Skip to Content
Applied NanoApplied Nano
  • Article
  • Open Access

24 November 2026

30 Pages

Reduction in Transmission Electron Microscopy Lamella Bending on the Micron-Scale Utilizing Finite Element Analysis and Applied Carbon Support

1
Department of Physics, Portland State University, Portland, OR 97207, USA
2
Metrology, Lam Research, Tualatin, OR 97062, USA

Abstract

Transmission electron microscopy (TEM) sample preparation is traditionally performed without stress analysis. Finite element analysis (FEA) was used to visualize stress in TEM lamella on the micron scale. FEA is used to evaluate stress reduction by application of a support structure to the TEM lamella. An electron transparent support structure is fabricated using electron beam deposition of a low-z carbon material. It is experimentally shown to reduce lamella warping. The technique was applied to a thick, high atomic weight tungsten film, and multiple sub-15 nm thick TEM lamella were obtained. Lamella thicknesses were validated using cross-sectional characterization. The technique was iterated into a plate-grid support structure, and the grid spacing and grid thickness were parameterized; this was shown to further reduce lamella bending by more than 50%.

1. Introduction

In the semiconductor industry, the standard metrology processes for critical dimensional analysis have evolved over the last 40 years with the development and maturation of the scanning electron microscope (SEM) and focused ion beam (FIB) dual-beam microscope [1,2,3,4,5,6]. The dual-beam microscope has developed into a highly capable tool for transmission electron microscopy (TEM) sample prep, energy dispersive x-ray (EDX) analysis, and electron backscatter diffraction (EBSD) crystal analysis. TEM sample preparation garners a vast quantity of time allocation from dual beams in many labs. TEM preparation is a time-consuming process that grants the ability to extract and characterize the critical dimensions from anywhere on a die surface. The most critical and time-consuming procedure for TEM preparation is the final thinning procedure [7]. This is the point where permanent and likely disastrous sample damage is most likely to occur. The standard procedure to mitigate sample damage is to perform a FIB mill using low accelerating voltages to minimize surface damage and to ultimately produce a lamella of under 100 nm for TEM and under 50 nm for scanning transmission electron microscopy (STEM). One critical hindrance to this technique is the decrease in FIB resolution at lower accelerating voltages such as 2–8 kV. Newer dual beams have improved upon FIB resolution [8] in recent years, yet newer systems are expensive and unaffordable for the majority of labs.
The two common TEM lamella geometries that are widely known are the upright and inversion geometries [7,9], as shown in Figure 1. Shown in Figure 1a, the upright TEM lamella configuration has an area of interest (AOI) near the top of the lamella with a protective cap above this. The protective cap prevents ion beam damage during sample processing. In the upright TEM lamellae configuration, the FIB is used to thin the sample from the top (Figure 1b), with both the front and back of the lamella being thinned until the protective cap is depleted (Figure 1c). These lamella are typically limited to a thickness of approximately 25–30 nanometers due to the beam broadening that occurs at low kV thinning, i.e., 2 kV and 5 kV. Even with these limitations, the upright TEM sample preparation process is a popular tool that allows rapid preparation of many sample types. The 25 nm minimum thickness of an upright lamella prevents its application to smaller logic structures.
Figure 1. Figure illustrates the upright and inverted lamella configurations. (a) shows the upright TEM lamella configuration. The protective cap is at the top, the area of interest (AOI) near the top of the lamella, and the silicon substrate is located below. (b) shows the FIB mill direction relative to the AOI location. (c) shows a plane cross-section of the upright lamella to illustrate where the thinnest regions of a TEM lamella are. The upright lamellae are thinnest at the top. (d) shows the inverted TEM lamella configuration. The protective cap is on the bottom, the AOI is just above this, and the silicon substrate is above both, acting as a cap material. (e) shows the FIB mill direction relative to the AOI region. (f) shows a plane cross-section of the inverted lamellae to illustrate where the thinnest regions of the TEM lamella are. The inverted geometry can be thinner than the upright geometry, but it utilizes a tapered mill which results in large AOI not being thinned uniformly.
The inversion TEM sample preparation process utilizes a TEM sample configuration where the TEM sample is flipped upside down to enable ultra-thin lamella fabrication using a wedge thinning approach as shown in Figure 1d. In the inverted TEM geometry, the AOI is placed near the bottom of the TEM lamella as shown in Figure 1d, and it is thinned from the top where the silicon substrate acts as the protective cap, as shown in Figure 1e. The inverted TEM process uses some mechanical process to flip the TEM lamella and thin it from the bottom of the sample [7,10,11]. The mechanical flipping process typically involves a double-weld [7] liftout process combined with stage and nano-manipulator needle rotations, which can result in sample loss due to poor weld geometry. Newer systems are able to perform inversion more reliably using a process of elaborate liftout angles (stage tilts and stage rotations) and nano-manipulator rotations that depend on system capability. The major benefit for the inversion process is that it negates the limitation from the beam broadening that occurs in the upright process. This is achieved by using an inverted wedge geometry, with the area of interest at the thinnest region of the wedge (Figure 1f). The inverted thinning process is much slower due to the need to thin through the Si substrate, which is typically 3–5 µm tall, whereas a typical protective cap thickness on the upright process is approximately 1 µm tall. The inversion process struggles with producing TEM lamella with large areas of uniform thickness due to the convergent angled nature of the sample geometry, as shown in Figure 1f. Figure 1c,f shows the cross-sections of TEM lamellae with upright and inverted geometries.
The process of making lamella is very much still an art form in regard to the lack of an engineered lamella. While there has been considerable work put into characterizing the stress in nanostructures using TEM [12,13,14,15,16,17,18], and even exploration of applying bracing to TEM samples [19,20,21,22], the micron-scale geometry of a TEM lamella is generally unrefined and unengineered.
In the field of cryo-electron microscopy, there have been multiple attempts at applying FEA simulations to evaluate the stress that develops in TEM lamellae in the presence of large temperature swings that are observed in the sample transfer process used in the sample fabrication process. Gorelick et al. [23] and Wachsmuth-Melm et al. [24] have investigated adding micro-expansion joints around the TEM lamella on the bulk sample stage and on the TEM grid for final thinning to reduce the stress observed with thermal expansion while milling at high FIB currents. Gorelick also explored the fabrication of a filet mill profile that allows a reduction in stress near the edges of the lamella window. Gorelick et al. were able to demonstrate a 40% improvement in overall yield by reducing lamella breakage. In both papers, FEA was applied using a static simulation and Von Mises stress was used to characterize the stress applied. The simulations were performed in the low stress, pre-yield regions, validating the use of a static simulation.
Engineering TEM lamella support structures is an active and ongoing field. Wolf et al. [25] have developed a support geometry to allow large-area thinning of cryo-TEM samples using a grounded ridge and furrow geometry that allows stable fabrication of TEM windows of approximately 3 × 40 μm2; however, the lamella was only thinned down to 150 nm, a relatively thick lamella for the semiconductor industry. The grounded ridge and furrow geometry is better described as a periodic window milling process, with thick support regions being placed between the thinned window regions. Wang et al. (2023) [26] developed a process for creating micro-expansion joints on the TEM lamella that minimize the transfer of stress from the TEM grid to the TEM window during large temperature changes observed in the cryo-electron microscopy workflow. Neither Wang nor Wolff performed finite element analysis on their support structure or expansion joints.
In this work, I propose the next steps to engineer a lamella using finite element analysis (FEA) and a novel coating process to reduce the structural bending in a lamella. By refining the geometry of a TEM lamella using FEA, I save significant tool time and cost on both a dual beam system for sample preparation and TEM time for sample characterization.
I propose a sample preparation technique that can be applied to existing dual beam systems that allow the preparation of thin lamella using the upright, or inversion lamella configurations. I utilize an in-situ carbon gas injection system (Carbon GIS) to apply an electron beam induced deposited carbon (EBID-Carbon) layer of 50–130 nm thickness to the frontside of the lamella. The carbon acts as a support material, allowing the sample to be further thinned than traditionally allowed. The EBID-Carbon is a low z material that is semi-transparent in the STEM imaging process. Further, it is amorphous [27], which reduces measurement interference while adding support to the lamella. I then refined the support structure from a single plate to a plate-and-grid geometry to further explore lamella bending reduction.

2. Materials and Methods

In this section, I will introduce FEA and then list the steps to perform the experiment with sufficient information for replicating the work. I will describe each topic in individual sections due to subject length.

2.1. Finite Element Analysis Simulation of TEM Window

Finite element analysis is a numerical method for solving differential equations that dictate the material response to an applied force with well-defined boundary conditions. Fusion 360 Simulation was used to qualitatively evaluate the static stresses on various lamella geometries [28]. Fusion evaluates the Von Mises stress as a criterion for yielding used for ductile materials such as metals. Von Mises stress states that an object will yield and fail if the stress components acting on it are greater than the yield limit of the material [29].
Our use of FEA simulation software is used as a test probe to evaluate, qualitatively, the weak points of a lamella geometry. The evaluation probes the relative stress and displacements of the TEM window as the TEM lamellae geometry is modified. The test force which is applied during the FEA simulation is intended to illuminate regions of high stress, not to replicate forces experienced during sample fabrication or handling.
I decided against performing FEA simulations on the actual FIB milling process due to the inability to accurately capture the dynamic nature of the FIB mill process. To elaborate on the dynamic FIB milling process, as a sample is milled, it experiences a temperature rise that is proportional to the FIB mill energy and current, and the material properties change as a function of temperature, which need to be accurately modeled. Second, the mill process itself is dynamic, with the FIB milling being performed in a rastered approach and the FIB only exposed to a single point per unit time, which is not easily simulated in FEA due to the FEA simulation using force over an area. Other difficulties with FEA modeling on the nanoscale is that the material properties are not the same as bulk properties, which make any quantified simulation to be rough at best. In addition, the FIB milling process itself damages the crystalline structure of the sample, changing it to an amorphous material which has differing material properties. Another challenge is the ion-induced plasticization of the FIB mill surface changes material properties that further degrade the simulation accuracy due to not being accounted for in material properties. In summary, the FEA modeling is applied as a test force to probe lamella geometric stresses and does not represent a realistic, applied force. I performed a static linear simulation for simple visualization of stress. A non-linear simulation would show the dynamic deformation of the TEM lamellae, but I question the value of the simulation based on the inability to capture the nano-scale material dynamics described above.

2.2. Materials Used for Simulations

In my simulations, I used bulk material properties for the silicon, tungsten and platinum materials. I used a diamond-like carbon material for the support material, which should be noted as significantly weaker than diamond material, with approximately 1–2% the strength of diamond. I list material properties used in the FEA simulation in Appendix Table A1.

2.3. Simulation Configuration

Autocad 123D was used to fabricate 3D files for simulation. The lamella geometry was closely modeled after a standard upright lamella as shown in Figure 2a. The 3D lamella object consisted of four layers, a silicon substrate, a FIB deposited tungsten layer, a platinum cap, and a support carbon, as shown in Figure 1c. A force vector shown as blue arrows in Figure 2b was applied to the back of each lamella. The force vector was 99% down along the y-axis and 1% into the z-axis as shown in Figure 2b. The magnitude of the force vector was approximately 1 µN. A rigid support surface shown in Figure 2f as a selected plane was placed at the bottom of the lamella since lamella are typically placed on flat, rigid surfaces. This plane acts as a non-deformable boundary. For the four simulated lamella, the first lamella had 0 nm of carbon, and a lamella thickness of 50 nm was used. For simulations of carbon-supported lamella, the non-supported region was 10 nm thick, and the carbon support layer was 70 nm, 140 nm, and 210 nm thick. The results of these four simulations are shown in Figure 3.
Figure 2. Figure illustrates the FEA model set up. (a) shows the thinned lamella geometry. From top to bottom, platinum cap, tungsten film, silicon substrate. (b) shows the force vectors applied to the back face of the lamella with the blue faces being the faces with a force applied. (c) shows the carbon support film being added to the front face of the lamella, visualized as the selected blue geometry. (d) Meshing for the front of the lamella. (e) Meshing for the back of the lamella. (f) shows the rigid support face at the bottom of the lamella.
Figure 3. FEA results showing Von Mises Stress, Y-displacement and Z-displacement for lamella with varying thickness carbon layers. For the carbon-supported lamella, the simulated carbon thickness is shown, 70 nm, 140 nm, 210 nm. (a) shows the Von Mises stress for non-supported TEM lamella. (b) shows the Von Mises stress in the carbon-supported TEM lamella. (c) shows the Y-displacement for non-supported TEM lamella. (d) shows the Y-displacement in the carbon-supported TEM lamella. (e) shows the Z-displacement for non-supported TEM lamella. (f) shows the Z-displacement in the carbon-supported TEM lamella. Note: The orientation axis is shown in (b).
A static, linear stress simulation was performed. A model-based simulation meshing was applied with a 3% target mesh size, and the adaptive mech refinement was configured to allow mesh convergence studies to be conducted for each simulation. Specifically, the adaptive mesh refinement was set to a maximum number of 8, the result convergence was set to a target of 5%, and the portion of elements to refine was set to 40%. Von Mises stress was used for evaluating convergence. This produced a variable mesh configuration that varied for each lamella geometry, but for the standard thin film geometries, it produced a mesh with approximately 139k cells and 223k nodes, as shown in Figure 2d,e. The automeshing produced more mesh in regions with high detail, such as the edges of the lamella where a large curvature of geometry is present.

2.4. Results of FEA

Qualitative results from the FEA are shown in Figure 3 for the Von Mises stress, Y-displacement and Z-displacement for comparison between a non-supported TEM lamellae and three carbon thin film-supported TEM lamellae. Please note that the scale comparison between the non-supported lamellae and the carbon thin film-supported lamellae are not the same due to the range of stress and displacement observed between the simulations. The maximum stress observed in the non-supported lamella is approximately 34× larger than that observed in the lamellae with support. For the lamella without support Figure 3a, one sees that the stress is concentrated around the edges of the lamella window, mainly in the tungsten thin film material. The edges act as anchor points that are fixed and cannot easily flex. Comparing the three lamella with increasingly thick carbon films in Figure 3b, one observes that lamellae have reduced stress in all regions, and a qualitative trend is that a reduction in stress is observed as more support is added.
The observed displacements were evaluated in the y and z directions due to this corresponding to the applied test force vector orientation. An orientation axis is shown to the right in Figure 3b. In the simulation configuration, the y-axis is in the vertical direction and the z-axis is normal to the TEM lamella surface, i.e., into the lamellae. The trend observed is that the magnitude of displacements decreases as more support is applied, as shown in Figure 3c,d. The maximum y displacement for the non-supported lamellae was approximately 1.6× that of the supported lamellae. The position of the maximum displacement in the z-axis on the non-supported lamella is located centrally below the tungsten film, as shown in Figure 3e. For the supported TEM lamellae, this maximum displacement region is located near the top of each lamella as shown in Figure 3f. The maximum z displacement for the non-supported lamellae was approximately 10× that of the supported lamellae. One cannot identify or interpret TEM lamella bending as occurring from these results due to these simulations being linear and static, whereas a bending process is inherently a non-linear process. Qualitatively interpreting the simulation results, one can expect that the TEM lamella will exhibit less stress and displacements with more carbon thin film support.
To validate the interpretation of these FEA results, I fabricated four lamellae, one without carbon support and three with increasingly thicker carbon supports. The thinned lamella were imaged using STEM and then cross-sectioned to evaluate window bending, the support film thickness and the tungsten film thickness.
As a follow-up experiment, I fabricated 12 more lamella with an additional carbon support structure added. The carbon support structure was applied in a plate-and-grid geometry, with the grid spacing parameter being swept between 100 nm, 200 nm, and 300 nm and grid thickness ranging between 18 nm and 80 nm. The plate thickness was kept constant at approximately 50 nm. The fabrication sequence was to fabricate the plate, then fabricate the grid on top of the plate. FEA simulations of these lamella geometries are shown in the supplementary materials file. The general trend observed in those simulations was that additional support decreases the observed stress and the y, z displacements are lowered. This was not always the observation, and, in some instances, the displacement was not always decreasing as support thickness increased. In all simulations, the observed stress in the carbon-supported lamellae was always lower than the non-supported TEM lamellae.

2.5. Experimental Procedure

The workflow implemented to perform the experiment is shown in Figure 4. The main sections are FIB deposition of W film, TEM sample preparation and liftout, front side processing, SEM deposition of support substrate on lamella, back side lamella processing, STEM characterization of W thin film, and finally, cross-sectional analysis to evaluate support performance.
Figure 4. Process workflow for the experiment.

2.5.1. Sample

A blanket 100 silicon wafer (Part Number 21610-510, Ted Pella, Redding, CA, USA) was used as the sample substrate for this work.

2.5.2. TEM Preparation Tool

A Thermo Scientific (Thermo Fisher Scientific, Hillsboro, OR, USA) 5FX dual-beam was used for TEM sample prep. This system has an in situ easy-lift nano-manipulator for TEM sample extraction, a multi-chemical Gas-Injection System (GIS) for in situ material deposition using the SEM or FIB, and an in-situ 30 kV STEM detector for STEM characterization capability.

2.5.3. TEM Preparation Procedure

The bulk preparation procedure is well described elsewhere [6,7,8,9]. I only list the basic steps to create a lamella and move it to the TEM grid for final thinning. Note that the TEM thinning and sample cross-sectioning were performed on an in situ TEM rod, called a compustage. This stage has both alpha and beta tilt capabilities. The alpha tilt replaces that traditional tilt axis of the bulk stage, i.e., it tilts the sample between the SEM and FIB. The beta axis is comparable to a bulk stage rotation, i.e., it allows the lamella to be flipped 180° so that the operator can view and process the other side of the lamella while maintaining visibility of the cut surface with the SEM. The design of the compustage allows zone axis alignment for ultra-high resolution in situ STEM imaging.

2.5.4. Bulk Prep

The standard TEM sample preparation procedure is described below and the process conditions are summarized in Table 1 below.
Table 1. Summary TEM lamella fabrication and thinning steps.
  • Tungsten deposited film was deposited on a Si wafer using a standard FIB deposition technique, using a low energy of 8 kV, 0.63 nA, and using an in-situ gas injection system. The tungsten application type was used with a rectangle pattern. The FIB used the internal chamber electronics (ICE) detector, with SE biasing.
    a.
    FIB deposition of tungsten was calibrated on the Si bulk. Three depositions were performed to get an estimate of the deposition rate. A target deposition of approximately 600 nm of tungsten was performed for the experiment.
    b.
    A protective platinum cap was applied on top of the FIB deposited tungsten cap. The same beam conditions were used. Approximately 1 µm of platinum was deposited. The platinum application type was used with a rectangle pattern.
  • Bulk Mill #1: The sample was bulk milled using a 30 kV, 9.9 nA FIB. A silicon application type was used with a regular cross-section pattern.
  • Bulk Mill #2: The sample was milled using a 30 kV, 2.4 nA FIB. A silicon application type was used with a regular cross-section pattern.
  • Undercut Mill: The sample was undercut milled using a 30 kV, 2.4 nA FIB. A silicon application type was used with a polygon pattern to create the standard j-cut.
  • Liftout: The sample was placed at beam coincidence. A sharpened easy-lift needle was welded to the TEM lamella using the FIB at 30 kV, 90 pA using carbon multi-Chem deposition. It was cut free from the bulk using 0.79 nA. The lamella was raised 100 µm above the sample and the needle was retracted.
  • Weld to grid: The TEM grid was placed at beam coincidence. The easy-lift needle was reinserted and lowered to the TEM grid and welded using 30 kV, 0.23 nA with carbon multi-Chem deposition. The easy-lift needle was cut free using 30 kV, 0.79 nA.
  • The TEM grid was tilted to 52° to place the top of the lamella to be normal to the FIB, and the front/back sides of the lamellae were cleaned up with a small cleaning cross-section mill. The mill was performed with a 30 kV, 0.44 nA FIB.
  • The sample windows were thinned to approximately 200 nm thickness using a 30 kV, 0.23 nA beam.

2.5.5. Calibration of SEM Deposition

Prior to final thinning the lamella, SEM deposition of carbon was calibrated. SEM carbon deposition was calibrated on the TEM lamella on an in situ TEM grid due to the non-uniformity of the gas flow observed on the TEM grid compared to the bulk sample stage. Three depositions were performed across the surface of a lamella and then cross-sectioned to get a measurement of the deposition rate. The lamella was extra wide to provide space for calibration depositions and the experiment. The lamella was approximately 25 µm wide. The SEM was used to deposit a carbon support material on the milled surface of the lamella. The SEM was set to 1 kV, 1.6 nA, immersion mode. The cross-over was verified prior to deposition to ensure proper beam alignment. Each deposition area was approximately 500 nm × 1000 nm. The z depth used with the patterns for depositions were 50 nm, 100 nm, and 150 nm. The standard c-dep application was used. The cross-section of each deposition was 59 nm, 109 nm, 159 nm. A constant 9 nm offset was used as a calibration.

2.5.6. Front-Side Thinning

With a lamella on the TEM grid, the front side was milled using a 5 kV, 12 pA ion beam using an overtilt of 1.5° on the alpha flip axis. The mill pattern depth was set to 4.0 µm depth using a vol per dose of 0.87 µm3/nC. The mill window was approximately 2.0 µm wide. A standard cleaning cross-section application file was used.

2.5.7. Single-Plate Fabrication Process

After front-side milling was completed, the SEM was then used to deposit a carbon support material on the milled face. The SEM was set to 1 kV, 1.6 nA, immersion mode. The cross-over was verified prior to deposition to ensure proper beam alignment. Three supported lamellae were fabricated using EBID carbon depositions with target thicknesses of 50 nm, 100 nm, and 150 nm respectively. The depth correction factor was used to calibrate the deposition. One non-supported lamella was fabricated without carbon deposition. These target plate deposition thicknesses are summarized in Table 2 below.
Table 2. Summary carbon support deposition parameters.

2.5.8. Plate and Grid Fabrication Process

Fabrication of the grid support structure used a 10 nm × 2 µm box pattern, and it was spaced using the array function of the microscope software. A grid of horizontal and vertical lines were fabricated. To evaluate the plate grid support geometry, 12 lamella were made, with a grid line spacing of 100 nm, 200 nm, and 300 nm; at each grid line spacing, the line thickness was varied with target thicknesses ranging through 18 nm, 36 nm, 54 nm and 80 nm. A plate of 2 µm × 2 µm with a target thickness of 50 nm was deposited onto each lamella window prior to fabrication of the grid structure. The depth correction factor was used to calibrate all depositions. These target plate and grid deposition thicknesses are summarized in Table 2 below.

2.5.9. Backside Thinning

The lamella were then backside thinned using a −1.5° under tilt on the alpha flip axis. A 5 kV, 12 pA beam was used to thin the lamella. The mill pattern depth was set to 4.0 µm depth using a vol per dose of 0.87 µm3/nC. The mill window was approximately 1.8 µm wide. For carbon-supported lamella, thinning was performed until the W film started to be milled away, at which point milling was stopped. For the non-supported lamella, thinning was performed until the protective cap was depleted. The SEM was used to view the lamella as they were thinned. The SEM was operated in HR mode, 20 kV, 100 pA, using an in situ STEM detector in bright field mode.

2.5.10. STEM Imaging

STEM imaging was performed in In-lens mode with a 1.9 mm working distance (WD) with a stage alpha flip tilt of 90°. The SEM was set to 30 kV, 25 pA, ultra-high resolution (UHR) mode. Bright field images were acquired. The zone axis alignment was performed on the bulk silicon region of the non-supported TEM window prior to STEM imaging.

2.5.11. Cross-Sectional Analysis of Thin Film-Supported Lamella

The TEM lamellae were cross-sectioned to characterize film thicknesses and the TEM lamella bending profile as shown in Figure 5. To perform the cross-sectional analysis of the lamella, the samples were moved to the neutral mill position with an alpha tilt of 52° relative to the SEM optical axis. The front of the lamella was coated with electron deposited platinum using a 1 kV, 0.8 nA beam using the in situ Multi-Chem with a platinum application as shown in Figure 5b. Deposition time was approximately 60 s using a pattern size to cover the W film, approximately 2.5 µm × 1 µm. The lamella were then flipped 180° using the beta axis rotation, and the backside of the lamellae were coated using the same process. The lamellae were tilted perpendicular to the FIB (alpha tilt of 142°) and the lamella windows were cross-sectioned at discrete heights down into the w film. The first cross-section cut was performed 200 nm into the W film, seen in Figure 5c,d, from the platinum–tungsten interface down into the tungsten film. The stage was set to an alpha tilt of 0° and the sample as SEM imaged at this time; see Figure 5e. The second cut was performed at approximately 400 nm into the W film. All lamella windows were processed on the same lamella liftout, and subsequently, the cross-section cuts were milled across all lamella windows simultaneously to ensure the analysis heights were consistent. After each cross-section cut, the lamella was imaged by the SEM at 0° tilt, 4.15 mm working distance. The SEM was operated at 3 kV 100 pA, UHR mode with the through lens detector (TLD), using a secondary electron bias (SE), TLD-SE.
Figure 5. The diagram illustrates the cross-section process. (a) The lamella stack labeled, from top to bottom—the platinum cap, the tungsten film, and the silicon substrate. Note: The center rectangle denotes the thinned region. (b) shows the SEM deposition of a protective platinum on both sides of the TEM lamellae. (c) illustrates (orange box) milling the tungsten film, creating a cross-section of the lamella. The mill is performed perpendicular to the surface. (d) Milled tungsten and silicon sample. (e) Top-down SEM view of cross-sectioned lamella with the protective platinum appearing as green rectangles; the carbon support layer is black, and the unthinned tungsten layer is gray.

2.5.12. Cross-Sectional Analysis for Plate and Grid Support

The TEM lamella that used a plate and grid support used the same method for cross-sectional characterization as the planar supported samples. The only difference was that the plate and grid lamella were only characterized at the mid-point of the tungsten film, at a height of 300 nm.

3. Results

3.1. EBID Plate Support

Figure 6 below shows the results from the STEM imaging of the four lamella windows. Figure 6a shows a non-supported window, and Figure 6b–d shows the carbon-supported lamella. In Figure 6a, the thinning process was insufficient to achieve electron transparency of the tungsten film. The cap was depleted due to the beam tails of milling at 5 kV, 12 pA. This lamella window would be useful for characterizing film thickness, but not for grain analysis or void inspection. In Figure 6b–d, the tungsten film is able to achieve electron transparency at the top of the film and maintain this transparency even as the film thickness increases. In Figure 6b–d, the lamella all exhibit non-uniform thinning across the horizontal width of the window. This is caused by the thinning window flexing while thinning with the center of the window bending away from the FIB. The edges of the window are fixed and therefore are milled away as the FIB mill progresses. It should be noted that the structures being analyzed can be completely milled away using this carbon support technique, and caution must be exhibited while thinning to prevent such occurrences.
Figure 6. STEM images of each lamella. Sample (a) was thinned until the protective cap was depleted. Samples (b–d) were thinned until W film started to be removed. (a) Non-supported lamella; (b) 44 nm thick carbon support and W film window; (c) 82 nm thick carbon support and W film window; (d) 112 nm thick carbon support and W film window. STEM images captured at 30 kV, 25pA, UHR, bright field mode.

3.2. Cross-Sectional Analysis of Planar Geometry

The SEM images from the cross-sectional analysis are shown in Figure 7 and Figure 8, and measurements are summarized in Table 3 and Table 4. The measurement process is shown in Appendix A.2. Two measurement processes are shown in the Appendix A. The first measurement process shown in Figure A1 used a box averaging over a 50 nm distance at two points and compared the bending of the lamella window at the center and edge of the thinned window. The second measurement process was used to extract the full lamellae bending profile for comparison of the profiles. The first measurement process is used to generate the measurement data in Table 3 and Table 4.
Figure 7. This diagram shows SEM images of cross-sectioned lamella windows with features of interest labeled. (a) Cross-sectioned SEM image of non-supported Tungsten lamella with materials labeled. (b) Cross-sectioned SEM image of carbon-supported tungsten lamella with materials labeled.
Figure 8. Cross-section SEM images of each lamella window to characterize bending. The left column shows cross-sections at 200 nm into W film. The right column shows cross-sections at 400 nm into the W film. Both depths are relative to the top of the W film. Total W film height was 690 nm. Images (a,b) show cross-sections of lamella with no carbon support added. Images (c,d) show cross-sections of lamella with 44 nm of carbon support added. Images (e,f) show cross-sections of lamella with 82 nm of carbon support added. Images (g,h) show cross-sections of lamella with 121 nm of carbon support added. SEM images captured at 3 kV, 100 pA, UHR, TLD secondary electron mode.
Table 3. Cross-sectional thickness and bending measurements for 200 nm into tungsten film. Note: Target carbon thicknesses are shown in the lamella window column. Measured thicknesses are in the carbon thickness column. Error is 2.5 nm (pixel size).
Table 4. Cross-sectional thickness and bending measurements for 400 nm into tungsten film. Note: Target carbon thicknesses are shown in the lamella window column. Measured thicknesses are in the carbon thickness column. Error is 2.5 nm (pixel size).
Figure 7a shows a top-down cross-section SEM image of the non-supported lamella with materials labeled. Figure 7b shows a top-down cross-section SEM image of the carbon-supported lamella with materials labeled. In Figure 7a,b, one can observe the remaining TEM window encapsulated in protective platinum films. The role of the platinum film is to make the edge measurements easier for carbon film thickness evaluation and bending characterization.
The cross-sectional bending analysis shown in Table 3 (200 nm from top of lamella) and Table 4 (400 nm from top of lamella) found that the carbon-supported lamella were all approximately 10–15 nm thick near (200 nm) the top of the tungsten film and approximately 20–25 nm near (400 nm) the bottom of the tungsten film. The non-supported tungsten lamella was 37 nm and 59 nm thick for the top and bottom of the film, respectively. No bending measurement was observed or made for the non-supported tungsten lamella due to it being thick and not exhibiting bending. The trend observed for the carbon-supported lamella was that as the thickness of the carbon support was increased, there was a reduction in the relative lamella bending.
Figure 8 shows the cross-sectional SEM images used to characterize the bending profile of each lamella. The left column of Figure 8 shows the cross-section profiles of each lamella with a cross-section depth of 200 nm. The right column of Figure 8 shows the cross-section figures of each lamella at a cross-section depth of 400 nm. Figure 9 shows higher magnification images of each cross-section profile with the image centered at the midpoint of the lamella window. These images were used to characterize the film/material thicknesses using the first measurement technique discussed in Appendix A.2. The material thicknesses are summarized in Table 3 and Table 4.
Figure 9. Higher magnification cross-section SEM images of each lamella window used to characterize film thicknesses. The top row shows cross-sections at 200 nm depth into W film. The bottom row shows cross-sections at 400 nm depth into W film. Images (a,b) show cross-sections of lamella with no carbon support added. Images (c,d) show cross-sections of lamella with 38–44 nm of carbon support added. Images (e,f) show cross-sections of lamella with 80–82 nm of carbon support added. Images (g,h) show cross-sections of lamella with 112–121 nm of carbon support added. SEM images captured at 3 kV, 100 pA, UHR, TLD secondary electron mode.

3.3. EBID Plate and Grid Support

The lamella bending measurement results from the plate- and grid-supported lamella are summarized in Table 5 and plotted in Figure 10. This set of data was obtained using measurement process #1 listed in Appendix A.2, which measured the positions of the center and edge of the lamella window. The general trend indicates that as the grid thickness is increased, the bending is reduced. The change in grid periodicity did not correspond to increased support. It was observed that the total carbon support thicknesses of 65 nm and 85 nm did not exhibit much difference in measured bending. This could indicate that the grid support was not sufficient to prevent distortion. The configurations with the best results were any lamella with greater than 100 nm of total carbon support thickness, as shown in Figure 10. The SE and STEM images of each configuration are shown in Figure 11 and Figure 12, respectively. All lamella with carbon support equal to or less than 100 nm total carbon support thickness exhibit lamella window edge thinning and window bending. For all lamella with greater than 100 nm total carbon support thickness, the lamella windows appeared to be uniformly thinned, indicating improvement in lamella window quality.
Table 5. Bending displacement measurements from plate and grid reinforced lamella. The error bar for these SEM measurements is 2.5 nm.
Figure 10. Bending displacement measurements for plate and grid reinforced lamella. A 2.5 nm error bar is shown from SEM measurement.
Figure 11. SEM SE images of the plate- and grid-supported lamella after EBID carbon application. (a–c) Lamella with 18 nm target deposition of EBID carbon with varied grid pitch: (a) 100 nm grid pitch, (b) 200 nm grid pitch, (c) 300 nm grid pitch. (d–f) Lamella with 37 nm target deposition of EBID carbon with varied grid pitch: (d) 100 nm grid pitch, (e) 200 nm grid pitch, (f) 300 nm grid pitch. (g–i) Lamella with 56 nm target deposition of EBID carbon with varied grid pitch: (g) 100 nm grid pitch, (h) 200 nm grid pitch, (i) 300 nm grid pitch. (j–l) Lamella with 80 nm target deposition of EBID carbon with varied grid pitch: (j) 100 nm grid pitch, (k) 200 nm grid pitch, (l) 300 nm grid pitch. SEM images captured at 3 kV, 100 pA, UHR, TLD secondary electron mode.
Figure 12. STEM BF images of the plate- and grid-supported lamella after EBID carbon application. (a–c) Lamella with 18 nm target deposition of EBID carbon with varied grid pitch: (a) 100 nm grid pitch, (b) 200 nm grid pitch, (c) 300 nm grid pitch. (d–f) Lamella with 37 nm target deposition of EBID carbon with varied grid pitch: (d) 100 nm grid pitch, (e) 200 nm grid pitch, (f) 300 nm grid pitch. (g–i) Lamella with 56 nm target deposition of EBID carbon with varied grid pitch: (g) 100 nm grid pitch, (h) 200 nm grid pitch, (i) 300 nm grid pitch. (j–l) Lamella with 80 nm target deposition of EBID carbon with varied grid pitch: (j) 100 nm grid pitch, (k) 200 nm grid pitch, (l) 300 nm grid pitch. STEM images captured at 30 kV, 25 pA, UHR, bright field mode.
It was found that curtaining artifacts were observed near the vertically oriented grid support, as shown in Figure 12a–i. FIB Curtaining is a term used in the TEM preparation field that describes the non-uniform milling that results from different milling rates caused by materials of different densities and material characteristics. This curtaining artifact was not observed with the thicker grid-supported lamella as shown in Figure 12j–l. A simple strategy to reduce the curtaining thinning artifacts would be to apply a scan rotation or pattern rotation to the grid pattern during the fabrication process to make the thinning material more uniform in the FIB mill direction (vertical).
Higher magnification images of the thicker carbon-supported lamella are shown in Figure 13. The purpose of these images is to demonstrate the uniformity of the thinning. Figure 13a shows an extreme example of the curtaining artifacts that can occur during the milling process. This curtaining artifact was not observed with increased carbon support material as shown in Figure 13b–d.
Figure 13. Higher magnification STEM BF images of the plate and grid supported lamella after EBID carbon application. Curtaining artifacts are demonstrated. (a) shows the curtaining artifact highlighted in a dotted green box. Notice the tungsten film is preferentially milled in regions with less carbon support. This image is from the TEM lamella using a 300 nm spaced grid with a 90 nm carbon support thickness. (b) shows the TEM lamellae with 100 nm grid spacing and approximately 128 nm of carbon support. (b) shows the TEM lamellae with 200 nm grid spacing and approximately 105 nm of carbon support. (c) shows the TEM lamellae with 300 nm grid spacing and approximately 118 nm of carbon support. In (b–d), there is minimal curtaining observed. STEM images captured at 30 kV, 25 pA, UHR, bright field mode.
The cross-sectional SEM images in Figure 14 show that bending occurred on all lamella, even the most supported. The cross-sectional SEM images of the bending for the 100 nm total carbon-supported lamellae show that the whole window was bent uniformly, not just the central portion of the window as observed with the lesser-supported lamella. This indicates that some form of displacement is occurring. Given that the final thickness of the lamella is under 15 nm in regions, one would expect that the amorphous damage region caused by the 5 kV FIB thinning is comparable to the sample thickness and is the source of the damage. A lower kV final thin would reduce this effect.
Figure 14. Top-down cross-sectional SEM SE images of the plate- and grid-supported lamella after EBID carbon application. Cross-section depth was 300 nm, approximately the midpoint of tungsten film. (a–c) Lamella with 18 nm target deposition of EBID carbon with varied grid pitch: (a) 100 nm grid pitch, (b) 200 nm grid pitch, (c) 300 nm grid pitch. (d–f) Lamella with 37 nm target deposition of EBID carbon with varied grid pitch: (d) 100 nm grid pitch, (e) 200 nm grid pitch, (f) 300 nm grid pitch. (g–i) Lamella with 56 nm target deposition of EBID carbon with varied grid pitch: (g) 100 nm grid pitch, (h) 200 nm grid pitch, (i) 300 nm grid pitch. (j–l) Lamella with 80 nm target deposition of EBID carbon with varied grid pitch: (j) 100 nm grid pitch, (k) 200 nm grid pitch, (l) 300 nm grid pitch. SEM images captured at 3 kV, 100 pA, UHR, TLD secondary electron mode.

4. Discussion

Summarizing the main findings, it was observed that the application of a carbon support structure allows lamella to be physically thinned more than the standard upright thinning process. The data shows that carbon support can reduce bending, but to sufficiently reduce the lamella bending and maintain the straightness of the TEM window profile, one needs to apply a minimum amount of carbon. I found that the application of approximately 100 nm of amorphous carbon material offers a measurable reduction in the total lamella bending.
The accepted approach to TEM preparation in the field of electron microscopy focuses on using a low energy FIB to remove amorphous material and to prevent further damage. The technique presented in this paper differs only slightly, with the application of an amorphous carbon material after a low kV thin, otherwise the techniques are the same. The question to ask is as follows: why add a carbon support material to a sample to produce a thinner sample if the previous technique works? The main limitation for upright lamella preparation is that the FIB tails consume the protective cap, and the beam can “spill over” to the front of the lamella and damage the front of the sample during the final thinning process. This issue can be prevented by using a very low FIB current, 7 pA, to reduce spillover and allow uniform thinning. This still only produces TEM lamella approximately 25–30 nm thick due to cap depletion. In this work, the carbon support material essentially creates a reinforced protective cap and barrier on the front of the lamella that prevents the FIB from remilling the front of the sample. It is essentially equivalent to having an “unlimited protective cap”, meaning that the carbon layer gets milled away prior to the front of the sample being remilled, allowing the back of the sample to be further thinned.
The first limitation of this study is that it did not provide atomic resolution images of the TEM lamella indicating that the quality is sufficient for TEM analysis. I processed the TEM lamella using a standard low kV process of thinning at 5 kV, which is well known in the field of TEM preparation to produce acceptable results for TEM analysis. However, this is usually used when the TEM samples are 30–50 nm thick, whereas the results demonstrate a TEM lamella approximately 15 nm thick. At this reduced thickness, the amount of amorphous material caused by FIB damage is a larger fraction of the total thickness. There is nothing inherent to the workflow that prevents the usage of a lower-energy FIB process. A proposal for the future would include the introduction of a 1 kV wash mill (rectangle pattern mill) to remove the amorphous damage from the 5 kV milling process. TEM analysis of a carbon-supported lamella would likely have a large amount of amorphous scattering in the diffraction pattern, which should not be mistaken as sample damage.
The FIB milling process is known to cause heating and thermal expansion of materials during the TEM fabrication process. In the supplementary materials section, I calculate the expected temperature rise of each material with respect to 5 kV and 30 kV FIB milling. I find a temperature rise of less than 10 K when milling at 30 kV 0.3 nA in all materials. This minimal amount of heating is attributed to the small FIB current used. I then use this calculated temperature rise to estimate the expected thermal expansion of each material within the TEM lamella. The calculation of the maximum thermal expansion for all materials was found to be less than 1 nanometer. I then compare this to an FEA thermal expansion calculation using a 10 K temperature rise. I find that the thermal expansion observed for 30 kV milling is less than a nanometer. This suggests that the bending that I observed in the milling process is not the result of thermal expansion of the lamella.
Another consideration when prepping TEM samples is the total electron dose acquired by a material during processing. In Appendix A.3, I calculate the dose that the surface receives. I calculate that the total electron dose (436 electrons/Å2) is very minimal and comparable to doses used for evaluating delicate samples (5 electrons/Å2).
An inconsistent deposition of carbon was observed. In Figure 10, Figure 11 and Figure 12, I list the target depositions and in Table 5, I list the actual measured depositions. I observe that the target depositions vary with each grid + plate TEM lamella. One suspected cause of this inconsistency is that during the cross-sectioning process, I did not perfectly target a horizontal grid line, resulting in measured carbon thickness variation. The SEM deposition process also does not produce perfect edges during the deposition process; it produces a gaussian profile. The deposition process on TEM grids also significantly affects the gas flow and generally reduces the deposited amount of material. The carbon deposition across each lamellae was fairly uniform. Overall, even with the inconsistencies observed with the measured carbon deposition, the trend observed in Figure 10 demonstrates the structural support capability of the carbon film.
In regard to a carbon support layer interfering with STEM/TEM characterization, it is industry standard in the ex situ TEM preparation process to place a lamella on a carbon-supported grid. Typical carbon thicknesses of carbon grids are 15–25 nm. In this work, I only start to see a granular effect in the STEM image from excessive EBID coatings, i.e., over 100 nm thickness.
The measurement process used two separate methods to evaluate the TEM lamella bending. While the first method was able to identify maximum bending displacement, I found that it did not sufficiently capture the bending that was occurring across the full lamella profile. To elaborate, by sampling at the center and the edge of the lamella window as used in the first measurement process, I was able to identify which lamella had the largest bending; however, when interpreting these results, I observed that this measurement technique failed to capture the bending offset that occurred near the edge of the lamella window. The second measurement process uses a first derivative gradient analysis to extract the full lamella edge profile and is shown in Figure A2 and Figure A3 in Appendix A.2. All the lamella were observed to be bending, but not with the same profile across the lamella window. The lamella with less than 100 nm of carbon support was found to be bending in an arc-like profile, with continuity from the unmilled edge of the lamella window to the center. The lamella with more than 100 nm of carbon support material was found to be bending with an abrupt offset near the edges of the TEM lamella and remained mostly flat across the full width of the TEM lamella. This indicates that the lamella is being supported across the width of the thinned window and that the bending is then “shifted” to the next weakest point on the TEM lamella, which I suspect is now the edges of the TEM lamella. There are two readily available options for future development with this workflow: one could decrease the forces on the lamella by milling with a lower FIB energy, which is currently the standard TEM processing approach. Additionally, one could add more support material to the surrounding edge regions to strengthen them.
I performed the FIBSEM evaluation due to it being the most direct way to characterize the bending of the TEM sample. What I found in the literature regarding TEM sample bending measurements involved quite complex evaluation methods. There are various methods for evaluating crystalline strain and lamella bending by using electron backscatter diffraction (EBSD) [30], transmission Kikuchi diffraction (TKD) [31], bend contours observed in TEM analysis that appear as dark bands of periodic contrast moving across a TEM window [32], the use of convergent beam electron diffraction (CBED) [33], edge-on sample measurement in the SEM, and the destructive FIBSEM process. Comparing these methods, the relative cost of edge-on sample measurement using the SEM and FIBSEM cross-section processes are significantly cheaper than EBSD, TEM, and CBED techniques, which all require expensive tools and equipment. In regard to utilizing EBSD, TEM bend contours, and CBED to characterize TEM lamella bending, this requires a crystalline sample which, in most cases on semiconductor samples, is a silicon substrate but is not always the case.
An interesting alternative to applying a support material is the utilization of a GAS assisted milling process that enables a selective etch procedure. Following the work of [34], it was found that by using a XeF gas assisted mill process, it was possible to uniformly thin a planar Cu film sample to produce a TEM sample that was used to observe crystalline structure and stacking faults. No lamella thickness or bending characterization was performed, limiting the interpretation of how much the technique can assist in producing thinner TEM windows. A limitation of this process is that XeF gas is limited to etching Si, SiOx, and SiNx materials, and subsequent workflows must be designed around how to utilize the selective removal of a Si based material to enable more advanced workflows.
Residual stress in thin films can play a role in how much force can be applied prior to sample deformation. The FIB deposited tungsten layer has little intrinsic stress. Future work could investigate the role that intrinsic stress plays in a carbon-supported lamella.
For future work, I propose the usage of an atomic layer deposition (ALD) system to apply a coating of a low atomic Z material (such as a carbon or boron film). This would minimize electron exposure to the imaging face and allow a systematic deposition approach with atomic thickness precision of the ALD process. The current process of using an electron beam to deposit material is not as reliable as the ALD coating process for controlling the total amount of material deposited. Another limitation of the current technique is that it cannot be applied to samples with carbon layers due to interference with sample characteristics such as material voids. In the semiconductor industry, a typical example of a carbon layer is a structure known as a carbon hard mask (CHM). In samples with a CHM, voids in such materials would be filled in by the EBID carbon coating process, preventing void characterization. One possible solution to CHM TEM samples would be to apply a thin atomic layer deposition of a dense material prior to support layer deposition. This would create a well-defined boundary conformal to the surface of the TEM lamella and around material voids in the sample, allowing TEM characterization. This dense conformal coating would delineate the sample CMH and the applied low-z support material in the TEM imaging process.
The implications of the work show a new technique that allows difficult-to-thin samples to be processed with extra support. It is not clear if this extra support is the result of a physical boundary between the front and back of the TEM lamella or if it is extra mechanical support that prevents warping. I suspect it is a bit of both. Further work would need to evaluate whether there are differences between reinforcing only the cap region compared with reinforcing the full lamella.

5. Conclusions

The exact cause of the TEM lamella bending was not sought or obtained in this work. This work was used to demonstrate a new approach to applying material support to TEM samples that enables further thinning. I used FEA to identify regions of stress and qualitatively compared these results to evaluate if the proposed material support would offer reduced stress. The SEM images of the lamella bending profiles indicate that the application of the support material reduces the lamella distortions.
In summary, I demonstrated a TEM sample preparation and thinning process that incorporates an electron transparent material that acts as a support structure, allowing the TEM sample to be further thinned prior to sample warping. I demonstrated a unique TEM sample preparation procedure that enables the ability to produce lamella with large regions of sub-20 nm thickness using an EBID carbon coating procedure. I demonstrated the feasibility of applying a carbon layer and its ability to reduce sample deformation as evidenced by cross-sectional analysis and STEM imaging. I used FEA to identify the stressed regions of a lamella and demonstrated the application of a support layer can reduce this stress. It was found that a total layer thickness between 100 and 130 nm is able to offer significant support and reduces the lamella bending. While this approach was not able to fully reduce the bending observed in the thinning process, it did reduce the magnitude of the bending and flatten the bending profile.
Long term, as semiconductor devices continue to shrink, the ability to characterize these materials will need to change and become more systematic and purposeful. The artesian nature of electron microscopy will need to be supplemented by carefully engineered processes to enable accurate characterization of devices. The work demonstrated in this paper is the initial steps towards the future of TEM lamella design. Simulation on structural stability will enable the development of new approaches to make the metrology of tomorrow possible today.

Supplementary Materials

The following supporting information can be downloaded at: https://www.mdpi.com/article/10.3390/applnano7040041/s1, Figure S1: 3D Models with side and angled views used for FEA simulation; Figure S2: FEA results for thin film plate configuration showing Von Mises Stress, Y-displacement and Z-displacement for lamella with varying thickness carbon layers; Figure S3: FEA results for 140 nm carbon plate and 100 nm grid spacing with varying grid thickness showing Von Mises Stress, Y-displacement and Z-displacement for lamella; Figure S4: FEA results for 140 nm carbon plate and 200 nm grid spacing with varying grid thickness showing Von Mises Stress, Y-displacement and Z-displacement for lamella; Figure S5: FEA results for 140 nm carbon plate and 300 nm grid spacing with varying grid thickness showing Von Mises Stress, Y-displacement and Z-displacement for lamella; Figure S6: FEA results for thermal evaluation by applying 10 k temperature rise on non-supported lamella showing Von Mises Stress, X-displacement for non-supported lamella; Table S1: Summary of Lamella Geometry FEA Results; Table S2: Temperature Rise Calculation; Table S3: Thermal Expansion Calculation. The supplementary file contains FEA simulations for plate and grid geometries. Temperature rise calculation and FEA simulations are performed to estimate thermal expansions of materials being FIB mill [35,36,37,38,39,40,41,42,43,44,45,46].

Funding

This research was funded by Lam Research.

Institutional Review Board Statement

Not applicable

Data Availability Statement

The data presented in this study are openly available in [Quantum-Monte/FEA-Simulation-Data-for-Engineered-TEM-lamella: Reference FEA simalation data, Zenodo ] at [https://doi.org/10.5281/zenodo.24316546], reference number [FEA Simalation Data. V. V1.1].

Acknowledgments

During the preparation of this manuscript, the author(s) used Fusion 360 for the purposes of performing finite element analysis. I would like to acknowledge Lam Research for their contribution of knowledge and microscope resources to perform this study. I would like to acknowledge Matt Hughes for his great insights into electron microscopy. I would like to acknowledge Erik Sanchéz for his knowledge and insights into FEA and experimental analysis.

Conflicts of Interest

The author declares no conflicts of interest.

Abbreviations

The following abbreviations are used in this manuscript:
TEMTransmission Electron Microscopy
FEAFinite Element Analysis
SEMScanning Electron Microscope
FIBFocused Ion Beam
EDXEnergy Dispersive X-ray Spectroscopy
EBSDElectron Backscatter Diffraction
STEMScanning Transmission Electron Microscopy
EBIDElectron Beam Induced Deposition
AOIArea of Interest
GISGas Injection System
ICEInternal Chamber Electronics
WDWorking Distance
UHRUltra-High Resolution
TLDThrough Lens Detector
SESecondary Electron
kVKilo Volt
ALDAtomic Layer Deposition
TKDTransmission Kikuchi Diffraction
CBEDConvergent Beam Electron Diffraction
CHMCarbon Hard Mask

Appendix A

Appendix A.1

The material properties used in FEA simulation are listed in Table A1.
Table A1. Material properties used for FEA simulations.

Appendix A.2

Two measurement approaches were performed. The first approach compared the center and edge of a lamella window to obtain the displacement between both points. A box average was used to improve reliability of each measurement. The measurement procedure is shown below. The second measurement approach used an automated script to extract the bending profile across the full lamellae window width. These plots were used for relative comparison of the bending profiles.
Measurement Process #1:
Figure A1. The diagram demonstrates the measurement process using a box average. (a) shows the measurement region bounded by a yellow box for the cross-section image of the structure. (b) shows the measurement region bounded by a yellow box for the front-side thickness SEM image of the structure. The arrow indicates measurement direction. Box-averaged cross-sections profiles with example measurements are shown in the right panel. The black profile is extracted from the center of the lamella window, and the red profile is extracted from the edge profile. The green lines represent the measured distance.
Measurement Procedure:
Measurements were taken using a box averaged over 100 nm in cross-section images.
  • Open Imagej (version 1.54d) software. Import image.
  • Set Scale.
  • The “Distance in Pixels” parameter uses the image dimension of 1024 pixels.
  • Set “Known distance” using the SEM image HFW.
  • Set units nm.
  • Draw a measurement rectangle on the SEM image.
  • Draw a rectangle box over the edge of the lamella window as shown in Figure A1 as reference feature. The box width and height were 90 nm × 150 nm, respectively.
  • Select Plot Profile. This will plot the average box profile.
  • Move the measurement rectangle box vertically over the SEM image without moving horizontally (this ensures the plot comparison is accurate). Place the measurement box over the center of the lamella window; this corresponds with the maximum bending of the lamella window.
  • Select Plot Profile. This will plot the average box profile.
  • You will now have two plotted profiles with a common reference line.
  • Select Data on the second plot, then select add from plot, then select data set 1, set the color to red. Click ok. This creates a new plot by combining the reference plot and the center of the lamella plot.
  • Draw a box on the plot profile. For the left and right side of the box, follow the procedure to define the edge.
  • Find the maximum and minimum at an edge as shown in Figure 12 (right panel) and define the measurement edge at the 50% mid-point vertically between them.
  • Select Measurement. This will measure the distance between edges and give a measurement of the lamella bending.
Measurement Process #2:
Figure A2. The diagram demonstrates the measurement process using a script to extract the full edge profile. (a) shows the measurement region bounded by a yellow box for extracting the edge profile. (b) shows the measurement profile after it has been converted into distance and centered on the zero axis. The non-deflected region is highlighted in red in both the cross-section SEM image and the cross-section profile. This region was used to define the vertical offset for each profile.
The code used for performing edge measurements using Imagej (version 1.54d) is available in the supplementary materials file. Note: This code was generated using Google Gemini 1.5 Pro.
This code works by taking a region bounded by a user selection box, extracting the horizontal lines, moving line by line vertically down, calculating the derivative of the horizontal line, and finding the maximum gradient as defining the edge. The horizontal position is logged in the results table, which can be saved in .csv format using Imagej software.
To use this code using Imagej, I used the following workflow:
  • File open image, select image for analysis.
  • Set scale for the image.
    a.
    Select analyze ≥ Set Scale.
    b.
    Set Distance in Pixels to 1024 pixels.
    c.
    Set Known Distance to image horizontal field width.
    d.
    Set Unit of Length to nm.
    e.
    Check Global if all images are the same magnification.
  • Create measurement macro.
    a.
    Select Plugins, select new, select macro.
    b.
    Paste the code into the new macro pop-up window.
  • Draw rectangle measurement across the edge of the lamella completely covering the cross-section on the lamella.
    a.
    Be sure to place the left measurement side of the rectangle in the carbon support region and the right side of the measurement rectangle just past the tungsten region. The measurement is based on an intensity defined edge; be sure to only have one edge present in the image.
  • Run the macro.
    a.
    The measurement rectangle will disappear and a results table will appear. Save the results table.
The output of the edge measurement is in pixels, and I convert this into nm by multiplying each pixel by the nm/pixel ratio. To calculate the pixel to nm conversion, I take the HFW of the image and divide by the number of pixels across the image. If an image is 1950 nm HFW and has an image resolution of 1024 pixels, the ratio is 1950/1024 nm/px, giving 1.9024 nm/px.
To perform comparisons between multiple edge plots, I needed to set the vertical zero point for each image. This was performed by calculating the average of the first 50 nanometers in the non-deflected, non-thinned window region shown in Figure A2a as a red box. The non-deflected region is the area where both the front and back of the lamella were not milled at the same time; therefore, it is thicker and undeflected. This generated a y-offset that I was able to apply to each edge measurement to center the edge at zero.
The full results from the second measurement process are shown in Figure A3. The relative trends observed in the profile comparisons match the results found with the first measurement procedure, with more supported lamella demonstrating reduced bending. Figure A3a shows the edge profiles from the thin film-supported lamella. Figure A3b–d shows the edge profiles for each plate and grid supported lamella. Two easy observations to make from analyzing the profiles is that the 100 nm + carbon-supported lamella show a flatter profile and each of these profiles are shifted near the edge. Figure A3e is a comparison plot between the most supported TEM lamella, where it can be observed that all plots have similar form and approximately the same deflection in bending. While the plot from the 200 nm grid spacing and 105 nm carbon support thickness shows a slight improvement, it is not enough to state definitively that it is the best result.
Figure A3. The figure shows the plot measurements for the extracted profiles of all TEM lamella presented in this paper. (a) shows the edge profiles from the thin film-supported lamella. (b) shows the edge profiles for 100 nm spaced grid-supported lamella. (c) shows the edge profiles for 200 nm spaced grid-supported lamella. (d) shows the edge profiles for 300 nm spaced grid-supported lamella. (e) shows a comparison plot for each of the most supported TEM lamella for each grid support.

Appendix A.3

The error estimates for the SEM measurements are estimated to be limited by the electron spot size, which from the tool manufacturer is approximately 1–3 nm. This value is dependent on the interaction volume and is therefore material dependent. I used a 3 nm value for the error estimates to remain conservative. The measurement calibration accuracy is generally specified at 1%. The error in the measurement from tilt error is estimated to be ±0.1 degrees. The tilt axis is a closed loop and little error is observed.
Measurement error from stage drift: The specification for stage drift is approximately 5 nm per minute. The total image acquisition time is 10 s when scanning at 1024 × 884 pixels with a line integrate of 2 and dwell time of 3 μs. This can result in a compression or expansion of the image. The error estimated from stage drift is 5 × (1 nm/60 s) × 10 s = 0.83 nm. This gives an error of ±0.83 nm.
Our largest source of error is measurement error in the SEM measurements and stage drift. I estimate the SEM contribution to be half of the uncertainty in the SEM spot size. This gives an error in SEM measurements of ±1.5 nm. I add the stage drift to the SEM image uncertainty and get a total estimated error of ±2.3 nm. This is used as the error in the measurement bars.

Appendix A.4. Estimating Electron Dose

Electron beam damage is a serious concern when performing any analysis on a semiconductor device. I estimate the electron dose that is accumulated during the deposition process and compare it to the literature. Electron dose is defined as the number of electrons that have reached a sample’s surface for a given dwell time [53,54].
d = I S t
With d being electron dose, I being incident beam current, S being irradiated surface area, and t being the dwell time. I performed the SEM deposition using a 1.6 nA beam, with a 1024 × 884 pixels in the SEM image with a horizontal field of view of 5000 nm, (5000/1024) giving a pixel size and irradiated surface length per pixel of 4.9 nm or 49 Å. The standard dwell time for patterning is 1 µs.
I calculate the total charge accumulated in the sample for a given time,
I × t = 1.6 nA × 1.0 µs = 1.6 × 10−15 C
Converting charge to the number of electrons,
1.6 × 10−15 C × e−/1.602 × 10−19 C = 9987 electrons
Using Equation (A1), I find an electron dose for electrons per unit area
d = 9987 electrons/(π × (49 Å)2) = 1.3 electrons/Å2
This is per pass. A rectangle pattern configured to deposit carbon using a 1 kV 1.6 nA SEM with a 100 nm deposition depth performs approximately 335 passes. In the literature, I find a low electron dose used in STEM to range from 5 electron/Å2 damaging some biological specimens, 100 electrons/Å2 being the dose used in cryo-EM for characterizing catalysts [55], and 100–5000 electrons/Å2 being a standard dose in HRTEM imaging [56]. The dose is on the lower end of exposure for most materials.

References

  1. Mayer, J.; Giannuzzi, L.A.; Kamino, T.; Michael, J. TEM Sample Preparation and FIB-induced Damage. MRS Bull. 2007, 32, 400–407. [Google Scholar] [CrossRef] [Scilit]
  2. Kim, J.T.; Kim, H.J.; Jo, Y.S.; Choe, S.H. Cross-sectional TEM Specimens Preparation of Precisely Selected Regions of Semiconductor Devices using Focused Ion Beam Milling. Korean J. Mater. Res. 1993, 3, 193–196. [Google Scholar]
  3. Giannuzzi, L.A.; Stevie, F.A. A review of focused ion beam milling techniques for TEM specimen preparation. Micron 1999, 30, 197–204. [Google Scholar] [CrossRef] [Scilit]
  4. Lekstrom, M.; McLachlan, M.A.; Husain, S.; McComb, D.W.; Shollock, B.A. Using the in situ lift-out technique to prepare TEM specimens on a single-beam FIB instrument. J. Phys. Conf. Ser. 2008, 126, 012028. [Google Scholar] [CrossRef] [Scilit]
  5. Bonifacio, C.S.; Ray, M.L.; Fischione, P.E.; Yu, Y.; Skowronski, M. Precise Final Thinning by Concentrated Ar Ion Beam Milling of Plan View TEM Specimens from Phase Change Memory Device Prepared in Xe Plasma FIB. In Proceedings of the ISTFA 2023: Conference Proceedings from the 49th International Symposium for Testing and Failure Analysis, Phoenix, AZ, USA, 12–16 November 2023; pp. 309–316. [Google Scholar] [CrossRef] [Scilit]
  6. Kim, H.J.; Choi, S.; Bae, H.-B.; Lee, T. Transmission Electron Microscopy (TEM) Sample Preparation of Si1–xGex in c-Plane Sapphire Substrate, NASA Technical Memorandum. 2012. Available online: https://ui.adsabs.harvard.edu/abs/2012ntrs.rept13304K/abstract (accessed on 29 December 2025).
  7. Yale West Campus Materials Characterization Core. TEM Sample Manual Preparation Procedure. Standard Operating Procedure. PDF. Available online: https://ywcmatsci.yale.edu/sites/default/files/files/FIB%20manual%20TEM%20sample%20preparation%20SOP.pdf (accessed on 29 December 2025).
  8. Giannuzzi, L.A.; Stevie, F.A. Introduction to Focused Ion Beams, 1st ed.; Springer: New York, NY, USA, 2005; pp. 73–142. [Google Scholar]
  9. Kozell, M. A Systematic Approach for Controlling TEM Sample Thicknesses. Nanomanufacturing 2026, 6, 23. [Google Scholar] [CrossRef] [Scilit]
  10. Liew, K.-N. Specimen Preparation Method. U.S. Patent No. US20150137003A1, 21 May 2015. [Google Scholar]
  11. Kang, H.-J.; Kim, J.H.; Oh, J.W.; Back, T.S.; Kim, H.J. Ultra-Thin TEM Sample Preparation with Advanced Backside FIB Milling Method. Microsc. Microanal. 2010, 16, 170. [Google Scholar] [CrossRef] [Scilit]
  12. Sari, B.; Dandu, M.; Wood, N.; Hochhalter, J.; Johnson, A.; Doeff, M.; Liu, F.; Raja, A.; Scott, M.; Dhall, R.; et al. Facile Tensile Testing Platform for In Situ Transmission Electron Microscopy of Nanomaterials. Adv. Mater. Interfaces 2025, 12, 2400750. [Google Scholar] [CrossRef] [Scilit]
  13. Cherkashin, N.; Denneulin, T.; Hÿtch, M.J. Electron microscopy by specimen design: Application to strain measurements. Sci. Rep. 2017, 7, 12394. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  14. Després, A.; Veron, M. Elastic strain field measurements in the TEM for metallurgical applications. Mater. Charact. 2023, 202, 113012. [Google Scholar] [CrossRef] [Scilit]
  15. Hÿtch, M.J.; Minor, A.M. Observing and measuring strain in nanostructures and devices with transmission electron microscopy. MRS Bull. 2014, 39, 138–146. [Google Scholar] [CrossRef] [Scilit]
  16. Gong, T.; Chen, L.; Wang, X.; Qiu, Y.; Liu, H.; Yang, Z.; Walther, T. Recent Developments in Transmission Electron Microscopy for Crystallographic Characterization of Strained Semiconductor Heterostructures. Crystals 2025, 15, 192. [Google Scholar] [CrossRef] [Scilit]
  17. Kang, S.; Wang, D.; Kübel, C.; Mu, X. Importance of TEM sample thickness for measuring strain fields. Ultramicroscopy 2024, 255, 113844. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  18. Cooper, D.; Denneulin, T.; Bernier, N.; Béché, A.; Rouvière, J.L. Strain mapping of semiconductor specimens with nm-scale resolution in a transmission electron microscope. Micron 2016, 80, 145–165. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  19. Cook, S.R. Warp-Free TEM Sample Preparation Methods Using FIB/SEM Systems. Microsc. Microanal. 2022, 28, 1961–1970. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  20. Ricci, E.; Cazzaniga, F.; Testai, S. TEM sample preparation of a SEM cross section using electron beam induced deposition of carbon. Microelectron. Reliab. 2015, 55, 2126–2130. [Google Scholar] [CrossRef] [Scilit]
  21. Kidwell, D.A. Transmission Electron Microscopy Supports and Methods of Making. U.S. Patent No. US9646803B2, 9 May 2017. [Google Scholar]
  22. Demuth, T.; Fuchs, T.; Beyer, A.; Janek, J.; Volz, K. Depo-all-around: A novel FIB-based TEM specimen preparation technique for solid state battery composites and other loosely bound samples. Ultramicroscopy 2024, 257, 113904. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  23. Gorelick, S.; Velamoor, S.; Cleeve, P.; Trépout, S.; Ying, L.; Naranbhai, V.; Ramm, G. Mind the corner: Fillets in cryo-FIB lamella preparation to minimise sample loss caused by stress concentration and lamella breakage. J. Struct. Biol. 2025, 217, 108249. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  24. Wachsmuth-Melm, M.; Mense, C.; Gomez Melo, S.; Zimmermann, L.; Schwarz, U.S.; Chlanda, P. On-lamella dual-axis cryo-electron tomography and modelling of lamella stability. BMC Methods 2026, 3, 5. [Google Scholar] [CrossRef] [Scilit]
  25. Wolff, G.; Limpens, R.W.A.L.; Zheng, S.; Snijder, E.J.; Agard, D.A.; Koster, A.J.; Bárcena, M. Mind the gap: Micro-expansion joints drastically decrease the bending of FIB-milled cryo-lamellae. J. Struct. Biol. 2019, 208, 107389. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  26. Wang, S.; Zhou, H.; Chen, W.; Jiang, Y.; Yan, X.; You, H.; Li, X. CryoFIB milling large tissue samples for cryo-electron tomography. Sci. Rep. 2023, 13, 5879. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  27. Balaur, E.; Peele, A.G. Tunnelling through diamond-like carbon nanofilms deposited by electron-beam-induced deposition. Thin Solid Films 2009, 517, 6520–6526. [Google Scholar] [CrossRef] [Scilit]
  28. SimScale: Cloud-Based Engineering Platform for Structural Mechanics Simulation. Available online: https://www.simscale.com/product/structural-mechanics/ (accessed on 31 December 2025).
  29. Von Mises: SimScale: What is Von Mises Stress? Available online: https://www.simscale.com/docs/simwiki/fea-finite-element-analysis/what-is-von-mises-stress (accessed on 31 December 2025).
  30. Wright, S.I.; Kacher, J.; Ruggles, T. Electron Backscatter Diffraction-Based Strain Analysis in the Scanning Electron Microscope. In Advances in Texture, Microtexture, and Allied Techniques; Suwas, S., Field, D.P., Eds.; Materials Horizons: From Nature to Nanomaterials; Springer: Singapore, 2025. [Google Scholar] [CrossRef] [Scilit]
  31. Kuběna, I.; Fintová, S.; Jambor, M.; Šmíd, M. TKD/EBSD and TEM analysis of microstructural changes ongoing in AISI 304L steel exposed to the cyclic loading. Mater. Sci. Eng. A 2023, 872, 144943. [Google Scholar] [CrossRef] [Scilit]
  32. Vas, J.V.; Ali, H.; Shi, W.; Denneulin, T.; Gupta, A.K.; Medwal, R.; Dunin-Borkowski, R.E. Quantitative magnetic mapping in TEM through accurate 2D thickness determination. Ultramicroscopy 2025, 275, 114140. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  33. Clément, L.; Pantel, R.; Kwakman, L.F.; Rouvière, J.L. Strain measurements by convergent-beam electron diffraction: The importance of stress relaxation in lamella preparations. Appl. Phys. Lett. 2004, 85, 651–653. [Google Scholar] [CrossRef] [Scilit]
  34. Kim, J.-S.; Nam, S.-Y.; Choi, Y.-H.; Park, J.-C. Preparation Method of Plan-View Transmission Electron Microscopy Specimen of the Cu Thin-Film Layer on Silicon Substrate Using the Focused Ion Beam with Gas-Assisted Etch. Appl. Microsc. 2015, 45, 195–198. [Google Scholar] [CrossRef] [Scilit]
  35. Orloff, J.; Swanson, L.; Utlaut, M. High Resolution Focused Ion Beams: FIB and its Applications; Springer: New York, NY, USA, 2004; Available online: https://www.academia.edu/65234377/High_resolution_focused_ion_beams_FIB_and_its_applications (accessed on 10 July 2026).
  36. Wolff, A.; Klingner, N.; Thompson, W.; Zhou, Y.; Lin, J.; Peng, Y.Y.; Ramshaw, J.A.M.; Xiao, Y. Modelling of Focused Ion Beam Induced Increases in Sample Temperature: A Case Study of Heat Damage in Biological Samples. J. Microsc. 2018, 272, 47–59. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  37. Yamasue, E.; Susa, M.; Fukuyama, H.; Nagata, K. Thermal conductivities of silicon and germanium in solid and liquid states measured by non-stationary hot wire method with silica coated probe. J. Cryst. Growth 2002, 234, 121–131. [Google Scholar] [CrossRef] [Scilit]
  38. Tungsten. QED Archives. Quantum Engineering and Design. Available online: https://qedfusion.org/LIB/PROPS/PANOS/w.html (accessed on 10 July 2026).
  39. Alaie, S.; Goettler, D.F.; Jiang, Y.B.; Abbas, K.; Baboly, M.G.; Anjum, D.H.; Chaieb, S.; Leseman, Z.C. Thermal Conductivity and Nanocrystalline Structure of Platinum Deposited by Focused Ion Beam. Nanotechnology 2015, 26, 085704. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  40. Bullen, A.J.; O’Hara, K.E.; Cahill, D.G.; Monteiro, O.; von Keudell, A. Thermal Conductivity of Amorphous Carbon Thin Films. J. Appl. Phys. 2000, 88, 6317–6320. [Google Scholar] [CrossRef] [Scilit]
  41. Ling, S.J.; Moebs, W.; Sanny, J. 1.3 Thermal Expansion. In University Physics Volume 2; OpenStax: Houston, TX, USA, 2016; Available online: https://openstax.org/books/university-physics-volume-2/pages/1-3-thermal-expansion (accessed on 10 July 2026).
  42. Watanabe, H.; Yamada, N.; Okaji, M. Linear Thermal Expansion Coefficient of Silicon from 293 to 1000 K. Int. J. Thermophys. 2004, 25, 221–236. [Google Scholar] [CrossRef] [Scilit]
  43. AZoM. “Tungsten.”. Available online: https://www.azom.com/properties.aspx?ArticleID=614 (accessed on 10 July 2026).
  44. Hidnert, P.; Sweeney, W.T. Thermal Expansion of Tungsten; Scientific Papers of the Bureau of Standards; Government Printing Office: Washington, DC, USA, 1925; Volume 20. Available online: https://nvlpubs.nist.gov/nistpubs/ScientificPapers/nbsscientificpaper515vol20p483_A2b.pdf (accessed on 10 July 2026).
  45. Edsinger, R.E.; Reilly, M.L.; Schooley, J.F. Thermal Expansion of Platinum And Platinum-Rhodium Alloys. J. Res. Nat. Bur. Stand. 1986, 91, 333–356. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  46. Champi, A.; Lacerda, R.G.; Viana, G.A.; Marques, F.C. Thermal expansion dependence on the sp2 concentration of amorphous carbon and carbon nitride. J. Non-Cryst. Solids 2004, 338–340, 499–502. [Google Scholar] [CrossRef] [Scilit]
  47. Pan, M.; Crozier, P.A. Quantitative imaging and diffraction of zeolites using a slow-scan CCD camera. Ultramicroscopy 1993, 52, 487–498. [Google Scholar] [CrossRef] [Scilit]
  48. Liu, Z. Temperature-dependent elastic constants and Young’s modulus of silicon single crystal. In Proceedings of the International Conference on Mechanical Engineering Design of Synchrotron Radiation Equipment and Instrumentation, Online, 24–29 July 2021; Available online: https://accelconf.web.cern.ch/medsi2020/papers/wepc09.pdf (accessed on 10 July 2026).
  49. AZoM. A Background to Silicon and its Applications. Available online: https://www.azom.com/properties.aspx?ArticleID=599 (accessed on 10 July 2026).
  50. Tungsten. 6.777J/2.751J Material Property Database; Massachusetts Institute of Technology: Cambridge, MA, USA; Available online: https://www.mit.edu/~6.777/matprops/tungsten.htm (accessed on 10 July 2026).
  51. AZoM. Platinum—Properties and Applications. Available online: https://www.azom.com/properties.aspx?ArticleID=601 (accessed on 10 July 2026).
  52. Ohtake, N.; Hiratsuka, M.; Kanda, K.; Akasaka, H.; Tsujioka, M.; Hirakuri, K.; Hirata, A.; Ohana, T.; Inaba, H.; Kano, M.; et al. Properties and Classification of Diamond-Like Carbon Films. Materials 2021, 14, 315. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  53. Utke, I.; Michler, J.; Winkler, R.; Plank, H. Mechanical Properties of 3D Nanostructures Obtained by Focused Electron/Ion Beam-Induced Deposition: A Review. Micromachines 2020, 11, 397. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  54. Arnoult, C.; Di Martino, J.; Ruch, D. Prediction and limitation of polymer degradation in Environmental SEM. Ultramicroscopy 2012, 122, 32–36. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  55. Grosso, D.R.; Commisso, M.; Cimino, R.; Larciprete, R.; Flammini, R.; Wanzenberg, R. Effect of the surface processing on the secondary electron yield of Al alloy samples. Phys. Rev. Spec. Top. Accel. Beams 2013, 16, 051003. [Google Scholar] [CrossRef] [Scilit]
  56. Buban, J.P.; Ramasse, Q.; Gipson, B.; Browning, N.D.; Stahlberg, H. High-resolution low-dose scanning transmission electron microscopy. J. Electron Microsc. 2010, 59, 103–112. [Google Scholar] [CrossRef] [Scilit] [PubMed]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations