Abstract
Sn-based perovskites offer lower lead content but face a major challenge: Sn2+ oxidizes readily, which has led most research groups to use gloveboxes and chemical additives during processing. Here, we investigate whether precursor molarity alone can mitigate this oxidation problem in ambient air. MAPb0.75Sn0.25I3 solar cells with mesoporous N–i–P architecture were prepared from 1.0 M and 0.9 M solutions by spin-coating with ethyl acetate antisolvent, under standard lab conditions (28–34 °C, 30–45% RH). The characterization included SEM, XRD, XPS, profilometry, and J–V measurements. The 0.9 M concentration produced thinner films (275 nm vs. 474 nm), better Sn2+/Sn4+ ratios (16.5%/83.5% vs. 77.6%/22.4% by XPS), lower band gaps (1.51–1.52 vs. 1.55–1.56 eV), and larger grains. Device efficiency increased from 1.61 ± 0.68% (1.0 M) to 4.53 ± 0.91% (0.9 M), with the best cell reaching 5.91%—about 85% of our MAPbI3 control (6.96%). After one month of storage, 0.9 M cells retained 61% efficiency compared to 37% for 1.0 M devices. These findings demonstrate that a simple reduction in precursor molarity can substantially suppress Sn4+ formation during ambient fabrication, providing a practical route for laboratories without controlled atmospheres.
1. Introduction
Silicon photovoltaics is a mature technology that currently dominates the solar-cell market (≈95% of installed PV). However, silicon refining can require up to 100 kWh per kilogram. Meeting this energy demand commonly involves non-renewable feedstocks (e.g., oil, coal, and coke) to deliver both high-temperature heat and electricity. As a result, silicon manufacturing is associated with substantial CO2 emissions. In addition, wafer cleaning and texturing/etching employ hazardous chemicals and gases, including hydrofluoric and nitric acids, raising further environmental and safety concerns [1,2,3,4].
These drawbacks have motivated the development of alternative photovoltaic technologies with lower energy requirements. Metal halide perovskites are particularly attractive because they can be deposited from solution under conditions that do not require the expensive infrastructure needed for conventional silicon wafer-based routes. Among them, lead methylammonium triiodide (CH3NH3PbI3, MAPbI3) stands out because single-junction photovoltaic devices achieved a reported efficiency of 26.96% in 2025. Despite their performance, lead-containing perovskites remain controversial due to Pb toxicity, which has intensified efforts to partially replace Pb2+ while limiting losses in device efficiency. A widely explored approach is substituting a fraction of Pb2+ with Sn2+ to form mixed organic–inorganic perovskites of the type MAPb1−xSnxI3, thereby lowering lead content, typically at the cost of reduced stability and/or efficiency.
A key obstacle is that Sn2+ is readily oxidized to Sn4+ in the presence of oxygen (O2), even in the dark. This oxidation generates defect/trap states that promote non-radiative recombination and can markedly deteriorate photovoltaic performance. For this reason, both precursor preparation and film deposition are often performed in inert-atmosphere gloveboxes. Importantly, previous successful attempts have been made to control the oxidation state of tin in such perovskite films; notably, vacuum-based co-evaporation techniques have demonstrated the ability to stabilize tin in a single oxidation state (Sn2+), effectively suppressing the formation of detrimental Sn4+ species [5].
In parallel, various additives have been introduced to suppress Sn oxidation, including hypophosphorous acid (H3PO2), hypophosphites (NaH2PO2, NH4H2PO2), ascorbic acid (vitamin C), tin(II) fluoride (SnF2), tin(II) oxalate (SnC2O4), and tetra-n-butylammonium fluoride (F-TBA), among others. Stability is further challenged by the hygroscopic and volatile nature of the methylammonium (MA+) cation, which can decompose under moderate heat and humidity, whereas formamidinium (FA) and cesium (Cs) based compositions are generally more robust. However, the manipulation of additives and the requirement for inert atmosphere processing increase complexity and cost, particularly for precursor preparation and perovskite nanofilm fabrication [6,7,8,9,10,11,12,13,14,15,16,17,18,19,20,21,22,23].
Alternative strategies have recently been explored to mitigate Sn2+ oxidation in tin-based perovskites. For example, mechanochemical pretreatment of precursor materials has been reported to improve oxygen tolerance and enhance device performance in Sn-based perovskite solar cells [24], highlighting the importance of precursor chemistry and processing conditions for stabilizing the Sn2+ oxidation state [25].
Here, we intentionally evaluate a simplified processing route: standard-atmosphere fabrication without glovebox and without stabilizing additives, using the perovskite precursor molarity as the main control parameter. We compare 1.0 M and 0.9 M MAPb0.75Sn0.25I3 precursor solutions as the active layer in a mesoporous N–i–P architecture. A Sn substitution level of x = 0.25 is selected as a practical compromise between reducing lead content and limiting tin oxidation [26,27].
We correlate microstructure (SEM and grain statistics), thickness/roughness, optical response, crystal structure, Sn2+/Sn4+ oxidation states, and device performance (J–V and EQE). The aim is to test whether a small concentration adjustment can reduce oxidation-related losses and improve charge collection under fully ambient processing.
2. Materials and Methods
2.1. Cell Architecture and Fabrication
Solar cells were fabricated using a mesoporous N–i–P architecture, in which N represents the Electron Transport Layer (ETL), i the perovskite active layer on the mesoporous scaffold, and P the Hole Transport Layer (HTL), as shown in Figure 1. The mesoporous structure increases the ETL/perovskite interfacial area and enhances charge extraction and transport, leading to improved photovoltaic performance relative to planar architectures [28,29].
Figure 1.
Direct or mesoporous N–i–P architecture.
2.2. Solar Device Fabrication
The materials and deposition protocols for each layer of the MAPbI3 perovskite solar cells follow the procedures reported by Quiñonez et al. (maximum efficiency 13.75%) and Arias et al. (maximum efficiency 18.04%, achieved by adding 4-tert-butylpyridine (tBP) to the antisolvent) [30,31].
- Substrate: Fluorine-doped tin oxide (FTO) coated glass (TEC 15, DYESOL, Queanbeyan, Australia).
- ETL: Compact titanium dioxide (c-TiO2) using a solution of isopropanol (20 mL), titanium isopropoxide (C12H28O4Ti, 97%, Aldrich, St. Louis, MO, USA, 1.2 mL), and hydrochloric acid (37%, Fermont ACS, Monterrey, Mexico, 400 µL). 400 µL are deposited via spin-coating at 3000 RPM for 30 s and subjected to thermal treatment at 450 °C for 30 min.
- Mesoporous Layer: Mesoporous titanium dioxide (m-TiO2) is prepared by diluting TiO2 paste (30NRD, Great Cell Solar, Queanbeyan, Australia) in ethanol (99.9%, Fermont ACS, Monterrey, Mexico) at a 1:5 weight ratio. 100 µL is deposited at 4000 RPM for 30 s and subjected to thermal treatment at 500 °C for 30 min.
- Perovskite Precursor Solution: For MAPbI3, the solution was prepared by mixing lead iodide (PbI2, 99.999%, Lumtec, Hsinchu, Taiwan, 461 mg), methylammonium iodide (MAI, 99.5%, Lumtec, Hsinchu, Taiwan, 144 mg), and dimethyl sulfoxide (DMSO, 99.9%, Aldrich, 78 mg) in a 1:1:1 molar ratio, dissolved in 1.0 mL of dimethylformamide (DMF, 99.8%, Aldrich). For MAPb0.75Sn0.25I3, it was prepared by mixing MAI, PbI2, tin(II) chloride (SnCl2, 99% Fagalab brand, Mocorito, México), and DMSO in a 1.25:0.75:0.25:1 molar ratio. To obtain the 0.9 M solution, the amounts of MAI, PbI2, and SnCl2 were reduced by 10% (Table 1). 70 µL are deposited at 5000 RPM for 20 s; after 7 s, 220 µL of ethyl acetate (EA, 99.8% anhydrous, Sigma-Aldrich, St. Louis, MO, USA) are deposited as a selective antisolvent. Upon completion of the spin-coating, a thermal treatment of 100 °C for 5 min is applied (Figure 2).
- HTL: The HTL was prepared by dissolving Spiro-OMeTAD (99%, Aldrich, St. Louis, USA, 60 mg) in chlorobenzene (99.9%, Aldrich, 750 μL), with the addition of Li-TFSI (99.95%, Aldrich, St. Louis, USA, 13.4 μL of a 1.81 M solution in acetonitrile). 30 µL are deposited via spin-coating at 4000 RPM for 30 s.
- Finally, a gold (Au) contact was thermally evaporated under high vacuum conditions (≈2.6 × 10−5 Torr). The preparation of the perovskite precursor solution and the synthesis of the nanofilms were carried out in a standard atmosphere, with temperatures ranging from 28 to 34 °C and relative humidity (RH) between 30 and 45%, with the exception of the HTL, which was processed in a glovebox due to the sensitivity of its compounds.
Table 1.
Key quantities for MAPb0.75Sn0.25I3 precursor solutions.
Figure 2.
Deposition of precursor solution (a), phase change time and deposition of selective antisolvent (b), and heat treatment (c).
2.3. Characterization
To determine the thickness and surface roughness of the mixed perovskite nanofilms, an AMBios XP-200 stylus profilometer (Ambios Technology Inc., Santa Cruz, CA, USA) was used. Transmittance and reflectance spectra were obtained using a Shimadzu UV-1800 UV-Vis spectrophotometer (Shimadzu Corporation, Kyoto, Japan). To verify the formation of the mixed perovskite structure, an X-ray diffraction (XRD) study was conducted using a Bruker D8 Advance diffractometer (Bruker AXS, Karlsruhe, Germany). The surface morphology of the films was evaluated via scanning electron microscopy (SEM) with a Hitachi S-5500 SEM (Hitachi High-Technologies Corp, Tokyo, Japan). X-ray photoelectron spectroscopy (XPS) was employed to determine the surface chemical composition and the relative ratio of Pb and Sn, using a Perkin-Elmer XPS 5100 system (PerkinElmer Inc., Waltham, MA, USA). To evaluate the efficiency, fill factor (FF), open-circuit voltage (Voc), short-circuit current density (Jsc), and other electrical characteristics of the cells, an ORIEL LCS-100 solar simulator (Oriel Instruments a Newport Corp. brand, Stratford, CT, USA) was used. Additionally, the external quantum efficiency was obtained with a Perkin-Elmer Lambda EQE meter (PerkinElmer Inc., Waltham, MA, USA).
2.4. Data Processing and Graphing
Thickness and roughness parameters (Ra) were obtained from the profilometry files through numerical signal analysis. This value is defined as z(x), representing the height deviations from the mean line over an evaluation length L [32]. In profilometry practice, n discrete samples z(x) are used, which are equally spaced, applying Equation (1):
Since the mixed Pb-Sn perovskite nanofilms are semitransparent and specular, the absorption coefficient α(λ) was calculated using the incoherent multiple reflections model for an absorbing film of thickness d derived from transmittance (T) and reflectance (R), according to Equation (2) [29]:
This approach is suitable for semitransparent films, as it avoids the restrictive assumptions of the classic Kubelka–Munk model. Several studies have employed this approximation for the optical analysis of hybrid perovskites, as it is more accurate under common experimental conditions. From α(hν), Tauc plots for direct allowed transitions were constructed by plotting (αhν)2 versus hν. The bandgap value was obtained through linear extrapolation of the quasi-linear region to the energy axis [33]. To identify the Sn4+ content level, X-ray Photoelectron Spectroscopy (XPS) was used. The Sn region was processed by applying Gaussian smoothing to stabilize detection without modifying the original intensity, followed by a deconvolution algorithm based on pseudo-Voigt profiles. This method combines Lorentzian and Gaussian contributions along with physicochemical constraints reported for Sn-perovskite analysis, as shown in Equation (3) [34,35,36].
The processing and graphing of data obtained from the characterization devices, as well as the calculations, were performed using custom-made programs developed in the Python 3.10.11 language using a programming methodology assisted by iteration with Artificial Intelligence (AI) [37].
3. Results
Figure 3 shows representative samples of MAPbI3 control solar cells and MAPb0.75Sn0.25I3 at 1.0 M and 0.9 M, fabricated without an inert atmosphere or additives added to the precursor solution. These confirm the reproducible acquisition of full cells with a well-defined contact pattern and a continuous surface at a macroscopic scale, which were used for the electrical and optical characterizations reported in the following sections.
Figure 3.
Representative photographs of fabricated perovskite solar cells: (a) MAPbI3 control device, (b) MAPb0.75Sn0.25I3 fabricated with 1.0 M precursor molarity, and (c) MAPb0.75Sn0.25I3 fabricated with 0.9 M precursor molarity.
3.1. Profilometry
Reducing the concentration from 1.0 M to 0.9 M resulted in a decrease in the thickness of the active perovskite layer from 474 nm to 275 nm (≈42%), as shown in Figure 4. This is consistent with the use of identical spin-coating parameters while applying a more dilute solution, in which reduced solute concentration lowers viscosity and facilitates fluid flow during spinning. Both concentrations produced films with a roughness below 10 nm, consistent with their mirror-like appearance. However, inspection of the Ra profiles (Table 2) reveals that the 0.9 M sample exhibits a more stable, lower-noise curve (Figure 5), suggesting more uniform crystallization, fewer irregular domains, and improved topographic homogeneity.
Figure 4.
Thickness measurement by profilometry: 1.0 M (a) and 0.9 M (b).
Table 2.
Surface roughness results of the samples MAPb0.75Sn0.25I3 at 1.0 M and 0.9 M.
Figure 5.
R curve: 1.0 M (a) and 0.9 M (b).
3.2. SEM
In all cases, a continuous polycrystalline film is observed, featuring grains with polygonal morphology and clearly defined grain boundaries (Figure 6). MAPbI3 exhibits the largest grains and a relatively more uniform distribution. In contrast, MAPb0.75Sn0.25I3 at 1.0 M shows smaller grains and a broader size distribution, implying a higher grain boundary density per unit area, which may introduce additional recombination sites and impede intergranular charge transport. Reducing the molarity to 0.9 M increases grain size and narrows the distribution, consistent with more homogeneous crystallization. This trend is in agreement with the profilometry results, where the 0.9 M film displayed a more stable, lower-noise Ra profile, indicative of greater topographic uniformity.
Figure 6.
Surface SEM micrographs: MAPbI3 (a), MAPb0.75Sn0.25I3 at 1.0 M (b) and 0.9 M (c).
The statistical quantification of the length of 60 grain samples (n) is summarized in Table 3 and in the histograms in Figure 7.
Table 3.
Statistical report of grain length of MAPbI3: (a), and MAPb0.75Sn0.25I3: 1.0 M (b) and 0.9 M (c).
Figure 7.
Histograms of the characteristic grain length for: MAPbI3 (a), MAPb0.75Sn0.25I3 at 1.0 M (b) and 0.9 M (c).
Taken together, SEM and statistical analysis confirm that 1.0 M produces a finer and more dispersed microstructure, while 0.9 M favors a more uniform morphology and relatively larger grains.
3.3. Bandgap
In both concentrations, a reduction in the bandgap was observed compared to the control nanofilms (MAPbI3), which was 1.61–1.62 eV. At 1.0 M, it decreased to 1.55–1.56 eV, and decreased further in the 0.9 M samples, ranging from 1.51 to 1.52 eV (Figure 8). This can be attributed to a lower oxidation of Sn2+ to Sn4+, likely resulting from improved precursor distribution during film formation, which promotes more complete crystallization of the mixed perovskite phase.
Figure 8.
Tauc curves to obtain the optical bandgap: MAPbI3 (1.61–1.62 eV) (a), MAPb0.75Sn0.25I3 (1.55–1.56 eV) at 1.0 M (b), and (1.51–1.52 eV) at 0.9 M (c). Each colored line corresponds to an individual sample from the same batch.
3.4. XRD
The presence of peaks at 2θ ≈ 14° (110), 28° (220), and 31–32° (310) in Figure 9 for both concentrations indicates the formation of the perovskite structure [38]. Furthermore, the slight shift in these peaks toward higher 2θ angles indicates the incorporation of Sn2+; due to its smaller ionic radius compared to Pb2+, it tends to contract the crystal lattice. The absence of the PbI2 peak at 2θ ≈ 12.7° is likely attributable to the reduced quantity of PbI2, which enables a more complete conversion of the precursors into the perovskite phase.
Figure 9.
Diffractogram of MAPbI3 (a), MAPb0.75Sn0.25I3 at 1.0 M (b), and at 0.9 M (c).
3.5. XPS
XPS analysis reveals a critical finding: the relative proportion of tin oxidation differs markedly between concentrations. At 1.0 M, the Sn2+/Sn4+ ratio is 16.5%/83.5%, whereas at 0.9 M, the ratio shifts favorably to 77.6%/22.4% (Figure 10). The pseudo-Voigt fitting parameters used for the Sn 3d deconvolution, including FWHM, Lorentzian fraction (η), spin–orbit splitting, and integrated areas, are summarized in Table 4. This suggests that at higher molar concentrations, a larger fraction of Sn2+ oxidizes during spin-coating, prior to the application of the selective antisolvent [39,40].
Figure 10.
Sn4+ and Sn2+ ratio in MAPb0.75Sn0.25I3 films with concentrations at: 1.0 M (a) and 0.9 M (b).
Table 4.
XPS Sn 3d pseudo-Voigt fitting parameters for MAPb0.75Sn0.25I3 films at 1.0 M and 0.9 M. Pseudo-Voigt model with shared FWHM.
3.6. J–V Curves
A total of 15 devices per condition, MAPbI3 control and MAPb0.75Sn0.25I3 at 1.0 M and 0.9 M, were analyzed in forward scan under AM1.5G illumination (100 mW cm−2) over an active area of 0.104 cm2, in order to evaluate process reproducibility (Table 5).
Table 5.
Photovoltaic Parameters of Perovskite Cells (n = 15).
Figure 11 shows the J–V curves of the champion cells, which achieved the highest efficiency for each condition. The box plot in Figure 12 provides a visualization of the efficiency distribution. The 1.0 M cells exhibit the lowest average efficiency (1.61%), indicating consistent reproducibility within a low-performance regime. In contrast, the 0.9 M cells show an average efficiency of 4.53%, which is consistently superior to the 1.0 M group. The control group presents the highest average efficiency (5.66%).
Figure 11.
J–V curves of champion cells with the highest efficiency: MAPbI3 control (6.96%) (a), MAPb0.75Sn0.25I3 at 1.0 M (2.84%) (b), and at 0.9 M (5.91%) (c).
Figure 12.
Comparative box plot of efficiencies: MAPbI3, MAPb0.75Sn0.25I3 at 1.0 M and 0.9 M.
The open-circuit voltage (Voc) remains relatively stable across the three groups (0.85–0.91 V on average), suggesting that Sn2+ incorporation and its oxidation primarily affect charge generation and transport processes rather than the interface energetics that determine Voc. The fill factor (FF) shows a trend in which the 1.0 M cells show the highest average FF (59.3 ± 7.27%), reaching up to 67.5% in the champion cell, followed by 0.9 M (48.7 ± 13.8%) and finally the control cells (37.6 ± 5.84%). This elevated FF in the 1.0 M group, despite its low efficiency, is explained by the dramatic reduction in average short-circuit current density Jsc (0.344 ± 0.190 mA/cm2), resulting in J–V curves with less influence from series resistance under low current generation conditions. The loss of Jsc is the dominant factor in the efficiency degradation of the 1.0 M group. The recovery of average Jsc in the 0.9 M group (3.43 ± 3.60 mA/cm2) correlates with the reduction in Sn4+ to 22.4%, which minimizes recombination centers. Additionally, the reduced thickness favors efficient charge extraction, and the improved microstructure, featuring more uniform grains and lower grain boundary density, further supports this recovery. The control group exhibits the highest average Jsc (10.8 ± 7.88 mA/cm2), consistent with the absence of Sn oxidation. These findings confirm that lowering the molarity from 1.0 to 0.9 M is an effective strategy to mitigate Sn2+ oxidation under ambient processing, achieving average efficiencies 2.8 times higher (4.53% at 0.9 M vs. 1.61% at 1.0 M) and champion cells that reach ≈ 85% of the control performance without additives or an inert atmosphere. The maximum efficiencies obtained were: 1.0 M reached 2.84% (≈41% relative to the 6.96% control), while 0.9 M more than doubled that with 5.91% (≈85% of the control).
3.7. EQE
The champion cells’ EQE spectra (Figure 13) reveal substantial differences in photon-to-electron conversion efficiency across the three samples. The control cell exhibits a broad response with a peak EQE of 99.2% and a Jsc of 15.241 mA/cm2, consistent with its superior J–V performance. The 0.9 M cell achieves a comparable peak EQE of 97.6% and an integrated Jsc of 14.307 mA/cm2, confirming that reducing precursor molarity effectively preserves charge extraction despite ambient processing conditions. In contrast, the 1.0 M cell shows a markedly lower peak EQE of 29.9% and an integrated Jsc of only 4.001 mA/cm2, which is consistent with the increased Sn4+ content introducing recombination centers that limit photocurrent generation (Table 6). The integrated Jsc values are in good agreement with those obtained from J–V measurements (Table 5), validating the measurement consistency.
Figure 13.
Quantum efficiencies of champion cells.
Table 6.
EQE-Integrated and J–V Short-Circuit Current Densities for Champion Cells.
3.8. Temporal Stability
Figure 14 shows the evolution of the photovoltaic parameters obtained under identical illumination and area settings, for the champion cells stored in the dark at 28–34 °C and 30–45% RH. The 1.0 M cell showed an efficiency decrease from 2.84% to 1.66% after one week, reaching 1.06% after one month (final retention ≈ 37%). In contrast, the 0.9 M cell degraded from 5.91% to 4.8% and finally to 3.61% over the same periods (final retention ≈ 61%). The 0.9 M cell maintains an absolute efficiency 3.4 times higher after one month (3.61% vs. 1.06%), verifying that the initial advantage derived from the lower Sn4+ content is preserved over time. This loss suggests that the dominant degradation mechanisms include: the progressive oxidation of residual Sn2+ to Sn4+, which introduces deep trap states, and the potential partial loss of MA+, which induces the gradual decomposition of the perovskite structure [14,15,18,20]. These results demonstrate that performance degradation over time is inevitable under ambient conditions without encapsulation; nevertheless, the strategy of reducing the precursor molarity provides a sustained advantage in photovoltaic performance over time.
Figure 14.
Efficiencies of the highest performing cells measured after one week and one month of storage in darkness (28–34 °C, 30–45% RH) at 1.0 M (a) and 0.9 M (b).
4. Conclusions
This work demonstrates that a small adjustment in precursor molarity, from 1.0 M to 0.9 M, for mixed Pb–Sn perovskites processed in ambient atmosphere:
- Favorably Modifies Morphology: Reduces thickness by 42% (474 nm → 275 nm) and increases grain size and uniformity, thereby decreasing recombination sites.
- Drastically Mitigates Oxidation: Reduces the Sn4+ fraction from 83.5% to 22.4%, as confirmed by XPS.
- Performance and Stability: It improves average efficiency (1.61% → 4.53%). The champion cell achieves approximately 85% of the performance of the MAPbI3 control (5.91% vs. 6.96%) and increases efficiency retention after one month (61% vs. 37%).
- Validates Charge Extraction via EQE: The 0.9 M champion cell achieves a peak EQE of 97.6% and an integrated Jsc of ≈14.31 mA/cm2, closely matching the control (99.2%, 15.24 mA/cm2), while the 1.0 M cell reaches only 29.9%, confirming that reduced Sn4+ content directly translates into improved photon-to-electron conversion.
These findings demonstrate that controlling precursor molarity alone can significantly mitigate Sn2+ oxidation during ambient processing, partially compensating for the absence of glovebox infrastructure and chemical additives. Achieving approximately 85% of the performance of the MAPbI3 control device without a glovebox positions this strategy as a promising route toward low-cost fabrication, particularly for laboratories with limited access to controlled-atmosphere facilities.
This approach also provides a systematic framework for exploring the relationship between precursor concentration and device efficiency in order to identify an optimal molarity. Once established, this strategy could be combined with complementary approaches, such as incorporating additives (e.g., KI or ascorbic acid), to further improve stability and efficiency. Future work will focus on enhancing performance under ambient conditions, increasing Sn content, implementing encapsulation, and advancing toward scalable industrial fabrication.
Author Contributions
Conceptualization, R.G.-G., J.E.E.-Q. and C.F.A.-R.; Methodology: J.E.E.-Q., O.E.C.-L., R.R.-S. and F.E.C.-G.; writing—review and editing: R.G.-G. and J.E.E.-Q.; Validation: R.G.-G.; Formal analysis: R.R.C., F.R.-G. and J.E.E.-Q.; data curation, J.E.E.-Q.; software, J.E.E.-Q.; Investigation: J.E.E.-Q., R.G.-G. and C.F.A.-R. All authors have read and agreed to the published version of the manuscript.
Funding
This research received no external funding.
Data Availability Statement
The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding authors.
Acknowledgments
The authors gratefully acknowledge the UNAM projects and the Secretaría de Ciencia, Humanidades, Tecnología e Innovación (SECIHTI) for financial support. The authors also acknowledge the use of the laboratory facilities kindly provided by Hailin Zhao Hu.
Conflicts of Interest
The authors declare no conflicts of interest. The funders had no role in the design of the study; in the collection, analyses, or interpretation of data; in the writing of the manuscript; or in the decision to publish the results.
Abbreviations
The following abbreviations are used in this manuscript:
| N–i–P | n-type/intrinsic/p-type (architecture) |
| ETL | Electron Transport Layer |
| HTL | Hole Transport Layer |
| FTO | Fluorine-doped Tin Oxide |
| RH | Relative Humidity |
| SEM | Scanning Electron Microscopy |
| XRD | X-Ray Diffraction |
| XPS | X-ray Photoelectron Spectroscopy |
| J–V | Current Density-Voltage |
| EQE | External Quantum Efficiency |
| FF | Fill Factor |
| Voc | Open-circuit Voltage |
| Jsc | Short-circuit Current Density |
| Ra | Average Roughness |
| PV | Photovoltaic |
| CV | Coefficient of Variation |
| AI | Artificial Intelligence |
| AM1.5G | Air Mass 1.5 Global (standard solar spectrum) |
References
- Stefani, B.V.; Kim, M.; Zhang, Y.; Hallam, B.; Green, M.A.; Bonilla, R.S.; Fell, C.; Wilson, G.J.; Wright, M. Historical market projections and the future of silicon solar cells. Joule 2023, 7, 2435–2451. [Google Scholar] [CrossRef] [Scilit]
- PV Tech. How Crystalline Silicon Will Dominate Global Energy by 2050. Available online: https://www.pv-tech.org/solars-ascendancy-how-crystalline-silicon-will-dominate-global-energy-by-2050/ (accessed on 6 May 2025).
- Philipps, S.; Warmuth, W. Photovoltaics Report; Fraunhofer Institute for Solar Energy Systems (ISE): Freiburg, Germany, 2025; Available online: https://www.ise.fraunhofer.de/content/dam/ise/de/documents/publications/studies/Photovoltaics-Report.pdf (accessed on 29 May 2025).
- Elkem, A.S.A. Elkem Signs New Agreement for Norwegian Biocarbon. Available online: https://www.elkem.com/es/media/news/article/?itemid=AA806B0C8B0E7A94 (accessed on 30 May 2025).
- Singh, A.; Hieulle, J.; Machado, J.F.; Gharabeiki, S.; Zuo, W.; Farooq, M.U.; Phirke, H.; Saliba, M.; Redinger, A. Coevaporation stabilizes tin-based perovskites in a single Sn-oxidation state. Nano Lett. 2022, 22, 7112–7118. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Kim, S.; Kim, S.H.; Hwang, H.U.; Kim, J.; Kim, J.W.; Kwak, I.C.; Kang, B.; Lee, S.; Jo, S.B.; Ryu, D.Y.; et al. Revisiting the role of oxidation in stable and high-performance lead-free perovskite-IGZO junction field-effect transistors. Nat. Commun. 2025, 16, 7427. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Tang, W.; Liu, T.; Zhang, M.; Yuan, F.; Zhou, K.; Lai, R.; Lian, Y.; Xing, S.; Xiong, W.; Zhang, M.; et al. The roles of metal oxidation states in perovskite semiconductors. Matter 2023, 6, 3782–3802. [Google Scholar] [CrossRef] [Scilit]
- National Renewable Energy Laboratory. Best Research-Cell Efficiency Chart. Available online: https://www.nrel.gov/pv/cell-efficiency (accessed on 2 November 2025).
- Leijtens, T.; Prasanna, R.; Gold-Parker, A.; Toney, M.F.; McGehee, M.D. Mechanism of tin oxidation and stabilization by lead substitution in tin halide perovskites. ACS Energy Lett. 2017, 2, 2159–2165. [Google Scholar] [CrossRef] [Scilit]
- Ayaydah, W.; Raddad, E.; Hawash, Z. Sn-Based Perovskite Solar Cells towards High Stability and Performance. Micromachines 2023, 14, 806. [Google Scholar] [CrossRef] [Scilit]
- Chepngetich, N.; Mumbi, G.M.; Richard, K.K.; Yegon, G.K.; Chepkwony, S.C.; Rono, C.; Sanni, D.; Bello, A.; Ntsoenzok, E. Recent trends on the application of phytochemical-based compounds as additives in the fabrication of perovskite solar cells. Energy Adv. 2024, 3, 741–764. [Google Scholar] [CrossRef] [Scilit]
- Kurisinkal Pious, J.; Zwirner, Y.; Lai, H.; Olthof, S.; Jeangros, Q.; Gilshtein, E.; Kothandaraman, R.K.; Artuk, K.; Wechsler, P.; Chen, C.; et al. Revealing the role of tin fluoride additive in narrow bandgap Pb-Sn perovskites for highly efficient flexible all-perovskite tandem cells. ACS Appl. Mater. Interfaces 2023, 15, 10150–10157. [Google Scholar] [CrossRef] [Scilit]
- Yang, F.; Zhu, K. Advances in Mixed Tin-Lead Narrow-Bandgap Perovskites for Single-Junction and All-Perovskite Tandem Solar Cells. Adv. Mater. 2024, 36, 2314341. [Google Scholar] [CrossRef] [Scilit]
- Saidaminov, M.I.; Spanopoulos, I.; Abed, J.; Ke, W.; Wicks, J.; Kanatzidis, M.G.; Sargent, E.H. Conventional solvent oxidizes Sn(II) in perovskite inks. ACS Energy Lett. 2020, 5, 1153–1155. [Google Scholar] [CrossRef] [Scilit]
- Huang, Y.; Zhang, W.; Xiong, Y.; Yi, Z.; Huang, C.; Jiang, Q.; Basit, A.; Shen, G.; Luo, Y.; Li, X.; et al. Recent Advancements in Ambient-Air Fabrication of Perovskite Solar Cells. Exploration 2025, 5, e20240121. [Google Scholar] [CrossRef] [Scilit]
- Zhang, Z.; Huang, Y.; Jin, J.; Jiang, Y.; Xu, Y.; Zhu, J.; Zhao, D. Mechanistic understanding of oxidation of tin-based perovskite solar cells and mitigation strategies. Angew. Chem. Int. Ed. 2023, 62, e202308093. [Google Scholar] [CrossRef] [Scilit]
- Jing, C.; Lin, Z.; Wu, Y.; Ouyang, X. Air-Processed Perovskite Solar Cells: Challenges, Progress, and Industrial Strategies. Small 2025, 21, 2504448. [Google Scholar] [CrossRef] [Scilit]
- Shah, S.A.A.; Sayyad, M.H.; Khan, K.; Guo, K.; Shen, F.; Sun, J.; Tareen, A.K.; Gong, Y.; Guo, Z. Progress towards high-efficiency and stable tin-based perovskite solar cells. Energies 2020, 13, 5092. [Google Scholar] [CrossRef] [Scilit]
- Krishna, B.G.; Ghosh, D.S.; Tiwari, S. Progress in ambient air-processed perovskite solar cells: Insights into processing techniques and stability assessment. Sol. Energy 2021, 224, 1369–1395. [Google Scholar] [CrossRef] [Scilit]
- Jokar, E.; Chien, C.H.; Fathi, A.; Rameez, M.; Chang, Y.H.; Diau, E.W.G. Slow surface passivation and crystal relaxation with additives to improve device performance and durability for tin-based perovskite solar cells. Energy Environ. Sci. 2019, 12, 2353–2362. [Google Scholar] [CrossRef] [Scilit]
- Chen, L.; Fu, S.; Li, Y.; Sun, N.; Yan, Y.; Song, Z. On the Durability of Tin-Containing Perovskite Solar Cells. Adv. Sci. 2024, 11, e2304811. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Pascual, J.; Nasti, G.; Aldamasy, M.H.; Smith, J.A.; Flatken, M.; Phung, N.; Di Girolamo, D.; Turren-Cruz, S.-H.; Li, M.; Dallmann, A.; et al. Origin of Sn(II) oxidation in tin halide perovskites. Mater. Adv. 2020, 1, 1066–1070. [Google Scholar] [CrossRef] [Scilit]
- Li, F.; Deng, X.; Qi, F.; Li, Z.; Liu, D.; Shen, D.; Qin, M.; Wu, S.; Lin, F.; Jang, S.-H.; et al. Regulating surface termination for efficient inverted perovskite solar cells with greater than 23% efficiency. J. Am. Chem. Soc. 2020, 142, 20134–20142. [Google Scholar] [CrossRef] [Scilit]
- Liu, T.; Cho, S.; Nishikubo, R.; Pylnev, M.; Ishiwari, F.; Wakamiya, A.; Saeki, A. Mechanochemical pretreatment of tin iodide perovskite precursors: Effects of grinding temperature and time on solar cell performance. EES Sol. 2025, 1, 78–88. [Google Scholar] [CrossRef] [Scilit]
- Lee, H.; Kang, S.B.; Lee, S.; Zhu, K.; Kim, D.H. Progress and Outlook of Sn–Pb Mixed Perovskite Solar Cells. Nano Converg. 2023, 10, 27. [Google Scholar] [CrossRef] [Scilit]
- Eperon, G.E.; Leijtens, T.; Bush, K.A.; Prasanna, R.; Green, T.; Wang, J.T.-W.; McMeekin, D.P.; Volonakis, G.; Milot, R.L.; May, R.; et al. Perovskite-perovskite tandem photovoltaics with optimized band gaps. Science 2016, 354, 861–865. [Google Scholar] [CrossRef] [Scilit]
- Alkhammash, A.A.; Alkhammash, H.I.; Alkhammash, E.H.; Alkhammash, M.A. Optimization of tin-doped hybrid perovskite solar cells. Open J. Appl. Sci. 2024, 14, 687–706. [Google Scholar] [CrossRef]
- Ašmontas, S.; Čerškus, A.; Gradauskas, J.; Grigucevičienė, A.; Juškėnas, R.; Leinartas, K.; Lučun, A.; Petrauskas, K.; Selskis, A.; Staišiūnas, L.; et al. Photoelectric Properties of Planar and Mesoporous Structured Perovskite Solar Cells. Materials 2022, 15, 4300. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Vasilopoulou, M.; Soultati, A.; Filippatos, P.-P.; Mohd Yusoff, A.R.B.; Nazeeruddin, M.K.; Palilis, L.C. Charge transport materials for mesoscopic perovskite solar cells. J. Mater. Chem. C 2022, 10, 11063–11104. [Google Scholar] [CrossRef] [Scilit]
- Quiñonez, J.E.; García Gutiérrez, R.; Arias-Ramos, C.F.; Cancino-Gordillo, F.E.; Segura, R.R. Analysis of the Effect of Ethyl Acetate on the Crystallization of MAPbI3 and its Impact on the Efficiency of the Perovskite Solar Cells. In Proceedings of the 10th Virtual International Conference on Science, Technology and Management in Energy (eNergetics 2024), Virtual, 20 January 2025. [Google Scholar] [CrossRef]
- Arias-Ramos, C.F.; Kumar, Y.; Abrego-Martínez, P.G.; Hu, H. Efficient and stable hybrid perovskite prepared at 60% relative humidity with a hydrophobic additive in antisolvent. Sol. Energy Mater. Sol. Cells 2020, 215, 110625. [Google Scholar] [CrossRef] [Scilit]
- Evident. Surface Roughness Measurement: Parameters. Available online: https://evidentscientific.com/es/applications/metrology/surface-roughness-measurement-portal/parameters#007 (accessed on 11 September 2025).
- Klein, J.; Kampermann, L.; Mockenhaupt, B.; Behrens, M.; Strunk, J.; Bacher, G. Limitations of the Tauc Plot Method. Adv. Funct. Mater. 2023, 33, 2304523. [Google Scholar] [CrossRef] [Scilit]
- Azaden, A.; Bhatt, P.; Liu, Y.; Wei, J.; Haque, S.; Palgrave, R. Towards reliable oxidation state analysis of tin halide perovskites with XPS. ChemRxiv 2024. [Google Scholar] [CrossRef] [Scilit]
- Wieczorek, A.; Lai, H.; Pious, J.; Fu, F.; Siol, S. Resolving oxidation states and Sn-halide interactions of perovskites through Auger parameter analysis in XPS. arXiv 2022, arXiv:2207.14123. [Google Scholar] [CrossRef] [Scilit]
- Nishimura, K.; Kamarudin, M.A.; Hirotani, D.; Hamada, K.; Shen, Q.; Iikubo, S.; Minemoto, T.; Yoshino, K.; Hayase, S. Lead-free tin-halide perovskite solar cells with 13% efficiency. Nano Energy 2020, 74, 104858. [Google Scholar] [CrossRef] [Scilit]
- Erro Quiñonez, J.E.; García Gutiérrez, R.; Arias-Ramos, C.F.; Cancino-Gordillo, F.E.; Verdugo Miranda, S.; Jiménez Sotomayor, C.Á. Automatización del procesamiento de datos experimentales en celdas solares de perovskita mediante una suite informática en Python con programación asistida por inteligencia artificial. Rev. Energ. Renov. 2025, 12, 31. [Google Scholar] [CrossRef]
- Qin, Z.; Pols, M.; Qin, M.; Zhang, J.; Yan, H.; Tao, S.; Lu, X. Over-18–efficiency quasi-2D Ruddlesden–Popper Pb–Sn mixed perovskite solar cells by compositional engineering. ACS Energy Lett. 2023, 8, 3188–3195. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Karim, A.; Matsuishi, K.; Kayesh, E.; He, Y.; Islam, A. Inhibition of Sn2+ Oxidation in FASnI3 Perovskite Precursor Solution and Enhanced Stability of Perovskite Solar Cells by Reductive Additive. ACS Appl. Mater. Interfaces 2023, 15, 47019–47027. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Nespoli, J.; Mugge, M.; van der Poll, L.M.; Lal, S.; Ibrahim, B.; Boshuizen, B.; Caselli, V.M.; Houtepen, A.J.; Bannenberg, L.J.; Savenije, T.J. Metastable Oxygen-Induced Light-Enhanced Doping in Mixed Sn–Pb Halide Perovskites. J. Am. Chem. Soc. 2024, 146, 30860–30870. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.