Abstract
This study investigated the properties of a composite NiCrFeSiB coating with fine-dispersed WC additives, deposited by the HVOF method. The NiCrFeSiB powder alloy with WC additives was applied to a steel substrate. The WC content in the coating was 10, 15, and 20% by weight. The particle size distribution of the mixture ranged from 3 to 10 µm. The WC used was the WC8 alloy (92% WC, 8% Co). The levels of stress, phase composition, hardness, wear resistance, and coating structure were investigated. The studies revealed that the structure was primarily composed of the γ-Ni-Fe solid solution phase, with secondary phases including Ni3B, Fe3B, (Cr,)2B, and carbides of the W2C, WC, M7C3 type. A small amount of the initial WC particles was also present. The use of a fine-dispersed NiCrFeSiB powder mixture with WC particles resulted in a nearly twofold increase in hardness and wear resistance compared to the same parameters of the coating without WC. The coating with 20% WC exhibited the highest hardness. However, its wear resistance was lower than that of the coating with 15% WC. This fact could be explained by a slight difference in the phase composition and an increase in the proportion of the unsolidified WC phase in the structure. This led to the spalling of fine particles and a reduction in wear resistance. The study demonstrated the feasibility of using a fine-dispersed NiCrFeSiB coating with WC additives without additional remelting. Similar hardness and wear resistance results were achieved immediately after HVOF spraying when using a fine-dispersed NiCrFeSiB + 15% WC/Co mixture with a 92/8 composition. This simplification of the technology reduced the coating application process time. It also lowered production costs by eliminating the remelting stage.
Keywords:
coating; fine-dispersed mixture; NiCrFeSiB; WC; structure; phase composition; hardness; wear resistance 1. Introduction
The primary cause of failure in components operating under frictional conditions is the change in surface relief, which is associated with low wear resistance. To enhance surface properties, various coatings are increasingly being used. Coatings can be applied to impart or improve specific operational properties of the surface, restore damaged areas, and more. Various materials are employed as coatings, with the current trend being the incorporation of mixtures with different compositions including both metallic and ceramic components.
Ni-based coatings, which also contained Si, Cr, B, and C, exhibit excellent wear resistance and corrosion resistance. These properties contribute to their widespread application [1]. The NiSiCrB composite coating is relatively low-melting, which is facilitated by the presence of B. At the same time, the inclusion of Cr, Si, and C promotes the formation of hard dispersed phases such as carbides and silicides. Surfaces coated with NiSiCrB exhibit microhardness values ranging from 474 HV0.5 to 810 HV0.5, depending on the deposition method [2,3]. These studies note that microhardness and wear resistance increase after remelting. This is due to the formation of fine boride particles and carbides that do not dissolve in the matrix.
Consequently, a significant portion of the research on NiSiCrB-based coatings has been dedicated to studying the effect of reinforcing this mixture with hard, refractory particles such as WC, TiC, SiC, and others [4,5,6,7,8,9,10].
In references [4,5,6], the morphology, structure, and properties of NiSiCrB coatings with WC-Co additives, applied by the HVOF method, were studied. As a result of reinforcing the mixture with WC-Co particles, the hardness increased to 1200 HV0.3.
In references [7,8,9], the influence of SiC and TiC on the NiSiCrB composition was investigated. The authors confirmed a decrease in the wear rate and friction coefficient.
In references [10,11], the authors studied the effect of Al2O3 and CrC on the NiSiCrB composition, applied by the flame spraying method. It was noted that in the first case, the microhardness increased to 673 HV compared to the initial 451 HV. In the case of reinforcement with CrC, the wear rate, depending on the spraying conditions, decreased by 3 to 8 times compared to the initial steel matrix.
The authors of reference [12] evaluated the effectiveness of reinforcing NiSiCrB with various particles. The study was conducted under dry friction conditions using a NiSiCrB coating, into which particles of WC (50/50), NiCr (80/20), WC/Co (88/12), WC/CoCr, and Cr3C2/NiCr (75/25) were added. The coating was applied by the flame spraying method, with an Al2O3 disc used as the counterbody. The authors made this conclusion based on a comparison of the hardness, roughness, and friction coefficient measurements. It was found that the coating with WC/Co particles exhibited the highest wear resistance, second only to the coating containing WC/CoCr particles.
The results of studies on the properties of coatings consisting of NiCrBSi-WC and NiBSi-WC were provided by Abdullah Cahit Karaoglanli and in reference [13]. The coatings were applied using the arc spraying method. It was found that in both cases, the structure consisted of a solid solution of the NiCrW or NiW type and a hard carbide phase, WC or W2C. Part of the boron in both cases appeared as inclusions. Although the NiBSi–WC coating had lower hardness than the NiCrBSi-WC coating, it exhibited higher wear resistance under dry wear conditions. The authors explained this by the better adhesive bond with the matrix, due to the significant solubility of the carbide phase in the matrix.
In reference [14], the properties and structure of NiCrBSi coatings with various WC additions were also studied. The coating was applied by laser cladding. The WC content ranged from 0 to 50% by weight. It was found that a significant portion of WC was deposited at the bottom of the molten coating. This meant that the WC content increased with the coating depth, and the actual WC content on the surface differed from the initial composition. It was also established that wear resistance increased exponentially with WC content. However, an increase in WC in the initial mixture did not lead to a significant increase in hardness.
Reference [15] was dedicated to the study of the properties of NiCrBSi coatings with WC additions after remelting. The remelting process initiated the decarburization of WC, leading to the formation of dispersed W2C. These dispersed particles played a significant role in strengthening the coating. The authors showed that the hardness of NiCrBSi, NiCrBSi/WC coatings, and the post-remelting NiCrBSi/WC coating with W2C particles was 674, 785, and 1061 HV, respectively. Furthermore, remelting reduced porosity and, consequently, increased the coating density.
In reference [16], the aim of the study was to determine the effect of coating thickness on the resulting microstructure and tribological properties. The coating used was a mixture of AMDRY 1371 (Mo-NiCrFeBSi), which was applied by atmospheric plasma spraying (APS) onto steel samples. To find the optimal thickness of the AMDRY 1371 coating, the samples were coated with five, seven, and nine passes, referred to as 5 L, 7 L, and 9 L, respectively. The friction coefficient was approximately 0.3 for all samples. However, depending on the coating thickness, initial roughness, and microstructure, the final wear volumes and wear rates were significantly different. The wear test results showed that the coatings produced with seven passes exhibited the highest wear resistance. Thicker coatings had scratches due to the segregation of hard particle phases containing Fe, Cr, and B.
In reference [17], two coatings were studied: the high-entropy alloy CoCrFeMnNi0.8V and a mixture of CoCrFeMnNi0.8V with WC, to evaluate their potential as innovative surface coatings. The CoCrFeMnNi0.8V alloy exhibited a unique microstructure with enhanced hardness and wear resistance. The addition of WC-Co particles improved impact toughness and durability. The coatings were applied using high-velocity oxygen-fuel thermal spraying (HVOF) on a steel substrate. The CoCrFeMnNi0.8V coating demonstrated high corrosion resistance due to the formation of an oxide protective layer. The introduction of WC as a reinforcing element enhanced the wear resistance of the coating. Thus, the authors claimed that the composite coating, consisting of CoCrFeMnNi0.8V reinforced with WC, created a unique combination of properties. This combination provided high corrosion resistance and wear resistance to the surface.
In reference [8], the authors evaluated the abrasion wear resistance of NiCrBSiFe coatings with 40% SiC additives, applied by flame spraying. Coatings with a thickness of 420 µm were applied to AISI 1020 steel substrates. The powder used was the commercial powder Metco ML16-C (Ni16Cr4Si4B3Cu3Mo2.5Fe0.5C) with a particle size range of −125 to +53 µm. It was mechanically mixed for 2 h with medium-sized SiC powder (29 µm). It was found that the addition of 40% SiC led to a significant increase in hardness and wear resistance. The authors of the study noted an interesting fact, confirmed by X-ray analysis: the mass loss of the surface occurred due to the wear of eutectic phases such as Ni3Si2 and Ni3B, as well as the spalling of borides and carbides, while wear of the austenitic matrix γ-Ni was almost nonexistent.
In reference [18], NiCrBSi powder mixtures with the addition of WC were used as materials for cladding. The amount of WC additives was 30% and 40% by mass. The authors used a particle size of NiCrBSi powder in the range of 30~170 μm, and the average particle size was 79.6 μm. The particle size of WC powder was in the range of 65~235 μm, and the average particle size was 139.38 μm. Medium-carbon steel 42CrMo was used as the substrate. The results showed that various phases, such as γ (Fe/Ni), Fe-Ni, FeSi, Fe3C, and M7C3, formed in the cladding layer. These phases made up the main part of the layer. Secondary phases were formed on the surface of the cladded layer. These phases are the primary phases in the Ni/WC plasma cladding layer. Diffusion and deposition of elements occurred in the molten pool. Complex secondary phases formed in the surface layer. The surface with 30% WC addition showed lower values of hardness, wear resistance, and corrosion resistance.
In reference [19], the effect of the plasma arc current on the properties of NiCrBSi coating applied to a steel substrate using the powder arc welding method was investigated. During the microstructure analysis of the coating, two distinct zones were identified: the center of the coating and the coating/substrate interface. In both cases, the structure consisted of dendrites enriched with chromium. A current of 70 A was found to be optimal. At this current, both corrosion resistance and tribological properties were improved. The microhardness increased from 488 HV to 832 HV, which reduced the wear rate from 2.9 × 10−2 m3/m to 1.8 × 10−2 m3/m.
In reference [20], the authors investigated the effect of WC content in NiCrBSi coating on hardness and wear resistance. The WC content ranged from 35% to 70%. The coating was applied using the laser hardfacing method. It was found that the hardness of the coating remained almost unchanged when the WC content was increased up to approximately 60%. However, when the WC content was increased to 70%, the hardness of the coating rose significantly. The wear resistance of the coating improved only when the WC content in the mixture was up to 40%. The particle size of WC also influenced the properties of the coating. The hardness of the coating increased with the WC particle size. However, the highest wear resistance was achieved with the finest WC fraction in the studied range—20–53 µm. The authors explained this phenomenon by the better distribution of fine WC particles throughout the volume. Cutting tests showed that the smallest particle size (20–53 µm) of carbide powder resulted in the lowest values of cutting edge wear and mass loss. This was mainly due to the better distribution of tungsten carbide particles in the volume, as well as the matrix’s resistance to the deposition of the Ni4W phase.
The authors [21] studied the structure of a composite NiCrBSi coating applied by plasma spraying. The structure mainly consisted of two types of grains: grains of 200 nm and larger grains of 2–8 µm. The phase composition included carbide and boride phases such as Cr7C3, M7C23, and Ni3B, evenly distributed in the Ni solution matrix. The microhardness of the coating reached a maximum value of HV0.5 640, nearly 2.5 times higher than the microhardness of stainless steel. The friction coefficient decreased from approximately 0.45 to 0.38.
In reference [22], the friction and wear characteristics of NiCrBSiFeC-WC coating were investigated. The results showed that both NiCrBSiFeC and composite NiCrBSiFeC-WC coatings exhibited high hardness and wear resistance due to the formation of well-dispersed high-hardness phases.
In reference [23], the effect of a composite coating consisting of Inconel 718 and WC particles applied to copper plates was studied. The results showed that the Inconel 718/WC coating mainly consisted of a solid γ-Ni solution and various hardening carbide phases, such as MC, MC3, W3C, and W2C. The average microhardness of the coating reached 851.7 HV0.5, which was 11.5 times higher than the microhardness of the substrate (74 HV0.5). At 400 °C, the wear rate of the coating was 3.48 × 10−4 mm3·H−1·m−1, which was only 35.7% of the wear rate of the substrate. The authors explained the high performance of the coating by the simultaneous effects of grain refinement, solid solution strengthening, and second-phase hardening, represented by various hard carbides.
In reference [24], single-layer and three-layer coatings based on nickel (Ni-Si-Fe-B) were fabricated on a 316LSS steel substrate using the laser deposition method. The results showed that the microstructure of the cross-section of the three-layer coating significantly differed from that of the single-layer coating. This difference was attributed to the varying cooling rates. In the three-layer coating, the structure at the center was represented by equiaxed crystals. In contrast, the single-layer coating, even at the center, exhibited well-defined columnar dendrites. The phase composition of the coatings in both cases consisted of a solid γ-(Fe,Ni) solution and hard phases such as Ni17Si3, Cr5B3, and Ni3B. The presence of these phases led to a significant increase in the wear resistance of the coating, and the microhardness was almost 2.5 times higher than that of the substrate. The microhardness of the three-layer coating was, on average, 48 HV0.2 higher than that of the single-layer coating, despite having the same phase composition. The authors explained this by differences in the size and shape of the grains.
In reference [25], metal-ceramic coatings based on WC with a CoCrNiAlTi binder were fabricated on 0.4Cr13Ni5Mo stainless steel substrates. The atmospheric high-velocity air-fuel (HVAF) spraying method was used for deposition. The results showed that the WC-CoCrNiAlTi coatings mainly consisted of WC, (Co,Ni)3W3C, and a face-centered cubic (FCC) binder phase as the matrix. The properties and composition of the coating were significantly influenced by the AFR (air-to-fuel) ratio. As the AFR increased, the coating density improved. This was attributed to the better melting state of the particles and the increased flight speed, which led to better flattening upon impact. At the optimal AFR of 1.130, the coating demonstrated the lowest friction coefficient (0.6435) and wear rate (1.15 × 10−6 mm3·N−1·m−1), indicating a wear resistance 34.85 times higher than that of the stainless steel substrate.
The authors of reference [26] also observed the positive effect of MeC-type carbides on the hardness and wear resistance of the coating. The effect of NiCr and NiCr–TiC coatings, applied by laser hardfacing, was studied on martensitic stainless steel AISI 420. It was further noted that the hardness of the composite coating containing strengthening particles was much higher than that of the coating without such particles. This was due to the enhanced nucleation effect and the presence of TiC particles. It was also found that the weight loss of the NiCr-TiC composite coating was lower than that of NiCr and the stainless steel substrate, while its erosion resistance was higher compared to both NiCr and the steel substrate.
Despite the numerous studies on the effect of reinforcement of coatings with WC particles, many questions remain unresolved. Almost all authors of the reviewed studies recommend remelting the coating to improve its properties and reduce porosity. For reinforcement, a WC-Co (80/20) mixture was predominantly employed in quantities of 30% by mass, with particle sizes ranging from approximately 49 µm and larger. Such conditions for using WC in the NiCrBSiFe composition, in practice, led to a significant increase in the cost of the final product.
The aim of this study was to investigate the properties and structure of NiCrBSiFeC coating with WC additives, produced by the HVOF method and using a fine-dispersed mixture.
The main distinction of this study was the use of a fine-dispersed powder mixture, with the dominant fraction size not exceeding 10 µm. Furthermore, WC-Co 8 powder with a WC/Co ratio of 92/8 was employed as reinforcing particles, and the remelting stage after coating deposition by the HVOF method was omitted.
2. Materials and Methods
A mixture of NiCrBSiFe powder (Metco-16C) and WC was used to create the composite coating. Metco-16C was a powder alloy based on Ni, which also contained B, Si, Fe, and C. WC hard alloy powder (ISO 513:75 [27]) with a composition of 92% WC and 8% Co was used as the reinforcing particles.
The NiCrBSiFe powder alloy (Metco-16C) was mixed with WC powder (92 WC/8 Co) in amounts of 10%, 15%, and 20% by mass. The substrate was S235 steel.
The mixture in the required ratio was blended for 20 min in a Schatz laboratory mixer and then ground in a Retsch PM 100 mill for 30 min.
The fractional composition of the resulting mixture was determined using an FSX-6K photo-sedimentometer (Perm Scientific-Industrial Instrument-Making Company, Perm, Russia).
Next, the obtained mixture was applied to steel samples (100 × 100 × 10 mm, S235 steel) using the gas flame spraying method. The chemical composition of the materials is given in Table 1.
Table 1.
Chemical composition of the starting materials.
The coating was applied using a Rototec 80 installation (Castolin AG, Industriestrasse 34a, 8108 Dällikon ZH, Switzerland) (Figure 1a). The spraying process parameters are provided in Table 2.
Figure 1.
The Rototec 80 burner: (a) appearance of the burner; (b) samples for research.
Table 2.
Main parameters of thermal spraying and remelted processes.
This was a specialized burner for thermal spraying (a hot method), designed for restoring parts and applying coatings. Before coating deposition, the steel substrate was thoroughly cleaned using shot blasting and an ultrasonic bath, and then heated to a temperature of 2200 °C. The parameters of the spraying process are provided in Table 2.
After complete cooling, the obtained samples were ground on a JET JBSM-75 machine (JET Tools, a JPW Industries brand, 427 New Sanford Rd, La Vergne, TN 37086, USA). The appearance of the samples after grinding is shown in Figure 1b. Semi-finish grinding was performed with a wheel rotation speed of 35 m/s and a feed rate of 250 mm/min. The surface roughness after grinding was Ra 1.2 µm, which met the surface cleanliness requirements for detachable joints.
The chemical composition of the coatings was determined using a Vanta Element-S spectrometer (Olympus Corporation, Tokyo, Japan) and a Spas-05 for carbon determination (Spectral Analytical Systems, Moscow, Russia).
The chemical composition of the coatings was determined using the Vanta Element-S and Spas-05 spectrometers. The Vanta Element-S analyzer utilized X-ray fluorescence analysis. The principle of operation was based on the excitation of sample atoms by X-ray radiation from an integrated tube. Secondary (fluorescent) radiation, characteristic of each element, was then detected. Since this analyzer was unable to detect light elements, the SPAS-0.5 analyzer was used to determine C, O, N, and B. Its operation was based on atomic emission spectral analysis. Data management and processing were performed through the integrated SPAS software provided with the SPAS-05 analyzer.
The stress levels on the obtained samples were measured using the multi-channel IKH-2M-8 device (Interunit, Moscow, Russia), which allowed the identification of stress concentration zones based on the magnetic field intensity (Hp).
The microstructure of the test samples was studied using a Jeol JCM-7000 electron microscope (JEOL Ltd., Tokyo, Japan) equipped with an energy-dispersive SDTM 30 attachment with Si detector. The analysis depth at the standard accelerating voltage (15 kV) was approximately from 1 to 3 µm. Since the coating thickness was about 700 µm, the substrate had no effect on the signal. The measurement area size in Mapping mode was set to 100 × 100 µm.
A 10% HNO3 solution was used as the etchant.
The phase composition of the samples was analyzed using a SmartLab X-ray diffractometer (Rigaku, Tokyo, Japan) equipped with a rotating Cu anode X-ray tube, operating at 9 kW. The following components were used:
- -
- Siemens KFL-CU-2K Cu–2K X-ray tube, 0.4 × 12 mm (copper anode);
- -
- Position-sensitive LYNXEYE detector;
- -
- Soller slit;
- -
- Primary and secondary X-ray beam collimation systems (additional slit—0.6 cm);
- -
- Nickel Kβ filter;
- -
- Anti-scattering screen (0.5 cm height).
- -
- The following conditions were selected for diffraction pattern acquisition:
- -
- Voltage: 30 kV;
- -
- Current: 10 mA;
- -
- Sample rotation: 15 rotations per minute (to obtain more complete data on the sample composition);
- -
- Scanning range: 10.4–80.6°;
- -
- Step size: 0.02°;
- -
- Scan delay time: 1 s.
Phase identification was carried out using the SmartLab Studio II programs (Rigaku Corporation, Tokyo, Japan). It should be emphasized that the objective of this study was not to quantitatively determine the phases in the structure. Therefore, data on the percentage phase composition and crystallite sizes were not provided.
The tribological characteristics were determined using a Microtest tribometer (Microtest S.A., Madrid, Spain). Dry sliding tests “ball on disk” were conducted. The test parameters were as follows: sliding distance—700 m; sliding speed—200 rpm; radius—1.5 mm; load—25 N; temperature—22 ± 1 °C; indenter—a 6 mm diameter ball made of WC6 hard alloy. The tribometer with the sample was placed in a sealed container to prevent the ingress of dust and other foreign particles.
The mass of the samples before and after the tribological tests was measured using an analytical balance Vesi Radwag AS/220 (Radwag, Radom, Poland). R2 with an accuracy of 0.00001 g. Before weighing, the test samples were cleaned in an ultrasonic bath for 10 min.
Wear resistance was calculated by dividing the sliding distance by the mass loss and was expressed in m/g.
where
- L—sliding distance, m;
- m—mass of wear debris, g.
The friction coefficients were calculated after excluding data from the first 4 m of the sliding distance, and the average values were presented.
where
- μ—friction coefficient (dimensionless);
- Ff—frictional force;
- Fn—load.
Microhardness was measured on a PMT-3M semi-automatic device (LOMO, Saint Petersburg, Russia) with a 100 g load and a 10 s dwell time. Tests were conducted at no less than 10 points.
All measurements were performed in triplicate. The reported values were the averages. The standard deviation for microhardness was ±0.1%. The mass measurement accuracy was 10−5 g, as specified in the instrument passports.
The adhesive strength of the coating was measured using the cross-cut method according to ASTM D 3359 [28] and DIN 53151 [29] on a PIG-byko-cut universal device (BYK-Gardner GmbH, Geretsried, Germany). According to the instructions, a blade with a 2 mm interval between cuts was used, since the coating thickness was at least 400 microns.
For the quantitative assessment of the residual amount of WC and pores in the structure, Thixomet Pro software 5.3 (Thixomet, Saint Petersburg, Russia) was used. This software was an image analysis system designed for materials science tasks and quality control in accordance with GOST, ISO, DIN, ASTM, and other standards. The quantitative analysis was conducted according to ASTM 1245-00 [30], “Standard method for determining the content of inclusions or second phases in metals by automatic image analysis”. The analysis was carried out in at least 10 fields of view; the table shows the average result.
3. Results and Discussion
The fractional composition of all mixtures was almost identical. Figure 2 showed the particle size distribution for all the samples. As seen in the histograms, all the mixtures exhibited a similar granulometric composition.
Figure 2.
Particle size distribution of the mixture: (a) example of a particle size distribution WC15; (b) a comparison histogram.
The dominant fraction consisted of particles in the 3–10 µm range. The high uniformity and similarity in the particle size distributions of the powders used did not require additional sieving after grinding. This particle distribution indicated high homogeneity of the mixture. It should ensure uniform spraying and good adhesion to the substrate.
The chemical composition of the coatings after grinding is presented in Table 3.
Table 3.
Shows the chemical composition of the coating after grinding.
Stress levels were measured on the obtained samples. The results are shown in Figure 3.
Figure 3.
Changes in the stress levels on the surface of the sample after coating application: (a) WC0; (b) WC10; (c) WC15; (d) WC20.
Figure 3 shows that the stress levels were almost identical for the WC0 and WC10 samples. A single peak in the magnetic field intensity (Hp) was observed. This was associated with surface changes caused by grinding. The highest stress values were observed in the 40–70° sectors, where the contours exhibited the largest radial size. This indicates the formation of a dominant stress axis, which remained consistent for all of the coating states investigated. In the opposite part of the diagram, approximately in the 220–260° range, the stress values were minimal. This reflected the direction of unloading or the path of least resistance in the material structure.
However, with an increase in WC content in the coating, the stress levels and peak positions changed. The most significant changes were observed in the blue contour, which exhibited the highest amplitude and the most elongated shape. This indicated considerable tensile stresses and a high gradient in their distribution. This condition could have been caused either by more intense surface deformation or by an increased proportion of strengthening phases, which was more likely in this case. The presence of elongated peaks might also suggest some anisotropy in the grain shape.
An important quality parameter of the coatings was the adhesion strength to the substrate. Figure 4 shows the results of adhesion strength measurements, which were conducted using the cross-cut method. As seen in the presented images, the adhesion of all samples was approximately the same. However, the WC20 sample differed slightly from the others. According to ISO/JIS classification, it received a score of 1, while all other samples had a score of 0. The relatively low adhesion strength of the WC20 coating may be misleading, as the detachment of particles from the surface layer was linked to the removal of hard WC particles. However, the coating as a whole could still exhibit good adhesion to the substrate. From an operational perspective, a score of 0 in the ISO/JIS classification corresponds to a “high-risk zone”. Therefore, the combination of this parameter with other low values justified the exclusion of the WC20 coating from further use.
Figure 4.
Results of adhesive strength measurements.
The hardness and wear resistance of the obtained samples were determined. The results are presented in Table 4.
Table 4.
Results of tribological property studies.
As seen from the data in Table 4, the WC15 sample exhibited the highest wear resistance. This was despite the logical assumption that an increase in the content of WC particles should lead to higher wear resistance and hardness. Indeed, as shown in Table 4, the microhardness of the WC20 sample was the highest. However, its wear resistance was lower than that of the WC15 sample. A comparison of the wear tracks (Figure 5) revealed that the wear process on the samples followed completely different patterns, despite the relatively similar friction coefficients.
Figure 5.
Wear tracks for the experimental samples: the friction coefficient is shown on the y-axis, and the distance in meters is shown on the x-axis: (a) WC0; (b) WC10; (c) WC15; (d) WC20.
The wear process of the WC0 and WC10 samples (Figure 5a,b) occurred evenly. The wear track was wide, and the wear intensity was nearly the same across the entire distance. The introduction of tungsten carbide into the coating altered the wear pattern. The wear tracks became narrower, and the wear rate was uneven. Small peaks appeared in the wear track. These peaks could be attributed to the spalling of fine solid-phase particles. For the WC15 sample, this phenomenon occurred at the beginning of wear (10–30 m distance). For the WC20 sample, it continued throughout the entire wear process, including the initial, middle, and final stages.
The structure exhibited pronounced porosity. The pores had both rounded and elongated shapes, which was characteristic of flame spraying due to gas release. The amount of pores was quantitatively determined using Thixomet Pro software (Thixomet, Saint Petersburg, Russia). Figure 6 shows an example of using this software. The same software was used to determine the amount of remaining WC particles after tribological testing. Table 5 shows the quantitative parameters of the structure obtained using Thixomet Pro software.
Figure 6.
Example of using Thixomet Pro for quantitative analysis.
Table 5.
Quantitative structure parameters obtained using Thixomet Pro software.
The discrepancy between hardness and expected wear resistance could be explained by the loss of WC particles during wear. Apparently, the proportion of the hard phase in the relatively soft matrix (the Sharpie principle) should not exceed a certain limit. Otherwise, the “spalling” process of the hard phase began, which led to increased wear despite the high surface hardness. As can be seen from the data in Table 5, the WC particle area in sample WC20 is lower than in sample WC15, although it should be higher since the WC content in this sample is inherently higher. This fact indicates that some WC was chipped off during tribological testing.
The pore area of all of the studied samples ranged from 1.85 to 2.1%. This was considered a satisfactory value for coatings of this type [31,32].
Figure 7 shows the wear spots obtained as a result of the conducted tribological tests.
Figure 7.
Wear spots of samples after tribological tests: (a) WC0; (b) WC10; (c) WC15; (d) WC20.
As illustrated in Figure 7, the wear mechanism exhibited a clear dependence on the WC content within the coating. For the coating without reinforcing particles (WC0 sample), the wear mechanism was primarily adhesive, as indicated by the smooth appearance of the wear tracks. In this case, the matrix, a nickel-based solid solution, was subjected to wear. However, with the addition of WC particles, the wear mechanism transitioned to an abrasive type. Groove-like marks, scratches, and ridges appeared within the wear spot, indicating that hard particles (either WC or the hard phases formed during spraying and interaction) were in contact with the surface and indenter, causing scratching and other forms of surface damage. With an increase in WC content (WC20), pitting was observed within the wear spot, indicating the spalling of hard particles. In this case, two wear mechanisms were identified: abrasive wear and fatigue wear. The presence of the additional fatigue wear mechanism accounted for the reduced wear resistance observed in the WC20 sample, despite it having the highest hardness among the tested samples.
To confirm the wear mechanism, the Hertz contact pressure was calculated using the following formula
where
- a—radius of the contact area;
- F—modulus of elasticity.
Assuming elastic modulus values of 210 GPa for γ-Ni and 530 GPa for WC, the Hertz contact pressure was calculated to be 3256 MPa. It was important to note that this value was an approximation. Several assumptions were made during the calculation, including the use of elastic modulus values corresponding to pure phases, among others. Nevertheless, this pressure represented the critical threshold at which a transition in the wear mechanism occurred.
At a WC content of 15%, the WC particles were dispersed within the matrix, with a certain distance between them. Under the applied Hertz contact pressure of 3256 MPa, the γ-Ni matrix plastically deformed, taking on the primary load. Meanwhile, the WC particles acted as reinforcement, remaining firmly embedded within the matrix. In this case, an adhesive wear mechanism was observed.
As the WC content increased to 20%, the distance between the particles decreased. Under the applied Hertz contact pressure of 3256 MPa, the WC particles began to make direct contact with each other or came close enough to transfer the load directly between them. This occurred because the amount of matrix material was insufficient to serve as a damping layer. The stresses at the grain boundaries of WC exceeded the bonding strength between the particles and the matrix. As a result, the particles began to spall, becoming an additional source of wear. At this stage, the wear mechanism became mixed, consisting of both abrasive and fatigue wear.
Understanding the operational process requires knowledge of the structure and phase composition.
Figure 8 shows the general appearance of the coating in cross-section at different magnifications. The coating structure was typical for self-fluxing nickel alloys with the addition of refractory reinforcing particles, in this case, WC.
Figure 8.
General appearance of the coating (section in the (100) plane): (a) ×60; (b) ×200.
The boundary between the substrate and the coating was relatively smooth, without deep melting, indicating good adhesion between the substrate and the coating. A thin, elongated diffusion zone of Fe → Ni and Ni → Fe was present in the contact area. However, at this magnification, no such intermediate zone was observed.
Numerous light and dark inclusions of irregular shape were also present. These inclusions were characteristic of partially melted WC particles, carbides such as W2C, Cr3C7, and intermetallics like NiSi2, NiB, and others.
The large light inclusions likely corresponded to unmelted WC, which had high electrical conductivity and a high atomic mass. As a result, they appeared brighter in the BSE mode.
A comparison of the structure in Figure 8a with the element distribution map (Figure 9) revealed inhomogeneity, particularly in the distribution of silicon, tungsten, and carbon. The presence of a dark region in the coating layer indicated the accumulation of phases such as silicides and borides, as Si, B, and C had low atomic masses. Such liquation may negatively affect adhesion, making it crucial to carefully control the spraying technique during the process.
Figure 9.
Elemental composition of the coating (section in the (100) plane).
As expected, almost all elements, except for Ni, were localized in the coating zone. They had a fairly uniform distribution, indicating a uniform distribution of carbides and other secondary phases. The behavior of Ni was somewhat different. As seen from the distribution map, it actively diffused into the substrate, forming an intermediate layer of γ-(Ni,Fe) solution, in which intermetallic phases were present in small quantities.
The coating quality was largely determined by the nature of hardness variation with respect to the distance from the surface to the substrate. It was evident that the more gradually the hardness decreased with depth, the longer the service life would be, assuming other conditions were equal. Figure 10 shows the hardness variation at different points along the coating depth.
Figure 10.
Hardness dependence on the distance from the surface to the substrate.
The microhardness in all the investigated samples decreased with depth. At a distance of 100 µm, it was almost comparable to the microhardness of the substrate. However, the nature of microhardness variation differed between the samples. For the WC0, WC10, and WC15 samples, the decrease in microhardness was gradual. For the WC20 sample, a significant drop in microhardness was observed at a depth of 40 µm, followed by further reduction. Such a catastrophic drop in microhardness in the middle of the coating could only be explained by the spalling of fine solid-phase particles. It should be noted that the nature of microhardness variation correlated well with the wear resistance data and the wear track characteristics.
During the coating process, partial melting of the surface layer of the substrate and the coating alloy occurred. The resulting melt, based on Ni and Fe, became saturated with C, W, Cr, Si, and B. The crystallization process began with the precipitation of carbides and intermetallics due to the decreased solubility of Cr and W in the solid Ni-Fe solution. The γ-Ni-Fe solid solution phase crystallized first. Ni3B, (Cr,Fe)7C3, and (W,Cr,Fe)6C precipitated from the melt. CrB2/CrB formed, creating small colonies. During crystallization, some WC particles retained their original structure (bright zones).
The coating structure (Figure 11) reflected the inhomogeneity of the composition, even within a single phase. Figure 11b presented the structure image in ImageJ mode, where each shade of gray was automatically assigned a corresponding color. The inhomogeneity of color within a single shade (e.g., pink) indicated variation in the composition. Based on the element distribution map (Figure 12), the elements present in the phase were indicated on the structure. For example, the white inclusion contained W (shown in blue on the distribution map), and so on.
Figure 11.
Surface structure of the WC15 sample: (a) BED-S mode image; (b) ImageJ mode image. Image processing was performed using ImageJ software (version 1.54).
Figure 12.
Element distribution map of the WC15 sample section in the (001) plane.
The main portion of the structure consisted of a solid solution based on Ni, alloyed with Fe and Cr (pink zone). The color heterogeneity indicated a varying composition of the solution. The green, light green, and blue transitional zones reflected products of interaction between the substrate, coating elements, and WC. The color visualization allowed the conclusion that the main precipitation of secondary phases occurred at the grain boundaries. Signs of melting were present at the WC particle boundaries, as evidenced by the presence of other elements. The particle boundaries exhibited a variable color. The microstructure showed pronounced heterogeneity and the presence of several types of phases distributed in the metal matrix.
The structure of the sample clearly displayed large and small reinforcing WC carbide particles, which were evenly distributed throughout the coating. The particles retained their original morphology. However, transitional zones were observed at the boundaries, caused by partial dissolution of WC in the molten matrix. In these areas, complex carbides of the composition (W,Cr)C were likely formed, along with zones of local tungsten enrichment. This was associated with the diffusion of Cr from the matrix and its interaction with WC.
When comparing the structure with the element mapping (Figure 10), it was observed that the elements C and Cr localized in the same points, forming carbides of different types. In the darker zones, B and Si were present, forming intermetallic compounds such as Ni3B and Ni3Si.
To refine the phase composition of the structure, XRD analysis was performed. Figure 13 presents the diffraction patterns of the WC15 (red line) and WC20 (violet line) samples.
Figure 13.
Comparative analysis of the diffraction patterns for WC15 (a) and WC20 (b).
For both samples, distinct peaks corresponding to γ-Ni were observed in the 40–45° range, which roughly matched the reflections of γ-Ni (111) and γ-Ni (100). The presence of these intense peaks from the nickel phase confirmed that the coating matrix was a solid solution based on γ-Ni, alloyed with Fe. These peaks showed slight deviations from the positions reported in previous studies [18,22] and shifted towards smaller angles. This suggested, in accordance with the Wulff–Bragg condition, that the lattice period of the solid solution in the experimental sample was slightly larger. Consequently, it contained more Fe compared to the samples examined in those studies. This assumption was based on the fact that the atomic radius of iron is larger than that of nickel. The dissolution of iron in nickel leads to an expansion of the lattice period. In other words, the greater the lattice distortion, the more iron was dissolved in the solution.
A significant intensity of the γ-Ni (100) peak in the region of 45° indicated a preferred grain orientation. This was confirmed by the surface structure (Figure 8a) and the peak positions of intensity (Figure 3c,d).
Characteristic peaks of tungsten carbide WC were observed in the 35°, 60°, and 70° ranges, which was consistent with data from other authors. For the WC20 sample, the WC peaks had higher intensity, indicating a higher content compared to the WC15 sample. Phases of W2C, Cr7C3, and FeSi were also observed, which is consistent with data from other authors. Intermetallic phases of the Ni3B, Fe3B, (Cr,Fe)2B type were noted in the range 51–52°. A peak identified as a NiCrFe solid solution is present in the high angle range (~75°). It indicates the mutual solubility of Fe and Cr in the nickel matrix. A comparative analysis of diffractograms allows us to draw the following conclusions. For the WC20 sample, the WC peaks have a higher intensity, indicating a higher content than in WC15. This may be due to the higher melting point due to the higher amount of WC, less interaction with the melt, and better preservation of the initial particles. This difference in phase composition fits well into the theory of the mechanism of dissolution of WC particles, which is presented in [18]. According to this theory, there are two mechanisms of dissolution of WC particles: partial and complete. In the case of partial dissolution, only the edges of the WC particles dissolve and only a small part of the carbon and tungsten diffuse in the melt to other elements (Cr, Fe) and form a small amount of the carbide phase. The rest of the WC remains undissolved. This is the mechanism that is most likely being implemented in this case. According to the second mechanism, WC particles dissolve completely; while part of the carbon is consumed to form W2C, the rest diffuses into the melt and forms a carbide phase.
Based on the obtained data regarding the structure and phase composition of the coatings on the WC15 and WC20 samples, it could be expected that the WC20 coating would exhibit higher hardness and wear resistance. The hardness of the WC20 coating was indeed significantly higher, as shown in Figure 5. However, it demonstrated lower wear resistance, which was also confirmed by the wear track characteristics. This discrepancy could be explained by the fact that undissolved WC particles were spalled during wear. This led to mass loss and changes in the surface topography.
Since the matrix (the dominant phase) in both samples was the same (γ-alloyed solid solution based on Ni), the most accurate comparison was the ratio of the WC peak intensity to the γ-Ni (111) peak intensity at approximately 44°. As the γ-Ni matrix was the dominant phase in both samples, the increase in WC peak intensity relative to the γ-Ni peaks clearly indicated an increase in the volumetric fraction of the carbide phase in the WC15 sample compared to the WC20 sample.
4. Conclusions
The conducted studies demonstrated that the use of a NiSiCrFeB mixture with WC/Co additives (92/8) at 15 and 20% by weight, with a dispersion of 3–10 μm, applied by the HVOF method, resulted in high hardness and wear resistance. Compared to the NiSiCrFeB coating without WC, the hardness and wear resistance of the experimental coatings were nearly 1.7 times higher.
Such results were comparable to the properties of coatings that contained significantly higher amounts of WC. The substantial increase in hardness and wear resistance with small additions of WC could be explained by the use of a much finer fraction of the mixture for spraying. In most studies, the authors used mixtures with larger particle sizes, ranging from 49 μm [4] to 230 μm [18], compared to the mixture used in this study.
This likely explained the wide variation in microhardness values of NiSiCrFeB + WC-based coatings, despite the spraying being conducted using the same method. The influence of the particle composition on the structural parameters was extensively examined in reference [3]. The authors highlighted the correlation between the fractional composition of the sprayed mixture, the structural parameters, and the resulting properties.
An additional contribution to the increase in hardness and wear resistance came from the composition of WC. In this study, WC with a WC/Co ratio of 92/8 was used. In contrast, most studies employed a WC/Co alloy with ratios of 80/20 or even 50/50.
The phase composition of the coating consisted of a γ-solid solution based on Fe-Ni, as well as FeSi, Fe3C, M7C3, WC, W2C, and NiCrFe phases.
The addition of more than 15% WC to the powder alloy NiSiCrFeB led to an increase in microhardness up to 1700 HV. However, it also resulted in a decrease in wear resistance. This was explained by the increased proportion of undissolved WC phase in the structure, which led to the spalling of small particles and a reduction in wear resistance.
The analysis of wear spots and the calculation of the Hertz contact pressure showed that the wear mechanism varied depending on the WC content in the coating. At lower WC content, the wear mechanism was abrasive. However, at 20% WC, the wear mechanism became mixed, consisting of both abrasive and fatigue wear. This transition led to a decrease in wear resistance.
Thus, the conducted study demonstrated the feasibility of using a NiSiCrFeB coating with WC additives without the need for additional remelting. Similar hardness and wear resistance results were achieved immediately after HVOF spraying when using a fine-dispersed fraction of 3–10 μm WC/Co with a composition of 92/8. This simplification of the technology allowed for a reduction in the surface treatment time and a decrease in production costs by eliminating the remelting stage.
For the calculation of the economic efficiency of simplifying the spraying technology (eliminating the second remelting operation), the following conditions were assumed:
Equipment: vacuum furnace (50 kW) + argon supply system.
Process: 1 remelting cycle = 4 h (heating, holding time of 2 h, cooling).
Direct electricity costs:
The furnace consumes 50 kW per hour. The industrial electricity rate was assumed to be 0.1 units per kW·h (this value was approximate and may vary by region).
The consumption per cycle: 50 kW × 4 h = 200 kW·h.
The electricity cost per cycle: 200 × 0.1 = 20 units.
For 1000 parts (assuming 50 parts fit into the furnace per cycle): 1000/50 = 20 cycles.
Thus, the total electricity savings were: 20 cycles × 20 units = 400 units.
Thus, the basic calculation showed electricity saving of 400 units per batch of 1000 parts. This calculation accounted only for electricity costs. Other expenses, such as labor, auxiliary costs (water, protective gas), and others, were not considered. It was clear that the actual savings from eliminating the remelting stage would be significantly higher.
It is worth noting that the study in [33] demonstrated the feasibility of producing a superhydrophobic coating, composed of a structure reinforced with micro-hBN/nano-Al2O3 ceramics. This was accomplished using a universal one-step spraying method. These results underscored the relevance and technical viability of the problem addressed in the current study.
Author Contributions
Conceptualization, S.S.K. and E.V.S.; data curation A.Z.I.; methodology A.Z.I. and S.K.A., formal analysis, T.V.K.; investigation S.S.K.; writing—original draft preparation, S.K.A.; writing—review and editing, S.S.K.; visualization, T.V.K. All authors participated in writing the paper. All authors have read and agreed to the published version of the manuscript.
Funding
This research was funded by the Committee of Science of the Ministry of Science and Higher Education of the Republic of Kazakhstan (Grant No. AP26103843).
Data Availability Statement
The original contributions presented in this study are included in the article; further inquiries can be directed to the corresponding author.
Conflicts of Interest
The authors declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this paper.
References
- Hemmati, I.; Rao, J.C.; Ocelík, V.; De Hosson, J. Electron microscopy characterization of Ni-Cr-B-Si-C laser deposited coatings. Microsc. Microanal. 2013, 19, 120–131. [Google Scholar] [CrossRef] [Scilit]
- Houdková, Š.; Smazalová, E.; Vostřák, M.; Schubert, J. Properties of NiCrBSi coating, as sprayed and remelted by different technologies. Surf. Coat. Technol. 2014, 253, 14–26. [Google Scholar] [CrossRef] [Scilit]
- Planche, M.; Liao, H.; Normand, B.; Coddet, C. Relationships between NiCrBSi particle characteristics and corresponding coating properties using different thermal spraying processes. Surf. Coat. Technol. 2005, 200, 2465–2473. [Google Scholar] [CrossRef] [Scilit]
- Praveen, A.S.; Sarangan, J.; Suresh, S.; Channabasappa, B. Optimization and erosion wear response of NiCrSiB/WC–Co HVOF coating using Taguchi method. Ceram. Int. 2016, 42, 1094–1104. [Google Scholar] [CrossRef] [Scilit]
- Tobar, M.J.; Álvarez, C.; Amado, J.; Rodríguez, G.; Yáñez, A. Morphology and characterization of laser clad composite NiCrBSi–WC coatings on stainless steel. Surf. Coat. Technol. 2006, 200, 6313–6317. [Google Scholar] [CrossRef] [Scilit]
- Ramesh, M.R.; Prakash, S.; Nath, S.; Sapra, P.K.; Venkataraman, B. Solid particle erosion of HVOF sprayed WC–Co/NiCrFeSiB coatings. Wear 2010, 269, 197–205. [Google Scholar] [CrossRef] [Scilit]
- Buytoz, S.; Ulutan, M.; Islak, S.; Kurt, B.; Çelik, O.N. Microstructural and wear characteristics of high velocity oxygen fuel (HVOF) sprayed NiCrBSi–SiC composite coating on SAE 1030 steel. Arab. J. Sci. Eng. 2013, 38, 1481–1491. [Google Scholar] [CrossRef] [Scilit]
- Fals, H.C.; Aguiar, D.; Fanton, L.; Belém, M.J.X.; Lima, C.R.C. A new approach of abrasive wear performance of flame sprayed NiCrSiBFeC/SiC composite coating. Wear 2021, 477, 203887. [Google Scholar] [CrossRef] [Scilit]
- Cai, B.; Tan, Y.-F.; He, L.; Tan, H.; Gao, L. Tribological properties of TiC particles reinforced Ni-based alloy composite coatings. Trans. Nonferr. Met. Soc. China 2013, 23, 1681–1688. [Google Scholar] [CrossRef] [Scilit]
- Praveen, A.S.; Sarangan, J.; Suresh, S.; Subramanian, J.S. Erosion wear behaviour of plasma sprayed NiCrSiB/Al2O3 composite coating. Int. J. Refract. Met. Hard Mater. 2015, 52, 209–218. [Google Scholar] [CrossRef] [Scilit]
- Harsha, S.; Dwivedi, D.K.; Agarwal, A. Influence of CrC addition in NiCrSiB flame sprayed coatings on microstructure, microhardness and wear behavior. Int. J. Adv. Manuf. Technol. 2008, 38, 93–101. [Google Scholar] [CrossRef] [Scilit]
- Karaoglanli, A.C.; Oge, M.; Doleker, K.M.; Hotamis, M. Comparison of tribological properties of HVOF sprayed coatings with different composition. Surf. Coat. Technol. 2017, 318, 299–308. [Google Scholar] [CrossRef] [Scilit]
- Niranatlumpong, P.; Koiprasert, H. Phase transformation of NiCrBSi–WC and NiBSi–WC arc sprayed coatings. Surf. Coat. Technol. 2011, 206, 440–445. [Google Scholar] [CrossRef] [Scilit]
- Fernández, M.; García, A.; Cuetos, J.; González, R.; Noriega, A.; Cadenas, M. Effect of actual WC content on the reciprocating wear of a laser cladding NiCrBSi alloy reinforced with WC. Wear 2015, 324–325, 80–89. [Google Scholar] [CrossRef] [Scilit]
- Sha, J.; Chen, L.-Y.; Liu, Y.-T.; Yao, Z.-J.; Lu, S.; Wang, Z.-X.; Zang, Q.-H.; Mao, S.-H.; Zhang, L.-C. Phase Transformation-Induced Improvement in Hardness and High-Temperature Wear Resistance of Plasma-Sprayed and Remelted NiCrBSi/WC Coatings. Metals 2020, 10, 1688. [Google Scholar] [CrossRef] [Scilit]
- Paleu, C.C.; Munteanu, C.; Istrate, B.; Bhaumik, S.; Vizureanu, P.; Bălţatu, M.S.; Paleu, V. Microstructural Analysis and Tribological Behavior of AMDRY 1371 (Mo–NiCrFeBSiC) Atmospheric Plasma Spray Deposited Thin Coatings. Coatings 2020, 10, 1186. [Google Scholar] [CrossRef] [Scilit]
- Kiape, S.; Glava, M.; Georgatis, E.; Kamnis, S.; Matikas, T.E.; Karantzalis, A.E. A Comparative Study between a Thermal Spray CoCrFeMnNi0.8V/WC-Co High Entropy Alloy Composite Coating and Plain CoCrFeMnNi0.8V and WC-Co Thermal Spray Coatings. J. Compos. Sci. 2024, 8, 120. [Google Scholar] [CrossRef] [Scilit]
- Feng, L.; Li, C.; Han, X.; Luo, F.; Sun, H. Experimental Study on Preparation of Tungsten-Carbide-Particle-Reinforced Nickel-Based Alloy Plasma Surfacing Layer on Descaling Roller Surface. Coatings 2024, 14, 729. [Google Scholar] [CrossRef] [Scilit]
- Appiah, A.N.; Wyględacz, B.; Matus, K.; Reimann, Ł.; Bialas, O.; Batalha, G.F.; Czupryński, A.; Adamiak, M. Microstructure and performance of NiCrBSi coatings prepared by modulated arc currents. Appl. Surf. Sci. 2024, 648, 159065. [Google Scholar] [CrossRef] [Scilit]
- Perrin, T.; Achache, S.; Meausoone, P.; Sanchette, J. Characterization of WC-doped NiCrBSi coatings deposited by Laser Cladding effects of particle size and content of WC powder. Surf. Coat. Technol. 2021, 425, 17460–17470. [Google Scholar] [CrossRef] [Scilit]
- Huang, S.; Zhou, J.; Sun, K.; Yang, H.; Cai, W.; Liu, Y.; Zhou, P.; Wu, S.; Li, H. Microstructural Charactistics of Plasma Sprayed NiCrBSi Coatings and Their Wear and Corrosion Behaviors. Coatings 2021, 11, 170. [Google Scholar] [CrossRef] [Scilit]
- Abderrahmane, A.; Gaceb, M.; Cheikh, M.; Le Roux, S. Wear Behavior and Microstructure of Thermally Sprayed NiCrBSiFeC and Composite NiCrBSiFeC-WC(Co) Coatings. Mater. Sci. 2021, 27, 175–183. [Google Scholar] [CrossRef] [Scilit]
- Liu, Y.; Jin, H.; Li, G.; Li, P.; Zhang, S.; Zhang, Z. Microstructure and Properties of Inconel 718/WC Composite Coating on Mold Copper Plate. Coatings 2025, 15, 1394. [Google Scholar] [CrossRef] [Scilit]
- Qian, S.; Zhang, Y.; Dai, Y.; Guo, Y. Microstructure and Mechanical Properties of Nickel-Based Coatings Fabricated through Laser Additive Manufacturing. Metals 2021, 11, 53. [Google Scholar] [CrossRef] [Scilit]
- Zhang, L.; Yu, Y.; Chen, X.; Huo, J.; Zhang, K.; Wei, X.; Zhang, Z.; Hui, X. Enhanced Resistance to Sliding and Erosion Wear in HVAF-Sprayed WC-Based Cermets Featuring a CoCrNiAlTi Binder. Materials 2026, 19, 178. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Saeedi, R.; Razavi, R.S.; Bakhshi, S.R.; Erfanmanesh, M.; Bani, A.A.; Erfanmanesh, M. Optimization and characterization of laser cladding of NiCr and NiCr–TiC composite coatings on AISI 420 stainless steel. Ceram. Int. 2021, 47, 4097–4110. [Google Scholar] [CrossRef] [Scilit]
- ISO 513:75; Application of Hardmetals for Machining by Chip Removal—Designation of the Main Groups of Chip Removal and Groups of Application. International Organization for Standardization (ISO): Geneva, Switzerland, 1975.
- ASTM D3359; Standard Test Methods for Rating Adhesion by Tape Test. ASTM International: West Conshohocken, PA, USA, 2023.
- DIN 53151; Testing of Paints, Varnishes and Similar Coating Materials; Cross-Cut Test on Paint Coatings and Similar Coatings. DIN Media GmbH: Berlin, Germany, 1981.
- ASTM E1245-00; Standard Practice for Determining the Inclusion or Second-Phase Constituent Content of Metals by Automatic Image Analysis. ASTM International: West Conshohocken, PA, USA, 2017.
- Bulnes, A.G.; Fuentes, V.A.; Cano, I.G.; Dosta, S. Understanding the Influence of High Velocity Thermal Spray Techniques on the Properties of Different Anti-Wear WC-Based Coatings. Coatings 2020, 10, 1157. [Google Scholar] [CrossRef] [Scilit]
- Senapati, P.; Sutar, H.; Murmu, R.; Bajpai, S. Experimental Design of Solid Particle Wear Behavior of Ni-Based Composite Coatings. J. Compos. Sci. 2021, 5, 133. [Google Scholar] [CrossRef] [Scilit]
- Yang, H.J.; Dong, Y.; Li, X.; Gao, Y.; He, W.; Liu, Y.; Mu, X.; Zhao, Y.; Fu, W.; Wang, X.; et al. Development of a mechanically robust superhydrophobic anti-corrosion coating using micro-hBN/nano-Al2O3 with multifunctional properties. Ceram. Int. 2025, 51, 491–505. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.