Abstract
Chalcopyrite-based thin-film solar cells have great potential for various applications, such as top or bottom cells in tandem devices, in addition to their use as standard single-junction modules due to their tuneable bandgap energy. A bandgap energy Eg > 1.5 eV should be targeted to realize a wide-bandgap top cell, e.g., by increasing the [Ga]/([Ga] + [In]) (GGI) ratio in Cu(In,Ga)Se2 (CIGS) cells to the range of 0.7–1. A second approach is targeting the second theoretical efficiency maximum at a little lower Eg = 1.34 eV with a GGI around 0.6 for high-efficiency single-junction applications with reduced electrical losses. An industry-relevant (Ag,Cu)(In,Ga)Se2 (ACIGS) co-evaporation process for wide-bandgap cells fabricated with GGI ratios above 0.6, with moderate [Ag]/([Ag] + [Cu]) (AAC) ratios < 0.1 and in-line RbF-PDT, was established on molybdenum-coated soda-lime glass substrates. Both measures, Ag alloying and RbF-PDT, can increase power conversion efficiency (PCE) mainly due to improved open-circuit voltage (VOC). In addition, Ag addition can increase fill factor (FF), leading to an increase in the PCE for cells with GGI > 0.6 compared to Ag-free reference cells. (Zn,Mg)O, either with a [Mg]/([Mg] + [Zn]) ratio of 0.15 or 0.25, is a good option as high-resistive layer replacing the commonly used i-ZnO in combination with a CdS buffer. Our best ACIGS wide-bandgap solar cells with RbF-PDT and Zn0.85Mg0.15O (without anti-reflective coating (ARC)) from various experimental campaigns show a PCE of 12.7% (Eg = 1.50 eV), and with a slightly reduced Eg of 1.45 eV a PCE of 15.5%, with VOC of 933 mV (VOC deficit of 517 mV), and a good FF of 73.2%. In the case when the bandgap is significantly lowered to 1.34 eV (GGI = 0.61), to the second theoretical efficiency maximum, we achieved a PCE of 18.2% with ARC for an Ag-free CIGS cell with RbF-PDT. For this cell with a CdS/i-ZnO buffer system the VOC deficit is 480 mV, and the FF is 78.1%.
1. Introduction
The chalcopyrite-type thin-film solar cells with a bandgap energy (Eg) around 1.5 eV or above are ideal candidates for application as stable inorganic top cell in tandem devices [1], either combined with a chalcopyrite-type bottom cell [2,3,4] or a silicon bottom cell [5,6,7]. Nevertheless, there remain challenges which have to be overcome for this application. First, the relatively low open-circuit voltage (VOC) values of wide-bandgap chalcopyrite-type cells result in high VOC deficits (Eg/e–VOC) of ΔVOC = 700–800 mV [8]. For comparison, high-efficiency Cu(In,Ga)Se2 (CIGS)-based cells with an absorber Eg in the range of 1.08–1.15 eV exhibit ΔVOC values below 400 mV (see Ref. [9] and references therein). Several origins for the large VOC deficit of wide-bandgap CIGS-based cells are under discussion such as recombination at the absorber/buffer interface due to an unfavorable band alignment and Shockley–Read–Hall recombination in the bulk as a result of deep defects, Cu-enriched grain boundaries, and increasing defect density (see Keller et al. [10], Spindler et al. [11] and references therein).
Besides the pronounced ΔVOC of chalcopyrite-type wide-bandgap cells, a general problem of these cells is also the relatively low fill factor (FF) around 70% (or below), e.g., for indium-free CuGaSe2 with Eg around 1.7 eV as presented in the review by Ishizuka (Ref. [12] and references therein) and the publication by Gong et al. (Ref. [13] and references therein), compared to FF values of 80% and above for well-performing CIGS-based cells with Eg below 1.2 eV [9,14,15]. As a consequence, the main research directions for the development of wide-bandgap CIGS-based cells should focus on the improvement of these two device parameters, first a reduction in the VOC deficit; and second, an increase in the FF.
In recent years, the power conversion efficiency (PCE) for sulfide-based Cu(In,Ga)S2 cells was significantly increased to 16.0% [16], and depending on small variations in the Ga content, different groups demonstrated substantial reduction in the ΔVOC down to 600 mV for Eg values of approximately 1.55 eV [16,17], 700 mV for Eg = 1.6 eV [18], 649 mV for Eg = 1.63 eV [19], and 638 mV for Eg = 1.58 eV, in this case with Ag addition to the absorber [20].
The best PCE value for an In-free CuGaSe2 was reported as 11.9% [21], and in the case where a pronounced Ag amount was added (AAC = 0.4), a PCE of 11.6% was achieved [22], both with ARC. A record value of PCE = 12.25% with VOC = 959 mV was achieved with a small Al addition to a CuGaSe2 absorber with Eg around 1.7 eV, resulting in ΔVOC = 741 mV [23]. The implementation of a state-of-the-art post-deposition treatment (PDT) with heavy alkali elements like Rb or Cs on wide-bandgap selenium-based CIGS with [Ga]/([Ga] + [In]) (GGI) ratios above 0.7 resulted in an increased VOC [24] whereas for pure CuGaSe2 the addition of heavy alkalis seems to have no beneficial effect [25]. Furthermore, the addition of Ag to wide-bandgap CIGS has been demonstrated as an effective measure to reach higher VOC values [10,26].
A second motivation to increase the bandgap of CuInSe2 or standard CIGS with Eg in the range of 1.1–1.2 eV (corresponding to GGIs of 0.2–0.3 as calculated with the values Eg = 1.04 eV for CuInSe2 and 1.68 eV for CuGaSe2, and a bowing coefficient b = 0.21 eV) is the improved performance of modules. An increased GGI results in lower current densities, which would lead to lower resistive losses in wide-bandgap CIGS modules compared to commonly used CIGS with Eg in the range of 1.1–1.2 eV [27].
From this point of view, besides the application as a top cell, a second approach would be to target the second theoretical efficiency maximum at Eg = 1.34 eV instead of the first maximum at Eg = 1.15 eV [28] with a single-junction CIGS cell or module that is normally envisioned for high-efficiency CIGS devices. Nevertheless, previous works have shown that the CIGS cell efficiencies decrease for Eg values above 1.20–1.25 eV [8], and the grain size is significantly reduced for GGIs higher than 0.23, corresponding to the pseudo-cubic point in the tetragonal crystal structure [29]. In general, the melting point of CuGaSe2 is around 70 °C higher compared to CuInSe2 [30]; thus, also higher substrate temperatures should be used during thin-film deposition of CuGaSe2 and wide-bandgap CIGS with high GGIs > 0.7. The melting points of the Ag-based chalcopyrites AgInSe2 and AgGaSe2 are around 200 °C lower compared to the Cu-based counterparts [30].
All the above-described measures for a performance increase were applied on a laboratory scale wide-bandgap CIGS or ACIGS cells statically grown using relatively small deposition systems. However, with regard to industrial manufacturing, a fast and scalable co-evaporation approach, such as in-line deposition, would be preferable for the growth of wide-bandgap CIGS absorbers. An in-line process for the absorber growth would be fast due to the moving carriers, without the need to break the vacuum after each deposition process, as required for the static process, and therefore also allow for a 24/7 production, resulting in a high throughput and a large quantity of devices. This approach, the upscaling to module size, and the combination of these wide-bandgap ACIGS top modules with the standard silicon cells/modules for tandem application, or, alternatively, for more efficient (A)CIGS single-junction modules with Eg around the second theoretical efficiency maximum optimized for an operation under outdoor conditions, would be the best-case scenario as a medium- or long-term vision.
In this work, we present our development of an industry-relevant in-line co-evaporation process for wide-bandgap CIGS-based solar cells, including measures such as in-line RbF-PDT, annealing, and/or various rinsing procedures of the absorber, Ag co-evaporation, and optimization of the stacking sequence of the thin-film solar cell device in order to reduce the VOC deficit, improve FF, and finally increase PCE.
2. Materials and Methods
2.1. Wide-Bandgap CIGS and ACIGS Solar Cell Fabrication
For the fabrication of solar cell devices, sputtered molybdenum (Mo) on soda-lime glass (SLG) served as a back contact. Wide-bandgap CIGS was deposited with a multi-stage co-evaporation process by adjusting the In and Ga evaporation sources to reach integral GGI values in the range of 0.3–0.9. [Cu]/([Ga] + [In]) (CGI) or ([Ag] + [Cu])/([Ga] + [In]) (ACGI) ratios were in the range of 0.64–0.74. In case Ag was added to the process, this was realized by an additional evaporation source providing Ag during the second stage of the CIGS growth process, aiming for [Ag]/([Ag] + [Cu]) (AAC) ratios < 0.1. Even a low AAC ratio of 0.05 can increase the grain size of our absorbers significantly compared to a Ag-free reference cell with GGI around 0.3 [31]. An enlarged grain size was also observed by Nishimura et al. for Ag addition on CuGaSe2 for AACs of 0.07 and above [32]. A similar AAC of 0.06 largely influenced the surface and interface with the CdS buffer of our ACIGS absorbers with GGI around 0.3 [33]. For some samples an additional in-line RbF-PDT process under Se atmosphere was performed after CIGS or ACIGS absorber deposition without breaking the vacuum. During the RbF-PDT the temperature of the evaporation source was in the range of 510–520 °C, and the substrate temperature was around 300 °C. The RbF-PDT reduces the Ga and increases the In concentration on the surface of our widegap CIGS (GGI = 0.9) without evidence for the formation of a distinct Rb-In-Se layer [34]. Besides Rb from PDT, Na and partially K are provided by the SLG/Mo glass substrate and diffuse through the Mo back contact into the CIGS absorber at elevated temperatures. The complete (A)CIGS process was carried out in an industry-relevant 30 × 30 cm2 coater and resulted in absorbers with thicknesses in the range of d = 2.2–2.7 µm. The average grain size, as extracted from electron back scatter diffraction, decreases significantly with increasing GGI ratio, e.g., from 0.7 µm (GGI = 0.34) to 0.2 µm (GGI = 0.83) for similarly processed CIGS samples [35]. Further details on the applied (A)CIGS deposition process can be found in Ref. [36]. Before the subsequent buffer deposition, most of the wide-bandgap (A)CIGS absorbers were exposed to different treatments like annealing for 5 min at 200 °C in air, rinsing procedures with 1.5 M ammonia or 0.05 M Na2S solution, or a combination of annealing followed by the Na2S solution rinsing. The rinsing effect of Na2S solution is quite similar to that of rinsing with ammonia. The idea is to remove superfluous Rb from PDT, which we observed for the ammonia rinsing [37], and for the case an annealing step was performed, to reduce the amount of surface oxides.
Solution-grown CdS with a standard thickness around 50 nm was deposited with a commonly used thiourea-based process prior to sputtering of the subsequent high-resistive (HR) layers. As precursor chemical, we used CdSO4 with a final reactor concentration CR = 1.4 mmol/L (supplier Thermo Scientific Chemicals, purity 99.996%), thiourea with CR = 0.12 mol/L (Merck/Sigma-Aldrich, Schnelldorf, Germany, ACS reagent grade ≥ 99.0%), and ammonium hydroxide solution with CR = 1.5 mol/L (Merck/Sigma-Aldrich, 25% for analysis). The CdS layer deposition was performed in horizontal reactors at 65 °C. Thinner CdS buffer layers were successfully introduced for standard CIGS (GGI = 0.3) due to the improved growth of the solution-grown CdS in combination with a KF-PDT process [38], so therefore we also tested CdS buffers with 30 and 40 nm thickness in combination with our wide-bandgap CIGS after RbF-PDT.
In the next step, the HR-layers, either rf-sputtered i-ZnO (Eg ≈ 3.2–3.3 eV), Zn0.85Mg0.15O (Eg ≈ 3.4–3.5 eV), or Zn0.75Mg0.25O (Eg ≈ 3.7–3.8 eV) were applied with an in-line deposition system. The optical bandgap energies of the ZnO-based layers increase with the Mg addition [39], which can slightly improve the carrier collection in the short-wavelength region.
Finally, dc-sputtered ZnO:Al (AZO) with Eg in the range of 3.7–3.8 eV was applied as transparent front contact with Ni/Al/Ni grids on top. The total cell area is 0.5 cm2. One selected cell was coated with a 105 nm thick MgF2 anti-reflective coating (ARC) deposited by thermal evaporation.
2.2. Device and Materials Characterization
Current density-voltage (J-V) curves were measured with a WACOM (Saitama, Japan) AM1.5G solar simulator without any additional light-soaking or post-annealing procedures. Cold-light soaking procedures, normally in the range of 5–30 min, as applied to our standard (A)CIGS cells, had a detrimental effect on the performance of our wide-bandgap (A)CIGS cells, therefore the cells were not exposed to a light-soaking procedure prior to J-V measurements. These were performed with a four-point geometry at standard testing conditions, and a Si cell served for calibration of the solar simulator. Due to the different Eg values (1.1 eV for Si reference cell vs. around 1.5 eV or above for the wide-bandgap (A)CIGS cells under investigation) the JSC values of selected cells were corrected by external quantum efficiency (EQE) as indicated.
EQE was acquired with a BENTHAM (Berkshire, UK) PVE 300 with an additional light bias of around 1/3 sun, and Si and Ge photodiodes were used for calibration. The Eg values of the (A)CIGS absorbers were evaluated by a linear fitting of the (E × EQE)2 vs. E plots.
The integral chemical composition and thickness of the (A)CIGS absorber layers were determined with X-ray fluorescence (XRF) using a Fischerscope X-ray XDV-SDD (Helmut Fischer GmbH, Sindelfingen, Germany). Our wide-bandgap absorbers exhibit only a slight single GGI grading, e.g., from GGI = 0.8 (front side) to 0.9 (back side) as extracted from glow discharge optical emission spectroscopy measurements [40].
3. Results and Discussion
3.1. Reduction in the VOC Deficit
3.1.1. Application of an In-Line RbF-PDT on Wide-Bandgap CIGS Combined with Different Absorber Pre-Treatments
Figure 1a shows the positive influence of the in-line RbF-PDT on the PCE of wide-bandgap CIGS with Eg = 1.60 eV (GGI = 0.90) mainly as a result of increasing VOC values (Figure 1b), in the best case by 30–40 mV compared to the non-treated samples. These values are in the range of the gain in VOC as reported by Zahedi-Azad et al. with a static RbF-PDT process applied to wide-bandgap CIGS [24]. For wide-bandgap ACIGS, Keller et al. reported a beneficial effect of RbF on VOC [41]. For In-free CuGaSe2 Ishizuka et al. observed no increase in VOC due to PDT with heavy alkalis such as Rb [25] and Cs [42]. Our result with a relatively low amount of In supports the hypothesis that the alkali PDT only has a beneficial effect on In-containing CIGS. Nevertheless, the PCE values below 8% and FF values below 70% (Figure 1c) are limited, and there is further room for improvement. The various pre-treatments of the CIGS absorbers before CdS buffer deposition have a minor impact on the performance of the cells (compared to the improvement with RbF-PDT), but the ammonia rinsing seems favorable for PCE and VOC (up to 20 mV increase for both absorber types) during this experimental campaign.
Figure 1.
Influence of in-line RbF-PDT on CIGS with Eg = 1.60 eV (GGI = 0.90; CGI ≈ 0.70; d = 2.3 µm) and different pre-treatments of the CIGS absorber before CdS buffer growth. Stacking sequence is SLG/Mo/CIGS/CdS/i-ZnO/AZO and the number of cells N is indicated. (a) Power conversion efficiency (η), (b) open-circuit voltage (VOC), (c) fill factor (FF), and (d) short-circuit current density (JSC).
For standard absorbers with GGI around 0.3 with RbF-PDT combined with sputtered Ga2O3 buffers, the ammonia rinsing was mandatory to achieve well performing cells [43], whereas for cells with sputtered InxSy buffers, rinsing with ammonia or water had no beneficial impact on cell performance [37]. The annealing procedure of the absorbers seems to have no beneficial effect, which was observed for our standard CIGS (GGI around 0.3) without PDT combined with solution-grown Zn(O,S) or CdS buffers. Air annealing or Na2S solution rinsing, or a combination of both, is often used on our standard CIGS and ACIGS absorbers with RbF-PDT with GGI values around 0.3 [36]. Diethelm et al. reported a beneficial effect on JSC due to KCN etching of wide-bandgap ACIGS cells with Eg of 1.46 eV and an influence of ammonia rinsing duration prior to CdS buffer deposition [44].
3.1.2. Optimization of the Solar Cell Stacking Sequence by Exchanging the ZnO HR Layer
The CdS buffer layer is not the ideal partner for wide-bandgap CIGS or CuGaSe2 absorbers due to a pronounced negative conduction band offset (cliff) at the absorber/buffer interface [45], resulting in a reduced VOC. A pronounced cliff of −0.53 eV was revealed between the CdS buffer and our widegap absorber (Eg = 1.60 eV, GGI = 0.90) with RbF-PDT and ammonia rinsing [46] (same procedure as shown for the samples in Figure 1). A similar absorber without PDT and a slightly higher GGI of 0.95 revealed a cliff of −0.57 eV, indicating no impact of RbF-PDT on the conduction band alignment of our wide-bandgap absorbers with CdS [47]. Only a few alternative buffer layers with higher bandgap energies than CdS were tested in combination with CuGaSe2 in the past, of which only ZnSnOx grown by atomic layer deposition resulted in a high VOC above 1 V and with ΔVOC = 603 mV [21]. Solution-grown Zn(O,S) combined with our CuGaSe2 showed significantly lower VOC values compared to CdS-buffered reference cells. CuGaSe2 combined with ZnSe achieved a high VOC of almost 1 V but with very poor JSC [48]. Interestingly, Ishizuka et al. reported a high VOC approaching 1 V for a CuGaSe2 cell with a very thick CBD-CdS buffer of 150 nm thickness [49]. Therefore, we decided to keep CdS as the buffer, testing two thicknesses but modifying the subsequent ZnO HR layer. (Zn,Mg)O was the HR layer of choice for several CIGS and Cu(In,Ga)(S,Se)2 [15] former world record solar cells with Eg around 1.1 eV in the past years and seemed to be an ideal candidate with its higher Eg compared to pure ZnO. In addition, we tried a thinner CdS buffer layer with 30 nm thickness compared to our standard with 50 nm in combination with our wide-bandgap CIGS with RbF-PDT, which was successfully introduced for KF-PDT combined with standard CIGS (GGI = 0.3) due to an improved growth of the solution-grown buffer in combination with the PDT process, resulting in a reduced parasitic absorption and higher JSC [38].
Figure 2 shows the influence of exchanging the commonly used i-ZnO with a Zn0.75Mg0.25O as HR-layer for the wide-bandgap CIGS cells with Eg = 1.54–1.53 eV (GGI = 0.83) using CdS buffer layers with 30 and 50 nm thicknesses, respectively. An increase in PCE for the cells with (Zn,Mg)O is observable (Figure 2a), mainly due to increased VOC values compared to cells with i-ZnO (Figure 2b), whereas the FF (Figure 2c) is not affected. The VOC values of cells with thinner CdS are a little bit lower compared to the standard thickness, but this deficit is compensated for by a slightly higher JSC due to the reduced parasitic absorption of the thinner CdS, resulting in quite similar PCEs. The comparison between (Zn,Mg)O and i-ZnO as HR layers revealed improved EQEs in the wavelength region below 400 nm. In the best case, there is a gain in VOC of more than 20 mV for the best cell with (Zn,Mg)O vs. i-ZnO, with a VOC value of 899 mV, resulting in a VOC deficit of 631 mV. Nevertheless, this cell and all other cells from this experimental campaign again suffer from relatively low FF values below 70%.
Figure 2.
Wide-bandgap CIGS solar cell parameters for an exchange of the HR-layer i-ZnO (ZnO) with Zn0.75Mg0.25O (ZMO) combined with thin (≈30 nm) and standard CdS buffer thickness (≈50 nm). The stacking sequence is SLG/Mo/CIGS:Rb/CdS/HR layer/AZO, the CIGS:Rb absorbers (Eg = 1.53–1.54 eV; GGI = 0.83; CGI = 0.71; d = 2.3 µm); all absorbers were rinsed with Na2S solution, and the number of cells N is indicated (cells with FF < 50% were excluded). (a) η, (b) VOC, (c) (FF), and (d) JSC.
3.1.3. Discussion on Origin of VOC Improvement
The VOC improvement as a result of the RbF-PDT could be partially explained with a reduced interface recombination as suggested by Zahedi-Azad et al. due to the activation energy close to the bandgap of the wide-bandgap CIGS:Rb cell compared to the reference cell without PDT, but VOC transient measurements still pointed to persistent interface recombination [24]. In addition, we observed improved bulk properties with increasing Rb dose on wide-bandgap CIGS such as increasing lifetime and enhanced quasi-Fermi level splitting as measured by time-resolved photoluminescence and photoluminescence, respectively [40].
In case Mg is added to ZnO, an increase in the conduction band offset between absorber and (Zn,Mg)O directly applied as buffer was reported either for standard CIGS absorbers [50] or sulfur-containing Cu(In,Ga)(S,Se)2 [51]. In case of (Zn,Mg)O applied as HR layer, something similar could affect the CIGS/buffer/HR layer interface, i.e., the Mg addition to ZnO could have a beneficial effect on the band alignment of the wide-bandgap CIGS/CdS/Zn0.75Mg0.25O interface compared to CIGS/CdS/ZnO, resulting in reduced interface recombination with a VOC increase as observed in our experiments.
3.2. Beneficial Effect with a Small Ag Addition on the Absorber
3.2.1. Improved Device Parameters
As described above, our Ag-free wide-bandgap CIGS solar cells suffer from relatively low FF values below 70%, whereas the best CIGS cells with Eg around 1.0–1.2 eV can reach values of 80% and above. Positive effects of Ag addition to wide-bandgap CIGS solar cells were reported in the past, especially with relatively high AAC ratios in the range of 0.1–0.4 [22,32]. This provided motivation to apply Ag addition also to our wide-bandgap material in the in-line process by co-evaporation. Both CIGS and ACIGS wide-bandgap absorbers were grown with the same substrate temperature within the same experimental campaign. Adding only a very small amount of Ag (AAC = 0.03) to the wide-bandgap CIGS solar cells with Eg = 1.59 eV (GGI = 0.87) increases the device performance significantly, mainly due to an improved FF, VOC, and JSC (see Figure 3). The increase in JSC is not only a result of better absorber quality and modified CIGS/buffer interface due to the Ag addition, but there is an additional effect which comes from a slightly reduced Eg = 1.55 eV of ACIGS, in this case mainly due to slightly lower GGI = 0.83 of the ACIGS absorber. The improved device performance for the ACIGS cells compared to Ag-free CIGS cells was observed independently of the absorber pre-treatment, either only Na2S solution rinsing or a combination of air annealing followed by the Na2S solution rinsing before buffer deposition.
Figure 3.
Positive influence on solar cell parameters as a result of small Ag addition (AAC = 0.03) to the wide-bandgap CIGS absorber layer. The stacking sequence is SLG/Mo/(A)CIGS:Rb/CdS/i-ZnO/ AZO and the bandgap energies (Eg) as extracted from EQE are 1.59 eV for CIGS (GGI = 0.87; CGI = 0.73; d = 2.5 µm) and 1.55 eV for ACIGS (GGI = 0.83; ACGI = 0.64; d = 2.5 µm). Some of the (A)CIGS:Rb absorbers were annealed as indicated and all were rinsed with Na2S solution before CdS deposition. (a) η, (b) VOC, (c) FF, and (d) JSC.
A moderate Ag addition (AAC < 0.1) helped to increase our FF values for standard CIGS (GGI ≈ 0.3) [36,52] whereas higher AAC ratios up to 0.76 as reported for standard and wide-bandgap ACIGS by Erslev et al. [26] seem to be detrimental in our case.
Taking a broader look at different absorbers with increasing GGI values from 0.31 to 0.87 and the influence of low Ag addition (AAC < 0.1) as depicted in Figure 4 for representative cells, we observe only an increase in PCE for cells with higher GGI values above 0.6 as a result of higher FF. In addition, the ACIGS cells exhibit higher VOC and reduced JSC, except for high GGIs, where JSC is on the same level. It should be noted that these CIGS and ACIGS cells with different GGI ratios stem from different deposition campaigns, and also different substrates temperatures were applied. Nevertheless, the data reflects a general trend we observe for our industry-relevant co-evaporation process in case of low Ag addition. Although for cells with GGI = 0.3 and 0.5 there is no significant improvement in device performance, Ag alloying shows a clear benefit in the wide-bandgap cells fabricated with the in-line coater.
Figure 4.
Ag-alloying improves the cell performance for wide-bandgap cells with GGI > 0.6 due to small Ag addition (AAC < 0.1), whereas PCEs for GGIs < 0.6 are not significantly increased for ACIGS cells. The stacking sequence is SLG/Mo/(A)CIGS:Rb/CdS/Zn0.85Mg0.15O/AZO. (a) η, (b) VOC, (c) FF, and (d) JSC.
If Ag is added at a given GGI in high amounts for AAC values > 0.5, a significant increase in the bandgap energy of 0.1 eV or a bit more should be observed [53]. In our case, for the low AAC values below 0.1, no significant influence on the bandgap should result. Nevertheless, the ACIGS/buffer interface and/or the absorber itself can significantly change, especially when the addition of Ag (even in small amounts) is combined with an RbF-PDT. In this case, the formation of an Rb-In-Se species with a high bandgap of 2.79 eV was found for an ACIGS absorber with GGI = 0.31 and AAC = 0.06 [33]. An Rb-In-Se formation was also found for wide-bandgap Cu-free Ag(In,Ga)Se2 cells with Eg = 1.5 eV in combination with RbF-PDT and the use of a CdS buffer [54].
3.2.2. Discussion on Origin of FF and VOC Improvement
The increase in FF for wide-bandgap CIGS with GGIs > 0.6 is most probably a result of a reduced diode factor as observed for our standard CIGS by adding small amounts of Ag [52]. A reduction in Urbach energy, as observed by Erslev et al. on CIGS with GGI = 0.8 [26] and Nishimura et al. for CuGaSe2 with Ag addition [32], could be an explanation for the increased VOC as a result of reduced structural disorder inside the absorber. In addition, modifications at the wide-bandgap ACIGS/buffer interface due to Ag incorporation can reduce interface recombination, as reported by Keller et al. [53]. We also observed a modified interface on our standard ACIGS with GGI around 0.3 [33], which could also play a role in the VOC enhancement of our wide-bandgap absorbers.
3.3. Combination of Different Measures to Improve Wide-Bandgap Solar Cell Efficiency
3.3.1. Best Wide-Bandgap ACIGS Cells with Eg = 1.45 and 1.50 eV
Combining the three measures, namely in-line RbF-PDT, rf-sputtering of (Zn,Mg)O as HR layer, and a slight Ag addition to the absorber by co-evaporation, we fabricated a wide-bandgap cell with a PCE = 12.7% (without ARC) as depicted in Figure 5a. The FF with 73.6% is quite good for this cell considering Eg = 1.50 eV, but with the low VOC value of 829 mV, the VOC deficit of 671 mV is still considerable. The pronounced VOC loss can be partially explained by the non-ideal band alignment between CdS and the ACIGS absorber, as observed for a similar Ag-free CIGS absorber with RbF-PDT and a 0.1 eV higher bulk Eg of 1.60 eV (GGI = 0.90) combined with a CdS buffer, resulted in a pronounced cliff of −0.53 eV considering the enlarged surface Eg of 1.79 eV [46]. On the other side, by increasing the source temperature of RbF during the PDT in combination with a wide-bandgap ACIGS absorber, we achieved VOC values up to and above 1 V [40]. Most probably, the small Ag addition in combination with an optimized RbF-PDT process has a beneficial impact on the band alignment with CdS. The EQE in Figure 5c shows a decent parasitic absorption in the short-wavelength region as a result of the CdS, but a rather steep decrease in the range of 800–900 nm, which is usually relatively flat due to the reduced effective collection length of widegap CIGS absorbers compared to CIGS with standard composition [55]. In case the Eg is lowered by a mere 0.05 eV to 1.45 eV, we fabricated our best wide-bandgap cell so far with a PCE of 15.5%, a good FF of 73.2%, and an even higher VOC of 933 mV, resulting in an improved VOC deficit of 517 mV (Figure 5b) compared to the cell with Eg = 1.50 eV.
Figure 5.
Characteristics of two wide-bandgap ACIGS solar cells and corresponding solar cell parameters. (a) J-V curves of the cell with Eg = 1.50 eV (GGI = 0.81; ACGI = 0.67; d = 2.7 µm) and the stacking sequence SLG/Mo/ACIGS:Rb/CdS (around 40 nm)/Zn0.85Mg0.15O/AZO. The AAC ratio is 0.05, the cell is without ARC, JSC is corrected with EQE, and the ACIGS:Rb absorber was annealed in air and rinsed with Na2S solution. (b) J-V curves of the cell with slightly lower Eg = 1.45 eV (GGI = 0.73; ACGI = 0.74; d = 2.2 µm) and the stacking sequence SLG/Mo/ACIGS:Rb/CdS/ Zn0.85Mg0.15O/AZO. The AAC ratio is 0.07, the cell is without ARC, JSC is corrected with EQE, and the ACIGS:Rb absorber was annealed in air (no rinsing procedure applied). (c) Corresponding EQE curves of both wide-bandgap ACIGS cells shown in (a) solid red curve and (b) dashed blue curve.
Keller et al. achieved a PCE of 16.3% at Eg = 1.43 eV and with another ACIGS cell (Eg = 1.44 eV) received their highest VOC of 926 mV, resulting in ΔVOC = 514 mV, all with a CdS buffer [41]. Recently, Yao et al. reported a similar PCE of 15.4% for an ACIGS wide-bandgap cell with Eg ≈ 1.46 eV, including a buffer consisting of a Zn(O,S)/CdS bilayer, but with a lower VOC of 866 mV, resulting in ΔVOC = 594 mV [56]. Kim et al. published a PCE of 14.8% with ARC with a VOC of 847 mV for Eg around 1.5 eV [57]. Besides the design of the (A)CIGS/buffer interface and therefore the resulting band alignment between absorber and buffer, the RbF source temperature during PDT can have a significant impact on the resulting VOC and, as described above, in the best case, we achieved a high VOC of 1007 mV with the maximum tolerable RbF amount provided to a wide-bandgap ACIGS cell with Eg = 1.55 eV, resulting in a VOC deficit of 543 mV [40].
3.3.2. Targeting the Second Theoretical Efficiency Maximum with an Absorber Bandgap of 1.34 eV
In case the bandgap is significantly reduced to Eg = 1.34 eV (GGI = 0.61), corresponding to the second theoretical efficiency maximum [28], a very good efficiency of 18.2% with ARC was achieved (see J-V curves and EQE in Figure 6). The Ag-free CIGS cell with an in-line RbF-PDT achieved a VOC of 856 mV, resulting in a VOC deficit of 480 mV in combination with a good FF of 78.1%. Nevertheless, this VOC deficit is still around 80–130 mV higher compared to CIGS-based record cells targeting the first theoretical efficiency maximum at Eg = 1.15 eV, with reported bandgap energies of the record cells in the range of 1.08–1.15 eV, all with ΔVOC < 400 mV (see Ref. [9] and references therein).
Figure 6.
(a) J-V characteristics with corresponding solar cell parameters and (b) EQE of the Ag-free CIGS solar cell with Eg = 1.34 eV (GGI = 0.61; CGI = 0.74; d = 2.2 µm) at the second theoretical efficiency maximum. The cell contains an ARC layer and JSC is corrected by EQE. The stacking sequence is SLG/Mo/CIGS:Rb/CdS/i-ZnO/AZO/MgF2 and the Ag-free CIGS:Rb absorber was rinsed with Na2S.
In the past, the second maximum was mostly included in bandgap (GGI) variations with CIGS-based solar cells rather than explicitly targeting this value. Nevertheless, recently a PCE of 15.6% was reported for a cell with MgF2 ARC with a slightly higher Eg of 1.36 eV for the corresponding ACIGS absorber on a titanium substrate, with a VOC of 804 mV and a VOC deficit of 559 mV [58]. Hanket et al. achieved a PCE of 17.6% with MgF2 ARC with a slightly lower Eg of 1.31 eV for the corresponding ACIGS absorber, with a VOC of 709 mV and a VOC deficit of 601 mV [30]. The best Ag-free CIGS cell on high-temperature substrate glass as published by Contreras et al. has a PCE of 17.7% with MgF2 ARC at Eg = 1.32 eV, a VOC of 801 mV, and a ΔVOC = 519 mV [8]. A remarkable result was published by Kim et al. for an ACIGS cell with a PCE of 17.4% with MgF2 ARC at a higher Eg around 1.4 eV, with a VOC of 788 mV [57].
4. Conclusions
An industry-relevant CIGS co-evaporation process for wide-bandgap Cu(In,Ga)Se2 with Ag co-evaporation with a moderate AAC < 0.1 and in-line RbF-PDT was established on Mo-coated SLG substrates, which could serve as a top cell in a tandem device when combined with a transparent back contact. Both measures can increase efficiency and reduce the VOC deficit in our experiments. In addition, the small Ag addition can increase FF and VOC values and improve PCE for GGIs > 0.6 compared to Ag-free CIGS reference cells. (Zn,Mg)O, either with a [Mg]/([Mg] + [Zn]) ratio of 0.15 or 0.25, is a good option as HR layer as an alternative to the commonly used i-ZnO in combination with a solution-grown CdS buffer. With this approach, we achieved a high VOC of 899 mV, resulting in a reduction in the VOC deficit to 631 mV for a wide-bandgap CIGS cell with Eg = 1.53 eV (GGI = 0.83). Our best wide-bandgap solar cells (without ARC) with ACIGS absorbers (AAC = 0.05) with RbF-PDT with Eg = 1.50 eV and Zn0.85Mg0.15O as HR layer showed a PCE of 12.7%, and with slightly reduced Eg = 1.45 eV, a PCE of 15.5%, a VOC of 933 mV, resulting in a VOC deficit of 517 mV, and a good FF of 73.2%.
When the bandgap is significantly lowered to 1.34 eV (GGI = 0.61), around the second theoretical efficiency maximum, we achieved a PCE of 18.2% with ARC for an Ag-free CIGS cell with RbF-PDT. For this cell with a CdS/i-ZnO buffer system, we have a VOC of 856 mV, the VOC deficit is 480 mV, and the FF exhibits 78.1%. Nevertheless, the PCE is significantly lower compared to the current ACIGS-based world record cell with PCE = 23.6% and with its Eg near the first theoretical efficiency maximum [9]. Our latter two PCE values are a step forward for cells with selenidic absorbers, and it should be possible to implement the proposed modifications easily in an existing CIGS production line without further increasing the production costs.
5. Outlook
For an application as wide-bandgap top cell, the industry-relevant ACIGS process should be transferred from opaque molybdenum to transparent back contacts like indium tin oxide or zirconium-doped indium oxide. The next step would be an upscaling to fabricate wide-bandgap sub-modules with monolithic interconnection of single cells either on transparent back contacts for the tandem approach, e.g., with a silicon bottom cell, or on opaque molybdenum back contacts for the single-junction application targeting the second theoretical efficiency maximum. The upscaling is straightforward due to the use of the industrially well-established deposition techniques such as co-evaporation, chemical bath deposition, and sputtering, whereas the transfer from opaque molybdenum back contact to transparent back contacts, and simultaneously maintaining the same efficiency level, remains challenging for high-temperature (A)CIGS absorber processes [59]. Further challenges for upscaling could be the uniformity of the absorber in terms of chemical composition, especially the homogeneous distribution of elements with very low concentration like rubidium from PDT, the moderate silver addition, and the sodium coming from the glass substrate, in case a transparent back contact is used without any diffusion barrier. As current transparent back contacts are mainly based on costly indium oxide, an exchange to indium-free materials would be desirable in terms of production costs for transparent full-size modules while still maintaining a high process reproducibility and device yield. In general, both routes would increase the energy yield per square meter under outdoor conditions, the tandem device due to its higher efficiency and the CIGS-based single-junction module optimized for the second efficiency maximum due to reduced electrical losses as a result of the higher bandgap.
Author Contributions
W.W.: conceptualization, project administration, funding acquisition, methodology, investigation, data curation, writing—original draft preparation, writing—review and editing. R.G. investigation, data curation, methodology, writing—review and editing. S.P. investigation, data curation, writing—review and editing. D.H. conceptualization, methodology, investigation, data curation, writing—review and editing. All authors have read and agreed to the published version of the manuscript.
Funding
This project has received funding from the German Federal Ministry for Economic Affairs and Energy (BMWi) within the EFFCIS project under contract number 0324076A, the German Federal Ministry for Economic Affairs and Climate Action (BMWK) under contract number 03EE1059A within the EFFCIS-II project, and from the European Union program HORIZON (Call: HORIZON-CL5-2021-D3-02), Project ID: 101075626 (SITA). Funded by the European Union. Views and opinions expressed are however those of the author(s) only and do not necessarily reflect those of the European Union or CINEA. Neither the European Union nor the granting authority can be held responsible for them.
Institutional Review Board Statement
Not applicable.
Informed Consent Statement
Not applicable.
Data Availability Statement
The data are available upon request to the corresponding author.
Acknowledgments
We thank the CIGS team at ZSW for solar cell fabrication and characterization.
Conflicts of Interest
The authors declare no conflicts of interest. The funders had no role in the design of the study; in the collection, analyses, or interpretation of data; in the writing of the manuscript; or in the decision to publish the results.
References
- Eperon, G.E.; Hörantner, M.T.; Snaith, H.J. Metal halide perovskite tandem and multiple-junction photovoltaics. Nat. Rev. Chem. 2017, 1, 95. [Google Scholar] [CrossRef] [Scilit]
- Nishiwaki, S.; Siebentritt, S.; Walk, P.; Lux-Steiner, M.C. A stacked chalcopyrite thin-film tandem solar cell with 1.2 V open-circuit voltage. Prog. Photovolt. Res. Appl. 2003, 11, 243–248. [Google Scholar] [CrossRef] [Scilit]
- Nakada, T.; Kijima, S.; Kuromiya, Y.; Arai, R.; Ishii, Y.; Kawamura, N.; Ishizaki, H.; Yamada, N. Chalcopyrite Thin-Film Tandem Solar Cells with 1.5 V Open-Circuit-Voltage. In Proceedings of the 2006 IEEE 4th World Conference on Photovoltaic Energy Conference, Waikoloa, HI, USA, 7–12 May 2006; pp. 400–403. [Google Scholar] [CrossRef] [Scilit]
- Wi, J.-H.; Han, W.S.; Lee, W.-J.; Cho, D.-H.; Yu, H.-J.; Kim, C.-W.; Jeong, C.; Yun, J.H.; Kim, C.-I.; Chung, Y.-D. Spectral Response of CuGaSe2/Cu(In,Ga)Se2 Monolithic Tandem Solar Cell with Open-Circuit Voltage Over 1 V. IEEE J. Photovolt. 2018, 8, 840–848. [Google Scholar] [CrossRef]
- Jeong, A.R.; Choi, S.B.; Kim, W.M.; Park, J.-K.; Choi, J.; Kim, I.; Jeong, J. Electrical analysis of c-Si/CGSe monolithic tandem solar cells by using a cell-selective light absorption scheme. Sci. Rep. 2017, 7, 15723. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Horstmann, J.; Hanser, M.; Polzin, J.-I.; Maiberg, M.; Scheer, R.; Hermle, M. Effect of top cell absorber thickness and bifacial illumination on monolithic (Ag,Cu)(In,Ga)Se2/Si tandem solar cells. J. Phys. Energy 2025, 7, 45004. [Google Scholar] [CrossRef] [Scilit]
- Mitmit, C.; Diethelm, M.; de Marzi, M.; Kochel, N.; Maciejewska, J.; Narasimhamurthy, A.; Miszczuk, A.; de Wild, J.; Reekmans, B.; Vermang, B.; et al. Improving VOC in wide bandgap (Ag,Cu)(In,Ga)Se2 solar cells for voltage-matched ACIGS/Si tandem modules. Sol. Energy Mater. Sol. Cells 2026, 302, 114335. [Google Scholar] [CrossRef] [Scilit]
- Contreras, M.A.; Mansfield, L.M.; Egaas, B.; Li, J.; Romero, M.; Noufi, R.; Rudiger-Voigt, E.; Mannstadt, W. Wide bandgap Cu(In,Ga)Se2 solar cells with improved energy conversion efficiency. Prog. Photovolt. Res. Appl. 2012, 20, 843–850. [Google Scholar] [CrossRef] [Scilit]
- Keller, J.; Kiselman, K.; Donzel-Gargand, O.; Martin, N.M.; Babucci, M.; Lundberg, O.; Wallin, E.; Stolt, L.; Edoff, M. High-concentration silver alloying and steep back-contact gallium grading enabling copper indium gallium selenide solar cell with 23.6% efficiency. Nat. Energy 2024, 9, 467–478. [Google Scholar] [CrossRef] [Scilit]
- Keller, J.; Pearson, P.; Shariati Nilsson, N.; Stolt, O.; Stolt, L.; Edoff, M. Performance Limitations of Wide-Gap (Ag,Cu)(In,Ga)Se2 Thin-Film Solar Cells. Sol. RRL 2021, 5, 2100403. [Google Scholar] [CrossRef] [Scilit]
- Spindler, C.; Babbe, F.; Wolter, M.H.; Ehré, F.; Santhosh, K.; Hilgert, P.; Werner, F.; Siebentritt, S. Electronic defects in Cu(In,Ga)Se2: Towards a comprehensive model. Phys. Rev. Mater. 2019, 3, 90302. [Google Scholar] [CrossRef] [Scilit]
- Ishizuka, S. CuGaSe2 Thin Film Solar Cells: Challenges for Developing Highly Efficient Wide-Gap Chalcopyrite Photovoltaics. Phys. Stat. Sol. A 2019, 216, 1800873. [Google Scholar] [CrossRef] [Scilit]
- Gong, J.; Gao, D.; Ma, Z.; Yang, X.; Zhang, J.; Liu, X.; Chen, C.; Tang, J.; Da, B.; Li, J.; et al. Over 11% Efficient CuGaSe2 Solar Cells Without Using KCN Treatment. Sol. RRL 2022, 6, 2200766. [Google Scholar] [CrossRef] [Scilit]
- Repins, I.; Contreras, M.A.; Egaas, B.; DeHart, C.; Scharf, J.; Perkins, C.L.; To, B.; Noufi, R. 19.9%-efficient ZnO/CdS/CuInGaSe2 solar cell with 81.2% fill factor. Prog. Photovolt. Res. Appl. 2008, 16, 235–239. [Google Scholar] [CrossRef] [Scilit]
- Nakamura, M.; Yamaguchi, K.; Kimoto, Y.; Yasaki, Y.; Kato, T.; Sugimoto, H. Cd-Free Cu(In,Ga)(Se,S)2 Thin-Film Solar Cell with Record Efficiency of 23.35%. IEEE J. Photovolt. 2019, 9, 1863–1867. [Google Scholar] [CrossRef] [Scilit]
- Barreau, N.; Bertin, E.; Crossay, A.; Durand, O.; Arzel, L.; Harel, S.; Lepetit, T.; Assmann, L.; Gautron, E.; Lincot, D. Investigation of co-evaporated polycrystalline Cu(In,Ga)S2 thin film yielding 16.0% efficiency solar cell. EPJ Photovolt. 2022, 13, 17. [Google Scholar] [CrossRef] [Scilit]
- Hiroi, H.; Iwata, Y.; Adachi, S.; Sugimoto, H.; Yamada, A. New World-Record Efficiency for Pure-Sulfide Cu(In,Ga)S2 Thin-Film Solar Cell with Cd-Free Buffer Layer via KCN-Free Process. IEEE J. Photovolt. 2016, 6, 760–763. [Google Scholar] [CrossRef] [Scilit]
- Shukla, S.; Sood, M.; Adeleye, D.; Peedle, S.; Kusch, G.; Dahliah, D.; Melchiorre, M.; Rignanese, G.-M.; Hautier, G.; Oliver, R.; et al. Over 15% efficient wide-band-gap Cu(In,Ga)S2 solar cell: Suppressing bulk and interface recombination through composition engineering. Joule 2021, 5, 1816–1831. [Google Scholar] [CrossRef] [Scilit]
- Adeleye, D.; Sood, M.; Valluvar Oli, A.; Törndahl, T.; Hultqvist, A.; Vanderhaegen, A.; Lanzoni, E.M.; Hu, Y.; Kusch, G.; Melchiorre, M.; et al. Wide-Bandgap Cu(In, Ga)S2 Solar Cell: Mitigation of Composition Segregation in High Ga Films for Better Efficiency. Small 2025, 21, 2405221. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Hu, Y.; Washbrook, E.; Oli, A.V.; Griesi, A.; Ivanov, Y.P.; Pelling, M.; Fairclough, S.M.; Kaur, K.; Melchiorre, M.; Hultqvist, A.; et al. Silver-Alloyed Wide-Bandgap (Ag,Cu)(In,Ga)S2 Thin-Film Solar Cells with 15.5% Efficiency. Prog. Photovolt. Res. Appl. 2026; Early View. [CrossRef] [Scilit]
- Larsson, F.; Nilsson, N.S.; Keller, J.; Frisk, C.; Kosyak, V.; Edoff, M.; Törndahl, T. Record 1.0 V open-circuit voltage in wide band gap chalcopyrite solar cells. Prog. Photovolt. Res. Appl. 2017, 25, 755–763. [Google Scholar] [CrossRef] [Scilit]
- Keller, J.; Stolt, L.; Törndahl, T.; Edoff, M. Silver Alloying in Highly Efficient CuGaSe2 Solar Cells with Different Buffer Layers. Sol. RRL 2023, 7, 2300208. [Google Scholar] [CrossRef] [Scilit]
- Ishizuka, S.; Nishinaga, J.; Kamikawa, Y.; Nishida, T.; Fons, P.J. Photovoltaic Efficiency Enhancement of Indium-Free Wide-Bandgap Chalcopyrite Solar Cells via an Aluminum-Induced Back-Surface Field Effect. ACS Appl. Mater. Interfaces 2025, 17, 3136–3145. [Google Scholar] [CrossRef] [Scilit]
- Zahedi-Azad, S.; Maiberg, M.; Clausing, R.; Scheer, R. Influence of heavy alkali post deposition treatment on wide gap Cu(In,Ga)Se2. Thin Solid Films 2019, 669, 629–632. [Google Scholar] [CrossRef] [Scilit]
- Ishizuka, S.; Taguchi, N.; Nishinaga, J.; Kamikawa, Y.; Tanaka, S.; Shibata, H. Group III Elemental Composition Dependence of RbF Postdeposition Treatment Effects on Cu(In,Ga)Se2 Thin Films and Solar Cells. J. Phys. Chem. C 2018, 122, 3809–3817. [Google Scholar] [CrossRef] [Scilit]
- Erslev, P.T.; Lee, J.; Hanket, G.M.; Shafarman, W.N.; Cohen, J.D. The electronic structure of Cu(In1−xGax)Se2 alloyed with silver. Thin Solid Films 2011, 519, 7296–7299. [Google Scholar] [CrossRef] [Scilit]
- Siebentritt, S.; Rau, U. Wide-Gap Chalcopyrites; Springer Series in Materials Science; Springer: Berlin/Heidelberg, Germany, 2006; Volume 86. [Google Scholar] [CrossRef] [Scilit]
- Rühle, S. Tabulated values of the Shockley–Queisser limit for single junction solar cells. Sol. Energy 2016, 130, 139–147. [Google Scholar] [CrossRef] [Scilit]
- Abou-Ras, D.; Caballero, R.; Kaufmann, C.A.; Nichterwitz, M.; Sakurai, K.; Schorr, S.; Unold, T.; Schock, H.W. Impact of the Ga concentration on the microstructure of CuIn1–xGaxSe2. Phys. Stat. Sol. (RRL) 2008, 2, 135–137. [Google Scholar] [CrossRef] [Scilit]
- Hanket, G.; Boyle, J.H.; Shafarman, W.N. Characterization and device performance of (AgCu)(InGa)Se2 absorber layers. In Proceedings of the 2009 34th IEEE Photovoltaic Specialists Conference (PVSC), Philadelphia, PA, USA, 7–12 June 2009; pp. 1240–1245. [Google Scholar] [CrossRef] [Scilit]
- Thomas, S.; Witte, W.; Hariskos, D.; Gutzler, R.; Paetel, S.; Song, C.-Y.; Kempa, H.; Maiberg, M.; Abou-Ras, D. Role of Ag Addition on the Microscopic Material Properties of (Ag,Cu)(In,Ga)Se2 Absorbers and Their Effects on Losses in the Open-Circuit Voltage of Corresponding Devices. Prog. Photovolt. Res. Appl. 2024, 32, 930–940. [Google Scholar] [CrossRef] [Scilit]
- Nishimura, T.; Doi, A.; Chantana, J.; Mavlonov, A.; Kawano, Y.; Minemoto, T. Silver-alloyed wide-gap CuGaSe2 solar cells. Sol. Energy 2021, 230, 509–514. [Google Scholar] [CrossRef] [Scilit]
- Hauschild, D.; Both, L.; Blankenship, M.; Wansorra, C.; Steininger, R.; Yang, W.; Hariskos, D.; Witte, W.; Gutzler, R.; Powalla, M.; et al. X-Ray and Electron Spectroscopy of the CdS/(Ag,Cu)(In,Ga)Se2 Interface with RbF Treatment. Adv. Mater. Interfaces 2025, 12, 2401002. [Google Scholar] [CrossRef] [Scilit]
- Both, L.; Hauschild, D.; Blankenship, M.; Steininger, R.; Witte, W.; Hariskos, D.; Paetel, S.; Powalla, M.; Heske, C.; Weinhardt, L. Impact of a RbF post-deposition treatment on the chemical structure of wide-gap CuIn0.1Ga0.9Se2 thin-film solar cell absorber surfaces. Appl. Phys. Lett. 2025, 126, 021603. [Google Scholar] [CrossRef] [Scilit]
- Thomas, S.; Witte, W.; Hariskos, D.; Paetel, S.; Song, C.-Y.; Kempa, H.; Maiberg, M.; El-Ganainy, N.; Abou-Ras, D. Effect of Ga Variation on the Bulk and Grain-Boundary Properties of Cu(In,Ga)Se2 Absorbers in Thin-Film Solar Cells and Their Impacts on Open-Circuit Voltage Losses. Prog. Photovolt. Res. Appl. 2025, 33, 265–275. [Google Scholar] [CrossRef] [Scilit]
- Gutzler, R.; Witte, W.; Kanevce, A.; Hariskos, D.; Paetel, S. Voc-losses across the band gap: Insights from a high-throughput inline process for CIGS solar cells. Prog. Photovolt. Res. Appl. 2023, 31, 1023–1031. [Google Scholar] [CrossRef] [Scilit]
- Witte, W.; Hempel, W.; Paetel, S.; Menner, R.; Hariskos, D. Effects of Sputtered InxSy Buffer on CIGS with RbF Post-Deposition Treatment. ECS J. Solid State Sci. Technol. 2021, 10, 55006. [Google Scholar] [CrossRef] [Scilit]
- Chirilă, A.; Reinhard, P.; Pianezzi, F.; Bloesch, P.; Uhl, A.R.; Fella, C.; Kranz, L.; Keller, D.; Gretener, C.; Hagendorfer, H.; et al. Potassium-induced surface modification of Cu(In,Ga)Se2 thin films for high-efficiency solar cells. Nat. Mater. 2013, 12, 1107–1111. [Google Scholar] [CrossRef] [Scilit]
- Minemoto, T.; Negami, T.; Nishiwaki, S.; Takakura, H.; Hamakawa, Y. Preparation of Zn1−xMgxO films by radio frequency magnetron sputtering. Thin Solid Films 2000, 372, 173–176. [Google Scholar] [CrossRef] [Scilit]
- Gutzler, R.; Bayat, S.; Hariskos, D.; Kanevce, A.; Hempel, W.; Paetel, S.; Siebentritt, S.; Witte, W. Effect of RbF post-deposition treatment on open-circuit voltage in wide-gap (Ag,Cu)(In,Ga)Se2 solar cells. EES Sol. 2026, 2, 479–490. [Google Scholar] [CrossRef] [Scilit]
- Keller, J.; Aboulfadl, H.; Stolt, L.; Donzel-Gargand, O.; Edoff, M. Rubidium Fluoride Absorber Treatment for Wide-Gap (Ag,Cu)(In,Ga)Se2 Solar Cells. Sol. RRL 2022, 6, 2200044. [Google Scholar] [CrossRef] [Scilit]
- Ishizuka, S.; Taguchi, N.; Nishinaga, J.; Kamikawa, Y.; Shibata, H. A comparative study of the effects of light and heavy alkali-halide postdeposition treatment on CuGaSe2 and Cu(In,Ga)Se2 thin-film solar cells. Sol. Energy 2020, 211, 1092–1101. [Google Scholar] [CrossRef] [Scilit]
- Witte, W.; Hempel, W.; Paetel, S.; Menner, R.; Hariskos, D. Influence of sputtered gallium oxide as buffer or high-resistive layer on performance of Cu(In,Ga)Se2-based solar cells. J. Mater. Res. 2022, 37, 1825–1834. [Google Scholar] [CrossRef] [Scilit]
- Diethelm, M.; Mitmit, C.; Hägglund, C.; Dimitrievska, M.; Vels, W.; Gharabeiki, S.; Nisika; Keller, J.; Carron, R. Enhancing photocurrent collection in wide-gap ACIGS solar cells. J. Phys. Energy 2026, 8, 15002. [Google Scholar] [CrossRef] [Scilit]
- Schulmeyer, T.; Kniese, R.; Hunger, R.; Jaegermann, W.; Powalla, M.; Klein, A. Influence of Cu(In,Ga)Se2 band gap on the valence band offset with CdS. Thin Solid Films 2004, 451–452, 420–423. [Google Scholar] [CrossRef] [Scilit]
- Blankenship, M.; Hauschild, D.; Both, L.; Pyatenko, E.; Witte, W.; Hariskos, D.; Paetel, S.; Powalla, M.; Weinhardt, L.; Heske, C. Conduction Band Cliff at the CdS/CuIn0.1Ga0.9Se2 Thin-Film Solar Cell Interface. J. Phys. Chem. C 2024, 128, 339–345. [Google Scholar] [CrossRef] [Scilit]
- Zahedi-Azad, S.; Scheer, R.; Hariskos, D.; Paetel, S.; Hempel, W.; Witte, W.; Luo, H.; Cojocaru-Mirédin, O.; Blankenship, M.; Hauschild, D.; et al. Progress Toward Efficient Wide-Gap Cu(In,Ga)(S,Se)2 Thin-Film Solar Cells. Prog. Photovolt. Res. Appl. 2026, 34, 567–588. [Google Scholar] [CrossRef] [Scilit]
- Rusu, M.; Gashin, P.; Simashkevich, A. Interface characterisation of ZnSe/CuGaSe2 heterojunction. Sol. Energy 2002, 72, 235–241. [Google Scholar] [CrossRef] [Scilit]
- Ishizuka, S.; Okamoto, R.; Ikeda, S. Enhanced Performance of Ternary CuGaSe2 Thin-Film Photovoltaic Solar Cells and Photoelectrochemical Water Splitting Hydrogen Evolution with Modified p–n Heterointerfaces. Adv. Mater. Interfaces 2022, 9, 2201266. [Google Scholar] [CrossRef] [Scilit]
- Minemoto, T.; Hashimoto, Y.; Satoh, T.; Negami, T.; Takakura, H.; Hamakawa, Y. Cu(In,Ga)Se2 solar cells with controlled conduction band offset of window/Cu(In,Ga)Se2 layers. J. Appl. Phys. 2001, 89, 8327–8330. [Google Scholar] [CrossRef] [Scilit]
- Tong, H.; Kou, Z.; Zhao, M.; Zhuang, D.; Wang, C.; Li, Y. Influences of Mg concentration in ZnMgO film on energy band alignment at CIGSSe/Zn1-xMgxO interface and performances of CIGSSe solar cells. Sol. Energy 2022, 246, 216–223. [Google Scholar] [CrossRef] [Scilit]
- Weiss, T.P.; Ramírez, O.; Paetel, S.; Witte, W.; Nishinaga, J.; Feurer, T.; Siebentritt, S. Metastable Defects Decrease the Fill Factor of Solar Cells. Phys. Rev. Appl. 2023, 19, 024052. [Google Scholar] [CrossRef] [Scilit]
- Keller, J.; Sopiha, K.V.; Stolt, O.; Stolt, L.; Persson, C.; Scragg, J.J.; Törndahl, T.; Edoff, M. Wide-gap (Ag,Cu)(In,Ga)Se2 solar cells with different buffer materials—A path to a better heterojunction. Prog. Photovolt. Res. Appl. 2020, 28, 237–250. [Google Scholar] [CrossRef] [Scilit]
- Keller, J.; Mudgal, S.; Martin, N.M.; Donzel-Gargand, O.; Edoff, M. Rubidium Fluoride Absorber Treatment for Wide-Gap and Bifacial Ag(In,Ga)Se2 Solar Cells. Sol. RRL 2025, 9, 2500423. [Google Scholar] [CrossRef] [Scilit]
- Kniese, R. Ladungstransport in Cu(In,Ga)Se2-Solarzellen Mit Unterschiedlichen Bandlückenenergien. Ph.D. Thesis, Universität Karlsruhe, Karlsruhe, Germany, 2005. [Google Scholar] [CrossRef]
- Yao, Y.; Ma, J.; Liu, Y.; Yang, X.; Meng, H.; Liu, F.; Zhang, Y.; Liu, W. Achieving over 860 mV Open-Circuit Voltage in Low-Ag Wide-Bandgap Cu(In,Ga)Se2 Solar Cells Through Ion Diffusion and Band Structure Optimization. Adv. Funct. Mater. 2025, 35, 2423228. [Google Scholar] [CrossRef] [Scilit]
- Kim, K.; Ahn, S.K.; Choi, J.H.; Yoo, J.; Eo, Y.-J.; Cho, J.-S.; Cho, A.; Gwak, J.; Song, S.; Cho, D.-H.; et al. Highly efficient Ag-alloyed Cu(In,Ga)Se2 solar cells with wide bandgaps and their application to chalcopyrite-based tandem solar cells. Nano Energy 2018, 48, 345–352. [Google Scholar] [CrossRef] [Scilit]
- Li, W.; Chen, L.; Wang, D.; Liang, B.; Shao, X.; Sun, Y.; Yang, C. Defect engineering via Ag and Na Co-doping in wide-bandgap CIGS: From interfacial suppression to bulk enhancement. Mater. Futur. 2025, 4, 45105. [Google Scholar] [CrossRef] [Scilit]
- Gutzler, R.; Song, C.-Y.; Hariskos, D.; Kempa, H.; Scheer, R.; Wuerz, R.; Ahlswede, E.; Paetel, S.; Witte, W. Assessment of transparent conductive oxides as back contacts for inline-fabricated Cu(In,Ga)Se2 solar cells. J. Phys. Energy 2025, 7, 45018. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.