Annealing-Induced Structural, Optical, and Electrical Tuning of Sputtered Ge-Doped ZnO Thin Films for Transparent Conducting Applications

and
1
Laser and Photonic Materials Laboratory, Faculty of Science, Department of Physics, International Islamic University, Islamabad 44000, Pakistan
2
Department of Physics, International Islamic University, Islamabad 44000, Pakistan
*
Author to whom correspondence should be addressed.

Abstract

Ge-doped ZnO thin films were fabricated using the RF magnetron sputtering system on Si and glass substrates at room temperature, followed by post-deposition annealing at various temperatures to investigate the effects of annealing on the structural, optical, and electrical properties of the films. The X-ray diffraction results show that all the films are polycrystalline and have a hexagonal wurtzite structure. The crystallite size of the film was found to increase after annealing at 650 °C. The wurtzite structure of ZnO was further confirmed by Raman scattering with a dominant band at 435–438 cm−1 corresponding to the E2 (high) phonon mode. The presence of the Zn–O framework and a Ge-related vibrational band at 565 cm−1 was confirmed by FTIR, which is in line with Ge–O bonding and Ge incorporation; no crystalline impurity phase could be found in the range of XRD and Raman sensitivity. The film was annealed at 650 °C and then analyzed by XPS, which revealed chemical states of Zn2+ and Ge4+ with no evidence of the presence of metallic Ge. The optical transmittance was at its maximum at the best-performing temperature, 650 °C, at which the optical band gap (Eg) of the film increased from 3.45 eV to 3.57 eV. Spectroscopic ellipsometry showed that both the refractive index and extinction coefficient changed smoothly with the annealing temperature. The carrier concentration of the film annealed at 650 °C was measured to be 4.71 × 1020 cm−3, with a mobility of 39 cm2/V.s, and resistivity of 3.40 × 10−4 (Ω·cm), corresponding to a Haacke figure of merit of 5.1 × 10−2 Ω−1. Some modest visible light photo-switching was observed in a photoresponse measurement under 555 nm illumination (preliminary data).

1. Introduction

Transparent conducting oxides are key materials in modern optoelectronic technologies such as gas sensors, touch panels, liquid crystal displays, and solar cells [1,2]. For many years, Indium Tin Oxide has been the dominant transparent conductor due to its great electrical conductivity and excellent optical transparency [3].
However, the increasing cost and inadequate availability of indium, along with toxicity concerns and poor stability in hydrogen-rich environments, have restricted its widespread and long-term use. These limitations have accelerated the search for alternative transparent conducting materials that are cost-effective, stable, and environmentally friendly [4]. Zinc Oxide has emerged as a strong candidate to replace Indium Tin Oxide because of its abundance, non-toxic nature, and favorable electronic and optical properties. ZnO is a wide-band-gap semiconductor with good thermal stability and a high exciton binding energy, which makes it suitable for optoelectronic applications [5]. ZnO is a semiconductor with a significant exciton binding energy (60 meV), a strong piezoelectric constant, good transmittance in the visible range, and a broad band gap (Eg = 3.2–3.4 eV at 300 K). It is used in the production of solar cells, gas sensors, optical waveguides, surface acoustic devices, piezoelectric transducers, and varistors due to its chemical and thermal stability [6]. Although pure ZnO is nominally an n-type semiconductor, its electrical and optical characteristics appear to be unstable, particularly at elevated temperatures [7]. In recent years, Germanium-doped Zinc Oxide has gained increasing attention compared to the more extensively studied Aluminum-doped ZnO systems. Germanium is an attractive dopant because its higher valence state allows it to contribute additional free charge carriers when it substitutes for Zinc in the ZnO lattice, leading to improved electrical performance [8]. Furthermore, the ionic radius of tetravalent Germanium, 0.53 Å, is much smaller than that of divalent Zinc, 0.74 Å. This change in ionic size may cause the lattice to change and strain in the crystal structure of ZnO, affecting the electronic band structure and thus lead to the changes in bands gap of the layers and other characteristics of optical properties [9].
The characteristics of a Ge-doped Zinc Oxide thin layer are strongly affected by the deposition process and the thermal treatment. The high quality of films obtained by the RF magnetron sputtering process, characterized by dense, uniform, and well-adhered films, and the ability to precisely control the composition of the film, is what makes this process widely used for growing high-quality films. As-deposited films, however, do tend to have defects in their structure and residual stresses. Therefore, post-deposition annealing is important for the improvement of crystallinity, the relaxation of internal stress and the reduction in defect density [10]. The annealing temperature plays a major role in the determination of the final structural, optical and electrical characteristics of the ZnO thin films [11]. Thermal treatment can be used to improve the quality of the treated material by promoting atomic diffusion, which in turn will result in a more perfect crystal, the activation of substitutional dopants, and reduction in lattice imperfections. The annealing temperature should be carefully optimized, though, because too little heat energy is not enough to give a good improvement in the crystal structure and too much heat energy will change the defect chemistry and influence the level of electrically active dopants [11]. So, the choice of the right annealing temperature is important in order to get a balance of crystal quality and function [7].
Earlier works on annealed Ge-doped ZnO have mainly focused on the microstructure, photoluminescence, and formation of Ge-related phases of co-sputtered or multilayer Ge/ZnO films on Si [12,13] or the electronic transport of ALD films annealed at moderate temperatures (≤673 K) [14]. To our knowledge, no systematic correlation of the structural, optical constants (n, k), and electrical properties of RF sputtered Ge-doped ZnO films over an annealing range up to 850 °C with a quantitative TCO figure of merit has been reported. Thus, a detailed study is necessary for the optimization of the performance of Ge-doped ZnO films for advanced electro-optical systems. The present work deals with the growth of Ge-doped ZnO thin films on Si and glass substrate using RF magnetron sputtering and subsequently post deposition annealed 650 °C, 750 °C and 850 °C. These temperatures were selected to explore, in a systematic way, the effect of thermal annealing on the properties of Ge-doped ZnO thin films and to find the best-performing annealing temperature in the range investigated. It is followed by the recrystallization process, which enhances the crystallinity of the thin films and, depending on the working temperature, increases their grain size. Therefore, the ideal annealing conditions can be used to reduce residual stress and to improve the quality of the films by minimizing surface roughness and imperfections [15,16]. X-ray diffraction, Raman spectroscopy, FTIR spectroscopy, Energy Dispersive X-rays, SEM, surface profilometry, UV-visible spectroscopy, spectroscopic ellipsometry, Hall-effect measurements, XPS and photocurrent measurements were used to investigate the crystal structure, surface morphology, optical properties, and optical constant characteristics of the deposited films as a function of annealing temperature.
The main objectives of this work are (i) to clarify the effect of post-deposition annealing on the structural, vibrational, morphological, optical, and electrical properties of Ge-doped ZnO thin films, and (ii) to identify the most suitable annealing temperature in the studied range that gives the best combination of structural quality and functional properties for potential optoelectronic applications.
The novelty of this work is the systematic correlation of the structural, vibrational, morphological, optical (including dispersion of refractive index and extinction coefficient), and electrical properties of sputtered Ge-doped ZnO films over a wide range of post-deposition annealing temperatures (RT–850 °C); identification of the favorable annealing temperature of 650 °C supported by a quantitative TCO figure of merit; and preliminary demonstration of visible-light photo-switching of the optimized film.

2. Experimental Details

2.1. Step-1: Solid State Target Synthesis and Thin-Film Processing

The chemical substances, including ZnO powder and Germanium powder with (Sigma Aldrich, Burlington, MA, USA, 99.99%), were used to prepare the desired samples. The raw powders, target fabrication route, substrate-cleaning protocols, and thin-film growth parameters are schematically represented as a complete workflow in Figure 1.
Figure 1. Schematic representation of the complete experimental workflow: (top) solid-state synthesis route for the ZnO:Ge ceramic target involving stoichiometric powder milling, calcination, binder compaction, and high-temperature sintering; (middle) substrate ultrasonic cleaning protocol and radio-frequency (RF), magnetron sputtering thin-film growth on Si and glass substrates; and (bottom) post-deposition thermal processing at 650 °C, 750 °C, and 850 °C paired with the comprehensive multi-technique characterization framework (XRD, Raman/FTIR, AFM, spectroscopic ellipsometry, and Hall-effect transport measurements).
  • Ceramic Target Synthesis: High-purity ZnO and Ge (powders were stoichiometrically weighed to yield a nominal composition of Zn0.985Ge0.015 (1.5 at. % Ge). The powders were wet-milled in ethanol using an agate mortar for 6 h, dried, and calcined in air at 400 °C for 4 h. The calcined powder was blended with a polyvinyl alcohol (PVA) binder, uniaxially pressed under 15 MPa for 180 s into a 50 mm × 2 mm disc, and sintered at 900 °C for 4 h in air.
  • Substrate Preparation and RF Sputtering: Si (100) and fused silica quartz glass substrates underwent sequential ultrasonic cleaning in acetone, ethanol, and deionized water for 10 min each before N2 blow-drying. Sputtering was executed at a base pressure of 4.3 × 10−3 Pa, RF power of 110 W, target-to-substrate distance of 7 cm, substrate rotation of 15 rpm, and an Ar/O2 flow ratio of 30:10 sccm.
  • Post-Deposition Thermal Treatment: As-deposited (RT) films were subjected to furnace annealing in air at 650 °C, 750 °C, and 850 °C for 1 h. The fused silica quartz glass substrates have a softening point (≈1600 °C) far above the highest annealing temperature (850 °C), so no substrate deformation is expected.

2.2. Step-2: Multi-Technique Characterization Framework

To evaluate the impact of thermal processing, films were investigated across several analytical platforms.
  • Structural and Vibrational Analysis: Phase purity and c-axis crystallographic orientation was determined via X-ray diffraction (XRD, Rigaku, Tokyo, Japan D/max-2600/PC, CuKα, λ = 1.5418 Å. Local vibrational modes and chemical bonding configurations were evaluated using Raman spectroscopy and Fourier-transform infrared spectroscopy (FTIR).
  • Surface and Morphological Analysis: Surface topography, microstructural evolution, and average surface roughness Ra were characterized via 3D optical profilometry over a 1.0 × 1.0 mm2 area. Chemical stoichiometry was verified using Energy Dispersive X-ray Spectroscopy (EDX). Surface morphology was examined using SEM.
  • Optical and Dielectric Properties: UV-Vis optical transmittance (250–800 nm) was measured using a Thermo Scientific Evolution 220 spectrophotometer (Thermo Fisher Scientific, Madison, Wisconsin, USA). Spectroscopic ellipsometry (ASMEC system, 70° incident angle) fitted with a Cauchy model was used to extract the dispersion profiles of the refractive index (n) and extinction coefficient (k).
  • Electrical Transport: Room-temperature Hall-effect measurements were performed in a van der Pauw four-probe configuration under a magnetic field of 0.46 T to calculate the charge carrier density (n), Hall mobility (µ), electrical conductivity (σ), and resistivity (ρ).
  • Photoresponse Measurement
We measured the photocurrent in a vertical two-terminal configuration at room temperature in air, with one Ag contact pad (0.5 × 0.5 mm2) on the ZnO:Ge film and the other on the Si (100) substrate, an illuminated junction area of 1 × 1 cm2, and a fixed bias of 2 V. The device was illuminated with a 555 nm light source, nominal power density 26.2 mW/cm2, turned on and off approximately every 31 s (period approximately 63 s, modulation frequency approximately 0.016 Hz). The rise and decay times were taken from the I–t curve as the 10–90% and 90–10% times, respectively.
  • Chemical-State Analysis
The ZnO:Ge (Zn0.985Ge0.015 O) target was used to deposit ZnO:Ge film at room temperature by RF magnetron sputtering. The chemical states of Zn, Ge, O, and C on the deposited ZnO:Ge film annealed at 650 °C (the best-performing annealing temperature in this study) were analyzed by X-ray photoelectron spectroscopy (X-ray photoelectron spectrometer, JEOL JPS-9030, Tokyo, Japan) using an Al Kα 1486.6 eV source. The binding energies have been charge-corrected to the adventitious C 1S line at 284.8 eV [17], and the spectra were fitted using Shirley background subtraction. XPS results are given in Section 3.3, Figure 6.
XRD, Raman, FTIR, EDX, SEM, surface profilometry, spectroscopic ellipsometry, and photocurrent measurements were performed on films deposited on Si (100) substrates, while UV-Vis transmittance measurements were carried out on films deposited on glass substrates. The substrate-related features (Si Raman line at 517–518 cm−1, Si–O–Si band at 850 cm−1, Si signal in EDX) were identified separately and excluded from the analysis of the films, and the SiO2 interfacial layer was included in the ellipsometric model. In the measurements done on Si, the thin SiO2 layer formed during annealing in air cannot be completely excluded.

3. Results and Discussion

3.1. Structural and Morphological Analysis

X-ray diffraction (XRD) measurements were performed to investigate the crystal structure of the Ge-doped ZnO thin films at room temperature (RT), 650 °C, 750 ° C, and 850 ° C with an advanced X-ray diffractometer (Rigaku D/max-2600/PC) using Cu Kα radiation (λ = 1.5418 Å). We examined all films by X-ray diffraction, and the patterns are shown in Figure 2. The diffraction patterns show characteristic reflections from the (002) and (103) planes at around 34° and 63°, respectively. The reflections confirm the hexagonal wurtzite structure of the ZnO crystallite. The strong (002) reflection also shows that the crystallites have a preferred orientation along the c-axis [17,18]. No other diffraction peaks corresponding to metallic Ge, Ge-containing secondary phases, or other impurity phases were found. This shows that the wurtzite ZnO crystal structure remained unchanged after Ge incorporation, as no new phases were detected. A noticeable change in the position of the dominant (002) diffraction peak was observed after thermal annealing. The 2θ value increased from 34.60° for the as-deposited ZnO:Ge-RT film to 34.71°, 34.76°, and 34.79° for the films annealed at 650 °C, 750 °C, and 850 °C, respectively. This systematic shift in the (002) diffraction peak towards higher 2θ angles also indicates the incorporation of Ge into the ZnO lattice [15]. The Bragg’s positions of diffraction peaks indicate the interplanar spacing; with a shift in a diffraction peak to higher 2θ values, the interplanar spacing decreases. These displacements observed during the annealing process may then be related to the structural rearrangements that occurred in the ZnO lattice. The variation in the full width at half maximum (FWHM) of the dominant (002) peak as a function of annealing temperature further reflects the effect of the annealing temperature on the structural characteristics. The FWHM of the RT film was found to be 0.00541 rad and 0.00401 rad after annealing at 650 °C. However, further increasing the annealing temperatures to 750 °C to 850 °C resulted in a gradual increase in FWHM to 0.00420 rad and 0.00453 rad, respectively, as shown in Figure 3 [19]. The lowest FWHM value of the ZnO:Ge-650 °C film shows that this sample has the maximum structural ordering in the investigated films. The peak broadening at 750 °C and 850 °C shows that annealing temperatures above the best-performing temperature may not be beneficial to the crystal growth and ordering, as this is also reflected by the quality of the crystal.
Figure 2. The XRD patterns of Germanium-doped ZnO thin films annealed at various temperatures (RT, 650 °C, 750 °C, and 850 °C).
Figure 3. Variation in the full width at half maximum (FWHM) and crystallite size of ZnO:Ge films as a function of annealing temperature.
The mean crystallite size was determined from the most intense (002) diffraction peak using the Scherrer equation:
D = 0.9 λ β cos θ
where K = 0.9 is the shape factor, λ = 1.5418 Å is the Cu Kα wavelength, β is the FWHM of the (002) peak in radians, and θ is the Bragg angle (half of the 2θ value given in Table 1). The calculated crystallite sizes were 27 nm for the RT film, 36 nm for the film annealed at 650 °C, 35 nm for the film annealed at 750 °C, and 32 nm for the film annealed at 850 °C. Thus, the crystallite size increased significantly with annealing at 650 °C, and decreased as the annealing temperature was further raised. This is similar to the FWHM results, as a smaller diffraction peak means a bigger crystallite size. The crystallite growth at 650 °C indicates a high enough processing temperature for the rearrangement of atoms and crystallite growth. The crystallite sizes were calculated from the measured FWHM without any instrumental correction and thus are lower-bound estimates; for a typical instrumental broadening of 0.03–0.05°, the correction would increase them by less than about 2% (≈0.3–2.2%) without changing the trend. The c-axis lattice parameter was obtained from the (002) position as
c = λ   sin θ
since d002 = c/2 and λ = 2d002sinθ. The strain along the c-axis was calculated as
ε c =   ( c − c o ) c o
where co = 5.2066 Å for bulk ZnO; negative values refer to contraction (compressive strain) along the c-axis. The c-axis lattice parameter decreased from 5.185 Å (RT) to 5.169, 5.162, and 5.157 Å for the films annealed at 650, 750, and 850 °C, respectively, corresponding to strains of −0.42%, −0.73%, −0.87%, and −0.95%. The maximum contribution of microstrain to the peak broadening,
ε β = β 4 tan θ
obtained from the strain term of the Williamson-Hall relation by neglecting the size term (an upper limit, not independent of D, since both derive from the same β), was 0.32–0.43%. The monotonic increase in lattice contraction with temperature, compared to the non-monotonic variation in the FWHM, indicates that the peak shift is caused by the substitution of Ge4+ and stress relaxation, not by crystallite-size effects. The summary of the XRD parameters is given in Table 1.
Table 1. Structural parameters of Ge-doped ZnO thin films annealed at (RT, 650, 750 and 850 °C). D = crystallite size, c = λ / sinθ is the c-axis lattice parameter, εc = (c − c0) / c0 is the strain along the c-axis (c0 = 5.2066 Å for bulk ZnO; negative values indicate contraction), and εβ = β / (4tanθ) is the maximum microstrain estimated from the peak broadening.

3.2. Raman Spectroscopic Analysis of Ge-Doped ZnO Thin Films

The vibrational properties and the structural characteristics of Ge-doped ZnO thin films were investigated using Raman spectroscopy. The Raman spectra are shown in the range of 50–1500 cm−1 in Figure 4. In all samples, two strong Raman peaks were found. The first peak was located at 435–438 cm−1 and was identified as the E2 (high) phonon mode of hexagonal ZnO [20,21]. This mode is regarded as the typical Raman mode of wurtzite ZnO and is typically attributed to the vibration of the oxygen atoms in the crystal lattice. This peak is present in all the samples, resulting from the hexagonal ZnO structure. The second Raman band was observed at 517–518 cm−1 and was assigned to the first-order optical phonon mode of the Si (100) substrate [22]. Since the thin films were directly grown on silicon substrates, the appearance of this peak was expected in all Raman spectra. The slight shift in the position of the ZnO-related Raman band was observed with increasing temperature. The ZnO Raman peak, which is seen at room temperature, shifts from its position to 435.4 cm−1 after annealing at 650 °C, and then to 435.0 cm−1 and 436.0 cm−1 for the films annealed at 750 °C and 850 °C, respectively. This shift was small and suggests the crystal structure of the ZnO is stable over the range of temperatures studied. These small differences can be linked to changes in the lattice strain, defects in the lattice, and incorporation of Ge into the ZnO matrix. The intensity of the ZnO Raman mode has increased with increasing temperature up to 650 °C, indicating an enhancement in crystal quality and structural ordering, which is in agreement with the XRD data. In none of the samples were any additional Raman bands related to secondary Ge-containing phases observed. The absence of any extra vibrational modes, along with the XRD results, suggests that the Ge atoms were substituted into the lattice of ZnO without forming a separate crystalline phase. Thus, the Raman study of the samples shows that the wurtzite structure of ZnO has not been altered and gives additional confirmation that the presence of Ge has changed the lattice environment of the local structure without altering the characteristic vibrational properties of the wurtzite structure of ZnO.
Figure 4. Raman Spectroscopy of ZnO:Ge thin films annealed at different temperatures.

3.3. FTIR and XPS Spectroscopic Analysis of Ge-Doped ZnO Thin Films

The vibrational characteristics and chemical bonding of the Ge-doped ZnO thin films annealed at different temperatures were studied by Fourier-transform infrared (FTIR) spectroscopy. The FTIR recorded range is from 400 to 1100 cm−1, as shown in Figure 5 below. The spectra show three characteristic absorption bands at 410, 565, and 850 cm−1. The absorption band around 410 cm−1 is assigned to the Zn–O stretching vibration, which indicates the formation of the ZnO framework in all deposited films [23]. The appearance of such a characteristic band means that the basic structure of ZnO is maintained over the investigated temperature range. The other absorption band is located at 565 cm−1 and is attributed to a Ge-related vibration. The appearance of this band suggests the incorporation of Ge into the ZnO matrix. There are published FTIR studies supporting this assignment. Ge–O stretching frequencies have been reported for Ge-containing oxide films in the range 500 to 800 cm−1 [24,25,26] and Ge–O related modes have been detected in addition to the ZnO bands in Ge-doped ZnO films on Si [24]. The 565 cm−1 band is therefore assigned to the Ge–O stretching mode of the GeO4-type local units around Ge incorporated into the ZnO matrix. The assignment is supported by the lack of Zn2GeO4 and GeO2 reflections in XRD, the lack of additional Raman modes, and the Ge4+ state as determined by XPS (see Figure 6 below). These results, combined with the absence of any Ge diffraction peak, GeO2 diffraction peak, or GeO4 diffraction peak in the XRD pattern, the lack of additional Raman modes other than the E2 (high) mode and the Si substrate peak, and the EDX observation of only Zn, O, and Ge, suggest that there exists no long-range-ordered secondary phase, and that Ge–O bonds form locally, below the XRD detection limit. The XRD results do not show any further diffraction peaks related to Ge-containing crystalline phases, while the FTIR spectra give information about the Ge-related bonding at the local level within the deposited films. It is observed that no second phase with long-range-ordered Ge structure is identifiable in the ZnO structure, and none is identified by the FTIR results, which show evidence for Ge–O bonding at the local scale [24]. A second strong absorption band was observed at 850 cm−1 and correlated with the Si–O–Si stretching vibration of the Si (100) substrate [27]. As the film itself was grown directly onto the silicon, there was anticipated to be a contribution from the silicon to the FTIR spectra. This band has been found in all four samples, thus demonstrating the effect of the annealing on the vibration response of the deposited films. The complete spectral profiles remained almost the same with increasing annealing temperature, suggesting that the chemical composition of the Ge-doped ZnO films was retained throughout. There were some slight differences in the intensity and shape of the bands of absorption, however. At 650 °C, the Zn–O absorption feature became stronger, indicating a better ordering of the structure. The XRD results showed that crystallinity increased with annealing; these observations can be correlated with the XRD results. The FTIR analysis thus validates the presence of Zn–O bonds and also gives further evidence to confirm the presence of Ge in the ZnO matrix, maintaining the characteristic structural properties of ZnO. No other additional absorption bands relating to other impurity phases have been identified, further confirming the formation of single-phase Ge-doped ZnO thin films.
Figure 5. FTIR spectra of ZnO:Ge thin films annealed at different temperatures.
The FTIR band at 565 cm−1 suggests the chemical state of Ge, so XPS was performed for the ZnO:Ge film annealed at 650 °C as shown in Figure 6, which is the favorable annealing temperature found in this work. The survey spectrum in Figure 6A includes only Zn, O, Ge, and adventitious C. The high-resolution C 1S spectrum in Figure 6B is deconvoluted into a main C–C/C–H component at 284.7 eV and a weak O–C=O component at 288.3 eV, which are typical of adventitious carbon and were used as the reference for the binding-energy correction. The Zn 2p spectrum in Figure 6D showing a doublet (2p3/2 = 1022.8 eV, 2p1/2 = 1045.9 eV, spin–orbit splitting 23.1 eV) is characteristic of Zn2+ in ZnO [28,29]. The Ge 3d line in Figure 6E is centered around 32.1 eV, corresponding to the Ge4+ state bound to oxygen. Within the signal-to-noise of the measurement, no component is seen near 29–30 eV where elemental Ge or low-valent Ge should be seen. This binding energy is also approximately 1 eV less than the binding energy of the stoichiometric GeO2, a trend that has been observed in Ge for the substitution of Zn in the lattice of ZnO [30]. The O 1s envelope in Figure 6C has two components at 530.0 eV (lattice O2-) and 531.7 eV (hydroxyl groups and oxygen-deficient regions) [30,31]. The presence of Ge4+ on Zn2+ sites is compatible with the smaller ionic radius of Ge4+, the shift in the (002) peak towards higher 2θ, and the high electron concentration, determined by the Hall effect, because each substitutional Ge4+ can donate two electrons. In addition to the 565 cm−1 band, these results suggest that Ge is incorporated in the oxidized form, Ge4+, within the ZnO matrix. The XRD, Raman, FTIR, and EDX data indicate that there was no presence of secondary phases at the other annealing temperatures; therefore, the results obtained from the XPS spectra have directly confirmed the oxidation state of Ge under a favorable annealing condition. These results imply the substitutional incorporation of Ge at the Zn sites. XPS indicates that there is no metallic Ge present; Ge is only in the form of GeO4+. The (002) reflection angle increases from 34.60° to 34.79°, corresponding to a decrease in the c-axis after annealing, which is due to the smaller ionic radius of Ge4+ (0.053 nm) compared with Zn2+ (0.074 nm) replacing each other, although stress relaxation during annealing may also play a role. No Ge, GeO2, or Zn2GeO4 reflections are detected, and Ge is an electron donor, as observed in the Hall measurements and in the band gap widening. All these results together suggest substitutional Ge4+ incorporation.
Figure 6. The XPS survey spectrum and high-resolution core-level spectra of (A) survey spectrum, (B) C 1s, (C) O 1s, (D) Zn 2p and (E) Ge 3d of the ZnO:Ge thin film after annealing at 650 °C.

3.4. Energy Dispersive X-Rays

The EDX spectra of the Ge-doped ZnO thin films deposited at room temperature (RT) and annealed at 650, 750, and 850 °C are shown in Figure 7a–d. The characteristic peaks of Zn, O, and Ge confirm the presence of the constituent elements in the films, and the Si signal is from the underlying silicon substrate. There are no other elemental peaks, which means that the films are chemically pure within the detection limit of EDX. The elemental composition is essentially constant after annealing up to 850 °C, and the differences in peak intensity are probably due to differences in surface morphology, electron interaction volume, and counting statistics, rather than significant changes in elemental composition [14].
Figure 7. Energy Dispersive X-rays (EDX) spectra of ZnO:Ge thin films annealed at various temperatures. (a) ZnO:Ge-RT, (b) ZnO:Ge-650 °C, (c) ZnO:Ge-750 °C (d) ZnO:Ge 850 °C.
The elemental mapping was further used to investigate the spatial distribution of the constituent elements as shown in Figure 8a–e. The individual maps for each element (Zn, Ge, Si, and O) and the composite map (e) display a uniform distribution of the elements detected on the film surface. There is no apparent localized clustering or segregation of Ge. These results suggest that after annealing, the films have experienced microstructural and morphological changes, as seen in the XRD and profilometry results, but the overall elemental homogeneity of the films has not changed. The EDX results and elemental maps reveal no sign of Ge segregation, Ge loss, or secondary-phase formation in the films annealed up to 850 °C, while XRD and Raman analysis do not reveal any presence of Ge-, Zn-, or Si-containing secondary phases. At the low Ge level of the present films (nominal 1.5 at. %), however, EDX is only a semi-quantitative technique and has a volume that encompasses the substrate. Hence, it is not possible to rule out conclusively with the present results whether the nominal Ge concentration is retained, and whether Ge diffusion or Ge loss or a thin interfacial reaction layer at 850 °C can contribute to this. Grain coalescence and Ostwald ripening are responsible for morphological degradation at 850 °C, as was discussed in Section 3.5.
Figure 8. Elemental mapping of ZnO:Ge thin films annealed at various temperatures. (a) ZnO: Ge-RT, (b) ZnO:Ge-650 °C, (c) ZnO:Ge-750 °C, (d) ZnO:Ge 850 °C, (e) mixed elemental overlay (Zn/Ge/Si/O).

3.5. SEM Surface Analysis

The surface microstructural evolution of the ZnO:Ge thin films as a function of thermal annealing temperature is illustrated in Figure 9a–d. The as-deposited film (RT) has a compact, fine-grained surface with a few microcracks and a fibrous, wavy structure, characteristic of films sputtered at room temperature, which typically have low adatom mobility and residual compressive stress. The film has the most uniform and smooth morphology in the series after annealing at 650 °C (Figure 9b), where the equiaxed grains are uniformly fine, closely packed, and free of breaking and porosity. This surface texture refinement is directly related to the smallest FWHM and the largest crystallite size observed in the Scherrer analysis at this temperature, suggesting that 650 °C is sufficient for thermal energy to relax the surface texture but is not high enough to produce significant grain scratching. When the annealing temperature is increased to 750 °C, the surface morphology transforms to an agglomerated structure with coarsening and nodular clustering, while also exhibiting intergranular porosity (Figure 9c). This coarsening is consistent with the trend of higher surface roughness and average grain size with higher post-annealing temperature. At the highest annealing temperature, 850 °C, Figure 9d gives the roughest film surface, with very large, coarse, rounded/spherical agglomerates, with some blocky, faceted crystallites in between. As the annealing temperature increases, voids and agglomeration between nanocrystallites become more apparent because of the dominance of the Ostwald ripening process that leads to the formation of larger grains at the expense of the smaller, less thermodynamically stable grains.
Figure 9. SEM surface micrographs of ZnO:Ge thin films: (a) as-deposited (RT), (b) annealed at 650 °C, (c) annealed at 750 °C, and (d) annealed at 850 °C.

3.6. Surface Profilometry

An optical profilometry analysis of the surface morphology was performed, and a scanned area of up to 1 × 1 mm2 of the ZnO:Ge thin films was examined after annealing at different temperatures (RT, 650 °C, 750 °C, and 850 °C). The three-dimensional surface profilometry maps of the ZnO:Ge thin films are presented in Figure 10a–d, illustrating the film’s temperature-dependent evolution of surface roughness. The roughness values for films annealed at room temperature and 650 °C, 750 °C, and 850 °C are summarized in Table 2.
Figure 10. Surface roughness of Germanium-doped ZnO thin films annealed at various temperatures. (a) ZnO:Ge-RT, (b) ZnO:Ge-650 °C, (c) ZnO:Ge-750 °C, (d) ZnO:Ge-850 °C.
Table 2. Surface roughness values for ZnO:Ge films annealed at RT, 650 °C, 750 °C and 850 °C.
The results reveal that the surface morphology of the Ge-doped ZnO thin films is significantly affected by the annealing process. The 650 °C annealed film is the most uniform and shows the lowest surface roughness. This behavior is due to the increased mobility of surface atoms at this temperature, which enables them to reach favorable sites. This means that stable nucleation sites are created, which promote the packing of the grains and prevent them from growing excessively, resulting in a smoother surface of the film. The surface of the film became slightly rougher at annealing temperatures of 750 °C, but still smoother than the as-deposited layer. The higher roughness of the sample placed at room temperature is correlated with the randomly oriented grains and defects formed during the deposition process. These defects limit the mobility of atoms and the formation of a uniform microstructure [32]. The roughness of the film annealed at 850 °C increased considerably, showing the deterioration of the surface morphology. This result parallels the XRD data indicating an increasing amount of lattice strain and partial structural degradation at high temperatures. At this higher annealing temperature, the Zn, O, and Ge atoms become more mobile, and grain growth and coalescence increase. The smaller grains will tend to fuse into larger grains to minimize the energy at the grain boundaries, resulting in the development of irregular surface characteristics [33].

3.7. Ge-Doped ZnO Thin Films’ Optical Characteristics

The design and analysis of optoelectronic devices greatly benefit from an understanding of the optical characteristics of materials. In addition, optical measurement is widely used to characterize the quality of the materials. The transmittance spectrum for as-deposited and thermally annealed films at 650 °C, 750 °C, and 850 °C is shown in Figure 11a. The spectra were collected at 250–800 nm using a Thermo Scientific Evolution 220 UV-Visible spectrophotometer. The transmittance of all the films is low in the ultraviolet region with an increase in the near-absorption edge, and high transparency in the visible region. The optical properties of these films are typical characteristics of the wide-band-gap semiconductor ZnO. The film produced at room temperature has a comparatively low transmittance over the visible range as compared to the other annealed films, suggesting a poorer optical quality. The change in optical transparency due to thermal annealing indicates that thermal treatment up to a certain temperature can improve the uniformity of the deposited films. The highest transmittance of around 95% was achieved for the film annealed at 650 °C, with the films annealed at 750 °C and 850 °C showing transmittance of almost 90% across most of the visible spectrum. The optical enhancement is very desirable for transparent conducting oxide (TCO) applications, which require low reflectance and high transparency performance [4]. It is observed that after annealing, the films are more transparent to light, which shows that the optical properties of the Ge-doped ZnO films are enhanced by thermal annealing. The absorption edge is present in all the samples in the ultraviolet (UV) region and changes with the increase in annealing temperature. The absorption edge of the room-temperature (RT) film is at around 359 nm. After annealing at 650 °C, the absorption edge shifts to a shorter wavelength of about 347 nm (blue shift), indicating that higher-energy photons are required to initiate electronic transitions across the band gap. With further increases in annealing temperature, the absorption edge undergoes a slight red shift, moving to approximately 351 nm for the film annealed at 750 °C and to around 354 nm for the film annealed at 850 °C. This reduction in transmittance suggests the onset of surface degradation or the formation of additional light-scattering centers, which may be associated with partial microstructural instability [34]. Furthermore, the shift in the absorption edge toward longer wavelengths with increasing annealing temperature indicates a slight reduction in the optical transition energy, corresponding to a marginal narrowing of the optical band gap.
Figure 11. Optical characterization of Germanium-doped ZnO thin films annealed at various temperatures: RT, 650 °C, 750 °C, and 850 °C (a) UV-visible Transmittance spectra (b) Tauc plots (c) Variation in ln(α) as a function of (hν) for determination of the Urbach energy.
Pure ZnO has a direct band gap semiconductor structure, wherein the conduction band minimum and the valence band maximum are both situated at the Γ point of the Brillouin zone of the wurtzite structure, thus allowing its fundamental absorption to take place under the conditions of a direct allowed transition [6,34]. The Tauc relation for a direct allowed transition (αhν)2 = A(hν − Eg) was used to calculate the optical band gap of the present Ge-doped ZnO films as shown in Figure 11b [35], where Eg is the direct optical band gap, α is the absorption coefficient, υ is the photon frequency, hν is the photon energy, and A is an energy-independent constant [34]. The estimated optical band gap values are 3.45, 3.57, 3.53, and 3.50 eV for the RT, 650 °C, 750 °C, and 850 °C samples, respectively. The optical band gap widens from 3.45 to 3.57 eV after annealing at 650 °C, as expected with the absorption edge shifting towards shorter wavelengths. This suggests that a higher-energy photon is needed to excite electrons between the conduction band and the valence band. With further increases in the annealing temperature up to 750 °C and 850 °C, the optical band gap reduces slightly to 3.53 eV and 3.50 eV, respectively. This decrease is followed by a gradual absorption edge’s shift towards longer wavelengths, indicating a gradual decrease in the optical transition energy. The changes in the optical band gap are small but the changes suggest that the post-annealing temperature has an effect on the optical properties of the Ge-doped ZnO thin film. The film subjected to annealing at 650 °C has the highest direct optical band gap (3.57 eV), while the films annealed at 750 °C and 850 °C have slightly lower direct optical band gaps of 3.53 eV and 3.50 eV, respectively, with a gradual shift in the absorption edge towards longer wavelengths [36]. To assess the effect of Ge doping on the optical band gap, un-doped ZnO deposited at room temperature under the same sputtering conditions was used as a reference (unpublished data from our group; manuscript under review). The band gap of the ZnO:Ge-RT (Supplementary Series) film is 3.43 eV, as displayed in Figure S1 and Table S1 of the Supplementary Materials, which is 0.38 eV wider than that of the un-doped ZnO film (3.05 eV). This broadening is in agreement with the Burstein–Moss shift due to the increased density of the electrons created by the Ge4+ donors [35]. They are reference films from a different series of as deposited and are only used to demonstrate the direction and size of the Ge effect. In addition, the deposited films show high optical transparency across the whole visible range, and the wide-band-gap properties of ZnO are retained, which demonstrates the successful tailoring of the optical properties of the ZnO thin films by Ge incorporation and thermal annealing without losing their transparency.
The Urbach energy of the films was obtained as indicated in Figure 11c to investigate the role of defects. The absorption coefficient in the absorption edge region is supposed to be a function of the photon energy and follows Urbach’s rule (α = α0 exp (hν/Eu), α0 is a constant, Eu is the Urbach energy) [37]. If the natural log is taken, then the equation becomes ln α = ln α0 + hν/Eu. The transmittance, T, was measured, and using the ellipsometric film thickness, d, the absorption coefficient, α, was calculated as α = −ln(T)/d. The reciprocal of the slope in the linear segment in the curve of ln α against hν (over 3.6–3.9 eV in this case) gave the value of Eu, as shown in Figure 11c. The Eu values are about 249, 209, 207, and 217 meV for the RT, 650 °C, 750 °C, and 850 °C films, respectively. The Urbach energy is the band-tail localized states’ width and is associated with structural and thermal disorder and defects. The RT film exhibits the highest Eu and the lowest optical band gap (Eg = 3.45 eV), while the annealed films show lower Eu and higher optical band gaps (between Eg = 3.50 and 3.57 eV), which is in accordance with the general trend that higher Eu corresponds to lower Eg and vice versa. The higher Urbach energy of the RT film suggests the existence of a greater number of localized states associated with defects in the film and a more disordered network of the films, both of which are consistent with the lower transmittance. The change in Eu after annealing suggests lower disorder within the films and fewer defect states in the band tail, corresponding to the larger size of the crystallites in the annealed films (32–36 nm) compared with the RT film (27 nm).
The role of the Burstein–Moss (BM) effect was determined by estimating the shift from the measured carrier density: ΔEBM = (ħ2/2m*)(3π2n)2/3, where the reduced effective mass m* is set to 0.19 mₑ. The values are about 0.40, 1.16, 0.90, and 0.47 eV for the RT, 650, 750, and 850 °C films. The band gap is widened in the same order as the carrier density, implying a contribution from the BM filling, but the difference in the gap with the RT film (+0.12, +0.08, and +0.05 eV) is much smaller than the BM estimates. Part of this BM shift is thus offset by the band-gap renormalization, which decreases the gap by roughly n1/3 at high electron density [35] and by band non-parabolicity. Structural defects also affect the apparent gap: the RT film has the smallest gap, the largest Urbach energy (about 249 meV as compared to 207–217 meV of the annealed films), and the Urbach energy is increased with the reduction in the structural defects after annealing, which contributes to the widening of the gap. The relative importance of the contributions from BM filling, band-gap renormalization, and defect-related tail states cannot be completely distinguished in the presently available data.

3.8. Ellipsometry Analysis

Spectroscopic ellipsometry has been employed to estimate the optical constants of the ZnO thin films. The Cauchy model was used to get the refractive index (n) and extinction coefficient (k). The ellipsometric data were analyzed using the ASMEC Electro-Physical Characterization System software by modeling the optical response with a multilayer structure, Air/ZnO:Ge/SiO2/Si. All spectra were collected at a fixed 70° angle of incidence, and the fitting was constrained by physically meaningful limits (n ≥ 1.00, k ≥ 0). The reliability of the extracted parameters was confirmed by the low mean squared error (MSE) of approximately 3%. The film thicknesses from the ellipsometric modeling were 293.12 nm for the RT film, 292.43 nm for the film annealed at 650 °C, 292.12 nm for the film annealed at 750 °C, and 292.10 nm for the film annealed at 850 °C. Cauchy model is valid only in the transparent or weakly absorbing spectral region. Therefore, the n and k values in the visible–NIR range, which are used for the main conclusions of this section, are considered reliable. In contrast, the k values in the vicinity of the absorption edge (350–360 nm) are model-dependent and are used only to show relative trends among the samples. The band gap and absorption edge values have been calculated separately from the values of transmittance and Tauc analysis (Figure 11a,b). A Tauc–Lorentz model that fulfills the Kramers–Kronig relations would be a more accurate description of the edge region and is proposed as a future direction.
The effect of post-annealing temperature on the optical loss behavior of Ge-doped ZnO (GZO) thin films was analyzed by examining the wavelength-dependent variation in the extinction coefficient k, as presented in Figure 12a. For all samples, a steep increase in the extinction coefficient (k) is observed in the wavelength range of 350–360 nm, which is associated with the absorption edge observed in Figure 11a,b. This peak is the smallest for the sample annealed at 650 °C (0.32) and gently increases with the annealing temperature, reaching 0.58 for the 850 °C film. It can be seen that for the visible–NIR range, the value of k for the 650 °C sample is the lowest one among all the samples, being even lower than that for the RT film. This may be because of the higher quality of the film for the sample annealed at 650 °C than the ones annealed at higher temperatures, according to XRD and profilometry results [38,39]. At the same time, a dramatic increase in k was observed for the 850 °C annealed film. It is related to additional optical losses caused by diffuse scattering and free-carrier absorption [40]. This increase in the optical loss is consistent with the lower transmittance (~80%) and the band gap narrowing (3.57 → 3.50 eV) for the 850 °C sample.
Figure 12. (a) Extinction Coefficient ‘k’, (b) refractive index ‘n’ of ZnO:Ge thin films annealed at different temperatures (RT, 650, 750 and 850 °C).
Figure 12b depicts the corresponding refractive-index dispersion. All films exhibit anomalous dispersion near the band edge, which is followed by normal dispersion in the visible–NIR range, which is characteristic of the optical response of wide-band-gap semiconductors. The band edge of the n peak decreases as a function of annealing temperature, from ~2.22 for the RT film to 2.13–2.15 for the 650–750 °C films and to ~2.09 for the 850 °C film, which suggests a trend of diminishing amplitude of the refractive-index anomaly with increasing annealing temperature. The refractive index of all films is ~ 1.9–2.0 (~ 400 nm) at the beginning of the visible region and diverges progressively at longer wavelengths. The film at 650 °C has the highest refractive index (~1.90 at 850 nm) in the NIR region, which is close to the reported values for ZnO in this spectral region. The film at 850 °C has the lowest refractive index (~1.71 at 850 nm) with a more pronounced wavelength dependence. This trend correlates with the behavior of k. The 650 °C film shows relatively low optical loss and a refractive index close to that reported for ZnO. The increased surface roughness and microstructure deterioration at 850 °C may explain the reduced refractive index.

3.9. Hall Effect

Hall-effect measurements were employed using a four-probe van der Pauw approach to explore the influence of post-deposition annealing temperature on the electrical transport properties of ZnO:Ge thin films. A magnetic field of 0.46 T was applied, and silver contacts were placed at the four edges of 1 × 1 cm2 samples. The measured negative Hall voltage confirmed n-type conductivity. All the measurements were conducted under room-temperature conditions, and the electrical parameters obtained, such as carrier concentration and mobility, were averaged over multiple scans to reduce experimental uncertainties. The results of the measurements of the carrier concentration, Hall mobility, electrical conductivity, and resistivity are provided in Table 3. These parameters are directly related to the transport of free charge carriers in the semiconductor and can give a lot of information about the electrical quality of the deposited films.
Table 3. The calculated values of Hall parameters of ZnO:Ge thin films annealed at (650, 750 and 850 °C).
The as-deposited (RT) film showed n = 9.60 × 1019 cm−3, μ = 28.0 cm2/V·s, and ρ = 2.33 × 10−3 Ω·cm. Upon annealing at 650 °C, both n and μ increased simultaneously to 4.71 × 1020 cm−3 and 39.0 cm2/V·s, giving the lowest resistivity (3.40 × 10−4 Ω·cm) and sheet resistance (11.63 Ω/sq). Increasing crystallite size in grain-boundary-limited transport decreases the height of the potential barriers at the grain boundaries and decreases electron scattering at grain boundaries, and thus leads to a simultaneous increase in carrier concentration and mobility, which is different from the ionized-impurity-scattering regime, in which mobility generally decreases with an increase in doping [41,42]. This increase in carrier density only in the grain region is not sufficient to explain the increase between RT and 650 °C films, as the crystallite size and the mobility are increased by only 1.4 times, keeping the EDX composition unchanged. The former effect is thermal activation of Ge, in which Ge atoms in interstitial sites, at the grain boundaries, or in the disordered regions become active as Ge4+, and each supplies up to two electrons to the conduction band, while the latter is due to a reduction in the number of compensating defects and in the number of electron traps at the grain boundaries. This is in line with the XRD crystallite size increase (27–36 nm). Since the annealing was done in air, oxygen incorporation and the modification of oxygen-related defects must also be considered. Annealing in air provides oxygen and is expected to reduce the concentration of oxygen vacancies, which in ZnO behave mainly as deep donors and contribute little to the free-electron density at room temperature. Therefore, the reduction of oxygen vacancies cannot be responsible for the nearly fivefold increase in the electron density at 650 °C and rather points to shallow donors, in particular Ge 4+ at Zn sites. The conductivity is enhanced by a factor of about 6.8, and about 80% of the enhancement is attributed to the increased electron density and only 20% to the increased mobility. Hence, the improved crystallinity is not the main origin of the higher conductivity. Moreover, the chemisorption of oxygen at grain boundaries and the reduction of oxygen-related trap states may improve the measured carrier density and mobility, and the lower Urbach energy of annealed films indicates fewer defect-related localized states. With further annealing at 750 and 850 °C, both n and μ progressively decreased, reaching 1.20 × 1020 cm−3 and 20.0 cm2/V·s at 850 °C, with resistivity rising to 2.60 × 10−3 Ω·cm. This degradation is related to the roughening of the surface (Ra = 60.89 nm) and the agglomerated grain morphology revealed by profilometry and SEM, which provide further interface and void scattering. The error bars in conductivity and resistivity come from the uncertainty in the geometry of the sample, such as the placement of contacts and the thickness of the film, the stability of the magnetic field applied to the sample, and the reproducibility of repeated Hall measurements, as illustrated in Figure 13. The optical band gap widened as the carrier concentration increased from RT to 650 °C, and then narrowed at 750 and 850 °C as the carrier concentration decreased, due to the Burstein–Moss effect; the Fermi energy level is shifted into the conduction band at high doping levels, and then many-body band-gap renormalization occurs at very high carrier densities [35].
Figure 13. The error bars for the conductivity and resistivity values of ZnO:Ge films annealed at various temperatures.
Finally, the overall TCO performance was quantitatively evaluated by calculating the Haacke figure of merit [43] φ = T10/Rs, where Rs = ρ/t is the sheet resistance, and t is the film thickness (292.1–293.1 nm), and T is the transmittance at 550 nm (Table 4). The ZnO:Ge-650 °C film exhibits the maximum value (5.1 × 10−2 Ω−1), about 36 times higher than that of the as-deposited film (1.4 × 10−3 Ω−1), and the values decrease to 1.7 × 10−2 and 3.1 × 10−3 Ω−1 for the films annealed at 750 and 850 °C, respectively. The ratio of DC to optical conductivity, σdc/σopt, shows the same trend (624 for the 650 °C film) [44]. These results confirm that annealing at 650 °C provides the optimum combination of low sheet resistance and high visible transparency in the films studied.
Table 4. Haacke figure of merit φ = T10/Rs, and the ratio of DC to optical conductivity, σdc/σopt = Z0 ÷ [2Rs(T(−1/2) − 1)] with Z0 = 377 Ω, using the sheet resistance Rs = ρ/t and the transmittance T at 550 nm).

3.10. Comparison of Optoelectronic Parameters of ZnO:Ge-650 °C with Recently Reported Doped ZnO Thin Films

The optoelectronic properties of the best-performing ZnO:Ge film annealed at 650 °C are summarized in Table 5 and compared with those of recently reported doped ZnO thin films. The present film exhibits a high optical transparency (~95%) and high Hall mobility (39 cm2/V·s, the highest among the films listed), with resistivity (3.40 × 10−4 Ω·cm) comparable to the lowest reported values. The optical band gap of the present film (3.57 eV) is within the range reported for doped ZnO films [45,46], although the carrier concentration (4.71 × 1020 cm−3) is lower than that of the PLD-grown ZnO:Ge [47] and GZO films [48] and the AZO film [49], its higher mobility compensates for this, giving a resistivity level similar to or slightly lower than those of GZO [48] and AZO. It demonstrates that the improved crystallinity, together with the reduced grain-boundary scattering after annealing at 650 °C, leads to the beneficial combination of transparency and conductivity. The comparison is indicative only, as the films differ in dopant, deposition technique, and processing conditions.
Table 5. Comparison of the deposition method, annealing/substrate temperature, optical band gap (Eg), transmittance, carrier concentration, Hall mobility and resistivity in the present ZnO:Ge-650 °C film with recently reported doped ZnO thin films.

3.11. Application of ZnO:Ge Thin Films

The ZnO:Ge-650 °C best-performing sample was further tested for its dynamic photoresponse characteristics to investigate its suitability as a visible-light-responsive optoelectronic switching device. The device structure and the measurement configuration for this study are illustrated in Figure 14a, which is a Ag electrode (0.5 × 0.5 mm2 pads)/ZnO:Ge film/Si (100) substrate geometry under 555 nm illumination. The film exhibits a photocurrent (I–t) response when repeatedly illuminated in on/off mode at a fixed applied bias of 2 V, as shown in Figure 14b.
Figure 14. (a) Schematic structure of the device and the measurement setup for the photoresponse test. (b) The time-dependent photocurrent (I-t) response of the best-performing sample of ZnO:Ge-650 °C under periodic ON/OFF illumination cycles.
In the dark condition, the current in the ZnO:Ge film is also low, with a value of 1.15 nA, which is attributed to the current being limited by the Ag/ZnO:Ge/Si device structure and contacts. Under the same conditions, when the light source is illuminated, its nominal power density is 26.2 mW/cm2, and the peak wavelength is 555 nm, which is visible light, and the current is increased to 2.03 nA, which corresponds to a photo-to-dark current ratio of 1.8. The increase in current under illumination is due to the photogeneration of electron-hole pairs and desorption of surface-adsorbed oxygen molecules that transfer trapped electrons back into the conduction band, thereby increasing the free-carrier density and the overall conductivity of the film. Since the energy of a 555 nm photon (2.23 eV) is much smaller than the optical band gap of the film (3.57 eV), the response cannot be related to band-to-band excitation. Sub-gap absorption of the film is due to defect states, a broad band tail (Figure 11c), Urbach energy ~209 meV, O 1s at 531.7 eV (Figure 6C) (indicative of oxygen deficiency), and the photodesorption of surface-adsorbed oxygen. When the light is turned off, the recombination and trapping of the charge carriers generated by the light can take place through the re-adsorption of the oxygen molecules at the surface of the film, which results in a fast decay of the current back to its dark-state value. The rise (10–90%) and decay (90–10%) times are 4s and 2.7 s, respectively, while steady state is approached in ~ 10 s. Such response times of a few seconds are consistent with an oxygen adsorption/desorption limited process taking place at the grain boundaries and the filling of the defect and band-tail states (Urbach energy ≈ 209 meV) but not with the carrier lifetime and additionally include effects related to the ZnO/Si junction and measurement circuit. This is a modest photo/dark-current ratio of ~1.8. The ZnO:Ge-650 °C film was tailored for conductivity; its high electron density (4.71 × 1020 cm−3) ensures that a small photogenerated carrier density will result in a small relative change in current. Moreover, the defects associated with Ge may serve as recombination centers, and the carrier lifetime may be reduced as well. The measured current also depends on the structure of the device Ag/ZnO:Ge/Si. The photocurrent response is again reproducible for the four cycles of the illumination with a small drift in the peak current and in the baseline from cycle to cycle. Therefore, the film acts like an optoelectronic switch for visible light, and lower carrier density or UV illumination would give better on/off ratios.
The I–t data of the ZnO:Ge-650 °C device in Figure 14b was used to quantitatively evaluate the photoresponse by calculating the key photodetector parameters, which are summarized in Table 6. The dark current was I dark = 1.15 nA, the current under illumination with 555 nm was I light = 2.03 nA; and the photocurrent was ΔI = I light − I dark = 0.88 nA. A nominal incident optical power density of P = 26.2 mW/cm2 was utilized, and an illuminated junction area of A = 1 cm2 was utilized. The Ag pads (0.5 × 0.5 mm2) serve only as electrical contacts; because the film is highly conductive (Rs = 11.63 Ω/sq), the photocurrent is collected from the whole illuminated 1 × 1 cm2 junction. The responsivity was calculated as R = ΔI/(P·A), giving ≈3.4 × 10−8 A/W. The external quantum efficiency was calculated using EQE = R·hc/(eλ) (≈7.5 × 10−6%), where h is Planck’s constant, c is the speed of light, e is the charge of an electron, and λ = 555 nm is the wavelength corresponding to the peak of the emission spectrum. Assuming that the shot noise from the dark current is the dominant noise source, the noise current is in = (2e·Idark)½ ≈ 1.9 × 10−14 A Hz-½. The noise-equivalent power, NEP = in/R, is then ≈5.7 × 10−7 W Hz−½, and the specific detectivity, D* = R·A½/in, is ≈1.7 × 106 Jones. The values given are modest, since the photons at 555 nm (2.23 eV) are quite far from the band gap of 3.57 eV, so only weak sub-gap defect-assisted absorption contributes, and because the film was optimized for high conductivity (n = 4.71 × 1020 cm−3), which increases the dark current. Since only shot noise was considered, D* and NEP should be regarded as estimates, as Johnson and 1/f noise were not measured. Thus, the ZnO:Ge-650 °C film is not an optimized high-sensitivity photodetector; rather, it can be regarded as a stable visible-light optoelectronic switch.
Table 6. The photoresponse parameters of the ZnO:Ge-650 °C device measured from the I–t data in Figure 14b under illumination with 555 nm light with a nominal P = 26.2 mW/cm2 at 2 V bias and an illuminated junction area A = 1 cm2. The estimates are shot-noise-limited (D* and NEP).

4. Conclusions

RF magnetron sputtering was successfully employed to synthesize Ge-doped Zinc Oxide thin films on Si and glass substrates at room temperature, followed by post-deposition annealing at 650 °C, 750 °C, and 850 °C to study the effects of post-deposition annealing on the structure, optical, and electrical properties of the thin films. All the ZnO:Ge films exhibited a polycrystalline hexagonal wurtzite crystal structure, and no secondary phases could be detected in the entire investigated range of annealing temperatures in the XRD analysis. The crystallite size was 27 nm for the RT film and 36 nm for the film annealed at 650 °C, indicating enhanced crystallite growth and improved structural quality upon increasing the annealing temperature up to a certain limit. This improvement is also supported by the enhanced intensity of the (002) diffraction peak at 650 °C, indicating improved crystallinity and a stronger preferential orientation along the c-axis. Raman spectroscopy further confirmed the wurtzite structure of ZnO through the dominant E2 (high) phonon mode at 435–438 cm−1, with no additional bands attributable to secondary Ge-containing phases. An FTIR analysis also verified the retention of the Zn–O framework and revealed a Ge-related vibrational band at 565 cm−1, providing additional evidence of Ge incorporation into the ZnO lattice without forming a Ge-related impurity phase. The XPS spectrum of the annealed ZnO:Ge film showed the presence of the Zn2+ and Ge4+ states, although the Ge metallic state was not detected, which suggests that Ge was incorporated into the ZnO matrix in an oxidized state. The optical characterization verified the role of thermal annealing in the modification of the optical properties of the Ge-doped ZnO thin films. The optical band gap exhibited an increase from 3.45 eV for the RT film to the maximum value of 3.57 eV after annealing at 650 °C. Further increase in annealing temperature decreased the band gap slightly to 3.53 eV and 3.50 eV for the films annealed at 750 °C and 850 °C, respectively. The spectroscopic ellipsometry also showed a high dependence of the refractive index and extinction coefficient on the annealing temperature. The film post-annealed at 650 °C possessed the maximum refractive index in the NIR region among the films annealed at different temperatures, which was close to the reported value for bulk ZnO, consistent with a relatively good optical quality and a dense microstructure for the 650 °C annealed film. Moreover, the film annealed at 650 °C exhibited the lowest extinction coefficient, implying that it has decreased optical losses compared with the other annealed films. The electrical transport properties were also found to be sensitive to thermal treatment, as shown by Hall-effect measurements. The film annealed at 650 °C showed the highest carrier concentration of 4.71 × 1020 cm−3, the maximum mobility of 39 cm2/V.s, the highest electrical conductivity of 2.94 × 103 (1/Ω.cm) and the smallest resistivity of 3.40 × 10−4 (Ω.cm). These findings show that the best electrical transport properties were obtained for the above annealing conditions. Overall, the structural, optical, and electrical results suggest that annealing at 650 °C provides the best balance of crystallinity, optical quality, and charge-transport properties of the films. The Haacke figure of merit of the 650 °C film (5.1 × 10−2 Ω−1) was about 36 times higher than that of the as-deposited film, indicating the benefits of annealing at 650 °C. As a preliminary device demonstration, the 650°C annealed ZnO:Ge film also showed a stable and reproducible visible-light photo-switching response with a photo-to-dark current ratio of ~1.8, demonstrating its potential for visible-light optoelectronic switching applications. Building upon these findings, future research will focus on integrating the best-supported ZnO films as transparent front electrodes into functional optoelectronic architectures, including perovskite solar cells, thin-film transistors (TFTs), and flexible device structures. Further investigations employing rapid thermal processing (RTP) or localized laser annealing may offer precise thermal budget control, enabling process compatibility with heat-sensitive flexible polymeric substrates.

Supplementary Materials

The following supporting information can be downloaded at: https://www.mdpi.com/article/10.3390/photonics13121106/s1. Figure S1:Tauc plots, (αhν)2 versus hν, of pure ZnO-RT and ZnO:Ge films deposited at RT, 250 °C, and 350 °C. Solid black lines indicate extrapolated band-gap values.; Table S1: Optical band gap of un-doped and Ge-doped ZnO thin films grown at different substrate temperatures. Figure S2 presents the UV–Vis absorbance and transmittance spectra of pure ZnO and Ge-doped ZnO thin films obtained at various substrate temperatures.

Author Contributions

S.S. conceived the research topic and designed the whole experiment. D.-e.-S.K., as part of her PhD thesis, developed the idea, performed the experiment, fabricated the films, characterized them, and analyzed the data. D.-e.-S.K. drafted the text, examined the measured data, and discussed the findings. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Data Availability Statement

The data presented in this study are available on request from the corresponding author.

Conflicts of Interest

The authors declare no conflicts of interest.

References

  1. Ginley, D.S.; Bright, C. Transparent conducting oxides. MRS Bull. 2000, 25, 15–18. [Google Scholar] [CrossRef] [Scilit]
  2. Minami, T. Transparent conducting oxide semiconductors for transparent electrodes. Semicond. Sci. Technol. 2005, 20, S35–S44. [Google Scholar] [CrossRef] [Scilit]
  3. Du, J.; Chen, X.-l.; Liu, C.-C.; Ni, J.; Hou, G.-F.; Zhao, Y.; Zhang, X.-D. Highly transparent and conductive indium tin oxide thin films for solar cells grown by reactive thermal evaporation at low temperature. Appl. Phys. A 2014, 117, 815–822. [Google Scholar] [CrossRef] [Scilit]
  4. Ellmer, K. Past achievements and future challenges in the development of optically transparent electrodes. Nat. Photonics 2012, 6, 809–817. [Google Scholar] [CrossRef] [Scilit]
  5. Look, D.C. Recent advances in ZnO materials and devices. Mater. Sci. Eng. B 2001, 80, 383–387. [Google Scholar] [CrossRef] [Scilit]
  6. Janotti, A.; Van de Walle, C.G. Fundamentals of zinc oxide as a semiconductor. Rep. Prog. Phys. 2009, 72, 126501. [Google Scholar] [CrossRef] [Scilit]
  7. Zhu, W.; Kammuri, T.; Kitamura, S.; Sturaro, M.; Martucci, A.; Pezzotti, G. Structure and composition evaluation of heavily Ge-doped ZnO nanocrystal films. J. Phys. D Appl. Phys. 2018, 51, 085302. [Google Scholar] [CrossRef] [Scilit]
  8. Salem, K.E.; Mokhtar, A.M.; Soliman, I.; Ramadan, M.; Shaheen, B.S.; Allam, N.K. Ge-doped ZnO nanorods grown on FTO for photoelectrochemical water splitting with exceptional photoconversion efficiency. Int. J. Hydrogen Energy 2021, 46, 209–220. [Google Scholar] [CrossRef] [Scilit]
  9. Baek, S.H.; Lee, D.K.; Kang, T.D.; Choi, S.H.; Lee, H.; Eom, S.H. Optical properties of Ge-doped ZnO thin films studied with spectroscopic ellipsometry. J. Korean Phys. Soc. 2008, 53, 451–460. [Google Scholar] [CrossRef] [Scilit]
  10. Jiang, M.; Wang, Z.; Ning, Z. Study of structural and optical properties of Ge doped ZnO films. Thin Solid Films 2009, 517, 6717–6720. [Google Scholar] [CrossRef] [Scilit]
  11. Arulraj, A. Enhanced photoconductive response of ZnO thin films with the impact of annealing temperatures on structural and optical properties. Sci. Rep. 2025, 15, 28851. [Google Scholar] [CrossRef] [Scilit]
  12. Fan, D.; Ning, Z.; Jiang, M. Characteristics and luminescence of Ge doped ZnO films prepared by alternate radio frequency magnetron sputtering. Appl. Surf. Sci. 2005, 245, 414–419. [Google Scholar] [CrossRef] [Scilit]
  13. Zheng, T.; Li, Z.; Chen, J.; Shen, K.; Sun, K. Transitions of microstructure and photoluminescence properties of the Ge/ZnO multilayer films in certain annealing temperature region. Appl. Surf. Sci. 2006, 252, 8482–8486. [Google Scholar] [CrossRef] [Scilit]
  14. Knura, R.; Skibińska, K.; Sahayaraj, S.; Marciszko-Wiąckowska, M.; Gwizdak, J.; Wojnicki, M.; Żabiński, P.; Sapeta, G.; Iwanek, S.; Socha, R.P. Evaluation of the electronic properties of atomic layer deposition-grown Ge-doped zinc oxide thin films at elevated temperatures. Electronics 2024, 13, 554. [Google Scholar]
  15. Sabeeh, S.H.; Jassam, R.H. The effect of annealing temperature and Al dopant on characterization of ZnO thin films prepared by sol-gel method. Results Phys. 2018, 10, 212–216. [Google Scholar]
  16. Kabir, M.H.; Ali, M.M.; Kaiyum, M.A.; Rahman, M. Effect of annealing temperature on structural morphological and optical properties of spray pyrolized Al-doped ZnO thin films. J. Phys. Commun. 2019, 3, 105007. [Google Scholar] [CrossRef] [Scilit]
  17. Jumidali, M.M.; Sulieman, K.M.; Hashim, M.R. Structural, optical and electrical properties of ZnO/Zn2GeO4 porous-like thin film and wires. Appl. Surf. Sci. 2011, 257, 4890–4895. [Google Scholar] [CrossRef] [Scilit]
  18. Bui, Q.C. Development of ZnO Thin Films and Nanowires by Pulsed-Liquid Injection Metal-Organic Chemical Vapor Deposition for Piezoelectric Applications. Doctoral Dissertation, Université Grenoble Alpes, Saint-Martin-d’Hères, France, 2022. [Google Scholar]
  19. Hyun, J.W.; Kim, Y.J.; Kim, G.B.; Lee, J.H.; Shin, J.S. Effect of annealing on ZnO thin films prepared by using the sol-gel method. J. Korean Phys. Soc. 2012, 60, 1118–1123. [Google Scholar] [CrossRef] [Scilit]
  20. Sobha, A.; Johnson, J.; Abhina, K. ZnO nanoparticles: Strain-engineered photocatalytic performance and optical properties validated by Mie theory. J. Alloys Compd. 2025, 1037, 182365. [Google Scholar] [CrossRef] [Scilit]
  21. Miranda, G.G.; e Silva, R.L.d.S.; dos Santos Pessoni, H.V.; Franco, A., Jr. Raman spectroscopy study of Ga-doped ZnO ceramics: An estimative of the structural disorder degree. Phys. B Condens. Matter 2021, 606, 412726. [Google Scholar]
  22. Lu, Z.; Quinn, T.; Reehal, H. Polarization-dependent Raman spectra of thin crystalline silicon films. J. Appl. Phys. 2005, 97, 033512. [Google Scholar] [CrossRef] [Scilit]
  23. Zamiri, R.; Rebelo, A.; Zamiri, G.; Adnani, A.; Kuashal, A.; Belsley, M.S.; Ferreira, J. Far-infrared optical constants of ZnO and ZnO/Ag nanostructures. RSC Adv. 2014, 4, 20902–20908. [Google Scholar] [CrossRef] [Scilit]
  24. Fan, D.; Zhang, R.; Su, W.; Zhang, J. Phase transition and optical properties of Ge doped ZnO films synthesised by sputtering. Mater. Sci. Technol. 2015, 31, 37–42. [Google Scholar] [CrossRef] [Scilit]
  25. Zhang, F.; Volodin, V.; Astankova, K.; Kamaev, G.; Azarov, I.; Prosvirin, I.; Vergnat, M. Determination of the infrared absorption cross-section of the stretching vibrations of Ge–O bonds in GeOx films. Results Chem. 2022, 4, 100461. [Google Scholar] [CrossRef] [Scilit]
  26. Kim, S.; Lee, D.K.; Hong, S.H.; Eom, S.H.; Oh, H.T.; Choi, S.-H.; Hwang, H.N.; Hwang, C.C. High-efficient ultraviolet emission in phonon-reduced ZnO films: The role of germanium. J. Appl. Phys. 2008, 103, 023514. [Google Scholar] [CrossRef] [Scilit]
  27. Raevskaya, A.; Panasiuk, Y.V.; Stroyuk, O.; Kuchmiy, S.Y.; Dzhagan, V.; Milekhin, A.; Yeryukov, N.; Sveshnikova, L.; Rodyakina, E.; Plyusnin, V. Spectral and luminescent properties of ZnO–SiO2 core–shell nanoparticles with size-selected ZnO cores. RSC Adv. 2014, 4, 63393–63401. [Google Scholar] [CrossRef] [Scilit]
  28. Ceylan, A.; Rumaiz, A.K.; Caliskan, D.; Ozcan, S.; Ozbay, E.; Woicik, J. Effects of rapid thermal annealing on the structural and local atomic properties of ZnO: Ge nanocomposite thin films. J. Appl. Phys. 2015, 117, 105303. [Google Scholar]
  29. Biesinger, M.C.; Lau, L.W.; Gerson, A.R.; Smart, R.S.C. Resolving surface chemical states in XPS analysis of first row transition metals, oxides and hydroxides: Sc, Ti, V, Cu and Zn. Appl. Surf. Sci. 2010, 257, 887–898. [Google Scholar] [CrossRef] [Scilit]
  30. Sahayaraj, S.; Knura, R.; Skibińska, K.; Starowicz, Z.; Bulowski, W.; Gawlińska-Nęcek, K.; Panek, P.; Wojnicki, M.; Iwanek, S.; Majchrowicz, Ł. Tuning the Optical and Electrical Properties of ALD-Grown ZnO Films by Germanium Doping. Materials 2024, 17, 2906. [Google Scholar] [CrossRef] [Scilit]
  31. Chen, M.; Wang, X.; Yu, Y.; Pei, Z.; Bai, X.; Sun, C.; Huang, R.; Wen, L. X-ray photoelectron spectroscopy and auger electron spectroscopy studies of Al-doped ZnO films. Appl. Surf. Sci. 2000, 158, 134–140. [Google Scholar] [CrossRef] [Scilit]
  32. Shkir, M.; Khan, M.T.; Marnadu, R.; Khan, A.; Ahmad, Z.; Alshahrani, T. Microstructural engineering of ZnO thin films: Large-crystallite, low-defect architectures enable superior NH3 chemisorption and electron percolation. Ceram. Int. 2026, 52, 55246–55259. [Google Scholar] [CrossRef] [Scilit]
  33. Cui, M.; Wu, X.; Zhuge, L.; Meng, Y. Effects of annealing temperature on the structure and photoluminescence properties of ZnO films. Vacuum 2007, 81, 899–903. [Google Scholar] [CrossRef] [Scilit]
  34. Özgür, Ü.; Alivov, Y.I.; Liu, C.; Teke, A.; Reshchikov, M.A.; Doğan, S.; Avrutin, V.; Cho, S.-J.; Morkoç, H. A comprehensive review of ZnO materials and devices. J. Appl. Phys. 2005, 98, 041301. [Google Scholar] [CrossRef] [Scilit]
  35. Jain, A.; Sagar, P.; Mehra, R. Band gap widening and narrowing in moderately and heavily doped n-ZnO films. Solid-State Electron. 2006, 50, 1420–1424. [Google Scholar] [CrossRef] [Scilit]
  36. Irimpan, L.; Ambika, D.; Kumar, V.; Nampoori, V.; Radhakrishnan, P. Effect of annealing on the spectral and nonlinear optical characteristics of thin films of nano-ZnO. J. Appl. Phys. 2008, 104, 033118. [Google Scholar] [CrossRef] [Scilit]
  37. Rai, R. Analysis of the Urbach tails in absorption spectra of undoped ZnO thin films. J. Appl. Phys. 2013, 113, 153508. [Google Scholar] [CrossRef] [Scilit]
  38. Vijay, N.K.; Maya, P.; Mukherjee, S.; Liedke, M.; Butterling, M.; Attallah, A.; Hirschmann, E.; Wagner, A.; Benoy, M. Effect of annealing temperature on the structure and optical properties of ZnO thin films. J. Phys. Condens. Matter 2023, 36, 135002. [Google Scholar] [CrossRef] [Scilit]
  39. Gao, W.; Li, Z. ZnO thin films produced by magnetron sputtering. Ceram. Int. 2004, 30, 1155–1159. [Google Scholar] [CrossRef] [Scilit]
  40. Bak, S.-Y.; Lee, S.-H.; Jang, H.; Kim, M.; Kim, S.; Yi, M. Transparent Al-doped ZnO thin films for high-sensitivity NO2 gas sensing. Sensors 2025, 25, 3622. [Google Scholar]
  41. Minami, T.; Miyata, T.; Tokunaga, H. Electron scattering from disordered grain boundaries in degenerate polycrystalline Al-doped ZnO thin films. Phys. Status Solidi (A) 2019, 216, 1700783. [Google Scholar]
  42. Mahapatra, B.; Sarkar, S. Understanding of mobility limiting factors in solution grown Al doped ZnO thin film and its low temperature remedy. Heliyon 2022, 8, e10961. [Google Scholar] [CrossRef] [Scilit]
  43. Bobadilla-Barrón, G.; Maldonado, A.; Olvera, M.d.l.L.; Zamora-Justo, J.A. Effect of solutions acidity on Haacke’s Figure of Merit of ZnO and ZnO: F thin films deposited by ultrasonic spray pyrolysis. Front. Nanotechnol. 2024, 6, 1445269. [Google Scholar] [CrossRef] [Scilit]
  44. Kim, D.; Jeong, S.; Lee, D.K.; Yi, W.; Yoon, H.; Jeon, J.; Kim, H.; Lee, B.; Hong, Y. High-performance transparent metal mesh electrodes utilizing a metal-vapor-desorption layer for organic light-emitting diode applications. Mater. Horiz. 2026, 13, 4863–4874. [Google Scholar] [CrossRef] [Scilit]
  45. Nulhakim, L.; Rozana, M.; Yuliarto, B.; Makino, H. Electrical and optical properties of Ga-doped ZnO thin films deposited by DC magnetron sputtering. J. Sci. Appl. Technol. 2020, 4, 15–20. [Google Scholar] [CrossRef] [Scilit]
  46. Clatot, J.; Campet, G.; Zeinert, A.; Labrugère, C.; Nistor, M.; Rougier, A. Low temperature Si doped ZnO thin films for transparent conducting oxides. Sol. Energy Mater. Sol. Cells 2011, 95, 2357–2362. [Google Scholar] [CrossRef] [Scilit]
  47. Yan, Z.; Bao, J.; Yue, X.-Y.; Li, X.-L.; Zhou, Y.-N.; Wu, X.-J. Impacts of preparation conditions on photoelectric properties of the ZnO: Ge transparent conductive thin films fabricated by pulsed laser deposition. J. Alloys Compd. 2020, 812, 152093. [Google Scholar] [CrossRef] [Scilit]
  48. Shewale, P.; Lee, S.; Yu, Y. Pulse repetition rate dependent structural, surface morphological and optoelectronic properties of Ga-doped ZnO thin films grown by pulsed laser deposition. J. Alloys Compd. 2017, 725, 1106–1114. [Google Scholar]
  49. Shih, N.-F.; Chen, J.-Z.; Jiang, Y.-L. Properties and analysis of transparency conducting AZO films by using DC power and RF power simultaneous magnetron sputtering. Adv. Mater. Sci. Eng. 2013, 2013, 401392. [Google Scholar] [CrossRef] [Scilit]
  50. Lekoui, F.; Ouchabane, M.; Akkari, H.; Hassani, S.; Dergham, D. Effect of annealing temperature on the properties of Ag doped ZnO thin films. Mater. Res. Express 2018, 5, 106406. [Google Scholar]
  51. Alam, M.; Cameron, D. Preparation and properties of transparent conductive aluminum-doped zinc oxide thin films by sol–gel process. J. Vac. Sci. Technol. A Vac. Surf. Films 2001, 19, 1642–1646. [Google Scholar] [CrossRef] [Scilit]
  52. Peng, L.; Fang, L.; Yang, X.; Li, Y.; Huang, Q.; Wu, F.; Kong, C. Effect of annealing temperature on the structure and optical properties of In-doped ZnO thin films. J. Alloys Compd. 2009, 484, 575–579. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Article metric data becomes available approximately 24 hours after publication online.