Abstract
This study aimed to address the clinical challenge of secondary caries prevention in dental restorations. Leveraging the sustained fluoride-releasing capacity of calcium fluoride (CaF2) and the broad-spectrum antibacterial activity of zinc oxide (ZnO), we designed and synthesized a novel core–shell CaF2@ZnO nanoparticle filler to synergistically enhance the functional performance of dental resin composites. The filler was successfully prepared via a co-precipitation-hydrothermal method, and its well-defined core–shell architecture was systematically confirmed using XRD, SEM, and TEM. When incorporated into the resin matrix at 10 wt.% loading, the composite containing CaF2@30ZnO demonstrated optimal overall performance. Notably, this formulation enabled sustained fluoride ion release, potent antibacterial efficacy, and excellent in vitro cytocompatibility. Collectively, these findings demonstrate that the CaF2@ZnO nanofiller confers multifunctional benefits—including improved mechanical integrity, long-term fluoride release stability, and targeted antibacterial action—thereby holding significant promise for clinical application in mitigating secondary caries around resin-based restorations.
1. Introduction
Dental caries is one of the most prevalent non-communicable diseases worldwide and statistically nearly 44% of dental caries cases remain untreated. Consequently, the prevention of dental caries is of critical importance. Among the key challenges in management of caries are the recurrence of the disease and the failure of dental restorations [1,2,3]. Addressing secondary caries and extending the service life of restorations remain pivotal challenges in contemporary dentistry. Conventional light-cured composite resins are widely employed in dental restorations owing to their rapid curing, favorable aesthetics, and good biocompatibility [4,5,6]. These materials are multi-phase composites typically consisting of an organic resin matrix, inorganic fillers, photoinitiators, and coupling agents [7]. Inorganic fillers, such as silica, hydroxyapatite, calcium fluoride, and various metal oxides, are integral to their performance [8,9,10,11]. By varying the particle size and composition of these fillers, the mechanical properties, fluoride release capability, and antibacterial efficacy of the composites can be significantly enhanced [12,13].
F− is essential trace elements for maintaining dental health [14,15]. The continuous release of fluoride is one of the most effective and widely used public health measures for preventing tooth decay, as it can enhance the teeth’s resistance to decay in multiple ways and inhibit the activity of cariogenic bacteria, thereby achieving the prevention goal. Compared to other fluoride compounds, CaF2 has good biocompatibility [16]. CaF2 is slightly soluble in water and can provide a longer period of fluoride ion release. It combines with Ca2+ and PO43−, promoting tooth remineralization [17,18,19], forming fluorapatite, enhancing the acid resistance of enamel, and reducing the erosion effect of acid on teeth. Fluoride ions can inhibit the key enzymes for sugar fermentation of cariogenic bacteria [20], reducing the production of lactic acid; it may also affect the adhesion ability of harmful bacteria on the tooth surface [21,22], reducing the formation of dental plaque biofilm. CaF2 serves as an unstable F− storage reservoir [23,24], featuring small size and a large specific surface area. It can be incorporated into the resin matrix at a relatively low content [25], ensuring the mechanical properties of the composite resin. However, traditional dental composite resins containing only CaF2 tend to exhibit a gradual decline in mechanical properties and diminished fluoride-releasing capacity over time [26].
To address these issues, the preparation of core–shell structure materials is of crucial importance. Unlike previous approaches that simply mixed CaF2 and ZnO nanoparticles as separate fillers or employed SiO2@ZnO core–shell systems without fluoride release capability, our CaF2@ZnO core–shell design integrates both fluoride release and antibacterial functions into a single hybrid particle. The nano-ZnO shell not only enhances the stability of the CaF2 core, reducing filler wear and detachment under stress and thereby enhancing the mechanical properties of the composite resin [27], but also effectively slows the release rate of F− ions. This facilitates sustained inhibition of demineralization and promotion of remineralization, endowing the material with long-term secondary caries prevention capability [28]. ZnO is recognized as a broad-spectrum antibacterial agent with excellent biocompatibility [29]. It inhibits oral pathogens through multiple mechanisms, including the generation of reactive oxygen species and the release of Zn2+ ions [30,31]. By combining the physical antibacterial effect of the ZnO shell with the chemical antibacterial environment created by the release of Zn2+ and F− ions from the core, the CaF2@ZnO structure establishes a dual antibacterial mechanism. This synergy significantly enhances its efficacy in preventing secondary caries [32] and contributes to prolonging the service life of the restoration [33]. Compared with CaF2@SiO2 fillers (which lack intrinsic antibacterial activity) and physical mixtures of CaF2 and ZnO (which suffer from poor dispersion and uncontrolled ion release), our core–shell design offers the advantages of local co-delivery of both therapeutic ions, enhanced mechanical properties, and sustained therapeutic effects.
This study provides a reproducible fabrication strategy and a systematic evaluation of the biomechanical properties for developing a new generation of dental restorative materials that integrate mechanical support with antibacterial function. Although the current results are limited to in vitro conditions, the material exhibits promising performance that warrants further investigation. Following successful validation in future in vivo and clinical studies, its potential applications may include posterior restorations in patients with high caries risk, early childhood caries intervention, and root surface caries prevention.
2. Materials and Methods
2.1. Chemical Reagents
Calcium nitrate tetrahydrate was purchased from Tianjin Damao Reagent Company (Tianjin, China). Zinc nitrate hexahydrate, γ-MPS, ammonium fluoride, and urea were obtained from Aladdin Reagent Company (Shanghai, China). Methanol was purchased from Concord Reagent Company (Tianjin, China). All reagents were of analytical purity.
2.2. Preparation and Modification of CaF2 and CaF2@ZnO Nanoparticles
2.2.1. Preparation of CaF2 Nanoparticles
A certain molar ratio of calcium nitrate tetrahydrate and ammonium fluoride respectively were dissolved in equal volumes of methanol. Then, the solutions were ultrasonicated for 20 min and stirred to make them uniformly dispersed in the methanol solvent, resulting in a calcium nitrate methanol solution and an ammonium fluoride methanol solution with certain molar concentrations. Next, the calcium nitrate methanol solution was slowly added to the rapidly stirred ammonium fluoride methanol solution. The resulting solution was stirred in a water bath at 25 °C for 10 min. Then, the completely reacted white solution was transferred to a centrifuge tube and washed three times with anhydrous ethanol (10,000 rpm, 5 min), obtaining a white filter cake, which was dried overnight in a vacuum drying box at 60 °C to obtain the precursor of CaF2.
2.2.2. Preparation of CaF2@ZnO Nanoparticles
Using the CaF2 prepared by the aforementioned co-precipitation method as the precursor, ZnO was coated onto the CaF2 substrate through the hydrothermal synthesis method to fabricate core–shell nanoparticles of ZnO encapsulated in CaF2. The experimental steps are as follows: Calcium fluoride powder was added to deionized water and ultrasonicated for 30 min to fully disperse the calcium fluoride particles, forming a uniform and stable suspension. Then, zinc nitrate and urea were added and stirred for 10 min. Subsequently, the fully mixed solution was transferred to the reaction vessel, reacted at 105 °C for 3 h, cooled to room temperature, and the reaction product was transferred to a centrifuge tube. The product was centrifuged and washed three times with anhydrous ethanol (10,000 rpm, 5 min) to obtain a white filter cake. The cake was dried overnight in a vacuum drying oven at 60 °C, and then heated at a temperature increase rate of 5 °C/min to 350 °C for 2 h to obtain CaF2@ZnO nanoparticles. The amount of zinc nitrate was varied to regulate the ZnO coating coverage and to identify the optimal synthesis parameters.
2.2.3. Modification of CaF2 and CaF2@ZnO Nanoparticles
To improve the interfacial bonding between inorganic fillers and the resin matrix, the nanoparticles were first surface-modified with γ-MPS prior to composite fabrication. The silanization procedure was performed as follows: 0.05 g of γ-MPS, 0.01 g of n-propylamine, 10 mL of cyclohexane, and 0.5 g of CaF2@ZnO or CaF2 nanoparticles were placed into a beaker and thoroughly mixed. The mixture was first stirred at 25 °C for 30 min, followed by continued stirring at 65 °C for another 30 min. Subsequently, the reaction solution was centrifuged three times (10,000 rpm, 5 min). The collected solid was then dried in a vacuum oven at 60 °C for 12 h.
2.3. Preparation of Composite Resin
The resin matrix is the commercial 3 M Z250 resin (3M ESPE Dental Products, St Paul, USA). Its main components are Bis-EMA, UDMA, PEGDMA, TEGDMA, Bis-GMA, zirconia, silica, and silicon particles. The mass proportion of inorganic fillers is 81.8%, and the size of the silicon particles is 20 nm. The size of zirconia and silica particles is 0.1–10 μm. The inorganic fillers are modified CaF2 and CaF2@ZnO nanoparticles. Nanoparticles were added to the resin paste at 5, 10, and 15 wt.% (based on the total final composite mass), manually stirred with a glass rod for 2 min, and then mechanically stirred at 500 rpm for 10 min to obtain the composite resin.
The resin paste was evenly filled into silicone molds of different shapes and sizes for subsequent mechanical property, fluoride ion release property, antibacterial property, and cytotoxicity tests. Then, each side of the resin was irradiated with an LED light curing lamp for 1 min to obtain the light-cured resin. After the resin was demolded, it was polished with 800# sandpaper in the dark for 48 h and stored under light protection for the subsequent tests.
2.4. Material Characterization
The composition and crystal form of CaF2 and CaF2@ZnO powders were detected using an X-ray diffractometer. The device used Cu Kα as the radiation source, with a scanning range of 10–90°, and the scanning speed and step size were 6°/min and 0.02° respectively. The size and particle size distribution of CaF2 and CaF2@ZnO nanoparticles were observed using a transmission electron microscope at an accelerating voltage of 100 kV. The ZnO coating effect and shell thickness of CaF2 and CaF2@ZnO were also observed. The powders were dispersed in ethanol (mass fraction of 0.5 wt.‰), ultrasonically homogenized, and then dropped onto a copper net covered with porous carbon to reduce agglomeration. After the liquid evaporated, the observation was carried out. The nitrogen adsorption–desorption curve was obtained using a surface area and pore size analyzer. The powder samples were analyzed and tested after being degassed at 150 °C for 12 h. Fourier transform infrared spectroscopy was used to test the surface functional groups of the modification agents of CaF2 and CaF2@ZnO nanoparticles before and after modification. The dry nanoparticles were mixed with spectral-grade KBr, ground evenly, and then pressed for testing. The valence states of elements were analyzed using X-ray photoelectron spectroscopy.
The compressive strength of the composite resin was tested using a universal testing machine. Circular samples (φ 4 mm × 6 mm, n = 3) were used for the compressive strength test under a crosshead speed of 0.75 mm/min. The microhardness of the sample under a 50 g load for 10 s was measured using a microhardness tester. Circular samples (φ 6 mm × 4 mm, n = 3) were used and tests were conducted at three points on the samples.
2.5. Test of Fluoride Release Performance of Composite Resin
Fluoride ion release was evaluated from a composite resin incorporated with 10 wt.% CaF2@30ZnO nanoparticles (Here, “30” means that the mass of ZnO is 30% of the mass of CaF2). A resin containing 7.7 wt.% CaF2 nanoparticles served as the experimental control, ensuring both groups had the same initial fluoride content (since the 10 wt.% CaF2@30ZnO composite contained 7.7 wt.% CaF2). Three disk samples (φ 10 mm × 1 mm) per group were immersed in 10 mL of deionized water in polyethylene bottles and maintained at 37 °C. Measurements were taken at specified intervals over 64 days (days 1, 2, 3, 4, 5, 7, 9, 11, 13, 15, 22, 29, 36, 43, 50, 57, and 64). At each measurement, the immersion medium was completely removed and replenished with fresh deionized water. The removed solution was combined with 10 mL of TISAB and assayed with a fluoride ion-selective electrode.
2.6. In Vitro Antibacterial Properties and Cytotoxicity of Composite Resins
A suspension of Staphylococcus aureus (1 × 106 CFU/mL, 100 μL) was inoculated onto a disc-shaped resin (φ 10 mm × 1 mm, containing 10 wt.% CaF2@30ZnO) and cultured at 37 °C for 24 h. The antibacterial performance of the resin was then evaluated.
Before conducting the cell experiments, a hemolysis performance test was first performed on the composite resin to preliminarily evaluate the biocompatibility of the material. A volume of 0.8 mL of fresh pig blood was mixed with 10 mL of physiological saline to prepare a diluted blood solution. A disc-shaped resin (φ 10 mm × 1 mm) containing 10 wt.% CaF2@30ZnO was immersed in 10 mL of physiological saline and incubated at 37 °C in a constant temperature shaker for 30 min. A volume of 0.2 mL of the diluted blood solution was dropped into deionized water (positive control group), physiological saline (negative control group), and the physiological saline of the immersed sample (experimental group), and incubated at 37 °C in a constant temperature shaker for 1 h. Then, the supernatants of each test tube were centrifuged and the absorbance was measured at a wavelength of 545 nm.
L929 mouse fibroblasts were used for initial cytotoxicity screening, as recommended by ISO 10993-5:2009 [34]. L929 cells were seeded at a density of 2000 cells per well in a 96-well plate, and complete medium was added. The cells were cultured in the incubator for 24 h. Then, the same volume of fresh complete medium was replaced as the control group, and the same volume of the extract of 10 wt.% CaF2@30ZnO nanoparticles composite resin was replaced as the experimental group. Disc-shaped specimens (φ 10 mm × 1 mm) were immersed in DMEM at a surface area to volume ratio of 1.25 cm2/mL and incubated at 37 °C for 24 h. These conditions comply with ISO 10993-12:2021 [35]. The cells were cultured for 1, 3, and 5 days respectively. The OD value was measured by CCK-8 to determine the biocompatibility. At different time points (1, 3, and 5 days), the Calcein AM/PI double staining kit (Beyotime, Shanghai, China) was used for live/dead fluorescence imaging.
2.7. Statistical Analysis
One-way ANOVA was carried out using SPSS software (version: 26.0), and Tukey’s honestly significant difference (HSD) test was used for post hoc multiple comparisons. * p ≤ 0.05 was considered statistically significant.
3. Results and Discussion
3.1. Material Characterization
Figure 1a shows the process flow chart for the preparation of CaF2@ZnO nanoparticles. The precursors were prepared by the co-precipitation method and the hydrothermal method. After calcination, the ZnO shell layer formed a porous structure due to the escape of gases, providing channels for the release of F−. Figure 1b shows the TEM image of the single CaF2 sample. The particles are circular or elliptical, with a relatively uniform particle size distribution. The particle size is approximately 15–25 nm, and the surface of the grains is smooth, without any amorphous layers or impurities. This indicates that the CaF2 sample is of high purity and has a complete lattice structure. Figure 1c shows CaF2@30ZnO nanoparticles. The microscopic morphology of the particles has undergone significant changes, and the particle size has significantly increased. At a coating content of 30 wt.% (Figure 1d), the particle size distribution of the prepared CaF2@ZnO nanoparticles is 30 nm to 50 nm. The particle shape is circular, and the CaF2 particles and ZnO are closely adhered, with a clear core–shell interface and a good coating effect. When the precursor concentration is high enough, it can quickly reach the nucleation critical condition on the active sites on the surface of the CaF2 core, triggering dense and uniformly distributed heterogeneous nucleation. After the formation of numerous initial nuclei, the precursor concentration remains sufficient to support their growth but is too low to induce extensive homogeneous nucleation. The nuclei grow in three dimensions and aggregate, eventually forming a continuous and dense shell layer. At a coating concentration of 20 wt.% (Figure S1a), uncoated CaF2 nanoparticles can be observed, indicating that the coating concentration is too low and fails to completely cover the CaF2 nanoparticles. Since the concentration of the precursor directly affects the nucleation rate and growth mode, when ZnO is at a low concentration, the nucleation sites are limited, and the precursor will preferentially expand and grow in two dimensions on the existing nuclei. Therefore, it is difficult to form a continuous and complete shell layer on the surface of CaF2. However, when the precursor concentration is too high, heterogeneous and homogeneous nucleation compete with each other, and the generated ZnO is physically adsorbed onto the existing ZnO-coated CaF2 nuclei or forms nuclei independently, resulting in uneven particle sizes, thick shells, and free ZnO particles at 40 wt.% of ZnO coating (Figure S1b). Figure 1e is a high-resolution transmission electron microscope image of the CaF2@30ZnO nanoparticles with a partially enlarged area. The lattice spacings are 0.315 nm and 0.281 nm, respectively, corresponding to the (111) and (100) crystal planes of the CaF2 cubic crystal and the hexagonal wurtzite crystal of ZnO, and the coating effect is good and uniform. The thickness of the ZnO coating layer is approximately 4 nm. Figure 1f–i are the EDS images of the CaF2@ZnO nanoparticles. It can be seen that the Ca and F elements are mainly in the core layer position, and the Zn element is in the shell layer position. This further confirms that ZnO has successfully covered the surface of CaF2, forming a core–shell structure nanoparticle.
Figure 1.
(a) Process flow mechanism diagram of CaF2 and CaF2@ZnO nanoparticles, (b) TEM image of CaF2 nanoparticles, (c) TEM image of CaF2@ZnO nanoparticles, (d,e) HRTEM images of CaF2@ZnO nanoparticles, (f–i) mapping images of CaF2@ZnO nanoparticles.
The CaF2@ZnO nanoparticles have a larger specific surface area compared to CaF2 nanoparticles, which can increase the contact area with γ-MPS and further enhance the grafting rate. According to the nitrogen adsorption isotherm, the corresponding particle pore size distribution was obtained through BJH. Figure 2a,b show that the micropores formed within the ZnO shell during calcination due to gas evolution provide diffusion channels for fluoride ions and also modulate the fluoride release rate. It is noted from Figure 2b that the type IV isotherm and the pore size range of 2–5 nm indicate the presence of intraparticle micropores, instead of interparticle voids, which are generally larger than 10 nm. This enables the composite resin to achieve long-term and stable fluoride release, which is of great significance for preventing dental caries and inhibiting enamel demineralization. Figure 2c presents the X-ray diffraction (XRD) patterns of the CaF2 and CaF2@ZnO nanoparticles. The characteristic peaks of CaF2@ZnO match well with the cubic lattice structure of CaF2 (PDF#35-0816) and the hexagonal wurtzite structure of ZnO (PDF#80-0075). The diffraction peaks of both CaF2 and ZnO crystals are narrow and sharp, indicating a high degree of crystallinity and purity, with no additional diffraction peaks from other phases observed. This further confirms that the ZnO coating does not alter the crystal structure of CaF2.
Figure 2.
N2 adsorption–desorption isotherms and pore size distributions (insets) of (a) CaF2 nanoparticles and (b) CaF2@ZnO nanoparticles. (c) XRD patterns of CaF2 and CaF2@ZnO.
The interfacial adhesion between inorganic fillers and organic resin matrices is typically weak, resulting in unsatisfactory mechanical properties of composite resins. To address this issue, silane coupling agents are commonly employed to modify the inorganic filler surfaces. Figure 3a presents the Fourier transform infrared (FTIR) spectra of CaF2@ZnO nanoparticles before and after γ-MPS modification. In contrast to the unmodified samples, the γ-MPS-modified CaF2@ZnO nanoparticles exhibit a distinct characteristic stretching vibration peak at 1703 cm−1, corresponding to the C=O bond derived from the carbonyl group of γ-MPS. This observation confirms the successful introduction of γ-MPS onto the nanoparticle surface. X-ray photoelectron spectroscopy (XPS) analysis (Figure 3b–f) further supports this conclusion. Compared with the unmodified nanoparticles (Figure S2), the binding energies of Ca 2p, F 1s, and O 1s core levels show no significant changes. However, the Zn 2p peak shifts toward a higher binding energy by 0.4 eV. This shift can be attributed to the fact that zinc in CaF2@ZnO primarily exists as Zn-O bonds prior to modification. Following the hydrolysis of γ-MPS, the generated Si-OH groups undergo condensation with Zn-OH groups on the particle surface, forming Zn-O-Si covalent bonds. Moreover, the appearance of the Si 2p signal indicates the presence of an organosilane layer, and the characteristic peak at 101.8 eV corresponding to Zn-O-Si bonds provides direct evidence for the covalent attachment of the coupling agent to the particle surface. Taken together with the FTIR results, these data unequivocally demonstrate the successful modification of the CaF2@ZnO nanoparticles.
Figure 3.
(a) FTIR spectra of CaF2@ZnO nanoparticles before and after silane modification. (b–f) XPS spectra of the modified CaF2@ZnO nanoparticles: (b) Ca 2p, (c) F 1s, (d) Zn 2p, (e) O 1s, and (f) Si 2p.
3.2. Mechanical Properties of Composite Resins
Figure 4a,d show the mechanical properties of the composite resins filled with different mass fractions of CaF2@30ZnO nanoparticles. As the filling amount increases from 0 to 10%, the mechanical properties of the composite resins increase, with the compressive strength and hardness increasing by 14.6% and 53.6% respectively. Due to the difference in rigidity between the inorganic fillers and the resin, an appropriate increase in the filling amount promotes the bonding degree between the inorganic fillers and the resin, making the stress distribution between the two more uniform, and further improving the mechanical properties of the composite resin. When the filler content is further increased to 15%, the mechanical properties of the composite resin decrease because the excessive filling amount restricts the movement of the resin and the fillers, causing uneven mixing between the fillers and the resin, slowing down the photopolymerization process, and thus leading to a decrease in the mechanical properties of the composite resin.
Figure 4.
Mechanical properties of composite resins. (a–c) Compressive strength: (a) effect of CaF2@ZnO loading (5–15 wt.%), (b) effect of filler type (CaF2, CaF2@ZnO at 10 wt.%), (c) effect of ZnO coating amount (20–40 wt.%) in CaF2@ZnO. (d–f) Microhardness: (d) effect of CaF2@ZnO loading, (e) effect of filler type, (f) effect of ZnO coating amount. Error bars represent SD (n = 3). * p < 0.05, one-way ANOVA with Tukey’s post hoc test.
Figure 4b,e show the compressive strength and hardness of the composite resins filled with CaF2 nanoparticles and CaF2@30ZnO nanoparticles respectively at the same mass fraction. It can be seen that the composite resin filled with CaF2@ZnO nanoparticles has higher mechanical properties than the composite resin filled with CaF2 nanoparticles, with the compressive strength and hardness increasing by 19.1% and 10.8% respectively. This further confirms that the coating of ZnO is beneficial for CaF2@ZnO nanoparticles to improve the mechanical properties of the composite resin. Figure 4c,f show the effects of ZnO coating amount on the compressive strength and microhardness of the composite resin filled with 10 wt.% CaF2@ZnO nanoparticles. Compared with CaF2 that was not coated with ZnO, CaF2@ZnO nanoparticles, as a dental resin filler, can effectively improve the mechanical properties of the composite resin. When the ZnO coating amount reaches 30%, the mechanical properties of the composite resin are optimal, with a compressive strength of 335.1 ± 14 MPa and a microhardness of 182.3 ± 8.5 HV. When the ZnO coating amount is 20%, ZnO partially fails to coat the CaF2 particles, resulting in a weak bonding interface between the resin matrix and the particles, and the low hardness of CaF2 itself. Excessive release of fluoride ions from CaF2 can cause the filler itself to be damaged, leading to the formation of voids in the filler and a subsequent decrease in resin performance. When the ZnO coating amount is 40%, the overly thick ZnO coating layer becomes brittle due to internal stress, and microcracks occur in the inorganic filler and resin during mixing or curing. An overly thick ZnO coating layer results in enlarged filler particles, whose poor dispersion in the resin matrix leads to a decline in mechanical performance.
3.3. The Fluoride Release Performance of Composite Resin
Figure 5 presents the fluoride ion release rate and cumulative release profiles for the composite resins filled with 7.7 wt.% CaF2 nanoparticles and 10 wt.% CaF2@ZnO nanoparticles, respectively. As shown in Figure 5a, the CaF2 composite exhibited a relatively high initial release rate (within 0–200 h), approaching 1 μg/(h·cm2), which indicates a rapid dissolution of fluoride ions from the nanoparticles at early stages. In contrast, the CaF2@ZnO composite displayed a lower release rate of approximately 0.8 μg/(h·cm2) during the same period. After 200 h, the release rate of the CaF2 composite stabilized around 0.2 μg/(h·cm2), while that of the CaF2@ZnO composite also reached a steady state but at a consistently lower value of about 0.15 μg/(h·cm2). These results demonstrate that the CaF2@ZnO composite maintains a sustained, slower fluoride release over the long term compared to the CaF2 composite.
Figure 5.
Fluoride release profiles of CaF2 and CaF2@ZnO composite resins (10 wt.% filler) over 64 days. (a) Fluoride release rate (μg/(h·cm2)). (b) Cumulative fluoride release (μg/cm2).
In Figure 5b, the cumulative fluoride release of both materials increased continuously with immersion time. At any given time point, the cumulative release from the CaF2 composite was higher than that of the CaF2@ZnO composite. After 1500 h, the cumulative release reached nearly 450 μg/cm2 for the CaF2 composite, compared to approximately 310 µg/cm2 for the CaF2@ZnO composite.
It can be inferred that the ZnO coating formed on the CaF2 particles acts as a barrier that impedes the outward diffusion of fluoride ions, thereby modulating the release kinetics. Meanwhile, the micropores within the ZnO shell provide sustained release channels, allowing fluoride ions to diffuse slowly over an extended period. This indicates that the ZnO coating effectively regulates fluoride ion release and enables long-term sustained release, contributing to a prolonged and stable fluoride release profile that may help extend the functional lifetime of dental restorative resins. The absolute fluoride release level can be further adjusted by increasing the CaF2@ZnO filler loading without compromising mechanical properties, which will be investigated in our future studies.
3.4. The Antibacterial Properties of Composite Resin
Figure 6b shows the antibacterial effect of the composite resin filled with 10 wt.% CaF2. Compared with Figure 6a, the number of colonies is reduced and their distribution is sparser, indicating that CaF2 nanoparticles have certain antibacterial ability and can effectively inhibit the expansion of bacteria. As shown in Figure 6c, the number of colonies in the culture dish was significantly reduced after 24 h of culture, indicating that the CaF2@ZnO composite resin exhibited superior antibacterial activity under the tested conditions compared to the composite resin filled with bare CaF2 nanoparticles. Figure 6d presents the quantitative analysis results, clearly demonstrating the antibacterial efficacy of the materials. The bacterial count in the control group was 6.1 × 106 CFU. After treatment with the CaF2 composite resin, the bacterial count decreased to 8 × 104 CFU. Following treatment with the CaF2@ZnO composite resin, the bacterial count further dropped to 9 × 103 CFU. These results confirm the synergistic enhancement of antibacterial performance conferred by the CaF2@ZnO nanoparticles. Figure 6e shows the antibacterial mechanism of the composite resin. When the size of inorganic fillers is reduced to the nanoscale, ZnO has excellent antibacterial activity [36]. The interaction between the nanoscale CaF2@ZnO core–shell particles and microorganisms enhances their antibacterial performance [37]. The ZnO shell and CaF2 core release Zn2+ and F−, respectively, which inhibit bacterial growth through different pathways. A possible explanation for this antibacterial effect is that CaF2 slowly releases F− and H+ to form HF molecules, inhibiting the glycolytic enzyme activity of cariogenic bacteria, reducing the production of lactic acid by bacteria, and improving the acidic environment that causes dental caries [38]. ZnO and the Zn2+ released from it can generate reactive oxygen species (ROS) such as H2O2 [39], which penetrate the cell membrane and damage cellular structures such as lipids and proteins [40], thereby inhibiting bacterial growth. However, it should be noted that ROS generation by ZnO is predominantly a photocatalytic process that requires light excitation. Considering that dental restorations function in an environment with very limited light exposure in vivo, the clinical relevance of ROS generation remains uncertain. ZnO inhibits bacterial growth by destroying bacterial structure, while CaF2 inhibits acid production. The synergistic effect of the two can significantly inhibit bacterial growth, providing a theoretical basis for long-term caries resistance and extending the service life of the resin.
Figure 6.
Antibacterial activity of composite resins against S. aureus after 24 h. (a) Blank control. (b) Composite resin filled with 10 wt.% CaF2. (c) Composite resin filled with 10 wt.% CaF2@30ZnO. (d) Statistical chart of bacterial quantities in each group. * p < 0.05, one-way ANOVA with Tukey’s post hoc test. (e) Antibacterial mechanism diagram of CaF2@ZnO.
A limitation of this study is that the antibacterial evaluation was performed only against S. aureus, rather than the primary cariogenic bacterium S. mutans. Future studies will employ clinically relevant cariogenic bacteria and multispecies biofilm models to fully assess the anti-caries potential of the CaF2@ZnO composite resin.
3.5. The Cytotoxicity of Composite Resins
The hemolytic properties of the composite resin were tested. According to Figure 7a, the OD value of the experimental group was 0.056, the hemolysis rate was calculated to be 2.5%, which is lower than 5% and can be applied in the biomedical field. The extract of the resin samples was co-cultured with fibroblasts for 1, 3, and 5 days. The results are shown in Figure 7b. The results indicated that there was no significant difference between the experimental group and the control group. The OD values on the 1st, 3rd, and 5th days were approximately 0.5, 1.3, and 1.6, respectively. After 3 days of culture, the viable cells in each group remained at a relatively high level.
Figure 7.
Cytocompatibility of the 10 wt.% CaF2@30ZnO composite resin. (a) OD value after diluting pig blood with 10 wt.% CaF2@30ZnO resin and incubating at 37 °C for 1 h. (b) OD value of fibroblasts co-cultured with the extract solution of 10 wt.% CaF2@30ZnO and CaF2 resin for 1, 3, and 5 days. * p < 0.05, one-way ANOVA with Tukey’s post hoc test.
According to the results of the live/dead staining in Figure 8, on the first day, the cells in the experimental group and the control group were spindle-shaped or polygonal, with moderate cell volume and appropriate cell spacing. The cell number increased with the days. On the third and fifth days, the cells grew rapidly, and the cell morphology did not change significantly. The cells were closely arranged and all were live cells (green), with no dead cells (red). The fibroblasts had good cell viability. These results indicate that, under the tested conditions, the extract of the 10 wt.% CaF2@30ZnO composite resin showed no detectable cytotoxicity and provided a suitable environment for cell growth and proliferation. This finding offers preliminary support for the potential application of this composite resin in dental medicine.
Figure 8.
Fluorescence images of fibroblasts co-cultured with 10 wt.% CaF2 (a–c) and CaF2@30ZnO (d–f) resin extract for 1, 3, and 5 days.
4. Conclusions
In this study, CaF2@ZnO core–shell nanoparticles were successfully prepared and applied as multifunctional active fillers in dental resin composites. Our design integrates fluoride release and antibacterial functions into a single CaF2@ZnO core–shell particle. The ZnO shell not only acts as a barrier to regulate sustained fluoride release from the CaF2 core but also serves as a Zn2+ source to provide light-independent antibacterial activity. Thus, our CaF2@ZnO design uniquely combines fluoride release and antibacterial activity within the same particle. The resulting nanocomposite resin achieved sustained fluoride release for over 64 days, excellent antibacterial activity against Staphylococcus aureus, and enhanced mechanical properties. The ZnO shell effectively regulated fluoride release, avoiding the burst release and associated deterioration of mechanical properties commonly observed with bare CaF2 nanoparticles, thereby demonstrating the advantages of the core–shell architecture. This study provides new insights and an experimental foundation for the development of dental restorative materials that integrate antibacterial and strengthening functions.
Supplementary Materials
The following supporting information can be downloaded at: https://www.mdpi.com/article/10.3390/coatings16060650/s1, Figure S1: TEM images (a) CaF2@20ZnO and (b) CaF2@40ZnO; Figure S2: XPS spectrum before modification with CaF2@ZnO nanoparticles: (a) Ca 2p, (b) F 1s, (c) Zn 2p, and (d) O 1s.
Author Contributions
Conceptualization, N.L. and C.L.; methodology, T.Y.; software, T.Y.; validation, N.L., H.W., and C.L.; formal analysis, Y.J.; investigation, T.Y.; data curation, T.Y.; writing—original draft preparation, T.Y.; writing—review and editing, N.L. All authors have read and agreed to the published version of the manuscript.
Funding
This research was funded by Natural Science Foundation of Hebei Province, grant number E2024202191.
Institutional Review Board Statement
Not applicable.
Informed Consent Statement
Not applicable.
Data Availability Statement
The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding authors.
Conflicts of Interest
The authors declare no conflicts of interest.
References
- Mei, P.; Tao, X.Y.; Ding, Z.D.; Li, R.M.; Zhu, Z.Y.; Liu, C.X.; Wang, R.Q.; Xia, L.G.; Huan, Z.G.; Fang, B. Multifunctional Lithium-Calcium-Silicon Bioceramic Resin Composite for Enhanced Dental Remineralization and Reparative Dentin Formation. Adv. Healthc. Mater. 2025, 14, 17. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Yang, Y.; Huang, J.; Hu, X.; Jing, M.; Zhang, Y.; Xu, C.; Tan, W.; Liu, X.; Niu, C.; Huang, Z. Surface prereacted glass-ionomer particles incorporated into resin composites promote biocompatibility for restoration of subgingival dental defects. Mater. Today Bio 2025, 31, 101499. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Gouveia, Z.; Finer, Y.; Santerre, J.P. Development of Functional and Hydrolytically Stable Vinyl Monomers as Methacrylate Dental Resin Restorative Alternatives. Adv. Healthc. Mater. 2025, 14, 11. [Google Scholar] [CrossRef] [Scilit]
- Musanje, L.; Ferracane, J.L. Effects of resin formulation and nanofiller surface treatment on the properties of experimental hybrid resin composite. Biomaterials 2004, 25, 4065–4071. [Google Scholar] [CrossRef] [Scilit]
- Duraccio, D.; Mussano, F.; Faga, M.G. Biomaterials for dental implants: Current and future trends. J. Mater. Sci. 2015, 50, 4779–4812. [Google Scholar] [CrossRef] [Scilit]
- Askar, H.; Krois, J.; Göstemeyer, G.; Bottenberg, P.; Zero, D.; Banerjee, A.; Schwendicke, F. Secondary caries: What is it, and how it can be controlled, detected, and managed? Clin. Oral Investig. 2020, 24, 1869–1876. [Google Scholar] [CrossRef] [Scilit]
- Ferracane, J.L. Resin composite—State of the art. Dent. Mater. 2011, 27, 29–38. [Google Scholar] [CrossRef] [Scilit]
- Sodagar, A.; Bahador, A.; Khalil, S.; Shahroudi, A.S.; Kassaee, M.Z. The effect of TiO2 and SiO2 nanoparticles on flexural strength of poly (methyl methacrylate) acrylic resins. J. Prosthodont. Res. 2013, 57, 15–19. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Zhao, S.N.; Yang, D.L.; Wang, D.; Pu, Y.; Le, Y.; Wang, J.X.; Chen, J.F. Design and efficient fabrication of micro-sized clusters of hydroxyapatite nanorods for dental resin composites. J. Mater. Sci. 2019, 54, 3878–3892. [Google Scholar] [CrossRef] [Scilit]
- Anusavice, K.J.; Zhang, N.Z.; Shen, C. Effect of CaF2 content on rate of fluoride release from filled resins. J. Dent. Res. 2005, 84, 440–444. [Google Scholar] [CrossRef] [Scilit]
- Kolb, C.; Gumpert, K.; Wolter, H.; Sextl, G. Highly translucent dental resin composites through refractive index adaption using zirconium dioxide nanoparticles and organic functionalization. Dent. Mater. 2020, 36, 1332–1342. [Google Scholar] [CrossRef] [Scilit]
- Zhang, L.L.; Ding, Y.L.; Povey, M.; York, D. ZnO nanofluids—A potential antibacterial agent. Prog. Nat. Sci. 2008, 18, 939–944. [Google Scholar] [CrossRef] [Scilit]
- Yang, D.L.; Cui, Y.N.; Sun, Q.; Liu, M.; Niu, H.; Wang, J.X. Antibacterial activity and reinforcing effect of SiO2-ZnO complex cluster fillers for dental resin composites. Biomater. Sci. 2021, 9, 1795–1804. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Dong, Z.H.; Yang, Q.; Mei, M.Y.; Liu, L.; Sun, J.X.; Zhao, L.; Zhou, C.C. Preparation and characterization of fluoride calcium silicate composites with multi-biofunction for clinical application in dentistry. Compos. Part B-Eng. 2018, 143, 243–249. [Google Scholar] [CrossRef] [Scilit]
- Zhou, S.L.; Zhou, J.; Watanabe, S.; Watanabe, K.; Wen, L.Y.; Xuan, K. In vitro study of the effects of fluoride-releasing dental materials on remineralization in an enamel erosion model. J. Dent. 2012, 40, 255–263. [Google Scholar] [CrossRef] [Scilit]
- Safronikhin, A.; Ehrlich, H.; Lisichkin, G. Double-jet precipitation synthesis of CaF2 nanoparticles: The effect of temperature, solvent, and stabilizer on size and morphology. J. Alloys Compd. 2017, 694, 1182–1188. [Google Scholar] [CrossRef] [Scilit]
- Xu, H.H.K.; Moreau, J.L.; Sun, L.M.; Chow, L.C. Chow, Strength and fluoride release characteristics of a calcium fluoride based dental nanocomposite. Biomaterials 2008, 29, 4261–4267. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Kielbassa, A.M.; Schulte-Monting, J.; Garcia-Godoy, F.; Meyer-Lueckel, H. Initial in situ secondary caries formation: Effect of various fluoride-containing restorative materials. Oper. Dent. 2003, 28, 765. [Google Scholar] [CrossRef] [Scilit]
- Roin-Grget, K.; Pero, K.; Sutej, I.; Bai, K. The cariostatic mechanisms of fluoride. Acta Med. Acad. 2013, 42, 179–188. [Google Scholar] [CrossRef] [Scilit]
- Yi, J.R.; Weir, M.D.; Melo, M.A.S.; Li, T.; Lynch, C.D.; Oates, T.W.; Dai, Q.; Zhao, Z.H.; Xu, H.H.K. Novel rechargeable nano-CaF2 orthodontic cement with high levels of long-term fluoride release. J. Dent. 2019, 90, 8. [Google Scholar] [CrossRef] [Scilit]
- Zheng, X.; Cheng, X.; Wang, L.; Qiu, W.; Wang, S.; Zhou, Y.; Li, M.; Li, Y.; Cheng, L.; Li, J.; et al. Combinatorial Effects of Arginine and Fluoride on Oral Bacteria. J. Dent. Res. 2015, 94, 344–353. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Koo, H. Strategies to Enhance the Biological Effects of Fluoride on Dental Biofilms. Adv. Dent. Res. 2008, 20, 17–21. [Google Scholar] [CrossRef] [Scilit]
- Chow, L.C.; Takagi, S.; Carey, C.M.; Sieck, B.A. Remineralization Effects of a Two-solution Fluoride Mouthrinse: An in situ Study. J. Dent. Res. 2000, 79, 991–995. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Chow, L.C.; Takagi, S.; Frukhtbeyn, S.; Sieck, B.A.; Parry, E.E.; Liao, N.S.; Schumacher, G.E.; Markovic, M. Remineralization effect of a low-concentration fluoride rinse in an intraoral model. Caries Res. 2002, 36, 136–141. [Google Scholar] [CrossRef] [Scilit]
- Dai, Q.; Weir, M.D.; Ruan, J.P.; Liu, J.; Gao, J.H.; Lynch, C.D.; Oates, T.W.; Li, Y.C.; Chang, X.F.; Xu, H.H.K. Effect of co-precipitation plus spray-drying of nano-CaF2 on mechanical and fluoride properties of nanocomposite. Dent. Mater. 2021, 37, 1009–1019. [Google Scholar] [CrossRef] [Scilit]
- Buchalla, W.; Attin, T.; Schulte-Mönting, J.; Hellwig, E. Fluoride uptake, retention, and remineralization efficacy of a highly concentrated fluoride solution on enamel lesions in situ. J. Dent. Res. 2002, 81, 329–333. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Choi, J.W.; Yang, S.Y. Effect of Zinc Oxide Incorporation on the Antibacterial, Physicochemical, and Mechanical Properties of Pit and Fissure Sealants. Polymers 2023, 15, 14. [Google Scholar] [CrossRef] [Scilit]
- Le, Y.; Hou, P.T.; Wang, J.X.; Chen, J.F. Controlled release active antimicrobial corrosion coatings with Ag/SiO2 core-shell nanoparticles. Mater. Chem. Phys. 2010, 120, 351–355. [Google Scholar] [CrossRef] [Scilit]
- Melo, M.A.S.; Garcia, I.M.; Mokeem, L.; Weir, M.D.; Xu, H.; Montoya, C.; Orrego, S. Developing Bioactive Dental Resins for Restorative Dentistry. J. Dent. Res. 2023, 102, 1180–1190. [Google Scholar] [CrossRef] [Scilit]
- Padovani, G.C.; Feitosa, V.P.; Sauro, S.; Tay, F.R.; Durán, G.; Paula, A.J.; Durán, N. Advances in Dental Materials through Nanotechnology: Facts, Perspectives anc Toxicological Aspects. Trends Biotechnol. 2015, 33, 621–636. [Google Scholar] [CrossRef] [Scilit]
- Ravi, P.; Reddy, M.C.; Chandrasekhar, T.; Chinni, S.V.; Adam, H.; Gopinath, S.C.B.; Lebaka, V.R. Biogenic Nano Zinc Oxide Particle Production and Their Antimicrobial Potentials: A Review. J. Clust. Sci. 2025, 36, 36. [Google Scholar] [CrossRef] [Scilit]
- Al-Eisa, A.; Al-Mosawi, M.; D’Souza, R.G.T.M.; Sharma, P.N. Attitudes of General Practitioners and Pediatricians to Management of Acute Pyelonephritis in Children. Med. Princ. Pract. 2000, 9, 119–124. [Google Scholar] [CrossRef] [Scilit]
- Al-hijazi, A.Y.; Hasan, N.; Nasr, B.K.; Al-Khafaji, H.H.J.; Al-Khafaji, B.; Alanssari, B.F.A.; Jalil, A.T. Recent advances in the use of inorganic nanomaterials as anti caries agents. Heliyon 2023, 9, 16. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- ISO 10993-5:2009; Biological Evaluation of Medical Devices—Part 5: Tests for In Vitro Cytotoxicity. ISO: Geneva, Switzerland, 2009.
- ISO 10993-12:2021; Biological Evaluation of Medical Devices—Part 12: Sample Preparation and Reference Materials. ISO: Geneva, Switzerland, 2021.
- Seil, J.T.; Webster, T.J. Antimicrobial applications of nanotechnology: Methods and literature. Int. J. Nanomed. 2012, 7, 2767–2781. [Google Scholar] [CrossRef] [Scilit]
- Xu, H.H.K.; Moreau, J.L.; Sun, L.; Chow, L.C. Novel CaF2 Nanocomposite with High Strength and Fluoride Ion Release. J. Dent. Res. 2010, 89, 739–745. [Google Scholar] [CrossRef] [Scilit]
- Eshed, M.; Lellouche, J.; Banin, E.; Gedanken, A. MgF2 nanoparticle-coated teeth inhibit Streptococcus mutans biofilm formation on a tooth model. J. Mater. Chem. B 2013, 1, 3985–3991. [Google Scholar] [CrossRef] [Scilit]
- Sunada, K.; Watanabe, T.; Hashimoto, K. Bactericidal Activity of Copper-Deposited TiO2 Thin Film under Weak UV Light Illumination. Environ. Sci. Technol. 2003, 37, 4785–4789. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Huang, Z.B.; Zheng, X.; Yan, D.H.; Yin, G.F.; Liao, X.M.; Kang, Y.Q.; Yao, Y.D.; Huang, D.; Hao, B.Q. Toxicological effect of ZnO nanoparticles based on bacteria. Langmuir 2008, 24, 4140–4144. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.