Abstract
This study presents a comparative morphological and elemental characterization of organomineral coatings composed of polydopamine (PDA) and nanocrystalline carbonate-substituted hydroxyapatite (nano-cHAp), formed on model Si(111) substrates and human enamel specimens. Three technologically distinct routes were investigated: sequential PDA/HAp/PDA deposition without an external field (NF), one-step PDA/HAp co-deposition without applied voltage (F0, U = 0 V), and one-step PDA/HAp co-deposition under applied voltage (F, U = 50 V). X-ray diffraction was employed to verify the apatite-like structure of the initial nanocrystalline HAp and to identify drying-related contributions from the TRIS-containing medium; however, it was not used as direct evidence of the HAp phase or texture in the final coatings. SEM segmentation of selected enamel areas showed that the area fraction assigned to the morphologically continuous surface-layer class was approximately 85% for NF, 73% for F0, and 95.5% for F. Representative AFM analysis on Si(111) revealed a rough, topographically heterogeneous F0 layer (Sq ≈ 68 nm, height range ≈ 440–490 nm), a pronounced island-like NF morphology (Sq ≈ 45 nm), and a lower-amplitude F morphology (Sq ≈ 4 nm). For the F coating, scratch-edge profiling indicated an apparent step height of approximately 88 nm, while a preliminary ultrasonic retention challenge in water for 5 min at a 30 mm sample-to-probe distance preserved this apparent step height and reduced Sq from approximately 12 to 5 nm. Point-EDX-derived visualization on Ca/P-free Si(111) supported the presence of Ca/P-containing domains and indicated different spatial organization of the mineral component across the NF–F0–F sequence. FTIR and micro-Raman spectroscopy were performed for the two terminal routes, NF and F, and were interpreted as qualitative evidence of PDA- and HAp-related spectral features rather than as a comprehensive quantitative comparison of all deposition modes. Overall, the data support a transition from island-like or domain-heterogeneous coatings toward a more laterally continuous, lower-amplitude surface layer in the one-step field-assisted route. The results remain morphology-oriented and do not demonstrate clinical remineralization, HAp texture, long-term oral stability, or quantitative adhesion strength.
1. Introduction
Biomimetic organomineral composites composed of calcium phosphate nanoparticles and bioadhesive biopolymer matrices are considered promising regenerative materials for minimally invasive dentistry [1,2,3]. Their potential lies primarily in the ability to control the morphology, continuity, and interfacial organization of the mineral-polymer layer [1,4,5]. This area of research is particularly relevant because mature enamel lacks intrinsic regenerative capacity, and simple replenishment of the mineral phase with various agents fails to replicate the hierarchical organization [6], interfacial adhesion [7,8], and mechanical compatibility of natural enamel [1,9,10,11]. Consequently, modern strategies are shifting from straightforward mineralization in calcium phosphate media toward the controlled formation of organomineral interfaces, where the polymer matrix influences nucleation, aggregation, and lateral distribution of hydroxyapatite-associated components [5,12,13,14].
The biopolymer polydopamine (PDA) is one of the most versatile matrices for such applications [15,16,17,18,19]. Its formation is based on the oxidative polymerization of dopamine, resulting in a structure that includes catechol, amine, indole/pyrrole, and quinone moieties [19,20,21]. These functional groups enable PDA to form bonds with a wide range of organic and inorganic materials, serving as a reactive platform for subsequent mineralization and functionalization [19,20,21,22]. At short deposition times, the chemical structure and local organization of the PDA film depend on the nature of the substrate; however, as deposition time increases and a more continuous layer forms, the substrate’s influence on the spectral response diminishes [23,24]. This phenomenon is particularly important when developing biomaterials intended to form organomineral interfaces on chemically and morphologically diverse surfaces [16,17,24,25]. The CuSO4/H2O2 system is widely used to accelerate PDA deposition, significantly reducing coating formation time and improving uniformity [26]. The accelerating effect of this system is attributed to the oxidative activation of dopamine and the rapid formation of PDA-containing oligomeric products [26]. In Cu(II)/H2O2-containing media, the literature data suggest the involvement of short-lived reactive oxygen species (ROS), whose composition and yield depend on the coordination environment of Cu2+ and the composition of the reaction medium [27].
Previously, we developed a method for the rapid layer-by-layer formation of PDA/HAp/amino acid biomimetic layers on Si(111) substrates and natural enamel [28]. In that study, monocrystalline Si(111) was used as a reference model substrate with a well-characterized surface relief, which is highly suitable for analyzing the morphology, thickness, and molecular composition of PDA/HAp coatings using AFM, Raman, and FTIR techniques. Employing model surfaces to optimize the formation of biomimetic organomineral composites is consistent with the current approach in enamel-like system research. For instance, the deposition of HAp/FHAp layers on model substrates enables the identification of growth, dissolution, and remineralization processes in enamel-like systems [6,29].
It was demonstrated that the method we proposed for layer formation is transferable to enamel, and that amino acid functionalization of hydroxyapatite (HAp) promotes the formation of a morphologically organized mineralized polydopamine (PDA)/nanocrystalline HAp layer [28]. However, the layer-by-layer chemical approach still carries the risk of uneven growth, localized PDA aggregation, and inconsistent incorporation of HAp into the polymer matrix.
Further development of this approach involved using an external electric field as a physical factor to control interfacial assembly, a technique applied in several related fields [30,31,32,33]. In a study on electric field-guided biomimetic enamel mineralization, it was demonstrated that isolated electrodes can generate an electrostatic field without Faradaic current passing through biological tissue. The resulting HAp/amino acid/PDA coating exhibited a pronounced organomineral architecture, chemical heterogeneity at the nanoscale, and increased apparent surface hardness of the coating–enamel system [34]. The use of an electric field to control HAp-containing coatings is also supported by the general principles of electrophoretic deposition of biomaterials, where factors such as charge, electrophoretic mobility, suspension stability, and field strength determine the deposition rate and microstructure of the coating [35]. In the work by Baştan et al., it was shown that electrophoretic deposition can produce oriented chitosan/HAp coatings with hierarchical architecture when suspension and field parameters are properly optimized [36]. Nevertheless, in our previous study [34], the focus was primarily on the multilayer coating formed on enamel, whereas analyzing the early morphological rearrangement of the PDA/HAp film during the transition to a field-assisted mode requires a separate comparative investigation.
Unlike our previous work [34], which primarily focused on electrically guided enamel mineralization, the formation of anisotropic ncHAp/AA/PDA coatings, and the changes in the mechanical response of the coating–enamel system, the present study addresses a fundamentally different technological issue: how the transition from the sequential NF route to the one-stage F0 mode, and further to the field-assisted F mode, affects the morphology, lateral continuity, and spatial organization of Ca/P-containing regions in biomimetic PDA/HAp coatings.
Therefore, this study involves a comparative morphological, topographical, and elemental characterization of PDA/HAp coatings formed on model Si(111) substrates and natural enamel under the NF, F0, and F modes.
2. Materials and Methods
2.1. Experimental Design
Monocrystalline silicon Si(111) wafers were used as model substrates, providing a standardized, low-roughness surface for AFM, FTIR, and micro-Raman mapping of the coatings. Fragments of natural enamel served as biological substrates to assess coating morphology under conditions of heterogeneous natural relief [6,10,37]. The results obtained from the two substrate types were considered complementary yet substrate-specific: AFM comparisons were performed on Si(111), while SEM analysis of coating continuity was conducted on enamel.
It is important to emphasize that NF and F are not control samples differing solely by the presence of an electric field. NF represents the sequential formation of PDA/HAp/PDA without an electric field, whereas F involves the one-step co-deposition of PDA and HAp under the influence of an electric field. Therefore, causal conclusions are drawn regarding the effect of transitioning between technological routes, without isolating the individual contributions of the electric field, one-step kinetics, the number of washings, or the total duration of component contact. The compared modes are summarized in Table 1. At the same time, the F0 mode was introduced as an intermediate control between NF and F. It preserves the single-stage co-presence of PDA precursors and HAp particles, characteristic of the F route, but excludes the applied voltage (U = 0 V). This comparison allows for isolating the contribution of the single-stage deposition scheme itself from the additional influence of the external field, although it is not a complete factorial experiment, since NF, F0, and F also differ in the sequence of coating formation.
Table 1.
Compared technological modes of forming PDA/HAp coatings.
To improve the reproducibility of the technological regimes, all three series were prepared in the same basic medium: 60 mL of 50 mM TRIS buffer, adjusted to pH 8.7 with 0.1 M HCl, containing dopamine at 2 mg/mL, HAp at 0.003 mg/mL, CuSO4·6H2O at 0.133 mg, and 390 µL of H2O2. The total coating formation time was 5 h. For NF, the process was divided into consecutive stages of 2 h, 1 h, and 2 h, whereas for F0 and F, a single-stage simultaneous presence of PDA precursors and HAp particles was maintained for 5 h. After coating formation, the samples were rinsed with distilled water and dried at room temperature (approximately 22 °C).
2.2. Preparation and Preliminary Inspection of Enamel Biotemplates
Fragments of native human coronal enamel were used as biologically relevant substrates. Teeth obtained after clinical extraction were preliminarily selected based on morphological criteria: only samples without visible carious lesions, erosions, wedge-shaped defects, or pronounced enamel structure disturbances were included in the study. Excitation was performed using radiation at 532 nm; the detected signal was separated from the reflected laser radiation using a notch filter and recorded with a digital camera for subsequent visual surface evaluation. After selection, the teeth were cleaned and stored individually in physiological saline containing sodium azide at 4 °C, which maintained tissue moisture until sample preparation. Enamel segments approximately 5 × 5 mm2 in size and about 2 mm thick were cut from the coronal part using a low-speed diamond saw with water cooling. Prior to mineralization, the obtained fragments were kept in sealed containers in a humid environment to prevent enamel drying and related morphological artifacts.
2.3. Preparation of Enamel and Si(111) Substrates
Before applying the coatings, enamel biotemplates and model Si(111) substrates underwent standardized surface activation, adapted from previously established protocols for biomimetic enamel mineralization [37] and consistent with contemporary enamel-conditioning approaches employing phosphoric-acid and calcium-phosphate systems [38]. For enamel, the preparation involved brief etching with 38% H3PO4, multiple rinses with deionized water, subsequent treatment with a diluted citric acid solution to remove loosely bound organic components, and repeated rinsing. In the final step, the biotemplates were immersed in a 12% Ca(OH)2 suspension, followed by rinsing with distilled water until the onset of coating precipitation. This pretreatment enhances surface reproducibility and facilitates the subsequent fixation of the calcium-phosphate component on the enamel [37,38]. Si(111) wafers served as smooth model substrates for morphological and spectral analysis of thin PDA/HAp layers. Prior to the experiment, they were treated using a simplified activation protocol: briefly immersed in 38% H3PO4, rinsed with distilled water, then placed in a 12% Ca(OH)2 suspension, and again rinsed with distilled water before coating application. Unlike enamel, Si(111) was not considered a chemical analog of dental tissue; its role was to provide a reproducible, low-roughness surface for AFM, Raman, and FTIR comparisons of NF and F modes.
2.4. Synthesis of HAp and Preparation of the Mineralizing Suspension
Nanocrystalline carbonate-substituted hydroxyapatite (HAp), used as the mineral component of the PDA/HAp coatings, was synthesized via liquid-phase precipitation from calcium- and phosphate-containing precursors, following a previously established method [39]. CaCO3, derived from a biogenic calcium source, served as the calcium precursor; this choice facilitates the formation of defective carbonate-substituted apatite, which closely resembles the mineral phase of hard dental tissues in several structural and chemical aspects [39,40]. After high-temperature treatment, the calcium-containing precursor was converted to its hydroxide form and then titrated under stirring with 0.3 M H3PO4 solution to achieve a mildly alkaline pH of approximately 8. The process was conducted near room temperature with constant stirring. The resulting suspension was aged for 24 h, after which the precipitate was separated, dried, and dispersed. Immediately prior to coating formation, the HAp powder was suspended in TRIS buffer at pH 8.7. To minimize initial aggregation, the suspension underwent a series of brief ultrasonic treatments with pauses between cycles to prevent significant overheating. For comparison of NF and F modes, a working HAp concentration of 0.003 mg/mL was employed; this concentration aligns with the descriptions of the solutions and coating formation procedures detailed below.
2.5. Solutions for PDA Polymerization and HAp Mineralization
The basic medium for coating formation was a TRIS buffer adjusted to pH 8.7 with 0.1 M HCl and containing CuSO4·6H2O. The polymerization solution was prepared by adding dopamine hydrochloride to a concentration of 2 mg/mL. To accelerate the oxidative polymerization of dopamine under constant mechanical stirring, H2O2 was introduced; in the presence of Cu2+, this initiated accelerated oxidation of dopamine and the formation of PDA-containing oligomeric products capable of depositing on the activated surface [26]. In this study, the CuSO4/H2O2 system was considered a general chemical trigger for accelerated oxidative polymerization of dopamine in all technological routes; individual reactive oxygen species (ROS) in the reaction medium were not directly identified or quantitatively determined. The mineralizing suspension was prepared immediately before use: HAp was dispersed in TRIS buffer at pH 8.7 at a working concentration of 0.003 mg/mL and additionally treated with ultrasound as described above. The low concentration of HAp was chosen to reduce rapid particle agglomeration in the alkaline medium and to maintain colloidal mobility of the mineral component during the deposition stage. The same working concentration of HAp was used in the NF, F0 and F modes; however, the process architecture was fundamentally different: in NF, accelerated PDA polymerization and the HAp-containing stage were performed sequentially, whereas in F0 and F, HAp was present in the solution simultaneously with accelerated PDA polymerization.
2.6. Sequential NF Mode: PDA/HAp/PDA Without External Field
In the NF mode, the sample was fabricated as a three-layer PDA/HAp/PDA structure without applying an external electric field. Initially, the activated substrate was immersed in a TRIS solution containing dopamine, CuSO4·6H2O, and H2O2, which accelerated dopamine polymerization and facilitated the deposition of the primary PDA layer. After this stage, the substrate was rinsed to remove loosely bound particles and then transferred to a suspension containing HAp, where mineralization and adsorption of HAp occurred on the PDA-modified surface. Finally, a second PDA layer was applied to stabilize the formed organomineral structure. This sequential process served as a technological analogue to previously developed layer-by-layer PDA/HAp approaches [28].
2.7. One-Step Field-Assisted Mode (F)
In mode F, a one-step co-deposition of PDA and HAp was performed under the influence of an external electric field. The experiment was conducted in a custom-designed cell fabricated from an inert photopolymer using 3D printing. Two copper electrodes inside the cell were arranged in parallel and completely isolated from both the solution and the substrate (Figure 1). The inter-electrode distance was approximately 3 mm, and the applied voltage was 50 V. The ratio of voltage to distance (U/d) was approximately 16.7 V/mm and was used as a geometric parameter of the cell. The electrode insulation prevented direct contact with the solution and the sample; since leakage current and medium conductivity were not measured, this mode is considered electrostatic field-assisted formation rather than classical electrophoretic deposition (Figure 1). A model silicon substrate or an enamel fragment was placed on the side of the negative electrode. Si(111) plates measuring 1.5 × 1.5 × 0.1 cm were used, while enamel segments were prepared from the crown part of a tooth, as described above. The cell was immersed in a sterile container with a TRIS solution containing HAp (0.003 mg/mL), dopamine (2 mg/mL), CuSO4·6H2O, and H2O2. Unlike mode NF, in mode F the polymerization of PDA and the incorporation of HAp-bound components occurred simultaneously in the presence of the external field. The working interpretation of mode F is based on the fact that at pH 8.7, PDA-containing oligomers/particles and the HAp dispersion may possess a pH-dependent charge state and polarizability (Figure 1b). The applied voltage can potentially influence the local distribution and aggregation of components near the substrate. However, ζ-potential, electrophoretic mobility, conductivity, leakage current, and the actual field in the solution were not measured; therefore, this interpretation remains a qualitative working hypothesis rather than a proven transport model.
Figure 1.
Experimental design and conceptual representation of the F route. (a) Cell geometry featuring insulated copper electrodes with an interelectrode distance of approximately 3 mm, an applied voltage of U = 50 V, and the nominal field direction; U/d ≈ 16.7 V/mm represents a geometric voltage-to-distance ratio rather than the actual measured electric field in the electrolyte. (b) Conceptual illustration of the possible field-sensitive redistribution of dopamine/PDA-containing species and HAp particles near the sample.
2.8. One-Step No-Field Control (F0)
The F0 mode was introduced to enable a more rigorous comparison between the sequential NF route and the field-assisted F route. F0 samples were prepared in the same reaction medium, with identical component concentrations, temperature, and a total process duration of 5 h, as the F samples, but without applying voltage to the electrodes (U = 0 V). Unlike the NF mode, F0 maintains the simultaneous one-stage presence of PDA precursors and HAp particles in the reaction medium; unlike the F mode, it excludes any external electrical influence. Therefore, F0 served as an intermediate control, allowing assessment of the contribution of one-stage deposition to the formation of the PDA/HAp coating and enabling a more accurate interpretation of the additional changes observed when switching to the F mode.
2.9. Research Methods
The phase composition of the initial HAp and dried nano-HAp-containing TRIS media, following preparation procedures and ultrasonic treatment, was analyzed using X-ray diffraction (XRD) with a modernized DRON-4-07 diffractometer in Bragg–Brentano geometry, employing Cu Kα1 radiation (λ = 1.54032 Å). In this study, XRD primarily served to confirm the presence of the hydroxyapatite phase in the initial mineral component and to evaluate the contribution of the buffer medium components. Diffractograms of the coatings were not used as direct evidence of the phase composition, texture, or orientation of HAp in the final NF/F0/F coatings. The surface morphology of the coatings on the enamel was studied using field emission scanning electron microscopy (FE-SEM, Quanta FEG 250) combined with energy-dispersive X-ray analysis (EDX). SEM images facilitated qualitative assessment of surface layer distribution and semi-quantitative calculation of the segmented area fraction. Segmentation of fields of view of equal area was performed using a unified thresholding algorithm. The resulting values represent the fraction of the image assigned by the algorithm to the selected morphological class; these are not chemically selective measurements of the PDA/HAp coating area nor results derived from inferential statistics. It was considered that secondary electron contrast is predominantly influenced by surface relief and local surface geometry.
SEM segmentation was performed using Gwyddion software (Version 3.12) on fields of view measuring 32 × 32 µm2. Prior to threshold processing, the images were converted to grayscale format. For consistency, the same analysis area was used after excluding scale bars and letter labels, and contrast was normalized by linear stretching of the intensity range without local sharpening. Masks representing the morphological class of the continuous surface layer were generated using a global threshold based on Otsu’s criterion; the same approach for selecting mask polarity was applied to all images. The calculated filling fraction corresponded to the ratio of pixels assigned to the selected morphological class to the total number of pixels in the analyzed area. These values serve as semi-quantitative morphological descriptors of the selected SEM regions and do not represent chemically selective maps of PDA/HAp nor results of inferential statistics.
For sample F, an additional preliminary test of coating retention under ultrasonic treatment was conducted. The treatment took place in an aqueous medium for 5 min using an ultrasonic probe with a nominal frequency of 20 kHz. The distance between the sample surface and the working part of the probe was approximately 30 mm. After exposure, the sample was analyzed by AFM. However, repeated SEM, EDX, Raman, and FTIR measurements following ultrasonic treatment were not performed in this study.
AFM was selected for monitoring after ultrasonic treatment because it enables repeated examination of the scratch edge area and direct comparison of the apparent step height of the coating and local topography before and after treatment. Repeated SEM, EDX, Raman, and FTIR measurements were not performed post-treatment due to challenges in reproducibly locating the same micrometer-scale area, potential artifacts from drying and remounting the sample, and weak local signals associated with Ca/P, all of which could introduce additional uncertainty. Therefore, this test is considered only a preliminary topographical assessment of ultrasonic retention and not definitive evidence of chemical preservation of hydroxyapatite or long-term coating stability.
The morphology of the original mineral component was further analyzed using transmission electron microscopy (TEM), including high-resolution TEM (HRTEM). High-resolution imaging of non-stoichiometric hydroxyapatite (HAp) samples was conducted on a Libra 120 transmission electron microscope manufactured by Carl Zeiss (Jena, Germany). To evaluate the nanocrystalline nature of HAp, selected area electron diffraction (SAED) was employed. Size analysis was performed on well-defined anisotropic nanocrystals by measuring their length along the major geometric axis; particles that significantly overlapped in projection or were part of dense aggregates were excluded from the quantitative analysis. Interplanar distances (d) for individual, well-resolved plane families were determined from HRTEM images, and the main diffraction rings of the original HAp were indexed on the SAED pattern.
Fourier-transform infrared (FTIR) spectra were obtained using a Vertex-70 spectrometer (Bruker) over the range of 4500–400 cm−1 with a Platinum attenuated total reflection (ATR) accessory. The spectral registration step was 4 cm−1, and the analysis area was approximately 2 mm2. This integral method was applied to record PDA- and HAp-related spectral features of the coatings. For coatings on Si(111) substrates, overlap of HAp phosphate bands with the Si–O contribution from the substrate was taken into account; therefore, FTIR data were interpreted in conjunction with local micro-Raman analysis and XRD characterization of the initial mineral component. Micro-Raman spectra were recorded using a RamMix 532 Raman microscope with 532 nm laser excitation, a spectral resolution of approximately 1 cm−1, radiation power around 30 mW, and a ×40 objective lens. The focal spot area on the sample was approximately 10 µm2. A two-axis motorized stage with a scanning step of 300 nm was employed to move the focal spot across the sample surface. Micro-Raman analysis was used to detect PDA-related bands and HAp-related phosphate vibrations at localized points on the sample. When interpreting spectra on Si(111), the contribution of the silicon transverse optical (TO) mode near 520 cm−1 and the second-order silicon contribution in the 935–990 cm−1 region were separately considered. If individual spectra were scaled to visualize weak bands, their intensities were not used for direct quantitative comparison of the PDA/HAp ratio. Atomic force microscopy (AFM) measurements were conducted using a Femtoscan-001 scanning probe microscope (NT-MDT) at room temperature in semi-contact mode. Rectangular silicon cantilevers with a nominal stiffness of approximately 3.5 N/m, resonance frequencies between 120 and 180 kHz, and tip radii less than 10 nm were employed. Scan areas ranged from 1 × 1 to 5 × 5 µm2. Map processing was performed using Gwyddion software: surfaces were leveled to the mean plane, low-frequency tilt was removed, and root mean square roughness (Sq) was calculated. Sq values served as topographical parameters of representative AFM areas, enabling comparison of the relief characteristics in NF, F0 and F modes. In this approach, quantitative roughness values should be regarded as morphological indicators of selected areas rather than statistically comprehensive comparisons of the entire sample series. Calculation of statistically significant differences requires analysis of original AFM maps from multiple independent areas and samples; exported composite images were not used to extract new statistical parameters. The root mean square roughness was calculated using the formula:
where N is the number of points in the analyzed area, zj is the height at the j-th point after leveling the AFM map, is the average surface height after tilt removal, and Sq is the root mean square deviation of the relief from the mean plane. In the present work, the notation Sq is used for the root mean square roughness calculated from leveled two-dimensional AFM maps. Height profiles were used only to assess profile-derived height variation and the local apparent step height of the coating; individual root mean square roughness parameters from linear profiles were not calculated. To evaluate the local thickness of the deposited coatings, areas of artificially created scratches on model Si(111) substrates were prepared and analyzed for the F0 and F modes. From AFM maps and profiles of the scratch edge, the local apparent step height of the coating was determined; these values were used as topographic/apparent height descriptors rather than as statistically averaged thickness or coating mass. AFM scratch-edge data are presented in Supplementary Figures S2–S6.
3. Results and Discussion
3.1. Structural and Morphological Characterization of the Initial HAp and Medium Components
The diffractogram of the originally synthesized HAp contains broad reflections whose positions correspond to the apatite phase, as confirmed by the ICDD database (No. 98-010-4653) (Figure 2). The diffractogram of the dried HAp/TRIS medium on Si(111) additionally shows intense, narrow reflections from the dried buffer components (TRIS) and a pronounced contribution from the substrate. Therefore, the low-angle peaks in the 10–25° (2θ) range should not be interpreted as indicating a new calcium phosphate phase. Consequently, X-ray diffraction confirms the apatite nature of the original nanocrystalline HAp and highlights the necessity of accounting for the contributions of the TRIS medium and the silicon substrate. It is important to note that, in apatite-containing media, the influence of buffer systems on the deposition processes of layers containing calcium hydroxyapatite nanocrystals is well documented [41,42]. Thus, when investigating the phase formation processes of HAp-like compounds, morphology and individual spectral features should be analyzed in conjunction with phase and morphological data [43].
Figure 2.
XRD analysis of the initial hydroxyapatite phase and the drying-related effects of the TRIS-containing medium. (A) Diffraction patterns of synthesized HAp powder and a dried HAp/TRIS drop on Si(111). (B) Low-angle region highlighting TRIS-related reflections after drying. XRD confirms the starting mineral phase and medium-related contributions but is not used to determine HAp texture in NF/F coatings.
TEM/HRTEM/SAED Characterization of the Initial HAp
The morphology of the initial HAp, used as the mineral component for forming PDA/HAp coatings, was further analyzed using TEM, HRTEM, and SAED techniques (Figure 3). Figure 3 presents a TEM image of the initial nanocrystalline HAp, a histogram of particle length distribution, an HRTEM fragment with measured interplanar spacings, and an SAED pattern with indexing of the main rings. As shown in Figure 3, the TEM image reveals predominantly anisotropic needle-like or rod-shaped nanocrystals, which partially overlap in projection and form weakly ordered aggregated ensembles. From a sample of 30 well-distinguished nanocrystals measured along their major axis, particle lengths ranged approximately from 45 to 175 nm, with an average value of 105.9 ± 32.2 nm; the most represented size range corresponds roughly to 80–120 nm. The HRTEM fragment identified lattice fringes with interplanar spacings of d ≈ 3.11 Å for (210), d ≈ 2.29 Å for (130), and d ≈ 1.88 Å for (230), consistent with the crystal lattice parameters of HAp. The SAED pattern exhibits a ring-like character with discrete azimuthal maxima; the main rings were assigned to reflections (002) with d ≈ 3.44 Å, (211) with d ≈ 2.81 Å, (112) with d ≈ 2.78 Å, (222) with d ≈ 1.94 Å, and (004) with d ≈ 1.72 Å, as well as additional reflections (201) with d ≈ 3.51 Å, (102) with d ≈ 3.17 Å, (003) with d ≈ 2.29 Å, (130) with d ≈ 2.26 Å, and (213) with d ≈ 1.84 Å. Thus, Figure 3 provides a direct characterization of the morphology, size distribution, and local crystallographic features of the initial mineral component.
Figure 3.
TEM/HRTEM/SAED characterization of the original HAp used as the mineral component for forming PDA/HAp coatings. (a) TEM image showing aggregated anisotropic HAp nanocrystals; (b) distribution of lengths of well-defined HAp nanocrystals measured along their major axis; (c) HRTEM image fragment with identified interplanar spacings; (d) SAED pattern of the original HAp.
3.2. SEM Morphology and SEM–EDX Verification of PDA/HAp Coatings
SEM images of the enamel surface after preliminary treatment and before coating application are shown in Figure 4. The images reveal a heterogeneous texture with rounded and rod-like features, consistent with the exposure of enamel prisms or rods [6,37]. This morphology corresponds to a mildly etched surface, where the mineral-organic surface layer has been partially removed [44].
Figure 4.
SEM morphology of enamel after surface pretreatment and prior to PDA/HAp coating formation. (A) 32 × 32 µm2 area and (B) 7.5 × 7.5 µm2 area. Highlighted regions indicate typical surface features related to enamel rods.
SEM images of enamel after coating formation, along with the corresponding threshold masks, reveal differences among the selected areas NF, F0, and F (Figure 5). For areas measuring 32 × 32 µm2, the proportion of pixels classified by the algorithm as belonging to the morphological class of a continuous surface layer was approximately 85% for NF, 73% for F0, and 95.5% for F. These values serve as semi-quantitative descriptors of the analyzed areas and should not be interpreted as statistically representative coverage across the entire series of samples. Nevertheless, the comparison among NF, F0, and F indicates that F0 occupies an intermediate position in the technological process but exhibits a smaller area of morphologically continuous layer compared to F.
Figure 5.
SEM-based comparison of surface-layer morphological continuity on enamel. (A) NF SEM image, (B) threshold-derived mask for NF, (C) F0 SEM image, and (D) threshold-derived mask for F0, (E) F SEM image, and (F) threshold-derived mask for F. The masks provide a semi-quantitative segmented area fraction for the selected morphological class and do not represent chemically selective maps of PDA/HAp coverage.
In the selected NF area, the coating surface exhibits pronounced lateral heterogeneity: SEM images reveal local agglomerates, regions with varying morphological contrast, and areas where the layer’s continuity is disrupted. At high magnification, submicron particles and aggregates are observed, consistent with the island-domain nature of sequential PDA/HAp/PDA deposition. In contrast, the F coating displays more extensive areas of continuous relief and fewer large aggregated domains.
Thus, the SEM comparison of NF–F0–F shows that the transition to one-stage co-deposition itself changes the nature of coating formation; however, the maximum lateral continuity is observed precisely in the field-assisted F mode. In this interpretation, F0 is a key control mode: it demonstrates that the one-stage architecture without a field does not fully reproduce the morphological pattern of F.
For additional elemental verification of the mineral component in PDA/HAp coatings on Si(111), EDX mapping was performed on morphologically distinct areas of the surface. Based on these analyses, Ca- and P-related signal visualizations were generated (Figure 6). The use of Si(111) is methodologically significant because the silicon substrate lacks an inherent calcium-phosphate background, unlike enamel. Therefore, detecting Ca and P in the selected coating areas provides elemental confirmation of the presence of a Ca/P-containing component. However, for thin coatings on Si, the EDX Ca/P ratios may deviate from the stoichiometric Ca/P ratio of 1.67 for HAp due to contributions from the substrate, layer thickness, surface relief, and local inhomogeneity of the coating [45].
Figure 6.
Visualization of calcium (Ca) and phosphorus (P) signals in PDA/HAp coatings on Si(111), based on SEM morphology and EDX measurements. The coatings were formed using three methods: NF—sequential formation of PDA/HAp/PDA without an external field; F0—one-step co-deposition of PDA and HAp without applied voltage (U = 0 V); and F—one-step field-assisted co-deposition of PDA and HAp with an applied voltage of U = 50 V. Panels (A,E,I) show actual SEM surface images; panels (B,F,J) display the Ca-associated signal; panels (C,G,K) illustrate the P-associated signal; and panels (D,H,L) present combined visualizations of Ca- and P-associated signals.
In NF mode, calcium- and phosphorus-related signals exhibit a pronounced domain character and are predominantly associated with morphologically heterogeneous aggregated areas of the coating. For NF, the maximum atomic Ca/P ratio among Ca/P-positive points is 1.52, while the area with the highest absolute Ca and P signals has a Ca/P ratio of 1.36. This pattern indicates not a chemically homogeneous layer but rather a spatially heterogeneous distribution of Ca/P-containing domains, consistent with the high yet uneven morphological surface coverage observed in SEM segmentation data.
In the F0 mode, the most distinct domain structure is observed: alongside a Ca/P-poor area, a Ca/P-rich domain with a Ca/P ratio of 1.52 is identified. Therefore, F0 should be considered an intermediate technological mode. The one-stage mixing of PDA precursors and HAp particles promotes the formation of an extended coating; however, without an external field, the distribution of the mineral component remains heterogeneous, exhibiting both Ca/P-rich and Ca/P-poor areas.
In F mode, the Ca/P-related signal is weaker in local intensity but more morphologically distributed. At the same time, the Ca/P ratio reaches approximately 1.74, the highest among the calculated ratios for the different coating formation modes. The combination of SEM and EDX data shows that the transition from NF to F0 to F is reflected not only in the surface relief and degree of coverage but also in the spatial organization of Ca/P-containing domains.
A comparison of the microscopic data presented in Figure 7 reveals that the selected area of the F coating on enamel exhibits a more morphologically continuous surface layer compared to the selected area of the NF coating. Additionally, Figure 7 should be regarded as a high-resolution morphological complement to the SEM segmentation shown in Figure 5, rather than as an independent quantitative validation of the coating’s chemical composition.
Figure 7.
High-magnification SEM comparison of PDA/HAp coatings on enamel in NF (A) and F (B) regimes. The 3 × 3 µm2 areas illustrate local differences in aggregate morphology and lateral continuity of the coating. These images complement the semi-quantitative coverage assessment shown in Figure 5.
3.3. AFM Morphology, Apparent Height and Ultrasonic Retention Challenge
AFM analysis characterizes the local final topography of coatings on a model Si(111) substrate (Figure 8, Figure 9, Figure 10 and Figure 11). The activated control surface of the silicon substrate exhibits an Sq of approximately 1.5 nm, with local height inhomogeneities reaching several tens of nanometers (Figure 8). Therefore, the subsequent increase in surface relief corresponds to the deposition of a surface layer. After preliminary treatment of Si(111), individual nanometer-sized objects with varying topographic and auxiliary AFM contrast are observed, displaying distinct dissipative characteristics (Figure 8B). Although their chemical nature was not determined in this study, considering the use of concentrated phosphoric acid for processing and profiling the silicon surface, it is reasonable to assume that the detected agglomerates are related to the activated surface and may influence the initial adsorption of PDA-containing components [24].
Figure 8.
AFM characterization of the activated Si(111) substrate after pretreatment: (A) 2D topography, (B) auxiliary AFM channel image exported by the instrument software, (C) 3D topography, and (D) representative height profile. The root mean square roughness (Sq) is approximately 1.5 nm, and the reported height range corresponds to the selected 5 × 5 µm2 area.
Figure 9.
AFM morphology of the PDA/HAp surface layer formed via the NF route. (A) 2D topography, (B) auxiliary AFM channel image exported by the instrument software, (C) 3D surface rendering, and (D) representative height profile. The selected 5 × 5 µm2 area is characterized by an Sq of approximately 45 nm and a submicron height range.
Figure 10.
AFM morphology of the PDA/HAp coating formed in the control F0 mode (one-step, U = 0 V). (A) 2D topography, (B) auxiliary AFM channel exported by the instrument software, (C) 3D surface visualization, and (D) representative height profile. The selected area of 5 × 5 µm2 is characterized by pronounced topographical heterogeneity, Sq ≈ 68 nm, an average height variation of about 221 nm, and an overall height range on the order of 440–490 nm.
Figure 11.
AFM morphology of the PDA/HAp surface layer formed using the one-step field-assisted F route. (A) 2D topography, (B) auxiliary AFM channel image exported by the instrument software, (C) 3D surface representation, and (D) representative height profile. The selected 5 × 5 µm2 area is characterized by an Sq of approximately 4 nm and a height range of about 65–68 nm.
In the selected NF area, AFM reveals a pronounced island-like relief characterized by large aggregates and local elevations; the height range reaches several hundred nanometers, and the root mean square roughness (Sq) is approximately 45 nm (Figure 9). This morphology is consistent with the heterogeneous accumulation of material during sequential PDA/HAp/PDA deposition, where PDA aggregates and HAp particles may be unevenly distributed across the surface. In the selected F area, the relief amplitude is significantly lower: the height range is about 65–68 nm, and Sq is around 4 nm. Large submicron protrusions are less pronounced than in the NF area; however, the lower Sq should not be interpreted as direct evidence of greater coating mass or improved adhesion, since the thickness and mass of the layer were not statistically measured across a series of independent samples. Representative AFM morphology of the F coating is shown in Figure 11.
AFM analysis of the control sample F0 revealed the formation of a topographically heterogeneous PDA/HAp coating characterized by large, branched, agglomerated domains (Figure 10). The average height variation within the selected area was approximately 221 nm, with an overall height range of about 440–490 nm. The Sq was approximately 68 nm. This morphology suggests that one-stage co-deposition without an external field results in the formation of an extensive but domain-heterogeneous organo-mineral layer, comprising large PDA/HAp-bound aggregates and regions with varying degrees of surface coverage.
For sample F, additional AFM analysis was conducted on the edge areas of an artificially created scratch, as shown in Supplementary Figures S3 and S5. Surface profiling enabled the assessment of the local apparent step height of the coating, which was approximately 88 nm. This value should be considered an estimate of the effective layer height in the selected area rather than the absolute coating thickness, since both the coating surface and the scratch area exhibit their own roughness and do not form a perfect geometric step. The root mean square (RMS) surface roughness in this area was approximately Sq ≈ 12 nm. Furthermore, local island-like formations with a lateral size of about 250 nm and a height of approximately 25 nm were observed in certain regions of the F coating.
After ultrasonic treatment of sample F in an aqueous medium for 5 min at a nominal probe frequency of 20 kHz and a distance of approximately 30 mm between the sample surface and the ultrasonic probe, the apparent step height of the coating remained around 88 nm, while the root mean square (RMS) roughness decreased to Sq ≈ 5 nm. Simultaneously, the local island-like formations observed before treatment nearly disappeared. This behavior is consistent with the preservation of the primary low-amplitude PDA/HAp-associated layer after the selected ultrasonic retention challenge and the removal of some protruding aggregates from the surface. Such a two-component morphology of PDA coatings, comprising a smoother film-like component and aggregates deposited on top, has been described in the literature for polydopamine layers [46]. The AFM profiles of the scratch areas for F0 and F coatings are presented in Supplementary Figures S2–S6. These profiles are used to estimate the local apparent step height of the coating and show that F0 retains pronounced variability in local height and an agglomerated structure, whereas F is characterized by a lower-amplitude and more laterally continuous surface layer. An additional profile of the F coating in Supplementary Figure S5 reveals local low-amplitude step changes on the order of 12–15 nm, consistent with a more uniform organization of the surface layer compared to F0.
The representative AFM roughness parameters and local apparent height descriptors for Si(111), NF, F0, and F are summarized in Table 2.
Table 2.
Representative AFM parameters of selected 5 × 5 µm2 areas and local layer-height descriptors for Si(111), NF, F0 and F. The values are presented as descriptors of selected maps/areas and do not result from inferential statistics.
3.4. FTIR and Micro-Raman Spectral Evidence for Organomineral Composition
FTIR spectra of HAp, Si(111), PDA/Si, and NF/F coatings are presented in Figure 12. In the 1700–1400 cm−1 region, the spectra of PDA/Si, NF, and F exhibit broad features consistent with combined contributions from C=O/C–O, C–N, and aromatic/heterocyclic fragments of PDA [23,25,28]. The 1100–950 cm−1 region includes HAp-related phosphate vibrations; however, on Si(111), it also contains a strong contribution from Si–O bonds of the substrate [47]. Changes in the profile of the ν3(PO43−) band may result from the formation of chemical bonds between the polydopamine organic matrix and hydroxyapatite, as previously described in several studies [48,49]. Concurrently with the alteration in the phosphate ν3(PO43−) band profile, spectral features appear in the frequency region associated with molecular groups of polydopamine. It should be noted that PDA is not a chemically homogeneous linear polymer; its spectral signatures reflect a mixture of catechol, quinone, amine, and indole/pyrrole fragments, which are sensitive to formation conditions [19,20,23]. The observed changes in the regions 1636–1590 cm−1 and 1510–1460 cm−1 correspond to differences in the spectral contributions associated with PDA in NF and F coatings. These spectral features reflect variations in the local environment of PDA fragments and components related to HAp. However, the FTIR data alone do not permit a quantitative determination of the degree of PDA polymerization or the concentration of oxidative intermediate products [23].
Figure 12.
FTIR spectra of HAp, Si(111), PDA/Si, and PDA/HAp coatings formed using the NF and F routes are presented. The broad PDA-associated region at 1700–1400 cm−1 and the overlapping HAp/Si–O region at 1100–950 cm−1 are highlighted.
Meanwhile, differences in the FTIR spectral profiles of NF and F samples arise from varying relative contributions of PDA- and HAp-related vibrational bands, which relate to differences in layer thicknesses deposited by the two modes, the distribution of organic and mineral components, and variations in the local environment of HAp nanocrystals. It is important to note that in the 1100–950 cm−1 region, phosphate modes of HAp overlap with Si–O bond contributions from the silicon substrate; thus, FTIR data provide evidence for the formation of an organomineral coating composition but do not reveal information about the crystallochemical organization of the mineral HAp-based phase. Differences in PDA-related spectral profiles between NF and F can be correlated with variations in the kinetics of PDA-containing oligomer formation in sequential versus one-step reaction schemes. However, FTIR data do not permit direct determination of the nature of short-lived oxidative intermediates or comparison of reactive oxygen species (ROS) concentrations between the modes.
Micro-Raman Spectral Characteristics of PDA/HAp Composites
Raman spectra of NF and F coatings on Si(111) exhibit combined contributions from both the substrate and the organo-mineral layer (Figure 13). In the 935–990 cm−1 region, the ν1(PO43−) signal of hydroxyapatite (HAp) around 960–962 cm−1 overlaps with the second-order silicon scattering; meanwhile, broad PDA-related bands are observed in the 1320–1600 cm−1 range [25,28,50]. Thus, the Raman spectroscopy data confirm the qualitative attribution of the observed spectral features related to PDA and those related to HAp/Si; however, they are not used as an independent quantitative assessment of the coating composition.
Figure 13.
Representative micro-Raman spectral profiles of HAp, Si(111), PDA/Si, and PDA/HAp coatings formed using the NF and F routes. Vertical guides indicate the overlapping Si second-order and HAp-related ν1(PO43−) regions, as well as the broad PDA-associated spectral domain. Spectra marked ×3 are scaled solely for visualization.
Spectra obtained from the central and edge areas of NF differ visually in band shape and relative intensity, consistent with local heterogeneity within the layer. The feature near 960–962 cm−1 in some NF spectra may include a phosphate contribution from HAp; however, it overlaps with the second-order silicon scattering (Figure 13). Therefore, the intensity ratio between the 960–962 cm−1 and 1320–1600 cm−1 regions was not employed as a quantitative indicator of HAp or PDA content. NF and F spectra differ in the shape and relative intensity of overlapping PDA-, HAp-, and Si-related features. These differences correspond to the uneven local organization of the surface layer and morphological data, as well as to nano-FTIR studies of PDA layers, which demonstrate that early PDA coatings exhibit chemical and topological variability depending on the substrate and deposition time [23]. Variations in the Raman response of NF and F coatings should primarily be attributed to differences in morphology and interphase organization of the PDA/HAp layer.
The principal spectral regions used for the interpretation of the FTIR and micro-Raman data are summarized in Table 3.
Table 3.
Spectral regions used for the interpretation of Raman and FTIR data.
3.5. Integrated Discussion of the Coating Formation Mechanism
The observed differences should be interpreted as resulting from the transition between three distinct technological states rather than from a single isolated variable. In all routes, the CuSO4/H2O2 system acts as a common chemical trigger that accelerates dopamine oxidation and promotes the formation of PDA-containing oligomeric products [26]. Within Cu(II)/H2O2-containing media, short-lived reactive oxygen species may be involved, but they were not directly identified or quantified in this study [27]. Because the oxidative trigger is common to NF, F0 and F, ROS are not used as the primary explanation for the observed morphological differences. The F0 control shows that one-step co-deposition alone changes the coating-formation scenario but does not reproduce the smoother, more laterally continuous F morphology. Therefore, the F route should be interpreted as a combined technological scenario in which one-step PDA formation, HAp incorporation and field-sensitive redistribution of charged or polarizable components occur simultaneously.
The obtained data allow for refining the mechanism underlying the differences between NF-, F0-, and F-coatings. In the NF mode, the sequential formation of PDA/HAp/PDA results in a high proportion of morphologically filled surface; however, the coating retains pronounced island-like heterogeneity and contains aggregated domains. The F0 mode demonstrates that the simultaneous presence of PDA precursors and HAp particles in the solution alters the coating formation process, but without an external field, the layer remains topographically heterogeneous, featuring large agglomerated PDA/HAp domains and a smaller proportion of morphologically continuous surface. In contrast, the F mode is characterized by the highest proportion of continuous surface layer and lower-amplitude morphology, indicating an additional contribution of the electric field to the redistribution, transport, and fixation of organo-mineral components near the Si(111) substrate. This interpretation aligns with the general concepts of field-assisted/electrophoretic deposition, according to which voltage and environmental parameters can significantly influence particle transport and coating microstructure [56,57].
The sequential NF route is maintained in this work not as an optimized final protocol but as a reference layer-by-layer architecture, building upon the previously used PDA/HAp approach. In this scheme, the first PDA step creates an adhesion-active organic interlayer for the subsequent fixation of the HAp-containing component, while the second PDA step acts as an overlapping and stabilizing organic layer for the mineral domains. Comparison with F0 and F demonstrates that this sequential architecture provides a significant area of morphologically filled surface but is accompanied by pronounced island-aggregated heterogeneity. Therefore, the single-stage field-assisted F mode is considered a more promising morphologically controlled alternative.
The obtained data indicate that the transition from NF to F0, and subsequently to F, is accompanied by changes in island-domain morphology, lateral continuity, and the spatial organization of Ca/P-containing regions. Notably, F0 demonstrates that the simultaneous presence of PDA precursors and HAp particles in a single stage alters the coating formation process. However, higher lateral continuity and a low-amplitude relief are most pronounced specifically in the F mode. Consequently, the comparison among NF, F0, and F suggests an additional contribution from the applied field but does not establish it as the sole influencing factor.
The combination of SEM segmentation data and AFM topography reveals that F0 is not merely an intermediate morphology between NF and F. On the contrary, with the simultaneous one-step presence of PDA precursors and HAp particles—but without applied voltage—F0 forms the highest-relief and most domain-heterogeneous layer among the studied modes. Therefore, the improved lateral continuity of the F coating cannot be explained solely by the transition from the sequential NF route to one-step deposition; rather, it is consistent with an additional contribution of the electric field in organizing the PDA/HAp-associated layer.
Particularly noteworthy is the result of ultrasonic treatment applied to the F coating in an aqueous medium for 5 min, using a nominal probe frequency of 20 kHz and maintaining a distance of approximately 30 mm between the sample surface and the ultrasonic probe. The preservation of the apparent step height at about 88 nm after treatment, coupled with a simultaneous reduction in roughness from Sq ≈ 12 nm to Sq ≈ 5 nm, indicates that ultrasonic exposure does not completely remove the coating but rather eliminates protruding island aggregates. This observation aligns with the understanding of PDA coatings as morphologically heterogeneous systems, where, in addition to the base film layer, secondary deposited aggregates of PDA or PDA-bound particles may be present. Such aggregates can significantly affect the measured AFM roughness and complicate the interpretation of coating thickness [46].
Thus, this result should not be interpreted as definitive proof of the coating’s overall stability but rather as topographical evidence indicating the separation of two components within the F-coating: protruding removable aggregates and a persistent low-amplitude layer associated with PDA/HAp. A generalized schematic summarizing the proposed interpretation of the formation of PDA/HAp coatings in NF and F modes is presented in Figure 14.
Figure 14.
Schematic working model of PDA/HAp coating formation. (A): sequential NF route with PDA/HAp/PDA stages. (B): one-step field-assisted F route, in which PDA polymerization and HAp incorporation occur simultaneously under an external electric field. In both routes, CuSO4/H2O2 acts as an oxidative trigger for dopamine polymerization. This scheme illustrates a working interpretation of the combined effects of deposition architecture and the field-sensitive redistribution of charged or polarizable components, rather than the independent action of ROS or the electric field alone.
In this system, polydopamine functions as an organic matrix and a potential adhesion interface due to its catechol, quinone, and amine groups [19,20,22]. The literature on PDA-containing coatings of enamel and dentin demonstrates their ability to retain functional ions and support mineralization [58]. The simultaneous presence of hydroxyapatite during PDA formation in the F-route may influence the local aggregation and fixation of components before the formation of large, isolated aggregates. Additionally, the lower Sq value observed in the F-area may depend not only on the lateral distribution of the material but also on the thickness or total mass of the deposited layer; however, these parameters were not measured and thus are excluded from the causal interpretation. The plate-like and scaly features observed in the AFM images of the F-area characterize the local surface morphology and do not provide evidence of the crystallographic texture of HAp. It is accurate to describe a lower relief amplitude in the selected F-area and greater morphological continuity in the chosen SEM fields of enamel. Disentangling the contributions of texture, possible amorphous calcium phosphate (ACP)/HAp transformations, layer thickness, and field-sensitive mobility of components requires techniques such as grazing incidence X-ray diffraction (GIXRD), transmission electron microscopy/selected area electron diffraction (TEM/SAED), chemical mapping, ζ-potential measurements, and specialized control routes.
3.6. Work Limitations
The primary limitation of this study is that NF, F0 and F do not constitute a complete factorial experimental design. Although the F0 route reduces the uncertainty associated with one-step deposition without applied voltage, the compared routes still differ in the presence of an applied voltage, the sequence and number of stages, rinsing procedures, and the conditions of contact between HAp and the forming PDA. Consequently, the independent causal effect of the electric field has not been established. Key parameters such as the actual electric field in the electrolyte, electrical conductivity, leakage current, ζ-potential, and electrophoretic mobility were not measured. SEM and AFM data were obtained from selected representative areas and do not provide inferential statistics across multiple independent samples. Reactive oxygen species were neither directly identified nor quantitatively measured; therefore, the CuSO4/H2O2 system is discussed only as a common oxidative trigger rather than as a route-specific mechanistic factor. AFM profiles of scratches for F0 and F provide local apparent thickness measurements but do not replace cross-sectional or fracture-surface SEM analysis and are not a direct quantitative assessment of interfacial strength or coating mass. After ultrasonic treatment, only AFM inspection was performed; repeated SEM, EDX, Raman, or FTIR measurements following ultrasonic treatment were not conducted in this study.
Ultrasonic exposure in water for 5 min at a nominal probe frequency of 20 kHz and a distance of approximately 30 mm from the sample surface should be regarded only as a preliminary test of coating retention. After ultrasonic treatment, only AFM inspection was performed; repeated SEM, EDX, Raman, and FTIR measurements after exposure were not conducted. Therefore, this test does not provide evidence of the long-term chemical, mechanical, or biological stability of the coating.
4. Conclusions
X-ray diffraction confirmed the apatite-like structure of the initial nanocrystalline HAp and revealed a significant contribution from components of the dried TRIS-containing medium; however, it was not used as direct evidence of the HAp phase or texture in the final coatings. FTIR and micro-Raman spectroscopy provided qualitative evidence of PDA- and HAp-related spectral features in the NF and F coatings, while also emphasizing the need to consider the overlap between phosphate-related bands and the response of the Si(111) substrate. In the selected enamel regions examined by SEM, the segmented area fraction assigned to the morphologically continuous surface-layer class was approximately 85% for NF, 73% for F0, and 95.5% for F. In representative Si(111) areas examined by AFM, F0 formed a topographically heterogeneous layer with an Sq value of approximately 68 nm and a height range of about 440–490 nm, whereas the F coating exhibited lower local height variation, with an Sq of approximately 4 nm. The comparison of NF, F0, and F supports the conclusion that the applied field contributed to forming a more laterally continuous and low-amplitude morphology in the F coating; however, it does not establish the field’s action as the sole or entirely isolated factor. SEM–EDX visualization on Si(111) confirms the presence of Ca/P-containing domains and differences in their spatial organization across the NF–F0–F series, but it does not provide evidence of the phase or texture of HAp.
Preliminary ultrasonic treatment of the F-coating in an aqueous environment for 5 min, using a nominal probe frequency of 20 kHz and maintaining a distance of approximately 30 mm between the sample surface and the ultrasound probe, did not eliminate the measurable coating step; its apparent height remained around 88 nm. At the same time, the reduction in Sq from approximately 12 nm to 5 nm is consistent with the removal of protruding aggregates while preserving the primary low-amplitude PDA/HAp-associated layer.
From a practical perspective, controlling the local topography and lateral continuity of PDA/HAp coatings may provide a materials design foundation for developing minimally invasive enamel surface modification strategies, as well as for the localized delivery or retention of calcium phosphate components. However, the current findings describe only the morphological stage of technology development and do not demonstrate clinically effective remineralization. Further studies are necessary to evaluate coating adhesion, mechanical and chemical stability, durability under oral-like conditions, biological safety, and the long-term response of the coating–enamel interface.
Supplementary Materials
The following supporting information can be downloaded at: https://www.mdpi.com/article/10.3390/macromol6030078/s1, Figure S1: AFM morphology of the PDA/HAp coating formed under the control mode F0 (one-step, U = 0 V) on Si(111); Figure S2: AFM scratch-edge analysis of the F0 coating on Si(111), representative region 1; Figure S3: AFM scratch-edge analysis of the F coating on Si(111) before ultrasonic treatment; Figure S4: AFM scratch-edge analysis of the F coating on Si(111) after ultrasonic treatment. The treatment was carried out in an aqueous environment for 5 min at a nominal ultrasonic probe frequency of 20 kHz and a distance of about 30 mm between the sample surface and the probe; Figure S5: additional AFM scratch-edge region of the F coating on Si(111); Figure S6: additional AFM scratch-edge region of the F0 coating on Si(111).
Author Contributions
Conceptualization, P.S.; methodology, P.S. and D.G.; validation, P.S., D.G. and D.P.; formal analysis, P.S., D.G. and D.P.; investigation, P.S., D.G., D.P. and Y.I.; resources, P.S.; data curation, P.S. and D.G.; writing—original draft preparation, P.S., D.G. and D.P.; writing—review and editing, P.S., D.G. and D.P.; visualization, D.G. and D.P.; supervision, P.S.; project administration, P.S.; funding acquisition, P.S. and D.G. All authors have read and agreed to the published version of the manuscript.
Funding
This work was supported by the grant of the Russian Science Foundation, grant number 26-15-20057, https://rscf.ru/project/26-15-20057 (accessed on 10 September 2026).
Institutional Review Board Statement
All procedures involving extracted human dental tissue were conducted in accordance with relevant guidelines and the Declaration of Helsinki. Teeth were obtained following clinically indicated extraction from adult donors who provided written informed consent for participation and for the research use of the extracted dental tissue. The study was approved by the Ethics Committee of Voronezh State University (protocol number Pr-017.02.2026, 10 February 2026).
Informed Consent Statement
Written informed consent for participation and for the research use of clinically extracted human dental tissue was obtained from all adult donors before the extracted teeth were transferred to the research team.
Data Availability Statement
The raw data supporting the conclusions of this article will be made available by the authors upon request.
Acknowledgments
This research used equipment of the IMBUIA beamline of the Brazilian Synchrotron Light Laboratory (LNLS) in the Brazilian Center for Research in Energy and Materials (CNPEM) through the beamtime proposal 20252761.
Conflicts of Interest
The authors declare no conflict of interest.
References
- Sedek, E.M.; Holiel, A.A. Next-Generation Strategies for Enamel Repair and Regeneration: Advances in Biomaterials and Translational Challenges. Tissue Eng. Regen. Med. 2025, 22, 771–789. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Wang, J.; Cui, Y.; Zhang, B.; Sun, S.; Xu, H.; Yao, M.; Wu, D.; Wang, Y. Polydopamine-Modified Functional Materials Promote Bone Regeneration. Mater. Des. 2024, 238, 112655. [Google Scholar] [CrossRef] [Scilit]
- Burelo, M.; Acosta, S.; Bedolla-Valdez, Z.I.; Ríos-González, J.A.; López-Sandoval, R.; Encinas, A.; Escobar-Barrios, V.; Gaytán, I.; Stringer, T. Bio-Based Polymer Composites and Nanocomposites: A Sustainable Approach. Macromol 2026, 6, 24. [Google Scholar] [CrossRef] [Scilit]
- Zhao, H.; Liu, S.; Wei, Y.; Yue, Y.; Gao, M.; Li, Y.; Zeng, X.; Deng, X.; Kotov, N.A.; Guo, L.; et al. Multiscale Engineered Artificial Tooth Enamel. Science 2022, 375, 551–556. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Elkhouly, M.A.; Emara, M.M.; Nady, N.; Elkadi, A.S.; Kandil, S.H. Bioinspired Enamel Repair via Inorganic Ionic Polymerization Using Calcium Phosphate Ionic Clusters and Nano-Hydroxyapatite. Sci. Rep. 2025, 15, 20207. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Zhao, H.; Liu, S.; Lu, J.; Yang, X.; Yang, Z.; Li, F.; Guo, L. Natural Tooth Enamel and Its Analogs. Cell Rep. Phys. Sci. 2022, 3, 100945. [Google Scholar] [CrossRef] [Scilit]
- Daher, R.; Krejci, I.; Mekki, M.; Marin, C.; Di Bella, E.; Ardu, S. Effect of Multiple Enamel Surface Treatments on Micro-Shear Bond Strength. Polymers 2021, 13, 3589. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Wilmers, J.; Bargmann, S. Nature’s Design Solutions in Dental Enamel: Uniting High Strength and Extreme Damage Resistance. Acta Biomater. 2020, 107, 1–24. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Ismail, B.; Soliman, Z.; El-Askary, F. Evaluation of the Effects of Different Remineralizing Agents on the Microhardness and Mineral Content of Bleached Enamel along Different Storage Times. BMC Oral Health 2026, 26, 416. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Lu, J.; Deng, J.; Wei, Y.; Yang, X.; Zhao, H.; Zhao, Q.; Liu, S.; Li, F.; Li, Y.; Deng, X.; et al. Hierarchically Mimicking Outer Tooth Enamel for Restorative Mechanical Compatibility. Nat. Commun. 2024, 15, 10182. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Luo, N.; Lu, B.-Q.; Deng, Y.-W.; Zeng, H.; Zhang, Y.; Zhan, J.-Y.; Xu, X.-C.; Cao, G.-Z.; Wen, J.; Zhang, Z.; et al. The Glycerol Stabilized Calcium Phosphate Cluster for Rapid Remineralization of Tooth Enamel by a Water-Triggered Transformation. Nat. Commun. 2025, 16, 58. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Tang, S.; Shen, Y.; Jiang, L.; Zhang, Y. Surface Modification of Nano-Hydroxyapatite/Polymer Composite for Bone Tissue Repair Applications: A Review. Polymers 2024, 16, 1263. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Lyu, D.; Zhang, Q.; Wu, Y.; Chen, L.; Li, X.; Ren, H.; Yan, Y. Effects of Particle Size of Hydroxyapatite on Mechanical Property and Cytocompatibility of Hydroxyapatite/Poly(Amino Acid) Composites. Polym. Compos. 2022, 43, 1107–1120. [Google Scholar] [CrossRef] [Scilit]
- Riau, A.K.; Venkatraman, S.S.; Mehta, J.S. Biomimetic vs. Direct Approach to Deposit Hydroxyapatite on the Surface of Low Melting Point Polymers for Tissue Engineering. Nanomaterials 2020, 10, 2162. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Kaushik, N.; Nhat Nguyen, L.; Kim, J.H.; Choi, E.H.; Kumar Kaushik, N. Strategies for Using Polydopamine to Induce Biomineralization of Hydroxyapatite on Implant Materials for Bone Tissue Engineering. Int. J. Mol. Sci. 2020, 21, 6544. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Sarkari, S.; Khajehmohammadi, M.; Davari, N.; Li, D.; Yu, B. The Effects of Process Parameters on Polydopamine Coatings Employed in Tissue Engineering Applications. Front. Bioeng. Biotechnol. 2022, 10, 1005413. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Coy, E.; Iatsunskyi, I.; Colmenares, J.C.; Kim, Y.; Mrówczyński, R. Polydopamine Films with 2D-like Layered Structure and High Mechanical Resilience. ACS Appl. Mater. Interfaces 2021, 13, 23113–23120. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Felfel, R.M.; Parsons, A.J.; Chen, M.; Stuart, B.W.; Wadge, M.D.; Grant, D.M. Water Resistant Fibre/Matrix Interface in a Degradable Composite: Synergistic Effects of Heat Treatment and Polydopamine Coating. Compos. A Appl. Sci. Manuf. 2021, 146, 106415. [Google Scholar] [CrossRef] [Scilit]
- Saraf, M.; Prateek; Ranjan, R.; Balasubramaniam, B.; Thakur, V.K.; Gupta, R.K. Polydopamine-Enabled Biomimetic Surface Engineering of Materials: New Insights and Promising Applications. Adv. Mater. Interfaces 2024, 11, 2300670. [Google Scholar] [CrossRef] [Scilit]
- Liebscher, J. Chemistry of Polydopamine—Scope, Variation, and Limitation. Eur. J. Org. Chem. 2019, 2019, 4976–4994. [Google Scholar] [CrossRef] [Scilit]
- Ball, V. Composite Materials and Films Based on Melanins, Polydopamine, and Other Catecholamine-Based Materials. Biomimetics 2017, 2, 12. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Lee, H.; Dellatore, S.M.; Miller, W.M.; Messersmith, P.B. Mussel-Inspired Surface Chemistry for Multifunctional Coatings. Science 2007, 318, 426–430. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Kral, M.; Dendisova, M.; Svoboda, J.; Cernescu, A.; Svecova, M.; Johnson, C.M.; Pop-Georgievski, O.; Matejka, P. Nano-FTIR Spectroscopy of Surface Confluent Polydopamine Films—What Is the Role of Deposition Time and Substrate Material? Colloids Surf. B Biointerfaces 2024, 235, 113769. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Svoboda, J.; Král, M.; Dendisová, M.; Matějka, P.; Pop-Georgievski, O. Unraveling the Influence of Substrate on the Growth Rate, Morphology and Covalent Structure of Surface Adherent Polydopamine Films. Colloids Surf. B Biointerfaces 2021, 205, 111897. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- García-Mayorga, J.C.; Rosu, H.-C.; Jasso-Salcedo, A.B.; Escobar-Barrios, V.A. Kinetic Study of Polydopamine Sphere Synthesis Using TRIS: Relationship between Synthesis Conditions and Final Properties. RSC Adv. 2023, 13, 5081–5095. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Zhang, C.; Ou, Y.; Lei, W.-X.; Wan, L.-S.; Ji, J.; Xu, Z.-K. CuSO4/H2O2-Induced Rapid Deposition of Polydopamine Coatings with High Uniformity and Enhanced Stability. Angew. Chem. Int. Ed. 2016, 55, 3054–3057. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Lázaro-Martínez, J.M.; Lombardo Lupano, L.V.; Piehl, L.L.; Rodríguez-Castellón, E.; Campo Dall’ Orto, V. New Insights about the Selectivity in the Activation of Hydrogen Peroxide by Cobalt or Copper Hydrogel Heterogeneous Catalysts in the Generation of Reactive Oxygen Species. J. Phys. Chem. C 2016, 120, 29332–29347. [Google Scholar] [CrossRef] [Scilit]
- Seredin, P.; Goloshchapov, D.; Emelyanova, A.; Eremeev, K.; Peshkov, Y.; Shikhaliev, K.; Potapov, A.; Ippolitov, Y.; Kashkarov, V.; Nesterov, D.; et al. Rapid Deposition of the Biomimetic Hydroxyapatite-Polydopamine-Amino Acid Composite Layers onto the Natural Enamel. ACS Omega 2024, 9, 17012–17027. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Chang, J.; Tavakol, M.; Besnard, C.; Korsunsky, A.M.; Tan, J.-C. Biomimetic Enamel-like Crystals: A Versatile Platform for Unraveling the Basic Mechanisms of Demineralization and Remineralization. ACS Appl. Mater. Interfaces 2025, 17, 50505–50518. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Nakamura, M.; Nagai, A.; Hentunen, T.; Salonen, J.; Sekijima, Y.; Okura, T.; Hashimoto, K.; Toda, Y.; Monma, H.; Yamashita, K. Surface Electric Fields Increase Osteoblast Adhesion through Improved Wettability on Hydroxyapatite Electret. ACS Appl. Mater. Interfaces 2009, 1, 2181–2189. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Ficai, A.; Andronescu, E.; Trandafir, V.; Ghitulica, C.; Voicu, G. Collagen/Hydroxyapatite Composite Obtained by Electric Field Orientation. Mater. Lett. 2010, 64, 541–544. [Google Scholar] [CrossRef] [Scilit]
- Kim, M.; Yun, H.; Kim, G.H. Electric-Field Assisted 3D-Fibrous Bioceramic-Based Scaffolds for Bone Tissue Regeneration: Fabrication, Characterization, and in Vitro Cellular Activities. Sci. Rep. 2017, 7, 3166. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Zhang, C.; Li, Y.; Li, H.; Zhang, Q.; Lu, J. Overview of Electric-Field-Induced Deposition Technology in Fabricating Organic Thin Films. J. Mater. Chem. C 2021, 9, 374–394. [Google Scholar] [CrossRef] [Scilit]
- Seredin, P.; Goloshchapov, D.; Litvinova, T.; Peshkov, Y.; Ippolitov, Y.; Freitas, R.O.; Maia, F.C.B.; Mahdy, I.A. Electric Field-Guided Biomimetic Mineralization of Enamel via Interfacial Engineering of Nanostructured HAp/PDA Coatings with Anisotropy and Enhanced Hardness. ACS Biomater. Sci. Eng. 2026, 12, 2130–2155. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Boccaccini, A.R.; Keim, S.; Ma, R.; Li, Y.; Zhitomirsky, I. Electrophoretic Deposition of Biomaterials. J. R. Soc. Interface 2010, 7, S581–S613. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Baştan, F.E.; Akhtar, M.A.; Krapf, A.; Roether, J.; Beltrán, A.M.; Göken, M.; Boccaccini, A.R. Bioinspired Nacre-like Hierarchical Chitosan/Hydroxyapatite Coatings by Electrophoretic Deposition. Appl. Mater. Today 2026, 48, 103002. [Google Scholar] [CrossRef] [Scilit]
- Seredin, P.; Goloshchapov, D.; Kashkarov, V.; Emelyanova, A.; Buylov, N.; Barkov, K.; Ippolitov, Y.; Khmelevskaia, T.; Mahdy, I.A.; Mahdy, M.A.; et al. Biomimetic Mineralization of Tooth Enamel Using Nanocrystalline Hydroxyapatite under Various Dental Surface Pretreatment Conditions. Biomimetics 2022, 7, 111. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Ibrahim, A.I.; Al-Hasani, N.R.; Al-Taai, N.T.; Ismail, H.M.; Abdulrahman, A.A.; Sauro, S. Enamel Conservation Orthodontic Paradigm via Treatment with Newly Developed Remineralizing Calcium-Phosphate Etchant Pastes. J. Dent. 2025, 157, 105776. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Goloshchapov, D.L.; Lenshin, A.S.; Savchenko, D.V.; Seredin, P.V. Importance of Defect Nanocrystalline Calcium Hydroxyapatite Characteristics for Developing the Dental Biomimetic Composites. Results Phys. 2019, 13, 102158. [Google Scholar] [CrossRef] [Scilit]
- Goloshchapov, D.; Buylov, N.; Emelyanova, A.; Ippolitov, I.; Ippolitov, Y.; Kashkarov, V.; Khudyakov, Y.; Nikitkov, K.; Seredin, P. Raman and XANES Spectroscopic Study of the Influence of Coordination Atomic and Molecular Environments in Biomimetic Composite Materials Integrated with Dental Tissue. Nanomaterials 2021, 11, 3099. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Manoj, M.; Subbiah, R.; Mangalaraj, D.; Ponpandian, N.; Viswanathan, C.; Park, K. Influence of Growth Parameters on the Formation of Hydroxyapatite (HAp) Nanostructures and Their Cell Viability Studies. Nanobiomedicine 2015, 2, 1. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Okada, M.; Matsumoto, T. Synthesis and Modification of Apatite Nanoparticles for Use in Dental and Medical Applications. Jpn. Dent. Sci. Rev. 2015, 51, 85–95. [Google Scholar] [CrossRef] [Scilit]
- Drouet, C. Apatite Formation: Why It May Not Work as Planned, and How to Conclusively Identify Apatite Compounds. BioMed Res. Int. 2013, 2013, 490946. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Risnes, S.; Saeed, M.; Sehic, A. Scanning Electron Microscopy (SEM) Methods for Dental Enamel. In Odontogenesis; Papagerakis, P., Ed.; Methods in Molecular Biology; Springer: New York, NY, USA, 2019; Volume 1922, pp. 293–308. ISBN 978-1-4939-9011-5. [Google Scholar]
- Murphy, B.; Baez, J.; Morris, M.A. Characterising Hydroxyapatite Deposited from Solution onto Novel Substrates: Growth Mechanism and Physical Properties. Nanomaterials 2023, 13, 2483. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Bogdan, D.; Grosu, I.-G.; Filip, C. How Thick, Uniform and Smooth Are the Polydopamine Coating Layers Obtained under Different Oxidation Conditions? An in-Depth AFM Study. Appl. Surf. Sci. 2022, 597, 153680. [Google Scholar] [CrossRef] [Scilit]
- Kopani, M.; Mikula, M.; Takahashi, M.; Rusnák, J.; Pinčík, E. FT IR Spectroscopy of Silicon Oxide Layers Prepared with Perchloric Acid. Appl. Surf. Sci. 2013, 269, 106–109. [Google Scholar] [CrossRef] [Scilit]
- Chen, S.; Liang, C.; Li, P.; Liu, C.; Zeng, X.; Xiong, X.; Ni, X. Polydopamine/Polyvinyl Alcohol/Graphene Oxide Transition Layer for Enhancing Adhesive Performance of HA Coating on Cf/C Composites Prepared by Hydrothermal Electrodeposition/Hydrothermal Treatment. J. Mater. Sci. Mater. Med. 2025, 36, 67. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Feng, P.; Qiu, X.; Yang, L.; Liu, Q.; Zhou, C.; Hu, Y.; Shuai, C. Polydopamine Constructed Interfacial Molecular Bridge in Nano-Hydroxylapatite/Polycaprolactone Composite Scaffold. Colloids Surf. B Biointerfaces 2022, 217, 112668. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Madhubala, M.M.; Mahalaxmi, S. Effect of Polydopamine Nanoparticle-Induced Surface Modification on Demineralized Dentin for Enhanced Functional Remineralization. J. Pharm. Bioallied Sci. 2024, 16, S4832–S4843. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Jiang, Y.; Katsura, K.A.; Badt, N.Z.; Didziokas, M.; Dougherty, S.; Bhoj, E.J.; Vining, K.H. Multimodal Characterization of Rodent Dental Development. ACS Appl. Mater. Interfaces 2025, 17, 33745–33755. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Iatsunskyi, I.; Nowaczyk, G.; Jurga, S.; Fedorenko, V.; Pavlenko, M.; Smyntyna, V. One and Two-Phonon Raman Scattering from Nanostructured Silicon. Optik 2015, 126, 1650–1655. [Google Scholar] [CrossRef] [Scilit]
- Ivanda, M. Raman Spectroscopy of Porous Silicon. In Handbook of Porous Silicon; Springer: Cham, Switzerland, 2016; pp. 1–10. ISBN 978-3-319-04508-5. [Google Scholar]
- Gunde, M.K. Vibrational Modes in Amorphous Silicon Dioxide. Phys. B Condens. Matter 2000, 292, 286–295. [Google Scholar] [CrossRef] [Scilit]
- Zangmeister, R.A.; Morris, T.A.; Tarlov, M.J. Characterization of Polydopamine Thin Films Deposited at Short Times by Autoxidation of Dopamine. Langmuir 2013, 29, 8619–8628. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Malisz, K.; Świeczko-Żurek, B.; Olive, J.-M.; Gajowiec, G.; Pecastaings, G.; Laska, A.; Sionkowska, A. Study of Nanohydroxyapatite Coatings Prepared by the Electrophoretic Deposition Method at Various Voltage and Time Parameters. Materials 2024, 17, 2242. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Tang, Y.; Xing, G.; Shu, X.; Yan, N.; Zhang, Y.; Yuan, H.; Wu, X.; Chen, Q. Electric Field-Induced Deposition of Polydopamine and Polydopamine-Based Composite Coating for Enhanced Osteogenesis. J. Colloid Interface Sci. 2026, 702, 139003. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Choi, S.-M.; Jung, H.-W.; Ryu, J.H.; You, H.-K. Effect of Polydopamine and Fluoride Ion Coating on Dental Enamel Remineralization: An in Vitro Study. BMC Oral Health 2023, 23, 526. [Google Scholar] [CrossRef] [Scilit] [PubMed]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.