Skip to Content
PolymersPolymers
  • Article
  • Open Access

27 November 2026

27 Pages

Fast-Setting Silicate Hybrid Binders for Foundry Core and Mould Materials

,
and
1
Faculty of Science, The University of Melbourne, Parkville, VIC 3010, Australia
2
Faculty of Mechanical Engineering and Mechatronics, West Pomeranian University of Technology in Szczecin, 70-310 Szczecin, Poland
*
Authors to whom correspondence should be addressed.
This article belongs to the Section Polymer Applications

Abstract

This paper presents the findings of an investigation into the seminal concept of crosslinking and self-setting hydrated silicate binders such as sodium and potassium silicates or geopolymers using CO2 released when isocyanates, such as MDI and TDI, react with the intrinsic water within these binders. Specifically, practical utilisation of this process for the fabrication of refractory composites such as moulding sands is investigated. The resultant composites exhibit: (i) rapid cure, (ii) compressive strength, up to 3.0 to 3.5 MPa at low binder contents (2.5–3.5%) and (iii) low fracture energy, approximately 100 joules, which is 400% lower than that of identical composites cured by CO2 gas purge. It is clearly demonstrated that sodium silicate films exhibit identical strength regardless of whether they are crosslinked by CO2 gas purge or its latent form released from NCO on contact with silicate’s intrinsic water—which proves that both technologies are self-consistent. The practical outcomes of this work found industrial applications in the Polish foundry industry, including Zamech/Alston Power Elblag, Warsaw Steel Works/Warsaw (Huta ArcelorMittal), Ferrum SA (Ferrum Steel Works)/Katowice, and Zabrze Steel Works SA/Zabrze. Preliminary results demonstrate the potential of this novel technology for additive manufacturing applications, including the 3D printing of precision moulds and cores.

1. Introduction

Binders for mould and core materials (colloquially: moulding sands) are subject to ever-increasing demands in order to achieve better casting quality. A good binder should exhibit the following performance criteria:
  • good adhesive properties and high cohesive strength achievable with a low binder content;
  • defect-free castings with minimal labour requirements in the preparation and processing of moulding and core materials, as well as during the mould shakeout, core knock-out and subsequent cleaning of castings;
  • limited or no environmental impact.
Apart from environmental friendliness, these requirements are met by only a few organic binders (furan, polyester and some urea resins). The key advantage of moulding materials with these binders is undoubtedly their excellent knock-out behaviour. Even complex and thin-section cores can be removed from the casting cavities without difficulty.
However, the use of organic binders is often limited by their toxic properties. Particularly hazardous are the gaseous decomposition products, such as hydrogen cyanide, carbon monoxide and amines, which are formed as a result of pyrolysis at high temperatures. Some harmful components of organic binders are also washed out of the deposited waste sand into the groundwater by rain.
On the other hand, inorganic binders such as sodium and potassium silicates and geopolymers or cements are odourless, produce near-zero emissions compared with organic resins during metal casting and hence attract growing attention of the global foundry industry.
The key representatives of this group are moulding sands bonded by sodium silicates. These are usually cured by powdered hardeners containing calcium silicates or by a purge with CO2 gas or its mixture with hot air. These materials, however, are burdened by numerous disadvantages, i.e.,:
  • very poor knock-out (demoulding) behaviour;
  • high susceptibility to form surface defects (particularly in steel and cast iron parts) due to binder sintering by high-temperature/low-viscosity molten metal and its affinity with silica sand;
  • inadequate lateral rigidity (consequence of low high-temperature bending strength) during metal casting and solidification.
These drawbacks limit industrial applications of liquid sodium silicates to the production of uncomplicated moulds and cores.
The above factors turned our interest to the development and validation of a novel concept of hybrid inorganic/organic binders comprising:
(1)
Sodium or potassium silicate and/or geopolymer as an inorganic phase, and
(2)
An ‘active’ organic constituent in the form of isocyanates performing a complex dual role as follows:
(i)
the reservoir of a latent hardener, CO2, which is released from isocyanates upon their contact with water, an intrinsic constituent of hydrated silicates, as well as
(ii)
a latent reservoir of a ‘post-reaction’ organic residue (polyurea), which is the by-product of the reaction of water with isocyanates. These (dispersed) residues drastically reduce fracture energy of the binder film including inter-granular pendular bridges connecting individual filler particles within the mould and cores (in its ‘pure form’, sodium silicate is sintered on contact with molten steel or cast iron, making the mould notoriously difficult to fracture on casting demoulding).
The overall aim of the research presented and discussed in the current paper is two-fold: (1) to present and validate our hypothesis that silicate binders represented in our work by sodium silicate can be viably crosslinked by CO2 gas delivered not externally as the decompressed gas flux purging the mould and/or cores, but by that generated in situ from the ingredient of the binder in the form of isocyanate, and (2) to ensure the technological properties of the developed moulding sands meet industrial standards, thereby enabling their application in the foundry industry.
It is also necessary to highlight the fact that in our paper we do not attempt to elucidate the details of all observed outcomes and underlying phenomena nor aim to develop a holistic model of these complex, interrelated phenomena occurring within the bulk and at the passive and active interfaces between materials participating in the formation of cohesively consolidated and highly permeable composite materials designated as moulding sands (moulding mixtures).

2. The Structure and Key Properties of Permeable Moulding Sand Composites

The key functional properties of particulate-filled permeable moulding sands are controlled by their 3-dimensional (3D) packing structure and morphology, and their chemical composition. These, in turn, depend on the following: (i) the filler particle chemistry, its size and size distribution, and packing density, (ii) the type of the binder and inter-particle bonding mechanism(s), e.g., physical (van der Waals) interactions or chemical bonding, and (iii) the 3-dimensional packing configuration of sand particles and geometry of connectivity between adjacent particles by either: (a) continuous or patchy binder film around the surface of each particle, or (b) the network of individual pendular bridges connecting adjacent filler particles. The geometrical aspects of some of these issues are depicted in Figure 1.
Figure 1. Schematics of internal structure of alternative categories of particulate-filled composites: (a) engineering composite (non-permeable) and (b–d) permeable composites, e.g., moulding sands. NOTE: red arrow brings attention to the actual appearance of inter-particle pendular bridges in an FCC-packed composite filled by spherical particles, 0.5 mm in diameter, bonded by a liquid binder used at 2.7%.
The structure of typical engineering composite reinforced with spherical particulate filler packed at the maximum achievable packing density (74%), Face-Centred Cubic packing, FCC is schematically depicted in Figure 1a. Filler particles are consolidated by 26% of binder (matrix material) completely filling all pores (cavities) between particles.
A model-permeable composite material, FCC packed with 74% of spherical filler particles illustrated in Figure 1b demonstrates a system resembling the structure of moulding sands bonded by liquid organic [1,2,3,4] or inorganic binders [5,6], with all particles coated by a thin continuous binder film. A photo in Figure 1c shows actual inter-particle pendular bridges in an FCC-packed composite filled by spherical particles, 0.5 mm in diameter, bonded by a liquid binder used at 2.7%. This example represents an optimum structure of moulding sands facilitating maximisation of composite strength whilst minimising the binder contents. Figure 1d, in turn, illustrates pendular bridges between spherical particles in a permeable model composite with the cubic lattice compacting configuration exhibiting packing density of 52.36% [7].
Achieving high quality, dimensionally accurate castings exhibiting smooth surface and devoid of pinhole defects necessitates the use of suitable binder system enabling: (i) high-level structural integrity of mould and cores through adequate strength and thermo-mechanical stability of composite dimensions [8,9] on exposure to high temperature and dynamic and static pressures [2] exerted by molten metal in mould cavity, (ii) fast-speed and low-cost fabrication of moulds and cores, (iii) minimal gaseous by-product formation and kinetics during the binder and residual moisture decomposition [9,10,11,12,13], (iv) adequate composite permeability enabling rapid evacuation of gaseous by-products evolving in mould cavity upon exposure to liquid metal at initial stages of its flow and solidification, whilst simultaneously preventing molten metal ingress into inherently porous composite structure, (v) low fracture energy of composite (moulding sand) essential for good mould/core system ‘collapsibility’ (shakeout) in the course of solidified casting removal and cleaning [2], and (vi) absence of sintered sand residues adhering to the surface of casting.

3. Principal Objectives

The principal objective of research presented in this paper was the development of rapid-setting, room-temperature cured moulding sands bonded with sodium silicate binders. These were required and indeed, demonstrated to fully satisfy all industrial standards and performance criteria pre-set by this technology end-users. This includes all requirements listed in Section 2 above, complemented by the following additional attributes: (i) effective inhibition of mould/core material shrinkage on exposure to high-temperature metal, (ii) absence of pinhole defects, and (iii) easy collapsibility of cores, which needed to be comparable with that shown by cores fabricated with the use of furan-bonded moulding sands.
It was demonstrated that upon the use of the new curing agent (isocyanate) the liquid silicate binder content can be practically reduced to between 2.2 and 2.5% by mass. As required by end-users, the shake out and knock-out performance of moulds and cores was significantly improved and assessed as comparable with that exhibited by same products fabricated with the use of furan resins.
The technology developed in this work initially aimed industrial applications for mould- and core-making materials utilised in production of medium-sized, complex-shape castings made of low-alloy steels and cast-iron for components of naval engine blocks and heavy-machinery gear boxes. Ultimately, the practical outcomes of this work were commercialised in Polish foundry industry [14,15,16,17], e.g.,: Ferrum Steel Works/Katowice, Warsaw Steel Works/Warsaw (currently Huta ArcelorMittal), Zabrze Steel Works/Zabrze and Zamech Elblag.
The authors would also like to highlight that:
(i)
The overall aim of our research presented and discussed in the current paper is to present and validate our hypothesis that liquid silicate binders (represented in this work by sodium silicate) can be viably crosslinked by CO2 gas delivered not externally as the gas flux purging the mould and/or cores in the process of forming a cohesively integrated composite material suitable for foundry applications, but by that an alternative means, as a by product CO2 generated in situ from one of the ingredients of the binder, i.e., isocyanate, and
(ii)
Within the scope of the current paper we do not attempt to elucidate the details of all observed outcomes and underlying phenomena nor aim to develop a holistic model of these complex, interrelated phenomena occurring within the bulk and at the passive and active interfaces between materials participating in the formation of cohesively consolidated and highly permeable composite materials designated as moulding sands.
Further outcomes of this research, which is also beyond the scope of the current paper, will be a subject of separate publications applicable to emerging transformational technologies such as 3D inkjet printing of moulds and cores, which currently revolutionise the process of mould and core manufacturing.

4. ‘State-of-The Art’ Overview: The Key Environmental and Technological Issues

There is a push for the development of liquid silicate binder systems exhibiting capabilities of organic resins regarding: mould/core structural integrity and shape retention; post-solidification mould shakeout and core knock-out and high casting quality; and all combined with low ecological impact footprint associated with inorganic nature of such binders.
In their recent paper, Garitaonandia et al., 2025 [18], presented an outcome of a systematic study comparing hazardous emissions from various foundry binder systems: organic resins (phenolic urethane, furan, and alkaline-phenolic) and compared these with those utilising inorganic alternatives (sodium silicate and geopolymer) during pilot-scale iron casting trials.
Their work involved approximately 50 kg iron alloy castings cast in moulds comprising two 50 kg semi-moulds with cores (~5 kg) fabricated from designated core and mould mixtures. This provided realistic representation of medium-sized industrial castings with the sand-to-metal ratio about 2:1.
Volatile organic compound (VOC) emissions including hazardous substances investigated were: (1) BTEX compounds (Benzene, Toluene, Ethylbenzene and Xylene) and (2) polycyclic aromatic hydrocarbons (PAHs).
The results of this work clearly demonstrated that inorganic binder systems (sodium silicate and geopolymer) significantly reduced hazardous emissions compared to organic resins (phenolic urethane, furan, and alkaline-phenolic) achieving reductions of over 90% in BTEX compounds and over 94% in PAHs [18].
Specifically, the furan binder system produced the highest BTEX emissions (323.7 mg/kg) and PAH emissions (5.86 mg/kg), while the inorganic sodium silicate system yielded the lowest BTEX (6.3 mg/kg) and PAH emissions (<0.046 mg/kg) [18].
The above outcomes form a platform substantiating growing interest in and resurgence of inorganic binders driven by both, increasingly stricter environmental demands and the need for improved casting performance. The industrial drive is led by the aluminium casting sector where modified silicate binders have been successfully implemented in the production of automotive components, such as engine heads and blocks [19]. Their success in aluminium foundries has sparked growing interest in transferring these benefits to iron and steel casting operations [20].
However, these materials exhibit numerous practical disadvantages, such as: very poor knock-out behaviour, a tendency to form surface defects (particularly in steel and cast iron parts), and have inadequate lateral rigidity (consequence of insufficiently low high-temperature bending strength) during melt casting and solidification.
The above drawbacks limit the application of liquid sodium silicates to the production of uncomplicated moulds and cores. As highlighted in [18] by Garitaonandia et al., in 2020 only 1% of European foundries used inorganic binders for mould and core manufacture predominantly in light metal foundries. According to these data, in Germany, out of 297 foundries just 11 use inorganic binders, primarily in the aluminium sector [21].
In their comprehensive reviews, Holtzer & Kmita [22] and Zi-tian Fan et al. [23] provide in-depth ‘state-of-the-art’ analyses of technical and performance-related details of silicate-bonded rapid-cure moulding sands.
Amongst other systems, as discussed in more detail below, the following three primary categories of hardening processes used for silicate binders are focused on in references [22,23]: (i) CO2 process: the mould/core mixture purge by carbon dioxide converts alkaline binder into silica gel triggering rapid strength increase at room temperature (RT); (ii) ‘No-bake’ ester cure: liquid organic esters (e.g., glycerol diacetate, etc.) mixed with the silicate binder initiate its setting at RT. These include commercially available products such as [24] Carset, Sidur, Gisacodur, Flotex, Flodur, etc., which offer notably better handling properties (particularly: better shakeup and knock-out behaviour), and (iii) hardening sodium silicate by physical factors, such as mineralized activators, hot air, irradiation by microwave energy, and proprietary hardeners comprising (amongst other ingredients) combination of phosphate, silica and borate groups.
Holtzer & Kmita [22] and Zi-tian Fan et al. [23] provide the following technical details in their comprehensive ‘state-of-the-art’ analyses of silicates-bonded rapid-cure moulding sands.

4.1. Sodium Silicate Cured by CO2 Purge

In this process sodium silicate water-based solutions (water glass) of a module 2.0–2.8 are used. Water glass in amounts 2–4% is mixed with sands and blown through by carbon dioxide, which is of a weak acidic character. The CO2 amount used should not exceed 1–2% parts by mass of sand and blowing through time should be from 10 to 60 s. Cores are usually made in the shooting machines. Under the CO2 influence, the sand hardening occurs in a short time. The surface hardening reaction by means of CO2 is also essential at other hardening methods [24,25,26].

4.2. Sodium Silicate Cured by Organic Esters System

Moulding sands with sodium silicate hardened by a mixture of esters, at a room temperature are currently finding the most intensive application out of all moulding sands with inorganic binders (apart from bentonite) for producing foundry moulds and cores.
A mixture of esters, typically amounting to 10%, is usually used as a hardener in this process, e.g., glycerine and ethylene esters, e.g.,: glycerine mono-, di-, and triacetate and glycol diacetate [24,25,27,28,29]. The main advantage of applying esters as sodium silicate hardeners is the possibility of decreasing the amount of water glass added to sands by up to 50% (only 2.0–3.0% of water glass can be used), as compared to other sodium silicate-based sands. This favourably influences decreasing the final strength of sands made in this technology [25]. Moulding sands made in this technology are applied mainly in cast steel foundries for making large- and medium-size castings.

4.3. Sodium Silicate Hardened by Physical Factors

4.3.1. INOTEC® Process

The INOTEC system (ASK Chemicals) [30,31] is the new, 100% inorganic, and emission-free binder variant based on water glass. It is typically used for aluminium, other non-ferrous metals alloys and cast iron the production of engine blocks and cylinder heads. The binder comprises a mixture of liquid silicates (1.8–2.5%), mineralized activators (0.1–1.0%), and, if needed, mineral additives (1–30%). No fumes are generated during casting process. The binder hardening occurs due to dehydration in the heated core box by purging with hot air of a temperature 180–200 °C.

4.3.2. CORDIS® Process

CORDIS® (Hüttenes-Albertus International) is the inorganic binder, in which the only solvent is water [32,33]. The binder is comprises modified aqueous solution of sodium silicates and the pulverised additive (Anorgit); a combination of phosphate, silica and borate groups.

4.3.3. AWB® Process

The AWB® technology (developed by the Minelco, Nemak Dillingen, and Audi Company) [34,35] is utilising modified sodium silicate of a decreased viscosity. Due to this a binder can be more easily mixed and homogenised with the sand filler. The binder hardening, with sand grains interconnected by silicate bridges, occurs as a result of a physical water removal, which is performed in two stages, i.e., (1) the initial hardening occurs in the core box (at 140–200 °C) connected with the vacuum pump for the water vapour removal. After ~10–60 s, depending on the core size and shape, the hardened shell is formed, strong enough to remove the core from the core box and to transport it; (2) the final hardening is performed by low power microwave radiation. Stage (2) is crucial, since any water remaining within the core can dissolve binder bridges, thus shortening the cores storage time.

4.3.4. SOLOSIL TX Process

The SOLOSIL TX binder (FOSECO) is the inorganic thermosetting binder based on liquid sodium silicate and exhibits properties comparable to organic binders whilst remaining environment-friendly. This binder consists of the following two components: solution of modified sodium silicate (approx. 2%) of a module of 2.0–2.4) and fine powder containing various minerals [36,37].
The hardening occurs in the core box heated to 150 °C. The strength of cores is significantly improved by the addition (to the binder) of an appropriate additive, reducing also residual moisture content within the cured binder.

5. Theoretical Principles of the Process

5.1. Principal Features of the Novel Liquid Silicate-Bonded Composites

The basic reaction of sodium silicate silicification triggered by CO2 [38] is expressed by the following equation:
m Na 2 O · n SiO 2 · x H 2 O + m CO 2 sodium   silicate → n SiO 2 · x − y H 2 O + m Na 2 CO 3 + y H 2 O silica   gel   Hydro -   or   xerogel
When hardened through the above mechanism, the silicate film produces exceptionally tough ‘adhesive’, frequently sintered onto the sand surface upon exposure to molten metal during castings fabrication. The resultant poor knock-out behaviour during demoulding hinders broader industrial acceptance of this otherwise advantageous process.
To improve the shakeup/knock-out properties of moulding mixtures utilising hydrated silicates, various organic compounds, particularly water-soluble resins are traditionally added to the binder [24]. Although successful, such approach brings a cost penalty.
To resolve the above problems, an alternative means of producing/releasing CO2 was considered based on the reaction known to us as generating considerable volumes of carbon dioxide upon contact of water with isocyanates concurrently used in our laboratories in the development of a process re-application of alkyd resins in moulding sands [39] for large alloy steel castings such as steam turbine casings.
It was hypothesised that incorporating isocyanates into the mixtures containing sodium silicate will utilise water inherently present within hydrated silicates as an activator for triggering generation of CO2, as per reaction (2) below:
OCN–R–NCO + 2 H2O → H2N–R–NH2 + 2 CO2↑
which, in turn, would result in self-hardening of such moulding sands.
It was also hypothesised that sodium silicate binder crosslinked by CO2 generated through the above reaction will exhibit important advantages over the classical hardening by CO2 purge.
The anticipated advantages are due to the fact that reaction (2) proceeds through specific stages as follows:
(i) R–NCO + H2O → R–NH–COOH
In step (i) water molecule contacting electrophilic carbon atom in the isocyanate group forms an unstable carbamic acid [R–NH–COOH]. The latter spontaneously decomposes; see reaction (4), to release a molecule of CO2 and a primary amine [R–NH2]:
(ii) R–NH–COOH → R–NH2 + CO2
Importantly, the amine-generated through reaction (4) rapidly reacts with the remaining unreacted isocyanate to form a stable polyurea chain, as follows:
R–NCO + R–NH2 → R–NH–CO–NH–R
The CO2 released as per reaction (4) and alkaline environment simultaneously trigger the gelation-silicification of the latter, embedding inorganic polysilicate particles or a silica network directly into the organic polyurea matrix, as schematically illustrated in Figure 2c above.
Figure 2. Schematic representation of: (a) 3-dimensional structure of self-setting moulding sand (core- and mould-forming mixture) representing a specific category of particulate-filled refractory composite material bonded by a liquid inorganic/organic hybrid binder, i.e., sodium silicate and isocyanate; (b) interconnecting pendular bridge—see ② in panel (b) spontaneously formed by meniscus of liquid binder film—see ① in panel (b) on particles surface; (c) schematics of internal structure of binder film cured (polymerised) through chemical reaction between liquid sodium silicate and isocyanate hardener. The following is formed during this reaction: (i) an amorphous hybrid film ① with embedded micro-voids formed by CO2; (ii) randomly dispersed organic post-crosslinking residues (polyurea: by-product of the crosslinking reaction).
Figure 3 below schematically depicts the flow of the above reactions, down to mixing the binder with particulate filler (sand) and illustrating schematic structure of the binder film around adjacent sand particles.
Figure 3. (a) Schematic flowchart of processes (including schematics of reactions) taking place during self-setting of sodium silicate binder crosslinked by polyisocyanates, and (b) SEM photo of binder bridges connecting adjacent particles of mineral filler (silicate sand) overcoated by binder film comprising sodium silicate and by-products of its crosslinking reaction. NOTE: colour-coding highlights the organic (light-brown/orange tones) and inorganic (blue tones) nature of reactants and products of the reaction.
At high temperatures exerted by the molten (and solidifying) metal, the organic bonds and discrete polyurea inclusions, which are stochastically distributed throughout the binder film, are decomposed, thereby reducing the strength of the sodium silicate film surrounding sand filler as well as inter-particulate binder bridges between adjacent sand particles.
It has been ultimately shown through the results of our research that, indeed, the fracture behaviour of sodium silicate films inter-dispersed with randomly distributed organic residues of reaction (5), e.g., polyurea, has been drastically improved (as discussed below), yielding the knock-out energy of moulding sands containing 2.5% of sodium silicate binder 4 times lower that exhibited by identical systems cured by CO2 gas purge.

5.2. Determination of CO2 Quantity for Sodium Silicate Cure at Any Silicate Module

The hardening of sodium silicate (see Equation (1)) can be described, in a generalised form, by the following reaction:
n Na2O + m SiO2 + n CO2 → n Na2CO3 + m SiO2
The silicate module is defined as follows:
M s = m   Si O 2 n   N a 2 O · 1.03
Here, the values m SiO2 and n Na2O express the corresponding content of SiO2 and Na2O in sodium silicate by mass [%].
According to reaction (6), the hardening process requires a molar quantity of CO2 equal to the molar quantity of Na2O. Taking into account Equation (7) and the molar masses M N a 2 O = 62 and M C O 2 = 44, the amount of CO2 required for the hardening of water glass with any modulus can be calculated using the following equation:
m C O 2 = 100 − x H 2 O M s + 1.03 · m w
where x H 2 O —water content of the water glass [mass %], Ms—silicate module of the water glass, and mw—amount of water glass used [g].

5.3. Calculation of Polyisocyanate Amount Required for Sodium Silicate Cure

Using the reaction (2), the amount of CO2 released from 1 g of polyisocyanate can be calculated as follows:
m C O 2 = 0.01 · X · m RNCO
where X—isocyanate content in the hardener [mass %]; mRNCO—polyisocyanate quantity [g].
This above constitutes the maximum amount of CO2 that can be released from 1 g of polyisocyanate. However, as some of the isocyanate groups are typically consumed in other reactions, the actual amount of CO2 present is always lower.
From 1 g of hardener containing, for example, 0.35 or 0.48 mass parts per gram of NCO groups, the quantity of 0.35 or 0.48 g of CO2 is released respectively. Equations (2)–(9) can therefore be used to calculate the theoretical amount of polyisocyanate required for the curing of any sodium silicate. This results in the following relationship:
m RNCO = 0.73 · 100 − x H 2 O M s + 1.03   X · m w
For a specific polyisocyanate containing, for example, 35% by mass of isocyanate groups, the mass ratio [k] can be calculated for different types of sodium silicate:
k = m RNCO m w
For the most commonly used types of water glass, the k-value remains in the range of 0.18–0.25, and is specifically as follows:
for Ms = 2.10 k = 0.24;
for Ms = 2.45 k = 0.21;
for Ms = 2.90 k = 0.20.

6. Experimental Section

6.1. Overview

The principal body of work discussed in this paper presents the outcome of overarching fundamental research targeting development of mathematical models of particulate-filled high-porosity composite materials for a range of specialty applications utilising a matrix of self-setting liquid inorganic and organic binders, e.g., in metal casting.
All performance criteria set by commercial end-users of the technology were met through an in-depth investigation of fundamental mechanisms controlling: (1) spatial morphology of moulding sands; (2) optimised adhesion (by investigating and modelling the strength of particulate-reinforced composites versus the following parameters (details of several of these are outside the scope of this paper): mean diameter of filler particles (d50); specific surface area of filler (SA); wetting angle of quartz surface by a binder (Ɵ); binder film thickness (gf); grain shape coefficient; binder’s dynamic viscosity (η); and binder surface tension (γB); (3) kinetics of binders crosslinking; and (4) mechanical and fracture properties of composites at the room and elevated temperatures. The outcomes of these provided seminal insight into interfacial phenomena at the solid–liquid interface [40,41,42,43,44,45,46,47,48] and binders crosslinking [14,15,16,17]. These, in turn, facilitated the optimisation of composite performance, including minimisation of the binder content (1.2 to 1.5%) through maximising interfacial adhesion [41,43,47] and optimising the filler particulate size, rheological and chemical properties of binder system and composite processing [14,41].
All experiments targeting validation of our concept of crosslinking/self-setting sodium silicate binder by CO2, released due to chemical reaction(s) between the inherent fraction of water within hydrated silicates and isocyanates presented in this paper, were conducted using refractory particulate filler in the form of silica sand from Ludwików deposits.

6.2. Materials and Methods

6.2.1. Principal Ingredients

Silica Sand and Its Properties
The granulometric characteristic of Ludwików sand (Ludwików quarry, Tomaszów Mazowiecki, Poland) was determined through sieve analyses of dried samples (100.00 g each) conducted as per DIN 4188 standard [48], which yielded data shown in Table 1, subsequently used for determining the average grain size, d50 = 0.358 mm (see Figure 4).
Table 1. Geometrical and surface characteristics of Ludwików sand.
Figure 4. The granulometric characteristic of Ludwików sand [47].
To facilitate systematic study regarding the influence of physicochemical properties and geometry of granulate and liquid binders on the strength and other technological properties of composites, the commercial stock of sand, as received from the supplier, was fractionised by vibrational sieve screening into fraction batches exhibiting the following granulate sizes: 0.8; 0.63; 0.40; 0.32; 0.20; 0.16 and 0.10 mm.
As seen in Table 1, fractions with diameter of 0.8 mm and 0.1 mm yielded insignificant quantities of (0.41 and 2.7% respectively) and hence were not included in these broader studies.
Determination of binder film thickness necessitated the knowledge of specific surface area of sand used in experiments. The latter was investigated and computed using experimental data collected through the use of designated apparatus designed by Christodoulu [47] for his work on the development of mathematical models of self-hardening moulding sands. The methodology and equipment utilise the principles of fluid dynamics embedded in Carman–Kozeny equation [49] to estimate the pressure drop and kinetics of flow of air through a packed column of granular solids, e.g., sands, thus facilitating estimation of specific surface energy of granulate used as filler in our work.
The principal body of work presented in the current paper (residing outside of the domain of mathematical modelling cohesive properties of composites, e.g., moulding and core mixtures) was carried out using the original commercial sand, as received, i.e., unfractionated. The key properties of it are: (i) average grain size (DIN): d50 = 0.358 mm [see Figure 4 for details]; (ii) specific surface area: SA = 151 cm2/g; (iii) shape factor (non-sphericity): 2.199; (iv) water adsorption: 1.8%; and (v) clay residue contents: 0.6%.
Binder: Hydrated Silicates
Hydrated sodium silicate binders listed in Table 2, sourced from Chemicals Company Rudniki, Częstochowa (Poland), were used as the principal silicate binder throughout our work.
Table 2. Composition of the types of sodium silicate used in experiments.
Binder Setting/Crosslinking Methods
Hydrated sodium silicates were cured/consolidated through the use of the following media:
  • Isocyanate compounds: see Table 2 for details;
  • Esters Carset 533, Flodur;
  • CO2 gas purge (i) pressure: 1 bar; (ii) flow rate: 10 litres/min; (iii) time: 30 and 60 s.
Isocyanate Compounds
Isocyanate compounds used in this work are listed in Table 3. These were obtained from the following sources: No. 1-3, from Zachem Chemical Plant, Bydgoszcz, Poland and No. 4 from Georg Fischer (+GF+), Schaffhausen, Switzerland.
Table 3. Isocyanate compounds used in experiments.

6.2.2. Moulding Sands (Composites) Preparation

Equipment and Mixing Protocol
All moulding sands were prepared using a +GF+ paddle mixer. The main body of work was conducted using the following mixing sequence: sand was first mixed with the isocyanate compound for 3 min and subsequently, after adding sodium silicate, for a further 1 min.
In an alternative procedure, sand was first mixed with sodium silicate for 3 min and subsequently, after adding isocyanate compound, for a further 1 min.
All mixtures designated for cure/solidification by CO2 purge were mixed for 3 min after the addition of sodium silicate.
Composites Cure
All composites were cured at 20 °C and were then tested (compressive and/or tensile strength) at the following time intervals lapsing between completion of composite mixing and samples fabrication: 15′; 20′; 30′; 40′; 1 h; 2 h; 3 h; 5 h and 24 h.
Assessment of Composites Mechanical and Other Critical Technological Properties
The principal mechanical properties of moulding sand composites, such as compressive strength and tensile strength, were determined using a designated LRu-2e mechanical tester supplied by Multiserw-Morek, Wadowice/Poland, and tested in accordance with the following standard protocols:
Compressive strength: determined using cylindrical specimens: Ø50 × 50 mm in accordance with Polish Standard PN 80/H-11073 [50]. Foundry Moulding Materials—Measuring of Strength.
Tensile strength: determined using dog-bone specimens with square cross-section load-bearing area of 25.4 × 25.4 mm in accordance with ASTM C307-18 [51].
Each experimental point involved testing of 10 samples.
The reproducibility of the strength data: each data point re-determination of the profile of strength kinetics involved testing 10 replicates. The reproducibility of strength data collected throughout all experiments is within ±8.5% of the nominal value for all data points.
The following additional properties of composites (moulding sands) were investigated:
(a) Cure characteristic
Determined by the strength increase versus time characteristics reflecting the kinetics of resin crosslinking reaction, with an initial onset of the reaction (crosslinking delay) defining the mixture’s shelf life. These samples were tested after the following time intervals lapsing between completion of composite mixing and samples fabrication: 15′; 20′; 30′; 40′; 1 h; 2 h; 3 h; 5 h and 24 h cure.
(b) Shelf-life
Material processing ‘window’, i.e., the allowable processing time span lapsing between composite pre-mixing and sample preparation (or core/mould fabrication) resulting in the cured composite (after 24 h room temperature cure), achieving the strength of not less than 90–95% of those fabricated from a freshly pre-mixed composite material.
(c) Kinetics of thermal decomposition of binders used in moulding sands.
Kinetics of gas evolution from binders used in moulding sands investigated in this work was investigated with the use of Georg Fischer PGD device illustrated in Figure 5.
Figure 5. Georg Fischer PGD device for determining kinetics of gaseous products evolution from moulding sands [52].
The procedure relies on measuring the rate of gas formation (cm3/g vs. time, presented in real time) evolving from composite samples heated from 20 °C to 1000 °C at a rate of 10 °C/min in inert nitrogen atmosphere in electrically heated tubular muffle furnace of this equipment. The inclined heating chamber of +GF+ equipment, as presented in Figure 5, ensures that the evolved gases remain in the hot zone and only the inert gas passes into the pressure recorder.
Readings of pressure of gas evolving during sample decomposition are converted to volumes by means of a calibration graph prepared at the range of relevant temperatures. The latter has been carried out as required by the equipment manual, as follows:
Pre-determined weights of analytical grade hydrogen KHCO3 generating known theoretical volume of gas (i.e., 224 mL per 1 g of dry KHCO3) adjusted to NTP (i.e., adjusted to what it would have been under ‘Normal Temperature’ of 20 °C and ‘Normal Pressure’, i.e., pressure of one atmosphere) were first pre-dried for 30 min at 105 °C and then enclosed in sealed copper sample tubes. The latter were subsequently ‘fired’ into the chamber of tubular furnace by a ‘sample gun’ to facilitate KHCO3 decomposition and subsequent recording of the maximum gas pressure attained.
The weights of KHCO3 and respective theoretical gas volume data recommended for calibration are shown in Table 4.
Table 4. Calibration data for preparation of calibration characteristic of Georg Fischer PGD [52].
The pressure-volume calibration characteristic of Georg Fischer PGD device used in our experiments is presented in Figure 6 below.
Figure 6. Calibration characteristic of Georg Fischer PGD device for determining kinetics of thermal decomposition (gaseous) products evolution.

6.3. Experimental Results

6.3.1. The Effect of Various Types of Isocyanate Compounds

Figure 7 shows the strength curves development as a function of curing time for moulding compounds containing three representative types of sodium silicate (silicate module: 2.1; 2.45 and 2.9) and the polyisocyanate “Isocyn TS” hardener. The quantities of polyisocyanate correspond to the previously calculated values.
Figure 7. Strength development curves as a function of curing time for moulding sands bonded with sodium silicate cured with TDI isocyanate (Isocyn TS) as follows: (a) Ms = 2.1 and content (C) = 2.5 parts by weight; (b) Ms = 2.45 and C = 3.5 parts by weight, and (c) Ms = 2.9 and C = 4.5 parts by weight. The curves presented are designated as follows: (1) k = 0.1; (2) k = 0.15; (3) k = 0.2 and (4) k = 0.25, where k—mass ratio of Isocyn TS to sodium silicate, Ms—silicate module, C—water-glass content in the moulding mixture.
It has been determined that the best technological properties of moulding sands were achieved with 2.5 mass % sodium silicate exhibiting silicate module of 2.1. In accordance with the theoretical calculations, these moulding compounds exhibit the best properties when the k-value is 0.25. However, if the practical pot life of the moulding sand is to be extended, it is advisable to set the k-value to 0.2.
It is apparent from graphs in Figure 7 that is makes little sense to use more than 2.5% sodium silicate binder, as this results in only a slight change in the ultimate strength of the cured mixture. By varying the amount of hardener, not only the pot life but also the curing rate of the moulding sand can be controlled.
For mixtures containing sodium silicate with a silicate module of 2.45, the most favourable technological properties are achieved when the binder content is 3.5% by weight and k is 0.25.
For compounds with a silicate module of 2.9, unfavourable technological parameters are obtained (excessive friability).
Figure 8 illustrates kinetics of hardening process of moulding sands bonded by sodium silicate cured with different types of isocyanate hardener (see Table 3). Figure 8a illustrates strength characteristics of moulding compounds cured with TDI, which provides rapid increase in strength, particularly at sodium silicate content of 4% by weight. The tensile strength is also quite high. As seen from the graphical data in Figure 8b, if Activator 300B or MDI are used as curing agents, the curing process proceeds considerably more slowly.
Figure 8. Hardening process over time for different types of isocyanate hardeners. (a) Toluene diisocyanate (TDI): (1) 2.5 parts by weight of sodium silicate, 0.6 parts by weight of TDI; (2) 4.0 parts by weight of sodium silicate, 0.5 parts by weight of TDI; (3) 4.0 parts by weight of sodium silicate, 0.75 parts by weight of TDI; (4) 4.0 parts by weight of sodium silicate, 1.5 parts by weight of TDI; (b) (MDIs) Activator 300B and diphenylmethane diisocyanate: (1) 2.5 parts by weight of sodium silicate, 0.6 parts by weight of Activator 300B; (2) 4.0 parts by weight of sodium silicate, 1.6 parts by weight of Activator 300B; (3) 2.5 parts by weight of sodium silicate, 0.6 moulded parts MDI solution; (4) 2.5 parts by weight of sodium silicate, 0.6 moulded parts made from MDI powder.
Furthermore, it was found that the kinetics of strength development during the curing process and the final strength also depend on the proportion of isocyanate groups in the curing agent (Figure 9a).
Figure 9. Influence of the isocyanate groups content in the hardener on strength development kinetics for moulding sands containing: sand: 100 parts per weight (ppw); sodium silicate (Ms = 2.1): 2.5 ppw, and isocyanate: 0.6 ppw. (a) Kinetics of the strength development over time for NCO contents designated as follows: (1) 27.0% NCO groups content in the hardener; (2) 30.3% NCO groups content in the hardener; (3) 35.0% NCO groups content in the hardener; (4) 48.2% NCO groups content in the hardener. (b) The curing rate of moulding sands during the first hour.
The volume of CO2 released in the moulding sand with sodium silicates cured by isocyanates depends on the inherent contents of NCO groups. Hence, by using isocyanate compounds with different NCO group contents, the curing process can be controlled accordingly.
The respective profiles of the moulding sand’s cure kinetics during the first hour as a function of the NCO group content in the hardener is shown in Figure 9b.

6.3.2. The Effect of Mixing Sequence of the Moulding Sand Ingredients

Figure 10 shows the curing characteristics of the sodium silicate-bonded moulding compounds cured with TDI (denoted as “1”) and Isocyn TS (denoted as “2”).
Figure 10. Dependence of the kinetics of strength development of sodium silicate-bonded mixtures cured by isocyanates on the sequence of mixing the individual ingredients: (1a) sand + TDI + sodium silicate; (1b) sand + sodium silicate + TDI; (2a). Sand + Isocyn TS + sodium silicate; (2b) sand + sodium silicate + Isocyn TS.
The individual components were added to the moulding compound in different sequences. A significantly higher curing rate is achieved when the isocyanate compound is added to the sand first. The final strength of the moulding compound is independent of the sequence of addition.
The data presented in Figure 10 highlight the potential of this novel technology for additive manufacturing applications, including the 3D printing of precision moulds and cores. This opportunity is clearly seen through the observation of the fact that when the hardener (isocyanate) is incorporated first, the excess of hardener exists at the pendular bridge attachment plane at the sand surface (i.e., at the substrate–binder interface, which controls the quality of adhesion), thus resulting in significantly faster composite cure (300% to 400% faster) than that in the case of sodium silicate applied as the first binder component.
The above observation is complemented by the fact that isocyanate-coated sand (or other types of granular filler) can be prepared and appropriately stored in advance of the printing process, consequently allowing an “on-demand” fabrication of a 3D printed mould or core when the need arises.
The details of the above concept are the subject of a separate research paper currently under preparation by the current co-authors.

6.3.3. The Effect of Room Temperature

For most self-setting moulding sands, ambient temperature has a significant influence on the curing process kinetics. Both, the rate of strength development and the final strength, are usually notably reduced at lower temperatures.
Considering the fact that tensile strength of particulate filled composite materials better represents unhindered physical and chemical interaction forces between and within all constituents of the material, including the kinetics of the binder crosslinking (cure) process, it can be seen from data presented in Figure 11b that the ultimate strength of moulding sands bonded by sodium silicate binders crosslinked by polyisocyanates is marginally only influenced by ambient temperature fluctuations within the range of 5 °C to 25 °C.
Figure 11. Effect of ambient temperature on the kinetics of strength development in composites bonded by sodium silicate/polyisocyanate binders: (a) compressive strength and (b) tensile strength [sand: 100 parts by weight (p.p.w.); sodium silicate: 2.5 p.p.w.; Isocyn TS: 0.6 p.p.w. (k = 0.175)]. Figure (a): sodium silicate with Ms = 2.1 and Figure (b): sodium silicate with Ms = 2.45.
However, the curing proceeds progress most favourably in the temperature range of 10 to 15 °C, where the increase in strength during the first hour is approximately 40 to 50% higher than at other temperatures, either lower or higher than within this optimal range.

6.4. Optimum Binder Content Determination

In the production of moulding mixtures, various types of sand from alternative deposits are used by individual foundries. Each of these supply resources yield filler exhibiting its specific geometry and size distribution resulting in a designated specific surface area (Ss). It is therefore essential to determine either—the film thickness around the individual grains of sand at which the maximum strength of the moulding material is achieved; see Equation (12):
g = c · 1 ρ w + k ρ i S s
where g—film thickness [10−4cm]; c—actual binder content [%]; Ss—specific surface area of sand [cm2/g]; ρw—specific density of water glass [g/cm3]; k—mass ratio of isocyanate to water glass; and ρi—specific density of isocyanate [g/cm3].
Conversely, it is possible to determine the quantity of binder required to formulate the composite mixture corresponding to the optimum film thickness around the filler grains, at which the maximum strength of the cured moulding material can be achieved—see Equation (13):
c = g · S s 1 ρ w + k ρ i [ % ]
Figure 12 below provides illustration of the effect of the sodium silicate film thickness on the surface of sand used in our development on (a) compressive strength and (b) tensile strength of mixtures cured by isocyanate.
Figure 12. Sodium silicate binder cured by CO2 generated by the reaction of their inherent water on contact with isocyanates: the effect of the binder thickness on (a) compressive strength and (b) tensile strength.
In these investigations, sand fractions of the following sizes (d50) were used: 0.16; 0.20; 0.32; 0.40; and 0.63 mm. The results compiled in Figure 12 clearly show that the optimum strength parameters (in compression and tensile mode) are achieved at a film thickness of 2 µm. This applies to moulding sands bonded by sodium silicate with silicate module of 2.1 to 2.9. These results were also confirmed by investigations on unfractionated sands.
The above results were benchmarked against moulding sands with sodium silicate binder cured by an alternative source of CO2, i.e., by carbon dioxide purge applied using parameters listed in Section 6.2.1 (Binder setting/crosslinking methods)—see Figure 13 below for experimental results.
Figure 13. Comparison of the influence of sodium silicate film thickness on the strength of moulding mixtures cured by alternative source of carbon dioxide: (a) CO2 generated from isocyanate reaction with binder’s intrinsic water; (b,c) cured by CO2 gas purge as applied at: (i) pressure: 1 bar; (ii) flow rate: 10 litres/min; (iii) time: 60 s. (Note: The reproducibility of strength data collected throughout all experiments is within ±8.5% of the nominal value for all data points presented).
A close analysis of data regarding sodium silicate film crosslinked by alternative means of CO2 source, i.e., in the form of compressed CO2 gas purge or that generated from the reaction between water within the binder and isocyanate, as presented in Figure 12 and Figure 13, clearly proves that both technologies are self-consistent.
This important discovery is apparent by superimposing data points re-optimum film thickness of about 2 μm applicable to NCO-generated carbon dioxide (imported from Figure 12) into the grid of strength data in Figure 13b,c compiled from experiments re-composites cured by CO2 gas purge (see ‘solid red’ data points in these panels). It is clearly evident that the strength vs. binder film thickness curves (solid black points) re-sodium silicate cured by carbon dioxide purge continue directly to the red data points collected from experiments in which NCO was the source of CO2.

6.5. Influence of the Type of Liquid Curing Agents on Binder Cure Kinetics

In order to assess the effectiveness of the new category of hardeners developed in this work more accurately, comparative tests were carried out, in which the properties of alternative categories of liquid organic hardeners were compared.
The following hardeners were used for this purpose:
  • Esters: Carset 533, Flodur;
  • Isocyanates: Isocyn TS, TDI, Activator 300B.
The compositions of the ester-based binders were adjusted in accordance with the manufacturers’ recommendations and amounted to 10% ester (relative to the binder).
The isocyanates, on the other hand, were always used at a proportion of 17.5% by weight with 2.5% by weight of sodium silicate (module Ms = 2.1).
Figure 14 shows the kinetics of strength development over time of 24 h for the above moulding compounds. It is clearly seen that the strength of moulding compounds with isocyanate hardeners is within the same range as that of those hardened by ester hardeners. Notably, the moulding sands containing Isocyn TS exhibit similar strength characteristics as the mixtures cured by Flodur.
Figure 14. Comparison of the strength characteristics of moulding sands bonded with sodium silicate (Ms = 2.1) when using different hardeners, i.e., (A) sand: 100 parts by weight (ppw), sodium silicate 2.5 ppw, Isocyn TS used at k = 0.175. (B) sand: 100 ppw; sodium silicate: 2.5 ppw; Flodur: 0.25 ppw, and (C) sand: 100 ppw; sodium silicate: 2.5 ppw; Carset 533: 0.25 ppw; (a) the kinetics of compressive strength development, and (b) the kinetics of tensile strength development.

6.6. Fracture Performance (Knock-Out Properties) of Moulding Sands with Isocyanate-Cured Sodium Silicate Binder

One of the principal aims of this work was verification of the hypothesis that spatially dispersed ‘post-reaction’ organic residues (polyurea) formed as a by-product of reaction of water with isocyanates should facilitate reduction in fracture energy of the binder film, including that within inter-granular bridges connecting individual filler particles.
To verify the above, a comprehensive study was conducted to compare knock-out performance of a broad range of moulding mixtures bonded with sodium silicate binder (Ms = 2.1) cured by ‘curing agents’ commonly used by industrial foundries around the world, i.e., CO2 purge and esters, and including isocyanate hardeners analysed in this work. These were compared with moulding sands bonded with furane resin used here as the benchmark considered as the ‘best-performing’ material regarding knock-out performance.
Table 5 presents comprehensive spectrum of mechanical properties of sodium silicate/NCO bonded moulding mixture assessed as the optimum formulation for potential industrial applications.
Table 5. Mechanical properties of moulding sands with 2.5% sodium silicate binder (Ms = 2.1) and Isocyn TS (0.6%) used as a hardener.
Figure 15 provides comparison of demoulding energy (knock-out energy) for cores (diameter Ø50 × 50 mm) made from various types of moulding sands investigated and developed in this work.
Figure 15. Comparison of knock-out work (demoulding energy) for cores fabricated using moulding sands bonded by sodium silicates and cured using different hardeners, as specified in the table embedded in the figure.
The assessment of knock-out performance was carried out in accordance with PN-85/H-11005 Polish standard [53]. It employed moulds with two cores inserted into mould cavity, as described in detail by procedure discussed in [24,54], and filled with chrome steel alloy poured at 1520 °C. Three moulds per each experimental point were used in these trials, thus yielding six samples for the assessment of fracture energy of each composite type.
The data presented in Figure 15 present the mean value of knock-out energy of each composition, including pertinent standard deviation. The data depictured in this illustration clearly demonstrate advantages of sodium silicate bonded moulding sands cured with isocyanate hardener (Isocyn TS) in comparison with traditional mixtures cured by classical CO2 gas purge.

7. Other Technological Properties

7.1. Gas Evolution on Contact with Molten Metal

The point of time when gases begin to evolve from a mould filled with molten metal and the rate at which such gases evolve are of much greater importance in practice than the total amount of gaseous by-products given off by the mould-/core-making mixture.
According to Figure 16, the gas evolution from the decomposition of commercial organic binders such as furane resin [FR], and alkyd/polyester resin [AP] cured with a commercial isocyanate denoted as Activator ‘B’ began to reach a significant level as soon as 2 to 4 s after filling the mould. In contrast to the above results, the evolution of gases from ‘slow-decomposing’ moulding materials bonded by polyester resins [PH1], [PH2] and alkyd resins [AH1], [AH2] developed in our earlier work [39] only began to occur when it was essentially over in the case of these much faster decomposing reference materials, i.e., furan (FR) and [AP-B binders].
Figure 16. Kinetics of formation of gaseous decomposition by-products from moulding materials utilising a range of binder systems investigated in this work upon contact with molten metal (low-alloy steel) [39].
The total volume of gas evolving from the moulding sands bonded with sodium silicate with the Isocyn TS (0.6%) isocyanate, as developed in this work, was investigated using analytical equipment and procedures described in Section 6.2.2. It was subsequently demonstrated that the gas emissivity from these novel moulding sands is within the range of 8–10 cm3/g, which is approximately 50–65% of that reached by commercially available commodity organic binders such as furane, alkyd and polyester resins presented in Figure 16.

7.2. Abrasion Resistance and Pot Life

Other important practical foundry floor handling and technological properties investigated and determined in our work were as follows:
  • Abrasion resistance (3 min rolling): 0.5%;
  • Pot life: 15–25 min.

8. Conclusions

The investigations carried out in this work have clearly shown that the use of new type of hardeners containing isocyanate groups offers significant advantages for the production of self-setting moulding sands bonded by sodium silicates.
The optimised moulding sands have the following composition:
Sand: 100 parts by weight (ppw);
Sodium silicate (Ms = 2.1): 2.2 to 2.5 ppw;
Isocyn TS (isocyanate): 0.43 to 0.5 parts by weight.
The key advantages of the novel technology presented in this work are as follows:
  • By using sodium silicate with a silicate module of 2.1, the binder content can be reduced by half (compared to existing technologies).
  • The isocyanate hardeners significantly improve knock-out (demoulding) properties of moulds and cores fabricated with the use of these mixtures reducing it 4-fold in comparison with traditional CO2 gas flux at identical binder contents (2.5%).
  • The new moulding mixture system presented in this paper, when utilising 2.2 to 2.5% (mass percentage) of sodium silicate as a binder exhibits performance properties similar to those of the best-performing resin-bonded (e.g., furan resin) moulding compounds with a comparable binder content.
    Sodium silicate can therefore be used as a binder even in applications where only organic binders have been used until now. This substitution of the organic binder (e.g., furan resin) by an inorganic sodium silicate binder drastically reduces the amount of gases generated during binder decomposition on contact with the molten and solidifying metal, thereby minimising detrimental environmental impact of metal casting processes.
  • The liquid hardeners (isocyanates) content is about eight times lower than that of conventional inorganic powdered hardeners, thus offering the following advantages: reduced storage requirements; easier transport; no dust formation in the workplace; simple and accurate dosing.
  • The moulds and cores produced with the use of new moulding sand material can be used at the industrial scale castings production utilising alloy-steel, cast iron and non-ferrous metal alloys.

9. Future Work

Future work aims an in-depth exploration and publication of fundamental aspects of mechanisms controlling fracture behaviour of sodium silicate binders polymerised by alternative sources of CO2 gas investigated in the current paper for moulding sands application. As highlighted in the final part of Section 6.3.2., the authors are also exploring the potential of this novel technology for additive manufacturing applications including the 3D printing of precision moulds and cores, particularly for the scenario of rapid ‘on-demand’ fabrication of a 3-D printed mould or core when the need arises.

Author Contributions

Conceptualization, W.S.G. and A.K.B.; methodology, W.S.G.; validation, A.K.B. and M.U.; formal analysis, W.S.G. and A.K.B.; investigation, W.S.G. and A.K.B.; data curation, W.S.G.; writing—original draft preparation, W.S.G. and A.K.B.; writing—review and editing, A.K.B., W.S.G. and M.U.; visualisation, W.S.G.; supervision, A.K.B.; project administration, M.U. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Institutional Review Board Statement

Not applicable.

Data Availability Statement

The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding authors.

Acknowledgments

We dedicate this article to Paweł Zięba, Chairman of the Committee of Materials Engineering and Metallurgy of the Polish Academy of Sciences, on the occasion of his 70th birthday. We wish to express our deep appreciation for his contributions across many fields—not only to Polish materials engineering, but also to the broader scientific community.

Conflicts of Interest

The authors declare no conflicts of interest.

References

  1. Hawaldar, N.; Zhang, J. A comparative study of fabrication of sand casting mold using additive manufacturing and conventional process. Int. J. Adv. Manuf. Technol. 2018, 97, 1037–1045. [Google Scholar] [CrossRef] [Scilit]
  2. Czerwiński, K.; Mir, M.; Kasprzak, M. Application of cores and binders in metalcasting. Int. J. Cast. Met. Res. 2015, 28, 129–139. [Google Scholar] [CrossRef] [Scilit]
  3. Hutera, B. The Effect of Solvent Content in Binder on the Nature of Surface Phenomena Taking Place in a Sand Grains–Binding Material System; Scientific Publishers AKAPIT: Krakow, Poland, 2008. [Google Scholar]
  4. Hutera, B.; Smyksy, K.; Drożyński, D. Evaluation of wettability of binders used in moulding sands. Arch. Foundry Eng. 2007, 7, 103–106. [Google Scholar]
  5. Kmita, A.; Roczniak, A. Nanocomposites based on water glass matrix as a foundry binder: Chosenphysicochemical properties. Arch. Foundry Eng. 2017, 17, 93–98. [Google Scholar] [CrossRef] [Scilit]
  6. Stachowicz, M.; Granat, K.; Nowak, D. Effect of hardening method and structure of linking bridges on strength of water glassmoulding sands. Arch. Foundry Eng. 2010, 10, 141–146. [Google Scholar]
  7. Weisstein, E.W. Sphere Packing from MathWorld—A Wolfram Web Resource. Available online: https://mathworld.wolfram.com/SpherePacking.html (accessed on 22 November 2021).
  8. Khandelwal, H.; Ravi, B. Effect of Binder Composition on the Shrinkage of Chemically Bonded Sand Cores. Mater. Manuf. Process. 2015, 30, 1465–1470. [Google Scholar] [CrossRef] [Scilit]
  9. Thiel, J. Thermal expansion of chemically bonded silica sands. AFS Trans. 2011, 116, 369–378. [Google Scholar]
  10. Łucarz, M.; Drożyński, D.; Jezierski, J.; Kaczmarczyk, A. Comparison of the Properties of Alkali-Phenolic Binder in Terms of Selection of Molding Sand for Steel Castings. Materials 2019, 12, 3705. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  11. Kmita, A.; Fischer, C.; Hodor, K.; Holtzer, M.; Roczniak, A. Thermal decomposition of foundry resins: A determination of organicproducts by thermogravimetry—Gas chromatography—Mass spectrometry (TG–GC–MS). Arab. J. Chem. 2018, 11, 380–387. [Google Scholar] [CrossRef] [Scilit]
  12. Wan, P.; Zhou, J.; Li, Y.; Yin, Y.; Huang, D.; Ji, X.; Shen, X. Experimental Study on Gas Evolution Process of Binders in Foundry Industry based on TG-MS. Process Manuf. 2019, 37, 311–318. [Google Scholar] [CrossRef] [Scilit]
  13. Wan, P.; Zhou, J.; Li, Y.; Yin, Y.; Peng, X.; Ji, X.; Shen, X. Kinetic analysis of resin binder for casting in combustion decompositionprocess. J. Therm. Anal. Calorim. 2021, 147, 6323–6336. [Google Scholar] [CrossRef] [Scilit]
  14. Zapalski, J.A.; Gutowski, W.; Kwasek, A.; Bledzki, A.; Krolikowski, W.; Chudzikiewicz, R. Moulding and Core Mixture. Polish Patent No. 117 082, 15 August 1983. [Google Scholar]
  15. Bledzki, A.; Gutowski, W.; Kwasek, A.; Zapalski, J. Core and Moulding Mixture. Polish Patent No.113 270, 27 February 1982. [Google Scholar]
  16. Bledzki, A.; Gutowski, W.; Krolikowski, W.; Kwasek, A. Core and Moulding Mixture. Polish Patent 109 017, 31 December 1980. [Google Scholar]
  17. Bledzki, A.; Gutowski, W.; Chudzikiewicz, R.; Krolikowski, W.; Christodulu, P. Core and Moulding Mixture. Polish Patent 113123, 30 December 1981. [Google Scholar]
  18. Garitaonandia, E.; Ibarra, A.; Kmita, A.; Dańko, R.; Holtzer, M. Assessment of Harmful Emissions from Multiple Binder Systems in Pilot-Scale Sand Casting. Molecules 2025, 30, 2765. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  19. Inorganic Binder Systems in Iron Casting—Current State of Development and Outlook. Available online: https://www.ask-chemicals.com/fileadmin/user_upload/Download_page/professional_articles/EN/CPT_03_2018_ASK_Chemicals_low.pdf (accessed on 24 February 2025).
  20. Zaretskiy, L. Modified Silicate Binders: New Developments and Applications. Int. J. Met. 2016, 10, 88–95. [Google Scholar] [CrossRef] [Scilit]
  21. Green Foundry LIFE. Improve the Use of Natural Resources: Inorganic Binders in Iron and Steel Foundries Case of the Green Foundry LIFE Project. Available online: https://greenfoundry-life.com/documentation/dissemination-material/improve-the-use-of-natural-resources-inorganic-binders-in-iron-and-steel-foundries-case-of-the-green-foundry-life-project/at_download/file (accessed on 3 March 2025).
  22. Holtzer, M.; Kmita, A. Sodium Silicate Molding Sands. In Chapter 9: Mold and Core Sands in Metalcasting: Chemistry and Ecology, 1st ed.; Springer Nature: Cham, Switzerland, 2020; pp. 83–107. [Google Scholar] [CrossRef] [Scilit]
  23. Gong, X.L.; Hu, S.L.; Fan, Z.T. Research, application and development of inorganic binder for casting process. China Foundry 2024, 21, 461–475. [Google Scholar] [CrossRef] [Scilit]
  24. Lewandowski, J.L. Materials for Foundry Moulds; AKAPIT: Cracow, Poland, 1997. (In Polish) [Google Scholar]
  25. Jelinek, P. Pojivove Soustavy Slevarenskych Formovacich Smeli. Chemie Slevarenskych Pojiv; P. Jelínek: Ostrava, Czech Republic, 2004. [Google Scholar]
  26. Beno, J.; Jelinek, P.; Spirutova, N. Moulding Mixtures; VŠB—Technical University of Ostrava: Ostrava, Czech Republic, 2015. [Google Scholar]
  27. Lipowska, B.; Jedynak, L. Fluorine-free coagulant of silicate based, acid-resistant, refractory putties. Pr. Inst. Ceram. Mater. Bud. 2010, 5, 81–91. (In Polish) [Google Scholar]
  28. Izdebska-Szanda, I.; Baliński, A. New generation of ecological silicate binder. Eng. Procedia 2011, 10, 887–893. [Google Scholar] [CrossRef] [Scilit]
  29. Baliński, A. Selected Problems of Molding Sand Technology with Inorganic Binders: The Structure of Hydrated Sodium Silicate and Its Influence on the Bonding of Molding Sands; Foundry Research Institute: Cracow, Poland, 2000. (In Polish) [Google Scholar]
  30. ASK Chemicals. INOTEC—Technological Advantages. 2014. Available online: http://www.ask-chemicals.com/fileadmin/user_upload/Download_page/foundry_products_brochures/EN/INOTEC_Overview_EN.pdf (accessed on 25 September 2026).
  31. Campbell, J. Complete Casting Handbook: Metal Casting Processes, Metallurgy, Techniques and Design; Butterworth-Heinemann: Oxford, UK, 2015. [Google Scholar]
  32. Müller, J.; Stötzel, R. New innovative solutions for foundries by inorganic concepts. In Proceedings of the 68th WFC–World Foundry Congress, Chennai, India, 7–10 February 2008. [Google Scholar]
  33. Gröning, P.M.; Strunk, D. The cold box process—A bridging technology. Cast. Plant Technol. 2011, 1, 14–17. [Google Scholar]
  34. Wolff, A.; Steinhaeuser, T. AWB—An environment friendly core production technology. Giesserei 2004, 91, 80–84. [Google Scholar]
  35. Steinhauser, T.; Wolff, A. AWB—Une technologie de noyautage respectueuse de l’environnement. Homes Fonderie 2007, 377, 11–15. [Google Scholar]
  36. Armbruster, S.; Dodd, S. New inorganic core and mold sand binder system. AFS Trans. 1993, 100, 853–856. [Google Scholar]
  37. Schrey, A. SOLOSIL TX—A new inorganic binder system. A new environment friendly binder system for core making. Foundry Pract. 2007, 263, 15–23. [Google Scholar]
  38. Grishchuk, S.; Castellà, N.; Karger-Kocsis, J. Hybrid resins from polyisocyanate/vinyl ester/water glass systems: Structure and properties. Eur. Polym. J. 2007, 43, 1245–1257. [Google Scholar] [CrossRef] [Scilit]
  39. Gutowski, W.S.; Błędzki, A.K. Fast-Setting Permeable Alkyd/Polyester Composites: Moulding Sands. Polymers 2021, 13, 4386. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  40. Gutowski, W.S.; Christodoulou, P. Fibre Matrix and Particulate-Matrix Stress Transfer in Composite Materials. Part I: Physico-Chemical Interfacial Interactions—Theoretical Models and Experimental Verification. In The Role of Casting Technology in Improvingthe Quality of Machines and Devises; University Press: Szczecin, Poland, 1993; pp. 75–94. [Google Scholar]
  41. Gutowski, W. Physico-chemical criteria for maximum adhesion. Part I: Theoretical concepts and experimental evidence. J. Adhes. 1985, 19, 29–49. [Google Scholar] [CrossRef] [Scilit]
  42. Gutowski, W. Physico-chemical criteria for maximum adhesion. Part II: A new comprehensive thermodynamic analysis. J. Adhes. 1985, 19, 51–70. [Google Scholar] [CrossRef] [Scilit]
  43. Gutowski, W.S.; Li, S.; Russell, L.; Filippou, C.; Hoobin, P.; Petinakis, S. Theoretical and Technological Aspects of Surface-Engineered Interface-Interphase Systems for Adhesion Enhancement. J. Adhes. 2003, 79, 483–519. [Google Scholar] [CrossRef] [Scilit]
  44. Gutowski, W.S.; Bilyk, A.; Li, S.; Espiritu, M.; Burgar, I. The influence of structure of the interface and interphase on paint adhesion. Compos. Interfaces 2005, 12, 817–835. [Google Scholar] [CrossRef] [Scilit]
  45. Gutowski, W.S. Interface-Interphase Engineering for Adhesion Enhancement. Micro-mechanical Aspects of Polymer Surface Reinforcement Through Surface-Grafted Molecular Brushes. J. Adhes. 2003, 79, 445–482. [Google Scholar]
  46. Gutowski, W.; Krzemien, F. Core and Moulding Mixture with Liquid Binders. Polish Patent 89 595, 30 August 1977. [Google Scholar]
  47. Christodoulou, P. Mathematical Model of Fast-Curing Moulding Mixtures. Master’s Thesis, Institute of Machine Construction, Technical University of Szczecin, Szczecin, Poland, 1976. (In Polish) [Google Scholar]
  48. DIN 4188-1:1977-10; Screening Surfaces; Wire Screens for Test Sieves, Dimensions (Original German Title: Siebböden; Drahtsiebböden für Analysensiebe, Maße). Beuth Verlag: Berlin, Germany, 1977.
  49. Carman, P.C. Permeability of saturated sands, soils and clays. J. Agric. Sci. 1939, 29, 262–273. [Google Scholar] [CrossRef] [Scilit]
  50. PN 80/H-11073:1980; Foundry Moulding Materials—Measuring of Strength. Polish Committee for Standardization: Warsaw, Poland, 1980.
  51. ASTM-C307:2018; Test Method for Tensile Strength of Chemical-Resistant Mortar, Grouts and Monolithic Surfacings. ASTM International: West Conshohocken, PA, USA, 2018. [Google Scholar] [CrossRef] [Scilit]
  52. +GF+ (Georg Fischer)—Das Gassdruckmessgerät PGD. In AFS Foundry Sand Testing Equipment Operating Instructions; Ridsdale & Company, Ltd.: Middlesbrough, UK, 1974; pp. 115–120. Available online: https://manualzz.com/doc/html/4162149/ridsdale-foundry-sand-testing-equipment-operating-instructions (accessed on 25 September 2026).
  53. PN-85/H-11005:1985; Foundry Moulding and Core-Making Compounds—Sampling and Preparation of Test Specimens. Polish Committee for Standardization: Warsaw, Poland, 1985.
  54. Major-Gabryś, K.; Grabarczyk, A.; Kaźnica, N. The Analysis of Moulding Sands’ Knock-Out Properties Measurement Methods. Arch. Foundry Eng. 2014, 14, 35–40. (In Polish) [Google Scholar]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.