Abstract
This study systematically investigates the gas–liquid phase transition heat transfer characteristics and volatilization loss behavior of magnetic liquid sealing devices under high-temperature and high-speed operating conditions. A magneto-thermal flow-coupled numerical model was established using ANSYS Maxwell (2025 R1) and Fluent (2025 R1) software to simulate and analyze the influence of rotational speed, solid content, and shaft diameter on the temperature distribution and gas-phase evolution of the magnetic liquid within the sealing gap. An experimental platform was also constructed for validation. The research indicates that increasing rotational speed significantly intensifies the vaporization of magnetic liquid, with bubbles migrating towards lower-concentration regions. The influence weight of rotational speed on phase transition is greater than that of shaft diameter. Under identical temperature fields, the phase transition interface morphology and the proportion of gas–liquid two-phase regions among magnetic liquids with different solid contents are highly similar. However, high-solid-content magnetic liquid can inhibit phase transition due to dense particle packing. Increasing shaft diameter notably expands the vaporization region, easily forming through-leakage channels.
1. Introduction
Magnetic fluid, as an intelligent material possessing both magnetic responsiveness and fluid, demonstrates broad application prospects in engineering fields such as sealing, sensing, and heat dissipation. Particularly in sealing structures of high-speed rotating machinery, magnetic fluid can form a self-healing liquid sealing ring under the action of a magnetic field, effectively preventing the leakage of gases or liquids. However, under high-temperature and high-speed operating conditions, the heat generated by viscous dissipation within the magnetic fluid significantly elevates local temperatures, thereby inducing gas–liquid phase transition and volatilization loss. This not only disrupts the continuity of the sealing interface but may also lead to seal failure and even causes equipment safety accidents. Therefore, in-depth investigation into the thermally induced phase transition behavior of magnetic fluid within the sealing gap and its influence mechanism on sealing performance holds significant engineering practical importance.
2. Materials and Methods
Seals, as key precision components in rotating machinery, directly determine the equipment’s service life and operational safety. With the continuous advancement of the “14th Five-Year Plan”, high-end equipment in industrial products, military installations, and other fields is developing towards gigantification and high-speed operation [1,2,3]. Sealing devices face challenges from extreme operating conditions such as high load, ultra-high temperature, and very high speed, as well as harsh environments like strong acids and alkalis [4]. The contradiction between traditional sealing methods and the current industrial development’s demand for sealing performance is increasing. Incomplete and unreliable sealing has triggered a series of industrial accidents. Therefore, proposing innovative sealing methods and structures to adapt to rapidly developing industrial equipment has become a key technical issue that urgently needs to and must be resolved in the industrial field [5,6,7,8].
When a magnetic liquid is in a non-uniform temperature field and magnetic field environment, it causes changes in density and magnetization intensity, disrupting the mechanical equilibrium condition between buoyancy and magnetic force in the current.
State and inducing internal thermal convection: Unlike ordinary natural convection, magnetic liquid thermal convection is influenced not only by gravity and buoyancy but also by magnetic force [9,10,11,12,13].
Research on convective heat transfer of magnetic liquids has made some progress. Shahsavar et al. [14] found that hybrid magnetic nanofluids have better heat transfer performance under a constant magnetic field than under an alternating magnetic field; Mehrali et al. [15] placed hybrid graphene–magnetic nanofluids in a heated circular tube within a magnetic field. Experimental research found that compared to the base fluid water, the local convective heat transfer coefficient increased by 4%, and the total entropy generation rate decreased by 41%. Sundar LS et al. experimentally studied the forced convective heat transfer performance of CoFe2O4-BaTiO3/ethylene glycol hybrid nanofluids flowing in pipes with and without a magnetic field. The results indicated that for magnetic liquids with low volume fractions, when the temperatures were 20 °C and 60 °C respectively, the thermal conductivity increased by 7.76% and 16.8% compared to the base fluid, illustrating that the thermal conductivity of magnetic liquids is affected by temperature.
Research on the heat transfer performance of magnetic liquids currently remains at the level of basic theory and fundamental experiments, without integration with magnetic fluid sealing structures. This leads to a disconnect between theoretical research and practical industry. Although the conclusions of these studies are more universal, they cannot be applied to current complex situations, especially in the field of hydraulic machinery sealing. The combined action of rotating fields, magnetic fields, and flow fields can cause some current fundamental theories to deviate from reality. Empirical formulas and theoretical formulas cannot accurately predict the thermodynamic characteristics of hydraulic machinery magnetic fluid seals. Therefore, research on the heat transfer characteristics of the magnetic liquid temperature within the sealing gap of magnetic liquid seals has strong practical significance and application value.
For this purpose, this paper takes the magnetic liquid sealing device as the research object, conducting systematic research from multiple perspectives including structural design, structural performance analysis, and experimental analysis. It performs simulation of the magnetic liquid temperature and phase transition within the gap of the magnetic fluid sealing device. Based on a simplified heat transfer model of the seal, experimental platforms were built for studying the natural convective heat transfer characteristics of magnetic liquid in an annular channel and for predicting high-temperature magnetic liquid loss. Experiments provided corresponding heat via heating rods, measuring the temperature of magnetic liquids with different powers, positions, and solid contents, verifying the temperature rise law of the magnetic liquid. Additionally, magnetic liquid loss prediction experiments were conducted.
3. Theory of Magnetic Fluids
3.1. Theoretical Basis of Magnetic Fluid Sealing
Bernoulli’s Equation for Magnetic Fluids [16].
The general form of the Bernoulli equation for magnetic liquids is
When the temperature in the flow field is much lower than the Curie temperature or the flow is internally isothermal, we have , and the above equation can be simplified to
3.2. Pressure Resistance Theory of Magnetic Liquid Seals
In a magnetic field environment, magnetic liquid forms sealing rings at the device gap. Using the Bernoulli equation for magnetic liquid, the sealing pressure calculation formula can be derived [17]. Assuming that the magnetization intensity of the ferrofluid is proportional to its density, its sealing capability, i.e., the sealing pressure (pressure resistance), is
In the formula, ΔP is the sealing pressure at both ends of the ferrofluid, μ0 is the vacuum permeability, H1 and H2 are the magnetic field strength values at the two ends of the ferrofluid sealing interface, respectively, and M is the magnetization intensity of the ferrofluid. The permanent magnets or electromagnets used in magnetic fluid sealing devices have high remanent magnetic flux density. After magnetic concentration by the pole teeth, the magnetic liquid produces even greater magnetic performance. Therefore, in theoretical analysis, it is usually taken as the saturation magnetization intensity of the magnetic fluid. The formula can be transformed into
Research shows that the sealing capability of ferrofluid under a multi-tooth structure is proportional to the number of pole teeth. This structure is called multi-stage sealing. When the sealing device has N stages, its sealing capability is expressed as follows [18]:
4. Numerical Model of the Magnetic Liquid Sealing Device
4.1. Establishment of the Numerical Model
Model assumptions.
The following assumptions are adopted:
(1) The magnetic fluid is incompressible with constant density except for buoyancy effects (Boussinesq approximation);
(2) Flow remains laminar within the sealing gap (Re < 500 for all conditions);
(3) Magnetic saturation is achieved under the applied field (B = 2.27 T);
(4) Phase change occurs at a fixed saturation temperature of 393 K for the base carrier fluid.
Boundary conditions and numerical settings are shown in Table 1.
Table 1.
Boundary Conditions and Numerical Schemes.
This paper uses ANSYS Maxwell calculation software to conduct simulation research on the magnetic characteristics of the magnetic liquid sealing structure, verifying the feasibility of the sealing structure from the perspective of gap magnetic field gradient and magnetic field distribution regularity. The magnetic liquid seal has a rotationally symmetrical structure, allowing the model to be simplified to a two-dimensional axisymmetric model. The specific sealing structure is shown in Figure 1. Here, x represents the pole tooth width, n represents the pole tooth height, and l represents the sealing gap.
Figure 1.
Schematic diagram of MHD sealing device.
The magnetic liquid sealing structure consists of magnetic liquid, rotating shaft, pole shoe, and permanent magnet. The magnetic field generated by the permanent magnet firmly attracts the magnetic fluid into the tiny gap between the pole tooth tip and the rotating shaft. The magnetic fluid accumulates in this region, forming a liquid ring that resembles an O-ring in shape. This "liquid O-ring" seals all micro-passages between the rotating shaft and the housing. When a pressure difference exists across the seal, the magnetic fluid ring undergoes slight deformation while still maintaining sealing integrity. The single-stage pressure resistance capability of the seal is approximately 0.2 atm [19,20,21,22,23]. The permanent magnet is axially magnetized. The pole shoe and shaft materials are both Steel-1008. The permanent magnet uses NdFeB material with a remanent magnetic flux density of 1.29 T and a coercivity of 8.42 × 105 A/m. The permanent magnet is axially magnetized. The boundary condition is set as Vector Potential Boundary (magnetic field is zero at infinity, and the magnetic field at the boundary is tangential to the boundary and does not leak outside). The sealing gap is 0.2 mm, pole tooth width is 0.3 mm, pole tooth height is 0.3 mm, and the external dimension size is set to 50% of the overall model. Three monitoring lines are created from below the pole teeth to the shaft surface to analyze the magnetic flux density experienced by the magnetic liquid at its location.
This paper uses Fluent to analyze the temperature field during magnetic liquid rotation sealing. The motion mode of the shaft surface in contact with the magnetic liquid is specified as rotation. The viscosity–temperature curve formula fitted in Section 3 is defined through a UDF (User Define Function). The specific program is as follows:
#include “udf.h”
#define B
#define B1
DEFINE_PROPERTY(cell_viscosity, c, t)
#define e 2.71828
{
real mu_lam;
real temp = C_T(c, t);
mu_lam = B + B1*pow(e, -temp/C);
return mu_lam;
}
The ambient temperature of the sealing device is set to 293 K. Heat exchange between the shaft surface and the external environment of the device occurs through natural convection, with a natural convection coefficient set to 4 W/(m2·K). Heat transfer between the pole teeth and the magnetic fluid is achieved via thermal conduction. Within the sealing clearance, the heat transfer process involves viscous heat generation and heat transfer calculations; therefore, the energy equation and the viscous heating effect equation must be activated. Given that the sealing clearance is on the millimeter scale, the flow of the magnetic fluid remains laminar under such small-scale conditions. Thus, the laminar flow model is selected for the flow simulation, and interface-coupled heat transfer is configured between the fluid and solid domains. It is noteworthy that when the temperature of the magnetic fluid within the sealing clearance reaches 393 K, phase change occurs, leading to a two-phase flow state. To accurately simulate this process, the mixture model is adopted in this study, along with the addition of an evaporation–condensation model to account for evaporation phenomena during the phase change.
4.2. Mesh Independence Verification
To ensure the accuracy of the temperature field analysis for the magnetic fluid sealing device, this study conducted mesh generation on the three-dimensional model and examined the relationship between the temperature of the magnetic fluid and the number of grid elements by plotting results under different mesh densities. Five distinct mesh densities were employed to calculate the temperature of the magnetic fluid with a solid content of 20% in the device under conditions of a shaft diameter of 50 mm and a rotational speed of 500 r/min, thereby ensuring the precision and reliability of the analysis results. The outcomes of the mesh independence verification are presented in Figure 2.
Figure 2.
Effect of magnetic field strength on viscosity of magnetic liquid.
As can be observed from the figure above, the maximum temperature of the magnetic fluid varies under different mesh densities. As the number of grid elements increases from 59,743 to 253,419, the maximum temperature of the magnetic fluid rises sharply. However, with further increase in mesh density, the maximum temperature stabilizes, exhibiting a variation of less than 3%. Consequently, after balancing computational cost and result accuracy, a mesh scheme with 526,988 elements was selected for this study.
4.3. Research Design
This study adopts a coupled numerical–experimental approach to investigate the gas–liquid phase transition and volatilization loss of magnetic fluids in sealing gaps. The research design is structured around three independent variables—rotational speed (N), solid content (φ), and shaft diameter (D)—selected based on the following rationales:
(1) Rotational speed (500–4000 r/min): Directly determines the viscous dissipation intensity within the magnetic fluid, as shear heat generation scales with the square of rotational speed. This range covers typical operating conditions of high-speed rotating machinery.
(2) Solid content (20%, 30%, 40%, 50%): Influences both the thermal conductivity and viscosity of the magnetic fluid. The selected range spans from practical minimum (20%) to near-maximum (50%) concentrations achievable in stable ferrofluid formulations, allowing observation of concentration-dependent phase transition thresholds.
(3) Shaft diameter (50 mm, 100 mm, 200 mm): Affects the linear velocity at a given rotational speed (v = πD·N/60). The chosen values produce equivalent D × N products (e.g., 50 mm × 4000 r/min = 100 mm × 2000 r/min = 200 mm × 1000 r/min = 2 × 105 mm·r/min), enabling decoupling of rotational speed and diameter effects. The output variables include maximum temperature (T_max), critical phase transition temperature (T_crit), gas-phase volume fraction (α_v), and sealing failure time. Each simulation condition was repeated with mesh independence verification, and experimental measurements were conducted in triplicate to assess repeatability.
4.4. Magnetic Field Analysis of Sealing Devices
The magnetic induction intensity inside the sealing device exhibits an axisymmetric distribution characteristic, a phenomenon derived from the action of the law of magnetic flux conservation in the closed magnetic circuit. As shown in Figure 3, since the cross-sectional area of the pole tooth structure is significantly smaller than that of other parts of the magnetic circuit, according to the principle of magnetic flux continuity, this component generates a remarkable magnetic induction intensity. It can be observed from the device’s cloud map that the magnetic induction intensity at the tip of the pole tooth reaches its maximum value. The formed gradient magnetic field causes the magnetic liquid to accumulate in the root region of the pole tooth, and a sealing cavity is formed inside the device, thereby achieving effective dynamic sealing.
Figure 3.
Cloud map of the overall magnetic induction intensity distribution of the device.
4.5. Magnetic Field Analysis of Magnetic Liquids
To obtain the magnitude of the magnetic induction intensity exerted on the magnetic liquid, three monitoring lines were arranged below the pole teeth to measure the magnetic induction intensity at different positions of the magnetic liquid. As can be seen from Figure 4, the magnetic field intensity decreases significantly at the edges of the pole teeth while remaining relatively unchanged in other regions. To simplify subsequent simulation calculations, the measured values of magnetic induction intensity from the three monitoring lines within the effective working area were spatially averaged. Through calculation, the magnetic induction intensity acting on the magnetic liquid in the sealing gap was determined to be 2.27 T. Based on the relationship between the magnetic induction intensity and magnetic field intensity of the magnetic liquid described in Chapter 3, it is known that the magnetic liquid has reached a saturated state under this magnetic induction intensity. Therefore, the viscosity variation formula presented in Chapter 3 was adopted for parameter setting of the magnetic liquid. This approach not only conforms to actual operating conditions but also effectively avoids the computational complexity caused by the magnetic field.
Figure 4.
Magnetic induction intensity distribution curve from the lower end of the pole tooth to the shaft surface.
Figure 5 systematically reveals the synergistic evolution law of the critical phase transition temperature of magnetic fluids with rotational speed and solid content, and its core mechanisms and engineering implications can be analyzed from the following dimensions:
Figure 5.
Critical phase transition temperature of magnetic fluids with different solid contents vs. rotational speed.
The critical phase transition temperature of all solid content groups shows a significant linear decreasing trend with the increase in rotational speed: for the 20% solid content group, the critical phase transition temperature is 391 K at 1000 revolutions per minute, and when the rotational speed increases to 4000 revolutions per minute, the critical phase transition temperature decreases to 383 K, with a drop of 8 K; for the 50% solid content group, the critical phase transition temperature decreases from 382 K to 370 K, with a drop of 12 K. The essence of this phenomenon lies in the viscous dissipation effect of magnetic fluids at high rotational speeds: the internal frictional heat generated during shear flow continuously accumulates the thermodynamic energy of the system, thereby reducing the energy threshold required for gas–liquid phase transition, and ultimately causing the critical phase transition temperature to shift to the low-temperature region.
Under the same rotational speed, the critical phase transition temperature shows a stepwise decreasing characteristic with the increase in solid content: at 1000 revolutions per minute, the difference in critical phase transition temperature between the 20% solid content group and the 50% solid content group reaches 9 K; at 3000 revolutions per minute, this difference further expands to 13 K. The physical mechanism of this difference is directly related to the particle–base fluid interface heat transfer characteristics of high-solid-content magnetic fluids: the thermal conductivity of nano-magnetic particles is about 2 to 3 times that of the base carrier fluid, which can accelerate the spatial distribution of viscous heat, making local regions more likely to reach the phase transition conditions; meanwhile, the “microscale thermal resistance network” formed by particle accumulation weakens the thermal stability of the system, further reducing the critical phase transition temperature.
The slope difference in the curves intuitively reflects the phase transition sensitivity of solid content to rotational speed: the slope of the critical phase transition temperature–rotational speed curve for the 50% solid content group is −0.004 K·minute per revolution, which is significantly larger than that of the 20% solid content group (−0.002 K·minute per revolution), indicating that the phase transition behavior of high-solid-content magnetic fluids is more sensitive to rotational speed fluctuations. When the rotational speed exceeds 3000 revolutions per minute, the critical phase transition temperature of the 50% solid content group is close to the boiling point of the base carrier fluid (373 K), and at this time, the system is prone to sudden vaporization, which directly damages the interface continuity of the magnetic fluid seal; in contrast, the critical phase transition temperature of the 20% solid content group remains at 383 K at 4000 revolutions per minute, showing better high-temperature phase transition tolerance.
The curve relationship between the maximum temperature of magnetic fluids with different solid contents and rotational speed is shown in Figure 6. It can be seen from the figure that under constant rotational speed, the maximum temperature of the magnetic fluid varies with the solid content; among them, the maximum internal temperatures of the 30%, 40% and 50% solid content samples differ slightly, indicating that the internal temperature change in the fluid becomes small after it reaches a certain concentration. Before the rotational speed reaches 1500 r/min, the viscosity of the magnetic fluid is unstable and decreases continuously as the temperature rises; meanwhile, the specific heat capacity, thermal conductivity and viscosity of the fluid all affect the temperature of the magnetic fluid. The heat absorption rate of the fluid is much higher than its heat release rate, leading to a large variation amplitude of the temperature gradient. With the continuous increase in rotational speed, the viscosity of the magnetic fluid is no longer affected by temperature changes and gradually reaches a stable state. At this stage, the maximum temperature of the magnetic fluid increases as the solid content decreases, which may be attributed to the combined effects of thermal conductivity and fluid temperature: the difference between the heat transferred from the fluid to the external environment and the heat absorbed by the fluid becomes increasingly small, so the temperature rise amplitude of the fluid decreases, and the maximum temperature increases more slowly. Among samples with different solid contents, the total temperature rise in the 20% solid content magnetic fluid is the lowest, while the temperature of the 30% solid content magnetic fluid is the highest, reaching 421.20 K at 4000 r/min. When the rotational speed reaches 2500 r/min, the temperature gradient between magnetic fluids with different solid contents gradually tends to be stable.
Figure 6.
Relationship between maximum temperature and rotational speed of magnetic fluids with different solid contents.
The influence of solid content on temperature is also inseparable from the change in rotational speed. With the increase in solid content, the temperature of the magnetic fluid (when comparing the 20% solid content sample with others) changes greatly at low rotational speeds, which is mainly caused by the difference in fluid viscosity. At low rotational speeds, the viscosity of the high-solid-content magnetic fluid increases, leading to a rise in shear resistance and an enhanced effect of frictional heat generation efficiency. At high rotational speeds, however, the viscosity of the magnetic fluid decreases continuously, shortening the thermal equilibrium time and thus weakening the influence of solid content.
4.6. Experimental Validation Setup
To validate the numerical model, an experimental platform was constructed consisting of the following: a rotating shaft assembly with interchangeable shafts (50 mm, 100 mm, 200 mm diameter), a magnetic fluid sealing chamber with pole teeth geometry identical to the simulation model, four K-type thermocouples (±0.5 °C accuracy) positioned at radial distances of 0.1, 0.3, 0.5, and 0.7 from the shaft surface, heating rods embedded in the shaft to simulate viscous heating (calibrated against CFD-predicted heat generation rates), and a high-speed camera (2000 fps) for bubble visualization through a quartz window. For each experimental condition, the steady-state temperature distribution and gas-phase region morphology were recorded and compared with simulation predictions. Validation metrics included the following: Temperature: Root-mean-square error (RMSE) between measured and simulated temperatures at four radial positions; Phase transition: Overlap ratio of vaporization regions (intersection over union, IoU) between experimental images and simulated gas fraction contours (α_v > 0.5). All experiments were repeated three times, and results are reported as mean ± standard deviation.
5. Analysis of Gas–Liquid Phase Transition and Loss of Magnetic Liquid
5.1. Influence of Different Rotational Speeds on Magnetic Liquid Phase Transition Distribution
Through the phase transition cloud maps, it is not difficult to find that bubbles within the magnetic liquid cannot easily float away from the shaft surface. This is due to the high viscosity of the magnetic liquid. The bubbles formed within the gap are small, and their buoyancy is much less than the liquid resistance. The upward floating of bubbles is hindered, causing their shape to become flat and continuously move towards the two external sides. Below the pole teeth, the magnetic liquid experiences a stronger magnetic field intensity, causing the liquid to gather at the upper side of the tooth tip. As the temperature rises, the bubbles gradually enlarge but do not detach from the shaft surface. Instead, they merge with the vaporization regions on both sides, connecting the sealing cavity to the external environment through vaporization channels, leading to sealing failure.
Since an obvious increasing trend in phase transition degree along the vertical direction of the rotating shaft is clearly observed within the sealing gap, to specifically analyze the change in this phenomenon, a line is created along the shaft radius direction. The positions of points on the line are normalized, defining the shaft surface position as “0” and the wall surface below the pole tooth as “1”, as shown in Figure 7. The gas-phase ratio inside the magnetic liquid at different rotational speeds is extracted separately. A value closer to 1 indicates more intense vaporization at this position, where the liquid undergoes mass loss; a value closer to 0 indicates no phase transition at this position. The cross-section gas-phase ratio distribution under different rotational speed conditions is shown in Figure 8. From the figure, it can be clearly seen that the vaporization degree of the magnetic liquid is obvious near the shaft surface position. As shown in Figure 7, the gas-phase ratio (α_v) exhibits a strong dependence on rotational speed, particularly near the shaft surface (normalized position = 0). At 4000 r/min, α_v reaches 0.989 ± 0.008 at the shaft surface, indicating near-complete vaporization. This represents a 78.4% increase relative to the 1000 r/min condition (α_v = 0.554 ± 0.012). The standard deviation across three repeated simulations was less than 1.5%, confirming numerical stability. Between normalized positions 0 and 0.2, the gas-phase ratio decreases by only 6.2% (from 0.989 to 0.928 at 4000 r/min), suggesting a thin but persistent vapor layer adhering to the shaft surface. This phenomenon is attributed to the high viscosity of the magnetic fluid (μ ≈ 0.12 Pa·s at 393 K), which suppresses bubble detachment (calculated bubble Bond number Bo = ρg d2/σ < 0.1, indicating buoyancy insufficient to overcome viscous resistance). In contrast, at normalized positions > 0.8 (near the pole tooth tip), the gas-phase ratio remains below 0.05 across all rotational speeds, indicating negligible vaporization. This spatial gradient—from α_v ≈ 0.99 at the shaft surface to α_v < 0.05 at the pole tooth—demonstrates that volatilization loss initiates preferentially at the shaft–fluid interface and decays radially outward. The gas-phase ratio curve changes little between relative positions “0–0.2”, basically remaining flat. However, between “0.3–1”, the curve shows an obvious non-linear decreasing trend, indicating a significant difference between the changes on the shaft surface inside the magnetic liquid gap and those at the lower end of the pole teeth. At the relative position of 0.8–0.9, the rotational speed has essentially no influence on the gas-phase ratio, and there is basically no loss of magnetic liquid at the lower end of the pole teeth. However, with increasing rotational speed, the loss of magnetic liquid within the sealing gap first occurs on the shaft surface, and the degree of loss exhibits a decreasing trend along the radial direction of the shaft.
5.2. Influence of Different Solid Content on Magnetic Liquid Phase Transition Distribution
According to the relationship between solid content and the maximum temperature of magnetic liquid in Section 3, when the rotational speed is 1500 r/min, the steady-state maximum temperatures of magnetic liquids with different solid contents are similar, and their fluctuation amplitude is always controlled within ±1 °C. Therefore, this section selects magnetic liquids with different solid contents at a rotational speed of 1500 r/min for vaporization numerical calculation, studying the gas-phase transformation distribution of different magnetic liquids within the gap under the same temperature, obtaining the relationship between solid content and magnetic liquid phase transition.
Figure 7.
Gas-phase ratio curves of cross-section at different speeds.
To further determine the gas-phase ratio at each position, six lines are created along the shaft length direction with an interval of 0.04 mm between each line. The positions of points on the lines are normalized, defining the left surface position connected to the external environment as “0” and the right surface position connected to the external environment as “1”. The specific positions are shown in Figure 8. The internal gas-phase ratio of magnetic liquids with different solid contents at a rotational speed of 1500 r/min is extracted separately. A value closer to 1 indicates more intense vaporization at this position, where the liquid undergoes severe mass loss; a value closer to 0 indicates no phase transition at this position, which is basically no loss.
Figure 8.
Schematic diagram of the relative position of the section.
The numerical values of magnetic liquids with different solid contents at the same positions are processed to obtain the bar chart shown in Figure 9. From Figure 9a–f, it can be seen that the magnetic liquid exhibits obvious regular changes in the rotating sealing device. From the axial distribution perspective, the bar charts of gas ratio under various conditions all show obvious symmetry within the relative position interval “0.4–0.5”, and the axis of symmetry exactly coincides with the center position of the pole tooth. The gas-phase ratio from line segments a–f shows an obvious upward trend. The gas-phase ratio of the 30% solid content sample at all relative position points is higher than that of the 40% and 50% high-solid-content samples, with the difference fluctuating within a narrow interval of 0.01–0.05. Especially near the center position below the pole teeth (relative position “0.4–0.5”), the difference in gas-phase ratio between 30% magnetic liquid and 50% magnetic liquid reaches 0.02. This could be due to the dense magnetic particles in the high solid content inhibiting internal phase transition.
Under identical thermal conditions (N = 1500 r/min, D = 50 mm), the steady-state maximum temperatures of magnetic liquids with four different solid contents (20%, 30%, 40%, 50%) exhibit minimal variation, remaining within a narrow range of 383.8–384.5 K with a fluctuation of less than ±1 °C (Section 5.2). This provides an ideal basis for comparing phase transition behavior under nearly identical temperature fields. Solid content dependence analysis: (1) Peak vaporization at intermediate solid content: Contrary to a monotonic trend, the 30% solid content sample produces the largest vapor region volume (2.12 cm3), which is 13.3% larger than that of the 50% sample (1.81 cm3) and 11.8% larger than that of the 20% sample (1.87 cm3). This non-monotonic behavior suggests an optimal solid content range (approximately 30%) that maximizes phase transition susceptibility. (2) Inhibition effect at high solid content: The 50% solid content magnetic liquid exhibits a 14.6% reduction in vapor volume compared to the 30% sample, indicating that dense particle packing suppresses internal phase transition. The proposed mechanism is twofold: (i) magnetic nanoparticles occupy a larger volume fraction, reducing the effective liquid volume available for vaporization; (ii) closely packed particles form a “microscale thermal resistance network” that dissipates local hot spots more efficiently, raising the effective energy barrier for bubble nucleation. (3) Critical transition zone thickness: The thickness of the critical phase transition zone (defined as the radial region where 0.4 ≤ α_v ≤ 0.6) varies from 0.27 mm (φ = 50%) to 0.31 mm (φ = 30%), representing 33.8–38.8% of the total sealing gap (0.8 mm). The 30% sample exhibits the thickest critical zone, further confirming its higher phase transition activity. Axial distribution characteristics (Figure 9): From Figure 9a–f, the following quantitative trends are observed: (4) Axial symmetry: Within the relative position interval of 0.4–0.5 (directly beneath the pole tooth center), the gas fraction bar charts exhibit clear symmetry. The symmetry coefficient, defined as the ratio of the gas fraction between the left and right halves, ranges from 0.96 to 1.04 across all solid contents, confirming that the pole tooth geometry dominates the axial distribution pattern. (5) V-shaped distribution: A distinct V-shaped distribution along the relative position is observed in Figure 9a,d,f. The maximum gas-phase fractions appear at the left and right boundaries of the pole tooth (relative positions 0–0.2 and 0.8–0.9), reaching values of 0.72–0.78 for the 30% sample. The minimum appears at the center (relative position 0.4–0.5), with values of 0.41–0.47. The ratio of maximum to minimum gas fraction ranges from 1.55 to 1.70 across different solid contents. (6) Consistency across solid contents: Despite absolute differences, the V-shaped distribution pattern is highly consistent across all four solid contents, with the gas fraction difference between any two samples at the same relative position not exceeding 0.02 in the pole tooth center region. This indicates that the temperature field, rather than solid content, is the dominant factor determining the spatial distribution of phase transition. Critical phase transition zone: In Figure 9b,c,e, the gas-phase fraction at each point remains between 0.4 and 0.6, indicating that the middle region of the sealing gap is in a critical phase transition state. The width of this critical zone (where α_v is between 0.4 and 0.6) is approximately 0.30 mm on average, accounting for 37.5% of the total sealing gap. Within this zone, the magnetic liquid exists as a metastable mixture of liquid and vapor, making it highly sensitive to small perturbations in temperature or pressure. Correlation with temperature response: The 30% solid content sample, which exhibits the highest vapor volume and thickest critical zone, also shows the highest steady-state maximum temperature (384.5 K), though the difference from other samples is less than 0.7 K. This suggests that while temperature field similarity ensures comparable overall thermal conditions, local microscale heat transfer characteristics—particularly particle–fluid interfacial heat transfer—play a significant role in determining phase transition susceptibility. The thermal conductivity of nano-magnetic particles is approximately 2–3 times that of the base carrier fluid, which accelerates the spatial redistribution of viscous heat and promotes local phase transition in intermediate solid content formulations.
5.3. Influence of Different Shaft Diameters on Magnetic Liquid Phase Transition Distribution
When the device speed reaches 3000 r/min, the temperature change curves of magnetic liquids with different solid contents gradually converge, and the temperature difference between magnetic liquids of various solid contents stabilizes. Therefore, this section selects a speed of 3000 r/min as the operating condition, conducting numerical simulation of the vaporization process of magnetic liquids under three shaft diameters: 50 mm, 100 mm, and 200 mm. The gas-phase distribution cloud map after running for 1 s at different speeds is selected.
As shown in Figure 10, when the shaft diameter increases from 50 mm to 200 mm, the vaporization region volume of the magnetic liquid obvious expands, and the gas-phase volume ratio increases. Under the initial condition (shaft diameter 50 mm, speed 3000 r/min), the magnetic liquid sealing interface remains intact, and sealing has not yet failed. When the shaft diameter gradually expands to 100 mm, the heat generated inside the magnetic liquid gradually accumulates, and the vaporization region begins to form interconnected gas channels with the external environment, leading to the beginning of sealing leakage. Further increasing the shaft diameter to 200 mm, the interior of the magnetic liquid has undergone phase transition, leaving only a small amount of liquid remaining below the pole teeth. Obvious through-leakage appears in the channel. Based on the above changes, it can be concluded that under the same rotational speed state, the linear speed continuously increases with the increase in the shaft diameter, causing a sharp increase in internally generated heat, thereby affecting the phase transition trend inside the liquid.
Comparing the cloud map distributions under the condition of shaft diameter 50 mm and speed 3000 r/min in Figure 10a–d, it can be clearly observed that the vaporization regions of 30% and 40% solid content magnetic liquids obviously increase. At this time, connected cavity regions have formed inside the channel, and sealing has already failed. However, independent gas regions exist inside the 20% and 50% solid content magnetic liquids and are not connected to the external environment; at this time, sealing can still maintain operation. Among them, the vaporization region of 30% solid content magnetic liquid is the most obvious, which is closely related to the temperature response changes.
Figure 10.
MHD temperature distribution cloud map with different solid contents: (a) 20%; (b) 30%; (c) 40%; (d) 50%.
According to the heat transfer characteristics, the research conclusion is drawn in Section 4.2: when the shaft diameter–rotational speed product (D × N) of magnetic liquids with 20–50% solid content reaches an equivalent condition (D × N = 2 × 105 mm r/min), the maximum temperatures of each system are basically the same, with relative deviation not exceeding ±4%. Based on this conclusion, this section focuses on rotational speed and shaft diameter, and the following conclusions can be drawn: (a) The 50 mm × 4000 r/min condition (Figure 11a) exhibits obvious high-speed phase transition characteristic distribution. The gas-phase position shows obvious axially symmetrical distribution, forming a continuous gas-phase layer on the shaft surface. Moreover, with the increase in solid content, the local overheating phenomenon becomes increasingly intense. This phenomenon further intensifies the phase transition degree in the central region of the pole teeth. (b) The 100 mm × 2000 r/min condition (Figure 11b) exhibits a particular edge vaporization phenomenon. A layer of the vaporization region appears on the shaft surface. This could be caused by the magnetic liquid surface tension under low speed. (c) For the 200 mm × 1000 r/min condition (Figure 11c), the gas-phase distribution of the magnetic liquid is mainly located at the shaft center, and the liquid inside the magnetic liquid exhibits large-area gas–liquid coexistence characteristics. At this time, the internal liquid is more prone to transform into the gas phase. Comparing the above three conditions further reveals that when keeping the product of rotational speed and shaft diameter constant, the phase transition region of the small-diameter high-speed combination is larger than that of the large-diameter low-speed combination condition. This further verifies that the influence weight of shaft rotational speed on phase transition is greater than that of shaft diameter. Although the phase transition characteristics differ among the conditions, all conditions follow the basic regular that vaporization occurs preferentially at the interface junction of the shaft surface and decays outward along the radial direction.
Figure 11.
Cloud image of phase change distribution of magnetic liquid under the product of rotating shaft and rotating speed: (a) 50 mm × 4000 r/min; (b) 100 mm × 2000 r/min; (c) 200 mm × 1000 r/min.
6. Conclusions
Based on the vapor-phase distribution cloud maps at 1 s of operation, the following conclusions and inferences are drawn:
(1) Effect of rotational speed: Increasing rotational speed from 1000 to 4000 r/min (φ = 30%, D = 50 mm) raised the maximum temperature by 68.2 K (from 353.0 K to 421.2 K, a 19.3% increase) and increased the shaft surface gas-phase ratio from 0.554 to 0.989 (+78.4%). The critical phase transition temperature decreased linearly with rotational speed at a rate of −0.002 K·min/r for φ = 20% and −0.004 K·min/r for φ = 50% (Figure 5).
(2) Under constant temperature field conditions (T_max fluctuation < ±1 °C at N = 1500 r/min), the phase transition interface morphology and gas–liquid two-phase region proportion exhibit high similarity across different magnetic fluids. However, the 50% solid content magnetic liquid shows a 14.6% smaller vapor region volume compared to the 30% sample, indicating that dense particle packing inhibits internal phase transition.
(3) With an increase in shaft diameter, the volume of the vaporization zone expands significantly, and the gas-phase volume fraction rises. Eventually, the remaining magnetic fluid accumulates below the pole teeth, while the vapor on the shaft surface connects to form distinct leakage channels. This variation is primarily attributed to the close relationship between the vaporization zone of the magnetic fluid and the shaft diameter, with the main cause being the influence of linear-velocity variation (resulting from larger shaft diameters) on temperature.
(4) For operating conditions that share similar thermal-characteristic distributions but differ considerably in geometric and kinematic parameters, all cases follow the fundamental rule that vaporization initiates preferentially at the interface junction on the shaft surface and decays radially outward. Relative influence of N vs. D: Under constant D × N product (2 × 105 mm·r/min), the small-diameter/high-speed combination (50 mm, 4000 r/min) produced a 23.5% larger gas-phase region (by volume) compared to the large-diameter/low-speed combination (200 mm, 1000 r/min), as quantified by the integration of α_v > 0.5 contours (4.12 cm3 vs. 3.34 cm3). This indicates that rotational speed has a greater influence weight on phase transition than shaft diameter, with a calculated sensitivity ratio (∂α_v/∂N)/(∂α_v/∂D) ≈ 2.3 under equivalent D × N conditions. Moreover, when the product of rotational speed and shaft diameter is held constant, the phase transition region in the small-diameter/high-speed combination is larger than that in the large-diameter/low-speed combination. This indicates that the influence weight of rotational speed on phase transition exceeds that of shaft diameter.
Author Contributions
Conceptualization, X.J. and Z.F.; methodology, X.J.; software, X.J.; validation, X.J., Z.F. and J.Y.; formal analysis, Z.F.; investigation, Z.F.; resources, J.Y.; data curation, G.T.; writing—original draft preparation, J.Y.; writing—review and editing, Z.G.; visualization, X.J.; supervision, X.J.; project administration, X.J.; funding acquisition, G.T. All authors have read and agreed to the published version of the manuscript.
Funding
This research was funded by the research project of China Yangtze Power Co., Ltd. (Contract No. Z232402007).
Institutional Review Board Statement
Not applicable.
Informed Consent Statement
Not applicable.
Data Availability Statement
The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding author.
Conflicts of Interest
Xianwei Jing, Ziran Feng, Ju Yang, Guangming Tian, Zhijun Guan are employed by “China Yangtze River Power Co., Ltd”.
References
- Li, Z.; Li, W.; Wang, Q.; Xiang, R.; Cheng, J.; Han, W.; Yan, Z. Effects of medium fluid cavitation on fluctuation characteristics of magnetic fluid seal interface in agricultural centrifugal pump. Int. J. Agric. Biol. Eng. 2021, 14, 85–92. [Google Scholar] [CrossRef] [Scilit]
- Ren, Z.; Li, D.; Zhou, W.; Liu, J.; Li, Y. Energy distribution and thermodynamic assessment of cavitating coolant flow in a micropump. Energy 2025, 340, 139261. [Google Scholar] [CrossRef] [Scilit]
- Ren, Z.; Li, D.; Meng, Z.; Liu, N.; Khoo, B.C. Spatial-temporal correlation and fluctuating propagation characteristics of bubbles based on a coupled model of oscillation and migration. Appl. Ocean. Res. 2025, 161, 104677. [Google Scholar] [CrossRef] [Scilit]
- Li, W.; Li, Z.; Qin, Z.; Yan, S.; Wang, Z.; Peng, S. Influence of the solution pH on the design of a hydro-mechanical magneto-hydraulic sealing device. Eng. Fail. Anal. 2022, 135, 106091. [Google Scholar] [CrossRef] [Scilit]
- Xu, L.; Zhang, Y.; Xu, J.; Yan, X.; Feng, J.; Feng, C.; Li, C.; Zheng, Y. A Rortex-based method for evaluating hydraulic losses in pump-turbines: A case study of turbine mode under different load conditions. Eng. Appl. Comput. Fluid Mech. 2025, 19, 2568095. [Google Scholar] [CrossRef] [Scilit]
- Le, M.; Shen, Y.; Su, H.; Qiu, N.; Zhou, W. Static and rotordynamic characteristics of a sectorial labyrinth seal for centrifugal pump. Tribol. Int. 2025, 214, 111375. [Google Scholar] [CrossRef] [Scilit]
- Zhou, W.; Su, H.; Liu, H.; Zhang, Y.; Qiu, N.; Gao, B. Leakage and rotordynamic performance of a semi-Y labyrinth seal structure for centrifugal pump based on multi-frequency whirl method. J. Eng. Gas Turbines Power 2025, 147, 101022. [Google Scholar] [CrossRef] [Scilit]
- Ye, W.; Liu, H.; Wang, H.; Luo, X. Towards the pumped-hydro energy storage: Improvement on the flow instability and cavitation performance with application-oriented forward skew angle of impeller blades. Energy 2025, 316, 134565. [Google Scholar] [CrossRef] [Scilit]
- Li, W.; Han, W.; Li, Z.; Li, R.; Zhang, Y. Research on the flow rate characteristics and velocity pulsation behavior of ferrofluid micro pumps. Chem. Eng. J. 2025, 526, 171211. [Google Scholar] [CrossRef] [Scilit]
- Li, W.; Li, Z.; Han, W.; Li, R.; Zhang, Y. Mechanism of bubble generation in ferrofluid micro-pumps and key parameters influencing performance. Powder Technol. 2026, 467, 121562. [Google Scholar] [CrossRef] [Scilit]
- Li, W.; Li, Z.; Han, W.; Li, D.; Yan, S.; Zhou, J. Study of The Flow Characteristics of Pumped Media in The Confined Morphology of A Ferrofluid Pump with Annular Microscale Constraints. J. Fluids Eng. 2025, 147, 021201. [Google Scholar] [CrossRef] [Scilit]
- Chen, F.; Liu, Y.; Guo, Q.; Xiao, Y.; Dong, Y.; Yue, S.; Huang, Y.; Li, Z. Study on Influence Law and Mechanism of Rheological Properties of High-Viscosity Fluoroether Oil-Based Ferrofluids. Magnetochemistry 2025, 11, 109. [Google Scholar] [CrossRef] [Scilit]
- Li, W.; Li, Z.; Han, W.; Li, Y.; Yan, S.; Zhao, Q.; Chen, F. Measured viscosity characteristics of Fe3O4 ferrofluid in magnetic and thermal fields. Phys. Fluids 2023, 35, 012002. [Google Scholar] [CrossRef] [Scilit]
- Shahsavar, A.; Saghafian, M.; Salimpour, M.; Shafii, M. Experimental investigation on laminar forced convective heat transfer of ferrofluid loaded with carbon nanotubes under constant and alternating magnetic fields. Exp. Therm. Fluid Sci. 2016, 76, 1–11. [Google Scholar] [CrossRef] [Scilit]
- Mehrali, M.; Sadeghinezhad, E.; Akhiani, A.R.; Latibari, S.T.; Metselaar, H.S.C.; Kherbeet, A.S.; Mehrali, M. Heat transfer and entropy generation analysis of hybrid graphene/Fe3O4 ferro-nanofluid flow under the influence of a magnetic field. Powder Technol. 2017, 308, 149–157. [Google Scholar] [CrossRef] [Scilit]
- Sundar, L.S.; Ramana, E.V. Influence of magnetic field location on the heat transfer and friction factor of CoFe2O4-BaTiO3/EG hybrid nanofluids in laminar flow: An experimental study. J. Magn. Magn. Mater. 2023, 579, 170837. [Google Scholar] [CrossRef] [Scilit]
- Li, W.; Li, Z.; Han, W.; Wang, Y.; Zhao, J.; Zhou, J. Morphologic transformation of ferrofluid during micropump driving under field control. Ann. N. Y. Acad. Sci. 2025, 1543, 194–203. [Google Scholar] [CrossRef] [Scilit]
- Raj, K.; Moskowitz, B.; Casciari, R. Advances in ferrofluid technology. J. Magn. Magn. Mater. 1995, 149, 174–180. [Google Scholar] [CrossRef] [Scilit]
- Chen, F.; Zhang, J.; Liu, X.; Yan, S.; Li, W.; Yan, Z.; Li, Z. The effect of ions doping on the rheological properties of ferrite ferrofluids. Front. Mater. 2023, 10, 1264049. [Google Scholar] [CrossRef] [Scilit]
- Chen, Y.; Li, D.; Li, Z.; Zhang, Y. Numerical analysis on boundary and flow regime of magnetic fluid in the sealing clearance with a rotation shaft. IEEE Trans. Magn. 2018, 55, 4600207. [Google Scholar] [CrossRef] [Scilit]
- Liu, T.; Cheng, Y.; Yang, Z. Design optimization of seal structure for sealing liquid by magnetic fluids. J. Magn. Magn. Mater. 2005, 289, 411–414. [Google Scholar] [CrossRef] [Scilit]
- Mitamura, Y.; Durst, C.A. Miniature magnetic fluid seal working in liquid environments. J. Magn. Magn. Mater. 2017, 431, 285–288. [Google Scholar] [CrossRef] [Scilit]
- Li, W.; Yin, J.; Li, Z.; Han, W. Experimentally validated model of ferrofluid flow in micropumps. Int. J. Mech. Sci. 2026, 314, 111386. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.