Skip to Content
MetalsMetals
  • Article
  • Open Access

21 November 2026

18 Pages

Ethylene Carbonate Modulates Copper(I) Coordination in Copper Electrodeposition from DMI–AlCl3–Cu2O Electrolytes

,
,
,
,
and
1
School of Intelligent Manufacturing, Jingchu University of Technology, Jingmen 448000, China
2
Aviation Key Laboratory of Science and Technology on Structure Corrosion Prevention and Control, China Special Vehicle Research Institute, Jingmen 448035, China
*
Author to whom correspondence should be addressed.
This article belongs to the Section Extractive Metallurgy

Abstract

Aqueous cyanide, sulphate, and acid copper baths are toxic, couple galvanically with aluminium and zinc substrates, or occlude hydrogen. Organic-solvent electrolytes avoid these routes, but their neutral additives remain little studied. Ethylene carbonate (EC) was added at 4.6–16.1 mol% to an 86.5DMI–9.6AlCl3–3.9Cu2O electrolyte (DMI: 1,3-dimethyl-2-imidazolidinone), and copper was electrodeposited at 333 K. Raman spectroscopy, conductivity, viscosity, voltammetry, electron microscopy, optical surface imaging, and density functional theory on Cu13(111) linked the solution structure to the deposit. EC raised the conductivity (323–363 K) to 4.19–8.23 mS cm−1 and the viscosity (323–373 K) to 6.3–13.2 mPa s, and shifted the onset potential from −0.4 to −0.85 V and the cathodic peak from −1.35 to −1.77 V. At −1.4 V, raising EC from 4.6 to 12.6 mol% reduced the apparent size of the surface features from 35 to 15 μm and peak-to-valley roughness from 1.7 to 0.9 μm, with smoothness ceasing to improve at 16.1 mol%. On Cu13(111), DMI adsorbed at −98.1 to −126.9 kJ mol−1 and 0.34–0.42 e, and EC at −38.7 to −62.4 kJ mol−1 and 0.11–0.19 e. Complexation energies fell from −79.7 to −57.4 kJ mol−1, so EC binds weakly in the first coordination shell. EC thus acts as a coordination modifier, not an adsorption inhibitor.

1. Introduction

Copper is the standard metallisation for printed circuits, decorative finishing, and mould repair [1]. Cyanide baths are being phased out because of their toxicity, sulphate baths couple galvanically with aluminium and zinc substrates, and acid baths occlude hydrogen in high-purity deposits [2,3]. Organic-solvent electrolytes sidestep all three problems: no hydrogen evolution, a wider working temperature range, and the direct dissolution of metal chlorides.
Ethylene carbonate (EC) and 1,3-dimethyl-2-imidazolidinone (DMI) are polar aprotic solvents with high boiling points and low toxicity. Both dissolve AlCl3 and Cu2O, and the vibrational spectra of the two liquids and the speciation of the dissolved aluminium are established [4,5,6,7]. In earlier work, the ternary system 90DMI–10AlCl3–4Cu2O (86.5DMI–9.6AlCl3–3.9Cu2O, mol%) was used to electrodeposit copper, and its speciation was resolved, revealing the coexistence of [AlCl2(DMI)4]+, AlCl3(DMI)2, and [AlCl4]−, with Cu2O dissolving through the six-coordinate aluminate cation [8]. The coatings, however, were rough. Between −1.1 and −1.3 V, copper grew as pom-pom-like agglomerates of 20–40 μm separated by pores; the peak-to-valley roughness reached 15–43 μm, and the deposit flaked off when the specimen was taken out. The Raman spectra on which this description rests are reported here: Figure 1 compares DMI, 90DMI–10AlCl3, and 86.5DMI–9.6AlCl3–3.9Cu2O, with the four quaternary electrolytes at 4.6 to 16.1 mol% EC; and the 27Al nuclear magnetic resonance (NMR) spectrum that identifies the chloroaluminate species is reported in [8].
Figure 1. Raman spectra of the electrolytes recorded at 298 K, with 633 nm excitation. (a) DMI, 90DMI–10AlCl3 and 86.5DMI–9.6AlCl3–3.9Cu2O; the band at 349 cm−1 (arrow) is assigned to [AlCl4]− and the band at 1702 cm−1 to the DMI carbonyl stretch, which weakens once Cu2O is dissolved. (b) The quaternary electrolytes with 4.6, 8.8, 12.6 and 16.1 mol% EC; the traces are shown as acquired, without background subtraction, and are, therefore, compared by the band position rather than by the band shape. Panel (a) is reproduced from [8].
A second solvent offers a different route. EC is miscible with DMI, dissolves AlCl3 through a similar mechanism [9,10], and, as in other DMI solvate electrolytes [11], adjusts viscosity and polarity; Cu2O remains soluble. In zinc and magnesium electrolytes, changing the solvent or adding a second component alters the solvation shell and, through it, the morphology of the deposit [12,13,14,15]. To our knowledge, neither the role of EC nor an appropriate concentration range has been reported for DMI–AlCl3–Cu2O.
Here, the surface and the ion are treated separately. The interface was modelled using a Cu13(111) cluster and the ion was modelled using four-coordinate complexes, [Cu(DMI)4]+, [Cu(EC)4]+, [Cu(DMI)3(EC)]+ and [Cu(DMI)2(EC)2]+. The two sets answer different questions: adsorption energies describe what a molecule does at a growing surface, whereas complexation and ligand-exchange energies describe how the first coordination shell of copper(I) is built. The ion is examined because the shift in the reduction potential is a property of the species that is discharged and not of the plane on which it discharges. The zinc electrode and the aluminium reference are the same in all five electrolytes; what changes is the composition of the copper complex, so the electrode is a constant of the experiment. The ternary complexes, with their Raman and 27Al NMR assignment, are reported in [8]. They are included here only as the reference against which the EC-containing shells are compared, and no adsorption or complexation data for EC in this electrolyte are reported in [8]. The adsorption calculation is included to test the alternative reading that EC acts at the interface rather than on the ion: if that were so, EC would have to compete with DMI for the growth sites, and its adsorption energy on the cluster would have to be the larger of the two.
Three points are new. First, EC is shown to act as a coordination modifier of the copper(I) ion in a chloroaluminate electrolyte, a role that, to our knowledge, has not been examined for a neutral organic additive in this class of bath. Second, the solution measurements and the calculations arrive at the same conclusion: conductivity and viscosity fix the bulk transport, voltammetry fixes the shift in the reduction potential, and the complexation energies show where EC sits in the shell, so the change in morphology follows from the solvation shell to the deposit instead of being inferred from the appearance of the coating alone. Third, a concentration window is located: the size of the surface features and the roughness fall between 4.6 and 12.6 mol% EC and stop improving at 16.1 mol%, where the roughness rises again to 2.0 μm. This paper follows that order: the Raman spectra and the physical properties of the five electrolytes (Section 3.1 and Section 3.2), the voltammetry that locates the shift (Section 3.3), the coatings obtained at fixed potential and at varied potentials (Section 3.4 and Section 3.5), the surface and ion calculations (Section 3.6 and Section 3.7), and the discussion that ties them together (Section 4).

2. Materials and Methods

2.1. Electrolyte Preparation

The ethylene carbonate (EC), 1,3-dimethyl-2-imidazolidinone (DMI), anhydrous AlCl3 and Cu2O were of analytical grade and were purchased from Shanghai Aladdin Biochemical Technology Co., Ltd. (Shanghai, China). AlCl3 and Cu2O hydrolyse in air, so the salts were weighed on a CP313 balance (OHAUS, Parsippany, NJ, USA), and the electrolytes were mixed and stored in an argon-filled glovebox (MBRAUN MB 200B, Garching, Germany) with water and oxygen contents below 0.1 ppm, the same box that housed the electrochemical cell. The ternary base was prepared at a molar ratio of 90DMI–10AlCl3–4Cu2O, that is, 86.5DMI–9.6AlCl3–3.9Cu2O in mole fractions, and stirred at 333 K until the melt was clear and free of visible suspension. Portions of this base were then used for the quaternary mixtures, EC being added at 4.6, 8.8, 12.6 and 16.1 mol% of the total, giving 82.5DMI–9.2AlCl3–3.7Cu2O–4.6EC, 78.9DMI–8.8AlCl3–3.5Cu2O–8.8EC, 75.6DMI–8.4AlCl3–3.4Cu2O–12.6EC and 72.6DMI–8.1AlCl3–3.2Cu2O–16.1EC, each mixture again being stirred at 333 K until clear. Taking these compositions together with the measured densities reported in Section 3.2, the four electrolytes contain 0.70, 0.68, 0.67 and 0.64 mol L−1 of copper(I) at 333 K: the copper concentration falls by about 8% across the series, while the EC content rises by a factor of 3.5.

2.2. Physical Properties and Spectra

Conductivity was measured with a DDS-307 meter (Shanghai INESA Scientific Instrument Co., Ltd., Shanghai, China) between 323 and 373 K, the cell constant having been calibrated against 1 mol L−1 KCl. Density was obtained using the Archimedes method, the volume of the platinum bob being established by water displacement. Viscosity was measured using a DV2T rotational viscometer (Brookfield AMETEK, Middleboro, MA, USA), with a tall beaker keeping the spindle fully immersed. Each temperature was held for 20 min before reading. Raman spectra of the four quaternary electrolytes were recorded at room temperature on a LabRAM Odyssey confocal Raman microscope (Horiba Jobin-Yvon, Longjumeau, France) with 633 nm excitation, 100 mW at the sample, a 50 × 0.75 objective, a 100 μm slit, and two 30 s accumulations, and the 27Al nuclear magnetic resonance spectrum of the ternary base was reported previously [8].

2.3. Electrochemistry and Deposition

Cyclic voltammetry and potentiostatic deposition were carried out with a CHI660E electrochemical workstation (Shanghai Chenhua Instrument Co., Ltd., Shanghai, China) in the same argon-filled glovebox in a three-electrode cell at 333 K, with a zinc sheet as the working electrode, glassy carbon as the counter electrode and an aluminium wire as the reference. Voltammograms were recorded at 50 mV s−1 in a three-segment scan over the range −2.0 to +0.9 V (vs. Al): the sweep started at 0 V, the open-circuit value of the cell ran first to −2.0 V, reversed to +0.9 V, and returned to the starting point. Deposits were produced at −1.0, −1.2, −1.4 and −1.6 V for 2 h, rinsed with acetonitrile and stored in the glovebox.

2.4. Coating Characterisation

Phases were identified by X-ray diffraction (Bruker D8 ADVANCE, Bruker AXS, Karlsruhe, Germany) with Cu Kα radiation, the patterns being indexed against the International Centre for Diffraction Data (ICDD) 03-065-9026 (Cu) and ICDD 03-065-3358 (Zn). Morphology and composition were examined using scanning electron microscopy (SEM; FEI Quanta 250 FEG, Brno, Czech Republic) at 20 kV; one specimen was prepared for each condition, and three points were analysed on it. The three-dimensional surface profile was recorded in air using the non-contact optical surface imaging (OSP) technique with a scanning electrochemical microscope (SECM; AMETEK, Berwyn, PA, USA): the height of the surface is obtained from the diffuse reflection of a laser in air, without contact, with a lateral resolution of 1–2 μm. The scan area was 1 mm × 1 mm with a step of 20 μm. The difference between the lowest and the highest point of a profile is taken as the peak-to-valley roughness value. Sizes quoted in the text are apparent diameters of the surface features, measured on the SEM images against the 50 μm scale bar; they are not crystallographic grain sizes, and no size distribution was measured.

2.5. Computational Details

Calculations were performed using the ORCA 6.1.1 program [16,17]. The Cu(111) surface was modelled by a 13-atom cuboctahedral copper cluster, one atom at the centre and twelve at the vertices, the closed-shell fragment of a face-centred cubic (fcc) lattice that exposes eight (111) facets. After relaxation, the twelve centre–vertex distances fell between 2.377 and 2.396 Å, and the thirty vertex–vertex contacts fell below 2.6 Å, lying between 2.500 and 2.524 Å. Every vertex atom, therefore, has six copper neighbours within 2.6 Å. The cluster carries 377 electrons, was treated as a doublet at zero charge, and was allowed to relax together with the adsorbate; the adsorption energies, therefore, include the substrate relaxation. EC and DMI were optimised at BP86-D3(BJ)/def2-SVP with the conductor-like polarisable continuum model (CPCM, ε = 37.6) for the complexation energies in Section 3.7 and in the gas phase at the same level for the adsorption energies in Section 3.6. B3LYP-D3(BJ)/def2-TZVP single-point calculations were computed on both sets of geometries, and the charges discussed below were taken from those single points; dispersion was included using the D3(BJ) correction from Grimme et al. [18]. Each adsorbate was attached through its carbonyl oxygen 2.1 Å above the top, the bridge, and the three-fold hollow site, and the whole system was optimised at BP86-D3(BJ)/def2-SVP, with a maximum of 250 geometry cycles and the TightSCF and VerySlowConv settings; the top and hollow sites were tested for DMI and the top, bridge, and hollow sites for EC. Final energies were obtained from B3LYP-D3(BJ)/def2-TZVP single-point calculations on the optimised geometries using the RIJCOSX approximation and the def2/J auxiliary basis, and the adsorption energy was taken as Eads = E(Cu13 + adsorbate) − E(Cu13) − E(free adsorbate), with 1 Hartree = 2625.499639 kJ mol−1. The charge transferred to the metal was taken as the increase in the summed CHELPG charge (charges from electrostatic potentials using a grid-based method) of the adsorbate atoms upon adsorption, a positive value, therefore, meaning donation to the cluster. CHELPG places a large negative charge on the buried central atom of the cluster, an artefact of the fit for an enclosed atom; only the twelve surface atoms are used in the discussion. No vibrational analysis was performed on the new cluster, so the adsorption energies are reported as electronic energies only and no statement is made about whether the optimised structures are minima. The eight (111) facets of this cluster are referred to below as the Cu13(111) surface. The input files, optimised coordinates and absolute energies of all calculations are given in the Supplementary Materials.
Adsorption energies were evaluated in the gas phase. The dielectric constant of the concentrated DMI–AlCl3–Cu2O–EC mixtures was not measured here, and adopting that of either pure component would assign a definite polarity to a mixture of two solvents and a dissolved salt. Both adsorbates are neutral molecules compared on the same cluster, so the ordering between them is the quantity expected to survive this approximation, whereas the absolute values carry the corresponding systematic uncertainty. As a check on this choice, the same optimised geometries were also evaluated using the conductor-like polarisable continuum model (CPCM, ε = 37.6); the ordering of the adsorption energies in Section 3.6 is unchanged, and every complex is stabilised by 49–51 kJ mol−1.
Because the reduction-potential shift in Section 3.3 is a property of the copper ion rather than of a surface, a second set of calculations treated Cu(I) as four-coordinate molecular complexes of the two solvents: [Cu(DMI)4]+, [Cu(EC)4]+, [Cu(DMI)3(EC)]+ and [Cu(DMI)2(EC)2]+, all closed-shell singlets at charge +1 (d10). The complexes were optimised at BP86-D3(BJ)/def2-SVP using CPCM (ε = 37.6) without symmetry constraints and given by B3LYP-D3(BJ)/def2-TZVP single-point calculations using the RIJCOSX approximation, def2/J auxiliary basis, and CHELPG charges, the same two levels and continuum as for the surface set. Ligand-exchange energies were evaluated from isodesmic reactions that conserve the number of copper atoms, DMI molecules and EC molecules, so that no free-ion or free-ligand reference is needed and no basis-set superposition error enters the difference. Absolute complexation energies were referenced to the four free ligands and to the solvated Cu+ ion, all computed at the same two levels in the same continuum, with Cu+ taken as a closed-shell singlet. As for the surface work, the complex energies are electronic: no zero-point or thermal correction is included. Vibrational analysis at the same level gave no imaginary mode for DMI, EC, [Cu(DMI)4]+, [Cu(EC)4]+, or [Cu(DMI)2(EC)2]+, and one imaginary mode of 8–9 cm−1 (0.1 kJ mol−1) for [Cu(DMI)3(EC)]+, so the energy of that complex is an upper bound at this level. Zero-point energies from the same frequency jobs shift the four complexation energies in Section 3.7 by +14.0 to +15.2 kJ mol−1, that is, almost uniformly. They change the two ligand-exchange energies in Section 3.7 from −6.6 to −6.3 and from −3.1 to −4.7 kJ mol−1. Neither the ordering nor the sign of any comparison changes, so the electronic values are quoted throughout.

3. Results

3.1. Raman and 27Al NMR Spectra of the Electrolytes

Raman spectra of the electrolytes are shown in Figure 1. In (a), the band at 1702 cm−1 is the carbonyl stretch of DMI and weakens once Cu2O is dissolved, and the band at 349 cm−1, marked by the arrow, is assigned to [AlCl4]−. The four traces in (b), which differ only in EC content, are shown as acquired, without background subtraction, and are, therefore, compared by band position, rather than by band shape. Between 4.6 and 16.1 mol% EC, the [AlCl4]− band remains at 349–350 cm−1 in all four electrolytes.
The 27Al NMR spectrum of the ternary base, reported in [8], resolves four signals: −2.2 ppm (six-coordinate [AlCl2(DMI)4]+), 32 and 66.5 ppm (five-coordinate AlCl3(DMI)2), and 104.6 ppm (four-coordinate [AlCl4]−).

3.2. Conductivity, Density and Viscosity

For the four quaternary electrolytes, measured between 323 and 373 K against the ternary base, conductivity rose with the temperature, and ln σ varied approximately linearly with T−1 (an Arrhenius representation, with T−1 the reciprocal temperature), with the measured points departing from the fits by up to about 5% at 373 K (Figure 2 and Figure 3). Between 323 and 363 K, it lay between 4.19 and 8.23 mS cm−1, slightly above the 3.10–7.98 mS cm−1 of the ternary electrolyte over the same interval; over the full 323–373 K range, the two systems span 4.19–9.27 and 3.10–9.16 mS cm−1. The effect of EC changes with temperature: between 323 and 363 K, the conductivity increased upon adding EC, whereas at 373 K, the measured conductivity of the 4.6, 8.8 and 16.1 mol% systems fell below that of the ternary electrolyte (8.73, 8.67 and 8.92 against 9.16 mS cm−1), and the 12.6 mol% system reached 9.27 mS cm−1. At lower temperatures, the mixtures are more viscous than the ternary base, yet conduct better. Conductivity activation energies were 14.62–15.02 kJ mol−1 (Table 1), below the 21.46 kJ mol−1 of the ternary system. Conduction and viscous flow do not share a single barrier: in every mixture the activation energy for conduction is the larger of the two (14.62–15.02 against 10.90–12.23 kJ mol−1). Against the ternary base, the quaternary mixtures are more viscous at every temperature (6.3–13.2 against 3.9–10.8 mPa s), and yet conduct slightly better and with a lower activation energy, so viscosity alone does not set the conductivity here. Within the quaternary series, the effect of EC is small. Taking the mean molar mass of each mixture as the weighted average of its components, the molar concentration stayed between 9.2 and 10.1 mol L−1 over 323–373 K, and the Walden product Λη, calculated from the conductivities, densities, and viscosities above, fell monotonically as the EC rose, from 6.1 to 4.8 S cm2 mPa s mol−1 at 323 K and from 7.7 to 5.9 at 373 K. The fall in viscosity and the fall in molar conductivity largely compensate, and the four conductivities stay within 4% of one another at 333 K. Bulk transport, therefore, does not distinguish the four electrolytes, and the changes in morphology reported below are not traced to it.
Figure 2. Conductivity of the four quaternary electrolytes between 323 and 373 K.
Figure 3. The plots of ln σ against T−1 for the four quaternary electrolytes.
Table 1. The conductivity–temperature relations and conductivity activation energies of the quaternary electrolytes. The relations are least-squares fits to the eleven temperatures from 323 to 373 K; the conductivity extremes quoted in the text are measured values.
Density fell linearly with temperature (Figure 4), from 1.133 to 1.063 g cm−3 against 1.028–1.082 g cm−3 for the ternary system. Density rose with the EC fraction; the fitted relations are given in Table 2. Viscosity also fell with temperature (Figure 5), lying between 6.3 and 13.2 mPa s against 3.9–10.8 mPa s for the ternary system; within the quaternary series, the viscosity fell as the EC content rose (Table 3). Viscous-flow activation energies were 10.90–12.23 kJ mol−1 (Table 3), below the 20.48 kJ mol−1 of the ternary electrolyte.
Figure 4. Density of the four quaternary electrolytes as a function of temperature.
Table 2. The density–temperature relations of the quaternary electrolytes.
Figure 5. Viscosity of the four quaternary electrolytes as a function of temperature.
Table 3. The viscosity–temperature relations and viscous-flow activation energies of the quaternary electrolytes.

3.3. Reduction in Copper

Figure 6 shows voltammograms recorded at 333 K and 50 mV s−1. The ternary electrolyte without EC, measured in the same cell at the same scan rate under the same conditions, serves as the reference: its onset of reduction is −0.4 V, and its cathodic peak lies at −1.35 V [8]. Adding EC moved the onset of reduction from −0.4 V to about −0.85 V and the cathodic peak from −1.35 to −1.77 V, and an anodic peak appeared at 0.08 V on the reverse scan. The cathodic peak moved 0.42 V negatively, and the onset moved 0.45 V. Complexes of the type [Cu(DMI)(4−x)/2x]+ were identified in the ternary system [8]. The peak current was largest at 8.8 mol% EC and dropped again at 16.1 mol%. The shift is an apparent one between electrolytes measured in the same cell and at the same scan rate (Section 4, point (i)); the 40 kJ mol−1 equivalent used in Section 3.7 assumes unit activity coefficients.
Figure 6. Cyclic voltammograms recorded at 333 K and 50 mV s−1 in the four quaternary electrolytes.

3.4. The Effect of the EC Content on the Structure and Roughness

All four systems gave metallic copper at −1.4 V and 333 K in 2 h, with the zinc reflections coming from the substrate. The current transients in Figure 7 fall into two groups. At 8.8 and 12.6 mol% EC, the current density was higher and continued to rise during deposition; at 4.6 and 16.1 mol%, it was lower, and the curves were flatter. The four conductivities differ by less than 4% at 333 K.
Figure 7. Current transients recorded during deposition at −1.4 V and 333 K from the electrolytes with different EC contents. One continuous recording for each electrolyte over the whole 2 h of deposition; the time axis is in seconds.
Figure 8 shows the morphology at the four EC contents. At 4.6 mol%, the copper grew as cauliflower-like nodules about 35 μm across and unevenly stacked, with local protrusions. At 8.8 mol%, the nodules were about 20 μm across and evenly distributed. At 12.6 mol%, the nodules had refined to about 15 μm. At 16.1 mol%, smoothness stopped improving, and large nodules reappeared locally.
Figure 8. Scanning electron micrographs of copper deposits obtained at −1.4 V and 333 K for 2 h from electrolytes containing (a) 4.6, (b) 8.8, (c) 12.6 and (d) 16.1 mol% EC.
Energy-dispersive analysis (Table 4) gave 95.02 mass% copper at 4.6 mol% EC and 97.06 mass% at 16.1 mol%, with the two intermediate compositions differing little from each other (96.10 and 96.08 mass%). Oxygen fell from 2.83 to 1.79 mass% as EC rose. Aluminium (0.12–0.62 mass%) and chlorine (0.33–0.94 mass%) stayed an order of magnitude below copper, and no aluminium- or chlorine-containing phase appears among the reflections indexed in Section 3.5. Oxygen had no crystalline host of its own in those patterns and is reported as measured: a copper surface picks up oxygen on transfer through air to the microscope, and the analysis does not separate that contribution from the oxygen retained from the electrolyte. Zinc, which comes from the substrate, did not exceed 1.06 mass% in the three coatings, where it was seen and was not detected at 16.1 mol% EC.
Table 4. Energy-dispersive analysis of coatings deposited at −1.4 V from electrolytes with different EC contents (mass%).
Table 5. Energy-dispersive analysis of coatings deposited from the 12.6 mol% EC electrolyte at different potentials (mass%).
The OSP profiles followed the same order (Figure 9), with roughness values of 1.7, 1.3, 0.9 and 2.0 μm at 4.6, 8.8, 12.6 and 16.1 mol% EC. Compared with the 15–43 μm of the ternary system, the roughness of the quaternary coatings was 0.9–2.0 μm. The lowest value, 0.9 μm, was measured at 12.6 mol%. Because the copper concentration falls monotonically across the series, from 0.70 to 0.64 mol L−1, a contribution from that fall cannot be separated from the effect of EC on roughness by these measurements alone; the roughness, however, does not follow it, since the coating is smoothest at 12.6 mol% and roughest at 16.1 mol%, where the copper concentration is lowest.
Figure 9. The OSP profiles of the coatings in Figure 8. The traces are plotted as recorded, each with its own vertical offset; the peak-to-valley values quoted in the text are those returned by the instrument software after its default tilt and form removal.

3.5. The Effect of the Deposition Potential

The 75.6DMI–8.4AlCl3–3.4Cu2O–12.6EC electrolyte was deposited at −1.0, −1.2, −1.4 and −1.6 V for 2 h. Copper was the only phase detected in every coating; the zinc reflections belong to the substrate (Figure 10). Current transients (Figure 11) held steady at −1.0 and −1.2 V, at about 6 and 11 mA cm−2, whereas at −1.4 and −1.6 V, the current climbed throughout and settled only late in the run at −1.6 V. The patterns were recorded to establish that one metallic phase is obtained at every potential, so that the differences in morphology described below are not a difference in phase. All four coatings in Section 3.4 were deposited at −1.4 V; the potential series here used the 12.6 mol% electrolyte. Deposition ran at 333 K for 2 h, at which temperature solid-state interdiffusion between copper and zinc is negligible, so a copper–zinc phase was not expected and none was indexed. The four potentials lie between the onset of reduction (−0.85 V) and the cathodic peak (−1.77 V) measured for this electrolyte in Section 3.3, so the deposit is compared at increasing driving force across that interval.
Figure 10. The X-ray diffraction patterns of copper deposits obtained from the 12.6 mol% EC electrolyte at −1.0, −1.2, −1.4 and −1.6 V.
Figure 11. Current transients recorded at −1.0, −1.2, −1.4 and −1.6 V from the 12.6 mol% EC electrolyte. One continuous recording for each potential over the whole 2 h of deposition; the time axis is in seconds.
Coatings deposited at −1.0, −1.2 and −1.4 V were smooth and of similar roughness; at −1.6 V the nodules were visibly coarser and separated by pores (Figure 12). Copper reached 98.38 mass% at −1.2 V, but only 95.85 mass% at −1.6 V, with oxygen and zinc rising at the higher potential (Table 5): Zn from 0.75 to 1.45 mass% and O from 0.70 to 2.35 mass%.
Figure 12. The scanning electron micrographs of the deposits in Figure 10: (a) −1.0, (b) −1.2, (c) −1.4 and (d) −1.6 V.
OSP (Figure 13) gave a roughness below 1 μm at −1.0, −1.2 and −1.4 V, and about 4.0 μm at −1.6 V. The profile at −1.2 V contains a bend caused by the slight distortion of the specimen and a tilted mounting, not by the coating; the envelope of the profile is the quantity to read. Weighing deposition rate against surface quality, −1.4 V is the most negative potential at which the roughness stays below 1 μm.
Figure 13. The OSP profiles of the deposits obtained from the 12.6 mol% EC electrolyte at different potentials, plotted as in Figure 9.

3.6. Adsorption of EC and DMI on Cu13

Table 6 lists the adsorption energies and geometries, and Figure 14 shows the sites. Figure 14a defines the three sites on a top view of the surface, and panels (b–f) show the optimised geometries. DMI binds through its carbonyl oxygen alone on the top site, at a Cu–O distance of 1.993 Å, and transfers 0.34 e. On the hollow site, the molecule lies across two copper atoms and becomes bidentate, with the carbonyl oxygen at 2.048 Å and one ring nitrogen at 2.08 Å; the adsorption energy becomes −126.9 kJ mol−1, 29 kJ mol−1 more negative than on the top site, with 0.42 e transferred. EC binds through its carbonyl oxygen on all three sites, at Cu–O distances of 2.071, 2.104 and 2.409 Å from top to bridge to hollow, with charge transfers of 0.11, 0.19 and 0.19 e. For EC, the bridge site is the most stable at −62.4 kJ mol−1, the top site lies 1.2 kJ mol−1 above it, and the three-fold hollow is the weakest at −38.7 kJ mol−1. That hollow geometry is also the one most sensitive to the starting orientation: a separate optimisation of the same site converged to another local minimum 26 kJ mol−1 lower, on a slightly different cluster conformation, so the value in Table 6 refers to the geometry reached from the standard starting arrangement. DMI binds more strongly than EC wherever both were computed, by 37 kJ mol−1 on the top site and by 88 kJ mol−1 on the hollow site. A single-point calculation using a continuum solvent on the same geometries (CPCM, ε = 37.6) returns the same ordering—for EC, bridge 0.0, top +2.3, and hollow +22.8 kJ mol−1; for DMI, hollow 0.0 and top +29.0—and stabilises every complex by 49–51 kJ mol−1, so the site preferences do not rest on the gas-phase approximation.
Table 6. Adsorption energy, charge transfer and shortest adsorbate–surface distance for EC and DMI on Cu13(111).
Figure 14. Adsorption of EC and DMI on the Cu13 cluster. (a) The top view of the relaxed cuboctahedral cluster with the top, bridge, and hollow sites marked; the twelve centre–vertex distances lie between 2.377 and 2.396 Å. The 2.556 Å marked in (a) is the ideal fcc nearest-neighbour distance before relaxation. Optimised geometries: (b) DMI on the top site, (c) DMI on the hollow site, (d) EC on the top site, (e) EC on the bridge site, and (f) EC on the hollow site. Geometries at BP86-D3(BJ)/def2-SVP with all of the atoms relaxed; adsorption energies from B3LYP-D3(BJ)/def2-TZVP single-point calculations. The dotted lines join the adsorbate to the surface Cu atoms closer than 2.45 Å. Cu, orange, O, red, N, blue, C, dark grey, and H, white.
The more strongly bound adsorbate also transfers more charge: DMI donates 0.34–0.42 e to the cluster, whereas EC only donates 0.11–0.19 e. The two DMI sites differ in binding mode as much as in energy. On the top site, the molecule stands upright on its carbonyl oxygen, the nearest ring nitrogen lying more than 3.1 Å from the surface; on the hollow site, it lies across two copper atoms with both the oxygen and one nitrogen within bonding distance, and the adsorption energy is 29 kJ mol−1 more negative. EC interacts mainly through one lone pair of its carbonyl oxygen at every site. Its weakest site is the three-fold hollow, where that oxygen is shared between two copper atoms at 2.41 Å, with a longer and more symmetric contact than the 2.104 Å reached on the bridge site. These are relative single-molecule energies and do not fix the coverage under deposition conditions, so a contribution from adsorption at the growth sites is not excluded by them.

3.7. Coordination of Cu(I) by DMI and EC

The reduction-potential shift in Section 3.3 belongs to the copper ion rather than to the surface, and it was examined on the four molecular complexes listed in Table 7. These are not purely model constructs: species of the form [Cu(DMI)(4−x)/2x]+ have been identified in this same ternary electrolyte [8], and the 27Al NMR spectrum reported in [8] resolves the aluminium as four-, five- and six-coordinate chloroaluminate species. A four-coordinate, chloride-free shell is nevertheless the model adopted here rather than a species proved to be the only one; a chloride-containing copper(I) complex was not computed, and this is stated as a limitation (Section 4, point (vi)). In the two single-solvent complexes, the first shell is regular: four Cu–O contacts fall between 2.043 and 2.095 Å, a spread of 0.05 Å for DMI and 0.05 Å for EC.
Table 7. Cu–O distances (Å), CHELPG charge on copper (e), and absolute complexation energies (kJ mol−1) of the four Cu(I) complexes. Geometries at BP86-D3(BJ)/def2-SVP + CPCM (ε = 37.6); charges and energies at B3LYP-D3(BJ)/def2-TZVP + CPCM (ε = 37.6). Complexation energies are referenced to Cu+ and the four free ligands at the same level.
The mixed complexes are not regular. [Cu(DMI)3(EC)]+ holds three DMIs at 1.963–2.125 Å, and one EC at 2.367 Å; [Cu(DMI)2(EC)2]+ holds its two DMIs at 1.981 and 2.115 Å, and its two ECs at 2.028 and 2.303 Å. In both, the longest contact is to an EC oxygen, 0.19–0.24 Å longer than the longest DMI contact in the same complex.
The CHELPG charge on copper hardly moves with the composition of the shell: +0.62 e in [Cu(DMI)4]+, +0.64 e in [Cu(EC)4]+, +0.53 e in [Cu(DMI)3(EC)]+, and +0.64 e in [Cu(DMI)2(EC)2]+, a spread of 0.1 e. By this measure, the two solvents donate comparable electron density to the ion, and the spread between the complexes exceeds the difference between the single-solvent ones.
Ligand exchange (Table 8) is slightly downhill in both directions that conserve stoichiometry. Exchanging two ECs for two DMIs, [Cu(DMI)4]+ + [Cu(EC)4]+ → 2 [Cu(DMI)2(EC)2]+, gives −6.6 kJ mol−1; exchanging one, [Cu(DMI)4]+ + [Cu(DMI)2(EC)2]+ → 2 [Cu(DMI)3(EC)]+, gives −3.1 kJ mol−1. Per EC entering the shell, the exchange energy is −3.3 and −3.1 kJ mol−1. Those numbers are electronic energies of single points taken on BP86 geometries and carry no zero-point or thermal correction, and the two values agree to within 0.3 kJ mol−1.
Table 8. Two isodesmic ligand-exchange reactions that conserve the numbers of copper atoms, DMI molecules, and EC molecules, at B3LYP-D3(BJ)/def2-TZVP + CPCM (ε = 37.6) on BP86-D3(BJ)/def2-SVP + CPCM geometries.
The isodesmic reactions compare the two solvents with each other but do not say how strongly either binds the ion. Once the ligands and the ion are computed at the same levels, the absolute complexation energies follow: −318.7, −299.6, −277.4 and −229.5 kJ mol−1 for [Cu(DMI)4]+, [Cu(DMI)3(EC)]+, [Cu(DMI)2(EC)2]+ and [Cu(EC)4]+ (Table 7). Per ligand, the series falls monotonically, from −79.7 to −74.9 and −69.4 to −57.4 kJ mol−1, so replacing a DMI with an EC raises the energy by 19.1, 22.2 and 47.9 kJ mol−1 in the three successive substitutions, that is 19, 22 and 24 kJ mol−1 per EC, and DMI binds the ion about 1.4 times as strongly as EC. That ratio has the same sign as the factor of about two found on the Cu13 surface in Section 3.6 but is somewhat smaller. The absolute values rest on a continuum description of a concentrated electrolyte and on a bare reference ion, so they are read here as a ranking of the two solvents rather than as free energies of complexation.
The longest Cu–O contact in the two mixed complexes is 2.30–2.37 Å, so EC does take part in the first coordination shell of copper(I). A peak shift of 0.42 V corresponds to nFΔE = 40 kJ mol−1 for a one-electron transfer (n = 1 for Cu(I) → Cu(0)), and it is negative, so an EC-containing complex would have to be 40 kJ mol−1 more stable than the DMI one; the calculations put it 19–24 kJ mol−1 less stable per EC. The static calculations here do not identify the path by which the mixed complex reduces.

4. Discussion

With EC present, the nodules fell from about 35 to about 15 μm, and the peak-to-valley roughness from 1.7 to 0.9 μm; the onset of reduction moved from −0.4 to about −0.85 V and the cathodic peak by 0.42 V; and the [AlCl4]− band of the four quaternary electrolytes remained at the same position as in the ternary base, so the aluminium coordination was not rebuilt. EC enters the first coordination shell of copper(I) and, through that change in the ion rather than in the interface, turns the rough coating of the ternary electrolyte into one of finer nodules, with a working window at 12.6 mol%.
Additive design for copper plating has been built on adsorption. Schmidt [19] set out the mechanistic guidelines in these terms; Han et al. [20] suppressed deposition with alkyl-terminated PEG that adsorbs on the copper surface; and Jin et al. [21] combined two molecules so that one anchors and the other blocks. Judged by that criterion, EC would be a poor additive: on Cu13(111), it adsorbs at 31–62% of the energy of DMI on sites where both were computed, transferring 0.11–0.19 e against 0.34–0.42 e. It nevertheless refines the coating. In a solvent that coordinates the metal ion as strongly as DMI does, the interface is, therefore, not the only place where a second component can act, and a criterion developed for aqueous baths does not transfer unchanged to solvated ionic liquids.
In electrolytes of this kind, EC has so far appeared mainly as a solvent or co-solvent: Guan et al. [12] electrodeposited zinc from EC–ZnCl2, Zhang et al. [13] electrodeposited magnesium in DMI, and Lu et al. [15] used a DMI-based electrolyte in zinc batteries. These studies attribute the effect to the solvation shell and to transport, without following the shell through to the morphology of the deposit. In our earlier ternary work [8], the same electrolyte at the same potential gave agglomerates of 20–40 μm, against nodules of about 15 μm once EC entered the shell.
Why a weak ligand shifts the deposition potential is an open question. EC does enter the first shell: in the mixed complexes, the longest Cu–O contact belongs to EC, 0.19–0.24 Å longer than the longest DMI contact. It is not held there firmly: each EC that replaces a DMI raises the complexation energy by 19–24 kJ mol−1, and the isodesmic exchanges run downhill by only 3.1 and 6.6 kJ mol−1, so entry costs little and stabilises little. A shift of 0.42 V would require the EC-containing complex to be about 40 kJ mol−1 more stable than [Cu(DMI)4]+, and the calculations give the opposite sign. The shift is, therefore, more likely to lie in the path by which the mixed complex is reduced, with ligand loss and reorganisation ahead of the electron transfer, than in the thermodynamics of the shell.
Limitations of the present data. Six points bound what the results above support, and they are stated here rather than left implicit in the individual sections.
(i) The aluminium wire served as the reference in every electrolyte, so the potentials are comparable within this series, but were not calibrated against an external standard, and no allowance was made for uncompensated resistance; the 0.42–0.45 V difference is consequently an apparent shift between electrolytes measured in the same cell, and the interpretation offered above is one of several consistent with it.
(ii) One specimen was prepared for each condition; the three profile measurements per specimen describe the surface rather than the reproducibility of the deposition, and the 12.6 mol% composition is the condition examined in most detail rather than a proven optimum. The four coatings were compared at a fixed potential and time, rather than at a fixed charge, so a difference in the extent of deposition is not separated from a difference in growth mode.
(iii) The peak-to-valley values are those returned by the instrument software after its default tilt and form removal, and the profile at −1.2 V in Figure 13 is distorted; neither was re-processed here, so the roughness values are reported as acquired.
(iv) The optical profiles were recorded with a 20 μm sampling interval, comparable to the size of the features themselves, and the diameters quoted from the micrographs are apparent sizes of surface features rather than crystallographic grain sizes; no size distribution was measured.
(v) Coating thickness was not measured, so the detection of zinc by energy-dispersive analysis at 20 kV is reported as an observation and is not used to infer incomplete coverage.
(vi) In the calculations, no counterpoise correction was applied, no cluster larger than Cu13 was used, and no chloride-containing copper complex was evaluated, so the calculated energies are bounded rather than tested.

5. Conclusions

(1) EC raises the conductivity and the viscosity of the melt together: 4.19–8.23 mS cm−1 between 323 and 363 K and 6.3–13.2 mPa s between 323 and 373 K, at densities of 1.063–1.133 g cm−3; the conductivity and viscous-flow activation energies fall to 14.62–15.02 and 10.90–12.23 kJ mol−1.
(2) EC shifts the reduction in copper to more negative potentials: onset from −0.4 to about −0.85 V and cathodic peak from −1.35 to −1.77 V, the peak current being largest at 8.8 mol% EC.
(3) At −1.4 V, the coating is finest at 12.6 mol% EC: nodules fall from about 35 to about 15 μm, and the peak-to-valley roughness from 1.7 to 0.9 μm, whereas at 16.1 mol%, the roughness returns to 2.0 μm. For the 12.6 mol% electrolyte, the roughness stays below 1 μm from −1.0 to −1.4 V and reaches about 4.0 μm at −1.6 V. The lowest roughness was obtained at 12.6 mol% EC, −1.4 V, 333 K, 2 h.
(4) Density functional theory points the same way for both sides: EC binds more weakly than DMI to the surface and to the ion alike. On Cu13(111), DMI adsorbs at −126.9 kJ mol−1 on the hollow site as an oxygen–nitrogen chelate and at −98.1 kJ mol−1 on the top site through the carbonyl oxygen alone, with 0.34–0.42 e transferred, whereas EC adsorbs at −38.7 to −62.4 kJ mol−1 with 0.11–0.19 e, and its top and bridge sites lie within 1.2 kJ mol−1 of each other. A continuum-solvent check returns the same ordering. In the coordination shell, EC does enter, with the longest Cu–O contact of the mixed complexes being EC at 2.30–2.37 Å, but each substitution raises the complexation energy by 19–24 kJ mol−1, the opposite of the 40 kJ mol−1 stabilisation that a 0.42 V shift would require. EC, therefore, acts on the coordination environment of the copper ion rather than on the electrode surface: the refinement from about 35 to about 15 μm and the 0.42 V shift accompany its entry into that shell. The comparison is offered as the reading of the calculations most consistent with the electrochemical and spectroscopic evidence; a relative single-molecule energy does not fix the coverage under deposition conditions, and based on the present evidence, adsorption at the growth sites cannot be excluded (Section 3.6).

Supplementary Materials

The following supporting information can be downloaded at: https://www.mdpi.com/article/10.3390/met16121283/s1. File S1: metals-16-01283-s001.zip (ORCA input files, optimised coordinates, absolute energies and convergence settings of all calculations in Section 2.5). A README file, included in the archive, lists every member and the level of theory of each job.

Author Contributions

Conceptualization, P.G.; methodology, P.G. and Y.L.; software, P.G.; validation, P.G.; investigation, P.G., Y.L., S.P., X.Y. (Xiaoming Yang) and X.Y. (Xingxing Yu); formal analysis, P.G.; data curation, P.G. and S.P.; resources, Y.L.; writing—original draft preparation, P.G.; writing—review and editing, P.G., Y.L., Z.W., X.Y. (Xiaoming Yang) and X.Y. (Xingxing Yu); visualization, P.G., S.P., Z.W. and X.Y. (Xingxing Yu); supervision, P.G.; project administration, P.G.; funding acquisition, P.G. All authors have read and agreed to the published version of this manuscript.

Funding

This research was funded by Jingchu University of Technology through the research project “Corrosion Protection Mechanism of Steel Pipeline Bodies for Oil Transportation” (grant number YYZ202641).

Data Availability Statement

The original contributions presented in this study are included in the article and its Supplementary Materials. Further inquiries can be directed to the corresponding author.

Acknowledgments

The authors acknowledge the use of DeepSeek, a generative artificial intelligence tool, for language editing of this manuscript. The experimental design, all measurements, the calculations, the interpretation of the results, and the conclusions are the work of the authors, who reviewed and take full responsibility for the content of this paper.

Conflicts of Interest

Yongqi Liu was employed by Aviation Key Laboratory of Science and Technology on Structure Corrosion Prevention and Control, China Special Vehicle Research Institute, Jingmen 448035, China. The remaining authors declare that the research was conducted in the absence of any commercial or financial relationships that could be construed as a potential conflict of interest.

References

  1. Xu, P.; Lu, W.; Qiao, L.; Zhu, Q.; Liu, H.; Song, K. Advanced Design of Electrodeposited Copper Foil: Modulating Grain Growth and Microstructure to Achieve Ultrahigh Mechanical Properties. J. Alloys Compd. 2025, 1040, 183680. [Google Scholar] [CrossRef] [Scilit]
  2. Brooks, N.R.; Schaltin, S.; Van Hecke, K.; Van Meervelt, L.; Binnemans, K.; Fransaer, J. Copper(I)-Containing Ionic Liquids for High-Rate Electrodeposition. Chem. Eur. J. 2011, 17, 5054–5059. [Google Scholar] [CrossRef] [Scilit]
  3. He, W.; Shi, Z.; Liu, F.; Yang, S. Electrodeposition of Copper Metal from the 1-Ethyl-3-methylimidazolium Fluoride ([EMIM]F)-urea-H2O System Containing CuO. Electrochemistry 2020, 88, 253–255. [Google Scholar] [CrossRef] [Scilit]
  4. Shaaban, I.A. Conformational Analysis, Infrared/Raman Spectral Assignment, and Electronic Structural Studies of 1,3-Dimethyl-2-imidazolidinone Using Quantum Chemical Calculations. J. Mol. Struct. 2019, 1175, 708–720. [Google Scholar] [CrossRef] [Scilit]
  5. Fortunato, B.; Mirone, P.; Fini, G. Infrared and Raman Spectra and Vibrational Assignment of Ethylene Carbonate. Spectrochim. Acta A 1971, 27, 1917–1927. [Google Scholar] [CrossRef] [Scilit]
  6. Paterno, D.; Rock, E.; Forbes, A.; Iqbal, R.; Mohammad, N.; Suarez, S. Aluminum Ions Speciation and Transport in Acidic Deep Eutectic AlCl3 Amide Electrolytes. J. Mol. Liq. 2020, 319, 114118. [Google Scholar] [CrossRef] [Scilit]
  7. Li, H.; Wu, Q.; Liu, Y.; Bao, J. Acidity Quantification and Structure Analysis of Amide-AlCl3 Liquid Coordination Complexes for C4 Alkylation Catalysis. Molecules 2023, 28, 7857. [Google Scholar] [CrossRef] [Scilit]
  8. Guan, P.; Liu, A.; Zhang, X.; Kang, H.; Su, K.; Meng, Q.; Liu, Z.; Shi, Z. Electrodeposition of Copper in 1,3-Dimethyl-2-imidazolidinone–AlCl3–Cu2O Ionic Liquid. Chin. J. Nonferrous Met. 2024, 34, 268–278. (In Chinese) [Google Scholar] [CrossRef]
  9. Liu, A.M.; Guo, M.X.; Lü, Z.Y.; Zhang, B.G.; Liu, F.G.; Tao, W.J.; Yang, Y.J.; Hu, X.W.; Wang, Z.W.; Liu, Y.B.; et al. Electrochemical Behavior of Tantalum in Ethylene Carbonate and Aluminum Chloride Solvate Ionic Liquid. Trans. Nonferrous Met. Soc. China 2020, 30, 2283–2292. [Google Scholar] [CrossRef] [Scilit]
  10. Zhang, B.; Wang, L.; Liu, Y.; Zhang, Y.; Zhang, L.; Shi, Z. AlCl3-Assisted Dissolution of NdCl3 in Organic Solvents for Nd Refining. Sep. Purif. Technol. 2021, 276, 119416. [Google Scholar] [CrossRef] [Scilit]
  11. Liu, A.M.; Guo, M.X.; Shi, Z.N.; Liu, Y.B.; Liu, F.G.; Hu, X.W.; Yang, Y.J.; Tao, W.J.; Wang, Z.W. Physicochemical Properties of 1,3-Dimethyl-2-imidazolinone–ZnCl2 Solvated Ionic Liquid and Its Application in Zinc Electrodeposition. Trans. Nonferrous Met. Soc. China 2021, 31, 832–841. [Google Scholar] [CrossRef] [Scilit]
  12. Guan, P.; Li, H.; Zhang, X.; Shi, Z.; Liu, A. Electrodeposition of Zinc from Ethylene Carbonate–ZnCl2 Electrolyte System. Ionics 2023, 29, 2947–2958. [Google Scholar] [CrossRef] [Scilit]
  13. Zhang, X.; Guan, P.; Kang, H.; Meng, Q.; Liu, A.; Liu, F.; Shi, Z. Theoretical and Experimental Studies on the Electrodeposition of Magnesium in 1,3-Dimethyl-2-imidazolidinone Organic Solvent at Room Temperature. Ionics 2024, 30, 4837–4844. [Google Scholar] [CrossRef] [Scilit]
  14. Ismail, H.K. Electrodeposition of a Mirror Zinc Coating from a Choline Chloride-Ethylene Glycol-Based Deep Eutectic Solvent Modified with Methyl Nicotinate. J. Electroanal. Chem. 2020, 876, 114737. [Google Scholar] [CrossRef] [Scilit]
  15. Lu, K.; Chen, C.; Wu, Y.; Liu, C.; Song, J.; Jing, H.; Zhao, P.; Liu, B.; Xia, M.; Hao, Q.; et al. Versatile 1,3-Dimethyl-2-imidazolidinone Electrolyte Additive: Enables Extremely Long Life Zinc Metal Batteries with Different Substrates. Chem. Eng. J. 2023, 457, 141287. [Google Scholar] [CrossRef] [Scilit]
  16. Neese, F. The ORCA Program System. WIREs Comput. Mol. Sci. 2012, 2, 73–78. [Google Scholar] [CrossRef] [Scilit]
  17. Neese, F. Software Update: The ORCA Program System—Version 6.0. WIREs Comput. Mol. Sci. 2025, 15, e70019. [Google Scholar] [CrossRef] [Scilit]
  18. Grimme, S.; Ehrlich, S.; Goerigk, L. Effect of the Damping Function in Dispersion Corrected Density Functional Theory. J. Comput. Chem. 2011, 32, 1456–1465. [Google Scholar] [CrossRef] [Scilit]
  19. Schmidt, R. Mechanistic Understanding of Copper Electrodeposition and Additive Design Guidelines. ECS Adv. 2026, 5, 043001. [Google Scholar] [CrossRef] [Scilit]
  20. Han, C.; Zhai, Y.; Chen, Y.; Li, J.; Cai, W.; Zhou, Z. Alkyl-Terminated PEG Suppressors for Copper Electroplating and Their Hydrophilic and Hydrophobic Properties. Surf. Coat. Technol. 2024, 484, 130848. [Google Scholar] [CrossRef] [Scilit]
  21. Jin, L.; Wang, Z.Y.; Cai, Z.Y.; Yang, J.Q.; Zheng, A.N.; Yang, F.Z.; Wu, D.Y.; Zhan, D. 1-(2-Pyridylazo)-2-naphthol as a Synergistic Additive for Improving Throwing Power of Through Hole Copper Electronic Electroplating. J. Ind. Eng. Chem. 2023, 125, 269–276. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.