Skip to Content
BuildingsBuildings
  • Article
  • Open Access

1 October 2026

29 Pages

Axial Compressive Behaviour of Intermediate-Length Concrete-Filled Steel Tubular Columns with Different CFRP Wrapping Configurations

,
,
,
and
1
School of Civil Engineering and Smart Construction, Chang’an University, Xi’an 710061, China
2
School of Civil Engineering, Harbin Institute of Technology, Harbin 150090, China
3
Qinghai Provincial Key Laboratory of Green Transportation Disaster Prevention and Reduction and Digital Technology, Qinghai Polytechnic University, Xi’ning 810003, China
*
Author to whom correspondence should be addressed.
This article belongs to the Section A. Building Structures

Abstract

The strengthening of intermediate-length concrete-filled steel tubular (CFST) columns using CFRP has attracted growing attention, but the effect of fibre orientation on the axial compressive behaviour—particularly for members where stability rather than strength governs—has not been fully clarified. This study therefore addressed the issue through a combined experimental, numerical, and analytical approach. Specimens were divided into four groups: unstrengthened controls, those with four longitudinal CFRP layers, those with four hoop layers, and a hybrid group with two longitudinal plus two hoop layers. All were tested under monotonic axial compression. The ultimate load-carrying capacity was enhanced by 23.0%, 20.5%, and 8.4% for the longitudinal, hybrid, and hoop-only CFRP wrapping schemes, respectively. These findings indicate that the strengthening efficiency is likely governed by the wrapping configuration under the conditions examined in the present test programme. Unstrengthened columns exhibited local buckling of the steel tube and crushing of the concrete core, a brittle failure mode. Longitudinal CFRP participated directly in load resistance and raised the flexural stiffness, thus effectively suppressing global buckling—the critical mode for intermediate-length columns. The hybrid configuration provided a reasonable strength gain and exhibited a relatively gentle descending branch together with favourable deformation compatibility. Hoop-only confinement, however, contributed little to stability improvement because it only provided lateral restraint without affecting bending resistance. A three-dimensional finite element model was constructed in ABAQUS, and its predictions of failure modes, load–displacement curves, and ultimate loads agreed well with the experimental data, confirming its reliability. Parametric studies using this model further revealed that the axial capacity decreased markedly with increasing slenderness ratio, whereas higher concrete and steel strengths both led to steady improvements. Finally, a simplified design formula was derived for the axial compressive capacity of CFRP-confined circular CFST intermediate-length columns. This formula includes a confinement efficiency coefficient that reflects the wrapping pattern and a stability coefficient suitable for intermediate-length members. Comparisons with both experimental and numerical results demonstrated that the proposed formula yields predictions within ±5% of the present dataset. The formula is applicable to circular CFST intermediate-length columns with 40 ≤ λ ≤ 80, concrete grades of C30–C50, steel grades of Q235–Q460, and the three wrapping configurations examined herein. Extension to slenderness ratios below 40 requires further validation, since the present tests and parametric study did not cover this range. Further independent validation is warranted prior to its adoption in general design.

1. Introduction

As structures increasingly move towards larger spans, greater heights, and heavier loads, column members are required not only to possess high load-bearing efficiency but also to meet stability and durability demands over long-term service. In a concrete-filled steel tube (CFST) column, the steel tube confines the lateral expansion of the concrete, whereas the concrete core retards local buckling of the tube; this interaction gives the composite member considerable load capacity, stiffness, and ductility, which is why CFST has been widely used in bridge piers, high-rise buildings, and industrial facilities. Existing studies have demonstrated that cross-section shape, diameter-to-thickness ratio, concrete strength, steel ratio, slenderness ratio, loading path, and service environment all significantly affect the axial compressive performance of CFST [1,2,3,4,5,6,7,8,9,10].
However, the long-term performance of CFST in aggressive environments remains a concern. Corrosive agents in marine, chemical, or humid settings can cause steel tube rusting, which impairs the steel strength, the interface interaction between the two components, and the confinement provided to the core concrete. For intermediate-length columns (20 < λ ≤ 80), the stability problem becomes increasingly pronounced with rising slenderness ratio, and the member capacity is no longer governed solely by material strength but also by geometric imperfections, initial stresses, and second-order effects. Available experimental and numerical studies have indicated that a larger slenderness ratio reduces the axial compressive capacity of CFST columns and alters the failure development from local buckling dominance to global flexural buckling dominance [11,12,13]. Therefore, for intermediate-length columns operating in harsh service environments with stability demands, it is imperative to develop strengthening techniques that simultaneously account for durability, material confinement, and overall stability against buckling.
Existing CFST strengthening approaches include steel jacketing, section enlargement, grouting repair, and external bracing, among others [14,15,16,17]. Steel jacketing and external concrete-filled steel tube (CFST) jacketing can improve section stiffness and bearing capacity, but they add self-weight and may introduce problems such as welding, corrosion protection, and on-site construction difficulties. Fiber-reinforced polymers (FRPs), owing to their light weight, high strength, corrosion resistance, and good constructability, have gradually become an important material for strengthening CFST structures. FRP wraps not only form an external protective barrier but also improve the mechanical behaviour of the member by restraining steel tube deformation and lateral expansion of the core concrete [18,19,20]. Mirmiran et al. [21] first proposed the concept of combining FRP with CFST, and subsequent studies have confirmed that the number of FRP layers, cross-sectional shape, and material parameters all influence the strength and ductility of the members [22]. Compared with rectangular sections, circular sections are subjected to more uniform hoop confinement from FRP, and consequently the increase in load-bearing capacity is generally more pronounced [23,24,25].
Carbon fiber-reinforced polymer (CFRP) possesses high tensile strength and elastic modulus, along with excellent corrosion resistance, and is therefore widely used among FRP materials [26]. In CFRP-confined circular CFST members, hoop fibers mainly restrain radial expansion and local bulging of the steel tube, thereby enhancing lateral confinement; longitudinal fibers help to improve the axial stiffness of the member and exert a certain restraining effect against global flexural buckling [27,28,29]. Existing studies have shown that hoop CFRP generally contributes to improving the ultimate load capacity and ductility of short columns, whereas longitudinal CFRP has a positive effect on the stiffness and stability capacity of members with intermediate slenderness ratios [30,31]. For members with partial or spaced wrapping, CFRP can also delay local buckling of thin-walled steel tubes [32]. Under adverse conditions such as post-fire exposure, corrosion, and impact, CFRP wrapping has also demonstrated a certain capacity for performance recovery and mitigation of degradation [33,34,35].
Although substantial progress has been made in the study of CFRP-confined CFST, existing work remains largely focused on short columns, unidirectional wrapping, or specific loading conditions. For intermediate-length CFST columns, the axial compressive response is governed by both global instability and sectional confinement, and the use of either hoop or longitudinal CFRP alone is insufficient to fully reveal the synergistic mechanism between the two fibre orientations. Most existing capacity models take the number of CFRP layers or a confinement coefficient as the primary parameter, but generally do not explicitly account for the differing contributions of wrapping direction to axial strengthening, lateral confinement, and stability enhancement. Consequently, their applicability to intermediate-length columns with hybrid wrapping has yet to be validated. Furthermore, the coupling relationship among CFRP stress transfer, steel tube buckling development, and core concrete damage progression under hybrid wrapping conditions remains to be further elucidated.
Motivated by these considerations, this study focuses on CFRP-confined circular CFST intermediate columns and employs a combined experimental, numerical, and analytical approach to investigate the axial compressive behaviour of members with different CFRP wrapping configurations. The test programme includes specimens with four layers of hoop CFRP, four layers of longitudinal CFRP, and a hybrid scheme combining two hoop layers with two longitudinal layers. Through measurements of load, axial displacement, mid-span lateral displacement, and strain responses, the effects of wrapping pattern on failure mode, yield load, ultimate capacity, stiffness, ductility, and buckling resistance are analysed. Subsequently, a refined finite element model is established in ABAQUS, incorporating material nonlinearity, interface contact, CFRP damage, and initial geometric imperfections, and parametric studies are carried out with respect to slenderness ratio, concrete strength, and steel strength. On this basis, and by integrating the experimental and numerical results, a calculation method for axial compressive capacity is proposed, which introduces a CFRP confinement efficiency coefficient, wrapping-pattern modification factors, and stability coefficients for intermediate columns, and is applicable to various wrapping arrangements. The findings are expected to serve as a reference for the performance evaluation and engineering design of CFRP-confined circular CFST intermediate columns.

2. Experimental Program

2.1. Specimen Design

In this test, four CFST intermediate-length column specimens were designed, three of which were strengthened with CFRP wrapping, with the specific configurations shown in Figure 1. It is worth noting that only one specimen was prepared for each wrapping configuration; consequently, the capacity improvements reported below derive from single tests and should be regarded as indicative rather than statistically validated.
Figure 1. Configuration of CFST intermediate-length columns with different CFRP wrapping patterns.
The CFST intermediate-length columns consist of circular steel tubes and core concrete, with a height of 1500 mm. The slenderness ratio is defined as λ = L0/i, where L0 denotes the effective length and i the radius of gyration of the cross-section. With both ends pinned, L0 = L = 1500 mm, and i = D/4 = 36.5 mm for the circular section, yielding λ = 41.1. According to GB 50936-2014 [36], CFST columns with 20 < λ ≤ 80 are categorized as intermediate-length columns. The outer diameter and inner diameter of the circular steel tube are 146 mm and 140 mm, respectively (tube wall thickness of 3 mm). The core concrete was cast using C40 concrete. To clarify the influence of CFRP wrapping patterns on the axial compressive behaviour of CFST intermediate-length columns, this study examined the failure modes, ultimate bearing capacity, and mid-span lateral displacement of the columns under three wrapping configurations: hoop wrapping, longitudinal wrapping, and hybrid hoop–longitudinal wrapping. The CFRP sheets were wrapped over the full height of each specimen, with an overlap length of 100 mm per layer, approximately one quarter of the column perimeter. The epoxy adhesive was applied at a nominal thickness of 0.5 mm per layer. Prior to wrapping, the steel tube surface was ground and cleaned with acetone. The hybrid specimens were laid up as two longitudinal layers followed by two hoop layers (0°/0°/90°/90°), and all wrapped specimens were cured at room temperature for 7 days. The basic parameters of the four groups of CFST intermediate-length columns are listed in Table 1.
Table 1. Specimen parameters.
The specimen designation consists of three parts: the first part denotes the specimen number; the second part indicates the number of longitudinal CFRP layers; and the third part gives the number of circumferential CFRP layers. For instance, specimen C3-L2-C2 refers to the third test column, which is a circular CFST intermediate-length column wrapped with two longitudinal and two circumferential layers of CFRP unidirectional sheets.

2.2. Material Properties

To obtain the basic mechanical properties of the core concrete in the CFST columns, three groups of C40 concrete cube specimens (150 mm × 150 mm × 150 mm) and prism specimens for axial compressive tests (150 mm × 150 mm × 300 mm) were prepared in accordance with the Chinese standard GB/T 50081-2019 [37]. After curing at room temperature for 28 days, uniaxial compression tests were conducted using a pressure testing machine at a loading rate of 0.5 MPa/s. The compressive strength of concrete cubes fcu, axial compressive strength fc, and elastic modulus Ec are presented in Table 2.
Table 2. Mechanical properties of concrete.
The mechanical properties of the steel were determined in accordance with the Chinese standard GB/T 228.1-2021 [38]. Three standard tensile specimens, with dimensions of Φ10 mm × 50 mm and a gauge length of 30 mm, were cut from the same batch of Q235 steel tubes. Tensile tests were performed using an electronic universal testing machine at a loading rate of 2 mm/min. The yield strength fy, ultimate tensile strength fu, elastic modulus Es, and Poisson’s ratio ν s of the steel are summarized in Table 3.
Table 3. Mechanical properties of steel.
The unidirectional carbon fiber sheets were woven from T700-grade carbon fiber yarns, with the product designation UT70-30. Three CFRP tensile coupons were prepared, measuring 250 mm × 25 mm × 0.167 mm. Tensile tests were performed using an electronic universal testing machine [39] at a loading rate of 1 mm/min. The tensile strength ff, elastic modulus Ef, and elongation at break ε f of the CFRP sheets obtained from the tests are listed in Table 4.
Table 4. Mechanical properties of unidirectional CFRP sheets.
The epoxy resin adhesive used in this test was an E2500S two-component system, supplied by Konishi Co., Ltd. Shanghai (Shanghai, China), and manufactured by Keyang Fine Chemical (Suzhou) Co., Ltd. (Suzhou, China). The adhesive was prepared by mixing the resin and hardener at a mass ratio of 2:1. The mechanical properties of the epoxy resin adhesive are presented in Table 5.
Table 5. Mechanical properties of epoxy resin adhesive.

2.3. Loading and Instrumentation

To capture the lateral deformation of the CFST columns during axial compression tests, displacement transducers were placed at the quarter-height, mid-height, and three-quarter-height positions of each specimen, as illustrated in Figure 2. Meanwhile, to measure the longitudinal and circumferential strains of the CFRP sheets under uniaxial compression, four pairs of strain gauges—one longitudinal and one circumferential in each pair—were attached along the column perimeter at the same three height levels, as shown in Figure 2c. The strain gauges with odd numbers were arranged in the longitudinal direction, while those with even numbers were placed in the circumferential direction. The circumferential strain gauges were used to capture the hoop deformation of the CFRP-wrapped steel tube, reflecting the confinement effect provided by the core concrete; the longitudinal gauges measured the axial deformation of the tube, which allowed for an assessment of the deformation compatibility between the steel tube and the core concrete. Initial geometric imperfections were measured prior to testing. The measured maximum out-of-straightness was 0.62 mm for C1-L0-C0, 0.78 mm for C2-L4-C0, 0.91 mm for C3-L2-C2, and 0.71 mm for C4-L0-C4, corresponding to L/2419, L/1923, L/1648, and L/2113, respectively, all below the L/1500 limit. The measured loading eccentricity was 1.2 mm for C1-L0-C0, 0.8 mm for C2-L4-C0, 1.6 mm for C3-L2-C2, and 1.1 mm for C4-L0-C4, all within the 2 mm control tolerance. These measured values confirm that the specimens met the intended pinned-end and centring conditions, and they are consistent with the imperfection amplitude of L/1000 adopted in the finite element model.
Figure 2. Loading apparatus and sensor layout.
Axial compression tests were conducted using a YDL-Y5000 electro-hydraulic servo-controlled testing machine in the laboratory of Chang’an University. Prior to the formal tests, each CFST column was preloaded to ensure close contact between all interfaces of the loading system and to allow the testing machine and all measuring instruments to reach a stable operating condition. During preloading, the loading rate was set at 1 mm/min, and the load was increased to approximately 10% of the estimated ultimate load, followed by gradual unloading to 0 kN. In the formal loading phase, the loading rate was reduced to 0.2 mm/min and maintained until the specimen reached the failure state.

3. Test Results and Analysis

3.1. Test Process and Failure Modes

The failure patterns of the CFST intermediate-length column specimens are shown in Figure 3. Specimen C1-L0-C0 served as the control specimen and was not strengthened with CFRP. During the early stage of loading, no obvious deformation or cracking appeared on the surface of C1-L0-C0, indicating that the specimen remained in the elastic deformation phase. At this stage, the steel tube mainly transmitted the axial load, while the concrete sustained the compressive stress, and the overall deformation of the specimen remained small and exhibited a linear relationship with the applied load. As the load continued to increase, the core concrete entered the elastoplastic stage earlier than the steel tube, and plastic deformation gradually developed. When the load reached approximately 800 kN, a crushing sound from the concrete could be heard. At 995 kN, the rate of increase in mid-span lateral displacement accelerated noticeably, accompanied by visible deformation of the steel tube. When the load attained 1022 kN, the specimen reached its ultimate bearing capacity; the load ceased to increase further, and apparent local buckling appeared on the surface of the steel tube.
Figure 3. Failure modes of specimens.
Specimen C2-L4-C0 was a CFST intermediate-length column wrapped with four layers of longitudinal CFRP, with the fibre direction aligned with the column axis. During the early stage of loading, both the steel tube and the core concrete remained in the elastic state. As the load increased, the hoop stress in the steel tube gradually rose owing to the lateral expansion of the concrete, and on the tension side of the column the CFRP began to sustain tensile forces. When the load reached approximately 1000 kN, faint cracking sounds from the CFRP could be heard. At 1257 kN, the specimen reached its ultimate bearing capacity, at which point distinct cracking noises from the CFRP were clearly audible, and fracture of the CFRP at the mid-span was observed. The load then dropped suddenly to 1050 kN, after which it declined gradually.
Specimen C3-L2-C2 was a CFST column wrapped with two longitudinal layers and two circumferential layers of CFRP. At the initial loading stage, the specimen remained in the elastic deformation regime. As the load increased further, the CFRP on the tension side at mid-span became taut, while wrinkles appeared on the compression side. When the load reached 1231 kN, the specimen attained its ultimate bearing capacity. With continued loading beyond this point, the displacement increased steadily while the load remained essentially unchanged, indicating favourable plastic behaviour of the specimen. Upon further loading, the specimen eventually failed by instability, and the load capacity gradually decreased.
Specimen C4-L0-C4 was a CFST column wrapped with four circumferential layers of CFRP, with the fibres oriented in the hoop direction of the steel tube. At the beginning of loading, the observed behaviour was similar to that of the previous specimens: the column remained in the elastic stage, and no visible changes occurred on the surface. As the load increased further, noticeable lateral displacement began to develop at the mid-span. When the load reached 1108 kN, the specimen attained its ultimate bearing capacity. Beyond this point, with continued loading, the displacement kept increasing while the load remained nearly constant, indicating that this specimen sustained a larger post-peak deformation than specimen C3-L2-C2, while the hybrid-wrapped specimen C3-L2-C2 showed the gentlest descending branch and the largest mid-span lateral displacement among the four specimens. The specimen eventually failed by instability.

3.2. Analysis of Test Results

3.2.1. Ultimate Bearing Capacity

The ultimate bearing capacity Nu and the corresponding mid-span lateral displacement um of the CFST intermediate-length columns with different CFRP wrapping patterns are presented in Figure 4. It can be seen from Figure 4 that CFRP confinement improves the ultimate bearing capacity of CFST columns, and the magnitude of enhancement varies with the wrapping configuration. Specifically, compared with specimen C1-L0-C0, the ultimate bearing capacity increased by 23% for C2-L4-C0, by 20.5% for C3-L2-C2, and by 8.4% for C4-L0-C4. Given that each configuration was represented by a single specimen, the exact magnitude of these differences warrants cautious interpretation, and the ranking should be regarded as indicative rather than statistically established. The ranking is nevertheless consistent with the mechanical roles of the two fibre orientations, which provides a physical basis for the observed order.
Figure 4. Ultimate bearing capacity of CFST column.
Based on the test results, the ultimate bearing capacity of specimens with longitudinal CFRP wrapping was significantly higher than that of specimens with hoop wrapping. Columns can be classified as short, intermediate, or slender depending on their slenderness ratio. Short columns generally fail by material crushing, which is essentially a strength-controlled failure. In contrast, the failure of intermediate-length columns is dominated by global instability. When the axial load reaches a critical value, the column loses its straight equilibrium configuration and undergoes lateral bending, i.e., buckling, which leads to a sudden loss of load-carrying capacity. During this process, the cross-section no longer sustains a uniform axial compressive stress; instead, bending-induced additional stresses are superimposed, resulting in increased compressive stress on one side and possible tensile stress on the opposite side. Therefore, the flexural stiffness largely governs the load-carrying capacity of intermediate-length columns.
The load–axial displacement curves of the CFST medium–long columns under different CFRP wrapping patterns are shown in Figure 5. The wrapping direction of CFRP sheets determines the distinctly different mechanical contributions they make to CFST columns. For circumferentially wrapped CFRP, the primary role is to provide hoop confinement. When the core concrete tends to expand laterally under axial compression owing to the Poisson effect, the outer steel tube first restrains this expansion, and the circumferentially wrapped CFRP further restricts the lateral deformation of the steel tube. According to the finite element results, the core concrete is placed in a strong triaxial compressive stress state, which enhances its compressive strength and ultimate compressive strain. This confinement effect, however, contributes only marginally to the overall flexural stiffness of the column, as indicated by the comparable lateral stiffness measured for C4-L0-C4 and C1-L0-C0 in Figure 6. From the mechanics of the composite section, flexural stiffness depends mainly on the elastic modulus of the material and the moment of inertia of the cross-section, and circumferential fibres hardly participate in axial load resistance. This interpretation is consistent with the small capacity gain measured for C4-L0-C4. Therefore, although the circumferentially wrapped specimens exhibit improved local strength and ductility, they cannot effectively resist buckling of intermediate-length columns, which explains the relatively modest increase in load-bearing capacity.
Figure 5. Load–axial displacement curves of specimens.
Figure 6. Load versus mid-span lateral displacement curves of specimens.
For CFST columns strengthened with longitudinally wrapped CFRP, the CFRP sheets directly participate in axial load resistance and bending resistance. The longitudinal CFRP works together with the inner concrete-filled steel tube as a composite load-bearing system, sharing the axial load and thereby increasing the effective compression area of the column. Meanwhile, because the CFRP is placed on the outermost surface of the column, it maximises the increase in the sectional moment of inertia. According to the Euler buckling formula, the critical buckling load is proportional to the flexural stiffness; hence, the column’s resistance to bending deformation is effectively improved, and the ultimate bearing capacity is raised. Furthermore, when buckling occurs, the longitudinal CFRP on the tension side, owing to its high tensile strength, can effectively restrain further bending deformation, thereby delaying or even preventing instability failure. This establishes a comprehensive protection mechanism that ranges from basic load capacity enhancement, through stiffness improvement, to deformation control.
In summary, circumferential wrapping mainly enhances the compressive strength and ductility of the core material and is effective against local buckling, but it cannot substantially improve the ultimate load-carrying capacity or buckling resistance of intermediate-length CFST columns. Longitudinal CFRP wrapping, on the other hand, directly increases both the axial and flexural stiffness of the column, thus effectively raising its ultimate capacity. Therefore, in the axial compression design of CFRP-confined CFST intermediate-length columns, the use of longitudinal wrapping or a hybrid scheme with predominantly longitudinal layers supplemented by circumferential ones leads to better axial compressive performance.

3.2.2. Load–Axial Displacement Curve

The load–axial displacement curves are presented in Figure 5. These curves capture the complete mechanical response of circular CFST intermediate columns under various CFRP wrapping patterns, covering the entire loading process from elastic deformation, through elastoplastic development, to eventual failure by instability.
The load–axial displacement curves of all specimens show three distinct stages: elastic, elastoplastic, and yielding.
(1)
Elastic stage: The load is linearly proportional to the axial displacement. During this stage, the steel tube and the core concrete deform compatibly, and the stress in the CFRP sheets remains relatively low. The stiffness of the member is provided by both the steel tube and the core concrete.
(2)
Elastoplastic stage: When the load increases to 60–70% of the ultimate capacity, the curve enters the elastoplastic stage, and the slope of the load–axial displacement curve begins to decrease gradually. At this point, the core concrete enters the plastic stage first, with micro-cracks developing internally and lateral expansion occurring. The steel tube begins to bear hoop tension, and the CFRP, depending on the wrapping direction, gradually starts to exert confinement or load-bearing effects, while the plastic deformation of the CFST column accumulates continuously.
(3)
Yielding stage: When the load reaches the peak point, the CFST column attains its ultimate bearing capacity. As the axial displacement further increases, the load-carrying capacity decreases continuously. The descending branch of the curve varies noticeably with the CFRP wrapping pattern, directly reflecting the improvement in ductility provided by different confinement schemes.
The load–axial displacement curves of CFST intermediate-length columns with different CFRP wrapping configurations are presented in Figure 5. After reaching its ultimate bearing capacity of 1022 kN, specimen C1-L0-C0 exhibited a rapid decrease in load, accompanied by only a limited increase in axial displacement. In the absence of CFRP confinement, the steel tube underwent local buckling and could not be effectively restrained, leading to rapid crushing of the core concrete.
The curve of specimen C2-L4-C0 exhibited the highest peak, with an ultimate bearing capacity of 1257 kN, indicating that longitudinal CFRP wrapping can effectively enhance the load-bearing capacity of CFST columns. After the peak load, the curve showed a sudden drop followed by a gradual decline; this sudden drop was attributed to cracking of the longitudinal CFRP.
The ultimate bearing capacity of specimen C3-L2-C2 was 1231 kN, slightly lower than that of C2-L4-C0. However, the descending branch of the curve was relatively gentle, indicating that the hybrid wrapping of longitudinal and circumferential CFRP layers produced a synergistic confinement effect: the longitudinal CFRP carried axial load and enhanced the compressive stiffness, while the circumferential CFRP restrained lateral expansion of the steel tube and core concrete and suppressed local buckling. The combined action of the two fibre orientations enabled the member to maintain a reasonable load-carrying capacity even after reaching the peak load, and the descending branch was gentler than those of the other specimens, with the mid-span lateral displacement developing more steadily.
The ultimate bearing capacity of specimen C4-L0-C4 was 1108 kN, which was lower than those of C2-L4-C0 and C3-L2-C2, while the descending branch of C4-L0-C4 was flatter. These observations indicate that although circumferential CFRP can enhance the compressive performance of the core concrete through hoop confinement, delay local buckling of the steel tube, and improve member ductility, its contribution to increasing the ultimate bearing capacity is limited.
In summary, the CFRP wrapping pattern exerts a significant modulating effect on the axial compressive behaviour of CFST intermediate columns: longitudinal CFRP wrapping mainly enhances the ultimate bearing capacity and overall compressive stiffness, and the hybrid longitudinal–circumferential wrapping improves both the ultimate bearing capacity and ductility, while circumferential wrapping alone offers only a relatively modest improvement in axial compressive performance. These comparisons are based on one specimen per configuration, and replicate tests would be required before the ranking can be treated as a statistically established trend.

3.2.3. Load–Mid-Span Lateral Displacement

The dominant failure mode of intermediate columns under axial compression is global instability. In this study, the instability initiation load is defined as the load at which the tangential stiffness of the load versus mid-span lateral displacement curve first drops below 10% of its initial value. This criterion is applied uniformly to all specimens. In this test, displacement transducers were installed at the quarter-height, mid-height, and three-quarter-height positions of the specimens, and the resulting load versus mid-span lateral displacement curves are presented in Figure 6.
During the initial loading stage, the specimens remained in the elastic range, with the axial load shared by the steel tube and the core concrete, and the members maintained an overall straight configuration. As the load further increased, the core concrete entered the elastoplastic stage and underwent lateral expansion, while the steel tube developed slight hoop deformation. At this point, the equilibrium state of the member began to deviate from the straight alignment, and the mid-span lateral displacement increased nonlinearly and rapidly with the increasing load, marking the onset of global instability. The plastic deformation of the member gradually transformed from axial compression to lateral bending. After the load reached the ultimate bearing capacity, the columns completely lost their stability capacity, with the load gradually decreasing while the mid-span lateral displacement continued to develop rapidly.
For specimen C1-L0-C0, the load at which instability initiated was approximately 60% of the ultimate bearing capacity (613 kN), making it the earliest among all specimens to begin losing stability. When the ultimate capacity (1022 kN) was reached, the corresponding mid-span lateral displacement was only 8.2 mm. Beyond this point, the load dropped rapidly, indicating a brittle instability behaviour.
When longitudinal CFRP wrapping was applied to the CFST columns, the instability initiation load increased to 72% of the ultimate bearing capacity (905 kN), representing the latest instability onset among all specimens. When the load reached the ultimate capacity (1257 kN), the corresponding mid-span lateral displacement was 14.5 mm, representing a 76.8% increase over that of C1-L0-C0. This indicates that longitudinal CFRP wrapping, by forming an integral load-bearing system with the concrete-filled steel tube, substantially enhances the flexural stiffness and overall lateral stiffness of the member, effectively delaying the onset of global instability and significantly improving the critical buckling load, axial ultimate capacity, and compressive stiffness of the CFST column. After the peak load, although a sudden drop in load occurred due to cracking of the longitudinal CFRP, the remaining CFRP and the steel tube were still able to jointly provide confinement to the member.
For the CFST columns strengthened with the hybrid longitudinal and circumferential CFRP wrapping, the instability initiation load was 69% of the ultimate bearing capacity (849 kN). When the load reached the ultimate capacity (1231 kN), the corresponding mid-span lateral displacement was 16.3 mm, which was the largest peak lateral displacement among all specimens. After the peak load, the load–lateral displacement curve exhibited the gentlest descending branch, and the accumulated lateral deformation during the failure stage was the largest. This is attributed to a synergistic confinement effect inferred from the finite element analysis: the longitudinal CFRP enhances the flexural stiffness of the member and delays the onset of instability, while the circumferential CFRP provides hoop confinement that restrains the lateral expansion of the steel tube and core concrete. The measured response alone does not isolate these two contributions, and the mechanism is therefore supported by the numerical results rather than by direct measurement. As a result, during the development of instability, the member not only exhibits improved resistance to instability but also shows better deformation performance after instability.
When circumferential CFRP wrapping was applied to the CFST columns, the instability initiation load was 65% of the ultimate bearing capacity (720 kN). When the load reached the ultimate capacity (1108 kN), the corresponding mid-span lateral displacement was 10.5 mm, representing a 28.1% increase over that of C1-L0-C0, but lower than those of C2-L4-C0 and C3-L2-C2. The overall trend of the load–mid-span lateral displacement curve was similar to that of C1-L0-C0, indicating that circumferential CFRP, through hoop confinement alone, enhances the compressive performance of the core concrete and delays local buckling of the steel tube, but contributes little to improving the overall flexural stiffness and lateral stiffness of the member. Therefore, circumferential CFRP wrapping provides only a modest improvement in the ultimate bearing capacity and buckling resistance of CFST columns.
In summary, the regulatory effect of CFRP wrapping patterns on the buckling resistance of CFST intermediate columns is closely aligned with the member’s loading characteristics and is also highly consistent with the observed trends in axial mechanical performance. Longitudinal wrapping, by enhancing the flexural stiffness of the member, effectively delays the onset of instability and raises the critical buckling load, and thus serves as the primary approach for improving both the buckling resistance and the axial ultimate capacity of intermediate-length columns. The hybrid longitudinal–circumferential wrapping, building upon the longitudinal CFRP, incorporates hoop confinement from the circumferential layers to optimise the post-instability deformation behaviour, resulting in the best overall performance in terms of both axial ductility and lateral buckling resistance. In contrast, circumferential wrapping alone can only marginally improve the instability characteristics and axial ductility of the member, and cannot fundamentally enhance its overall buckling resistance or axial ultimate capacity.

3.2.4. Load–Strain Curve

During the tests, no debonding was observed at the interface between the CFRP and the steel tube, indicating good composite action. The locations of strain gauges attached on the CFST columns are shown in Figure 2.
The load–longitudinal strain curves of the CFST intermediate-length columns at mid-height are shown in Figure 7. Before the load reached 60% of the ultimate capacity, the member was under axial compression, with no significant tensile stress on the tension side and relatively small strains. When the load increased to 60–70% of the peak load, the lateral deformation at mid-span grew, and the tension side experienced combined tension and bending, causing the tensile strain to rise rapidly and nonlinearly. After the load dropped, the lateral bending at mid-span intensified, and the tension side became the dominant tensile region, where the tensile strain increased sharply and exceeded the compressive strain by a large margin. The tensile strain of C1-L0-C0 increased at the fastest rate. For C2-L4-C0, the rate of increase was lower, which is consistent with the longitudinal CFRP sharing part of the tensile stress. C3-L2-C2 showed a more gradual development of tensile strain, consistent with the combined action of the hybrid wrapping. C4-L0-C4 only slightly alleviated the sharp increase in tensile strain. These interpretations are based on the measured surface strains, which reflect the behaviour of the outermost layer and not the stress state within the core concrete.
Figure 7. Load–longitudinal strain curves at mid span.

4. Finite Element Analysis

4.1. Material Constitutive Model

The concrete constitutive model follows the plastic damage model for confined concrete proposed by Han Linhai [40], which accounts for the dual confinement from the steel tube and CFRP. This model is capable of accurately capturing the enhancement in compressive strength and the improvement in ductility of the core concrete under triaxial compression. The key parameters of the model were assigned as follows: dilation angle ψ = 30°, eccentricity ef = 0.1, ratio of biaxial to uniaxial compressive strength fb0/fc0 = 1.162, ratio of the second stress invariant on the tensile meridian to that on the compressive meridian K = 2/3, and viscosity parameter VP = 0.0001.
The constitutive model proposed by Tao [41] for steel tubes was adopted to characterise the mechanical response of ordinary carbon steel under loading. This model accurately reproduces the full-range behaviour of carbon steel from elasticity, yielding, and strain hardening to ultimate failure, matching the actual stress–strain characteristics of Q235 steel under axial compression. The stress–strain relationship consists of four stages, elastic, yielding, strain hardening, and ultimate failure, and is expressed as follows:
σ = E s ε ( ε ≤ ε y ) f y ( ε y < ε ≤ ε u ) f y + K p ( ε − ε u ) ( ε u < ε ≤ ε cu ) 0 ( ε > ε cu )
where Es is the elastic modulus of steel, taken as 200 GPa from the material property tests; fy is the yield strength of steel, taken as 290 MPa; εy is the yield strain of steel, εy = fy/Es; εu is the strain at the onset of strain hardening, taken as 0.01; Kp is the strain-hardening modulus of steel, taken as 2 GPa; εcu is the ultimate strain of steel, taken as 0.2; σ is the steel stress; and ε is the steel strain. The Poisson’s ratio of steel is taken as 0.3, based on the material property tests.
The CFRP sheets were treated as an orthotropic elastic–brittle composite material with distinct directional dependence: high tensile strength was exhibited only along the fibre direction, while the tensile strength perpendicular to the fibre direction was negligible. Once the ultimate tensile stress was reached, brittle fracture occurred and the load-carrying capacity was lost. The Hashin damage criterion was adopted to simulate the initiation, progression, and failure of damage in the CFRP sheets. This criterion comprehensively accounts for four damage modes—fibre tension, fibre compression, matrix tension, and matrix compression—and characterises the degree of damage through progressive degradation of material stiffness [42], which aligns well with the actual damage evolution of CFRP sheets under axial compression. The longitudinal tensile strength of 4200 MPa and elastic modulus of 240 GPa were determined from the coupon tests reported in Table 4. The Hashin criterion was adopted to capture fibre tension, fibre compression, matrix tension, and matrix compression, with stiffness degradation characterizing the damage progression. This criterion has been extensively employed for CFRP-strengthened CFST members. The longitudinal tensile strength of 4200 MPa governs the CFRP fracture at mid-span observed in specimen C2-L4-C0, while the remaining strength values follow the manufacturer’s data for the UT70-30 sheet. The fracture energies were taken as 60 kJ/m2 for fibre tension and 1 kJ/m2 for matrix tension, and a viscosity coefficient of 1 × 10−5 was applied to all four damage modes to stabilise the implicit solution [43]. The complete parameter set is listed in Table 6.
Table 6. Mechanical and Hashin damage parameters of CFRP composite plies.

4.2. Finite Element Modelling

The core concrete was modelled using 8-node reduced-integration solid elements (C3D8R) [44]. The Q235 steel tube, being a thin-walled hollow member with wall thickness much smaller than the radial and axial dimensions, represents a typical shell structure and was modelled using 4-node reduced-integration shell elements (S4R). The CFRP sheets, as orthotropic composite materials with high tensile strength only along the fibre direction, were also modelled using 4-node reduced-integration shell elements (S4R). The end steel platens and knife-edge hinges, which served as load-transfer and boundary-condition components, were modelled using C3D8R elements and were defined as rigid bodies. A mesh-sensitivity study was performed on the unstrengthened specimen C1-L0-C0 to determine these sizes. The mesh size for the concrete and steel tube was varied among 15 mm, 20 mm, 25 mm, and 30 mm, while the CFRP mesh size was fixed at 15 mm. The corresponding ultimate capacities were 1043 kN, 1035 kN, 1031 kN, and 1021 kN, giving deviations of +0.8%, 0%, −0.4%, and −1.4% relative to the 20 mm mesh. Refining the mesh below 20 mm changed the capacity by less than 1% while substantially increasing the computational cost. The 20 mm mesh was therefore adopted, and the same mesh density was retained for all specimens. The mesh discretization of the individual components of the specimen column is shown in Figure 8.
Figure 8. Mesh generation.
The mesh size was set to 20 mm for the core concrete and the steel tube, 15 mm for the CFRP sheets, and 30 mm for the end steel platens and knife-edge hinges. As the CFRP-confined CFST intermediate column is a composite member, the interface between the steel tube and the core concrete was simulated using surface-to-surface contact, with the inner surface of the steel tube defined as the master surface and the outer surface of the concrete as the slave surface. The normal behaviour was defined as hard contact, ensuring that no separation occurs at the interface during compression and that normal pressure is effectively transferred. The tangential behaviour was modelled using the Coulomb friction model to represent the bond–slip effect between the steel tube and the concrete, with a friction coefficient of 0.25. This value lies within the range of 0.2–0.6 commonly reported for the steel–concrete interface in CFST members. In the tests, the CFRP sheets were bonded to the steel tube using epoxy resin adhesive, with full deformation compatibility and no relative slip or debonding throughout the loading process. Therefore, a tie constraint was used between the CFRP sheets and the steel tube. Tie constraints were also applied between the ends of the steel tube and concrete and the end steel platens. The contact between the steel platens and the knife-edge hinges was defined as surface-to-surface, with hard contact in the normal direction to ensure effective transfer of normal pressure, and the Coulomb friction model in the tangential direction with a friction coefficient of 0.3. The adhesive layer was not explicitly modelled; instead, a tie constraint was employed between the CFRP and the steel tube. This simplification is justified by the experimental observation that no debonding occurred at the CFRP–steel interface in any specimen, including in the vicinity of the CFRP fracture zone. The measured shear and tensile strengths of the E2500S adhesive were 24 MPa and 42 MPa, respectively (Table 5). It is worth noting, however, that the interface stresses were not extracted from the model; consequently, the interface stress demand relative to the adhesive strength was not quantified. Although the tie constraint may slightly overestimate the local interface stiffness, this effect is considered negligible for the global capacity prediction [43].
In practical engineering, members inevitably possess initial geometric imperfections due to fabrication, installation, transportation, and other factors. Such imperfections significantly affect the overall stability of intermediate-length columns and reduce their ultimate axial capacity.
The imperfection shape was taken as the first buckling mode obtained from a linear eigenvalue analysis, with the amplitude set to L/1000 (1.5 mm), consistent with both the measured out-of-straightness of less than L/1500 and GB/T 50152-2012. The nonlinear analysis was performed in ABAQUS using the modified Riks method. The initial increment was 0.001 of the total displacement, the maximum increment was 0.01, and the minimum increment was 1 × 10−6. The convergence tolerances were 0.5% for the residual force and 1% for the displacement. To reproduce the pinned-end conditions of the test, the boundary conditions were applied to the knife-edge hinge reference points. The bottom hinge was pinned, with all translational degrees of freedom restrained (U1 = U2 = U3 = 0) and rotation about the horizontal axis free; this provided a fixed support and eliminated the end moment. At the top hinge, the horizontal translations were restrained (U1 = U2 = 0), the rotations were free (UR1, UR2, UR3), and the axial degree of freedom U3 was retained for loading. The member therefore deformed only along its axis, with both ends free to rotate. Displacement-controlled loading was applied at the top hinge reference point in the U3 direction, with a total downward displacement of 20 mm and a linear ramp amplitude. Axial load, axial displacement, mid-span lateral displacement, and stresses and strains in each component were recorded during loading. The analysis was terminated when the member failed by global instability and the load dropped below 85% of the ultimate capacity, reproducing the full response from elastic deformation through elastoplastic development to instability failure.

4.3. Finite Element Model Validation

The failure modes obtained from the numerical simulation are shown in Figure 9. The unstrengthened specimen C1-L0-C0 failed by global flexural buckling, with local bulging observed at the mid-height of the steel tube. Longitudinal CFRP wrapping enhanced the flexural stiffness of specimen C2-L4-C0, resulting in a reduced degree of instability, and failure was characterised by fracture of the CFRP and slight buckling of the steel tube. Specimen C3-L2-C2, with hybrid longitudinal and circumferential wrapping, exhibited a uniform bending pattern without local bulging, and the CFRP and steel tube deformed compatibly, consistent with its optimal ductility. Specimen C4-L0-C4, with circumferential wrapping alone, failed predominantly by global flexural buckling with pronounced lateral displacement. The simulated failure modes of all specimens were in good agreement with the experimental observations.
Figure 9. Comparison of load–displacement curves.
The load–displacement curves obtained from the finite element simulations and the experimental curves show good agreement across the four stages—elastic ascending, elastoplastic transition, peak, and descending. In the initial stage, the simulated and experimental curves follow the same ascending trend, which supports the reasonableness of the constitutive models, contact definitions, and boundary conditions. In the elastoplastic stage, the simulated curves reproduce the general transition observed in the tests. After the peak, the gentleness of the descending branch in the simulations is close to that observed in the tests, with specimen C3-L2-C2 showing the mildest decline, followed by C2-L4-C0, while C4-L0-C4 and C1-L0-C0 descend more rapidly; this trend is consistent with the experimental results. The model is able to effectively reproduce the full-range axial compressive response of members with different CFRP wrapping patterns.
The ultimate bearing capacities obtained from the finite element simulations were compared with the experimental values, and the results are presented in Table 7. The ratios of simulated to experimental values for all specimens range from 1.018 to 1.054, with deviations all within 5.5%, indicating good overall agreement. This confirms that the finite element model established in this study can accurately predict the axial compressive ultimate capacity of CFRP-confined CFST intermediate columns, and the model accuracy meets the requirements for analysis. Validation in this study is confined to the failure modes, the ultimate capacities listed in Table 7, and the overall shape of the load–displacement curves in Figure 9. For specimen C2-L4-C0, the predicted CFRP fracture location is at mid-span, which agrees with the test observation.
Table 7. Comparison of test and finite element results.
From the perspective of the capacity enhancement pattern, the finite element results also exhibit the same trend in ultimate bearing capacity, with the longitudinal CFRP wrapping producing the largest increase, followed by the hybrid wrapping, and the circumferential wrapping giving the smallest gain. The model can effectively capture the influence of CFRP wrapping patterns on the axial compressive capacity of the members, and can accurately distinguish the differences in confinement efficiency among the various wrapping configurations. The model was validated only against the four specimens tested in this study. Independent experimental data from the literature were not used. The perfect-bond assumption at the CFRP–steel interface means that the model does not capture debonding, and the interface stresses were not extracted for comparison with the measured adhesive strengths. The validation therefore supports the global capacity prediction for the present specimens, in which no debonding was observed, rather than the general case where interfacial failure may govern.

4.4. Parametric Study

Given the limited number of specimens in this test programme, which resulted in a relatively narrow range of variables, a parametric study was carried out based on the finite element model to investigate the effects of slenderness ratio (41.1, 54.8, 68.5, and 80), concrete strength grade (C30, C40, and C50), and steel strength (Q235, Q355, and Q460) on the ultimate bearing capacity of CFST columns.

4.4.1. Effect of Slenderness Ratio

To clarify the influence of slenderness ratio on the axial compressive capacity of CFRP-confined CFST intermediate columns, a parametric analysis was carried out using the validated finite element model, with four slenderness ratios of 41.1, 54.8, 68.5, and 80 selected. The steel strength was Q235, the concrete strength grade was C40, and the remaining parameters were kept consistent with those of the test specimens. The effect of slenderness ratio on the bearing capacity of CFST columns is shown in Figure 10.
Figure 10. Effect of slenderness ratio on ultimate bearing capacity.
For all specimens, the ultimate axial compressive capacity decreased as the slenderness ratio increased. When the slenderness ratio increased from 41.1 to 80, the capacity reduction for the unstrengthened specimen C1-L0-C0 was about 15.6%, while for the CFRP-strengthened specimens the reduction ranged from 17.0% to 19.1%. This indicates that the slenderness ratio has a significant controlling effect on the stability capacity of intermediate-length columns.
For a given slenderness ratio, the order of capacity enhancement remains unchanged: longitudinal wrapping gives the largest increase, followed by hybrid wrapping, and circumferential wrapping the smallest. This indicates that the strengthening effect of longitudinal CFRP on flexural stiffness and stability capacity is independent of the slenderness ratio, and thus it remains the optimal strengthening method for columns with large slenderness ratios.
As the slenderness ratio increases, the member becomes more prone to global flexural buckling, and the resulting reduction in load-bearing capacity is greater than the enhancement provided by CFRP confinement. Therefore, in engineering practice, priority should be given to controlling the slenderness ratio of the member, followed by the application of CFRP wrapping to achieve further performance optimisation.

4.4.2. Effect of Concrete Strength

To clarify the influence of concrete strength on the axial compressive capacity of CFRP-confined CFST intermediate columns, a parametric analysis was carried out using the validated finite element model. Three commonly used concrete strength grades, C30, C40, and C50, were selected for the analysis, with the steel strength taken as Q235 and the slenderness ratio as 41.1, while the remaining parameters were kept consistent with those of the test specimens. The influence of concrete strength grade on the bearing capacity of CFST columns is presented in Figure 11.
Figure 11. Effect of concrete strength on ultimate bearing capacity.
Increasing the concrete strength from C30 to C50 resulted in a noticeable improvement in the load-bearing capacity of all specimens. For the unstrengthened specimen C1-L0-C0, the increase was about 20.7%, while for the CFRP-strengthened specimens the increase ranged from 14.0% to 15.5%. This indicates that raising the concrete strength directly enhances the core compression capacity of the member, and is therefore an effective means of improving the load-bearing performance.
CFRP works well with high-strength concrete; the CFRP confinement effectively restrains the lateral expansion and brittle failure of the concrete, and the three components exhibit excellent cooperative performance, ensuring a stable increase in the load-bearing capacity.

4.4.3. Effect of Steel Strength

To investigate the influence of steel tube strength on the axial compressive capacity of CFRP-confined CFST intermediate columns, a parametric analysis was carried out using the validated finite element model. Three commonly used steel grades in engineering practice, Q235, Q355, and Q460, were selected for the analysis, with the concrete strength grade fixed at C40 and the slenderness ratio at 41.1, while the remaining parameters were kept consistent with those of the test specimens. The influence of steel tube strength grade on the bearing capacity of CFST columns is illustrated in Figure 12.
Figure 12. Effect of steel strength on ultimate bearing capacity.
When the yield strength of the steel tube was increased from Q235 to Q460, the bearing capacity of the unconfined specimen C1-L0-C0 rose from 1035 kN to 1239 kN, representing an increase of approximately 19.7%. For the CFRP-strengthened specimens, the capacity improvement ranged from 14.0% to 27.2%. This indicates that steel strength is a key factor in enhancing the axial compressive capacity of the members.
Longitudinal CFRP can share the axial load with the high-strength steel tube, and the two components work together effectively. Among all strengthened specimens, the longitudinally wrapped one (C2-L4-C0) exhibited the largest increase in capacity, which further confirms the contribution of longitudinal CFRP to axial load resistance. In contrast, the circumferentially wrapped specimen (C4-L0-C4) showed a smaller increase compared with the other strengthened groups, because the circumferential CFRP provides only hoop confinement and does not participate in resisting axial compression, thus contributing little to the enhancement associated with higher steel strength.

5. Formula for Axial Compressive Capacity

5.1. Fardis and Khalili Model

This formula [45] is based on the hoop confinement effect of FRP on concrete, and establishes a calculation model by introducing the ratio of the lateral confining stress to the axial compressive strength of concrete. The expression is as follows:
f cc ′ = f c ′ 1 + 4.1 f 1 / 2 f c ′
ε cc ′ = 0.002 + 0.001 E f t / D f c ′
where f cc ′ is the compressive strength of confined concrete; f c ′ is the compressive strength of unconfined concrete; f l = 2 t f f / D is the lateral confining stress provided by FRP; ε cc ′ is the axial strain corresponding to the compressive strength of confined concrete; E f is the elastic modulus of the FRP composite; f f is the tensile strength of the FRP composite; D is the diameter of the column cross-section; and t f is the thickness of the FRP composite.
This formula is concise in form and physically clear, but it does not take into account the confining contribution of the steel tube to the concrete. Therefore, it is only applicable to plain FRP-confined concrete columns and cannot be directly applied to CFRP–steel–concrete composite members.

5.2. Mander Model

The model proposed by Mander et al. [46] takes into account the actual stress state of the confining material, refines the calculation of the lateral confining stress, and is applicable to concrete columns with various confinement configurations. The expression is as follows:
f cc ′ = f c ′ − 1.254 + 2.2541 + 7.94 f 1 ′ / f c ′ − 2 f 1 ′ / f c ′
ε cc ′ = ε c ′ 1 + 5 f cc ′ / f c ′ − 1
where f l ′ = 2 f f t / ( D − 2 t ) and ε c ′ are the strains corresponding to the ultimate strength of unconfined concrete.
This formula accounts for the effect of FRP thickness on the effective diameter of the section, but it does not take into account the confining contribution of the steel tube. For CFRP-confined CFST members, the confinement effect of the steel tube should be incorporated in the modification.

5.3. Simplified Formula of Yu Qing

Based on a summary of existing studies, Yu Qing [47] introduced the confinement effect coefficient ξ = 2 f f t f / ( D c f c ′ ) and derived a simplified calculation model through fitting experimental data as follows:
f cc ′ = φ f c ′ 1 + 2.3 ξ
ε cc ′ = ε c ′ + 0.01 f 1 / f c ′
where φ is the stability coefficient and Dc is the diameter of the cross-section of the core concrete.
The formula is clear and straightforward in concept, and the calculated results show good agreement with the experimental data. However, it does not explicitly consider the influence of CFRP wrapping patterns, and the values of the stability coefficient φ have not been specifically calibrated for the slenderness ratio range of intermediate-length columns.

5.4. ACI 440 Recommended Formula

The ACI 440R-07 guideline [48] adopts the model proposed by Mander (1998), which accounts for the combined confining action of the steel tube and FRP, with the lateral confining stress taken as the sum of the contributions from both. The expression is as follows:
f cc ′ = f co ′ 2.25 1 + 7.9 f l f co ′ − 2 f l f co ′ − 1.25
f l = 2 f s t s d + 2 f FRP t FRP d
where f cc ′ is the compressive strength of the unconfined concrete; f l is the total lateral confining stress; f s and t s are the yield strength and wall thickness of the steel tube, respectively; f FRP and t FRP are the tensile strength and thickness of the FRP, respectively; and d is the diameter of the core concrete.
This formula is applicable to circular-section members with combined confinement from FRP and steel tube, but it does not account for the influence of CFRP wrapping pattern on confinement efficiency, nor does it provide a clear method for calculating the stability coefficient for intermediate-length columns.

5.5. Leng Yun Formula for Intermediate Columns

For CFRP-strengthened CFST intermediate columns with slenderness ratios of 5.7 ≤ L/D ≤ 8, Leng Yun [49] proposed a bearing capacity formula based on the limit equilibrium method, which incorporates the stability coefficient:
N u , cf = φ ( A f c A c + B f sy A s + C f cf A cf )
φ = 1 − 0.1337 L / D − 5.7
where φ is the stability coefficient; A, B, and C are regression coefficients; fc is the axial compressive strength of concrete; Ac, As, and Acf are the cross-sectional areas of concrete, steel tube, and CFRP, respectively; fsy is the yield strength of the steel tube; fcf is the effective tensile strength of CFRP; L is the length of the member; and D is the outer diameter of the steel tube.
The formula accounts for the stability effect of intermediate columns, but it does not distinguish the influence of different CFRP wrapping configurations on the effective tensile strength, making it difficult to accurately reflect the differences in confinement provided by longitudinal, circumferential, and hybrid wrapping.

5.6. Bearing Capacity Model Considering CFRP Wrapping Patterns

5.6.1. Basic Assumptions

To simplify the calculation and theoretical analysis, the following basic assumptions are proposed based on the experimental observations and mechanical characteristics.
(1)
The plane section assumption is adopted, meaning that the cross-section of the member remains plane and perpendicular to the longitudinal axis during axial compression.
(2)
Perfect bonding is assumed between the steel tube, concrete, and CFRP up to the ultimate limit state, with no relative slip and full deformation compatibility. This assumption pertains solely to interfacial slip and does not imply that the CFRP attains its full tensile strength over the entire wrapped area.
(3)
The effects of concrete shrinkage, creep, and temperature are neglected.
(4)
Longitudinally wrapped CFRP contributes to both axial load resistance and partial lateral confinement; circumferentially wrapped CFRP provides only hoop confinement; hybrid wrapping exhibits both functions.
(5)
The radial stresses in the steel tube and CFRP are ignored, and the hoop stress is assumed to be uniformly distributed.

5.6.2. Definition and Calculation of Key Parameters

(1)
Calculation of lateral confining stress
The total lateral confining stress fl consists of the confining stress provided by the steel tube fls and that provided by the CFRP flcf, as follows:
f l = f ls + f lcf
The confining stress provided by the steel tube, fls, is calculated based on the yield strength and geometric parameters of the steel tube, and is expressed as follows:
f ls = 2 f sy t s D c
where Dc is the diameter of the core concrete, taken as the inner diameter of the steel tube.
The CFRP confining stress flcf is determined by incorporating the confinement efficiency coefficient η to account for the influence of the wrapping pattern, and is expressed as follows:
f lcf = η 2 f cf t cf D c
where tcf = ntcf,l, with n being the number of CFRP layers and tcf,l the thickness of a single CFRP layer; η is a weighting factor that converts the CFRP tensile capacity into an equivalent lateral confining stress within the capacity model. It reflects the combined contribution of each wrapping pattern to the axial capacity, rather than the hoop confinement alone. Longitudinal CFRP contributes both axial resistance and flexural stiffness, and its contribution is captured jointly by η and the axial term in Equation (18); hoop CFRP, by contrast, provides lateral confinement only. The values η = 0.9 for longitudinal wrapping, 0.6 for circumferential wrapping, and 0.8 for hybrid wrapping were assigned according to the relative contribution of each wrapping pattern to the axial capacity and subsequently checked against the test results in Table 8; fcf is the effective tensile strength of CFRP, taken as 0.7 times its ultimate tensile strength. This factor reflects the non-uniform distribution of hoop strain in the CFRP at the ultimate limit state, where the peak strain is localised near the mid-height of the column and the CFRP does not attain its full tensile strength over the entire wrapped area. The value of 0.7 was determined by calibrating the calculated capacities against the four test results and the finite element results in Table 7, which yielded deviations within ±5%. This value is consistent with the effective-strain factors of 0.6–0.8 commonly adopted for FRP-confined columns in the literature. All empirical coefficients in the proposed formula were calibrated using the present test and finite element data. Independent validation is warranted before they are applied outside the parameter range studied.
Table 8. Comparison of Calculated and Experimental Load-Carrying Capacities.
(2)
Compressive strength of confined concrete
Adopting the modified Mander formula, which accounts for the effect of CFRP wrapping patterns on confinement efficiency, the expression is as follows:
f cc ′ = f c 2.254 1 + 7.94 f l f c − 2 f l f c − 1.254
(3)
Stability coefficient calculation
Based on the slenderness ratio range of the specimens from the present tests and finite element simulations, and in combination with existing research results, the calculation formula for the stability coefficient φ is derived by fitting the experimental data as follows:
φ = 1.0 λ ≤ 30 1.022 − 0.00073 λ 30 < λ ≤ 50 1.105 − 0.00237 λ 50 < λ ≤ 80
(4)
Concrete strength modification factor
Based on the parametric analysis of C30, C40, and C50, the fitting expression is obtained as follows. This coefficient is empirical and remains valid only within the parameter range examined in this study:
α c = 0.82 + 0.0027 f c

5.6.3. Final Formula for Bearing Capacity

The ultimate axial compressive capacity of CFRP-confined circular concrete-filled steel tubular (CFST) intermediate columns is provided jointly by the confined concrete, the steel tube, and the longitudinal CFRP, and is expressed as follows:
N u = φ ( α c f cc ′ A c + f y A s + f cf , ax A cf , ax )
where φ is the stability coefficient; α c is the concrete strength modification factor; f cc ′ is the compressive strength of the confined concrete; Ac is the cross-sectional area of the core concrete; fy is the yield strength of the steel tube; As is the cross-sectional area of the steel tube; fcf,ax is the axial compressive strength of the CFRP, taken as 0.4 times its tensile strength; and Acf,ax is the area of CFRP participating in axial load resistance. For longitudinal wrapping, Acf,ax = Acf, where Acf is the total cross-sectional area of the CFRP sheets; for circumferential wrapping, Acf,ax = 0; and for hybrid wrapping, Acf,ax = 0.5 Acf.

5.7. Formula Verification and Error Analysis

The ultimate bearing capacities of the four specimens from the present tests were calculated using the formula proposed in this paper, and the calculated values were compared with the experimental results. The comparison is presented in Figure 13.
Figure 13. Comparison of Nu between the simulated and calculated results.
As shown in Table 8, the ratios of the calculated values from the proposed formula to the experimental values range from 0.993 to 1.003, and those to the finite element values range from 1.006 to 1.046. The overall deviations are all within ±5%, indicating that the accuracy of the proposed formula is significantly better than that of the simple superposition formula without considering confinement efficiency. The proposed formula can accurately predict the axial compressive stability capacity of members with different CFRP wrapping patterns. The formula was calibrated using the present test and finite element data. Its applicability to other slenderness ratios, material grades, and CFRP layouts requires validation against independent experimental data. The deviations within ±5% therefore indicate the accuracy of the formula within the present dataset rather than its general validity. The formula is applicable to circular CFST intermediate-length columns with 40 ≤ λ ≤ 80, concrete grades of C30-C50, steel grades of Q235-Q460, and the three wrapping configurations examined in this study. Verification for 20 < λ < 40 remains to be carried out. The formula was calibrated and validated using the four tests and the finite element results derived from the same specimens. The deviations within ±5% therefore reflect the accuracy within the present dataset rather than an independent validation.

6. Conclusions

The present study addresses CFRP-confined CFST intermediate columns, with particular emphasis on the CFRP wrapping pattern as the key influencing factor. A combined methodology of experimental testing, ABAQUS finite element simulation, and theoretical analysis was adopted to systematically clarify the effects of longitudinal, circumferential, and hybrid wrapping on the axial compressive behaviour, failure mechanisms, and stability capacity of the columns. A simplified calculation model for the axial compressive capacity is proposed, which explicitly incorporates the influence of CFRP wrapping patterns. The findings are of practical engineering significance.
(1)
The results show that external CFRP confinement can significantly improve the axial compressive performance of CFST intermediate columns, and the wrapping pattern is a key factor governing the confinement efficiency and the degree of capacity enhancement. Longitudinal CFRP, by directly participating in axial load resistance and substantially increasing the flexural stiffness of the member, effectively suppresses global instability from the outset and provides the greatest improvement in ultimate bearing capacity, with an increase of 23% over the unstrengthened specimen. Hybrid longitudinal–circumferential wrapping combines axial strengthening with hoop confinement, giving a capacity increase of 20.5% and showing a relatively gentle post-peak response with favourable deformation performance. Circumferential CFRP alone offers only hoop confinement and contributes little to overall stability, resulting in a modest capacity gain of 8.4%. The three wrapping patterns rank as follows in terms of performance: longitudinal wrapping > hybrid wrapping > circumferential wrapping. This ranking is based on a single specimen per configuration, and repeated tests would be needed to quantify the associated scatter. Accordingly, the ranking is presented as an indication of the relative effectiveness of the three wrapping schemes under the present test conditions, rather than as a statistically established result.
(2)
Both experimental and numerical results confirm that the unstrengthened specimens are characterised by brittle instability involving local buckling of the steel tube and crushing of the core concrete. The failure of longitudinally wrapped specimens is governed by CFRP fracture, accompanied by substantially reduced flexural deformation. Hybrid-wrapped specimens exhibit a uniform flexural buckling mode with no obvious local bulging, and their post-peak deformation develops more steadily than that of the other strengthened specimens, while circumferentially wrapped specimens still fail predominantly by global flexural buckling, with only marginal mitigation of local buckling. The finite element model, validated against the test data, gives ultimate capacity deviations of less than 5.5%, and is capable of accurately reproducing the full-range mechanical response and failure modes. Parametric analysis further reveals that the axial compressive capacity decreases notably with increasing slenderness ratio, while it rises steadily with higher concrete strength and steel tube strength. Among all combinations, longitudinal CFRP works most effectively with high-strength steel and high-strength concrete.
(3)
Based on the experimental and numerical results, this paper introduces a simplified calculation formula for the axial compressive capacity that incorporates the CFRP confinement efficiency coefficient, the wrapping-pattern modification factor, and the stability coefficient for intermediate columns, enabling differentiation among various wrapping configurations. For the present dataset, the deviations between the calculated values and the experimental results remain within ±5%. The formula is applicable to circular CFST intermediate-length columns with 40 ≤ λ ≤ 80, concrete grades of C30-C50, steel grades of Q235-Q460, and the three wrapping configurations examined in this study. The lower bound of 40 reflects the range of slenderness ratios covered by the present tests and parametric study; the formula has not been verified for 20 < λ < 40. Independent validation against experimental data from other laboratories is warranted before the formula can be recommended for general design use. Within the parameter range examined, the formula addresses the limitations of existing formulas that do not account for the CFRP wrapping pattern and do not address the stability behaviour of intermediate columns, thereby offering a basis for further theoretical refinement and engineering application of such composite members.
The experimental programme comprises only four specimens—one per wrapping configuration—and is confined to a single slenderness ratio (λ = 41.1), concrete grade (C40), steel grade (Q235), and CFRP layer number (four layers). The proposed capacity model was validated solely against the authors’ own tests and finite element results, without independent validation from other laboratories. The study addresses only monotonic axial compression under pinned-end conditions, with the CFRP–steel tube interface modelled as perfectly bonded; debonding is therefore not captured. Although this assumption is supported by the absence of visible debonding in the tests, the interface stresses were not extracted, and the assumption may overestimate the capacity of members with thin adhesive layers, large hoop strains, or long-term environmental exposure, for which a cohesive zone formulation should be employed. Consequently, the finite element model and the proposed capacity formula should be regarded as valid for the global response of the present specimens and parameter range, and not as a general tool for cases in which interfacial debonding controls the behaviour. A sensitivity study on the interfacial friction coefficient was not performed, and the mesh and contact parameters calibrated for the test specimens were retained throughout the parametric study, which may affect the accuracy of the parametric results. Future work should therefore encompass repeated specimens to quantify the scatter of the capacity enhancement; a wider range of slenderness ratios, concrete and steel grades, and CFRP layouts; independent experimental datasets for validating the proposed formula; explicit modelling of interface debonding; and further investigation of eccentric loading, end restraint conditions, and long-term environmental exposure.

Author Contributions

Z.W.: Writing—original draft, Validation. Q.L.: Writing—review & editing, Formal analysis. C.L.: Resources, Methodology. B.W.: Investigation, Data curation. J.H.: Supervision, Funding acquisition. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by the Natural Science Foundation of Qing Hai Province [Grant No. 2026-QY-206].

Data Availability Statement

Data will be made available on request.

Acknowledgments

The authors gratefully acknowledge funding from the Natural Science Foundation of Qing Hai Province (Grant No. 2026-QY-206).

Conflicts of Interest

The authors declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this paper.

References

  1. Evirgen, B.; Tuncan, A.; Taskin, K. Structural behavior of concrete filled steel tubular sections (CFT/CFSt) under axial compression. Thin-Walled Struct. 2014, 80, 46–56. [Google Scholar] [CrossRef] [Scilit]
  2. Ibañez, C.; Hernández-Figueirido, D.; Piquer, A. Shape effect on axially loaded high strength CFST stub columns. J. Constr. Steel Res. 2018, 147, 247–256. [Google Scholar] [CrossRef] [Scilit]
  3. Chen, C.C.; Ko, J.W.; Huang, G.L.; Chang, Y.M. Local buckling and concrete confinement of concrete-filled box columns under axial load. J. Constr. Steel Res. 2012, 78, 8–21. [Google Scholar] [CrossRef] [Scilit]
  4. Wang, Z.B.; Tao, Z.; Han, L.H.; Uy, B.; Lam, D.; Kang, W.H. Strength, stiffness and ductility of concrete-filled steel columns under axial compression. Eng. Struct. 2017, 135, 209–221. [Google Scholar] [CrossRef] [Scilit]
  5. Han, L.H.; Hou, C.; Hua, Y.X. Concrete-filled steel tubes subjected to axial compression: Life-cycle based performance. J. Constr. Steel Res. 2020, 170, 106063. [Google Scholar] [CrossRef] [Scilit]
  6. Lai, M.H.; Song, W.; Ou, X.L.; Chen, M.T.; Wang, Q.; Ho, J.C.M. A path dependent stress-strain model for concrete-filled-steel-tube column. Eng. Struct. 2020, 211, 110312. [Google Scholar] [CrossRef] [Scilit]
  7. Linhai, H.; Youfu, Y. Study on behavior of concrete filled square steel tubes under axial load. China Civ. Eng. J. 2001, 34, 17–25. [Google Scholar]
  8. Linhai, H.; Youfu, Y. Study on axial bearing capacity of concrete-filled steel tube columns with rectangular section. China Civ. Eng. J. 2001, 34, 22–31. [Google Scholar]
  9. Tan, Q.H.; Gardner, L.; Han, L.H.; Song, T.Y. Performance of concrete-filled stainless steel tubular (CFSST) columns after exposure to fire. Thin-Walled Struct. 2020, 149, 106629. [Google Scholar] [CrossRef] [Scilit]
  10. Xu, J.; Wang, Y.; Ren, R.; Wu, Z.; Ozbakkaloglu, T. Performance evaluation of recycled aggregate concrete-filled steel tubes under different loading conditions: Database analysis and modelling. J. Build. Eng. 2020, 30, 101308. [Google Scholar] [CrossRef] [Scilit]
  11. Romero, M.L.; Moliner, V.; Espinos, A.; Ibañez, C.; Hospitaler, A. Fire behavior of axially loaded slender high strength concrete-filled tubular columns. J. Constr. Steel Res. 2011, 67, 1953–1965. [Google Scholar] [CrossRef] [Scilit]
  12. Liu, Z.; Liu, H.; Chen, Z.; Zhang, G. Structural behavior of cold-formed thick-walled rectangular steel columns. J. Constr. Steel Res. 2018, 147, 277–292. [Google Scholar] [CrossRef] [Scilit]
  13. Shehnaz, S.M.; Shah, S.M.I.; Ganesh, G.M. Experimental and theoretical study on rectangular concrete filled steel tube columns subjected to axial compression. Mater. Today Proc. 2022, 65, 771–776. [Google Scholar] [CrossRef] [Scilit]
  14. Li, X.; Zhang, S.; Song, B.; Huang, Z. Eccentric compression behavior of CFST columns strengthened with steel tube and sandwiched grout jackets. Thin-Walled Struct. 2025, 215, 113565. [Google Scholar] [CrossRef] [Scilit]
  15. Liang, H.; Li, W.; Huang, Y.; Lu, Y. Axial behaviour of CFST stub columns strengthened with steel tube and sandwiched concrete jackets. Thin-Walled Struct. 2020, 155, 106942. [Google Scholar] [CrossRef] [Scilit]
  16. Huang, Y.; Li, W.; Lu, Y.; Liang, H.; Yan, Y. Behaviour of CFST slender columns strengthened with steel tube and sandwiched concrete jackets under axial loading. J. Build. Eng. 2022, 45, 103613. [Google Scholar] [CrossRef] [Scilit]
  17. Hassam, M.; Guo, L.; Atasham Ul Haq, M.; Tahir, M. Strengthening schemes of special-shaped concrete-filled steel tubes: A review. Structures 2024, 63, 106417. [Google Scholar] [CrossRef] [Scilit]
  18. Zhao, X.; Chen, Z.; Du, Y.; Du, M. Axial compressive behavior of FRP confined square high-strength CFST columns with artificial corrosion pits. Constr. Build. Mater. 2025, 496, 143781. [Google Scholar] [CrossRef] [Scilit]
  19. Liu, J.; Ji, C.; Zhao, Q.; Wang, J.; Li, J. Energy absorption and rate-dependent axial resistance of FRP-CFST stub columns under seismic-relevant compression demands. Structures 2026, 90, 112331. [Google Scholar] [CrossRef] [Scilit]
  20. Zhang, Y.; Ren, C.; Qian, L.; Wei, Y.; Liu, J.; Li, G. Machine learning-based capacity model for CFST columns with damaged BFRP jackets. Compos. Struct. 2025, 362, 119120. [Google Scholar] [CrossRef] [Scilit]
  21. Mirmiran, A.; Shahawy, M. A new concrete-filled hollow FRP composite column. Compos. Part B Eng. 1996, 27, 263–268. [Google Scholar] [CrossRef] [Scilit]
  22. Zhong, T.; Zhuang, J.; Qing, Y. Mechanical behavior of stub columns of FRP-confined concrete-filled steel tubes. Ind. Constr. 2005, 35, 20–23. [Google Scholar]
  23. Cao, S.; Wu, C.; Wang, W. Behavior of FRP confined UHPFRC-filled steel tube columns under axial compressive loading. J. Build. Eng. 2020, 32, 101511. [Google Scholar] [CrossRef] [Scilit]
  24. Hassanein, M.; Hamed, A.Y.; Cashell, K.; Shao, Y.-B. Confinement-based direct design method for fibre reinforced polymer confined CFST short columns. Thin-Walled Struct. 2023, 192, 111207. [Google Scholar] [CrossRef] [Scilit]
  25. Li, Y.; Liu, F.; Ma, J.; Xu, S. A unified method for predicting cross-sectional capacity of confined CFST columns. J. Constr. Steel Res. 2026, 239, 110224. [Google Scholar] [CrossRef] [Scilit]
  26. Dong, W.; Karalis, G.; Liebscher, M.; Wang, T.; Liu, P.; Li, W.; Mechtcherine, V. Multifunctional carbon fibre reinforced polymer (CFRP) composites for sustainable and smart civil infrastructure: A comprehensive review. Sustain. Mater. Technol. 2025, 45, e01594. [Google Scholar] [CrossRef] [Scilit]
  27. Alam, I.; Fawzia, S.; Zhao, X.-L.; Remennikov, A.M.; Bambach, M.; Elchalakani, M. Performance and dynamic behaviour of FRP strengthened CFST members subjected to lateral impact. Eng. Struct. 2017, 147, 160–176. [Google Scholar] [CrossRef] [Scilit]
  28. Na, L.; Yiyan, L.; Shan, L.; Lan, L. Slenderness effects on concrete-filled steel tube columns confined with CFRP. J. Constr. Steel Res. 2018, 143, 110–118. [Google Scholar] [CrossRef] [Scilit]
  29. Wang, Z.B.; Yu, Q.; Tao, Z. Behaviour of CFRP externally-reinforced circular CFST members under combined tension and bending. J. Constr. Steel Res. 2015, 106, 122–137. [Google Scholar] [CrossRef] [Scilit]
  30. Gao, X.Y.; Balendra, T.; Koh, C.G. Buckling strength of slender circular tubular steel braces strengthened by CFRP. Eng. Struct. 2013, 46, 547–556. [Google Scholar] [CrossRef] [Scilit]
  31. Du, Y.; Zhang, Y.; Chen, Z.; Yan, J.-B.; Zheng, Z. Axial compressive performance of CFRP confined rectangular CFST columns using high-strength materials with moderate slenderness. Constr. Build. Mater. 2021, 299, 123912. [Google Scholar] [CrossRef] [Scilit]
  32. Shen, Q.; Wang, J.; Wang, J.; Ding, Z. Axial compressive performance of circular CFST columns partially wrapped by carbon FRP. J. Constr. Steel Res. 2019, 155, 90–106. [Google Scholar] [CrossRef] [Scilit]
  33. Tao, Z.; Han, L.H. Behaviour of fire-exposed concrete-filled steel tubular beam columns repaired with CFRP wraps. Thin-Walled Struct. 2007, 45, 63–76. [Google Scholar] [CrossRef] [Scilit]
  34. Li, G.; Hou, C.; Shen, L. Life-cycle analysis of FRP-strengthened offshore CFST columns suffering from steel corrosion. Compos. Struct. 2021, 277, 114607. [Google Scholar] [CrossRef] [Scilit]
  35. Alam, M.I.; Fawzia, S.; Zhao, X.L. Numerical investigation of CFRP strengthened full scale CFST columns subjected to vehicular impact. Eng. Struct. 2016, 126, 292–310. [Google Scholar] [CrossRef] [Scilit]
  36. GB 50936-2014; Technical Code for Concrete Filled Steel Tubular Structures. China Architecture & Building Press: Beijing, China, 2014.
  37. GB/T 50081-2019; Standard for Test Methods of Concrete Physical and Mechanical Properties. China Architecture & Building Press: Beijing, China, 2019.
  38. GB/T 228.1-2021; Metallic MATERIALS-TENSILE TESTING-Part 1: Method of Test at Room Temperature. Standards Press of China: Beijing, China, 2021.
  39. GB/T 3354-2014; Test Method for Tensile Properties of Orientation Fiber Reinforced Polymer Matrix Composite Materials. Standards Press of China: Beijing, China, 2014.
  40. Han, L.H.; Yao, G.H.; Tao, Z. Performance of concrete-filled thin-walled steel tubes under pure torsion. Thin-Walled Struct. 2007, 45, 24–36. [Google Scholar] [CrossRef] [Scilit]
  41. Zhong, T.; XingQiang, W.; Brian, U. Stress-strain curves of structural and reinforcing steelsafter exposure to elevated temperatures. J. Mater. Civ. Eng. 2012, 25, 1306–1316. [Google Scholar] [CrossRef] [Scilit]
  42. Qin, X.D.; Li, Y.H.; Wang, B.; Ji, C.H.; Guo, C.Y.; Wang, H.; Xin, H.G. Simulation of effect of fiber direction on cutting process of CFRP. Mech. Sci. Technol. Aerosp. Eng. 2016, 35, 472–476. [Google Scholar]
  43. Zarringol, M.; Patel, V.I.; Liang, Q.Q. Artificial neural network model for strength predictions of CFST columns strength-ened with CFRP. Eng. Struct. 2023, 281, 115784. [Google Scholar] [CrossRef] [Scilit]
  44. Tao, Z.; Wang, Z.B.; Yu, Q. Finite element modelling of concrete-filled steel stub columns under axial compression. J. Constr. Steel Res. 2013, 89, 121–131. [Google Scholar] [CrossRef] [Scilit]
  45. Fardis, M.; Khalili, H. FRP-encased concrete as a structural material. Mag. Concr. Res. 1982, 34, 191–202. [Google Scholar] [CrossRef] [Scilit]
  46. Mander, J.B.; Priestley, M.J.N.; Park, R. Theoretical stress-strain model for confined concrete. J. Struct. Eng. 1988, 8, 1804–1826. [Google Scholar] [CrossRef] [Scilit]
  47. Qing, Y. Calculation of bearing capacity and strength of FRP-confined concrete columns. Ind. Constr. 2000, 30, 31–34. [Google Scholar]
  48. ACI 440R-07; Report on Fiber-Reinforced Polymer (FRP) Reinforcement for Concrete Structures. American Concrete Institute: Farmington Hills, MI, USA, 2007.
  49. Yun, L. The Study on Mechanical Properties of Concrete-Filled Circular CFRP-steel Meddle Long Columns Under Axial Compression; Hubei University of Technology: Wuhan, China, 2021. [Google Scholar]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.