Skip to Content
BuildingsBuildings
  • Article
  • Open Access

25 November 2026

32 Pages

Numerical Investigation of the Out-of-Plane Impact and Shear Behavior of Steel Plate Concrete Walls for Nuclear Power Applications

,
,
,
and
1
School of Civil Engineering and Architecture, Northeast Electric Power University, Jilin 132012, China
2
State Grid Gansu Electric Power Company Liujiaxia Hydropower Plant, Yongjing 731600, China
*
Author to whom correspondence should be addressed.
This article belongs to the Section A. Building Structures

Abstract

Steel plate concrete (SC) walls combine the tensile strength of steel plates with the energy-dissipation and radiation-shielding capabilities of concrete, providing greater blast resistance than conventional reinforced-concrete structures. Although SC walls are increasingly used in nuclear power plant shielding structures, simple methods for predicting their dynamic response under low-velocity impact remain limited. In this study, we developed an ABAQUS finite element model of SC walls under drop-weight impact and validated it against published experimental data. Parametric analyses show that residual displacement is most sensitive to the thickness of the concrete core. Increasing the core thickness from 1000 to 1200 mm reduces residual displacement by 38.5%. Reducing the span-to-thickness ratio (the stud spacing-to-plate thickness ratio) from 50 to 37.5 decreases residual displacement. However, a further reduction to 25 sharply increases the peak impact force. Thus, 37.5 provides an optimal balance between these responses. Based on yield-line theory and the concrete punching-shear failure mechanism, we derived a multilinear resistance function that accounts for flexural yielding, punching-shear cracking, ultimate capacity, and post-failure resistance. We also developed a corresponding method for calculating stiffness. We incorporated the resistance function and stiffness method into an equivalent single-degree-of-freedom (SDOF) system and solved the equations of motion to rapidly predict maximum and residual displacements. We validated the proposed method against experimental data and finite element simulations. The mean ratios of calculated to reference displacements were 1.073 for maximum displacement and 0.978 for residual displacement. These results indicate good agreement with the reference data, supporting the use of the method for rapid assessment of SC walls during preliminary impact-resistant design.

1. Introduction

With the advancement of China’s dual-carbon strategy, which aims to peak carbon emissions and achieve carbon neutrality, the strategic importance of nuclear power as a low-carbon baseload energy source has become increasingly evident. According to Jiang Ziying et al. [1], a 1000-MW-class nuclear power plant can reduce annual carbon dioxide emissions by approximately 6 million tons compared with a coal-fired power plant of equivalent capacity. Therefore, nuclear power represents a viable option for facilitating the low-carbon transition of the energy sector. Nuclear safety is a fundamental prerequisite for the sustainable development of nuclear power. The nuclear accidents at Three Mile Island, Chernobyl, and Fukushima have demonstrated that radioactive material releases can result in severe and far-reaching consequences. In response to these safety concerns, the nuclear power industry has established a four-barrier safety system consisting of the fuel matrix, fuel cladding, the reactor coolant pressure boundary, and the containment structure. The containment structure provides radiation shielding, protects against missile impacts, and prevents the release of radioactive materials into the environment. The steel plate concrete (SC) composite structure, which constitutes a critical load-bearing component of the containment structure, is the primary focus of this study. China’s Code for Seismic Design of Nuclear Power Plants (GB 50267-97) [2] stipulates that, under design-basis accident conditions, the characteristic values of local effects must account for three types of loading: loads resulting from pipe rupture (including self-weight), jet impingement loads, and missile impact loads. Steel-concrete (SC) structures typically consist of external steel faceplates, tie bars, shear connectors, and a concrete core. The steel faceplates resist tensile forces, confine the concrete core, and provide structural enclosure. The tie bars improve composite action between the steel plates and concrete, while the concrete core carries compressive loads and restrains local buckling of the steel faceplates. Furthermore, the steel faceplates on both sides can serve as permanent formwork, thereby facilitating modular construction. This construction approach has been adopted in AP1000 nuclear power plant projects at Tianwan, Fangchenggang, and Haiyang. During their service life, SC structures may be subjected to both static loads and accidental dynamic actions, such as vehicle impacts, ship or floating-ice collisions, flying-debris impacts, and pipe-whip loads. However, conventional design approaches primarily rely on static analysis and may therefore inadequately capture the dynamic response of SC structures under impact loading. Owing to the penetration resistance of the steel faceplates and the energy-dissipation capacity associated with concrete deformation, SC structures exhibit favorable resistance to impact loading. In recent years, numerous experimental and numerical studies have investigated the behavior of SC structures under low-velocity impact loading [3,4,5].
At the component level, Kim et al. [6] conducted comparative impact tests on 10 large-scale steel-concrete (SC) and reinforced concrete (RC) walls, with wall thickness and steel plate thickness as the main test parameters. The measured responses included the projectile’s initial and residual velocities, as well as the strain, acceleration, and local damage characteristics of the rear plate. The results indicated that existing design methods were overly conservative and required further refinement for impact scenarios beyond the design basis. Wang et al. [7] conducted eccentric drop-weight impact tests on nine steel-concrete-steel (SCS) sandwich beams incorporating bolted connectors. The specimens exhibited three distinct failure modes: flexural failure, flexural–shear failure, and bottom-plate fracture. The bolted connectors effectively prevented separation between the steel plates. In addition, the authors developed an analytical model to predict the displacement time response of the beams. Yan et al. [8] conducted low-velocity impact tests on nine curved SCS sandwich shells. The impact response was divided into three stages: inertia, loading, and unloading. The observed failure modes included plastic deformation, fracture, and penetration of the steel plates, while the concrete core served as the primary energy-dissipating component. Wang et al. [9] investigated the impact behavior of SCS sandwich beams strengthened with stiffening ribs on the tension-side steel plate. All specimens exhibited flexural failure. The stiffening ribs significantly improved the impact resistance of the beams. In addition, the authors developed both finite element and analytical models to investigate their impact behavior. Yan Chen [10] conducted 13 static tests and nine impact tests on arched double-skin steel-concrete (SCS) wall panels. The specimens had a span and width of 1200 mm, a rise-to-span ratio of 0.25, core thicknesses ranging from 70 to 90 mm, and steel plate thicknesses ranging from 2.87 to 4.54 mm. The specimens were impacted by an 800 kg drop hammer released from a height of 3 m in most tests, with the drop height increased to 5 m in some cases. The base plate was fully restrained to simulate fixed support conditions. The predominant failure mechanism was local indentation, which manifested in three forms: local plastic deformation of the steel plates, tearing of the top steel plate, and complete penetration. Based on these experimental findings, the authors developed an equivalent single-degree-of-freedom (SDOF) method for calculating displacement, together with a critical failure curve. Remennikov et al. [11] conducted large-mass impact tests and numerical simulations on scaled-down, non-composite SCS sandwich panels subjected to axial restraint. The study examined the effects of axial restraint on the impact response and identified the tensile membrane action of the steel plates as the primary mechanism contributing to the load-bearing capacity. The panels exhibited considerable ductility, remaining intact at end rotation angles of up to 18°. The experimental findings were subsequently incorporated into simulations of full-scale barrier structures subjected to truck impacts. Zhang et al. [12] conducted drop-weight impact tests on seven full-scale sandwich panels comprising two steel faceplates and a rubberized lightweight aggregate concrete core. The impact responses were also simulated using LS-DYNA. Comparisons between the numerical predictions and experimental results demonstrated that the two-degree-of-freedom (TDOF) model provided more accurate predictions of peak impact force and residual deformation than the single-degree-of-freedom (SDOF) model. Yang Yaotang et al. [13] numerically investigated the behavior of double-skin steel-concrete composite walls subjected to combined fire and impact loading, focusing on their impact resistance and post-fire mid-span deflection. The typical specimens measured 1 m in length, 0.7 m in width, and 80 mm in overall thickness, and incorporated 3 mm thick steel faceplates. The specimens were impacted by a 240 kg drop weight traveling at a velocity of 6 m/s. The boundary conditions comprised a fixed support at one end and an axially sliding restraint at the other. At ambient temperature, the walls primarily failed through local punching shear. Following fire exposure, however, the dominant failure mode shifted to global flexural deformation. With regard to plate-type structural components, Sun Jihong et al. [14] compared the impact performance of single-layer and double-layer steel-concrete composite slabs. The impact process was divided into four stages. Their results demonstrated that double-layer slabs exhibited superior impact resistance compared with single-layer slabs. The effects of the steel ratio and drop height were also investigated. An Guoqing et al. [15] investigated the dynamic response of double-steel plate slabs incorporating recycled aggregate concrete. Their results showed that the steel ratio, impact velocity, and recycled aggregate replacement ratio significantly influenced the structural response. Furthermore, an empirical formula was proposed to predict the maximum mid-span deflection; Yu Yue et al. [16] conducted high-velocity impact tests on steel-concrete (SC) composite targets with three different tie-bar configurations. The specimens were designed at scale ratios of 1:20 and 1:10, with plan dimensions of 1650 mm × 1500 mm and thicknesses of 75 mm and 150 mm, respectively. The targets were fixed along their left and right edges and simply supported along their top and bottom edges. A light-gas gun was employed to launch projectiles at velocities of up to 160 m/s. The failure process was characterized by the progressive development of steel plate buckling, followed by localized perforation. Plate thickness was identified as the dominant factor governing the impact response. Among the investigated tie-bar configurations, the lap-joint arrangement with end anchorage was the most effective in limiting deformation and reducing the peak response in the impact zone. In terms of engineering applications and computational methods, Fan Jiansheng et al. [17] presented a comprehensive review of the research and applications of steel-concrete (SC) structures in nuclear power plants. The review covered typical structural configurations, the mechanical behavior of structural components and elements, and design methods for various accident scenarios, including large-aircraft impact events. Zhu Limeng et al. [18] developed an analytical model to predict the out-of-plane impact response of double-skin steel-concrete walls with fully bolted, weld-free connections. Their parametric analysis showed that a lower axial compression ratio improved the impact performance of the walls and that specimens incorporating tie-bolts exhibited superior resistance. In addition, they proposed a formula for predicting plastic displacement. Wang Wu et al. [19] developed an energy-based method for assessing the perforation resistance of SC structures based on the principle of energy conservation. They derived equations for predicting the critical perforation velocity and residual projectile velocity. The predictions showed good agreement with experimental penetration results. Han et al. [20] developed a perforation model for double-skin steel-concrete walls and investigated the effects of tie-bar and shear-stud arrangements on their failure modes.
Although previous studies have investigated various components of steel plate concrete (SC) structures, including the concrete core, steel faceplates, and shear connectors, several research gaps remain. First, most studies have focused on static behavior, while the response of SC structures to severe dynamic loading, particularly impact loading, has received comparatively limited attention. Theoretical investigations in this area are also scarce. Second, although SC structures exhibit favorable blast resistance, existing design provisions provide limited guidance on their behavior under dynamic loading, and the associated failure mechanisms remain insufficiently understood. Third, the load-transfer capacity of some existing connectors may be inadequate, rendering them susceptible to shear failure or debonding under impact loading and potentially compromising structural integrity under extreme loading conditions. Therefore, further investigation is needed into the out-of-plane punching-shear resistance of SC walls used in nuclear power facilities under low-velocity impact loading. In this study, a finite element (FE) model of a double-skin SC wall subjected to drop-weight impact loading was developed using ABAQUS. After the FE model was validated against published experimental results, a parametric study was conducted to examine the effects of steel faceplate thickness, steel and concrete strengths, concrete core thickness, and span-to-thickness ratio (The stud spacing-to-plate thickness ratio). The results indicated that residual displacement was most sensitive to concrete core thickness. Specifically, increasing the core thickness from 1000 mm to 1200 mm reduced the residual displacement by 38.5%. Based on these findings, a simplified analytical method was developed to predict the impact-induced displacement of SC walls. By combining plastic hinge-line theory with the punching-shear failure mechanism of concrete, a multilinear resistance function was derived. The function consists of four stages: flexural yielding, punching-shear cracking, ultimate resistance, and post-failure resistance. A corresponding stiffness calculation method was also developed. The resistance function was then incorporated into an equivalent single-degree-of-freedom (SDOF) model, and the equations of motion were solved to rapidly predict the maximum and residual displacements of the wall. The proposed method was validated against experimental results and FE simulations. The ratios of the predicted displacements to the corresponding reference values ranged from approximately 0.98 to 1.07. These results demonstrate good agreement between the predictions and the reference results, indicating that the proposed method provides a practical analytical tool for the preliminary impact-resistant design of SC walls in nuclear power facilities.

2. Analytical Model for Out-of-Plane Impact-Shear of Steel Plate Concrete Walls

2.1. Development of the Finite Element Model

2.1.1. Modeling of Individual Components

As shown in Figure 1, the steel-concrete (SC) wall model developed for nuclear power engineering consists of a drop hammer, steel faceplates, a concrete core, shear connectors (bolts or steel channels), and tie bars. The overall dimensions of the model are 10 m × 8 m × 1.04 m. The steel faceplates are 20 mm thick, whereas the concrete core is 1000 mm thick, corresponding to 50 times the thickness of the steel faceplates. The shear connectors have a height of 750 mm. The bolts have a diameter of 25 mm and a length of 200 mm, equivalent to eight times their diameter. The steel channels have cross-sectional dimensions of 200 mm × 75 mm × 9 mm × 11 mm × 75 mm. The two steel faceplates are connected by 40-mm-diameter high-strength tie bars arranged at 1500 mm intervals. The drop hammer is equipped with a rigid hemispherical impact head with a diameter of 800 mm.
Figure 1. Cutaway view of the finite element model.

2.1.2. Boundary Conditions and Loading Procedure

In the numerical model, the wall is restrained by steel frames at its top and bottom, while hinged boundary conditions are imposed along all four edges. Specifically, the three translational degrees of freedom are constrained, whereas the rotational degrees of freedom are left free to simulate the actual support conditions. The drop hammer is modeled as a rigid body, with all degrees of freedom constrained except for the translational degree of freedom along the impact direction. The mass of the drop weight is 67 tons. An initial velocity of v0 = 9.39 m/s is prescribed at the reference point using a predefined field to simulate the impact event.
Two types of interactions are defined in the model. Surface-to-surface contact is employed at the steel plate-concrete core interfaces, with hard contact enforced in the normal direction and a penalty-based formulation used to describe tangential friction. The friction coefficient is set to 0.6. Regarding the constraint conditions, tie constraints are imposed between the steel plates and the shear studs, as well as between the steel plates and the tie bars, to simulate welded connections. The shear studs and tie bars are embedded in the concrete core.

2.1.3. Element Types and Meshing

The element types are selected according to the mechanical characteristics and expected deformation behavior of each component. The steel faceplates and channel sections are modeled using four-node, reduced-integration shell elements (S4R), which are suitable for capturing bending and membrane responses. Five integration points are specified through the thickness to improve the accuracy of through-thickness stress evaluation. The concrete core, drop hammer, and steel frames are discretized using eight-node, linear, reduced-integration solid elements (C3D8R) to capture their three-dimensional stress states. Hourglass control is activated to suppress nonphysical zero-energy deformation modes associated with reduced integration. The tie bars are modeled using two-node, three-dimensional truss elements (T3D2). The shear studs are modeled using two-node beam elements (B31) to account for their resistance to shear forces and bending moments. Alternatively, two-node truss elements (T3D2) may be employed to represent the shear studs as equivalent axial-force-carrying members; however, these elements cannot capture their bending behavior.
Mesh density has a significant influence on numerical accuracy and computational efficiency; therefore, an appropriate mesh size must be carefully selected. In this study, a structured meshing approach is adopted. As shown in Figure 2, the steel faceplates and concrete core are initially discretized using a regular mesh with a nominal element size of 250 mm × 250 mm. Considering that the drop hammer impacts the center of the wall, the mesh in the impact region is locally refined to 125 mm × 125 mm. A transition region with element dimensions of 125 mm × 250 mm is introduced to ensure a gradual change in mesh density. Therefore, the mesh size in the impacted region is 125 mm × 125 mm. The mesh sizes of the shear connectors and tie bars are selected according to their geometric characteristics and modeling requirements. Relatively coarse meshes are adopted for the drop hammer and the steel frames to reduce the computational cost. A mesh sensitivity analysis was performed for the core impact zone of the steel plate concrete structure. Three mesh schemes, 125 mm × 125 mm, 62.5 mm × 62.5 mm, and 31.25 mm × 31.25 mm, were adopted for comparative calculations. The differences in peak impact force, maximum displacement, and residual displacement obtained from the three models are only within the range of 1.1–2.5%. This demonstrates that the mesh size of 125 mm × 125 mm selected for the core impact zone achieves favorable computational accuracy while balancing computational efficiency.
Figure 2. Mesh generation. (a) Mesh of the concrete component; (b) Mesh of the steel plate component; (c) Mesh of the drop hammer component.

2.1.4. Material Constitutive Models

A bilinear elastic–plastic constitutive model with strain hardening is adopted to describe the mechanical behavior of steel, as illustrated in Figure 3. The model is characterized by a yield strength of fy = 235 MPa. A bilinear elastic-plastic constitutive model with strain hardening is adopted to describe the mechanical behavior of steel, as illustrated in Figure 3. The model is characterized by a yield strength of Es = 2 × 105 MPa and Poisson’s ratio of ν = 0.3 . Beyond the yield point, the stress-strain relationship is represented by a linear strain-hardening branch with a reduced tangent modulus. Take E s ′ = 0.01   E s = 200   MPa . The steel constitutive parameters in this section are based on the measured material properties of the benchmark specimen tested in Section 2.2, with a yield strength of 235 MPa.
Figure 3. Stress-strain relationship of steel.
Abaqus, three principal constitutive models are commonly used to simulate the mechanical behavior of concrete: the smeared cracking model, the concrete damaged plasticity (CDP) model, and the brittle cracking model [21]. In this study, the CDP model is adopted to investigate the dynamic response and damage evolution of double-skin steel-concrete composite walls subjected to impact loading. This model is capable of capturing the nonlinear tensile and compressive behavior of concrete, as well as stiffness degradation associated with tensile cracking and compressive crushing. The concrete material parameters are determined according to the tensile and compressive constitutive relationships specified in the Code for Design of Concrete Structures (GB 50010-2010) [22]. The post-peak and inelastic responses are characterized using the relevant CDP parameters listed in Table 1.
Table 1. Plasticity parameters of the concrete damage plasticity model.
The uniaxial tensile and compressive stress-strain relationships of concrete are illustrated in Figure 4 and are described by the following equations:
σ = ( 1 − d t ) E t ε
d t = 1 − ρ t [ 1.2 − 0.2 x 5 ] x ≤ 1 1 − ρ t α t ( x − 1 ) 1.7 + x x > 1
x = ε ε t
ρ t = f t E c ε t
Figure 4. Uniaxial stress-strain curve of concrete. (a) Uniaxial tensile stress-strain curve of concrete; (b) Uniaxial compressive stress-strain curve of concrete.
The uniaxial compressive stress-strain relationship of concrete is illustrated in Figure 4 and is described by the following equation:
σ = ( 1 − d c ) E c ε
d c = 1 − ρ c n n − 1 + x n x ≤ 1 1 − ρ c α c ( x − 1 ) 2 + x x > 1
ρ c = f c E c ε c
ρ t = f t E c ε t
x = ε ε t
where αt and αc are the parameters characterizing the descending branches of the uniaxial tensile and compressive stress-strain curves of concrete, respectively; ft and fc denote the uniaxial tensile and compressive strengths of concrete, respectively; εt and εc represent the peak tensile and compressive strains of concrete, respectively; dt and dc represent the damage evolution parameters of concrete under uniaxial tension and compression, respectively.

2.2. Model Validation

To evaluate the reliability of the numerical model and the applicability of the proposed modeling approach, experimental results reported in the literature were used as benchmarks [23]. The proposed modeling strategy and constitutive models were employed to simulate the corresponding test specimens. The specimens had plan dimensions of 1000 mm × 800 mm and consisted of a 75-mm-thick concrete core sandwiched between two 2.90-mm-thick steel faceplates. The steel faceplates were connected to the concrete core by 5-mm-diameter shear studs arranged at 75-mm intervals, with an effective anchorage length of 30 mm. The two faceplates were interconnected by 10-mm-diameter high-strength tie bars spaced at 150 mm. The specimen was restrained by a steel frame with dimensions of 750 mm in both directions, which was anchored to a rigid platform. In the experiments, a drop hammer was lifted to a prescribed height and then released to impact the specimen. The impact energy was controlled by varying the drop height and hammer mass. Full-scale numerical simulations were conducted using ABAQUS. Four representative test cases were selected to compare the predicted responses and failure patterns with the corresponding experimental observations, thereby assessing the validity of the proposed modeling approach.

2.2.1. Comparison of Displacement-Time History Curves at the Center of the Bottom Surface

Figure 5 compares the experimentally measured and numerically predicted displacement-time histories at the center of the bottom surface of specimens H15–H60 [23]. The comparison demonstrates that the finite element model can effectively capture the dynamic deformation response of the specimens. Overall, the numerical predictions agree well with the experimental results throughout the impact response. During the initial impact stage, the simulation captures the rapid increase in displacement, with a displacement growth rate consistent with the experimental measurements. At the peak-response stage, the predicted maximum displacements under different impact heights are in good agreement with the measured values. During the unloading stage, the model also reproduces the gradual displacement rebound and the variation in residual deformation with impact energy.
Figure 5. Displacement-time histories at the center of the bottom surface (a) H15 (b) H30 (c) H45 (d) H60.
The constitutive model adopted in the finite element analysis adequately captures the strain-hardening behavior of the steel, thereby enabling the numerical model to reproduce the mechanical response of the steel plates observed experimentally.

2.2.2. Comparison of Impact Force-Time History Curves

Figure 6 compares the experimentally measured and numerically predicted impact force-time histories for specimens H15–H60. The numerical results show good agreement with the experimental measurements in terms of peak impact force, impact duration, and force decay characteristics. Although some discrepancies remain between the numerical predictions and experimental measurements, the overall agreement indicates that the proposed modeling approach is capable of capturing the impact response of the specimens. These discrepancies may be associated with uncertainties in contact interactions and boundary conditions, which warrant further investigation and refinement.
Figure 6. Impact force-time histories (a) H15 (b) H30 (c) H45 (d) H60.

3. Design Parameters Affecting Out-of-Plane Impact-Shear of Double-Skin Steel-Concrete Walls

3.1. Effects of Design Parameters on the Out-of-Plane Impact-Shear Resistance

3.1.1. Thickness of the External Steel Faceplates

To investigate the influence of external steel faceplate thickness on the out-of-plane impact-shear resistance of double-skin steel-concrete composite walls, four plate thicknesses (20, 22, 24, and 26 mm) were considered. In all cases, the drop hammer had an initial impact velocity of 9.39 m/s. The mass of the drop weight is 67 tons. Table 2 summarizes the maximum and final residual deformations measured on the rear (non-impact) surface of the walls, whereas Figure 7a presents the impact force-time histories. Relative to the 22-mm reference plate, reducing the plate thickness to 20 mm (a 9.1% decrease) increased the maximum deformation and final residual deformation by 2.0% and 4.0%, respectively. Increasing the plate thickness to 24 mm (a 9.1% increase) reduced the maximum deformation and final residual deformation by 2.1% and 2.7%, respectively. A further increase in plate thickness to 26 mm (an 18.2% increase) resulted in reductions of 3.1% and 5.1% in the maximum and final residual deformations, respectively. The results indicate that: (1) Increasing the external steel faceplate thickness improves the wall’s resistance to impact-induced deformation. However, the improvement is relatively modest, with an approximately 10% increase in plate thickness resulting in only a 2–3% reduction in deformation; (2) Increasing the steel faceplate thickness is more effective in reducing residual deformation than in limiting maximum deformation. Specifically, an 18.2% increase in plate thickness reduces the final residual deformation by approximately 1.6 times as much as it reduces the maximum deformation; (3) From a material-efficiency perspective, increasing the steel faceplate thickness alone may not be an economically efficient approach to improving impact resistance. Instead, a coordinated design strategy that considers multiple parameters, such as concrete strength and shear connector arrangement, should be adopted to improve the impact resistance while maintaining material efficiency.
Table 2. Deformation responses of walls with different external steel faceplate thicknesses.
Figure 7. Effect of external steel plate thickness on the impact resistance of the wall. (a) Displacement-time history curve; (b) Impact force-time history curve.
Figure 7b illustrates the impact force-time histories of the wall with different external steel plate thicknesses. The corresponding peak impact forces are 15,320.0, 18,628.1, 24,494.3, and 27,025.5 kN for plate thicknesses of 20, 22, 24, and 26 mm, respectively, representing increases of 21.6%, 59.9%, and 76.4%, respectively, relative to the 20 mm case. Increasing the steel plate thickness enhances the overall structural stiffness, thereby increasing the peak impact force. Structural performance is primarily evaluated in terms of deformation. Under the same impact energy, increasing the steel plate thickness reduces both the maximum and residual deformations, thereby improving deformation control, albeit at the expense of greater impact force transmission.
Figure 8 illustrates the von Mises stress distributions in the wall subjected to drop-weight impact, with the 20 mm thick wall shown as an example in Figure 8a. On the impact side, the steel plate exhibits localized indentation, with the stress gradually decreasing from the center of the indentation toward the surrounding region. On the rear side, the steel plate undergoes outward bulging, accompanied by a gradual decrease in stress with increasing distance from the bulging region. Notably, the high-stress region on the rear side extends over a larger area than that on the impact side. A comparison of Figure 8a–c shows that increasing the steel plate thickness leads to higher stress concentrations in the directly impacted region, while reducing the spatial extent of the high-stress zone. Similarly, the high-stress region on the rear side becomes progressively more localized around the center, with the stress influence decreasing with increasing distance from this region.
Figure 8. Effect of steel plate thickness on the load-bearing behavior of the wall. (a) external steel plate 20 mm; (b) external steel plate 22 mm; (c) external steel plate 24 mm; (d) external steel plate 26 mm.

3.1.2. Different Concrete Strength Grades

This section investigates the impact performance of steel plate concrete walls incorporating three concrete strength grades: C40, C50, and C60. Numerical simulations were conducted to obtain the displacement-time and impact force-time histories of the walls, as shown in Figure 9.
Figure 9. Effect of concrete strength on the impact resistance of the wall. (a) Displacement-time history curve; (b) Impact force-time history curve.
As shown in Figure 9a, the maximum wall deformation decreases slightly with increasing concrete strength. Specifically, the maximum deformations of the C50 and C60 walls are 2.6% and 3.5% lower, respectively, than that of the C40 wall. This marginal reduction suggests that the compressive strength of the concrete core has a relatively limited influence on the overall deformation response of the wall. The out-of-plane stiffness of the wall is primarily governed by the steel plates and their composite interaction with the concrete core. Moreover, higher concrete strength is generally associated with increased brittleness and reduced ductility. As shown in Figure 9b, the peak impact forces of the C40, C50, and C60 walls are 15,121.8, 20,123.3, and 23,916.4 kN, respectively. These values correspond to increases of 33.1% and 58.2% for the C50 and C60 walls, respectively, relative to the C40 wall. This trend can be attributed to the higher compressive strength and elastic modulus of high-strength concrete. The peak impact force reflects the dynamic load-carrying response of the wall. Under the same impact energy, walls with higher-strength concrete exhibit slightly smaller deformations but substantially greater impact force transmission. Therefore, the selection of an appropriate concrete strength grade should consider the trade-off between deformation control, impact force transmission, and failure characteristics. Simply increasing the concrete strength does not necessarily improve the overall impact resistance of the wall.

3.1.3. Effect of Concrete Thickness

Three concrete core thicknesses of 1000, 1100, and 1200 mm were considered, while the steel plate thickness was kept constant. Figure 10 presents the time histories of the rear-face displacement and impact force. For a concrete core thickness of 1000 mm, the maximum and residual displacements are 179 and 156 mm, respectively. When the concrete core thickness increases to 1100 mm, the maximum and residual displacements decrease to 162 and 118 mm, respectively, corresponding to reductions of 9.5% and 24.4%, respectively, relative to the 1000 mm case. At a thickness of 1200 mm, the corresponding displacements further decrease to 141 and 96 mm, representing reductions of 21.2% and 38.5%, respectively, relative to the 1000 mm case. The reduction in residual displacement is substantially greater than that in maximum displacement, indicating that increasing the concrete core thickness is particularly effective in mitigating permanent deformation. In terms of peak impact force, the values for concrete core thicknesses of 1100 and 1200 mm are 18,688.6 and 21,637.2 kN, respectively, representing increases of 21.9% and 41.2%, respectively, relative to the 1000 mm case. These results indicate that the reduction in deformation is accompanied by increased impact force transmission. Overall, increasing the concrete core thickness effectively suppresses residual deformation. However, the incremental reduction in residual displacement diminishes as the thickness increases, decreasing from 24.4% to 18.6%, whereas the peak impact force continues to increase. Therefore, the concrete core thickness should be optimized in conjunction with the steel plate thickness and connector configuration, rather than being increased indiscriminately to improve the impact resistance of the wall.
Figure 10. Effect of concrete core thickness on the impact response of the wall. (a) Displacement-time history curve; (b) Impact force-time history curve.

3.1.4. Influence of Steel Strength Grade

The steel plates on both sides play a critical role in determining the impact resistance of the wall. Therefore, the effect of steel strength grade on the structural response warrants further investigation. Accordingly, four steel grades (Q355, Q390, Q420, and Q460) were considered for the external steel plates. The corresponding material properties were determined in accordance with GB 50017-2017 [24] and GB/T 1591 [25], as summarized in Table 3. Table 4 summarizes the maximum displacement, residual displacement, and failure modes of the steel plates for each steel grade. Figure 11 compares the rear-face displacement-time histories and impact force-time histories. Figure 12 shows the stress contours of the steel plates on the impact side and the rear side of the walls with steel plates of different strength grades.
Table 3. Mechanical properties of the steel plates.
Table 4. Deformation characteristics of the wall with different steel grades.
Figure 11. Effect of steel grade on the impact response of the wall. (a) Displacement-time history curve; (b) Impact force-time history curve.
Figure 12. Stress contours of steel plates with different strength grades on the impact and rear sides. (a) Q355 impact-resistant steel plate; (b) Q355 steel plate on the impact side; (c) Q390 impact-resistant steel plate; (d) Q390 steel plate on the impact side; (e) Q420 impact-resistant steel plate; (f) Q420 steel plate on the impact side; (g) Q460 impact-resistant steel plate; (h) Q460 steel plate on the impact side.

3.1.5. Span-to-Thickness Ratio

The span-to-thickness ratio (s/t) is defined as the ratio of the spacing between adjacent shear connectors, such as headed studs, to the thickness of the steel plate. This dimensionless parameter governs the degree of composite action between the steel plates and the concrete core, thereby affecting the overall mechanical response of the wall.
This section investigates the effect of the connector spacing-to-thickness ratio on the impact performance of walls incorporating channel-steel shear connectors. The steel plate thickness was fixed at 20 mm, and three spacing-to-thickness ratios—50, 37.5, and 25—were considered, representing conventional, moderately strengthened, and high-density configurations, respectively. Figure 13 shows the detailed drawing of the stud layout. Apart from the connector spacing, all three specimens had identical configurations. The channel-steel connectors were arranged in a symmetric staggered pattern to promote balanced mechanical performance in all directions. The impact response, damage evolution, and failure modes of the three cases were compared to evaluate the influence of the spacing-to-thickness ratio on impact resistance and to provide guidance for engineering design.
Figure 13. Arrangement of shear connectors at different spacing-to-thickness ratios. (a) The span-to-thickness ratio is 50; (b) The span-to-thickness ratio is 37.5; (c) The span-to-thickness ratio is 25.
Figure 14 presents the displacement and impact-force time-history curves of steel-concrete composite walls with spacing-to-thickness ratios of 50, 37.5, and 25 under identical impact-energy conditions. As the spacing-to-thickness ratio decreased from 50 to 37.5 and 25, the maximum midspan displacement decreased by 16.7% and 33.1%, respectively. These results indicate that a higher density of shear connectors effectively restrains relative slip at the steel-concrete interface and limits local buckling and global flexural deformation, thereby increasing the flexural stiffness of the wall. Furthermore, compared with the specimen with a ratio of 50, the residual displacement decreased by 16.2% and 33.7% for ratios of 37.5 and 25, respectively. This finding demonstrates that a denser connector arrangement enhances interfacial restraint, reduces plastic deformation accumulation, and promotes post-impact elastic recovery. Therefore, the reduction in deformation can be attributed primarily to enhanced interfacial restraint and the suppression of relative slip and local buckling resulting from the increased connector density. Under identical impact-energy conditions, the peak impact force increased by 13.9% and 54.4% for ratios of 37.5 and 25, respectively, owing to the combined enhancement of structural stiffness and steel-concrete interfacial interaction. Notably, the higher peak impact force reflects an increased load response rather than a direct improvement in structural resistance. For each 1% reduction in residual displacement, the configurations with ratios of 37.5 and 25 exhibited peak-force increases of approximately 0.86% and 1.61%, respectively; thus, the former required approximately half the increase in peak force of the latter. Therefore, a spacing-to-thickness ratio of 37.5 provides a favorable balance between deformation control and the accompanying increase in force transmission, making it a suitable reference value for most engineering applications. Although a ratio of 25 achieves the greatest deformation reduction, it causes a substantial increase in force transmission and should therefore be adopted only where deformation limits are stringent and the supporting structure has sufficient load-bearing capacity. Figure 15 shows the stress contours of the front and rear steel plates under impact loading with different spacing-to-thickness ratios.
Figure 14. The effect of the spacing-to-thickness ratio on the impact resistance of walls. (a) Displacement-time history curve; (b) Impact force-time history curve.
Figure 15. Stress contour plots of the steel plate on the front (impact) and rear surfaces at different span-to-thickness ratios. (a) The span-to-thickness ratio is 50; (b) the span-to-thickness ratio is 37.5; (c) The span-to-thickness ratio is 25.
This chapter presents a parametric analysis of five categories of design variables across 17 load cases. Although all variables contributed to reducing wall deformation, their effects differed substantially. Taking residual deformation as the performance indicator, a 10% variation in concrete thickness, external steel plate thickness, concrete strength, and steel strength produced deformation changes of 19.2%, 2.83%, 1.28%, and 0.52%, respectively. The influence of concrete thickness varies across different thickness intervals. When the wall thickness increased from 1000 to 1100 mm, the residual and maximum deformations decreased by 24.4% and 9.5%, respectively. When the thickness increased from 1100 to 1200 mm, the corresponding reductions were 18.6% and 13.0%, respectively. These results indicate that the response of thinner walls is governed primarily by local punching-shear failure, whereas thicker walls progressively transition to a global flexure-controlled response. Therefore, wall thickness should not be selected solely on the basis that a thicker wall is preferable; instead, an appropriate thickness within the range of 1100–1200 mm should be determined according to the governing failure mode.
The benefits associated with deformation control do not increase proportionally with the cost associated with force transmission. A cost–benefit ratio was defined as the relative increase in peak force divided by the relative reduction in residual deformation. The corresponding ratios were approximately 1.07, 9.0, and 10.4 for increases in concrete thickness, steel plate thickness, and concrete strength, respectively. In particular, increasing the steel plate thickness raised the peak force by 76.4% while reducing residual deformation by only 8.5%; similarly, increasing concrete strength reduced residual deformation by 3.2% but increased the peak force by 33.1%. This difference arises from their distinct mechanisms: increasing material strength primarily raises the resistance level while causing little change in elastic modulus, whereas increasing thickness enhances both the sectional moment of inertia and the ultimate resistance. Consequently, increasing material strength primarily improves load-bearing capacity rather than deformation control. Therefore, concrete thickness, steel plate thickness, and material strength grade should be selected according to the governing design objectives—deformation control, penetration resistance, and load-bearing capacity, respectively—and should not be regarded as interchangeable parameters.
The connector spacing-to-thickness ratio exhibits a threshold effect. Reducing the ratio from 50 to 37.5 increased the peak force by only 13.9%, whereas a further reduction from 37.5 to 25 resulted in a pronounced 54.4% increase. This change can be attributed to the saturation of steel-concrete interfacial interaction. Therefore, a connector spacing-to-thickness ratio of approximately 37.5 provides an appropriate balance between interfacial restraint and the increase in force transmission.
In summary, the design process should proceed as follows. First, the concrete thickness should be determined within the range of 1100–1200 mm to achieve effective deformation control. Next, the steel plate thickness should be selected according to the required penetration resistance and local bearing capacity. Because the marginal benefit decreases markedly when the plate thickness exceeds 24 mm, local deficiencies should preferably be addressed by providing stiffening ribs. The material strength grade should then be selected primarily to satisfy load-bearing-capacity requirements. Finally, the connector spacing-to-thickness ratio should be set to approximately 37.5. Although these design measures reduce wall deformation, they also increase the peak impact force; therefore, the effects on supporting members and shear connectors should be verified concurrently when evaluating alternative designs.

4. Displacement Response of Double-Skin Steel-Concrete Composite Walls Subjected to Impact Loading

4.1. Analytical Model for the Resistance Function of Double-Skin Steel-Concrete Composite Walls

4.1.1. Development and Description of the Analytical Model

The failure modes of double-skin steel-concrete composite walls subjected to impact loading are generally similar to those under static loading. When inertial effects are negligible, the dynamic response may be approximated using an equivalent static loading configuration. Before failure, the wall exhibits two principal deformation modes: global flexural deformation induced by overall bending and local punching-shear deformation caused by shear failure of the concrete core. These modes are governed by distinct resistance mechanisms, namely the global flexural resistance, Rf, and the punching-shear resistance, RP. The governing failure mode is determined by comparing these resistances: when Rf < RP, the flexural resistance is reached first, and flexural failure governs; conversely, when RP < Rf, punching-shear failure occurs first. In both cases, ultimate failure is accompanied by tearing of the front steel plate at the impact location, indicating that the ultimate load-bearing capacity has been reached.
The nonlinear response of the wall is represented by the piecewise-linear resistance function shown in Figure 16.
Figure 16. Resistance function model. (a) Flexural deformation mode (Rf < RP); (b) Shear deformation mode (RP < Rf). Where Rf denotes the flexural yield resistance; Rp denotes the punching-shear cracking resistance; Ru denotes the ultimate resistance; Rr denotes the post-failure residual resistance; VC denotes the resistance loss caused by concrete punching-shear failure; k denotes the initial stiffness; αh denotes the stiffness-hardening coefficient accounting for membrane action; and αs denotes the stiffness-softening coefficient associated with failure.

4.1.2. Flexural Yield Resistance

When a four-edge-supported wall undergoes flexural deformation under a concentrated load, plastic hinge lines develop along the diagonals. According to yield-line theory, the flexural yield resistance Rf of the wall can be calculated as follows:
R f = 8 m f L L S − C − 0.172
In this expression, mf denotes the yield bending moment per unit width of the plate strip along the yield line; L denotes the side length of the wall panel; Ls denotes the panel span; and C denotes the side length of the loading plate.
For the wall configuration considered herein, the front and rear steel plates have identical thicknesses. At flexural yielding, the concrete neutral axis is assumed to coincide with the mid-depth of the concrete core; therefore, the yield moment is resisted entirely by the steel plates on both faces, as expressed below:
m f = σ s t s t c + t s
In this expression, σs denotes the normal stress in the steel plate, whereas ts and tc denote the thicknesses of the steel plate and concrete core, respectively.
The stress state of a steel plate-concrete composite wall is governed by the capacity and arrangement of the interfacial shear connectors. When the connector capacity is sufficient to prevent interfacial slip, the stress in the steel plate may reach its yield strength. Conversely, when the number of connectors is insufficient and interfacial slip occurs, the steel plate stress is calculated from the shear resistance provided by one-quarter of the total number of connectors on one face of the steel plate, where ndenotes the total number of connectors on that face. The normal stress in the steel plate is calculated as follows:
σ s = min 2 n Q u 8 t s L ,     f y
where n denotes the total number of welded shear connectors on one face of the steel plate.
According to Eurocode 4, the shear resistance Qu of an individual connector is calculated as follows:
Q u = min ( 0.29 α d 2 f c E c ,     0.8 σ u π d 2 / 4 )
In the formula, α is a coefficient. If the ratio of the length hs of the connecting element to its diameter d satisfies 3 ≤ hs/d ≤ 4, then α = 0.2(hs/d + 1); if hs/d > 4, then α = 1.

4.1.3. Punching-Shear Cracking Resistance

As shown in Figure 17, the out-of-plane concentrated load, F, applied to the wall is collectively resisted by the shear force in the front steel plate, VS, the shear force in the concrete core, VC, and the tensile force in the tie bars, T. When the load reaches Point A′, cracks propagate through the concrete core and the concrete approaches a fully cracked state. Concurrently, deformation of the steel plate and tie bars increases, and these components enter the yielding stage. At this stage, the shear force in the front steel plate and the tensile force in the tie bars are Vsy and Ty, respectively. Accordingly, the punching-shear cracking resistance of the wall is calculated as follows:
R P = V sy + V c + n V T y
Figure 17. Analytical model for calculating punching-shear cracking resistance.
In this expression, nV denotes the number of tie bars intersecting the concrete failure plane.
Yan et al. [10] proposed that the value of Vsy should be determined by comparing two mechanical models: (1) the shear yield capacity of the steel plate and (2) the punching-shear capacity of the concrete slab calculated using an equivalent slab thickness. The lower of the two calculated capacities should be adopted.
V sy = min 0.33 f C ′ E S E c t s S , f y 3 t s S
In this expression, f c ′ denotes the cylinder compressive strength of concrete; ES and Ec denote the elastic moduli of the steel plate and concrete, respectively; fy denotes the yield strength of the steel plate; ts denotes the steel plate thickness; and S denotes the perimeter of the loaded area.
In general, connector capacity may be governed by four potential failure modes: concrete breakout of the punching cone, Tbr; connector pull-out, Tpl; tensile failure of the connector, Tty; and shear failure of the steel plate, Tpy. The headed studs used in the double-skin steel-concrete composite walls examined in this study are short studs and rarely intersect the failure surface of the concrete punching cone. Therefore, their contribution to the punching-shear cracking resistance of the wall is neglected in the calculations. For tie bars, only the tensile capacity of the tie bars, Tty, and the shear-failure resistance of the steel plate, Tpy, need to be considered. In this study, the tensile force in the connectors, T, is calculated using the yield-strength expression recommended by Zhao Weiyi et al. [26], as follows:
T y = min T ty = π d t 2 σ ty / 4 T py = π d t t p f py / 3
In this expression, Tty denotes the tensile yield resistance of the tie bars; Tpy denotes the shear yield resistance of the steel plate; dt denotes the diameter of the tie bars; σty denotes the yield strength of the tie bars; tp denotes the thickness of the steel plate; and fpy denotes the yield strength of the steel plate.
The shear capacity of the concrete core, VC, is calculated as follows:
V C = 0.33 f c b 0 t c
In this expression, fc denotes the axial compressive strength of concrete; tc denotes the thickness of the concrete core; and b0 denotes the perimeter of the concrete punching cone measured at mid-depth of the concrete core.

4.1.4. Ultimate Resistance

The ultimate resistance of the wall, Ru, comprises the shear resistance of the steel plate, Vsu, and the tensile resistance of the connectors, Tu. In this study, Ru is calculated assuming a punching-shear deformation mode:
R u = n v T u + V su
The shear force in the steel plate and the tensile force in the tie bars are determined based on the ultimate strengths of their respective materials. Analogous to the calculation of the yield resistance, Ty, of the tie bars, their ultimate tensile capacity is calculated as follows [27]:
V su = f u ⋅ t s s / 3
T u = min T tu = π d t 2 σ tu / 4 T pu = π d t t p f pu / 3
In this expression, Ttu denotes the ultimate tensile resistance of the connector, and Tpu denotes the ultimate shear resistance of the steel plate.

4.1.5. Stiffness Calculation

Contact stiffness refers to the stiffness at the interface between the impactor and the double-skin steel-concrete composite wall. Based on the relationship between resistance and local indentation derived by Sohel et al. [28], the contact stiffness, k0, can be expressed as follows:
k 0 = 2 π r f c
In this expression, r denotes the radius of the impactor.
Previous studies have shown that wall deformation comprises two components: global deformation caused by flexural yielding of the wall and local bulging deformation caused by the reverse bearing action of the concrete punching-failure cone on the rear steel plate [29]. Before wall yielding, the resistance, R, may be assumed to vary linearly with the displacement, w, as follows:
R = kw
In the formula, k represents the initial stiffness of the wall.
As illustrated in Figure 18, the wall deformation can be represented by a series-spring model. The total wall displacement, w, comprises the global deformation, δg, and the local bulging deformation, δb. The corresponding stiffnesses for global and local deformation are denoted by kg and kb, respectively; therefore:
k = k g k b k g + k b
Figure 18. Decomposition of wall deformation.
According to plate and shell theory, within the elastic range, the elastic stiffness of a steel-concrete composite plate—simply supported on all four sides and subjected to a concentrated load—is given by:
k g = D 0.0116 L s 2
During formation of the concrete punching cone, the load is progressively transferred to the rear steel plate, resulting in local bulging. In this study, continuous tie bars extend through the wall thickness to restrain local bulging of the rear steel plate and enhance its local out-of-plane stiffness. This restraint limits the development of membrane action in the steel plate surrounding the punching zone. To incorporate this effect into the resistance function, the stiffness contribution of the tie bars is combined with the overall wall stiffness, as expressed by the following equation:
k b = 4 π f y t s + 0.1 β k g
In this expression, ρs denotes the steel ratio of the steel plates, and ρT denotes the steel ratio of the connectors.

4.1.6. Unified Expression for the Resistance Function

Based on the characteristic resistance values and initial stiffness derived above, the piecewise-linear resistance function of the double-skin steel-concrete composite wall can be expressed as follows:
R ω = k ω ,   0 ≤ ω ≤ ω A R f + α h k ( ω − ω A )   ω A < ω < ω C R U − α U K ( ω − ω C )   ω C < ω < ω D R r         ω > ω D
In this equation, K denotes the initial stiffness of the wall, whereas αH, αU, and αS denote the stiffness coefficients associated with hardening, softening, and unloading, respectively. The displacement corresponding to each characteristic point is denoted by ω A = R f k ,   ω c = R u − R f α h k ,   ω D = ω c + R u − R r α u k , when Rf > Rp, Rf is reached before the punching-shear resistance; the wall exhibits a flexure-dominated deformation mode; otherwise, it exhibits a punching-shear-dominated deformation mode.

4.2. Analysis Using the SDOF Method

In dynamic response analysis, the single-degree-of-freedom (SDOF) method represents the overall motion of a wall by the displacement at a selected characteristic point and idealizes the structure as a one-dimensional mass-spring-damper system. Based on energy equivalence, the equivalent mass, stiffness, and damping are determined by considering the actual mass distribution and assumed deformation shape. This approach can capture the structural response from the elastic stage to the plastic stage. It assumes that the structural response is governed by a single global deformation mode and that localized failure does not occur. The piecewise-linear resistance function presented in the preceding section provides the basis for solving the SDOF system.
As illustrated in Figure 19, the system comprises a mass element representing the effective structural mass, me; a spring element representing the structural stiffness, k; and a damping element representing the structural damping, c. The governing equation of motion is:
m e w ¨ t + c w ˙ ( t ) + R w t = 0
Figure 19. Equivalent single-degree-of-freedom system.
In this equation, w ¨ ( t ) , w ˙ ( t ) , and w(t) denote the acceleration, velocity, and displacement of the equivalent mass, respectively; R[w(t)] denotes the structural resistance function; and me denotes the equivalent mass of the SDOF system.

4.2.1. Equivalent Mass

Because actual structures have continuously distributed mass and theoretically infinite degrees of freedom, they must be idealized using equivalent lumped masses to establish a single-degree-of-freedom model. This idealization is based on two principles: (1) displacement compatibility and (2) kinetic-energy equivalence.
After establishing the equivalent model, the combined equivalent mass of the structure and impactor is denoted by me:
m e = k m m s + m h
In this expression, ms denotes the mass of the wall panel, mh denotes the mass of the impactor, and km denotes the equivalent mass coefficient. The calculation method for km is f A ( ρ s t s + ρ c t c ) ϕ 2 dA ( ρ s t s + ρ c t c ) A , and the meaning of the formula is detailed in the preceding text. Following Biggs’ two-stage plastic hinge assumption, α takes the value of αe in the elastic stage and αp in the plastic stage, and switches with the segmentation of resistance.
As illustrated in Figure 20, a simply supported wall panel is subjected to a concentrated force, F(t), at its center. The deformation shape of the panel is described by the shape function ϕ(x,y), which attains a maximum value of 1 at the panel center, (0, 0), where the maximum displacement occurs, and varies over the remainder of the panel. The center of the rear surface is selected as the characteristic point, and its vertical displacement, w(t), is used to represent the motion of the entire panel. Let A denote the total area of the wall panel and m(x,y) denote the mass per unit area. According to displacement compatibility, the displacement of the equivalent mass, m(e), is assumed to equal w(t). Applying kinetic-energy equivalence then yields:
1 2 m e w ˙ t 2 = ∬ 1 2 m x , y ⋅ w ˙ t ϕ x , y 2 dxdy
Therefore:
m e = ∬ m x , y ⋅ ϕ x , y dxdy
Figure 20. Schematic diagram of the forces and deformation of a wall panel.
If m(x,y) is a constant, then Equation (30) can be simplified to:
K m = ∬ ϕ x , y 2 dxdy A
During structural deformation, the shape function evolves continuously, causing the equivalent mass factor to vary and making an exact determination of the equivalent mass difficult. Based on the ideal plastic-hinge assumption, Biggs divided the deformation process into elastic and plastic stages. For a simply supported plate, the shape function is a three-dimensional surface and must be approximated using a high-order polynomial. For example, Grisaro et al. [30] used a 12th-order polynomial to describe the deformation of steel-concrete (SC) plates; however, neglecting the tensile force in the boundary studs resulted in an error of approximately 10%. Sohel [31] adopted a mass factor of 0.17 for SC panels in the plastic range. Using finite element analysis, Bruhl et al. [32] determined that mass factors of 0.20 and 0.10 are appropriate for SC plates before and after yielding, respectively. Accordingly, this study adopts the values proposed by Bruhl et al. [32]; thus, according to Equation (31):
m e =     0.2 m s + m h               0 ≤ w t ≤ w y 0.1 m s + m h                           w t > w y

4.2.2. Damping Ratio and Spring Stiffness

The maximum structural response to impact loading occurs during the first response cycle. Because damping has little influence on this peak response, it is neglected during the loading phase. During unloading, however, the amplitude of free vibration decays rapidly; damping must therefore be considered at this stage. The calculation formula for the damping ratio adopted in this study is as follows:
c = 0 0 ≤ w ( t ) ≤ w max 2 ζ m e k = 2 m e k × 50 % w ( t ) > w max
Through calculation and comprehensive evaluation in this study, the damping ratio is taken as 0.02. In a single-degree-of-freedom (SDOF) system, the spring stiffness characterizes the overall resistance to deformation and corresponds to the stiffness of the actual structure. The spring resistance is represented by the resistance function, R[x(t)]. As illustrated by the resistance-function model, the hardening response along segments AC and B′C′ is governed by the hardening stiffness, αhk; the softening response along segments A′B′, CD and C′D′ is governed by the softening stiffness, −αsk; and the unloading response is governed by the unloading stiffness, αuk.
The values for each stiffness coefficient are presented in Table 5:
Table 5. Values of stiffness coefficients for the SDOF method.
In dynamic analysis, the strain-rate sensitivity of constituent materials should be considered where appropriate. Sukontasukkul [33] reported that strain-rate effects in concrete members subjected to two-way bending are substantially lower than those in members subjected to one-way bending. The further demonstrated that, for simply supported steel-concrete (SC) panels under impact loading, strain rates in most regions remain below 1 s−1, which is comparable to the quasi-static range. Accordingly, strain-rate effects are neglected in the present study [34].

4.2.3. Numerical Solutions

The governing differential equation for the SDOF system is given in Equation (28). Its initial conditions are specified as follows. The response variables w(0) = 0 and w ˙ 0 = m h m e v 0 are obtained by solving the equation of motion using the finite-difference method. The displacement, velocity, and acceleration of the equivalent mass at time ti can then be expressed as:
w t i = w i
w ˙ t i = w ˙ i = w i + 1 − w i − 1 2 Δ t
w ¨ t i = w ¨ i = w i + 1 − 2 w i + w i − 1 Δ t 2
In the formula, Δt = 5 × 10−5 s represents the time step.
Then, Equation (33) can be transformed into:
m e w i + 1 − 2 w i + w i − 1 Δ t 2 + c w i − w i − 1 Δ t + R w i = 0
Further solving for the displacement at time ti+1 yields the following recurrence relation:
w i + 1 = 2 w i − w i − 1 − c Δ t m e w i − w i − 1 − Δ t 2 m e R w i
The first two terms of the recurrence relation are:
w 0 = 0
w 1 = w 0 + w ˙ Δ t = m h m e v 0 Δ t

4.3. Comparison of Calculation Results

4.3.1. Comparison with Test Results

Table 6 compares SDOF predictions with displacement measurements reported in published impact tests to assess the method’s ability to predict the displacement response at the center of the wall base. The ratio is defined as the SDOF-predicted value divided by the corresponding experimental value. For maximum displacement, the ratios range from 0.89 to 1.14, with a mean value of 1.073. Thus, the SDOF method overpredicts maximum displacement by 7.3% on average, although it underpredicts the response of some individual specimens by approximately 11%. For residual displacement, the mean ratio is 0.978, corresponding to an average underprediction of 2.2%. Overall, the SDOF method provides slightly conservative predictions of maximum displacement on average, while slightly underestimating residual displacement.
Table 6. Comparison of SDOF method results with experimental values.
The comparison shows that the maximum displacements predicted by the SDOF method are, on average, 7.3% greater than the experimental values. This discrepancy is likely attributable to idealizations in the equivalent parameters, including the use of the static deformation profile as the assumed mode shape and the adoption of ideal fixed-end boundary conditions. In contrast, the predicted residual displacements agree closely with the experimental results because the resistance function is derived directly from static analysis, and the stiffness in the post-yield and strain-hardening ranges closely represents the actual hysteretic response. In addition, the SDOF displacement time history directly provides the residual displacement after unloading without requiring further constitutive assumptions. Although stiffness degradation in cracked concrete is complex and nonlinear, the SDOF method captures the principal features of the structural dynamic response by employing displacement-dependent, piecewise-defined equivalent stiffness and mass. This approach provides an effective balance between computational efficiency and engineering accuracy, making it suitable for rapid assessment and parametric screening during preliminary design; however, it should not replace detailed finite element analysis or experimental validation.

4.3.2. Comparison with Finite Element Simulation Results

The results in Table 7 demonstrate that the SDOF model developed in this study can effectively predict the dynamic displacement response of the wall. For maximum displacement, the ratio of the SDOF prediction to the finite element result has a mean of 1.029, a standard deviation of 0.126, and a variance of 0.0159. For residual displacement, the corresponding ratio has a mean of 1.032, a standard deviation of 0.153, and a variance of 0.0234. The mean deviations of 2.9% and 3.2%, respectively, are within an acceptable range. Moreover, the ratios are distributed closely around 1.0 without an apparent systematic bias, indicating that the model provides reliable estimates of both maximum and residual displacements.
Table 7. Comparison of SDOF method results with simulated values.
However, close-to-unity mean ratios do not imply low dispersion. The coefficients of variation for maximum and residual displacement are 12.3% and 14.8%, respectively, which are approximately four to five times their corresponding mean deviations. This finding indicates that the typical relative error of an individual prediction is substantially greater than that implied by the mean deviation; therefore, the model has limited reliability for precise prediction of a single response. In addition, the variance of the residual-displacement ratio is approximately 47% greater than that of the maximum-displacement ratio, suggesting that the predictive accuracy of the model deteriorates during the later stages of the response.
This discrepancy primarily arises from changes in the structural response during the later stages of loading. Once the structure enters the plastic regime, material nonlinearity, interfacial contact conditions, and energy-dissipation mechanisms become increasingly coupled. Because the SDOF model represents these complex phenomena using simplified equivalent parameters, its loss of accuracy is more pronounced in the plastic stage than in the elastic stage.
Overall, this model is well-suited for applications centered on relative comparisons—such as assessing response trends, analyzing the influence of parameters, and evaluating or selecting between different design schemes. However, when precise displacement values are required, accurate verification should still be performed using finite element analysis.

5. Conclusions

This study combines numerical simulation and theoretical analysis to investigate the out-of-plane impact and punching-shear resistance of steel-concrete (SC) composite walls for nuclear-power applications subjected to low-velocity drop-weight impact. The main work includes the development of a finite element model for drop-weight impact, validated against published experimental data; a systematic parametric investigation of steel plate thickness, steel strength, concrete strength, concrete-core thickness, and span-to-c (The stud spacing-to-plate thickness ratio); and the establishment of a piecewise-linear resistance function and an equivalent single-degree-of-freedom (SDOF) method for predicting structural displacement. The principal conclusions are as follows:
(1)
A finite element model of a double-skin steel-concrete composite wall subjected to drop-weight impact was developed in ABAQUS. Concrete was represented using the concrete damaged plasticity (CDP) model, whereas steel was modeled using a bilinear strain-hardening constitutive relationship. The steel plates and concrete core were discretized using S4R shell elements and C3D8R solid elements, respectively, and the boundary conditions were simplified as four-edge constraints to replicate the experimental setup. The model reproduced the impact-force and displacement time histories, as well as the observed failure characteristics, including steel plate yielding and concrete crushing. The predicted peak responses and response durations agreed well with the experimental results, demonstrating the reliability of the modeling approach.
(2)
The parametric analysis indicates that residual deformation is substantially more sensitive to geometric parameters than to material-strength parameters. Increasing the concrete-core thickness from 1000 to 1200 mm reduced the residual displacement by 38.5%, whereas reducing the connector spacing-to-thickness ratio from 50 to 25 reduced it by 33.7%. However, further reducing this ratio from 37.5 to 25 increased the peak impact force by approximately 54.4%; therefore, a spacing-to-thickness ratio of 37.5 provides the most balanced performance. For a 10% variation in each parameter, the corresponding changes in deformation were 19.2% for concrete thickness, 2.83% for steel plate thickness, 1.28% for concrete strength, and 0.52% for steel strength. Increasing material strength primarily enhanced load-bearing capacity but had limited influence on deformation control. Accordingly, concrete-core thickness should be adjusted to control deformation, whereas material strength grades should be selected to satisfy load-bearing requirements.
(3)
Based on yield-line theory and the concrete punching-shear failure mechanism, a piecewise-linear resistance function was developed, comprising the stages of flexural yielding, punching-shear cracking, ultimate resistance, and post-failure resistance. Calculation methods for the resistance and stiffness at each characteristic point were established and incorporated into an equivalent single-degree-of-freedom (SDOF) system, thereby providing a rapid method for predicting the maximum and residual displacements of walls. The proposed approach was validated against both experimental data and finite element analysis (FEA) results. The mean ratios of the predicted maximum and residual displacements to the experimental values were 1.073 and 0.978, respectively, whereas the corresponding ratios to the FEA results were 1.029 and 1.032. Despite a scatter of approximately 12–15% for individual data points, the model showed good overall agreement and is suitable for rapid assessment and parameter screening during the design of impact-resistant structures.

Future Work

In future research, the fracture behavior of high-strength steel plates with different ductility levels will be further explored. High-strength steels with low elongation may suffer premature tearing and fracture under high-speed impact, while high-ductility high-strength steel is promising for improving the anti-penetration performance of steel-concrete composite walls used in nuclear engineering. The influence of elongation limits and strain-rate-dependent fracture criteria on the impact resistance of single-sided steel plate concrete structures will be systematically investigated to provide more comprehensive guidance for the material selection of protective nuclear walls.

Author Contributions

Methodology, Y.Z.; validation, X.Z. (Xinwen Zhang); formal analysis, X.Z. (Xinwen Zhang) and Y.Z.; resources, Y.Z. and X.Z. (Xin Zhang); data curation, X.Z. (Xin Zhang), Y.X.; writing—original draft, X.Z. (Xinwen Zhang), Y.Z.; writing—review and editing, Y.Z.; visualization, X.Z. (Xu Zhang); supervision, Y.Z.; funding acquisition, Y.Z. All authors have read and agreed to the published version of the manuscript.

Funding

The National Natural Science Foundation of China (Grant No. 51508074).

Data Availability Statement

Data is contained within the article.

Conflicts of Interest

Author Xin Zhang is employed by State Grid Gansu Electric Power Company, Liujiaxia Hydropower Plant. The remaining authors declare that this research was conducted in the absence of any commercial or financial relationships that could be construed as a potential conflict of interest.

References

  1. Jiang, Z. Nuclear Power Development for Greenhouse Gases Emission Reduction under Climate Change. Clim. Change Res. 2010, 6, 376–380. [Google Scholar]
  2. GB 50267-97; Code for Seismic Design of Nuclear Power Plants. China Planning Press: Beijing, China, 1998.
  3. Varma, A.H.; Malushte, S.R.; Sener, K.C.; Lai, Z. Steel-plate composite (SC) walls for safety related nuclear facilities: Design for in-plane forces and out-of-plane moments. Nucl. Eng. Des. 2014, 269, 240–249. [Google Scholar] [CrossRef] [Scilit]
  4. Zhao, W.; Wang, L.; Guo, Q.; Gao, Z. Research Advances on Impact Resistance of Steel-concrete Composite Structures. Steel Constr. (Chin. Engl.) 2020, 35, 26–36. [Google Scholar] [CrossRef]
  5. Li, X.; Li, X. Study on In-plane Flexural Behavior of Double Steel Plates and Concrete Infill Composite Shear Walls for Nuclear Engineering. Eng. Mech. 2017, 34, 43–53. [Google Scholar] [CrossRef]
  6. Kim, K.; Lee, K.; Shin, J.; Lee, J.; Varma, A. A study on the resistance of SC walls subjected to missile impact using large-scale impact tests. Int. J. Impact Eng. 2026, 139, 103507. [Google Scholar] [CrossRef] [Scilit]
  7. Wang, Y.; Sah, T.P.; Lu, J.; Zhai, X. Behavior of steel-concrete-steel sandwich beams with bolt connectors under off-center impact load. J. Constr. Steel Res. 2021, 186, 106889. [Google Scholar] [CrossRef] [Scilit]
  8. Yan, C.; Wang, Y.; Zhai, X. Low velocity impact performance of curved steel-concrete-steel sandwich shells with bolt connectors. Thin-Walled Struct. 2020, 150, 106672. [Google Scholar] [CrossRef] [Scilit]
  9. Lu, J.; Wang, Y.; Zhai, X. Response of flat steel-concrete-corrugated steel sandwich panel under drop-weight impact load by a hemi-spherical head. J. Build. Eng. 2021, 9, 102890. [Google Scholar] [CrossRef] [Scilit]
  10. Yan, C. Research on Impact Performance of Curved Double Steel-Concrete Composite Shells; Harbin Institute of Technology: Harbin, China, 2021. [Google Scholar]
  11. Remennikov, A.M.; Kong, S.Y.; Uy, B. The response of axially restrained non-composite steel–concrete–steel sandwich panels due to large impact loading. Eng. Struct. 2013, 49, 806–818. [Google Scholar] [CrossRef] [Scilit]
  12. Zhang, W.; Huang, Z.; Li, R.; Zhao, X.; Ye, J. Impact Response of Double-Layer Steel-RULCC-Steel Sandwich Panels: Experimental, Numerical, and Analytical Approaches. J. Struct. Eng. 2022, 148, 17. [Google Scholar] [CrossRef] [Scilit]
  13. Yang, Y.; Wang, R.; Zhao, H.; Hou, C. Impact Resistence Mechanism and Deflection Prediction of Steel-concrete Composite Wall under Fire Exposure. Explos. Shock Waves 2024, 44, 012101. [Google Scholar] [CrossRef]
  14. Sun, J.; An, G.; Wamh, R. Research on Mechanical Properties of Steel-Concrete Composite Panels Under Impact Loading. Ind. Constr. 2024, 54, 108–116. [Google Scholar] [CrossRef]
  15. An, G.; Yang, B.; Zong, Z.; Huang, D. Dynamic Response of Double-skin Steel Recycled Aggregate Concrete Composite Panels Under Low-velocity Impact. Eng. Mech. 2026, 43, 210–218. [Google Scholar] [CrossRef]
  16. Yu, Y.; Cai, L.; Tang, R.; Ding, R.; Fan, J.; Liu, J. Experimental Research on Impact Resistance of Half Steel Plate Concrete Structures with Different Tie Bar Details. Ind. Constr. 2024, 54, 19–27. [Google Scholar] [CrossRef] [Scilit]
  17. Fan, J.; Ding, R.; Sun, Y. Research on the Application of Steel-plate Concrete Structures in Nuclear Plant Engineering. Ind. Constr. 2023, 53, 18–28. [Google Scholar] [CrossRef]
  18. Zhu, L.; Gao, X.; Zhang, C. Finite Element Analysis for Out-of-plane Anti-impact Performance of Unwelded Steel Plate-concrete-steel Plate Composite Shear Wall with All Bolted Joints. J. Vib. Shock 2021, 40, 166–174. [Google Scholar] [CrossRef]
  19. Wang, W.; Yang, J.; Wang, A.; Zhou, B.; Li, X. A Study of the Design and Calculation Method of Double-skin Steel-concrete Shield Based on Energy Approach. Explos. Shock Waves 2023, 43, 114203. [Google Scholar] [CrossRef]
  20. Han, P.; Liu, J.; Fei, B.; Wang, F. A Study on Steel-Concrete-Steel Wall to Resist Perforation from Rigid Projectile Impact; Hindawi Limited: London, UK, 2021. [Google Scholar] [CrossRef] [Scilit]
  21. Lubliner, J.; Oliver, J.; Oller, S.; Oñate, E. A plastic-damage model for concrete. Int. J. Solids Struct. 1989, 25, 299–326. [Google Scholar] [CrossRef] [Scilit]
  22. GB 50010-2010; Code for Design of Concrete Structures. Ministry of Housing and Urban-Rural Development of the PRC: Beijing, China, 2010.
  23. Zhao, W.; Guo, Q. Study on Behavior of Double-skin Steel-concrete Composite Walls Subjected to Low-velocity Impact. China Civ. Eng. J. 2018, 51, 88–94. [Google Scholar] [CrossRef]
  24. GB 50017-2017; Standard for Design of Steel Structures. Ministry of Housing and Urban-Rural Development of the PRC: Beijing, China, 2017.
  25. GB/T 1591-2018; High Strength Low Alloy Structural Steels. Standardization Administration of the PRC: Beijing, China, 2018.
  26. Zhao, W.; Gao, Z.; Wang, L.; Chen, P. Mechanical Performance of Two-way Simply Supported Steel-plate Composite Slabs under Concentrated Load. Eng. Mech. 2022, 39, 158–170+192. [Google Scholar] [CrossRef]
  27. Mhalhal, J.M.; Alawsi, M.A.; Al-Gasham, T.S.; Abid, S.R. Impact the shear connector properties onthe behavior of steel–concrete-steel sandwich beams. Mater. Today Proc. 2021, 56, 2043–2047. [Google Scholar] [CrossRef] [Scilit]
  28. Sohel, K.M.A.; Liew, J.Y.R. Behavior of steel-concrete-steel sandwich slabs subject to impact load. J. Constr. Steel Res. 2014, 100, 163–175. [Google Scholar] [CrossRef] [Scilit]
  29. Guo, Q.; Zhao, W. Displacement response analysis of steel-concrete composite panels subjected to impact loadings. Int. J. Impact Eng. 2019, 131, 272–281. [Google Scholar] [CrossRef] [Scilit]
  30. GB/T 51340-2018; Technical Standard for Steel Plate Concrete Structures in Nuclear Power Plants. China Planning Press: Beijing, China, 2018.
  31. Sohel, K.M.A. Impact Performance of Steel-Concrete-Steel Sandwich Structures; National University of Singapore: Singapore, 2008. [Google Scholar]
  32. Bruhl, J.C.; Varma, A.H.; Kim, J.M. Static resistance function for steel-plate composite (SC) walls subject to impactive loading. Nucl. Eng. Des. 2015, 295, 843–859. [Google Scholar] [CrossRef] [Scilit]
  33. Sukontasukkul, P. Impact Behaviour of Concrete Under Multiaxial Loading; The University of British Columbia: Vancouver, BC, Canada, 2002. [Google Scholar]
  34. Liu, C.; Gao, F.; Deng, S.; Wang, Z.; Lu, H.; Deng, G.; Wang, M. Investigation on the damage and assessment of steel-concrete-steel composite structures subjected penetration and explosive loadings. Structures 2025, 83, 110841. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.