  • Article
  • Open Access

1 June 2026

22 Pages

Durability Assessment of Self-Compacting Sand Concrete Incorporating Windshield Glass Aggregate Under Extreme Environmental Conditions: High Temperature and Freeze–Thaw Cycling

,
,
,
,
and
1
Materials and Environment Laboratory, Yahia Fares University of Medea, Urban Pole, P.O. Box 164, Medea 26000, Algeria
2
Civil Engineering Department, Yahia Fares University of Medea, Urban Pole, P.O. Box 164, Medea 26000, Algeria
3
Department of Chemical Engineering, Materials, Environment, Sapienza University of Rome, 00184 Rome, Italy
*
Authors to whom correspondence should be addressed.

Abstract

This study evaluates the durability of Self-Compacting Sand Concrete (SCSC) incorporating Windshield Glass Aggregate (WGA) as a sustainable replacement for natural sand, utilizing Blast Furnace Slag (BFS) as a constant filler component. Eleven mixtures were investigated: a control mix and ten variants with WGA substitution levels ranging from 10% to 100% in 10% increments. The specimens were exposed to elevated temperatures of 200–800 °C and to 240 freeze–thaw cycles between −18 °C and +9 °C. Under heating, mass loss increased with temperature, but WGA-rich mixtures generally showed lower mass loss and higher residual mechanical performance than the control. At 400 °C, WGA100 reached about 96 MPa in compressive strength and 15 MPa in flexural strength, corresponding to residual values of approximately 110.34% and 166.7%, respectively. After freeze–thaw cycling, all mixtures showed limited surface deterioration and mass loss below 1%, decreasing from about 0.76% for the control mixture to about 0.05% for WGA100. The improved durability is mainly attributed to the physical effect of WGA replacement and the baseline matrix refinement associated with BFS.

1. Introduction

Concrete is the most widely used material in the construction industry, but its production and use are associated with considerable environmental burdens [1,2]. Two of the approaches to improving the sustainability of concrete are replacing natural sand with waste-derived aggregates and increasing the durability and service life of cement-based materials. The replacement of natural sand with waste-derived aggregates can limit natural-resource depletion, reduce extraction-related environmental impacts, and divert solid wastes from landfills [3,4]. Among available waste streams, glass waste is particularly attractive because of its high availability, low water absorption, dimensional stability, hardness, and silica-rich composition [5]. Previous studies have also shown that, when the particle size and mixture design are properly controlled, waste-glass aggregate can maintain or improve selected mechanical and durability-related properties of cementitious composites [6]. The second approach is to improve durability, because longer-lasting concrete requires fewer repair, rehabilitation, and replacement interventions and therefore reduces cumulative material consumption, energy demand, and environmental impact over the life cycle of structures [7,8,9]. These two strategies are closely connected in severe service environments, where the use of alternative aggregates is meaningful only if the resulting concrete can maintain adequate performance under deterioration mechanisms such as fire exposure and freeze–thaw cycling [10,11].
Among durability-related properties, resistance to elevated temperature is especially important for concrete used in fire-prone applications. Exposure to high temperatures causes both physical and chemical changes in the cementitious matrix. At temperatures of about 100–200 °C, evaporation of free water and the loss of physically and weakly bound water reduce the stability of the hydrated paste [12]. With further heating, dehydration of hydration products, vapor-pressure build-up in the pore network, and differential thermal expansion between paste and aggregate promote internal cracking and spalling. Georgali and Tsakiridis [13] reported that dehydration up to about 540 °C is associated with microcracking and pore-pressure development. In addition, the decomposition of portlandite in the range of about 450–550 °C and the progressive degradation of Calcium Silicate Hydrate (C-S-H) at higher temperatures further weaken the matrix and the interfacial transition zone (ITZ), leading to substantial losses in residual mechanical performance [13,14,15].
Resistance to freeze–thaw cycling is another key durability requirement for cement-based materials used in cold climates. Freeze–thaw damage develops when water confined in pores freezes and expands, generating hydraulic and crystallization-related pressures within the microstructure [16,17,18]. When these pressures exceed the tensile capacity of the matrix, internal microcracking, scaling, and progressive surface deterioration occur [16,17]. Repeated cycles also increase pore connectivity and facilitate further moisture ingress, which accelerates damage accumulation and loss of mechanical integrity [16,18]. For this reason, freeze–thaw attack is widely regarded as one of the most severe threats to the long-term performance of concrete pavements in cold regions [11].
Recent studies have shown that glass-based aggregates can improve the durability of cementitious composites under both thermal and freeze–thaw exposure when the mix design is properly controlled. In the case of elevated temperature, Zaetang et al. [19] reported that mortars incorporating auto glass waste sand retained significant residual strength after heating, with the WGA100 mixture reaching 66 MPa at 300 °C and maintaining 44.6 MPa at 600 °C, which was about twice the value of the control specimen at the same temperature. Under freeze–thaw conditions, Kim et al. [20,21] found that glass-containing concrete exhibited favorable durability indicators because of the low absorption capacity of the glass phase. Krstic et al. [16] further showed that freeze–thaw resistance in recycled-glass concrete is closely related to the pore structure and air-void system. In addition, Adhikary et al. [22] identified expanded glass aggregate as a promising material for frost-resistant concrete applications. These findings indicate that the low water absorption of glass, reduced freezable water, controlled pore structure, and matrix quality are key factors in the durability of glass-containing cementitious composites [16,20,22,23].
Because windshield glass aggregate (WGA) is a soda–lime silicate material containing amorphous silica, the potential risk of alkali–silica reaction (ASR) should also be considered, particularly at high glass replacement levels [6]. Waste glass used as sand in cementitious materials may produce deleterious expansion if reactive silica, sufficient alkalis, and moisture are simultaneously present; therefore, ASR risk cannot be excluded only on the basis of short-term mechanical or freeze–thaw results [24]. Previous studies have shown that the use of supplementary cementitious materials can mitigate ASR expansion by reducing alkali availability, binding alkalis within hydration products, and refining the pore structure [25]. In the present mixtures, blast furnace slag (BFS) may therefore contribute to lowering ASR susceptibility; however, this effect was not directly verified because accelerated mortar-bar, concrete-prism, or long-term expansion tests were not performed. Accordingly, the results of this study should be interpreted as durability performance under elevated-temperature and freeze–thaw exposure, while the long-term ASR safety of high WGA replacement levels requires dedicated verification.
On this basis, the present study investigates the durability of self-compacting sand concrete (SCSC) incorporating WGA as a volumetric replacement for natural sand and BFS as filler. The study is a continuation of previous work by the authors, Beladzar et al. [26], on the same SCSC mixture family, in which fresh-state behavior, mechanical properties, water absorption, porosity, ultrasonic pulse velocity, and pre-exposure SEM observations were evaluated. In the present work, the focus is shifted toward residual durability under two severe exposure conditions: elevated temperature and freeze–thaw cycling. Eleven mixtures were examined, including a control mixture and ten mixtures in which natural sand was replaced by WGA from 10% to 100% in 10% increments. The objective is to evaluate mass stability, residual compressive strength (RCS), residual flexural strength (RFS), and surface condition after thermal and freeze–thaw exposure.

2. Materials and Methods

2.1. Raw Materials

The SCSC investigated in this study was produced using CEM II/B-L 42.5 N ordinary Portland cement (OPC) (MASCARA factory, Mascara, Algeria), BFS, natural dune sand, WGA, water, and a polycarboxylate-based superplasticizer (SP). The cement complied with NF EN 197-1 [27]. BFS obtained from the El Hadjar plant (Annaba, Algeria) was used as a mineral filler. The natural fine aggregate was a siliceous dune sand collected from southern Algeria, with a maximum particle size of 4 mm. WGA was prepared from discarded laminated automobile windshields collected and processed in the Materials and Environment laboratory of Yahia Fares University of Medea, Medea, Algeria, and used as a volumetric replacement for natural sand. The windshield glass consisted of laminated glass layers separated by a polyvinyl butyral (PVB) interlayer (Figure 1). The chemical admixture used was a SP (Sika® ViscoCrete®-4037 RMX, Sika, Algiers, Algeria), compliant with NF EN 934-2 [28].
Figure 1. Laminated automobile windshield components.
Raw materials were characterized by X-ray diffraction (XRD), X-ray fluorescence (XRF), and scanning electron microscopy coupled with energy-dispersive spectroscopy (SEM/EDS). The main equipment used comprised a PANalytical Empyrean diffractometer (Almelo, The Netherlands), a PANalytical Zetium XRF spectrometer (Almelo, The Netherlands), and a Tescan MIRA 3 scanning electron microscope (Tescan, Brno, Czech Republic) equipped with an EDS analyzer (EDAX, Mahwah, NJ, USA) for SEM/EDS analyses. Additional physical characterization of the raw materials, including density, granulometry, fineness modulus, specific surface area, maximum particle size, sand equivalent, and water absorption, has been reported in the authors’ previous publication, Beladzar et al. [26] and is therefore not repeated here.
SEM analysis (Figure 2) revealed that the natural sand particles possess angular, irregularly shaped grains with rough surface textures and vary in size from 50 to 200 micrometers, while the WGA particles demonstrated smooth, glassy surface textures with characteristic conchoidal fracture patterns. XRD analysis (Figure 3) of the BFS confirms its predominantly vitreous nature, evidenced by a broad halo in the 2θ range of 24° to 32°, with detectable diffraction signals corresponding to gehlenite (2CaO·Al2O3·SiO2) and calcite (CaCO3). XRD characterization of the natural sand revealed major crystalline phases including quartz, albite, and microcline, confirming its essentially siliceous composition, whereas the XRD pattern of the WGA indicates a predominantly amorphous silica structure, characterized by a diffuse peak reaching approximately 2000 counts at 2θ ≈ 20°. Energy-dispersive X-ray spectroscopy (EDS) analysis (Figure 4) further confirmed the compositional differences among the raw materials. The natural sand was mainly composed of O (66.58 At.%, 54.15 Wt.%) and Si (21.19 At.%, 30.23 Wt.%), with minor amounts of Al, Fe, Na, Mg, Ca, and K and trace S, confirming its predominantly siliceous nature. The WGA exhibited a typical soda-lime silicate glass composition, mainly consisting of O (59.07 At.%, 45.60 Wt.%), Si (23.49 At.%, 31.74 Wt.%), Na (10.84 At.%, 12.03 Wt.%), and Ca (3.58 At.%, 6.88 Wt.%), with minor Mg, Al, and K. The BFS was mainly composed of O (61.46 At.%, 43.14 Wt.%), Ca (19.43 At.%, 32.32 Wt.%), and Si (11.81 At.%, 14.67 Wt.%), together with lower amounts of Al and Mg and minor Mn, Ti, K, S, and Na. Figure 5 also shows the oxide composition of the raw materials.
Figure 2. SEM images of sand (a) and WGA (b).
Figure 3. XRD analysis of (a) sand, (b) BFS, and (c) WGA.
Figure 4. EDS analysis of (a) sand, (b) WGA, and (c) BFS.
Figure 5. XRF analysis of (a) sand, (b) WGA, (c) BFS, and (d) cement.

2.2. Mixture Proportions

Eleven SCSC mixtures were prepared, and their exact proportions are detailed in Table 1. One mixture served as the control and contained only natural sand, whereas in the remaining ten mixtures, WGA replaced natural sand by volume at levels of 10, 20, 30, 40, 50, 60, 70, 80, 90, and 100%. A constant water-to-binder ratio (w/b) of 0.44 was adopted for all formulations. The SP dosage, expressed as a percentage by mass of binder, was adjusted for each mixture to maintain the required self-compacting behavior. The fresh-state workability of the same SCSC mixture family was previously evaluated using the mini-slump flow test, and has been reported in the authors’ previous publication [26]. The measured flow diameter values indicate that all mixtures remained within the target flow range of the adopted SCSC design approach.
Table 1. Mix proportions.

2.3. Mixing, Casting, and Curing

The reference SCSC mixture was designed according to the mix design methodology established by the national SABLOCRETE project [29]. Mixing was carried out under laboratory conditions at 20 ± 2 °C and 50–60% relative humidity using a 1.6 L laboratory mixer (Matest, Treviolo, Italy). The sample preparation procedure is shown in Figure 6. The dry constituents were first blended, after which the mixing water and SP were added, and mixing was continued until a homogeneous fresh mixture was obtained. The fresh concrete was then cast into prismatic molds measuring 40 × 40 × 160 mm. The specimens were demolded after 24 h and stored in water for 90 days at approximately 20 °C until the test age.
Figure 6. Sample preparation procedure.

2.4. Testing

For each mixture and each exposure condition, three prismatic specimens were tested. The values reported for mass loss, compressive strength, flexural strength, residual compressive strength (RCS), and residual flexural strength (RFS) correspond to the average of three specimens. Standard deviations were calculated and are reported as error bars in the corresponding figures.

2.4.1. Exposure to Elevated Temperatures

The resistance of SCSC to elevated temperatures was evaluated on prismatic specimens measuring 40 × 40 × 160 mm using a 9 L capacity laboratory muffle furnace (LT 9/11 SKM, Nabertherm, Lilienthal, Germany), capable of reaching 1100 °C within 90 min. The test procedure was conducted in accordance with RILEM TC 129-MHT [30]. Before thermal exposure, the specimens were oven-dried at 80 °C for 48 h to reduce internal moisture and minimize the risk of thermal spalling. They were then stored under laboratory conditions for 24 h before testing.
For the heating test, the specimens were placed inside the furnace with adequate spacing to ensure uniform heat distribution. The temperature increased at a constant rate of 10 °C/min until reaching the target temperatures of 200, 400, 600, or 800 °C, as shown in Figure 7. Each target temperature was maintained for 1 h to ensure thermal equilibrium between the specimen surface and core.
Figure 7. Time–temperature curves for different heating temperatures. The vertical dashed lines indicate the end of the 60-min holding period for each temperature profile.
After the thermal exposure period, the furnace was switched off, and the specimens were allowed to cool naturally to room temperature inside the closed chamber. After cooling, the visual appearance of the specimens was recorded, and their residual properties were evaluated in terms of mass loss, flexural strength, and compressive strength. Mechanical tests were carried out using a 2000 kN hydraulic press (UTEST, Ankara, Turkey), following a procedure adapted from EN 196-1 [31] (Figure 8).
Figure 8. Experimental setup and testing workflow for the elevated temperature resistance assessment.
For each temperature level, mass loss, residual compressive strength (RCS), and residual flexural strength (RFS) were determined using the following relationships:
M A S S   L O S S % = M 1 − M 2 M 1 × 100
R C S   ( % ) = R C 2 R C 1 × 100
R F S   ( % ) = RF 2 RF 1 × 100
where:
  • M1: mass of the specimen before heating (kg);
  • M2: mass of the specimen after heating (kg);
  • RCS: residual compressive strength (%);
  • RC1: compressive strength of the specimen before heating (MPa);
  • RC2: compressive strength of the specimen after heating (MPa);
  • RFS: residual flexural strength (%);
  • RF1: flexural strength of the specimen before heating (MPa);
  • RF2: flexural strength of the specimen after heating (MPa).

2.4.2. Freeze–Thaw Test

Freeze–thaw resistance was evaluated on 40 × 40 × 160 mm prismatic specimens after 90 days of curing in water. A climatic chamber with microprocessor temperature control for automatic execution of set cycles (C314/315+C315-02, Matest, Treviolo, Italy) was used. The procedure followed the European standards NF P 18-424 [32] and NF P 18-425 [33]. The specimens were subjected to 240 freeze–thaw cycles between −18 °C and +9 °C as shown in Figure 9.
Figure 9. Temperature profile of a single freeze–Thaw Cycle. The horizontal dashed line indicates the 0 °C threshold (freezing point), while the vertical dashed lines delineate the time intervals for each phase of the cycle.
Before the start of the test, the specimens were immersed in tap water for three days to obtain a saturated condition. After this conditioning period, excess surface water was removed using a fabric, and the saturated-surface-dry mass was recorded as M1. The specimens were then placed in the climatic chamber and remained submerged in water during the freeze–thaw cycles. After 240 cycles, the specimens were removed from the water, excess surface water was again removed using a fabric, and the final saturated-surface-dry mass was recorded as M2. Surface scaling was not collected separately. Therefore, the reported mass loss corresponds to the mass difference in the whole specimen before and after cycling. Mass measurements were performed using a balance with a readability of 0.01 g.
At the end of the cycling program, durability was evaluated through visual inspection, mass loss, flexural strength, and compressive strength. Mechanical tests were carried out using a 2000 kN hydraulic press (UTEST, Ankara, Turkey), following a procedure adapted from EN 196-1 [31] (Figure 10).
Figure 10. Experimental setup and testing workflow for the freeze–thaw durability assessment.

3. Results

3.1. Residual Properties After Exposure to Elevated Temperatures

3.1.1. Mass Loss

The mass loss of the SCSC mixtures increased progressively with increasing exposure temperature, as shown in Figure 11. After exposure to 200 °C, the mass loss ranged from 2.55% to 4.02%. At this temperature level, the reduction in mass can be mainly attributed to the evaporation of capillary and free water, together with the progressive removal of physically bound water from the cementitious matrix [19]. A clear effect of WGA incorporation was observed, with higher replacement levels resulting in lower mass loss values. In particular, the control mixture (WGA0) exhibited the highest mass loss (4.02%), whereas WGA100 showed the lowest value (2.55%). This trend is associated with the very low water absorption capacity of WGA compared with natural sand, which limits the amount of evaporable water stored within the aggregate skeleton.
Figure 11. Mass Loss of SCSC mixtures after exposure to elevated temperatures.
At 400 °C, the mass loss ranged from 4.55% to 6.55%, indicating continued dehydration and the onset of more pronounced thermal decomposition within the hydrated cement paste. At 600 °C, the mass loss varied between 5.00% and 8.77%, while at 800 °C it reached 9.22% to 11.77%. This increase is consistent with the progressive dehydration/decomposition of hydration products, including C-S-H and portlandite, which are commonly reported as major sources of mass loss and property degradation in cement-based materials exposed to temperatures above approximately 400–600 °C [34]. The results also agree with recent observations on waste-glass concrete, where mass loss increased with increasing temperature and was mainly governed by dehydration and decomposition processes in the binder phase rather than by the glass aggregate itself. Therefore, as the exposure temperature increased, the cementitious matrix became the dominant contributor to mass reduction [35]. This interpretation agrees with the findings of Zaetang et al. [19], who reported limited mass loss of auto glass waste even at very high temperatures, indicating that the main source of mass reduction in cement-based composites is the binder phase. Similar conclusions were reported by Kodur and Sultan [36], who observed that siliceous aggregates show only limited mass change under high-temperature exposure. Therefore, the present data should be interpreted mainly in terms of cement-matrix dehydration and decomposition, with the aggregate phase playing an indirect role through its absorption, thermal compatibility and interface characteristics.
The results also indicate that the beneficial effect of WGA on mass retention was more pronounced at lower temperatures than at higher temperatures. Between 400 °C and 800 °C, the differences among mixtures became less marked, suggesting that once dehydration and decomposition of the binder dominate the response, the role of aggregate water absorption becomes less influential. This behavior is in agreement with the observations of Xing et al. [37], who showed that aggregate absorption strongly influences mass loss at moderate temperatures, whereas at higher temperatures the thermally induced degradation of the matrix becomes the governing factor.
Overall, the reduction in mass loss with increasing WGA content can be attributed to the fact that glass particles have negligible porosity and extremely low water absorption. This physical barrier prevents moisture from being stored within the aggregate itself. The use of BFS promotes a more compact and refined cementitious matrix. This densification significantly limits the pathways for moisture ingress and the redistribution of water within the pores.

3.1.2. Compressive Strength and Residual Compressive Strength

The compressive strength and RCS results shown in Figure 12 and Figure 13 indicate that the thermal response of the SCSC mixtures depended strongly on the WGA replacement level. At room temperature, the mixtures already exhibited high compressive strength, and the highest absolute strength before heating was recorded for WGA20. Therefore, the unheated condition remained the reference state with the highest strength for many mixtures. However, the effect of heating was not uniform. While the control mixture and the mixes with low WGA contents generally lost strength progressively as temperature increased, the mixtures with high WGA contents, particularly WGA80–WGA100, showed a markedly better response at moderate temperature and retained substantially more strength at severe temperature.
Figure 12. Compressive strengths before and after exposure to high temperatures.
Figure 13. RCS after exposure to high temperatures.
After exposure to 200 °C, only limited changes in compressive strength were observed. For the control mixture and most mixtures containing up to 70% WGA, the strength remained close to the corresponding 25 °C value, with only a slight reduction. This behavior is consistent with the fact that, at relatively moderate temperatures, the dominant processes are mainly the evaporation of free water and the removal of physically bound water, whereas severe decomposition of the cement hydration products has not yet become dominant [12,13,38]. In addition, moderate heating may promote further drying of the matrix without causing severe internal cracking, which helps preserve compressive strength [12,39,40]. The WGA-rich mixtures showed the most favorable response at this stage, with compressive strengths approaching, and in the highest-replacement mixtures slightly exceeding, their corresponding room-temperature values. This more stable response can be attributed to the low water absorption of WGA, which reduces internal vapor-pressure build-up during heating [19,26,39,40,41].
A clearer separation among mixtures appeared after exposure to 400 °C. At this temperature, the control mixture and the mixtures with low and intermediate WGA content remained below their corresponding room-temperature strengths. By contrast, the mixtures with high WGA contents showed a distinct improvement, and WGA80, WGA90, and WGA100 exhibited compressive strengths higher than those measured at 25 °C, with WGA100 reaching about 96 MPa and an RCS of about 110.34%. Strength gains after moderate heating have been reported in some cement-based and glass-containing systems and are commonly related to drying-induced stiffening, limited continued hydration of unhydrated cement, thermal activation of the binder phase, or changes in the paste–aggregate interface before severe decomposition begins [38,42,43]. For glass-containing concretes, Ling et al. [41], Zaetang et al. [19] and Bisht et al. [44] also reported improved post-heating mechanical performance when recycled glass or auto-glass sand was incorporated.
At 600 °C, a pronounced reduction in compressive strength occurred for all mixtures, confirming the onset of severe thermal degradation. The sharp loss at this stage is consistent with portlandite dehydroxylation, progressive damage to C-S-H/C-A-S-H type hydrates, coarsening of the pore structure, and the development of microcracks in the matrix and ITZ [13,14,15,34,45]. For Portland cement paste, C-S-Hdehydration occurs over a broad temperature range, whereas portlandite decomposition is commonly reported around 400–550 °C; these transformations increase porosity and reduce the load-bearing capacity of the binder phase [46]. Nevertheless, the detrimental effect of temperature was mitigated as WGA content increased. The control mixture retained only about 31 MPa, whereas WGA100 maintained about 50 MPa. The RCS followed the same pattern, increasing progressively with increasing WGA replacement level. The result suggests that replacing natural sand with WGA changed the thermal response of the aggregate skeleton and paste–aggregate interface. Similar observations were reported by Khan and Sarker [38], who found that mortars containing waste glass fine aggregate showed high resistance after 200–800 °C exposure and, based on microstructural observations, exhibited fewer microcracks and improved ITZ bonding after heating.
After exposure to 800 °C, all mixtures experienced severe deterioration, and this temperature produced the lowest compressive strengths and RCS in the entire test series. The control mixture retained only about 23 MPa, whereas WGA100 still maintained about 39 MPa, confirming that WGA-rich mixtures retained a clear advantage even under extreme thermal loading. At this temperature, extensive decomposition of the hydrated cement matrix, coalescence of thermally induced microcracks, and major disruption of the paste–aggregate system become dominant [13,14,15]. In addition, the behavior of soda–lime windshield glass must be considered. Soda–lime silicate glasses undergo a transition from rigid glassy behavior to increasingly viscous behavior over the glass-transition/softening range; therefore, at 600–800 °C, WGA may experience thermal expansion, structural relaxation, and local viscous softening depending on its exact composition [47]. This may have two opposite effects: partial viscous relaxation or local filling of microvoids may improve stress redistribution in some regions, but thermal expansion mismatch between glass and cement paste, followed by cooling, can also generate residual stresses and ITZ microcracking [42,47].
Overall, the results demonstrate that incorporating WGA improved the compressive performance of SCSC after thermal exposure, although the magnitude of the benefit depended on both temperature and replacement ratio. The most favorable post-heating response was observed for mixtures containing 80–100% WGA, particularly at 400 °C, where the compressive strength exceeded the corresponding room-temperature value. At 600 °C and 800 °C, all mixtures deteriorated substantially, but WGA-rich mixtures consistently retained more strength than the control mixture. Further post-exposure SEM/EDS, XRD, TGA, or pore-structure analysis would be required to directly confirm the evolution of the ITZ, hydration products, and crack network after thermal exposure.

3.1.3. Flexural Strength and Residual Flexural Strength

The flexural strength and RFS of the SCSC mixtures after exposure to elevated temperatures are presented in Figure 14 and Figure 15. At 25 °C, the flexural strength did not increase continuously with WGA content. Instead, the initial flexural strength increased from the control mixture to WGA20, which exhibited the highest value, and then decreased progressively with further increase in WGA replacement up to WGA100. In the unheated state, the reduction in flexural strength at high WGA contents may be associated with the smooth glass surface and possible weakening of the paste–aggregate bond, despite the angular morphology of WGA particles [5,26]. After heating, however, the response changed substantially. At 200 °C and 400 °C, and more moderately at 600 °C and 800 °C, flexural strength generally increased with increasing WGA content, with the highest post-heating values recorded for the WGA-rich mixtures. The RFS values shown in Figure 15 confirm that the strongest residual response occurred at moderate temperature, especially around 400 °C, whereas the residual ratios decreased at 600 °C and 800 °C as thermal damage became dominant.
Figure 14. Flexural strengths before and after exposure to high temperatures.
Figure 15. RFS after exposure to high temperatures.
After exposure to 200 °C, the flexural strength of the control mixture was lower than its corresponding 25 °C value, whereas the mixtures containing high WGA contents showed improved residual flexural performance. At this temperature, the main thermal processes are evaporation of free water and loss of weakly bound water, while extensive decomposition of hydrated phases has not yet become dominant [12,13]. Moderate heating can therefore reduce internal moisture and promote a temporary dry-hardening effect without causing severe microstructural damage, a behavior also reported for other cementitious systems exposed to moderate temperatures [39,40,45,48,49]. For the present mixtures, the favorable response of the WGA-rich concretes is attributed primarily to the low water absorption of the glass aggregate, which limits moisture-related internal pressure during heating, together with the generally refined BFS-containing matrix.
At 400 °C, the same trend became more pronounced. WGA100 reached about 15 MPa, corresponding to an RFS of about 166.7%, which was the highest residual flexural value among the heated specimens. This increase may reflect a combination of drying-induced densification, further hydration or thermal activation of unhydrated cementitious phases, reduced moisture-related cracking due to the low absorption of WGA, and the presence of a BFS-containing matrix [39,40,45,48,49].
When the temperature increased to 600 °C, a marked reduction in flexural strength occurred for all mixtures compared with the values at 200 and 400 °C. Nevertheless, the beneficial effect of increasing WGA content remained clear. The control mixture retained only about 6 MPa, whereas WGA100 maintained about 12 MPa, corresponding to an RFS of about 133.3%. The reduction at 600 °C is consistent with the onset of severe thermal degradation of the hydrated cement matrix, including portlandite decomposition, progressive C-S-H degradation, and the development of microcracks in the matrix and ITZ [13,14,15]. Because flexural behavior is strongly controlled by crack initiation and propagation, it is particularly sensitive to thermally induced microcracking. The higher flexural strength of WGA-rich mixtures at this temperature may be related to the thermal response of the glass-containing aggregate skeleton and the interface, but this interpretation remains indirect in the absence of post-exposure microstructural observations.
After exposure to 800 °C, all mixtures exhibited lower flexural strengths than at 200 and 400 °C, confirming severe thermal damage and loss of matrix cohesion. The control mixture showed the lowest flexural strength, whereas WGA100 still retained about 10 MPa, corresponding to an RFS of about 111.1%. At this temperature, the behavior of soda–lime windshield glass becomes particularly relevant. Soda–lime silicate glass may undergo structural relaxation and local viscous softening in the high-temperature range, while the surrounding cementitious matrix experiences extensive dehydration and cracking [47]. This can produce competing effects: local softening or re-solidification of glass may partly fill microvoids or relax stresses in some regions, whereas thermal expansion mismatch between glass and paste during heating and cooling may also promote residual stresses and ITZ microcracking [47,50]. Therefore, the residual flexural performance of WGA-rich mixtures at 800 °C should be regarded as the net result of several competing mechanisms rather than as direct evidence of improved post-heating microstructure.
Overall, the flexural results show that WGA had a more favorable effect after heating than under unheated conditions. At 25 °C, WGA20 showed the highest flexural strength, whereas at elevated temperatures the highest absolute flexural strengths were generally obtained for mixtures with high WGA contents, especially WGA100. These findings support the use of WGA for improving residual flexural performance after heating, while the proposed mechanisms should be verified in future work using post-heating microstructural and porosity analyses.

3.2. Residual Properties After Freeze–Thaw Cycles

3.2.1. Surface Appearance After Freeze–Thaw Cycling

The visual condition of the specimens after freeze–thaw exposure is shown in Figure 16. No major visible changes were observed in any of the mixtures during the early stages of cycling, regardless of the WGA replacement ratio. After 240 freeze–thaw cycles, slight surface deterioration and the appearance of a limited number of surface voids were detected. The damage was mainly superficial; no severe spalling, corner loss or wide visible cracking was observed. However, the extent of visible surface alteration differed among mixtures. The control mixture exhibited the highest number of surface defects and the most noticeable surface change, whereas the mixtures containing WGA showed less visible deterioration. Among them, WGA100 displayed the most stable surface appearance after cycling. This observation is consistent with the freeze–thaw mechanism reported for cement-based materials, in which surface scaling and pore opening develop when cyclic freezing of absorbed water generates hydraulic, crystallization and fatigue-related stresses that exceed the local tensile resistance of the surface mortar [16,18,51].
Figure 16. Surface appearance before and after freeze–thaw cycling.
These observations indicate that WGA incorporation improved the resistance of SCSC to freeze–thaw-induced surface distress. The improvement is attributed primarily to the very low water absorption of WGA compared with natural sand, which limits the amount of water retained in the aggregate phase and reduces the potential for local frost-related pressure development [26]. A secondary contribution may come from the BFS-containing cementitious matrix, because slag-based binders can refine the pore structure and reduce transport pathways when curing is sufficient [52]. However, since BFS was kept constant in all mixtures, the progressive reduction in visible deterioration from WGA0 to WGA100 should be assigned mainly to the replacement of natural sand by WGA rather than to a varying BFS effect.
The results are consistent with previous studies on glass-containing concretes, where satisfactory freeze–thaw resistance was linked to limited water uptake, controlled pore structure, and stable mass or dynamic modulus after cycling [16,20,21]. However, this interpretation should be limited to the visible external condition of the specimens. Visual inspection is a qualitative indicator and cannot exclude the presence of internal microcracking or changes in the pore network. Previous freeze–thaw studies have shown that internal damage may develop in the cement paste and ITZ even when surface scaling remains limited, and that techniques such as dynamic modulus monitoring, X-ray microtomography, SEM, or MIP are more suitable for quantifying internal deterioration [16,53].

3.2.2. Mass Loss After Freeze–Thaw Cycling

The mass loss after freeze–thaw cycling is presented in Figure 17. After 240 cycles, the mass loss ranged from approximately 0.05% to 0.76%, with the highest value recorded for the control mixture and the lowest value recorded for WGA100. All mixtures therefore remained below 1% mass loss, indicating limited freeze–thaw surface deterioration under the present testing conditions. However, the trend is clear: replacing natural sand with WGA substantially reduced the amount of material lost during cyclic freezing and thawing.
Figure 17. Percentage of mass loss in the specimens subjected to freeze–thaw cycles.
The low mass-loss values are consistent with the visual observations reported in Figure 16, where no severe surface scaling or spalling was observed after 240 cycles. In the previous study by the authors, Beladzar et al. [26], on the same SCSC mixture family, increasing the WGA content was associated with lower water absorption and porosity of the hardened material, and SEM observations indicated a more compact pre-exposure microstructure and improved ITZ quality in WGA-containing mixtures. These characteristics can reduce water transport and limit the amount of freezable water in the connected pore system, thereby decreasing the likelihood of surface scaling and particle detachment during repeated freezing and thawing [16,21,53,54]. A secondary contribution may arise from the BFS-containing matrix, which can refine pore structure and reduce transport pathways when sufficiently cured [52]. Because BFS was constant in all mixtures, the monotonic decrease in mass loss with increasing WGA content should be assigned mainly to the replacement of natural sand by low-absorption WGA rather than to a varying BFS effect.

3.2.3. Compressive and Flexural Strength After Freeze–Thaw Cycling

Figure 18 presents the compressive strength of the SCSC mixtures before and after 240 freeze–thaw cycles. The results indicate that mixtures containing higher WGA contents, especially those exceeding 80% replacement, showed better post-freeze–thaw mechanical performance than both the control mixture and mixtures with lower WGA replacement ratios. After 240 cycles, the mixture with 100% WGA replacement retained the highest compressive strength, about 85 MPa, whereas the control mixture recorded about 76 MPa. This difference indicates that WGA-rich mixtures maintained their load-bearing capacity more effectively after repeated freezing and thawing.
Figure 18. Compressive strength after exposure to freeze–thaw cycles.
The improved compressive response of WGA-rich mixtures can be explained mainly by the hardened-state characteristics previously reported for the same mixture family. In a previous study by the authors, Beladzar et al. [26] reported that increasing WGA content was associated with lower water absorption and porosity, and SEM observations indicated a more compact pre-exposure microstructure and improved ITZ quality in selected WGA-containing mixtures. These characteristics can reduce the amount and mobility of freezable water in the composite, thereby limiting hydraulic pressure, crack propagation, and strength loss during repeated freezing and thawing [16,20,21,54]. The BFS-containing matrix may also contribute through pore refinement and reduced transport pathways, but BFS was kept constant in all mixtures; therefore, the differences among WGA replacement levels are mainly associated with the replacement of natural sand by WGA. Nevertheless, because no SEM/EDS, MIP, air-void analysis, or relative dynamic modulus measurements were performed after freeze–thaw cycling in the present study, this explanation should be considered indirect and cannot be used as direct proof of post-exposure matrix densification.
Figure 19 presents the flexural strength of the SCSC mixtures after 240 freeze–thaw cycles in comparison with the corresponding unexposed specimens. The incorporation of WGA improved the residual flexural performance, and the effect became more pronounced at high replacement levels. The mixture with 100% WGA achieved the highest post-cycling flexural strength, about 14 MPa, whereas the control mixture recorded about 4.9 MPa. Because flexural strength is highly sensitive to surface flaws, microcracking and ITZ quality, this result is consistent with the limited surface deterioration observed in Figure 16 and with the low mass-loss values measured after cycling.
Figure 19. Flexural strength after exposure to freeze–thaw cycles.
The high post-cycling flexural strength of WGA-rich mixtures may be related to the combined contribution of the WGA skeleton and the pre-existing quality of the paste–aggregate interface. The previous SEM observations on the same material family showed fewer voids and a stronger ITZ in WGA-containing SCSC before environmental exposure [26]. Such an ITZ can delay crack initiation and crack propagation under bending after freeze–thaw cycling. In addition, the angular and faceted morphology of WGA particles may contribute to mechanical interlocking with the surrounding matrix, although this effect must be balanced against the generally smooth glass surface, which can weaken bonding in some glass-aggregate concretes [5,21]. Similar relationships between glass aggregate use, low water absorption, reduced freeze–thaw mass loss, and improved post-exposure mechanical performance have been reported for waste-glass concrete systems [21,55].
Overall, the compressive and flexural strength results indicate that WGA-containing SCSC mixtures exhibited better post-freeze–thaw mechanical performance than the control mixture under the adopted test conditions. Among the studied mixtures, WGA100 showed the highest post-cycling compressive and flexural strengths. However, this should not be generalized as proof that 100% WGA is universally optimal for all performance requirements. The technical optimum should also consider fresh-state behavior, room-temperature mechanical performance, long-term ASR risk, and durability indicators not measured in this study, including relative dynamic modulus, air-void characteristics, and post-exposure microstructural damage.

4. Conclusions

Based on the experimental results obtained for SCSC incorporating WGA as a natural-sand replacement and BFS as a constant filler component, the following conclusions can be drawn:
  • The incorporation of WGA improved the measured durability-related responses of SCSC under both elevated-temperature exposure and freeze–thaw cycling, with the benefit becoming more pronounced at high replacement levels, particularly WGA80-WGA100.
  • Under elevated temperatures, mass loss increased for all mixtures as the temperature rose from 200 to 800 °C, but increasing WGA content reduced the magnitude of this loss, especially at low and moderate temperatures, due to the low water absorption of the glass aggregate.
  • The most favorable residual compressive and flexural response after heating was observed for WGA-rich mixtures, especially WGA80–WGA100. At 400 °C, WGA100 reached about 96 MPa in compressive strength and about 15 MPa in flexural strength, corresponding to residual values of about 110.34% and 166.7%, respectively.
  • At 600 and 800 °C, all mixtures showed substantial deterioration in compressive and flexural performance. Nevertheless, WGA-rich mixtures consistently retained higher residual strengths than the control mixture, indicating better retention of mechanical capacity after severe thermal exposure.
  • After 240 freeze–thaw cycles, all mixtures remained below 1% mass loss, with the values decreasing from approximately 0.76% for WGA0 to approximately 0.05% for WGA100. Visual inspection confirmed only limited surface deterioration, with no severe spalling, corner loss, or wide visible cracking.
  • The highest post-freeze–thaw mechanical performance was recorded for WGA100, which reached about 85 MPa in compressive strength and about 14 MPa in flexural strength after 240 cycles, compared with about 76 MPa and 4.9 MPa, respectively, for the control mixture.
  • Overall, recycled windshield glass aggregate can be considered a promising alternative to natural sand for producing more sustainable SCSC with improved performance under the specific thermal and freeze–thaw exposure conditions investigated in this work. However, future studies should include post-exposure microstructural characterization, pore-structure analysis, relative dynamic modulus measurements, and dedicated ASR expansion tests to verify the long-term safety of high WGA replacement levels.

Author Contributions

Conceptualization, Z.B., D.B., M.G. and M.V.; methodology, Z.B., D.B. and M.G.; validation, Z.B., D.B. and M.G.; investigation, Z.B. and S.M.N.; resources, D.B., M.G. and M.V.; data curation, Z.B. and S.M.N.; writing—original draft preparation, Z.B., S.M.N. and I.B.; writing—review and editing, Z.B., S.M.N. and I.B.; supervision, D.B., M.G. and M.V.; project administration, D.B., M.G. and M.V. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Institutional Review Board Statement

Not applicable.

Data Availability Statement

The data presented in this study are available in this article.

Acknowledgments

The authors acknowledge Tommaso Pini for his assistance with the EDS analyses.

Conflicts of Interest

The authors declare no conflicts of interest.

Abbreviations

The following abbreviations are used in this manuscript:
SCSCSelf-Compacting Sand Concrete
WGAWindshield Glass Aggregate
BFSBlast Furnace Slag
PVBPolyvinyl Butyral
XRDX-ray Diffraction
XRFX-ray Fluorescence
SEMScanning Electron Microscopy
EDSEnergy-Dispersive X-ray Spectroscopy
w/bWater-to-Binder Ratio
RCSResidual Compressive Strength
RFSResidual Flexural Strength
OPCOrdinary Portland Cement
SPSuperplasticizer
C-S-HCalcium Silicate Hydrate
ASRAlkali-Silica Reaction
ITZinterfacial transition zone
TGAThermogravimetric Analysis
C-A-S-HCalcium Aluminosilicate Hydrate
MIPMercury Intrusion Porosimetry

References

  1. UNCCHL Champions. The Breakthrough Agenda Report 2023; IEA: Paris, France, 2023. [Google Scholar]
  2. Sambucci, M.; Nouri, S.M.; Tayebi, S.T.; Valente, M. Synergic Effect of Recycled Carbon Fibers and Microfibrillated Cellulose Gel for Enhancing the Mechanical Properties of Cement-Based Materials. Gels 2023, 9, 981. [Google Scholar] [CrossRef] [Scilit]
  3. Sambucci, M.; Biblioteca, I.; Valente, M. Life Cycle Assessment (LCA) of 3D Concrete Printing and Casting Processes for Cementitious Materials Incorporating Ground Waste Tire Rubber. Recycling 2023, 8, 15. [Google Scholar] [CrossRef] [Scilit]
  4. Al-Noaimat, Y.A.; Sambucci, M.; Chougan, M.; El-Seidy, E.; Biblioteca, I.; Valente, M.; Tirillo, J.; Al-Kheetan, M.J.; Ghaffar, S.H. Sustainable repurposing of polyvinyl chloride waste as aggregates in limestone-calcined clay cement. J. Clean. Prod. 2025, 491, 144862. [Google Scholar] [CrossRef] [Scilit]
  5. Afshinnia, K.; Rangaraju, P.R. Impact of combined use of ground glass powder and crushed glass aggregate on selected properties of Portland cement concrete. Constr. Build. Mater. 2016, 117, 263–272. [Google Scholar] [CrossRef] [Scilit]
  6. El-Seidy, E.; Chougan, M.; Sambucci, M.; Al-Kheetan, M.J.; Biblioteca, I.; Valente, M.; Hamidreza Ghaffar, S. Lightweight alkali-activated materials and ordinary Portland cement composites using recycled polyvinyl chloride and waste glass aggregates to fully replace natural sand. Constr. Build. Mater. 2023, 368, 130399. [Google Scholar] [CrossRef] [Scilit]
  7. Li, C.; Li, J.; Ren, Q.; Zheng, Q.; Jiang, Z. Durability of concrete coupled with life cycle assessment: Review and perspective. Cem. Concr. Compos. 2023, 139, 105041. [Google Scholar] [CrossRef] [Scilit]
  8. Adesina, A.; Zhang, J. Impact of concrete structures durability on its sustainability and climate resiliency. Next Sustain. 2024, 3, 100025. [Google Scholar] [CrossRef] [Scilit]
  9. Alexander, M.; Beushausen, H. Durability, service life prediction, and modelling for reinforced concrete structures–review and critique. Cem. Concr. Res. 2019, 122, 17–29. [Google Scholar] [CrossRef] [Scilit]
  10. de Silva, D.; Andreini, M.; Bilotta, A.; De Rosa, G.; La Mendola, S.; Nigro, E.; Rios, O. Structural safety assessment of concrete tunnel lining subjected to fire. Fire Saf. J. 2022, 134, 103697. [Google Scholar] [CrossRef] [Scilit]
  11. Luo, S.; Bai, T.; Guo, M.; Wei, Y.; Ma, W. Impact of freeze–thaw cycles on the long-term performance of concrete pavement and related improvement measures: A review. Materials 2022, 15, 4568. [Google Scholar] [CrossRef] [Scilit]
  12. Lin, W.-M.; Lin, T.; Powers-Couche, L. Microstructures of fire-damaged concrete. Mater. J. 1996, 93, 199–205. [Google Scholar]
  13. Georgali, B.; Tsakiridis, P.E. Microstructure of fire-damaged concrete. A case study. Cem. Concr. Compos. 2005, 27, 255–259. [Google Scholar] [CrossRef] [Scilit]
  14. Liu, C.; Chen, J. High temperature degradation mechanism of concrete with plastering layer. Materials 2022, 15, 398. [Google Scholar] [CrossRef] [Scilit]
  15. Khoury, G.A. Effect of fire on concrete and concrete structures. Prog. Struct. Eng. Mater. 2000, 2, 429–447. [Google Scholar] [CrossRef] [Scilit]
  16. Krstic, M.; Davalos, J.F.; Rossi, E.; Figueiredo, S.C.; Copuroglu, O. Freeze–thaw resistance and Air-void analysis of concrete with recycled glass–Pozzolan using X-ray micro-tomography. Materials 2020, 14, 154. [Google Scholar] [CrossRef] [Scilit]
  17. M Al-Akhras, N. Performance of glass concrete subjected to freeze-thaw cycling. Open Constr. Build. Technol. J. 2012, 6, 392–397. [Google Scholar] [CrossRef] [Scilit]
  18. Yang, H.J.; Usman, M.; Hanif, A. Suitability of liquid crystal display (LCD) glass waste as supplementary cementing material (SCM): Assessment based on strength, porosity, and durability. J. Build. Eng. 2021, 42, 102793. [Google Scholar] [CrossRef] [Scilit]
  19. Zaetang, Y.; Lao-un, J.; Wongkvanklom, A.; Wongsa, A.; Sata, V.; Chindaprasirt, P. Fire-resistant and Thermal Insulation Improvements of Cement Mortar with Auto Glass Waste Sand. KSCE J. Civ. Eng. 2023, 27, 4032–4042. [Google Scholar] [CrossRef] [Scilit]
  20. Kim, J.; Moon, J.-H.; Shim, J.W.; Sim, J.; Lee, H.-G.; Zi, G. Durability properties of a concrete with waste glass sludge exposed to freeze-and-thaw condition and de-icing salt. Constr. Build. Mater. 2014, 66, 398–402. [Google Scholar] [CrossRef] [Scilit]
  21. Kim, I.S.; Choi, S.Y.; Yang, E.I. Evaluation of durability of concrete substituted heavyweight waste glass as fine aggregate. Constr. Build. Mater. 2018, 184, 269–277. [Google Scholar] [CrossRef] [Scilit]
  22. Adhikary, S.K.; Ashish, D.K.; Rudžionis, Ž. Expanded glass as light-weight aggregate in concrete—A review. J. Clean. Prod. 2021, 313, 127848. [Google Scholar] [CrossRef] [Scilit]
  23. Ramakrishnan, S.; Ramesh, A.; Pasupathy, K.; Mechtcherine, V.; Manalo, A.C.; Sanjayan, J. Enhancing the printability and sustainability of 3D concrete printing using recycled waste glass as a cement substitute. J. Sustain. Cem.-Based Mater. 2026, 1–12. [Google Scholar] [CrossRef] [Scilit]
  24. Du, H.; Tan, K.H. Use of waste glass as sand in mortar: Part II–Alkali–silica reaction and mitigation methods. Cem. Concr. Compos. 2013, 35, 118–126. [Google Scholar] [CrossRef] [Scilit]
  25. Thomas, M. The effect of supplementary cementing materials on alkali-silica reaction: A review. Cem. Concr. Res. 2011, 41, 1224–1231. [Google Scholar] [CrossRef] [Scilit]
  26. Beladzar, Z.; Boukhelkhal, D.; Guendouz, M.; Hadjadj, M. Contribution to the reinforcement of cement composites using aggregates from industrial windshield waste. Bud. I Archit./Civ. Archit. Eng. 2026, 25, 1–13. [Google Scholar] [CrossRef] [Scilit]
  27. BS EN 197-4:2004; Cement—Part 4: Composition, Specifications and Conformity Criteria for Common Cements. British Standard Institution: London, UK, 2004.
  28. BS EN 934-2; Admixtures For Concrete, Mortar and Grout—Part 2: Concrete Admixtures; Definitions, Requirements, Conformity, Marking and Labelling. British Standards Institution: London, UK, 2009.
  29. Sablocrete, S. Concrete: Characteristics and Use Practices; Presses de l’Ecole Nationale des Ponts et Chaussées LCPC: Paris, France, 1994. [Google Scholar]
  30. Rilem, T. Test methods for mechanical properties of concrete at high temperatures, Recommendations, Part 3: Compressive strength for service and accident conditions. Mater. Struct. 1995, 28, 410–414. [Google Scholar]
  31. EN 196-1:2016; Methods of Testing Cement—Part 1: Determination of Strength. CEN: Brussels, Belgium, 2016.
  32. Norme, P. P 18-424–Bétons–Essai de Gel Sur Béton Durci. Gel Dans L’eau–Dégel Dans L’eau; AFNOR: Paris, France, 1994. [Google Scholar]
  33. Bouteille, S. Outils de Caractérisation et Analyse du Comportement des Matériaux Cimentaires Soumis à des Cycles de Gel-Dégel en Présence de Sels; Université Paris-Est: Créteil, France, 2013. [Google Scholar]
  34. Alhamad, A.; Yehia, S.; Lublóy, É.; Elchalakani, M. Performance of Different Concrete Types Exposed to Elevated Temperatures: A Review. Materials 2022, 15, 5032. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  35. Wen, B.; Wang, H.; Gao, G.; Zhang, L.; Yu, Z.; Wang, Z. The Synergistic Utilization of Glass Aggregates and Glass Powder on the Thermal and Mechanical Properties of Concrete. Materials 2025, 18, 2405. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  36. Kodur, V.; Sultan, M. Effect of temperature on thermal properties of high-strength concrete. J. Mater. Civ. Eng. 2003, 15, 101–107. [Google Scholar] [CrossRef] [Scilit]
  37. Xing, Z.; Beaucour, A.-L.; Hebert, R.; Noumowe, A.; Ledesert, B. Aggregate’s influence on thermophysical concrete properties at elevated temperature. Constr. Build. Mater. 2015, 95, 18–28. [Google Scholar] [CrossRef] [Scilit]
  38. Khan, M.N.N.; Sarker, P.K. Effect of waste glass fine aggregate on the strength, durability and high temperature resistance of alkali-activated fly ash and GGBFS blended mortar. Constr. Build. Mater. 2020, 263, 120177. [Google Scholar] [CrossRef] [Scilit]
  39. Zemri, C.; Bachir Bouiadjra, M. Comparison between physical–mechanical properties of mortar made with Portland cement (CEMI) and slag cement (CEMIII) subjected to elevated temperature. Case Stud. Constr. Mater. 2020, 12, e00339. [Google Scholar] [CrossRef] [Scilit]
  40. Saeed, N.M.; Omer, B.; Jamal, A.S.; Dheyaaldin, M.H. Performance of cement mortar modified with GGBFS at elevated temperatures with various w/b ratios and superplasticizer dosages. Constr. Build. Mater. 2023, 368, 130493. [Google Scholar] [CrossRef] [Scilit]
  41. Ling, T.-C.; Poon, C.-S.; Kou, S.-C. Influence of recycled glass content and curing conditions on the properties of self-compacting concrete after exposure to elevated temperatures. Cem. Concr. Compos. 2012, 34, 265–272. [Google Scholar] [CrossRef] [Scilit]
  42. Terro, M.J. Properties of concrete made with recycled crushed glass at elevated temperatures. Build. Environ. 2006, 41, 633–639. [Google Scholar] [CrossRef] [Scilit]
  43. Morsy, M.; Rashad, A.; Shebl, S. Effect of elevated temperature on compressive strength of blended cement mortar. Build. Res. J. 2008, 56, 173–185. [Google Scholar]
  44. Bisht, K.; Ramana, P. Experimental investigation of strength, drying shrinkage, freeze and thaw and fire attack properties of concrete mixes with beverage glass waste as fine aggregate. In Structures; Elsevier: Amsterdam, The Netherlands, 2022; pp. 358–371. [Google Scholar]
  45. Pachta, V.; Anastasiou, E.K. Utilization of industrial byproducts for enhancing the properties of cement mortars at elevated temperatures. Sustainability 2021, 13, 12104. [Google Scholar] [CrossRef] [Scilit]
  46. Zhang, Q.; Ye, G. Dehydration kinetics of Portland cement paste at high temperature. J. Therm. Anal. Calorim. 2012, 110, 153–158. [Google Scholar] [CrossRef] [Scilit]
  47. Bansal, N.P.; Doremus, R.H. Handbook of Glass Properties; Elsevier: Amsterdam, The Netherlands, 2013. [Google Scholar]
  48. Tang, C.-W. Residual Mechanical Properties of Fiber-Reinforced Lightweight Aggregate Concrete after Exposure to Elevated Temperatures. Appl. Sci. 2020, 10, 3519. [Google Scholar] [CrossRef] [Scilit]
  49. Shumuye, E.D.; Zhao, J.; Wang, Z. Effect of fire exposure on physico-mechanical and microstructural properties of concrete containing high volume slag cement. Constr. Build. Mater. 2019, 213, 447–458. [Google Scholar] [CrossRef] [Scilit]
  50. Guo, M.-Z.; Chen, Z.; Ling, T.-C.; Poon, C.S. Effects of recycled glass on properties of architectural mortar before and after exposure to elevated temperatures. J. Clean. Prod. 2015, 101, 158–164. [Google Scholar] [CrossRef] [Scilit]
  51. Guo, J.; Sun, W.; Xu, Y.; Lin, W.; Jing, W. Damage mechanism and modeling of concrete in freeze–thaw cycles: A review. Buildings 2022, 12, 1317. [Google Scholar] [CrossRef] [Scilit]
  52. Özbay, E.; Erdemir, M.; Durmuş, H.İ. Utilization and efficiency of ground granulated blast furnace slag on concrete properties–A review. Constr. Build. Mater. 2016, 105, 423–434. [Google Scholar] [CrossRef] [Scilit]
  53. Tian, W.; Han, N. Evaluation of damage in concrete suffered freeze-thaw cycles by CT technique. J. Adv. Concr. Technol. 2016, 14, 679–690. [Google Scholar] [CrossRef] [Scilit]
  54. He, Y.; Zhang, J.; Jiang, Z.; Zhou, B.; Zheng, Z.; Wang, Y.; Lu, Q.; Huang, W. Evaluation of the freeze-thaw resistance of concrete incorporating waste rubber and waste glass. Compos. Commun. 2024, 50, 102020. [Google Scholar] [CrossRef] [Scilit]
  55. Mansour, M.A.; Ismail, M.H.B.; Imran Latif, Q.B.a.; Alshalif, A.F.; Milad, A.; Bargi, W.A.A. A Systematic Review of the Concrete Durability Incorporating Recycled Glass. Sustainability 2023, 15, 3568. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.