Skip to Content
MetalsMetals
  • Article
  • Open Access

23 November 2026

24 Pages

Fracture Morphology and In Situ Crack Growth in Q420 Steel Under Different Loading Conditions

,
,
,
,
,
and
1
Jiuquan Iron and Steel (Group) Co., Ltd., Jiayuguan 735100, China
2
State Key Laboratory of Advanced Processing and Recycling of Non-Ferrous Metals, School of Materials Science and Engineering, Lanzhou University of Technology, Lanzhou 730050, China
*
Author to whom correspondence should be addressed.
Metals2026, 16(12), 1287;https://doi.org/10.3390/met16121287 
(registering DOI)
This article belongs to the Section Metal Failure Analysis

Abstract

Q420 high-strength low-alloy steel serves as a structural material for wind turbine towers, and its deformation and fracture behaviors under different loading conditions are relevant to service safety. In this study, commercially produced hot-rolled Q420 steel was investigated. A series of mechanical tests were conducted, including uniaxial tensile tests at quasi-static strain rates of 0.0001–0.01 s−1, fracture tests on notched and nominal-shear specimens, in situ SEM tensile tests, axial fatigue tests, and room-temperature Charpy impact tests. Combined with EDS analysis of selected particles, the mechanical response and regional fracture morphologies were compared. Dimpled fracture dominated the displayed terminal tensile, impact, and fatigue-overload fields, accompanied by local shear-lip and tear-ridge features. Equiaxed and elongated dimples coexisted without a monotonic change in measured mean opening size. Particle-containing cavities showed local elemental enrichment. In situ cracks became visible after peak nominal stress and showed geometric path deflection. Fatigue propagation and final-overload regions were distinguished in the comparison with impact fracture. These findings provide experimental references for comparative fracture interpretation under the tested loading conditions.

1. Introduction

Q420 high-strength low-alloy steel possesses high load-bearing capacity and favorable plasticity, making it widely used in engineering structures such as wind turbine towers [1]. With the increase in structural size and the complexity of service loads, local stress concentration and cyclic loads have raised higher requirements for the steel’s fracture resistance [2,3]. The failure of steel not only depends on the strength level but is also closely related to the formation of local damage and the crack propagation process [4,5]. The fatigue fracture surface of Q420 base material also shows different stages such as crack initiation, stable propagation, and ultimate instability [6]. Therefore, clarifying the damage initiation and surface-crack evolution laws of Q420 steel under different load conditions is an important foundation for understanding its fracture failure behavior and comparative failure diagnosis.
The stress state is an important factor influencing the local plastic deformation and ductile fracture of steel [7,8]. Stress triaxiality (η) reflects the relative magnitude of hydrostatic stress to equivalent stress, while the Lode angle parameter describes the deviatoric stress state. Both of them affect the microvoid growth and shear failure [9,10]. The Johnson–Cook fracture model characterizes the fracture strain with variables such as stress triaxiality [9]. Li and Jing further combined the theory of microvoid growth with the shear failure condition to establish a structural steel fracture model that considers both stress triaxiality and Lode angle parameters [10]. Research on Q690 and Q960 steel also indicates that the initiation of fracture and damage evolution are related to the stress state [11,12]. At the same time, the nonuniformity of the microstructure will also change the distribution of local deformation [13]. Additionally, Vermeij and Hoefnagels [14] studied the plastic localization and damage of ferritic–pearlitic steel at the nanoscale using digital image correlation. Related research also revealed the local damage process near inclusions [15]. External loading and microstructure together govern the fracture mechanism of the steel [16]. However, the fracture laws of the aforementioned structural steels cannot be directly used to explain the local damage behavior of Q420 steel. Existing research on Q420 steel has involved constitutive relationships related to strain rate and fatigue performance [4,6]. Three key issues still need to be clarified. First, how notch constraint and shear loading alter dimple morphology and microvoid coalescence. Second, what particle-cavity associations and surface-crack paths are visible. Third, what differences exist in fracture characteristics between monotonic and cyclic loading. It is difficult to fully track the process from local deformation to crack formation and propagation based solely on macroscopic mechanical curves or the final fracture surface. Therefore, a combination of in situ observation and post-fracture characterization is necessary for comparative analysis.
In this study, commercially produced hot-rolled Q420 steel plate was used. Uniaxial tensile tests at different strain rates, tension tests with different notch radii, nominal single-shear and double-shear tests, in situ tension tests using scanning electron microscope (SEM), axial fatigue tests, and Charpy impact tests were conducted. Combined with microscopic structure observation, fractographic analysis, and energy-dispersive X-ray spectroscopy (EDS) characterization, the plastic deformation, dimple morphology, and crack paths under different loading conditions were compared. This work focuses on the correlation between fracture characteristics under notched and shear conditions and the local cracking process observed via in situ testing. It compares selected particle-containing cavities and regional fracture features under the tested loading modes. The opposite rankings of specimen-level fracture displacement and minimum-section contraction, together with the post-peak visible-crack sequence, provide complementary evidence for the fracture behaviors of Q420 steel.

2. Materials and Methods

2.1. Experimental Materials

Commercially produced hot-rolled Q420 steel plate with a thickness of 4 mm was used for the smooth tensile, nominal-shear, and axial-fatigue specimens. The round-notched bars were machined from thicker stock, and full-size Charpy specimens were prepared from a separate plate. The chemical composition was measured using a SPECTRO spark optical emission spectrometer (SPECTRO Analytical Instruments GmbH, Kleve, Germany), and the results for the 4 mm plate are presented in Table 1. Figure 1 and Figure 2 also describe this plate. Comparisons across different parent stocks are restricted to qualitative fracture features.
Table 1. Chemical composition of Q420 steel (mass fraction, wt%).
Figure 1. Q420 steel of (a) OM image, (b) enlarged view of the yellow-boxed region in (a), (c) enlarged view of the blue-boxed region in (b).
Figure 2. Q420 steel of (a) SEM micrograph, (b) enlarged view of a selected region in (a), (c) EDS spectrum and elemental composition of the region shown in (b).
The microstructure was examined by an Axio Scope 5 optical microscope (OM) (Carl Zeiss Microscopy GmbH, Jena, Germany) and an Axia ChemiSEM scanning electron microscope (SEM) (Thermo Fisher Scientific, Waltham, MA, USA). After mechanical grinding, the specimens were polished to a mirror finish and etched with a 4 vol% nitric-acid solution for 10 s before observation. The results showed a microstructure consisting of light-contrast ferrite and dark-contrast pearlite distributed along ferrite grain boundaries (Figure 1). The ferrite consisted predominantly of quasi-polygonal ferrite (QF) with curved or serrated grain boundaries, together with a small amount of acicular ferrite (AF) (Figure 2a,b). The EDS spectrum of the selected region is shown in Figure 2c.

2.2. Experimental Methods

2.2.1. Quasi-Static Uniaxial Tensile Tests and Tests on Notched and Nominal-Shear Specimens

Fracture surfaces were examined with the Axia ChemiSEM at 20 kV using an Everhart–Thornley detector in secondary electron mode, with working distances of approximately 10.9–22.2 mm. The Quanta 450 in situ SEM (Thermo Fisher Scientific, San Jose, CA, USA) was operated at 20 kV with an Everhart–Thornley detector and working distances of approximately 19.4–19.9 mm. The EDS point spectra were acquired at 20 kV for 115 and 59 s, respectively. The corresponding SEM images were recorded at working distances of approximately 11.9 and 16.9 mm.
Uniaxial tensile tests on smooth specimens, notched tensile tests, and tensile tests on nominal-shear specimens were all conducted using a WDW-100D electronic universal testing machine (Shandong Hairui Testing Instrument Co., Ltd., Jinan, China) equipped with an extensometer. The tensile loading direction was parallel to the rolling direction. Smooth specimens were tested under strain-rate control at three quasi-static strain rates of 0.0001, 0.001, and 0.01 s−1. Their geometries were designed in accordance with the Chinese National Standard “Metallic materials-Tensile testing-Part 1: Method of test at room temperature” (GB/T 228.1-2021) [17], as shown in Figure 3. Three specimens were tested at each rate.
Figure 3. Geometry and dimensions of the smooth tensile specimen (unit: mm).
Round-notched specimens were designed with notch radii of R = 2, 4, and 6 mm, designated NR2, NR4, and NR6. Shear specimens were categorized into single-shear and double-shear types. Nominal single-shear specimens with ligament inclinations α = 0° and 45° relative to a section transverse to loading were labeled SN0 and SN45, while nominal double-shear specimens with included V-notch angles θ = 60° and 90° were labeled SV60 and SV90. All specimens were tested under a strain rate of 0.001 s−1. Geometric parameters are given in Table 2, and specimen geometries and dimensions are illustrated in Figure 4 and Figure 5. Three replicate specimens were prepared for each test condition, and the average values are reported. The minimum-section radius of the round-notched specimens was a0 = 3 mm. The SN and SV geometries were designed to promote shear deformation in the ligament during axial loading. The local stress state in such specimens depends on geometry and changes as deformation proceeds [18,19]. ASTM B831 provides a methodological comparison for shear testing of thin aluminum alloy products [20].
Table 2. Parameters of specimens for different stress states.
Figure 4. Geometry and dimensions of the notched tensile specimens (unit: mm).
Figure 5. Geometries and dimensions of the shear specimens (unit: mm). (a,b) Double-shear specimens, (c,d) single-shear specimens.

2.2.2. In Situ SEM Observation During Tensile Loading

The in situ tensile specimen was a thin, dog-bone-shaped sheet with locating holes on both sides to constrain misalignment during loading. A U-shaped notch at the center of the gauge section concentrated deformation in the observation area, as shown in Figure 6. The gauge section was sequentially ground with 240# to 1500# abrasive papers and then mechanically polished. It was subsequently lightly etched with a 10 vol% perchloric acid–ethanol solution for 10 s to reveal the grain boundaries. At room temperature, displacement-controlled loading was applied at 0.2 mm/min using an MTEST 2000 in situ tensile stage (Gatan Inc., Pleasanton, CA, USA) installed in an FEI Quanta 450 environmental SEM. Surface morphology and the load-displacement curve were recorded in real time to track crack initiation and propagation. One specimen was examined throughout the in situ test. Nominal stress was calculated as F/(2.142 mm2). Apparent strain was calculated from the tensile-stage extension divided by the 4 mm reference length and expressed as a percentage, using the recorded extension without a machine-compliance correction.
Figure 6. Geometry and dimensions of the in situ tensile specimen (unit: mm).

2.2.3. Axial Fatigue Tests

Fatigue specimens were machined in accordance with the Chinese National Standard “Metallic materials-Fatigue testing-Axial force-controlled method” (GB/T 3075-2021) [21], with their dimensions shown in Figure 7. The specimen faces were progressively ground using 240-, 600-, 800-, 1200-, and 2000-grit papers, while the curved side surfaces were ground with corresponding abrasive rings. The specimens were then polished to reduce machining marks and obtain consistent surface conditions.
Figure 7. Geometry and dimensions of the axial fatigue specimen (unit: mm).
Fatigue tests were performed on an INSTRON 8801 servohydraulic fatigue testing machine (Instron, Norwood, MA, USA). All tests were carried out at room temperature under fully reversed axial sinusoidal loading with a stress ratio of R = −1 and a frequency of 20 Hz. The stress amplitudes were σa = 340.42, 316.59, 292.76, and 268.93 MPa, corresponding to approximately 100%, 93%, 86%, and 79% of the 340.42 MPa reference stress from a simplified ABAQUS tower wind-load calculation. All four amplitudes were below the baseline yield strength of 438.51 MPa. Three specimens were tested at each amplitude, and the tests continued to fracture or 3 × 106 cycles.
Five of the nine failed specimens were selected for fractography. At σa = 340.42 MPa, specimens with recorded lives Nf = 30,060.50 and 55,794.50 cycles were examined. At σa = 316.59 MPa, specimens with Nf = 82,164.50 and 121,302.25 cycles were selected. At σa = 292.76 MPa, the specimen with Nf = 616,721.25 cycles was examined. These values are the recorded lives of the selected specimens. The group means and standard deviations are reported in Section 3.4.1. The full test record, including the three specimens that reached the stopping criterion without fracture, is provided in Section 3.4.1.

2.2.4. Charpy V-Notch Impact Tests

Three full-size V-notch impact specimens measuring 10 × 10 × 55 mm3 were machined from the separately sampled plate in accordance with the Chinese National Standard “Metallic materials-Charpy pendulum impact test method” (GB/T 229-2020 [22]), as shown in Figure 8. After machining, the specimen surfaces were progressively ground and polished with 400# to 2000# abrasive papers to reduce milling marks and obtain consistent surface conditions on the notched face and side faces. Impact tests were conducted at room temperature using a JB-300B pendulum impact testing machine (Shandong Hairui Testing Instrument Co., Ltd., Jinan, China), and the absorbed impact energy was recorded. The three room-temperature tests gave a mean absorbed energy of 251.2 J.
Figure 8. Geometry and dimensions of the Charpy impact specimen (unit: mm). (a) Front view, (b) side view, (c) partial enlarged view of point A at the notch area.

3. Results and Discussion

3.1. Tensile Response and Dimple Morphology at Different Strain Rates

According to the Chinese National Standard “High strength low alloy structural steels” (GB/T 1591-2018) [23], the specified chemical composition and mechanical property limits for Q420 steel are given, and the measured values in Table 3 are compared against these requirements. The baseline tensile test at 0.5 mm/min gave a yield strength of 438.51 MPa, a tensile strength of 560.22 MPa, and an elongation after fracture of 29.27%. The separately sampled Charpy specimens gave a mean absorbed energy of 251.2 J at room temperature. Table 4 and Figure 9 summarize the tensile properties and representative engineering stress–strain curves at the three quasi-static strain rates. From 0.0001 to 0.01 s−1, mean yield strength increased from 440.17 to 495.30 MPa, and tensile strength increased from 562.82 to 590.16 MPa, corresponding to increases of 12.52% and 4.86%, respectively.
Table 3. Room-temperature mechanical properties of Q420 steel.
Table 4. Tensile properties of Q420 steel under different strain rates.
Figure 9. Engineering stress–strain curves of Q420 steel at the three quasi-static strain rates.
Tensile fracture surfaces obtained at different strain rates were examined by the Axia ChemiSEM, as shown in Figure 10. The macroscopic surfaces in Figure 10a–c contained prominent cavities or separations along the mid-thickness plane at all three rates. Enlarged views in Figure 10d–f revealed smaller irregular or elliptical cavities near the main openings, while micrometer-scale dimples were visible at higher magnification in Figure 10g–i. Similar fracture-surface separations in ferrite–pearlite steels have been associated with band-shaped pearlite and transverse tensile stress [24]. Through-thickness heterogeneity introduced during rolling may therefore contribute to the central separations observed here.
Figure 10. Tensile fracture surface morphologies at different strain rates. 0.0001 s−1: (a,d,g); 0.001 s−1: (b,e,h); 0.01 s−1: (c,f,i).
The tensile fracture surfaces of Q420 steel contained numerous dimples at all strain rates, indicating typical ductile fracture [25]. Equiaxed and elongated dimples coexisted at all three rates. Using Image J 1.54p measured 44 spatially calibrated opening contours gave mean equivalent diameters of 3.66 ± 1.01, 3.33 ± 0.43, and 3.66 ± 1.73 μm at 0.0001, 0.001, and 0.01 s−1, respectively (n = 14, 15, and 15 openings). The corresponding mean long-/short-axis ratios of the fitted ellipses were 1.24, 1.23, and 1.25. The equivalent diameter was calculated from the projected opening area. One field was analyzed at each rate, and the reported SD describes the variation among openings within that field. The three groups had similar mean diameters and aspect ratios, with no systematic increase or decrease over the tested strain-rate range. Table 4 also shows an increase in mean elongation after fracture from 19.60% to 30.50% across the tested range. The higher-rate tests therefore combined greater mean strength with more overall extension before fracture. The tensile curves reflect the evolving response of the gauge section, while the SEM measurements describe local openings left after void growth and coalescence. These quantities capture different aspects of deformation: the macroscopic properties changed as the rate increased, while the selected fields retained mixed equiaxed and elongated dimples with similar mean opening diameters and aspect ratios.

3.2. Fracture Morphologies Under Different Nominal Stress States

Tensile fracture surfaces under different nominal stress states were examined by SEM. Table 5 summarizes the peak loads, fracture displacement, and representative load-displacement curves for the seven geometries. Figure 11 presents the corresponding load-displacement curves. From NR2 to NR6, peak load decreased from 24.479 to 22.208 and 20.443 kN, while fracture displacement decreased from 9.302 to 6.954 and 6.660 mm. Across the NR, SN, and SV specimens, the load response also reflects differences in ligament geometry.
Table 5. Peak loads and fracture displacements of notched tensile and nominal-shear specimens.
Figure 11. Load-displacement curves under different stress states.
The notched tensile fracture morphologies are shown in Figure 12, while the nominal-shear fracture morphologies are shown in Figure 13 and Figure 14 (see Section 3.2.2 and Section 3.2.3 for details).
Figure 12. Microscopic fracture surface morphologies of ductile fracture in notched tensile specimens of Q420 steel. NR2: (a,a1–a3); NR4: (b,b1–b3); NR6: (c,c1–c3).

3.2.1. Notched Tensile Fracture Characteristics and Effects of Stress Triaxiality

Figure 12a–c shows the macroscopic fracture surfaces of notched tensile specimens NR2-NR6. All specimens exhibited typical cup-and-cone ductile fracture characteristics. The rough, serrated central region was the fibrous zone. The relatively smooth peripheral region, inclined at approximately 45° to the tensile axis, was the shear-lip zone. No pronounced radial patterns were observed, consistent with ductile fracture. Surface relief in the fibrous zone increased as the notch radius decreased. It was most pronounced in NR2 and relatively subdued in NR4 and NR6.
The microscopic morphologies in Figure 12(a1–c3) contained mixtures of rounded and elongated dimple openings separated by tearing ridges. Elongated openings are visible in Figure 12(a1,b2), while pronounced ridges between neighboring openings are evident in Figure 12(a2,b1). These features are consistent with void enlargement followed by stretching and tearing of the intervening ligaments. Together with the rough central fibrous region and inclined peripheral shear lip, the mixed dimple morphology illustrates the variation in plastic flow across the fracture surface. To compare notch constraint at the specimen level, a Bridgman-type estimate was calculated from the initial round-notch geometry [26]. The corresponding fracture strain was calculated from the change in minimum cross-sectional area,
η geo = 1 3 + ln ( 1 + a 0 2 R )
ε A = ln ( A 0 A f )
Here, ηgeo is the nominal geometric triaxiality. The parameter a0 = 3 mm is the initial minimum-section radius, and R is the notch radius in mm. A0 and Af are the initial and final minimum cross-sectional areas in consistent units. Equation (1) gives ηgeo = 0.892949, 0.651787, and 0.556477 for NR2, NR4, and NR6, respectively. The initially uniform smooth reference is assigned 1/3. For the ideal axisymmetric tensile centerline, the normalized Lode-angle parameter is +1, with −1 denoting axisymmetric compression. The four tensile cases were fitted using a three-parameter Johnson-Cook-type relationship [9]:
ε A , fit = D 1 + D 2 exp ( D 3 η geo )
Equal-weight nonlinear least squares gave dimensionless parameters D1 = 0.815099, D2 = 2.479383, and D3 = −3.928715, with R2 = 0.99940 in strain space and a maximum deviation of 0.82% from the four input points (Table 6). The area-based fracture strains were 0.887, 1.015, 1.087, and 1.485 for NR2, NR4, NR6, and the smooth reference, respectively. The corresponding reductions in area, calculated as 100[1 − exp(−εA)], were 58.81%, 63.76%, 66.28%, and 77.35%. Thus, NR2 sustained a larger overall displacement before fracture but underwent less section contraction than NR6. The two measures describe specimen extension and minimum-section necking, respectively. Hydrostatic tension promotes microvoid growth [27], providing a basis for discussing the effect of notch constraint on fracture. The empirical fit describes these four tensile cases over ηgeo ≈ 0.333~0.893. Its application to evolving local damage would require further calibration.
Table 6. Four-point nominal-constraint comparison and area-based strain fitting.

3.2.2. Shear Fracture Morphologies and Tear Ridge Characteristics

Figure 13 shows the fracture surface morphologies of the nominal single-shear tensile specimens. The macroscopic fracture surface of SN0 in Figure 13a exhibited a rough morphology characteristic of plastic deformation. At 2000× magnification, tear ridges with a pronounced orientation were visible in Figure 13(a2). Elliptical and elongated dimples with downward-extending major axes were observed in Figure 13(a1). Transverse tear ridges were present in the middle of the fracture surface (Figure 13(a3)), with fine dimples scattered along their edges. The elongated dimples and interconnecting tear ridges are consistent with directional plastic flow and void coalescence during ligament fracture.
Figure 13b shows the macroscopic fracture morphology of SN45. The fracture surface was also rough and exhibited pronounced plastic deformation. At 2000× magnification, region (b1) contained elongated dimples with relatively consistent directions of extension. The morphologies in Figure 13(b1,b2) were similar: both contained tearing ridges, with fine dimples scattered along their edges and smooth, flat elongated dimples nearby. Region b3 was dominated by large elongated dimples. The similar orientation of these features reflects directional plastic deformation in the ligament before fracture.
Figure 13. Microscopic fracture surface morphologies of Q420 steel single-shear tensile specimens. SN0: (a,a1–a3); SN45: (b,b1–b3).
Figure 14 shows the tensile fracture morphologies of the nominal double-shear specimens. The central regions in Figure 14(a2–b2) contained horizontally elongated dimples, while the adjacent fields in Figure 14(a1–b1) showed a mixture of dimple shapes. This variation in opening shape and orientation indicates nonuniform plastic flow across the ligament. The mechanical results in Table 5 and Figure 11 provide additional context for these directional fracture features. SN45 reached a higher peak load than SN0, 3.635 versus 3.173 kN, but fractured at a smaller displacement, 2.258 versus 2.998 mm. Changing the ligament inclination therefore altered the balance between load capacity and overall deformation before fracture. The SV60 and SV90 specimens had similar peak loads of 16.285 and 16.047 kN, with fracture displacements of 2.703 and 2.514 mm, respectively. Across the SN and SV configurations, elongated dimples and interconnected tearing ridges are consistent with directional stretching and rupture of ligaments between neighboring voids. The variation in opening shape and orientation across Figure 14(a1–a3,b1–b3) further indicates that this deformation varied with position within the fractured ligament. The mechanical and morphological differences thus reflect the influence of specimen geometry on the deformation preceding final separation.
Figure 14. Microscopic fracture surface morphologies of Q420 steel double-shear tensile specimens. SV60: (a,a1–a3); SV90: (b,b1–b3).

3.2.3. Characterization and Compositional Analysis of Selected Particles on Fracture Surfaces

Particles were observed in cavities on the fracture surfaces of both smooth and notched tensile specimens (Figure 15). EDS point analysis at a1 showed enrichment of Ca, Al, O, and S in the smooth-tensile particle, while b1 showed Ca and S enrichment in the notched-tensile particle. These elemental associations are commonly found in inclusions in calcium-treated steels [28]. The two particles had maximum feret diameters of 9.67 and 6.39 μm and equivalent projected diameters of 7.81 and 5.71 μm, respectively. Two additional Fe-rich features on notched fracture surfaces had maximum feret diameters of 3.30 and 2.93 μm, and a particle on a fatigue fracture surface measured 8.56 μm. These measurements cover five selected objects from four image groups. Their location within cavities is consistent with particle-assisted local void formation. A similar association between inclusions and local damage was reported for microalloyed steel by Tinoco et al. [15].
Figure 15. Selected particles and corresponding EDS point spectra on tensile fracture surfaces of Q420 steel. (Tensile fracture surface at a strain rate of 0.0001 s−1). (a) The fracture surface of the stretched specimen; (b) fracture surface of notched tensile specimen NR2; (a1) EDS point analysis in (a); (b1) EDS point analysis in (b).

3.3. Crack Initiation and Propagation Paths During In Situ Tensile Testing

Figure 16 compares the test steel before and after in situ tensile testing. Pronounced necking was observed after loading (Figure 16b), indicating substantial plastic deformation.
Figure 16. Sample photos (a) before and (b) after tensile testing.
Figure 17 shows the nominal stress-apparent strain curve obtained during in situ tensile testing. The letters A-E mark selected image-acquisition stages along the curve. At peak loading, F = 1197.9 N and the tensile-stage extension was 0.825 mm, giving a nominal stress of 559.24 MPa and an apparent strain of 20.625%. The first visible side crack was recorded at approximately 533 MPa on the descending branch after the peak. Pronounced necking was observed in the fractured specimen (Figure 16b).
Figure 17. Nominal stress-apparent strain curve obtained during in situ tensile testing.
Figure 18 shows successive stages of surface-crack initiation and propagation during the in situ test. Figure 18a presents the specimen surface before loading. After substantial plastic deformation, Crack 1 was first recorded near the right-hand edge of the U-shaped notch at a nominal stress of approximately 533 MPa (Figure 18b). At approximately 429 MPa (Figure 18c), Crack 1 showed little further visible extension, while the main crack, Crack 2, appeared near the notch center. Here, the initiation site of Crack 1 is marked as location A, and the initiation site of Crack 2 is marked as location B, corresponding to points A and B in Figure 17, respectively. Crack 2 initially lay at approximately 78° to the loading-axis reference. As loading continued, the crack grew through the deformed region and approached 90° at approximately 334 MPa (Figure 18d). Its direction then changed to about 88° at approximately 214 MPa (Figure 18e) and to 86° in the final displayed frame (Figure 18f). The angles were measured in the image plane between the marked crack direction and the loading-axis reference. The sequence shows limited extension of the initial side crack, followed by growth and deflection of the dominant crack near the notch center.
Figure 18. SEM images acquired during in situ tensile testing. (a) Surface before loading; (b) ~533 MPa, Crack 1 at right notch edge; (c) ~429 MPa, Crack 1 stalled, main Crack 2 initiated at notch center (~78°); (d) ~334 MPa, crack approached 90°; (e) ~214 MPa, direction ~88°; (f) final frame, direction 86°.

3.4. Axial Fatigue Fracture Morphologies and Their Response to Stress Amplitude

3.4.1. Macroscopic Zonation of Fatigue Fracture Surfaces

To illustrate the overall differences in fatigue life under different stress amplitudes, the Basquin relationship is adopted [6] for expressing stress amplitude-life. Its general form is given by
σ a = σ f ′ ( 2 N f ) b
In Equation (4), σa is stress amplitude and σ′f is the fatigue-strength coefficient, both in MPa. Nf is life in cycles, 2Nf is the number of reversals, and b is dimensionless. Least-squares regression of lg 2Nf against lg σa for the nine failed specimens in Table 7 gave σ′f = 700.51 MPa, b = −0.06337, and R2 = 0.7430 in log-life space [29]. The mean ± sample SD lives at 340.42, 316.59, and 292.76 MPa were 61,511.33 ± 34,664.63, 93,103.75 ± 24,624.22, and 715,103.00 ± 518,046.50 cycles, respectively (n = 3 specimens per group, sample SD calculated using n − 1). The three run-outs were excluded from the regression. At 268.93 MPa, all three specimens completed 3 × 106 cycles without fracture, giving an observed run-out level for these tests at R = −1 and 20 Hz.
Table 7. Fatigue test data for Q420 steel.
Figure 19 shows the macroscopic morphologies of the five examined fatigue fracture surfaces. Three characteristic regions could be identified: the crack initiation zone (CIZ), stable propagation zone (SPZ), and final overload region, conventionally termed the instantaneous fracture zone (IFZ). On all five surfaces, the small CIZ was located near a specimen edge, and the crack propagated inward. Surface condition and edge geometry may contribute to localization of cyclic deformation in this region. The SPZ occupied most of the fracture surface and contained striation-like ridges and secondary cracks associated with progressive crack advance. When the remaining section could no longer sustain the load, final overload produced the dimpled IFZ. Some surfaces also exhibited stepped relief between neighboring regions.
Figure 19. Macroscopic axial fatigue fracture surfaces of Q420 steel at different fatigue lives. (a) σa = 340.42 MPa, Nf = 30,060.5; (b) σa = 340.42 MPa, Nf = 55,794.5; (c) σa = 316.59 MPa, Nf = 82,164.5; (d) σa = 316.59 MPa, Nf = 121,302.25; (e) σa = 292.76 MPa, Nf = 616,721.25.

3.4.2. Microscopic Morphology near the Crack Initiation Zone (CIZ)

Figure 20 shows the microscopic morphologies around the fatigue crack initiation sites. Near the specimen edges, relatively flat areas were accompanied by small cracks. Adjacent fields contained striation-like features associated with subsequent local crack advance. These features occur around the initiation region as the crack begins to propagate. The stable propagation features and their local spacing are examined further in Section 3.4.3.
Figure 20. Axial fatigue crack initiation zones of Q420 steel at different fatigue lives. (a) σa = 340.42 MPa, Nf = 30,060.5; (b) σa = 340.42 MPa, Nf = 55,794.5; (c) σa = 316.59 MPa, Nf = 82,164.5; (d) σa = 316.59 MPa, Nf = 121,302.25; (e) σa = 292.76 MPa, Nf = 616,721.25.

3.4.3. Striations and Secondary Cracks in the Stable Propagation Zone (SPZ)

Figure 21 shows striation-like ridges and secondary cracks in the SPZ. Image J measurements of 42 local projected ridge intervals from nine regions of four micrographs gave mean ± sample SD spacings of 0.91 ± 0.21, 1.30 ± 0.19, 1.46 ± 0.32, and 1.12 ± 0.20 μm in Figure 21a–e, respectively (n = 9, 15, 10, and 8 intervals). Panel (c) was omitted from measurement because the interval boundaries were insufficiently clear. The reported SD describes variation among the measured intervals within the selected fields. The first two fields were both obtained at 340.42 MPa yet had different mean spacings. The four means varied nonmonotonically with nominal stress amplitude. Local crack length, crack-tip driving force, and ridge orientation can contribute to the differences between fields. Roven and Nes observed a one-cycle-per-striation correspondence over a limited range of crack-growth rates in ferritic steel [30]. Determination of da/dN requires crack-length and cycle records, as specified in ASTM E647 [31]. Thus, the present intervals provide a local morphological comparison. The secondary cracks in Figure 21 occur within or alongside areas containing striation-like ridges and locally interrupt the propagation surface. Their association with these ridged areas is consistent with localized separation during repeated deformation around the advancing fatigue crack. Together, the ridges and secondary cracks record progressive crack advance with spatial variations in the fracture path. This local information complements the fatigue-life records: the mean lives increased as nominal stress amplitude decreased, while the measured ridge intervals varied between fields, including fields tested at the same amplitude. The observed amplitude-life trend and the local differences in propagation morphology therefore describe the fatigue response at different scales.
Figure 21. Axial fatigue crack propagation zones of Q420 steel at different fatigue lives. (a) σa = 340.42 MPa, Nf = 30,060.5; (b) σa = 340.42 MPa, Nf = 55,794.5; (c) σa = 316.59 MPa, Nf = 82,164.5; (d) σa = 316.59 MPa, Nf = 121,302.25; (e) σa = 292.76 MPa, Nf = 616,721.25.

3.4.4. Dimple Morphology in the Final-Overload Zone (IFZ)

Figure 22 shows the microscopic IFZ morphologies at different stress amplitudes and fatigue lives. Dimples and tearing features were present in all examined final overload regions. The fields in Figure 22a–c contained elongated dimples and rough surface relief, whereas Figure 22d,e showed more equiaxed openings mixed with elongated dimples. The variation in opening shape reflects differences in the direction and extent of local plastic deformation during final fracture.
Figure 22. Axial fatigue instantaneous fracture zones of Q420 steel at different fatigue lives. (a) σa = 340.42 MPa, Nf = 30,060.5; (b) σa = 340.42 MPa, Nf = 55,794.5; (c) σa = 316.59 MPa, Nf = 82,164.5; (d) σa = 316.59 MPa, Nf = 121,302.25; (e) σa = 292.76 MPa, Nf = 616,721.25.
The IFZ forms when the remaining ligament fails by overload. Its dimple morphology therefore depends on the ligament geometry, local constraint, and available void-nucleation sites. Hydrostatic tension promotes void enlargement [27], while directional plastic flow favors elongated openings and tearing ridges. These final fracture conditions provide the basis for interpreting the differences between the IFZ fields.

3.5. Dimple Morphology and Room-Temperature Toughness Characterization on Impact Fracture Surfaces

Figure 23 shows the Charpy impact fracture morphologies of Q420 steel. The macroscopic fracture surface in Figure 23a consisted of a central fibrous region surrounded by a shear lip. At 3000× magnification, the fibrous region contained elongated and equiaxed dimples (Figure 23b). The intermediate field in Figure 23c showed a nonuniform dimple-size distribution and some relatively flat openings. The shear-lip region in Figure 23d contained more directional dimples, consistent with a greater shear contribution to local deformation. Together with the mean absorbed energy of 251.2 J from three specimens, these observations characterize the room-temperature impact response. No clear cleavage or quasi-cleavage facets were identified in the examined tensile, impact, and fatigue final overload fields.
Figure 23. SEM images of the impact fracture surface. (a) Macroscopic overview showing a central fibrous region bounded by peripheral shear lips, indicative of ductile fracture under impact loading. (b) High-magnification SEM image (3000×) of the fibrous region (area a in panel (a)), characterized by elongated and equiaxed dimples typical of ductile rupture. (c) High-magnification SEM image (2000×) of the near-crack region (area b in panel (a)), displaying nonuniform dimples of varying size and morphology; the complex local stress state and stress gradients near the crack tip, together with material heterogeneity, promote rapid microvoid nucleation but constrain void growth, yielding a limited fraction of relatively flat dimples. (d) High-magnification SEM image (2000×) of the shear-lip region (area c in panel (a)), exhibiting dimple features with a pronounced shear-dominated deformation character. The presence of shear lips confirms that edge regions experience combined tensile and shear stresses, further corroborating the inherent ductility of Q420 steel.
Comparison by fracture region and stage provides a physical basis for interpreting the different surfaces [32]. The central fibrous regions of the round-notched tensile and Charpy specimens contained rounded and elongated dimples with intervening tearing ligaments, while the peripheral shear lips showed a more directional fracture morphology. These features are consistent with microvoid coalescence accompanied by local stretching and shear during final separation. A similar terminal process is recorded by the dimpled IFZ of the fatigue specimens, where the remaining ligament failed by overload. The fatigue SPZ contains striation-like ridges and secondary cracks associated with progressive crack advance under repeated loading. The common dimpled terminal regions and the distinct fatigue-propagation features provide complementary evidence for reconstructing the sequence of fracture.
The mechanical results add a further distinction: NR2 sustained a larger fracture displacement but a smaller area-based fracture strain than NR6, showing that overall extension and minimum-section contraction provide different measures of ductility. Regional morphology supplies complementary information about the local opening and tearing involved in final separation. These comparisons are qualitative across the different parent stocks and specimen geometries. During failure analysis, an edge-adjacent origin followed by an SPZ and a dimpled IFZ helps identify progressive fatigue cracking followed by final overload. Mid-thickness separations and particle-containing cavities identify areas for further metallographic examination. The fatigue records provide a laboratory baseline at R = −1 and 20 Hz for comparisons under matched conditions. Application to welded tower components additionally requires weld-specific properties, service loading spectra, and temperature-dependent toughness data.

4. Conclusions

  • Within the quasi-static strain-rate range of 0.0001–0.01 s−1, mean yield strength increased from 440.17 to 495.30 MPa and mean tensile strength increased from 562.82 to 590.16 MPa, corresponding to increases of 12.52% and 4.86%, respectively. Equiaxed and elongated dimples coexisted at all three rates. The selected fields had mean equivalent opening diameters of 3.66, 3.33, and 3.66 μm and mean aspect ratios of 1.24, 1.23, and 1.25, showing similar projected dimple geometries over this range. The large mid-thickness cavities and separations were present at all three rates and were distinct from these micrometer-scale dimples. From NR2 to NR6, nominal initial triaxiality decreased from approximately 0.893 to 0.556, while area-based fracture strain increased from 0.887 to 1.087 and fracture displacement decreased from 9.302 to 6.660 mm. The opposite rankings of displacement and area-based strain demonstrate the different contributions of overall extension and minimum-section contraction to the measured ductility. A four-point empirical J-C-type relationship summarized the tensile area-strain results over nominal ηgeo ≈ 0.333~0.893. Nominal single-shear surfaces contained oriented elongated dimples and interconnected tearing ridges, while the central fields of the nominal double-shear surfaces showed horizontally elongated dimples, consistent with directional plastic flow during ligament fracture.
  • EDS point analyses showed local Ca-Al-O-S enrichment in a selected smooth-tensile particle and Ca-S enrichment in a selected notched-tensile particle. Their maximum Feret diameters were 9.67 and 6.39 μm, respectively. The occurrence of these particles within fracture-surface cavities supports particle-assisted local void formation and provides a microstructural explanation for some of the local fracture heterogeneity. During the single in situ tensile test, the first visible side crack was recorded near the right-hand notch edge at approximately 533 MPa, after the nominal-stress peak of 559.24 MPa. This crack subsequently showed little further visible extension, while the dominant crack appeared near the notch center at approximately 429 MPa and continued to grow as the load decreased. Its successive in-plane directions relative to the loading-axis reference were approximately 78°, 90°, 88°, and 86°. The sequence distinguishes the first recorded surface crack from the later development of the dominant crack and documents its growth and geometric deflection during post-peak deformation.
  • Under fully reversed axial fatigue loading at R = −1 and 20 Hz, mean life increased from 61,511.33 to 715,103.00 cycles as stress amplitude decreased from 340.42 to 292.76 MPa. The nine failure records gave Basquin parameters σ′f = 700.51 MPa and b = −0.06337. At 268.93 MPa, all three specimens reached 3 × 106 cycles without fracture, defining the observed run-out level under these test conditions. The five examined fracture surfaces showed a small edge-adjacent crack initiation zone (CIZ), a stable propagation zone (SPZ) containing striation-like ridges and secondary cracks, and a dimpled final-overload zone (IFZ). Measurements of 42 local projected ridge intervals in four selected SPZ fields gave mean spacings of 0.91, 1.30, 1.46, and 1.12 μm. Their nonmonotonic variation, including different means at the same nominal stress amplitude, highlights the field-to-field variation in local propagation morphology. The IFZ contained elongated and equiaxed dimples with differing surface relief. These features record the local plastic deformation and constraint of the remaining ligament during final overload, complementing the progressive crack-growth features preserved in the SPZ.
  • Three full-size Charpy specimens from the separately sampled impact plate gave a mean absorbed energy of 251.2 J at room temperature. Their fracture surfaces consisted of a central fibrous region and a peripheral shear lip. Equiaxed and elongated dimples with nonuniform sizes were present in the fibrous region, while the shear lip contained more directional openings, consistent with a greater shear contribution to local deformation. The dimpled fracture morphology and absorbed energy indicate substantial plastic deformation during room-temperature impact fracture. A qualitative comparison with the terminal tensile and fatigue-overload regions identifies void coalescence and ligament tearing as common features of final separation under the tested conditions. For failure analysis, the fracture origin and SPZ-IFZ boundary help distinguish progressive fatigue cracking from subsequent overload and are consistent with ductile behavior under the tested conditions.

Author Contributions

Conceptualization, J.S., X.L. and X.T.; Methodology, J.S., X.L. and X.T.; Software, Z.S. and X.C.; Validation, Z.S. and X.C.; Formal analysis, H.J. and D.Y.; Investigation, H.J. and D.Y.; Data curation, Z.S. and H.J.; Writing—original draft, H.J.; Writing—review & editing, J.S. and X.T.; Visualization, X.C. and X.L.; Supervision, J.S. and X.T.; Project administration, X.T.; Funding acquisition, X.T. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by the National Key R&D Program of China (grant number 2025YFE0105500), Jiayuguan Science and Technology Bureau Project of Jiayuguan City “Open Competition” Program (grant number 25-01).

Data Availability Statement

The original contributions presented in the study are included in the article, further inquiries can be directed to the corresponding authors.

Conflicts of Interest

Authors Zongliang Song, Xingrun Chen and Danni Yang were employed by the Jiuquan Iron and Steel (Group) Co., Ltd. The remaining authors declare that the research was conducted in the absence of any commercial or financial relationships that could be construed as a potential conflict of interest.

References

  1. Cao, J.; Ren, W.B.; Zhang, G.D.; Yin, S.B.; Liu, Z.Z.; Sun, X.J. Effect of Weld Surface Quality on the Fatigue Performance of Q420 Steel Used in Offshore Wind Tower Tube. Metals 2026, 16, 148. [Google Scholar] [CrossRef] [Scilit]
  2. Li, Q.Y.; Xu, C.B.; Luo, Z.C.; Huang, F.H.; Zang, X.S.; Zhang, D.C. Fatigue Performance of Q420C Steel Fillet-Welded Joints at Low Temperatures. Structures 2023, 51, 1341–1353. [Google Scholar] [CrossRef] [Scilit]
  3. Weng, S.; Meng, C.; Deng, J.H.; Zhao, L.H.; Pei, X.J.; Zhu, M.L. Fatigue Life Assessment of Q345 Steel Fillet Welded Joints with Competitive Failure Modes. Eng. Fract. Mech. 2024, 298, 109913. [Google Scholar] [CrossRef] [Scilit]
  4. Sheng, J.; Ma, J.J.; Wei, F.F.; Meng, Y.H.; Ma, Z.W.; Liang, Y.J.; Duan, H.Y. Study on The Mechanical Properties and Constitutive Model of Q420 Steel under Different Strain Rates. Nano 2025, 20, 2550023. [Google Scholar] [CrossRef] [Scilit]
  5. Wang, C.A.; Kim, T.H. Computational Fatigue Analysis of The Almen Strip Treated with Double-Sided Shot Peening and Its Experimental Verification. Int. J. Adv. Manuf. Technol. 2024, 134, 4505–4517. [Google Scholar] [CrossRef] [Scilit]
  6. Yang, L.G.; Xing, Y.M. Experimental Study on High-Cycle Fatigue Properties of Q420C Steel at Room Temperature. Mater. Res. 2022, 25, 20210589. [Google Scholar] [CrossRef] [Scilit]
  7. Nambirajan, T.; Kumar, P.C.; Aggarwal, S.; Gurudutt, A. Uncoupled Fracture Model For E250, E350, And E450 Grades of Structural Steel under Monotonic Loading. Eng. Fract. Mech. 2023, 292, 109638. [Google Scholar] [CrossRef] [Scilit]
  8. Tang, Z.Z.; Yang, X.; Liu, H.; Xue, H.Y. Numerical Simulation with an Improved Ductile Fracture Model for Steel Connections Considering Effect of Element Size. J. Constr. Steel Res. 2024, 223, 109031. [Google Scholar] [CrossRef] [Scilit]
  9. Johnson, G.R.; Cook, W.H. Fracture Characteristics of Three Metals Subjected to Various Strains, Strain Rates, Temperatures and Pressures. Eng. Fract. Mech. 1985, 21, 31–48. [Google Scholar] [CrossRef] [Scilit]
  10. Li, W.C.; Jing, Y. A Simple Calibrated Ductile Fracture Model and Its Application in Failure Analysis of Steel Connections. Buildings 2022, 12, 1358. [Google Scholar] [CrossRef] [Scilit]
  11. You, Q.; Wang, J.T.; Wu, X.H.; Sun, Q.; Zhao, B.Z. Uncoupled Fracture Model of Q690 High-Strength Steel Based on Stress Triaxiality and Lode Angle Parameter. Fatigue Fract. Eng. Mater. Struct. 2022, 45, 2890–2907. [Google Scholar] [CrossRef] [Scilit]
  12. Shang, M.; Yang, H.; Münstermann, S. Characterization of the Stress-state Dependent Ductile Fracture Behavior for Q960 Ultra-high-strength Structural Steel. Thin-Walled Struct. 2024, 205B, 112508. [Google Scholar] [CrossRef] [Scilit]
  13. Watanabe, Y.; Matsuno, T.; Hama, T.; Matsuda, T.; Okitsu, Y.; Hayashi, S.; Takada, K.; Naito, T. Microstructural Ductile Fracture Analysis of 1180-MPa Class Martensite-matrix Dual-phase Steel via in Situ Tensile Test. ISIJ Int. 2024, 64, 116–125. [Google Scholar] [CrossRef] [Scilit]
  14. Vermeij, T.; Hoefnagels, J.P.M. Plasticity, Localization, and Damage in Ferritic-pearlitic Steel Studied by Nanoscale Digital Image Correlation. Scr. Mater. 2022, 208, 114327. [Google Scholar] [CrossRef] [Scilit]
  15. Tinoco, H.A.; Fintova, S.; Heikkila, I.; Herrero, D.; Vuoristo, T.; Dlouhy, L.; Hutar, P. Experimental and Numerical Study of Micromechanical Damage Induced by MnS-based Inclusions. Mater. Sci. Eng. A 2022, 856, 144009. [Google Scholar] [CrossRef] [Scilit]
  16. Long, H.X.; Wang, G.P.; Wang, P.X.; Ma, J.J.; Luo, X.; He, H. Study on the influence of heat input on microstructure and properties of Q420C steel welded joints. Coatings 2025, 15, 957. [Google Scholar] [CrossRef] [Scilit]
  17. GB/T 228.1-2021; Metallic Materials-Tensile Testing-Part 1: Method of Test at Room Temperature. Standardization Administration of China: Beijing, China, 2021.
  18. Bao, Y.; Wierzbicki, T. On fracture locus in the equivalent strain and stress triaxiality space. Int. J. Mech. Sci. 2004, 46, 81–98. [Google Scholar] [CrossRef] [Scilit]
  19. Mohr, D.; Henn, S. Calibration of stress-triaxiality dependent crack formation criteria: A new hybrid experimental-numerical method. Exp. Mech. 2007, 47, 805–820. [Google Scholar] [CrossRef] [Scilit]
  20. ASTM B831-19; Standard Test Method for Shear Testing of Thin Aluminum Alloy Products. ASTM International: West Conshohocken, PA, USA, 2019.
  21. GB/T 3075-2021; Metallic Materials-Fatigue Testing-Axial Force-Controlled Method. Standardization Administration of China: Beijing, China, 2021.
  22. GB/T 229-2020; Metallic Materials-Charpy Pendulum Impact Test Method. Standardization Administration of China: Beijing, China, 2020.
  23. GB/T 1591-2018; High Strength Low Alloy Structural Steels. Standardization Administration of China: Beijing, China, 2018.
  24. Xiong, J.; Dong, X.; Wang, F.; Qiu, Y. The formation mechanism of fracture surface separations and their effects on the toughness for ferrite-pearlite steels. Mater. Today Commun. 2024, 41, 110269. [Google Scholar] [CrossRef] [Scilit]
  25. Roth, C.C.; Mohr, D. Effect of Strain Rate on Ductile Fracture Initiation in Advanced High Strength Steel Sheets: Experiments and Modeling. Int. J. Plast. 2014, 56, 19–44. [Google Scholar] [CrossRef] [Scilit]
  26. Peng, J.; Wang, Y.; Dai, Q.; Liu, X.; Liu, L.; Zhang, Z. Effect of stress triaxiality on plastic damage evolution and failure mode for 316L notched specimen. Metals 2019, 9, 1067. [Google Scholar] [CrossRef] [Scilit]
  27. Rice, J.R.; Tracey, D.M. On the ductile enlargement of voids in triaxial stress fields. J. Mech. Phys. Solids 1969, 17, 201–217. [Google Scholar] [CrossRef] [Scilit]
  28. Ren, Y.; Wang, W.J.; Yang, W.; Zhang, L.F. Modification of Non-metallic Inclusions in Steel by Calcium Treatment: A Review. ISIJ Int. 2023, 63, 1927–1940. [Google Scholar] [CrossRef] [Scilit]
  29. Johnston, C. Statistical analysis of fatigue test data. In Proceedings of the ASME 2017 36th International Conference on Ocean, Offshore and Arctic Engineering, Trondheim, Norway, 25–30 June 2017; p. V004T03A040. [Google Scholar] [CrossRef] [Scilit]
  30. Roven, H.J.; Nes, E. Cyclic deformation of ferritic steel-II. Stage II crack propagation. Acta Metall. Mater. 1991, 39, 1735–1754. [Google Scholar] [CrossRef] [Scilit]
  31. ASTM E647-24; Standard Test Method for Measurement of Fatigue Crack Growth Rates. ASTM International: West Conshohocken, PA, USA, 2024. [Google Scholar] [CrossRef] [Scilit]
  32. Maruschak, P.; Konovalenko, I.; Sorochak, A. Methods for evaluating fracture patterns of polycrystalline materials based on the parameter analysis of ductile separation dimples: A review. Eng. Fail. Anal. 2023, 153, 107587. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Article metric data becomes available approximately 24 hours after publication online.