Abstract
Cu–Cr alloys are attractive candidates for aerospace and defense applications owing to their favorable strength-conductivity combination, although the intrinsic trade-off between strength and conductivity limits their engineering application. In this study, a CuCrNiCoSi0.6 (wt.%) alloy was fabricated by vacuum melting. The combined effects of cryorolling and aging on microstructural evolution, mechanical properties and electrical conductivity were studied, and the strengthening mechanisms and precipitation kinetics were clarified. Primary Cr3Si, Ni2Si and Co2Si phases exist in the as-cast alloy. After high-temperature treatment, Ni2Si and Co2Si dissolve into the matrix, whereas Cr3Si is retained. Cryorolling (CR) exhibits a higher dislocation density compared with room temperature rolling (RTR), which refines the width of deformation bands and the thickness of twin layers. Aging induces the formation of Cr-rich domains and (Ni,Co)2Si precipitates, which pin the boundaries of deformation bands and twin layers, and maintain structural stability. The alloy obtains optimal comprehensive performance after CR 90% deformation and aging at 440 °C for 60 min, with the ultimate tensile strength, yield strength, elongation and electrical conductivity of 753.8 MPa, 687.2 MPa, 5.6% and 48.3% IACS, respectively. The main strengthening contributions come from precipitation, grain-boundary and dislocation strengthening. Precipitation kinetic equations at different aging temperatures were established, and the precipitation activation energy was determined to be 36.3 kJ/mol.
1. Introduction
Copper and copper alloys exhibit desirable mechanical properties, favorable electrical conductivity and superior thermal stability, making them indispensable materials for aerospace and national defense equipment applications [1,2]. However, the rapid development of high-end equipment such as new energy devices, rail transit and integrated circuits toward miniaturization, high power and long service life has raised rigorous requirements for materials to achieve a synergistic balance between high strength and high electrical conductivity [3,4,5]. It is well known that pure copper possesses excellent electrical and thermal conductivity, while its tensile strength is generally lower than 350 MPa [6], failing to satisfy the comprehensive performance demands under extreme conditions. Therefore, enhancing the mechanical properties of copper alloys without significantly reducing electrical conductivity has become a key goal pursued by numerous researchers.
Cu–Cr alloys belong to thermodynamically immiscible systems. Nano-sized Cr-rich domains formed via phase separation during aging can greatly improve mechanical strength while inducing only minor conductivity loss, which renders Cu–Cr alloys promising candidates for high-performance copper materials. Microalloying is widely utilized to tailor phase separation behavior and regulate the morphology and distribution of these nano-sized domains, so as to simultaneously optimize the mechanical properties and electrical conductivity of Cu–Cr alloys [7,8,9,10,11,12]. Meng et al. [7] discovered that the CuCr0.4Zr0.3 alloy achieves an ultimate tensile strength of 568 MPa and electrical conductivity of 75.3% IACS after aging at 450 °C for 3 h, followed by CR 80% deformation. Feng et al. [8] reported that the CuCr0.4Ti0.06 alloy exhibits a microhardness of 158.8 HV, an ultimate tensile strength of 440.0 MPa, electrical conductivity of 71.6% IACS, and an elongation of 19.7% after aging at 450 °C for 3 h. Zhou et al. [9] demonstrated that the CuCr1.90Ag0.28 alloy acquires an ultimate tensile strength of 620 MPa, a yield strength of 600 MPa, electrical conductivity of 85.6%IACS and an elongation of 15.7%, after CR 50% deformation, aging at 500 °C for 5 min, secondary CR 50% deformation and aging at 400 °C for 1 h. Guo et al. [10] investigated the CuCr0.33Mg0.14 alloy, which reaches an ultimate tensile strength of 853.4 MPa, a yield strength of 809.4 MPa and electrical conductivity of 76% IACS after cold drawing with a true strain of 9.21 and aging at 150 °C for 1 h. Furthermore, Guo et al. [11] found that the CuCr0.47Nb0.16 alloy possesses an ultimate tensile strength of 549 MPa, a yield strength of 492 MPa, an elongation of 6.08% and electrical conductivity of 84.2%IACS via CR 80% deformation, aging at 450 °C for 0.5 h and CR 80% deformation. Wang et al. [12] confirmed that the co-addition of Fe and P enables the Cu-0.8Cr alloy to reach an ultimate tensile strength of 569 MPa and electrical conductivity of 64% IACS after CR 50% deformation, aging at 500 °C for 1 h and CR 95% deformation.
Apart from microalloying elements, cryorolling and aging are also effective methods for enhancing the mechanical properties of Cu–Cr alloys. In comparison to RTR, CR introduces more vacancies and dislocations within the alloy, which supply additional nucleation sites and diffusion channels for precipitates during aging. Li et al. [13] reported that the CuCr0.65Zr0.07 alloy achieves an ultimate tensile strength of 712 MPa and electrical conductivity of 70.2% IACS after aging at 550 °C for 1 h, combined with subsequent CR 90% deformation. Zhang et al. [14] demonstrated that the cryorolled CuCr0.5 alloy possesses a microhardness of 167.4 HV, yield strength of 486 MPa, ultimate tensile strength of 531 MPa and electrical conductivity of 92.5% IACS after aging at 450 °C for 2 h. Li et al. [15] reported that the CuCrZr0.2 (wt.%) alloy achieves a yield strength of 607 MPa, ultimate tensile strength of 624 MPa and electrical conductivity of 79.80% IACS after CR 90% deformation and aging at 450 °C for 1.5 h.
In this study, Ni and Si are introduced into the Cu–Cr matrix. Cr has low solubility in the Cu matrix and forms Cr-rich domains through phase separation, while Ni2Si can form as nano-sized precipitates during aging, which contribute to high tensile strength similar to Cu–Ni–Si alloys. However, since Ni and Si significantly degrade the electrical conductivity of copper alloys, their concentrations in the Cu–Cr alloy can be appropriately reduced to minimize electrical conductivity deterioration [16]. Co, which also shows low solubility in the Cu matrix and a weak adverse effect on electrical conductivity, readily reacts with Si to form Co2Si precipitates during aging, thereby improving the mechanical properties and electrical conductivity simultaneously [17]. Previous studies [18,19] reported that Co partially substitutes for Ni in Cu–Ni–Si alloys, accelerating the precipitation of solute Ni and the formation of (Ni,Co)2Si precipitates, which further enhances mechanical properties and electrical conductivity. Nevertheless, the co-addition of Ni, Co and Si in Cu–Cr alloys has rarely been investigated. Accordingly, a novel CuCrNiCoSi0.6 alloy is developed in this study, and the effects of cryrolling and aging on microstructure, mechanical properties and electrical conductivity are investigated. By clarifying the internal relationships among process parameters, microstructural evolution and properties, the study provides valuable insights into the composition regulation and process optimization of high-performance Cu–Cr alloys, which is conducive to technical upgrading and large-scale application in high-end equipment.
2. Materials and Methods
Commercial pure metals Cu, Cr, Ni, Co and Si (with purity ≥ 99.9 wt.%) were used as raw materials. The CuCr and CuCrNiCoSi0.6 (wt%, denoted as Cu–Cr and Cu–Cr–Ni–Co-Si in this paper) alloys were melted in a ZG-0.01L vacuum induction melting furnace (Huahong, Shanghai, China) under high-purity argon atmosphere protection and subsequently cast in a steel mold measuring 55.5 × 55.5 × 160 mm3. X-ray fluorescence spectrometry (XRF-1800, Shimadzu, Kyoto, Japan) was employed to identify the real chemical compositions of the as-cast ingots, and the corresponding data are listed in Table 1. A measurement uncertainty of ±0.5 at.% is adopted for the XRF analysis throughout this study.
Table 1.
Chemical compositions of the Cu–Cr and Cu–Cr–Ni–Co–Si alloys (wt.%).
Subsequently, the as-cast Cu–Cr and Cu–Cr–Ni–Co–Si ingots were subjected to homogenization at 900 °C for 240 min, followed by hot rolling with a total deformation of 40% at 880 °C. After hot rolling, the samples were tempered at 980 °C for 240 min and immediately water-quenched to room temperature. The Cu–Cr alloy was set as a control group and characterized only in the as-cast and tempered states for microstructural comparison. In contrast, the Cu–Cr–Ni–Co–Si alloy underwent additional RTR, CR and aging to explore its microstructural evolution and mechanical properties. The solution treated Cu–Cr–Ni–Co–Si alloy was processed by RTR and CR to a total deformation of 90%, respectively, with an average thickness reduction of 10% for each pass. For CR, the samples were immersed in liquid nitrogen (−196 °C) for 30 min prior to rolling, and re-immersed for 15 min after each pass to achieve adequate and homogeneous low-temperature cooling throughout the entire deformation process. Finally, the samples were subjected to isothermal aging at temperatures of 400–520 °C, and isochronal aging for durtaions of 0–300 min. It should be emphasized that the homogenization treatment was carried out to eliminate as-cast segregation and dissolve coarse eutectic phases. The hot rolling temperature was selected above the recrystallization temperature of the alloy to ensure sufficient hot workability and fragment the cast microstructure. The high-temperature tempering treatment aims to dissolve Cr, Ni, Co and Si alloying elements into the Cu matrix to obtain a metastable supersaturated solid solution, and the temperature was kept below the solidus to avoid local melting. The aging procedure was optimized to promote uniform precipitation of nano-sized strengthening phases, balancing mechanical properties and electrical conductivity, following the established processing window of Cu–Cr alloys reported in the previous literature [9,14,15,20]. The detailed manufacturing process route is illustrated in Figure 1.
Figure 1.
The manufacturing process of the Cu–Cr–Ni–Co–Si alloy.
The microstructures of the samples were characterized using an optical metallurgical microscope (OM, MEF-3, Leica, Wetzlar, Germany) and a field emission scanning electron microscope (SEM, Zeiss Supra 55, Carl Zeiss, Oberkochen, Germany) at an accelerating voltage of 15 kV. For OM and SEM characterization, samples were ground sequentially using 60#, 240#, 400#, 800#, 1200#, 2000# and 3000# SiC abrasive papers. Subsequently, mechanical polishing was performed on velvet cloth affixed to a polishing machine with 0.5-μm water-based diamond paste until a bright, scratch-free mirror-like surface was obtained. Chemical etching was conducted at room temperature in an FeCl3–HCl–ethanol etchant (3 g FeCl3 + 2 mL HCl + 95 mL ethanol) for 15 s. Following etching, the samples were rapidly cleaned with deionized water and ethanol, then dried by cold air. For transmission electron microscopy (TEM) analysis, disc specimens with a diameter of 3 mm were cut from the longitudinal plane. After grinding to a thickness of 30 µm, the samples were subjected to ion thinning in the PIPS 691 instrument (Gatan, Pleasanton, CA, USA). An FEI Tecnai G220 TEM ( Hillsboro, OR, USA) operating at 200 kV was used for high-resolution TEM (HRTEM) observations. XRD data were collected on the EMPYREAN diffractometer (Malvern Panalytical, Almelo, The Netherlands), equipped with a Cu target. The scan step was 0.016°, and the 2θ range covered 20° to 100°.
Vickers hardness tests were performed on samples with a cross-section of 15 × 15 mm2 using an MH5L microhardness tester (Huayin, Laizhou, China) under a load of 300 g and a dwell time of 15 s. Seven indentations were made at distinct positions on each sample, and the average value was adopted to ensure measurement accuracy. Tensile tests were carried out on an Instron 5500 R universal testing machine (Instron, Norwood, MA, USA) for samples with a gauge length of 50 mm at an initial displacement rate of 2 mm/min. Each tensile test was repeated three times, and the averaged results were reported to guarantee experimental reliability. Samples for electrical conductivity characterization were machined to a cross-section of 15 × 15 mm2 and measured using a D60K conductivity tester (Foerster, Reutlingen, Germany), with five independent sites examined per sample and a measurement repeatability within 0.3% IACS.
3. Results
3.1. Microstructure of the As-Cast Cu–Cr and Cu–Cr–Ni–Co–Si Alloys
Figure 2 presents the microstructures of the as-cast Cu–Cr and Cu–Cr–Ni–Co–Si alloys. It can be observed from Figure 2a that the Cu–Cr alloy exhibits coarse equiaxed grains, with a small quantity of Cr-rich particles segregated at grain boundaries and within grain interiors. With the addition of Ni, Co and Si (Figure 2b), new phases form in the alloy; some second-phase particles are heterogeneously distributed within grains, whereas others segregate along grain boundaries.
Figure 2.
Optical images of the as-cast (a) Cu–Cr and (b) Cu–Cr–Ni–Co–Si alloys.
To further characterize the phase constituents, SEM observations were performed on the as-cast Cu–Cr and Cu–Cr–Ni–Co-Si alloys, as presented in Figure 3. Figure 3a shows that granular Cr phases are uniformly dispersed in the Cu matrix, with an average size of 1.4 µm. The addition of Ni, Co and Si promotes the formation of new secondary phases with different sizes and morphologies (Figure 3b). EDS analysis on individual particles was conducted to clarify elemental compositions, and the acquired data are summarized in Table 2. The results verified that the large irregular particles in the Cu–Cr–Ni–Co–Si alloy correspond to Cr3Si phases. Nevertheless, EDS cannot precisely characterize fine precipitates owing to its inherent detection limitations. Accordingly, XRD analysis was further adopted to accurately identify the fine secondary phases of the as-cast alloys.
Figure 3.
SEM images of the as-cast (a) Cu–Cr and (b) Cu–Cr-–Ni–Co–Si alloys.
Table 2.
EDS results of as-cast Cu–Cr and Cu–Cr–Ni–Co–Si alloys at different positions.
The XRD patterns of the as-cast Cu–Cr and Cu–Cr–Ni–Co–Si alloys are presented in Figure 4. As observed from Figure 4a, the three dominant diffraction peaks are indexed to the α-Cu matrix. In addition, weak Cr diffraction peaks are also detected in the Cu–Cr alloy. Moreover, the addition of Ni, Co and Si yields new diffraction peaks in the Cu–Cr–Ni–Co–Si alloy. Combined with standard PDF card matching, the large particles in the alloy are confirmed to be Cr3Si phases, and the weak diffraction peaks of the Cr3Si phase are attributed to its low volume fraction. Notably, the fine secondary phases can hardly be identified in the XRD pattern due to their small size. For this reason, the rectangular region marked in Figure 4a was locally magnified, and the weak diffraction signals obtained from Figure 4b demonstrate the formation of Ni2Si and Co2Si phases in the Cu–Cr–Ni–Co–Si alloy.
Figure 4.
The XRD patterns of the as-cast Cu–Cr and Cu–Cr–Ni–Co–Si alloys. (a) XRD patterns in the range of 20~100°; (b) magnified patterns of the area in the rectangle box of (a).
3.2. Microstructure of the Cu–Cr and Cu–Cr–Ni–Co–Si Alloys After Solid Solution
Figure 5 presents the SEM images of the Cu–Cr and Cu–Cr–Ni–Co–Si alloys after high-temperature tempering at 980 °C. As shown in Figure 5a, most Cr phases are dissolved into the Cu matrix during tempering. Nevertheless, some Cr particles remain undissolved, because the Cr content in the alloy exceeds its maximum solubility in the Cu matrix under this condition. For the Cu–Cr–Ni–Co–Si alloy, the coarse primary Cr3Si particles formed during solidification possess superior high-temperature stability and thus cannot dissolve into the matrix during tempering. In contrast, most fine Ni2Si and Co2Si precipitates gradually dissolve into the Cu matrix upon tempering, yielding a metastable supersaturated solid solution (Figure 5b).
Figure 5.
SEM images of the (a) Cu–Cr and (b) Cu–Cr–Ni–Co–Si alloys after high-temperature tempering at 980 °C.
3.3. Microstructure of the Cu–Cr–Ni–Co–Si Alloy After RTR and CR 90% Deformation
To explore the effect of CR on the microstructural evolution of the Cu–Cr–Ni–Co–Si alloy, TEM characterization was performed along the rolling direction of the samples subjected to RTR and CR 90% deformation, as shown in Figure 6. After RTR 90% deformation, abundant deformation bands nearly parallel to the rolling direction were observed throughout the alloy. Meanwhile, subgrain structures and a minor fraction of deformation twins formed within the microstructure (Figure 6a). The subgrain size was quantified via the linear intercept method using bright-field TEM images, where subgrain boundaries were distinguished by visible dislocation walls and dislocation arrays. More than 60 subgrains were sampled from 20 randomly acquired TEM images to calculate the average value and corresponding standard deviation. Statistical analysis based on these TEM micrographs gave an average deformation band width of 103 nm, a twin lamella thickness of 38 nm, and a subgrain size of 545 nm, respectively (Figure 7a–c). Figure 6b displays the bright-field TEM images of the alloy after CR 90% deformation. Analogous to the RTR microstructure, deformation bands, deformation twins, and subgrains were also detected in the CR sample. The deformation band width and twin layer thickness decreased to 96 nm and 32 nm, corresponding to reductions of 6.8% and 15.8% compared with the RTR counterpart (Figure 7d,e). In contrast, the subgrain size exhibited no significant variation, with a size of 539 nm (Figure 7f).
Figure 6.
TEM bright-field images of the Cu–Cr–Ni–Co–Si alloy with (a) RTR and (b) CR 90% deformation.
Figure 7.
Size statistics of the Cu–Cr–Ni–Co–Si alloy with (a–c) RTR and (d–f) CR 90% deformation.
3.4. Microstructures of the Cu–Cr–Ni–Co–Si Alloy During Aging
Figure 8 presents the bright-field TEM images along the rolling direction of the Cu–Cr–Ni–Co–Si alloy after RTR and CR 90% deformation and aging at 440 °C for 60 min. The corresponding statistical results of deformation band width, twin layer thickness and subgrain size are summarized in Figure 9. TEM observations and statistical analysis revealed that slight recovery and recrystallization occurred in both RTR and CR samples during aging, which marginally increased the subgrain size to 547 nm and 543 nm, respectively. Nevertheless, abundant deformation bands and twins were well retained after aging, with no significant dimensional variation relative to the as-rolled state, demonstrating excellent structural stability of the deformed microstructure. Moreover, high-density dislocations induced by RTR and CR 90% deformation (Figure 6) acted as preferential nucleation sites for the precipitation of numerous nano-sized particles. These precipitates intertwined with dislocations to form stable dislocation cell structures, which provided nucleation sites for recrystallized grains and efficient diffusion channels for supersaturated solute atoms in the Cu matrix, thereby alleviating matrix supersaturation and enabling simultaneous improvements in mechanical properties and electrical conductivity.
Figure 8.
TEM bright-field images of the Cu–Cr–Ni–Co–Si alloy along the rolling direction with (a) RTR and (b) CR 90% deformation and aging at 440 °C for 60 min.
Figure 9.
Size statistics of the Cu–Cr–Ni–Co–Si alloy with (a–c) RTR and (d–f) CR 90% deformation and aging at 440 °C for 60 min.
To further clarify the chemical composition and crystal structure of precipitates in the Cu–Cr–Ni–Co–Si alloy during aging, HRTEM analysis was carried out on the alloy with CR 90% deformation and aging at 440 °C for 60 min, as illustrated in Figure 10. Spherical particles with an average diameter of 2.1 μm are clearly observed in Figure 10a. Based on the corresponding SAED pattern (Figure 10b), the particles are identified as the Cr3Si phase, with lattice constants a = 0.8763 nm, b = 0.8763 nm and c = 0.4561 nm. This observation is consistent with the results presented in Figure 4. Apart from the Cr3Si particles, two types of nano-precipitates with different sizes and morphologies are detected within the alloy (Figure 10c,d). From their respective FFT patterns, the precipitate with an average diameter of 13 nm is confirmed to be the fcc structure Cr-rich domains (Figure 10c), with lattice constants a = 0.4588 nm, b = 0.4588 nm and c = 0.4588 nm. The other precipitate, with an average diameter of 7 nm, is the orthorhombic (Ni,Co)2Si phase (Figure 10d), whose lattice constants are a = 0.708 nm, b = 0.502 nm and c = 0.371 nm.
Figure 10.
TEM images of the Cu–Cr–Ni–Co–Si alloy with CR 90% deformation and aging at 440 °C for 60 min. (a) the Cr3Si phase; (b) the corresponding SAED pattern; (c) HRTEM of Cr-rich domains and the corresponding FFT image; (d) HRTEM of (Ni,Co)2Si precipitates and the corresponding FFT image.
3.5. Properties of the Cu–Cr–Ni–Co–Si Alloy During Aging
To explore the optimal aging parameters for superior comprehensive performance of the Cu–Cr–Ni–Co–Si alloy with RTR and CR 90% deformation, hardness and electrical conductivity were investigated under varied aging time and temperatures, as illustrated in Figure 11. As demonstrated in Figure 11a, hardness rises sharply at the early stage of aging and subsequently increases gently for both CR and RTR samples, with peak hardness values of 231 ± 6.8 HV and 219 ± 4.1 HV achieved after aging at 440 °C for 60 min, respectively. Meanwhile, electrical conductivity rises sharply at the initial aging stage and gradually stabilizes after aging for 60 min, with the values of 47.9% IACS and 48.3% IACS, respectively, as shown in Figure 11b. On this basis, the hardness variation of the alloy aging for 60 min at different temperatures was further examined (Figure 11c). Hardness peaks at 440 °C and subsequently declines markedly with a continuous temperature increase. By comparison, electrical conductivity increases monotonically as the aging temperature rises (Figure 11d). In addition, the alloy with CR 90% deformation exhibits marginally higher electrical conductivity than its RTR counterpart under identical aging conditions.
Figure 11.
Hardness and electrical conductivity of the Cu–Cr–Ni–Co–Si alloy after CR and RTR 90% deformation. (a) hardness and (b) electrical conductivity of the samples aging at 440 °C for various time; (c) hardness and (d) electrical conductivity of the samples aging at different temperatures for 60 min.
As stated in the preceding section, aging at 440 °C for 60 min yields an excellent combination of hardness and electrical conductivity for both RTR and CR samples. Thus, the tensile tests were carried out under this optimal aging condition. The engineering stress–strain curves of the Cu–Cr–Ni–Co–Si alloy after RTR and CR 90% deformation and aging at 440 °C for 60 min are presented in Figure 12. The YS and UTS of the alloy with CR 90% deformation and aging at 440 °C for 60 min can reach 687.2 MPa and 753.8 MPa, showing increments of 24.4 MPa and 48.7 MPa relative to the RTR counterpart. In contrast, its elongation reaches 5.6%, merely 0.3% lower than that of the RTR sample.
Figure 12.
The engineering stress–strain curve of the Cu–Cr–Ni–Co–Si alloy after RTR and CR 90% deformation and aging at 440 °C for 60 min.
4. Discussion
4.1. Effect of Cryorolling and Aging on Microstructural Evolution in the Cu–Cr–Ni–Co–Si Alloy
As shown in Figure 6 and Figure 7, the Cu–Cr–Ni–Co–Si alloy with CR 90% deformation exhibits finer deformation bands and thinner twin lamellae compared with RTR 90% deformation. The correlation between the deformation band width and the dislocation density can be described by the following equation [20]:
where D denotes the deformation band width, m is a constant, and ρd refers to the dislocation density. The Williamson–Hall approach [21] was adopted to calculate dislocation densities for the samples processed by RTR and CR, as expressed in Equation (2):
where ε is the microstrain measured by fitting the XRD diffraction pattern, dgrain denotes the average grain size, and b is the Burgers vector (0.2556 nm). The relation linking the full width at half maximum (FWHM), microstrain and grain size from XRD measurements is given by Equation (3) [22]:
where β represents the FWHM of the Cu diffraction peak (in radians), θ is the diffraction angle of the Cu matrix peak, λ corresponds to the wavelength of Cu–Kα radiation (0.15405 nm), and k is a constant (0.9). Figure 13 displays XRD pattens and Williamson–Hall fitting curves of the Cu–Cr–Ni–Co–Si alloy with RTR and CR 90% deformation. The microstrain ε is determined by the slope of the fitted line. Inserting the calculated ε into Equation (2) yields the dislocation density ρd. The dislocation densities for the Cu–Cr–Ni–Co–Si alloy with RTR and CR 90% deformation are 22.78 × 1013 m−2 and 29.12 × 1013 m−2, respectively. This result indicates that CR increases the dislocation density and reduces the deformation band width.
βcos (θ) = 4εsin (θ) + kλ/dgrain
Figure 13.
XRD pattens and Williamson–Hall fitting curves of the Cu–Cr–Ni–Co–Si alloy with RTR and CR 90% deformation. (a) XRD paterns; (b) Williamson–Hall fitting curves.
Furthermore, the rolling temperature exerts an influence on twin layer thickness, and the relationship can be expressed as [23]:
where λc is the critical thickness of a twin embryo capable of nucleating and growing into a mature twin; ρ represents the ratio between the thickness and diameter of twin nuclei, which is a constant; γTB denotes twin-boundary energy, which is positively correlated with stacking fault energy; and Ω is the nucleation driving force for twin formation, which presents an inversely proportional to deformation temperature. Accordingly, CR provides a higher driving force for twin nucleation relative to RTR, leading to a reduction in twin layer thickness.
Cryorolling introduces high-density dislocations to strengthen the alloy, and these dense dislocations act as preferential nucleation sites for precipitates during subsequent aging. Meanwhile, the nano-sized Cr-rich domains and (Ni,Co)2Si precipitates formed upon aging can impede dislocation motion and pin boundaries during deformation and recovery. As illustrated in Figure 8, most deformation bands and twin lamellae therefore remain stable after aging at 440 °C for 60 min, without obvious recrystallization.
4.2. Analysis of Strengthening Mechanisms in the Cu–Cr–Ni–Co–Si Alloy with CR 90% Deformation and Aging
As discussed in Section 3.5, the Cu–Cr–Ni–Co–Si alloy subjected to CR 90% deformation and aging at 440 °C for 60 min achieves the optimal combination of mechanical properties and electrical conductivity. Accordingly, the strengthening mechanisms of the alloy under such processing conditions are clarified in this subsection.
The designed alloy is mainly strengthened by multiple synergistic mechanisms, including dislocation strengthening (σDis), grain-boundary strengthening (σGB), twin-boundary strengthening (σTB), precipitation strengthening (σOrowan), and solid-solution strengthening (σSS), which can be quantified by the following equation [20,24]:
where σ0 is taken as 52 MPa for the Cu matrix [25].
σtotal = σ0 + σDis + σGB + σTB + σOrowan + σSS
- (1)
- Dislocation strengthening
As revealed from TEM images in Figure 8, substantial dislocation multiplication takes place within the alloy after CR 90% deformation and aging at 440 °C for 60 min. The high-density dislocation networks act as strong barriers against dislocation glide, thereby elevating the load-bearing capacity of the Cu matrix. The strengthening increment due to dislocation strengthening can be computed from the Taylor relation [26]:
σDis = MαGbρd1/2
In this formula, M corresponds to the Taylor factor, α represents a constant, G is the shear modulus of Cu alloys, b stands for Burgers vector, and ρd refers to the measured dislocation density. According to the parameters listed in Table 3, the calculated yield-strength increment contributed by dislocation strengthening reaches 84.5 MPa.
Table 3.
Parameters for quantitative calculation of yield strength.
- (2)
- Grain-boundary strengthening
Apart from the dislocation strengthening, grain refinement induced by CR deformation also makes a considerable contribution to yield-strength improvement. The strengthening effect from grain-boundary obstacles is evaluated through the Hall–Petch equation [35]:
where KH−P is the Hall–Petch constant and dgrain denotes the grain size. It is noted that the dgrain used in the Hall–Petch equation is the measured subgrain size rather than the high-angle grain size. After CR 90% deformation, the microstructure is dominated by dislocation cells and subgrains. These low-angle subgrain boundaries serve as barriers to dislocation motion, and such treatment has been widely accepted in quantitative strengthening analysis of Cu–Cr alloys [3,7,11]. On this basis, the grain-boundary strengthening increment is calculated as 152.0 MPa.
- (3)
- Twin-boundary strengthening
Deformation twins formed during the CR process also provide a certain contribution to the yield-strength improvement of the alloy. Analogous to the grain-boundary strengthening, the yield-strength enhancement from twin-boundary strengthening can be estimated by a modified Hall–Petch formulation [36]:
Here, Vft represents the volume fraction of deformation twins; KTB is the twin-boundary strengthening coefficient, which is taken equal to the Hall–Petch coefficient KH−P; and dTB denotes the average thickness of twin layers. Based on the parameters given in Table 3, the increment in yield strength originating from twin-boundary strengthening is calculated to be 23.1 MPa.
- (4)
- Precipitation strengthening
As shown in Figure 10c,d, nano-sized Cr-rich domains and (Ni,Co)2Si precipitates with an average radius of 6.5 nm and 3.5 nm, respectively, form in the alloy during aging. These precipitates can hinder grain-boundary migration and facilitate dislocation accumulation within grains. The yield-strength increment originating from precipitation strengthening can be described by the Orowan model [22,37]:
where dpre are the average sizes of Cr-rich domains and (Ni,Co)2Si precipitates, which were statistically measured using NanoMeasure software, λ stands for the average inter-precipitate spacing, and f is precipitate volume fraction. Specifically, A denotes the total measured area and N corresponds to the number of precipitates, with both values statistically measured from 20 TEM micrographs. Based on the parameters listed in Table 3, the precipitation strengthening contributions derived from the nano-sized Cr-rich domains and (Ni,Co)2Si precipitates are calculated to be 105.8 MPa and 206.6 MPa, respectively, yielding a total precipitation strengthening increment of 314.2 MPa.
- (5)
- Solid-solution strengthening
Ni, Co and Si solute atoms differ from Cu matrix atoms in both atomic radius and shear modulus. The dissolved solute atoms produce localized lattice distortion, while modulus mismatch changes the strain energy of dislocation lines. The strength increment from solid-solution strengthening can be quantified using Equation (12) [38]:
where εSS is the misfit strain and c represents the solute concentration (wt%) within the Cu matrix. In the present study, Cr atoms preferentially react with Si to form the Cr3Si phase due to the higher inter-atomic binding energy between Cr and Si atoms. Accordingly, approximately 0.18 wt.% of Si is consumed to fully react with 1 wt.% of solute Cr. The remaining 0.42 wt.% Si participates in the formation of (Ni,Co)2Si precipitates, which requires approximately 1.76 wt.% of Ni and Co atoms. As a result, the residual 0.24 wt.% Ni and Co atoms remain as solute atoms inside the Cu matrix. The parameters are summarized in Table 3, and the yield-strength increment contributed by solid-solution strengthening is estimated to be 48.7 MPa.
In summary, the calculated yield strength of the Cu–Cr–Ni–Co–Si alloy with CR 90% deformation and aging at 440 °C for 60 min reaches 674.5 MPa, which shows good consistency with the experimental measurement of 687.2 MPa, yielding an error of merely 1.88%. Such minor deviation mainly stems from uncertainties in the statistical determination of precipitate size and volume fraction, deformation band width and volume fraction, as well as dislocation density.
The percentage contribution of each strengthening mechanism toward the overall yield strength is illustrated in Figure 14. Precipitation strengthening makes the most dominant contribution to strength enhancement, accounting for 46.6% of total yield strength, followed by grain-boundary strengthening (22.5%), dislocation strengthening (12.5%), solid-solution strengthening (7.2%), and twin-boundary strengthening (3.5%).
Figure 14.
The percentage contribution of each strengthening mechanism toward the overall yield strength of the Cu–Cr–Ni–Co–Si alloy.
4.3. Analysis of Precipitation Kinetics in the Cu–Cr–Ni–Co–Si Alloy with CR 90% Deformation and Aging
Precipitation kinetics dominate the nucleation, growth, and coarsening of nanoscale precipitates, which essentially determine the mechanical properties and electrical conductivity of the Cu–Cr–Ni–Co–Si alloy. To elucidate the microstructural origins of property evolution and establish the correlation among aging parameters, precipitate characteristics, mechanical properties, and electrical conductivity of the alloy, the precipitation kinetics behavior at different temperatures are investigated in this section.
The progress of precipitation transformation can be tracked by monitoring the evolution of electrical conductivity during isothermal aging, and the transformed precipitate volume fraction f is given by [39]:
where Vt denotes the precipitate volume formed per unit matrix volume at a given aging time and Ve corresponds to the equilibrium precipitate volume per unit matrix volume at a specified aging temperature. Furthermore, following Matthiessen’s law, electrical conductivity exhibits a linear dependence on the transformed precipitate fraction f, which can be formulated as [40]:
where σ0 is defined as the electrical conductivity prior to aging, σt is the electrical conductivity at a given aging time, and σe is the equilibrium electrical conductivity after the complete precipitation of precipitates during aging. The transformed precipitate volume fraction f at 440 °C, 480 °C, and 520 °C can be directly computed using experimental electrical conductivity data, as summarized in Table 4.
σt − σ0 = (σe − σ0)f
Table 4.
Electrical conductivity and volume fraction of precipitates of the Cu–Cr–Ni–Co–Si alloy with CR 90% deformation and aging at different temperatures for various times.
The precipitate phase transformation kinetics can be empirically expressed using the Avrami equation [41]:
where t represents the aging time, b is the rate constant related to the nucleation and growth of precipitates, and n is the Avrami exponent. The Avrami exponent reflects atomic diffusion behavior, and its value is determined by the transformation mechanism and the type of nucleation sites. Taking the natural logarithms of both sides of Equation (15) yields the linear form:
where n stands for the slope of the line and lnb is the intercept. The plots of ln[ln(1/(1 − f))] versus lnt at different temperatures are shown in Figure 15.
f = 1 − exp(−btn)
Figure 15.
The plots of ln[ln(1/(1 − f))] versus lnt at different temperatures.
According to Figure 15 and Equation (16), the volume fraction of precipitates f at a given time can be evaluated. The corresponding precipitate phase transformation kinetic curves are presented in Figure 16, and the fitted kinetic equations at each temperature are listed in Table 5.
Figure 16.
Precipitate phase transformation curves of the Cu–Cr–Ni–Co–Si alloy with CR 90% deformation and aging at different temperatures.
Table 5.
Fitted precipitation kinetic equations for the Cu–Cr–Ni–Co–Si alloy at different aging temperatures.
Precipitation relies on the diffusion and rearrangement of solute atoms, which must overcome an energy barrier termed activation energy Q. The dependence of the rate constant on temperature follows the Arrhenius relation [42]:
where R is the universal gas constant (8.3145 J/(mol∙K)) and T denotes the thermodynamic temperature. The logarithmic of Equation (17) is derived as follows:
The reaction rate constants b obtained from Table 5 were used to construct the linear fit of ln b against 1/T, as presented in Figure 17. The precipitation activation energy of the Cu–Cr–Ni–Co–Si alloy is determined to be 36.3 kJ/mol from the slope of the linear fit.
Figure 17.
Linear fitting curve of Inb and temperature.
5. Conclusions
In the present study, a novel Cu–Cr–Ni–Co–Si alloy was developed, and the effects of cryorolling and aging on the microstructure, mechanical properties and electrical conductivity were investigated. The main conclusions are summarized as follows:
- (1)
- Primary Cr3Si, Ni2Si and Co2Si phases are formed in the as-cast alloy. Upon high-temperature tempering at 980 °C, Ni2Si and Co2Si phases dissolve into the matrix, while the Cr3Si phase exhibits no obvious change. After CR 90% deformation, the average deformation bands width and twin layers thickness reach 96 nm and 32 nm, respectively, which are 6.8% and 15.8% lower than those of the alloy with RTR 90% deformation. During aging, nano-sized Cr-rich domains and (Ni,Co)2Si precipitates form within the alloy. Partial precipitates pin the boundaries of deformation bands and twin layers, which effectively maintains the structural stability.
- (2)
- A good combination of comprehensive performance of the alloy is achieved after CR 90% deformation and aging at 440 °C for 60 min, with the ultimate tensile strength, yield strength, elongation and electrical conductivity of 753.8 MPa, 687.2 MPa, 5.6% and 48.3% IACS, respectively. The precipitation strengthening, grain-boundary strengthening, and dislocation strengthening serve as the dominant strengthening mechanisms for the alloy, with contribution ratios of 46.6%, 22.5% and 12.5%, respectively.
- (3)
- Precipitation kinetic equations at 440 °C, 480 °C and 520 °C are established using the relationship between electrical conductivity and precipitate volume fraction. The precipitation activation energy of the alloy is calculated as 36.3 kJ/mol.
Author Contributions
Conceptualization, Y.G.; Funding acquisition, X.S.; Investigation, X.S. and Y.G.; Methodology, T.L.; Supervision, X.W. and J.B.; Writing—review and editing, X.S. and J.J. All authors have read and agreed to the published version of the manuscript.
Funding
The authors gratefully acknowledge the support of the Education Department of Liaoning Province (No. JYTQN2023056).
Data Availability Statement
The original contributions presented in the study are included in the article; further inquiries can be directed to the corresponding author.
Conflicts of Interest
The authors declare no conflicts of interest.
References
- Shang, Y.; Cen, G.B.; Sun, J.N.; Hu, J.K.; Wu, J.L.; Pi, J.H. Enhanced strength and ductility of Cu-Cr-Zr alloy via constrained cold forging with retained conductivity. J. Alloys Compd. 2026, 1064, 187939. [Google Scholar] [CrossRef] [Scilit]
- Yang, K.; Wang, Y.H.; Guo, M.X.; Wang, H.; Mo, Y.D.; Dong, X.G.; Lou, H.F. Recent development of advanced precipitation-strengthened Cu alloys with high strength and conductivity: A review. Prog. Mater. Sci. 2023, 138, 101141. [Google Scholar] [CrossRef] [Scilit]
- Qi, F.X.; Fu, H.W.; Yun, X.B. Achieving high strength and high electrical conductivity Cu-Cr-Zr alloys by continuous extrusion and thermomechanical treatment. Mater. Sci. Eng. A 2024, 915, 147242. [Google Scholar] [CrossRef] [Scilit]
- Peng, L.Z.; Gao, Z.F.; Huang, X.X.; Xie, G.L. Precision interruption and deformation: A kinetic strategy for synergistic strength-conductivity enhancement in Cu-Cr-Nb Alloys. J. Alloys Compd. 2026, 1080, 190564. [Google Scholar] [CrossRef] [Scilit]
- Fu, H.D.; Xu, S.; Li, W.; Xie, J.X.; Zhao, H.B.; Pan, Z.J. Effect of rolling and aging processes on microstructure and properties of Cu-Cr-Zr alloy. Mater. Sci. Eng. A 2017, 700, 107–115. [Google Scholar] [CrossRef] [Scilit]
- Aghayar, Y.; Moazzen, P.; Kestens, L.A.I.; Mohammadi, M. Tailoring the microstructure, physical, and mechanical properties of pure copper using various additive manufacturing techniques. J. Alloys Compd. 2025, 1010, 178332. [Google Scholar] [CrossRef] [Scilit]
- Meng, A.; Nie, J.F.; Wei, K.; Kang, H.J.; Liu, Z.J.; Zhao, Y.H. Optimization of strength, ductility and electrical conductivity of a Cu-Cr-Zr alloy by cold rolling and aging treatment. Vacuum 2019, 167, 329–335. [Google Scholar] [CrossRef] [Scilit]
- Feng, L.; Li, J.N.; Lu, Q.; You, Y.Q.; Xu, Z.Y.; Liu, L.Y.; Fu, L.; Gao, P.; Yi, J.H.; Li, C.J. Accelerated development of high-strength and high-conductivity Cu-Cr-Ti alloys based on data-driven design and experimental validation. Mater. Des. 2025, 253, 113948. [Google Scholar] [CrossRef] [Scilit]
- Zhou, S.; Lei, Q.; Yin, J.; Liu, W.; Yan, X.; Hu, H.L.; Mo, X.D.; Wei, T.S.; Wang, J.Y. Effect of Si addition on the microstructure and mechanical properties of a Cu-Cr-Ag alloy with high strength and electrical conductivity. Mater. Sci. Eng. A 2025, 934, 148310. [Google Scholar] [CrossRef] [Scilit]
- Guo, J.L.; Wan, H.; Xu, H.D.; Yan, H.; Shao, Y.; Hu, Z.; Zhao, C.Q.; Hu, Q. Effects of different Cr contents on the microstructure, mechanical and electrical properties of Cu-Mg-Cr alloy. J. Mater. Res. Technol. 2026, 40, 3741–3757. [Google Scholar] [CrossRef] [Scilit]
- Guo, X.L.; Xiao, Z.; Qiu, W.T.; Li, Z.; Zhao, Z.Q.; Wang, X.; Jiang, Y.B. Microstructure and properties of Cu-Cr-Nb alloy with high strength, high electrical conductivity and good softening resistance performance at elevated temperature. Mater. Sci. Eng. A 2019, 749, 281–290. [Google Scholar] [CrossRef] [Scilit]
- Wang, Y.T.; Fu, H.D.; Wang, J.; Zhang, H.T.; Li, W.D.; Xie, J.X. Enhanced combination properties of Cu-0.8Cr alloy by Fe and P additions. J. Nucl. Mater. 2019, 526, 151753. [Google Scholar] [CrossRef] [Scilit]
- Li, G.Y.; Li, S.Y.; Li, L.; Zhang, D.T.; Wang, J.D.; Tong, Y.X. A high strength and high electrical conductivity CuCrZr alloy prepared by aging and subsequent cryorolling. Vacuum 2021, 190, 110315. [Google Scholar] [CrossRef] [Scilit]
- Zhang, P.C.; Shi, J.F.; Yu, Y.S.; Sun, J.C.; Li, T.J. Effect of cryorolling on microstructure and property of high strength and high conductivity Cu-0.5wt.%Cr alloy. Trans. Nonferrous Met. Soc. China 2020, 30, 2472–2479. [Google Scholar] [CrossRef] [Scilit]
- Li, R.G.; Guo, E.Y.; Chen, Z.N.; Kang, H.J.; Wang, W.; Zou, C.L.; Li, T.J.; Wang, T.M. Optimization of the balance between high strength and high electrical conductivity in CuCrZr alloys through two-step cryorolling and aging. J. Alloys Compd. 2019, 771, 1044–1051. [Google Scholar] [CrossRef] [Scilit]
- Zhou, S.; Lei, Q.; Yin, J.; Qin, D.Y.; Hu, H.L.; Fan, J.L.; Jiang, Y.B.; Li, Z. Low-cost and performance-balanced Cu-Ni-Cr-Si copper strips designed with machine learning and fabricated with short processing route. Mater. Des. 2026, 271, 117075. [Google Scholar] [CrossRef] [Scilit]
- Yang, H.R.; Chi, T.D.; Fan, Y.C.; Zhou, J.H.; Lin, N.; Wang, B.S.; Wang, C. Effects of Si and Co co-addition on the comprehensive properties and microstructure of Cu-Cr-Zr alloy. J. Alloys Compd. 2026, 1079, 189988. [Google Scholar] [CrossRef] [Scilit]
- Zhao, Z.; Zhang, Y.; Tian, B.H.; Jia, Y.L.; Liu, Y.; Song, K.X.; Volinsky, A.A. Co effects on Cu-Ni-Si alloys microstructure and physical properties. J. Alloys Compd. 2019, 797, 1327–1337. [Google Scholar] [CrossRef] [Scilit]
- Zhang, Y.T.; Liu, Z.X.; Luo, Y.; Xiao, S.S.; Liu, F.; Lei, Q. High conductivity and high strength Cu-Ni-Co-Si alloys with hierarchical nanoscale and microscale precipitates. J. Alloys Compd. 2026, 1054, 186321. [Google Scholar] [CrossRef] [Scilit]
- Li, L.J.; Kang, H.J.; Zhang, S.R.; Li, R.G.; Yang, X.; Chen, Z.N.; Guo, E.Y.; Wang, T.M. Microstructure and properties of Cu-Cr-Zr (Mg) alloys subjected to cryorolling and aging treatment. J. Alloys Compd. 2023, 938, 168656. [Google Scholar] [CrossRef] [Scilit]
- He, J.Y.; Wang, H.; Huang, H.L.; Xu, X.D.; Chen, M.W.; Wu, B.Y. A precipitation hardened high-entropy alloy with outstanding tensile properties. Acta Mater. 2016, 102, 187–196. [Google Scholar] [CrossRef] [Scilit]
- Zhang, Y.M.; Niu, C.C.; Wang, Z.; Song, K.X.; Xu, Y.K.; Liu, F.Y.; Feng, J. Study on microstructure, properties and precipitation kinetics of Cu-3Ti-1.2 Mg alloy under three-stage aging. Mater. Charact. 2026, 240, 116787. [Google Scholar] [CrossRef] [Scilit]
- Zhang, Y.; Tao, N.R.; Lu, K. Effect of stacking-fault energy on deformation twin thickness in Cu-Al alloys. Scr. Mater. 2009, 60, 211–213. [Google Scholar] [CrossRef] [Scilit]
- Huang, F.F.; Xiao, Z.; Li, L.H.; Jiang, Y.; Li, Z.; Jia, Y.L.; Li, S.F.; Cao, H.; Meng, X.P. Microstructure and properties of the Cu-Co-Si-Ni-Cr-Zr alloy with high strength, high electrical conductivity and good softening resistance performance. J. Mater. Res. Technol. 2026, 42, 6497–6508. [Google Scholar] [CrossRef] [Scilit]
- Hansen, N. Polycrystalline strengthening. Metall. Trans. A 1985, 16, 2167–2190. [Google Scholar] [CrossRef] [Scilit]
- Balogh, L.; Ungár, T.; Zhao, Y.H.; Zhu, Y.T.; Horita, Z.J.; Xu, C.; Langdon, T.G. Influence of stacking-fault energy on microstructural characteristics of ultrafine-grain copper and copper-zinc alloys. Acta Mater. 2008, 56, 809–820. [Google Scholar] [CrossRef] [Scilit]
- Staker, M.R.; Holt, D.L. The dislocation cell size and dislocation density in copper deformed at temperatures between 25 and 700 °C. Acta Metall. 1972, 20, 569–579. [Google Scholar] [CrossRef] [Scilit]
- Gottstein, G. Physical Foundations of Materials Science; Springer: Berlin/Heidelberg, Germany, 2004. [Google Scholar]
- Correia, J.B.; Davies, H.A.; Sellars, C.M. Strengthening in rapidly solidified age hardened Cu-Cr and Cu-Cr-Zr alloys. Acta Mater. 1997, 45, 177–190. [Google Scholar] [CrossRef] [Scilit]
- Gladman, T. Precipitation hardening in metals. Mater. Sci. Technol. 1999, 15, 30–36. [Google Scholar] [CrossRef] [Scilit]
- Davis, J.R. ASM Specialty Handbook: Copper and Copper Alloys; American Technical Publishers Ltd.: Orland Park, IL, USA, 2001. [Google Scholar]
- Meyers, M.A.; Chawla, K.K. Mechanical behavior of materials. Mater. Today 2005, 8, 83–85. [Google Scholar] [CrossRef] [Scilit]
- Zhang, S.R.; Kang, H.J.; Li, R.G.; Zou, C.L.; Guo, E.Y.; Chen, Z.N.; Wang, T.M. Microstructure evolution, electrical conductivity and mechanical properties of dual-scale Cu5Zr/ZrB2 particulate reinforced copper matrix composites. Mater. Sci. Eng. A 2019, 762, 138108. [Google Scholar] [CrossRef] [Scilit]
- Lu, R.; Wang, L.Y.; Wei, H.; Shi, X.L.; Yang, Y.; Xiao, K.Y.; Yang, H.T.; Li, Z.L. Investigation of strengthening mechanisms and conductive behavior of Cu-Ni-Co-Si alloys based on first-principles calculations and experimental verification. J. Alloys Compd. 2026, 1079, 190125. [Google Scholar] [CrossRef] [Scilit]
- Hansen, N. Hall-Petch relation and boundary strengthening. Scr. Mater. 2004, 51, 801–806. [Google Scholar] [CrossRef] [Scilit]
- Wen, H.M.; Topping, T.D.; Isheim, D.; Seidman, D.N.; Lavernia, E.J. Strengthening mechanisms in a high-strength bulk nanostructured Cu-Zn-Al alloy processed via cryomilling and spark plasma sintering. Acta Mater. 2013, 61, 2769–2782. [Google Scholar] [CrossRef] [Scilit]
- Ding, Y.; Xiao, Z.; Fang, M.; Gong, S.; Dai, J. Microstructure and mechanical properties of multi-scale α-Fe reinforced Cu-Fe composite produced by vacuum suction casting. Mater. Sci. Eng. A 2023, 864, 144603. [Google Scholar] [CrossRef] [Scilit]
- Wu, Y.K.; Li, Y.; Lu, J.Y.; Tan, S.; Jiang, F.; Sun, J. Effects of pre-deformation on precipitation behaviors and properties in Cu-Ni-Si-Cr alloy. Mater. Sci. Eng. A 2019, 742, 501–507. [Google Scholar] [CrossRef] [Scilit]
- Su, J.H.; Dong, Q.M.; Liu, P. Research on aging precipitation in a Cu-Cr-Zr-Mg alloy. Mater. Sci. Eng. A 2005, 392, 422–426. [Google Scholar] [CrossRef] [Scilit]
- Yi, Z.; Volinsky, A.A.; Hai, T.T.; Zhe, C.; Ping, L.; Tian, B.H.; Yong, L. Aging behavior and precipitates analysis of the Cu-Cr-Zr-Ce alloy. Mater. Sci. Eng. A 2016, 650, 248–253. [Google Scholar] [CrossRef] [Scilit]
- Han, Z.Y.; Zhou, M.; Jing, K.; Chu, C.H.; Zhang, Y.; Tian, B.H.; Li, Z.A.; He, W.H.; Song, L.H. Effect of Mg addition on the microstructure and mechanical properties of Cu-Ti-Zr alloy. J. Alloys Compd. 2024, 1004, 175897. [Google Scholar] [CrossRef] [Scilit]
- Rafiei, M.; Mirzadeh, H.; Malekan, M.; Sohrabi, M.J. Homogenization kinetics of a typical nickel-based superalloy. J. Alloys Compd. 2019, 793, 277–282. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.