Abstract
The core architecture and face–core load transfer govern the bending response of additively manufactured sandwich structures. This study examines carbon-fiber-reinforced polyamide (PA-CF) and glass-fiber-reinforced polyamide (PA-GF) faces combined with thermoplastic polyurethane (TPU) cores in 22 configurations. Grid, Cross 3D, Honeycomb, Line and Gyroid cores were evaluated at 20% and 40% nominal infills, with solid-core controls. Beams measuring 100 × 20 × 10 mm were loaded for four-point bending over an 80 mm support span and a 40 mm loading span. Total force and crosshead displacement were used to determine the initial structural stiffness, apparent modulus, operational offset yield, maximum force and work accumulated to maximum force. Increasing the patterned infill from 20% to 40% increased the descriptive mean stiffness across the five topologies by 50.1% for PA-CF and 49.9% for PA-GF. PA-CF Grid at 40% infill provided the highest patterned stiffness and maximum force at 173.2 N/mm and 837.0 N. PA-GF Line at 40% infill gave the greatest patterned work to maximum force, 8.30 J, closely followed by PA-CF Gyroid at 8.21 J. PA-GF Grid illustrated the competing effects of reinforcement: maximum force increased by 50.8%, while displacement at the maximum force and prepeak work decreased by 53.4% and 45.9%. The PA-CF solid control reached 1615.6 N and 18.80 J. The contribution is the joint comparison of these competing design responses across the same material–topology–infill matrix. An equivalent-core finite-element model with linear-elastic materials and large-deflection kinematics underestimated displacement by 45.28–88.03%, showing the limitations of the assumed infill-scaled homogeneous core. The findings support the joint selection of face material, topology, and infill according to stiffness, load capacity, and deformation requirements; prepeak work is a structural test-system quantity rather than fracture energy.
1. Introduction
Sandwich construction separates the structural functions of the faces and core. The outer layers resist longitudinal tension and compression while the core maintains their separation, transfers transverse shear, and supports the faces against local deformation. Material-extrusion additive manufacturing extends this arrangement by allowing the internal geometry and material distribution to be varied within a common external envelope. Fully integrated polymer sandwiches, hybrid composite skins and printed cellular cores have consequently been investigated as routes to adaptable structural performance [1,2,3,4].
Nominal infill alone does not define the mechanical behavior of a printed core. Member orientation, connectivity, unsupported length, wall continuity and junction geometry determine whether its deformation is dominated by axial extension, member bending, shear, or local contact. Significant differences in structural stiffness and load behaviors have been observed with the deposition angle and core pattern for both printed sandwich structures and FFF-fabricated components [5,6,7,8,9]. This suggests that increasing the material volume may result in an increased initial stiffness without a proportional increase in the deformation or load carried through subsequent deformation. TPU cores offer an additional difference between initial stiffness and behavior under large deformations. TPU lattices themselves show variation in their structures and loading conditions, and the internal structure of printed TPU has also been shown to have an impact on time-dependent behavior [10,11,12]. Sandwich structures with flexible cores and relatively stiff faces have also been shown to carry relatively high deformation in flexible core sandwiches and PLA/TPU core structures [13,14]. This has prompted the inclusion of both the maximum load and the area under the load deformation curve. A separation between the work supplied externally and irreversibly lost energy is also included in the analysis. Interface behaviors and face materials are also important in a structure. Longitudinal stiffness may be provided by fiber-reinforced polyamides, but the extent to which this is utilized depends on the local load transfer and directionality of the printing process [6,7,15]. The importance of interface behavior and face support has also been shown in skin–core debonding and gyroid core sandwich structures [16,17]. Elhassan et al. investigated the effects of slicer-induced mechanical interlocking in TPU core sandwich structures using PET, PLA, and PA faces under three-point bending [18]. The current research investigates a different design space, which uses PA-GF and PA-CF faces, five different core patterns, and two nominal infill values and is loaded under four-point bending without slicer-induced mechanical interlocking. Four-point bending produces a nominal constant bending moment in the central region between the loading nose and a shear-dominated region in the outer spans. The analysis of four-point bending is also impacted by the definition of applied force, the measured displacement and the relative contribution of bending and shear behaviors [19,20,21]. In the current work, F represents the total force applied by the machine. Under symmetric loading, this means that each loading nose experiences a force of F/2. The measured displacement represents the movement of the loading nose/crosshead and not the measured midspan deflection of the sample itself. The resulting slope thus represents the behavior of the test and loaded structures. An analytical bending model, a simplified finite-element analysis and experimental testing are used in the current work. The aim is to identify the impacts of nominal infill and structural topology on stiffness, operational offset yield, maximum load, and work prior to the peak load. The effect of face material on the ranking of structural topology is also investigated, as well as the limits of representing structural behavior using a homogeneous core. Analyses within the current work draw upon knowledge of cellular materials and printed sandwich structures [2,9,13,21,22]. The measured structural behavior is separated from material behavior and the proposed mechanisms.
The recent work reinforces the need to distinguish between material arrangement, architecture, and loading history. Jeong et al. examined friction and material damping in nonlinearly elastic TPU metamaterials and showed why loading work and dissipated energy require separate treatments [23]. O’Connor compared dual TPU/nylon arrangements and found that the material placement and infill pattern affected their mechanical responses [24]. Wu et al. investigated the energy absorption and rebound in TPU lattices under cyclic compression [25]. These studies provide a complementary context, but their geometries and loading paths do not supply quantitative predictions for the present reinforced-polyamide sandwich beams.
The contribution of the present study is a comparison of two reinforced-polyamide face materials, five TPU core architectures and two nominal infill levels within a common beam geometry and four-point loading arrangement, with solid-core controls. Evaluating stiffness, peak force, displacement and prepeak work together reveals when a design favors load capacity at the expense of deformation capacity. Relative to the slicer-interlocked interfaces studied by Elhassan et al. [18], the present beams use co-printed interfaces without designed mechanical interlocks. The equivalent-core calculation is included to expose the limits of a common simplifying assumption; it is not proposed as a new topology-resolved or validated predictive model [26].
2. Materials and Methods
2.1. Materials
The face materials were Nylforce carbon-fiber-reinforced nylon (PA-CF) and Nylforce glass-fiber-reinforced nylon (PA-GF), supplied by FiberForce Italy. UltiMaker TPU 95A formed the common core. Both faces of each beam used the same reinforced polyamide, and each face-material set used its corresponding feedstock throughout. Manufacturer documentation identifies these feedstocks and provides orientation-dependent printed-coupon properties [27,28,29]. The carbon-fiber-reinforced polyamide (PA-CF) and glass-fiber-reinforced polyamide (PA-GF) filaments were supplied by Fiber Force Italy S.r.l. (Treviso, Italy). The thermoplastic polyurethane (TPU 95A) filament was supplied separately by UltiMaker B.V. (Geldermalsen, The Netherlands).
The manufacturer lists densities of 1.00 g/cm3 for PA-CF and 1.07 g/cm3 for PA-GF [27,28]. Its 100% infill XY coupon results give tensile strengths of 66.3 and 64.7 MPa and tensile moduli of 2758 and 2534 MPa, respectively. The flexural moduli of 3606 MPa for PA-CF and 2820 MPa for PA-GF used in the numerical model correspond to specific supplier flexural-test entries, rather than measured properties of the faces in these beams. For TPU, the specified modulus (63 MPa) approximates the supplier flexural modulus (62.6 MPa) and is used only as an uncalibrated scalar elastic input. Data from the manufacturer are used for context and to show the source of the model rather than to replace tests at the beam level.
The supplier conditions differ from the present beam fabrication. The FiberForce sheets report 100% infill XY coupons printed on an Ultimaker 2+ with an Olsson Ruby nozzle, a 45° raster, a 260 °C nozzle, a 70 °C bed and a 40 mm/s speed; the quoted flexural moduli are ISO 178 entries [27,28]. The TPU sheet reports ISO 178 flexural data for fully filled coupons printed with an UltiMaker S5 Pro Bundle, an AA 0.4 mm print core and 0.15 mm layers [29]. The present beams instead used the co-printing settings in Table 1, including 0.20 mm layers and reinforced-polyamide CC 0.6 mm print cores. Coupon geometry, deposition direction, moisture condition and the thermal history of co-printing therefore limit direct transfer of the supplier moduli. These scalar inputs define an uncalibrated elastic baseline; no measured constituent moduli or independent correction factors are available for these beams [15,27,28,29].
Table 1.
Experimental factors and levels.
2.2. Experimental Design
Two face materials, five patterned TPU cores and two levels of nominal infill were used; 20% and 40% infill for Grid, Cross 3D, Honeycomb, Gyroid and Line cores were used and a solid/100% TPU core was used for each face material. The matrix therefore comprised 20 patterned configurations and two solid-core controls, giving 22 configurations in total. This design is a factorial design with the design parameters chosen all existing within a common beam structure. This is common when looking at design for architecture in printed sandwich structures [3,4,5,6,7]. The design and response parameters are shown in Figure 1 and the parameters are detailed in Table 1.
Figure 1.
Design factors and structural response quantities. The 20% and 40% levels denote nominal slicer infill, and the solid-core controls are considered separately.
2.3. Specimen Architecture
The nominal thickness, width and length of the beam were 10 mm, 20 mm and 100 mm, respectively. The samples consisted of a 6 mm core of TPU with two faces of reinforced polyamide that were 2 mm thick each. Nominal outer dimensions and layer thicknesses were maintained in order to compare global behavior across different topology, nominal infill and face materials. Assuming perfect bonding and elastic behavior [21], the nominal neutral surface is midway through the part thickness. The manufactured samples are shown in Figure 2.
Figure 2.
PA-CF/TPU and PA-GF/TPU sandwich specimens representing the investigated core architectures and infill levels.
2.4. Specimen Fabrication
The beams were produced using FFF on an UltiMaker S5 with core shapes taken from the slicer. The UltiMaker S5 3D printer was manufactured by UltiMaker B.V. (Geldermalsen, The Netherlands). Specimen slicing, infill architecture selection, and toolpath generation were performed using UltiMaker Cura software (version 5.x; UltiMaker B.V., Geldermalsen, The Netherlands). Both face and core were printed as a multi-material single beam. No mechanical interlock was created by the slicer and no separate adhesive-bonding step was used between the layers. Toolpath and model examples can be seen in Figure 3. The animated Cura layer view for 20% infill is available in the Supplementary Video S1. The preview illustrates the prescribed deposition paths rather than the resulting interfacial properties or measured core density. Designed mechanical interlocking, as used in other studies, was not introduced in this process [18]. A summary of the printing parameters that were used can be found in Table 2. The nozzle and bed temperatures for the PA-GF and PA-CF materials match the information provided by the material suppliers [27,28]. The reinforced polyamides and the TPU all used the same build platform during co-print. The build platform temperature range listed therefore refers to co-printing. Configuration-specific values cannot be recovered from the reported ranges. The effects of print orientation and deposition are also important to the final printed part [7,12,15].
Figure 3.
UltiMaker Cura model and toolpath views. Colors indicate slicer line types; the displayed percentages are nominal infill settings. Supplementary Video S1 shows the progression of the 20% layer preview. The model and toolpath previews were generated using UltiMaker Cura software (version 5.x; UltiMaker B.V., Geldermalsen, The Netherlands).
Table 2.
Recorded printing settings for the integrated beams.
Table 2 records the available process ranges, rather than configuration-specific set points or measured equipment variability. Face material, core topology and nominal infill were the intended design factors; the available records do not establish which value within each range was applied to every configuration. It is therefore not possible to confirm that all other settings were identical or to assign differences solely to topology. Configuration-resolved machine records, actual thermal histories and moisture-conditioning records would be needed to separate these contributions in a future controlled comparison [7,12,15].
Figure 2 documents the manufactured specimens, while Figure 3 links the specimen geometry to the slicer representation. The 20% and 40% previews in Figure 3 illustrate changes in prescribed material occupancy; they do not establish measured relative density. A configuration-resolved record of raster angles and cell orientation is not available for all five patterns, so the present results cannot isolate an orientation effect independently of core topology [6,7,10].
2.5. Four-Point Bending and ASTM Applicability
Four-point bending tests were performed using a WDW-10 universal testing machine (Shimadzu, Kyoto, Japan) equipped with a four-point bending fixture. The lower supports were spaced a distance L = 80 mm apart and the upper noses were spaced 40 mm apart. The distance between each nose and the corresponding support was the shear span, a = 20 mm. A total machine force of F was applied half on each upper nose (F/2). The nominal reactions were F/2 at the lower supports. Positive displacement denotes downward movement of the loading fixture or crosshead. The nominal configuration and force application scheme are shown in Table 3 and Figure 4, respectively.
Table 3.
Nominal specimen and loading geometry.
Figure 4.
Nominal four-point fixture and layered section. F is the total applied force; each upper nose carries F/2.
ASTM D6272-25 is the four-point flexural test method for plastics and includes a loading span equal to one-half of the support span [19]. For sandwich-specific properties, ASTM C393/C393M-20 addresses core shear by beam flexure, ASTM D7249/D7249M-20 addresses facesheet properties by long-beam flexure, and ASTM D7250/D7250M-20 provides a practice for determining flexural and shear stiffness [20,30,31]. These standards provide methodological context; the present geometry is used for comparative structural testing rather than a claim of full compliance with constituent-property determination. The span-to-thickness ratio is L/h = 8 and the face-to-core thickness ratio is tf/tc = 0.333. These ratios fall outside the simple-sandwich-theory guidance in ASTM D7250/D7250M and D7249/D7249M, which recommends a span-to-thickness ratio above 20 and a face-to-core thickness ratio below 0.1 [20,31]. Maximum force is reported directly and is not converted to a standardized core-shear or facesheet strength. Loading proceeded through substantial deformation, without establishing a common fully separated fracture endpoint. Analysis is therefore restricted to the response up to maximum force.
Four-point bending was selected to compare complete sandwich beams under a common structural loading path, with a central constant-moment region and outer regions carrying transverse shear. It does not independently identify tensile, compressive, core-shear or interfacial properties, and the short span makes local contact and shear compliance particularly relevant [19,20,21,30,31]. Separate constituent tests, interface fracture or adhesion tests, and tests at additional span ratios would be required to resolve those properties and their contributions. Such measurements are outside the present dataset; the conclusions are consequently limited to comparative beam response under the stated geometry [32].
2.6. Force–Displacement Processing
The force–displacement records were processed using total force and positive crosshead displacement. The initial seating/slack segment, including the recurring plateau near 110 N, was excluded from the elastic regression. Candidate fit starts within the first 0.50 mm of the main loading branch were evaluated over windows spanning 0.40–1.20 mm. The longest initial window attaining R2 of at least 0.997 was selected; the threshold was relaxed successively to 0.995 and 0.990 when necessary. No smoothing was applied to the regression or offset-intersection data. This is a study-specific processing rule; its output is interpreted through the force–deflection framework of beam mechanics [20,21].
Initial structural stiffness Ke was the ordinary-least-squares slope of the selected branch. The same slope was converted to a geometry-specific apparent modulus using the loading-point, rather than midspan, Euler–Bernoulli relation derived in Section 4 [21]:
In Equation (1), the overbars are averages over the N data points in the selected fit interval. With force in N and displacement in mm, Ke has units N/mm. For the nominal geometry, Eapp in MPa equals 3.2 times Ke in N/mm. This apparent modulus includes the effects of core shear, contact indentation, interface deformation and fixture/machine compliance present in the measured displacement. It is neither a constituent modulus nor the separately identified sandwich bending rigidity of ASTM D7250 [20].
The fitted intercept c defines a displacement-origin translation. Subtracting δt removes the extrapolated toe offset but does not remove load-dependent compliance:
An operational 0.2% offset was defined from the ideal homogeneous-beam outer-fiber strain relation. Combining εmax = Fah/(4D) with the loading-point deflection in Section 4 gives εmax = 3hδb/[a(3L − 4a)]. The corresponding displacement offset is therefore as follows [21]:
The operational yield force Fy is the first post-elastic intersection of the measured curve with the parallel offset line:
The 0.2% offset is an operational comparison convention, not a measured 0.2% strain in either face or an ASTM-defined sandwich yield property [19,20]. In a compliant-core beam, crosshead displacement contains shear, indentation and system contributions in addition to the ideal bending term. Equation (3) therefore does not establish local yielding; it only fixes the same displacement-offset rule for all curves. No offset-sensitivity study is available, so Fy rankings are conditional on this chosen convention and should be considered together with Ke, Fmax and Up rather than as intrinsic material yield values.
The peak force (Fmax) and corresponding translated displacement (δ*max) were determined. This is important for TPU parts due to time-dependent and recoverable deformation that can occur well before the peak force is reached [10,11]. Up represents the work done up to the peak force. It is the area under the positive force curve from the translated origin to the point of peak force. F is in N, δ is in mm and Up is in J. The units are provided for clarity.
F+ = max(F, 0), where j denotes the chronological peak-force point and the integration ends are interpolated. A trapezoidal sum is computed first in units of N·mm and then multiplied by a factor of 10−3 to yield J. Up is generated by the crosshead and thus includes contributions due to local contacts, compliance in the testing system, and energy in the specimen. The measured work accounts for the system and structural response plus any test system effects, without accounting for the dissipative versus recoverable portions of the response. The work is considered to be accumulated to maximum force and not fracture energy. Energy-based comparisons to architected sandwiches must account for differences in load paths and integration endpoints [9,14]. Separating dissipation from recoverable work requires unloading or cyclic information, as illustrated in recent TPU metamaterial studies; such information is not provided by the present monotonic prepeak integral [23,25].
2.7. Comparative Response Measures
The change between nominal infill values was determined to be 100(X40 − X20)/X20 for each value X. The mean values at each infill level are calculated as an arithmetic average across the five topology variants. For face material comparisons, equivalent topology/infill combinations are used. These values pertain to the design of the test collection and the nominal infill value is not used as a value relative to measured porosity. Efficiencies on a per-mass basis are not made and stiffness and work are measured in absolute structural units [6,22].
The means across the five topologies describe a set of different designs; the topologies are not repeated observations of one material–geometry condition. Configuration-level repeat counts and individual repeat measurements are not available in the present analysis, so within-condition standard deviations, confidence intervals and significance tests cannot be established. Computing a standard deviation across unlike topologies would describe design variation rather than experimental repeatability. Accordingly, the reported percentage changes and rankings are descriptive, and small differences should not be interpreted as statistically resolved. Independent repeated specimens with documented conditioning and configuration-specific records are required before population-level comparisons can be made [7,19]. Surface roughness measurements were performed using a PosiTector RTR 3D surface profile measurement instrument (DeFelsko Corporation, Ogdensburg, NY, USA). Surface texture characterization was conducted using the ASME B46 surface texture framework. The measured surface roughness parameters and three-dimensional surface topography maps are presented in Section 5.9.
3. Finite Element Method
3.1. Geometry and Loading
A static 3D model of the structure was created using ANSYS Workbench 2026 R1 (ANSYS, Inc., Canonsburg, PA, USA). The model included the nominal dimensions of the 100 × 20 × 10 mm beam, both 2 mm faces and the 6 mm core. Four cylindrical rollers were also incorporated to simulate the experimental 40 mm load and 80 mm support spans. Figure 5 displays the model and mesh. The layered beam is compared to previous studies that have utilized finite element analysis to investigate the behavior of printed sandwich structures while continuing to employ the same level of material simplification as outlined below [9,13].
Figure 5.
Finite-element assembly and mesh. Patterned cores were represented by equivalent homogeneous regions, without explicit internal topology.
The lower rollers were constrained in translation. The upper rollers were free to translate in the vertical direction but constrained in all other directions. The total force applied was shared equally between the upper rollers. The load conditions used were the measured values of Fy and Fmax. These values were specified inputs and were not a computed value for yield or failure. Inertial and gravitational effects were turned off and thus density had no effect on the solution via body forces. For displacement purposes, the vertical displacements of the two upper-roller loading regions were averaged and this value can be related to motion of the loading fixture/crosshead rather than midspan displacement [20,21].
3.2. Constitutive Assumptions and Equivalent Core
The faces were modeled as homogeneous isotropic linear elastic materials. For PA-CF, the elastic modulus E was 3606 MPa and, for PA-GF, 2820 MPa. These are supplier data for the flexural modulus [27,28] and used as scalar elastic proxies for each face. These are not independently determined Young’s moduli for the printed face material. The assumption of isotropy neglects the directional effects found in printed-fiber-reinforced polymers [15]. The modulus of the solid TPU was taken to be 63 MPa, in line with the supplier data for the flexural modulus [29]. For the patterned cores, a continuous material was used with a modulus of 12.6 MPa for the 20% infill and 25.2 MPa for the 40% infill. These values are calculated by multiplying the nominal infill by the modulus of the solid. This relation is assumed and is neither a constitutive relation nor a topology-derived homogenization [22]. All materials were assigned a Poisson’s ratio of 0.30 in order to simplify the linear-elastic finite element model. An explicit material model for TPU would need to be defined for a more accurate model. The data used and their sources can be seen in Table 4.
Table 4.
Material inputs for the finite-element baseline. Density is inactive in the stated loading; ν is assumed.
Equivalent cores are not capable of distinguishing between Gyroid, Cross 3D, Honeycomb, Line, or Grid at the same nominal infill. The idealization omits discrete cell-level face support, collapse, deposition-induced directionality, and the bending, rotation and deformation of individual cell walls. However, these factors have been shown to impact mechanical properties separate from nominal material at certain lattice structures printed with TPU [10,11,12]. For this reason, the numerical examples along with the Grid tests use equivalent core at the same nominal material and are not topology-resolved Grid tests.
3.3. Contact and Interface Representation
All roller-face contacts were assumed to be frictional with a coefficient of 0.20. No relative sliding or opening was assumed at the face-core interfaces. Such assumptions provide an ideal load transfer mechanism, but do not imply that the actual printed interfaces between the skin and core are perfectly bonded through deformation. Instead, the potential influence of variations in interface transfer on the overall behavior of the sandwich structure can be explained by studies on printed interlock and skin-core debonding [17,18]. Interface deterioration and fixture compliance are beyond the scope of this study.
The co-printed face–core interface was not characterized by peel, shear or fracture tests, and no measured interfacial temperature history is available. Perfect bonding is therefore an idealization, not a measured interface property. Studies on carbon-fiber-filled polyamide/TPU and glass-fiber-filled nylon/TPU show that thermal treatment, overlap and interface geometry can affect adhesion [33,34], while nylon interlayer cohesion also depends on thermal history and crystallization [35]. The external-surface measurements are discussed in Section 5.9; they do not measure the buried interface or validate the bonded contact condition. Dedicated interface characterization is needed before introducing calibrated slip, separation or cohesive-damage laws.
3.4. Mesh and Solver Scope
A swept solid mesh based predominantly on quadrilateral face elements used a nominal element size of 1.0 mm and a defeature size of 0.10 mm. There were 23,460 3D solid elements and 107,527 nodes in the model. Large Deflection was turned on. This implies geometric nonlinearity with linear elastic materials and cannot be characterized as a small-deflection linear-static simulation. This includes kinematic effects but does not model the material nonlinearity or deposition-dependent constitutive behavior exhibited by printed polymers [12,15]. TPU viscoelasticity, nonlinear material response, core crushing, interface debonding, and progressive face damage were not included in the model. A specific mesh/contact setup is used in the numerical study to create an equivalent core that can be compared to the experimental results. A study on contact sensitivity and mesh convergence in quantitative terms is beyond the scope of the current baseline. The comparison is consequently used to assess the limits of the idealization, with topology-sensitive and constitutive approaches in the literature providing the basis for more detailed modeling [9,11,15].
3.5. Comparison with the Experiment
Equivalent-core cases paired with Grid at 20% and 40% infill and with the solid controls were assessed for both face materials. The total support reaction was checked against the total applied force. Numerical loading-point displacement was compared with the translated experimental displacement δ*, using the same positive-downward convention. The relative discrepancy was calculated as 100|δFEA − δ*exp|/δ*exp. This discrepancy quantifies disagreement at the prescribed loading states; it does not establish agreement or identify an individual deformation mechanism [20,21].
The experimentally measured operational-yield and maximum-force loads specify two states on each curve. Because the model does not predict damage or failure, these states are comparison loads only. Quantitative conclusions about material strength, failure sequence or absorbed energy are not inferred from these solutions. The results in Section 5.7 are interpreted alongside the model’s topology and material limitations [9,10,11,12,15,17].
4. Theoretical Analysis
An analytical reference relates the section rigidity to the initial loading-point response. It assumes a symmetric, perfectly bonded beam with identical faces and small-deflection Euler–Bernoulli bending [21]. Cellular-material scaling is used to explain why the nominal infill and effective stiffness must be distinguished [22]. The analysis is a mechanics reference and does not fit the measured curves.
4.1. Relative Density and Core Stiffness
The relative density of the printed core can be defined by Equation (6). For this investigation, the nominal slicer infill was used as the design parameter between core types and core mass fractions were not measured. For this reason, the nominal infill is used as a design parameter and not a value for the relative core density [22]:
The mc,p is the mass of TPU in the core and Vc,p is the volume of the gross core excluding the face areas. The infill volume within a nominal slicer does not directly define rp. The printed shape, solid layers and walls all add to the overall mass. The bulk density of a printed cellular core can be related to the density of solid TPU by the relative density of the core (Equation (6) [22]). For this work, the nominal slicer infill was used as the design variable of interest across different core designs. The nominal infill is not used to represent a specific relative density since the mass of the cores was not measured experimentally. Instead, the effective properties used in the finite element model rely on an explicit simplification and not an experimentally derived value for the core density:
The architecture parameters Cp and np influence the effective longitudinal modulus Ec,p. However, neither parameter was determined in this study and there is no common exponent across the five lattice types. This is expected due to the architecture and direction dependence exhibited by printed TPU lattices [10,12]. Instead, the finite element reference uses the explicit model assumption:
With the assigned solid TPU modulus of 63 MPa, Equation (8) gives 12.6, 25.2 and 63 MPa. It documents the numerical inputs and is not an experimentally established instance of Equation (7). It also assigns the same modulus to every topology at a given nominal infill [22].
4.2. Layered Section Bending Rigidity
For width b, face thickness tf and core thickness tc, the total thickness is h = 2tf + tc. Symmetry places each face centroid a distance d from the neutral axis. The parallel-axis theorem then gives the complete elastic bending rigidity of the three layers, including the local bending contribution of each face [21]:
For b = 20 mm, tf = 2 mm and tc = 6 mm, Equation (10) becomes the following:
D has units N·mm2 when the moduli are expressed in MPa. Ec,eff is the effective modulus of the longitudinal core. The examples in this paper utilize the face modulus approximations given in Table 4 but these do not establish the properties of the actual printed faces. A thin-face approximation [21] is not applied since the thickness of the face is significant in comparison to the core. Thus, the local face contribution of btf3/12 is kept.
4.3. Loading-Point Response and Compliance
With total force F shared equally between the noses, the constant moment in the inner span is Fa/2. Integrating the piecewise beam curvature, or differentiating the bending strain energy with respect to the generalized force F, gives the displacement at either loading point [21]:
Using D = Ebh3/12 in Equation (14) for a homogeneous rectangular section results in the apparent modulus formula shown in Equation (1). This confirms the coefficients for displacement at the loading points and total load. A coefficient derived for midspan deflection would be inconsistent with the displacement measured here. The strain-induced displacement in Equation (3) is derived using the same small deflection assumption as mentioned in [21].
The shear flexibility of a beam provides an explanation for the observed slope being lower than the ideal bending-only slope. For a constant effective shear rigidity in the plane of bending, S, the shear displacement at the loading point is Fa/(2S). The measured incremental compliance in the initial branch can therefore be represented schematically as follows [20,21]:
S has units N. Csystem and Clocal represent the machine/fixture and local specimen/contact effects, respectively. Both are incremental compliances with units mm/N. Equation (15) represents an analysis of compliance contributions, not a fitted constitutive model. The contributions are not separated using only one span and crosshead displacement. The geometric limits noted in Section 2.5 and the large later deflections further restrict the analytical equations to an initial elastic reference [20,21,31].
5. Results and Discussion
5.1. Force-Displacement Response
The patterned configurations exhibited an approximately linear branch followed by nonlinear load–displacement behavior (Figure 6). The maximum-force-to-offset-yield-force ratio ranged from 1.43 to 2.42, while δ*max/δ*y ranged from 2.38 to 6.55. The operational offset criterion therefore identified an early structural departure from the fitted slope, with a substantial additional load or deformation possible afterward. Such separation between the initial response and subsequent deformation is consistent with the flexible TPU lattice and sandwich behavior [10,11,13,14].
Figure 6.
Total machine force versus translated loading-point/crosshead displacement for the patterned beams. The retained initial plateaus are acquisition features excluded from the elastic fits; a displacement-origin translation does not remove them: (a) force at PC-CF 20%, (b) force at PC-CF 40%, (c) force at PC-GF 20%, and (d) force at PC-GF 40%.
Line and Gyroid structures often showed load over a greater range of displacement. Grid showed the highest initially patterned stiffness for both face types. Honeycomb showed only a small response to the nominal increase in infill. Such observations highlight the importance of not using a single criterion of maximum force to rank structures, as it would mask the behavior of the internal structures. Previous research into pattern-sensitive behavior has also shown the importance in ranking force, deformation, and stiffness together rather than using a single parameter [5,6,7,9], but has not provided insight into the specific behavior of the current structures.
5.2. Effect of Nominal Infill
For PA-CF, the mean for Ke increased from 77.0 to 115.6 N/mm as the nominal infill was increased from 20% to 40%. The mean for Fy increased from 241.6 to 344.2 N. The mean for Fmax increased from 421.9 to 657.0 N. The mean for Up increased from 4.008 to 5.908 J. The corresponding increases were 50.1%, 42.5%, 55.7% and 47.4%, while the mean δ*max decreased by 3.5%. For PA-GF, the increases were 49.9%, 38.4%, 42.6% and 21.1%, with the mean δ*max decreasing by 13.4%. These are descriptive averages across different topologies, subject to the statistical limitations in Section 2.7.
The observed similarity in the increase in stiffness between the two face types is also in agreement with the expected enhancement in load and support transfer with increasing nominal core volume. The observed differences in work reveal that the late response also depends on the interaction between the faces and deformable core. Cellular scaling relates stiffness to both the absolute relative density and structure [22]. Simply doubling the nominal slicer infill does not result in a proportionally increasing stiffness. There are also other factors contributing to a subproportional response including local contact, deformation that varies with topology, and the fixed contribution of the faces [6,10,21].
5.3. Core Topology
The Grid shape displayed the most stiffness driven response. For the PA-CF Grid with the 40% infill, the values of Ke = 173.2 N/mm and Fmax = 837.0 N were the highest among the patterned configurations in the test matrix. PA-GF Grid with the 40% infill showed the greatest patterned stiffness for this face material at 150.0 N/mm. The value for Fmax (709.2 N) was also very similar to PA-GF Gyroid (709.8 N). This can likely be attributed to the relatively straightforward load transfer through the part and support for the face. This can also be related to studies of pattern-dependent bending [5,6,7]. The global curves do not, however, indicate a purely stretching-dominated deformation.
Gyroids exhibited a large deformation and sustained force. For PA-CF at 40% infill, Up was 8.21 J and δ*max was 14.84 mm. For PA-GF at 40% infill, Up was 7.77 J and δ*max was 15.07 mm. There exists potential for the deformation to be transmitted via curved load paths. There have been previous works on TPU lattices and gyroid core sandwiches that display structure-related force transmission [10,16]. These works use varying loads and materials, and are not meant to provide a transferrable quantitative value, but rather do show that deformation can be transmitted via structure.
The Line showed the best performance in the PA-GF 40% condition with 8.30 J of patterned Up, 16.39 mm of displacement and a force of 656.0 N. The work advantage of Line is due to the area under the curve up to the peak rather than the peak force itself. The direction of the loading paths may play a role due to the effect of the raster and infill angle on FFF [6,7]. A deposition orientation and/or in situ load transmission effect is possible based on the response exhibited in this study. The effects of each, however, cannot be separated from the overall force-displacement responses.
Cross 3D demonstrated moderate stiffness with significant later deformation. For the 40% infill, PA-CF had Up values of 7.67 J and PA-GF had 7.15 J. The intersection may allow for face support and/or the bending or rotation of members. However, this assumption depends on the actual printed structure. Research on printed lattices has shown that deposition and connectivity may affect deformation apart from the apparent degree of infill [6,10,12].
The least response to an increase in nominal infill was shown by the honeycomb. PA-CF specimens experienced a 0.7% increase in Ke, but a 6.5% reduction in Fy, 2.6% in Fmax and 4.4% in Up. PA-GF specimens experienced an 8.2% reduction in Ke, but a 2.8% increase in Fmax and a 2.0% increase in Up. This suggests that the added nominal infill did not result in a consistent structural gain for this part. Cell-wall bending, local face support and honeycomb orientation are known to play a role in other studies [5,8,10]. However, the present curves do not separate these effects from interface or indentation effects.
5.4. Interaction with Face Material
The influence of the face material depended on the core topology (Figure 7). At 40% infill, PA-CF showed greater stiffness than PA-GF for Grid, Line and Gyroid. For Honeycomb and Cross 3D, PA-GF was slightly stiffer. PA-CF showed the greatest patterned force across all structures and PA-GF Line showed the greatest patterned work. This suggests that the advantage gained from using a particular face material is dependent on the load path through the core. The higher supplier flexural modulus of PA-CF alone therefore cannot predict every beam ranking [27,28].
Figure 7.
Comparison of initial stiffness, operational offset-yield force, maximum force and prepeak work. Up denotes work to maximum force: (a) initial stiffness, (b) yield strength, (c) max force, and (d) work at max force.
Printed-fiber directionality, face porosity, local core support and interface transfer can all influence the effective rigidity of the layered section. Scapin and Peroni showed the importance of directional material representation for printed reinforced nylon, while the deposition studies identify similar issues in TPU lattices [12,15]. The present comparisons consequently concern integrated beam configurations. They do not isolate carbon- versus glass-fiber reinforcement as a constituent-level causal effect.
5.5. Load Capacity, Deformation and Work
PA-GF Grid shows the clearest competition between stiffness and prepeak work. Increasing the infill raised Ke by 59.1%, Fy by 15.8% and Fmax by 50.8%, but δ*max fell from 16.09 to 7.49 mm and Up from 6.19 to 3.35 J. Thus, a 53.4% reduction in the displacement to maximum force outweighed the increased load, producing a 45.9% work reduction. This follows directly from Equation (5). Work-based selection in architected sandwiches must therefore account for the full loading path and its endpoint [9,14].
PA-CF Line showed a milder version of this tradeoff: Fmax increased by 79.0%, δ*max decreased by 24.1%, and Up increased by only 17.8%. PA-CF Gyroid instead combined a 104.1% force increase with a nearly unchanged δ*max, raising Up by 96.1%. These contrasting outcomes support a conditional design choice: Grid favors the highest initial rigidity in this matrix, while Line and Gyroid merit attention when greater displacement before maximum force is useful. Such choices remain specific to the present geometry and displacement measure [6,9,10,16].
The solid-core controls reached the largest load capacities (Figure 8). PA-CF attained 1615.6 N and 18.80 J, respectively, 93.0% and 129.0% above the best patterned PA-CF values. Its initial stiffness, 170.8 N/mm, was nevertheless 1.4% below that of PA-CF Grid at 40%. PA-GF solid gave the highest overall stiffness, 199.7 N/mm, and reached 1194.6 N and 11.98 J. Dense core support can improve later load resistance, while the initial measured slope remains sensitive to the full face–core–contact system [20,21]. These absolute results do not establish mass-specific superiority.
Figure 8.
Solid-core force–displacement responses. Markers identify the operational offset-yield and maximum-force states. The PA-GF trace includes a local load drop before further loading.
5.6. Observed Deformation
There is pronounced global curvature and local deformation under and between the load noses in the solid core samples. There is also no evidence of a single fully separated fracture tip. The combination of a small span-to-thickness ratio and the presence of these features makes variations in the contact, indentation, core shear and changing contact conditions possible explanations for the response observed in the crosshead [20,21,30,31]. The deformation observations presented here focus on the solid-core controls, while the patterned configurations are compared using their measured force-displacement responses.
The PA-GF solid-core sample displayed an initial decrease in force locally before the reappearance of load. This behavior may indicate a shift in load transfer within the structure. Such a response could also be attributed to a modification in local contact or to a mechanism occurring at the interfaces. These possibilities were explored in previous studies on sandwich structures [17,18]. The force–displacement data and deformation images do not distinguish between these potential causes.
The direct evidence comprises the global force–displacement records and the macroscopic deformation photographs in Figure 6, Figure 7, Figure 8 and Figure 9. It does not include fracture-surface microscopy, internal imaging or local strain fields. Cell-wall bending, indentation, core shear and interface damage are therefore candidate explanations, not experimentally identified failure modes. Distinguishing between these processes requires local deformation measurements and post-test section or fracture examination, because multiple sandwich failure mechanisms can interact [32]. The external topography in Section 5.9 provides surface-texture context but cannot establish the state of a buried interface or a fracture path; interface-specific evidence of the type reported by Jafor et al. would be needed for that attribution [33].
Figure 9.
Deformation of the solid TPU-core controls with PA-GF faces (a,b) and PA-CF faces (c,d). The photographs document global curvature and local deformation at different loading stages.
5.7. Analytical and Finite Element Comparisons
The analytical reference predicts a bending-only initial stiffnesses of 884.3 and 885.2 N/mm for PA-CF at the 20% and 40% nominal infill, and 691.8 and 692.6 N/mm for PA-GF. The measured Grid values were 112.1 and 173.2 N/mm for PA-CF, and 94.3 and 150.0 N/mm for PA-GF. The difference is consistent with the distinction between ideal section bending and measured crosshead compliance in Equation (15), but it cannot be assigned solely to the core shear because the face properties, contact and test-system compliance were not independently identified [15,20,21]. The analytical model is also almost insensitive to the infill change: its stiffness rises by approximately 0.10% for PA-CF and 0.12% for PA-GF, compared with measured Grid increases of 54.5% and 59.1%. Equation (11) explains this result. The ideal longitudinal rigidity is dominated by the face terms, so changing the small longitudinal core term barely alters D. The substantial experimental change therefore involves responses not represented by this bending-only substitution, including core-mediated shear transfer and local face support [20,21,22].
The support reaction forces computed by finite elements compared well to the total loading applied but the displacement at the loading point was computationally less than the measured displacement for all tests performed. The relative displacement discrepancy between the computational and measured results varied between 45.28% and 88.03%. At the operational yield load for the 20% infill PA-GF Grid, the computed displacement was 2.022 mm compared to the 3.695 mm measured and, at maximum load, 2.627 mm compared to the 16.092 mm measured. For the solid PA-CF part at maximum load, the computed displacement was 2.099 mm compared to the 17.529 mm measured. All other displacement discrepancies demonstrate that the structural sensitivity to core design, interface properties, constitutive properties and experimental implementation is not completely captured by the equivalent core model. At the operational yield load, the computed secant stiffness (F/δ) for PA-CF Grid is about 94.5–109.6% higher than measured. At maximum load, the computed secant stiffness (F/δ) is about 223.4–241.4% higher than measured. These results for different loading conditions are not directly comparable to the initially fitted Ke because they are not equivalent values. Geometric nonlinearity was accounted for in the numerical solution; other errors in displacement likely result from the interaction of several additional factors not captured in the simplified model. Other effects that are not accounted for include material nonlinearity, deformation associated with part geometry, anisotropy due to the printing process, interfacial degradation, real contact and compliance within the testing system [9,10,11,12,15,17]. The equivalent core model shows the limitations of the reference model used for quantitative displacement prediction. The model is used to examine the global displacement response rather than topology ranking or failure prediction. A prediction model would require direction-dependent material properties in the printed faces, an appropriately calibrated nonlinear TPU model, an explicitly resolved or adequately homogenized anisotropic core, calibrated interface and contact behavior, and mesh/contact convergence [9,11,12,15,17]. Static solutions cannot be enhanced using only the density variation because inertia and gravity are not present. This analysis is focused on the limitations of the modeling approach used.
The numerical contribution is thus a documented test of the equivalent-core assumption against the measured global displacement at prescribed loads. The reaction balance checks the equilibrium, not predictive accuracy. The reported displacement discrepancies are too large to regard the model as quantitatively validated, and the available results do not provide validated stress or displacement-field comparisons. Stress contours from this idealization would not identify failure in the unrepresented cells or interfaces. Topology-sensitive homogenization or explicit cell models, as illustrated for lattice-core beams by Nampally et al. [26], and independently calibrated nonlinear TPU behavior, as used in a different metamaterial setting by Jeong et al. [23], are appropriate future developments. They require material and interface data, convergence studies and independent validation that are not part of this revision.
5.8. Interpretation Limits and Design Implications
The results presented are for the specific design and geometry of the beam, the fabrication process used and the displacement measured via the crossheads. The apparent modulus, operational offset force and prepeak work represent responses of the structure while the nominal infill is considered as a design variable and not a relative density measured via the printed polymer. A fundamental bending solution is provided and a comparison is made to a homogenized structure using an equivalent core model rather than by attempting to model individual cell deformation within the structure. This methodology has previously been used in both printed polymer and sandwich structure testing [15,20,21,22,30,31].
The research also makes a design distinction that is useful within this context. By increasing the initial stiffness, the peak force location can shift and the displacement range over which energy can be stored can decrease. For this reason, a combination of face and topology selection is more revealing than either maximum force or nominal infill alone. This analysis is furthered by comparing the different designs (Grid, Line and Gyroid) and by continuing the material-design interaction seen in previous studies of printed sandwich structures [2,9,13,14,16,18].
5.9. Surface Roughness and Interfacial Bonding
The FDM-printed sandwich beams comprised either carbon-fiber-reinforced polyamide skins surrounding a thermoplastic polyurethane core (PA-CF/TPU/PA-CF) or glass-fiber-reinforced polyamide skins surrounding the same core material (PA-GF/TPU/PA-GF). Both systems exhibited a pronounced difference between the rough, last-printed external top surface and the smoother, bed-contact bottom surface. This distinction is relevant to contact during flexural testing and to the interpretation of manufacturing-related defects. Figure 10 presents the four original surface topography maps, and Table 5 summarizes the principal height parameters. The external surface texture and adhesion at the buried skin–core interfaces are considered separately because their mechanical roles differ.
Figure 10.
Original surface topography maps: (a) CF top, (b) CF bottom, (c) GF top and (d) GF bottom. Each panel retains its own height and color scales; x and y are in mm and z is in µm. Apparent relief and color must therefore be interpreted using the individual scales.
Table 5.
Selected texture parameters (µm); one reported field per surface.
For PA-CF, Sa decreased from 15.3 µm at the top to 1.9 µm at the bottom, corresponding to an 87.6% reduction and a top to bottom ratio of 8.1. For PA-GF, Sa decreased from 16.9 to 2.3 µm, an 86.4% reduction and a ratio of 7.3. The profile arithmetic mean roughness, Ra, likewise decreased from 16.7 to 1.9 µm for CF and from 18.3 to 1.3 µm for GF. The aligned ridges and valleys on the upper faces are consistent with the geometry of the final deposited roads. Contact with the smooth build plate plausibly constrained the first layer surface, producing the much lower bottom surface amplitudes. Abas et al. [36] reported a similar dependence of the nylon CF surface finish on printed face and processing conditions.
The GF top surface had 10.5% higher Sa and 14.5% higher Sq than the CF top surface, indicating a greater average and root mean square height variation over the measured area. The corresponding profile RMS roughness, Rq, was 21.8 µm for GF and 18.1 µm for CF, a 20.4% difference. RMS parameters give greater weight to large height deviations than arithmetic mean parameters. The Sq/Sa ratios were 1.13 and 1.17 for the CF and GF top faces, respectively, compared with 1.21 and 1.30 for their bottom faces. Thus, the smoother bottom surfaces still contained deviations that were appreciable relative to their smaller mean amplitudes. These ratios describe the shape of the sampled height distribution; they are not coefficients of variation between specimens.
The extreme height parameters add information that is lost when the comparison is restricted to Ra or Sa. The top GF profile had Rz = Rt = 84.4 µm, compared with 64.3 µm for CF. This difference was associated principally with the greater GF profile peak height, Rp = 57.2 µm versus 34.4 µm; its profile valley depth was slightly smaller, Rv = 27.2 µm versus 29.9 µm. The areal maximum valley depth followed the same ranking, with Sv = 74.7 µm for CF and 69.1 µm for GF, despite the lower CF average roughness. Consequently, a larger average amplitude does not necessarily imply a deeper most severe valley. In every report, Rz equals Rt, so these values should not be treated as independent evidence of different texture characteristics without establishing the software evaluation and segmentation procedures.
On the bottom face, GF had the lower profile Ra, but the higher areal Sa, Sq and Sz: 2.3, 3.0 and 26.1 µm, respectively, versus 1.9, 2.3 and 18.9 µm for CF. This ranking reversal is consistent with the spatial heterogeneity and sensitivity of a single profile to its location and direction. The areal peak density, Spd, was 0.9 mm−2 for both rough top faces, increasing to 5.0 mm−2 for the CF bottom and 4.6 mm−2 for the GF bottom. More detected peaks therefore coexisted with smaller height amplitudes. Peak density measures a different aspect of texture from the roughness magnitude and depends on feature detection; it does not, by itself, establish a greater true contact area or stronger adhesion.
The numerical contrasts are descriptive comparisons of individual measured fields. Sa and Sq summarize spatial heights within a field; they do not provide a specimen-level mean and standard deviation. The four reports do not establish replication within each material face condition, so confidence intervals, significance tests and an independent effect of fiber type cannot be inferred. Differences in matrix grade, fiber content, moisture condition and printing parameters may also contribute. In these measurements, the top to bottom change was substantially greater than the difference between the two top faces, making the manufacturing face the clearest observed distinction.
During flexural testing, each beam was positioned with its rough top surface facing the loading probe and its smooth bottom surface resting on the two support rollers. This maintained the same surface orientation for the CF and GF series. Under the resulting global flexural stress state, the upper skin was predominantly in compression and the lower skin in tension. Accordingly, the larger top surface valleys were situated on the globally compressed side; they should not be described as tensile crack initiation sites solely because they were rougher. Smooth support contact may reduce the seating variability associated with prominent asperities, although that effect was not measured. At the loading probe, the rough upper face may generate nonuniform local contact pressures. These contact stresses, together with the compliance of the TPU core, can contribute to local indentation and must be distinguished from the global stress distribution.
In a sandwich beam, the separated reinforced polyamide skins principally resist flexural normal stresses, while the core transfers transverse shear and supports the skins against local deformation. Skin core debonding disrupts this load transfer and reduces composite action. Relevant failure mechanisms include tensile skin fracture, compressive skin failure or wrinkling, core shear, local indentation and interfacial debonding [32]. Surface valleys may contribute to local stress concentration, but their severity also depends on root radius, orientation and connectivity. The present height parameters therefore cannot identify the governing failure mechanism or establish that one sandwich system has greater strength.
Within each printed polyamide skin, interlayer cohesion depends on intimate contact and molecular mobility during deposition, followed by cooling and crystallization. Vaes et al. [35] demonstrated that thermal history and crystalline morphology influence the interlayer bond strength in nylon copolymers. A smooth external face consequently does not prove strong internal fusion, and a rough external face does not necessarily indicate poor fusion. Pizzorni et al. [37] further showed, in the adhesive joining of printed carbon fiber/nylon 6, that effective surface treatment could shift failure from the adhesive interface into the printed substrate. Although that work did not concern TPU cores, it illustrates why external adhesion and internal interlaminar cohesion must be distinguished.
At the PA-CF/TPU and PA-GF/TPU junctions, surface texture can provide additional accessible area and mechanical interlocking when the deposited material wets the substrate and fills its grooves. If the melt cannot conform to the texture, the same valleys can remain as voids or unbonded regions that interrupt shear transfer. Polymer chemistry, melt viscosity, contact temperature and available bonding time therefore determine whether a textured interface is beneficial. The exposure of carbon or glass fibers, including any sizing, could also alter local wetting, but the external maps do not establish fiber exposure or interfacial chemical composition.
Direct evidence for the CF system is provided by Jafor et al. [33], who studied carbon-fiber-filled polyamide/TPU interfaces and found that bead ironing and hot air treatment improved interfacial fracture toughness; their combined use reduced the average interfacial void volume fraction by 24%. This result links better bonding to thermal history and void reduction rather than to maximum roughness alone. For the GF system, Stano et al. [34] demonstrated that interface geometry, material overlap and annealing affected the bonding between glass-fiber-filled nylon and TPU. These studies support the feasibility of both material pairings, but their different geometries and processing conditions prevent a direct ranking of the two present sandwich systems.
A further qualification comes from Slapnik et al. [38]: within their investigated range, substrate roughness had no statistically significant effect on the tear off strength of TPU overprinted onto injection-molded, unfilled PA6. Their result cannot be transferred quantitatively to the present fiber-filled printed skins, but it shows that increasing roughness does not universally improve PA/TPU adhesion. Moreover, the measured external faces are not the buried interfaces. If the sandwiches were printed sequentially, the lower TPU on the PA junction and upper PA on the TPU junction would also experience different deposition and reheating histories [33]. Neither the higher GF top Sa nor the deeper CF top Sv is therefore sufficient to predict which skin–core interface is stronger. Interface microscopy and dedicated adhesion or fracture measurements would be needed to resolve that relationship.
For the standard-based interpretation of the assembled beams, ASTM C393/C393M-20 [30] provides a relevant framework for flexural testing directed at core shear or core to facing shear strength and sandwich load–deflection behavior. When the intended property is skin strength, ASTM D7249/D7249M-20 [31] addresses facesheet properties in sandwich flexure. ASTM D7250/D7250M-20 [20] provides the associated framework for separating flexural and shear stiffness from suitable load–deflection measurements, with its calculations restricted to a linear force–deflection response. This distinction is especially relevant for a compliant TPU core because the measured deflection can contain an appreciable shear contribution. Standard selection must therefore follow the target property, specimen geometry and observed failure mode. Specimen dimensions, spans, loading arrangement, rate and conditioning are necessary reporting variables for a reproducible comparison of the two sandwich systems. Local indentation or premature skin failure must not be interpreted automatically as a measured interfacial shear strength.
Surface metrology requires a separate standards distinction. ASTM D4417-21 [39] concerns the surface profiling of blast-cleaned steel and does not, by itself, validate roughness measurements on printed polyamide. ISO 25178-2:2021 [40] supplies the terminology and parameter framework for areal texture. Here, both the short-wavelength and cutoff filters were reported as “None,” so longer-wavelength contributions may remain in the reported heights. Comparisons with filtered literature data therefore require matched measurement conditions. The identical top-surface Sz values of 125.0 µm also warrant checking the raw height fields for a possible range limit; equality alone does not establish clipping. If a PosiTector RTR 3D was used, the bottom Ra readings of 1.9 and 1.3 µm are below its specified minimum roughness of 2 µm [41]. Their precise ranking would then require validation with a method suited to that range before being linked to failure or adhesion.
5.10. Finite Element Analysis and Discussion
For the same PA-CF beam with a TPU core at the 20% nominal infill (Figure 11), the highest equivalent stress bands are located near the loading noses. The largest displacement spans the midsection of the beam. Both datasets are based on its Grid test where two upper rollers each support half of the prescribed total force. Both models employ the same elastic material law until the end of loading.
Figure 11.
PA-CF beam with 20% equivalent TPU core. Panel (a) shows maximum equivalent stress of 57.846 MPa. Panel (b) shows maximum total deformation of 89.737 MPa. Panel (c) shows minimum total deformation of 2.0339 mm. Panel (d) shows maximum total deformation of 2.8966 mm. Minimum for this data is 0. Originally, data was in Pa and m. Each plot has its own color scale. The 1 s indicates the end of the static load step.
Based on Table 4, both the core and faces use an isotropic linear-elastic material law. Using a large deflection formulation, the geometry is considered in changing contact conditions as load is applied. Because contact is through frictional rollers, it can change based on the load. Additionally, the face-core contact is considered bonded. Due to these considerations, the plotted data has particular significance. Equivalent (von Mises) stress is a measure of a multiaxial stress state’s strength. Total deformation is the magnitude of the three directional displacement components at a given location [42]. These are depicted in Figure 11 at the specified loads.
Between Fy and Fmax, the maximum total deformation increases by 42.4% while the peak equivalent stress increases by 55.1%. Overall, they occur in different locations. The narrow peaks at the upper rollers show where the beam initially receives the load. Further along, between these two points, there is a wide peak of high deformation that aligns with the bent portion of the beam despite having a lower equivalent stress. Generally, these lines collectively show how applying the load at the noses locally affects the bent beam overall in shape.
5.10.1. Stress Distribution Across Core Configurations
Mainly, Figure 12 displays the mesh and three PA-GF stress fields under their respective maximum loads. Table 6 lists the extrema of the legend under both load conditions. The listed values correspond to the displayed field. Due to different stresses being represented by the same color in some comparisons, the numerical legends are used when comparing between panels.
Figure 12.
PA-GF models stress and mesh contours. (a) Swept mesh: 23,460 elements, 107,527 nodes. (b–d) Under experimental maximum force, stress levels are shown as 0.015032–74.14 MPa for the 20% core, 0.051538–91.353 MPa for the 40% core, and 0.12463–126.43 MPa for the solid core. Simulated specimens with patterned cores are shown using homogeneous core sections.
Table 6.
Minimum and maximum equivalent stress in the displayed fields (MPa).
As described in Section 5.5, we can differentiate between elastic stress and force changes. In the case of PA-GF Grid with the 20% and 40% infill, the force increased by 50.8% but the calculated elastic stress only increased by 23.2% (from 74.14 to 91.353 MPa). When dividing the stresses by their respective forces, in the 40% case, the ratio is approximately 18.3% lower. Based on (91.353/74.14)/1.508, this ratio represents the elastic stress per unit force in both of these conditions. To compare using an equal force method, each core would need to be solved at the same force. In the case of Fy, using the same PA-GF pair, the applied force increased by 15.8% but the calculated elastic stress decreased (from 53.959 to 47.848 MPa). Using a maximum load of 1194.6 N for a solid core (Section 5.5), this stress is 126.43 MPa. Based on this data, using what load condition to compare these elastic stresses determines their order. Using a failure criterion defined independently of the printed material would be necessary in order to determine a strength order with additional evidence regarding what type of failure is occurring.
5.10.2. Comparison with Measured Displacement
As discussed in Section 3.5, the loading fixture comparison uses the following: Model quantity is the average downward displacement of the upper roller loading regions. The experimental quantity is the crosshead displacement converted to the fitted origin (as defined in Section 2.6). This adjusts for the initial offset during seating but maintains stress-dependent compliance. Using the maximum total deformation in Figure 11 would alter both the displacement and what is being compared [42]. Table 7 illustrates a comparison for the two sets of composite materials used, PA-GF and PA-CF, at different infill pattern densities regarding the experimental and FE results.
Table 7.
Selected loading-point comparisons from Section 5.7, with differences calculated from the reported displacements.
At 20% PA-GF, between Fy and Fmax, the computed roller travel is 0.605 mm and the measured crosshead travel is 12.397 mm. Even after adjusting the origin of the measured travel (as a constant difference between two measurements from the same curve cancels each other), this difference continues to increase. At maximum load, there is also a large difference in the solid PA-CF comparison. At this specimen maximum load, there is no patterned core that can be used for homogenization. Based on this, it makes sense to look at the TPU and face properties, compliance and local contact, along with how the patterned core is modeled. In Section 5.7, using the reaction check, we verify that the loads are supported as required. In addition, using displacement (as outlined in Section 4), we can assess the stiffness under that load. In the theoretically perfectly symmetric case, the two outer spans (each 20 mm long) each experience a shear force of magnitude F/2. Additionally, the middle span (totaling 40 mm) experiences a uniformly applied moment of Fa/2, where a is the shear span. Overall, then, a constant moment across a beam between two equivalent-stress bands near the loading noses is possible. This moment refers to the overall stress effect over a section while the contour relates to the local 3D stress condition [21,42]. As stated in [21], under sagging bending, one face (top) experiences longitudinal tension away from the contact area, while the other face (bottom) experiences longitudinal compression. Because reversing the sign of all stress components would not affect the equivalent stress, a longitudinal normal stress contour would differentiate between these two stresses [42]. Based on the solid core images in Figure 9, the overall curvature is present along with localized deformation near the noses. Overall, this roughly illustrates how the load applies. To compare using a point-wise field, we would need to measure displacement (or strain) at a known location on the same (or similar) configuration at the same load. In Section 5.7, increasing the nominal infill from 0 to 1 roughly only alters the analytical bending only stiffness by about 0.1%. In contrast, the measured initial Grid stiffness increases by 59.1% for PA-GF and 54.5% for PA-CF. As outlined in Equation (11), this minor change mainly relates to how separately applied faces contribute to longitudinal stiffness. According to Equation (15), bending, as well as other potential compliance factors, are listed together. Based on all of this, it makes sense to differentiate between the initial slope (Ke) and secant stiffness (F/δ) at either stated load as each relates to different aspects of the response.
5.10.3. Th Elastic Core Analysis
One central assumption is how the longitudinal and shear stiffness are related, since this is important for the short span beam. Using the typical Poisson ratio of ν = 0.30 listed in Table 4, applying the isotropic equation G = E/[2(1 + ν)] yields shear moduli of 4.85, 9.69 and 24.23 MPa for the solid, 40% and 20% TPU regions respectively. As will be explained, based on the assigned elastic property, both assigned moduli for the patterned region would double if the nominal infill were doubled regardless of how the walls are connected or oriented. However, according to the five printed structures discussed in Section 5.3, each structure exhibits distinct force versus displacement behavior. Each specimen is labeled with a Grid designation, indicating which specimen was used to calculate the equivalent core. This distinction also applies to the faces and their interaction. Based on experiments conducted in various orientations, Scapin and Peroni [15] determined the elastic properties using printed glass and carbon fiber nylon specimens. In this case, each face uses a flexural modulus as a scalar value. Since the faces are bonded, displacement must be continuous across the boundary between the core and face. Additionally, based on using rollers, a friction factor of 0.20 is used to indicate interaction at the roller points. Overall, because stress maps are used to indicate force transfer under continuous bonding, the data characterizes exposed faces based on the findings in Section 5.9. To evaluate the hidden connection, a traction (or separation) measurement between the face and core would be necessary. Bandinelli et al. [43] discussed in their compression models of printed carbon-fiber polyamide both direction-dependent hardening and yielding, demonstrating a further type of data that would be required in order to understand how a local stress value indicates yielding has begun. Two papers discuss how some aspects of this model could be evaluated independently using TPU. De la Rosa et al. [44] reported how changing the size and shape of printed lattice structures resulted in varying compression stiffness, which were then linked to potential defects in the printing process. Additionally, Diosdado De la Peña et al. [45] discussed fitting a hyperplastic equation for TPU while also comparing compression experiments to simulated Kelvin lattices broken down by each cell. While both of these are directly related to evaluating lattices under compression, based on this specific bending specimen, they are primarily related to being able to separate the effect of the material versus that of the structure itself using an effective equation, as outlined in Nampally et al. [26]. As discussed in Section 3.4, using a discretization of one contact and a nominal mesh size of 1.0 mm determines how the reported stresses are resolved. To fully compare using mesh refinement, it would be necessary to individually track the stress near each nose compared to an averaged roller displacement [42]. Based on the data available, the stress maps indicate where bending occurs and how the load is becoming concentrated. An actual numerical comparison comes from the crosshead response, showing that there is a greater displacement difference at maximum load.
6. Conclusions
The four-point bending response of PA-GF/TPU and PA-CF/TPU sandwich beams depended on the face material, nominal infill and core topology. Increasing the patterned infill from 20% to 40% increased the descriptive mean initial stiffness across the five topologies by 50.1% for PA-CF and 49.9% for PA-GF. The corresponding changes in maximum force, deformation and prepeak work varied by topology. These averages compare different designs and do not establish statistical significance or within-configuration repeatability. The observed dependence is consistent with the roles of geometry and load transfer in printed TPU lattices and sandwich structures [6,9,10].
PA-CF Grid at the 40% infill gave the highest patterned stiffness and maximum force, 173.2 N/mm and 837.0 N, respectively. PA-GF Line at 40% gave the highest patterned work to maximum force, 8.30 J, followed closely by PA-CF Gyroid at 8.21 J. For PA-GF Grid, raising the infill increased the maximum force by 50.8% while reducing the prepeak work by 45.9%, illustrating the need to distinguish load capacity from deformation capacity. Solid-core controls provided the highest absolute forces; the PA-CF control reached 1615.6 N and 18.80 J. Honeycomb showed little consistent benefit from the increased nominal infill. These findings support selecting the face material and core architecture jointly for the required combination of stiffness, load capacity and prepeak work [9,14,16].
The equivalent-core finite-element model underestimated the loading-point displacement by 45.28–88.03% and is not quantitatively validated for the measured response. The discrepancy shows that an infill-scaled elastic core alone is insufficient; it does not identify the separate contributions of the core architecture, nonlinear constitutive behavior, interface deformation and contact compliance. Predictive modeling requires independent constituent and interface characterization, topology-sensitive representation and convergence and validation studies [15,20,21,26].
The surface measurements distinguish rough last-printed top faces from smoother bed-contact bottom faces, but they do not determine the buried interface strength or the governing failure mechanism. Future repeated beam tests, local deformation and fracture observations, and dedicated interface measurements are needed in order to assess statistical robustness and the proposed mechanisms. Until then, the design implications remain specific to the stated geometry, processing records and crosshead-based response measures [32,33,34].
Supplementary Materials
The following supporting information can be downloaded at: https://www.mdpi.com/article/10.3390/polym18232968/s1, Video S1: Simulation of the 3D Printing process using Cura software.
Author Contributions
Conceptualization, A.A., H.A., A.M., H.M. and W.A.; methodology, A.A. and A.E.; software, A.M. and A.E.; validation, H.A., A.M., A.E. and W.A.; formal analysis, H.A. and A.M.; investigation, A.A., H.A., A.M. and A.E.; resources, W.A.; data curation, W.A.; writing—original draft preparation, A.A.; writing—review and editing, A.A., H.M. and W.A.; visualization, A.M.; supervision, H.M. and W.A.; project administration, H.M. and W.A.; funding acquisition, W.A. All authors have read and agreed to the published version of the manuscript.
Funding
This research is funded by (DEWA) Research and Development (R&D) Center and UAE University under fund 23N000.
Data Availability Statement
The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding author.
Conflicts of Interest
The authors declare no conflicts of interest.
References
- de Castro, B.D.; de Castro Magalhães, F.; Panzera, T.H.; Rubio, J.C.C. An Assessment of Fully Integrated Polymer Sandwich Structures Designed by Additive Manufacturing. J. Mater. Eng. Perform. 2021, 30, 5031–5038. [Google Scholar] [CrossRef] [Scilit]
- Forés-Garriga, A.; Gómez-Gras, G.; Pérez, M.A. Lightweight Hybrid Composite Sandwich Structures with Additively Manufactured Cellular Cores. Thin-Walled Struct. 2023, 191, 111082. [Google Scholar] [CrossRef] [Scilit]
- Zaharia, S.M.; Enescu, L.A.; Pop, M.A. Mechanical Performances of Lightweight Sandwich Structures Produced by Material Extrusion-Based Additive Manufacturing. Polymers 2020, 12, 1740. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Fareed, M.I.; Wu, C.-M.; Sood, M. Mechanical Characterization of a 3D Printed Lattice Core Sandwich Structure. Polym. Compos. 2025, 46, 3308–3320. [Google Scholar] [CrossRef] [Scilit]
- Tunay, M.; Bodur, M.F. Bending Behavior of 3D Printed Polymeric Sandwich Structures with Various Types of Core Topologies. Int. J. Automot. Sci. Technol. 2023, 7, 285–294. [Google Scholar] [CrossRef] [Scilit]
- Bonada, J.; Pastor, M.M.; Buj-Corral, I. Influence of Infill Pattern on the Elastic Mechanical Properties of Fused Filament Fabrication (FFF) Parts through Experimental Tests and Numerical Analyses. Materials 2021, 14, 5459. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Martín, M.J.; Auñón, J.A.; Martín, F. Influence of Infill Pattern on Mechanical Behavior of Polymeric and Composites Specimens Manufactured Using Fused Filament Fabrication Technology. Polymers 2021, 13, 2934. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Gohar, S.; Hussain, G.; Ali, A.; Ahmad, H. Mechanical Performance of Honeycomb Sandwich Structures Built by FDM Printing Technique. J. Thermoplast. Compos. Mater. 2023, 36, 182–200. [Google Scholar] [CrossRef] [Scilit]
- Yazdani Sarvestani, H.; Akbarzadeh, A.H.; Mirbolghasemi, A.; Hermenean, K. 3D Printed Meta-Sandwich Structures: Failure Mechanism, Energy Absorption and Multi-Hit Capability. Mater. Des. 2018, 160, 179–193. [Google Scholar] [CrossRef] [Scilit]
- Beloshenko, V.; Beygelzimer, Y.; Chishko, V.; Savchenko, B.; Sova, N.; Verbylo, D.; Voznyak, A.; Vozniak, I. Mechanical Properties of Flexible TPU-Based 3D Printed Lattice Structures: Role of Lattice Cut Direction and Architecture. Polymers 2021, 13, 2986. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Pelayo, F.; Blanco, D.; Fernández, P.; González, J.; Beltrán, N. Viscoelastic Behaviour of Flexible Thermoplastic Polyurethane Additively Manufactured Parts: Influence of Inner-Structure Design Factors. Polymers 2021, 13, 2365. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Ursini, C.; Collini, L. FDM Layering Deposition Effects on Mechanical Response of TPU Lattice Structures. Materials 2021, 14, 5645. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Ahmed, W.; Ahmed, S.; Alnajjar, F.; Zaneldin, E. Mechanical Performance of Three-Dimensional Printed Sandwich Composite with a High-Flexible Core. Proc. Inst. Mech. Eng. Part L J. Mater. Des. Appl. 2021, 235, 1382–1400. [Google Scholar] [CrossRef] [Scilit]
- Hashemi, M.; Hatami, O.; Tajbakhsh, M.R. Investigation of the Performance of the Structure and Energy Absorption in Sandwich Panels of PLA/TPU Manufactured by the FFF Technique. Proc. Inst. Mech. Eng. Part L J. Mater. Des. Appl. 2024, 238, 416–429. [Google Scholar] [CrossRef] [Scilit]
- Scapin, M.; Peroni, L. Numerical Simulations of Components Produced by Fused Deposition 3D Printing. Materials 2021, 14, 4625. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Junaedi, H.; Abd El-baky, M.A.; Awd Allah, M.M.; Sebaey, T.A. Mechanical Characteristics of Sandwich Structures with 3D-Printed Bio-Inspired Gyroid Structure Core and Carbon Fiber-Reinforced Polymer Laminate Face-Sheet. Polymers 2024, 16, 1698. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Bragagnolo, G.; Crocombe, A.D.; Ogin, S.L.; Mohagheghian, I.; Sordon, A.; Meeks, G.; Santoni, C. Investigation of Skin-Core Debonding in Sandwich Structures with Foam Cores. Mater. Des. 2020, 186, 108312. [Google Scholar] [CrossRef] [Scilit]
- Elhassan, A.; Alhefeiti, H.; Al Karbi, M.; Alseiari, F.; Alshehhi, R.; Ahmed, W.; Al-Marzouqi, A.H.; Al-Mazrouei, N. Enhanced Energy Absorption and Flexural Performance of 3D Printed Sandwich Panels Using Slicer-Generated Interlocking Interfaces. Polymers 2026, 18, 94. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- ASTM D6272-25; Standard Test Method for Flexural Properties of Unreinforced and Reinforced Plastics and Electrical Insulating Materials by Four-Point Bending. ASTM International: West Conshohocken, PA, USA, 2025. [Google Scholar] [CrossRef] [Scilit]
- ASTM D7250/D7250M-20; Standard Practice for Determining Sandwich Beam Flexural and Shear Stiffness. ASTM International: West Conshohocken, PA, USA, 2020. [Google Scholar] [CrossRef] [Scilit]
- Allen, H.G. Analysis and Design of Structural Sandwich Panels; Pergamon Press: Oxford, UK, 1969. [Google Scholar] [CrossRef] [Scilit]
- Gibson, L.J.; Ashby, M.F. The Mechanics of Three-Dimensional Cellular Materials. Proc. R. Soc. Lond. A 1982, 382, 43–59. [Google Scholar] [CrossRef] [Scilit]
- Jeong, E.; Calius, E.; Ramezani, M. Energy Dissipation in Nonlinearly Elastic Auxetic and Non-Auxetic Mechanical Metamaterials with Friction and Material Damping. Adv. Eng. Mater. 2025, 27, 2500558. [Google Scholar] [CrossRef] [Scilit]
- O’Connor, L. The Mechanical Behavior of Dual TPU/Nylon 3D Printed Parts. J. Appl. Polym. Sci. 2026, 143, e70504. [Google Scholar] [CrossRef] [Scilit]
- Wu, Y.; Wang, L.; Yi, Z.; Su, Q.; Qin, Y.; Cui, B. Energy Absorption and Rebound Behavior of 3D-Printed TPU Lattice Structures. Sci. Rep. 2026, 16, 9072. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Nampally, P.; Karttunen, A.T.; Reddy, J.N. Nonlinear Finite Element Analysis of Lattice Core Sandwich Beams. Eur. J. Mech. A Solids 2019, 74, 431–439. [Google Scholar] [CrossRef] [Scilit]
- FiberForce Italy. Nylforce Carbon Fiber Technical Data Sheet; Revision 2.1. 29 April 2019. Available online: https://www.fiberforce.it/wp-content/uploads/2019/07/TDS_NY-CARBON_REV-2.1.pdf (accessed on 30 October 2026).
- FiberForce Italy. Nylforce Glass Fiber Technical Data Sheet; Revision 2.0. 29 April 2019. Available online: https://www.fiberforce.it/wp-content/uploads/2019/07/TDS_NY-GLASS_REV-2.0.pdf (accessed on 30 October 2026).
- UltiMaker. UltiMaker TPU 95A Technical Data Sheet; Version 2.00. 29 April 2022. Available online: https://um-support-files.ultimaker.com/materials/2.85mm/tds/TPU-95A/Ultimaker-TPU95A-TDS-v5.00.pdf (accessed on 30 October 2026).
- ASTM C393/C393M-20; Standard Test Method for Core Shear Properties of Sandwich Constructions by Beam Flexure. ASTM International: West Conshohocken, PA, USA, 2020. [Google Scholar] [CrossRef] [Scilit]
- ASTM D7249/D7249M-20; Standard Test Method for Facesheet Properties of Sandwich Constructions by Long Beam Flexure. ASTM International: West Conshohocken, PA, USA, 2020. [Google Scholar] [CrossRef] [Scilit]
- Daniel, I.M.; Gdoutos, E.E.; Wang, K.-A. Failure of Composite Sandwich Beams. Adv. Compos. Lett. 2002, 11, 101–109. [Google Scholar] [CrossRef] [Scilit]
- Jafor, M.A.; Sayah, N.; Smith, D.E.; Stano, G.; Fleck, T.J. Systematic Evaluation of Adhesion and Fracture Toughness in Multi-Material Fused Deposition Material Extrusion. Materials 2024, 17, 3953. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Stano, G.; Al Islam Ovy, S.M.; Percoco, G.; Zhang, R.; Lu, H.; Tadesse, Y. Additive Manufacturing for Bioinspired Structures: Experimental Study to Improve the Multimaterial Adhesion Between Soft and Stiff Materials. 3D Print. Addit. Manuf. 2023, 10, 1080–1089. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Vaes, D.; Coppens, M.; Goderis, B.; Zoetelief, W.; Van Puyvelde, P. The Extent of Interlayer Bond Strength during Fused Filament Fabrication of Nylon Copolymers: An Interplay between Thermal History and Crystalline Morphology. Polymers 2021, 13, 2677. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Abas, M.; Al Awadh, M.; Habib, T.; Noor, S. Analyzing Surface Roughness Variations in Material Extrusion Additive Manufacturing of Nylon Carbon Fiber Composites. Polymers 2023, 15, 3633. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Pizzorni, M.; Parmiggiani, A.; Prato, M. Adhesive Bonding of a Mixed Short and Continuous Carbon-Fiber-Reinforced Nylon-6 Composite Made via Fused Filament Fabrication. Int. J. Adhes. Adhes. 2021, 107, 102856. [Google Scholar] [CrossRef] [Scilit]
- Slapnik, J.; Lorber, R.; Pulko, I.; Huskić, M.; Pušnik Črešnar, K. Overprinting of TPU onto PA6 Substrates: The Influences of the Interfacial Area, Surface Roughness and Processing Parameters on the Adhesion between Components. Polymers 2024, 16, 650. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- ASTM D4417-21; Standard Test Methods for Field Measurement of Surface Profile of Blast Cleaned Steel. ASTM International: West Conshohocken, PA, 2021. [Google Scholar] [CrossRef] [Scilit]
- ISO 25178-2:2021; Geometrical Product Specifications (GPS)—Surface Texture: Areal—Part 2: Terms, Definitions and Surface Texture Parameters. ISO: Geneva, Switzerland, 2021. Available online: https://www.iso.org/standard/74591.html (accessed on 30 October 2026).
- DeFelsko. PosiTector RTR 3D: Specifications and Instruction Manual. Available online: https://www.defelsko.com/positector-rtr-3d (accessed on 30 October 2026).
- ANSYS, Inc. Mechanical User’s Guide, Release 2026 R1., Sections 19.3.1.1 (Deformation); 19.3.1.2.1 (Equivalent (von Mises)) and 18.11 (Using Adaptive Convergence). Available online: https://ansyshelp.ansys.com/public/Views/Secured/corp/v261/en/wb_sim/ds_Home.html (accessed on 5 November 2026).
- Bandinelli, F.; Scapin, M.; Peroni, L. Effects of anisotropy and infill pattern on compression properties of 3D printed CFRP: Mechanical analysis and elasto-plastic finite element modelling. Rapid Prototyp. J. 2024, 30, 142–158. [Google Scholar] [CrossRef] [Scilit]
- de la Rosa, S.; Mayuet Ares, P.F.; Rodríguez-Parada, L. Design of Flexible TPU-Based Lattice Structures for 3D Printing: A Comparative Analysis of Open-Cell Versus Closed-Cell Topologies. Polymers 2025, 17, 1133. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Diosdado-De la Peña, J.A.; Dwyer, C.M.; Krzeminski, D.; MacDonald, E.; Saldaña-Robles, A.; Cortes, P.; Choo, K. Low Impact Velocity Modeling of 3D Printed Spatially Graded Elastomeric Lattices. Polymers 2022, 14, 4780. [Google Scholar] [CrossRef] [Scilit] [PubMed]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.