Skip to Content
MoleculesMolecules
  • Article
  • Open Access

15 March 2026

17 Pages

Temperature Evolution of Crystal Structure, Ferroelectricity and Ionic Conductivity of Ca9La(VO4)7

,
,
,
,
,
,
and
1
Faculty of Chemistry, MSU-BIT University, Shenzhen 518172, China
2
Department of Chemistry, Lomonosov Moscow State University, 119991 Moscow, Russia
3
Laboratory of Arctic Mineralogy and Material Sciences, Kola Science Centre, Russian Academy of Sciences, 14 Fersman Str., 184209 Apatity, Russia
*
Author to whom correspondence should be addressed.

Abstract

The properties of a Ca9La(VO4)7 single crystal were studied using dielectric spectroscopy and second-harmonic generation. The crystal structure of Ca9La(VO4)7 grown using the Czochralski technique was refined using single-crystal data. The distribution of Ca2+ and La3+ cations over structural positions was determined. The crystal structure refinement results were compared with those obtained previously from powder X-ray diffraction data. It was shown that the refinement carried out using two different data sets leads to approximately the same results for the distances in the polyhedra, but their distortion is significantly less in the case of using single-crystal data for calculation. Dielectric properties and conductivity measurements were performed on polished single-crystal wafers cut parallel and perpendicular to the c axis. Second-harmonic generation and dielectric temperature measurements revealed the presence of a reversible ferroelectric first-order phase transition at about 1224 K from the ferroelectric β-phase (space group R3c) to the paraelectric β′-phase. The ferroelectric–paraelectric phase transition is accompanied by a complex structural rearrangement, including a 60° rotation of the V1O4 tetrahedron, as well as slight displacements of the Ca2+ and La3+ cations. It has been shown that the conductivity differs only slightly along the polar axis and perpendicular to it. Above the phase transition temperature, the activation energy of the conductivity is the same for all directions, Ea~1.2 eV. The influence of composition on the phase transition temperature and the formation of ferroelectric and nonlinear optical properties is discussed.

1. Introduction

Phosphate and vanadate compounds crystallizing in the β-Ca3(PO4)2-type (β-TCP) structure (space group (SG) R3c, Z = 21) [1] are characterized by high chemical and thermal stability, as well as an appropriate band gap for optoelectronic applications. Among these, Ca3(VO4)2—which adopts a β-TCP-related structure (R3c, Z = 21; also reported as Ca10.5(VO4)7, Z = 6)—has been extensively employed as a host matrix for rare earth element (REE) cations to generate photoluminescence from REE3+ ions [2,3,4,5]. Depending on the specific REE ion (REE3+ or REE2+), these doped materials can generate emission across the visible [6,7,8,9] and near-infrared spectral regions [10,11]. Moreover, certain β-TCP-type vanadates lack a center of symmetry and demonstrate nonlinear optical properties [12,13,14], making them promising candidates for multifunctional materials through strategic cationic substitutions.
Among these, Ca9La(VO4)7 (CLVO) crystallizes in the β-TCP-type structure [15,16] and has been extensively investigated as a host for luminescent materials. Although the undoped CLVO matrix does not exhibit significant photoluminescence, it readily accommodates activator ions, particularly REE cations, into its crystal lattice. Numerous studies have characterized doped CLVO:REE, including its luminescence [6,8,9,17,18,19,20,21,22], laser performance [11,12,13,23,24], nonlinear optical behavior [12,13,14,23], thermal properties [25,26], spectral characteristics [13,21,22], refractive indices [27], ion-conducting properties [28,29], and Raman spectra [30,31]. Further motivation for investigating such vanadates is the possibility of growing them as large single crystals with excellent optical quality [10,11,12,13,23,25,32,33]. As follows from the analysis of the literature, CLVO activated by REE cations exhibits polyfunctional properties and is actively studied. However, data on the dielectric, nonlinear optical, and ion-conducting properties of CLVO are absent in the literature.
In this paper, we investigate the CLVO single crystal grown using the Czochralski method. The structure of CLVO is refined on single-crystal data, and dielectric, nonlinear optical, and ion-conducting properties are studied over a wide temperature range. It was demonstrated that CLVO single crystals combine ferroelectric behavior with nearly isotropic ionic conductivity, and fundamental insights into structure-property relationships in β-TCP-type materials are provided. Deeper structural confirmation of all these properties stimulates the development of new multifunctional materials based on CLVO and related compounds.

2. Results

2.1. SHG and DSC Study

Figure 1a shows the temperature dependences of the SHG signal (I2ω/I2ω(SiO2) upon heating/cooling of CLVO. The presence of the SHG response (I2ω/I2ω(SiO2) = ~40) at room temperature (TR) indicates the absence of a symmetry center in this structure, confirming the non-centrosymmetric structure with SG R3c. Upon heating, the signal regularly decreases and disappears above Curie temperature Tc ≈ 1220 K (Figure 1a), thus indicating the appearance of a symmetrical center in the CLVO structure. Upon cooling, the SHG signal is restored with a small temperature hysteresis. This behavior reveals a reversible phase transition: the structure shifts from non-centrosymmetric to centrosymmetric upon heating and reverts to the former upon cooling.
Figure 1. Temperature dependence of the SHG signal (a) and heating/cooling DSC curves (b) of Ca9La(VO4)7.
During a first-order phase transition, the SHG signal should change stepwise with temperature, as observed in Ca9Fe(PO4)7 [34]. However, CLVO shows a smoother change in the SHG signal when approaching Tc, both during heating and cooling (Figure 1). This smooth change indicates a gradual structural transition over a wide temperature range. The SHG signal probably decreases smoothly (heating) or increases smoothly (cooling) due to the smooth ordering (or disordering) of cations and tetrahedrons. The order/disorder in the structure is described in detail in the Section 3.
Figure 1b shows fragments of the DSC heating/cooling curves for CLVO. These curves exhibit two peaks in the temperature range of 1210–1250 K (heating) and 1200–1244 K (cooling). Two endothermic (Tc1 = 1226 K and Tc2 = 1243 K) and two exothermic (Tc1 = 1217 K and Tc2 = 1234 K) effects on the heating/cooling curves, respectively, indicate the presence of two reversible first-order phase transitions in CLVO. Similar peaks in the DTA curves at 1215 K and 1231 K were also previously observed for CLVO [29]. Two peaks in the DSC curves are apparently associated with a change in symmetry, R3c → R 3 ¯ c and R 3 ¯ c → R 3 ¯ m , as in Ca9Yb(VO4)7 [14]. Small values of the thermal effects of the phase transitions upon heating (Q = 5.65 kJ/mol) and cooling (Q = 6.67 kJ/mol) indicate an order–disorder transition in CLVO without a significant change in the chemical bond energy. Similar order–disorder phase transitions were discovered in the ferroelectrics LaBSiO5 and LaBGeO5, where Q ≈ 0.4–0.7 kJ/mol [35].

2.2. Dielectric Properties of Ca9La(VO4)7

To measure the dielectric properties, two polished crystalline wafers were prepared: one with a 53 mm2 (9.3 mm × 5.7 mm) area and 1.55 mm thickness (crystal no. 1, (║)) and one with a 47 mm2 area (7.1 mm × 6.6 mm) and 1.45 mm thickness (crystal no. 2, (┴)) (Figure 2).
Figure 2. Images of Ca9La(VO4)7 polished crystal wafers cut parallel (1—║) and perpendicular (2—┴) to the c axis.
Figure 3 shows the temperature dependence of the permittivity (ε) and the dielectric loss tangent (tgδ) for the CLVO crystal wafers. All ε(T) curves exhibited a maximum in the range of 1200–1250 K. The position of this maximum was independent of the applied electric field frequency and measurement direction (║ or ┴). The permittivity (ε) decreased with increasing electric field frequency. The CLVO crystal showed higher permittivity along the c axis (Figure 3).
Figure 3. Dielectric permittivity ε (top) and dielectric loss tangent tgδ (bottom) at frequencies of 30 (1), 50 (2), 100 (3), 300 (4) and 1000 kHz (5) for Ca9La(VO4)7 crystal wafers: 1 (a,c) and 2 (b,d).
The temperature position (Tc = 1224 K) of the maximum of peaks on the ε(T) curves approximately coincides with the phase transition temperature found using the SHG and DTA methods, which is Tc = 1215 K [29]. The behavior of the ε(T) curves near Tc obeys the Curie–Weiss law, confirming a ferroelectric (FE) nature of the phase transition. The tgδ(T) curves show a characteristic minimum (Figure 3), which relates to domain mobility near the phase transition temperature. As the system approaches the phase transition temperature, the domains disappear, reducing their contribution to the electrical conductivity. This disappearance creates a characteristic minimum in the tgδ(T) curve at Tc. Such a minimum is typical of FE phase transitions. In contrast, antiferroelectrics (AFE) of similar composition, which lack domains, do not exhibit this minimum [36]. These results confirm that CLVO undergoes a reversible FE phase transition at the Curie temperature Tc = 1224 K.
Cole–Cole diagrams of the complex impedance for single-crystal wafers at various temperatures are shown in Figure 4. The impedance diagram exhibits typical semicircles associated with bulk resistance. The impedance curves were used to calculate the temperature dependence of conductivity (σ), which is independent of crystal orientation (Figure 5).
Figure 4. Complex impedance curves of Ca9La(VO4)7 at temperatures of 900, 925, 950, 975 and 1000 K for Ca9La(VO4)7 crystal wafers: 1 (a) and 2 (b).
Figure 5. Temperature dependences of the conductivity calculated (1) from the impedance curves and the conductivity at frequencies of 100 Hz (2), 1 kHz (3), 10 kHz (4), 100 kHz (5) and 1 MHz (6) for Ca9La(VO4)7 crystal plates: 1 (a) and 2 (b).
Figure 5 shows the temperature dependence of conductivity in two crystal directions. The conductivity curves exhibit kinks, the temperature positions of which coincide with the maximum permittivity and the temperature at which the polar phase disappears in the SHG curves. The conductivity values along the two directions in the CLVO differ only slightly, indicating that ion transport in the structure is isotropic. Above the phase transition, the calculated activation energy of conductivity (Ea~1.2 eV) is the same for both crystal directions. Below the phase transition (around 1200 K), the activation energy differs only slightly between the two directions: Ea~1.8 eV for crystal wafer 1 and 1.6 eV for crystal wafer 2.

2.3. Crystal Structure of Ca9La(VO4)7 Based on Single-Crystal Data

A crystal (0.11 × 0.10 × 0.15 mm) of CLVO was used for single-crystal X-ray data collection. A total of 20,426 reflections within the sphere limited by θ = 30.56° were registered. The details of the experimental data collection process and refinement results are listed in Table 1.
Table 1. Crystallographic data for Ca9La(VO4)7.
The following trigonal lattice parameters were obtained by least-squares refinement: a = 10.9018(2) Å, c = 38.1593(6) Å, γ = 120°. In accordance with the analysis of systematic absence of reflections, there are two possible space groups, R 3 ¯ c and R3c, which differ in the presence/absence of the center of symmetry. Based on the SHG data and the |E2-1| statistics, we have suggested a non-centrosymmetric space group, R3c (which is traditional for the β-TCP-related structure). After averaging equivalent reflections, the experimental data set contained 1197 reflections with I > 3σ(I).
The initial model for CLVO structure refinement was based on the atomic coordinates of the same compound obtained using the Rietveld method [16]. There are six cationic (M1–M6) sites in β-TCP-related structures. The M1–M3 (18-fold) and M5 (6-fold) sites are always occupied, while the occupation of the M4 (6-fold) site can change from 0 to 1, and the M6 (6-fold) site is usually vacant. According to Belik et al. [16], the La3+ and Ca2+ cations occupy M1–M3, and only Ca2+ cations occupy M5 sites of the CLVO structure. The distribution of La3+ and Ca2+ cations over the M1–M3 sites was refined considering their multiplicities, (M1–M3) = nCa2+ + (1 – n)La3+), with stoichiometric constraints on the overall La/Ca ratio. The positional (x; y; z) parameters and atomic displacement parameters (ADP) of La3+ and Ca2+ cations over the M1–M3 sites were refined to be identical. The final refinement cycles converged with R1 = 1.78, wR2 = 1.84, and GOOF = 1.14 for all data. Analysis of the difference electron density map [ρdif: (x; y; z)] revealed the absence of additional peaks with noticeable intensity. The highest peak and the deepest minimum in the final residual electron density were equal to 0.32 e × Å3 and −0.61 e × Å3, respectively. Figure 6 illustrates difference electron density around the M4 site. As one can see, there is no noticeable electron density around the M4 and M5 sites. These data confirm the chemical composition of the single crystal as Ca9La(VO4)7, and its composition does not change during crystal growth and corresponds to the stoichiometry of the initial batch. These data are of practical importance because they allow the growth of single crystals of a given composition. During single-crystal growth, its stoichiometry could change due to a decrease in lanthanum content and charge compensation due to the incorporation of calcium cations into the M4 site. If stoichiometry is disrupted, the crystal composition will be described by the formula Ca9+2x/3La1−x(VO4)7. The properties of such a single crystal will differ significantly from the stoichiometric one (see the Section 3). As a result of the structure refinement, it was established that calcium and lanthanum cations statistically occupy the positions M1 = 0.94Ca2+ + 0.06La3+, M2 = 0.97Ca2+ + 0.03La3+ and M3 = 0.76Ca2+ + 0.24La3+ (Figure 7a, Table S1 of the Supplementary Materials). The M5 position is occupied by calcium cations. The high quality of the obtained results and the absence of correlation between pseudo-symmetrical sites confirm the correct choice of the noncentrosymmetric SG.
Figure 6. The difference electron density map around the M4 and M5 positions of the Ca9La(VO4)7 crystal structure. Solid lines indicate positive electron density and dashed lines indicate negative electron density. M4 position is shown in the green ellipse. Contour intervals are 0.05 e × Å3. A color scale for the positive electron density is shown.
Figure 7. General view of the structure of Ca9La(VO4)7 (a), L1-layer (b) and L2-layer (c).
Table S1 of the Supplementary Materials lists the fractional atomic coordinates, occupancy, site symmetry, and equivalent atomic displacement parameters. Anisotropic atomic displacement parameters are given in Table S2 of the Supplementary Materials. Selected inter-atomic distances and angles in VO43− tetrahedra are given in Table S3 of the Supplementary Materials. The CSD deposition number is 2524264.

3. Discussion

Figure 7a shows the general view of the CLVO structure. The structure is constructed from two types of columns elongated along the c-axis. The first column sequentially alternates between tetrahedrons and occupied and unoccupied polyhedra: …-V1O4-M4O15-M5O6-M6O13-.… (Figure 7a). The M4O15 and M6O13 polyhedra in the CLVO structure are unoccupied, and the M5O6 polyhedron is occupied by calcium cations. The second column is constructed from tetrahedra and MO8 polyhedra: …-V2O4-V3O4-M1O8-M3O8-M2O8-… The M1, M2, and M3 positions are occupied by calcium and lanthanum cations (Figure 7a). VO43− tetrahedra link MOn polyhedra into a 3D framework. The 3D framework consists of 12 layers of two types formed by M3O8 + M5O6 + V2O4 + V3O4-polyhedra (L1-layer) and M1O8 + M2O8 + V1O4-polyhedra (L2-layer) alternating along the [001] direction (Figure 7b,c). The L1-layer contains M3O8 and M5O6 polyhedra, which are linked by V2O4 and V3O4 tetrahedra (Figure 7b). The six-membered cavities in the L1-layer are formed by the edge of the three M3O8 and three VO4 tetrahedra (Figure 7b), while M4 or M6 sites (do not occupy in the CLVO structure) are located in these cavities. The M3O9 polyhedra, linked by common edges, form the [M33O22] cluster, and adjacent clusters are linked by the VO4 tetrahedra edge. The O1 atom is shared by the three M3O9 polyhedra forming the [M33O22] cluster. The L2-layer contains M1O8 and M2O8 polyhedra, which form a six-membered ring. The center of each ring is occupied by V1O4 tetrahedra (Figure 7c).
The CLVO structure was previously refined using PXRD data [16]. Table 2 lists the comparison of the CLVO structure refined from single-crystal and PXRD data. The lattice parameters and cation site occupancies differ slightly between the two refinements. The average M1-O, M2-O, M3-O and M5-O remain virtually unchanged. The difference between two refinements is observed for the polyhedra distortion index and tetrahedral distortion parameters. The following formula was used to estimate the polyhedra distortion index (DI):
D I =   1 n ∑ i = 1 n l i − l a v l a v ,
where n is the coordination number of central cation, li is the distance from the central cation to the O atom and lav is the average bond length. The calculated DI values are presented in Table 2.
Table 2. Comparison of the lattice parameters, cation site occupancies, selected distances (Å), polyhedra distortion index (DI) and tetrahedral distortion parameters ∆d and ∆α for Ca9La(VO4)7 structure refined from single-crystal and powder data.
In the CLVO structure, the V-O bonds are the strongest. Cations with different charges and sizes within the structure distort the VO43− tetrahedra. The distortion of the tetrahedra is associated with the stretching of the V-O bonds or the bending of the O-V-O bond angles. The distortions of the VO43− tetrahedra were estimated by the change in the distance Δd and the deformation Δα, which characterize the deviations of the V-O distances from the average value and the deviations of the O-V-O angles from the ideal tetrahedral angle (109.5°) (Table 2). The distortion parameters of the VO4 tetrahedra were estimated as follows:
∆ d = 1 4 ∑ n = 1 − 4 d n − d d 2 ,   ∆ α = 1 6 ∑ n = 1 − 6 α n − α α 2 ,
where dn is the individual V-O bond length, d is the average V-O bond length, αn is the individual O-V-O bond angle and α is the perfect tetrahedral angle of 109.5°.
According to Table 2, the DI for the M2O8 and M3O8 polyhedra differ slightly between the two refinements, while the difference for the M1O8 polyhedra is more noticeable (approximately 1.4 times). The DI value for M5O6 calculated from the refinement of the single-crystal data is approximately 4.5 times smaller than the one calculated from the PXRD data. The tetrahedral distortion parameters Δd and Δα show a different trend. The Δd for all VO4 and the Δα for the V1O4 and V2O4 tetrahedra are significantly smaller for the single-crystal data refinement, while the Δα for the V3O4 tetrahedron is the same. Thus, the refinement carried out using two different data leads to approximately the same results for the distances in O polyhedra, but their distortion is significantly less in the case of using single-crystal data for the calculation.
For a CLVO single crystal, the calculated σ value at 1200 K does not demonstrate anisotropy and differs slightly along the two directions: (σ = 0.13 × 10−3 S/cm for crystal wafer 1 and σ = 0.097 × 10−3 S/cm for crystal wafer 2) (Figure 5). The σ value for CLVO is lower than for Ca9Bi(VO4)7 ceramics (σbulk = 0.86 × 10−3 S/cm at 1200 K) [37]. The activation energy (Ea) for the conductivity above the phase transition is the same for both directions (Ea~1.2 eV). The conductivity in the framework of the CLVO structure results from the mobility of Ca2+ cations. Using the diffusion labeling method with the radioactive isotope 45Ca2+ (R = Eu3+) [38] and Tubandt method (R = La3+) [28], it has been shown that the conductivity in Ca10.5–1.5xRx(VO4)7 (R = La3+, Eu3+) solid solutions is provided by Ca2+ cations (rVIII = 1.12 Å [39]). Larger cations, such as Pb2+ (rVIII = 1.29 Å [39]), can also move in the β-TCP-type structure [40]. The β-TCP-type structure includes a 3D migration network for cations and is characterized by the 3D nature of ionic conductivity in accordance with bond valence energy landscape (BVEL) analysis [41]. The β-TCP-related framework contains three conductivity pathways; Ca2+ or Pb2+ cations can migrate along all pathways through the common faces of polyhedra or between faces of neighboring polyhedra. The M4 sites are involved in all pathways [40,41].
According to crystal structure refinement, the M5O6 octahedra in CLVO are occupied by Ca2+, while Ca2+ and La3+ cations occupy M1–M3 sites. The M4 and M6 sites are vacant. The occupancy of the M4 site in the β-TCP-related compounds can vary from 0 to 1. For example, the M4 site is half occupied by Ca2+ in the Ca3(VO4)2 structure [42], while it is completely occupied by K+ in Ca10K(VO4)7 [43]. The M6 site is always vacant in all known compounds with the β-TCP-type structure. Thus, the M4 and M6 sites are not structure-forming in comparison to the M1-M3 and M5 sites. However, they play an important role in the ferroelectric–paraelectric (FE-PE) phase transition [41] and take part in the ionic mobility of cations [40,41] within the β-TCP-type framework.
The crystal structure Ca9Fe(PO4)7 [34] were studied at 300 K (ferroelectric phase) and 973 K (paraelectric phase). Experimental data on the structures of the paraelectric phase of Ca9R(PO4)7 (R = Fe, In) were used to describe the structure of the paraelectric phase of CLVO. In the ferroelectric phase of CLVO, all V1O4 tetrahedra are oriented along the three-fold axis in the same direction (Figure 8, left). This orientation of V1O4 tetrahedra makes up the main contribution to the formation of the polar direction. Analysis of the CLVO structure showed cations in the M1 and M2 positions, and V2O4 and V3O4 tetrahedra deviate only slightly from the centrosymmetric arrangement, as in Ca9Fe(PO4)7 [34]. In CLVO, the M3 position is located close to the center of symmetry. Apparently, for this reason, the contribution of the cations in the M1, M2 and M3 positions and the V2O4 and V3O4 tetrahedra to the formation of the polar direction is much smaller than that of the V1O4 tetrahedra. During the ferroelectric ↔ parelectric transition or vice versa, the cations in the M1, M2, and M3 positions and the V2O4 and V3O4 tetrahedra should only shift slightly and become ordered upon heating or shift and become disordered upon cooling. Apparently, such small displacements are accompanied by an insignificant change in the SHG signal in the temperature range of 600–1100 K (Figure 1a). Since all V1O4 tetrahedra in the FE phase are oriented in the same direction, the transition to the PE phase should be accompanied by a rotation of half of the V1O4 tetrahedra, forming the opposite orientation. For the transition from the FE phase to the PE phase, it is sufficient for the V1O4 tetrahedra to rotate by 60° (Figure 8).
Figure 8. Alternation of VO4 tetrahedra, M5O6 octahedra, M4 and M6 sites polyhedra in the ferroelectric (left, SG R3c, cell parameter c doubled) and paraelectric (right, SG R 3 ¯ ) phases of the Ca9La(VO4)7 structure.
This rotation results in neighboring V1O4 tetrahedra on the 3-fold axis being linked by a center of symmetry (at the M5 site). This tetrahedron rotation is accompanied by a very small change in the thermal effect: Q~6.0 kJ/mol. After this rotation, three O2 oxygen atoms remain in their original positions, while half of the O1 oxygen atoms on the 3-fold axis move to another location (Figure 8). During the FE-PE phase transition, half of the M4 sites transform into M6 sites and vice versa (Figure 8).
X-ray diffraction cannot detect these structural changes [44] because the main difference is the repositioning of some O1 oxygen atoms along the 3-fold axis. Consequently, many studies have misdetermined the symmetry [45,46] of compounds with the β-TCP-type structure. Only the SHG method or dielectric spectroscopy can unambiguously determine whether compounds are centrosymmetric or non-centrosymmetric.
Near the phase transition temperature, when the V1O4 tetrahedron rotates, the SHG response drops sharply. This sharp drop occurs when half of the V1O4 tetrahedron rotates (Figure 8). It should also be noted that in CLVO, the M1 and M2 positions are unequally occupied by La3+ cations (Figure 7). For this reason, near the phase transition temperature, some La3+ cations must transform from the M1 position to the M2 position.
This transition equalizes the occupancies of these sites with Ca2+ or La3+ cations. In cases where the M1 and M2 positions are occupied by the same cations, the SHG signal value changes sharply only at the phase transition temperature, for example, Ca9Fe(PO4)7 [34].
At the TR temperature, both centrosymmetric and non-centrosymmetric phases with a β-TCP-type structure exist [36,44]. Depending on the cation composition, the structure exhibits either FE [14,34,37] or AFE [36] properties. These properties are more characteristic of phosphates. However, vanadium-based compounds are always non-centrosymmetric at TR and transform into a centrosymmetric state as temperature increases. The centrosymmetric state appears at the TR temperature only when some vanadium cations are replaced by phosphorus [47].
In CLVO, as in other isostructural compounds, the V1O1(O2)3 tetrahedra are strongly bonded to neighboring Ca2+ or La3+ cations located at the M1-M3 sites at distances of 2.524 Ǻ (M1-O2), 2.392 Ǻ (M2-O2), 2.921 Ǻ (M3-O2), and 2.575 Ǻ (3M3-O1) (Figure 9 and Table S3 of the Supplementary Materials). Each O2 oxygen atom is bonded to three cations in the M1, M2 and M3 sites, while the O1 oxygen atom binds three cations at the M3 site (Figure 7b). However, with increasing temperature, the M-O bonds break, and the V1O4 tetrahedra rotate by 60° (Figure 9). The phase transition temperature varies widely depending on cations present in the structure. Among the vanadates, Ca3(VO4)2 exhibits the highest FE-PE phase transition temperature (Tc = 1383 K) [48], while Ca6Pb4.5(VO4)7 shows the lowest one (Tc = 770 K) [42]. Phosphates consistently have lower phase transition temperatures than similar vanadates [49]. The M4 site occupancy significantly affects the phase transition temperature. When a cation occupies the M4 site, it hinders the rotation of the V1O4 tetrahedra (Figure 7). When Ca2+ is replaced by La3+ in CLVO according to the scheme 3Ca2+ = 2La3+ + ☐, vacancies form in the M4 site, and the phase transition temperature decreases significantly to Tc = 1224 K (ΔT = 159 degrees).
Figure 9. The surrounding of the V1O4 tetrahedra by positions M1, M2 and M3 in the Ca9La(VO4)7 structure: projections along (a) and perpendicular (b) the three-fold axis.
The occupancy of the M4 site significantly affects the laser characteristics of vanadate single crystals with the β-TCP structure. Single crystals with an unoccupied M4 position, such as Ca9La(VO4)7 [12,13], Ca9Yb(VO4)7 [14], and Ca9La(VO4)7:Nd3+ [23], exhibit noticeable scattering of laser radiation. In contrast, for single crystals with an occupied M4 position, for example, Nd:Ca8.53K1.09La0.95(VO4)7 [12] and Nd:Ca9.03Na1.08La0.62(VO4)7 [13], scattering is not observed. The scattering of laser radiation is associated with the formation of a domain structure, which is found in Ca9La(VO4)7 [50] (the M4 position is unoccupied) and not found in Ca10Li(VO4)7 [50] (the M4 position is occupied).
CLVO single crystals were grown at temperatures above 1773 K, which is significantly higher than the FE-PE phase transition temperature (Tc = 1224 K). During crystal growth, a centrosymmetric structure (SG R 3 ¯ c or R 3 ¯ m) forms. Upon cooling to Tc = 1224 K, a transition to a non-centrosymmetric (SG R3c) structure occurs. As shown above, this transformation involves the rotation of half of the V1O4 tetrahedra. In the CLVO structure, the empty M4 site imposes no restrictions on tetrahedron rotation in different parts of the crystal. Consequently, numerous domains form, scattering laser radiation. In Nd:Ca8.53K1.09La0.95(VO4)7 [12] and Nd:Ca9.03Na1.08La0.62(VO4)7 [13] single crystals, the M4 site is completely occupied by alkali metal cations. At TR temperature, these phases crystallize in a trigonal non-centrosymmetric SG R3c [12,13]. Apparently, when single crystals with an occupied M4 site form at high temperatures, a non-centrosymmetric structure develops that remains stable upon cooling. No additional domains form, and therefore, these crystals do not scatter laser radiation.
CLVO serves as a versatile matrix for incorporating various rare earth elements and other cations. Vacancies in its structure enable both isovalent substitutions—replacing lanthanum with other rare earth elements or calcium with strontium or barium—and heterovalent substitutions (2Ca2+ = RE3+ + Me+), creating compounds with multifunctional properties. By introducing Nd3+, Er3+, Yb3+ or other cations into the CLVO lattice, it is possible to create self-frequency-doubling laser materials that operate in various spectral regions [12,13,14,23].

4. Materials and Methods

Experimental Details

A CLVO single-crystal boule was grown using the Czochralski method. The Czochralski growth conditions were described previously [32].
Powder X-ray diffraction (PXRD) data for the milled CLVO single crystal were obtained on a Thermo ARL X’TRA powder diffractometer (Waltham, MA, USA, CuKα radiation, λ = 1.5418 Å, Bragg–Brentano geometry, scintillation detector). PXRD data were collected in the 2θ range from 5 to 60° with a resolution of 0.02°. The X-ray diffraction pattern of the milled single-crystal matched literature data is given in the ICDD powder database (PDF2 46-0430). All reflections in the CLVO X-ray diffraction patterns are indexed in the R3c space group (SG), which is standard for the β-TCP-type structure.
The single-crystal X-ray data for CLVO were collected at room temperature (TR) on a Rigaku XtaLAB Synergy-S diffractometer (Akishima-shi, Japan) with MoKα radiation (λ = 0.71073 Å) and a Hyrid Pixel Array detector using the ω-θ scanning mode. A colorless crystal (0.11 × 0.10 × 0.15 mm) of CLVO was used for single-crystal X-ray data collection. A total of 20,426 reflections found within the range of 3.73 ≤ θ ≤ 30.56°, and −12 ≤ h ≤ 15; −14 ≤ k ≤ 13; and −50 ≤ l ≤ 54 were measured. The initial model for CLVO structure refinement was based on the atomic coordinates of the same compound obtained using the Rietveld method [16]. CLVO structure refinement was carried out using the JANA2006 program packages [51]. Illustrations were produced with the JANA2006 program packages in combination with the DIAMOND program [52].
A Tescan VEGA3 scanning electron microscope (TESCAN, a.s., Brno, Czech Republic) was used to determine the chemical composition of CLVO by energy-dispersive X-ray (SEM-EDX) analysis. The CaK, VK and LaL lines in the EDX spectra were used. The oxygen and phosphorus contents were not quantified by EDX. The elemental composition of the CLVO single crystal corresponded to the specified stoichiometry (wt. %), theoretical/experimental: Ca(42.1/42.9 ± 0.5), La(16.2/16.5 ± 0.3), and V(41.6/40.5 ± 0.5).
The second optical harmonic generation study was carried out for the synthesized ceramic powders using the “reflection” scheme [53] on particles sized 400–500 µm. The SHG at the wavelength of λω = 532 nm was excited by a Minilite-I YAG (Amplitude Laser Inc., Santa Clara, CA, USA): Nd-laser operating in a Q-switched mode at λω = 1064 nm and registered in the reflection geometry. Polycrystalline α-SiO2 with 3–5 µm sized particles was used as a standard in order to calibrate the intensity of the SHG response I2ω according to the q = I2ω/I2ω(SiO2) relationship. The part of the CLVO single crystal was previously milled into 3–5 µm powder for the sake of comparability with the reference α-SiO2 sample.
The SDT Q600 V8.1 thermal analyzer Build 99 (TA Instruments, New Castle, DE, USA) was used to perform differential scanning calorimetry (DSC). The studies were carried out in Pt crucibles in air at temperatures of 303–1300 K with a heating/cooling rate of 10 degrees/min.
The dielectric properties in the heating/cooling mode were measured on a Novocontrol Beta-N (Montabaur, Germany) setup with a “ProboStat” measurement cell using a four-wire two-contact method in the frequency range of 10–1 × 106 Hz at 280–1300 K in air. The frequency dependences of the complex impedance Z*(ω) = Z’(ω) + iZ’’(ω) were measured during step heating under temperature stabilization conditions (the average heating rate was 2 K/min). The dielectric property measurements were performed on polished crystal wafers cut parallel (║) and perpendicular (┴) to the c axis (Figure 2). A gold paste was put on the flat parallel surfaces of the crystal wafer. After applying the paste, the sample was kept in a drying oven at 400 K for 20 min to dry. Additional annealing at 1025 ± 25 K for 1 h in air was performed to ensure good electrical contact between the sample and Au electrodes thus formed. Electrical conductivity (σ) was calculated from impedance spectra by means of equivalent electric circuits.

5. Conclusions

The crystal structure of CLVO grown using the Czochralski technique was refined using single-crystal data, and dielectric, nonlinear optical, and ion-conducting properties were studied. The distribution of Ca2+ and La3+ cations over structural sites was established and compared with the one refined previously using powder X-ray diffraction (PXRD) data. Dielectric spectroscopy and second-harmonic generation (SHG) methods revealed a reversible first-order ferroelectric phase transition at Tc = 1224 K on heating and 1215 K on cooling. This ferroelectric–paraelectric phase transition involves a complex structural rearrangement, including a 60° rotation of the V1O4 tetrahedron and minor displacements of calcium and lanthanum cations. The conductivity varies little across different crystal directions. The activation energy for conductivity above the phase transition is Ea~1.2 eV for all directions. The influence of composition on the phase transition temperature, laser scattering, and the formation of ferroelectric and nonlinear optical properties is discussed. The causes of laser scattering in a CLVO single crystal activated with Nd3+, Er3+, and Yb3+ cations are substantiated.

Supplementary Materials

The following supporting information can be downloaded at https://www.mdpi.com/article/10.3390/molecules31060984/s1, Table S1: Fractional atomic coordinates and isotropic atomic displacement parameters (Uiso) for Ca9La(VO4)7; Table S2: Anisotropic atomic displacement parameters in Ca9La(VO4)7; Table S3: Selected interatomic distances (Å) and angles in the [VO4]3− tetrahedra for Ca9La(VO4)7.

Author Contributions

Conceptualization, B.I.L. and S.Y.S.; methodology, V.A.M.; software, E.M.G.; validation, S.M.A., A.V.M. and D.V.D.; formal analysis, E.M.G.; investigation, S.M.A. and A.V.M.; resources, D.V.D. and B.I.L.; data curation, O.V.B. and S.M.A.; writing—original draft preparation, V.A.M. and S.M.A.; writing—review and editing, B.I.L., S.Y.S., D.V.D. and V.A.M.; visualization, V.A.M.; supervision, B.I.L.; project administration, B.I.L.; funding acquisition, B.I.L. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by the Russian Science Foundation (RSF Project 24-13-00148), available online at https://rscf.ru/en/project/24-13-00148/ (accessed on 8 May 2024).

Institutional Review Board Statement

Not applicable.

Data Availability Statement

The research data are available upon official, reasonable request.

Conflicts of Interest

The authors declare no conflicts of interest.

References

  1. Yashima, M.; Sakai, A.; Kamiyama, T.; Hoshikawa, A. Crystal structure analysis of β-tricalcium phosphate Ca3(PO4)2 by neutron powder diffraction. J. Solid State Chem. 2003, 175, 272–277. [Google Scholar] [CrossRef] [Scilit]
  2. Kim, K.Y.; Yoon, S.J.; Park, K. Synthesis and photoluminescence properties of red-emitting Ca3−3x/2(VO4)2:xEu3+ phosphors. J. Lumin. 2015, 160, 78–84. [Google Scholar] [CrossRef] [Scilit]
  3. Chauhan, V.; Pandey, P.K.; Dixit, P.; Pandey, P.C. Structural and optical of Sm3+ doped Ca3(VO4)2 phosphors. Mater. Today Proc. 2022, 67, 605–608. [Google Scholar] [CrossRef] [Scilit]
  4. Singh, V.; Bhat, A.A.; Radha, M.; Seshadri, M.; Nandyalad, S.H.; Joo, J.B. Investigation on structure and photoluminescence properties of Ho3+ doped Ca3(VO4)2 phosphors for luminescent devices. RSC Adv. 2024, 14, 18777. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  5. Zhang, H.; Li, M.; Xiu, Z.; Wang, S.; Zhou, G.; Zhou, Y.; Wang, S.; Qiu, Z.; Zhang, A. Synthesis and photoluminescence properties of a new red emitting phosphor: Ca3(VO4)2:Eu3+; Mn2+. Mater. Res. Bull. 2007, 42, 1145–1152. [Google Scholar] [CrossRef] [Scilit]
  6. Solanki, D.; Devi, P.; Dalal, H.; Sehrawat, N.; Kumar, M.; Garg, O.; Malik, R.K. Intense red emission from trivalent Eu3+ doped Ca9La(VO4)7 nanophosphor for lighting and latent fingerprinting applications. Indian J. Phys. 2024, 99, 1867–1879. [Google Scholar] [CrossRef] [Scilit]
  7. Zhang, C.; Yao, C. Synthesis and luminescence enhancement of white-emitting Ca9La(VO4)7:Dy3+ phosphors through Gd3+ and Al3+ codoping for white-light-emitting diodes. Ceram. Int. 2023, 49, 13000–13010. [Google Scholar] [CrossRef] [Scilit]
  8. Dai, M.; Qiu, K.; Zhang, P.; Zhang, W. Synthesis and luminescence properties of orange–red-emitting Ca9La(VO4)7:Sm3+ phosphors co-doped with alkali metal ions. J. Mater. Sci. Mater. Electron. 2019, 30, 9184–9193. [Google Scholar] [CrossRef] [Scilit]
  9. Yang, P.; Tian, L.-H.; Tian, R. Photoluminescence properties of Ca9R(VO4)7 (R = Y, La, Gd) phosphors activated with Eu3+ ions. Chin. J. Lumin. 2009, 30, 768–772. [Google Scholar]
  10. Hu, P.N.; Wang, G. Growth and spectral properties of Er3+:Ca9La(VO4)7 crystal. Mater. Res. Innov. 2011, 15, 75–77. [Google Scholar] [CrossRef] [Scilit]
  11. Li, M.; Sun, S.; Zhang, L.; Yuan, F.; Huang, Y.; Lin, Z. Growth and Spectral Properties of a Promising Laser Crystal Yb3+/Er3+:Ca9La(VO4)7. J. Cryst. Growth 2016, 451, 52–56. [Google Scholar] [CrossRef] [Scilit]
  12. Hu, X.; Chen, X.; Zhuang, N.F.; Wang, R.F.; Chen, J.Z. Growth, nonlinear frequency-doubling and spectral properties of Nd:Ca8.53K1.09La0.95(VO4)7 crystal. J. Cryst. Growth 2008, 310, 5423–5427. [Google Scholar] [CrossRef] [Scilit]
  13. Chen, X.; Zhuang, N.F.; Hu, X.; Zhuang, F.J.; Chen, J.Z. Growth and spectral properties of self-frequency doubling crystal, Nd:Ca9.03Na1.08La0.62(VO4)7. Appl. Phys. B 2007, 88, 449–455. [Google Scholar] [CrossRef] [Scilit]
  14. Lazoryak, B.I.; Aksenov, S.M.; Stefanovich, S.Y.; Dorbakov, N.G.; Belov, D.A.; Baryshnikova, O.V.; Morozov, V.A.; Manylov, M.S.; Lin, Z. Ferroelectric crystal Ca9Yb(VO4)7 in the series of Ca9R(VO4)7 non-linear optical materials (R = REE, Bi, Y). J. Mater. Chem. C 2017, 5, 2301–2310. [Google Scholar] [CrossRef] [Scilit]
  15. Evans, J.S.O.; Huang, J.; Sleight, A.W. Synthesis and structure of ACa9(VO4)7 compounds, A = Bi or a rare earth. J. Solid State Chem. 2001, 157, 255. [Google Scholar] [CrossRef] [Scilit]
  16. Belik, A.A.; Morozov, V.A.; Khasanov, S.S.; Lazoryak, B.I. Crystal Structures of Double Vanadates Ca9R(VO4)7: I. R = La, Pr, and Eu. Crystallogr. Rep. 1997, 42, 751–757. [Google Scholar]
  17. Liu, L.; Xie, R.-J.; Hirosaki, N.; Li, Y.; Takeda, T.; Zhang, C.-N.; Li, J.; Sun, X. Crystal Structure and Photoluminescence Properties of Red-Emitting Ca9La1-x(VO4)7:xEu3+ Phosphors for White Light-Emitting Diodes. J. Am. Ceram. Soc. 2010, 93, 4081–4086. [Google Scholar] [CrossRef] [Scilit]
  18. Hu, Z.; Meng, T.; Zhang, W.; Cui, Y.-P.; Lou, L.; Wang, Y.-H. Preparation and Luminescence Properties of Dy3+-Doped Full-Color Emitting Ca9La(PO4)7 Phosphors. Acta Phys.-Chim. Sin. 2013, 29, 2271–2275. [Google Scholar]
  19. Zhao, J.; Guo, C.; Bu, J.; Yu, R. Spectroscopy properties of Eu3+ doped Ca9R(VO4)7 (R = Bi, La, Gd and Y) phosphors by sol–gel method. Opt. Laser Technol. 2013, 45, 62–68. [Google Scholar] [CrossRef] [Scilit]
  20. Li, L.; Liu, X.G.; Noh, H.M.; Jeong, J.H. Chemical bond parameters and photoluminescence of a natural-white-light Ca9La(VO4)7:Tm3+,Eu3+ with one O2-→V5+ charge transfer and dual f-f transition emission centers. J. Solid State Chem. 2015, 221, 95–101. [Google Scholar] [CrossRef] [Scilit]
  21. Liang, Z.; Mu, Z.; Wang, Q.; Zhu, D.; Wu, F. The synthesis and luminescence properties of a novel red-emitting phosphor: Eu3+-doped Ca9La(PO4)7. Appl. Phys. A 2017, 123, 612. [Google Scholar] [CrossRef] [Scilit]
  22. Dai, M.; Qiu, K.; Zhang, Q.; Tang, W. Synthesis and photoluminescence enhancement of Ca9La(VO4)7:Eu3+ red phosphors by Mg2+ co-doping for white LEDs. J. Mater. Sci. Mater. Electron. 2018, 29, 15052–15059. [Google Scholar] [CrossRef] [Scilit]
  23. Zhuang, N.; Liu, X.; Xu, Q.; Chen, X.; Zhao, B.; Hu, X.; Chen, J. Crystal Growth, Nonlinear Frequency-Doubling and Spectral Characteristic of Nd:Ca9La(VO4)7 Crystal. J. Alloys Compnd. 2014, 595, 113–119. [Google Scholar] [CrossRef] [Scilit]
  24. Demesh, M.P.; Yasukevich, A.S.; Kuleshov, N.V.; Kosmyna, M.B.; Mateychenko, P.V.; Nazarenko, B.P.; Shekhovtsov, A.N.; Kornienko, A.A.; Dunina, E.B.; Orlovich, V.A.; et al. Growth and spectroscopic properties of Ca9Nd(VO4)7 single crystal. Opt. Mater. 2016, 60, 387–393. [Google Scholar] [CrossRef] [Scilit]
  25. Loiko, P.A.; Yasukevich, A.S.; Gulevich, A.E.; Demesh, M.P.; Kosmyna, M.B.; Nazarenko, B.P.; Puzikov, V.M.; Shekhovtsov, A.N.; Kornienko, A.A.; Dunina, E.B.; et al. Growth, spectroscopic and thermal properties of Nd-doped disordered Ca9(La/Y)(VO4)7 and Ca10(Li/K)(VO4)7 crystals. J. Lumin. 2013, 137, 252–258. [Google Scholar] [CrossRef] [Scilit]
  26. Popov, P.A.; Skrobov, S.A.; Matovnikov, A.V.; Kosmyna, M.B.; Puzikov, V.M.; Nazarenko, B.P.; Shekhovtsov, A.N.; Behrooz, A.; Paszkowicz, W.; Khodasevich, I.A.; et al. Thermal Conductivity Investigation of Ca9RE(VO4)7 (RE = La, Nd, Gd) and Ca10M(VO4)7 (M = Li, Na, K) Single Crystals. Int. J. Thermophys. 2017, 38, 10. [Google Scholar] [CrossRef] [Scilit]
  27. Lingxiong, H.; Naifeng, Z.; Ge, Z.; Jianzhong, C.; Chenghui, H.; Bin, Z.; Yong, W.; Xiaolin, H.; Min, W. Accurate measurement of refractive indices of Ca9La(VO4)7 crystal. Opt. Mater. 2008, 31, 372–374. [Google Scholar] [CrossRef] [Scilit]
  28. Leonidov, I.A.; Leonidova, O.N.; Surat, L.L.; Samigullina, R.F. Ca3(VO4)2–LaVO4 Cation Conductors. Inorg. Mater. 2003, 39, 616–620. [Google Scholar] [CrossRef] [Scilit]
  29. Leonidov, I.A.; Surat, L.L.; Leonidova, O.N.; Samigullina, R.F. System Ca3(VO4)2–Na3VO4–LaVO4. Russ. J. Inorg. Chem. 2003, 48, 1720–1724. [Google Scholar]
  30. Kosyl, K.M.; Paszkowicz, W.; Ermakova, O.; Wlodarczyk, D.; Suchocki, A.; Minikayev, R.; Domagala, J.Z.; Shekhovtsov, A.N.; Kosmyna, M.; Popescu, C.; et al. Equation of State and Amorphization of Ca9R(VO4)7 (R = La, Nd, Gd): A Combined High-Pressure X ray Diffraction and Raman Spectroscopy Study. Inorg. Chem. 2018, 57, 13115−13127. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  31. Khodasevich, I.A.; Voitikov, S.V.; Orlovich, V.A.; Kosmyna, M.B.; Shekhovtsov, A.N. Raman Spectra of Crystalline Double Calcium Orthovanadates Ca10M(VO4)7 (M = Li, K, Na) and their Interpretation Based on Deconvolution into Voigt Profiles. J. Appl. Spectrosc. 2016, 83, 555–561. [Google Scholar] [CrossRef] [Scilit]
  32. Dobrotvorskaya, M.V.; Gorobets, Y.N.; Kosmyna, M.B.; Mateichenko, P.V.; Nazarenko, B.P.; Puzikov, V.M.; Shekhovtsov, A.N. Growth and Characterization of Ca9Ln(VO4)7 Crystals (Ln = Y, La, or Gd). Crystallogr. Rep. 2012, 57, 959–961. [Google Scholar] [CrossRef] [Scilit]
  33. Zhang, Z.; Loiko, P.; Wu, H.; Mateos, X.; Serres, J.M.; Lin, H.F.; Chen, W.D.; Zhang, G.; Zhang, L.Z.; Díaz, F.; et al. Disordered Tm:Ca9La(VO4)7: A novel crystal with potential for broadband tunable lasing. Opt. Mater. Express 2017, 7, 487. [Google Scholar] [CrossRef] [Scilit]
  34. Lazoryak, B.I.; Morozov, V.A.; Belik, A.A.; Stefanovich, S.Y.; Grebenev, V.V.; Leonidov, I.A.; Mitberg, E.B.; Davydov, S.A.; Lebedev, O.I.; Van Tendeloo, G. Ferroelectric phase transition in the whitlockite-type Ca9Fe(PO4)7; crystal structure of the paraelectric phase at 923K. Solid State Sci. 2004, 6, 185–195. [Google Scholar] [CrossRef] [Scilit]
  35. Strukov, B.A.; Onodera, A.; Ragula, E.P.; Stefanovich, S.Y.; Shnaidshtein, I.V.; Arkhangel’skya, S.V. Ferroelectric Phase Transition in LaBSiO5 Crystals from Results of Thermal and Dielectric Measurements. Phys. Solid State 1998, 40, 1193–1195. [Google Scholar] [CrossRef] [Scilit]
  36. Belik, A.A.; Morozov, V.A.; Deyneko, D.V.; Savon, A.E.; Baryshnikova, O.V.; Zhukovskaya, E.S.; Dorbakov, N.G.; Katsuya, Y.; Tanaka, M.; Stefanovich, S.Y.; et al. Antiferroelectric properties and site occupations of R3+ cations in Ca8MgR(PO4)7 luminescent host materials. J. Alloys Compd. 2017, 699, 928–937. [Google Scholar] [CrossRef] [Scilit]
  37. Lazoryak, B.I.; Baryshnikova, O.V.; Stefanovich, S.Y.; Malakho, A.P.; Morozov, V.A.; Belik, A.A.; Leonidov, I.A.; Leonidova, O.N.; Van Tendeloo, G. Ferroelectric and Ionic-Conductive Properties of Nonlinear-Optical Vanadate, Ca9Bi(VO4)7. Chem. Mater. 2003, 15, 3003–3010. [Google Scholar] [CrossRef] [Scilit]
  38. Leonidov, I.A.; Khodos, M.Y.; Fotiev, A.A.; Zhukovskaya, A.S. Effect of vacancies on 45Ca diffusion in the solid solutions Ca3(1-x)Eu2x(VO4)2. Inorg. Mater. 1988, 24, 280–281. [Google Scholar]
  39. Shannon, R.D. Revised effective ionic-radii and systematic studies of interatomic distances in halides and chalcogenides. Acta Crystallogr. 1976, 32, 751–767. [Google Scholar] [CrossRef] [Scilit]
  40. Morozov, V.A.; Deyneko, D.V.; Dzhevakov, P.B.; Leonidova, O.N.; Leonidov, I.A.; Baryshnikova, O.V.; Savilov, S.V.; Lazoryak, B.I. Concurrent Ca2+ and Pb2+ ions transport in Ca6.25Pb4.25(VO4)7 with the β-Ca3(PO4)2-type structure. Solid State Ion. 2021, 359, 115518. [Google Scholar] [CrossRef] [Scilit]
  41. Deyneko, D.V.; Petrova, D.A.; Aksenov, S.M.; Stefanovich, S.Y.; Baryshnikova, O.V.; Fedotov, S.S.; Burns, P.C.; Kosmyna, M.B.; Shekhovtsov, A.N.; Lazoryak, B.I. Ferroelectricity, ionic conductivity and structural paths for large cation migration in Ca10.5-xPbx(VO4)7 single crystals, x = 1.9, 3.5, 4.9. CrystEngComm 2019, 21, 1309–1319. [Google Scholar] [CrossRef] [Scilit]
  42. Gopal, R.; Calvo, C. The structure of Ca3(VO4)2. Z. Krist. 1973, 137, 67–85. [Google Scholar]
  43. Sandström, M.H.; Boström, D. Ca10K(PO4)7 from single-crystal data. Acta Crystallogr. E 2006, 62, i253–i255. [Google Scholar] [CrossRef] [Scilit]
  44. Deyneko, D.V.; Nikiforov, I.V.; Spassky, D.A.; Dikhtyar, Y.Y.; Aksenov, S.M.; Stefanovich, S.Y.; Lazoryak, B.I. Luminescence of Eu3+ as a probe for the determination of the local site symmetry in β-Ca3(PO4)2-related structures. CrystEngComm 2019, 21, 5235–5242. [Google Scholar] [CrossRef] [Scilit]
  45. Chen, M.; Xia, Z.; Molokeev, M.S.; Wang, T.; Liu, Q. Tuning of photoluminescence and local structures of substituted cations in xSr2Ca(PO4)2-(1-x)Ca10Li(PO4)7:Eu2+ phosphors. Chem. Mater. 2017, 29, 1430−1438. [Google Scholar]
  46. Lazoryak, B.I. Comment on “Tuning of Photoluminescence and Local Structures of Substituted Cations in xSr2Ca(PO4)2-(1-x)Ca10Li(PO4)7:Eu2+ phosphors. Chem. Mater. 2017, 29, 3800−3802. [Google Scholar] [CrossRef] [Scilit]
  47. Kosmyna, M.B.; Mateychenko, P.V.; Nazarenko, B.P.; Shekhovtsov, A.N.; Aksenov, S.M.; Spassky, D.A.; Mosunov, A.V.; Stefanovich, S.Y. Novel laser crystals in Ca9Y(VO4)7-x(PO4)x mixed system. J. Alloys Compnd. 2017, 708, 285–293. [Google Scholar] [CrossRef] [Scilit]
  48. Glass, A.M.; Abrahams, S.C.; Ballman, A.A.; Loiacono, G. Calcium Orthovanadate A New High Temperature Ferroelectric. Ferroelectrics 1978, 17, 579–582. [Google Scholar] [CrossRef] [Scilit]
  49. Lazoryak, B.I.; Belik, A.A.; Stefanovich, S.Y.; Morozov, V.A.; Malakho, A.P.; Baryshnikova, O.V.; Leonidov, I.A.; Leonidova, O.N. Ferroelectric–Ionic Conductor Phase Transitions in Optical Nonlinear Ca9R(VO4)7 Vanadates. Dokl. Phys. Chem. 2002, 384, 144–148. [Google Scholar] [CrossRef] [Scilit]
  50. Bedarev, V.A.; Kosmyna, M.B.; Mateychenko, P.V.; Merenkov, D.N.; Paszkowicz, W.; Poperezhai, S.N.; Fitch, A.; Romanowski, P.; Shekhovtsov, A.N. Structure refinement, ferroelectric domains and mechanical properties of Czochralski-grown Ca9La(VO4)7 and Ca10Li(VO4)7 single crystals. Funct. Mater. 2024, 31, 487–494. [Google Scholar] [CrossRef] [Scilit]
  51. Petricek, V.; Dusek, M.; Palatinus, L. Crystallographic Computing System JANA2006: General Features. Z. Krist. 2014, 229, 345–352. [Google Scholar]
  52. Brandenburg, K.; Putz, H. DIAMOND, Version 3; Crystal Impact GbR: Bonn, Germany, 2005. [Google Scholar]
  53. Kurtz, S.K.; Perry, T.T. A Powder Technique for the Evaluation of Nonlinear Optical Materials. J. Appl. Phys. 1968, 39, 3798–3813. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.