Skip to Content
  • Feature Paper
  • Article
  • Open Access

9 July 2026

24 Pages

Utilization of Biomass Ash from Réunion Island as a Cementitious Binder

,
,
,
and
1
Univ Toulouse, INSA Toulouse, LMDC, 31400 Toulouse, France
2
Rhinnov Réunion, 97140 Saint-Pierre, France
3
Albioma Océan Indien, 97438 Sainte Marie, France
*
Author to whom correspondence should be addressed.

Abstract

Since 2024, most electricity production on Réunion Island has been achieved through combustion of biomass, using either imported wood pellets or locally produced bagasse. Their combustion generates two types of ash, depending on the biomass source: Wood Biomass Fly Ash (WBFA) and SugarCane Bagasse Ash (SCBA). Their chemical compositions differ significantly, leading to different potential applications. The composition of SCBA is similar to that of Coal Fly Ash (CFA), with low variability between batches. Therefore, SCBA could be used as an alternative to CFA, as a Supplementary Cementitious Material (SCM) or in composite cements. SCBA also meets most of the requirements of the NF EN 450-1 standard. However, grinding of SCBA appears necessary to achieve mechanical performance required by the standard. In contrast, WBFA exhibits variable chemical composition, mainly due to differences in pellet origin prior to combustion. Nevertheless, WBFA contains significant levels of chloride ions and sulfate, which may act as activators for materials such as GGBS or metakaolin (MK). Although the high unburned carbon content of WBFA increases water demand, their incorporation into GGBS-based binders (SSC or CEM III) or metakaolin-based systems shows promising potential, particularly for improving early strength.

1. Introduction

Since 2024, Réunion Island has produced the majority of its electricity from renewable energy sources [1]. The largest proportion comes from biomass combustion (~67%), using either wood pellets or bagasse. Before 2024, the most widely used energy sources were fossil fuels (particularly coal), which were responsible for significant carbon dioxide emissions, representing 42% in 2023 according to the General Commission for Sustainable Development [2]. Following this change in fuel, CO2 emissions from electricity production on Réunion Island decreased from 1.7 Mt to 0.2 Mt between 2022 and 2024 [3].
However, biomass combustion produces biomass ash, in the same way that coal combustion produces Coal Fly Ash (CFA). CFA can be utilized, particularly in the cement or concrete industry, provided that it complies with NF EN 197-1 and NF EN 450-1 standards, respectively [4,5]. However, no standard currently exists for the use of SugarCane Bagasse Ash (SCBA) or Wood Biomass Fly Ash (WBFA). Their use in cementitious binders would therefore offer two advantages: valorizing a by-product and reducing the consumption of clinker, which is responsible for nearly 10% of global CO2 emissions [6]. The aim of this paper is to explore potential uses of these two types of ashes in cementitious binders.
For SCBA, previous research has shown that it can be considered a pozzolanic material, due to its chemical composition, which is similar to that of CFA [7,8], and its amorphous content [9]. However, for WBFA, studies do not report a consistent chemical composition, with significant variability observed between samples, making comparison with CFA difficult [6].
Among the potential applications reported in the literature, biomass ashes can be used as SCMs, although this application is more commonly reported for SCBA [8,10,11] than for WBFA [6,12,13]. In addition, the use of WBFA in alkali-activated materials has been documented, particularly as a precursor [6,14,15]. However, thermal and/or mechanical treatment has been commonly applied to improve the reactivity of the ash [8,11,16,17,18,19,20]. Finally, several authors have used WBFA or SCBA in bricks [16,21,22] or as fillers in cementitious materials [23,24]. For this application, particularly in the case of WBFA, a washing process is generally carried out to remove soluble phases.
In the present study, both WBFA and SCBA will first be analyzed. The chemical composition and compliance with relevant standards will be discussed to differentiate potential applications depending on the ash type. The following two sections will focus on the potential applications of SCBA and WBFA, particularly in cementitious materials. Finally, in the discussion section, the first part will aim to explain the variability observed in WBFA, both in terms of chemical composition and differences observed at the binder level. The last point will be more methodological, addressing the determination of a more appropriate temperature for measuring loss on ignition in biomass ash.

2. Materials and Methods

2.1. Materials

The biomass ashes used in this study come exclusively from Réunion Island. Two types of ashes were studied: Wood Biomass Fly Ash (WBFA) and SugarCane Bagasse Ash (SCBA). WBFA is produced from the combustion of wood pellets sourced from various countries, including Australia, Canada, the United States of America (USA), Portugal, Malaysia, and Vietnam. SCBA is produced from the combustion of bagasse, a sugarcane residue. Unlike the pellets, all the bagasse is locally sourced from Réunion Island. The characterization of these two types of ashes is presented in the following sections.
Nevertheless, the production of WBFA and SCBA took place under the same conditions: the identical boiler, the same biomass combustion temperature, and the same sampling point. Only the production period varies, with SCBA being produced only between August and November, i.e., during the sugarcane harvesting season, while WBFA is produced continuously throughout the year.
To produce cementitious binders containing WBFA or SCBA, an Ordinary Portland Cement (OPC) compliant with EN 197-1 [4] was used (from Teralta, Le Port, France). To investigate the use of WBFA, two Supplementary Cementitious Materials (SCMs) were used: Ground Granulated Blast Furnace Slag (GGBS, from Teralta, compliant with NF EN 15167–1 [25]) and metakaolin (MK, from Argeco, Fumel, France; compliant with NF P18-513 [26]). Coal Fly Ash (CFA, from Teralta, Le Port, France; compliant with NF EN 450-1 [5]) was also used as a reference for comparison with SCBA. Other components were included in the binder compositions, described in Section 3.3.3, such as lime (from Lhoist, Sauveterre-la-Lémance, France) and plaster (from Sud Traitement Services, Saint Pierre, France). An inert siliceous filler (SF, from Sibelco, Durance, France) was also used in the preparation of biomass ash-based binders.

2.2. Methods

The chemical characterization of the ashes, WBFA or SCBA, was carried out using the same procedure, following the requirements of NF EN 450-1 [5] and NF EN 196-2 [27]. Loss on ignition (LOI) measurements were partly based on the recommendations of article 5.5.2 of NF EN 450-1 [5], using two combustion temperatures: 550 °C and 950 °C.
For X-ray diffraction (XRD), measurements were taken for one hour on ashes ground to 80 µm (WBFA or SCBA), over the angular range 2θ between 4° and 70°, with a step size of 0.02° and a counting time of 0.25 s per step.
Isothermal calorimetry tests were carried out on SCBA following the R3 protocol [28]: SCBA was mixed with calcium carbonate (CaCO3, ratio 1:3), calcium hydroxide (Ca(OH)2, ratio 1:0.5), and with a potassium solution (4 g/L KOH and 20 g/L K2SO4, ratio 1:5.4). For each SCBA, 15 g of paste were placed in a vial and inserted in the calorimeter for seven days at 40 °C. It should be noted that all the materials and vials were preconditioned at 40 °C before testing.
One selected SCBA was milled using a ball mill (TM300 from Retsch, Eragny, France), operating at a rotation speed of 60 rpm and with a ball/SCBA ratio of 10 by mass. Several milling times were tested: 5, 15, 30, 60, and 120 min. For each milling time, 200 g of dried raw SCBA was ground, without any water added in the mill.
The measurement of Strength Activity Index (SAI) was performed in accordance with point 5.3.2 of NF EN 450-1 [5]: standardized mortars with a water-to-binder ratio (W/B) of 0.5, containing 25% of ash (CFA or SCBA) and 75% of OPC. Standardized mixers were used for all SAI measurements, as well as for mortars containing WBFA. After casting, the mortars were stored at 20 °C and sealed to prevent water loss until the compressive strengths were performed (2 or 7 days, then 28 and 90 days depending on the binders/ash).

3. Results

3.1. Chemical Composition of Biomass Ashes

3.1.1. Chemical Composition

Figure 1 presents an overview of the chemical compositions obtained from biomass ashes: Wood Biomass Fly Ash (WBFA, 66 batches, Figure 1a) and SugarCane Bagasse Ash (SCBA, 16 batches, Figure 1b). For both types of ash, the results are presented as simplified box plots, showing the minimum, mean, and maximum values.
Figure 1. Chemical composition of (a) WBFA and (b) SCBA. Blue box plots = local data; red box plot = literature data [6,7,8].
The first observation concerns the difference in composition between WBFA and SCBA (more details on these compositions are provided below). Nevertheless, it should be noted that, despite identical production conditions (same boiler, same combustion temperature, same sampling point, etc.), two different types of biomass result in different chemical composition.
Depending on the batch, the WBFA composition varies greatly, but silica, calcium, and potassium oxides (see SiO2, CaO, and K2O) were the most prevalent, with average contents between 15% and 20% (see blue box plot in Figure 1a). Aluminum oxide and sulfate (Al2O3 and SO3) can also reach values close to 10%, whereas the other oxides were generally present at average levels below 5% (Fe2O3, Na2O, or P2O5), such as chloride ions (Cl−).
It should also be noted that there is significant variability between WBFA batches. For example, SiO2 content varied from 2.1% to 41.3%. All chemical elements exhibited this variability, with ratios ranging from 1 to 19 on average between the minimum and maximum values. A preliminary explanation will be given in Section 4.1, based on an analysis of the chemical composition of the pellets prior to combustion.
However, this variability is not specific to the WBFA produced locally; it has already been documented in the literature. For example, in their bibliographic review, Liang et al. [6] studied approximately 100 WBFA, summarized in Figure 1a (red box plot). They found that the SiO2 content varied between 2% and 55%. Similarly, for K2O, the values ranged from 4% to 31% for local WBFA and from 1% to 26% for WBFA reported in the literature. Furthermore, the average composition of local WBFA is consistent with the trends reported in the literature, with SiO2, CaO, and K2O as the dominant oxides [6].
Local SCBA were mainly composed of silica oxide (SiO2), with an average content of 50% (see blue box plot in Figure 1b). Aluminum and iron oxides (Al2O3 and Fe2O3) were also present in significant amounts, with average levels of around 15%. Calcium and magnesium oxides were detected in amounts below 5% (CaO and MgO). Traces of alkalis were also present, with levels below 1% for Na2O and 3% for K2O. Finally, sulfate and chloride (SO3 and Cl−) were detected at average contents below 0.5%.
A comparison with data from the literature reveals two major differences: local SCBA contains less SiO2 (49% compared to 70% on average), but higher contents of Al2O3 (14% compared to 7%) and Fe2O3 (14% compared to 4%). For the other elements, the average values are similar between the local SCBA and data reported in the literature (62 SCBA batches from review papers [7,8]).
In cases where biomass ashes are used as substitutes for Coal Fly Ash, NF EN 450-1 imposes criteria on the chemical composition of the ash [5]. To summarize these requirements, Table 1 presents the criteria specified by the standard and, for each type of ash, the percentage of samples that comply with these criteria.
Table 1. Compliance of WBFA and SCBA with NF EN 450-1—Chemical composition.
With SCBA, the criteria were generally met, with only one batch out of ten showing an excessively high magnesium oxide (MgO) content (0.1% above the limit value). However, WBFA did not comply with the requirements of NF EN 450-1, except for the criterion concerning phosphate oxide (P2O5). Thus, compared to the requirements of the standard, WBFA showed excessively high levels of magnesium oxide (MgO, 27% compliant) and alkalis (Na2Oeq, 14% compliant), and insufficient levels of silica, aluminum, and iron oxides (S + A + F, 3% compliant).

3.1.2. Loss on Ignition

Figure 2a shows the LOI of biomass ash for the two combustion temperatures studied: 550 °C and 950 °C (noted LOI550 and LOI950, respectively). As with the chemical compositions, the results are presented in simplified box plots (maximum, mean, and minimum values).
Figure 2. (a) Loss on ignition of WBFA and SCBA. (b) Compliance of WBFA with NF EN 450-1 according to TOC values.
In the case of WBFA, a higher temperature resulted in a higher average LOI, from an average of less than 10% at 550 °C to approximately 20% at 950 °C. There is significant variability between WBFA batches. At 550 °C, the LOI550 ranged from 0.3% to 77.1%, while at 950 °C, the range was from 4.0% to 65.8%. These high LOI values indicate incomplete combustion of the WBFA, which could cause problems when using WBFA in a cementitious binder, particularly due to increased water demand, as reported in the literature [12,23].
From a normative perspective, article 5.2.2 of NF EN 450-1 specifies that LOI950 must be less than 9% for WBFA to be used as an SCM [5]. Out of the 70 batches tested, only 13 met this criterion (~19%), confirming the difficulty of using WBFA as an alternative to CFA.
To complete these elements, Total Organic Carbon (TOC) measurements can also be used. According to NF EN 450-1, the objective of the article is to limit the residue of unburnt carbon in the fly ash. This standard allows TOC measurement to be used as a direct measurement of unburnt carbon residue [5]. Like LOI950, the TOC value must be less than 9% for the ash to comply with the standard. As shown in Figure 2b, of the 87 batches tested, 74% met this requirement (see “Cat A” + “Cat B” + “Cat C”).
This last point shows that LOI950 should perhaps not be considered for WBFA. While only 19% of batches complied with NF EN 450-1 based on LOI950, the use of TOC measurements, permitted by NF EN 450-1 as a substitute for LOI950, increased the proportion of compliant WBFA batches to 74% (see Figure 2b). This aspect is discussed in greater detail in Section 4.2, where an alternative to the 950 °C LOI test is proposed, based on additional thermogravimetric analysis (TGA) tests.
When the same study was carried out on SCBA, using fewer datasets (30 batches tested at 550 °C and 16 at 950 °C), lower LOI values were obtained: 4.3% and 6.8% on average at 550 °C and 950 °C (Figure 2a). By comparison, 8.2% and 19.9% were obtained with WBFA. Another significant difference is the lower variability observed for SCBA: the difference between minimum and maximum values was 13% at 550 °C and 15% at 950 °C with SCBA, compared to 62% and 77% for WBFA.
From a standard perspective, 82% of the 16 SCBA batches complied with the requirements of article 5.2.2 of NF EN 450-1 (LOI950 < 9%); this rate reached 100% for TOC measurements in the 24 batches tested (TOC < 9%).

3.1.3. Biomass Ashes Compared to Supplementary Cementitious Materials by Chemical Composition of CaO, SiO2, and Al2O3

The objective of this section is to present the potential applications of locally produced biomass ashes. To this end, following the approach proposed in the review by Liang et al. [6], Figure 3 presents the ternary diagram Al2O3-CaO-SiO2 for SCBA and WBFA. In addition to ashes, these diagrams show the regions typically occupied by Ordinary Portland Cement (OPC) and various SCMs (GGBS, Natural Pozzolan, coal fly ash).
Figure 3. Positioning of local (a) SCBA and (b) WBFA in the ternary diagram Al2O3–CaO–SiO2 and comparison with the literature [6,7,8].
Local SCBA is located at the boundary between Natural Pozzolan and Coal Fly Ash, with a cluster of data (see blue marks in Figure 3a), but the local cluster differs slightly from that found in the literature (red marks) [7,8]. Thus, in the following section, the objective will be to evaluate the use of SCBA as an SCM, particularly as a substitute for OPC. This investigation is presented in Section 3.2.
The WBFA data, both local and reported in the literature [6] (blue and red marks, respectively, in Figure 3b), do not form a cluster; instead, they are distributed across the left side of the diagram. This makes it difficult to find similarities between WBFA and OPC or SCMs. Therefore, considering both the high variability and the non-compliance with several NF EN 450-1 criteria, WBFA cannot easily be used as an SCM. In Section 3.3, several alternative approaches for using WBFA are investigated.

3.2. Use of SugarCane Bagasse Ash as a Supplementary Cementitious Material

Based on the chemical composition of SCBA, it was decided to investigate its use as an SCM, as a potential alternative to Coal Fly Ash (CFA). In this section, a more detailed characterization of SCBA is presented. Next, their potential for use as an SCM will be evaluated using a reactivity test (R3 calorimetry) and Strength Activity Index (SAI) measurements. This entire experimental campaign was conducted on 20 SCBA batches produced between 2023 and 2024. To evaluate the performance of SCBA, the same tests were carried out using a reference CFA, compliant with NF EN 450-1.

3.2.1. Mineralogy of SugarCane Bagasse Ash

Figure 4 shows some of the XRD spectra obtained from the 20 SCBA batches. Four batches are presented as examples, with the names of the batches corresponding to the SCBA production date. It can be seen that the four spectra were identical, showing the same peaks and similar intensities. This consistency was also observed for the other SCBA batches tested. The main phases identified were Anorthite (CaAl2Si2O8), Corundum (Al2O3), Cristobalite (SiO2), Forsterite (Mg2SiO4), Hematite (Fe2O3), Lime (CaO), Microcline (KAlSi3O8), Sanidine (KAlSi3O8), and Tridymite (SiO2). The presence of an amorphous phase is also indicated by the broad bump between 25 and 40° (see “Amorphous phase” in Figure 4).
Figure 4. XRD spectra of four local SCBA.
These phases are consistent with those reported in the literature [7,8,10,11,16,17]. However, these publications report the presence of quartz [7,8,10,11,16,17], which was not detected in the locally produced SCBA. The silica polymorphs identified here were cristobalite and tridymite. Regarding Al2O3, corundum was found in the local SCBA, whereas the literature mainly reports the presence of gibbsite (Al(OH)3) [8].
To supplement the above observations, a Rietveld analysis was performed on some SCBAs. The addition of fluorite, representing 9% of the SCBA mass, enabled the quantification of the amorphous content in the SCBA. Figure 5 summarizes these quantifications, showing relatively low variability between SCBA batches.
Figure 5. Mineralogical composition of local SCBA via Rietveld analysis.
The amorphous phase content also indicates pozzolanic potential for SCBA, with an average value of 27.9%, which is close to values reported in the literature for untreated SCBA [9,29]. Considering this pozzolanic potential and the similarity in chemical composition between SCBA and CFA, it remains relevant to investigate SCBA as an SCM.

3.2.2. Physical Characteristics

Figure 6 shows the particle size distributions of local SCBA and those reported for seven SCBA from other regions (Brazil, Thailand, Vietnam…) [29,30,31,32,33,34]. Rather than showing all the curves for the local SCBA, Figure 6 shows the average curve obtained for the 20 batches in green, with the particle size ranges obtained shown in transparency. Analysis of this range indicates relatively low variability in the locally produced SCBA, as evidenced by the relative width of the confidence interval for d50, which was less than 6% (d50: 26.4 ± 1.5 µm).
Figure 6. Particle size distribution curve of local SCBA and comparison with data from the literature [29,30,31,32,33,34].
A comparison between the particle size distributions of SCBA reported in the literature and the average curve obtained for the local SCBA reveals that the local SCBA had a finer particle size than most values reported in the literature. Only the SCBA studied by Chusilp et al. [32], derived from Thailand sugarcane, has a lower d50 (10 µm compared to an average of 26.4 µm for those from Réunion Island).
From a normative perspective, article 5.3.1 of NF EN 450-1 imposes a cumulative retention of less than 40% at a sieve size of 0.045 mm [5]. For each local SCBA, this cumulative residue was below the limit specified in the standard (21 ± 7%), which further supports the potential use of SCBA as a substitute for Coal Fly Ash.

3.2.3. Reactivity of SugarCane Bagasse Ash

In accordance with the R3 protocol [28], isothermal calorimetry tests were conducted. Figure 7a shows the heat flows obtained for four local SCBAs, corresponding to the same batches analyzed by XRD (see Figure 4). Among the batches tested, variability in the heat flow curves was observed, despite similar mineralogy (see Figure 4) and similar particle sizes (d50 between 23 and 29 µm, see Figure 6).
Figure 7. (a) Heat flow of four local SCBA and one CFA according to the R3 protocol. (b) Temporal evolution of the cumulative heat of local SCBA and comparison with CFA—Literature data from [28].
For SCBA batch 230810, a double hydration peak was obtained on the first day of hydration, with maximum intensities of 0.23 and 0.25 mW/g paste, respectively. For batch 230817, the pattern was identical, although the maximum intensities were lower (0.15 and 0.18 mW/gpaste, respectively). However, for the other two batches presented (241204a and 241204b), the pattern was different, with a first peak higher than the second.
Based on measured heat flows, Figure 7b presents an overview of the evolution of cumulative heat over time. The solid green line represents the average curve obtained from the 20 SCBAs tested. The band surrounding this line shows the range of cumulative heat values obtained. The evolution of the cumulative heat of the tested CFA is also shown (dotted orange line). Finally, at 7 days, the data collected by Londono-Zuluaga et al. are included [28]. These data correspond to eight CFA samples and are presented as a simplified box plot, showing the maximum, mean, and minimum values.
By comparing the average trend obtained with local SCBA and the evolution of the tested CFA, a similarity in their evolution can be observed. For local SCBA, the range showed significant variability, with values between 52 and 175 J/gSCM at 24 h and between 200 and 316 J/gSCM at 7 days, for example. However, this variability was also observed for the CFA reported by Londono-Zuluaga et al., with cumulative heat ranging from 166 to 362 J/gSCM at 7 days [28]. Furthermore, the average values are comparable, with 289 J/gSCM for the local SCBA and 285 J/gSCM for the reported CFA.

3.2.4. Strength Activity Index (SAI)

Figure 8a shows the compressive strengths of standardized mortars made with SCBA or CFA, as well as the reference OPC mortar (the complete dataset appears in Appendix A). After two days, the OPC mortar had a compressive strength (fc,2d) of 27.6 MPa compared to 23.7 MPa with 25% CFA (SAI2d = 82.7%, see Figure 8b). The fc,2d values of OPC/SCBA mortars ranged from 15.0 to 24.5 MPa, with an average of 18.8 MPa (SAI2d = 65.8%). The calculation of SAI2d showed that 12 out of the 20 SCBAs can be considered inert, i.e., with SAI2d values lower than 67%.
Figure 8. Impact of SCBA incorporation (a) on the compressive strength of standard mortars and (b) on the Strength Activity Index of the ash. The horizontal line represents the minimum limit defined by the EN 450-1 standard.
At 28 days, the fc,28d of OPC/SCBA mortars ranged from 36.5 to 55.4 MPa. The reference mortar reached 62.1 MPa, while the mortar containing 25% CFA reached 50.7 MPa (SAI28d = 81.7%). According to NF EN 450-1 [5], mortars containing ash must reach 75% of the fc,28d of OPC mortar. Thus, 3 of the 20 SCBA batches tested met this criterion. In addition, seven mortars had an SAI28d lower than 67%, meaning that the SCBA could be considered inert.
In the literature, raw SCBA, i.e., without thermal activation or additional grinding, also shows SAI28d values below the standard requirements [17,18,20]. Local SCBA even appeared to exhibit higher SAI28d values than those reported in the compiled literature data.
Finally, at 90 days, the fc,90d ranged from 35.4 MPa to 65.6 MPa, compared to 70.6 MPa for the reference mortar and 56.6 MPa for the mortar with CFA (SAI90d = 80.2%). At this age, the SAI90d must reach 85% according to NF EN 450-1 [5], which means that only one SCBA batch met this criterion (SAI90d = 93% maximum, with an average value of 72.0%). For the other batches, this limit was not reached, with values often lower than those obtained with CFA. As at 28 days, six SCBA batches can even be considered inert.
In summary, bagasse ash from Réunion Island does not meet the mechanical requirements of the NF EN 450-1 standard, with SAI values lower than required at 28 and 90 days. To improve SAI values, thermal activation [17,18,19,20] and additional grinding [11,16,17,18,19] of SCBA are the most commonly investigated approaches in the literature. In the present study, grinding of SCBA was therefore implemented to improve its reactivity, and the results are presented in the following section.

3.2.5. Grinding of SugarCane Bagasse Ash

Physical Properties and Mineral Composition
Following the previous results, one batch of SCBA was milled to enhance its reactivity and ensure compliance with article 5.3.2 of NF EN 450-1 [5]. To evaluate the effectiveness of the milling process, the SCBA sample with the lowest reactivity and a low SAI was selected.
Figure 9a illustrates the evolution of particle size as a function of grinding time. A significant refinement was observed, indicated by a shift in the particle size distribution curve toward smaller diameters. Specifically, the median particle size (d50) decreased from 26.66 µm for the reference SCBA to 9.63 µm after 120 min of grinding. The cumulative retained at a sieve size of 0.045 mm also decreased from 25% to 0.5% after 120 min.
Figure 9. (a) Particle size distribution curve and (b) XRD spectrum of ground SCBA.
It was considered pertinent to verify whether the mineralogy of the SCBA was affected by the grinding process. An X-ray diffraction (XRD) analysis was performed on the SCBA with the longest grinding time (i.e., 120 min). The result, shown in Figure 9b, validates this aspect, as the spectra were similar before/after grinding.
Calorimetry Tests and Strength Activity Index
Figure 10a presents the heat flow obtained during the R3 test for the raw SCBA (Raw) and four milled samples (5 min, 15 min, 60 min, and 120 min). For the raw SCBA, the main peak reached 0.11 mW/g. After grinding, an increase in heat flow was observed, accompanied by an approximate doubling of the peak intensity. For example, after 120 min of grinding, the first peak had an intensity of 0.17 mW/g, and the main peak reached 0.18 mW/g.
Figure 10. (a) Heat flow of ground SCBA and CFA according to the R3 protocol. (b) Impact of grinding time of SCBA on the cumulative heat.
For comparison, the heat flow curve obtained with CFA is also shown in Figure 10a. The CFA also exhibited a double-peak structure, but with the second peak more intense than the first. Nevertheless, the shape of the heat flow curve is comparable to that of the SCBA milled for 120 min.
Figure 10b shows the evolution of cumulative heat at different ages (1, 2, and 7 days) as a function of SCBA grinding time. For the three ages, the value obtained with CFA is also shown (see orange dotted line). Regardless of the age considered, the longer the grinding time, the higher the cumulative heat. Thus, compared to the raw SCBA, grinding for 120 min resulted in increases of +48, +50, and +79 J/gSCM at 1, 2, and 7 days, respectively. Finally, after 120 min of grinding, the cumulative heat values approach those obtained with CFA.
Figure 11 shows the evolution of the SAI as a function of grinding time at 2, 28, and 90 days. At two days (see Figure 11a), the raw SCBA had an SAI2d of 63%, with the SCBA considered inert (i.e., <67%). Grinding the SCBA increased this SAI2d to over 80%; the longer the grinding time, the higher the SAI2d. After 15 min, the SCBA was no longer considered inert, but 120 min of grinding was required to achieve the SAI2d of CFA (≈80%).
Figure 11. Impact of grinding time of SCBA on Strength Activity Index at (a) 2 days, (b) 28 days and (c) 90 days.
At 28 days, the two conclusions observed at 2 days were confirmed: without grinding, SAI28d was too low for the requirements of the standard (63% compared to the required 75%, see red line), and grinding time had a positive effect on SAI28d (see Figure 11b). To reach the required 75%, grinding must be carried out for more than 30 min: 72% was obtained after 30 min, and 80% after 60 min. The CFA exhibits an SAI28d similar to that of an SCBA milled for 60 min (i.e., 83%), while milling for 120 min provided the highest value (i.e., 89%).
At 90 days, the standard requires an SAI90d of 85%. This level was only achieved with an SCBA milled for 120 min (i.e., 88%). While 60 min of milling was sufficient at 28 days, this duration resulted in an SAI90d of 83%. However, it should be noted that this value is similar to that obtained with CFA, which would indicate that the tested CFA would not comply with NF EN 450-1.

3.3. Use of Wood Biomass Fly Ash as Activator

In Section 3.1, it has been shown that WBFA has a chemical composition very different from that of CFA or SCBA, which makes their use as an SCM complex. Furthermore, the variability of this composition could make the repeatability of results at the mortar/concrete scale uncertain. After a more detailed mineralogical analysis to identify possible activation mechanisms, several types of binders containing WBFA will be tested.

3.3.1. Mineralogy of Wood Biomass Fly Ash

In addition to the chemical composition of the WBFA (see Figure 1a), XRD tests were carried out to determine their mineralogy. Rather than detailing each batch individually, Figure 12 presents the spectra of three WBFA (250204, 250304, and 250312) and allows for an initial analysis. These three WBFA were deliberately chosen because they were produced during the same period, between February and March 2025.
Figure 12. XRD spectra of three local WBFA.
Figure 12 also shows the main phases identified in the spectra: Arcanite (K2SO4), Calcite (CaCO3), Hematite (Fe2O3), Lime (CaO), Periclase (MgO), Portlandite (Ca(OH)2), Quartz (SiO2), and Sylvite (KCl). In the scientific literature, similar phases have been identified, as highlighted in the review by Liang et al. [6]. Of the 27 articles analyzed by the authors, Arcanite, Calcite, Hematite, Lime, Periclase, Portlandite, Quartz and Sylvite were detected in 24%, 85%, 10%, 60%, 44%, 56%, 76% and 20% of compiled WBFA, respectively.
Among the other phases identified, and not detected in local WBFA, were Anhydrite, Larnite, Fairchildite, Gehlenite, Wollastonite, Halite or Syngenite, but these were reported in less than 10% of the analyzed papers.
Moreover, in some batches, a hydrated mineral appears to be present (Hydrate Ca8Al2Fe2O12CO3(OH)2·22H2O, see batch 250212). This could be due to excessive humidification of the WBFA at the boiler outlet.
Each batch shows a relatively different XRD spectrum. For example, Portlandite and the Hydrate phase were only present in batch 250212. In contrast, Quartz was only detected in batch 250304. The other phases (Arcanite, Calcite, Hematite, and Sylvite) were present in all three batches, but in varying proportions.
A semi-quantitative analysis via Rietveld refinement was performed on 19 WBFA batches, considering only the crystallized mineral. Figure 13 provides a summary of these approximate quantifications.
Figure 13. Mineralogical composition of local WBFA using Rietveld analysis.
To make the analysis clearer, some phases were grouped and represented with similar colors. This is the case, for example, with the soluble salts Arcanite and Sylvite. The other groups are as follows: Lime/Portlandite/Periclase and Calcite/Hematite/Quartz.
Variability in mineralogy was again very high, as already observed for the chemical composition. For example, the alkaline phases, Arcanite and Sylvite, represent on average 40% of the phases, but this ranges from 16% to 85% depending on the batch. The same observation applies to the Lime/Portlandite/Periclase group (22% on average, ranging from 6% to 36%) and the Calcite/Hematite/Quartz group (38.6% on average, ranging from 12% to 66%).

3.3.2. Sulfate and Chloride Contents in Wood Biomass Fly Ash

Mineralogical analyses have shown the presence of significant quantities of Arcanite and Sylvite (K2SO4 and KCl), making it relevant to study the content of sulfate and chloride ions (SO3 and Cl−, respectively) in WBFA. The summary of this study is presented in Figure 14, based on 154 batches of local WBFA.
Figure 14. Chloride and sulfate ion content in local WBFA.
In line with the chemical composition of WBFA (see Figure 1a) and their mineralogy (see Figure 13), the first observation concerns the high variability: from 0.12% to 10.80% for chlorides Cl−, and from 0.13% to 18.30% for sulfates SO3. This variability is not specific to local WBFA, as several authors have reported similar ranges when studying WBFA [6,23,35].
An “average” WBFA would have chloride/sulfate contents of 2.15% and 4.25% respectively. For comparison, an “average” SCBA would have contents of 0.07% and 0.43% (based on 20 batches), while the CFA studied showed contents of 0.09% and 1.77%. As with the other chemical elements, there is a clear compositional difference between WBFA and SCBA.
Finally, it is interesting to analyze two other aspects of the NF EN 450-1 standard: compliant ash must have Cl− and SO3 contents below 0.10% and 3.00%, respectively. Of the batches tested, none of the WBFA batches met the chloride criterion, and only 17 batches had a sulfate content compliant with the standard, i.e., fewer than 30% of the WBFA batches. These elements once again highlight the difficulty of using WBFA as a substitute for CFA, as an SCM or in cement compliant with NF EN 197-1.
Nevertheless, these high chloride and sulfate levels suggest another possible application. The literature has already documented the positive effect of these ions on the activation of cementitious binders, whether GGBS-based or not. It was therefore this approach that was explored in the remainder of the study.

3.3.3. Introduction of Wood Biomass Fly Ash in Cementitious Binders

Three different types of binders were produced to incorporate WBFA. The first was a supersulfated cement (SSC), the second an equivalent of CEM III/C (GGBS/OPC), and the third a metakaolin/lime/plaster-based binder. All the compositions are listed in Table 2.
Table 2. Composition of binders containing WBFA.
For SSC, starting from an initial composition of 75% GGBS, 20% plaster, and 5% OPC, the binders produced were composed of 75%, 15%, and 5%, respectively. Thus, 5% of the plaster was replaced with 5% WBFA. This choice ensures compliance with the composition limits of standard NF EN 15,743 [36].
Next, for the CEM III/C equivalent binder, it was decided to replace 10% of OPC with WBFA. Thus, the initial formula corresponded to a mixture of 70% GGBS and 30% OPC, while the mixture containing WBFA was composed of 70%, 20% and 10% WBFA.
For the last binder (called MkLiPl), the procedure was identical: the initial binder was composed of 60% MK, 25% lime, and 15% plaster; the binder containing WBFA was composed of 54%, 22.5%, and 13.5%, respectively, with the addition of 10% WBFA.
For each binder, seven batches of WBFA were tested. These batches, illustrated in Figure 14, provided an overview of the range of chloride and sulfate contents observed throughout the study. The same formulations were also prepared by replacing WBFA with a siliceous filler (SF), allowing evaluation of whether WBFA incorporation produced a real effect or only a dilution effect on the reference binder.
The reference SSC achieved a 7-day compressive strength (fc,7d) of 8 MPa (see Figure 15a). The addition of WBFA had a positive effect, with fc,7d reaching an average of 16 MPa. With SSC, the effect of WBFA was positive, since the SSC containing SF only reached 15 MPa, which is nevertheless higher than the reference SSC. It should be noted that there was variability depending on the WBFA batch, as shown by the standard deviation (~1.6 MPa). This variability will be examined in more detail in Section 4.3.
Figure 15. Compressive strength of mortars containing WBFA at (a) 2/7 days and (b) 28 days.
At 28 days, the incorporation of WBFA had a negative effect, since the reference SSC had the highest fc,28d: 33.4 MPa for the reference mortar and 22.4 MPa on average for WBFA (Figure 15b). It even appears that WBFA had a deleterious effect, as the values obtained were lower than those of the SSC containing filler (29.1 MPa).
For the GGBS/OPC binder, the impact of WBFA was also positive at two days: 6.1 MPa for the reference mortar compared to 6.9 MPa with 10% WBFA (Figure 15a). As with SSC, WBFA did not simply produce a dilution effect, since the mortar containing SF reached 4.3 MPa. Again, variability was observed in fc,2d, which will be discussed in Section 4.3. At 28 days, similar conclusions were observed: a negative contribution of WBFA (40.1 MPa for the reference compared to 37.0 MPa with WBFA, see Figure 15b) and slight variability depending on the WBFA batch.
For MkLiPl binder, the fc,2d values were similar: 1.2 MPa for the reference, 0.9 MPa with WBFA, and 1.6 MPa with SF (Figure 15a). The small differences did not allow any clear conclusion regarding a positive impact of WBFA. However, at 28 days, the use of WBFA appeared beneficial: on average 21.3 MPa for the reference mortar, 21.8 MPa for the mortar containing 10% SF, and 25.3 MPa for the mortar containing 10% WBFA. Again, depending on the WBFA batch, there was some variability in the fc,28d, which will be discussed in Section 4.3.

4. Discussion

4.1. Understanding the Variability in Compositions

In order to explain the variability obtained at the WBFA level, particularly regarding their chemical composition, it seems relevant to examine the pellets prior to combustion. The data provided by pellet suppliers were processed, particularly the contents of chlorine, sulfur, and alkalis (sodium and potassium). This choice was made because the WBFA analyses revealed variability in chloride and sulfate contents (see Figure 14), as well as in alkali oxide (Figure 1a). Since the pellets used for combustion originated from different sources (Australia, Canada, the United States, Portugal, Malaysia and Vietnam), the data were grouped according to their source.
First, Figure 16 shows the chlorine, sulfur, and alkali contents according to the pellet source. For chlorine, clear differences were observed. The pellets with the lowest chlorine contents came from Australia, Canada, and the United States, with values generally below 0.01%. In contrast, pellets from Asia (Malaysia/Vietnam) contained the highest levels of chlorine, with values reaching up to 0.05%.
Figure 16. Chlorine, sulfur and alkaline content in wood pellets.
For sulfur, similar trends were observed, with levels ranging from 0.01% (Australia, Canada) to over 0.04% (Malaysia). It should also be noted that pellets from the United States and Vietnam showed some variability in sulfur content.
Finally, regarding alkaline content, the differences depending on origin were even more pronounced, with pellets from Australia, Malaysia, the United States, and Vietnam having the highest content. There was a factor of five between the pellets with the lowest alkali content and those with the highest levels (ranging from 0.04% to 0.20%).
These last paragraphs showed that the variability observed at the WBFA level also exists at the pellet level. In order to confirm the link between pellets and WBFA, Figure 17 shows the temporal evolution of the chlorine/chloride (Figure 17a), sulfur/sulfate (Figure 17b), and alkali (Figure 17c) contents in pellets and WBFA. To capture representative trends, the data covers the years 2024 and 2025, including more than 60 pellet samples and approximately 150 WBFA batches. It should be noted that the shipment dates correspond to the introduction of pellets into the silos, while the dates of the WBFA correspond to the day of pellet combustion.
Figure 17. Chlorine, sulfur and alkaline content in wood pellets.
Comparing the temporal evolution of chlorine content in pellets with the chloride ion content in WBFA revealed a certain level of correlation (see Figure 17a). For instance, most increases in chloride content in WBFA coincide with the arrival of pellets containing high chlorine levels. This trend was particularly evident around May 2024, September 2024, and May 2025.
The variations in sulfur and sulfate levels were also similar, but to a lesser extent. Again, during the same three periods, increases in sulfate levels in WBFA appeared to correspond to the introduction of pellets with higher sulfur content. This correlation also appeared to hold for the alkali content measured in the pellets and in the resulting WBFA.
This section has therefore provided, at least partially, an explanation for the variability observed in the chemical composition of WBFA through analysis at the pellet level. The high variability in pellet composition directly affects the properties of the resulting ash, despite the pellets being burned. To further understand the mechanisms involved, it would be interesting to continue the analysis by studying, for example, the types of wood (and the soil where the wood grew) used to produce pellets in each country.

4.2. Determination of the Optimal Temperature for the LOI Test

The NF EN 450-1 standard requires the measurement of LOI at 950 °C [5]. When this temperature is applied to WBFA, only 13 of the 70 batches tested comply with article 5.2.2, i.e., 19%. As explained in Section 3.1.2, TOC measurement can be used as an alternative to LOI950, allowing 72% of WBFA batches to comply with the requirements of the standard (see Figure 2b).
However, this test is more complex to perform than an LOI measurement. In the following, an alternative to LOI950 is proposed for WBFA. This temperature selection was made based on XRD and TGA tests. Examination of the TGA curves of four WBFA samples shows that water loss occurs around 450 °C, corresponding to the decomposition temperature of Portlandite [37] and/or the oxidation of organic carbon [38] (see Figure 18). After 600 °C, another peak appears in all WBFA samples, with varying intensity. This peak corresponds mainly to the decarbonation of calcite [37,38], also identified by XRD.
Figure 18. Thermogravimetric curve of four local WBFA.
However, calcite cannot be considered organic carbon, because it does not contain hydrogen atoms. Therefore, the mass loss resulting from its decarbonation is not taken into account in TOC measurements, which explains why more WBFA batches comply with the TOC requirement than with LOI950.
Based on this assumption, the LOI measurement for WBFA could be carried out at 550 °C, allowing complete decomposition of organic carbon while excluding the contribution of inorganic carbon such as calcite. Using this approach, and taking a maximum acceptable value of 9% as for LOI950 or TOC, 76% of the 186 batches tested would comply with the criterion when using LOI at 550 °C. This number greatly exceeds the value obtained at 950 °C (i.e., 19% out of 70 batches) and is close to that obtained using TOC (i.e., 72% out of 82 batches).
Finally, to validate the relationship between TOC and LOI550, Figure 19 shows the relationship between these two datasets. There appears to be a proportional relationship between these two quantities (LOI550/TOC = 1.04), with a very high coefficient of determination (R2 = 0.97). These data therefore illustrate a possible alternative to the LOI950 measurement for WBFA.
Figure 19. Correlation between TOC values and LOI550 for WBFA.

4.3. Impact of Chloride/Sulphate Content on WBFA Binders

To better understand the role of Cl− and SO3 ions in the hydration of the tested binders, Figure 20 shows the strength gains obtained as a function of the Cl−/SO3 contents in the WBFA. The gains in fc were calculated relative to the mixture containing the siliceous filler (SF), which is indicated at the top of each figure.
Figure 20. Impact of chloride and sulfate contents on (a) 24-h and (d) 28-day compressive strength gains in SSC mortars. Also applies to (b,e) GgbsOpc and (c,f) MkliPl mortars.
For example, for SSC at 7 days (Figure 20a), the mortar containing SF achieved an fc,7d of 14.75 MPa. Using WBFA containing 4.45% Cl− and 4.56% SO3, the gain was +3.39 MPa compared with the mortar containing SF. Looking at the data as a whole, two groups of WBFA can be distinguished: when the SO3 content is less than 6%, an increase in fc,7d is observed (~+2.5 MPa), whereas values similar to those obtained with SSC containing SF are observed for WBFA with an SO3 content higher than this value. The impact of chlorides appears to be positive, since for the same SO3 content, WBFA with higher Cl− levels results in higher fc,7d.
At 28 days, compared with SF, WBFA has a negative effect, with losses ranging from −4.4 to −10.0 MPa (see Figure 20d). As at 7 days, the WBFA performing best are those with lower Cl−/SO3 contents, although the gains remain negative compared with SF, whereas they were positive at 7 days.
For the GGBS/OPC binder, the conclusions after two days were different from those for SSC. Here, WBFA containing the highest SO3 content maximized fc,2d, with average gains of +3.2 MPa when the SO3 content was above 6%, compared with +1.8 MPa when it was below this value. The impact of Cl− ions was also different from what was observed for SSC: at the same SO3 content, WBFA with higher chloride resulted in lower fc,2d values.
At 28 days, all gains were negative, with values ranging from −2.7 to −6.7 MPa depending on the WBFA batch, compared to 41.7 MPa obtained using SF (see Figure 20e). It is more difficult to draw conclusions here, because the maximum and minimum gains were obtained for WBFA with similar chloride/sulfate contents: −2.7 MPa for WBFA with 6.77%/9.13% and −6.7 MPa for the most concentrated WBFA (9.62%/13.42%).
Finally, concerning the MkLiPl binder, considering the very low fc,2d values, which were consistently below 1.5 MPa, it is difficult to draw any conclusions (see Figure 20c). At 28 days, an fc,28d of 21.8 MPa was obtained for the mixture containing 10% SF. Using WBFA, strength gains were consistently observed, ranging from +0.1 to +8.4 MPa. There also appeared to be a dependence on Cl−/SO3 levels: the higher the contents, the lower the strength gains. Optimum gains were obtained for WBFA with a Cl− content slightly below 2%. However, it appeared that excessively low contents also resulted in lower gains (see +3.8 MPa in Figure 20f).

5. Conclusions

This study investigated the possibility of using biomass ash from Reunion Island in cementitious binders. Two types of ash were studied: Wood Biomass Fly Ash (WBFA) and Sugarcane Bagasse Ash (SCBA). The following conclusions can be drawn:
  • The mineralogical composition and potential uses depend on the type of biomass, i.e., pellet or bagasse. Moreover, even for the same type of biomass, the properties of the ash depend strongly on the characteristics of the biomass.
  • Local SCBA has a chemical composition similar to Coal Fly Ash (CFA), validating most of the requirements of the NF EN 450-1 standard. In addition, SCBA contains a significant amorphous phase, indicating its potential use as a Supplementary Cementitious Material (SCM).
  • However, grinding SCBA appears necessary to achieve mechanical strength consistent with the requirements of the standard, thereby enabling its use in cementitious binders.
  • For WBFA, in addition to large variability in chemical composition between batches, it seems difficult to compare it with cement or standardized SCMs. Furthermore, WBFA frequently fails to meet the requirements of the standard.
  • On the other hand, WBFA contains relatively high concentrations of sulfate and chloride ions, which can contribute to the activation of cementitious binders. Tests have shown the beneficial effect of these ions on the early-age strength of supersulfated cement or CEM III type cement.

Author Contributions

Conceptualization, M.P., P.D., L.P. and M.C.; methodology, M.P., P.D., L.P. and M.C.; validation, P.D., L.P. and M.C.; formal analysis, M.P. and M.C.; investigation, M.P.; writing—original draft preparation, M.P.; writing—review and editing, P.D., L.P., N.N. and M.C.; visualization, M.P.; supervision, P.D., L.P., N.N. and M.C.; project administration, P.D., L.P., N.N. and M.C.; funding acquisition, M.C. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Data Availability Statement

The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding author.

Conflicts of Interest

Mathieu Pellerano, Pierrick Dupuy and Laurent Poulizac are currently employed at RHINNOV Réunion, and Nelly Noel is currently employed at Albioma. All authors declare no conflict of interest.

Appendix A

Table A1. Compressive strength and the Strength Activity Index of OPC, OPC + CFA and OPC + SCBA mortars.

References

  1. Observatoire Energie Réunion, Production d’Electricité|Observatoire Énergie Réunion. (n.d.). Available online: https://oer.energies-reunion.com/electricite/production-electricite-la-reunion (accessed on 1 April 2026).
  2. General Commission for Sustainable Development, Global Overview of GHG Emissions, Clim. Change Obs.—2025 Ed. Available online: https://www.statistiques.developpement-durable.gouv.fr/edition-numerique/2025/chiffres-cles-du-climat/en/6-global-overview-of-ghg-emissions.php (accessed on 1 April 2026).
  3. Observatoire Energie Réunion, CO2 Issu de la Combustion de Produits Énergétiques|Observatoire Énergie Réunion. Available online: https://oer.energies-reunion.com/emissions-de-ges/co2-combustion-produits-energetiques (accessed on 1 April 2026).
  4. AFNOR, NF EN 197-1; Cement—Part 1: Composition, Specifications and Conformity Criteria for Common Cements. 2012. Available online: https://www.boutique.afnor.org/en-gb/standard/nf-en-1971/cement-part-1-composition-specifications-and-conformity-criteria-for-common/fa149898/1234 (accessed on 1 April 2026).
  5. AFNOR, NF EN 450-1: Fly Ash for Concrete—Part 1: Definition, Specifications and Conformity Criteria, (2012). Available online: https://www.boutique.afnor.org/en-gb/standard/nf-en-4501/fly-ash-for-concrete-part-1-definition-specifications-and-conformity-criter/fa166018/40053 (accessed on 1 April 2026).
  6. Liang, X.; Li, Z.; Dong, H.; Ye, G. A review on the characteristics of wood biomass fly ash and their influences on the valorization in cementitious materials. J. Build. Eng. 2024, 97, 110927. [Google Scholar] [CrossRef] [Scilit]
  7. Thomas, B.S.; Yang, J.; Bahurudeen, A.; Abdalla, J.A.; Hawileh, R.A.; Hamada, H.M.; Nazar, S.; Jittin, V.; Ashish, D.K. Sugarcane bagasse ash as supplementary cementitious material in concrete—A review. Mater. Today Sustain. 2021, 15, 100086. [Google Scholar] [CrossRef] [Scilit]
  8. Yadav, A.L.; Sairam, V.; Muruganandam, L.; Srinivasan, K. An overview of the influences of mechanical and chemical processing on sugarcane bagasse ash characterisation as a supplementary cementitious material. J. Clean. Prod. 2020, 245, 118854. [Google Scholar] [CrossRef] [Scilit]
  9. Xu, Q.; Ji, T.; Gao, S.-J.; Yang, Z.; Wu, N. Characteristics and Applications of Sugar Cane Bagasse Ash Waste in Cementitious Materials. Materials 2019, 12, 39. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  10. Batool, F.; Masood, A.; Ali, M. Characterization of Sugarcane Bagasse Ash as Pozzolan and Influence on Concrete Properties. Arab. J. Sci. Eng. 2020, 45, 3891–3900. [Google Scholar] [CrossRef] [Scilit]
  11. Francioso, V.; Lemos-Micolta, E.D.; Elgaali, H.H.; Moro, C.; Rojas-Manzano, M.A.; Velay-Lizancos, M. Valorization of Sugarcane Bagasse Ash as an Alternative SCM: Effect of Particle Size, Temperature-Crossover Effect Mitigation & Cost Analysis. Sustainability 2024, 16, 9370. [Google Scholar] [CrossRef] [Scilit]
  12. Dossa, J.G.; Page, J.; Vanhove, Y.; Djelal, C. Influence of using wood biomass fly ash as filler on the rheological and physical properties of cementitious pastes. J. Build. Eng. 2025, 114, 114361. [Google Scholar] [CrossRef] [Scilit]
  13. Carević, I.; Bajto, J.Š.; Grubor, M.; Štirmer, N. Wood biomass ash as a clinker substitute in advancing next-generation blended cement: Croatian case study. Sci. Rep. 2026. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  14. Ates, F.; Park, K.T.; Kim, K.W.; Woo, B.-H.; Kim, H.G. Effects of treated biomass wood fly ash as a partial substitute for fly ash in a geopolymer mortar system. Constr. Build. Mater. 2023, 376, 131063. [Google Scholar] [CrossRef] [Scilit]
  15. De Rossi, A.; Simão, L.; Ribeiro, M.J.; Hotza, D.; Moreira, R.F.P.M. Study of cure conditions effect on the properties of wood biomass fly ash geopolymers. J. Mater. Res. Technol. 2020, 9, 7518–7528. [Google Scholar] [CrossRef] [Scilit]
  16. Alavéz-Ramírez, R.; Montes-García, P.; Martínez-Reyes, J.; Altamirano-Juárez, D.C.; Gochi-Ponce, Y. The use of sugarcane bagasse ash and lime to improve the durability and mechanical properties of compacted soil blocks. Constr. Build. Mater. 2012, 34, 296–305. [Google Scholar] [CrossRef] [Scilit]
  17. Bahurudeen, A.; Santhanam, M. Influence of different processing methods on the pozzolanic performance of sugarcane bagasse ash. Cem. Concr. Compos. 2015, 56, 32–45. [Google Scholar] [CrossRef] [Scilit]
  18. Bayapureddy, Y.; Muniraj, K.; reddy Gangireddy Mutukuru, M. Enhancing material properties of agro-industrial waste sugarcane bagasse ash—Way towards sustainable development. Sustain. Futur. 2024, 7, 100154. [Google Scholar] [CrossRef] [Scilit]
  19. Martins Torres, S.; Estolano de Lima, V.; de Azevedo Basto, P.; de Araújo Júnior, N.T.; de Melo Neto, A.A. Assessing the pozzolanic activity of sugarcane bagasse ash using X-ray diffraction. Constr. Build. Mater. 2020, 264, 120684. [Google Scholar] [CrossRef] [Scilit]
  20. Patil, C.; Manjunath, M.; Hosamane, S.; Bandekar, S.; Athani, R. Pozzolonic activity and strength activity index of bagasse ash and fly ash blended cement mortar. Mater. Today Proc. 2021, 42, 1456–1461. [Google Scholar] [CrossRef] [Scilit]
  21. Balagosa, J.A.; Lee, M.J.; Choo, Y.W.; Kim, H.S.; Kim, J.M. Effect of wood pellet fly ash on strength and microstructure of Korean weathered granite soil. Geomech. Eng. 2024, 38, 335–352. [Google Scholar] [CrossRef]
  22. Kazmi, S.M.S.; Abbas, S.; Saleem, M.A.; Munir, M.J.; Khitab, A. Manufacturing of sustainable clay bricks: Utilization of waste sugarcane bagasse and rice husk ashes. Constr. Build. Mater. 2016, 120, 29–41. [Google Scholar] [CrossRef] [Scilit]
  23. Berra, M.; Mangialardi, T.; Paolini, A.E. Reuse of woody biomass fly ash in cement-based materials. Constr. Build. Mater. 2015, 76, 286–296. [Google Scholar] [CrossRef] [Scilit]
  24. Moretti, J.P.; S. Nunes, A. Sales, Self-compacting concrete incorporating sugarcane bagasse ash. Constr. Build. Mater. 2018, 172, 635–649. [Google Scholar] [CrossRef] [Scilit]
  25. AFNOR, NF EN 15167-1: Ground Granulated Blast Furnace Slag for Use in Concrete, Mortar and Grout—Part 1: Definitions, Specifications and Conformity Criteria. 2006. Available online: https://www.boutique.afnor.org/en-gb/standard/nf-en-151671/ground-granulated-blast-furnace-slag-for-use-in-concrete-mortar-and-grout-p/fa137602/28082 (accessed on 1 April 2026).
  26. AFNOR, NF P18-513: Addition for Concrete—Metakaolin—Specifications and Conformity Criteria. 2012. Available online: https://www.boutique.afnor.org/en-gb/standard/nf-p18513/addition-for-concrete-metakaolin-specifications-and-conformity-criteria/fa175740/39605 (accessed on 1 April 2026).
  27. AFNOR, NF EN 196-2: Methods of Testing Cement—Part 2: Chemical Analysis of Cement. 2013. Available online: https://www.boutique.afnor.org/en-gb/standard/nf-en-1962/methods-of-testing-cement-part-2-chemical-analysis-of-cement/fa178507/41905 (accessed on 1 April 2026).
  28. Londono-Zuluaga, D.; Gholizadeh-Vayghan, A.; Winnefeld, F.; Avet, F.; Ben Haha, M.; Bernal, S.A.; Cizer, Ö.; Cyr, M.; Dolenec, S.; Durdzinski, P.; et al. Report of RILEM TC 267-TRM phase 3: Validation of the R3 reactivity test across a wide range of materials. Mater. Struct. 2022, 55, 142. [Google Scholar] [CrossRef] [Scilit]
  29. Cordeiro, G.C.; Tavares, L.M.; Toled o Filho, R.D. Improved pozzolanic activity of sugar cane bagasse ash by selective grinding and classification. Cem. Concr. Res. 2016, 89, 269–275. [Google Scholar] [CrossRef] [Scilit]
  30. Arenas-Piedrahita, J.C.; Montes-García, P.; Mendoza-Rangel, J.M.; López Calvo, H.Z.; Valdez-Tamez, P.L.; Martínez-Reyes, J. Mechanical and durability properties of mortars prepared with untreated sugarcane bagasse ash and untreated fly ash. Constr. Build. Mater. 2016, 105, 69–81. [Google Scholar] [CrossRef] [Scilit]
  31. Arulrajah, A.; Kua, T.-A.; Suksiripattanapong, C.; Horpibulsuk, S.; Shen, J.S. Compressive strength and microstructural properties of spent coffee grounds-bagasse ash based geopolymers with slag supplements. J. Clean. Prod. 2017, 162, 1491–1501. [Google Scholar] [CrossRef] [Scilit]
  32. Chusilp, N.; Jaturapitakkul, C.; Kiattikomol, K. Utilization of bagasse ash as a pozzolanic material in concrete. Constr. Build. Mater. 2009, 23, 3352–3358. [Google Scholar] [CrossRef] [Scilit]
  33. Cordeiro, G.C.; Barroso, T.R.; Toledo Filho, R.D. Enhancement the Properties of Sugar Cane Bagasse Ash with High Carbon Content by a Controlled Re-calcination Process. KSCE J. Civ. Eng. 2018, 22, 1250–1257. [Google Scholar] [CrossRef] [Scilit]
  34. Ríos-Parada, V.; Jiménez-Quero, V.G.; Valdez-Tamez, P.L.; Montes-García, P. Characterization and use of an untreated Mexican sugarcane bagasse ash as supplementary material for the preparation of ternary concretes. Constr. Build. Mater. 2017, 157, 83–95. [Google Scholar] [CrossRef] [Scilit]
  35. Teixeira, E.R.; Camões, A.; Branco, F.G. Valorisation of wood fly ash on concrete. Resour. Conserv. Recycl. 2019, 145, 292–310. [Google Scholar] [CrossRef] [Scilit]
  36. AFNOR, NF EN 15743+A1: Supersulfated Cement—Composition, Specifications and Conformity Criteria. 2015. Available online: https://www.boutique.afnor.org/en-gb/standard/nf-en-15743-a1/supersulfated-cement-composition-specifications-and-conformity-criteria/fa059609/45272 (accessed on 1 April 2026).
  37. Scrivener, K.; Snellings, R.; Lothenbach, B. (Eds.) A Practical Guide to Microstructural Analysis of Cementitious Materials; CRC Press: Boca Raton, FL, USA, 2018. [Google Scholar] [CrossRef] [Scilit]
  38. Protić, M.; Miltojević, A.; Zoraja, B.; Raos, M.; Krstić, I. Application of Thermogravimetry for Determination of Carbon Content in Biomass Ash as an Indicator of the Efficiency of the Combustion Process. Teh. Vjesn. 2021, 28, 1762–1768. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.