Highlights
- Nano-SiO2 and nano-Al2O3 were applied in alkali-activated ferro-sulphoaluminate cement mortars.
- At 3 d, flexural strength means were 3.79–4.99 MPa and the overall difference was not significant (p = 0.089).
- Activator–binder compatibility should be further investigated in alkali-activated ferro-sulphoaluminate cement systems.
- A high-alkali activator could cause substantial reductions in compressive strength in ferro-sulphoaluminate cement.
Abstract
Ferro-sulphoaluminate cement is a potential precursor for inorganic protective coatings, yet the early-age mechanical response of alkali-activated formulations containing nano-oxide powders remains insufficiently defined. This exploratory study characterized the constituent powders and compared the 3 d flexural and compressive responses of five complete mortar formulations as follows: a non-activated reference, two nano-SiO2 formulations, and two nano-Al2O3 formulations. One independently prepared batch with three replica prisms was tested per formulation. Mean flexural strengths ranged from 3.79 to 4.99 MPa, with no statistically conclusive overall formulation difference (p = 0.089). N0 reached 45.80 MPa in compression, but with the lowest flexural strength, the activated nano-modified formulations had higher flexural strength and retained 46.5%–53.9% of the compressive strength of the N0 mean. Potential activator–binder incompatibility, excessively rapid early reactions, reduced workability, and impaired compaction are literature-supported hypotheses that may help explain this reduction. The high alkalinity of the activator may have contributed to rapid early reactions. Adding nano-additives (nano-SiO2 and nano-Al2O3) only could not modify this reverse effect. Future work should consider using a low-alkali activator and adding a setting retarder in ferro-sulphoaluminate cement. This study provides an early-stage dataset and further in situ validation and long-term performance testing must be performed in the future to evaluate adhesion, permeability, and durability properties.
1. Introduction
Chloride deicers such as sodium chloride (NaCl), calcium chloride (CaCl2), and magnesium chloride (MgCl2) accelerate concrete deterioration in cold regions through coupled physical and chemical processes, including freeze–thaw scaling, salt crystallization, and, for CaCl2 and MgCl2, calcium oxychloride formation [1,2]. The resulting damage and cracking can increase transport pathways for chloride-bearing water; corrosion may initiate when the chloride concentration at the reinforcement exceeds a critical threshold [1,3]. Surface treatments are therefore used to reduce water and chloride ingress and extend service life [4,5].
Cementitious coatings form a low-permeability layer on concrete and are used for both surface protection and repair [6]. Their effectiveness depends on adhesion and compatibility with the substrate; mismatches in stiffness, shrinkage, or thermal movement can concentrate interfacial stress and promote debonding [7,8]. Barrier performance must therefore be considered together with mechanical and dimensional compatibility.
The binder was commercially designated as ferro-sulphoaluminate cement (R·FAC 42.5). Its original material-inspection record reported CaO 45.30 wt.%, Al2O3 18.60 wt.%, SO3 12.50 wt.%, SiO2 7.23 wt.%, Fe2O3 4.30 wt.%, MgO 1.35 wt.%, TiO2 0.87 wt.%, and loss on ignition 10.05 wt.%; qualitative XRD indicated ye’elimite, ferrite/brownmillerite, β-belite, gypsum, calcite, and minor quartz, although clinker-phase fractions were not quantified. In related calcium sulfoaluminate and ferro-sulphoaluminate cements, aluminate and ferrite reactions with sulfate produce ettringite and Al/Fe hydroxide gels, supporting rapid hardening and, for ferro-sulphoaluminate cement, a dense matrix with low permeability [9,10,11]. These features motivated the present coating-mortar study, while the unquantified clinker assemblage limits direct phase-level interpretation.
Alkali activation can redirect, rather than simply accelerate, hydration in aluminate-rich cements. In calcium aluminate cement, highly alkaline NaOH favors C3AH6, whereas soluble silicate promotes Si-bearing katoite and an alkali aluminosilicate hydrate [12]. In calcium sulfoaluminate cement, 0.1–1 M NaOH accelerates ettringite–AH3 formation, but 4–8 M NaOH destabilizes or suppresses ettringite and promotes U-phase, with lower strength [13]. Sodium silicate can additionally promote strätlingite [14], while pH alters the crystallinity and morphology of Fe-bearing (A/F)H3 phases [15]. These observations identify alkalinity and soluble-silicate supply as plausible controls on hydrate selection in ferro-sulphoaluminate cement. Ferro-sulphoaluminate cement contains rapidly reacting aluminate-bearing phases, including qualitatively identified ye’elimite (C4A3), which contributes to rapid setting and early strength development. Introducing NaOH and sodium silicate into this binder may further accelerate aluminate dissolution and alter hydrate precipitation. If these reactions proceed excessively rapidly, the workable period may be shortened before adequate placement and compaction are completed, potentially producing entrapped air, capillary voids, and spatially heterogeneous hardened regions. Activator alkalinity and compatibility with the rapidly reacting binder must therefore be controlled carefully [9,10,11,12,13,14,15].
Previous studies show that nano-SiO2 and nano-Al2O3 can alter mechanical, rheological, and transport-related properties, but the response varies with binder composition and dosage [16,17]. Nano-SiO2 can accelerate C3S dissolution and C–S–H formation [18], whereas nano-Al2O3 can modify aluminate reactions and promote microstructural densification in Portland and calcium aluminate cements [19,20,21]. These effects depend on dispersion: agglomerates can create weak zones, and the mixing sequence can alter particle distribution and hardening [22,23,24]. Comparable alkali-activated mortar studies involve other precursor and reinforcement systems [25]; the relative response of these nanoparticles under identical conditions in alkali-activated ferro-sulphoaluminate cement coating mortars therefore remains unresolved.
Accordingly, this study characterized the available constituent-powder properties and compared the 3 d flexural and compressive responses of five complete formulations containing nano-SiO2 or a nano-Al2O3 product. The present scope was limited to early-age mechanical evaluation; coating-specific adhesion, transport, and long-term durability were not measured. The objectives were to (i) document the available raw-material characteristics, (ii) compare mixture-level early-age mechanical performance under the project mixing protocol, and (iii) identify a priority formulation for subsequent coating-specific evaluation. The working hypothesis was that nano-oxide chemistry and dosage would differentially affect heterogeneous nucleation and matrix densification, thereby modifying reaction-product development and early-age mechanical performance under the project formulation conditions.
2. Materials and Methods
2.1. Experimental Design and Variables
Five mortar formulations were prepared to compare the 3 d mechanical strengths of complete mortar formulations containing two nano-oxide products at two nominal addition levels. N0 was a non-activated, nanoparticle-free reference. S1 and S2 contained nano-SiO2 at 2.0% and 4.0% of cement mass, respectively, whereas A1 and A2 contained the nominal nano-Al2O3 product at the same addition levels. GB/T 17671-2021 [26] specifies a reference cement:sand:water mass ratio of 1:3:0.5; because the present work evaluated non-standard alkali-activated, nano-oxide-modified mortars, the nominal deionized-water-to-cement ratio was set to 0.42 for all formulations.
No matched alkali-activated, nanoparticle-free control was included; N0 therefore served only as a non-activated reference, and comparisons with N0 cannot isolate the effects of alkali activation or nano-oxide addition. Within the activated series, nano-oxide product and nominal dosage were the intended formulation variables, while water-reducer dosage varied with nano-oxide dosage. Consequently, S1–S2 and A1–A2 are complete-formulation contrasts rather than isolated dosage effects, whereas S1–A1 and S2–A2 compare nano-oxide product type at matched nominal nano-oxide and water-reducer dosages. The other formulation components and experimental conditions were kept constant within the activated series. Formulation identity was the categorical grouping variable, and the response variables were 3 d flexural and compressive strengths.
2.2. Raw Materials
The binder was a gray powder commercially designated as ferro-sulphoaluminate cement (R·FAC 42.5) and supplied through Jiuqi Building Materials (Weifang, China). The material was manufactured and inspected before the implementation of GB/T 45920—2025 [27], and the original record cites GB/T 20472—2006 [28] as the applicable production and inspection standard. Accordingly, R·FAC 42.5 is reported as the documented product designation and conformity with GB/T 45920—2025 [27] is not claimed. The chemical composition recorded in the original material-inspection documentation was CaO 45.30 wt.%, Al2O3 18.60 wt.%, SO3 12.50 wt.%, SiO2 7.23 wt.%, Fe2O3 4.30 wt.%, MgO 1.35 wt.%, TiO2 0.87 wt.%, and loss on ignition 10.05 wt.%. For terminology, GB/T 45920—2025 [27] defines ferro-sulphoaluminate clinker as being mainly composed of ye’elimite (C4A3Ŝ), ferrite (C4AF), and belite (C2S). This general definition is not used to assign batch-specific clinker-phase fractions.
Deionized water was used as mixing water. China ISO Standard Sand (Xiamen ISO Standard Sand Co., Ltd., Xiamen, China; particle-size range: 0.08–2.00 mm) was used as the standardized fine aggregate. The material was supplied in accordance with GB/T 17671-2021 [26], a modified adoption of ISO 679:2009 [29] and was associated with the Chinese national reference-material specification GSB 08-1337 [30]. The standard-specified cumulative sieve residues at 2.00, 1.60, 1.00, 0.50, 0.16, and 0.08 mm were 0%, 7 ± 5%, 33 ± 5%, 67 ± 5%, 87 ± 5%, and 99 ± 1%, respectively, and the specified moisture content was below 0.2%.
The nano-SiO2 and nano-Al2O3 powders were Chuangshi-brand products purchased from Zancheng (Tianjin) Technology Co., Ltd. (Tianjin, China). The nano-SiO2 product (AI04666; CAS 60676-86-0) had a supplier-declared purity of 99.5% and a nominal particle size of 30 ± 5 nm. The nano-Al2O3 product (MJ10933; CAS 1344-28-1) was specified as 99.99% metals basis, γ phase, with a nominal particle size of 20 nm. No target mortar-flow value or formulation-specific flow result was recorded; the PCE dosage was prescribed by formulation.
Sodium hydroxide (Energy Chemical, Anhui Zesheng Technology Co., Ltd., Anqing, China; W810069; CAS 1310-73-2; ACS reagent, ≥99%) and powdered sodium silicate (Acmec, Shanghai Acmec Biochemical Technology Co., Ltd., Shanghai, China; S95590-500g; CAS 1344-09-8) were used as dry alkali-activator precursors. The sodium silicate product was catalog-specified as containing 18% Na2O and 60% SiO2. No aqueous sodium silicate/NaOH activator solution was prepared.
The water reducer was DFTR-PCE, a standard-type liquid polycarboxylate high-performance water-reducing admixture manufactured by Sichuan Dongrun Xinsheng FRP Technology Co., Ltd. (Changzhi, China). It was dosed by mass as received. A manufacturer-provided release report for the same product model listed a solid content of 20.1%, a pH of 6.4, and a density of 1.025 g/cm3.
2.3. Raw-Material Characterization
Raw-material characterization was based on the available product specifications, original material-inspection records, BET (N2) surface-area records, XRF oxide data, and qualitative XRD patterns.
2.3.1. Particle-Size Distribution
The particle-size distribution of China ISO standard sand was specified by the supplier and GB/T 17671-2021 [26]. The standard-specified cumulative sieve residues at 2.00, 1.60, 1.00, 0.50, 0.16, and 0.08 mm were 0%, 7 ± 5%, 33 ± 5%, 67 ± 5%, 87 ± 5%, and 99 ± 1%, respectively. The nano-SiO2 and nano-Al2O3 products had supplier-declared nominal particle sizes of 30 ± 5 nm and 20 nm, respectively.
2.3.2. Nitrogen-Adsorption Specific Surface Area
Specific surface area was measured by N2 physisorption using an SI-MP analyzer (Quantachrome Instruments, Boynton Beach, FL, USA) following the BET framework of ISO 9277:2022 [31]. Approximately 2.0 g of dry powder was vacuum-degassed at 40 °C for 24 h, and adsorption data were collected at −195.8 °C. BET fitting used the recorded linear region, nominally P/P0 = 0.05–0.30, and 0.162 nm2 as the N2 molecular cross-sectional area. Table 1 reports the available descriptive BET (N2) values.
Table 1.
BET (N2) specific surface areas of the raw materials (descriptive values).
2.3.3. X-Ray Fluorescence
For XRF, powders were ground to pass a 75 μm sieve and pressed into 32 mm pellets. Major oxides were measured using an ARL PERFORM’X wavelength-dispersive XRF spectrometer (Thermo Fisher Scientific, Waltham, MA, USA) under vacuum at 45 kV and 100 mA, with the available calibration record referencing NIST SRM 1880a [32] and Compton-scattering matrix correction.
2.3.4. X-Ray Diffraction
For XRD, raw powders were gently ground, back-loaded, and scanned with a Rigaku MiniFlex diffractometer (Rigaku Corporation, Akishima, Tokyo, Japan) using Cu Kα radiation (40 kV, 15 mA; 5–70° 2θ; 0.02° step; 2°/min). Jade 9.5 and the ICDD PDF-4+ 2023 database were used for qualitative identification. The available raw-powder patterns indicated ye’elimite, ferrite/brownmillerite, β-belite, gypsum, calcite, and minor quartz in the cement, quartz in the sand, γ-Al2O3 in the alumina-rich product, and a broad diffuse feature consistent with amorphous silica in the nano-SiO2 powder. The available records did not include divergence-slit configuration, sample rotation, Kβ-filter or monochromator details, instrumental-broadening data, PDF card numbers, or background-treatment parameters. No internal standard, Rietveld quantification, amorphous-content measurement, or hardened-specimen XRD was performed; the scans therefore cannot establish clinker-phase fractions, hydrate formation, or phase–strength links.
2.4. Activator Preparation
For each activated three-prism batch, 31.802 g powdered sodium silicate and 18.198 g solid NaOH were weighed as dry activator precursors, giving a total dry activator mass of 50.000 g and a powdered sodium silicate/NaOH mass ratio of 1.748:1. The dry activator-to-cement ratio was 10.0%. Based on the catalog-specified sodium silicate composition and the declared 99% NaOH purity basis, the dry activator provided 19.683 g Na2O equivalent and 19.081 g SiO2 per 500 g cement, corresponding to 3.937 wt.% Na2O and 3.816 wt.% SiO2 relative to cement. The silicate modulus was defined on a molar basis as Ms = n(SiO2)/n(Na2O) = 1.00. Because both precursors were added as solids, aqueous-activator concentration, solution density, solution solids content, and solution aging, cooling, or equilibration time are not applicable.
2.5. Mixture Proportions and Liquid Balance
Every three-prism batch contained 500 g cement, 1500 g standard sand, and 210 g deionized water. The dry activator was used only in S1, S2, A1, and A2. The PCE (Polycarboxylate ether) water reducer was dosed as received at 5, 10, or 15 g per batch. Its reported solid content was 20.1%; therefore, the PCE-derived water was calculated as 79.9% of its as-received mass. The nominal deionized-water-to-cement ratio was 0.420 for all mixtures. Total liquid-to-cement ratio was calculated from the deionized water plus the as-received liquid PCE mass, whereas effective water-to-cement ratio was calculated from the deionized water plus PCE-derived water. The dry activator was excluded from both liquid numerators. The resulting water inputs and liquid-balance calculations are summarized in Table 2. The dry-activator, PCE, and nano-oxide dosages for each formulation are summarized in Table 3.
Table 2.
Water inputs and liquid-balance calculations for three-prism batches.
Table 3.
Dry-activator, PCE, and nano-oxide dosages for three-prism batches.
2.6. Specimen Preparation and Curing
For each formulation, one batch was prepared and cast in a three-gang 40 mm × 40 mm × 160 mm prism mold. Standard sand was placed in the mortar mixer first, followed by ferro-sulphoaluminate cement and, where applicable, the nano-SiO2 or nano-Al2O3 powder and dry activator precursors. Deionized water and the liquid PCE water reducer were then added. The original laboratory record did not retain the mixer model or a rotational-speed calibration. For reference, the low- and high-speed categories for the planetary mortar mixer specified through GB/T 17671-2021 [26] are blade self-rotation/orbital rotation of 140 ± 5/62 ± 5 r/min.
The nano-oxide powders were added dry without ultrasonic, high-shear, or chemical pre-dispersion. To maximize the practicable in-mixer blending time for these powders, mixing was continued for at least 5 min in total, exceeding the 240 s mixing schedule in GB/T 17671-2021 [26]. The exact duration at each speed was not recorded.
Fresh mortar was placed in the three-gang mold in two layers and compacted using the same jolting procedure for every formulation. The reference procedure in GB/T 17671-2021 [26] specifies 60 jolts for each of two layers. After compaction, the specimen surfaces were leveled and the molds were covered to limit moisture loss.
The specimens were demolded after 24 h and kept in a standard curing room at 20 ± 1 °C and relative humidity of at least 95% until the nominal 3 d test age. This curing condition is reported as an adaptation: GB/T 17671-2021 [26] uses 24 h moist curing in the mold followed by water curing at 20 ± 1 °C, whereas the present records document room curing rather than water curing.
2.7. Mechanical Testing
Mechanical testing used the 40 mm × 40 mm × 160 mm prism geometry and test configuration in GB/T 17671-2021 [26] as an adapted reference. Flexural and compressive failure loads were recorded using a TONI NORM 2000 electro-hydraulic servo testing system (Toni Technik Baustoffprüfsysteme GmbH, Berlin, Germany) equipped with separate flexural and compression testing units. The load-measurement accuracy class was ±1%. Each prism was tested first in three-point bending with an 80 mm support span. The two retained half-prisms were then tested in compression through 40 mm × 40 mm platens (loaded area = 1600 mm2), provided that the loading region was intact.
For the recorded center-point three-point-bending configuration, flexural strength, Rf (MPa), was calculated for each parent prism as Rf = 3FfL/(2bd2) [26], where Ff is the peak flexural load (N), L = 80 mm is the support span, and b = d = 40 mm are the specimen width and depth. For Ff expressed in kN, this reduces to Rf = 1.875Ff. Compressive strength, Rc (MPa), was calculated for each tested half-prism as Rc = Fc/A [26], where Fc is the peak compressive load (N) and A = 1600 mm2. For Fc expressed in kN, Rc = 0.625Fc.
In accordance with the respective GB/T 17671-2021 [26] loading provisions, flexural loading was applied at 50 ± 10 N/s until fracture, whereas compressive loading was applied at 2400 ± 200 N/s until failure. Thus, the flexural and compressive tests used different load rates as required by the reference method.
Three parent prisms were tested for each formulation (flexural n = 3). For compression, one suitable half-prism from each parent was available for N0 and S1 (three recorded half-prism results per formulation); both half-prisms were suitable for S2, A1, and A2 (six recorded half-prism results per formulation). For S2, A1, and A2, the two half-prism results from the same parent prism were averaged before group-level analysis. Accordingly, the parent prism was the within-batch observational unit for both strength outcomes (n = 3 per formulation), whereas the mortar batch was the experimental unit.
2.8. Statistical Analysis
The formulation treatment was applied at the mortar-batch level; therefore, an independently prepared mortar batch constituted the experimental unit for formulation-level inference. Only one batch was prepared for each formulation. The three parent prisms cast from that batch were within-batch observational units, not independent formulation replicates. Parent-level flexural and compressive values were constructed as described in Section 2.7, including within-parent averaging of paired compression subsamples. Thus, each formulation was summarized using three parent-level observations.
All supplied individual parent-prism flexural values, half-prism compressive values, and derived parent-level compressive values are reported in Table 4 and were retained in the analysis dataset for distributional reporting. Results were summarized as the arithmetic mean ± sample standard deviation (SD) across the three parent-level observations. Two-sided 95% confidence intervals (CIs) were calculated as follows: . With n = 3, these intervals describe uncertainty among specimens within the tested batch and are not precise CIs for a formulation population. Formal normality, variance-homogeneity, and outlier tests were not used to claim that distributional assumptions had been established.
Table 4.
Individual specimen-level mechanical-strength data (MPa).
Statistical analyses were performed in Python 3.12.13 using NumPy 2.5.2, SciPy 1.18.0, pandas 3.0.5, statsmodels 0.14.6, and Pingouin 0.6.1. Overall differences among the five observed formulation batches were examined using Welch’s one-way analysis of variance (statsmodels.stats.oneway.anova_oneway; use_var = “unequal”, welch_correction = True, trim_frac = 0). When the omnibus test yielded p < 0.05, Games–Howell pairwise comparisons were performed using pingouin.pairwise_gameshowell. A nominal two-sided α = 0.05 was used. Unstandardized differences between formulation means, expressed in MPa, were the primary effect-size measures. As a secondary omnibus standardized measure, Welch-compatible squared Cohen’s f (fW2) was calculated using , , and . The calculation was implemented with statsmodels.stats.oneway.effectsize_oneway using use_var = “unequal” and ddof_between = 0. Conventional η2 was not reported. Because each group variance was estimated from three observations, fW2 was treated as descriptive and was not interpreted using fixed magnitude thresholds.
Because each formulation was represented by a single independently prepared batch, between-batch variability could not be estimated. The CIs, Welch ANOVA, Games–Howell, and effect-size outputs were therefore interpreted strictly as exploratory, conditional descriptions of the five tested batches; they do not establish reproducible, population-level, or causal formulation effects. Formulation contrasts were interpreted according to the component confounding defined in Section 2.1. The individual specimen-level mechanical-strength data underlying these analyses are listed in Table 4.
2.9. Candidate-Screening Procedure
Candidate status was assigned using a two-stage screening procedure. First, the activated formulations were jointly compared using their corrected mean flexural and compressive strengths. Formulations that were not outperformed by another activated formulation in both responses were retained as priority candidates. This hierarchy reflected the project priority of maintaining the observed compressive-strength level while favoring the higher flexural response for subsequent coating evaluation. The procedure was used only to reduce the candidate set and was not interpreted as evidence of statistical superiority or coating qualification.
3. Results and Discussion
3.1. Raw-Material Chemistry and Mineralogy
The BET (N2) specific surface areas of nano-Al2O3 and nano-SiO2 were 136.47 and 123.37 m2/g, respectively, substantially higher than those of the ferro-sulphoaluminate cement (0.94 m2/g) and quartz sand (0.02 m2/g). These values demonstrate a pronounced difference in the gas-accessible surface areas of the dry powders and indicate that the nano-oxides potentially provide greater interfacial area for adsorption and heterogeneous nucleation. However, BET surface area alone does not establish nucleation efficiency in the cement pore solution. According to ISO 9277:2022, BET analysis determines the overall gas-accessible external and internal surface area of dispersed or porous solids [31], but it does not quantify particle dispersion, agglomeration, water-reducer adsorption, water demand, or chemical reactivity in mortar. Because the nano-oxides were added without ultrasonic or high-shear pre-dispersion, the effective surface available after contact with the alkaline pore solution would depend strongly on their dispersion and agglomeration state. The BET results are therefore interpreted as descriptive dry-powder properties rather than direct evidence of enhanced nucleation behavior or increased mortar water demand.
The available laboratory XRF result for the nano-SiO2 powder was 96.84 wt.% SiO2, confirming its silica-rich composition. The cement composition used in this manuscript is taken from the original material-inspection documentation reported in Section 2.2; the earlier laboratory cement-XRF values were not retained because their representativeness for the tested batch could not be verified. An initial XRF measurement of the nano-Al2O3 powder returned 89.68 wt.% Al2O3 and 9.39 wt.% CaO. This apparent CaO content conflicted with the rechecked product documentation, which specified the purchased powder as 99.99% metals-basis γ-Al2O3, and it was not supported by the qualitative XRD pattern. Because repeat XRF verification was unavailable, the origin of the discrepancy could not be confirmed. The value is therefore reported as unresolved, is not assumed to be an analytical error, and is excluded from mechanistic interpretation of A1 and A2. The material is identified according to the supplier specification and qualitative XRD as nano-γ-Al2O3, while the unresolved XRF discrepancy remains a raw-material-characterization limitation.
The qualitative XRD patterns further distinguished the mineralogical characteristics of the raw materials (Figure 1). The cement pattern was consistent with the principal clinker phases expected in ferro-sulphoaluminate cement as follows: ye’elimite (Y, C4A3Ŝ; PDF 33-0256), ferrite/brownmillerite (F, C4AF; PDF 30-0226), and β-belite (B, C2S; PDF 33-0302). Gypsum (G; PDF 33-0311), calcite (Cc; PDF 05-0586), and minor quartz (Q; PDF 46-1045) were also identified. The reflection near 11.6° 2θ was assigned to gypsum, while features near approximately 23.4° and 30.9° were consistent with ye’elimite. The intense region between approximately 29° and 34° contained overlapping contributions from calcite and the principal clinker phases and was therefore not assigned to a single phase. Reflections near approximately 41.2° and 51.7° were consistent with contributions from belite and/or ferrite.
Figure 1.
Qualitative XRD patterns of the raw powders.
The standard-sand pattern was dominated by α-quartz, with representative experimental reflections at approximately 20.7°, 26.3°, 36.5°, 42.3°, 50.0°, 59.8°, and 67.9° 2θ. The nano-Al2O3 pattern exhibited broadened reflections near 32.5°, 36.8°, 39.2°, 45.3°, 60.8°, and 66.9° 2θ, consistent with nanocrystalline γ-Al2O3 (PDF 10-0425). No distinct crystalline Ca-bearing phase was resolved. The nano-SiO2 pattern contained a broad diffuse band extending from approximately 18° to 29° 2θ and centered near 22.5°, consistent with predominantly amorphous SiO2 (PDF 29-0085). Because this diffuse feature represents short-range structural order rather than a discrete Bragg reflection, no crystallographic plane index was assigned. The revised Figure 1 and its reference-card list already reflect these identifications.
The raw-material characterization nevertheless has several limitations. The available BET and XRF results were descriptive measurements without replicate analyses or reported measurement uncertainty. Dispersion, agglomeration, zeta potential, water-reducer adsorption, formulation-specific water demand, and nanoparticle dissolution were not measured in water, activator solution, or simulated pore solution. Although the anomalous CaO result for nano-Al2O3 was inconsistent with both the verified product specification and qualitative XRD identification, repeat XRF analysis of the retained powder was unavailable; its origin therefore could not be experimentally confirmed. In addition, the XRD analysis was qualitative and did not include an internal standard, Rietveld refinement, amorphous-content quantification, or instrumental-broadening correction. No XRD or complementary phase analysis was conducted on the hardened mortars. The available results therefore establish the principal dry-powder chemistry, gas-accessible surface-area contrast, and qualitative phase assemblages, but they do not establish effective nanoparticle dispersion, nucleation efficiency, quantitative clinker-phase fractions, hydration-product formation, or causal phase–strength relationships.
3.2. Mechanical Performance
3.2.1. Flexural Strength
At 3 d, the mean flexural strengths of N0, S1, S2, A1, and A2 were 3.81, 3.79, 4.99, 4.46, and 4.60 MPa, respectively (Table 5 and Figure 2). N0 and S1 showed nearly identical mean values, whereas S2 exhibited the highest numerical mean, followed by A2 and A1. Relative to N0, the mean values of S2, A1, and A2 were numerically higher by 30.8%, 17.0%, and 20.7%, respectively. Within the activated nano-SiO2 series, S2 was 31.7% higher than S1, whereas the numerical separation between A2 and A1 was comparatively small. The parent-prism-level flexural and compressive distributions underlying this ordering are shown in Figure 2.
Table 5.
Integrated evaluation of the activated formulations using corrected 3 d mechanical-strength means.
Figure 2.
(a) Parent-prism-level flexural strength; (b) parent-prism-level compressive strength. Colored circles show the three individual observations for each formulation; black diamonds and whiskers show the mean and two-sided t-based 95% confidence interval (n = 3).
Despite this separation among the observed means, the exploratory Welch ANOVA did not provide statistically conclusive evidence of an overall formulation difference (F(4, 4.22) = 4.25, p = 0.089). This result should not be interpreted as demonstrating equivalent flexural performance among the formulations. Rather, the tested specimens showed appreciable numerical separation, but the small number of parent-prism observations and the associated uncertainty prevented a conclusive formulation-level inference. Accordingly, the higher means observed for S2, A1, and A2 are treated as numerical trends rather than confirmed improvements. The individual observations, confidence intervals, and implications of the limited replication are examined further in Section 3.2.3.
The percentage differences relative to N0 describe contrasts between complete formulations rather than isolated nanoparticle effects because N0 contained neither the dry activator nor nano-oxide and also had a lower PCE dosage. Similarly, S1–S2 and A1–A2 represent within-matrix formulation contrasts, not pure nano-oxide dosage effects, because both the nominal nano-oxide content and PCE dosage changed between the paired formulations. Therefore, the results support only a provisional within-study ordering under the tested formulation and mixing conditions.
3.2.2. Compressive Strength
The dominant compressive-strength result was the substantial reduction associated with the tested activated nano-modified formulations. As shown in Figure 2, the 3 d compressive strength decreased from 45.80 MPa for the conventional reference N0 to 21.30–24.67 MPa for S1, S2, A1, and A2. The activated nano-modified mixtures therefore retained only 46.5%–53.9% of the N0 strength, corresponding to reductions of approximately 46.1%–53.5%. This loss was considerably greater than the differences observed among the four activated formulations and should consequently be regarded as the principal mechanical finding. Under the investigated mixture proportions and curing conditions, the activation/nanoparticle strategy did not improve early-age compressive strength relative to the non-activated ferro-sulphoaluminate cement reference.
Among the activated formulations, A2 exhibited the highest mean compressive strength of 24.67 MPa, whereas S1 showed the lowest value of 21.30 MPa. The difference of approximately 3.37 MPa between A2 and S1 was statistically significant in the exploratory Games–Howell comparison. However, this contrast does not isolate the effect of nanoparticle chemistry or demonstrate that nano-Al2O3 was superior to nano-SiO2. A2 and S1 differed simultaneously in nanoparticle type, nanoparticle dosage, polycarboxylate superplasticizer dosage, and potentially effective liquid balance, particle packing, and water demand. The observed difference should therefore be interpreted only as a formulation-level contrast within the present dataset. Isolating the influence of nanoparticle chemistry would require comparisons at identical nanoparticle contents, matched workability or water-reducer dosage, and inclusion of an activated control without nanoparticles.
The engineering significance of these results must also be distinguished from their statistical significance. GB 18445-2012 [33] specified a minimum compressive strength of 15.0 MPa at 28 d for cementitious capillary crystalline waterproofing coatings, but it did not provide a 3 d compressive-strength acceptance criterion. The measured values of 21.30–24.67 MPa were numerically higher than this 15.0 MPa benchmark; however, the different test ages and material/test scope prevent these results from being treated as direct evidence of standards compliance. This legacy benchmark is retained only as historical context.
Activator–binder incompatibility is considered a literature-supported hypothesis for the pronounced compressive-strength reduction observed in the activated formulations relative to the non-activated reference N0. The ferro-sulphoaluminate cement contained a high amount of ye’elimite and other rapidly reacting aluminate- and ferrite-bearing phases, whereas the activator had a high alkali content and no set retarder was added in these mixes. Dissolution of the dry activator may therefore have generated a high-pH early-reaction environment that accelerated aluminate dissolution and hydrate precipitation. Excessively rapid reactions may have produced flash-set-like behavior, shortened the workable period, and impaired placement and compaction, leaving more pores and heterogeneous regions in the hardened mortar. High alkalinity may also have altered ettringite stability and promoted alternative aluminate- or aluminosilicate-bearing products with a less favorable microstructure [13]. Adding nano-SiO2 or nano-Al2O3 only could not modify this reverse effect. However, this mechanism remains unverified because setting time, fresh-state behavior, calorimetry, compaction quality, hardened-phase assemblage, and pore structure were not measured.
Differences in effective water content, PCE dosage, nanoparticle agglomeration, entrapped air extent, shrinkage, and microcracking may have contributed additional effects. Nevertheless, the present study did not measure setting time, mortar flow, calorimetry, air content, compaction quality, hardened-phase assemblage, or pore structure. The results therefore identify excessively rapid activation as the leading hypothesis, but they do not demonstrate that flash setting occurred or establish the governing physicochemical mechanism.
The unusually small variation recorded for A2 (24.67 ± 0.34 MPa; coefficient of variation approximately 1.4%) was verified using the three parent-prism averages, and no observations were removed. Nevertheless, this low dispersion represents the behavior of a single experimental batch with limited replication and should not be generalized as evidence of inherently stable performance.
3.2.3. Statistical Uncertainty and Raw-Data Distribution
The mechanical results should be interpreted in light of the limited number of independent observations. Each formulation was represented by three parent-prism values (n = 3). For compressive strength, the results obtained from the two broken halves of each prism were averaged before statistical analysis; thus, the two halves were treated as technical measurements of the same parent specimen rather than as independent replicates. All parent-level values were retained, and no observations were excluded. The complete raw data are provided in Table 4 and are displayed individually in Figure 2 to avoid concealing the within-group distributions behind the reported means and standard deviations.
Because only three independent observations were available per formulation, the estimated group means and variances were highly sensitive to individual specimens. The corresponding two-sided, t-based 95% confidence intervals were therefore wide for groups with appreciable dispersion and should not be interpreted as precise estimates of the population means. Conversely, a narrow interval for one group does not necessarily demonstrate reproducible material performance. For example, A2 exhibited a compressive strength of 24.67 ± 0.34 MPa, corresponding to a coefficient of variation of approximately 1.4%. Rechecking the three parent-prism averages confirmed the reported mean and sample standard deviation, and no value had been removed. Nevertheless, this unusually low variability was obtained from specimens produced within the same experimental batch and is not generalized beyond the present dataset.
The small sample size also prevented meaningful assessment of normality and other distributional assumptions. Formal normality tests have very low diagnostic power at n = 3, whereas visual inspection of such small groups cannot reliably establish an underlying distribution. Welch’s ANOVA was therefore used to reduce sensitivity to unequal variances, but its results remain dependent on the limited replication and observed group dispersions. The inferential analyses are consequently treated as exploratory rather than confirmatory.
For flexural strength, Welch’s ANOVA indicated no statistically conclusive overall group effect (p = 0.089). The appreciable numerical separation among the observed means and the nonsignificant p-value are not contradictory: the former describes the tested specimens, whereas the latter reflects the wide uncertainty arising from low replication and within-group variation. The result is therefore not summarized as evidence of equivalence or of “no difference.” Instead, the observed separation is reported as an exploratory trend whose reproducibility cannot be established from one batch and three parent-prism observations per formulation. Conventional eta-squared is not used to support the magnitude of the effect.
For compressive strength, the statistical comparison among the activated formulations must be considered secondary to the much larger reduction relative to N0. Although the exploratory Games–Howell analysis identified a significant difference between A2 and S1, the contrast may have been influenced partly by the very small within-group variance of A2. In addition, the two formulations differed simultaneously in nanoparticle chemistry, nanoparticle content, water-reducer dosage, and liquid balance. The statistical result therefore establishes only that the observed formulation means differed within this dataset; it does not isolate a causal effect of nanoparticle type or dosage.
Taken together, the raw-data distributions support two levels of interpretation. First, the reduction in compressive strength from 45.80 MPa for N0 to 21.30–24.67 MPa for the activated nano-modified mixtures was large and consistent in magnitude, making it the dominant mechanical result. Second, the smaller differences among S1, S2, A1, and A2 remain uncertain because they were derived from only three parent specimens per formulation and from mixtures in which several compositional factors changed simultaneously. Accordingly, means, sample standard deviations, confidence intervals, effect sizes, and individual observations are reported together, while statistical significance is not treated as proof of engineering importance or mechanistic causation. Additional independently prepared batches and greater parent-level replication are required to confirm the observed rankings and obtain more stable estimates of formulation variability.
3.3. Integrated Candidate Evaluation
The corrected 3 d strength results were used to identify the formulation to be carried forward for coating-specific evaluation. Among the activated formulations, S2 had the highest flexural-strength mean of 4.99 MPa, whereas A2 had the highest compressive-strength mean of 24.67 MPa. The corresponding values were 23.95 MPa in compression for S2 and 4.60 MPa in flexure for A2. Thus, S2 exceeded A2 by 0.39 MPa in flexure, while A2 exceeded S2 by 0.72 MPa in compression. The exploratory comparisons did not detect a significant difference between these formulations in either response. The results therefore do not establish S2 as mechanically superior to A2.
The two-stage candidate-evaluation procedure described in Section 2.9 was then applied. In the combined flexural–compressive comparison, S2 and A2 were retained as the priority candidates because neither formulation outperformed the other in both responses. S2 provided the highest flexural response but a slightly lower compressive response, whereas A2 provided the highest activated-series compressive response but a lower flexural response. In descriptive terms, S2 retained 97.1% of the A2 compressive-strength mean, while A2 retained 92.2% of the S2 flexural-strength mean. S1 and A1 were not retained because their combined mechanical responses were lower than those of the two priority candidates.
Only one formulation could be carried forward because the available material and subsequent experimental scope did not permit parallel coating-evaluation programs. Under the stated screening hierarchy, the corrected flexural-strength mean was therefore used as the final ranking criterion after the exploratory analysis showed no compressive-strength separation between S2 and A2. S2 was provisionally selected because it had the highest flexural-strength mean while maintaining a compressive-strength mean close to the activated-series maximum. A2 nevertheless remains a credible alternative candidate, particularly because it represents a different nano-oxide pathway. The selection of S2 is therefore an operational decision for the next experimental stage rather than evidence that it is statistically or generally superior to A2. The resulting mechanical-strength comparison and provisional candidate selection are illustrated in Figure 3.
Figure 3.
Mechanical-strength comparison used for candidate evaluation.
This selection does not constitute coating qualification. The present screening was based only on 3 d flexural and compressive strengths from one batch per formulation. Qualification for protective-coating application remains pending until independently prepared batches are assessed using predefined requirements for pull-off adhesion, interfacial integrity, shrinkage and cracking, permeability or sorptivity, chloride transport, water resistance, freeze–thaw stability, abrasion or scrub resistance, application properties, and longer-term durability.
3.4. Possible Origins of the Mechanical Response
The dominant mechanical observation was the reduction in compressive strength from 45.80 MPa for N0 to 21.30–24.67 MPa for the four activated nano-modified formulations. By contrast, the flexural-strength means ranged from 3.79 to 4.99 MPa, and the overall formulation effect was not statistically conclusive. These results describe the performance of the complete formulations rather than isolated effects of nano-SiO2 or nano-Al2O3. N0 contained neither the dry activator nor nano-oxide and also had a lower PCE dosage, while only one independently prepared batch was available for each formulation. The possible origins discussed below must therefore be treated as competing hypotheses rather than experimentally established mechanisms. The competing hypotheses discussed below are summarized schematically in Figure 4.
Figure 4.
Hypothesized mechanism for the flexural improvement and compressive-strength limitation.
Activator–binder compatibility is one possible contributor to the observed mechanical response. The activated formulations contained a dry sodium-silicate/NaOH activator at 10.0% of cement mass, with a powdered sodium-silicate/NaOH mass ratio of 1.748:1 and a molar silicate modulus of 1.00. Based on the declared precursor compositions, the activator supplied 3.937 wt.% Na2O equivalent and 3.816 wt.% SiO2 relative to cement. External alkali addition is not mechanically neutral in cementitious binders. In Portland-cement systems, increasing the alkali content by adding NaOH has been reported to reduce compressive, splitting-tensile, direct-tensile, and flexural strengths [34], while the addition of 2–4 wt.% Na2CO3 reduced compressive and flexural strengths and increased porosity relative to the corresponding water-mixed control [35]. NaOH may accelerate very early hydration, but elevated alkalinity can also modify the subsequent hydration process and paste microstructure [36]. More directly relevant to the present aluminate-rich binder, calcium sulfoaluminate clinker hydrated with water and NaOH solutions showed concentration-dependent changes in strength development and hydrate assemblage; at high alkalinity, ettringite was suppressed and alternative products were formed [37]. These findings demonstrate that the alkaline activator itself can materially influence mechanical performance. Therefore, the 46.1%–53.5% compressive-strength reduction measured in the present study cannot be attributed specifically to nano-SiO2 or nano-Al2O3. In the absence of a matched alkali-activated, nanoparticle-free control, the contributions of the NaOH/sodium-silicate activator, nano-oxide addition, PCE dosage, and effective liquid balance remain confounded. Because the cited studies used different binders, alkaline species, and concentrations, they support the plausibility of an activator effect but do not quantify its contribution in the present ferro-sulphoaluminate cement system.
Liquid balance also differed among the formulations. Every batch contained 210 g of deionized water per 500 g of cement, corresponding to a nominal deionized-water-to-cement ratio of 0.420. Nevertheless, the liquid PCE was dosed as received at 5, 10, or 15 g per batch and contained 20.1% solids. The resulting effective water-to-cement ratios were 0.428 for N0, 0.436 for S1 and A1, and 0.444 for S2 and A2. The activated formulations therefore contained more PCE-derived water than N0. A higher effective water content could increase capillary pore volume after hardening, while differences in PCE dosage could influence dispersion, air entrainment, bleeding, setting, and early reaction. At the same time, PCE performance may be altered by the high alkalinity and ionic composition produced by the dry activator. These factors are partly controlled in the matched S1–A1 and S2–A2 comparisons, which had identical PCE and effective-water contents, but they remain confounded in the S1–S2 and A1–A2 contrasts.
Nanoparticle dispersion may also have affected the response, but it should not be assigned causal priority. Nano-SiO2 and nano-Al2O3 were introduced as dry powders without ultrasonic, high-shear, or chemical pre-dispersion. The total in-mixer blending time was at least 5 min, although the exact speed sequence and duration at each speed were not recorded. The literature on other cementitious systems shows that nano-oxide particles may agglomerate in aqueous and ion-rich media, reducing their effective surface area and generating heterogeneous regions [22,23,24]. Direct dry addition therefore makes agglomeration plausible in the present mixtures, but neither adequate nor inadequate dispersion was demonstrated.
The measured BET surface areas do not establish particle packing or microvoid filling. Such effects depend on primary-particle size, agglomerate size, morphology, spatial distribution, suspension stability, and fresh-state rheology. The supplier-declared particle sizes of 30 ± 5 nm for nano-SiO2 and 20 nm for nano-Al2O3 describe nominal powder characteristics and do not establish the agglomerate dimensions present in the mortar. Without particle-size measurements in the relevant liquid medium, microscopy, or spatial-distribution analysis, neither beneficial packing nor harmful agglomeration can be confirmed.
Possible phase-chemistry effects must likewise remain hypothetical. The raw-powder XRD patterns identified predominantly amorphous nano-SiO2 and nanocrystalline γ-Al2O3, together with ye’elimite, ferrite/brownmillerite, β-belite, gypsum, calcite, and minor quartz in the cement. As established in Section 3.1, the anomalous CaO value obtained in the initial XRF analysis of nano-Al2O3 conflicted with the verified product documentation and qualitative XRD result and was excluded from compositional and mechanical interpretation. The A1 and A2 formulations are therefore interpreted as nano-γ-Al2O3-containing formulations, without attributing their response to a hypothetical Ca-bearing alumina component.
In related calcium-rich cementitious systems, nano-SiO2 has been reported to accelerate silicate dissolution and promote silicate-containing hydrates, whereas nano-Al2O3 may influence aluminate reactions and early microstructural development [18,19,20,21]. These findings indicate possible reaction pathways but do not demonstrate that the same products formed in the present ferro-sulphoaluminate cement system. High alkalinity, soluble silicate, sulfate availability, ferrite-bearing clinker phases, and the use of a dry activator may produce reaction pathways different from those of Portland cement or conventional calcium aluminate cement. Ettringite destabilization, formation of alternative aluminate- or aluminosilicate-bearing products, rapid precipitation, delayed reaction, or phase conversion are therefore literature-supported possibilities rather than identified explanations.
The numerical flexural response should not be assigned a separate beneficial mechanism. Agglomerated, porous, or poorly compacted regions could reduce both compressive and flexural strength because bending is sensitive to defects within the tensile zone. The higher numerical flexural means of S2, A1, and A2 may alternatively reflect specimen variability, differences in moisture condition, stiffness, compaction, preferential crack paths, or unmeasured shrinkage microcracking. Because the flexural ANOVA was not statistically conclusive and only three parent-prism observations were available per formulation, the results do not demonstrate that nanoparticle packing, nucleation, or phase formation improved flexural resistance.
Accordingly, the present evidence establishes the formulation compositions, dry-powder BET/XRF/XRD characteristics, and 3 d mechanical responses. It does not establish activator incompatibility, increased hardened porosity, abnormal fresh-state behavior, entrapped air, inadequate dispersion, microvoid filling, hydrate formation, phase conversion, or a distinct mechanism governing flexural and compressive behavior. These factors should be considered competing hypotheses. Their relative contributions can be resolved only through independently replicated batches, an alkali-activated nanoparticle-free control, matched effective-water and PCE contents, predefined fresh-state performance, direct dispersion characterization, calorimetry, hardened-state XRD, TGA/DTG, FTIR or Raman spectroscopy, SEM–EDS, and pore-structure measurements.
3.5. Comparison with Previous Studies
Published 3 d results for nano-SiO2-modified mortars with a sand-to-cement ratio of 3.0, water-to-cement ratios of 0.40–0.50, and 40 × 40 × 160 mm prisms provide the closest available context for the S2 formulation (Table 6).
Table 6.
Three-day nano-SiO2-modified mortar datasets used for restricted numerical context.
The absolute results show a broadly consistent early-age strength range. The S2 flexural and compressive strengths of 4.99 and 23.95 MPa are close to the corresponding values of 5.30 and 26.30 MPa reported by Behnia et al. [38] and fall within the ranges of 4.8–5.2 and 22.5–28.1 MPa reported by Ng et al. [40]. Thus, the corrected S2 results are of a similar order to those of the referenced 3 d nano-SiO2 mortars. The remaining differences in materials and testing conditions, however, preclude claims of direct equivalence or superiority.
Normalized within-study results further indicate that the mechanical response to nano-SiO2 depends on dosage and formulation. Behnia et al. [38] reported increases of 23.25% in flexural strength and approximately 10.5% in compressive strength for their 4% nano-SiO2 mixture relative to its internal control. Liu et al. [39] observed an initial increase followed by a weaker response at higher nano-SiO2-sol contents in HBSAC mortar, with the most favorable response occurring at approximately 1%. Ng et al. [40] reported 3 d compressive-strength increases of 23.7% and 25.4% at 3% and 5% alkaline nano-SiO2 sol, respectively, indicating diminishing returns beyond 3%. Collectively, these trends show that increasing nano-SiO2 content does not produce a proportional or universally positive strength response. An equivalent normalized nano-SiO2 effect cannot be calculated for the present study because an activated nanoparticle-free control was not included; the S2–N0 contrast incorporates the combined effects of activation, nano-SiO2, PCE dosage, and liquid balance.
3.6. Limitations and Required Validation
The present study should be interpreted as an exploratory, batch-specific screening of complete mortar formulations rather than a confirmatory evaluation of isolated nanoparticle effects or coating suitability. The first limitation is the absence of a matched alkali-activated, nanoparticle-free control (AA0). N0 differed from the activated formulations not only in nanoparticle addition but also in activator use, PCE dosage, and effective water content. Consequently, the large contrasts between N0 and the activated nano-modified formulations combine several simultaneous formulation changes, and the individual effects of alkali activation, nano-oxide chemistry, and nano-oxide dosage cannot be separated. Similarly, the S1–S2 and A1–A2 contrasts are not isolated dosage comparisons because the PCE dosage and effective liquid balance also changed.
The second and most important limitation concerns the replication structure. Only one mortar batch was independently prepared for each formulation. The three parent prisms were within-batch observational units, whereas the mortar batch was the experimental unit. Between-batch variability could therefore not be estimated, and the reported confidence intervals, Welch ANOVA, Games–Howell comparisons, and effect-size estimates represent conditional descriptions of the tested batches rather than population-level evidence of reproducible formulation effects. All parent-level observations were retained and reported, with no data excluded. A descriptive leave-one-parent-out sensitivity check showed that the large compressive-strength separation between N0 and the activated formulations persisted. However, the smaller differences within the activated series were less stable: the recalculated S2 compressive-strength mean ranged from 23.03 to 25.26 MPa, whereas that of A2 ranged from 24.47 to 24.78 MPa. Thus, the dominant compressive-strength loss was more robust than the relative ranking of the activated formulations. The provisional selection of S2 should consequently not be interpreted as a reproducible or statistically established ranking.
Third, mechanical performance was evaluated only at 3 d. This predefined test age was appropriate for the intended early-age screening of the rapid-hardening system, but a single age cannot establish the subsequent development or persistence of strength, possible later-age recovery or deterioration, or the stability of the observed formulation ordering. Additional testing ages are therefore required before the mechanical response can be generalized beyond the early-age condition examined here.
Fourth, the available characterization was restricted primarily to the constituent powders. No hardened-mortar XRD, quantitative phase analysis, calorimetry, TGA/DTG, FTIR or Raman spectroscopy, SEM–EDS, or pore-structure measurements were performed. Nanoparticle dispersion and agglomeration in the activator or mortar were also not directly characterized. The available evidence therefore cannot identify the hardened reaction products, quantify porosity, verify effective nanoparticle dispersion, or determine whether activator–binder incompatibility, altered hydrate assemblage, agglomeration, entrapped air, or microcracking governed the measured mechanical response.
Finally, the study did not evaluate coating-specific properties. Flexural and compressive strengths alone do not establish adhesion to concrete, interfacial integrity, shrinkage and cracking resistance, permeability or sorptivity, chloride transport resistance, water resistance, freeze–thaw stability, abrasion or scrub resistance, application thickness, or open time. Accordingly, S2 should be regarded only as a provisional formulation selected for subsequent evaluation and cannot presently be described as an optimized or qualified protective coating.
4. Conclusions
This exploratory study characterized the constituent powders and evaluated the 3 d flexural and compressive responses of five complete ferro-sulphoaluminate cement mortar formulations under the adopted dry-activator and direct-powder mixing protocol. Only one independently prepared batch was available per formulation; consequently, the three parent prisms are within-batch observations and the conclusions are conditional on the tested batches rather than population-level formulation effects. Within this explicitly limited scope, the following conclusions were drawn:
1. Activator–binder incompatibility is considered, based on the available literature, to be a possible reason for the substantial compressive-strength reduction in the activated mixes compared to the control group, and an excessively rapid early reaction may have resulted in flash-set-like behavior. The NaOH/sodium-silicate activator generated a high-pH environment, thus accelerating dissolution and hydrate precipitation in the activated binder. The possible effects of flash-set-like behavior on workability and compaction have been proposed in the literature. Future work will consider using a lower-alkalinity activator and adding a setting retarder to investigate their effects on the performance of this coating material.
2. The BET (N2) specific surface areas of nano-SiO2 and nano-γ-Al2O3 were 123.37 and 136.47 m2/g, respectively, substantially exceeding those of the ferro-sulphoaluminate cement (0.94 m2/g) and quartz sand (0.02 m2/g). Qualitative XRD identified predominantly amorphous SiO2 in the nano-silica powder and nanocrystalline γ-Al2O3 in the nano-alumina powder, together with ye’elimite, ferrite/brownmillerite, β-belite, gypsum, calcite, and minor quartz in the cement.
3. The corrected mean flexural strengths of N0, S1, S2, A1, and A2 were 3.81, 3.79, 4.99, 4.46, and 4.60 MPa, respectively, giving the numerical order S2 > A2 > A1 > N0 > S1. However, the overall flexural-strength difference was not statistically conclusive (p = 0.089). The observed separation should therefore be regarded as an exploratory numerical trend rather than as evidence of a demonstrated nano-oxide improvement.
4. In compression, N0 reached 45.80 MPa, whereas the activated nano-modified formulations reached only 21.30–24.67 MPa and retained 46.5%–53.9% of the N0 mean. The exploratory analysis identified significant differences between N0 and each activated formulation. Thus, the dominant mechanical result was the approximately 46.1%–53.5% compressive-strength reduction: alkali activation combined with nano-oxide addition did not improve 3 d compressive strength under the adopted formulation and direct-powder mixing conditions.
5. Comparisons within the activated series did not reveal a consistent advantage for either nano-oxide product. At the 2% nominal addition level, A1 showed numerically higher flexural and compressive means than S1, whereas at the 4% level, S2 had the higher flexural mean but A2 had the higher compressive mean value.
6. In the activated binder, S2 and A2 were retained as priority formulations because neither outperformed the other in both mechanical responses. S2 had the highest flexural mean of 4.99 MPa and a compressive mean of 23.95 MPa, corresponding to 97.1% of the A2 compressive-strength mean; A2 had a flexural mean of 4.60 MPa and the highest activated-series compressive mean of 24.67 MPa. No statistically conclusive separation between S2 and A2 was detected in either response. S2 was therefore provisionally selected only under the predefined evaluation hierarchy that favored the higher corrected flexural mean after no compressive-strength separation was observed, while A2 remains a credible alternative. Further work should include independently prepared batches, a matched activated nanoparticle-free control, controlled PCE dosage and effective water content, target-flow and other fresh-state measurements, validated nanoparticle dispersion, later-age strength testing, and hardened-phase and pore-structure characterization. Pull-off adhesion, interfacial integrity, shrinkage and cracking, permeability or sorptivity, chloride transport, water resistance, freeze–thaw stability, abrasion resistance, application properties, and long-term durability must also be evaluated before either formulation can be considered suitable for protective-coating application. Within these boundaries, the present study contributes a transparent early-age benchmark showing that the adopted activation/nano-oxide strategy imposed a substantial compressive-strength penalty. Identifying this constraint is directly useful to protective-coating development because it defines the formulation problem that must be resolved before coating-specific qualification.
Author Contributions
Conceptualization, Y.W. and J.W.; methodology, Y.W. and J.W.; software, Y.W.; validation, Y.W., Y.L., D.W. and J.W.; formal analysis, Y.W. and J.W.; investigation, Y.W., Y.L. and D.W.; resources, Y.L., D.W. and J.W.; data curation, Y.W., Y.L. and D.W.; writing—original draft preparation, Y.W.; writing—review and editing, Y.W. and J.W.; visualization, Y.W. and J.W.; supervision, J.W.; project administration, J.W.; funding acquisition, J.W. All authors have read and agreed to the published version of the manuscript.
Funding
This research was funded by National Key Research and Development Program of China (Grant No. 2023YFC3902802) and Anhui Provincial Key Laboratory of Green and Low-Carbon Technology in Cement Manufacturing, No. GLCT202401.
Institutional Review Board Statement
Not applicable.
Informed Consent Statement
Not applicable.
Data Availability Statement
The data presented in this study are available from the corresponding author upon reasonable request.
Acknowledgments
The authors wish to acknowledge the financial support provided by the National Key Research and Development Program of China (Grant No. 2023YFC3902802) and Anhui Provincial Key Laboratory of Green and Low-Carbon Technology in Cement Manufacturing, No. GLCT202401.
Conflicts of Interest
Author Yinjie Liu was employed by the Hefei Cement Research & Design Institute Corporation Ltd. The remaining authors declare that the research was conducted in the absence of any commercial or financial relationships that could be construed as a potential conflict of interest.
References
- Sajid, H.U.; Jalal, A.; Kiran, R.; Al-Rahim, A. A Survey on the Effects of Deicing Materials on Properties of Cement-Based Materials. Constr. Build. Mater. 2022, 319, 126062. [Google Scholar] [CrossRef] [Scilit]
- Jones, C.; Ramanathan, S.; Suraneni, P.; Hale, W.M. Calcium Oxychloride: A Critical Review of the Literature Surrounding the Formation, Deterioration, Testing Procedures, and Recommended Mitigation Techniques. Cem. Concr. Compos. 2020, 113, 103663. [Google Scholar] [CrossRef] [Scilit]
- Angst, U.; Elsener, B.; Larsen, C.K.; Vennesland, Ø. Critical Chloride Content in Reinforced Concrete—A Review. Cem. Concr. Res. 2009, 39, 1122–1138. [Google Scholar] [CrossRef] [Scilit]
- Pan, X.; Shi, Z.; Shi, C.; Ling, T.-C.; Li, N. A Review on Concrete Surface Treatment Part I: Types and Mechanisms. Constr. Build. Mater. 2017, 132, 578–590. [Google Scholar] [CrossRef] [Scilit]
- Liao, J.; Wang, Y.; Sun, X.; Wang, Y. Chloride Penetration of Surface-Coated Concrete: Review and Outlook. Materials 2024, 17, 4121. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Coffetti, D.; Crotti, E.; Gazzaniga, G.; Gottardo, R.; Pastore, T.; Coppola, L. Protection of Concrete Structures: Performance Analysis of Different Commercial Products and Systems. Materials 2021, 14, 3719. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Song, X.; Song, X.; Liu, H.; Huang, H.; Anvarovna, K.G.; Ugli, N.A.D.; Huang, Y.; Hu, J.; Wei, J.; Yu, Q. Cement-Based Repair Materials and the Interface with Concrete Substrates: Characterization, Evaluation and Improvement. Polymers 2022, 14, 1485. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Hassan, K.E.; Brooks, J.J.; Al-Alawi, L. Compatibility of Repair Mortars with Concrete in a Hot-Dry Environment. Cem. Concr. Compos. 2001, 23, 93–101. [Google Scholar] [CrossRef] [Scilit]
- Winnefeld, F.; Lothenbach, B. Hydration of Calcium Sulfoaluminate Cements: Experimental Findings and Thermodynamic Modelling. Cem. Concr. Res. 2010, 40, 1239–1247. [Google Scholar] [CrossRef] [Scilit]
- Gartner, E.; Sui, T. Alternative Cement Clinkers. Cem. Concr. Res. 2018, 114, 27–39. [Google Scholar] [CrossRef] [Scilit]
- Cheng, Z.; Zhao, J.; Cui, L. Exploration of Hydration and Durability Properties of Ferroaluminate Cement with Compare to Portland Cement. Constr. Build. Mater. 2022, 319, 126138. [Google Scholar] [CrossRef] [Scilit]
- Fernández-Jiménez, A.; Vázquez, T.; Palomo, A. Effect of Sodium Silicate on Calcium Aluminate Cement Hydration in Highly Alkaline Media: A Microstructural Characterization. J. Am. Ceram. Soc. 2011, 94, 1297–1303. [Google Scholar] [CrossRef] [Scilit]
- Tambara, L.U.D.; Cheriaf, M.; Rocha, J.C.; Palomo, A.; Fernández-Jiménez, A. Effect of Alkalis Content on Calcium Sulfoaluminate (CSA) Cement Hydration. Cem. Concr. Res. 2020, 128, 105953. [Google Scholar] [CrossRef] [Scilit]
- Tambara Júnior, L.U.D.; Rocha, J.C.; Cheriaf, M.; Padilla-Encinas, P.; Fernández-Jiménez, A.; Palomo, A. Effect of Alkaline Salts on Calcium Sulfoaluminate Cement Hydration. Molecules 2021, 26, 1938. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Li, J.; Zeng, T.; Chang, J. Nanostructure Evolution of (A/F)H3 Phase with Different Alkali Concentrations Based on Calcium Sulfoaluminate Cement. Cem. Concr. Res. 2023, 172, 107216. [Google Scholar] [CrossRef] [Scilit]
- Oltulu, M.; Şahin, R. Single and Combined Effects of Nano-SiO2, Nano-Al2O3 and Nano-Fe2O3 Powders on Compressive Strength and Capillary Permeability of Cement Mortar Containing Silica Fume. Mater. Sci. Eng. A 2011, 528, 7012–7019. [Google Scholar] [CrossRef] [Scilit]
- Mohseni, E.; Miyandehi, B.M.; Yang, J.; Yazdi, M.A. Single and Combined Effects of Nano-SiO2, Nano-Al2O3 and Nano-TiO2 on the Mechanical, Rheological and Durability Properties of Self-Compacting Mortar Containing Fly Ash. Constr. Build. Mater. 2015, 84, 331–340. [Google Scholar] [CrossRef] [Scilit]
- Björnström, J.; Martinelli, A.; Matic, A.; Börjesson, L.; Panas, I. Accelerating Effects of Colloidal Nano-Silica for Beneficial Calcium–Silicate–Hydrate Formation in Cement. Chem. Phys. Lett. 2004, 392, 242–248. [Google Scholar] [CrossRef] [Scilit]
- Barbhuiya, S.; Mukherjee, S.; Nikraz, H. Effects of Nano-Al2O3 on Early-Age Microstructural Properties of Cement Paste. Constr. Build. Mater. 2014, 52, 189–193. [Google Scholar] [CrossRef] [Scilit]
- Zhou, J.; Zheng, K.; Liu, Z.; He, F. Chemical Effect of Nano-Alumina on Early-Age Hydration of Portland Cement. Cem. Concr. Res. 2019, 116, 159–167. [Google Scholar] [CrossRef] [Scilit]
- Chen, J.; Liang, C.; Li, B.; Wang, E.; Li, G.; Hou, X. The Effect of Nano-γ-Al2O3 Additive on Early Hydration of Calcium Aluminate Cement. Constr. Build. Mater. 2018, 158, 755–760. [Google Scholar] [CrossRef] [Scilit]
- Kong, D.; Du, X.; Wei, S.; Zhang, H.; Yang, Y.; Shah, S.P. Influence of Nano-Silica Agglomeration on Microstructure and Properties of the Hardened Cement-Based Materials. Constr. Build. Mater. 2012, 37, 707–715. [Google Scholar] [CrossRef] [Scilit]
- Reches, Y.; Thomson, K.; Helbing, M.; Kosson, D.S.; Sanchez, F. Agglomeration and Reactivity of Nanoparticles of SiO2, TiO2, Al2O3, Fe2O3, and Clays in Cement Pastes and Effects on Compressive Strength at Ambient and Elevated Temperatures. Constr. Build. Mater. 2018, 167, 860–873. [Google Scholar] [CrossRef] [Scilit]
- Hou, P.; Shi, J.; Prabakar, S.; Cheng, X.; Wang, K.; Zhou, X.; Shah, S.P. Effects of Mixing Sequences of Nanosilica on the Hydration and Hardening Properties of Cement-Based Materials. Constr. Build. Mater. 2020, 263, 120226. [Google Scholar] [CrossRef] [Scilit]
- Dheyaaldin, M.H.; Mosaberpanah, M.A.; Alzeebaree, R. Performance of Fiber-Reinforced Alkali-Activated Mortar with/without Nano Silica and Nano Alumina. Sustainability 2022, 14, 2527. [Google Scholar] [CrossRef] [Scilit]
- GB/T 17671-2021; Test Method of Cement Mortar Strength (ISO Method). Standardization Administration of China: Beijing, China, 2021.
- GB/T 45920-2025; Ferro-Sulphoaluminate Cement. Standardization Administration of China: Beijing, China, 2025.
- GB/T 20472-2006; Sulphoaluminate Cement. Standardization Administration of China: Beijing, China, 2006.
- ISO 679:2009; Cement—Test Methods—Determination of Strength. 2nd ed. International Organization for Standardization: Geneva, Switzerland, 2009.
- GSB 08-1337; China ISO Standard Sand. National Standard Sample of China: Beijing, China.
- ISO 9277:2022; Determination of the Specific Surface Area of Solids by Gas Adsorption—BET Method. 3rd ed. International Organization for Standardization: Geneva, Switzerland, 2022.
- National Institute of Standards and Technology. Certificate of Analysis, Standard Reference Material 1880a: Portland Cement; NIST: Gaithersburg, MD, USA, 2002.
- GB 18445-2012; Cementitious Capillary Crystalline Waterproofing Materials. Standardization Administration of China: Beijing, China, 2012.
- Smaoui, N.; Bérubé, M.-A.; Fournier, B.; Bissonnette, B.; Durand, B. Effects of Alkali Addition on the Mechanical Properties and Durability of Concrete. Cem. Concr. Res. 2005, 35, 203–212. [Google Scholar] [CrossRef] [Scilit]
- Janotka, I. Hydration of the Cement Paste with Na2CO3 Addition. Ceramics-Silikaty 2001, 45, 16–23. [Google Scholar]
- Juenger, M.C.G.; Jennings, H.M. Effects of High Alkalinity on Cement Pastes. ACI Mater. J. 2001, 98, 251–255. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Padilla-Encinas, P.; Palomo, A.; Blanco-Varela, M.T.; Fernández-Jiménez, A. Calcium Sulfoaluminate Clinker Hydration at Different Alkali Concentrations. Cem. Concr. Res. 2020, 138, 106251. [Google Scholar] [CrossRef] [Scilit]
- Behnia, B.; Safardoust-Hojaghan, H.; Amiri, O.; Salavati-Niasari, M.; Anvari, A.A. High-Performance Cement Mortars-Based Composites with Colloidal Nano-Silica: Synthesis, Characterization and Mechanical Properties. Arab. J. Chem. 2021, 14, 103338. [Google Scholar] [CrossRef] [Scilit]
- Liu, H.; Li, Q.; Su, D.; Yue, G.; Wang, L. Study on the Influence of Nanosilica Sol on the Hydration Process of Different Kinds of Cement and Mortar Properties. Materials 2021, 14, 3653. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Ng, P.-L.; Chen, J.; Kwan, A.K.H. Use of Nano Silica Sol for Performance Improvement of Marine Cement-Based Mortar. Adv. Mater. Lett. 2025, 16, 25011769. [Google Scholar]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |