CO2 Capture by Hydrotalcite-Derived Sorbents in Pressure Swing Adsorption for Sorption-Enhancing

,
,
and
Department of Industrial and Information Engineering and Economics (DIIIE), University of L’Aquila, Piazzale E. Pontieri 1-loc, Monteluco di Roio, 67100 L’Aquila, Italy
*
Author to whom correspondence should be addressed.

Highlights

What are the main findings?
  • CO2 sorbents are effective under relevant industrial conditions, and they are suitable for the sorption-enhanced water gas shift.
  • The addition of a catalytic phase for water gas shift does not affect sorption capacity in the combined sorbent/catalyst material.
What is the implication of the main finding?
  • Scaling of sorption-enhanced water gas shift by a combined sorbent/catalyst hydrotalcite material is possible.
  • New materials can be developed for process intensification and clean energy integration, producing pure hydrogen.

Abstract

This work investigated hydrotalcite-derived sorbents for CO2 capture at 350 °C, 10 or 14 bar, and 38.5 vol% CO2 in wet or dry gas flow under dynamic Pressure Swing Adsorption (PSA) in a packed-bed laboratory reactor. The chosen conditions enabled a preliminary assessment of the suitability of hydrotalcite-derived sorbents for Sorption-Enhanced-Water-Gas-Shift (SEWGS), a promising process for producing pure hydrogen from syngas. Two starting sorbents were considered: derived from commercial hydrotalcite, and from hydrotalcite synthesized by low-supersaturation. Both sorbents were doped with 20 wt% K2CO3. In addition, a hydrotalcite bifunctional catalyst-sorbent for SEWGS was studied. K2CO3-doping and higher pressure significantly improved the CO2-sorption capacity; the highest value (1.51 mmolCO2∙g−1) was measured under wet conditions at 14 bar. The bifunctional material showed good, stable CO2 sorption capacity (1.39 mmolCO2∙gsolid−1 on average out of five PSA cycles under wet conditions at 14 bar). Materials derived from commercial hydrotalcite doped with K2CO3 showed promising performances for future industrial SEWGS applications.

1. Introduction

Water Gas Shift (WGS, R.1) industrially occurs at 310–450 °C by Fe-Mg-Cr catalyst (High-Temperature-Swing) and 200–250 °C by Cu/ZnO-Al2O3 catalyst (Low-Temperature-Swing). WGS usually follows reforming processes to obtain high-purity H2 (e.g., for Haber-Bosch NH3 synthesis) [1].
The Sorption-Enhanced Water Gas Shift (SEWGS) process has increasingly gained attention as a new solution to get H2 from syngas; when syngas derives from wastes or biomasses, the hydrogen from SEWGS can be labelled as low-carbon up to carbon-neutral [2,3]. SEWGS operates by integrating the WGS (R.1) with in situ CO2-capture performed by solid sorbents ( ∑ ( s ) , R.2); the removal of CO2 shifts the WGS equilibrium towards H2 production, improving CO and H2O conversion and simultaneously purifying the gas product [4].
C O + H 2 O ⇆ H 2 + C O 2
C O 2 + ∑ ( s ) → ∑ C O 2 ( s )
In general, sorption-enhancing would require that the sorbent have [5,6,7]: (i) fast capture kinetics at those temperatures and pressures suitable for enhanced reactions; (ii) cyclic stability in continuous productions to alternate process conditions of sorption-enhancing and those of sorbent regeneration (i.e., CO2 release to restore sorption capacity). Furthermore, the integration of catalytic functionalities within sorbent particles could promote process intensification of H2 production and CO2 capture [8].
Adsorbents for CO2 capture are usually classified according to their working temperature (low, medium, or high) [9]: activated carbon, zeolites, and metal–organic frameworks (MOFs) are commonly employed for applications at low temperatures (below 200 °C) [9]; hydrotalcites usually work at medium range (200–400 °C); oxides are usually applied at high temperatures (higher than 400 °C) [10].
As to SEWGS, hydrotalcites can capture CO2 at conditions suitable for WGS, such as 300–500 °C at 10–40 bar [5]. Moreover, hydrotalcites can be regenerated by Pressure Swing Adsorption (PSA), a cyclic operation that allows continuous processes by batteries of parallel packed beds [5].
Hydrotalcites belong to the class of Layered Double Hydroxides (LDH); they have emerged as promising candidates for CO2 capture due to their basicity, large surface area after calcination, and structural tunability through metal substitution and post-synthesis modifications [11,12,13]. Hydrotalcites belong to compounds with the general formula M 1 − x 2 + M x 3 + O H 2 x + A n − x / n m H 2 O , where: M 2 + is the divalent cation Mg2+; M 3 + is the trivalent cation Al3+; A n − is an interlayer anion (e.g., CO32−, SO42−); x is typically between 0.17 and 0.33. Hydrotalcites thermally decompose into mixed oxides, which can reversibly adsorb CO2 through surface basic sites, and restore the original layered structure if hydrated (a phenomenon known as “memory effect”) [14,15].
Several studies prove that the CO2-sorption capacity of hydrotalcites can be increased by doping with potassium carbonate (K2CO3), which introduces additional basic sites and promotes bicarbonate formation in the presence of steam [16,17,18]. Moreover, the Mg2+/Al3+ molar ratio and synthesis conditions can influence the physicochemical properties and sorption behaviors of hydrotalcites [19,20].
Although the use of hydrotalcites for CO2 capture is widely acknowledged [21,22,23], experimental investigations under SEWGS-relevant conditions proposed in this work (350 °C, including both dry and wet atmospheres, pressure variations above 10 bar, and different synthesis strategies) remain limited in the literature [24]. Stadler et al. [25] investigate the application of a commercial hydrotalcite loaded with 20 wt% of K2CO3 for SEWGS, coupled with a commercial Cu-based WGS catalyst, at 5 bar and 225–300 °C. Martins et al. [26] study commercial hydrotalcite loaded with 20 wt% of K2CO3 at 250–350 °C for biogas upgrading at atmospheric pressure. Xin et al. [27] test the cyclic stability of potassium-promoted hydrotalcite-based adsorbent by thermogravimetric analyses, under dry conditions at atmospheric pressure, with 0.15 bar of CO2 and 0.30 bar of H2O, at 400 °C for CO2 capture and 600 °C for sorbent regeneration.
This work aims to systematically evaluate the CO2 capture performance of five different hydrotalcite-based materials: sorbents derived from commercial hydrotalcite, as such or doped with K2CO3; sorbents from hydrotalcite synthesized by low–super saturation [28], as such or doped with K2CO3; a bifunctional catalyst-sorbent for SEWGS, synthesized at laboratory scale (under patenting procedure [29]). These materials were tested under dynamic PSA cycles in a packed-bed rig at 350 °C, 10 or 14 bar, under both dry and wet conditions, with a fed CO2 concentration of 38.5 mol%. Those operating conditions were chosen to mimic the real case of shifted syngas produced by the industrial waste gasification plant operating in Swindon (UK) [30]. In addition, this work compares synthesis approaches: (i) low supersaturation (LS) method entirely developed at lab-scale, which starts from nitrate precursors; (ii) wet impregnation of readily available commercial hydrotalcite. This comparison aims to highlight the potential scalability of sorbent production by identifying greener, simpler methods. So, the proposed experimental campaign is valuable as a preliminary and original evaluation of sorbent materials for SEWGS, in terms of CO2-sorption capacity and applicability in novel PSA operations; the experiments provide a database to improve previous modelling studies of scaled-up SEWGS [7] to produce low-carbon pure H2 from syngas.

2. Materials and Methods

2.1. Materials

The following precursors were used to synthesize tested sorbents: commercial hydrotalcite (Mg6Al2(CO3) (OH)16∙4H2O) Sigma Aldrich CAS 11097-59-9 (Merck KGaA, Darmstadt, Germany); magnesium nitrate hexahydrate (Mg(NO3)2∙6H2O) Sigma Aldrich CAS 13446-18-9; aluminum nitrate nonahydrate (Al(NO3)3∙9H2O) Sigma Aldrich CAS 7784-27-2; sodium hydroxide (NaOH) Sigma Aldrich 1310-73-2; sodium carbonate (Na2CO3) Sigma Aldrich CAS 497-19-8; potassium carbonate (K2CO3) Sigma Aldrich CAS 584-08-7; and iron (III) nitrate nonahydrate (Fe(NO3)3∙9H2O) Sigma Aldrich CAS 7782-61-8. Distilled water was used in the synthesis steps and as the source of steam. In the PSA experiments, carbon dioxide (99.99%) and nitrogen (99.99%) from Nippon Gases were used.

2.2. Production of Hydrotalcite-Derived Sorbent

Five different types of materials were examined in this study (Table 1). Four of them are solo-sorbent materials (Table 1): sorbent derived from commercial hydrotalcite, as such (HT) and doped with 20 wt% K2CO3 (20KHT); sorbent derived from hydrotalcite synthesized by Low-Supersaturation (LS) [28], as such (HTLS) and doped with 20 wt% K2CO3 (20KHTLS); HT and 20KHT have Mg2+/Al3+ molar ratio of 3:1; HTLS and 20KHTLS have Mg2+/Al3+ of 2:1 (Table 1). The fifth (MeKHT, Table 1) is a bifunctional hydrotalcite-like catalyst-sorbent for SEWGS, purposely synthesized at laboratory scale and under patent application (ref. [29], submission of patent on 12 March 2025).
Table 1. Identification and description of investigated materials.
The Mg2+/Al3+ ratios are derived from commercial choices in the HT cases, and from previous experiences of this research group [31] for materials synthesized by LS. The 20 wt% load of K2CO3 on hydrotalcites is acknowledged in literature [27,32,33] as an optimized value for CO2-capture purposes.
Figure 1 summarizes the synthesis steps for obtaining HT, HTLS, 20KHT, and 20KHTLS (Table 1); the synthesis of MeKHT was not disclosed due to patent coverage.
Figure 1. Syntheses of sorbent materials.

2.2.1. Synthesis of HT Sorbent

HT was originated from commercial hydrotalcite (Mg2+/Al3+ of 3:1). With reference to Figure 1 numbering, the preparation steps of HT were: (i) First calcination: commercial hydrotalcite was calcined in a muffle furnace under stagnant air (heating ramp at 5 °C∙min−1 up to 450 °C, 5-h dwell at 450 °C, cooling until 120 °C); (ii) Hydration: the calcined hydrotalcite, previously cooled in a desiccator, was hydrated with distilled water at a solid-to-liquid ratio of 1:8, stirring at 350 rpm and 60 °C for 1 h; (ix) Drying: the hydrated solution was dried at 120 °C for 12 h; (x) Second calcination: the dried material was calcined like in step (i); (xi) Storing: calcined powder was kept in sealed pillboxes within a desiccator, to limit adsorption of room moisture and CO2.

2.2.2. Synthesis of HTLS Sorbent

HTLS originated from a hydrotalcite co-precipitated at laboratory scale by the LS method detailed by Narayanan et al. [28]. The LS method was chosen to ensure the formation of highly crystalline materials [11,28,34]. The main synthesis steps of HTLS were (numbering in Figure 1): (iii) Preparation of solutions: “A” contained Mg2+ and Al3+ precursor salts at Mg2+/Al3+ molar ratio of 2:1, and “B” was an aqueous solution of NaOH and Na2CO3; (iv) Co-precipitation: solutions A and B were added dropwise in 300 mL of distilled water at 60 °C stirred 350 rpm, keeping pH between 9 and 10; (v) Aging: the milky white resulting suspension was aged for 18 h at 60 °C under continuous stirring; (vi) Filtration and washing: the aged suspension was filtered, and the separated solid was washed until a neutral pH was reached. Afterwards, steps (ix), (x), and (xi) were performed, as described in Section 2.2.1.

2.2.3. K2CO3 Doping

First, 20KHT and 20KHTLS were obtained by doping HT and HTLS with proper amounts of K2CO3, respectively, to achieve a final K2CO3 load of 20 wt% of the initial mass of HT or HTLS [34,35,36,37]. The doping occurred by wet impregnation (see the numbering in Figure 1): (vii) Preparation of impregnation solution: a proper amount of K2CO3 was solubilized in distilled water [24,25,26] (mass solid/water ratio of 1:8); (viii) Wet impregnation: HT or HTLS powders were stirred in the K2CO3 solution at 60 °C and 350 rpm for 1 h. Subsequently, steps (ix), (x), and (xi) were operated as described in Section 2.2.1.

2.3. Characterization of Solids

A Quantachrome NOVA 1200e Surface Area and Pore Size Analyzer (Quantachrome Instruments, Boynton Beach, Florida, USA.) recorded N2 adsorption and desorption isotherms at −196 °C; the samples consisted of 100–200 mg of powder, previously degassed in high vacuum at 200 °C for 1 h. BET surface area (SBET), BJH cumulative pore volumes from desorption (VBJH), and BJH average cylindrical pore diameter (Dav, BJH) were determined. Shapes of isotherms and possible hysteresis were compared with the IUPAC (International Union of Pure and Applied Chemistry) classification [38].
Fourier Transform Infrared Spectroscopy (FTIR) was used to identify functional groups by a Bruker VERTEX 70v analyzer (Bruker Optics GmbH & Co. KG, Ettlingen, Germany). Spectra were compared with the Bruker FTIR-ATR library.
The elemental composition of MeHT and 20KHT was measured by Inductively-Coupled-Plasma-Optical-Emission-Spectroscopy (ICP-OES) using Agilent 5100 instrument (Agilent Technologies, Mulgrave, Victoria, Australia).
The measurements of powder X-Ray Diffraction (XRD) were carried out using a PANalytical X’Pert PRO diffractometer (PANalytical, Almelo, The Netherlands) with Bragg-Brentano geometry and a Cu anode (CuKα1 = 1.5406 Å). Diffractograms were recorded in the 5–80° 2θ range, with a scanning speed of 0.01°·min−1 and a step size of 0.026°. Crystalline phases were identified by ICDD and ICSD reference databases.

2.4. PSA CO2-Capture Tests

2.4.1. Test Rig

The laboratory test rig for dynamic PSA CO2-capture tests (Figure 2) consisted of a heated vertical packed-bed reactor (AISI 316L stainless steel (Supplier: Europa Acciai S.r.l., Giulianova (TE), Italy), 1 cm internal diameter, 55 cm length). The reactor was fed with CO2, N2, and steam and equipped with a downstream online measurement of CO2 concentration [39]. CO2 and N2 flow rates were controlled by Bronkhorst EL-FLOW mass flow controllers (Bronkhorst High-Tech B.V., Ruurlo, The Netherlands) (MFC1 and MFC2, Figure 2). For tests under wet conditions, an HPLC pump (PUMP 422-KONTRON INSTRUMENT (Kontron AG, Ismaning, Germany)) injected a controlled flow rate of distilled water within the heated reactor (at the inlet of active packed-bed) to generate in situ steam, which was conveyed by fed CO2 and N2 (Figure 2); for downstream separation of water, a condenser with gas disengaging operated below the packed bed, cooled by a HAAKE D8 cryostat (Haake Buchler Instruments Inc., Vreden Germany) with ethylenic glycol at −4 °C. A Bronkhorst EL-PRESS backpressure controller (BPC) (Bronkhorst High-Tech B.V., Ruurlo, The Netherlands) regulated the overall pressure by operating on the dried effluent. Eventually, the dry, cooled, depressurized effluent passed through the online CO2 analyzer SIEMENS ULTRAMAT 23 (Siemens AG, Karlsruhe, Germany), which required a minimum flow rate for proper operation; therefore, a constant flow rate of N2 was fed to the analyzer (MFC3, Figure 2).
Figure 2. Layout of the laboratory-scale test rig for PSA CO2-Capture tests (adapted from [24]).

2.4.2. Conditions and Procedure

The reactor was loaded at its center with a packed bed of active granular sorbent (about 5 g, particle diameter of 425–1180 µm, bulk density around 0.35 g cm−3). That active packed bed was between two inert packed beds of zirconia beads (with dimensions similar to active particle size), which filled the entire reactor length and ensured good mixing and heat transfer.
The five materials in Table 1 were tested for dynamic CO2 capture in PSA at operating pressures of 10 and 14 bar under dry and wet conditions. Each CO2-capture PSA test counted five cycles; each PSA cycle included the sequence of “pressurization” in N2, “adsorption” of CO2 until saturation (dry or wet conditions), “depressurization”, and “backwashing” (counter-current N2 flow), all managed manually by valves and controls in Figure 2. The adsorption step was always performed at 350 °C (a temperature compatible with WGS). Table 2 shows the N2, CO2, and water (for steam) inlet flow rates set during the adsorption steps; these values were chosen to maintain a constant CO2 molar fraction of 0.385.
Table 2. Feeding flow rates of the adsorption step during the CO2-capture experimental tests.
For each set of operating conditions (10 or 14 bar, dry or wet inlet, 350 °C constant), a blank test was performed, with five PSA cycles on a dummy reactor filled entirely with inert zirconia beads. Blank tests worked as references to quantify CO2-sorption capacities (see Section 2.4.3).
Operating conditions were chosen to mimic the syngas produced by the industrial waste gasification plant operating in Swindon (UK) [30], in terms of temperature, pressure, moisture, and CO2 content. So, the experimental campaign was valuable as a preliminary evaluation of sorbent properties for future SEWGS applications to obtain low-carbon H2 from syngas.

2.4.3. Quantification of CO2 Sorption Capacity

The adsorption steps of dynamic PSA tests lasted until sorbent saturation was observed (i.e., a plateau in CO2 outlet concentration vs. time was observed at values corresponding to the fed CO2 flow rate net of dilutions). Therefore, an integral quantification of CO2 moles and system holdups in the generic adsorption step of the ith cycle (i = 1, …, 5) allowed enucleating of the CO2 captured per unit mass of active bed until saturation, i.e., the sorption capacity (q). This was done by Equation (1), where: qi was the CO2 sorption capacity of the ith cycle (mmolCO2∙gsolid−1); m was the mass of active packed bed [g]; F C O 2   i n was the inlet CO2 molar flow rate (mmolCO2∙min−1); t f was the duration of adsorption step (min); C C O 2 ( t ) was the outlet CO2 concentration as a function of time (vol%); C C O 2   m a x was the outlet CO2 concentration at saturation (vol%); quantities with “b” subscript referred to the blank test at the same conditions of the ith cycle.
q i = F C O 2   i n m s o l i d ∫ 0 t f C C O 2     b t C C O 2     b   m a x d t − ∫ 0 t f C C O 2 t C C O 2   m a x d t
Equation (1) is based on results by Di Felice et al. [39], who propose to model the gas-phase response curves of continuous-flow systems as a combination of one dead volume and one perfectly mixed volume: their approach, applied to the tests of this work, allowed excluding the gas-phase system holdup from integral CO2 quantifications. The outcomes of Di Felice et al. [39] well interpret the shifting of sigmoidal responses due to the sequestration of a component within the system, net of the gas-phase holdup estimated from the blank sigmoidal curves [24,40,41,42].

3. Results and Discussion

The starting commercial hydrotalcite (Mg6Al2(CO3) (OH)16∙4H2O, Sigma Aldrich CAS 11097-59-9) was used as a reference in characterization results; it was named “HT®”, to avoid confusion with the derived sorbent HT (synthesized as described in Section 2.2.1). The CO2-capture performance of the bifunctional material MeKHT was discussed separately due to its distinct nature.

3.1. Characterizations

3.1.1. Textural Properties

Figure 3a–f show N2 adsorption and desorption isotherms for all the synthesized materials. HT® (Figure 3a), 20KHT (Figure 3c), MeKHT (Figure 3d), HTLS (Figure 3e), and 20KHTLS (Figure 3f) presented the same features: (i) no knee at low P/P0 (relative pressure of adsorbed N2) and hysteresis, similar to Type V of IUPAC’s classification of physisorption isotherms [38]; (ii) a vertical asymptote at P/P0 approaching 1, which matched well with IUPAC’s Type II [38]. IUPAC attributed Type V [38] to weak adsorbent–adsorbate interactions, such as those of water with hydrophobic microporous and mesoporous materials, and Type II [38] to unrestricted multilayer adsorption on macroporous or nonporous structures. The experimental shape of hysteresis (Figure 3a,c–f) resembled IUPAC’s [38] H3 shape, which can concern non-rigid aggregates of plate-like structures. These attributions appeared compatible with materials of hydrotalcitic origin, such as those investigated in this work.
Figure 3. N2 adsorption and desorption isotherms at 77 K on the synthesized material: (a) HT®; (b) HT; (c) 20KHT; (d) MeKHT; (e) HTLS; (f) 20KHTLS.
Due to the absence of hysteresis, the isotherm of HT (Figure 3b) is better compared to the IUPAC’s Type II [38] in the particular case of no distinction of knee-point, which pertains to a non-porous or macroporous adsorbent that rapidly favors unrestricted multilayer physisorption; no hysteresis loop appeared, as the adsorption and desorption branches overlapped. It results from unrestricted monolayer–multilayer gas adsorption, even at high P/P0 values. The multilayer adsorbate thickness is not limited as pressure increases, leading the isotherm to approach a vertical asymptote near P/P0 = 1. The isotherms for HT® (Figure 3a), 20KHT (Figure 3c), MeKHT (Figure 3d), HTLS (Figure 3e), and 20KHTLS (Figure 3f) were classified according to IUPAC as Type IV, with partial residual features of Type II [38]. Such isotherms are typical of mesoporous materials, where low P/P0 adsorption involves single-layer and multilayer processes, like non-porous materials. At the same time, the distinct hysteresis at higher P/P0 suggests capillary condensation within the mesopores. The hysteresis is closest in shape to the H2(b) type, which arises from more complex pore structures with network effects, attributed to mesoporous networks of a “broad” structure [38].
Table 3 reports experimental measurements of BET’s specific surface area (SBET), BJH cumulative pore volume calculated from the desorption branch (VBJH), and consequent estimation of average pore diameter (Dav, BJH). The SBET and VBJH increased significantly by producing HT from HT® (Table 3); HTLS had a lower SBET but a higher VBJH than HT [29]. K2CO3 doping of HT and HTLS led to a decrease of SBET and VBJH in both 20KHT (−76.5% of SBET, −54% of VBJH, Table 3) and 20KHTLS (−70% of SBET, −80% of VBJH, Table 3). Those effects were ascribed to the impregnation procedure and the deposition of K2CO3, which could potentially approach pore blocking [33].
Table 3. Measured BET surface area (SBET), BJH cumulative volume (VBJH), and average pore diameters (Dav, BJH) for as-synthesized materials.
Further details about impregnation results can be considered. Zhenissova et al. [31] investigated a K-promoted hydrotalcite with 20 wt% of K2CO3, finding—by Scanning Electron Microscopy with Energy Dispersive X-ray Spectroscopy (SEM-EDS)—that the needle-like bodies of K2CO3 were deposited nearly exclusively on the external surface. As to the impregnated samples in this work, the content of elemental K was verified by ICP-OES, ranging from 8 to 10 wt% for 20KHT and MeKHT. This range reasonably corresponded to the addition of 20wt% of K2CO3 to hydrotalcite.

3.1.2. FTIR Profiles

Figure 4 compares the FTIR spectra of the investigated materials.
Figure 4. FTIR spectra of commercial hydrotalcite powder (a) HT®; (b) HT; (c) 20KHT; (d) MeKHT; (e) HTLS; (f) 20KHTLS.
The spectrum of HT® may work as a reference; according to the current knowledge [43], the characteristic bands of commercial hydrotalcite HT® were shown in Figure 4 as dashed red lines. The region between 2600–4000 cm−1, also known as the hydroxyl-stretching-region [44], was characterized by broad bands centered at 3460–3490 cm−1 (Figure 4a), attributed to the stretching mode of hydroxyl group that are part of the brucite-like layers and the water molecules present in the interlayer, as well as the water molecules present in the external surface of the sample [43,45]. The shoulder recorded at around 3100 cm−1 (Figure 4a) was associated with the CO3-H2O bridging mode [46]. The medium-intensity band at around 1640 cm−1 (Figure 4a) was attributed to the -OH deformation mode of the water molecules in the hydrotalcite interlayer [47]. The sharper band at 1374 cm−1 was assigned to the stretching mode of the antisymmetric carbonate species in the hydrotalcite interlayer space [48]. The other bands with wavenumbers between 900 and 400 cm−1 were due to vibrations of M-O and O-M-O (M = Mg, Al, or Fe), which are representative of hydrotalcite structures [49,50,51].
Figure 4b–f show the FTIR spectra of the synthesized materials HT, 20KHT, MeKHT, HTLS, and 20KHTLS, respectively: the bands of carbonate-related species (1365.71 and 1491.04 cm−1) and hydroxyl group region (3474.91 and 3072.74 cm−1) decreased, indicating CO2 release and the loss of the characteristic layered structure of hydrotalcite, respectively. Nonetheless, residuals persisted of the sharper band at 1374 cm−1 (stretching mode of antisymmetric carbonate in hydrotalcite interlayer space [52]), indicating that the operated calcination temperature did not lead to complete decomposition of the hydrotalcite-like structures and could, therefore, favor the manifestation of the memory effect of these materials. This mild decomposition would preserve the inter-dispersion of Mg and Al atoms from the original structure.

3.1.3. XRD

Figure 5 reports the XRD spectra of HT® and 20KHT to exemplify changes due to the treatments of hydrotalcites performed in this work (Figure 1). The spectrum of untreated commercial HT® (Figure 5a) showed a sole crystal phase, i.e., the hydrotalcite ICSD 00-014-0191. In contrast, the fresh 20KHT highlighted two main phases (Figure 5b): the MgO (ICSD 00-003-0998) and the K2CO3 (ICSD 00-049-1093), similarly to what was found by Zherenissova et al. [31] for materials synthesized by LS; this confirmed the oxidation of the originating hydrotalcite and the addition of the K2CO3.
Figure 5. X-ray diffractograms of: (a) HT® and (b) fresh 20KHT.

3.2. Results of PSA CO2-Capture Tests

Table 4 collects the experimental qi quantified for each adsorption step of PSA cycles (i = 1, …, 5), with dry or wet feed, at 10 or 14 bar, and 350 °C. Sorption capacities reported in the literature for hydrotalcite-based materials range from 0.28 to 8 mmol/g [12,13,53,54,55,56]. However, these values vary significantly depending on the chemical composition, interlayer anions, and specific operating conditions: for non-promoted hydrotalcites, the sorption capacity at 200 °C and 1 atm is reported between 0.53 and 0.71 mmol/g [55]; doping with 20 wt% of K2CO3 increases the capacity to 0.85 mmol/g at 300 °C [53]. Other K-promoted variants have reached capacities up to 1.43 mmol/g at 300 °C [57]. Under high-pressure (43.5 bar), K-promoted hydrotalcites achieve a high uptake of 5.7 mmol/g at 300 °C [57]. Table 5 summarizes sorption capacities of hydrotalcites from the literature, at some conditions similar to those exerted in this work: overall, the results in Table 4 are acceptable when compared with Table 5.
Table 4. Sorption capacity from the adsorption steps of the five PSA cycles (qi, i = 1, …, 5) and average sorption capacity (qav) with related standard deviation (σ).
Table 5. Sorption capacities of Mg-Al-hydrotalcites from literature (adapted from [53]).
The acceptable performances in Table 4 might promote the possible use of investigated sorbents for SEWGS, since the operating conditions (wet, 350 °C, 10–14 bar) are within the ranges of 300–500 °C and 10–40 bar for the SEWGS with hydrotalcites [5].
For each dynamic PSA test (i.e., each row of Table 4), qi did not show clear trends with cycle number i, suggesting that the tested sorbents were stable and fully regenerated over multiple adsorption–desorption cycles. Figure 6 provides an example of CO2 breakthrough curves, representative of features common to all tests in Table 4: the delay between blank and test curves highlights the effectiveness of the material for CO2 capture (Equation (1)); the test curves (I-V) overlap one another, confirming CO2-capture repeatability among cycles. This behavior allowed considering qi as responses from statistical replications of CO2 captures at each test condition; consequently, the sorbent performance could be better evaluated in terms of arithmetic averages of CO2-sorption capacity (qav, out of five replications) and standard deviation (σ), as shown in Table 4 and Figure 7.
Figure 6. Breakthrough curves of 20KHT at 350 °C and 14 bar, with wet feed (Table 2).
Figure 7. Average sorption capacity out of five PSA cycles (qav) for HT, 20KHT, HTLS, 20KHTLS, and MeKHT, at 10 bar and 14 bar, 350 °C, in dry and wet conditions (Table 2); error bars are standard deviations.

3.2.1. Effect of Pressure on qav

The change from 10 to 14 bar significantly increased sorption capacities for all investigated samples (Table 4, Figure 7). At dry conditions, qav at 14 bar was higher than qav at 10 bar by +110% for HT, +181% for 20KHT, +12% for HTLS, +172% for 20KHTLS, and +41% for MeKHT (Table 4). At wet conditions, qav at 14 bar was higher than qav at 10 bar by +12% for HT, +27% for 20KHT, +31% for HTLS, +27% for 20KHTLS, and +58% for MeKHT (Table 4).
These results agreed with the increase in sorption capacity documented in the literature with increasing pressure [57,62]. Notably, the materials had acceptable performances even at 10 bar—i.e., the lowest limit of the 10–40 bar range indicated in literature for SEWGS based on hydrotalcites [5]. This is a general process advantage, since milder pressures (i.e., lower pressurization costs) would be required to operate sorption-enhancing.

3.2.2. Effect of K2CO3-Doping on qav

The comparison of 20KHT vs. HT and 20KHTLS vs. HTLS allowed for the evaluation of the influence of K2CO3 doping (Table 4, Figure 7).
As to sorbents derived from commercial hydrotalcite (20KHT and HT, Table 4, Figure 7), at dry conditions and 14 bar, qav of 20KHT was +16% higher than qav of HT, while the effect of the K2CO3 doping was slightly negative at 10 bar (although they were contained in error bars, Figure 7). Conversely, at wet conditions, qav of 20KHT increased by about +62% at 14 bar, and +43% at 10 bar, when compared to qav of HT (Table 4, Figure 7).
As to sorbents derived from LS hydrotalcite (20KHTLS vs. HTLS, Table 4, Figure 7), at dry conditions and 14 bar, qav of 20KHTLS was +9% higher than qav of HTLS but strongly decreases at 10 bar (about −55%, 20KHTLS vs. HTLS). Under wet conditions, K2CO3 doping of HTLS caused a slightly positive effect on qav (about +14% at 10 bar, and +10% at 14 bar, Table 4, Figure 7).
Impregnation with potassium carbonate is a strategy to enhance the CO2-sorption capacity of hydrotalcite-based materials [63,64]. Moreover, steam facilitates the mobility of potassium species and improves the regeneration of active sites, leading to higher bed usage efficiency and increased reactivity, sometimes up to 70% higher than in dry conditions [65,66,67]; in other words, wet conditions may be more favorable for CO2 capture by K2CO3-doped sorbents. Regarding the materials used in this work, K2CO3 doping consistently increased CO2-sorption capacity, which is in agreement with the aforementioned literature, except for tests at 10 bar and under dry conditions (Table 4, Figure 7). Ineffectiveness of K2CO3 doping at 10 bar and dry conditions (Table 4, Figure 7) could be explained by the fact that K2CO3-doped hydrotalcites worked better in wet environments [66,67,68] and by the textural properties of investigated materials (Table 3): the impregnation with K2CO3 significantly reduced SBET and VBJH of both sorbents derived from commercial hydrotalcite (20KHT vs. HT, Table 3) and LS one (20KHTLS vs. HTLS, Table 3); at lower pressure and dry environment, the influence from lowered SBET and VBJH prevailed since potassium-based species did not take advantage of the wet environment; this made HT and HTLS perform better than their impregnated counterparts at 10 bar dry (Table 3).
A closer look at K2CO3-doped sorbents revealed that qav of 20KHT was always higher than qav of 20KHTLS (Figure 7), although they had very similar texture (SBET, VBJH, Dav,BJH, Table 3). This difference could be attributed to the details of the impregnation step (viii, Section 2.2.3): average particle size of the impregnated 20KHT was approximately one order of magnitude smaller than that of 20KHTLS (10−1 mm vs. 100 mm); this may have influenced the distribution of K2CO3.

3.2.3. Effect of Mg2+/Al3+ on qav

HTLS had a higher qav than its commercial counterpart HT at 10 bar wet and dry, and at 14 bar wet; qav of HTLS and HT were close at 14 bar dry (Figure 7). Better performances of HTLS vs. HT were attributed to the different Mg2+/Al3+ molar ratios (2:1 for HTLS, 3:1 for HT); Zhe et al. [68] suggest that hydrotalcites with a Mg2+/Al3+ molar ratio of 2:1 exhibit higher sorption capacities compared to those with a 3:1 ratio (no K2CO3-doping, 400 °C, CO2 partial pressure of 1 bar [68]).
However, this effect of Mg2+/Al3+ in the parent sorbents did not affect K2CO3-doped ones (Figure 7): 20KHT (Mg2+/Al3+ of 3:1) performed slightly better than 20KHTLS (Mg2+/Al3+ of 2:1) despite its higher Mg2+/Al3+. For hydrotalcites with Mg2+/Al3+ molar ratios of 3:1, sorption capacities up to 1.78 mmolCO2∙gad−1 at 300 °C have been reported after K2CO3 doping, which are slightly higher than those with a 2:1 ratio under similar conditions [68,69].

3.2.4. Effect of Steam on qav

All materials exhibited higher sorption capacities under wet conditions at equal pressure (Figure 7, Table 4). HT and HTLS showed an increase in qav due to the switch from dry to wet conditions (Figure 7): at 10 bar, qav increased by +23% for HT and +94% for HTLS; at 14 bar, it increased by +48% for HT and +12% for HTLS. Also, 20KHT and 20KHTLS showed the most significant enhancements when comparing wet to dry tests (Figure 7): at 10 bar, qav increased by +358% for 20KHT and +391% for 20KHTLS; at 14 bar, by +107% for 20KHT and +128% for 20KHTLS.
The improvement of CO2-sorption capacity under wet conditions could be attributed to an increased number of available basic sites and the formation of bicarbonates due to hydration effects, as reported in the literature [4,17]. The increase of basicity due to alkali metal carbonates helps to adsorb more CO2 on the hydrotalcite [33,70]; the CO2 sorption capacity could be furtherly increased by K2CO3 on hydrotalcite in the presence of steam, according to the reaction R.3 [17] (reversible by heating).
K 2 C O 3 + C O 2 + H 2 O → 2 K H C O 3 + H e a t

3.2.5. Bifunctional Material

Values of qav of MeKHT ranged between 0.75–1.39 mmolCO2·gsolid−1 (Figure 7), which were satisfying for CO2-capture applications compared to the literature ranges (0.94–1.43 mmol/g [35]). MeKHT ensured a balanced performance when switching from dry to wet conditions: qav increased by +17% at 10 bar and +31% at 14 bar.
At dry conditions and 14 bar, MeKHT outperformed HT, 20KHT, HTLS, and 20KHTLS, with qav of 1.08 mmolCO2∙gsolid−1 vs. 0.63, 0.73, 0.55, 0.60 mmolCO2∙gsolid−1, respectively (Figure 7). At wet conditions and 14 bar, MeKHT had a qav close to the best one (of 20KHT), i.e., 1.39 mmolCO2∙gad−1 vs. 1.51 mmolCO2∙gad−1 (Figure 7).
Furthermore, MeKHT ensured a high stability and reproducibility of CO2 capture for five PSA cycles, maintaining qi standard deviation (σ) within 0.06–0.05 mmolCO2∙gsolid−1 (Table 4).
Overall, the introduction of the catalytic metallic element for WGS did not adversely affect the CO2-sorption capacity of MeKHT.

4. Conclusions

This study demonstrated that hydrotalcite-derived sorbents can capture CO2 with profitable sorption capacity under conditions relevant to SEWGS, with sorbent regeneration via PSA. Increasing the pressure from 10 to 14 bar and feeding steam markedly increased CO2 Sorption capacity, confirming the synergistic role of solid basicity and hydration in adsorbing CO2. Among the investigated materials, 20KHT and MeKHT gave the most promising CO2-capture performances, i.e., 1.51 mmolCO2∙gsolid−1 and 1.39 mmolCO2∙gsolid−1 at 14 bar and wet conditions. The beneficial influence on CO2-sorption capacity from pore texture (i.e., higher specific surface area and pore volume) prevailed only at lower pressure (10 bar) and dry environment; at other tested conditions (14 bar, dry or wet), the improvements due to potassium-impregnation appeared more determinant. The performances of MeKHT demonstrated that incorporating the metallic catalytic element for WGS did not compromise CO2-sorption capacity, introducing a novel bifunctional approach for process intensification through sorption enhancement. These findings established a solid foundation for the development of hydrotalcite-based bifunctional sorbent-catalyst materials that enable integrated CO2 Capture and hydrogen production in future advanced SEWGS systems. The measured sorption capacities under dynamic PSA conditions can inform new modelling and scaling-up studies, oriented toward applications of hydrotalcite-derived materials for CO2 Capture and process intensification.

Author Contributions

Conceptualization, A.D.G. and K.G.; methodology, A.D.G. and K.G.; software, B.M. and G.D.; validation, A.D.G. and K.G.; formal analysis, B.M., A.D.G. and K.G.; investigation, B.M. and G.D.; resources, K.G.; data curation, B.M., A.D.G. and K.G.; writing—original draft preparation, B.M., A.D.G. and K.G.; writing—review and editing, B.M., A.D.G. and K.G.; visualization, B.M., A.D.G. and K.G.; supervision, A.D.G. and K.G.; project administration, K.G.; funding acquisition, A.D.G. and K.G. All authors have read and agreed to the published version of the manuscript.

Funding

This work was supported by MUR (Italian Ministry of University and Research) [PON 2014–2020–CUP E19J21012860001–DOT13LHQ8Y-2].

Data Availability Statement

The original contributions presented in this study are included in the article. Further inquiries may be directed to the corresponding author.

Acknowledgments

The authors thank Fabiola Ferrante for technical support in N2 physisorption and Angelo Sarra for technical support in FTIR. The authors also thank Francesco Di Luca for hosting Greta D’Antonio’s internship.

Conflicts of Interest

The authors declare no conflicts of interest.

Abbreviations

BETBraunauer-Emmet-Teller
BJHBarret-Joyner-Helenda
FTIRFourier Transform InfraRed spectroscopy
ICP-OESInductively Coupled Plasma—Optical Emission Spectroscopy
LSLow-Supersaturation
PSAPressure Swing Adsorption
SEM-EDSScanning Electron Microscopy—Energy Dispersive X-ray Spectroscopy
SEWGSSorption-Enhanced Water-Gas Shift
WGSWater Gas Shift
XRDX-Ray Diffraction

References

  1. Satterfield, C.N. Heterogeneous Catalysis in Practice, 416, 1980. Available online: https://books.google.com/books/about/Heterogeneous_Catalysis_in_Practice.html?hl=it&id=QrZTAAAAMAAJ (accessed on 22 December 2025).
  2. Dawood, F.; Anda, M.; Shafiullah, G.M. Hydrogen production for energy: An overview. Int. J. Hydrogen Energy 2020, 45, 3847–3869. [Google Scholar] [CrossRef] [Scilit]
  3. Rolo, I.; Costa, V.A.F.; Brito, F.P. Hydrogen-Based Energy Systems: Current Technology Development Status, Opportunities and Challenges. Energies 2024, 17, 180. [Google Scholar] [CrossRef] [Scilit]
  4. Yong, Z.; Rodrigues, A.E. Hydrotalcite-like compounds as adsorbents for carbon dioxide. Energy Convers. Manag. 2002, 43, 1865–1876. [Google Scholar] [CrossRef] [Scilit]
  5. Boon, J.; Cobden, P.D.; van Dijk, H.A.J.; van Sint Annaland, M. High-temperature pressure swing adsorption cycle design for sorption-enhanced water-gas shift. Chem. Eng. Sci. 2015, 122, 219–231. [Google Scholar] [CrossRef] [Scilit]
  6. Fatigati, F.; Di Giuliano, A.; Carapellucci, R.; Gallucci, K.; Cipollone, R. Experimental Characterization and Energy Performance Assessment of a Sorption-Enhanced Steam–Methane Reforming System. Processes 2021, 9, 1440. [Google Scholar] [CrossRef] [Scilit]
  7. Malsegna, B.; Sebastiani, A.; da Gama Paz-Dias, J.G.; Di Luca, F.; Di Giuliano, A.; Gallucci, K.; Materazzi, M. Simulation of a sorption-enhanced water gas-shift pilot technology for pure hydrogen production from a waste gasification plant. Fuel Process. Technol. 2024, 254, 108032. [Google Scholar] [CrossRef] [Scilit]
  8. Gonçalves, R.G.L.; Catuzo, G.L.; Assaf, J.M.; Assaf, E.M. Evaluation of the potassium incorporation method in MgFe catalysts derived from layered double hydroxides in the hydrogenation of CO2. Catal. Today 2025, 448, 115166. [Google Scholar] [CrossRef] [Scilit]
  9. Cavallo, M.; Dosa, M.; Porcaro, N.G.; Bonino, F.; Piumetti, M.; Crocella, V. Shaped natural and synthetic zeolites for CO2 capture in a wide temperature range. J. CO2 Util. 2023, 67, 102335. [Google Scholar] [CrossRef] [Scilit]
  10. Wang, Q.; Luo, J.; Zhong, Z.; Borgna, A. CO2 capture by solid adsorbents and their applications: Current status and new trends. Energy Environ. Sci. 2010, 4, 42–55. [Google Scholar] [CrossRef] [Scilit]
  11. Cavani, F.; Trifirò, F.; Vaccari, A. Hydrotalcite-type anionic clays: Preparation, properties and applications. Catal. Today 1991, 11, 173–301. [Google Scholar] [CrossRef] [Scilit]
  12. Yong, Z.; Mata, V.; Rodrigues, A.E. Adsorption of carbon dioxide onto hydrotalcite-like compounds (HTlcs) at high temperatures. Ind. Eng. Chem. Res. 2001, 40, 204–209. [Google Scholar] [CrossRef] [Scilit]
  13. Reddy, M.K.R.; Xu, Z.P.; Lu, G.Q.; Da Costa, J.C.D. Layered double hydroxides for CO2 capture: Structure evolution and regeneration. Ind. Eng. Chem. Res. 2006, 45, 7504–7509. [Google Scholar] [CrossRef] [Scilit]
  14. Zhu, X.; Chen, C.; Suo, H.; Wang, Q.; Shi, Y.; O’Hare, D.; Cai, N. Synthesis of elevated temperature CO2 adsorbents from aqueous miscible organic-layered double hydroxides. Energy 2019, 167, 960–969. [Google Scholar] [CrossRef] [Scilit]
  15. Ye, H.; Liu, S.; Yu, D.; Zhou, X.; Qin, L.; Lai, C.; Qin, F.; Zhang, M.; Chen, W.; Chen, W.; et al. Regeneration mechanism, modification strategy, and environment application of layered double hydroxides: Insights based on memory effect. Coord. Chem. Rev. 2022, 450, 214253. [Google Scholar] [CrossRef] [Scilit]
  16. Ding, Y.; Alpay, E. Equilibria and kinetics of CO2 adsorption on hydrotalcite adsorbent. Chem. Eng. Sci. 2000, 55, 3461–3474. [Google Scholar] [CrossRef] [Scilit]
  17. Reddy, M.K.R.; Xu, Z.P.; Lu, G.Q.; Da Costa, J.C.D. Influence of Water on High-Temperature CO2 Capture Using Layered Double Hydroxide Derivatives. Ind. Eng. Chem. Res. 2008, 47, 2630–2635. [Google Scholar] [CrossRef] [Scilit]
  18. Walspurger, S.; Cobden, P.D.; Safonova, O.V.; Wu, Y.; Anthony, E.J. High CO2 Storage Capacity in Alkali-Promoted Hydrotalcite-Based Material: In Situ Detection of Reversible Formation of Magnesium Carbonate. Chem.—A Eur. J. 2010, 16, 12694–12700. [Google Scholar] [CrossRef] [Scilit]
  19. Hutson, N.D.; Speakman, S.A.; Payzant, E.A. Structural effects on the high temperature adsorption of CO2 on a synthetic hydrotalcite. Chem. Mater. 2004, 16, 4135–4143. [Google Scholar] [CrossRef] [Scilit]
  20. Aschenbrenner, O.; McGuire, P.; Alsamaq, S.; Wang, J.; Supasitmongkol, S.; Al-Duri, B.; Styring, P.; Wood, J. Adsorption of carbon dioxide on hydrotalcite-like compounds of different compositions. Chem. Eng. Res. Des. 2011, 89, 1711–1721. [Google Scholar] [CrossRef] [Scilit]
  21. Lalaut, A.; Courson, C.; Gallucci, K. Development of a High Temperature CO2 Sorbent Based on Hydrotalcite for a H2-Rich Syngas Production. Waste Biomass Valorization 2021, 13, 117–133. [Google Scholar] [CrossRef] [Scilit]
  22. Bhatta, L.K.G.; Subramanyam, S.; Chengala, M.D.; Olivera, S.; Venkatesh, K. Progress in hydrotalcite like compounds and metal-based oxides for CO2 capture: A review. J. Clean. Prod. 2015, 103, 171–196. [Google Scholar] [CrossRef] [Scilit]
  23. Sikander, U.; Sufian, S.; Salam, M.A. A review of hydrotalcite based catalysts for hydrogen production systems. Int. J. Hydrogen Energy 2017, 42, 19851–19868. [Google Scholar] [CrossRef] [Scilit]
  24. Malsegna, B.; Materazzi, M.; Di Luca, F.; Di Giuliano, A.; Gallucci, K. Preliminary Assessment of Sorption Capacity on Solid CO2-Sorbents at Conditions for Sorption-Enhanced Processes. Chem. Eng. Trans. 2023, 100, 685–690. [Google Scholar] [CrossRef]
  25. Stadler, T.J.; Barbig, P.; Kiehl, J.; Schulz, R.; Klövekorn, T.; Pfeifer, P. Sorption-Enhanced Water-Gas Shift Reaction for Synthesis Gas Production from Pure CO: Investigation of Sorption Parameters and Reactor Configurations. Energies 2021, 14, 355. [Google Scholar] [CrossRef] [Scilit]
  26. Martins, J.A.; Miguel, C.V.; Rodrigues, A.E.; Madeira, L.M. Novel Adsorption–Reaction Process for Biomethane Purification/Production and Renewable Energy Storage. ACS Sustain. Chem. Eng. 2022, 10, 7833–7851. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  27. Xin, K.; Boon, J.; van Dijk, H.A.J.; van Sint Annaland, M. Stability of potassium-promoted hydrotalcites for CO2 capture over numerous repetitive adsorption and desorption cycles. Front. Chem. Eng. 2024, 6, 1272152. [Google Scholar] [CrossRef] [Scilit]
  28. Narayanan, S.; Krishna, K. Hydrotalcite-supported palladium catalysts Part I: Preparation, characterization of hydrotalcites and palladium on uncalcined hydrotalcites for CO chemisorption and phenol hydrogenation. Appl. Catal. A Gen. 1998, 174, 221–229. [Google Scholar] [CrossRef] [Scilit]
  29. Gallucci, K.; Di Giuliano, A.; Malsegna, B.; Materazzi, M.; Sebastiani, A. Metodo per la Preparazione di un Materiale Solido Particellare Bifunzionale. Application Number 102025000005046, 2025. [Google Scholar]
  30. Swindon Plant | Advanced Biofuel Solutions Ltd. 2023. Available online: https://absl.tech/swindon-plant (accessed on 18 April 2023).
  31. Zhenissova, A.; Micheli, F.; Rossi, L.; Stendardo, S.; Foscolo, P.U.; Gallucci, K. Experimental evaluation of Mg- and Ca-based synthetic sorbents for CO2 capture. Chem. Eng. Res. Des. 2014, 92, 727–740. [Google Scholar] [CrossRef] [Scilit]
  32. Halabi, M.H.; De Croon, M.H.J.M.; Van Der Schaaf, J.; Cobden, P.D.; Schouten, J.C. High capacity potassium-promoted hydrotalcite for CO2 capture in H2 production. Int. J. Hydrogen Energy 2012, 37, 4516–4525. [Google Scholar] [CrossRef] [Scilit]
  33. Yang, J.I.; Kim, J.N. Hydrotalcites for adsorption of CO2 at high temperature. Korean J. Chem. Eng. 2006, 23, 77–80. [Google Scholar] [CrossRef] [Scilit]
  34. Gallucci, K.; Micheli, F.; Poliandri, A.; Rossi, L.; Foscolo, P.U. CO2 Sorption by Hydrotalcite-Like Compounds in Dry and Wet Conditions. Int. J. Chem. React. Eng. 2015, 13, 335–349. [Google Scholar] [CrossRef] [Scilit]
  35. Silva, J.M.; Trujillano, R.; Rives, V.; Soria, M.A.; Madeira, L.M. High temperature CO2 sorption over modified hydrotalcites. Chem. Eng. J. 2017, 325, 25–34. [Google Scholar] [CrossRef] [Scilit]
  36. Miguel, C.V.; Trujillano, R.; Rives, V.; Vicente, M.A.; Ferreira, A.F.P.; Rodrigues, A.E.; Mendes, A.; Madeira, L.M. High temperature CO2 sorption with gallium-substituted and promoted hydrotalcites. Sep. Purif. Technol. 2014, 127, 202–211. [Google Scholar] [CrossRef] [Scilit]
  37. Hanif, A.; Dasgupta, S.; Divekar, S.; Arya, A.; Garg, M.O.; Nanoti, A. A study on high temperature CO2 capture by improved hydrotalcite sorbents. Chem. Eng. J. 2014, 236, 91–99. [Google Scholar] [CrossRef] [Scilit]
  38. Thommes, M.; Kaneko, K.; Neimark, A.V.; Olivier, J.P.; Rodriguez-Reinoso, F.; Rouquerol, J.; Sing, K.S.W. Physisorption of gases, with special reference to the evaluation of surface area and pore size distribution (IUPAC Technical Report). Pure Appl. Chem. 2015, 87, 1051–1069. [Google Scholar] [CrossRef] [Scilit]
  39. Di Felice, L.; Foscolo, P.U.; Gibilaro, L. CO2 capture by calcined dolomite in a fluidized bed: Experimental data and numerical simulations. Int. J. Chem. React. Eng. 2011, vol. 9. [Google Scholar] [CrossRef] [Scilit]
  40. Mammarella, D.; Gallucci, K.; Di Giuliano, A. Biochar from waste vineyard pruning as a selective sorbent for biogas upgrading by pressure swing adsorption: Experimental and modelling study. Chem. Eng. J. Adv. 2026, 25, 101050. [Google Scholar] [CrossRef] [Scilit]
  41. Mammarella, D.; Gallucci, K.; Di Giuliano, A. Biochar from Waste Vineyard Pruning as a CO2 Sorbent in Pressure Swing Adsorption: Experimental and Modeling Study. ACS Omega 2025, 10, 25394–25404. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  42. Mammarella, D.; Di Giuliano, A.; Freda, C.; De Bari, I.; Gallucci, K. Upgrading of Biogas to Biomethane by Using Biochars as CO2 Sorbent in a Pressure Swing Adsorption Device. Chem. Eng. Trans. 2024, 109, 79–84. [Google Scholar] [CrossRef]
  43. Heriyanto Heraldy, E.; Nugrahaningtyas, K.D. X-RAY Diffraction and Fourier Transform Infrared Study of Ca-Mg-Al Hydrotalcite from Artificial Brine Water with Synthesis Hydrothermal Treatments. IOP Conf. Ser. Mater. Sci. Eng. 2018, 333, 012006. [Google Scholar] [CrossRef] [Scilit]
  44. Colthup, N.B. Infrared Spectroscopy. Encycl. Phys. Sci. Technol. 2003, 793–816. [Google Scholar] [CrossRef] [Scilit]
  45. Macedo, M.S.; Soria, M.A.; Madeira, L.M. High temperature CO2 sorption using mixed oxides with different Mg/Al molar ratios and synthesis pH. Chem. Eng. J. 2021, 420, 129731. [Google Scholar] [CrossRef] [Scilit]
  46. Kloprogge, J.T.; Hickey, L.; Frost, R.L. The effects of synthesis pH and hydrothermal treatment on the formation of zinc aluminum hydrotalcites. J. Solid State Chem. 2004, 177, 4047–4057. [Google Scholar] [CrossRef] [Scilit]
  47. Kloprogge, J.T.; Hickey, L.; Frost, R.L. The effect of varying synthesis conditions on zinc chromium hydrotalcite: A spectroscopic study. Mater. Chem. Phys. 2005, 89, 99–109. [Google Scholar] [CrossRef] [Scilit]
  48. Hickey, L.; Kloprogge, J.T.; Frost, R.L. Effects of various hydrothermal treatments on magnesium-aluminum hydrotalcites. J. Mater. Sci. 2000, 35, 4347–4355. [Google Scholar] [CrossRef] [Scilit]
  49. Zhou, H.; Tan, Y.; Gao, W.; Zhang, Y.; Yang, Y. Selective nitrate removal from aqueous solutions by a hydrotalcite-like absorbent FeMgMn-LDH. Sci. Rep. 2020, 10, 16126. [Google Scholar] [CrossRef] [Scilit]
  50. Warmuz, K.; Madej, D. Synthesis and evaluation of Mg-Al hydrotalcite formation and its influence on the microstructural evolution of spinel-forming refractory castables under intermediate temperatures. J. Eur. Ceram. Soc. 2022, 42, 2545–2555. [Google Scholar] [CrossRef] [Scilit]
  51. Chang, Z.; Evans, D.G.; Duan, X.; Vial, C.; Ghanbaja, J.; Prevot, V.; De Roy, M.; Forano, C. Synthesis of [Zn-Al-CO3] layered double hydroxides by a coprecipitation method under steady-state conditions. J. Solid State Chem. 2005, 178, 2766–2777. [Google Scholar] [CrossRef] [Scilit]
  52. Teodorescu, F.; Pǎlǎduţǎ, A.M.; Pavel, O.D. Memory effect of hydrotalcites and its impact on cyanoethylation reaction. Mater. Res. Bull. 2013, 48, 2055–2059. [Google Scholar] [CrossRef] [Scilit]
  53. Wang, Q.; Wu, Z.; Tay, H.H.; Chen, L.; Liu, Y.; Chang, J.; Zhong, Z.; Luo, J.; Borgna, A. High temperature adsorption of CO2 on Mg–Al hydrotalcite: Effect of the charge compensating anions and the synthesis pH. Catal. Today 2011, 164, 198–203. [Google Scholar] [CrossRef] [Scilit]
  54. Wang, Q.; Tay, H.H.; Ng, D.J.W.; Chen, L.; Liu, Y.; Chang, J.; Zhong, Z.; Luo, J.; Borgna, A. The effect of trivalent cations on the performance of Mg-M-CO3 layered double hydroxides for high-temperature CO2 capture. ChemSusChem 2010, 3, 965–973. [Google Scholar] [CrossRef] [Scilit]
  55. Hutson, N.D.; Attwood, B.C. High temperature adsorption of CO2 on various hydrotalcite-like compounds. Adsorption 2008, 14, 781–789. [Google Scholar] [CrossRef] [Scilit]
  56. Gao, Y.; Zhang, Z.; Wu, J.; Yi, X.; Zheng, A.; Umar, A.; O’Hare, D.; Wang, Q. Comprehensive investigation of CO2 adsorption on Mg-Al-CO3 LDH-derived mixed metal oxides. J. Mater. Chem. A Mater. 2013, 1, 12782–12790. [Google Scholar] [CrossRef] [Scilit]
  57. Santamaría, L.; Korili, S.A.; Gil, A. Layered double hydroxides for CO2 adsorption at moderate temperatures: Synthesis and amelioration strategies. Chem. Eng. J. 2023, 455, 140551. [Google Scholar] [CrossRef] [Scilit]
  58. Chen, C.; Wangriya, A.; Buffet, J.C.; O’Hare, D. Tuneable ultra high specific surface area Mg/Al-CO3 layered double hydroxides. Dalton Trans. 2015, 44, 16392–16398. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  59. Wang, Q.; Tay, H.H.; Zhong, Z.; Luo, J.; Borgna, A. Synthesis of high-temperature CO2 adsorbents from organo-layered double hydroxides with markedly improved CO2 capture capacity. Energy Environ. Sci. 2012, 5, 7526–7530. [Google Scholar] [CrossRef] [Scilit]
  60. Garcés-Polo, S.I.; Villarroel-Rocha, J.; Sapag, K.; Korili, S.A.; Gil, A. Adsorption of CO2 on mixed oxides derived from hydrotalcites at several temperatures and high pressures. Chem. Eng. J. 2018, 332, 24–32. [Google Scholar] [CrossRef] [Scilit]
  61. Boon, J.; Cobden, P.D.; van Dijk, H.A.J.; Hoogland, C.; van Selow, E.R.; van Sint Annaland, M. Isotherm model for high-temperature, high-pressure adsorption of CO2 and H2O on K-promoted hydrotalcite. Chem. Eng. J. 2014, 248, 406–414. [Google Scholar] [CrossRef] [Scilit]
  62. Zhao, C.; Wang, L.; Huang, L.; Musyoka, N.M.; Xue, T.; Rabeah, J.; Wang, Q. Recent advances in intermediate-temperature CO2 capture: Materials, technologies and applications. J. Energy Chem. 2024, 90, 435–452. [Google Scholar] [CrossRef] [Scilit]
  63. Vicente, M.A.; Trujillano, R.; Labajos, F.M.; Suescum-Morales, D.; Jiménez, J.R.; Fernández-Rodríguez, J.M. Review of the Application of Hydrotalcite as CO2 Sinks for Climate Change Mitigation. ChemEngineering 2022, 6, 50. [Google Scholar] [CrossRef] [Scilit]
  64. Shareef, U.; Rownaghi, A.A.; Rezaei, F. Monometallic and bimetallic hydrotalcite adsorbents for high-temperature CO2 capture. Chem. Eng. J. 2025, 523, 167884. [Google Scholar] [CrossRef] [Scilit]
  65. Silva, J.M.; Trujillano, R.; Rives, V.; Soria, M.A.; Madeira, L.M. Dynamic behaviour of a K-doped Ga substituted and microwave aged hydrotalcite-derived mixed oxide during CO2 sorption experiments. J. Ind. Eng. Chem. 2019, 72, 491–503. [Google Scholar] [CrossRef] [Scilit]
  66. Gallucci, K.; Micheli, F.; Barisano, D.; Villone, A.; Foscolo, P.U.; Rossi, L. CO2 sorption-enhanced processes by hydrotalcite-like compounds at different temperature levels. Int. J. Chem. React. Eng. 2015, 13, 143–152. [Google Scholar] [CrossRef] [Scilit]
  67. Coenen, K.; Gallucci, F.; Hensen, E.; Van Sint Annaland, M. CO2 and H2O chemisorption mechanism on different potassium-promoted sorbents for SEWGS processes. J. CO2 Util. 2018, 25, 180–193. [Google Scholar] [CrossRef] [Scilit]
  68. Zhu, X.; Chen, C.; Wang, Q.; Shi, Y.; O’Hare, D.; Cai, N. Roles for K2CO3 doping on elevated temperature CO2 adsorption of potassium promoted layered double oxides. Chem. Eng. J. 2019, 366, 181–191. [Google Scholar] [CrossRef] [Scilit]
  69. Shahid, M.Z.; Farooqi, A.S.; Fajri, K.; El-Adawy, M.; Hamdy, M.; Farooqi, A.S.; Abdelaziz, O.Y.; Hossain, M.M.; Nemitallah, M.A. Clean hydrogen production via sorption enhanced water gas shift reaction: A comprehensive review. Int. J. Hydrogen Energy 2025, 100, 1483–1512. [Google Scholar] [CrossRef] [Scilit]
  70. Hoffman, J.S.; Pennline, H.W. Investigation of Regenerable Sorbents for CO2 Capture; National Energy Technology Laboratory: Pittsburgh, PA, USA, 1999. [Google Scholar]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.