Abstract
In soft–rigid robotics, it is necessary to join flexible polymers to each other and to rigid thermoplastics without using adhesives or fasteners. However, little is known about ultrasonic welding of elastomers. In this study, we examine the 20 kHz ultrasonic welding of fused deposition modelling (FDM)-printed thermoplastic polyurethane (TPU) and its joining to polylactic acid (PLA). Flat interfaces did not weld in any of the 63 pair-thickness conditions tested (n = 5 per pair), with the halves separating at mean peak loads of 5.0–8.0 N. A hexagonal energy director, which was developed for use with rigid polymers, was ineffective. However, an interlocking toothed profile (tooth thickness 0.7–1.0 mm, pitch 1 mm, height 1 mm) was able to weld TPU–TPU with a total thickness of up to 5 mm with 80% amplitude, using a soft vibration ramp and a weld time of 2–3 s (peak load 29.0 ± 1.6 N). The same profile was used to join TPU to PLA. At a total thickness of 5 mm, the joints failed at the weld line (39.0 ± 1.6 N); at 10 mm, four out of five specimens failed in the base material at 62.0 ± 3.4 N. The need for an energy director is attributed to the low stiffness and high damping of TPU. Only macroscopic and optical microscopic examinations were performed; the positioning was manual and only quasi-static loading was tested. Polished sections, fatigue and creep tests are still needed.
1. Introduction
The structural integration of lightweight polymer materials that are dissimilar from each other is an increasingly important task in modern robotics. Mobile robots, manipulator grippers, damping elements and protective coatings often employ flexible, rubber-like materials that must be joined to each other and to rigid structural polymers to create lightweight, functional, modular assemblies [1]. Ultrasonic welding (UW) is a fastener-free method of joining thermoplastics using high-frequency mechanical vibration. Earlier work by the authors demonstrated that UW provides stable, strong joints for rigid thermoplastics such as ABS, PLA and PETG when a hexagonal energy-director geometry is used [2].
Thermoplastic polyurethane (TPU) is a flexible elastomer that combines the elasticity of rubber with the processability of plastic. It can be easily processed using fused deposition modelling (FDM) or selective laser sintering (SLS). TPU’s wear resistance, impact resistance and chemical resistance make it ideal for use in flexible grippers, joints, shock absorbers, pneumatic tubing, seals and protective coatings in robotics, automotive interiors, medical devices, wearable electronics and footwear. TPU can be joined to itself and to rigid engineering polymers such as polylactic acid (PLA) or polycarbonate (PC) without the need for adhesives or mechanical fasteners. This allows lightweight hybrid components to be produced using a single joining technology, for example, a rigid robot body combined with a flexible TPU gripper [3,4,5].
However, TPU behaves fundamentally differently to rigid thermoplastics when subjected to ultrasonic excitation. As an elastomer, it strongly absorbs ultrasonic vibration, converting wave energy into heat within the material rather than transmitting it efficiently to the joint interface. Therefore, geometries and process parameters developed for rigid polymers cannot simply be transferred to TPU. Moreover, the fundamental relationships between joint geometry, specimen thickness and generator settings for TPU have not yet been systematically established [6].
The present study aims to determine the following through a structured experimental campaign: (i) an energy-directing geometry and specimen thickness that enable reliable ultrasonic welding of TPU to itself; (ii) suitable ultrasonic generator settings; (iii) whether the same approach can be extended to join flexible TPU to rigid PLA, including the effect of total joint thickness on weld strength and failure mode. The results will provide robotics designers with practical guidance on creating lightweight, flexible–rigid hybrid polymer joints through ultrasonic welding.
The energy directors of triangular, semicircular and mesh types have been studied for rigid and composite adherends [2,7,8,9,10,11]. One earlier study optimised the ultrasonic welding of a TPU device with a hermetic seal [12]. To our knowledge, no previous study has combined the results presented in this work (i) a controlled negative result showing that flat FDM-printed TPU interfaces do not weld under any of the 63 pair–thickness conditions accessible to the generator; (ii) a dense, interlocking, toothed profile with a matching recess in the mating half the thickness limit and generator settings at which TPU welding occurs and an explanation of why TPU welding fails when using directors designed for rigid polymers on an adherend with a modulus of about 20 MPa; and (iii) TPU–PLA joints with the same geometry, exhibiting a shift from failure at the weld line to failure in the base material as the total thickness increases from 5 mm to 10 mm. Process parameters and director shape have been optimised statistically for rigid thermoplastics [13,14,15], and viscoelastic and frictional heat generation has been modelled and measured for composites with flat energy directors [16,17]. Earlier work on multi-material fused filament fabrication has examined adhesion in TPU–PLA as a function of printing parameters and interface geometry [18,19], but none of these studies address the ultrasonic welding of TPU.
2. Materials and Methods
2.1. Materials
Thermoplastic polyurethane (TPU) filament was used as the flexible material under investigation. Preliminary trials showed no significant effect of colour on weld quality for two commercially available filament colours (white and translucent) (Figure 1) [20].
Figure 1.
Laboratory experimental setup for ultrasonic welding: ultrasonic generator, transducer (converter), specimen sample.
- Welding Equipment
Welding was performed using a JYD-2900SP-LCD commercial ultrasonic welding system (Jinguan Ultrasonic, Guangzhou, China) (Figure 1), which consists of a generator, a piezoelectric converter, a booster and a sonotrode. The system operates at a nominal frequency of 20 kHz with automatic resonance tracking. The sonotrode applies vibration to the parts under static force, creating frictional heat that melts a thin layer of material at the joint interface. This layer then solidifies under pressure to form the weld [21,22,23].
To make heat generation more efficient and consistent, many ultrasonic welding setups, particularly those used for additively manufactured parts, incorporate energy directors. These are small, triangular or rectangular protrusions that are moulded or printed onto one of the mating surfaces. As discussed by Villegas [7], these energy directors concentrate ultrasonic vibrational energy at specific contact points, promoting rapid, localised melting at the interface and improving weld quality.
The effectiveness of ultrasonic welding (UW) depends on the conversion of high-frequency vibratory energy into viscoelastic heat at the joint interface. This process involves transmitting ultrasonic energy through the materials and converting it into heat at the contact surface [24]. Of the various process parameters, weld time and pressure are the most influential, while time and vibration amplitude have also been identified as key factors in joint optimisation [25].
The relationship between welding parameters and joint quality is not always linear. While increasing weld time can initially improve joint strength, excessive welding time can lead to thermal degradation, porosity and reduced mechanical performance [24]. Fu et al. [21,25] reported that specific ranges of welding time and load (4–6 s and 5–7 N, respectively) produced defect-free microstructures; exceeding these limits, however, caused structural defects such as bubbles and voids. The type of thermoplastic material also has a strong impact on weldability, particularly with regard to the distinction between amorphous and semi-crystalline polymers. Amorphous polymers such as ABS generally weld more easily and utilise ultrasonic energy more efficiently than semi-crystalline polymers such as PE or HDPE. This difference relates to energy absorption behaviour: the energy director (ED) in ABS was found to absorb approximately 48.5% of the welding energy, compared to 21.1% for PE [2,8].
This principle has specifically been extended to thermoplastic parts printed using fused deposition modelling (FDM). A recent study of MEX-printed PLA and ABS specimens optimised the shape of the energy director, infill density, welding time and vibration amplitude using a design of experiments approach, the Taguchi method and analysis of variance (ANOVA) [9]. The study revealed that ultrasonic welding is an effective post-processing method for joining 3D-printed parts and overcoming the build-volume limitations of desktop 3D printers. A related study examined the ultrasonic welding of printed and moulded sustainable polymer specimens with energy directors [26].
Regarding the flexible material used in the present setup, thermoplastic polyurethane (TPU) has been the subject of increasing study as an FDM feedstock in other application contexts. For example, medical-grade TPU has been evaluated for FDM printing and gamma sterilisation in the manufacture of implantable devices, given the tunable mechanical properties that TPU offers, together with the cost and precision advantages of 3D printing. TPU has also been combined with a PLA–graphene composite filament via FDM to fabricate highly sensitive piezoresistive tactile sensors for use in soft robotics applications [27,28]. While these studies demonstrate the relevance of TPU as a flexible engineering filament, they do not address its ultrasonic welding properties. Compared with rigid PLA and ABS, the ultrasonic weldability of TPU has received little attention. The present study of hybrid PLA–TPU joints addresses this gap [9].
All specimens were fabricated using FDM on a Bambu Lab X1 Carbon 3D printer (Bambu Lab, Shenzhen, China). This high-performance printer has a fully enclosed chamber and an actively heated build plate to help maintain stable printing temperatures and minimise residual stresses in the printed polymer components. The following printing parameters were applied to all materials: a layer height of 0.2 mm, 100% infill density and the extrusion temperatures recommended by the filament manufacturers (240 °C for ABS, 210 °C for PLA and 235 °C for PETG). The build plate temperature was set to 100 °C for ABS and 70 °C for PLA and PETG. For TPU, a 0.4 mm nozzle was used with an extrusion temperature of 225 °C, a build-plate temperature of 50 °C and a printing speed of 25 mm/s, within the ranges recommended by the manufacturer [29]. Each specimen consisted of two complementary halves that were subsequently joined by ultrasonic welding (UW). Before welding, each half had a nominal wall thickness of 5 mm in the region surrounding the joint. At the interface, one half incorporated a 1 mm-high protruding ED, while the other half contained a corresponding 1 mm-deep recess. Consequently, the overall thickness of the assembly in the weld region remained at 5 mm since the protrusion and recess interlocked without increasing the total thickness. During ultrasonic welding, only the 1 mm interface layer was intended to melt, while the surrounding material remained solid. The outer walls therefore acted as a constraint, preventing the parts from displacing laterally and promoting uniform melting along the entire joint contour. Thus, a new design concept was adopted: the two specimen halves were locked together mechanically before welding by inserting the protrusion into the recess. In this arrangement, ultrasonic exposure melted only a thin (1 mm) layer of material, while the outer walls remained cold, holding the parts in place and ensuring uniform melting along the entire joint contour [2].
The flexible material used was Creality CR-TPU 95A filament (Creality Co., Ltd., Shenzhen, China) with a diameter of 1.75 mm and a nominal hardness of 95 Shore A. The manufacturer recommended a nozzle temperature of 210–240 °C and a build plate temperature of 25–60 °C [29]. For the hybrid joining experiments, rigid polylactic acid (PLA) filament from the same manufacturer (Creality, 1.75 mm) was used as the counterpart material [30]. The principal properties and typical robotics applications of the TPU material class, compiled from manufacturer data and the general literature, are summarised in Table 1 together with the nominal data of the grade used [31]. All specimens were produced by fused deposition modelling (FDM) 3D printing.
Table 1.
Main properties and applications of TPU relevant to robotics and additive manufacturing. The first four rows show the nominal data for the filaments used in this study, while the remaining rows show typical values for the TPU material class.
2.2. Energy-Director Geometries
The hexagonal energy-director profile, which had previously been used successfully with rigid thermoplastics (ABS, PLA and PETG), was first tested with TPU specimens that had a total joint thickness of 5 mm [9,32,33]. Based on the hypothesis that the high ultrasonic energy absorption of TPU requires a reduction in joint-zone thickness and sharper energy concentration, three additional geometric profiles were designed in SolidWorks 2024 (Dassault Systèmes, Vélizy-Villacoublay, France) and evaluated (Figure 2): (i) a wave-shaped profile with a smooth, curved contact surface to increase the contact area; (ii) a toothed profile consisting of a sequence of 1–2 mm high rectangular projections and recesses; and (iii) pointed profiles with narrowed and sharpened toothed projections to concentrate ultrasonic energy at the tip.
Figure 2.
Geometric energy-directing profiles developed for ultrasonic welding of TPU: a wave-shaped profile (left) and toothed/pointed profile variants (right). The toothed profile features rectangular projections and recesses measuring 1–2 mm in height. Please note that the CAD views are not to scale.
Following the preliminary trials, a refined ‘toothed’ profile was selected for a detailed parametric study (Figure 3). This profile features rectangular projections and recesses, each measuring 1 mm in height, which interlock with the mating part to prevent lateral displacement.
Figure 3.
Toothed energy director profile developed for TPU: (a) a general view in the SolidWorks 2024 (Dassault Systèmes, Vélizy-Villacoublay, France) CAD environment, including a magnified detail of the tooth profile; and (b) the specimens after ultrasonic welding trials. The tooth height is 1 mm, the tooth thickness is d = 0.7–1.0 mm, and the inter-tooth distance is l = 1–3 mm (see Table 2). The CAD view is not to scale.
For the wave-shaped (curved) profile, the underlying rationale—trading a sharp point for a rounded contact surface to enlarge the initial contact area and make the melt-front more repeatable—is well documented in the literature. Chuah et al. compared energy-director shapes in far-field ultrasonic welding of thermoplastics and found that the shape of the director strongly affects heat generation and weld strength independent of other process parameters [8]. Round/curved energy directors have also been shown industrially to reduce part-to-part geometric variability compared with sharp triangular tips, which in high-volume multi-cavity molding improves weld repeatability and reduces the incidence of squeeze-out defects [34]. Rani et al.’s statistical study of ultrasonic-welding parameters likewise found that for glass-fiber-filled composites, a semicircular (curved) energy director produced the highest joint strength, while a triangular one was preferable for the unfilled polymer [10]. A curved director may therefore be preferable to a pointed one when the flow behavior of the material changes, as expected for the elastomeric adherend studied here.
For the toothed profile (sequential rectangular projections/recesses), the closest documented analogue is the family of segmented, or ‘net-like’, energy directors. Yue et al. describe a woven-mesh energy director for thermoplastic composites which distributes multiple discrete contact points across the joint, rather than concentrating energy at a single point. They report improved strength and hygrothermal resistance relative to a single continuous director [11]. The same multi-point logic underlies the keyway-type geometry that was tested by the authors in their earlier work on rigid thermoplastics [2], providing a natural precedent for the toothed design adopted here for TPU [11].
For the pointed profile, the classical justification is the original triangular-energy-director mechanism, whereby stress and strain are highest at the tip, meaning melting initiates there and progresses along the ridge, concentrating ultrasonic energy into the smallest practical contact area and shortening weld time [35,36]. Potente’s foundational work on the principles of ultrasonic welding established this heat concentration mechanism for rigid thermoplastics, and it remains the standard explanation cited in contemporary energy director reviews [36].
Finally, to support the TPU-specific framing of this subsection, two sources are directly relevant. Espinoza’s DETC’04 ASME study involved optimising the ultrasonic welding of a thermoplastic polyurethane (TPU) device that required a hermetic seal. This study used a robust design approach and burst testing to assess weld strength and leak-tightness [12]. This study sets a precedent for the distinct process sensitivity of TPU. Additionally, Bhudolia et al.’s review of ultrasonic welding of thermoplastic composites explicitly identifies polyurethanes as a poorly researched material for energy-directed ultrasonic welding, thereby supporting the novelty of the present TPU energy-director study [20].
2.3. Specimen Design
To determine the effect of tooth geometry, specimens measuring 20 mm by 200 mm with a total thickness of 5 mm were designed, with the 200 mm length divided into three sections. Within each section, the thickness of the tooth (d) and the distance between teeth (l) were varied, while the height of the tooth was kept constant at 1 mm (Table 2). All specimens were asymmetrically designed, i.e., with an unequal wall thickness on either side of the joint. This allowed the thinner side to be placed under the sonotrode, thus minimising the ultrasonic vibration path length to the joint zone.
Table 2.
Geometric parameters of the three test sections used to study the effect of tooth geometry on the quality of TPU–TPU joints.
For the hybrid TPU–PLA joining trials, dog-bone-shaped tensile specimens were prepared using the selected toothed profile described in Section 3.4 (1 mm tooth height, width and pitch). Two configurations with a total thickness of 5 mm or 10 mm were produced, with an asymmetric wall thickness design on both the TPU and PLA sides, so that the thinner wall of each specimen could be placed towards the sonotrode (Figure 4). The specimen edges were designed to coincide exactly upon assembly, with no projections beyond the nominal geometry.
Figure 4.
FDM-printed TPU (white) and PLA (blue) specimens with the toothed interlocking geometry prior to ultrasonic welding, with the outer pair having a total thickness of 10 mm and the inner pair having a total thickness of 5 mm.
To determine whether the toothed energy-director geometry was responsible for the successful welding of TPU, a control group with a flat interface was prepared. These control specimens had plain faying surfaces and were printed with the same parameters as the toothed specimens, but without an energy director or a mating recess. Five control specimens were prepared for each investigated material combination (TPU–TPU, TPU–ABS and TPU–PLA; PETG and other combinations were not tested) and the joint thickness varied from 1.0 to 5.0 mm in 0.2 mm increments. The control specimens were welded using the same equipment and fixturing as the toothed specimens, within the generator settings working range described in Section 2.3 (including the settings selected in Section 3.5). Five toothed specimens were produced and welded for each section and material combination.
Welding was performed using a JYD-2900SP-LCD ultrasonic welding generator. The controllable process parameters were vibration amplitude (A, expressed as a percentage of the maximum sonotrode displacement, corresponding to an amplitude range of approximately 10–30 μm at the lower settings used for TPU) and the pre-weld soft-start ramp settings were FreeAcc and SoftSet. The dimensionless generator settings control the acceleration and softness of the initial vibration ramp-up. Other parameters included welding time and static contact force. For soft materials such as TPU, low static force (10–20 N) was applied to avoid premature deformation and welding times of 1–10 s were used for the thin sections and soft materials investigated in this study. These are the ranges explored throughout the study; the values used at each stage are given in Table 5 (Section 3.6). Specimens were positioned under the sonotrode by hand by the same operator for all experiments. In the second experimental series (Section 3.5), the amplitude and the FreeAcc and SoftSet settings were systematically varied. A dash (“–”) in the results table indicates that a parameter was left unchanged from the previous experiment. As the working width of the sonotrode (approximately 11 mm) was smaller than the 20 mm width of the specimens, wide specimens were welded in two sequential passes.
2.4. Evaluation of Joint Quality
The quality of the joint was assessed both visually and quantitatively. Visual inspection recorded melting at the interface, thermal deformation of the specimen, and adhesion of the material to the sonotrode. The mechanical performance was determined using a universal testing machine (Shenzhen Keepleader Machinery Co., Ltd., Shenzhen, China, model SKM1020, with a 5 kN load cell) to test the specimens to failure. The specimens were clamped in wedge-type jaws (Figure 5) and loaded at a constant crosshead speed of 10 mm/min at a temperature of 20 °C. Five specimens were tested for each welding condition. The testing procedure followed the general provisions of ISO 527-1 [37] and ASTM D638 [38] for tensile testing of plastics. As the bonded area does not correspond to a standard gauge section, the peak load of the joint is reported directly.
Figure 5.
The specimen is fixed between the wedge-type jaws of the universal testing machine.
The peak load (Fmax) and the displacement at failure (mm) were recorded for every welded specimen (Figure 6). Each specimen’s failure mode was classified as interfacial if separation occurred along the weld plane, or cohesive if the specimen tore in the base material away from the weld plane. All reported values are means over five specimens, with the corresponding standard deviation. Individual values for all specimens are given in Tables 5 and 6.
Figure 6.
Peak load (a) and displacement at failure (b) of representative ultrasonically welded TPU–TPU and TPU–PLA joints with a toothed profile, as recorded on the universal testing machine. The joints were welded with A = 80%, FreeAcc = 30% and SoftSet = 20%, for 2–3 s under the weight of the sonotrode, with a specimen width of 20 mm. Each bar represents the group mean ± SD (n = 5). TPU–PLA joints with a total thickness of 5 mm and 10 mm are shown (Table 6). The flat-interface control specimens separated at only 3–9 N and are not shown.
Forces were recorded with the 5 kN load cell of the universal testing machine (SKM1020, Jinan Chengyu Testing Equipment Co., Ltd., Jinan, China; China Certification Center calibration certificate, calibrated 10 September 2025). The load cell is calibrated to ISO 7500-1 Class 1 [13] (permissible relative error ±1% of the indicated force reading). The expanded measurement uncertainty (k = 2, 95% confidence) is ±0.08 N at 5 N and ±0.72 N at 62 N; in both cases it is well below the within-group standard deviation (1–5 N). Only the peak load and the displacement at failure were stored for each specimen, not the full load–displacement curves; individual peak load and displacement values are listed in Table A1 (Appendix A).
The toothed and flat-interface groups were compared for each material combination using the exact two-sided Mann–Whitney U test (n = 5 per group, α = 0.05 significance level), which does not require normally distributed data and is appropriate for small samples. With five specimens per group, the smallest attainable two-sided p-value is 0.008 (2/252). As this is the lower limit for this sample size, the p-values indicate complete separation of the two groups rather than the size of the effect. Therefore, the effect size is reported as the difference in mean peak load with a 95% confidence interval (Welch).
For the purposes of the screening experiments reported in Section 3.2 and Section 3.3, a joint was classified as successful if the contact surfaces of the mated materials reached their melting temperature under ultrasonic vibration, forming a continuous bond in the contact zone that could sustain a measurable load in the subsequent tensile test. All experimental settings and outcomes were recorded in a laboratory logbook.
The weld region was examined in reflected light using a ZEISS Axio Vert A1 inverted microscope (Carl Zeiss Microscopy, Oberkochen, Germany), with cross-sections cut through the weld being examined at 50× and 200× magnification. The cross-sections were not polished and images were recorded using the microscope’s camera.
2.5. Comparative Analysis of Materials
As the quality of specimen fixation directly affects the measured peak load and elongation, all specimens—flat-interface and toothed, TPU, PLA and hybrid—were tested under identical clamping conditions. The specimens were held between opposing wedge-type jaws, tightened to the same torque and aligned along the centreline of the grips (Figure 5), so that bending moments, pre-stressing and slippage, which would otherwise distort the axial stress distribution, were avoided. Standardised fixation ensures that the differences in measured strength reported in Section 3.9 reflect the joint and the material rather than the test setup.
Thermoplastic polyurethane (TPU) is a melt-processable thermoplastic elastomer with a low initial modulus and an elongation at break of several hundred percent. Hence, the displacement at failure of a welded TPU specimen differs markedly from that of a rigid engineering polymer [39]. Consequently, a joint between two TPU halves can extend by tens of millimetres before failing, whereas a joint with a rigid PLA half is constrained to much smaller extension.
Two quantities are recorded and used throughout Section 3.9. The peak load is the joint’s maximum load-bearing capacity. Displacement at failure characterises the joint’s deformability and, together with the failure mode, indicates whether failure occurred in the weld or the base material. Both quantities are sensitive to welding parameters since these govern the degree of interfacial melting. Insufficient energy produces a low peak load, while excessive energy causes thermal degradation or expulsion of melt from the interface, which likewise reduces the measured strength [40].
3. Results
3.1. Flat-Interface Baseline: Exhaustion of the Process Window
Before introducing any interlocking geometry, a flat-interface baseline was established to determine if ultrasonic welding could be used to join FDM-printed parts with plane faying surfaces in TPU, given any combination of accessible geometry and process parameters. Three material pairs—TPU–TPU, TPU–ABS and TPU–PLA—with plane, unstructured faying surfaces were produced directly by fused deposition modelling without the use of any energy director. The total joint thickness was varied from 1.0 to 5.0 mm in increments of 0.2 mm for each pair, resulting in 21 thickness levels per pair and 63 geometric conditions in total. Five specimens were welded for each material combination. For each geometric condition, the generator parameters were varied across the full working range of the equipment: vibration amplitude from 50 to 100%, static contact force from 10 to 20 N, and welding time from 5 to 7 s. Welding was performed at the nominal operating frequency of 20 kHz, with automatic resonance tracking. This was done using the same JYD-2900SP-LCD system and fixturing as was used for all subsequent experiments.
No combination of thickness and process parameters produced a weld (see Table 3). In every case, the mated surfaces separated adhesively at the faying plane under very low force after the welding cycle. There was no visible melt front at the interface, nor any material transfer between the two surfaces. Therefore, the flat-interface specimens carried no weld load; the peak separation loads measured were only 5.0 ± 1.6 N (range 3–7 N) for TPU–TPU, 7.0 ± 0.7 N (range 6–8 N) for TPU–ABS, and 8.0 ± 0.7 N (range 7–9 N) for TPU–PLA (Table 6). Where melting was observed, it occurred at the sonotrode contact surface rather than the faying surface. This was accompanied by local deformation of the TPU and, at the highest amplitudes, adhesion of the specimen to the horn.
Table 3.
Flat-interface baseline (control group): material pairs, thickness range and outcome. All specimens were welded with plane faying surfaces and without an energy director across the full accessible range of generator parameters at each thickness level. Five specimens were welded for each material combination. The force in parentheses is the range of separation forces measured on the five specimens.
Three conclusions can be drawn from this baseline. Firstly, insufficient thinning is not the cause of the failure: reducing the vibration path through the damping adherend by a factor of five, from 5.0 to 1.0 mm, produced no joint at any of the 21 intermediate levels. Secondly, the failure is not due to an unsuitable parameter set since the accessible process window was exhausted at every thickness level without altering the outcome. Thirdly, the inherent surface texture of FDM-printed parts—the regular 0.2 mm layer ridges that act as natural micro-energy directors in rigid thermoplastics and often allow director-free welding of PLA and ABS—is ineffective in TPU. Therefore, the absence of a geometrically stable interfacial stress concentrator is identified as the governing obstacle to ultrasonic welding of elastomeric adherends, rather than the vibration path length or the generator setting. This result motivated the interlocking profiles developed in Section 2.2.
3.2. Preliminary Experiments with the Standard Hexagonal Geometry
Initial trials on TPU specimens (5 mm total thickness) using the hexagonal energy-director profile that had previously provided a stable, strong joint for rigid thermoplastics failed completely: no joint formed, the material did not melt sufficiently and only weak surface adhesion was observed in the welding zone. This behaviour can be attributed to TPU’s intrinsic ability to absorb and dissipate ultrasonic vibration as heat rather than transmitting it efficiently to the energy directors. This is compounded by the fact that the total joint thickness of 5 mm is too large relative to the original design intent for rigid polymers.
3.3. Development and Screening of New Energy-Director Geometries
Figure 2 shows the wave-shaped, toothed and pointed profiles that were tested to evaluate whether a geometry with sharper, more concentrated energy direction could compensate for the high vibrational damping of TPU. Some specimens with a total thickness of 2 mm were successfully joined, which confirms the importance of reducing the thickness of the joint zone. However, stable joining could not be achieved for most other specimens at this stage because suitable generator settings for TPU had not yet been selected. Thus, the theoretical advantage of the sharply pointed profiles could not be conclusively demonstrated.
Three principles were established for the ultrasonic welding of flexible polymers at this screening stage: (1) The total material thickness in the joint zone should be minimised to a maximum of 5 mm owing to TPU’s strong absorption of ultrasonic energy. (2) The energy-directing geometry should concentrate ultrasonic energy into a small volume, for example, sharp edges and small-cross-section projections. (3) Unlike rigid polymers, TPU requires the precise, individual selection of generator parameters: vibration amplitude from 50 to 100%, static contact force from 10 to 20 N, and welding time from 5 to 7 s. These parameters are selected for each specific geometry and thickness (screening stage, Table 5).
3.4. Effect of Geometric Profile Parameters on TPU–TPU Joints
Using the three-section specimens described in Section 2.3 (Table 2), with an initial generator setting of A = 100%, FreeAcc = 30 and SoftSet = 20, and a welding time of 2–4 s, the toothed profile with the densest tooth spacing (test Section 1 (d = 0.7 mm and l = 1 mm)) produced the strongest and most compact joint. The section with d = 0.8 mm and l = 2 mm produced a weak joint with unwelded areas, while the section with d = 1.0 mm and l = 3 mm failed to join altogether. These results demonstrate that the dense combination (d = 0.7 mm, l = 1 mm) produced the strongest joint of the three combinations tested and that joint quality deteriorated significantly when the inter-tooth distance increased from 1 to 3 mm. As d and l were varied together, it is not possible to distinguish their separate effects. Five specimens were welded for each section.
3.5. Selection of Ultrasonic Generator Operating Modes
A second experimental series was conducted using specimens with the most successful geometric parameters from Section 3.4 (d ≈ 0.7–1.0 mm, l = 1 mm, total thickness 5 mm). This series varied amplitude (A), FreeAcc and SoftSet to identify a combination that would produce a strong joint without causing thermal deformation (see Table 4). The quality of the joints in this series was classified visually (joint formed, overheating, sticking to the sonotrode, deformation); tensile strength was only measured for the selected setting.
Table 4.
Results of the ultrasonic generator operating mode selection for TPU–TPU joints (5 mm total thickness). A dash (“–”) indicates that the parameter remained unchanged from the previous experiment.
Even a short exposure of 2–4 s at the maximum amplitude setting (A = 100%) caused rapid overheating: the material melted not only in the joint zone, but also at the sonotrode contact surface. This resulted in the material adhering to the sonotrode and undergoing irreversible thermal deformation. Increasing the FreeAcc and SoftSet to 60/30 (Experiment 3) resulted in poorer joint quality, suggesting that TPU requires a ‘soft’, gradual ramp-up of vibration rather than an abrupt one. Experiment 5, with a welding time of 2–3 s and minimal static force (contact limited to the weight of the sonotrode), was selected: the combination of A = 80%, FreeAcc = 30 and SoftSet = 20 produced a strong, homogeneous joint with negligible deformation and no sticking to the sonotrode.
3.6. Selected Conditions for Ultrasonic Welding of TPU
The following conditions were selected for ultrasonic welding of TPU–TPU joints, combining the results of Section 3.4 and Section 3.5: a toothed energy-director profile with a tooth thickness of 0.7–1.0 mm, a pitch of 1 mm and a tooth height of 1 mm; an asymmetric specimen design with minimal material thickness on the sonotrode side; and a JYD-2900SP-LCD generator setting of A = 80%, FreeAcc = 30%, SoftSet = 20%, welding time of 2–3 s and minimum static force of 10 N (contact under the sonotrode’s own weight only). The total joint thickness should not exceed 5 mm (see Table 5).
Table 5.
Process parameters by experimental stage.
3.7. Effect of Printing Parameters on Weld Quality
Although this study focuses on the welding process itself, it was observed that the quality of FDM printing can also influence the outcome. TPU appears to be more susceptible than rigid polymers to local over- or under-heating during printing. This can result in weak interlayer adhesion or microvoids, which may act as stress concentrators and reduce the strength of the subsequent welded joint. A systematic investigation of this interaction is planned for future research.
3.8. Joining TPU to Rigid PLA by Ultrasonic Welding
The selected toothed geometry was used to ultrasonically weld TPU and PLA specimens with a total thickness of 5 mm and 10 mm (Figure 4). It was found that joining was fundamentally possible and that strong joints could be obtained in individual sections (Figure 7 and Figure 8). Due to the different chemical natures of the two polymers, molecular intermixing is not expected, so the bond is attributed to mechanical interlocking within a thin contact zone. This may be assisted by the fibrous microstructure produced by FDM printing. This interpretation is based on macroscopic observations and low-magnification optical micrographs (Figure 9). No spectroscopic examinations or electron microscopy of the interface were carried out in this study. The measured peak loads are reported in Section 3.9.
Figure 7.
Ultrasonically welded TPU–PLA joints: (a) Specimens with a total thickness of 5 mm showing a continuous, translucent weld zone; (b) specimen with a total thickness of 10 mm after tensile testing showing tearing of the base materials rather than separation at the weld line. Subfigure labels (a,b) correspond to the left and right images, respectively.
Figure 8.
Cross-section of the toothed joint interface between the PLA (blue) and TPU (white) specimens with a total thickness of 10 mm, showing the interlocking of the teeth and the melted zone. Digital macro photograph of the cross-section; see Section 3.8 for optical micrographs.
Figure 9.
Reflected-light optical micrographs of the weld region of ultrasonically welded joints: (a) TPU–PLA, 50×; (b) TPU–PLA, 200×; (c) TPU–TPU, 200×.
Several process-related features and limitations were identified. Firstly, PLA transmits ultrasonic vibration efficiently to the joint zone as a rigid polymer, whereas TPU rapidly absorbs this energy and converts it to heat. Consequently, most of the heating is expected to occur at the PLA surface. Molten PLA may penetrate the TPU teeth, and molten TPU may fill the spaces between the PLA teeth. This would effectively make the TPU act as a filler material. Secondly, when a thin TPU layer was positioned closest to the sonotrode, local surface melting and severe deformation were observed, possibly due to residual micro-air bubbles from the 3D printing process or uneven manual application of static force. Thirdly, since the width of the sonotrode (~11 mm) was smaller than that of the specimen (20 mm), welding was performed in two sequential sections. Incomplete cooling of the first section before welding the second could result in additional heat accumulation and deformation.
The most notable result was obtained for the 10 mm total-thickness specimens: despite the strong energy absorption of TPU, macroscopic inspection of the cross-section (Figure 8) suggests that both materials softened or melted in the joint zone, whether the melts mixed at the interface was not determined. The bond failed cohesively in the tensile test, tearing the base material away from the weld plane rather than separating the weld seam (Section 3.9).
Reflected-light optical micrographs of the weld region were taken at 50× and 200× magnification using a ZEISS Axio Vert A1 inverted microscope (ZEISS, Oberkochen, Baden-Württemberg, Germany). The specimens were cross-sectioned and examined without polishing (Figure 9). At 50× magnification (Figure 9a), the regular layer ridges of the printed TPU–PLA parts are visible, along with a central region of glossy, deformed-looking material, which we believe to be the weld zone. At 200× magnification (Figure 9b), the TPU–PLA joint shows a bright band and a layered zone containing small bright inclusions at the transition between the translucent and darker materials. In contrast, the TPU–TPU joint (Figure 9c) exhibits smooth, elongated, flow-like striations containing small bright inclusions, which may represent voids or debris. The depth of field at these magnifications is small, meaning that parts of each image are out of focus. Therefore, the micrographs demonstrate that the material in the weld zone was deformed and displaced; however, they do not permit an assessment of bond-line continuity, void content, tooth deformation, or intermixing of the melts. Polished cross-sections examined by optical microscopy or SEM are needed for that.
3.9. Quantitative Evaluation of Joint Strength
All flat-interface and toothed configurations were tested on the universal testing machine until failure occurred, under the conditions given in Section 2.5. The 63 conditions mentioned in Section 3.1 refer to the flat-interface baseline screening (3 material pairs × 21 thickness levels); in every case, no weld formed, and the flat-interface group in Table 6 comprises n = 5 specimens per pair. One specimen was tested at each thickness level in this screening (63 specimens in total); the outcome was the same in every case—no weld formed. The tensile groups reported in Table 6 are the final toothed-profile tests at the confirmed welding thicknesses, with n = 5 specimens per group. Individual values for all specimens are listed in Table A1 (Appendix A). Figure 6 shows the group means ± SD of the peak load and displacement at failure.
Table 6.
Peak load and displacement at failure by group (tensile test at 10 mm/min and 20 °C). Mean ± SD, n = 5 per group. Individual specimen values are listed in Table A1 (Appendix A).
The quantitative data confirm the qualitative trends established in the preceding sections. In the flat-interface group, the halves separated at peak loads of just 5.0 ± 1.6 N for TPU–TPU, 7.0 ± 0.7 N for TPU–ABS, and 8.0 ± 0.7 N for TPU–PLA (ranging from 3 to 7 N, 6 to 8 N, and 7 to 9 N, respectively) at displacements of only 1.0 to 2.1 mm. There was no melt front at the interface, meaning no weld had formed. This residual load most likely reflects friction and mechanical contact between the faying surfaces rather than a bonded joint. By contrast, the toothed joints carried considerably higher loads (Table 6). The group means ± SD (n = 5) of the peak load were 29.0 ± 1.6 N for TPU–TPU and 39.0 ± 1.6 N at 5 mm and 62.0 ± 3.4 N at 10 mm for TPU–PLA, reached at displacements of 72.0 ± 3.8 mm, 43.0 ± 1.6 mm, and 31.0 ± 2.5 mm, respectively (see Figure 6 and Table 6). Compared with TPU–TPU joints, those made from TPU–PLA withstood peak loads that were approximately 1.3 and 2.1 times higher at 5 and 10 mm, respectively, while failing at displacements that were approximately 40% and 57% smaller. Relative to the mean flat-interface load of the same pair (8.0 N), the toothed TPU–PLA joints carried approximately five and eight times the load at 5 and 10 mm, respectively.
This difference reflects the contrasting compliance of the two adherends. In the TPU–TPU joint, both halves are elastomeric, so the load is carried at a high elongation rate and the specimen extends by more than 70 mm before failure. In contrast, in the TPU–PLA joint, the rigid PLA half does not deform significantly, confining the extension to the TPU half and the interface. Consequently, the joint reaches a higher load at a shorter displacement. For the hybrid joints, the failure mode depended on the total thickness. At 5 mm, the specimens failed interfacially along the weld plane. In contrast, at 10 mm, four out of five specimens failed cohesively in the base material without separation of the weld seam (Table 6; mean peak load of 39.0 ± 1.6 N at 5 mm and 62.0 ± 3.4 N at 10 mm). Therefore, the values for this configuration represent the lower bound of the joint’s strength. Cohesive failure only shows that the weld carried at least the load at which the base material failed. The base material was not tested separately, so the result does not show that the joint is stronger than the base material.
The two-sided exact Mann–Whitney U test was applied separately to the TPU–TPU and TPU–PLA groups, comparing the five peak loads of the toothed and flat-interface groups. The resulting p-values were p = 0.008 for both groups (the smallest attainable value for n = 5 versus n = 5 is 0.008, so these p-values are at their lower limit, indicating complete separation of the groups rather than the size of the effect). The difference in mean peak load between the toothed and flat groups, with its 95% confidence interval (Welch), is TPU–TPU: 24.0 N [21.7, 26.3]; TPU–PLA (5 mm): 31.0 N [29.1, 32.9], calculated from the group means and SDs in Table 6. Section 3.2 (hexagonal-director trial) and Section 3.3 (profile screening) compare the toothed profile with other energy-director geometries. The flat-interface control compares it with the absence of a director. Further energy-director geometries will be designed and compared in future work.
4. Discussion
As reported in Section 3.1, the flat-interface control group establishes that an energy-directing geometry is not only beneficial for TPU, but necessary. The sonotrode imposes a displacement amplitude rather than a stress. With a Young’s modulus of around 20 MPa, TPU is approximately two orders of magnitude more compliant than rigid thermoplastics, for which conventional energy directors were developed (PLA ≈ 3500 MPa and ABS ≈ 2200 MPa). This means that the TPU wall acts as a compliant element in series with the joint plane, with the imposed stroke being accommodated almost entirely by the elastic deformation of the bulk. Consequently, the relative interfacial displacement required to generate frictional heating approaches zero. The volumetric heat generation rate under cyclic loading, q = π f E″ ε02, is proportional to the square of the strain amplitude, ε0. The strain is largest in the compliant bulk beneath the sonotrode and smallest at the faying surface; therefore, most of the heat is generated away from the joint. Furthermore, this heat cannot reach the joint by conduction; with a thermal diffusivity of approximately 0.1 mm2/s, the conduction length over a 3-s weld is around 0.55 mm. Consequently, the interface must be heated in situ rather than by conduction from the contact face. This also explains why the surface of the sonotrode reached its Vicat softening point (approximately 99 °C) and adhered to the horn at high amplitude, while the interface itself remained unmelted. For the hybrid pairs, the mechanism is more complex: the rigid adherend transmits vibrations efficiently, reaching its processing window, while the TPU remains cold. This means that a flat interface cannot bring both surfaces into a mutually compatible viscosity range simultaneously. However, this is only an interpretation: temperature was not measured, no numerical simulations were performed and the dynamic modulus of TPU at 20 kHz is higher than its quasi-static value of approximately 20 MPa. Therefore, the stiffness ratios quoted here are upper bounds. Infrared thermography or embedded thermocouples, together with a coupled thermo-viscoelastic finite-element model, are planned to verify this.
The behaviour of the as-printed surface texture is informative in itself. In rigid thermoplastics, the 0.2 mm layer ridges left by material extrusion act as distributed micro-energy directors and are often enough to allow director-free welding. However, in TPU, this is not the case for three reasons. Firstly, at a modulus of approximately 20 MPa, the asperities are flattened by the static contact force before vibration is applied, which eliminates the concentration they would otherwise provide. Secondly, any residual texture recovers elastically with each cycle, rather than sustaining a fixed contact point. This returns the dissipation to the bulk. Thirdly, the air retained in the layer valleys is not displaced by a melt front. This leaves a thermally insulating layer at the very plane that must be heated. TPU therefore requires not a stress concentrator as such, but rather a geometrically stable, mutually interlocking one that maintains a defined relative displacement at the tooth flanks under static load. This is consistent with the sharp degradation of joint quality observed in Section 3.4 when the inter-tooth distance was increased from 1 to 3 mm, and with the failure of the hexagonal profile in the authors’ earlier work, which was dimensioned for adherends that were two orders of magnitude stiffer.
The results show that the ultrasonic welding of TPU differs fundamentally from that of rigid thermoplastics due to TPU’s high capacity to absorb and dampen ultrasonic vibrations. While rigid polymers such as ABS, PLA and PETG can be welded using relatively thick, hexagonal energy-director geometries, TPU requires: (i) strict limitation of total joint thickness to ≤5 mm; (ii) an energy-director geometry that concentrates vibrational energy; in this study, this was achieved using a densely spaced toothed profile with a 1 mm pitch; and (iii) individually tuned generator settings. This is because excessive amplitude and an excessively fast vibration ramp-up (high FreeAcc/SoftSet) lead to overheating, sticking or incomplete melting rather than stronger joints. As the tooth thickness and spacing were varied together (Table 2), the data only identify a working combination, rather than the effect of each parameter separately.
Successfully joining TPU to rigid PLA shows that, in principle, ultrasonic welding can produce hybrid flexible–rigid polymer assemblies without the need for adhesives or mechanical fasteners. The failure mode depended on the total thickness; the joints failed at the weld line at 5 mm, and due to tearing of the base material at 10 mm. Within the range studied, this suggests that a thicker rigid PLA component helps direct heat generation towards the interface. One possible explanation for this is the significant difference in acoustic impedance between the two polymers. With the quasi-static moduli quoted above (approximately 3500 MPa for PLA and 20 MPa for TPU), and given that the two polymers have similar densities, the impedance ratio is approximately 13. This means that most of the wave is reflected at the interface, resulting in concentrated strain and frictional heating. In contrast, in TPU–TPU, the vibration must traverse material that dissipates it as heat. As the dynamic modulus of TPU at 20 kHz is higher than its quasi-static value, the true ratio is lower. This favours interfacial melting. Whether the melts mixed at the interface was not determined, because neither the macroscopic inspection (Figure 8) nor the micrographs in Figure 9 resolve it. Only two total thicknesses were tested for the hybrid joints, so thickness cannot be separated from other differences between the two series.
Several limitations should be noted. All specimens were positioned manually and static force was applied by hand in the screening stages. In the final settings, static force was limited to the weight of the sonotrode. The process was found to be highly sensitive to sonotrode/specimen alignment and the uniformity of static force application, which limited reproducibility under manual control. The load cell was calibrated to ISO 7500-1 Class 1 (±1% of reading; China Certification Center, 10 September 2025). The expanded measurement uncertainty is ±0.08 N at 5 N and ±0.72 N at 62 N, which is below the within-group standard deviation at all load levels and does not affect the group comparisons or the failure-mode classification. The elasticity of TPU means that joints subjected to repeated dynamic loading or sustained tensile strain may weaken over time. This durability aspect was not quantitatively assessed in this study, but should be examined in future work through methods such as cyclic loading or long-term creep testing. Furthermore, the interaction between FDM printing quality (e.g., interlayer adhesion and microvoids) and the resulting weld strength (see Section 3.7) merits systematic investigation. Finally, translating the present manually controlled process to an industrial setting will require the consistent and automated application of static force, the use of dedicated specimen-fixturing devices and the extensive optimisation of generator settings across a wider range of geometries and material combinations. Microstructural characterisation was limited to the reflected-light micrographs in Figure 9. These do not resolve the interface sufficiently to assess bond-line continuity, void content, tooth deformation or thermal degradation. Optical or electron microscopy of polished sections, as well as ATR-FTIR analysis of the mating fracture surfaces, were not performed. Therefore, statements regarding the interfacial structure, including the melted zone seen in Figure 8, are based on macroscopic observation and require confirmation in future work. Tooth thickness and spacing were varied together; generator settings were visually compared rather than compared by strength; and no temperature measurements were taken. The statistical comparison is based on five specimens per condition. Further energy-director geometries, in addition to the hexagonal, wave-shaped, pointed and toothed profiles examined here, will be designed and compared in future work.
5. Conclusions
This study established the relationships between processes and geometry for ultrasonically welding flexible TPU and hybrid joining it to rigid PLA. The main conclusions are as follows:
- Plane faying surfaces of FDM-printed TPU did not weld. In 63 pair-thickness conditions (TPU–TPU, TPU–ABS and TPU–PLA; 1.0–5.0 mm in 0.2 mm increments; n = 5 per pair), no weld formed and the halves separated at mean peak loads of 5.0–8.0 N.
- The hexagonal energy director, which works for ABS, PLA and PETG, did not weld TPU at a total thickness of 5 mm.
- An interlocking toothed profile (tooth thickness 0.7–1.0 mm, pitch 1 mm, height 1 mm) was found to weld TPU–TPU at total thicknesses of up to 5 mm, with a peak load of 29.0 ± 1.6 N (n = 5). The effects of varying tooth thickness and spacing together are not resolved.
- The selected generator settings for the JYD-2900SP-LCD system were: A = 80%, FreeAcc = 30%, SoftSet = 20%, weld time = 2–3 s, and static force was limited to the weight of the sonotrode assembly (10 N). A = 100% caused the TPU to overheat and stick to the sonotrode, and a faster ramp (60/30) resulted in weaker joints.
- With the same geometry, TPU was joined to PLA. At 5 mm, the joints failed at the weld line at 39.0 ± 1.6 N. At 10 mm, four of the five specimens failed in the base material at 62.0 ± 3.4 N; therefore, the weld can carry at least this load. Whether the melts mixed at the interface was not determined.
- These results apply to quasi-static tensile loading of manually positioned specimens. Polished-section microscopy, temperature measurement, single-factor tooth studies and fatigue and creep tests are required before the joints can be approved for use in soft robotics.
Author Contributions
Conceptualization, H.C.; methodology, H.C.; validation, D.Z., S.C.; formal analysis, S.G.; investigation, G.C.; resources, S.C.; data curation, S.G.; writing—original draft preparation, D.Z.; writing—review and editing, S.G.; visualization, A.K.; supervision, D.Z.; project administration, A.K.; funding acquisition, H.C. All authors have read and agreed to the published version of the manuscript.
Funding
The research was supported by the Higher Education and Science Committee of MESCS RA (Research project № 25AA-2D054).
Data Availability Statement
The data presented in this study are available on request from the corresponding author.
Conflicts of Interest
The authors declare no conflicts of interest.
Appendix A
Table A1.
Individual peak load (N) and displacement at failure (mm) for all specimens. Only these two quantities were stored by the machine; full load–displacement curves were not recorded. Tensile test: 10 mm/min, 20 °C, SKM1020, 5 kN load cell calibrated to ISO 7500-1 Class 1.
References
- Dzedzickis, A.; Petronienė, J.J.; Petkevičius, S.; Bučinskas, V. Soft Grippers in Robotics: Progress of Last 10 Years. Machines 2024, 12, 887. [Google Scholar] [CrossRef] [Scilit]
- Chibukhchyan, H.; Yukhanaev, G.; Grigoryan, S.; Zakaryan, N. The Effect of Joint Geometry and Thermoplastic Type on the Ultrasonic Welding Strength of Fused Deposition Modeling Components. Eng. Technol. Appl. Sci. Res. 2026, 16, 37577–37583. [Google Scholar] [CrossRef] [Scilit]
- Hopmann, C.; Dahlmann, R.; Weihermüller, M.; Wipperfürth, J.; Sommer, J. Determination of the Frequency- and Temperature-Dependent Stiffness and Damping Properties of Thermoplastics for the Prediction of the Vibration and Heating Behaviour during Ultrasonic Welding. Weld. World 2023, 67, 435–445. [Google Scholar] [CrossRef] [Scilit]
- Jongbloed, B.; Teuwen, J.; Palardy, G.; Fernandez Villegas, I.; Benedictus, R. Continuous Ultrasonic Welding of Thermoplastic Composites: Enhancing the Weld Uniformity by Changing the Energy Director. J. Compos. Mater. 2020, 54, 2023–2035. [Google Scholar] [CrossRef] [Scilit]
- Richter, F.; Wu, D. Interfacial Adhesion between Dissimilar Thermoplastics Fabricated via Material Extrusion-Based Multi-Material Additive Manufacturing. Mater. Des. 2025, 252, 113688. [Google Scholar] [CrossRef] [Scilit]
- Khatri, B.; Roth, M.F.; Balle, F. Ultrasonic Welding of Additively Manufactured PEEK and Carbon-Fiber-Reinforced PEEK with Integrated Energy Directors. J. Manuf. Mater. Process. 2023, 7, 2. [Google Scholar] [CrossRef] [Scilit]
- Villegas, I.F. Ultrasonic welding of advanced thermoplastic composites: An investigation on energy-directing surfaces. Adv. Polym. Technol. 2010, 29, 112–121. [Google Scholar] [CrossRef] [Scilit]
- Chuah, Y.K.; Chien, L.-H.; Chang, B.C.; Liu, S.-J. Effects of the shape of the energy director on far-field ultrasonic welding of thermoplastics. Polym. Eng. Sci. 2000, 40, 157–167. [Google Scholar] [CrossRef] [Scilit]
- Tiwary, V.K.; Malik, V.R. Ultrasonic Welding of Similar/Dissimilar MEX-3D Printed Parts Considering Energy Director Shape, Infill, Welding Time and Amplitude. J. Mater. Res. Technol. 2025, 84, 5111–5131. [Google Scholar] [CrossRef] [Scilit]
- Rani, R.M.; Suresh, K.S.; Prakasan, K.; Rudramoorthy, R. A Statistical Study of Parameters in Ultrasonic Welding of Plastics. Exp. Tech. 2007, 31, 53. [Google Scholar] [CrossRef] [Scilit]
- Yue, D.; Zhao, G.; Pan, J.; Liu, J.; Quan, D. Ultrasonic welding of thermoplastic composites with woven mesh energy directors: Enhanced strength and hygrothermal resistance. J. Mater. Res. Technol. 2025, 36, 9699–9712. [Google Scholar] [CrossRef] [Scilit]
- Espinoza, A.A.; Renaud, J.E. An Optimization Study of the Ultrasonic Welding of Thin Film Polymers. In Proceedings of the DETC’04, ASME 2004 Design Engineering Technical Conferences, Salt Lake City, UT, USA, 28 September–2 October 2004. [Google Scholar]
- Fernandez Villegas, I. Ultrasonic Welding of Thermoplastic Composites. Front. Mater. 2019, 6, 291. [Google Scholar] [CrossRef] [Scilit]
- Ultrasonic Resistance Welding Process and Apparatus. U.S. Patent No. 12,240,051, 4 March 2025. Available online: https://image-ppubs.uspto.gov/dirsearch-public/print/downloadPdf/12240051 (accessed on 7 October 2026).
- Liu, S.J.; Lin, W.F.; Chang, B.C.; Wu, G.M.; Hung, S.W. Optimizing the Joint Strength of Ultrasonically Welded Thermoplastics. Adv. Polym. Technol. 1999, 18, 125–135. [Google Scholar] [CrossRef] [Scilit]
- Levy, A.; Le Corre, S.; Fernandez Villegas, I. Modeling of the Heating Phenomena in Ultrasonic Welding of Thermoplastic Composites with Flat Energy Directors. J. Mater. Process. Technol. 2014, 214, 1361–1371. [Google Scholar] [CrossRef] [Scilit]
- Palardy, G.; Fernandez Villegas, I. On the Effect of Flat Energy Directors Thickness on Heat Generation during Ultrasonic Welding of Thermoplastic Composites. Compos. Interfaces 2017, 24, 203–214. [Google Scholar] [CrossRef] [Scilit]
- Brancewicz-Steinmetz, E.; Sawicki, J.; Byczkowska, P. The Influence of 3D Printing Parameters on Adhesion between Polylactic Acid (PLA) and Thermoplastic Polyurethane (TPU). Materials 2021, 14, 6464. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Ribeiro, M.; Sousa Carneiro, O.; Ferreira da Silva, A. Interface Geometries in 3D Multi-Material Prints by Fused Filament Fabrication. Rapid Prototyp. J. 2019, 25, 38–46. [Google Scholar] [CrossRef] [Scilit]
- Bhudolia, S.K.; Gohel, G.; Leong, K.F.; Islam, A. Advances in Ultrasonic Welding of Thermoplastic Composites: A Review. Materials 2020, 13, 1284. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Fu, X.; Yuan, X.; Li, G.; Wu, Y.; Tong, H.; Kang, S.; Luo, J.; Pan, Z.; Lu, W. A study on ultrasonic welding of thermoplastics with significant differences in physical properties under different process parameters. Mater. Today Commun. 2022, 33, 105009. [Google Scholar] [CrossRef] [Scilit]
- Unnikrishnan, T.G.; Kavan, P. A review study in ultrasonic-welding of similar and dissimilar thermoplastic polymers and its composites. Mater. Today Proc. 2022, 56, 3294–3300. [Google Scholar] [CrossRef] [Scilit]
- RapidDirect. What Is Ultrasonic Welding: Working Principle, Applications, Advantages; RapidDirect: Shenzhen, China, 2025; Available online: https://rapiddirect.com/blog/ultrasonic-welding (accessed on 7 October 2026).
- Zhi, Q.; Li, Y.; Tan, X.; Hu, Y.; Ma, Y. Ultrasonic Welding of Acrylonitrile—Butadiene—Styrene Thermoplastics without Energy Directors. Materials 2024, 17, 3638. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Fu, X.; Wu, X.; Huang, G.; Li, W.; Kang, S.; Wang, L.; Luo, J.; Pan, Z.; Lu, W. Fusion Bonding Possibility for Incompatible Polymers by the Novel Ultrasonic Welding Technology: Effect of Interfacial Compatibilization. ACS Omega 2022, 7, 14797–14806. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Singh Rana, R.; Singh, I.; Kumar Sharma, A. Ultrasonic Welding of Printed/Molded Sustainable Polymer Specimens with Energy Directors. Ultrasonics 2023, 134, 107078. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- M’Bengue, M.S.; Mesnard, T.; Chai, F.; Maton, M.; Gaucher, V.; Tabary, N.; García-Fernandez, M.J.; Sobocinski, J.; Martel, B.; Blanchemain, N. Evaluation of a Medical Grade Thermoplastic Polyurethane for the Manufacture of an Implantable Medical Device: The Impact of FDM 3D-Printing and Gamma Sterilization. Pharmaceutics 2023, 15, 456. [Google Scholar] [CrossRef] [Scilit] [PubMed] [PubMed Central]
- Mousavi, S.; Howard, D.; Wu, S.; Wang, C. An Ultrasensitive 3D Printed Tactile Sensor for Soft Robotics (TPU/PLA-graphene, FDM). arXiv 2018, arXiv:1810.09236. [Google Scholar]
- Creality Co., Ltd. CR-TPU Filament (TPU 95A, 1.75 mm): Product Specification and Technical Data; Shenzhen, China. Available online: https://crealityuae.ae/products/filament-creality-cr-tpu-black-1kg-1-75mm (accessed on 7 October 2026).
- Creality Co., Ltd. PLA Filament, 1.75 mm: Product Specification and Technical Data; Shenzhen, China. Available online: https://teams.public.onecdn.static.microsoft/evergreen-assets/safelinks/2/atp-safelinks.html (accessed on 7 October 2026).
- SpecialChem. Thermoplastic Polyurethane: Key Properties, Processing, and Applications. Available online: https://www.specialchem.com/plastics/guide/thermoplastic-polyurethanes-tpu (accessed on 7 October 2026).
- Tarrés, N.; Garcia-Romeu, M.L.; Ferrer, I. On the Interlaminar Bonding Adhesion of the PLA-TPU Printed Multimaterial. Int. J. Adv. Manuf. Technol. 2025. [Google Scholar] [CrossRef] [Scilit]
- Adhindra, V.S.; Vins, B.; Singh, J.; Gupta, A. Optimizing Mechanical Performance of 3D-Printed PLA–TPU Composites through Heat Treatment and Geometric Interlocking. Proc. Inst. Mech. Eng. Part E J. Process Mech. Eng. 2025. online first. [Google Scholar] [CrossRef] [Scilit]
- Savitski, A. Round Energy Directors for Ultrasonic Welding; Industrial Process Reference on Round vs. Sharp Energy Director Consistency; ASSEMBLY Magazine: Elk Grove Village, IL, USA, 3 September 2015. [Google Scholar]
- ASSEMBLY Magazine. Joint Design for Ultrasonic Welding; ASSEMBLY Magazine: Elk Grove Village, IL, USA, 2019. [Google Scholar]
- Potente, H. Ultrasonic welding—Principles & theory. Mater. Des. 1984, 5, 228–234. [Google Scholar] [CrossRef] [Scilit]
- ISO 527-1:2019; Plastics—Determination of tensile properties—Part 1: General principles. International Organization for Standardization: Geneva, Switzerland, 2019.
- ASTM D638-22; Standard Test Method for Tensile Properties of Plastics. ASTM International: West Conshohocken, PA, USA, 2022.
- Lang, L.; Antunes, R.; Dutra, T.A.; Lima de Aguiar, M.; Pereira, N.; Gaspar, P.D. Mechanical Characterization and Computational Analysis of TPU 60A: Integrating Experimental Testing and Simulation for Performance Optimization. Materials 2025, 18, 240. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Zhi, Q.; Li, Y.; Shu, P.; Tan, X.; Tan, C.; Liu, Z. Double-Pulse Ultrasonic Welding of Carbon-Fiber-Reinforced Polyamide 66 Composite. Polymers 2022, 14, 714. [Google Scholar] [CrossRef] [Scilit] [PubMed]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.