 10, 100, 1000, etc.), the transfer curves are measured again. Before each transfer curve measurement, a de-trapping bias of VGS = 1 V and VDS = 1 V is applied for 60 s, and the transfer curves are measured 10 s after the de-trapping bias is removed.
Figure 2. Measured DC characteristics of fresh GaN HEMTs with and without MN, including ID–VD curves, gate leakage curves, and transfer characteristic curves.
Figure 3. Equivalent circuit diagram for the DUTs with MN and without MN: (a) HBM ESD testing with CHBM of 100 pF and RHBM of 1500 Ω; (b) TLP testing with RTL1 and RTL2 of 50 Ω.

3. Results and Discussions

The measured HBM and TLP results for the DUTs with and without MN are shown in Figure 4a,b. Under positive HBM stress, the HBM ESD robustness exceeds +8 kV, reaching the limitation of our test instrument. Under negative HBM stress, the failure voltage is −350 V, which is much lower than that under positive stress. This is because the gate of the DUT is used as the Schottky gate. Under positive stress, the gate is biased in the forward-conduction state and thus has a high current-discharge capability. Under negative stress, the Schottky gate remains in the reverse-blocking state and has a weak current-discharge capability [22,23]. For comparison, the ESD robustness of the DUT without MN does not differ from that of the DUT with MN. The TLP curve results show that the DUT exhibits a conduction feature under positive TLP pulses. The secondary breakdown current (It2) is larger than 6 A for both the DUTs with MN and without MN, which is also nearly the limitation of our TLP instrument. Under negative TLP stress, It2 is 0.0361 A and 0.0356 A for the DUTs with MN and without MN, respectively. This demonstrates that It2 shows a negligible difference (0.5 mA difference) between the DUTs with MN and without MN. It is also noted that, under negative stress, the HBM ESD voltage does not comply with the conventional correlation VHBM = 1500 × It2 [24], as reported and investigated in other studies [10,12,25].
Figure 4. Measured ESD robustness of the DUT with MN and without MN: (a) positive and negative gate HBM test results; (b) positive and negative TLP-measured curves.
Based on the results of the ESD robustness measured under HBM stress and TLP stress, non-destructive positive and negative stress levels are selected for HBM and TLP testing, respectively. As shown in Figure 5, the transfer curves shift toward more positive voltages, and the shift persists after de-trapping when VHBM = +6 kV is applied repetitively to the DUT with MN. Vth changes from −2.537 V to −2.367 V after 104 stress cycles. Comparatively, the DUT without MN has the same results, with a difference in Vth (∆Vth) of 0.168 V. Under negative HBM stress, the transfer curves also shift toward more positive voltages, and the shift persists after de-trapping. However, it is noted that ∆Vth is 0.168 V for the DUT with MN, whereas it is 0.205 V for the DUT without MN after the 104 stress cycles. There is a 0.037 V difference, which differs from that under positive stress. Repetitive TLP stresses are also applied, and the results are shown in Figure 6. After positive TLP stress at VTLP = +140 V, the transfer curves shift and Vth increases after de-trapping. A negligible difference in ∆Vth is found between the DUTs with MN and without MN (0.004 V difference). Under negative TLP stress at VTLP = −60 V, ∆Vth is about 0.213 V for the DUT with MN, while it is about 0.206 V for the DUT without MN. A negligible difference (0.007 V) is observed between the DUTs with and without MN, which differs from the phenomenon under negative HBM stress.
Figure 5. Measured transfer curves of GaN HEMTs before and after repetitive HBM ESD stresses at VDS = 0.1 V. (Top left): GaN HEMT with MN under HBM stress at VHBM = +6 kV. (Top right): GaN HEMT without MN under HBM stress at VHBM = +6 kV. (Bottom left): GaN HEMT with MN under HBM stress at VHBM = −300 V. (Bottom right): GaN HEMT without MN under HBM stress at VHBM = −300 V.
Figure 6. Measured transfer curves of GaN HEMTs before and after repetitive TLP stresses at VDS = 0.1 V. (Top left): GaN HEMT with MN under TLP stress at VTLP = +140 V. (Top right): GaN HEMT without MN under TLP stress at VTLP = +140 V. (Bottom left): GaN HEMT with MN under TLP stress at VTLP = −60 V. (Bottom right): GaN HEMT without MN under TLP stress at VTLP = −60 V.
These GaN HEMTs are mainly used for power-amplifier applications [1,3,8]. To understand the influence of Vth degradation on RF performance, the S-parameters of the DUTs with and without MN are measured when the DUTs are biased at the Class-AB condition (VDS = 15 V and VGS = −2.5 V) after the repetitive negative HBM stress (VHBM = −300 V). In our previous work, S11 and S22 changed after stress, indicating changes in the input and output impedances [13]. Therefore, S11 and S22 are not further presented herein. S21 is measured here to evaluate the forward transmission gain of the DUTs with and without MN, as shown in Figure 7a,b. S21 decreases for the DUTs with and without MN, which is attributed to Vth degradation causing a decrease in the bias drain current. This indicates that the gain decreases after HBM stress, thereby affecting the amplification performance of RF power amplifiers. More severe S21 degradation is observed in the DUT without MN, which results from its more severe Vth degradation.
Figure 7. Measured S21 of GaN HEMTs before and after VHBM =−300 V when biased at VDS = 15 V and VGS = −2.5 V. (a) GaN HEMT with MN. (b) GaN HEMT without MN.
To understand the degradation mechanism, technology computer-aided design (TCAD) simulations Sentaurus (v2018) have been carried out. The simulated electrical performance of the DUT is calibrated against the measured results, including the transfer and ID-VD curves. In addition, the mixed-mode simulations are used to reproduce the discharge behavior under HBM and TLP stresses based on the equivalent circuit shown in Figure 3. The calibrated short-circuit currents for different VHBM values in the simulation are shown in Figure 8a. Their peak current (Ips) and rising time (tr) of these waveforms comply with the waveform specification defined in the standard [16]. Therefore, the simulation results are consistent with the standardized waveforms generated by the commercial ESD test system. For the TLP simulation, a square-like pulse with a 100 ns pulse width and 10 ns rising/falling time is defined and applied to a 50 Ω resistor (see Figure 8b). The TLP current waveforms exhibit a square-like shape, consistent with the definition of a square wave in TLP measurements. According to previous works [13,22,26], under positive HBM stress, the gate is biased in the forward-conduction state, and a large current flows from the Schottky gate to the grounded source and drain. Consequently, the unstable Schottky interface is easily damaged because of the high current density. The total current density distributions of the DUT with MN under HBM stress at VHBM = +6 kV and TLP stress at VTLP = +140 V are depicted in Figure 9a. The results demonstrate that a high current density appears at the Schottky interface, which induces permanent damage generation and further causes Vth degradation [22,26,27]. Similarly, the electric field distributions under negative HBM stress at VHBM = −300 V and TLP stress at VTLP = −60 V are depicted in Figure 9b. High electric field peaks are located at the edge of the gate under both the negative HBM and TLP stresses. These high electric fields can further induce pits, defects, and related damage due to the inverse piezoelectric effect, thereby degrading the Vth of the GaN devices [12,27,28,29]. The DUT without the MN has the same results, and the corresponding simulation results are not presented further.
Figure 8. Calibrated current waveforms under different stress voltages in the simulation: (a) simulated HBM short-circuit current waveforms; (b) simulated TLP current waveforms across 50 Ω.
Figure 9. Simulation results for GaN HEMTs with MN under the HBM and TLP stresses: (a) total current density distributions at VHBM = +6 kV and VTLP = +140 V, respectively; (b) electric field distributions at VHBM = −300 V and VTLP = −60 V, respectively.
Figure 10 shows the measured Vth difference from the fresh device versus increasing ESD stress cycles under different HBM voltages. Under positive HBM stress, the Vth degradation trend of the DUT with MN is similar to that of the DUT without MN under different HBM voltages. As the positive VHBM increases, the Vth differences accordingly become larger. This is because a high VHBM produces a higher current density at the Schottky gate, which results in more damage. Under negative HBM stress, the Vth difference between the DUTs with MN and without MN exhibits an obvious discrepancy under different negative VHBM values. The Vth degradation of the DUT without MN is more severe than that of the DUT with MN, and this difference becomes more obvious as the magnitude of the negative VHBM increases. The Vth degradation results are also measured under different VTLPs, as demonstrated in Figure 11. For both the positive and negative TLP stresses, the Vth difference from the fresh device increases with the increasing TLP stress level, which is consistent with the results under HBM stress. However, it is noted that under negative TLP stress, there is no difference in the Vth difference between the DUTs with MN and without MN, which differs from the phenomenon under negative HBM stress. It should be noted that the results presented in Figure 10 and Figure 11 are obtained from the individual DUTs such as those shown in Figure 5 and Figure 6, respectively. For the other individual DUTs, the differences in ∆Vth between the DUTs with and without MN are 0.039 V and 0.035 V under −300 V HBM stress, and 0.005 V and 0.004 V under +6 kV HBM stress after 104 cycles, respectively. Similarly, the corresponding differences are 0.001 V and 0.003 V under −60 V TLP stress, and 0.004 V and 0.005 V under +140 V TLP stress after 104 cycles, respectively. These results further confirm that the MN significantly affects Vth degradation under negative HBM stress, whereas its influence is negligible under positive HBM stress and under both positive and negative TLP stresses.
Figure 10. Measured Vth difference in the DUTs with MN and without MN from the fresh device versus ESD stress cycles under different HBM voltages: (a) positive HBM stresses for VHBM = +8 kV, +6 kV, and +4 kV; (b) negative HBM stresses for VHBM = −300 V, −200 V, and −100 V.
Figure 11. Measured Vth difference in the DUTs with MN and without MN from the fresh device versus ESD stress cycles under different TLP voltages: (a) Positive TLP stresses for VTLP = +160 V, +140 V and +120 V. (b) Negative TLP stresses for VTLP = −60 V, −40 V and −20 V.
To explain the difference in Vth degradation between the DUTs with and without MN under HBM and TLP stress, the voltage waveforms across the gate of the DUTs with MN and without MN are simulated and measured. Figure 12a shows the simulated VHBM waveform for the DUTs with MN and without MN under different HBM stress levels. Because the gate Schottky diode is in the forward-conduction state, VDUT stays at a low level, and there is no difference between the DUTs with MN and without MN. Thus, their Vth degradation behaviors are similar. However, under different negative stresses, the VDUT waveforms for the DUT with MN differ from those for the DUT without MN. As shown in Figure 12b, the VDUT waveform of the DUT with MN is suppressed compared with that of the DUT without MN. The higher voltage can result in a higher electric field at the gate edge, and further induce severe Vth degradation in the DUT without MN. This explains the difference in Vth degradation between the DUTs with MN and without MN in Figure 10b. In addition, as the magnitude of the negative VHBM increases, the difference in VDUT between points A and B becomes larger. For example, the difference is 32 V at VHBM = −300 V, while it is 23 V at VHBM = −100 V. This explains why the difference in Vth degradation increases with the magnitude of the negative VHBM in Figure 10b.
Figure 12. Simulated VDUT waveforms of the DUTs with MN and without MN during the discharge process. (a) VDUT under the positive HBM stresses for VHBM = +8 kV, +6 kV, and +4 kV; (b) VDUT under the negative HBM stresses for VHBM = −300 V, −200 V, and −100 V.
The measured VDUT waveforms under TLP stress for the DUTs with MN and without MN are shown in Figure 13. Under positive TLP stress, the VDUT waveform shows no difference between the DUTs with MN and without MN. Meanwhile, VDUT also stays at a low level within the quasi-static state sampling interval, which verifies the forward-conduction state of the Schottky diode. Under negative TLP stress, no difference in VDUT is found between the DUTs with MN and without MN under different VTLP values. Therefore, the Vth degradation of the DUT with MN is the same as that of the DUT without MN under both positive and negative TLP stress.
Figure 13. Measured VDUT waveforms of the DUTs with MN and without MN during the discharge process. (a) VDUT under the positive TLP stresses for VTLP = +160 V, +140 V and +120 V; (b) VDUT under the negative TLP stresses for VTLP = −60 V, −40 V and −20 V.
Although HBM and TLP stresses are broadband transient events, they also involve frequency-dependent signals, and their frequency spectra have been investigated [30,31,32,33]. Therefore, a simplified analytical model for HBM and TLP stresses is proposed in which each circuit element is treated as a frequency-dependent impedance. In this way, this model can be readily understood from fundamental circuit principles. These simplified models are used to facilitate understanding of why Vth degradation differences occur between the DUTs with MN and without MN, whereas no such difference occurs under the other stress condition. However, a limitation of this simplified model is its inability to accurately predict the gate-voltage waveforms, because HBM and TLP waveforms are difficult to model as a function of frequency. For HBM stress, the maximum frequency is lower than 350 MHz, and the frequency of the dominant amplitude is below 100 MHz [30,31]. For the square-like TLP with a 10 ns rise/fall time and a 100 ns pulse width, its frequency characteristic is analyzed using the Fourier transform, as shown in Figure 14. Most of the amplitude is at low frequencies; its maximum frequency is lower than 50 MHz. Based on the principle of the time-domain reflectometer (TDR)–TLP system [17,34], the charging-line voltage VTLP is applied to the DUT through a section of transmission line with a 50 Ω impedance. If the impedance of the DUT is not matched to 50 Ω, reflection occurs at the DUT terminal. Thus, the actual voltage is the superposition of the incident wave voltage (V+) and the reflected wave voltage (V−) [34]. Under the open-circuit condition, the impedance approaches infinity. Therefore, the incident wave voltage undergoes total reflection, and the measured voltage approaches 10 V. The values of Lm1 and Lm2 are approximately 0.63 nH and 1.04 nH, respectively. Even at 350 MHz, the impedances of Lm1 and Lm2 are 1.38 jΩ and 2.29 jΩ, respectively, which are much lower than the impedance of Cm (−45.5 jΩ). Therefore, the impedances of Lm1 and Lm2 in the MN can be neglected due to their small values at low frequencies. Under HBM stress, VDUT of the DUT with MN (VDUT,MN) can be expressed by Equation (1), and VDUT of the DUT without MN (VDUT,noMN) can be expressed by Equation (2)
V DUT , MN = V HBM j ω R HBM C m + R HBM R DUT + 1 = V HBM ω R HBM C m 2 + R HBM R DUT + 1 2
V DUT , noMN = V HBM R HBM R DUT + 1
whereas RDUT denotes the on-resistance from the gate. ω denotes angular frequency. Under positive HBM, RDUT is much smaller than RHBM due to the forward turn-on of the Schottky gate diode. As a result, RHBM/RDUT + 1 >> ꞷRHBMCm. The value of VDUT,MN is mainly dominated by RHBM/RDUT + 1 and is independent of Cm. Therefore, VDUT,MN ≈ VDUT,noMN and the gate voltage waveforms are the same in Figure 12a. In this case, no difference in Vth degradation is found between the DUTs with MN and without MN. The difference between VDUT,noMN and VDUT, MN as a function of RHBM and frequency at VHBM = +6 kV is plotted in Figure 15a. Since the maximum frequency of the HBM signal is relatively low, the input impedance of the DUT can be approximately treated as a variable resistor. RDUT is calculated from the simulated gate voltage and gate current waveforms at VHBM = +6 kV. Under this condition, the maximum simulated voltage across the DUT is 2.18 V, and the maximum simulated current is 4.19 A. RDUT is calculated to be approximately 0.52 Ω. It can be seen that, regardless of changes in RHBM and frequency, especially at RHBM = 1500 Ω (orange line), the difference value is lower than 5 × 10−4 V, which verifies the above analyses. This means that Cm of the MN does not work under the positive HBM stress.
Figure 14. Measured TLP waveform in the open circuit at VTLP = 5 V and its Fourier transform results in the frequency domain.
Figure 15. Calculated VDUT difference between the DUTs with MN and without MN for the different RHBM and frequencies under HBM stresses: (a) under the condition of RDUT = 0.52 Ω at VHBM = +6 kV; (b) under the condition of RDUT = 3160 Ω at VHBM = −100 V.
Under negative HBM stress, RDUT becomes large because the Schottky gate diode is in the reverse-blocking state. Under this condition, the values of RHBM/RDUT + 1 and ꞷRHBMCm can be of the same order of magnitude. Consequently, VDUT,MN is smaller than VDUT,noMN. The distribution of their difference as a function of RHBM and frequency is also plotted in Figure 15b. Similarly, at VHBM = −100 V, the maximum simulated voltage across the DUT is −114.31 V and the maximum simulated current is 36.17 mA. RDUT is calculated to be approximately 3160 Ω. Under the condition of RHBM = 1500 Ω, the difference increases obviously when the frequency exceeds 1 MHz. Therefore, the MN can affect VDUT and thus cause the difference in Vth degradation between the DUTs with MN and without MN.
V DUT = V + + V − = 1 + Γ V + = 1 + Z DUT − 50 Z DUT + 50 V + = 2 Z DUT Z DUT + 50 V +
V ′ DUT , MN = 2 V TLP j ω R TL 2 C m + R TL 2 R DUT + 1 = 2 V TLP ( ω R TL 2 C m ) 2 + ( R TL 2 R DUT + 1 ) 2
V ′ DUT , noMN = 2 V TL 2 R TL 2 R DUT + 1
Similarly, VDUT under TLP stress is also calculated based on the principle of the TDR–TLP system mentioned above. The actual VDUT is the superposition of the incident wave voltage (V+) and the reflected wave voltage (V−), which can be expressed by Equation (3). Based on Equation (3), under TLP stress, VDUT for the DUT with MN (V′DUT,MN) and for the DUT without MN (V′DUT,noMN) can be expressed by Equations (4) and (5), respectively. In Equation (4), ZDUT is the impedance of the parallel combination of RDUT and Cm. In Equation (5), ZDUT is RDUT. Their variations as functions of RTL2 and frequency at VTLP = +140 V are plotted in Figure 16. At VTLP = +140 V, the maximum measured voltage is approximately 10.38 V, while the maximum measured current is 5.19 A, based on the measured quasi-static TLP I-V curves in Figure 4b. RDUT is calculated to be approximately 2 Ω. As shown in Figure 16a, regardless of RTL2 and frequency, the difference between V′DUT,MN and V′DUT,noMN is lower than 0.001 V. This is also because RDUT is much lower than RTL2 when the Schottky gate is in the forward-conduction state. Under negative TLP stress, the maximum measured voltage is about 117.42 V, while the maximum measured current is 22.8 mA based on the measured quasi-static TLP I-V curves in Figure 4b. RDUT is calculated to be approximately 5150 Ω at VTLP = −60 V. As shown in Figure 16b, the difference between V′DUT,MN and V′DUT,noMN becomes obviously larger at a high frequency of 1 MHz when RTL2 is larger than 500 Ω. However, for the TLP system, RTL2 is standardized at 50 Ω, as indicated by the pink line in Figure 16b. Under this condition, the difference is smaller than 3 V within the frequency range from 0 to 50 MHz. This explains why, under negative HBM stress, the DUTs with MN and without MN exhibit a large difference between VDUT,MN and VDUT,noMN, whereas under negative TLP stress they exhibit only a small difference between V′DUT,MN and V′DUT,noMN, owing to the difference in RHBM and RTL2. As a result, different Vth degradation occurs under repetitive negative HBM stress, whereas no such difference occurs under repetitive negative TLP stress.
Figure 16. Calculated VDUT difference between the DUTs with MN and without MN for different RTL2 and frequencies under TLP stresses: (a) under condition of RDUT = 2 Ω at VTLP = +140 V; (b) under condition of RDUT = 5150 Ω at VTLP = −60 V.
To further verify the above analyses based on the simplified model, the gate waveforms across the DUTs with and without MN under ESD stress are simulated again using the TCAD simulations. Figure 17a shows the simulated gate waveform across the DUTs with MN and without MN under the negative HBM stress for different RHBM values. The results demonstrate that, for the DUT with MN, the peak of the gate waveform is gradually suppressed as RHBM increases from 300 Ω to 1200 Ω, which is consistent with the calculated results for VDUT,MN and VDUT,noMN. Under the negative TLP stress, as shown in Figure 17b, V′DUT,MN decreases with increasing RTL2. However, for the standard 50 Ω impedance, the difference between V′DUT,MN and V′DUT,noMN is small.
Figure 17. Simulated VDUT waveform of the DUTs with MN and without MN for different RHBM and RTL2: (a) under negative HBM stress of VHBM = −300 V; (b) under negative TLP stress of VTLP = −60 V.

4. Conclusions

This study investigates repetitive non-destructive ESD-induced Vth degradation in packaged RF GaN HEMTs with and without MNs under HBM and TLP stress. For positive HBM and TLP stress, the Schottky gate is forward-biased, and the high current density at the Schottky interface causes damage and Vth degradation. Because RDUT is much smaller than the stress source resistance, the MN has a negligible effect on VDUT, and the Vth degradation trends are similar for DUTs with and without MN. Under negative HBM stress, the Schottky gate is reverse-biased, and high electric fields at the gate edge induce defects and Vth degradation. In this case, the MN suppresses VDUT, so the DUT without MN exhibits more severe Vth degradation, and the difference increases with the magnitude of the negative VHBM. In contrast, under negative TLP stress, the standardized 50 Ω impedance keeps the VDUT difference between the DUTs with MN and without MN small. No obvious difference in Vth degradation is observed between the DUTs with and without MN. The new insight is that the matching network effectively suppresses gate degradation under negative repetitive HBM stress, while this suppression effect disappears under standard 50 Ω repetitive TLP stress, revealing that TLP results cannot be directly extrapolated to predict repetitive HBM reliability for packaged RF GaN HEMTs with integrated matching networks.

Author Contributions

Conceptualization, R.Y.; methodology, S.W. and Z.H.; validation, J.Y., S.J. and Z.H.; formal analysis, Z.H.; investigation, R.Y. and S.L. (Siyang Liu); resources, S.W.; data curation, S.W. and J.Y.; writing—original draft preparation, R.Y.; writing—review and editing, R.Y. and S.W.; visualization, S.L. (Sheng Li); supervision, S.L. (Siyang Liu); project administration, L.S.; funding acquisition, L.S. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded in part by the National Natural Science Foundation of China under Grant 62404043 and the Natural Science Foundation of Jiangsu Province under Grants BK20241293 and BK20243055.

Institutional Review Board Statement

Not applicable.

Data Availability Statement

The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding author.

Conflicts of Interest

The authors declare no conflicts of interest.

References

  1. Kim, J. A Review of Ku-Band GaN HEMT Power Amplifiers Development. Micromachines 2024, 15, 1381. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  2. Chen, K.J.; Haberlen, O.; Lidow, A.; Tsai, C.L.; Ueda, T.; Uemoto, Y.; Wu, Y. GaN-on-Si Power Technology: Devices and Applications. IEEE Trans. Electron Devices 2017, 64, 779–795. [Google Scholar] [CrossRef] [Scilit]
  3. Nakajima, S. GaN HEMTs for 5G base station applications. In Proceedings of the IEEE IEDM, San Francisco, CA, USA, 1–5 December 2018. [Google Scholar]
  4. Wang, Y.; Huang, S.; Jiang, Q.; Wang, X.; Fan, J.; Yin, H.; Wei, K.; Zheng, Y.; Liu, X. Ultralow ohmic contact in recess-free ultrathin barrier AlGaN/GaN heterostructures across a wide temperature range. Chin. J. Electron. 2025, 34, 137–145. [Google Scholar] [CrossRef] [Scilit]
  5. Calvillo-Cortes, D.A.; Shi, K.; Langen, M.; Rijs, F.; Vreede, L.C.N. On the design of package-integrated RF high-power amplifiers. In Proceedings of the IEEE/MTT-S International Microwave Symposium Digest, Montreal, QC, Canada, 17–22 June 2012. [Google Scholar]
  6. Namaki, P.; Masoumi, N.; Nezhad-Ahmadi, M.-R. Characterization and Performance Improvement of Bondwire Interconnects in QFN Packages for Bandpass MM-Wave Applications. IEEE Trans. Compon. Packag. Manuf. Technol. 2024, 14, 71–80. [Google Scholar] [CrossRef] [Scilit]
  7. Heijden, M.P.; Acar, M.; Maroldt, S. A package-integrated 50W high-efficiency RF CMOS-GaN class-E power amplifier. In Proceedings of the IEEE MTT-S International Microwave Symposium Digest, Seattle, WA, USA, 2–7 June 2013. [Google Scholar]
  8. Helalian, H.; Zhu, X.; Atarodi, M. A Multioutput and Highly Efficient GaN Distributed Power Amplifier for Compact Subarrays in Wideband Phased Array Antennas. IEEE Trans. Microw. Theory Tech. 2023, 71, 4800–4813. [Google Scholar] [CrossRef] [Scilit]
  9. Shankar, B.; Raghavan, S.; Shrivastava, M. ESD Reliability of AlGaN/GaN HEMT Technology. IEEE Trans. Electron Devices 2019, 66, 3756–3763. [Google Scholar] [CrossRef] [Scilit]
  10. Sun, J.; Zheng, Z.; Zhang, L.; Chen, K.J. Correlation between Pulse I-V and Human Body Model (HBM) Tests for Drain Electrostatic Discharge (ESD) Robustness Evaluation of GaN Power HEMTs. In Proceedings of the IEEE 34th International Symposium on Power Semiconductor Devices and ICs (ISPSD), Vancouver, BC, Canada, 22–25 May 2022. [Google Scholar]
  11. Wang, Y.; Wang, Y. A New Method to Correlate Human Body Model and Transmission Line Pulse Based on RC Thermal Equivalent Model. IEEE Trans. Electron Devices 2020, 67, 3775–3780. [Google Scholar] [CrossRef] [Scilit]
  12. Wu, W.-M.; Ker, M.-D.; Chen, S.-H.; Sibaja-Hernandez, A.; Yadav, S.; Peralagu, U.; Yu, H.; Alian, A.; Putcha, V.; Parvais, B.; et al. ESD HBM Discharge Model in RF GaN-on-Si (MIS)HEMTS. IEEE Trans. Electron Devices 2022, 69, 2180–2187. [Google Scholar] [CrossRef] [Scilit]
  13. Ye, R.; Luo, H.; Wang, S.; Hu, Z.; Bian, J.; Kang, Q.; Li, S.; Liu, S.; Sun, W. Repetitive Gate-HBM-ESD-Induced Vth Degradation for RF GaN HEMT with Matching Networks. IEEE J. Electron Devices Soc. 2026, 14, 41–48. [Google Scholar] [CrossRef] [Scilit]
  14. Xue, H.; Benedik, C.R.; Zhang, X.; Li, S.; Ren, S. Numerical Solution for Accurate Bondwire Modeling. IEEE Trans. Semicond. Manuf. 2018, 31, 258–265. [Google Scholar] [CrossRef] [Scilit]
  15. Mouthaan, K.; Tinti, R.; de Kok, M.; de Graaff, H.C.; Tauritz, J.L.; Slotboom, J. Microwave modelling and measurement of the self- and mutual inductance of coupled bondwires. In Proceedings of the Bipolar/BiCMOS Circuits and Technology Meeting, Minneapolis, MN, USA, 28–30 September 1997. [Google Scholar]
  16. ANSI/ESDA/JEDEC JS-001; ESDA/JEDEC Joint Standard for Electrostatic Discharge Sensitivity Testing—Human Body Model (HBM)—Device Level. JEDEC Solid State Technology Association: Arlington, VA, USA, 2023.
  17. Voldman, S.H.; Ashton, R.; Barth, J.; Bennett, D.; Bernier, J.; Chaine, M.; Daughton, J.; Grund, E.; Farris, M.; Gieser, H.; et al. Standardization of the transmission line pulse (TLP) methodology for electrostatic discharge (ESD). In Proceedings of the 2003 Electrical Overstress/Electrostatic Discharge Symposium, Las Vegas, NV, USA, 21–25 September 2003. [Google Scholar]
  18. Mukherjee, K.; De Santi, C.; Rzin, M.; Gao, Z.; Meneghesso, G.; Meneghini, M.; Zanoni, E. Investigation into Trapping Modes and Threshold Instabilities of State-of-Art Commercial GaN HEMTs. Microelectron. Reliab. 2019, 100–101, 113464. [Google Scholar] [CrossRef] [Scilit]
  19. Mitrofanov, O.; Manfra, M. Mechanisms of Gate Lag in GaN/AlGaN/GaN High Electron Mobility Transistors. Superlattices Microstruct. 2003, 34, 33–53. [Google Scholar] [CrossRef] [Scilit]
  20. Joh, J.; Del Alamo, J.A. A Current-Transient Methodology for Trap Analysis for GaN High Electron Mobility Transistors. IEEE Trans. Electron Devices 2010, 58, 132–140. [Google Scholar] [CrossRef] [Scilit]
  21. Meneghesso, G.; Meneghini, M.; De Santi, C.; Ruzzarin, M.; Zanoni, E. Positive and Negative Threshold Voltage Instabilities in GaN-Based Transistors. Microelectron. Reliab. 2017, 80, 257–265. [Google Scholar] [CrossRef] [Scilit]
  22. Sun, J.; Zheng, Z.; Shu, J.; Chen, K.J. Investigating Forward Gate ESD Mechanism of Schottky-Type P-GaN Gate HEMTs Using a SiC-Based High-Speed Pulsed I-V Test System. IEEE Electron Device Lett. 2024, 45, 1265–1268. [Google Scholar] [CrossRef] [Scilit]
  23. Chen, J.; Liu, J.; Zou, W.; Ma, J. Investigation of On-Wafer ESD Characteristics (HBM and TLP) of Lateral GaN-on-Si SBDs. IEEE Trans. Electron Devices 2023, 70, 6691–6694. [Google Scholar] [CrossRef] [Scilit]
  24. Stadler, W.; Guggenmos, X.; Egger, P.; Gieser, O.; Musshoff, C. Does the ESD-failure Current Obtained by Transmissionline Pulsing Always Correlate to Human Body Model Tests? In Proceedings of the Electrical Overstress/Electrostatic Discharge Symposium, Santa Clara, CA, USA, 23–25 September 1997. [Google Scholar]
  25. Wu, W.-M.; Chen, S.-H.; Putcha, V.; Peralagu, U.; Sibaja-Hernandez, A.; Yadav, S.; Parvais, B.; Alian, A.; Collaert, N.; Ker, M.-D.; et al. ESD failures of GaN-on-Si D-mode AlGaN/GaN MIS-HEMT and HEMT devices for 5G telecommunications. In Proceedings of the 43rd Annual EOS/ESD Symposium (EOS/ESD), Tucson, AZ, USA, 26 September–1 October 2021. [Google Scholar]
  26. Shankar, B.; Gupta, S.D.; Soni, A.; Raghavan, S.; Shrivastava, M. ESD Behavior of AlGaN/GaN Schottky Diodes. IEEE Trans. Device Mater. Reliab. 2019, 19, 437–444. [Google Scholar] [CrossRef]
  27. Zanoni, E.; Meneghini, M.; Chini, A.; Marcon, D.; Meneghesso, G. AlGaN/GaN-Based HEMTs Failure Physics and Reliability: Mechanisms Affecting Gate Edge and Schottky Junction. IEEE Trans. Electron Devices 2013, 60, 3119–3131. [Google Scholar] [CrossRef] [Scilit]
  28. Marcon, D.; Meneghesso, G.; Wu, T.-L.; Stoffels, S.; Meneghini, M.; Zanoni, E.; Decoutere, S. Reliability Analysis of Permanent Degradations on AlGaN/GaN HEMTs. IEEE Trans. Electron Devices 2013, 60, 3132–3141. [Google Scholar] [CrossRef] [Scilit]
  29. Chen, S.-H.; Griffoni, A.; Srivastava, P.; Linten, D.; Thijs, S.; Scholz, M.; Denis, M.; Gallerano, A.; Lafonteese, D.; Concannon, A.; et al. HBM ESD Robustness of GaN-on-Si Schottky Diodes. IEEE Trans. Device Mater. Reliab. 2012, 12, 589–598. [Google Scholar] [CrossRef] [Scilit]
  30. Lo, T.L.; Wong, S.; Alexander, P.H. Fast Fourier transform analysis of published ESD waveforms and narrowband frequency domain measurement of human ESD events. In Proceedings of the Electrical Overstress/Electrostatic Discharge Symposium, Santa Clara, CA, USA, 23–25 September 1997. [Google Scholar]
  31. Dawson, T.W.; Stuchly, M.A.; Kavet, R. Electric Fields in the Human Body Due to Electrostatic Discharges. IEEE Trans. Biomed. Eng. 2004, 51, 1460–1468. [Google Scholar] [CrossRef] [PubMed]
  32. Wu, C.-Y.; Rudko, M.; Chang, Y. On the Frequency Domain Specification of ESD Waveforms. J. Electrost. 1990, 24, 197–206. [Google Scholar] [CrossRef] [Scilit]
  33. He, Q.; Liu, S.; Chen, J. Study on frequency spectrum of Air Electrostatic Discharge. In Proceedings of the 2006 4th Asia-Pacific Conference on Environmental Electromagnetics, Dalian, China, 1–4 August 2006. [Google Scholar]
  34. Muhonen, K.; Dunnihoo, J.; Grund, E.; Peachey, N.; Brankov, A. Failure detection with HMM waveforms. In Proceedings of the 2009 31st EOS/ESD Symposium, Anaheim, CA, USA, 30 August–4 September 2009. [Google Scholar]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.