Abstract
This study developed ESSC–FA–WESS foamed lightweight soil using early-strength supersulfated cement (ESSC), fly ash (FA), and waste engineering slurry sediment (WESS), and evaluated its performance and reliability. Twelve mixtures combined water-to-binder ratios of 0.55, 0.60, and 0.65 with wet densities of 700–1000 kg/m3. Fluidity, 7 d and 28 d unconfined compressive strength (UCS), and durability were tested. Individual failure probabilities for the softening coefficient (Ks), freeze–thaw strength reduction rate (δf), and wet–dry strength loss rate (Ldw) were estimated using Student’s t-distribution; system reliability was evaluated using a series system. Weakly bound water in WESS could be converted into free water. Fluidity increased with water-to-binder ratio and wet density. UCS and durability improved with wet density; with increasing w/b, UCS and durability first improved and then declined, both peaking at 0.60. All 12 mixtures met the fluidity criterion, and 11 met the 28 d UCS criterion. Four mixtures satisfied all three durability criteria in terms of average values, and A8 achieved the highest system reliability (97.30%), with Ks being the most critical factor limiting overall system reliability. A8 (1000 kg/m3, w/b = 0.60) is recommended for high-reliability engineering applications. This study provides a practical route for utilizing waste engineering slurry in foamed lightweight soil.
1. Introduction
Backfilling in narrow or geometrically complex areas is often constrained by limited working space and equipment. Traditional construction methods may have difficulty achieving the required degree of compaction in such areas, potentially leading to significant post-construction settlement. Foamed lightweight soil is a low-density building material that requires no rolling or vibration and can self-level and self-compact, thereby effectively addressing the above issues. Its simple construction and low self-weight provide broad prospects for engineering applications [1,2,3].
The production of foamed lightweight soil typically consumes substantial quantities of fillers and fresh water, prompting extensive research into alternative sustainable materials. Various soils and industrial solid wastes have been investigated as potential fillers. For instance, silty clay [4], volcanic cohesive soil [5], expansive soil [6], saline soil [7,8], marine sand [9], and excavated soil [10] have been successfully utilized in the production of foamed lightweight soil, with results confirming that the resulting materials meet the mechanical requirements. Furthermore, solid wastes such as bauxite tailings [11], waste dredged soil [12], oil sludge pyrolysis residues [13], and power plant cinder [14] have also been investigated as alternative filling materials. While these studies have significantly broadened the range of feasible fillers, the preparation process still requires significant amounts of fresh water. Waste engineering slurry derived from underground construction activities is characterized by its high water content and abundance of soil particles. It thus presents a promising dual-purpose opportunity: recycling solid waste while conserving water. However, systematic studies on the utilization of waste engineering slurry for foamed lightweight soil preparation remain scarce [15,16], despite the urgent need for its eco-friendly disposal.
Regarding the binder system, ordinary Portland cement (OPC) is widely used but is associated with high energy consumption and significant CO2 emissions. To reduce OPC consumption, industrial by-products and solid wastes, such as electric arc furnace slag [17], ground waste concrete [18], and fly ash and GGBS [3], have been used to develop novel low-carbon cementitious materials. Among these emerging low-carbon cementitious materials, supersulfated cement (SSC) is particularly noteworthy. Primarily composed of ground granulated blast-furnace slag (GGBS) activated by sulfate and alkaline sources, SSC exhibits promising strength development and densification [19,20]. However, SSC inherently suffers from slow early-age strength development [19], which is particularly detrimental to foamed lightweight soil, as the slurry requires rapid stiffening to stabilize the foam structure and prevent collapse during the initial curing period. To address this issue, various modification strategies have been explored, including increasing powder fineness [21] and incorporating chemical additives, such as calcium formate [22,23], or supplementary cementitious materials such as metakaolin [24], ultrafine iron ore tailings [25], and carbide slag [20,26]. Advanced methods, such as nano-modification [27,28], co-activation strategies combining carbide slag with ferroaluminate silicate phases [29], and seed-induced acceleration [30,31], have also been shown to enhance early strength. Nevertheless, many of these approaches are constrained by high costs, complex preparation processes, or potential stability issues, limiting their large-scale engineering applicability. Therefore, it is imperative to develop an economically viable and practical SSC tailored for foamed lightweight soil.
In addition to material development, the performance evaluation of foamed lightweight soil has mainly focused on average mechanical and durability properties, while the variability and failure probability of multiple durability indicators have received limited attention. To address the above research gap, this study used a self-developed early-strength supersulfated cement (ESSC), fly ash (FA), and waste engineering slurry sediment (WESS) to prepare ESSC–FA–WESS foamed lightweight soil. Fluidity, unconfined compressive strength (UCS), and durability tests were conducted for various mix proportions, and the effects of water-to-binder ratio and wet density on the performance of ESSC–FA–WESS foamed lightweight soil were analyzed. Furthermore, given the extensive application of probabilistic analysis in civil engineering [32,33,34] and its potential for the evaluation of foamed lightweight soil, Student’s t-distribution [35,36] was employed to perform reliability analysis on the three durability indicators, and the optimal water-to-binder ratio corresponding to each wet density was determined.
2. Materials and Methods
2.1. Raw Materials
The ESSC used in this study was formulated from GGBS, FGD gypsum, 42.5-grade ordinary Portland cement (OPC 42.5), and 42.5-grade rapid-hardening sulfoaluminate cement (R-SAC 42.5). The mix proportion was determined through preliminary tests as 73.64% GGBS, 13.94% FGD gypsum, 4.54% OPC 42.5, and 7.88% R-SAC 42.5 by mass. All cementitious raw materials, together with the fly ash, were supplied by a company in Xinji City. The waste engineering slurry was obtained from a construction site in Shijiazhuang, China. The slurry was treated with a flocculant (Dongying Nuoer Chemical Co., Ltd., Dongying, China) to obtain the waste engineering slurry sediment (WESS). The foaming agent and foam stabilizer were manufactured by Guangzhou Taili Chemical Co., Ltd. (Guangzhou, China). Photographs of GGBS and FGD gypsum are shown in Figure 1.
Figure 1.
Raw materials.
The physical properties and chemical compositions of the raw materials (including the cementitious components and fly ash) are summarized in Table 1 and Table 2, respectively. The main performance indicators of the formulated ESSC are presented in Table 3, while Table 4 lists the fundamental properties of both the waste engineering slurry and the WESS after flocculant treatment.
Table 1.
Density and specific surface area of raw materials.
Table 2.
Chemical composition of raw materials.
Table 3.
Main performance indicators of ESSC.
Table 4.
Basic properties of waste engineering slurry and WESS.
2.2. Mix Proportion Design
This experimental program was designed to investigate the effects of the water-to-binder ratio (w/b) and wet density on the performance of ESSC–FA–WESS foamed lightweight soil. Based on preliminary tests, the mass ratio of ESSC/FA/WESS was fixed at 0.33:0.24:0.43.
In accordance with the technical specification for cast-in-place foam lightweight soil roadbed (DB 13/T 5600-2022) [37], the constituent dosages per unit volume were calculated for 12 mix combinations, covering three w/b levels and four wet density levels. The detailed mix proportions are given in Table 5.
Table 5.
Mix proportions of ESSC–FA–WESS foamed lightweight soil.
Water originally present in the WESS participates in the mixing process and the hydration reactions; therefore, this water fraction was included in the total system water content for the calculation of the w/b ratio, as expressed in Equation (1):
where m1 is the mass of water contained in the WESS, m2 is the mass of additional mixing water, and mb is the total mass of cementitious materials.
The ESSC–FA–WESS foamed lightweight soil specimens were prepared according to the following standardized procedure. First, GGBS, FGD gypsum, OPC 42.5, and R-SAC 42.5 were mixed in a mechanical mixer (TLD-WHJ 60, Tai’an Luda Highway Instrument Manufacturing Co., Ltd., Tai’an, China) to ensure homogeneity. Then, FA, WESS, and additional water were introduced and blended for no less than 2 min. Finally, the preformed foam was incorporated into the mixture and stirred until a uniform dispersion was achieved.
2.3. Test Methods
2.3.1. Fluidity Test
The fluidity of the ESSC–FA–WESS foamed lightweight soil slurry was measured in accordance with the technical specification for foamed mixture lightweight soil filling engineering (CJJ/T 177-2012) [38].
2.3.2. UCS Test
The tests were conducted in accordance with reference [38]. The cured specimens were tested at 7 d and 28 d, and their dimensions were measured to compute the load-bearing area. Compression tests were performed using a universal testing machine (WD-300B, Guangzhou Guangcai Testing Instrument Co., Ltd., Guangzhou, China) until specimen failure, and the UCS was calculated from the recorded failure load.
2.3.3. Durability Tests
- (1)
- Water Resistance Test: The water resistance test was conducted in accordance with the reference [38]. After 28 d of standard curing, the specimens were immersed in water for durations of 7, 14, 28, 56, 90, and 120 days, and the softening coefficient (Ks) was subsequently calculated.
- (2)
- Freeze–Thaw Cycle Test: The freeze–thaw cycle test was conducted with reference to the test methods of autoclaved aerated concrete (GB/T 11969-2020) [39]. All specimen groups were subjected to freeze–thaw cycling. The UCS was measured every three cycles, and the strength reduction rate (δf) was calculated at each measurement point.
- (3)
- Wet–Dry Cycle Test: The wet–dry cycle test was conducted with reference to the test methods of autoclaved aerated concrete (GB/T 11969-2020) [39]. Specimens with wet densities of 800–1000 kg/m3 and w/b ratios of 0.55, 0.60, and 0.65 were subjected to wet–dry cycling. The 700 kg/m3 groups were excluded from the wet–dry cycle test because none of them simultaneously satisfied the acceptance criteria for both water resistance and freeze–thaw resistance. The UCS was measured every three cycles, and the strength loss rate (Ldw) was calculated at each measurement point.
2.4. Performance Evaluation and Reliability Analysis Method
2.4.1. Performance Evaluation Criteria
The performance of ESSC–FA–WESS foamed lightweight soil was evaluated based on five performance indicators: fluidity (fresh-state workability), 28 d UCS, Ks (after 120 d of water immersion), δf (after 30 freeze–thaw cycles), and Ldw (after 30 wet–dry cycles). The acceptance criteria for 28 d UCS were based on reference [37], fluidity followed reference [38], Ks followed reference [40], and δf and Ldw followed reference [41]. A failure event is defined as a test result that does not meet the corresponding acceptance criterion (Table 6).
Table 6.
Acceptance criteria for performance indicators.
2.4.2. Reliability Analysis Method
Reliability assessment was conducted on mix proportions that met the average-value acceptance criteria for all five indicators. Fluidity and 28 d UCS served as fundamental prerequisites and were therefore excluded from the subsequent reliability analysis, which focused on the three durability indicators (Ks, δf, and Ldw).
Owing to the limited sample size for each indicator (n ≤ 30) and the unknown population standard deviations, Student’s t-distribution was employed to assess the failure risk of a future individual specimen [35,36]. According to Table 6, failure was defined as Ks < 0.75, δf > 20%, or Ldw > 15%. Based on the sample mean μi, standard deviation si(si = μi × CV, where CV is the coefficient of variation), and sample size ni, the t-statistic was calculated as:
where i = 1, 2, 3 represent Ks, δf, and Ldw, respectively.
The corresponding one-sided tail probability gives the individual failure probability:
where T follows the t-distribution, with df = ni − 1.
The acceptance criteria for all three durability indicators (Ks, δf, and Ldw) must be satisfied simultaneously; therefore, the durability reliability was modeled as a series system [42]. In the absence of paired data for joint distribution, the indicators are assumed to be mutually independent as a simplifying assumption. The system reliability for these three indicators is [32,43]:
The resulting Rsys can be used for relative comparison among different mix proportions to identify mix schemes with higher reliability, providing a basis for engineering optimization.
3. Results
3.1. Fluidity Test
The fluidity test results for each ESSC–FA–WESS foamed lightweight soil group are presented in Figure 2 (all test data in Section 3 are mean values).
Figure 2.
Fluidity of ESSC–FA–WESS foamed lightweight soil.
3.1.1. Effect of the Water-to-Binder Ratio
As shown in Figure 2a, at a wet density of 700 kg/m3, the fluidity values were 164, 167, and 174 mm for w/b ratios of 0.55, 0.60, and 0.65, respectively, indicating that fluidity increased with increasing w/b ratio. This trend was consistently observed under the other three wet density conditions.
3.1.2. Effect of Wet Density
As shown in Figure 2b, at a w/b ratio of 0.55, the fluidity values of ESSC–FA–WESS foamed lightweight soil at wet densities of 700, 800, 900, and 1000 kg/m3 were 164, 169, 176, and 180 mm, respectively, demonstrating a positive correlation between fluidity and wet density. This pattern remained consistent at w/b ratios of 0.60 and 0.65.
3.2. UCS Test
3.2.1. Effect of Wet Density
The UCS test results of ESSC–FA–WESS foamed lightweight soil at different wet densities are presented in Figure 3. At a w/b ratio of 0.60, as the wet density increased from 700 to 1000 kg/m3, the 7 d UCS rose from 0.93 to 2.23 MPa, and the 28 d UCS rose from 1.54 to 2.93 MPa. Both 7 d and 28 d UCS exhibited a consistent increasing trend with wet density, and this pattern was similarly observed under the other two w/b ratio conditions.
Figure 3.
Effect of wet density on UCS.
3.2.2. Effect of the Water-to-Binder Ratio
Figure 4 presents the UCS test results of ESSC–FA–WESS foamed lightweight soil at different w/b ratios. As shown in Figure 4, at a wet density of 700 kg/m3, the UCS under the three w/b ratios all exhibited a trend of initial increase followed by a decrease. The same trend was observed at the other three wet densities. Across all four wet densities, when the w/b ratio increased from 0.55 to 0.60, the 7 d UCS increased by 10–29%, and the 28 d UCS increased by 11–26%. When the w/b ratio increased from 0.60 to 0.65, the 7 d and 28 d UCS decreased by 20–30% and 15–38%, respectively. Both 7 d and 28 d UCS consistently peaked at a w/b ratio of 0.60.
Figure 4.
Effect of w/b on UCS.
3.3. Water Resistance Test
3.3.1. Effect of Wet Density
Figure 5a illustrates how the Ks of the ESSC–FA–WESS foamed lightweight soil varies with wet density. At a w/b ratio of 0.60, after 120 d of water immersion, the Ks values of specimens with wet densities of 700, 800, 900, and 1000 kg/m3 were 0.74, 0.79, 0.85, and 0.93, respectively, demonstrating an increasing trend with wet density. The same trend was observed at w/b ratios of 0.55 and 0.65.
Figure 5.
Ks of ESSC–FA–WESS foamed lightweight soil.
3.3.2. Effect of the Water-to-Binder Ratio
Figure 5b illustrates how Ks of the ESSC–FA–WESS foamed lightweight soil varies with the w/b ratio. At a wet density of 1000 kg/m3, after 120 d of water immersion, the Ks values for w/b ratios of 0.55, 0.60, and 0.65 were 0.90, 0.93, and 0.88, respectively, indicating that Ks first increased and then decreased with increasing w/b ratio. The same pattern was observed under the other three wet density conditions.
3.4. Freeze–Thaw Cycle Test
3.4.1. Effect of Wet Density
Figure 6 presents the δf of ESSC–FA–WESS foamed lightweight soil under freeze–thaw cycling for various wet densities at different w/b ratios. As shown in Figure 6b, at a w/b ratio of 0.60, after 30 freeze–thaw cycles, the δf values of specimens with wet densities of 700, 800, 900, and 1000 kg/m3 were 26.3%, 17.5%, 13.4%, and 9.8%, respectively, demonstrating a decreasing trend with increasing wet density. This same trend was observed under the other two w/b ratio conditions.
Figure 6.
δf versus freeze–thaw cycles for various wet densities at different w/b ratios.
3.4.2. Effect of the Water-to-Binder Ratio
Figure 7 presents δf for various w/b ratios at different wet densities. As shown in Figure 7a, at a wet density of 700 kg/m3, after 30 freeze–thaw cycles, δf values for w/b ratios of 0.55, 0.60, and 0.65 were 33.9%, 26.3%, and 45.5%, respectively, indicating that δf first decreased and then increased with increasing w/b ratios. The same trend was observed at the other three wet densities.
Figure 7.
δf versus freeze–thaw cycles for various w/b ratios at different wet densities.
3.5. Wet–Dry Cycle Test
3.5.1. Effect of Wet Density
Figure 8 presents the Ldw of ESSC–FA–WESS foamed lightweight soil under wet–dry cycles for various wet densities at different w/b ratios. As shown in Figure 8b, at a w/b ratio of 0.60, the negative Ldw values during the first six wet–dry cycles indicate that the UCS of specimens with wet densities of 800, 900, and 1000 kg/m3 increased slightly during this period, followed by a gradual decrease thereafter. After 30 wet–dry cycles, the Ldw values were 18.28%, 12.62%, and 7.94%, respectively, showing a decreasing trend with increasing wet density. This same trend was observed under the other w/b ratio conditions.
Figure 8.
Ldw versus wet–dry cycles for various wet densities at different w/b ratios.
3.5.2. Effect of the Water-to-Binder Ratio
Figure 9 presents the Ldw values for various w/b ratios at different wet densities. As shown in Figure 9c, at a wet density of 1000 kg/m3, after 30 wet–dry cycles, the Ldw values for w/b ratios of 0.55, 0.60, and 0.65 were 10.34%, 7.94%, and 11.86%, respectively, indicating that Ldw first decreased and then increased with increasing w/b ratios. The same trend was observed under the other wet density conditions.
Figure 9.
Ldw versus wet–dry cycles for various w/b ratios at different wet densities.
3.6. Reliability Analysis of Durability Indicators
Based on the evaluation criteria described in Section 2.4.1 (Table 6) and the test results presented in Figure 2, Figure 3, Figure 4, Figure 5, Figure 6, Figure 7, Figure 8 and Figure 9, all 12 groups met the fluidity criterion, and 11 groups met the 28 d UCS criterion. A9 (0.95 MPa) did not meet the required 28 d UCS criterion (1.00 MPa) (Figure 3 and Figure 4). For the durability-related indicators, the following groups met their respective criteria: Ks—A3, A4, A6, A7, A8, A9, and A12; δf—A3, A4, A6, A7, A8, A11, and A12; Ldw—A4, A7, A8, and A12. Among these, four groups (A4, A7, A8, and A12) satisfied all three durability criteria simultaneously in terms of average values and also met the UCS prerequisite.
For these four qualifying groups, Table 7 summarizes the means and coefficients of variation of each durability indicator, together with the individual failure probabilities and system reliability calculated according to the method described in Section 2.4.2.
Table 7.
Reliability assessment of durability indicators.
4. Discussion
4.1. Conversion of Weakly Bound Water into Free Water
The free water in the foamed lightweight soil system provides fluidity and participates in the hydration reactions. In this experiment, the amount of added water was significantly less than that required for preparing conventional foamed lightweight soil, because water from the WESS was utilized. In the ESSC–FA–WESS foamed lightweight soil system, the utilizable water consists of three components: (1) the free water added during preparation, (2) the free water originally existing in the WESS, and (3) the weakly bound water adsorbed on the surface of soil particles within the WESS. The first two components can be directly used, while the weakly bound water has the potential to be converted into free water. During the preparation, part of the weakly bound water was converted into free water under the mechanical action of mixing, and another portion was converted through cation exchange.
Figure 10 schematically illustrates how the weakly bound water is converted into free water through cation exchange. The waste engineering slurry used in this study had been pre-treated with Na2CO3 for modification. Consequently, Na+ ions were adsorbed on the surface layers of soil particles in the WESS before mixing. Because Na+ has a weak capacity to neutralize negative charges, a substantial number of Na+ ions were adsorbed on the soil particle surfaces. Moreover, due to mutual repulsion among Na+ ions, they were distributed at relatively greater distances from the soil particle surfaces, forming thicker ionic layers and correspondingly thicker weakly bound water films. During the mixing process, high-valence cations such as Ca2+ and Mg2+ released from the hydration of cementitious materials can displace the Na+ ions adsorbed on the soil particle surfaces. High-valence cations possess a stronger neutralization capacity and are therefore required in smaller quantities. They tend to distribute in regions closer to the soil particle surfaces, resulting in thinner ionic layers and thinner weakly bound water films. As a consequence, the excess weakly bound water can detach from the soil particles and be converted into free water that can participate in the system [44,45]. Since sodium-based bentonite slurries are widely used in underground construction and commonly contain abundant Na+, the proposed approach may have broad applicability to the recycling of such waste engineering slurries.
Figure 10.
Schematic diagram of water conversion.
4.2. Effect of Wet Density
Both the fluidity and UCS of ESSC–FA–WESS foamed lightweight soil show a clear increasing trend with increasing wet density (Figure 2b and Figure 3). This trend is consistent with that observed in other foamed lightweight soils.
For fluidity, this improvement is attributed to the reduced foam volume fraction at higher wet densities. At lower wet densities, the high foam content leads to close packing of bubbles, which increases inter-bubble contacts and deformational resistance, thereby elevating the yield stress of the fresh slurry and reducing its fluidity. As wet density increases, the foam bubbles become more widely spaced, the slurry phase becomes more continuous, and the flow resistance decreases accordingly, resulting in improved fluidity, as reflected in the flow spread measurements (Figure 2b).
For the UCS, as shown in Figure 3, this improvement is attributed to the reduction in foam volume fraction at higher wet densities, which decreases the porosity of the material. As a result, the effective load-bearing area increases and stress concentrations are reduced, thereby inhibiting crack initiation and propagation and consequently enhancing the UCS [46,47].
4.3. Effect of the Water-to-Binder Ratio
The effects of the water-to-binder ratio on the fluidity and UCS are distinctly different: fluidity increased monotonically with increasing w/b ratios, while the UCS first increased and then decreased, peaking at w/b = 0.60 (Figure 2a and Figure 4).
In terms of fluidity, a higher w/b ratio increases the free water content. The free water acts as a lubricant in the slurry, reducing inter-particle friction and cohesion, thereby facilitating slurry flow.
In terms of the UCS, the initial increase followed by a decrease reflects a trade-off between the degree of hydration and porosity [48,49,50]. At w/b = 0.55, the limited water content may restrict hydration, resulting in limited formation of hydration products, weak cementitious bonding, and relatively low strength. At w/b = 0.60, the water content is sufficient to ensure adequate hydration, allowing hydration products to fill the pores originally occupied by free water. Consistent with the general trends reported for foamed cementitious materials [48,49,50], this is the condition under which the matrix can be expected to achieve a more favorable pore structure and form a denser cementitious network. At w/b = 0.65, the excess free water evaporates during hardening. Following the established relationship between the water-to-binder ratio, pore connectivity, and strength [49,50], this would result in a coarsened pore structure with increased capillary and interconnected pores. Although hydration is more complete at this ratio, the strength reduction due to the inferred increase in porosity outweighs the gains from hydration, leading to a decline in strength.
4.4. Durability Analysis
The results of the three durability indicators—Ks, δf, and Ldw—were consistent: durability improved with increasing wet density, while it first improved and then deteriorated with increasing w/b ratios, with the best performance at w/b = 0.60 (Figure 5, Figure 6, Figure 7, Figure 8 and Figure 9). The underlying mechanisms are discussed below from the perspectives of wet density and the w/b ratio.
4.4.1. Effect of Wet Density
Ks increased with wet density (Figure 5a), while δf decreased with wet density (Figure 6), along with Ldw (800–1000 kg/m3, Figure 8). Specimens with a lower wet density had a higher foam content and greater porosity, making them more susceptible to water ingress [46]. During freeze–thaw cycling, pore water freezes and generates frost heave forces, initiating microcracks and converting some closed pores into interconnected pores, forming a positive feedback deterioration cycle of cracking, pore interconnection, and further water ingress [51]. Low-wet-density specimens, with more closed pores available for conversion, exhibited more significant strength loss. During wet–dry cycling, the repeated ingress and egress of water induced shrinkage stresses; low-wet-density specimens with thinner pore walls had weaker resistance, while high-wet-density specimens, with lower porosity and thicker pore walls, exhibited slower damage progression [46,52].
4.4.2. Effect of the Water-to-Binder Ratio
Ks, δf, and Ldw all reached their optimum values at w/b = 0.60 (Figure 5b, Figure 7 and Figure 9). Unlike the static strength mechanism discussed in Section 4.3, the durability performance reflects the damage evolution rate under cyclic environmental actions.
At w/b = 0.55, the weak interfacial bonding due to insufficient hydration not only reduces initial strength but also provides preferential pathways for water penetration. Under freeze–thaw or wet–dry cycling, these weak interfaces accelerate crack initiation and propagation, leading to a faster deterioration rate per cycle.
At w/b = 0.60, the dense cementitious network minimizes the connectivity of capillary pores. This restricts the transport of water into the matrix, reducing the internal stress amplitude during each cycle. Consequently, the damage accumulation per cycle is minimized, resulting in the best durability performance.
At w/b = 0.65, although hydration is more complete, the increased porosity and pore connectivity allow rapid water ingress. During freeze–thaw cycles, the abundant capillary pores provide ample nucleation sites for ice crystallization, generating localized tensile stresses that exacerbate fatigue damage. The cumulative damage at w/b = 0.65 is therefore the greatest, leading to the most rapid performance degradation [50,53].
4.4.3. Initial Strength Increase During Wet–Dry Cycles
During wet–dry cycling, specimens with wet densities of 800, 900, and 1000 kg/m3 exhibited a slight increase in UCS during the first six cycles (Figure 8), followed by a decline thereafter.
Further analysis of the magnitude of the initial strength increase across different water-to-binder ratios revealed a distinct pattern: the initial strength increase was most pronounced at w/b = 0.55, while it was the smallest at w/b = 0.60. This pattern is consistent with the proposed mechanism. At w/b = 0.55, the initially insufficient hydration may leave a relatively larger amount of unhydrated cementitious particles and a relatively porous matrix. Upon re-exposure to water during wet–dry cycles, these particles resume hydration, generating products that fill micropores and temporarily outweigh the damage caused by shrinkage stresses [54]. In contrast, at w/b = 0.60, the matrix is expected to be relatively well hydrated, with fewer unhydrated particles and limited void space for product deposition, resulting in the weakest rehydration enhancement. With increasing cycles, cumulative damage becomes dominant across all ratios as the hydration-enhancing effect saturates.
4.5. Reliability Analysis
As shown in Table 7, the individual failure probabilities for δf are consistently low (≤ 0.01%) across all four groups. In contrast, Ks exhibits the highest failure probabilities, ranging from 2.70% (A8) to 9.70% (A7), indicating that Ks is the most critical factor limiting the overall system reliability among the three durability indicators. Ldw shows intermediate failure probabilities, from 0.00% (A8) to 2.32% (A7).
Among the four groups, A8 achieves the highest system reliability (Rsys = 97.30%), followed by A4 (96.49%), A12 (92.16%), and A7 (88.20%). This ranking can be explained by the combined effects of the w/b ratio and wet density. A8, with w/b = 0.60 and a wet density of 1000 kg/m3, benefits from both optimal hydration (as discussed in Section 4.3) and a dense matrix with low porosity (as discussed in Section 4.2), resulting in superior overall reliability. A4 (w/b = 0.55, 1000 kg/m3) shows slightly lower reliability than A8; although its high wet density ensures low porosity, insufficient hydration at this w/b ratio may weaken interfacial bonding and adversely affect durability performance. A12 (w/b = 0.65, 1000 kg/m3) shows lower reliability than A4, which is attributed to the coarsened pore structure resulting from excess free water evaporation. A7, despite having the same w/b = 0.60 as A8, shows the lowest reliability (Rsys = 88.20%), which is primarily due to its lower wet density (900 kg/m3); the higher foam content leads to increased porosity and consequently less favorable durability performance, with Ks and Ldw values closer to their corresponding acceptance limits.
From a practical perspective, A8 is recommended as the preferred mix proportion for engineering applications requiring high reliability. For A7, although it satisfies all average-value criteria, its relatively high system failure probability suggests that additional quality control measures should be implemented if adopted in practice. Nevertheless, the relative ranking of the four groups in terms of system reliability remains valid, as all groups were evaluated using the same statistical framework.
The present results were obtained using raw materials from specific sources under controlled laboratory conditions and should therefore be generalized with caution. Variations in raw material properties and environmental exposure may affect hydration, strength, and durability. Further validation is needed for materials from different sources and under different environmental conditions. In addition, the utilization of WESS in foamed lightweight soil provides a potential approach for utilizing waste engineering slurry and reducing the environmental burden associated with its disposal. Economic feasibility was not quantitatively evaluated in this study and should be further assessed using project-specific cost data.
5. Conclusions
- (1)
- A portion of the weakly bound water in WESS can be released from soil particle surfaces through cation exchange and converted into utilizable free water in the ESSC–FA–WESS foamed lightweight soil system.
- (2)
- The fluidity of ESSC–FA–WESS foamed lightweight soil increases with increasing water-to-binder ratios and wet density. Both UCS and durability improve with increasing wet density. With increasing water-to-binder ratios, UCS and durability first improve and then decline.
- (3)
- All 12 groups met the fluidity criterion, and 11 groups met the 28 d UCS criterion. Among the four groups (A4, A7, A8, and A12) that simultaneously satisfied all three durability criteria in terms of average values, δf showed the lowest failure probability (≤0.01%), followed by Ldw (0.00–2.32%), whereas Ks showed the highest failure probability (2.70–9.70%). Ks was therefore identified as the most critical factor limiting the overall system reliability. The system reliability ranking was A8 > A4 > A12 > A7.
- (4)
- Based on the comprehensive consideration of UCS, durability indicators, and fluidity, the recommended mix proportion for ESSC–FA–WESS foamed lightweight soil in this study is a design wet density of 1000 kg/m3 and a water-to-binder ratio of 0.60. When a lower wet density is required for specific engineering applications, the wet density may be reduced to 900 kg/m3 at a w/b ratio of 0.60, but additional quality control measures should be implemented.
- (5)
- Future studies should investigate the long-term performance of ESSC–FA–WESS foamed lightweight soil using raw materials from different sources and under individual or coupled environmental actions, including freeze–thaw cycling, wet–dry cycling, and water immersion. Field-scale validation is also needed to assess the engineering applicability of the recommended mix proportion and reliability analysis method.
Author Contributions
Conceptualization, Y.L. and Q.Z.; Methodology, Y.L. and Q.Z.; Formal analysis, Y.J.; Investigation, T.W. and H.X.; Data curation, H.X.; Writing—original draft preparation, T.W. and Y.J.; Writing—review and editing, Q.Z. and H.X.; Visualization, T.W.; Supervision, Y.L. and Q.Z.; Resources, Y.L.; Project administration, Q.Z.; Funding acquisition, Q.Z. and Y.J. All authors have read and agreed to the published version of the manuscript.
Funding
This research was funded by Research on Key Technologies for the Development of Green Low-Carbon Fluidized (Lightweight) Solid Waste Soil and the PhD Research Initiation Fund of Hebei University of Science and Technology (grant number 1181244).
Data Availability Statement
The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding authors.
Acknowledgments
During the preparation of this manuscript/study, the authors used Gemini 3.1 to generate MATLAB code for plotting Figure 10. MATLAB R2019a (The MathWorks, Inc., Natick, MA, USA) was used to execute the generated code and produce Figure 10. DeepSeek-V4 Preview and Qwen 3.7 were used to assist with the translation. The authors have reviewed and edited the output and take full responsibility for the content of this publication.
Conflicts of Interest
Author Yongxian Li was employed by the Hebei JiaoTou HengDe Expressway Development Co., Ltd. The remaining authors declare that the research was conducted in the absence of any commercial or financial relationships that could be construed as a potential conflict of interest.
References
- Yuan, X.; Lu, Z.; Yao, H.; Tan, X.; Zhao, Y.; Tang, C.; Cheng, M.; Gao, Y. Engineering properties and applications of air-foamed lightweight soil. Adv. Mater. Sci. Eng. 2022, 2022, 4967037. [Google Scholar] [CrossRef] [Scilit]
- Liu, Y.; Li, Y.; Sun, Y. Dynamic characteristics of geogrid-reinforced foamed lightweight soil under cyclic loading. Buildings 2026, 16, 2426. [Google Scholar] [CrossRef] [Scilit]
- Shen, C.; Liu, H.; Wan, H.; Li, J.; Liu, P.; He, Q.; Xuan, J. Effect of Cementitious Material Composition on the Performance of Low-Carbon Foamed Lightweight Soil. Buildings 2023, 13, 759. [Google Scholar] [CrossRef] [Scilit]
- Liu, Y.; Zhang, P.H.; Zhao, X.G. Experimental Study on Property of Foamed Lightweight Soil Mixed with Silty Clay. J. Highw. Transp. Res. Dev. 2024, 41, 20–26. [Google Scholar]
- Furukawa, Y.; Kawamata, S. Utilization of Volcanic Cohesive Soil to Foamed Mixture Light-Weight Soil. J. Jpn. Soc. Civ. Eng. Ser. C (Geosph. Eng.) 2013, 69, 480–490. [Google Scholar] [CrossRef] [Scilit][Green Version]
- Zheng, S.W.; Liu, S.Y.; Li, D.; Tong, L.Y.; Wu, K. Experimental study on mechanical properties of expansive soil-based lightweight foam soil. Rock Soil Mech. 2025, 46, 1455–1465. [Google Scholar]
- Zhang, R.; Zhao, B.; Zheng, X.C.; Chen, L.; Lu, Z.; Zhao, Y. Salt-inhibiting mechanism and effect of new saline soil-based foamed lightweight soil separation fault. Rock Soil Mech. 2025, 46, 515–526, 538. [Google Scholar]
- Lu, Z.; Zhang, R.; Zhao, Y.; Qin, L.; Liu, J.; Yan, T.Z.; Li, J.; Li, B.W.; Zhang, J. Experimental study on engineering characteristics of foamed lightweight soil based on saline soil. Chin. J. Rock Mech. Eng. 2025, 44, 206–218. [Google Scholar]
- Que, Y.; Chen, X.; Zhu, T.; Zhang, H.Y.; Huang, W.F.; Leung, A.K.; Jiang, Z.L.; Xue, B.; Lu, D. Characterizing the engineering properties of marine sand-amended foamed lightweight soil: Macroscopic and microscopic perspectives. Constr. Build. Mater. 2023, 367, 130305. [Google Scholar] [CrossRef] [Scilit]
- Lu, Z.; Ze, Z.H.; Zhao, Y.; Chai, S.Q.; Liu, B.; Li, Y.B.; Yao, H.L. Physical-mechanical properties and durability analysis of foamed lightweight soil based on excavated soil and fly ash. Rock Soil Mech. 2026, 47, 1917–1928. [Google Scholar]
- Peng, Y.; Jiang, J.; Ou, X.; Qin, J. Investigating the Properties of Foamed Mixture Lightweight Soil Mixed with Bauxite Tailings as Filler. Adv. Mater. Sci. Eng. 2019, 2019, 6295348. [Google Scholar] [CrossRef] [Scilit]
- Xia, X.; Chen, X.; Zhuang, N.; Xiao, W.; Wang, Y. Study on the Properties of Foamed Mixture Lightweight Soil Prepared from Waste Dredged Soil for Ecological Floating Landscapes. Materials 2026, 19, 2512. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Ren, K.Q.; Wang, Y.; Lei, B.B.; Zhang, J.P.; Liu, J. Research on performance of foamed lightweight soil of aeolian sand and oil sludge pyrolysis residues. China Powder Sci. Technol. 2025, 31, 141–151. [Google Scholar]
- Zhu, Z.; Hu, X.; Liu, X.; Liu, Y.; Ye, X.; Liu, Y. Experimental Study on Physical and Mechanical Properties of Foamed Lightweight Soil for Underwater Backfilling. J. Phys. Conf. Ser. 2022, 2390, 012024. [Google Scholar] [CrossRef] [Scilit]
- Lu, D.H.; Zhang, H.B.; Hu, X.L.; Hu, G.X. Indoor experimental study on making foam cement banking from waste mud. Sichuan Build. Mater. 2024, 50, 37–38,50. [Google Scholar]
- Zhang, H.B.; Lu, D.H.; Hu, X.L.; Hu, G.X. Experimental Study on the Preparation of Cement-Fly Ash Foamed Lightweight Soil Using Waste Slurry from Bridge Pile Foundations. North. Commun. 2025, 6, 1–4+9. [Google Scholar]
- Tadić, N.; Brašanac-Vukanović, S.; Nikolić, I.; Radmilović, V.V.; Radmilović, V.R. Thermal Stability and Leaching Behavior of Alkali-Activated Slag Doped with Electric Arc Furnace Dust. Sci. Sinter. 2025, 57, 411–423. [Google Scholar] [CrossRef] [Scilit]
- Jelić, I.V.; Savić, A.R.; Miljojčić, T.A.; Šljivić-Ivanović, M.Z.; Dimović, S.D.; Janković, M.M.; Perović, I.M.; Zakić, D.M.; Antonijević, D.L. Development of Low Carbon and Energy-Efficient Geopolymer-Based Paving Blocks. Sci. Sinter. 2025, 57, 273–286. [Google Scholar]
- Wu, Q.; Xue, Q.; Yu, Z. Research status of super sulfate cement. J. Clean. Prod. 2021, 294, 126228. [Google Scholar] [CrossRef] [Scilit]
- Qi, G.; Zhang, Q.; Sun, Z. Effect of Calcium Aluminate and Carbide Slag on Mechanical Property and Hydration Mechanism of Supersulfated Cement. Buildings 2024, 14, 930. [Google Scholar] [CrossRef] [Scilit]
- Gao, Y.X.; Wang, J.; Xiang, J.Y.; Chen, J.; Liu, D. Study on mechanical properties of supersulphated cement based on powder particle size variation. China Concr. Cem. Prod. 2014, 3, 14–18. [Google Scholar]
- Ma, J.; Bai, X.; Sun, J.; Wu, P.; Yu, Z.; Xia, B. The role of calcium formate in supersulfated cement: A multiscale study on hydration mechanisms, pore structure and environmental benefits. Process Saf. Environ. Prot. 2026, 205, 108250. [Google Scholar] [CrossRef] [Scilit]
- Geng, C.H.; Liu, B.B.; Sun, G.L.; Chen, H.; Hou, P.K.; Li, Q.F.; Jiao, R.Q.; An, H.R.; Cheng, X. New insight into the role of alkaline activator in the hydration of supersulfated cement and the regulation effect of calcium formate. Constr. Build. Mater. 2025, 463, 140108. [Google Scholar] [CrossRef] [Scilit]
- Wang, X.; Gu, X.; Wang, S.; Ge, X.; Hu, Z.; Liu, J.; Zhang, X.; Wang, X. Using Metakaolin as an Enhancing Component in Supersulfated Cement: A Comprehensive Evaluation. Environ. Res. 2026, 295, 123903. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Zhang, M.; Chen, B.; Zhu, W. Performance and hydration mechanisms of ultrafine iron ore tailings enhanced supersulfated cement with high phosphogypsum content. Cem. Concr. Compos. 2025, 157, 105891. [Google Scholar] [CrossRef] [Scilit]
- Cui, S.H.; Fan, K.J.; Yao, Y. Effect of carbide slag dosage on hydration behavior and mechanical properties of supersulfated cement. Constr. Build. Mater. 2025, 491, 142823. [Google Scholar] [CrossRef] [Scilit]
- Chen, H.; Hou, P.; Zhou, X.; Black, L.; Adu-Amankwah, S.; Feng, P.; Cui, N.; Glinicki, M.A.; Cai, Y.M.; Zhang, S.P.; et al. Toward performance improvement of supersulfated cement by nano silica: Asynchronous regulation on the hydration kinetics of silicate and aluminate. Cem. Concr. Res. 2023, 167, 107117. [Google Scholar] [CrossRef] [Scilit]
- Cai, T.Z.; Hou, P.K.; Chen, H.; Zhao, P.Q.; Du, P.; Wang, S.D.; Zhou, X.M.; Wang, X.W.; Cheng, X. Effects of nanosilica on supersulfated cements of different clinker-activation degree. Constr. Build. Mater. 2023, 365, 130118. [Google Scholar] [CrossRef] [Scilit]
- Sun, Z.N.; Wang, B.X.; Mu, R.; Chen, H.; Huang, T.S.; Guo, J.H. Mechanistic insights into hydration kinetics and strength enhancement of supersulfated cement co-activated by carbide slag and ferroaluminate-silicate synergy. Constr. Build. Mater. 2026, 520, 146008. [Google Scholar] [CrossRef] [Scilit]
- Huang, X.M.; Guo, J.L.; Li, Y.C.; Xu, C.X.; Deng, J.Y.; Zheng, Y.Z.; Jin, Y.J.; Chang, C.; Zhou, Y. Field-ready acceleration of supersulfated cement using ambient-synthesized ettringite seeds: Early-age hydration kinetics and constructability enhancement. J. Build. Eng. 2026, 120, 115405. [Google Scholar] [CrossRef] [Scilit]
- Luo, Z.T.; Yang, Y.F.; Liu, X.H.; Liu, L.; Yang, H.T.; Ye, J.Y.; Gao, M.K.; Ge, M.X.; Hu, Z.F. Effects of C-S-H seeds on the early performance of low-carbon supersulfated cement. Constr. Build. Mater. 2025, 458, 139764. [Google Scholar] [CrossRef] [Scilit]
- Zhang, J.; Xiao, T.; Ji, J.; Zeng, P.; Cao, Z. Geotechnical Reliability Analysis: Theories, Methods and Algorithms; Springer: Singapore, 2023. [Google Scholar]
- Anwar, G.A.; Akber, M.Z.; Ahmed, H.A.; Hussain, M.; Nawaz, M.; Anwar, J.; Chan, W.-K.; Lee, H.-H. Life-Cycle Performance Modeling for Sustainable and Resilient Structures under Structural Degradation: A Systematic Review. Buildings 2024, 14, 3053. [Google Scholar] [CrossRef] [Scilit]
- Wang, Q.-A.; Chen, J.; Ni, Y.; Xiao, Y.; Liu, N.; Liu, S.; Feng, W. Application of Bayesian networks in reliability assessment: A systematic literature review. Structures 2025, 71, 108098. [Google Scholar] [CrossRef] [Scilit]
- Brereton, R.G. The t-distribution and its relationship to the normal distribution. J. Chemom. 2015, 29, 481–483. [Google Scholar] [CrossRef] [Scilit]
- Casella, G.; Berger, R.L. Statistical Inference, 2nd ed.; Duxbury Press: Pacific Grove, CA, USA, 2002. [Google Scholar]
- DB13/T 5600-2022; Technical Specification for Cast-in-Place Foam Lightweight Soil Roadbed. Hebei Provincial Administration for Market Regulation: Shijiazhuang, China, 2022.
- CJJ/T 177-2012; Technical Specification for Foamed Mixture Lightweight Soil Filling Engineering. China Architecture & Building Press, Ministry of Housing and Urban-Rural Development of the People’s Republic of China: Beijing, China, 2012.
- GB/T 11969-2020; Test Methods of Autoclaved Aerated Concrete. Standards Press of China, Standardization Administration of the People’s Republic of China: Beijing, China, 2020.
- Zhang, P.H. Research on the Properties of Foam Light Soil and Its Application in Highway Engineering. Master’s Thesis, North China University of Science and Technology, Tangshan, China, 2023. [Google Scholar]
- Jiang, H.; Ma, M.; Xie, Q.; Wang, C.; Gong, Y.; Ma, C.; Yao, Z. Study on the environmental resistance of foamed lightweight soil material from sintered dust. Chin. J. Rock Mech. Eng. 2024, 43, 4032–4043. [Google Scholar]
- He, Y.; Xue, H.J.; Du, J. Reliability analysis of the freeze-thaw cycle of aeolian sand concrete based on a dual neural network in series structure failure mode. Symmetry 2024, 16, 782. [Google Scholar] [CrossRef] [Scilit]
- JGJ 284-2012; Code for Electrical Design of Financial Buildings. China Architecture & Building Press, Ministry of Housing and Urban-Rural Development of the People’s Republic of China: Beijing, China, 2012.
- Li, Y.; Wang, X.J.; Wang, J.F. Cation exchange, interlayer spacing, and thermal analysis of Na/Ca-montmorillonite modified with alkaline and alkaline earth metal ions. J. Therm. Anal. Calorim. 2012, 110, 1199–1206. [Google Scholar] [CrossRef] [Scilit]
- Wan, Y.; Guo, D.; Hui, X.; Liu, L.; Yao, Y. Studies on hydration swelling and bound water type of sodium- and polymer-modified calcium bentonite. Adv. Polym. Technol. 2020, 2020, 9361795. [Google Scholar] [CrossRef] [Scilit]
- Yuan, H.; Ge, Z.; Sun, R.; Xu, X.; Lu, Y.; Ling, Y.; Zhang, H. Drying shrinkage, durability and microstructure of foamed concrete containing high volume lime mud-fly ash. Constr. Build. Mater. 2022, 327, 126990. [Google Scholar] [CrossRef] [Scilit]
- Liu, J.; Li, H.; Zhang, B.; Liu, B.; Hao, B.; Jiang, N. Pore structure analysis of foamed lightweight soil based on X-ray CT scanning technique. J. Beijing Univ. Technol. 2024, 50, 1228–1236. [Google Scholar]
- Ma, C.Y.; Yu, T.T.; Zhang, N.; Li, Z.F.; Zhang, J. Study on rheological properties and regulation of Bayer red mud-based foamed lightweight soil. Chin. J. Eng. 2024, 46, 1912–1920. [Google Scholar]
- Jierula, A.; Li, H.; Chen, Y.; Wu, C.; Wu, X.; Yin, H. Study on the Influence of Density and Water-Cement Ratio on the Cement Utilization, Fluidity, Mechanical Properties, and Water Absorption of Foam Concrete. Buildings 2024, 14, 3550. [Google Scholar] [CrossRef] [Scilit]
- Liu, Z.; Zhao, K.; Hu, C.; Tang, Y. Effect of water-cement ratio on pore structure and strength of foam concrete. Adv. Mater. Sci. Eng. 2016, 2016, 9520294. [Google Scholar] [CrossRef] [Scilit]
- Gao, Z.; Chen, B.; Chen, J.; Yuan, Z. Pore structure and mechanical properties of foam concrete under freeze-thaw environment. Acta Mater. Compos. Sin. 2024, 41, 827–838. [Google Scholar]
- Zhang, Z.; Zhang, Y.; Ye, G.; Zhang, S.; Shen, H.; Chen, Y. Strength degradation of foamed lightweight soil due to chemical erosion and wet-dry cycle and its empirical model. Materials 2023, 16, 6505. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Qin, L.; Zheng, L.; Guo, C.; Shao, Z.; Mou, C.; Zhang, X. Study on preparation and properties of alkali-activated foamed concrete. Processes 2025, 13, 64. [Google Scholar] [CrossRef] [Scilit]
- Li, L.S.; Wang, Y.; An, M.Z.; Yu, P.Y.; Hou, X. The influence of rehydration on the properties of Portland cement-based materials with low water/binder ratios: A review of existing research. Materials 2023, 16, 970. [Google Scholar] [CrossRef] [Scilit] [PubMed]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.