Abstract
Titanium dioxide nanotubes (TNTs) have favorable biocompatibility and nanoscale morphologies, and they have been extensively explored for titanium implant surface modifications. However, they are limited by their mechanical strength and weak interfacial adhesion between the nanotube layer and the titanium substrate. This restricts their clinical applications. In this study, a two-step electrochemical anodization method is developed to achieve in situ tantalum (Ta) doping into TNT arrays to enhance their mechanical performance without altering their nanotubular structure. The surface morphology, element and crystal phase composition, surface roughness, wettability, and mechanical properties of the Ta-doped TNTs were then thoroughly characterized. Scanning electron microscopy revealed that the Ta doping did not change the nanotube architecture. In addition, X-ray diffraction confirmed anatase TiO2 formation in all the samples. X-ray photoelectron spectroscopy demonstrated that Ta5+ doping significantly reduced oxygen vacancies, and this was a concentration-dependent effect. Nanoindentation and scratch tests showed that the hardness, the Young’s modulus of the nanotube layer, and the adhesion strength between the nanotubes and the titanium substrate were markedly improved compared to those of the undoped TNTs. These mechanical enhancements may be attributed to lattice densification due to Ta doping. In vitro cell assays further demonstrated that the Ta-TNTs promoted rat bone marrow mesenchymal stem cell adhesion, proliferation, and osteogenic differentiation. This was evidenced by increased alkaline phosphatase activity, enhanced mineralization, and upregulated gene expression levels. The results suggest that the Ta-doped TNTs offer a pathway for the development of mechanically robust and bioactive implant surfaces for dental and orthopedic applications.
1. Introduction
Implant technology and biomaterials have advanced continuously, leading to an increasing number of patients with partial or complete edentulism opting for dental implants to restore missing teeth [1]. Titanium (Ti) and its alloys possess excellent biocompatibility, mechanical strength, and corrosion resistance, and have been widely applied as dental implant materials [2]. To further enhance the biological and physicochemical properties of titanium implants, various surface modification strategies have been developed [3]. Among these, the fabrication of titanium dioxide nanotubes (TNTs) on titanium surfaces by anodic oxidation has become a major research focus, as these nanostructures offer a high surface area, enhanced hydrophilicity, and the potential to improve osseointegration, drug loading performance, and antibacterial performance compared to smooth titanium surfaces [4,5,6,7,8].
Despite their promising features, clinical application of pure TNTs remains restricted by insufficient mechanical strength and a limited osteogenic capacity [9,10]. Consequently, recent studies have increasingly turned to biofunctionalization strategies to impart enhanced mechanical stability and biological activity while preserving the advantageous nanotopography. One effective approach involves the incorporation of metallic elements into the TNT’s structure [11]. Various methods have been used to introduce metallic elements into TNTs, including electrochemical deposition [12], plasma immersion ion implantation [13], atomic layer deposition [14], and hydrothermal process [15]. Recent studies underscore the importance of combining inorganic dopants and organic coatings to engineer multifunctional TNTs-based interfaces with improved biomechanical and biological performance. However, such approaches can significantly alter the nanotubular morphology, and the surface-deposited particles often exhibit poor adhesion, which can lead to particle detachment and burst release in biological environments, causing cytotoxic effects [16].
Anodic oxidation is one of the most mature and controllable techniques for TNTs fabrication [12]. Several studies have demonstrated that in situ metal doping can be achieved during nanotube formation by the addition of metal ion precursors directly into the anodization electrolyte [17]. This process allows the dopant ions to incorporate into the TiO2 lattice without disrupting the nanotubular structure. This enables the nanotubes to retain their morphology and gain new functional properties. Further research has shown that metal ions with ionic radii similar to that of Ti4+ can substitute Ti4+ sites through substitutional doping, thus integrating into the TiO2 lattice and minimizing morphological changes caused by doping [18].
Tantalum (Ta) has received growing attention in recent years due to its outstanding corrosion resistance, biocompatibility and high surface energy, which promotes protein adsorption and osteogenic responses [19,20]. However, the high density and elastic modulus of bulk tantalum limit its direct use as an implant material [21]. Instead, tantalum is often employed as a coating or dopant on titanium substrates to enhance their bioactivity [22]. The ionic radius of Ta5+ (0.64 Å) is close to that of Ti4+ (0.61 Å); hence, it is feasible to achieve the substitutional doping of tantalum into the TiO2 lattice without altering the nanotube morphology.
In this study, we employed a two-step anodization method to achieve in situ Ta doping into TiO2 nanotube arrays. The aim of this approach was to enhance the mechanical strength and osteogenic potential of TNTs while preserving their nanoscale morphology. The present study provides a theoretical foundation for the clinical translation of Ta-doped TiO2 nanotube–modified titanium implants and offers a new pathway toward the development of mechanically robust and biologically active implant surfaces.
2. Materials and Methods
2.1. Material Preparation
2.1.1. Pure Ti Group
Commercially pure titanium sheets (5 cm × 5 cm × 0.2 mm, 99.99%; the Cuibolin Nonferrous Metal Industry Co., Ltd., Beijing, China) were polished using 500-, 1000-, and 2000-grit silicon carbide sandpapers. The samples were then ultrasonically cleaned (CD-4862, Codyson, Shenzhen, China) at an operating frequency of 38 kHz and nominal power of 110 W for 5 min each in acetone, anhydrous ethanol (Hushi, Shanghai, China), and deionized water, and subsequently air-dried. These samples served as the Ti group.
2.1.2. TNTs Group
TNTs were fabricated on polished Ti substrates using a two-step anodization process. The first anodization was conducted using Ti as the anode and platinum as the cathode in an ethylene glycol–based electrolyte that contained 0.5% ammonium fluoride (w/v), 0.25% hydrofluoric acid (v/v) (Hushi, Shanghai, China), and 10% deionized water (v/v) at 50 V for 30 min. The electrolyte was continuously stirred with a magnetic stirrer to maintain the temperature and electric field uniformity. After the first anodization, the Ti sheets were ultrasonically cleaned with ethanol and deionized water. They were then acid-etched in a 10% dilute sulfuric acid solution (v/v) to remove the initially formed oxide layer.
The second anodization was conducted under the same conditions using the same Ti sheets as the anode and platinum as the cathode. Following anodization, the samples were rinsed with ethanol and deionized water, air-dried, and annealed in an oxygen-rich atmosphere by heating to 500 °C at a rate of 4 °C/min, held for 4 h, and then cooled to room temperature. The resulting specimens were designated as the TNTs group.
2.1.3. Ta-Doped TNTs (Ta-TNTs) Group
The Ta-TNTs were prepared using Ti sheets that underwent the same initial anodization, acid etching, and cleaning steps as described above. Tantalum metal was dissolved in hydrofluoric acid to prepare Ta-ion solutions of varying concentrations. These were then added to the anodization electrolyte to 0.5%, 1.0%, 1.5% and 2.0% Ta5+ (mol/v) concentrations in the solution. A consistent fluoride concentration and pH were maintained by the amount of hydrofluoric acid and ammonium fluoride that were proportionally adjusted. A second anodization was then performed with Ti as the anode and platinum as the cathode. The total ionic concentration changed after the addition of the Ta ions; hence, the anodization rate was adjusted by tuning the applied voltage and maintaining an electrolyte temperature of 20 °C using a water bath.
After anodization, the samples were rinsed with ethanol and deionized water, then annealed in an oxygen-rich atmosphere at 500 °C for 4 h (heating rate: 4 °C/min) to form the Ta-doped TiO2 nanotubes. Samples with different Ta-ion concentrations were labeled 0.5Ta-TNTs, 1.0Ta-TNTs, 1.5Ta-TNTs, and 2.0Ta-TNTs.
2.2. Sample Characterization
2.2.1. Surface Morphologies
The surface morphologies of the Ti, TNTs, and all of the Ta-TNTs samples (0.5–2.0Ta) were mounted on the SEM stage using conductive carbon tape without additional conductive metal coating, then observed using field-emission scanning electron microscopy (FE-SEM) (JSM-7500F, JEOL, Tokyo, Japan) operated in secondary electron imaging (SEI) mode at an accelerating voltage of 5 kV and a working distance of 8 mm. at magnifications of ×10,000 and ×50,000. The nanotube diameters were measured under high magnification (×50,000), and nine random nanotubes were measured in three randomly selected fields for each group (n = 9). The side-view structures were examined by mechanically bending or scraping the nanotube layers of the TNTs and Ta-TNTs samples to expose the cross-sections. These were then imaged using FE-SEM (JSM-7500F, JEOL, Tokyo, Japan).
2.2.2. Element and Crystal Phase Composition
The surface elemental compositions of the Ti, TNTs, and Ta-TNTs groups were analyzed using energy-dispersive X-ray spectroscopy (EDS) (EDAX OCTANE SUPER, AMETEK, Berwyn PA, USA) attached to the FE-SEM. EDS spectra and mapping were acquired at an accelerating voltage of 20 kV with a working distance of approximately 12 mm under high-vacuum conditions. Nanotube layers from the TNTs, 1.0Ta-TNTs and 2.0Ta-TNTs samples were scratched and ultrasonically detached into individual nanotubes in ethanol and dispersed onto copper grids. The cross-sectional morphology and elemental distribution of a single nanotube were characterized using transmission electron microscopy (TEM) (TEM, JEM-2100F, JEOL, Tokyo, Japan) coupled with EDS mapping.
The surface element states were analyzed using an XPS spectrometer (AXIS SUPRA+, Shimadzu, Kyoto, Japan). The C–C peak at 284.6 eV was used for the charge correction. Element mapping of the Ti-2p, O-1s and Ta-4d orbital electrons of all the groups was then analyzed. The area under the characteristic peak curve of the 1s orbital electrons of the surface oxygen elements and the area under the characteristic peak curve of Ta–O and Ta5+–O at 530.8 eV were measured. The relative content of the Ta–O bonds was calculated based on the area ratio of the Ta5+–O peaks to the total O 1s peaks.
The crystal structures of the Ti, TNTs, and all Ta-TNTs samples were examined using X-ray diffraction (X’Pert PRO MPD, Panalytical, Almolo, The Netherlands).
2.2.3. Surface Roughness and Wettability
The surface roughness values were measured using an atomic force microscope (Bruker Dimension Icon, Karlsruhe, Germany). The surface height variations (indentation depth vs. distance) were recorded, and the roughness (Ra) values were calculated.
The static water contact angles were measured using a video optical contact angle analyzer (OCA15 Pro, Dataphysics, Stuttgart, Germany) at 20 °C and 21% relative humidity. A 10 µL droplet of deionized water was deposited on each sample, and the contact angle was calculated as the average of the left and right tangent angles. Three samples per group were measured.
2.2.4. Mechanical Strength
The mechanical properties of the TNTs and Ta-TNTs were tested using a nanoindenter (100BA-1C, MTS, Eden Prairie, MN, USA). Nanoindentation and nanoscratch tests were conducted under a controlled maximum load and holding time. The obtained load–displacement curves were analyzed to calculate the hardness, the Young’s modulus, and the critical load for coating delamination.
2.2.5. Tantalum Ion Release Test
An ion release test was performed to quantify the tantalum released from the Ta-TNTs samples. Each Ta-TNTs specimen was immersed in Hank’s solution and incubated at 37 °C for 1 and 7 days. At each time point, the immersion medium was collected for elemental analysis. The Ta ion concentration in the extracts was measured by inductively coupled plasma mass spectrometry (NexION 300X, PerkinElmer, Waltham, MA, USA) following standard instrument operating procedures.
2.3. Cell Compatibility and Osteogenic Properties Characterization In Vitro
2.3.1. Cell Adhesion
Rat bone marrow mesenchymal stem cells (rBMSCs) (RASMX-01001, Oricell, Suzhou, China) were seeded onto the Ti, TNTs, and all Ta-TNTs samples at a density of 1 × 105 cells/well in 24-well plates. Incubation was conducted for 1 h and 4 h at 37 °C with 5% CO2. The non-adherent cells were then removed by phosphate-buffered solution washing. Cell adhesion was quantified using the cell counting kit-8 (CCK-8) assay (CCK-8 Kit, Biyotime, Shanghai, China), and the absorbance was measured at 450 nm. Adherent cells were fixed and stained using 4′,6-diamidino-2-phenylindole (DAPI) (Biyotime, Shanghai, China) for fluorescence visualization, and the cell attachment was observed under an inverted fluorescence microscope.
2.3.2. Cell Proliferation and Live-Dead Cell Staining
The rBMSCs were seeded on the Ti, TNTs, and all Ta-TNTs samples at 5 × 104 cells/well and cultured for 1, 3, and 5 days. At each time point, the cells were evaluated using the CCK-8 assay, and the absorbance was recorded at 450 nm.
Live/dead cell staining was performed using a Calcein AM/PI Double Staining Kit (Elabscience, Wuhan, China). The rBMSCs were seeded on each sample at a density of 5.0 × 104 cells/well and cultured for 24 h. The samples were then rinsed gently with PBS and incubated with the staining solution prepared according to the manufacturer’s instructions. After staining, fluorescence images were acquired using an inverted fluorescence microscope, and the live/dead cells were calculated.
2.3.3. Alkaline Phosphatase (ALP) Activity
The cells were seeded at 1 × 105 cells/well and cultured in an osteogenic induction medium that contained β-glycerophosphate, L-ascorbic acid, and dexamethasone for 3, 5, and 7 days. The total protein content was quantified using the bicinchoninic acid assay method (BCA Protein Assay Kit, Biyotime, Shanghai, China), and the ALP activity was determined using an ALP assay kit (Biyotime, Shanghai, China). The absorbance values at 405 nm were measured and normalized to the total protein concentration to obtain the relative ALP activity.
2.3.4. Mineralized Matrix Formation
After 7, 14, and 21 days of osteogenic induction, the rBMSCs cultured on the Ti, TNTs, and Ta-TNTs were fixed and stained with Alizarin Red S (Biyotime, Shanghai, China) to evaluate the extracellular matrix mineralization. The bound dye was extracted using a 10% cetylpyridinium chloride solution (Hushi, Shanghai, China), and the absorbance values at 560 nm were measured to quantify the calcium deposition.
2.3.5. Quantitative Real-Time PCR (qRT-PCR) for Osteogenic Gene Expression
qRT-PCR was performed to evaluate the osteogenesis-related gene expressions in the rBMSCs cultured on the Ti, TNTs, and Ta-TNTs specimens. The cells were cultured in an osteogenic induction medium for 7 and 14 days. At each time point, the total RNA was extracted using the TRIzol reagent (Invitrogen, Carlsbad, CA, USA). The RNA concentrations and purity were measured using a NanoDrop spectrophotometer. cDNA was synthesized using the PrimeScript First Strand cDNA Synthesis Kit (Takara, Kyoto, Japan) according to the manufacturer’s instructions. The gene expression levels of BMP-2, ALP, OCN, and Runx2 were quantified using SYBR Green-based qRT-PCR on a Bio-Rad Real-Time PCR System (Bio-Rad, Hercules, CA, USA). Glyceraldehyde 3-phosphate dehydrogenase was used for normalization. Primers were commercially synthesized (Sangon Biotech, Shanghai, China). The primer sequences are listed in Table 1. Each reaction was performed in triplicate. The gene expression values were normalized to β-actin using the 2-ΔΔCt method.
Table 1.
Primers for the qRT-PCR.
2.4. Statistical Analyses
All statistical analyses were conducted using the IBM SPSS Statistics (version 19.0 IBM Corp., Chicago, IL, USA). All data are presented in the form of means ± standard deviations. Statistical significance was assessed using an analysis of variance, with the significance set at p < 0.05.
3. Results
3.1. Surface Morphologies
The surface morphologies of the Ti, TNTs, and all of the Ta-TNTs samples were characterized using FE-SEM (Figure 1a). The Ti group showed polished surfaces with only minor grinding scratches. The TNTs and all Ta-TNTs samples exhibited well-aligned and vertically oriented nanotube arrays with uniform pore diameters of approximately 106 nm. The result indicates that after Ta doping, the nanotubular morphologies were preserved in all of the groups, with no obvious difference in surface morphology and nanotube diameter among the groups, as shown in Table 2. Increases in the Ta concentrations caused no significant changes in tube diameters or surface morphologies either. This result confirmed that the two-step anodization method allowed for in situ Ta incorporation without compromising the nanotube morphology.
Figure 1.
(a) FE-SEM images of surface morphologies at different magnifications for different specimens; (b) FE-SEM cross-sectional images of the different specimens.
Table 2.
Measurement results of the nanotube diameters in each specimen.
Cross-sectional SEM images (Figure 1b) revealed that all of the nanotube layers in TNTs and all the Ta-TNTs groups had uniform tubular structures, and the outer diameters of the nanotubes did not change significantly from the nozzle to the bottom of the tube. The outer walls of the nanotubes in each group were uniform and smooth. The results also confirmed that different concentrations of Ta doping caused no significant changes in surface morphology as well as the nanotube diameter.
3.2. Elemental Composition and Distribution
The EDS surface analysis in Figure 2 showed that the Ti group exhibited characteristic peaks of Ti, whereas the TNTs group exhibited characteristic peaks of Ti and O, confirming the formation of TiO2 nanotubes. For all Ta-TNTs groups, Ti and O peaks remained dominant. The Ta-related peaks were not clearly visible in the EDS spectra, which is likely due to the low Ta content and the limited sensitivity of EDS for trace-level dopants.
Figure 2.
EDS characterization of the different specimens.
TEM–EDS mapping of the TNTs, 1.0Ta-TNTs and 2.0Ta-TNTs (Figure S1) further verified that the nanotubes were composed of titanium dioxide. In addition, the uniform Ta distribution throughout the nanotube walls in the Ta-TNTs confirmed successful in situ doping rather than surface deposition.
The XPS element mapping of the Ti-2p, O-1s, and Ta-4d orbital electrons of all the groups is shown in Figure 3a. The results revealed that the surface of each of the Ta-TNTs was doped with tantalum, and the distribution of tantalum on the surface of the material was uniform, validating that the tantalum atoms were successfully and uniformly doped into the whole titanium dioxide nanotube, which was consistent with the FE-SEM and TEM characterization results.
Figure 3.
XPS analysis of all the specimens. (a) Element mapping of Ti-2p, O-1s, and Ta-4d orbital electrons in all the specimens; (b) peaking of the O-1s orbital electrons in the TNTs and all Ta-TNTs samples.
The 1s orbital electrons of the surface oxygen elements in the TNTs group and all Ta-TNTs groups were peaked, and the results are shown in Figure 3b. The primary peaks of the 1s orbital electrons of the oxygen element in the TNTs group could be divided into Ti-O double peaks with binding energies of 529.8 eV and 530.4 eV and an -OH peak with a binding energy of 532.0 eV, where 529.8 eV is the characteristic peak of Ti4+-O, and 530.4 eV is the characteristic peak of Ti3+-O. However, after the primary peak of the O-1s orbital electron in each Ta-TNTs group was divided, in addition to the Ti-O characteristic peak at 529.8 eV and 532.0 eV, the Ta5+-O characteristic peak appeared at 530.8eV. The results discussed above further confirmed that tantalum doping had occurred in all Ta-TNTs groups and found that tantalum in the Ta-TNTs group was doped into nanotubes in the valence state of Ta5+.
The relative content of the Ta5+–O bonds was calculated, and the results are shown in Table 3. The proportion of Ta5+-O on the surface of each Ta-TNTs gradually increased alongside an increase in the tantalum doping concentration. This increase was from 8.50% in the 0.5Ta-TNTs group to 30.33% in the 2.0Ta-TNTs group. This result indicated that the tantalum content in the Ta-TNTs was positively correlated with the tantalum ion concentrations in the electrolyte. In addition, different Ta-TNTs were prepared by adjusting the tantalum ion concentration in the electrolyte.
Table 3.
Area ratio of the Ta5+–O peaks to the total O-1s peaks.
3.3. Phase Composition Analysis
The XRD patterns of all the samples are shown in Figure 4. Only diffraction peaks of α-Ti (PDF#44-1294) were detected on the surfaces of the Ti group samples, which can be indexed to (100), (002), (101), (102), and (110) planes. For the TNTs and all Ta-TNTs groups, in addition to the α-Ti substrate peaks. For the TNTs and all Ta-TNTs groups, in addition to the α-Ti diffraction peaks, characteristic reflections of anatase TiO2 (PDF#21-1272) were observed at 25.37° (101), 37.80° (004), 38.57° (112), 48.12° (200), 53.97° (105), 55.10° (211), 62.7° (204), and 68.8° (116). No characteristic diffraction peaks of the rutile phase were detected, indicating that the nanotube layers in the TNTs and all Ta-TNTs groups predominantly consist of the anatase phase.
Figure 4.
XRD analysis of all the samples.
3.4. Surface Wettability and Roughness
The surface wettability values of all the groups are summarized in Figure 5. The contact angle for the Ti group was 73.58°. After anodizing to form the nanotubes, the hydrophilicity of the TNTs group material surface increased significantly, and the water contact angle decreased to 40.97°. The water contact angles for the 0.5Ta-TNTs, 1.0Ta-TNTs, 1.5Ta-TNTs, and 2.0Ta-TNTs groups were 38.63°, 36.80°, 34.53°, and 33.20°, respectively. The water contact angles of the TNTs group and all Ta-TNTs groups were significantly less than those of the Ti group, while the water contact angles of the 1.0Ta-TNTs, 1.5Ta-TNTs, and 2.0Ta-TNTs groups were significantly less than those of the TNTs group (p < 0.05).
Figure 5.
Surface wettability values of all the specimens. (a) Digital pictures of the water contact angle for each specimen; (b) statistics of each group. (a: p < 0.05 vs. Ti group; b: p < 0.05 vs. TNTs group; c: p < 0.05 vs. 0.5Ta-TNTs group; d: p < 0.05 vs. 1.0Ta-TNTs group; e: p < 0.05 vs. 1.5Ta-TNTs group; f: p < 0.05 vs. 2.0Ta-TNTs group).
The surface roughness values of all the groups are summarized in Figure 6. The Ti group exhibited significantly lower surface roughness than that of the TNTs and all Ta-TNTs groups, indicating that the formation of the nanotube layer increases the surface roughness. However, no statistically significant differences in the surface roughness between the TNTs and Ta-TNTs groups across the tested Ta concentrations were observed, suggesting that in situ tantalum doping does not affect the nanotopographical roughness values of the nanotube layers.
Figure 6.
Surface roughness of all the specimens. (a) AFM images of the surface roughness for each specimen; (b) statistics of each group. (* p < 0.05 vs. Ti group).
3.5. Mechanical Properties
The mechanical performances of the TNTs and Ta-TNTs coatings were evaluated using nanoindentation and nanoscratch tests (Figure 7). The nanoscratch test reveals the adhesion between the nanotube layer and the titanium substrate. The results shown in Figure 7b demonstrated an improved adhesion strength between the nanotube layer and the titanium substrate after Ta doping. The hardness of the nanotube layer was demonstrated through the nanoindentation test. The hardness of the nanotube layer was improved after Ta doping, and the hardness values of the 1.0Ta-TNTs, 1.5Ta-TNTs and 2.0Ta-TNTs were significantly higher than that of the TNTs.
Figure 7.
Mechanical strength of the TNTs and all Ta-TNTs. (a) Lateral forces in nanoscratch tests of all the specimens, the inverted triangle in the figure represents critical load.; (b) critical load values of the TNTs and all Ta-TNTs; (c) hardness values of the TNTs and all Ta-TNTs (a: p < 0.05 vs. TNTs group; b: p < 0.05 vs. 0.5Ta-TNTs group; c: p < 0.05 vs. 1.0Ta-TNTs group; d: p < 0.05 vs. 1.5Ta-TNTs group; e: p < 0.05 vs. 2.0Ta-TNTs group).
These results confirmed that moderate Ta doping effectively enhanced the mechanical integrity of the nanotube layer. The reason might relate to a reduction in the oxygen vacancies, an increase in the lattice cohesion, and a strengthening of the nanotube–Ti substrate interface.
3.6. Tantalum Ion Release Test
Figure S2 shows the concentration of tantalum ions released by all Ta-TNTs groups after soaking in Hank’s solution for 1 day and 7 days. The results showed that the concentration released by each group at 7 days was increased at 1 day, and the higher concentration group was also increased at the same time, compared with the lower concentration group.
3.7. Cell Adhesion, Cell Proliferation and Live-Dead Cell Staining
The adhesion of rBMSCs to the surface of the Ti, TNTs, and all Ta-TNTs group was detected using a CCK-8 assay at 1 and 4 h. The results are shown in Figure 8b. At the time points of 1 and 4, the 1.5Ta-TNTs and 2.0Ta-TNTs groups showed significantly higher cell optical density (OD) values compared to those of the other groups. In addition, the groups with higher Ta doping concentrations also had higher OD values. The DAPI staining results for the cell adhesion at 1 and 4 h were consistent with the results of the CCK-8, and the number of cells on the surface of each group of materials gradually increased with a culture time extension, as shown in Figure 8a.
Figure 8.
Cell adhesion and proliferation of rBMSCs in all the samples. (a) DAPI stains of the cell adhesion at 1 and 4 h; (b) CCK8 assays of the cell adhesions at 1 and 4 h; (c) CCK8 assays of the cell proliferations at 1, 3, and 5 days; (d) Counting of live/dead cells at 24 h. (a: p < 0.05 vs. Ti group; b: p < 0.05 vs. TNTs group; c: p < 0.05 vs. 0.5Ta-TNTs group; d: p < 0.05 vs. 1.0Ta-TNTs group; e: p < 0.05 vs. 1.5Ta-TNTs group; f: p < 0.05 vs. 2.0Ta-TNTs group; ns: no significant difference among the groups).
The proliferation of rBMSCs on the surface of each group was detected using the CCK-8 assay on days 1, 3, and 5 (Figure 8c). On days 1, 3, and 5, the number of rBMSCs on the surface of all Ta-TNTs was significantly higher than that of the Ti group. In addition, the number of cells on the surface of the 2.0Ta-TNTs group was significantly higher than that of the Ti and TNTs group.
The results of cell live/dead staining (Figure S3) showed that the cells on the surface of all the samples expressed high cell viability. The counting of live/dead cells (Figure 8d) showed that most of the rBMSCs in each group were alive after 24 h, indicating the surface materials had good biocompatibility.
3.8. Osteogenic Differentiation
The relative ALP activities of the rBMSCs after osteogenic induction and culture for 3, 5, and 7 days are shown in Figure 9a. On days 3, 5, and 7, the relative ALP activities of the rBMSCs on the surface of each Ta-TNTs group were significantly higher than those of the Ti group. Furthermore, the relative ALP activities of the 1.5Ta-TNTs and 2.0Ta-TNTs groups were significantly higher than those of the TNTs and Ti groups. The ALP activities of each Ta-TNTs group increased with an increasing tantalum ion doping concentration.
Figure 9.
Relative ALP activities at 3, 5, and 7 days (a) and the extracellular matrix mineralization at 7, 14, and 21 days (b) of each sample. (a: p < 0.05 vs. Ti group; b: p < 0.05 vs. TNTs group; c: p < 0.05 vs. 0.5Ta-TNTs group; d: p < 0.05 vs. 1.0Ta-TNTs group; e: p < 0.05 vs. 1.5Ta-TNTs group; f: p < 0.05 vs. 2.0Ta-TNTs group).
The semi-quantitative determinations of the calcium ions in the surface mineralization matrix of the rBMSCs at 7, 14, and 21 days after osteogenic induction are shown in Figure 9b. The results indicated that at each time point, the extracellular matrix mineralization degrees of the TNTs group and each Ta-TNTs group were significantly better than those of the Ti group. Moreover, the extracellular matrix mineralization degrees of the 1.0, 1.5, and 2.0Ta-TNTs group were significantly better than that of the TNTs group at all time points.
qRT-PCR was performed to assess the expression levels of genes related to osteogenic differentiation, including BMP2, ALP, OPN, and Runx 2. The results are shown in Figure 10. All of the Ta-TNTs groups exhibited significantly enhanced expressions of BMP2 at 7 and 14 days compared to that of the Ti group. The 1.0, 1.5, and 2.0 Ta-TNTs showed higher expressions of OPN at 14 days and higher expressions of Runx2 at 7 days compared to those of the Ti group. The 1.5 and 2.0 Ta-TNTs showed higher expressions of ALP at 7 days and higher expressions of OPN at 7 days compared to those of the Ti group.
Figure 10.
The mRNA levels of osteogenic differentiation-related genes in cells cultured on the different specimens at 7 and 14 days. (* p < 0.05 vs. Ti group).
4. Discussion
Ti implant surface modification to enhance osseointegration represents a continued challenge in the design of implants. In recent years, Ta and its oxides have garnered attention for their enhanced osteogenic and antibacterial properties compared to titanium [23]. However, tantalum has a high density and a large elastic modulus (185.7 GPa) that is much greater than the elastic modulus of human cortical bone (7–30 GPa) [24]. This can cause stress shielding in an implant and lead to bone absorption [25]. Currently, Ta and its oxides are primarily used as coating materials that are deposited on the surface of titanium metal or other scaffold materials. It has been previously shown that the morphology of the TiO2 nanotube array has a significant effect on osseointegration [26]. Therefore, it is necessary to ensure that the morphologies of TiO2 nanotube arrays with different Ta-doping levels are similar. To obtain a uniform surface and uniform morphology of the nanotubes, we improved the anodic oxidation method and the composition of the electrolyte, doped Ta ions in the lattice of TiO2 nanotubes, and successfully prepared Ta-doped TiO2 nanotubes on the surface of Ti metal.
Additionally, the biological properties of TNTs are closely related to their surface morphologies. It was found that when the diameters of the TNTs were in the range of 70–100 nm, this induced the adhesion and extension of bone marrow MSCs on the surface, promoted their osteogenic differentiation, and upregulated the expression of osteogenic-related genes [27]. In addition, nanotubes with a diameter of 100 nm have better hydrophilicity and better surface roughness, which can inhibit the formation of plaque biofilm on the material surface and enhance the antibacterial properties of the material [28]. Based on the research described above, we hoped to control the diameters of the TNTs groups and all Ta-TNTs groups to approximately 100 nm. However, in the process of Ta doping, we found that the doping concentration exceeding 2.0% would significantly reduce the diameter of nanotubes, so we took 2.0% as the highest doping concentration.
Titanium dioxide has three crystal structures: brookite, anatase, and rutile. As a biomaterial, anatase has superior biological properties and is better than rutile for the promotion of extracellular matrix mineralization [29,30]. However, anatase has more oxygen vacancies than rutile, which results in a lower relative density than rutile; hence, its mechanical strength is insufficient [31]. As for the oxygen vacancies during the anatase phase, we used XPS to scan the 1s orbital electrons of oxygen on the surface of each group of samples after doping TNTs with tantalum. We then performed peaking. The results showed that obvious Ti3+ ion peaks could be observed in the TNTs group, that is, oxygen vacancies in the material. Since the radius of the Ti3+ ions (67 pm) is larger than that of Ti4+ ions (61 pm), oxygen vacancies and defects exist in the material. The tantalum-doped titanium dioxide nanotube assembly did not show a significant Ti3+ ion peak, but instead exhibited a Ta5+ ion peak. This result indicated that tantalum doping removed oxygen vacancies within the material. Furthermore, the nanotube hardness and the bonding strength between the nanotube layer and the substrate were significantly improved. Therefore, based on previous studies and our results, we can infer that tantalum doping removed oxygen vacancies [32], thereby improving the mechanical strength of the nanotubes on the material surface and their bonding strength with the titanium substrate.
The property of a material to be wetted by water when in contact with it is called hydrophilicity. When the water contact angle is less than 90°, the material is considered hydrophilic. The hydrophilicity of a material surface depends not only on the composition of the material surface but also on the surface morphology [33]. After anodizing, more hydrogen bonds appear on the surface of a material, which makes the material and water molecules form a stronger bond, thus increasing the hydrophilicity of the material surface [34]. Tantalum has slightly better hydrophilicity than titanium, and it has a larger surface energy than titanium [35]. Therefore, the hydrophilicity of TNTs will be slightly improved after tantalum doping. It can be inferred that Ta-TNTs are more conducive to the adhesion of bioactive small molecules, thereby promoting an improvement in the biological properties of the material surface. In this study, we doped TNTs with tantalum, which improved the hydrophilicity of the material surface. The Ta-TNTs groups exhibited superior hydrophilicity values compared to those of the TNTs and Ti groups. In addition, the hydrophilicity increased with increased tantalum doping concentrations. The adhesion of rBMSCs to the material surface was also examined. An analysis of the results suggested that Ta-TNTs groups achieved superior hydrophilicities compared to those of both the TNTs group and the Ti group. This enhanced hydrophilicity resulted in better cell adhesion on the tantalum-doped surface. In addition, cell proliferation and staining of living dead cells showed that there was no obvious cell death in all Ta-TNTs groups compared with TNTs and Ti, which proved that Ta doping would not decrease the biocompatibility of the material.
Osteogenic differentiation of rBMSCs on the surface of the Ta-TNTs was also important for implant materials and was assessed in this study using relative ALP activity, an early osteogenic differentiation indicator, and tissue matrix mineralization level, an indicator of mid-to-late-stage osteogenic stage [36]. The expression levels of genes related to osteogenic differentiation were also assessed. The results showed that the Ta-TNTs exhibited superior osteogenic capacities compared to those of both the TNTs and the Ti group in both early and mid-to-late stages. Additionally, with higher concentrations of tantalum, the doped TNTs demonstrated even better osteogenic capacities. We found that the surface morphologies of the Ta-TNTs were not significantly different from those of the pure TNTs. Their surface roughness and crystal structure were also essentially the same. The improvement in the hydrophilicity through tantalum doping suggested that this improved hydrophilicity promoted osteogenic differentiation of rBMSCs on the material surface.
In this study, we performed in situ tantalum doping on TNTs using a secondary anodizing method that improved the material’s hydrophilicity, mechanical strength, biocompatibility, and osteogenic properties. However, further experiments are required to investigate the biosafety and osteogenic properties of the Ta-TNTs in vivo, as well as the related molecular mechanisms of osteogenic formation. It is hoped that in situ Ta-TNTs can provide a theoretical basis for future implant surface modifications.
5. Conclusions
In this study, a two-step anodization process was developed to achieve the in situ Ta doping into TNT arrays on titanium substrates. The Ta5+ ion incorporation successfully preserved the nanotubular morphology while significantly improving the mechanical and biological performance of the coating. Moderate Ta doping enhanced the hardness, elastic modulus, and adhesion strength, transforming the mechanically fragile nanotube layer into a robust and durable coating. The optimized 2.0Ta-TNTs group exhibited the best combination of mechanical integrity and surface stability. Moreover, the improved hydrophilicity and modified surface chemistry induced by the Ta incorporation promoted rBMSC adhesion, proliferation, and osteogenic differentiation, as evidenced by elevated ALP activity, increased mineralized matrix formation, and upregulated gene expressions.
These findings demonstrated that in situ Ta doping is a simple and effective strategy to reinforce the mechanical and osteogenic performance of anodized TiO2 nanotubes. The resulting Ta-TNTs surface provides a promising platform for the next generation of load-bearing dental and orthopedic implants that combine long-term mechanical stability with enhanced biological functionality.
Supplementary Materials
The following supporting information can be downloaded at https://www.mdpi.com/article/10.3390/jfb17020088/s1, Figure S1: TEM image of TNTs, 1.0 and 2.0Ta-TNTs. Figure S2: Tantalum ion concentrations released by each samples after immersed in Hank’s solution for 1 day and 7 days. Figure S3: Live/Dead cell stain of rBMSCs cultured on each samples for 24 h.
Author Contributions
Conceptualization, Y.Y. and R.L.; methodology, Y.Y.; software, N.W.; validation, Y.Y., Y.M. and W.L.; formal analysis, Y.Y.; investigation, Y.Y.; resources, Y.Y. and Y.M.; data curation, Y.Y.; writing—original draft preparation, Y.Y.; writing—review and editing, Y.Y. and R.L.; visualization, W.L.; supervision, S.C.; project administration, S.C.; funding acquisition, S.C. All authors have read and agreed to the published version of the manuscript.
Funding
This research was funded by Beijing Hospitals Authority’s Ascent Plan, grant number DFL20221301, and the Natural Science Foundation of Capital Medical University, grant number PYZ24183.
Institutional Review Board Statement
Not applicable.
Informed Consent Statement
Not applicable.
Data Availability Statement
The original contributions presented in the study are included in the article; further inquiries can be directed to the corresponding author.
Conflicts of Interest
The authors declare no conflicts of interest.
References
- Alghamdi, H.S.; Jansen, J.A. The development and future of dental implants. Dent. Mater. J. 2020, 39, 167–172. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Awad, N.K.; Edwards, S.L.; Morsi, Y.S. A review of TiO2 NTs on Ti metal: Electrochemical synthesis, functionalization and potential use as bone implants. Mater. Sci. Eng. C 2017, 76, 1401–1412. [Google Scholar] [CrossRef] [Scilit]
- Chouirfa, H.; Bouloussa, H.; Migonney, V.; Falentin-Daudre, C. Review of titanium surface modification techniques and coatings for antibacterial applications. Acta Biomater. 2019, 83, 37–54. [Google Scholar] [CrossRef] [Scilit]
- He, Y.; Luo, J.; Zhang, Y.; Li, Z.; Chen, F.; Song, W.; Zhang, Y. The unique regulation of implant surface nanostructure on macrophages m1 polarization. Mater. Sci. Eng. C 2020, 106, 110221. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Wang, C.; Wang, X.; Lu, R.; Gao, S.; Ling, Y.; Chen, S. Responses of human gingival fibroblasts to superhydrophilic hydrogenated titanium dioxide nanotubes. Colloids Surf. B Biointerfaces 2021, 198, 111489. [Google Scholar] [CrossRef] [Scilit]
- Zhao, X.; Wang, T.; Qian, S.; Liu, X.; Sun, J.; Li, B. Silicon-doped titanium dioxide nanotubes promoted bone formation on titanium implants. Int. J. Mol. Sci. 2016, 17, 292. [Google Scholar] [CrossRef] [Scilit]
- Kandel, R.; Jang, S.R.; Shrestha, S.; Lee, S.Y.; Shrestha, B.K.; Park, C.H.; Kim, C.S. Biomimetic Cell-Substrate of Chitosan-Cross-linked Polyaniline Patterning on TiO2 Nanotubes Enables hBM-MSCs to Differentiate the Osteoblast Cell Type. ACS Appl. Mater. Interfaces 2021, 13, 47100–47117. [Google Scholar] [CrossRef] [Scilit]
- Hajjaji, A.; Elabidi, M.; Trabelsi, K.; Assadi, A.A.; Bessais, B.; Rtimi, S. Bacterial adhesion and inactivation on ag decorated TiO2-nanotubes under visible light: Effect of the nanotubes geometry on the photocatalytic activity. Colloids Surf. B Biointerfaces 2018, 170, 92–98. [Google Scholar] [CrossRef] [Scilit]
- Alves, S.A.; Rossi, A.L.; Ribeiro, A.R.; Werckmann, J.; Celis, J.-P.; Rocha, L.A.; Shokuhfar, T. A first insight on the bio-functionalization mechanisms of TiO2 nanotubes with calcium, phosphorous and zinc by reverse polarization anodization. Surf. Coat. Technol. 2017, 324, 153–166. [Google Scholar] [CrossRef] [Scilit]
- Liao, C.; Li, Y.; Tjong, S.C. Visible-light active titanium dioxide nanomaterials with bactericidal properties. Nanomaterials 2020, 10, 124. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Zazpe, R.; Prikryl, J.; Gartnerova, V.; Nechvilova, K.; Benes, L.; Strizik, L.; Jager, A.; Bosund, M.; Sopha, H.; Macak, J.M. Atomic layer deposition AL2O3 coatings significantly improve thermal, chemical, and mechanical stability of anodic TiO2 nanotube layers. Langmuir 2017, 33, 3208–3216. [Google Scholar] [CrossRef] [Scilit]
- Alves, S.A.; Patel, S.B.; Sukotjo, C.; Mathew, M.T.; Filho, P.N.; Celis, J.-P.; Rocha, L.A.; Shokuhfar, T. Synthesis of calcium-phosphorous doped TiO2 nanotubes by anodization and reverse polarization: A promising strategy for an efficient biofunctional implant surface. Appl. Surf. Sci. 2017, 399, 682–701. [Google Scholar] [CrossRef] [Scilit]
- Yan, Y.; Wei, Y.; Yang, R.; Xia, L.; Zhao, C.; Gao, B.; Zhang, X.; Fu, J.; Wang, Q.; Xu, N. Enhanced osteogenic differentiation of bone mesenchymal stem cells on magnesium-incorporated titania nanotube arrays. Colloids Surf. B Biointerfaces 2019, 179, 309–316. [Google Scholar] [CrossRef] [Scilit]
- Cai, H.; Liang, P.; Hu, Z.; Shi, L.; Yang, X.; Sun, J.; Xu, N.; Wu, J. Enhanced photoelectrochemical activity of zno-coated TiO2 nanotubes and its dependence on zno coating thickness. Nanoscale Res. Lett. 2016, 11, 104. [Google Scholar] [CrossRef] [Scilit]
- Kandel, R.; Jang, S.R.; Shrestha, S.; Ghimire, U.; Shrestha, B.K.; Park, C.H.; Kim, C.S. A bimetallic load-bearing bioceramics of TiO2 @ ZrO2 integrated polycaprolactone fibrous tissue construct exhibits anti bactericidal effect and induces osteogenesis in MC3T3-E1 cells. Mater. Sci. Eng. C Mater. Biol. Appl. 2021, 131, 112501. [Google Scholar] [CrossRef] [Scilit]
- Paradowska, E.; Arkusz, K.; Pijanowska, D.G. The influence of the parameters of a gold nanoparticle deposition method on titanium dioxide nanotubes, their electrochemical response, and protein adsorption. Biosensors 2019, 9, 138. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Alivov, Y.; Singh, V.; Ding, Y.; Cerkovnik, L.J.; Nagpal, P. Doping of wide-bandgap titanium-dioxide nanotubes: Optical, electronic and magnetic properties. Nanoscale 2014, 6, 10839–10849. [Google Scholar] [CrossRef] [Scilit]
- Zhang, D.; Chen, J.; Xiang, Q.; Li, Y.; Liu, M.; Liao, Y. Transition-metal-ion (Fe, Co, Cr, Mn, Etc.) doping of TiO2 nanotubes: A general approach. Inorg. Chem. 2019, 58, 12511–12515. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Lu, M.; Xu, S.; Lei, Z.X.; Lu, D.; Cao, W.; Huttula, M.; Hou, C.H.; Du, S.H.; Chen, W.; Dai, S.W.; et al. Application of a novel porous tantalum implant in rabbit anterior lumbar spine fusion model: In vitro and in vivo experiments. Chin. Med. J. 2019, 132, 51–62. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Piglionico, S.; Bousquet, J.; Fatima, N.; Renaud, M.; Collart-Dutilleul, P.Y.; Bousquet, P. Porous tantalum vs. Titanium implants: Enhanced mineralized matrix formation after stem cells proliferation and differentiation. J. Clin. Med. 2020, 9, 3657. [Google Scholar] [CrossRef] [Scilit]
- Bencharit, S.; Byrd, W.C.; Altarawneh, S.; Hosseini, B.; Leong, A.; Reside, G.; Morelli, T.; Offenbacher, S. Development and applications of porous tantalum trabecular metal-enhanced titanium dental implants. Clin. Implant. Dent. Relat. Res. 2014, 16, 817–826. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Lu, R.J.; Wang, X.; He, H.X.; E, L.L.; Li, Y.; Zhang, G.L.; Li, C.J.; Ning, C.Y.; Liu, H.C. Tantalum-incorporated hydroxyapatite coating on titanium implants: Its mechanical and in vitro osteogenic properties. J. Mater. Sci. Mater. Med. 2019, 30, 111. [Google Scholar] [CrossRef] [Scilit]
- Zhang, K.; Wang, S.; Zhou, C.; Cheng, L.; Gao, X.; Xie, X.; Sun, J.; Wang, H.; Weir, M.D.; Reynolds, M.A.; et al. Advanced smart biomaterials and constructs for hard tissue engineering and regeneration. Bone Res. 2018, 6, 31. [Google Scholar] [CrossRef] [Scilit]
- Bobyn, J.D.; Stackpool, G.J.; Hacking, S.A.; Tanzer, M.; Krygier, J.J. Characteristics of bone ingrowth and interface mechanics of a new porous tantalum biomaterial. J. Bone Jt. Surgery. Br. Vol. 1999, 81, 907–914. [Google Scholar] [CrossRef]
- Huiskes, R.I.K.; Weinans, H.; Van Rietbergen, B. The relationship between stress shielding and bone resorption around total hip stems and the effects of flexible materials. Clin. Orthop. Relat. Res. 1992, 274, 124–134. [Google Scholar] [CrossRef] [Scilit]
- Oh, S.; Brammer, K.S.; Li, Y.S.J.; Teng, D.; Engler, A.J.; Chien, S.; Jin, S. Stem cell fate dictated solely by altered nanotube dimension. Proc. Natl. Acad. Sci. USA 2009, 106, 2130–2135. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Wang, N.; Li, H.; Lü, W.; Li, J.; Wang, J.; Zhang, Z.; Liu, Y. Effects of TiO2 nanotubes with different diameters on gene expression and osseointegration of implants in minipigs. Biomaterials 2011, 32, 6900–6911. [Google Scholar] [CrossRef] [Scilit]
- Anitha, V.C.; Lee, J.-H.; Lee, J.; Banerjee, A.N.; Joo, S.W.; Min, B.K. Biofilm formation on a TiO2 nanotube with controlled pore diameter and surface wettability. Nanotechnology 2015, 26, 065102. [Google Scholar] [CrossRef] [Scilit]
- Cheng, W.; Xu, X.; Lang, Y.; Cheng, Z.; Rizwan, M.; Tang, X.; Xie, L.; Liu, Y.; Xu, H.; Liu, Y. Anatase and rutile TiO2 nanoparticles lead effective bone damage in young rat model via the igf-1 signaling pathway. Int. J. Nanomed. 2021, 16, 7233–7247. [Google Scholar] [CrossRef] [Scilit]
- Lorenzetti, M.; Biglino, D.; Novak, S.; Kobe, S. Photoinduced properties of nanocrystalline TiO2-anatase coating on ti-based bone implants. Mater. Sci. Eng. C 2014, 37, 390–398. [Google Scholar] [CrossRef] [Scilit]
- He, J.; Du, Y.-e.; Bai, Y.; An, J.; Cai, X.; Chen, Y.; Wang, P.; Yang, X.; Feng, Q.J.M. Facile formation of anatase/rutile TiO2 nanocomposites with enhanced photocatalytic activity. Molecules 2019, 24, 2996. [Google Scholar] [CrossRef] [Scilit]
- Huai, X.; Rizzi, G.A.; Wang, Y.; Qi, Q.; Granozzi, G.; Fu, W.; Zhang, Z. Suppressed charge carrier trap states and double photon absorption in substitutional ta-doped TiO2-nt array. Nano Today 2022, 43, 101407. [Google Scholar] [CrossRef] [Scilit]
- Phan, A.; Stoner, H.M.; Stamatakis, M.; Koh, C.A.; Striolo, A. Surface morphology effects on clathrate hydrate wettability. J. Colloid. Interface Sci. 2022, 611, 421–431. [Google Scholar] [CrossRef] [Scilit]
- Shin, D.H.; Shokuhfar, T.; Choi, C.K.; Lee, S.-H.; Friedrich, C.J.N. Wettability changes of TiO2 nanotube surfaces. Nanotechnology 2011, 22, 315704. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Balla, V.K.; Bodhak, S.; Bose, S.; Bandyopadhyay, A.J.A.b. Porous tantalum structures for bone implants: Fabrication, mechanical and in vitro biological properties. Acta Biomater. 2010, 6, 3349–3359. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Stein, G.S.; Lian, J.B.; Van Wijnen, A.J.; Stein, J.L.; Montecino, M.; Javed, A.; Zaidi, S.K.; Young, D.W.; Choi, J.-Y.; Pockwinse, S.M.J.O. Runx2 control of organization, assembly and activity of the regulatory machinery for skeletal gene expression. Oncogene 2004, 23, 4315–4329. [Google Scholar] [CrossRef] [Scilit] [PubMed]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.