Abstract
The present work investigated the thermodynamic behaviors of oxygen in a liquid Fe–Ti alloy over a wide Ti concentration range of 11.6–71.2 wt% at 1873 K by integrating equilibrium experiments with thermodynamic modeling. To prevent excessive oxidation during the equilibrium experiments, the liquid alloys were equilibrated in a purified Ar atmosphere with an oxygen partial pressure below ~10−20 atm. Two quenching methods—furnace quenching with He gas injection and water quenching via quartz tube suction—were employed to evaluate the effect of cooling rate on total oxygen measurements. While He gas quenching led to higher measured oxygen contents owing to the formation of secondary Ti oxides, the quartz tube suction quenching method consistently yielded significantly lower oxygen values. The dissolved oxygen content increased with increasing Ti content. Electron probe microanalysis identified TiO as a stable equilibrium oxide phase above 11.6 wt% Ti, which was characterized as a face-centered cubic (FCC) rock-salt structure via electron backscatter diffraction analysis. Based on these results, a thermodynamic assessment of oxygen behavior in a liquid Fe–Ti alloy in equilibrium with TiO was performed for the first time using a modified quasichemical model. Consequently, the present model successfully reproduced the Ti–O relationship in the liquid Fe–Ti alloy across both the high-Ti concentration region saturated with TiO and the low-Ti concentration region saturated with Ti2O3 and Ti3O5.
1. Introduction
The commercial production of Ti metal has historically relied on techniques such as the Kroll process, an indirect production process utilizing a chloride feed. Along with issues such as low productivity, high electrical energy consumption, and large-scale production difficulties, the extremely strong affinity between Ti and O hinders the development of efficient extraction technologies [1]. The large volume of Ti scrap generated during the manufacturing of Ti alloy parts, Fe-contaminated Ti sponges, and in-house Ti-containing by-products can be low-CO2-emission Ti sources. After blending with sponge Ti, the Ti sources are recycled to form ferrotitanium using vacuum arc remelting and induction melting technologies [2]. The production of high-purity Ti and ferrotitanium alloys requires a fundamental understanding of oxygen solubility and the influence of Fe in Ti-rich melts. However, thermodynamic data and the assessment of oxygen in the high-Ti region of the Fe–Ti system are limited.
The addition of Ti to molten iron significantly influences the oxygen solubility, thereby governing the oxygen partial pressure equilibrated at the interface with the generated oxide phase. Depending on the and Ti concentration, Ti ions undergo stepwise reduction from tetravalent (Ti4+) to trivalent (Ti3+) and finally to divalent (Ti2+) states [3], causing the evolution of the oxide phase from Ti3O5 through Ti2O3 to TiO in equilibrium with the Fe–Ti melt at 1873 K. Most previous studies have focused on the low-Ti region of commercial steels or stainless steels saturated with Ti3O5 or Ti2O3 [4,5,6,7,8,9]. Previous studies primarily focused on titanium as a deoxidizer in conventional steelmaking, and thus their investigations were largely limited to the stability regions of Ti3O5 or Ti2O3 in dilute iron melts. However, for the ferrotitanium recycling and high-purity Ti alloy production, there is a critical need to understand the phase equilibria and oxygen behavior in highly concentrated Ti region. A few researchers measured the Ti–O relationship in equilibrium with TiO [10,11]. Hadley and Derge [10] pioneered the measurement of the equilibrium oxygen content in the high-Ti concentration range of Fe–Ti melts, up to approximately 46 wt% Ti at 1873 K. Using X-ray diffraction analysis, they observed the TiO phase to be the main equilibrium oxide above 5 wt% Ti in Fe–Ti melts. Cha et al. [11] investigated the Ti-O equilibria in Fe–Ti melts at 1873 K, extending the broad compositional spectrum from 4 ppm to 16.6 wt% Ti. They confirmed the stability of the cubic structure of TiO above 10.6 wt% Ti in Fe–Ti melts. Furthermore, according to Wagner’s formalism, the equilibrium relationship between Ti and O has been described up to approximately 5 wt% Ti melt in equilibrium with Ti2O3 [12]. Crucially, the conventional interaction parameter formalism is predicated on the infinite dilution of a liquid solution, and previous researchers could not apply Wagner’s formalism to a high-Ti concentration range, where TiO is the stable phase.
Establishing the optimal conditions for both Ti alloy extraction and ferrotitanium recycling requires precise thermodynamic data, including the Ti activity, oxygen partial pressure, and oxide phase stability in the high-Ti region. Therefore, this study investigated the thermodynamic behavior of oxygen in the TiO-saturated Fe–Ti melts over a wide Ti concentration range of 11.6–71.2 wt% at 1873 K. To ensure the accuracy of dissolved oxygen measurements, Fe–Ti alloy samples after equilibration were quenched via two methods: blowing highly purified He gas into the alloy sample and rapid water-quenching following quartz tube suction. Based on the experimental results, a thermodynamic assessment of the Fe–Ti–O phase at 1873 K was conducted using a modified quasichemical model (MQM) [13,14]. By integrating the optimized parameters for the Fe–Ti and Ti-O binaries with previous Fe–O data [15], the effects of temperature and Ti concentration on the equilibrated oxygen partial pressure in the Fe–Ti–O ternary system were evaluated over the entire liquid composition spectrum, ranging from pure Fe to pure Ti.
2. Experimental Procedures
At 1873 K, the equilibrium oxygen content in the Fe–Ti melt was experimentally determined over a high-Ti concentration range of 11.6 to 71.2 wt%. As shown in Figure 1, 300 g of the pre-melted Fe–Ti alloy was prepared using high-purity Fe (purity: 99.9%, JITECH&KOREA, Incheon, Republic of Korea), and Ti (purity: 99.99%, RNDKOREA, Gwangmyeong, Republic of Korea) was charged in a TiO-lined MgO crucible to acquire equilibrium data under TiO saturation (purity: 99.9%, RNDKOREA, Gwangmyeong, Republic of Korea). In preliminary experiments, the initial oxygen content of the pre-melted master alloys was forcibly controlled below the equilibrium oxygen content by blowing them with an Ar–3%H2 gas mixture. Thermal equilibration was achieved within 2 h using a high-frequency induction furnace (ELTek HF20K30CH, 20 kW and 30 kHz). To ensure a constant melting temperature, a B-type thermocouple protected by a magnesia tube was immersed directly in the liquid phase. To ensure uniform temperature distribution in the melt, the reaction crucible was positioned inside a graphite crucible and further encased in a porous alumina insulator.
Figure 1.
Schematic of the experimental system.
To suppress the excessive generation of Ti oxide inclusions during the equilibrium experiments, the atmosphere in the quartz reaction tube was maintained at 0.001 m3/min under a high-purity Ar flow. To establish a highly reducing atmosphere, a subfurnace with high-purity Ti sponge (99.9%) was heated to 1173 K. As shown in Figure 2, the content of the gas mixture rapidly dropped below 10−20 atm and stabilized within 1 h. The gas flow rate was maintained at 0.001 m3/min using a mass flow controller (MFC, KOFLOC, Kyoto, Japan). After reaching the desired melting temperature of 1873 K, the gas mixture was switched to high-purity Ar (purity level 5). Even though the gradually increased over time by the removal of oxygen from the Ar gas and oxidation of the outer layer of the sponge Ti, the was maintained at approximately 10−20 atm for 300 min. The in the outlet gas was measured using a zirconia oxygen sensor (TB-IIF -R, Daiichi Nekken, Ashiya, Japan) (Daiichi Nekken TB-IIF and monitored during the equilibrium experiments. Because the reaction time of the equilibrium experiment in this study was 2 h (120 min), re-oxidation of the melts by purified Ar gas was prevented in all experiments.
Figure 2.
Changes in log in the off-gas and temperature of Fe–Ti melts over time.
The total oxygen content and microstructure of the equilibrated samples were compared between the two cooling methods: inert gas injection into the furnace and silica tube suction, followed by water quenching. Helium gas was directly injected through a stopper hole at the top of the furnace. After blowing gas for 10 min to cool the heated graphite outer crucible, the melted alloy was completely solidified. In contrast, the alloy sample was suction sampled into a quartz tube and immediately quenched in water, with the entire transfer process completed in less than 5 s. To ensure an accurate bulk composition, the solidified samples were carefully sectioned for chemical analysis, and the surface oxide scales were removed by grinding and polishing. The overall oxygen concentration in the metal samples was measured using an N/O analyzer (ON-900ELTRA, Haan, Germany) based on inert gas fusion infrared absorptiometry. Additionally, inductively coupled plasma atomic emission spectroscopy (ICP-AES, Optima 5300 DV, Perkin Elmer Ltd., Waltham, MA, USA) was used to quantify the Ti content in the alloy. The boundary between the metallic phase, titanium oxides, and the generated inclusions was characterized using an electron probe microanalyzer (EPMA, JEOL JXA-8100, JEOL, Tokyo, Japan). High-accuracy quantitative data were obtained using wavelength-dispersive spectrometersof EPMA, which provide high-energy resolution. The crystal structures of the equilibrium oxide and alloy phases were identified using Kikuchi patterns generated by electron backscatter diffraction (EBSD; S-4300SE, HITACHI, Tokyo, Japan).
3. Thermodynamic Model for Fe–Ti–O Ternary System
Thermodynamic assessment of the equilibrium oxygen content in Fe-M melts requires the ternary solution model (Fe-M-O system), especially for alloying elements ‘M’ that exhibit a strong affinity for oxygen.
In this study, the Ti–O relationship was thermodynamically analyzed using MQM to consider the significant interatomic attraction between Ti and O, which was modeled as short-range ordering (SRO) in the molten Fe–Ti–O alloy. The essential Gibbs energies for the various titanium oxide phases were obtained from the NIST-JANAF database [16]. FactSage8.2 thermochemical software was employed to perform simulations of the Fe–Ti–O ternary system [17]. The thermodynamic framework for ternary liquid solutions was previously established and validated for the Fe-Al-O system [15], providing a theoretical basis for current simulations of Fe–Ti–O ternary systems. By adopting the exchange reaction of pairs for alloying elements of Ti shown below, SRO was evaluated as a number of Ti–O pairs as determined by the negative formation energy required for the establishment of Ti–O pairs in the melt. In the present study, the exchange reactions of the three pairs of Fe–Ti–O ternary solutions are described as follows:
In these equations, (i-j) and ∆gij mean the first-nearest neighbor pair and the changes in formation energy of (i-j) pairs, respectively.
For the Fe–Ti–O liquid phase, the ternary Gibbs energy is formulated as follows:
where ni, nj, and nij represent the molar quantities of i, j, and the (i-j) pair, respectively. The standard Gibbs energies for the pure components (, , and ) were obtained from the Scientific Group Thermodata Europe database [18]. In Equation (4), , the configurational entropy of mixing, is defined based on the random distribution of (i-i), (j-j) and (i-j) pairs in Equations (1)–(3). The approximate term for the nonideal configuration entropy caused by SRO is as follows:
where Xi, Xj, and Xij denote the mole fractions of i, j, and (i-j) pairs, respectively, and Yi represents the fraction of the coordination equivalents of element i. The relationship among the coordination equivalent fraction, mole fraction, and coordination number () obeys the following equation:
In the MQM, can have a composition dependence in each binary i-j system based on the following equation:
In this expression, and indicate the values for configurations in which element i is surrounded by i and j neighbors, respectively. In the present thermodynamic modeling, the coordination numbers were set to 6 for pure species (, , and ) and Fe–Ti solution (, ), whereas a value of 2 was applied to the Fe–O solution ( and ) and Ti-O solution ( and ) to describe the SRO between the metal and oxygen atoms.
In the present study, the thermodynamic parameters, and , in Equation (4) were refined to achieve the best fit with the experimental Ti–O relationship in the Fe–Ti melt. The optimized values are provided in Table 1. The value of was adopted from the previous work [15] on the sub-binary of the Fe–Al–O system. For the Fe–Ti–O system, the parameter is formulated as a function of pair fractions as follows:
where modifies the total Gibbs energy of the molten Fe–Ti system, whereas and primarily affect the Henrian activity coefficients in the Fe- and Ti-rich corners, respectively. To fine-tune the ternary Gibbs energy, the ternary parameter was incorporated into Equation (10). The parameters established in this study are listed in Table 1. Furthermore, to ensure thermodynamic consistency across the entire Fe–Ti phase diagram, the interaction parameters for the solid phases were optimized. The parameters of solid phases established in this study are listed in Table 2.
Table 1.
Fitting parameters optimized or used for the Fe–Ti–O ternary liquid alloy in the present study (J/mol).
Table 2.
Fitting parameters optimized or used for the solid phases of the Fe–Ti system in the present study (J/mol).
4. Results and Discussions
4.1. Measurement of Ti–O Relationship in Fe–Ti Alloy Melt
Figure 3 shows images of the pre-melted master alloy with 50 wt% Ti and Fe–Ti alloy samples obtained by He gas injection and quartz tube suction. As shown in Figure 3A, the cross-sectional views of the pre-melted master alloy are very clear, whereas the cross-sectional views (Figure 3B) of the Fe–Ti alloy obtained by He gas injection show relatively darker Ti oxide phases distributed throughout almost the entire metal phase. The Fe–Ti alloy obtained by quartz tube suction in Figure 3C reveals that the oxide phase was distributed in a localized portion of the metal phase. The oxygen content in the alloy obtained via quartz tube suction was measured while carefully avoiding the oxide phase to ensure analysis of the dissolved oxygen.
Figure 3.
Photo images of the Fe–Ti alloy samples: (A) pre-melted master alloy with 50 wt% Ti, (B) Fe–Ti alloy obtained by He gas injection, and (C) by quartz tube suction. The circle in Figure (B) indicates the observed Ti oxide phases.
Figure 4 compares the oxygen content in the Fe–Ti metal phase measured using the two quenching methods with those reported in previous studies [10,11]. The measured Ti and O contents are listed in Table 3. The equilibrium state of Ti deoxidation within the Fe–Ti system can be represented by the relationship between the dissolved Ti and O contents in equilibrium with the solid Ti oxide. As mentioned earlier, the stability of various Ti-oxide phases, including Ti3O5, Ti2O3, and TiO, is determined by the Ti content of liquid Fe. This dependence arises because the Ti levels modulate the oxygen partial pressure at the phase boundary, thereby altering the valence states of the Ti species. Ti2+ ions are enhanced within the Ti-rich phase owing to the low , therefore the Fe–Ti–O melt achieves equilibrium with the TiO phase. Hadley and Derge [10] and Cha et al. [11] measured the solubility product of TiO above 10 wt% Ti in liquid Fe at 1873 K. Their data correlate well with each other, as indicated by the open symbols and dotted lines in Figure 4. Experimental data from previous literature at lower Ti concentrations (below approximately 10 wt% Ti) obtained under Ti2O3 or Ti3O5 saturated conditions are excluded from this figure.
Figure 4.
Influence of Ti concentration on the oxygen concentration in Fe–Ti sample at 1873 K. Results from two quenching methods in the present study (in equilibrium with TiO above 11.6 wt.% Ti) are compared with literature data [10,11]. Experimental data from previous literature at lower Ti concentrations (below approximately 10 wt% Ti) correspond to Ti2O3 or Ti3O5 saturated conditions.
Table 3.
Experimental results of equilibrium Ti and O contents in the Fe–Ti melt at 1873 K.
Regarding the liquid phase, the variation in dissolved oxygen concentration in the high-Ti region is fundamentally governed by the strong attractive interaction between Ti and O atoms. This affinity leads to significant Ti–O short-range ordering (SRO) in the melt, where oxygen atoms are preferentially surrounded by Ti atoms rather than Fe atoms. This SRO effects thermodynamically stabilizes oxygen in the liquid phase and lowers the activity coefficient of dissolved oxygen (γO) [9]. Consequently, at high-Ti concentrations, the depressed γO allows the liquid melt to increase a concentration of dissolved oxygen to maintain equilibrium with the stable oxide phase, resulting in the observed increase in oxygen solubility shown in Figure 4.
In this study, the equilibrium oxygen content was measured at approximately 50 wt% Ti to validate the high-Ti content region data originally reported by Hadely and Derge [10]. As mentioned in the experimental section, the equilibrated alloy melts were quenched in a furnace via He gas injection and in water via quartz tube suction. The oxygen content of the sample quenched in the furnace is represented by the gray circle in Figure 4. This result is in good agreement with the reported data for an Fe–46 wt% Ti alloy. In contrast to the data from Hadely and Derge and the furnace-quenched results, the oxygen content of the suction-quenched sample, plotted as a solid circle, was significantly lower. This pronounced discrepancy is presumably attributable to the excessive oxide formation during cooling and solidification, as shown in Figure 3.
To clarify the dependence of oxide formation on the cooling rate, the microstructure of each sample obtained by different quenching methods was observed using EPMA, as shown in Figure 5. The quantitative analysis data are presented in Table 4. A thick oxide layer was observed to form on the furnace-quenched sample indicated as phase ‘1’ in Figure 5A. The dark oxide phase was characterized as TiO with a small deviation from the stoichiometric equimolar ratio of Ti and O. The dark oxide phase can be expressed as a TiO0.91 solid solution with the lack of oxygen arising from the stoichiometry of the vacancy fraction in the oxygen sublattice of the δ-TiO structure [19]. During the solidification of the remaining liquid alloy, phase separation occurred by forming a Laves phase, Fe2Ti (phase ‘3’) in the matrix of the FeTi compound (phase ‘2’). In contrast, the phase separation and oxide formation were minimized by rapid suction quenching, as shown in Figure 5B. Phase ‘4’ reflects the TiO inclusions formed during water quenching by suction. Compared to phase ‘1’ in Figure 5A, rapid cooling and solidification dramatically decreased oxide formation in the matrix phase ‘5’ FeTi compound. Although the Fe content in phase ‘4’ was measured as 10.3 wt% by quantitative analysis in Table 4, this value could result from a background effect due to the small size of the inclusion in the metal phase. The rapid quenching method led to a reduction in phase separation, but the solute-enriched FeTi2 phase (phase ‘6’) remained, as did the FeTi matrix. The higher oxygen content of the furnace-quenched samples can be attributed to the extensive formation of TiO owing to the insufficient cooling rate compared with that of the suction-quenched samples. Thus, in the present study, the equilibrium oxygen content data for a wide range of Ti concentrations (10–70 wt%) were precisely established by employing the rapid quenching method in water.
Figure 5.
Cross-section of the Fe–Ti samples with 50 wt% Ti obtained via (A) the furnace-quenching (40× magnification) and (B) suction-quenching (100× magnification) using EPMA. The numbers in the figures indicate the specific spots where EPMA analysis was conducted as shown in Table 4.
Table 4.
Compositions of the observed phases in Figure 5 (units: wt%).
The crystallographic information of the suction-quenched samples was analyzed using EBSD, as shown in Figure 6. As shown in Figure 6A, the oxide particles formed in the Fe–50 wt% Ti alloy were TiO, and the alloy was confirmed to be in the FeTi phase. The formed TiO oxide inclusions (~40 μm) adopt a NaCl-type rock-salt structure, where the face-centered cubic (FCC) arrangement uses Kikuchi patterns. These inclusions can be clearly distinguished from the FeTi base metal, which has a body-centered cubic (BCC) structure. The δ-TiO structure of the inclusions was observed for all water-quenched samples above 11.63 wt% Ti in the Fe–Ti alloys. As previously mentioned, Cha et al. [11] reported that the equilibrium Ti-oxide phase of an Fe–Ti melt can be transformed into Ti3O5, Ti2O3, and TiO by increasing the Ti concentration in liquid iron. The TiO inclusions observed at Ti concentrations higher than 10.6 wt% were characterized as NaCl-type cubic structures via EBSD analysis. This observation is in good agreement with the experimental results reported for Ti-rich domains. Since no α-Ti2O or β-TiO3 phases were detected in the present study, we concluded that the high-Ti-containing Fe–Ti alloy melt was in equilibrium with pure solid TiO under the unit activity of TiO.
Figure 6.
Results of EBSD analysis of the water suction-quenched Fe–50 wt% Ti alloy: (A) phase map and (B) EBSD patterns.
4.2. Thermodynamic Analysis of Ti–O Relationship in Fe–Ti Alloy Melt
Figure 7 shows the phase equilibria of the Fe–Ti system calculated using MQM with previous experimental results [20,21,22,23,24,25,26,27,28]. As shown in Figure 7, the simulated results (solid line) exhibit a high degree of consistency with the experimental data points over the full concentration range from the Fe-rich and Ti-rich side [20,21,22,23,24,25,26,27,28]. Precise modeling of the liquid-phase stability of the Ti-rich region is essential for accurately predicting the deoxidation equilibria within the Fe–Ti–O melt. Because the deoxidation behavior of Ti is highly sensitive to Ti activity in liquid Fe, establishing the accuracy of the Fe–Ti binary system is integral to the overall reliability of the ternary model. Therefore, the accuracy of the model in the Ti-rich region was confirmed by analyzing the mixing enthalpies and activity.
Figure 7.
Comparison of the presently calculated Fe–Ti phase diagram with the experimental and calculated data reported in the literature [20,21,22,23,24,25,26,27,28].
The calculated integral and partial enthalpies of the Fe–Ti liquid phase, denoted by the solid lines in Figure 8 were initially validated against previously reported experimental data [27,28,29,30,31]. This validation established an essential baseline for ensuring the reliability of the parameters before calculating the Fe–Ti–O ternary deoxidation curves. Because the stability of the liquid phase in the Ti-rich region directly dictates the oxygen content in molten Fe–Ti, ensuring the accuracy of the Fe–Ti binary system is a necessary condition for ternary modeling.
Figure 8.
Integral enthalpies of mixing for the liquid Fe–Ti system: comparison between the current MQM calculations and literature data [27,28,29,30,31].
Figure 8 shows the integral enthalpy of mixing calculated using MQM in the liquid Fe–Ti phase. The MQM-predicted curves (solid line) are consistent with the experimental measurements reported by Thiedemann et al. [29], particularly in the composition range of XTi < 0.5. The mixing enthalpy curve shows a minimum value of approximately −19 kJ/mol around XTi = 0.45. While previous studies [27,28] provided enthalpy calculations for the XTi = 0.4–0.6 region, the present calculation more accurately determined the enthalpy minimum, as reported in experimental measurements [29,30,31].
Figure 9 presents the partial enthalpies of mixing for the liquid Fe–Ti system calculated using the MQM compared with previously reported data [27,28,32]. Although previous research using the regular solution model produced insufficiently consistent predictions for the partial enthalpy in the high-Fe region [27,28] and lacked experimental validation in the high-Ti region, the present MQM results demonstrated good agreement with the experimental data reported by Esin et al. [32].
Figure 9.
Partial enthalpies of mixing for the liquid Fe–Ti system: comparison between the current MQM calculations and literature data [27,28,32].
Figure 10 reveals the activities of the Fe–Ti melt at 1873 K by comparing the current MQM calculations with both experimental and predicted data from the literature [27,28,33]. The presently calculated activity curves exhibit slightly more positive values in the range of XTi = 0.5 to 0.7 compared to the results reported in previous studies [27,28]. Furthermore, the current calculations aligned more closely with the experimental results obtained via Knudsen cell-mass spectrometer measurements [33], particularly within the high-Ti concentration range (XTi = 0.7 to 0.9).
Figure 10.
Comparison of the calculated activities of Fe and Ti in the liquid Fe–Ti system at 1873 K using the MQM with reported experimental and calculated data from the literature [27,28,33].
Figure 11 compares the presently predicted (MQM) and measured deoxidation equilibria of Ti in a liquid Fe–Ti-O melt at 1873 K with the results from Wagner’s formalism and Japan Society for the Promotion of Science (JSPS) data [34], as well as other literature data [4,5,6,7,8,9,10,11]. Based on Wagner’s formalism, the JSPS provides a set of suggested interaction parameters for Ti and O derived from previous studies to describe the deoxidation equilibrium of Ti in dilute liquid iron [34]. According to Wagner’s formalism and the suggested JSPS parameters, the calculated Ti–O relationship in the liquid Fe–Ti-O system is represented by the dashed line in Figure 11 for comparison with experimental literature data. Although the reported Ti deoxidation data are significantly scattered, the predicted deoxidation curve can describe the variation in O solubility in Fe–Ti melts as a function of Ti concentration under Ti3O5 and Ti2O3 saturation conditions [4,5,6,7,8,9,10,11]. However, the thermodynamic equilibrium between TiO and liquid iron has not been established in previous studies owing to the mathematical limitations of the dilute solution model. As shown in Figure 11, calculating the equilibrium without accounting for the Gibbs energy of TiO dissolution, even when using the JSPS-recommended high-order interaction parameters, resulted in an impossible local maximum in the predicted oxygen content near the TiO saturation condition.
Figure 11.
Equilibrium relationship between Ti and O in a liquid Fe–Ti-O melt at 1873 K under oxide saturation conditions. The small vertical solid lines indicate the boundaries between the stability regions of Ti3O5, Ti2O3, and TiO: comparison of the current results (calculations and measurements) with Wagner’s formalism [34] and literature data [4,5,6,7,8,9,10,11].
In the present study, TiO was determined to be the equilibrium solid oxide phase within the Ti concentration range of 11.63–71.19 wt% in the Fe–Ti melt at 1873 K. To achieve a high degree of agreement with the Ti-rich experimental data, the following standard Gibbs free energy of formation for pure solid TiO was obtained from the NIST-JANAF thermochemical tables [16] and directly incorporated into the thermodynamic calculations.
The Ti–O relationship at low-Ti concentrations was calculated based on the thermodynamic data of Ti3O5 and Ti2O3 from NIST-JANAF [16] as follows:
The standard Gibbs energies for the formation of titanium oxides, presented in Equations (11)–(13) represent the chemical potentials of oxygen in the oxide saturation region. These equations were simultaneously incorporated with the liquid Fe–Ti–O solution properties calculated using the MQM to calculate the Ti deoxidation equilibria in liquid iron.
The thermodynamic characteristics of the molten Fe–Ti–O system were modeled using MQM by combining the parameters from their respective binary subsets: Fe–O [15], Fe–Ti, and Ti–O systems. The Ti deoxidation equilibria in the Fe–Ti–O ternary system were modeled based on the calculated Fe–Ti binary parameters (Figure 7, Figure 8, Figure 9 and Figure 10). Measuring the liquid properties of pure Ti alloy melts is difficult because of the large amount of fumes generated above the melting point of Ti (1941 K). The oxygen solubility within the Ti–O binary system was derived via extrapolation by correlating the binary behavior with the measured observations of the ternary Fe–Ti–O melt. Based on the Ti–O relationships observed in the Ti-rich molten Fe–Ti system, the Gibbs energy change for the Ti–O pair exchange reaction was calculated at 1873 K. Unit activity of TiO was assumed within the Ti-rich domain (11.63–71.19 wt%), primarily because FeO exhibits insignificant solubility under a strong reduction condition characteristic of this system [35].
While Wagner’s formalism and the JSPS data are applicable only to dilute solutions, the present MQM calculations provide a thermodynamic description over the entire Ti concentration range. As shown in Figure 11, the model calculation (solid line) under the TiO-saturated condition shows good correlation with the lower-level oxygen content data, including the regions of Ti3O5 and Ti2O3 saturation [4,5,6,7,8,9]. In general, a lower oxygen content is preferred for dissolved O data because O analysis data can be easily overestimated by insoluble O from suspended oxide inclusions. Therefore, our model calculations were conducted to fit the lower level of oxygen content among the experimental results in the high-Ti concentration region saturated with TiO.
Figure 12 shows the predicted Ti–O relationship and equilibrium oxygen partial pressure in the molten Fe–Ti system at temperatures varying from 1673 to 1973 K. Since the present optimization was conducted based on the experimental data at 1873 K, the model parameters for the interactions involving oxygen, specifically and values, were assumed to be temperature-independent and kept constant at their 1873 K values for the calculations at other temperatures shown in Figure 12. As shown in Figure 12A, the relationship between the dissolved oxygen and Ti content indicates that the oxygen solubility at a constant Ti concentration is significantly enhanced by increasing the temperature. The high dissolved oxygen content in the Ti-rich region led to the formation of numerous TiO inclusions during cooling. Figure 12B presents the equilibrium oxygen partial pressure as a function of the Ti content and temperature. In the Ti-rich region at 1873 K, the equilibrium decreased to as low as 10−20 atm; consequently, oxidation of the melt could not be completely avoided despite the application of vacuum and Ar blowing. As shown in Figure 12, appropriate process conditions can be predicted by tracking the oxygen solubility limit and its temperature dependence, providing a practical guide for oxygen control in Fe–Ti melts.
Figure 12.
Influence of temperature and Ti concentration on (A) the oxygen solubility and (B) the equilibrium oxygen partial pressure in the liquid Fe–Ti-O system.
5. Conclusions
To establish the deoxidation equilibria in the molten Fe–Ti–O system, the dissolved oxygen content and the stable oxide phases in Ti-rich iron melts were investigated at 1873 K across a wide Ti concentration range (11.6–71.2 wt%). Experimentally, the study refined dissolved oxygen measurements by employing a rapid suction-quenching method, which successfully minimized inclusion formation compared to in situ He gas injection quenching. Theoretically, a modified quasi-classical model (MQM) was applied to describe the nonideal behavior of the Fe–Ti–O ternary system, integrating the stability of various titanium oxides into a consistent predictive model. The following results were obtained:
- (1)
- The quartz tube suction-quenching method significantly reduced oxygen pickup and secondary inclusion formation compared to in situ He gas injection quenching, providing more reliable dissolved oxygen values in Fe–Ti melts. The discrepancy in the high-Ti oxygen solubility data was resolved by demonstrating that the previously reported high values resulted from insufficient cooling rates, which led to excessive inclusion formation during solidification.
- (2)
- For alloys with Ti > 11.6 wt%, TiO was identified as the stable equilibrium oxide phase. The EBSD analysis and Kikuchi patterns confirmed the NaCl-type rock-salt (FCC) structure of the TiO inclusions, which was clearly distinguished from the Fe–Ti matrix (BCC).
- (3)
- By incorporating the ternary parameter ( into Equation (10), MQM was successfully implemented to resolve complex Ti–O interactions in nondilute Fe–Ti solutions. The accuracy of the Fe–Ti binary system was validated using phase diagrams and enthalpy calculations, ensuring precise descriptions of the Fe and Ti activities. The model successfully integrated the TiO, Ti2O3, and Ti3O5 stability regions, providing consistent deoxidation equilibria across the entire compositional range of the molten Fe–Ti–O system.
In this study, the oxygen solubility limit was established as a function of Ti concentration, providing a critical guideline for deoxidation practices in high-Ti steels and superalloys. Furthermore, the developed MQM parameters serve as a baseline for calculating the deoxidation curves and equilibrium oxygen partial pressure, facilitating future simulations of pure titanium production and high-alloy refining.
Author Contributions
Conceptualization, Y.-W.K., M.-K.P. and S.-J.K.; validation, Y.-W.K., M.-K.P. and S.-J.K.; investigation, Y.-W.K. and S.-J.K.; data curation, Y.-W.K. and M.-K.P.; writing—original draft preparation, Y.-W.K. and M.-K.P.; writing—review and editing, Y.-W.K., M.-K.P. and S.-J.K.; visualization, Y.-W.K. and M.-K.P.; supervision, S.-J.K.; project administration, S.-J.K.; funding acquisition, S.-J.K. All authors have read and agreed to the published version of the manuscript.
Funding
This research was funded by the Korea Institute of Energy Technology Evaluation and Planning and the Ministry of Trade, Industry, and Energy of the Republic of Korea (grant number: 20212010100060). This work was supported by the National Research Foundation of Korea (NRF) grant funded by the Korean Government (MSIT) (No. RS-2025-02233037).
Data Availability Statement
The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding authors.
Acknowledgments
During the preparation of the present manuscript, the authors used Gemini 3.1 Pro for checking grammatical errors. After using this tool, the authors reviewed and edited the content as needed and takes full responsibility for the content of the publication.
Conflicts of Interest
The authors declare no conflicts of interest.
References
- Takeda, O.; Ouchi, T.; Okabe, T.H. Recent Progress in Titanium Extraction and Recycling. Metall. Mater. Trans. B 2020, 51, 1315–1328. [Google Scholar] [CrossRef] [Scilit]
- Sohn, H.-S. Current status of titanium recycling technology. Resour. Recycl. 2021, 30, 26–34. [Google Scholar] [CrossRef] [Scilit]
- Paek, M.-K.; Jang, J.-M.; Jo, J.-O.; Holappa, L.; Pak, J.-J. Aluminum-titanium complex deoxidation equilibria in Fe-Cr-Al-Ti-O melts. Metall. Mater. Trans. B 2021, 52, 236–244. [Google Scholar] [CrossRef] [Scilit]
- Smellie, A.; Bell, H. Titanium deoxidation reactions in liquid iron. Can. Metall. Q. 1972, 11, 351–361. [Google Scholar] [CrossRef]
- Janke, D.; Fischer, W. Deoxidation equilibria of Ti, Al and Zr in Fe melts at 1600 °C. Arch. Eisenhuttenwes. 1976, 47, 195–198. [Google Scholar]
- Kojima, Y.; Inouye, M.; Ohi, J.I. Titanoxyd im Gleichgewicht mit Eisen-Titan-Legierungen bei 1600 °C. Arch. Eisenhuttenwes. 1969, 40, 667–671. [Google Scholar] [CrossRef] [Scilit]
- Pak, J.-J.; Jo, J.-O.; Kim, S.-I.; Kim, W.-Y.; Chung, T.-I.; Seo, S.-M.; Park, J.-H.; Kim, D.-S. Thermodynamics of titanium and oxygen dissolved in liquid iron equilibrated with titanium oxides. ISIJ Int. 2007, 47, 16–24. [Google Scholar] [CrossRef] [Scilit]
- Yoshikawa, T.; Morita, K. Influence of alloying elements on the thermodynamic properties of titanium in molten steel. Metall. Mater. Trans. B 2007, 38, 671–680. [Google Scholar] [CrossRef] [Scilit]
- Fruehan, R. Activities in liquid Fe–Al–O and Fe–Ti–O alloys. Metall. Mater. Trans. 1970, 1, 3403–3410. [Google Scholar] [CrossRef] [Scilit]
- Hadley, R.; Derge, G. Equilibrium between titanium in liquid iron and titanium oxides. JOM 1955, 7, 55–60. [Google Scholar] [CrossRef] [Scilit]
- Cha, W.-Y.; Miki, T.; Sasaki, Y.; Hino, M. Identification of titanium oxide phases equilibrated with liquid Fe–Ti alloy based on EBSD analysis. ISIJ Int. 2006, 46, 987–995. [Google Scholar] [CrossRef] [Scilit]
- Wagner, C.; Mellgren, S.; Westbrook, J.H.; Cohen, M. Thermodynamics of Alloys; Addison-Wesley: Cambridge, MA, USA, 1952. [Google Scholar]
- Pelton, A.D.; Degterov, S.A.; Eriksson, G.; Robelin, C.; Dessureault, Y. The modified quasichemical model I—Binary solutions. Metall. Mater. Trans. B 2000, 31, 651–659. [Google Scholar] [CrossRef] [Scilit]
- Pelton, A.D.; Chartrand, P. The modified quasi-chemical model: Part II. Multicomponent solutions. Metall. Mater. Trans. A 2001, 32, 1355–1360. [Google Scholar] [CrossRef] [Scilit]
- Paek, M.-K.; Pak, J.-J.; Kang, Y.-B. Aluminum deoxidation equilibria in liquid iron: Part II. Thermodynamic modeling. Metall. Mater. Trans. B 2015, 46, 2224–2233. [Google Scholar] [CrossRef] [Scilit]
- Chase, M.W. NIST-JANAF Thermochemical Tables 4th ed. J. Phys. Chem. Ref. Data 1998, 6, 1529–1564. [Google Scholar]
- Bale, C.W.; Bélisle, E.; Chartrand, P.; Decterov, S.; Eriksson, G.; Hack, K.; Jung, I.-H.; Kang, Y.-B.; Melançon, J.; Pelton, A.; et al. FactSage thermochemical software and databases—Recent developments. Calphad 2009, 33, 295–311. [Google Scholar] [CrossRef] [Scilit]
- Dinsdale, A.T. SGTE data for pure elements. Calphad 1991, 15, 317–425. [Google Scholar] [CrossRef] [Scilit]
- Cao, Z.; Xie, W.; Jung, I.-H.; Du, G.; Qiao, Z. Critical evaluation and thermodynamic optimization of the Ti-CO system and its applications to carbothermic TiO2 reduction process. Metall. Mater. Trans. B 2015, 46, 1782–1801. [Google Scholar] [CrossRef] [Scilit]
- Hellawell, A.; Hume-Rothery, W. The constitution of alloys of iron and manganese with transition elements of the first long period. Philos. Trans. R. Soc. London. Ser. A Math. Phys. Sci. 1957, 249, 417–459. [Google Scholar] [CrossRef] [Scilit]
- Booker, P. Ternary Phase Equilibria in the Systems Ti-Fe-C, Ti-Co-C and Ti-Ni-C; Oregon Graduate Center: Beaverton, OR, USA, 1979. [Google Scholar]
- Ko, M.; Nishizawa, T. Effect of magnetic transition on the solubility of alloying elements in alpha iron. J. Jpn. Inst. Met. 1979, 43, 118–126. [Google Scholar] [CrossRef] [Scilit]
- Murakami, Y.; Kimura, H.; Nishimura, Y. An investigation on the titanium–iron–carbon system. Trans. Nat. Res. Inst. Met. 1959, 1, 7–21. [Google Scholar]
- Kivilahti, J.; Tarasova, O. The determination of the Ti-rich liquidus and solidus of the Ti-Fe system. Metall. Trans. A 1987, 18, 1679–1680. [Google Scholar] [CrossRef] [Scilit]
- VanThyne, R.; Kessler, H.; Hansen, M. The systems titanium-chromium and titanium-iron. Trans. Am. Soc. Met. 1952, 44, 974–989. [Google Scholar]
- McQuillan, A. The application of hydrogen equilibrium-pressure measurements to the investigation of titanium alloy systems. J. Inst. Metals 1951, 79, 73. [Google Scholar]
- Jonsson, S. Assessment of the Fe–Ti system. Metall. Mater. Trans. B 1998, 29, 361–370. [Google Scholar] [CrossRef] [Scilit]
- Dumitrescu, L.; Hillert, M.; Sounders, N. Comparison of Fe-Ti Assessments. J. Phase Equilibria 1998, 19, 441. [Google Scholar] [CrossRef] [Scilit]
- Thiedemann, U.; Qin, J.; Schaefers, K.; Rösner-Kuhn, M.; Frohberg, M.G. Mixing enthalpy measurements of liquid Fe-Ti alloys by levitation alloying calorimetry and calculation of the thermodynamic properties of mixing. ISIJ Int. 1995, 35, 1518–1522. [Google Scholar] [CrossRef] [Scilit]
- Batalin, G.; Kurach, V.; Sudavtsova, V. Enthalpies of Mixing of Fe-Cr and of Fe-Ti Melts. Russ. J. Phys. Chem. 1984, 58, 289–291. [Google Scholar]
- Hai, W.; Lück, R.; Predel, B. Calorimetric determination of the enthalpy of mixing of liquid iron-titanium alloys. Int. J. Mater. Res. 1991, 82, 659–665. [Google Scholar] [CrossRef] [Scilit]
- Esin, Y.O.; Valishev, M.; Ermakov, A.; Geld, P.; Petrushevskii, M. Partial and integral enthalpy of mixing of liquid Fe−Ti alloys. Izv. Akad. Nauk. SSSR. Met. 1981, 3, 30–32. [Google Scholar]
- Furukawa, T.; Kato, E. Thermodynamics of binary liquid iron-titanium alloys by mass spectrometry. Trans. Iron Steel Inst. Jpn. 1976, 16, 382–387. [Google Scholar] [CrossRef] [Scilit]
- The Japan Society for the promotion of science. The 19th Committee on Steelmaking (1988) Steelmaking Data Sourcebook; Gordon and Breach Science Publisher: New York, NY, USA, 1988; pp. 38–45. [Google Scholar]
- Cha, W.-Y.; Miki, T.; Sasaki, Y.; Hino, M. Temperature dependence of Ti deoxidation equilibria of liquid iron in coexistence with ‘Ti3O5’and Ti2O3. ISIJ Int. 2008, 48, 729–738. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.