Method for Obtaining Strength and Dynamic Modulus of Existing Asphalt Pavement Materials Based on Size Effect

,
,
,
,
,
,
,
and
1
Shandong Key Laboratory of Highway Technology and Safety Assessment, Jinan 250098, China
2
Shandong Hi-Speed Group Co.LTD Innovation Research Institute, Jinan 250098, China
3
National Engineering Research Center of Highway Maintenance Technology, Changsha University of Science & Technology, Changsha 410114, China
4
National Key Laboratory of Green and Long-Life Road Engineering in Extreme Environment (Changsha), Changsha University of Science & Technology, Changsha 410114, China

Highlights

  • The size effect of strength and dynamic modulus is revealed.
  • The mapping relationships between uniaxial compression and indirect tensile test results are established.
  • A method for obtaining existing asphalt pavement materials’ strength and dynamic modulus parameters is proposed.

Abstract

Extending the service life of in-service asphalt pavement is an essential subject for the sustainable development of roadway engineering. In order to address the issue of difficulty in obtaining design parameters for the asphalt layer of in-service pavements, this research, based on the structural size effect, investigates the effects of various thicknesses (30 mm, 40 mm, 70 mm, 100 mm, 130 mm, and 150 mm) and various gradations (Asphalt Concrete-13 mm (AC-13), Stone Mastic Asphalt-13 mm (SMA-13)) on uniaxial compressive strength (UCS) and dynamic modulus (UCM), as well as indirect tensile strength (ITS) and dynamic modulus (ITM). Furthermore, mapping relationships between strength, dynamic modulus, and thickness are established. Finally, a method is proposed for obtaining in-service pavement asphalt layers’ strength and dynamic modulus based on the size effect. The results indicate that UCS and UCM decrease, and ITS and ITM increase, with the thickness of AC-13 and SMA-13 increasing. The strength and modulus conversion coefficients show good regularity with thickness variation. The Weibull size effect law can match the uniaxial compression test data well. The size effect law related to the area can fit well with indirect tensile test data. The significance of this study is that it provides a laboratory-calibrated conversion framework for obtaining strength and dynamic modulus parameters from small-thickness asphalt specimens, which may support the mechanical evaluation and life extension design of in-service asphalt pavements after further field validation.

1. Introduction

In the context of climate change and increasing pressure on natural resources, the sustainable management of existing infrastructure has become increasingly important, and extending the service life of asphalt pavements is now an important strategy for sustainable road infrastructure [1]. Compared with full reconstruction, life extension maintenance can reduce material consumption, construction disturbance, and waste generation. However, the effectiveness of life extension design depends on the accurate characterization of the mechanical properties of in-service asphalt layers. If the strength and modulus parameters of existing pavement materials cannot be reliably obtained, maintenance decisions may be either overly conservative or insufficient, resulting in unnecessary resource consumption or premature structural failure. Recent studies on sustainable pavement management have also shown that life extension maintenance and material reuse can reduce the environmental burden of road infrastructure compared with full-depth reconstruction [2,3,4,5,6].
This issue is particularly relevant in countries with large-scale highway networks that have entered the maintenance stage. Taking China as an example, 60% of the built expressway asphalt pavements have reached or are close to the designed service life. Asphalt pavements have been in service for numerous years under the influence of vehicles and the natural environment, resulting in frequent pavement distresses [7]. Moreover, with the increasing traffic volume in recent years and the demand for reconstruction and extension, it is necessary to conduct maintenance and repairs to enhance transportation infrastructure’s safety, reliability, and sustainability [8]. One of the critical issues in extending the lifespan of existing asphalt pavements is accurately obtaining the strength and dynamic modulus parameters [9,10] of each structural layer. These data are essential for establishing a reliable life extension design model and formulating reasonable maintenance plans. If these data cannot be accurately determined, the life extension design and maintenance plan will fail to be scientifically set based on the actual situation of the existing pavements, leading to inefficient use of maintenance resources.
There are two main methods for obtaining strength and dynamic modulus parameters of in-service asphalt pavement structural layers: indirect and direct. Indirect measurement is mainly achieved using high-precision, non-destructive testing equipment to obtain structural parameters of in-service asphalt pavements [11]. It can qualitatively and quantitatively evaluate the remaining life of in-service pavement structures based on structural integrity and modulus attenuation [12]. For example, some scholars used ground-penetrating radar to detect internal defects in road structures and evaluate their structural integrity [13]. Some scholars used the Falling Weight Deflectometer (FWD) to detect pavement deflection basin data and calculate the modulus of the existing pavement structural layers in reverse [14,15]. Some researchers indirectly judged the degree of structural layer modulus attenuation by detecting the rebound deflection value of the pavements using an Automatic Deflectometer or Beckman beam deflection instrument [16]. The indirect measurement method can only obtain the modulus of the asphalt layer, the subgrade, and the soil base. However, the reverse calculation cannot further determine the modulus of each stratum of an asphalt layer [17]. Direct measurement refers to measuring by drilling core samples into actual road surfaces. Studies have shown that core sampling from actual pavements is the most effective method for evaluating the mechanical properties of existing asphalt pavements and for checking the compliance of the modulus and strength of the structural layers of the pavements [18]. Moreover, it can compensate for the shortcomings of indirect measurement methods and obtain the parameters of each stratum of the asphalt layers. Nevertheless, the thickness of most asphalt pavement surface layers is typically determined based on the principle of 2.5 to 3 times the maximum particle size. According to the Standard Test Methods of Bitumen and Bituminous Mixtures for Highway Engineering (JTG E20-2011) [19] in China, currently, the core sampling thickness of a typical asphalt surface layer falls far below the height of 100 mm required for uniaxial compression strength (UCS) testing and the height of 150 mm for uniaxial compression dynamic modulus (UCM) testing. This fact makes it difficult to directly use the uniaxial compression test method to determine the modulus and strength of the asphalt mixture in actual pavement structures. Smaller sample sizes (38 mm in diameter and 110 mm in thickness) are beginning to be used in the United States. This method facilitates testing the modulus and strength parameters of in-service asphalt pavements. However, it only applies to asphalt layer thicknesses exceeding 50 mm. It does not apply to pavement structures with asphalt layer thicknesses below 50 mm, like the semi-rigid base asphalt pavements prevalent in China. Therefore, it is necessary to further explore a method for testing the modulus and strength of in-service asphalt pavements that applies to any thickness to help test the structural layers of thinner asphalt pavements. Recent studies have also shown that the dynamic modulus is a key input for pavement structural evaluation, remaining-life prediction, and overlay design. However, the modulus of asphalt layers in service is affected by material aging, field compaction, traffic loading, and temperature history. Therefore, reliable testing and conversion methods for field cores, especially small-thickness cores, are still needed [20,21,22].
Studying the correlation between the UCS and UCM of small-thickness samples and the UCS and UCM of standard samples [23,24] provides new ideas for solving this problem. The size effect refers to the mechanical properties of materials that no longer remain constant but vary with changes in geometric sizes of the structure and materials [25]. Specifically, the size effect is manifested as follows: with an increase in sample size, there is a corresponding increase in its fracture energy and a decrease in strength. Conversely, as the sample size decreases, its fracture energy decreases, and strength increases accordingly. In recent years, numerous scholars have studied the size effect phenomena of brittle materials such as rock [26] and concrete [27,28,29,30] from experimental [31,32], theoretical [33], and numerical simulations [34] and have achieved rich results. However, the effect of sample size on the mechanical properties of asphalt mixtures is rarely reported [35,36,37,38]. Wagoner et al. [39] investigated the effect of sample size on the fracture energy of asphalt mixtures. The research found that samples with smaller thicknesses exhibit higher crack resistance, while samples with larger sizes exhibit lower crack resistance. In addition, the influence of size effect on the fracture energy of asphalt mixtures was analyzed, and the correlation between sample size and fracture energy was revealed. The results of the study are important for the parametric design of asphalt mixtures. Li et al. [40] investigated the feasibility of using small-sized samples in dynamic modulus and fatigue testing in an asphalt mixture performance tester (AMPT). The research shows that small-sized samples can effectively perform testing in AMPT and provide dynamic modulus and fatigue data similar to standard-size samples. In conclusion, research progress in the United States indicates that the use of small-sized samples in AMPT testing is feasible. This method is gradually being recognized and widely applied, potentially becoming an important method for evaluating and designing the performance of asphalt mixtures in the future.
In addition, the standard sample size specified in the indirect tensile test has the advantage of being small in size, which can overcome the problem of the core sample of the in-service asphalt pavement surface layer failing to meet the indoor standard sample size height. This fact provides another new approach for in-service asphalt pavement modulus and strength testing. Numerous research results have shown significant differences and correlations between the UCS and indirect tensile strength (ITS), as well as the UCM and indirect tensile dynamic modulus (ITM) of the asphalt mixture [41,42,43,44,45,46]. Ebrahimi, Saleh, and Gonzalez [47] conducted uniaxial compression and indirect tensile tests on two common asphalt mixture types at three different volumes of air voids. After comparing the results of uniaxial compression and indirect tensile test methods, researchers found that the dynamic modulus determined by the indirect tensile and the uniaxial compression tests had a high degree of agreement. Qin, Ma, and Wang [48] conducted a comparative study on two test methods: indirect tensile and uniaxial compression. Scholars found significant differences in the asphalt mixture’s dynamic modulus, phase angle, and shift factors measured using the two test modes. The correlation in the fitting formula indicates a significant relationship between UCM and ITM. Lv et al. [49] compared the correlation and distinction between the moduli garnered through four testing methods. Researchers found that the modulus derived from the indirect tensile test bears a closer resemblance to the modulus of road materials under actual stress conditions. Recent studies have further confirmed the importance of comparing indirect tensile and uniaxial compression testing modes for asphalt mixtures. Chen et al. compared these two test methods and analyzed their influence on the dynamic modulus and stress–strain state of AC and SMA mixtures. Their results indicate that the measured dynamic modulus is affected by the loading mode and the corresponding stress distribution. This provides an important reference for establishing conversion relationships between UCM and ITM in the present study [45,50]. Therefore, existing studies have extensively investigated the correlation between the UCM and ITM of the asphalt mixture. However, few studies have focused on mapping relationships between uniaxial compression and indirect tensile test results, including strength and dynamic modulus with different thickness sizes [51]. The purpose of this study is to address the problem of the core sampling of the existing asphalt pavement surface layers not being able to reach the indoor standard sample size height. Therefore, it is necessary to investigate this in depth.
For example, as stipulated in China’s JTG E20-2011, the test for measuring the strength and dynamic modulus of the asphalt mixture mandates a uniaxial compression test [52]. Furthermore, small-thickness uniaxial compression samples can be obtained from existing pavements. Consequently, this study utilized the uniaxial compression test [53,54,55,56] to probe the size effect variation laws of UCS and UCM. Considering that the indirect tensile test is a biaxial stress state [57,58], the stress state at the center point of the indirect tensile test sample is very similar to the stress state at the bottom of the asphalt layer [59,60]. Under vertical compression, tension occurs in longitudinal and transverse directions [61]. Moreover, samples of the indirect tensile standard-size asphalt specified in JTG E20-2011 in China can be obtained by drilling cores from the existing asphalt pavements with a thickness of 40 mm and a diameter of 100 mm or 150 mm. Therefore, this study selected the indirect tensile test for the size effect variation laws of ITS and ITM.
In summary, the United States is actively studying the feasibility of using small samples instead of standard samples. However, the currently proposed method is not yet applicable to semi-rigid base pavements with thin thicknesses. This study aims to extend the service life of in-service asphalt pavements, solve the problem of difficulty in obtaining design parameters of asphalt layers on in-service pavement, and explore a more applicable method for obtaining design parameters of asphalt layers on in-service pavement.

2. Objectives

The objectives of this study are to:
  • Investigate the effects of different thicknesses (30 mm, 40 mm, 70 mm, 100 mm, 130 mm, and 150 mm) and gradation (Asphalt Concrete-13 mm (AC-13), Stone Mastic Asphalt-13 mm (SMA-13)) on UCS, ITS, UCM, and ITM based on the structural size effect, and establish a mapping relationship between strength, dynamic modulus, and sample thickness.
  • Develop a laboratory-calibrated conversion framework for obtaining strength and dynamic modulus parameters from small-thickness asphalt specimens, which may support the evaluation of thin asphalt layers in in-service pavements. The technical framework diagram is shown in Figure 1.
    Figure 1. Technical framework diagram.

3. Mix Design and Experiment Approach

3.1. Mix Design

This section describes the mix-design procedure for the AC-13 and SMA-13 asphalt mixtures used in this study. First, the basic properties of the asphalt binder, aggregate, and mineral filler were tested to verify whether the raw materials satisfied the specification requirements. Then, the gradation designs of AC-13 and SMA-13 were determined according to the target gradation ranges. Finally, the Marshall mix-design method was used to determine the optimum asphalt–aggregate ratios of the two mixtures. The properties of the raw materials are listed in Table 1, Table 2 and Table 3, the gradation curves are shown in Figure 2, and the Marshall test results are summarized in Table 4 and Figure 3.
Table 1. Test results of asphalt.
Table 2. Technical indexes of aggregate.
Table 3. Technical indexes of filler.
Figure 2. Gradation curves.
Table 4. Marshall test results.
Figure 3. Analysis of the Marshall test results.

3.1.1. Materials

Road petroleum asphalt has high elasticity and durability. Basalt has excellent wearability, strong compression strength, and good adhesiveness. Limestone filler can increase the surface area of aggregates, thereby enhancing the bonding properties of the asphalt mixture. Therefore, these materials are widely used in asphalt pavement construction in China. To better match the existing asphalt pavement material standards, this study utilized No. 90 Grade A road petroleum asphalt (PG 58-22), basalt aggregate, and limestone filler to prepare samples for UCS, UCM, ITS, and ITM tests. No. 90 Grade A road petroleum asphalt was provided by China Panjin Dali Special Asphalt Co., Ltd. The aggregates and filler come from Zhongshan City, Guangdong Province, China. Test parameter results for No. 90 Grade A road petroleum asphalt are shown in Table 1. The results of basalt aggregate test indexes are shown in Table 2, and the fundamental test parameters for limestone filler are shown in Table 3. These test results confirm that all parameters for No. 90 Grade A road petroleum asphalt, basalt aggregates, and limestone filler complied with the technical requirements of the Technical Specification for Construction of Highway Asphalt Pavements (JTG F40-2004) [64] in China.

3.1.2. Gradation Design

Continuous and intermittent gradation asphalt mixtures are commonly used for asphalt pavements in China. The suspended-dense structure asphalt mixture has the advantages of high density, good water stability, excellent low-temperature crack resistance, good durability, is less prone to coarse and fine aggregate segregation, and is convenient for construction. The skeleton-dense structure of the asphalt mixture has the advantages of good skid resistance, strong deformation resistance, and noise reduction. They have been widely used in asphalt pavement construction. This study adopted the AC-13 and SMA-13 asphalt mixtures as the research objects to better match the existing pavement structure requirements. According to the JTG F40-2004 [64] in China, the grading designs of the mineral materials required in the asphalt mixture test were carried out, and the gradation curves are shown in Figure 2. The composite gradation curves were used for asphalt mixture manufacturing.

3.1.3. Optimum Asphalt–Aggregate Ratio

This research used the Marshall test according to JTG F40-2004 in China to obtain the optimal asphalt–aggregate ratios for AC-13 and SMA-13 gradation curves. Five asphalt–aggregate ratios, namely 4.0%, 4.5%, 5.0%, 5.5%, and 6.0%, were selected for preparing Marshall specimens. For each asphalt–aggregate ratio, the bulk specific gravity, air voids, voids in mineral aggregate, voids filled with asphalt, Marshall stability, and flow value were measured. These indexes were used to evaluate the volumetric characteristics, strength stability, and deformation performance of the asphalt mixture. Taking AC-13 as an example, the results of the Marshall test under different asphalt–aggregate ratios are shown in Table 4. The analysis of the Marshall test results is shown in Figure 3. According to Figure 3, a1 = 5.69%, a2 = 5.0%, a3 = 4.66%, a4 = 4.39%, OACmin = 4.24%, and OACmax = 4.71%. The optimum asphalt–aggregate ratio for AC-13 was calculated using Equation (1) and determined to be 4.71%. The same method was used to determine the optimum asphalt–aggregate ratio for SMA-13 as 5.2%.
O A C 1 = a 1 + a 2 + a 3 + a 4 4 = 5.69 % + 5 . 0 % + 4 . 66 % + 4 . 39 % 4 = 4.94 % O A C 2 = O A C min + O A C max 2 = 4.24 + 4.71 2 = 4.48 % O A C = O A C 1 + O A C 2 2 = 4.94 + 4.48 2 = 4.71 %
where a1 is the asphalt–aggregate ratio corresponding to the maximum bulk specific gravity; a2 is the asphalt–aggregate ratio corresponding to the maximum Marshall stability; a3 is the asphalt–aggregate ratio corresponding to the target air voids; a4 is the asphalt–aggregate ratio corresponding to the median value of the specified range of voids filled with asphalt; OACmin and OACmax are the lower and upper limits of the asphalt–aggregate ratio range satisfying the specification requirements, respectively; OAC1 is the average value of a1, a2, a3 and a4; OAC2 is the average value of OACmin and OACmax; and OAC is the final optimum asphalt–aggregate ratio.

3.2. Experiment Approach

3.2.1. Sample Preparation

The specimen thicknesses were selected according to both field-core availability and standard laboratory testing requirements. The 30 mm and 40 mm specimens were used to represent small-thickness asphalt layers that may be obtained from in-service pavements, especially thin surface courses. The 70 mm specimens were selected to represent an intermediate asphalt-layer thickness commonly encountered in pavement cores. The 100 mm specimens correspond to the standard height used for the uniaxial compressive strength test, while the 150 mm specimens correspond to the standard height used for the uniaxial compression dynamic modulus test. The 130 mm specimens were introduced as a transition size between the two standard dimensions. In addition, the selected thickness range covers values below and above approximately 3~4 times the nominal maximum aggregate size of AC-13 and SMA-13 mixtures, which allows the thickness-dependent size effect to be evaluated over both small-thickness and relatively stable-size ranges.
To carry out UCS, ITS, UCM, and ITM tests on the asphalt mixture with different thicknesses of samples, cylindrical samples with rotary compaction molding diameters of 100 mm and heights of 100 mm, 130 mm, and 150 mm were used. The quantity and composition of samples with different thicknesses are shown in Table 5. The specimens with heights of 30 mm, 40 mm, and 70 mm were cut from 150 mm cylindrical specimens using a water-cooled cutting machine to minimize heat accumulation and cutting-induced disturbance. The cut surfaces were then trimmed to ensure parallelism between the upper and lower loading faces. Specimens showing visible edge defects, aggregate loosening, or abnormal air void contents were excluded from testing. Nevertheless, minor cutting-induced microdamage or local disturbance of the internal structure may still remain, which represents a potential source of uncertainty in the present laboratory calibration. The diameter of the formed samples should be controlled within 100 mm ± 2.0 mm, and the height error should not exceed 2 mm. The volumes of air voids in the different thickness samples were measured to ensure that this parameter related to formal samples deviated within ±0.50% of its target values. The target porosity is 4.0%. Five parallel tests were conducted under each size condition, and the prepared asphalt mixture samples with different thicknesses are shown in Figure 4A. For each test condition, the average value of the five replicate specimens was used as the representative result. The standard deviation and coefficient of variation were calculated to evaluate data dispersion and repeatability.
Table 5. Quantity and composition of samples with different thicknesses.
Figure 4. Asphalt mixture samples and tests with different thicknesses.

3.2.2. Uniaxial Compression Test

UCS and UCM tests were conducted using the Material Testing System (MTS). Before the test, each sample was positioned in a thermostatically controlled box at 20 °C for at least five hours. The tests were conducted at a controlled temperature of 20 °C. The loading speed for the UCS test was regulated at 2 mm/min. The frequency for the UCM test was maintained at 10 Hz. The stress control mode was used in the loading process, and a sine wave was applied to the sample. The maximum value of the sine wave was taken as 10% of the peak load of the UCS test, and the minimum value was taken as 1% of the peak load of the UCS test. The strain of the sample during the loading process was measured using extensometers. The UCS and UCM tests of the asphalt mixtures are shown in Figure 4B.
The UCS and UCM tests were performed using a servo-hydraulic Material Testing System (Landmark, MTS Systems Corporation, Eden Prairie, MN, USA) with a maximum loading capacity of 100 kN. The system included a loading frame, a load cell, a temperature-controlled chamber, displacement sensors, and data acquisition software. During the UCS test, axial load, actuator displacement, and loading time were continuously recorded until failure. During the UCM test, cyclic load, recoverable axial deformation, loading time, and phase information were collected. Axial deformation was measured by two extensometers symmetrically mounted on opposite sides of the cylindrical specimen within the central gauge length to reduce the influence of local deformation and eccentric loading. The UCM was calculated using the average load amplitude and recoverable deformation amplitude of the last five stable loading cycles.
The general steps of the UCS test are as follows: First, place the lower pressing plate and base at the center of the MTS lifting platform. Then, remove the sample from the constant temperature box, put it at the center line of the lower pressing plate, and add the upper pressing plate. Finally, a uniform loading rate of 2 mm/min is applied until failure occurs. Extensometers must be installed on both sides of the sample for the UCM test. Additionally, before the test, the sample must undergo a preload treatment. The preload method involves applying sinusoidal axial compressive stress to the sample at a frequency of 25 Hz for 200 cycles. The MTS collects force, vertical displacement, and time data.
According to JTG E20-2011, uniaxial compression strength (UCS) was calculated by using Equation (2).
U C S = 4 P π D 2
where P and D are measured failure load (N) and diameter (mm), respectively.
According to the dynamic modulus test method for asphalt mixtures in JTG E20-2011, the uniaxial compression dynamic modulus (UCM) was calculated by using Equation (3).
U C M = P i l 0 A Δ i
where P i is the average amplitude of the axial load in the last five loading cycles (N); l 0 is the measurement spacing of the extensometer (mm); A is the cross-sectional area (mm8); and Δ i is the average amplitude of the recoverable axial deformation in the last five loading cycles (mm).

3.2.3. Indirect Tensile Test

The operational procedures for the indirect tensile test of the asphalt mixture were largely similar to uniaxial compression tests. The main difference is the sample loading mode. The loading speed for the ITS test was controlled at 50 mm/min. It is noteworthy that the dynamic modulus test was considered a non-destructive test. In order to contrast the correlation between the UCM and ITM more accurately, this study used the same asphalt mixture samples to conduct the UCM and ITM tests sequentially. The ITS and ITM tests of the asphalt mixture are shown in Figure 4C.
The testing system consists of a loading frame, a load cell, a temperature-controlled chamber, displacement sensors, and data acquisition software. For the ITS test, the cylindrical specimen was placed between the upper and lower loading strips, and the load was applied along the vertical diameter. The applied load, vertical displacement, and loading time were continuously recorded until splitting failure occurred. For the ITM test, cyclic compressive loading was applied along the vertical diameter. The recoverable deformation was measured at the central region of the specimen using extensometers. The cyclic load, recoverable deformation, loading time, and phase information were collected. Similar to the UCM test, the average load amplitude and recoverable deformation amplitude of the last five stable loading cycles were used to calculate the ITM.
According to the indirect tensile test method in JTG E20-2011, indirect tensile strength (ITS) was calculated by using Equation (4).
I T S = 2 P t π D L
where P t and L are measured failure load (N) and thickness (mm), respectively.
In the indirect tensile test, the cross-section disk was placed in central compression. The loading schematic diagram and the force schematic diagram of the indirect tensile test sample are shown in Figure 5.
Figure 5. Loading and force schematic diagrams of the indirect tensile test sample.
Taking the center point of the circular cross-section as the vertical coordinate, assuming that the distance of any point T ( x , y ) inside the circular cross-section to the top of the section is r 1 , and the distance to the bottom is r 2 , and the angle between the O Y -axis and r 1 is θ 1 , and the angle between the O Y -axis and r 2 is θ 2 , the stress state of any point T ( x , y ) inside the circular disk can be represented by Equation (5) [49].
σ x = 2 P π L sin 2 ( θ 1 ) c o s ( θ 1 ) r 1 + sin 2 ( θ 2 ) c o s ( θ 2 ) r 2 − 2 P π D L σ y = 2 P π L c o s 3 ( θ 1 ) r 1 + c o s 3 ( θ 2 ) r 2 − 2 P π D L τ x y = 2 P π L sin ( θ 1 ) c o s 2 ( θ 1 ) r 1 + sin ( θ 2 ) c o s 2 ( θ 2 ) r 2
where σ x and σ y represent the normal stress in the x and y directions of any point T ( x , y ) inside the disk, respectively (MPa); τ x y represents the shear stress at any point T ( x , y ) inside the disk (MPa); P is the load applied to the upper indenter (N); and the meaning of θ 1 , θ 2 and r 1 , r 2 is shown in Figure 5B.
According to the analytical solution of elastic mechanics of plane stress problems [54] and the geometric characteristics of the O X -axis and O Y -axis, as well as the geometric relationship r 1 = r 2 , r 1 = r 2 , r 1 2 = R 2 + x 2 , tan θ = x / R along the O X -axis direction, the stress state at any point on the O X -axis and O Y -axis can be determined as follows [49].
In the direction of the O X -axis, by Equation (6):
σ x ( x ) = 2 P π D L 1 − 16 D 2 x 2 4 x 2 + D 2 2 σ y ( x ) = 2 P π D L 1 − 4 D 4 4 x 2 + D 2 2 τ x y ( x ) = 0
In the direction of the O Y -axis, by Equation (7):
σ x ( y ) = 2 P π D L σ y ( y ) = 2 P π D L 1 − D 2 R 2 − y 2 τ x y ( y ) = 0
where σ x ( x ) and σ y ( x ) represent the tensile stress and compression stress at any point on the O X -axis, respectively (MPa); σ x ( y ) and σ y ( y ) represent the tensile stress and compression stress at any point on the O Y -axis, respectively (MPa); τ x y ( x ) and τ x y ( y ) represent the shear stress at any point on the O X -axis and O Y -axis, respectively (MPa); and R is the radius (mm).
Performing integration calculation on the above formula, taking into account the symmetric distribution of stress, take the value range of x between 0 and 0.5 L ′ , and calculate the mean tensile stress σ x ¯ and mean compressive stress σ y ¯ within the range of 0–0.5 L ′ , as shown in Equation (8).
σ x ¯ = ∫ 0 0.5 L ′ σ x ( x ) d x 0.5 L ′ = 4 P π L L ′ arctan L ′ D − D L ′ L ′ 2 + D 2 − 0.5 L ′ D σ y ¯ = ∫ 0 0.5 L ′ σ y ( x ) d x 0.5 L ′ = 4 P π L L ′ arctan L ′ D + D L ′ L ′ 2 + D 2 − 0.5 L ′ D
According to generalized Hooke’s law under plane stress state in elastic theory, as shown in Equation (9):
E = σ x − μ σ y ε x
Substituting Equation (8) into Equation (9), the indirect tensile dynamic modulus (ITM) calculation formula can be obtained, as shown in Equation (10):
I T M = − 4 P π L L ′ ε x ¯ arctan L ′ D − D L ′ L ′ 2 + D 2 − 0.5 L ′ D − μ ( arctan L ′ D + D L ′ L ′ 2 + D 2 − 0.5 L ′ D )
where P is the average amplitude of the test load in the last five loading cycles (N); μ is the Poisson’s ratio; L ′ is the measurement spacing of the extensometer (mm); and ε x ¯ is the average amplitude of recoverable strain in the last five loading cycles.

4. Theoretical Research of Size Effect

The size effect has been widely studied in quasi-brittle materials, such as concrete and rock. Although the classical theories proposed by Weibull, Bažant, and Carpinteri remain the fundamental basis for explaining size-dependent strength variation, recent studies have extended size effect analysis to asphalt mixtures by considering aggregate distribution, internal heterogeneity, fracture process, and specimen geometry [65]. Therefore, the classical size effect models were retained in this study as theoretical references, while recent asphalt-mixture-related studies were also introduced to support the applicability of size effect analysis to asphalt materials.

4.1. Basic Theory of Size Effect

4.1.1. Weibull Statistical Size Effect Theory

In 1939, Weibull [66] proposed the statistical size effect theory of material strength, which states that the size effect is mainly caused by the random distribution of material strength. Due to the randomness of strength, the probability of encountering a low-strength material unit increases with an increase in structural size. The failure of the weakest unit will lead to the failure of the entire structure.
The formula for the Weibull statistical size effect law is shown in Equation (11):
σ N = σ 0 D 0 l c h 3 m = a b l c h 3 c
where σ N is the compressive strength (MPa); σ 0 and D 0 are parameters related to the geometric sizes of the structure; l c h is the characteristic size of the material (mm); m is the Weibull parameter; a is the strength-scale parameter (MPa); b is the reference size parameter (mm), and c is the Weibull parameter controlling the sensitivity of strength to specimen size.

4.1.2. Bažant Energy Release Size Effect Theory

Bažant [67,68] proposed the size effect theory caused by energy release, which expresses that the size effect of materials is motivated by stress redistribution and energy release during crack propagation.
The formula for the Bažant energy release size effect law is shown in Equation (12):
  σ N = B f t 1 + β = B f t 1 + l c h / D 0 = a 1 + l c h / b
where B is a dimensionless constant; f t is the material’s tensile strength (MPa); and β is the brittle index, β = l c h / D 0 .

4.1.3. Carpinteri Multiple Fractal Size Effect Theory

In 1944, Carpenteri [69] proposed the multiple fractal size effect theory based on the randomness of material strength and the microscopic characteristics of fractals. Carpenteri exposed that the strength of each point inside quasi-brittle materials was different. Hence, under the action of the external force field, the propagation process of internal cracks in materials had fractal characteristics, and the differences in characteristics were the root cause of the size effects.
The formula for the Carpinteri multiple fractal size effect law is shown in Equation (13):
  σ N = f t 1 + D 0 l c h = a + b l c h

4.2. The Causes of Size Effect

Similar to the factors affecting the strength size effect of concrete, the strength size effect of asphalt mixtures may be influenced by the following five factors:
(1)
Boundary effects [70]. Large aggregates tend to be distributed in the central area of the samples, while small aggregates tend to be distributed in the boundary area of the samples. Thus, a boundary layer is formed that is independent of the size of the component itself, and the thickness of this layer depends on the particle size of the maximum aggregate. In smaller components, the boundary layer occupies most of the cross-sectional area. In contrast, in larger components, the boundary layer only occupies a small portion of the cross-sectional area, leading to size effects.
(2)
Diffusion phenomenon [71]. Because the diffusion time is proportional to the square of the component size, diffusion itself changes the material’s properties and generates residual stress, ultimately leading to nonlinear strain and cracking. Therefore, for large and small samples, differences in diffusion time and stored energy result in varying crack densities for different degrees of cracking.
(3)
Statistical size effect [72]. The strength of each point in the component has randomness, which increases the probability of encountering a low-strength material unit as the structural size increases, leading to size effects.
(4)
Fracture mechanics size effect [73]. The Bažant size effect theory suggests the main reason for the size effect is the stable propagation of a long crack or a fracture area containing microcracks. Macroscopic cracks lead to stress redistribution and internal energy release during stable growth and diffusion, resulting in size effects.
(5)
The fractal characteristics of the crack surface [74,75,76,77]. The Carpenteri fractal size effect theory suggests that cracks caused by external force fields are discontinuous and random. Hence, the evolution process of internal microcracks in materials has fractal characteristics, leading to size effects.

5. Results and Discussion

5.1. Size Effect of Strength Test Results

5.1.1. Uniaxial Compression Strength

Figure 6A depicts the asphalt mixture’s UCS failure mode. Figure 6B shows the force–displacement curves of the UCS tests. From the microscopic perspective of the compression process of the asphalt mixtures, the failure mechanism can be summarized as follows: Microcracks are first formed at the interface of coarse aggregates and inside the asphalt mortar. As the stress increases, microcracks expand and extend into macroscopic cracks. When the damage to asphalt mortar accumulates and causes a disconnection with the aggregates, the integrity of the asphalt mixture is destroyed, and its bearing capacity is lost.
Figure 6. Uniaxial compression failure mode and force–displacement curves.
Figure 7A depicts the variations in UCS with sample thickness. Figure 7A shows that asphalt mixture UCS values decrease as the sample thickness increases. They exhibit a pattern similar to that of concrete [28]. The variation trends of UCS with thickness for different graded asphalt mixtures are basically the same. When the thickness of the sample is less than 3~4 times the maximum particle size of the aggregates, the test data have greater discreteness, and the UCS values change more significantly with the thickness of the sample. When the thickness of the sample is greater than 3~4 times the maximum particle size of the aggregates, the discreteness of the test data decreases, and the UCS values tend to flatten with the variation in sample thickness. The research results are consistent with those of Ge et al. [35]. This phenomenon may be due to the end effect. Figure 7B shows the uniaxial compression tests of asphalt mixtures with different thicknesses related to this phenomenon. The end effect refers to the constraint effect caused by the friction of the test machine’s press head on the ends of the sample, which restrains the sample from free lateral deformation. Due to the presence of the end effect, the distribution of stress near the end of the sample becomes more complex. The three-dimensional stress state at both ends of the sample has a certain interference effect on the sample’s deformation characteristics, failure modes, and peak strength. When the height of the sample is relatively high, the middle part of the sample is not affected by the end effect, allowing for free lateral deformation, which makes the sample more prone to failure. Conversely, when the sample’s height is low, it is influenced by the overlapping end effects from the top and bottom, making it less likely to fail. Therefore, a critical height exists at which the sample is fully affected by the end effect without overlapping.
Figure 7. Variations in UCS with sample thickness and end effect.
The end effect was not explicitly corrected in this study. In short cylindrical specimens, friction at the loading platens restrains lateral deformation and may produce overlapping confined zones near the specimen ends. This effect can increase the apparent UCS and UCM of small-thickness specimens. Therefore, the proposed conversion equations should be interpreted as empirical relationships under the present loading boundary conditions.
The size effect of UCS gradually tends to a certain constant with the increase in sample size, and its ultimate limit may be related to the bearing capacity of the asphalt mixture in the elastic stage. The correlation equations between the UCS and sample thickness were obtained by fitting the experimental data, as shown in Equation (14).
A C − 13 : U C S = − 7.23 + 18.99 x − 29.34 0.11     R 2 = 0.99 S M A − 13 : U C S = 0.37 + 300.09 x 1.01     R 2 = 0.97
where UCS is the uniaxial compressive strength (MPa), and x is the thickness (mm).
The experimental data were fitted with the size effect theoretical formulas of Weibull, Bažant, and Carpinteri, resulting in the fitting coefficients shown in Table 6. According to Table 6, the UCS test data fit well with the theories of Weibull, Bažant, and Carpinteri. Among them, Weibull’s correlation coefficient is the highest, while Bažant’s is the lowest. In practice, the magnitude of correlation coefficients of the fitting parameters can be used to initially analyze the main factors affecting the size effect of asphalt mixtures.
Table 6. Fitting coefficients of UCS.

5.1.2. Indirect Tensile Strength

Figure 8A illustrates the asphalt mixture’s ITS failure mode. A main crack can be seen near the center axis between the upper and lower loading plates. The main reasons for failure are low-strength units or defects concentrated at the interface between the coarse aggregate and the asphalt mortar. Figure 8B illustrates the force–displacement curves of the ITS tests for the asphalt mixtures. Figure 8C shows the schematic diagram of the ITS stress–strain curve. Figure 8B,C depict that indirect tensile failure can be divided into the compaction stage, the elastic stage, and the stage of transition to plastic deformation until failure [58]. Under pressure, the asphalt mixture is first compacted. After compaction, it enters the elastic stage. During this process, the generation of new cracks and the stable expansion of pre-existing ones are the primary outcomes. During the yield stage, the sample transitions from elasticity to plasticity. After reaching peak strength, the internal pores and cracks of the sample continue to expand, eventually piercing the sample and causing failure. Figure 8B indicates that the curves become flatter with decreasing thickness. The reason is that a smaller thickness leads to a smaller area of the fracture surface and less work required for failure, resulting in a smaller load to be applied. Secondly, when the sample’s thickness decreases, fewer pores are present within the sample [31], leading to a shorter time required for the compaction process. Therefore, in the force–displacement curves of the ITS tests, the stages of compaction, elasticity, and the transition to plastic deformation until failure are also flatter.
Figure 8. Indirect tensile failure forms and force–displacement curves.
Figure 9 displays the ITS variations with sample thickness. Figure 9 indicates that the asphalt mixture’s ITS increases with sample thickness, exhibiting results opposite to concrete [30]. The ITS variation trend with thickness for different graded asphalt mixtures is basically the same. The size effect phenomenon of ITS is less pronounced than that related to UCS. When the sample thickness is less than 3~4 times the maximum aggregate size, the test data show significant dispersion. However, when the sample thickness exceeds 3~4 times the maximum aggregate size, the discreteness of the test data decreases. The correlation equations between ITS and sample thickness were obtained by fitting the experimental data, which are shown in Equation (15).
A C − 13 : I T S = 1.19 + 0.0026 x     R 2 = 0.99 S M A − 13 : I T S = 0.93 + 0.0024 x     R 2 = 0.89
where ITS represents the indirect tensile strength (MPa) and x is the thickness (mm).
Figure 9. Variations in ITS with sample thickness.
After fitting the experimental data to the size effect theories of Weibull, Bažant, and Carpinteri, it was observed that the fitting performance for both ITS and the size effect law was poor. Numerous scholars believe that the most important factor affecting ITS is the splitting surface area of the sample [25]. As a result, the researchers established a functional relationship between ITS and splitting surface area, obtaining a size effect calculation formula related to the area, which is shown in Equation (16).
R N = α ⋅ A − m
where R N is the ITS (MPa); A is the splitting surface area (mm8); and α and m are parameters.
The ITS test data were fitted to Equation (16), and the resulting fit equations are shown in Equation (17). Equation (17) shows a high correlation coefficient, indicating a strong correlation between ITS and the splitting surface area. Notably, the ITS of asphalt mixtures increases with the enlargement of the splitting surface area, contrary to the pattern observed in concrete [30].
A C − 13 : R N = 0.42 ⋅ A 0.14     R 2 = 0.96 S M A − 13 : R N = 0.56 ⋅ A 0.16     R 2 = 0.94
where R N is the ITS (MPa); and A is the splitting surface area (mm8).

5.2. Size Effect of Dynamic Modulus Test Results

5.2.1. Uniaxial Compression Dynamic Modulus

The UCM test is a non-destructive procedure, and no deformation or failure of the sample was observed during the test. Figure 10 displays the variations in the UCM with sample thickness. According to Figure 10, it can be seen that the UCM of asphalt mixtures decreases with an increase in sample thickness, indicating a significant size effect phenomenon. The variation trend of UCM with thickness for different graded asphalt mixtures is basically the same. When the thickness of the sample is less than 3~4 times the maximum particle size of the aggregates, the test data have greater discreteness, and the UCM changes more significantly with the thickness of the sample. When the thickness of the sample is greater than 3~4 times the maximum particle size of the aggregates, the discreteness of the test data decreases, and the UCM tends to flatten with the variation in sample thickness. The relationship equations between the UCM and the sample thickness were obtained by fitting the experimental data, as shown in Equation (18).
A C − 13 : U C M = 0.49 x 2 − 151.81 x + 15993.90     R 2 = 0.92 S M A − 13 : U C M = 0.64 x 2 − 179.01 x + 18121.33     R 2 = 0.95
where UCM is the uniaxial compression dynamic modulus (MPa), and x is the thickness (mm).
Figure 10. Variations in UCM with sample thickness.
With reference to the UCS size effect law, the experimental data were fitted to the theoretical formulas of Weibull, Bažant, and Carpinteri, resulting in the fitting coefficients as shown in Table 7. According to Table 7, the fitting of the Bažant size effect law was unsuccessful. Both Weibull and Carpenteri can match the UCM test data well.
Table 7. Fitting coefficients of UCM.
Similar to UCS, the UCM results may also be affected by platen confinement in small-thickness specimens. Therefore, the UCM conversion equations should also be interpreted as empirical relationships under the present uniaxial compression boundary condition.

5.2.2. Indirect Tensile Dynamic Modulus

During the ITM test of the asphalt mixture, no deformation or failure of the samples was observed. Figure 11 exhibits the variations in the ITM with the thickness of the sample. Figure 11 displays that the asphalt mixture’s ITM increases with sample thickness, but the trend tends to stabilize. The size effect of ITM is less significant than that of UCM. The variation trend of ITM with thickness for different gradation asphalt mixtures is basically the same. The correlation equations between the ITM and sample thickness were derived by fitting the experimental data, as shown in Equation (19).
A C − 13 : I T M = 2735.53 + 9.53 x     R 2 = 0.96 S M A − 13 : I T M = 3152.01 + 8.71 x     R 2 = 0.94
where ITM is the indirect tensile dynamic modulus (MPa), and x is the thickness (mm).
Figure 11. Variations in the ITM with sample thickness.
With reference to the ITS size effect law, the ITM test data were fitted to Equation (16), and the resulting fit equations are shown in Equation (20). Equation (20) shows a high correlation coefficient, indicating a strong correlation between ITM and the splitting surface area.
A C − 13 : R N = 546.80 ⋅ A 0.21     R 2 = 0.96 S M A − 13 : R N = 1855.08 ⋅ A 0.17     R 2 = 0.98
where R N is the ITM (MPa); and A is the splitting surface area (mm8).

5.3. Research on the Method of Obtaining Parameters of Existing Asphalt Pavements

5.3.1. Research on Parameter Acquisition of Existing Asphalt Pavements Based on the Uniaxial Compression Test

The standard sample size specified by JTG E20-2011 for the UCS test is a diameter of 100 mm and a height of 100 mm. The standard specimen size for the UCM test is a diameter of 100 mm and a height of 150 mm. However, the asphalt layers on general existing asphalt pavements, including the upper surface course, middle surface course, and the lower surface course, have thicknesses of 40 mm, 60 mm, and 80 mm, respectively, which fall far short of the standard sample size in terms of height. Therefore, it is not possible to directly evaluate the mechanical properties or verify the compliance of the pavement structure layer parameters by directly sampling from the actual pavement.
This article fitted the experimental data and obtained the conversion rates of U C S 100 / U C S x and U C M 100 / U C M x , as shown in Table 8. According to Table 8, there is a good regularity between the conversion coefficient and thickness. When the thickness exceeds 100 mm, the conversion coefficient for UCM tends towards 1.0. For specimens with thicknesses of 30~70 mm, the UCS conversion coefficients ranged from 0.30 to 0.85, while the UCM conversion coefficients ranged from 0.41 to 0.60.
Table 8. Conversion rates of U C S 100 / U C S x and U C M 100 / U C M x .
The correlation curves between the UCS and UCM of the asphalt mixture are shown in Figure 12. It is evident from the figure that there is a nonlinear positive correlation between the UCS and UCM as the sample thickness increases. By fitting the test data, the correlation formulas between the UCM and UCS were obtained by Equation (21).
A C − 13 : U C M = − 158.27 U C S 2 + 3232.14 U C S − 3956.71     R 2 = 0.97 S M A − 13 : U C M = − 279.78 U C S 2 + 2731.30 U C S − 142.34     R 2 = 0.92
where UCM is the dynamic modulus of uniaxial compression (MPa), and UCS is the uniaxial compression strength (MPa).
Figure 12. Correlation curves between UCS and UCM.
Equation (22) shows the fitting equation for the conversion coefficients of U C S 100 / U C S x . Equation (23) shows the fitting equation for the conversion coefficients of U C M 100 / U C M x . Hence, the method for obtaining the strength and dynamic modulus of existing asphalt pavement materials based on uniaxial compression tests is as follows: Firstly, obtain small-thickness samples through core sampling from the existing asphalt pavement. Then, UCS and UCM tests will be conducted to determine the UCS and UCM of the small-thickness samples. Finally, they can be converted to UCS and UCM at standard sizes based on proportional relationships.
A C − 13 : K f 100 = − 4.7 × 10 − 5 x 2 + 1.55 × 10 − 2 x − 0.03     R 2 = 0.96 S M A − 13 : K f 100 = − 6.0 × 10 − 5 x 2 + 1.74 × 10 − 2 x − 0.21     R 2 = 0.98
A C − 13 : K E 150 = − 3.64 × 10 − 5 x 2 + 1.2 × 10 − 2 x + 0.043     R 2 = 0.85 S M A − 13 : K E 150 = − 3.54 × 10 − 5 x 2 + 1.2 × 10 − 2 x + 0.086     R 2 = 0.87
where K f 100 and K E 150 are the conversion rates, and x is the thickness (mm).

5.3.2. Research on Obtaining Parameters of Existing Asphalt Pavements Based on the Indirect Tensile Test

The variation laws between UCS and ITS, as well as between UCM and ITM of the asphalt mixture, are shown in Figure 13. Figure 13 shows that as the thickness of the sample increases, there is a negative correlation change between UCS and ITS, as well as between UCM and ITM. The UCS is greater than the ITS, and the UCM is greater than the ITM. Moreover, as the sample thickness increases, the numerical difference between UCS and ITS and between UCM and ITM diminishes. The variation in the values of ITS and ITM is not obvious under different thicknesses. This fact indicates that, while ensuring experimental errors, it is possible to obtain samples by drilling cores outdoors and obtain relatively stable ITS and ITM with small-thicknesses through experiments. Furthermore, when the thickness exceeds 100 mm, the values of UCS and UCM exhibit no significant changes with variations in thickness. This phenomenon indicates that relatively stable proportional coefficients of U C S 100 / I T S x and U C M 150 / I T M x can be obtained. After obtaining accurate proportion coefficients, small thickness samples can be obtained by outdoor core drilling. Subsequently, indirect tensile tests will be conducted to obtain ITS and ITM values. Finally, the strength and dynamic modulus data of the existing pavement can be determined using the proportion coefficients.
Figure 13. Variation laws between UCS and ITS, as well as between UCM and ITM of the asphalt mixture.
The correlation curves between ITS and ITM of the asphalt mixture are shown in Figure 14. Figure 14 illustrates that there is an excellent linear positive correlation between ITS and ITM with an increase in sample thickness. By fitting the experimental data, the correlation equations between ITM and ITS were obtained, as exhibited in Equation (24).
A C − 13 : I T M = − 1687.31 + 3714.19 I T S     R 2 = 0.97 S M A − 13 : I T M = − 86.88 + 3528.94 I T S     R 2 = 0.98
where ITM is the indirect tensile dynamic modulus (MPa), and ITS is the indirect tensile strength (MPa).
Figure 14. Correlation curves between ITM and ITS.
This article fitted the experimental data and obtained the conversion rates of U C S 100 / I T S x and U C M 150 / I T M x , as shown in Table 9. According to Table 9, there is a good regularity between the conversion coefficient and thickness. The ITS of small-thickness samples is 2.7~3.1 times that of U C S 100 . The ITM of small-thickness samples is 1.5~1.8 times that of U C M 150 . Equation (25) shows the fitting equation for the conversion coefficients of U C S 100 / I T S x . Equation (26) shows the fitting equation for the conversion coefficients of U C M 150 / I T M x . Hence, the method for obtaining the strength and dynamic modulus of existing asphalt pavement materials based on indirect tensile tests is as follows: Firstly, obtain small-thickness samples through core sampling from the existing asphalt pavement. Then, ITS and ITM tests will be conducted to determine the ITS and ITM of small-thickness samples. Finally, they can be converted to UCS and UCM under standard sizes based on proportional relationships.
Table 9. Conversion coefficients of U C S 100 / I T S x and U C M 150 / I T M x .
A C − 13 : K f 100 = 1.05 × 10 − 5 x 2 − 0.0068 x + 3.22     R 2 = 0.99 S M A − 13 : K f 100 = 4.54 × 10 − 5 x 2 − 0.014 x + 3.35     R 2 = 0.86
A C − 13 : K E 150 = 2.61 × 10 − 5 x 2 − 0.0085 x + 1.90     R 2 = 0.94 S M A − 13 : K E 150 = 2.51 × 10 − 5 x 2 − 0.0079 x + 1.96     R 2 = 0.93
where K f 100 and K E 150 are the conversion rates, and x is the thickness (mm).
The schematic diagrams of the existing asphalt pavement material strength and dynamic modulus parameter acquisition method based on uniaxial compression and indirect tensile tests are shown in Figure 15. As transportation infrastructure construction enters a large-scale maintenance stage, extending the service life of existing asphalt pavements has become an essential means of achieving sustainable development in road engineering. Accurately obtaining the strength and dynamic modulus parameters of existing pavement materials is a prerequisite for establishing reliable life extension design models and formulating reasonable maintenance and repair plans. According to the method proposed in this study, the structural design parameters of the materials can be obtained by conducting on-site core sampling tests and inspections of the existing asphalt pavements. This procedure can provide a scientific basis for evaluating the remaining service life of the pavements and formulating maintenance and repair plans, thereby extending the service life of the pavements. This procedure provides a potential approach for obtaining mechanical parameters of small-thickness asphalt layers. However, because the conversion relationships were established using laboratory-prepared specimens, further validation using actual field cores and in situ pavement evaluation data is required before direct application to pavement rehabilitation design.
Figure 15. Schematic diagram of obtaining strength and dynamic modulus parameters of existing asphalt pavement materials.

5.4. Applicability and Limitations of the Proposed Method

The proposed method should be interpreted as a laboratory-calibrated conversion framework, rather than as a field-validated procedure for direct engineering application. AC-13 and SMA-13 were selected in this study because they are commonly used asphalt surface mixtures. The test temperature was fixed at 20 °C to reduce the influence of thermal variation and to focus on the effects of specimen thickness and gradation on strength and dynamic modulus. Such a controlled experimental design is necessary for establishing thickness-dependent conversion relationships. Nevertheless, asphalt mixtures in service are subjected to seasonal temperature changes, aging, moisture damage, traffic-induced densification, field compaction differences, and construction variability. These factors may change the measured mechanical properties and the corresponding size effect behavior. Therefore, the conversion relationships obtained in this study should be applied to other mixture types or field conditions only after further calibration.
In addition, the conversion relationships were not validated using actual field cores or in situ pavement evaluation data in this study. Field-core testing and comparison with in situ evaluation results are therefore required before the proposed method is used for direct rehabilitation design.

6. Conclusions

This paper investigated the impact of different thicknesses and gradations on the UCS, UCM, ITS, and ITM of asphalt mixtures. A method for obtaining design parameters of in-service pavement asphalt layers based on the size effect was proposed. This method facilitates the testing of thinner asphalt pavement structural layers. According to the research results and discussions, the following conclusions have been drawn:
(1)
The UCS of asphalt mixtures increased with decreasing specimen thickness, whereas the ITS increased with increasing specimen thickness. This trend was observed for both AC-13 and SMA-13 mixtures. For the uniaxial compression test, the UCS conversion coefficients of small-thickness specimens ranged from 0.30 to 0.85 before reaching the standard specimen height of 100 mm. The Weibull size effect model provided the best fit to the UCS results, with correlation coefficients of 0.85 and 0.97 for AC-13 and SMA-13, respectively. In contrast, the classical Weibull, Bažant, and Carpinteri models showed limited applicability to the ITS results, while the area-related size effect relationship better described the variation in ITS with specimen thickness.
(2)
The UCM of asphalt mixtures increased with decreasing specimen thickness, whereas the ITM increased with increasing specimen thickness. The two gradations showed the same thickness-dependent variation pattern. For specimens with thicknesses of 30~70 mm, the UCM conversion coefficients ranged from 0.41 to 0.60, and the coefficients tended to approach 1.00 when the specimen thickness exceeded 100 mm. The Weibull and Carpinteri models described the UCM results well, with correlation coefficients of 0.89~0.92 and 0.93~0.94, respectively. For the indirect tensile test, the ITM to UCM conversion coefficients ranged from 1.21 to 1.79, and the area-related size effect relationship showed good applicability to the ITM results.
(3)
Based on the thickness-dependent size effect relationships, a parameter conversion method was established for obtaining the standard-size UCS and UCM of asphalt mixtures from small-thickness specimens. For the uniaxial compression test, small-thickness UCS and UCM results can be converted to standard-size parameters using thickness-dependent conversion coefficients. For the indirect tensile test, ITS and ITM results can be further related to standard-size UCS and UCM through proportional conversion relationships. This method provides a feasible laboratory-calibrated approach for estimating the strength and dynamic modulus parameters of thin asphalt layers in in-service pavements.
(4)
The established conversion coefficients provide a basis for linking small-thickness specimen results with standard-size mechanical parameters. This is particularly useful for thin asphalt layers in in-service pavements, where field cores often fail to meet the height requirements of standard uniaxial compression tests. Therefore, the proposed framework may support the mechanical evaluation of thin asphalt pavement layers after field validation.
(5)
The proposed method is limited to laboratory-prepared AC-13 and SMA-13 mixtures tested at 20 °C. The effects of aging, moisture damage, traffic densification, field compaction, and temperature–frequency dependence were not fully considered. Moreover, the conversion relationships were not validated using actual field cores in this study. Therefore, further validation using pavement cores, additional mixture types, and different temperature conditions is required before direct engineering application.

Author Contributions

Conceptualization, G.X., W.L. and S.L.; methodology, G.X., P.Z. and W.L.; validation, L.L., Q.C. and H.R.; formal analysis, G.X., P.Z. and L.L.; investigation, P.Z., Q.C. and H.R.; resources, L.L., W.L. and S.L.; data curation, P.Z. and L.L.; writing—original draft preparation, G.X. and P.Z.; writing—review and editing, P.Z., L.L. and H.R.; visualization, P.Z., Q.C. and H.R.; supervision, Y.H. and P.C.; project administration, Y.H. and P.C.; funding acquisition, G.X., W.L. and S.L. All authors have read and agreed to the published version of the manuscript.

Funding

The research was supported by the Traffic Transportation Science and Technology Projects in Shandong Province (2023B83) and the Open Research Project of Shandong Key Laboratory of Highway Technology and Safety Assessment (SH202301).

Data Availability Statement

The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding author.

Conflicts of Interest

Author Yuxi He was employed by Hunan Expressway Engineering Consulting Co., Ltd., and authors Gongfeng Xin and Li Li were employed by Shandong Hi-Speed Group Co.LTD Innovation Research Institute. The remaining authors declare that the research was conducted in the absence of any commercial or financial relationships that could be construed as a potential conflict of interest.

References

  1. Pierrehumbert, R. There Is no Plan B for Dealing with the Climate Crisis. Bull. At. Sci. 2019, 75, 215–221. [Google Scholar] [CrossRef] [Scilit]
  2. Santero, N.J.; Horvath, A. Global Warming Potential of Pavements. Environ. Res. Lett. 2009, 4, 34011. [Google Scholar] [CrossRef] [Scilit]
  3. Santero, N.J.; Masanet, E.; Horvath, A. Life-Cycle Assessment of Pavements. Part I: Critical Review. Resour. Conserv. Recycl. 2011, 55, 801–809. [Google Scholar] [CrossRef] [Scilit]
  4. AzariJafari, H.; Yahia, A.; Ben Amor, M. Life Cycle Assessment of Pavements: Reviewing Research Challenges and Opportunities. J. Clean. Prod. 2016, 112, 2187–2197. [Google Scholar] [CrossRef] [Scilit]
  5. Wang, T.; Lee, I.-S.; Kendall, A.; Harvey, J.; Lee, E.-B.; Kim, C. Life Cycle Energy Consumption and GHG Emission from Pavement Rehabilitation with Different Rolling Resistance. J. Clean. Prod. 2012, 33, 86–96. [Google Scholar] [CrossRef] [Scilit]
  6. Liu, Z.; Balieu, R.; Kringos, N. Integrating Sustainability into Pavement Maintenance Effectiveness Evaluation: A Systematic Review. Transp. Res. Part D Transp. Environ. 2022, 104, 103187. [Google Scholar] [CrossRef] [Scilit]
  7. Hsie, M.; Lin, C.T.; Ho, Y.F. A New Approach to Model Asphalt Pavement Overlay Cracking. Adv. Mater. Res. 2011, 250–253, 1757–1760. [Google Scholar] [CrossRef] [Scilit]
  8. Hong, F. Asphalt Pavement Overlay Service Life Reliability Assessment Based on Non-Destructive Technologies. Struct. Infrastruct. Eng. 2013, 10, 767–776. [Google Scholar] [CrossRef] [Scilit]
  9. Nivedya, M.; Murru, P.T.; Veeraragavan, A.; Krishnan, J.M. Estimation of Dynamic Modulus of Bitumen Stabilized Mixes. Constr. Build. Mater. 2017, 136, 202–216. [Google Scholar] [CrossRef] [Scilit]
  10. Fan, X.; Lv, S.; Zhang, N.; Xia, C.; Li, Y. Characterization of Asphalt Mixture Moduli under Different Stress States. Materials 2019, 12, 397. [Google Scholar] [CrossRef] [Scilit]
  11. Cheng, H.; Wang, Y.; Liu, L.; Sun, L. Effects of Using Different Dynamic Moduli on Predicted Asphalt Pavement Responses in Mechanistic Pavement Design. Road Mater. Pavement Des. 2021, 23, 1860–1876. [Google Scholar] [CrossRef] [Scilit]
  12. Lv, S.; Fan, X.; Xia, C.; Zheng, J.; Chen, D.; You, L. Characteristics of Moduli Decay for the Asphalt Mixture under Different Loading Conditions. Appl. Sci. 2018, 8, 840. [Google Scholar] [CrossRef] [Scilit]
  13. Wang, S.; Zhao, S.; Al-Qadi, I.L. Real-Time Density and Thickness Estimation of Thin Asphalt Pavement Overlay During Compaction Using Ground Penetrating Radar Data. Surv. Geophys. 2019, 41, 431–445. [Google Scholar] [CrossRef] [Scilit]
  14. Gopalakrishnan, K.; Manik, A. Co-Variance Matrix Adaptation Evolution Strategy for Pavement Backcalculation. Constr. Build. Mater. 2010, 24, 2177–2187. [Google Scholar] [CrossRef] [Scilit]
  15. Guzzarlapudi, S.D.; Adigopula, V.K.; Kumar, R. Comparative Study of Flexible Pavement Layers Moduli Backcalculation Using Approximate and Static Approach. Mater. Today Proc. 2017, 4, 9812–9816. [Google Scholar] [CrossRef] [Scilit]
  16. Liu, H.; Yang, X.; Jiang, L.; Lv, S.; Huang, T.; Yang, Y. Fatigue-Creep Damage Interaction Model of Asphalt Mixture under the Semi-Sine Cycle Loading. Constr. Build. Mater. 2020, 251, 119070. [Google Scholar] [CrossRef] [Scilit]
  17. Lin, S.; Ashlock, J.C.; Williams, R.C. Nondestructive Quality Assessment of Asphalt Pavements Based on Dynamic Modulus. Constr. Build. Mater. 2016, 112, 836–847. [Google Scholar] [CrossRef] [Scilit]
  18. Yang, S.; Braham, A.; Underwood, S.; Hanz, A.; Reinke, G. Correlating Field Performance to Laboratory Dynamic Modulus from Indirect Tension and Torsion Bar. Road Mater. Pavement Des. 2016, 18, 104–127. [Google Scholar] [CrossRef] [Scilit]
  19. JTG E20-2011; Standard Test Methods of Bitumen and Bituminous Mixtures for Highway Engineering. Communication Press: Beijing, China, 2011.
  20. Cooper, S.B.; Mohammad, L.N.; Elseifi, M.A.; Raghavendra, A. Laboratory-Measured Dynamic Modulus and Predicted Performance of Asphalt Mixtures: Effects of Specimen Orientation. Transp. Res. Rec. 2015, 2507, 78–89. [Google Scholar] [CrossRef] [Scilit]
  21. Solatifar, N.; Kavussi, A.; Abbasghorbani, M. Dynamic Modulus Predictive Models for In-Service Asphalt Layers in Hot Climate Areas. J. Mater. Civ. Eng. 2021, 33, 04020438. [Google Scholar] [CrossRef] [Scilit]
  22. Wang, D.; Luo, C.; Li, J.; He, J. Study on Dynamic Modulus Prediction Model of In-Service Asphalt Pavement. Buildings 2024, 14, 2550. [Google Scholar] [CrossRef] [Scilit]
  23. Zheng, Z.; Zeng, C.; Tian, C.; Wei, X. Mesoscale Numerical Investigation on the Size Effect of Concrete Uniaxial Compressive Strength under Different Contact Friction. Constr. Build. Mater. 2022, 346, 128416. [Google Scholar] [CrossRef] [Scilit]
  24. Jin, L.; Yu, W.; Du, X.; Yang, W. Meso-Scale Simulations of Size Effect on Concrete Dynamic Splitting Tensile Strength: Influence of Aggregate Content and Maximum Aggregate Size. Eng. Fract. Mech. 2020, 230, 106979. [Google Scholar] [CrossRef] [Scilit]
  25. Bažant, Z.P. Size Effect. Int. J. Solids Struct. 2000, 37, 69–80. [Google Scholar] [CrossRef] [Scilit]
  26. Bažant, Z.P. Size Effect in Blunt Fracture: Concrete, Rock, Metal. J. Eng. Mech. 1984, 110, 518–535. [Google Scholar] [CrossRef] [Scilit]
  27. Rahman, S.; Khattak, M.J.; Adhikari, B.; Adhikari, S. Discrete Element Modeling of Bonded Soil Mixtures under Uniaxial Compression and Indirect Tension Test. Transp. Geotech. 2021, 26, 100438–100463. [Google Scholar] [CrossRef] [Scilit]
  28. He, X.X.; Wu, S. Experimental Study on Size Effect in Strength of Pervious Concrete and its Associated Factor. Adv. Mater. Res. 2013, 634–638, 2684–2692. [Google Scholar] [CrossRef] [Scilit]
  29. Jin, L.; Li, J.; Yu, W.; Du, X. Mesoscopic Simulations on the Strength and Size Effect of Concrete under Biaxial Loading. Eng. Fract. Mech. 2021, 253, 107870. [Google Scholar] [CrossRef] [Scilit]
  30. Gao, D.Y.; Song, S.Q.; Hu, L.M. Relationships of Strengths and Dimensional Effect of Plastic Concrete. Adv. Mater. Res. 2011, 306–307, 1029–1037. [Google Scholar] [CrossRef] [Scilit]
  31. Lei, W.-S.; Yu, Z. A statistical Approach to Scaling Size Effect on Strength of Concrete Incorporating Spatial Distribution of Flaws. Constr. Build. Mater. 2016, 122, 702–713. [Google Scholar] [CrossRef] [Scilit]
  32. Mansur, M.A.; Islam, M.M. Interpretation of Concrete Strength for Nonstandard Specimens. J. Mater. Civ. Eng. 2002, 14, 151–155. [Google Scholar] [CrossRef] [Scilit]
  33. Zainal, S.M.I.S.; Hejazi, F.; Aziz, F.N.A.A.; Jaafar, M.S. Constitutive Modeling of New Synthetic Hybrid Fibers Reinforced Concrete from Experimental Testing in Uniaxial Compression and Tension. Crystals 2020, 10, 885. [Google Scholar] [CrossRef] [Scilit]
  34. Zhu, X.; Yu, H.; Qian, G.; Yao, D.; Dai, W.; Zhang, H.; Li, J.; Zhong, H. Evaluation of Asphalt Mixture Micromechanical Behavior Evolution in the Failure Process Based on Discrete Element Method. Case Stud. Constr. Mater. 2023, 18, e01773. [Google Scholar] [CrossRef] [Scilit]
  35. Ge, L.-N.; Yi, F.; Zhao, Q.-Q. Size Effect and Influence Factors of Asphalt Mixture Based on Particle Discrete Element. J. Highw. Transp. Res. Dev. 2020, 14, 1–11. [Google Scholar] [CrossRef] [Scilit]
  36. Falchetto, A.C.; Le, J.; Turos, M.I.; Marasteanu, M.O. Indirect Determination of Size Effect on Strength of Asphalt Mixtures at Low Temperatures. Mater. Struct. 2013, 47, 157–169. [Google Scholar] [CrossRef] [Scilit]
  37. Falchetto, A.C.; Wistuba, M.P.; Marasteanu, M.O. Size Effect in Asphalt Mixture at Low Temperature: Types I and II. Road Mater. Pavement Des. 2016, 18, 235–257. [Google Scholar] [CrossRef] [Scilit]
  38. Wu, K.; Deng, Q.; Deng, N.; Cai, X.; Huang, W. Size Effects of Finite Element Model for Three-Dimensional Microstructural Modeling of Asphalt Mixture. Adv. Mater. Sci. Eng. 2019, 2019, 1754567. [Google Scholar] [CrossRef] [Scilit]
  39. Wagoner, M.P.; Buttlar, W.G. Influence of Specimen Size on Fracture Energy of Asphalt Concrete (with discussion). J. Assoc. Asph. Paving Technol. 2007, 76, 391–426. [Google Scholar]
  40. Li, X.; Gibson, N.H. Using Small Scale Specimens for AMPT Dynamic Modulus and Fatigue Tests. J. Assoc. Asph. Paving Technol. 2013, 82, 579–615. [Google Scholar]
  41. Cerni, G.; Bocci, E.; Cardone, F.; Corradini, A. Correlation Between Asphalt Mixture Stiffness Determined Through Static and Dynamic Indirect Tensile Tests. Arab. J. Sci. Eng. 2017, 42, 1295–1303. [Google Scholar] [CrossRef] [Scilit]
  42. Júnior, J.L.O.L.; Babadopulos, L.F.A.L.; Soares, J.B. Effect of Aggregate Shape Properties and Binder’s Adhesiveness to Aggregate on Results of Compression and Tension/Compression Tests on Hot Mix Asphalt. Mater. Struct. 2020, 53, 43. [Google Scholar] [CrossRef] [Scilit]
  43. Ping, W.V.; Xiao, Y. Empirical Correlation of Indirect Tension Resilient Modulus and Complex Modulus Test Results for Asphalt Concrete Mixtures. Road Mater. Pavement Des. 2011, 9, 177–200. [Google Scholar] [CrossRef] [Scilit]
  44. Ali, Y.; Irfan, M.; Zeeshan, M.; Hafeez, I.; Ahmed, S. Revisiting the Relationship of Dynamic and Resilient Modulus Test for Asphaltic Concrete Mixtures. Constr. Build. Mater. 2018, 170, 698–707. [Google Scholar] [CrossRef] [Scilit]
  45. Chen, H.; Alamnie, M.M.; Barbieri, D.M.; Zhang, X.; Liu, G.; Hoff, I. Comparative Study of Indirect Tensile Test and Uniaxial Compression Test on Asphalt Mixtures: Dynamic Modulus and Stress-Strain State. Constr. Build. Mater. 2023, 366, 130187. [Google Scholar] [CrossRef] [Scilit]
  46. Nyamuhokya, T.P.; Romanoschi, S.; Hu, X.; Abdullah, A.; Walubita, L.F. Preliminary Investigation of the Relationship between HMA Compressive and Tensile Dynamic Modulus. Constr. Build. Mater. 2016, 128, 461–470. [Google Scholar] [CrossRef] [Scilit]
  47. Ebrahimi, M.G.; Saleh, M.; Gonzalez, M.A.M. The Interrelationship between Indirect Resilient Modulus and Dynamic Modulus for Dense Graded Hot Mix Asphalt. Int. J. Pavement Res. Technol. 2013, 6, 465–471. [Google Scholar] [CrossRef]
  48. Qin, X.; Ma, L.; Wang, H. Comparison Analysis of Dynamic Modulus of Asphalt Mixture: Indirect Tension and Uniaxial Compression Test. Transp. A Transp. Sci. 2018, 15, 165–178. [Google Scholar] [CrossRef] [Scilit]
  49. Lv, S.; Liu, C.; Yao, H.; Zheng, J. Comparisons of Synchronous Measurement Methods on Various Moduli of Asphalt Mixtures. Constr. Build. Mater. 2018, 158, 1035–1045. [Google Scholar] [CrossRef] [Scilit]
  50. Zhang, J.; Cui, J.; Wang, X. A Testing Theory for Simultaneously Determining Asphalt Mixture’s Dynamic Modulus in Compression and Tension by Use of IDT Test. Constr. Build. Mater. 2024, 440, 137334. [Google Scholar] [CrossRef] [Scilit]
  51. Rashadul, I.M.; Weldegiorgis, M.T.; Rafiqul, A.T. Correlating the Dynamic Modulus and the Indirect Tensile Strength of Asphalt Concrete. Adv. Mater. Res. 2013, 723, 268–275. [Google Scholar] [CrossRef] [Scilit]
  52. Liu, S.; Liu, J. Effect of Test Method on Evaluating Dynamic Modulus of Asphalt Mixture. J. China Foreign Highw. 2019, 5, 269–273. [Google Scholar] [CrossRef]
  53. Zhu, D.; Zhou, L.; Zhang, X.; Zhao, J. Simultaneous Determination of Multiple Mechanical Parameters for a DNAN/HMX Melt-Cast Explosive by Brazilian Disc Test Combined with Digital Image Correlation Method. Propellants Explos. Pyrotech. 2017, 42, 864–872. [Google Scholar] [CrossRef] [Scilit]
  54. Li, D.; Wong, L.N.Y. The Brazilian Disc Test for Rock Mechanics Applications: Review and New Insights. Rock Mech. Rock Eng. 2012, 46, 269–287. [Google Scholar] [CrossRef] [Scilit]
  55. Li, Y.; Chen, J.; Wang, S.; Huang, M.; Huang, K. Multi-Scale Research on Mechanical Characteristics of Splitting Fatigue Damage of Asphalt Mixture. J. Chang. Univ. Sci. Technol. (Nat. Sci.) 2022, 12, 81–91. [Google Scholar] [CrossRef]
  56. Kim, Y.R.; Seo, Y.; King, M.; Momen, M. Dynamic Modulus Testing of Asphalt Concrete in Indirect Tension Mode. Transp. Res. Rec. 2004, 1891, 163–173. [Google Scholar] [CrossRef] [Scilit]
  57. Wei, J.; Niu, L.; Song, J.J.; Xie, L. Estimation of Rock Tensile and Compressive Moduli with Brazilian Disc Test. Geomech. Eng. 2019, 19, 353–360. [Google Scholar] [CrossRef]
  58. Lee, H.S. Application of the Viscoelastic Continuum Damage Mechanics to Asphalt Mixtures under Indirect Tensile Load. J. Eng. Mech. 2015, 141, 4014154. [Google Scholar] [CrossRef] [Scilit]
  59. Zhang, X.; Chen, H.; Saba, R.G.; Hannasvik, L.T. Lateral and Longitudinal Variations in Dynamic Modulus of Asphalt Pavement: Surface Layer and Base Layer. Constr. Build. Mater. 2023, 381, 131304. [Google Scholar] [CrossRef] [Scilit]
  60. Lv, S.; Wang, S.; Liu, C.; Zheng, J.; Li, Y.; Peng, X. Synchronous Testing Method for Tension and Compression Moduli of Asphalt Mixture under Dynamic and Static Loading States. J. Mater. Civ. Eng. 2018, 30, 4018268. [Google Scholar] [CrossRef] [Scilit]
  61. Ming, F.; Li, D.; Zhang, M.; Zhang, Y. A Novel Method for Estimating the Elastic Modulus of Frozen Soil. Cold Reg. Sci. Technol. 2017, 141, 1–7. [Google Scholar] [CrossRef] [Scilit]
  62. JTG E42-2005; Test Methods of Aggregate for Highway Engineering. China Communications Press: Beijing, China, 2005.
  63. JTJ 058-2000; Test Methods of Aggregate for Highway Engineering. China Communications Press: Beijing, China, 2000.
  64. JTG F40-2004; Technical Specification for Construction of Highway Asphalt Pavement. Communication Press: Beijing, China, 2004.
  65. Zhao, P.; Shi, S.; Lu, W.; Lv, S.; Chen, Q.; Duan, H.; Yang, Y. Analysis of Strength Size Effect and Failure Mechanism of Asphalt Mixtures based on Discrete Element Method. Case Stud. Constr. Mater. 2024, 21, e03482. [Google Scholar] [CrossRef] [Scilit]
  66. Weibull, W. A Statistical Distribution Function of Wide Applicability. J. Appl. Mech. 1951, 18, 293–297. [Google Scholar] [CrossRef] [Scilit]
  67. Bažant, Z.P. Probability Distribution of Energetic-Statistical Size Effect in Quasibrittle Fracture. Probabilistic Eng. Mech. 2004, 19, 307–319. [Google Scholar] [CrossRef] [Scilit]
  68. Bažant, Z.P.; Yavari, A. Is the Cause of Size Effect on Structural Strength Fractal or Energetic–Statistical? Eng. Fract. Mech. 2005, 72, 1–31. [Google Scholar] [CrossRef]
  69. Carpinteri, A. Fractal Nature of Material Microstructure and Size Effects on Apparent Mechanical Properties. Mech. Mater. 1994, 18, 89–101. [Google Scholar] [CrossRef] [Scilit]
  70. Duan, K.; Hu, X.; Wittmann, F.H. Boundary Effect on Concrete Fracture and Non-Constant Fracture Energy Distribution. Eng. Fract. Mech. 2003, 70, 2257–2268. [Google Scholar] [CrossRef] [Scilit]
  71. Rahimi-Aghdam, S.; Bažant, Z.P.; Cusatis, G. Extended Microprestress-Solidification Theory for Long-Term Creep with Diffusion Size Effect in Concrete at Variable Environment. J. Eng. Mech. 2018, 145, 4018131. [Google Scholar] [CrossRef] [Scilit]
  72. Bažant, Z.P.; Novak, D. Energetic-Statistical Size Effect in Quasibrittle Failure at Crack Initiation. ACI Mater. J. 2000, 97, 381–392. [Google Scholar] [CrossRef] [Scilit]
  73. Bažant, Z.P. Size Effect on Structural Strength: A Review. Arch. Appl. Mech. 1999, 69, 703–725. [Google Scholar] [CrossRef] [Scilit]
  74. Carpinteri, A.; Puzzi, S. The Fractal-Statistical Approach to the Size-Scale Effects on Material Strength and Toughness. Probabilistic Eng. Mech. 2009, 24, 75–83. [Google Scholar] [CrossRef] [Scilit]
  75. Carpinteri, A.; Chiaia, B.; Cornetti, P. On the Mechanics of Quasi-Brittle Materials with a Fractal Microstructure. Eng. Fract. Mech. 2003, 70, 2321–2349. [Google Scholar] [CrossRef] [Scilit]
  76. Carpinteri, A.; Pugno, N. Fractal Fragmentation Theory for size Effects of Quasi-Brittle Materials in Compression. Mag. Concr. Res. 2015, 54, 473–480. [Google Scholar] [CrossRef]
  77. Carpinteri, A.; Ferrara, G.; Imperato, L. Scaling Laws for Strength and Toughness of Disordered Materials: A Unified Theory based on Fractal Geometry. Eng. Fract. Mech. 1994, 48, 673–689. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations