Skip to Content
ActuatorsActuators
  • Article
  • Open Access

3 March 2026

21 Pages

Active Composite Plates with Embedded Shape-Memory Alloy Wires for Vibration Damping

,
and
Department of Mechanical Engineering, California State University Northridge, Northridge, CA 91330, USA
*
Author to whom correspondence should be addressed.

Abstract

The integration of shape-memory alloy (SMA) wires into composite laminates offers a promising approach for active vibration damping. Towards this goal, this study investigates the damping behavior of hybrid random mat E-glass/epoxy composite plates with embedded SMA wires under electrically active and inactive conditions. The composites are tested using a Laser Doppler Vibrometer (LDV) and an impact hammer to assess the effect of SMA wire activation on the natural frequencies and vibration behavior of composites. For a fixed number of active SMA wires, differences in vibration behavior are evaluated between outer- and inner-wire activation configurations in both two-ply and four-ply composite plates. The results show that SMA wire activation significantly affects damping behavior, while the mode shapes remain unchanged. The magnitude and frequency of the first natural frequency as well as the quality factor (Q-factor) decrease in composites with activated SMA wires compared to the inactive configuration, indicating enhanced energy dissipation. Under the fully active condition, a reduction in vibrational amplitude of approximately 42–60% and a frequency shift of approximately 10–17% are observed. Compared to outer-wire activation, inner-wire activation results in greater reductions in vibration magnitude, reaching approximately 7–13%.

1. Introduction

The aerospace industry has conducted extensive research on advanced materials specifically designed to reduce vibrations, as these vibrations can have long-term detrimental effects on structural integrity [1,2,3]. The reduction of vibrations can be beneficial for small-scale aerospace applications such as drones, which have far greater restrictions on added structural reinforcement weight that reduces their efficiency. Among these materials, fiber-reinforced polymer (FRP) composites are notable due to their lightweight and high-strength characteristics, making them widely used in aerospace applications [4,5,6,7]. A key aspect of vibration control is damping capacity, which refers to a material’s ability to convert mechanical vibrational energy into heat that is then dissipated within the material [8,9]. This property is crucial for effectively absorbing mechanical energy during vibrations [10]. The interface between plies contributes to vibration damping through the viscoelastic behavior of the matrix, which enables stress relaxation as heat is generated by micro-scale friction between fibers [9,11,12]. The volume fraction of the composite’s constituents significantly influences damping, with the matrix playing the primary role. Increasing the matrix volume fraction enhances damping but compromises the overall stiffness of the composite [13]. Damping behavior in composites can also be influenced by manufacturing or fastening defects, such as cracks introduced by applied pressure. These micro-cracks can introduce additional friction, which aids in vibration damping, particularly under cyclic loading conditions, where repeated frictional interactions lead to increased heat generation [14,15]. While FRP composites generally offer superior damping capacity compared to metallic materials, their performance can be further optimized by tailoring the characteristics of their constituents and the orientation of their layers [16,17].
Recent innovations have led to the development of hybrid SMA–FRP composites, where shape-memory alloys (SMA) are embedded into FRP composites [18,19,20,21,22,23,24,25]. This integration provides active damping capabilities, significantly enhancing vibration suppression beyond the passive limits of conventional FRP composites. SMAs offer several effective approaches for vibration control, including their high damping characteristics, hysteretic damping behavior, variable stiffness properties, and the shape-memory effect [26,27]. Yet the thermal activation required for these alloys may limit their effectiveness in high-frequency vibration control, making them more suitable for low-frequency and quasi-static responses [28].
The integration of SMAs into FRP composites varies by application. For instance, for enhanced vibration damping, SMAs are placed in-plane along the neutral axis, while for improved impact resistance, they are integrated as stitches or similarly positioned in-plane along the neutral axis [29,30]. Additionally, the manufacturing of hybrid SMA–FRP composites presents several challenges, such as selecting an appropriate SMA wire diameter to prevent delamination, ensuring compatibility with the matrix and fibers, controlling the activation temperature of the SMAs, and optimizing wire placement and composite curing conditions [31]. Proper selection of the SMA wire diameter is particularly important, as larger diameter wires can generate excessive recovery forces that risk damaging the matrix–wire interface. Thinner wires may offer better adhesion as fabric plies do not deform as much to conform to the wires surface area, yet a larger SMA wire volume fraction is required to achieve equivalent net recovery stresses to that of thicker wires and may potentially increase the overall weight of samples [32]. Moreover, Wang et al. [33] discussed that polishing SMA wires with sandpaper and cleaning them with acetone before embedding can increase the pull-out force and prevent debonding.
The free vibration response of hybrid composite plates was analyzed in Ref. [34], using First-Order Shear Deformation Theory (FSDT) and Fourier series, showing that SMA wires altered natural frequencies. Factors such as SMA recovery stress, pre-strain, and the plate aspect ratio also influence these natural frequencies. Jin et al. [35] theoretically and numerically studied the nonlinear vibration of a cantilever hybrid composite beam driven by pre-stretched SMA fibers, revealing that the beam showed linear vibration near the phase transformation temperature and nonlinear behavior beyond it. In linear vibration, increasing temperature or eccentric distance raises the transverse amplitude while decreasing frequency, while in nonlinear vibration, both the amplitude and frequency increase with temperature or eccentric distance, exciting additional fundamental frequencies.
Zaman et al. [36] studied the effect of SMA orientation on composite properties, finding that a 45° SMA fiber orientation reduced the natural frequency but increased the damping ratio compared to a 0° orientation. Khalili et al. [37] investigated the low-velocity impact response of hybrid composite structures using FSDT and Fourier series with a springs–masses (SM) model for analytical solutions. The study demonstrated that incorporating SMA wires within the composite plates enhanced impact resistance by enhancing energy dissipation, damage tolerance, and reducing deflection, in-plane strains, and stresses.
The vibration control potential of SMA layers in elastic beams under blast loads at low temperatures was also studied in Ref. [38], showing that SMAs with high pre-strain at low temperatures offer superior passive vibration control compared to those exhibiting pseudo-elastic behavior. Oliveira et al. [39] showed that SMA microstructures have a large influence on the passive vibrational behavior of composite plates as detwinned martensite possesses larger hysteretic loops which dissipate more energy when compared to twinned martensite. Birman et al. [40] developed a micromechanical model to optimize the design of SMA fibers embedded in cross-ply composite plates for improved resistance to low-velocity impact. Their findings indicate that embedding SMA fibers in composite plates significantly reduces deflections, especially when distributed strategically, although higher activation temperatures can reduce their effectiveness due to temperature-induced compressive forces. Ke et al. [41] analyzed basalt-Kevlar plates with woven SMA wires to determine the dynamic stiffness and vibration characteristics. The results demonstrated an increase in damping behavior after full austenitic transformation when compared to non-hybrid samples. It is also reported that at increased frequencies, the effect of the SMA wires in their austenitic phase is negligible. Murugesan et al. [42] investigated the use of SMA Nitinol wires to enhance the vibration and damping characteristics of filament-wound CFRP hollow shafts. The results showed that embedding pre-stressed Nitinol wires in CFRP shafts improves their damping ratio and natural frequency, with a 7% increase in the first natural frequency and a 100% increase in the damping ratio at 6% pre-strain compared to plain CFRP shafts.
While prior studies have primarily focused on either fully activated wires to evaluate maximum achievable damping, or on passive damping enhancement, there is a lack of research that introduces a selective activation strategy. For example, Pappada et al. [43] analyzed the damping behavior of hybridized composite plates incorporating steel wires and SMA wires in their austenitic phase at room temperature due to a low Af of −15 °C without any applied pre-strain, thus functioning as a passive damping mechanism. An increase in damping ratio for the first bending frequency of the SMA hybrid sample was reported when compared to counterparts, while the non-hybrid sample had a larger damping coefficient for the second bending frequency. Moreover, Fallah et al. [44] performed numerical analysis on the effect of the SMA wire volume fraction with varying SMA wire distribution between plies for a carbon/epoxy microbeam to determine optimal SMA wire placement with respect to the neutral plane. It was reported that larger SMA wire density furthest from the neutral plane had the largest impact on damping. In addition, Zhang et al. [45] discussed the behavior of the natural frequency with respect to the SMA wire volume fraction near the top surface of a plate and temperature, showing that smaller SMA volume fractions led to a larger decrease in frequency at lower temperatures and larger volume fractions increased the logarithmic attenuation coefficient before the austenitic phase transformation. Consequently, the influence of the SMA wires geometric positioning, particularly the distinction between inner and outer activation, has not been investigated.
Building on these findings, this study advances the current understanding of the vibration behavior of hybrid SMA–FRP composites and investigates the effect of selective activation of wires, either in the inner or outer configuration, on damping performance. The research involves the fabrication of hybrid two- and four-ply, random mat E-glass/epoxy composite laminates incorporating SMA wires using a wet lay-up vacuum bagging process. To assess the effect of SMA wire activation within the neutral plane, the composites are evaluated using an LDV and an impact hammer. This analysis includes exploring how different activation scenarios influence natural frequencies, vibration behavior, and mode shapes of the composites. A temperature control circuit is used to actuate the SMA wires and prevent overheating. The study aims to explore how SMA wires affect vibration damping and mode shape patterns, providing insights into their effectiveness in improving the overall performance of FRP composites.

2. Materials and Methods

The Nickel Titanium (NiTi) alloy SMA wire under the trademark of FLEXINOL®LT, from Dynalloy Inc. (Irvine, CA, USA), with a 375 µm diameter was chosen in this study with phase transformation temperatures at austenite start (As) of ~30–40 °C, and austenite finish (Af) of 70 °C. This work considers single activation, without cyclic thermal loading; therefore, the full thermal hysteresis behavior is not critical to the present investigation. The number of wires embedded and their diameter were chosen based on achieving a balance between recovery stress, minimal disturbance to the laminate structure, manufacturability, and thermal considerations. Smaller-diameter SMA wires experience increased hysteresis and energy dissipation in their austenitic phase when compared to larger-diameter size wires, as reported by Chen and Shuh [46]. In contrast, Mahmood et al. [31] discussed that larger diameters may introduce stress concentrations arising from recovery stress and interlaminar defects, leading to delamination between plies.
The manufacturer of SMA wires specifies a resistance of 8.3 Ω/m, a recommended deformation of 3–5%, and a recommended current of 2250 mA. Randomly oriented chopped strand glass fiber preforms with a planar density of 0.427–0.488 kg/m2 from Fiberglast (part #250) were selected as the reinforcement for their planar isotropy and independence of fabric direction, ensuring that the damping energy remains invariant of direction, allowing for the dynamic damping of SMA wires to be the only varying effect of the samples. Also, planar isotropy of fabrics minimizes manufacturing variability caused by fiber misalignment in the wet lay-up process. The matrix system consisted of Rhino 1382 epoxy resin and 3182 epoxy hardener from Rhino Linings Co. (San Diego, CA, USA), which have a curing cycle of 24 h at room temperature. In particular, considering the transition temperature of 70 °C for SMA wires to achieve a full austenitic phase, a resin system that cures at room temperature is needed. The polymer is comprised of a 1:1 ratio by volume. The Rhino 1382/3182 resin system is suitable for this study due to its capacity to elongate up to 50% of its original length. The Rhino 1382 epoxy resin has a viscosity of 0.95–1.2 Pa s, and Rhino 3182 has a viscosity of 10–11 Pa s at room temperature. To further reduce the matrix viscosity and improve wetting capability, Flexer Epoxy Flexibilizer from Smooth-on Co. (Macungie, PA, USA) was utilized by 20% of the resin mass. This epoxy additive has a viscosity of 0.395 Pa·s room temperature.
The SMA wires were cut to 20.3 cm (8″) in length and were crimped at both ends. The wires were heated above their transition temperature to remove any residual strain introduced during the manufacturing process by the manufacturer. Each wire was pre-strained by 3% of its original length by applying a weight, as shown in Figure 1a. Prior to the integration of the SMA wires into the FRP composites, the surfaces of the wires were polished with 220-grit sandpaper and cleaned with acetone to ensure proper bonding with the matrix. The SMA–FRP laminates were manufactured using a wet layup vacuum bagging process, as shown in Figure 1. While randomly oriented glass fiber polymer composites fabricated using wet-lay-up vacuum bagging are not typically used in high-performance aerospace structures, primarily due to their lower fiber volume fraction and higher void content [5], they remain relevant for cost-sensitive and weight-restricted applications such as unmanned aerial vehicles (UAVs) as well as in secondary structural and non-aerospace applications, where effective vibration damping is important and material simplicity is favorable.
Figure 1. (a) Crimped SMA wire with 3% pre-straining, original wire length: 17.3 cm, final wire length after loading 600 g of weights: 17.8 cm; (b) Integration of six (or eight) SMA wires utilizing 3D-printed guides and mold to secure SMA wires in place; (c) Composite lay-up in the vacuum bag; (d) Fabricated hybrid SMA–FRP composite after 24 h cure cycle.
A 3D-printed mold and fixtures were utilized to keep the wires parallel to one another and maintain a low level of tension to prevent movement during the lay-up process. The mold was covered with a release film and sprayed with a release agent around the pins to prevent adhesion from the resin to the mold. Depending on the manufacturing scenario, either two or four layers of randomly oriented chopped E-glass fiber mats were cut into 10.16 × 17.78 cm2 (4″ × 7″). The wet lay-up was prepared by applying one coat of resin and one ply of dry fiber mat on the mold. A small amount of additional resin was poured over the fiber mat, ensuring it was thoroughly saturated. A roller was utilized to press and remove excess resin from the ply before subsequent plies. After half the number of plies were laid up, the wires were placed with the 3D-printed wire fittings onto the mold and secured by the pins, as shown in Figure 1b. John and Hariri [47] discussed that a simple linear spatial arrangement on or in a structure can be adequate in inducing a dynamic structural change. Accordingly, the SMA wires were placed on the neutral plane of the laminate, i.e., between the second and third ply for the four-ply samples and between the first and second ply for the two-ply samples. This choice was based on preserving laminate symmetry and avoiding unintended curvature by SMA wire activation. In the 6-wire specimens, the wires were spaced approximately 10.89 mm apart, while in the 8-wire specimens, the spacing was reduced to about 8.47 mm to accommodate the additional wires and maintain even spacing between each wire and the edge of the laminate. Additional resin was brushed onto the wires before the subsequent fabric plies were placed. The remaining fabric plies were applied, with each layer thoroughly saturated with resin as in the previous steps. A perforated release film was utilized to allow for the extra resin to seep through and be absorbed by the breather. A vacuum bag was placed over the entire layup and secured with sealant tape. Vacuum was pulled by a pump and held for 24 h until the laminate was fully cured, as displayed by Figure 1c. The cured laminate was demolded, as shown in Figure 1d, and trimmed to a 7.62 × 15.24 cm2 (3″ × 6″) rectangular shape utilizing a bandsaw.
This study aimed to evaluate whether increasing the number of active wires would result in improved damping performance. For this reason, configurations with 6 and 8 SMA wires were considered to examine the effect of wire quantity. Increasing the number of wires reduces the spacing between adjacent wires, potentially complicating fabrication and affecting laminate integrity. Additionally, incorporating more wires would increase the overall heating demand during activation, leading to higher power requirements and potential thermal management challenges.
Accordingly, four laminates were manufactured and tested; 2P-8W (2 fabric plies and 8 wires), 4P-8W (4 fabric plies and 8 wires), 2P-6W (2 fabric plies and 6 wires), and 4P-6W (4 fabric plies and 6 wires), as listed in Table 1. In the sample notation, P denotes the number of plies and W denotes the number of wires. Table 1 also reports the mass of each composite specimen and the mass of the embedded SMA wires. The resulting SMA wire weight fraction was calculated by dividing the weight of the embedded SMA wires by the total weight of the SMA–FRP composite specimen. It can be seen that the SMA wire mass contributed between 6.81 and 19.91% of the total composite weight, changing with the number of fabric plies and wire count. This variation is also influenced by local differences in the areal density of the glass fiber mat, which can differ slightly, especially in composites fabricated by a wet lay-up process. Similarly, due to the local differences of plies and manufacturing processes, 20 points (n) were measured near the edges and center of the sample to determine the thickness of the samples to a 95% confidence. The activation status of the SMA wires in each laminate is denoted using the labels NA, OA, IA, and FA, as defined in Table 2. SMA wires were numbered sequentially from top to bottom (see Figure 1d). NA denotes no activation, while FA corresponds to the activation of all embedded wires. To investigate the influence of wire embedment location within the neutral plane on damping performance, the number of active wires was held constant, while their positions were changed within the width of the laminate. Specifically, in laminates with six embedded wires, the OA configuration (outer two wire pairs active) was compared against the IA configuration (inner four wires active), with both configurations having a total of four active wires. Additionally, in laminates with eight embedded wires, the OA configuration (outer three wire pairs active) was compared against the IA configuration (inner six wires active), with both configurations having a total of six active wires.
Table 1. Manufactured SMA–FRP composite samples (n = 20 for average laminate thickness with 95% confidence intervals).
Table 2. Activation code of SMA wires for manufactured samples. The numbering and locations of the active wires are illustrated in Figure 1d; NA (no activation), OA (outer activation), IA (inner activation), and FA (full activation) are used to denote the four SMA wire activation configurations investigated in this study.
A Proportional Integral Derivative (PID) temperature control circuit (see Figure 2) was utilized to regulate the applied electrical current and hence maintain the wires at a predetermined temperature threshold of 70 °C, which is the full austenitic phase transformation of SMA wires. The conservative temperature threshold was set to prevent thermal degradation of the samples due to repeated heating of the wires during testing. The PID controller adjusted the current in real time based on the difference between the setpoint and the actual temperature, which was measured by a thermocouple placed on the surface of the composite, directly above an embedded SMA wire. Accurate measurement of the temperature of thin SMA wires embedded in thicker laminates was more challenging, due to the greater thermal lag, with increased laminate thickness compared to thinner laminates. Kazi et al. [48] mentioned that it is impossible to directly measure the temperature of thin wires, especially through direct contact as it affects the thermal response. Moreover, Yang et al. [49] reported discrepancies between numerical and experimental results of a 1 mm thick SMA wire due to attached thermocouples enhancing heat dissipation. Additionally, Theodore and Bishay [18] stated that isolating and attaching a thermocouple directly on an SMA wire greatly affected the system since the convection heat losses led to non-uniform phase transformations. In this study, the temperature was referenced at the surface of the laminates. This approach was justified by the relatively small heat capacity of SMA wires compared to the surrounding material, causing most of the heat generated by the SMA wires to be absorbed by the laminate until a steady state was reached, ensuring uniform phase transformation. In thicker laminates, thermal lag was increased, so it was expected that the system would require more time to reach steady state. A Fluke thermal camera was utilized to validate the actual wire temperature. Figure 3 shows a sample image from the thermal camera. The thermal camera confirmed the temperature distribution across the samples, showing how heat propagated from the wires through the laminate. The average time required to reach the threshold temperature was approximately 3 min and 50 s for the two-ply samples, and around 6 min and 8 s for the four-ply samples, with an applied current of 0.9–1 A, trimmed edge, consistent with the increased thermal mass and thermal lag of the thicker laminate. This increased thermal resistance in thicker laminates slows the measurement of wire temperature for the thermocouple as well as the thermal camera, which measures the surface temperature instead of the wire temperature.
Figure 2. PID control circuit used to regulate current passed through SMA wires with the use of a current sensor thermocouple and MOSFET to maintain set temperature. MOSFET regulates current applied to the SMA wires in tandem with the LCS712 current sensor.
Figure 3. Thermal camera image of 2P-8W sample after PID controller has reached its threshold temperature after 3:30 min at 0.9 A, where the + mark denotes the temperature of an SMA wire and the white box represents an average snip with temperatures denoted on the top.
A metal vice fixture was utilized to secure the composite samples in a vertical orientation, as shown in Figure 4a. The fixture was clamped to the workbench using a C-clamp to prevent unwanted movement of the fixture during excitation. The sample was secured to the vice fixture, where the length that was in contact with the fixture was 12.7 mm; the entire contact area was 967.74 mm2, which left a free length of 25.4 mm to the end of the tabs where the wires protruded or 146.05 mm to the trimmed edge. The sample was secured by tightening two screws utilizing a torque screwdriver to 2.5 Nm. All four configurations were tested while the sample remained secured to avoid discrepancies during fastening that could affect the results. A lead from the LCS712 current sensor was connected to the first terminal of the SMA wire, and the positive lead was connected to the wire at the opposite end to complete the circuit, as illustrated in Figure 4a. A Polytec Scanning Laser Doppler Vibrometer (PSV-500HV with PSV-I-550 Xtra Scanning Head) sourced from Polytec, Irvine, CA, USA was used to measure the velocity of different points on the surface of the laminate (see Figure 4c). The laser beam was focused on the blue square shown in Figure 4b when performing single shot measurements. The sample was excited using an impact hammer with a built-in force transducer, applying an impact force of 60 mN with 5% uncertainty (i.e., range 57–63 mN). The sample was struck near its fixed end. The frequency response (FRF) graphs of the velocity magnitude of excitation divided by the force applied by the impact hammer at the targeted point were collected.
Figure 4. (a) Testing fixture with temperature-regulating PID controller; (b) SMA–FRP hybrid sample in vice fixture with marked striking point for the impact hammer and test point for the SLDV, (c) Testing setup of vibration tests.

3. Results and Discussion

3.1. Experimental Modal Analysis of Two-Ply SMA–FRP Samples

The average thickness of the two-layer 2P-6W and 2P-8W laminates was measured to be about 0.867 and 1.049 mm, respectively, as presented in Table 1. The samples were tested under several activation configurations: NA (no activation) for both 2P–6W and 2P–8W samples; OA (outer activation) corresponding to activation of the two outermost wire pairs in the 6-wire sample and the three outermost wire pairs in the 8-wire sample; IA (inner activation) corresponding to activation of the four inner wires in the 6-wire sample and the six inner wires in the 8-wire sample; and FA (full activation) for both the 6-wire and 8-wire samples. The activation code of the samples can be referenced in Table 2. The combination of wires was chosen to maintain symmetrical actuation of SMA wires across the sample and to analyze the effects of zone activation of wires. An impact force of 60 mN with an allowable 5% deviation (3 N) was utilized as previously stated to excite the samples and a current ranging from 0.9–1 A was applied to actuate the wires. Figure 5 demonstrates the SMA wire activation for the 2P–8W-OA and 2P-8W-IA configurations.
Figure 5. Two representative activation patterns were selected for the 2P-8W sample, where the red lines depict the electrical connection path for: (a) Outer-wire activation (2P-8W-OA), in which the outer 3 wires of the sample are active for a total of 6 wires, and the two middle wires are inactive; (b) Inner-wire activation (2P-8W-IA), where the inner 6 wires of the sample are active, and the outermost wires are inactive.
To identify the mode shapes associated with the observed modes, an experimental modal analysis was performed. All previous activation configurations were analyzed in this analysis. A grid of 15 scan points was created across the surface of the samples to measure the frequency response of these points. As the sample was excited, the vibrational behavior was mapped to create an overlay of the sample’s oscillations with respect to each mode. A total of three measurements were recorded for each point and complex averaging was utilized to determine the averaged value, maintaining the coherence at each point above 0.85, which is why the study was limited to a bandwidth of 312.5 Hz as elevated noise levels were obtained past 400 Hz. The Q-factor was obtained from the measured frequency–response curve using the half-power (−3 dB) bandwidth method, as computed through Polytec’s software (PSV 10.1) during the frequency sweep. The frequency resolution was 97.66 mHz. Complex averaging was utilized since an impulse hammer was utilized to excite the sample and 3 strikes were averaged. The peaks of interest are the bending modes which are determined by the 15-point scans taken of the samples, as shown in Figure 6.
Figure 6. The colors of the samples correspond to the magnitude (mm/s/N) where the light red color corresponds to the maximum +z value and green corresponds to the maximum -z value, with black being equal to 0 magnitude: (a) First and (b) second mode shapes for 2P-8W-NA; (c,d) are first and second mode shapes for 2P-8W-FA.
Figure 7 shows the frequency response graphs of the two-ply 8-wire 2P-8W sample at the different wire activation configurations. Figure 6 shows the first and second modes for no active wires and with all 8 active wires. These are the first and second bending modes with no active wires and with all 8 wires active. Figure 6 reveals that the activation of wires did not alter the mode shapes, highlighting the ability of SMA wires to improve vibration performance without altering the fundamental characteristics of the structure. Table 3 lists the magnitude, frequency, and quality factor (Q-factor) of the first two observed modes of vibration within the bandwidth of the study (312.5 Hz) for the four activation configurations. It can be observed that the first natural frequency shifted to lower values with the activation of wires. A maximum shift of 2.15 Hz was observed between no active wires (2P-8W-NA) and all 8 active wires (2P-8W-FA), indicating a 16.9% reduction. In addition, the amplitude of vibration of the first mode also decreased significantly. A maximum reduction of 190.2 (mm/s)/N was observed between the no-activation configuration (2P-8W-NA) and the full-wire activation configuration (2P-8W-FA). This is a 59.5% reduction in vibration amplitude. Compared to the no-activation configuration (2P-8W-NA), the inner-wire activation configuration (2P-8W-IA) showed a 47.4% reduction in amplitude, whereas the outer-wire activation configuration (2P-8W-OA) showed a 40.5% reduction. The shift of the first mode to lower frequencies was 15.4% and 13.1% for the outer-wire activation configuration (2P-8W-OA) and the inner-wire activation configuration (2P-8W-IA), respectively, when compared to the no-activation configuration (2P-8W-NA). These results indicate that activating the inner wires leads to a more significant reduction in vibration amplitudes compared to activating the outer wires due to potentially improved thermal and mechanical stability within the central region of the laminate. However, activating the inner wires leads to slightly more reduction in the first natural frequencies. The deformation from the scanning tests revealed that the second hump in the curves, that appears between 50 and 100 Hz, is not associated with a specific mode, but rather a combination of modes. The second bending mode corresponds to the third peak in curves, happening between 100 and 150 Hz. Interestingly, the trend in amplitude and frequency reduction with activation of more SMA wires disappeared at higher frequencies. The configuration 2P-8W-FA, for example, had a higher magnitude in the second mode compared to 2P-8W-NA. It was also observed that 2P-8W-FA had a second mode occurring at a higher frequency than that of 2P-8W-NA. Moving to even higher frequencies, it was seen that the vibration amplitudes of all configurations with active wires were lower than 2P-8W-NA within the chosen bandwidth, highlighting the nonlinearity of SMA wires. Configuration 2P-8W-NA had a fourth peak at 284.4 Hz with an amplitude of 61.6 (mm/s)/N, corresponding to the torsional mode. The mode was not present for the test configuration where SMA wires were active, which can entail that it was outside the range being measured due to a possible increase in frequency at which it occurs. This suggests that the effect of material nonlinearities was more pronounced at higher frequencies, further complicating the behavior of such hybrid active composite plates, as was presented by Sanchez et al. [50]. This also correlates with the observation by Yuvaraja and Senthilkumar [2] that the natural frequencies shift to larger values due to the nonlinear behavior of the SMA wires.
Figure 7. FRF graph for 2P-8W sample, tested in various configurations: 2P-8W-NA (no activated wires), 2P-8W-OA (wires 1, 2, 3, 6, 7, 8 are active), 2P-8W-IA (wires 2, 3, 4, 5, 6, 7 are active), 2P-8W-FA (all wires are active). The insert shows a zoomed in view of the first mode.
Table 3. Magnitude, frequency, and quality factor from FRF data for the 2P-8W sample.
Looking at the Q-factors in Table 3, it can be observed that the Q-factor decreased with activation of SMA wires for both the first and second bending mode, where this trend is consistent across all studied configurations. The samples were clamped at one end and excited near their midpoint close to the fixture, which primarily induced bending vibrations; so, as a result, torsional mode was not observed. For the first mode, all configurations with active wires had a lower Q-factor than 2P-8W-NA with no active wires. Since the Q-factor is inversely related to damping capacity, this indicates that lower Q-factors correspond to higher damping. The activation of SMA wires notably reduced the Q-factor, particularly in the first mode, enhancing the composite’s ability to dissipate energy and effectively reduce vibrations. For the second mode, the effect of activation on the Q-factor was not as significant as that of the first mode.
Figure 8 shows the frequency response of the targeted point at the cantilevered 2P-6W SMA–FRP plate’s tip at all considered SMA wire activation configurations. To verify repeatability, two additional specimens of the selected configuration (2-ply laminate with six SMA wires) were fabricated using similar materials and processing conditions. The FRF magnitude plots for the inactive (NA) and fully activated (FA) states are provided in the Supplementary Material. As can be seen in Figure 8, the magnitude and frequency of the first mode decreased with the activation of the SMA wires, similar to the 2P-8W sample. When comparing 2P-6W-OA (outer wires active), the peak corresponding to first bending occurred at a lower frequency than 2P-8W-NA (no activated wires) as well as 2P-6W-IA (inner wires active), even though 2P-6W-IA and 2P-6W-OA have the same number of active wires. Configuration 2P-6W-OA showed a greater shift in frequency (1.29 Hz) than 2P-6W-IA (0.75 Hz). Similar to the two-ply, eight-wire sample, activation of SMA wires near the edges of the sample caused a larger decrease in frequency, while activation of the wires near the center of the sample had a larger effect in reducing the overall magnitude of the mode. Configuration 2P-6W-OA had a decrease in magnitude of 102.6 (mm/s)/N, while 2P-6W-IA had a decrease of 120.1 (mm/s)/N. The Q-factor exhibited a similar trend where the largest difference was observed for the activation of the outer wires (2P-6W-OA) such that the Q-factor decreased by 6.73, while in inner activation (2P-6W-IA), the Q-factor decreased by 5.99. The second mode of the 2P-6W sample also showed a similar decrease in amplitude and frequency with the activation of SMA wires. However, for the second mode, activating the outer wires yielded a more prominent decrease in frequency as well as magnitude when compared to the first mode, where 2P-6W-IA yielded lower magnitude values, as observed in Table 4. The Q-factor for both the first mode and second mode decreased with subsequent SMA activation. The fully active configuration yielded the largest decrease, which equivalently signifies an increase in the damping coefficient. The effects were more prominent for the first mode, with 2P-6W-OA having the second largest decrease followed by 2P-6W-IA.
Figure 8. FRF graph for 2P-6W sample, tested in various configurations: 2P-6W-NA (no activated wires), 2P-6W-OA (wires 1, 2, 5, 6 are active), 2P-6W-IA (wires 2, 3, 4, 5 are active), and 2P-6W-FA (all wires are active). The insert shows a zoomed in view of the first mode.
Table 4. Magnitude, frequency, and quality factor from FRF data for the 2P-6W sample.

3.2. Experimental Modal Analysis of Four-Ply SMA–FRP Samples

The average thickness of the four-layer 4P-6W and 4P-8W laminates was measured to be about 2.463 and 2.187 mm, respectively, as listed in Table 1. The samples were tested under several activation configurations: NA (no activation) for both 4P–6W and 4P–8W samples; OA (outer activation), corresponding to activation of the two outermost wire pairs in the 6-wire sample and the three outermost wire pairs in the 8-wire sample; IA (inner activation), corresponding to activation of the four inner wires in the 6-wire sample and the six inner wires in the 8-wire sample; and FA (full activation) for both the 6-wire and 8-wire samples. The activation code of the samples can be referenced in Table 2. These combinations of wires were chosen to analyze the effects of zone activation of the wires, while maintaining symmetrical activation of the SMA wires across the sample. An impact force of 60 mN with an allowable 5% deviation (3 mN) was applied to excite the samples and a current ranging from 0.9 to 1 A was applied to activate the wires.
Figure 9 shows the frequency response curves of the targeted point for all configurations of SMA wire activation in the 4P-8W sample, while Table 5 lists the extracted magnitude, frequency, and Q-factor for all observed modes of vibration in the same frequency bandwidth of the study. Since this four-ply sample was much thicker than the two-ply samples analyzed in the last section, it was observed that the effect of SMA wire activation on the first natural frequencies was less prominent due to the low volume fraction of SMA wires. The first mode occurred at almost the same natural frequency for all configurations: 35.55–36.05 Hz. However, the magnitude of vibration was reduced significantly with the activation of SMA wires, where a decrease of 42.1% was seen in 4P-8W-IA (inner wire activation) and a decrease of 33.5% was seen in 4P-8W-OA (outer activation of SMA wires). A maximum reduction of 60.4% in magnitude of vibration was achieved in 4P-8W-FA (with all SMA wires active) when compared to 4P-8W-NA (no active wires). The second bending mode was not observed for 4P-8W-NA, which can entail the mode being outside the range being analyzed. The absence of the mode in the NA case is due to a combination of measured bandwidth limitations and signal-to-noise considerations. Preliminary tests performed at larger bandwidths past 400 Hz showed elevated noise levels. The second bending mode was present for the rest of the configurations, where 4P-8W-OA had the largest magnitude of vibration of 11.24 Hz. The second bending mode in 4P-8W-IA and 4P-8W-FA had magnitudes of vibration of 5.80 and 6.73 (mm/s)/N, respectively. The second bending mode occurred at 241.99 Hz in 2P-8W-IA, at 266.89 Hz in 4P-8W-OA, and at 270.12 Hz in 4P-8W-FA.
Figure 9. FRF graph for 4P-8W sample, tested in various configurations: 4P-8W-NA (no activated wires), 4P-8W-OA (wires 1, 2, 3, 6, 7, 8 are active), 4P-8W-IA (wires 2, 3, 4, 5, 6, 7 are active), and 4P-8W-FA (all wires are active). The insert shows a zoomed in view of the first mode.
Table 5. Magnitude, frequency, and quality factor from FRF data for the 4P-8W sample.
The Q-factor did not follow the trend of the previous samples, with 4P-8W-FA (full SMA wire activation) yielding the lowest Q-factor or largest damping increase, possibly because of a higher matrix volume fraction in the 4P-8W sample compared to the rest of the samples. In the first bending mode, 4P-8W-IA saw the largest damping increase which was closely followed by 4P-8W-FA. The second bending mode followed the same trend as the first bending mode, where 4P-8W-IA had the lowest Q-factor followed by 4P-8W-FA, and lastly by 4P-8W-OA.
Figure 10 shows the frequency response curves of the targeted point for all cases of SMA wire activation in the 4P-6W sample, while Table 6 lists the extracted magnitude, frequency, and Q-factor for all observed modes of vibration in the same frequency bandwidth of the study. The first natural frequency shifted to lower values with activation of SMA wires in the sample, where a maximum shift of 15.9% occurs between the no active (4P-6W-NA) and full activation of all wires (4P-6W-FA) configurations. Again, the shift to lower frequencies was slightly more in the case of outer wire activation (4P-6W-OA) than in the case of inner wire activation (4P-6W-IA) for the first bending mode as in the two-ply samples. Configurations 4P-6W-OA and 4P-6W-OA exhibited a shift of 4.30 and 3.61 Hz, respectively, in the first mode. The maximum reduction in the amplitude of vibration of the first mode was 47.4%, occurring between the no active (4P-6W-NA) and all active wires (4P-6W-FA) configurations. Configurations 4P-6W-OA and 4P-6W-IA had a reduction in amplitude of around 29.5% and 23.9%, respectively, compared to the no active (4P-6W-NA) configuration, following the previously seen trend where activation of outer wires had a more prominent effect in shifting the modal frequency and the inner activation had a more prominent impact on reducing the magnitude of the mode. Moreover, there was no observable second bending mode for 4P-6W-NA (no activated wires), possibly due to it occurring past the measured range. In the 4P-6W-OA configuration, a second bending mode occurred at 255.47 Hz, with a magnitude of 12.95 (mm/s)/N, while in 4P-6W-IA, a second bending mode occurred at 232.91 Hz, with a magnitude of 23.20 (mm/s)/N.
Figure 10. FRF graph for 4P-6W sample, tested in various configurations: 4P-6W-NA (no activated wires), 4P-6W-OA (wires 1, 2, 5, 6 are active), 4P-6W-IA (wires 2, 3, 4, 5 are active), and 4P-6W-FA (all wires are active). The insert shows a zoomed in view of the first mode.
Table 6. Magnitude, frequency, and quality factor from FRF data for the 4P-6W sample.
Activating the innermost four wires (4P-6W-IA) led to further reduction in the magnitude and Q-factor of the first natural frequencies with respect to the case of activating the outermost two wires (4P-6W-OA); however, the difference was minimal, as listed in Table 6.
Overall, while the SMA wire mass contributed between 6.81% and 19.91% of the total specimen weight (see Table 1), the normalized percent change in the Q-factor did not scale proportionally with the SMA weight fraction. Notably, the 4P-6W specimen with 6.81% SMA content by weight exhibited the highest relative change in the Q-factor on the first mode (~39%), whereas the 2P-8W sample with 19.91% SMA content by weight showed the lowest (~17.5%). This suggests that simply increasing the SMA mass does not linearly enhance damping performance. Instead, the observed trends indicate that the effect of SMA activation on energy dissipation is dominant, beyond what might be expected from added mass alone.
A visual inspection of the specimens was conducted after testing. According to Theodore and Bishay [18], when debonding between the wires and the resin occurs, discoloration around the wires is observed. This happened in their study when the samples were significantly deformed. The samples of the current study were not significantly deformed, and no discoloration around the wires was noticed upon careful visual evaluation. This indicates no macroscopic debonding. Future studies can focus on microscopic evaluation of debonding around embedded SMA wires at various levels of deformation.
Several factors may influence the vibrational behavior of a hybrid SMA–FRP composite system. One such factor is passive damping, as reported by Zhang et al. [51], where it was shown that passive vibration control in NiTi-steel-rope-reinforced composites can be achieved without significantly affecting the natural frequency. Damanpack et al. [38] also discussed the inherent passive damping by having embedded pre-strained SMA wires at low temperatures due to martensite reorientation. This mechanism contributes to the dynamic behavior observed in NA configurations where all wires are inactive and the wires remain in the martensitic phase. The partially active cases IA and OA are a combination of passive damping due to the inactive wires as well as active damping due to the pseudoelastic wires and phase-transformation-induced energy dissipation which requires a smaller critical stress to activate with increasing temperature, as reported by Bayat et al. [52]. A comparison between SMA–FRP and pure FRP laminates is also discussed by Verma et al. [53], demonstrating that SMA–glass–FRP hybrid specimens exhibited higher damping ratios compared to baseline glass–FRP (SMA-free) specimens, indicating that SMAs have energy dissipation capabilities, thus acting as dampers. Beyond the damping contribution, thermal activation of the hybrid system introduces additional thermomechanical effects. Heating the polymer matrix leads to thermal softening as the temperature approaches the glass transition temperature of the polymer, thus reducing the effective stiffness and the natural frequency [54]. Prior analytical work on glass fiber composite beams with embedded SMA wires has shown that changes in tensile modulus, internal recovery stress, thermal expansion mismatch, and overall density must all be considered when evaluating natural frequency variations in SMA composites [55].
Furthermore, it should be noted that environmental conditions, particularly forced convection and room temperature variations, may influence SMA phase transformation and actuation stability, as noted by Kazi et al. [47] and Theodore and Bishay [18]. While these effects are negligible under controlled laboratory conditions, they should be considered in real-world applications, where environmental temperature and airflow conditions may change.
The proposed hybrid composite laminates have practical limitations. The addition of SMA wires increases the overall weight of the composites as well as the manufacturing cost. In addition, activation requires electrical power for joule heating, which may limit implementation in power-sensitive applications. Despite the increase in structural mass, manufacturing cost, and activation energy required, the system provides active damping, which makes it suitable for applications where adaptive dynamic performance is critical. In this context, the proposed hybrid laminate may be investigated as a potential candidate within the broader class of morphing structural materials [56].

4. Conclusions

This study demonstrates the promising potential of embedding SMA wires within FRP composites to achieve active vibration control. The improvement in damping performance was investigated experimentally by comparing the behavior of laminates with wire activation to their behavior without wire activation. The results show that activating SMA wires significantly enhances the damping behavior of the composites, particularly in the bending modes, by reducing the magnitude and frequency of the first natural frequency. For instance, in the two-ply, 8-wire configuration, a comparison between no active wires and all active wires revealed a 16.9% reduction in frequency to 10.55 Hz and a 59.5% decrease in vibration amplitude to 129.3 (mm/s)/N. Yet the benefits may diminish or even result in adverse effects at higher frequencies due to the nonlinear behavior of SMA wires, which can lead to an increase in both amplitude and frequency. Additionally, across all tested cases, the Q-factors for samples with active SMA wires were consistently lower than that of the case with no active wires. Since the Q-factor is inversely related to the damping capacity, this trend indicates that SMA activation enhances energy dissipation, with the most notable improvement observed in the first bending mode. The FFT plots also revealed that the mode shapes remained unchanged by the activation of the SMA wires, while the response magnitudes were reduced. This demonstrates the ability of SMA wires to actively improve vibrational performance without changing the key modal parameters of the hybrid structure, such as the mode shapes. In thicker samples, the influence of SMA wire activation on the natural frequencies was often less pronounced, yet significant reductions in vibration magnitude, up to 60.4%, were achieved. Additionally, it was found that activating inner SMA wires within the FRP composites significantly reduced the vibration amplitude compared to activating the outer wires, as demonstrated in the two-ply, 8-wire sample, which achieved a 47.4% reduction in amplitude for the inner wires’ versus 40.5% for the outer wires’ activation. While the inner wire activation resulted in a slightly smaller shift in the first natural frequency, this trend of reduced vibration amplitude and natural frequency persisted at higher frequencies. The results of this study may open avenues for future research and applications of embedding SMA wires within FRP composites, showcasing their potential for tunable vibration control.

Supplementary Materials

The following supporting information can be downloaded at: https://www.mdpi.com/article/10.3390/act15030148/s1, Figure S1: The FRF response is presented in Figure S1a, while a zoomed-in view of the first resonance peak is provided in Figure S1b to highlight the frequency shift and magnitude changes. NA and FA indicate the non-activated and fully activated SMA configurations, respectively. The labels 2P–6W–NA and 2P–6W–FA correspond to the results presented in the main manuscript. S1 and S2 denote the two additional specimens fabricated for repeatability assessment, and T1 and T2 indicate repeated measurements conducted on the same specimen.

Author Contributions

Methodology, validation, visualization data curation, investigation, A.P. and M.P.; formal analysis, A.P., M.P. and P.L.B.; writing—original draft preparation, A.P.; writing—review and editing, M.P. and P.L.B.; conceptualization, supervision, resources, project administration, funding acquisition, M.P. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Institutional Review Board Statement

Not applicable.

Data Availability Statement

The original contributions presented in this study are included in the article/Supplementary Material. Further inquiries can be directed to the corresponding author.

Acknowledgments

The authors acknowledge the support of the Department of Mechanical Engineering and Multi-Scale Mechanical Characterization Laboratory (MMCL) at California State University, Northridge (CSUN).

Conflicts of Interest

The authors declare no conflict of interest.

Abbreviations

The following abbreviations are used in this manuscript:
SMAShape-Memory Alloy
FRPFiber-Reinforced Polymer
PIDProportional Integral Derivative
AfAustenite finish
AsAustenite start

References

  1. Mccombe, G.P.; Etches, J.A.; Bond, I.P.; Mellor, P.H. Magnetostrictive Actuation of Fiber-Reinforced Polymer Composites. J. Intell. Mater. Syst. Struct. 2009, 20, 1249–1257. [Google Scholar] [CrossRef] [Scilit]
  2. Yuvaraja, M.; Senthilkumar, M. Comparative Study on Vibration Characteristics of a Flexible GFRP Composite Beam Using SMA and PZT Actuators. Procedia Eng. 2013, 64, 571–581. [Google Scholar] [CrossRef] [Scilit]
  3. Kireitseu, M.; Hui, D.; Tomlinson, G. Advanced Shock-Resistant and Vibration Damping of Nanoparticle-Reinforced Composite Material. Compos. Part B Eng. 2008, 39, 128–138. [Google Scholar] [CrossRef] [Scilit]
  4. Amirkhosravi, M.; Pishvar, M.; Cengiz Altan, M. Fabricating High-Quality VARTM Laminates by Magnetic Consolidation: Experiments and Process Model. Compos. Part A Appl. Sci. Manuf. 2018, 114, 398–406. [Google Scholar] [CrossRef] [Scilit]
  5. Amirkhosravi, M.; Pishvar, M.; Altan, M.C. Improving Laminate Quality in Wet Lay-up/Vacuum Bag Processes by Magnet Assisted Composite Manufacturing (MACM). Compos. Part A Appl. Sci. Manuf. 2017, 98, 227–237. [Google Scholar] [CrossRef] [Scilit]
  6. Mace, T.; Schwingshackl, C.W. Predicting Damping in Geometrically Complex Composite Structures via Increased Interlaminar Homogenisation. Compos. Part B Eng. 2024, 286, 111769. [Google Scholar] [CrossRef] [Scilit]
  7. Chandra, R.; Singh, S.P.; Gupta, K. Damping Studies in Fiber-Reinforced Composites—A Review. Compos. Struct. 1999, 46, 41–51. [Google Scholar] [CrossRef] [Scilit]
  8. Yin, F.; Iwasaki, S.; Ping, D.; Nagai, K. Snoek-Type High-Damping Alloys Realized in β-Ti Alloys with High Oxygen Solid Solution. Adv. Mater. 2006, 18, 1541–1544. [Google Scholar] [CrossRef] [Scilit]
  9. Treviso, A.; Van Genechten, B.; Mundo, D.; Tournour, M. Damping in Composite Materials: Properties and Models. Compos. Part B Eng. 2015, 78, 144–152. [Google Scholar] [CrossRef] [Scilit]
  10. Zhao, J.; Wang, F.; Zhang, X.; Liang, L.; Yang, X.; Li, Q.; Zhang, X. Vibration Damping of Carbon Nanotube Assembly Materials. Adv. Eng. Mater. 2018, 20, 1700647. [Google Scholar] [CrossRef] [Scilit]
  11. Swain, A.; Palani, V.; Francis, S.; Thomas, B.; Roy, T. Viscoelastic Modelling and Analysis of Two-Dimensional Woven CNT-Based Multiscale Fibre Reinforced Composite Material System. Discov. Nano 2024, 19, 74. [Google Scholar] [CrossRef] [Scilit]
  12. Agarwal, G. Comparative Investigations on Fracture Toughness and Damping Response of Fabric Reinforced Epoxy Composites. J. Polym. Mater. 2023, 39, 255–267. [Google Scholar] [CrossRef] [Scilit]
  13. Ni, R.G.; Adams, R.D. A Rational Method for Obtaining the Dynamic Mechanical Properties of Laminae for Predicting the Stiffness and Damping of Laminated Plates and Beams. Composites 1984, 15, 193–199. [Google Scholar] [CrossRef] [Scilit]
  14. Guild, F.J.; Adams, R.D. A New Technique for the Measurement of the Specific Damping Capacity of Beams in Flexure. J. Phys. E Sci. Instrum. 1981, 14, 355–363. [Google Scholar] [CrossRef] [Scilit]
  15. Mo, J.; Zhou, C. A Micromechanical Model on Specific Damping Capacity Caused by Micro Cracks. J. Vibroeng. 2015, 17, 1634–1644. [Google Scholar]
  16. Maheri, M.R.; Adams, R.D. Vibration Properties of Structural FRP Composites. JSME Int. J. Ser. A 1999, 42, 307–320. [Google Scholar] [CrossRef] [Scilit]
  17. Maheri, M.R. The Effect of Layup and Boundary Conditions on the Modal Damping of FRP Composite Panels. J. Compos. Mater. 2011, 45, 1411–1422. [Google Scholar] [CrossRef] [Scilit]
  18. Theodore, A.J.; Bishay, P.L. Experimental Analysis of Fiber-Reinforced Laminated Composite Plates with Embedded SMA Wire Actuators. Compos. Struct. 2022, 292, 115678. [Google Scholar] [CrossRef] [Scilit]
  19. Bishay, P.L.; Sofi, A.R. Sensitivity Analysis of a Smart Soft Composite Robotic Finger Design Using Geometrically Nonlinear Laminated Composite Finite Beam Elements. Mater. Today Commun. 2018, 16, 111–118. [Google Scholar] [CrossRef] [Scilit]
  20. Micelli, F.; Angiuli, R.; Corvaglia, P.; Aiello, M.A. Passive and SMA-Activated Confinement of Circular Masonry Columns with Basalt and Glass Fibers Composites. Compos. Part B Eng. 2014, 67, 348–362. [Google Scholar] [CrossRef] [Scilit]
  21. Eilbeigi, S.; Tavakkolizadeh, M.; Masoodi, A.R. Enhancing Mechanical Behavior and Energy Dissipation in Fiber-Reinforced Polymers through Shape Memory Alloy Integration: A Numerical Study on SMA-FRP Composites under Cyclic Tensile Loading. Materials 2023, 16, 5695. [Google Scholar] [CrossRef] [Scilit]
  22. Hübler, M.; Gurka, M.; Schmeer, S.; Breuer, U.P. Performance Range of SMA Actuator Wires and SMA–FRP Structure in Terms of Manufacturing, Modeling and Actuation. Smart Mater. Struct. 2013, 22, 094002. [Google Scholar] [CrossRef] [Scilit]
  23. Jang, B.-K.; Koo, J.-H.; Toyama, N.; Akimune, Y.; Kishi, T. Influence of Lamination Direction on Fracture Behavior and Mechanical Properties of TiNi SMA Wire-Embedded CFRP Smart Composites. In Proceedings Volume 4326, Smart Structures and Materials 2001: Modeling, Signal Processing, and Control in Smart Structures; Rao, V.S., Ed.; SPIE: Newport Beach, CA, USA, 2001; pp. 188–197. [Google Scholar]
  24. Nissle, S.; Hübler, M.; Gurka, M.; Schmeer, S.; Voll, N. Integration of Shape Memory Alloy Wires in Fiber Reinforced Polymers for Endless Crash Absorber Structures. In Proceedings of the Volume 2: Mechanics and Behavior of Active Materials; Integrated System Design and Implementation; Bioinspired Smart Materials and Systems; Energy Harvesting; American Society of Mechanical Engineers: Newport, RI, USA, 2014; p. V002T04A005. [Google Scholar]
  25. Xu, L.; Shi, M.; Wang, Z.; Zhang, X.; Xue, G. Experimental and Numerical Investigation on the Low-Velocity Impact Response of Shape Memory Alloy Hybrid Composites. Mater. Today Commun. 2021, 26, 101711. [Google Scholar] [CrossRef] [Scilit]
  26. Mohd Jani, J.; Leary, M.; Subic, A.; Gibson, M.A. A Review of Shape Memory Alloy Research, Applications and Opportunities. Mater. Des. 2014, 56, 1078–1113. [Google Scholar] [CrossRef] [Scilit]
  27. Shukla, U.; Garg, K. Journey of Smart Material from Composite to Shape Memory Alloy (SMA), Characterization and Their Applications—A Review. Smart Mater. Med. 2023, 4, 227–242. [Google Scholar] [CrossRef] [Scilit]
  28. Liang, C.; Rogers, C.A. Design of Shape Memory Alloy Springs with Applications in Vibration Control. J. Vib. Acoust. 1993, 115, 129–135. [Google Scholar] [CrossRef] [Scilit]
  29. Cohades, A.; Hostettler, N.; Pauchard, M.; Plummer, C.J.G.; Michaud, V. Stitched Shape Memory Alloy Wires Enhance Damage Recovery in Self-Healing Fibre-Reinforced Polymer Composites. Compos. Sci. Technol. 2018, 161, 22–31. [Google Scholar] [CrossRef] [Scilit]
  30. Ozair, H.; Baluch, A.H.; Ur Rehman, M.A.; Wadood, A. Shape Memory Hybrid Composites. ACS Omega 2022, 7, 36052–36069. [Google Scholar] [CrossRef] [Scilit]
  31. Mahmood Baitab, D.; Laila Abang Haji Abdul Majid, D.; Junita Abdullah, E.; Faisal Abdul Hamid, M. A Review of Techniques for Embedding Shape Memory Alloy (SMA) Wires in Smart Woven Composites. Int. J. Eng. Technol. 2018, 7, 129–136. [Google Scholar] [CrossRef] [Scilit]
  32. Bhaskar, J.; Kumar Sharma, A.; Bhattacharya, B.; Adhikari, S. A Review on Shape Memory Alloy Reinforced Polymer Composite Materials and Structures. Smart Mater. Struct. 2020, 29, 073001. [Google Scholar] [CrossRef] [Scilit]
  33. Wang, Z.; Xu, L.; Sun, X.; Shi, M.; Liu, J. Fatigue Behavior of Glass-Fiber-Reinforced Epoxy Composites Embedded with Shape Memory Alloy Wires. Compos. Struct. 2017, 178, 311–319. [Google Scholar] [CrossRef] [Scilit]
  34. Malekzadeh, K.; Mozafari, A.; Ghasemi, F.A. Free Vibration Response of a Multilayer Smart Hybrid Composite Plate with Embedded SMA Wires. Lat. Am. J. Solids Struct. 2014, 11, 279–298. [Google Scholar] [CrossRef] [Scilit]
  35. Jin, F.; Zhao, C.; Xu, P.; Xue, J.; Lin, J. Nonlinear Vibration of SMA Hybrid Composite Beams Actuated by Embedded Pre-Stretched SMA Wires with Tension-Bending Coupling Effect. J. Sound Vib. 2024, 568, 117964. [Google Scholar] [CrossRef] [Scilit]
  36. Zaman, I.; Manshoor, B.; Khalid, A.; Araby, S.; Bin Ghazali, M.I. Vibration Characteristics of Composite Plate Embedded with Shape Memory Alloy at Elevated Temperature. Appl. Mech. Mater. 2013, 393, 655–660. [Google Scholar] [CrossRef] [Scilit]
  37. Khalili, S.M.R.; Shokuhfar, A.; Ashenai Ghasemi, F.; Malekzadeh, K. Dynamic Response of Smart Hybrid Composite Plate Subjected to Low-Velocity Impact. J. Compos. Mater. 2007, 41, 2347–2370. [Google Scholar] [CrossRef] [Scilit]
  38. Damanpack, A.R.; Bodaghi, M.; Aghdam, M.M.; Shakeri, M. On the Vibration Control Capability of Shape Memory Alloy Composite Beams. Compos. Struct. 2014, 110, 325–334. [Google Scholar] [CrossRef] [Scilit]
  39. De Oliveira, R.; Bigi, E.; Sigg, A.; Michaud, V.; Månson, J.-A.E. Passive Damping of Composites with Embedded Shape Memory Alloy Wires. In Proceedings of the SPIE Smart Structures and Materials + Nondestructive Evaluation and Health Monitoring, San Diego, CA, USA, 7–11 March 2010. [Google Scholar]
  40. Birman, V.; Chandrashekhara, K.; Sain, S. An Approach to Optimization of Shape Memory Alloy Hybrid Composite Plates Subjected to Low-Velocity Impact. Compos. Part B Eng. 1996, 27, 439–446. [Google Scholar] [CrossRef] [Scilit]
  41. Ke, J.; Chen, L.; Gao, J.; Wu, Z. Improving the Dynamic Stiffness and Vibration Characteristics of 3D Orthogonal Woven by Implanting SMA Instead of a Warp Yarn. Compos. Struct. 2023, 307, 116637. [Google Scholar] [CrossRef] [Scilit]
  42. Murugesan, K.; Kalaichelvan, K.; Jenarthanan, M.P.; Sornakumar, T. Enhancement of Vibration Characteristics in Filament Wound FRP Composite Shafts Using Nitinol Wires. Pigment. Resin Technol. 2018, 47, 377–385. [Google Scholar] [CrossRef] [Scilit]
  43. Pappadà, S.; Gren, P.; Tatar, K.; Gustafson, T.; Rametta, R.; Rossini, E.; Maffezzoli, A. Mechanical and Vibration Characteristics of Laminated Composite Plates Embedding Shape Memory Alloy Superelastic Wires. J. Mater. Eng Perform. 2009, 18, 531–537. [Google Scholar] [CrossRef] [Scilit]
  44. Fallah, A.; Dehkordi, M.B.; Nourbakhsh, S.H. Nonlinear Dynamic Analysis of Microbeam Containing Graded Shape Memory Microwires. Compos. Struct. 2021, 257, 113085. [Google Scholar] [CrossRef] [Scilit]
  45. Zhang, R.; Ni, Q.-Q.; Masuda, A.; Yamamura, T.; Iwamoto, M. Vibration Characteristics of Laminated Composite Plates with Embedded Shape Memory Alloys. Compos. Struct. 2006, 74, 389–398. [Google Scholar] [CrossRef] [Scilit]
  46. Chen, Y.; Schuh, C.A. Size Effects in Shape Memory Alloy Microwires. Acta Mater. 2011, 59, 537–553. [Google Scholar] [CrossRef] [Scilit]
  47. John, S.; Hariri, M. Effect of Shape Memory Alloy Actuation on the Dynamic Response of Polymeric Composite Plates. Compos. Part A Appl. Sci. Manuf. 2008, 39, 769–776. [Google Scholar] [CrossRef] [Scilit]
  48. Kazi, A.; Hauber, M.; Honold, M. Thermomechanical Characterization of Phase Transformation Surfaces for Thin SMA Wires. J. Intell. Mater. Syst. Struct. 2023, 34, 2293–2306. [Google Scholar] [CrossRef] [Scilit]
  49. Yang, S.; Kang, S.; Lim, Y.-M.; Lee, Y.; Kim, J.; Nam, T. Temperature Profiles in a Ti–45Ni–5Cu (At%) Shape Memory Alloy Developed by the Joule Heating. J. Alloys Compd. 2010, 490, L28–L32. [Google Scholar] [CrossRef] [Scilit]
  50. Sanchez, D.; Pishvar, M.; Bishay, P. Innovations in Composite Laminates: Experimental Exploration of SMA Wire Integration. In Proceedings of the SAMPE 2024, Long Beach, CA, USA, 20–23 May 2024. [Google Scholar]
  51. Zhang, Y.-W.; Wang, Z.-J.; Cao, M.; Song, X.-Y.; Zang, J.; Lacarbonara, W.; Chen, L.-Q. Vibration Control of Composite Laminate via NiTiNOL-Steel Wire Ropes: Modeling, Analysis, and Experiment. Mech. Syst. Signal Process. 2023, 204, 110775. [Google Scholar] [CrossRef] [Scilit]
  52. Bayat, Y.; EkhteraeiToussi, H. A Nonlinear Study on Structural Damping of SMA Hybrid Composite Beam. Thin-Walled Struct. 2019, 134, 18–28. [Google Scholar] [CrossRef] [Scilit]
  53. Verma, L.; Andrew, J.; Sivakumar, S.M.; Balaganesan, G.; Vedantam, S.; Dhakal, H.N. Ballistic Impact Behaviour of Glass/Epoxy Composite Laminates Embedded with Shape Memory Alloy (SMA) Wires. Molecules 2020, 26, 138. [Google Scholar] [CrossRef] [Scilit]
  54. Droste, D.H.; Dibenedetto, A.T. The Glass Transition Temperature of Filled Polymers and Its Effect on Their Physical Properties. J. Appl. Polym. Sci. 1969, 13, 2149–2168. [Google Scholar] [CrossRef] [Scilit]
  55. Lau, K.T.; Zhou, L.M.; Tao, X.M. Control of Natural Frequencies of a Clamped–Clamped Composite Beam with Embedded Shape Memory Alloy Wires. Compos. Struct. 2002, 58, 39–47. [Google Scholar] [CrossRef] [Scilit]
  56. Riley, D.K.; Chen, Y.; Lu, C.; Mohagheghian, I.; Hassanin, H.; Sareh, P. Morphing Structural Materials Used in Wind Turbine Blades. Renew. Sustain. Energy Rev. 2025, 216, 115618. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.