Skip to Content
MaterialsMaterials
  • Article
  • Open Access

24 February 2026

25 Pages

Enhanced Mechanical and Surface Performance of Three-Dimensionally Printed Denture Base Resin via Zinc Oxide and Samarium Oxide Nanoparticle Reinforcement

,
,
,
and
1
Prosthodontics Department, College of Dentistry, Al Muthana University, Samawah 66001, Iraq
2
Prosthodontics Department, College of Dentistry, Al Mustansiriyah University, Baghdad 10001, Iraq
3
Branch of Prosthodontics, College of Dentistry, University of Al-Ameed, Karbala 56001, Iraq
4
Botany and Microbiology Department, Faculty of Science, Tanta University, Tanta 31527, Egypt
This article belongs to the Section Manufacturing Processes and Systems

Abstract

The increasing adoption of digital light processing (DLP) three-dimensional (3D) printing in prosthodontics has enabled the rapid fabrication of denture bases with improved dimensional accuracy and reproducibility. However, the mechanical performance and surface characteristics of 3D-printed denture base resins remain inferior to those of conventional heat-polymerized polymethyl methacrylate (PMMA), limiting their long-term clinical reliability. This study aimed to investigate the effect of incorporating zinc oxide (ZnO) and samarium oxide (Sm2O3) nanoparticles, individually and as hybrid nanofiller systems, on the mechanical and wettability properties of a DLP 3D-printed denture base resin. ZnO and Sm2O3 nanoparticles were incorporated into a photopolymerizable denture base resin at concentrations of 1 and 2 wt.%, producing seven experimental formulations, including a control group. A total of 280 specimens were fabricated using a DLP 3D printer and subjected to standardized post-processing. Nanoparticle dispersion and morphology were examined using field-emission scanning electron microscopy (FE-SEM), while Fourier-transform infrared spectroscopy (FTIR) was employed to assess possible chemical interactions between the nanofillers and the polymer matrix. Mechanical performance was evaluated through impact strength, transverse strength, and flexural strength tests, and surface wettability was assessed using static water contact angle measurements. Statistical analysis was conducted using one-way ANOVA followed by Tukey’s post hoc test (α = 0.05). The results demonstrated that all nanoparticle-reinforced groups exhibited significantly enhanced mechanical properties compared with the unmodified control resin. The incorporation of 1 wt.% nanofillers yielded the most pronounced improvements, with the 1 wt.% ZnO group achieving the highest transverse strength and the 1 wt.% ZnO–Sm2O3 hybrid group exhibiting the maximum flexural strength. Increasing the nanofiller concentration to 2 wt.% resulted in partial reductions in impact and flexural strength, which were attributed to nanoparticle agglomeration and increased light scattering during photopolymerization. FTIR analysis revealed no evidence of chemical bonding between the resin matrix and the nanofillers, indicating that the observed enhancements were primarily governed by physical reinforcement mechanisms. Wettability analysis showed that Sm2O3-containing formulations significantly reduced the water contact angle, indicating increased surface hydrophilicity, whereas ZnO incorporation produced more hydrophobic surfaces. Within the limitations of this in vitro study, the findings suggest that low-concentration incorporation of ZnO and Sm2O3 nanoparticles represents an effective strategy to enhance the mechanical integrity and tailor the surface properties of DLP 3D-printed denture base resins. These results suggest potential clinical relevance of nanoparticle-reinforced printed denture bases, emphasizing the importance of optimized filler loading to avoid agglomeration-induced performance degradation.

1. Introduction

The integration of additive manufacturing (AM) technologies into prosthodontic workflows has profoundly transformed the fabrication of removable dental prostheses, particularly denture bases. Among the available AM techniques, vat photopolymerization—most notably digital light processing (DLP)—has gained widespread adoption due to its high resolution, rapid fabrication, and ability to produce complex geometries with excellent dimensional accuracy [1]. Three-dimensionally printed denture base resins enable streamlined digital workflows, reduced laboratory time, and improved reproducibility compared with conventional fabrication methods. These advantages have positioned three-dimensional printing as a promising alternative to traditional heat-cured polymethyl methacrylate (PMMA) systems for denture base applications. Stereolithography (SLA) and DLP are the two leading vat photopolymerization technologies used in dentistry. Unlike SLA, which cures resin point-by-point using a scanning ultraviolet laser, DLP polymerizes entire layers simultaneously using a projected light source. While SLA can achieve high resolution, it typically requires longer build times, whereas DLP offers clinically acceptable accuracy with significantly shorter fabrication times. Both technologies are employed in dental applications; however, DLP is often preferred for denture base fabrication due to its higher throughput, efficiency, and suitability for larger build volumes [2,3].
Despite these advantages, the mechanical reliability of three-dimensionally printed denture base resins remains a major limitation that restricts their long-term clinical performance. Numerous studies have reported that printed resins exhibit inferior impact strength, fatigue resistance, and long-term dimensional stability compared with heat-polymerized materials, raising concerns regarding fracture susceptibility and service life under functional loading conditions [4,5]. Denture bases are routinely subjected to repetitive masticatory stresses, accidental dropping, and environmental challenges within the oral cavity; therefore, insufficient mechanical strength may compromise clinical durability. Consequently, enhancing the mechanical performance of printed denture base materials without sacrificing their manufacturing advantages has become a critical research priority. One effective strategy to address these limitations involves the incorporation of inorganic nanofillers into polymer matrices. When homogeneously dispersed, nanoparticles can improve load transfer, inhibit crack initiation and propagation, and modify surface characteristics while maintaining acceptable esthetics and processability [6,7]. In dental polymers, nanofiller reinforcement has demonstrated the potential to improve key mechanical properties such as flexural strength, impact resistance, and wear behavior, thereby extending the functional lifespan of prosthetic devices.
Among the various inorganic fillers investigated, metal oxide nanoparticles have attracted considerable attention due to their dual role as mechanical reinforcements and antimicrobial agents. This dual functionality is particularly advantageous for denture base materials, which are susceptible to biofilm accumulation and microbial colonization in the oral environment [8,9]. Zinc oxide nanoparticles have been extensively studied in dental polymer systems and have consistently demonstrated improvements in mechanical properties, surface hardness, and antimicrobial performance. Their favorable biocompatibility, chemical stability, and cost-effectiveness have established zinc oxide as one of the most widely investigated nanofillers for prosthodontic applications. However, the incorporation of nanoparticulate fillers inevitably alters the physicochemical characteristics of the polymer matrix, and these changes may be beneficial or detrimental depending on filler concentration, dispersion quality, and matrix compatibility. Accordingly, systematic evaluation of zinc oxide-modified denture base resin remains essential to ensure that performance enhancements do not compromise material safety, durability, or clinical applicability [10].
In contrast to zinc oxide, samarium oxide and other rare-earth oxides have received limited attention in dental polymer research, despite their well-documented advantages in ceramic and composite systems. Samarium oxide exhibits high hardness, excellent thermal stability, and notable wear resistance—properties that are desirable for reinforcing load-bearing polymer composites [11,12]. These characteristics suggest that samarium oxide may function as an effective reinforcing phase within denture base resins, particularly in applications where resistance to deformation and surface degradation is critical. However, the potential of samarium oxide as a reinforcing nanofiller in dental photopolymers remains largely unexplored. The strategic combination of zinc oxide and samarium oxide as a hybrid nanofiller system offers the possibility of synergistic reinforcement, whereby zinc oxide may contribute antimicrobial activity and surface-related effects, while samarium oxide may enhance mechanical resilience and resistance to localized deformation. Such hybrid nanocomposites have the potential to simultaneously address multiple failure mechanisms of denture bases, including fracture, wear, and surface degradation [13]. Nevertheless, the effectiveness of hybrid nanofillers is strongly dependent on their dispersion, interfacial compatibility, and relative concentration within the polymer matrix.
Effective nanoparticle reinforcement requires uniform dispersion, strong filler–matrix interactions, and optimized filler loading. Excessive nanoparticle agglomeration or weak interfacial adhesion can create stress concentration sites that adversely affect mechanical performance [14,15]. These challenges are further amplified in three-dimensionally printed resins, where additional factors such as photopolymerization kinetics, light scattering by nanoparticles, and reduced curing depth may influence the degree of conversion and polymer network formation. Such effects can directly impact both the mechanical integrity and surface properties of the printed material [16,17]. Therefore, careful optimization of nanofiller concentration is particularly critical for photopolymerizable denture base resins.
Previous investigations have demonstrated that metal oxide nanoparticles—including titanium dioxide, aluminum oxide, and zinc oxide—can enhance flexural strength, surface hardness, and wear resistance of PMMA-based and light-cured dental resins. However, reported outcomes vary considerably depending on particle size, surface treatment, concentration, and incorporation method [18,19,20]. Importantly, comprehensive studies evaluating samarium oxide either alone or in combination with zinc oxide in three-dimensionally printed denture base resins remain scarce. In particular, systematic evaluation of concentration-dependent effects on both mechanical performance and surface wettability in digitally manufactured denture materials is lacking.
Accordingly, the present study aimed to systematically investigate the influence of zinc oxide and samarium oxide nanoparticles, individually and as hybrid nanofillers, on the mechanical and surface properties of a three-dimensionally printed denture base resin. Nanofillers were incorporated at graded concentrations into a commercially available photopolymerizable resin, and their effects on impact strength, transverse strength, flexural strength, and surface wettability were evaluated. The null hypothesis was that incorporation of zinc oxide and samarium oxide nanoparticles, irrespective of concentration, would not produce statistically significant improvements in the mechanical or physical properties of the printed denture base resin compared with the unmodified control material.

2. Materials and Methods

2.1. Study Design

This experimental in vitro study was designed to evaluate the influence of zinc oxide and samarium oxide nanoparticle incorporation on the mechanical and surface properties of a three-dimensionally printed denture base resin. Specimens were fabricated using a desktop three-dimensional printer (Phrozen Sonic Mini 8K S, Phrozen Technology, Hsinchu, Taiwan) operating under digital light processing conditions. A commercially available, biocompatible photopolymer resin specifically formulated for denture base applications (3D FLEXO Denture Base Resin, Senertek, İzmir, Turkey) was used as the polymer matrix throughout the study.
Zinc oxide nanoparticles with a nominal particle size range of 10–30 nm and samarium oxide nanoparticles with particle sizes below 100 nm were obtained from a commercial supplier (Skyspring Nanomaterials, Inc., Houston, TX, USA). The nanoparticles were incorporated into the uncured denture base resin at concentrations of 1 and 2 wt.%, either individually or as hybrid nanocomposites containing equal proportions of zinc oxide and samarium oxide at the same total filler loadings. These concentrations were selected based on previous reports indicating that low nanofiller loadings are most effective for improving mechanical performance while minimizing nanoparticle agglomeration and interference with photopolymerization in light-cured resins [21]. To achieve homogeneous nanoparticle dispersion, the calculated quantities of nanoparticles were gradually introduced into the liquid resin matrix and mixed using a high-speed planetary mixer (DAC 150.1 FVZ, Hauschild Engineering, Hamm, Germany) at 3500 rpm for 2 min. This standardized mixing protocol was applied to reduce nanoparticle agglomeration and ensure consistent filler distribution across all experimental formulations. Following mixing, all resin–nanoparticle mixtures were stored at 23 °C in a dark environment prior to printing to prevent premature photopolymerization and maintain material stability [21]. Specimen fabrication was performed using a 405 nm LED light source, with a layer thickness of 50 µm and an exposure time of 3 s per layer, in accordance with the manufacturer’s recommendations. All specimens were printed using the same build orientation (90°) and identical exposure parameters to minimize processing variability. After printing, specimens were cleaned with isopropyl alcohol to remove residual uncured resin, followed by post-curing for 30 min using a 405 nm light-curing unit, as recommended for denture base materials [22]. Post-curing was performed to ensure sufficient polymerization and to enhance mechanical properties and surface stability.
A total of 280 specimens were fabricated and distributed according to the intended testing protocols. Of these, 210 specimens were allocated for mechanical testing, while 70 specimens were prepared for surface wettability assessment using the water contact angle test. Seven experimental groups were established, with ten specimens per group for each test condition (n = 10). Group I served as the unmodified control resin. Group II contained 1 wt.% zinc oxide nanoparticles, while Group III contained 2 wt.% zinc oxide nanoparticles. Group IV incorporated 1 wt.% samarium oxide nanoparticles, and Group V incorporated 2 wt.% samarium oxide nanoparticles. Group VI consisted of a hybrid nanocomposite containing 1 wt.% total filler composed of zinc oxide and samarium oxide, whereas Group VII incorporated a 2 wt.% hybrid zinc oxide–samarium oxide nanocomposite.
Sample size determination was performed using G*Power statistical software (version 3.1.9.7). The analysis was based on seven experimental groups, with a statistical power of 85%, an alpha error probability of 0.05, and a medium effect size of 0.3. Based on these parameters, a minimum sample size of ten specimens per group was determined to be sufficient to detect statistically significant differences among the groups.

2.2. Samples Preparation

Zinc oxide and samarium oxide nanopowders were accurately weighed using an electronic analytical balance with a precision of 0.01 mg to ensure precise control of filler loading. The required quantities of nanoparticles were gradually incorporated into the liquid denture base resin to minimize agglomeration and promote uniform dispersion. Mixing was performed using a speed mixer to obtain a homogeneous resin–nanoparticle suspension free from visible particle clustering. To further enhance dispersion, a two-step mixing protocol was employed. Initially, half of the predetermined nanoparticle mass was incorporated into the resin and mixed at 2000 rpm for 5 min. The remaining half of the nanoparticle powder was then added to the partially mixed resin and subjected to an additional mixing cycle under identical conditions. This staged incorporation approach was adopted to reduce the likelihood of nanoparticle agglomeration, particularly at higher filler loadings, and to ensure consistent distribution throughout the resin matrix [23]. Following mixing, the prepared nanocomposite resins were poured into the printer resin tray and immediately used for specimen fabrication.
For the control, 1 wt.%, and 2 wt.% experimental groups, nanoparticle masses of 0.0 g, 2.5 g, and 5.0 g, respectively, were incorporated into the resin formulations. Specimens of different geometries were designed and fabricated according to the specific requirements of each experimental test. Rectangular bar-shaped specimens measuring 64 mm in length, 10 mm in width, and 3.3 mm in thickness were prepared for transverse strength and flexural strength testing in accordance with established standards [22]. Disk-shaped specimens with a diameter of 10 mm and a thickness of 2 mm were fabricated for surface wettability assessment using the water contact angle method [24]. For impact strength evaluation, rectangular specimens measuring 80 mm in length, 10 mm in width, and 4 mm in thickness were prepared.
All specimens were fabricated using a three-dimensional printing process with a fixed layer thickness of 50 μm and a build orientation of 0°. Each layer was exposed for approximately 3 s using a 405 nm LED light engine with a projector intensity of approximately 10–15 mW/cm2, in accordance with the manufacturer’s recommendations. Upon completion of printing, specimens were carefully removed from the build platform and cleaned with isopropyl alcohol to eliminate residual uncured resin. The cleaned specimens were then post-cured in a UV curing chamber (Phrozen Cure Series, Phrozen Technology, Hsinchu, Taiwan) equipped with 405 nm LEDs at an irradiance of approximately 20 mW/cm2 for 30 min to ensure complete polymerization and stabilization of the printed structures [25]. Following post-curing, all specimens were polished using a water-cooled rotary polishing system to standardize surface conditions prior to mechanical, morphological, and wettability testing.

2.3. Characterization and Testing Methods

2.3.1. Morphological Characterization

The surface morphology and microstructural features of the three-dimensionally printed denture base resin, with and without nanoparticle reinforcement, were examined using field-emission scanning electron microscopy (FE-SEM; Inspect F50, FEI Company, Eindhoven, The Netherlands). Representative specimens from each experimental group were selected to ensure that the observed microstructural features were representative of overall material behavior rather than localized artifacts. Prior to SEM analysis, specimens were rinsed with distilled water and subsequently cleaned by ultrasonic agitation for 5 min to remove surface debris and residual contaminants. The samples were then air-dried at room temperature for 24 h to eliminate surface moisture. Dried specimens were sputter-coated with a gold conductive layer approximately 5–10 nm thick using a vacuum sputter coater to prevent charging during imaging. SEM observations were performed under high-vacuum conditions with an accelerating voltage of 5–10 kV. The applied preparation protocol was selected to preserve surface features while ensuring sufficient conductivity and image resolution for evaluating nanoparticle dispersion, surface morphology, and agglomeration behavior.
FE-SEM imaging was conducted to qualitatively evaluate the dispersion state of zinc oxide and samarium oxide nanoparticles within the polymer matrix, with particular attention given to the degree of nanoparticle embedding, interfacial continuity between the fillers and the resin, and the presence of surface features such as polishing traces or nanoparticle protrusions. The examination also focused on identifying potential agglomeration phenomena, especially in specimens containing higher nanofiller loadings, as nanoparticle clustering can act as stress concentration sites and negatively influence mechanical performance.
The morphological observations obtained from FE-SEM analysis were used to establish correlations between nanofiller distribution and the measured mechanical and surface properties. Uniformly dispersed and well-embedded nanoparticles are expected to promote effective load transfer and crack deflection mechanisms, whereas poorly dispersed or agglomerated nanoparticles may disrupt the polymer network and compromise structural integrity. Additionally, surface-related features observed at the microscale were considered in relation to wettability behavior, as exposed nanoparticles and surface heterogeneities can influence surface energy and water contact angle measurements. Overall, FE-SEM analysis provided critical microstructural insight necessary for interpreting the concentration-dependent effects of zinc oxide and samarium oxide nanoparticles on the performance of the printed denture base resin.

2.3.2. Fourier Transform Infrared Spectroscopy (FTIR) Analysis

Fourier transform infrared spectroscopy was employed to investigate potential chemical interactions between the denture base resin matrix and the incorporated zinc oxide and samarium oxide nanoparticles. FTIR analysis was performed using an infrared spectrometer (Tensor 27, Bruker Optics GmbH, Ettlingen, Germany) to obtain absorption spectra characteristic of the molecular structure of the polymer matrix before and after nanoparticle incorporation. Measurements were conducted over the relevant spectral range to identify functional groups associated with the photopolymerizable resin and to detect any changes induced by the presence of inorganic nanofillers. The acquired FTIR spectra were carefully analyzed to identify characteristic absorption bands corresponding to the functional groups of the resin matrix, such as carbonyl, ester, and aliphatic groups. Particular attention was paid to the position, intensity, and shape of these bands, as shifts in peak positions or the emergence of new absorption features may indicate chemical interactions, such as covalent bonding or coordination between the polymer chains and nanoparticle surfaces. Comparisons were made between the spectra of the unmodified control resin and those of the nanoparticle-reinforced formulations to determine whether nanofiller incorporation altered the chemical structure of the resin.
The FTIR spectra obtained from all experimental groups served as molecular “fingerprints” of the corresponding formulations, enabling differentiation between chemical and physical reinforcement mechanisms. The absence of new absorption bands or significant peak shifts would indicate that the nanoparticles were physically embedded within the polymer matrix without participating in chemical reactions, whereas observable spectral changes would suggest chemical modification of the resin network. Consequently, FTIR analysis provided essential insight into the nature of the filler–matrix interaction and supported interpretation of the mechanical and surface property results by clarifying whether observed enhancements were attributable to chemical bonding or predominantly physical reinforcement effects.

2.4. Mechanical Testing

2.4.1. Impact Strength Test

Impact strength was evaluated using a Charpy impact testing method to assess the resistance of the printed denture base materials to sudden fracture. Prior to testing, all impact specimens were immersed in distilled water at 37 °C for 48 h to simulate intraoral conditions and water absorption effects [26].
Impact testing was conducted using a Charpy impact testing instrument (Beijing Time Vision Al Instrument Ltd., Beijing, China) with unnotched specimens. Each specimen was positioned horizontally and subjected to impact by a freely swinging pendulum with a maximum energy of 5 J. The absorbed energy required to fracture the specimen was recorded directly from the instrument scale. Impact strength was calculated using the following equation [27]:
Impact Strength = (E/B × D) × 103
where E is the absorbed energy at fracture (J), B is the specimen width (mm), and D is the specimen thickness (mm). The resulting impact strength values were expressed in kJ/m2.

2.4.2. Transverse Strength Test

To simulate oral environmental conditions, transverse strength specimens were immersed in distilled water at 37 °C for 48 h prior to testing [28]. Transverse strength testing was performed using a universal testing machine (Instron CZL203, Instron Corporation, Norwood, MA, USA) equipped with a 10 kN load cell. Specimens were positioned on a three-point bending fixture with a support span of 50 mm and loaded at a crosshead speed of 1 mm/min until fracture occurred. Transverse strength (σ, MPa) was calculated using the following equation [28]:
Transverse Strength = 3PL/2bd2
where P is the applied load at fracture (N), L is the support span length (50 mm), b is the specimen width (mm), and d is the specimen thickness (mm).

2.4.3. Flexural Strength Test

Flexural strength testing was conducted in accordance with ISO 178:2019 using a three-point bending configuration [29]. Specimens were tested on a universal testing machine (Instron CZL203, Instron Corporation, Norwood, MA, USA) equipped with a 10 kN load cell, with a support span of 53 mm and a crosshead speed of 0.5 mm/min. The test was performed until fracture occurred. Flexural strength (σ, MPa) was calculated using the following equation [29]:
Flexural Strength (FS) = 3PL/2Wt2
where P is the fracture load (N), L is the support span length (mm), W is the specimen width (mm), and t is the specimen thickness (mm).

2.5. Surface Wettability Measurement

Surface wettability of the printed denture base resin specimens was evaluated by measuring the static water contact angle using the sessile drop technique. Contact angle measurements were performed using a contact angle goniometer (Si-Plasma CAM 110, Creating Nano Technologies, Hsinchu, Taiwan), which enables quantitative assessment of surface wetting behavior. Measurements were conducted in accordance with ISO 19403-2:2024 for contact angle (sessile drop) analysis [30]. Prior to testing, specimens were conditioned for 24 h at 23 ± 2 °C and approximately 45% relative humidity. Contact angle measurements were performed under controlled ambient conditions (23 ± 2 °C, 40–50% relative humidity) to minimize environmental variability. Each specimen was positioned horizontally at the center of the measurement platform to ensure consistent droplet placement and accurate angle determination. A calibrated sterile syringe was used to dispense a distilled water droplet with a controlled volume of 4 µL onto the specimen surface. Care was taken to deposit the droplet gently to avoid dynamic effects such as splashing or droplet deformation. Images of the droplet profile were captured immediately after deposition to minimize the influence of evaporation or liquid absorption by the material surface. The static contact angle was determined by measuring the angles formed between the tangent to the water droplet and the specimen surface on both the left and right sides of the droplet. The mean value of the two measurements was calculated and recorded as the final contact angle for each specimen. This averaging approach was employed to reduce measurement variability and improve accuracy [24]. Contact angle measurements provided insight into the influence of nanoparticle incorporation on surface wettability, which is a clinically relevant parameter affecting saliva spreading, denture retention, and potential microbial adhesion on denture base materials.

2.6. Statistical Analysis

All experimental data were compiled and initially processed using Microsoft Excel (Microsoft Excel, Microsoft Corporation, Redmond, WA, USA). Statistical analysis was subsequently performed using the Statistical Package for the Social Sciences (SPSS, version 25.0, IBM Corp., Armonk, NY, USA). Descriptive statistics, including mean values and standard deviations, were calculated for all measured parameters. Inferential statistical analysis was conducted to evaluate differences among the experimental groups. One-way analysis of variance (ANOVA) was applied to determine whether statistically significant differences existed between group means. When the ANOVA indicated significant differences, post hoc multiple comparisons were performed using Tukey’s honestly significant difference (HSD) test to identify specific intergroup differences. The level of statistical significance was set at α = 0.05 for all analyses.

3. Results

The outcomes of all experimental evaluations performed to assess the influence of nanoparticle incorporation on the properties of the 3D-printed denture base resin are discussed. Data are organized according to the principal analytical domains, including morphological characterization, chemical assessment, mechanical performance, and surface wettability. Statistical analyses were applied to determine the significance of differences among the tested groups. The following subsections provide a structured presentation of these findings, highlighting the comparative behavior of the modified and unmodified materials.
Representative field-emission scanning electron microscopy micrographs of the three-dimensionally printed denture base resin specimens are presented in (Figure 1). The micrographs illustrate the surface morphology of the unmodified control group and the nanoparticle-reinforced groups containing zinc oxide, samarium oxide, and hybrid zinc oxide–samarium oxide fillers at concentrations of 1 wt.% and 2 wt.%. The surface of the control group (Figure 1a) exhibited a relatively uniform morphology characterized by pronounced polishing traces and a smooth polymeric matrix without visible particulate features. No embedded or protruding particulate structures were observed, indicating the absence of inorganic fillers and confirming the homogeneous nature of the unmodified resin surface following post-processing and polishing procedures. In contrast, specimens containing 1 wt.% zinc oxide nanoparticles (Figure 1b) displayed the presence of finely distributed nanoscale features embedded within the polymer matrix. The surface appeared generally uniform, with polishing traces still evident, although partially interrupted by dispersed nanoparticle inclusions. Similar morphological characteristics were observed for the 1 wt.% samarium oxide group (Figure 1d), where nanoscale particulate features were visible and appeared to be well integrated within the resin surface, without the formation of large clusters or surface discontinuities.
Figure 1. Field-emission scanning electron microscopy (FE-SEM) images showing the surface morphology of the three-dimensionally printed denture base resin: (a) control group without nanoparticle reinforcement; (b) 1 wt.% ZnO; (c) 2 wt.% ZnO; (d) 1 wt.% Sm2O3; (e) 2 wt.% Sm2O3; (f) 1 wt.% hybrid ZnO–Sm2O3 nanocomposite; and (g) 2 wt.% hybrid ZnO–Sm2O3 nanocomposite.
Specimens incorporating 2 wt.% nanoparticle concentrations exhibited more pronounced surface features. The 2 wt.% zinc oxide group (Figure 1c) demonstrated a higher density of visible particulate structures compared with the corresponding 1 wt.% group. Discrete nanoparticle agglomerates were occasionally observed, appearing as localized clusters protruding slightly from the polymer surface. A comparable trend was noted in the 2 wt.% samarium oxide group (Figure 1e), where increased nanoparticle content resulted in more frequent particle-rich regions and reduced visibility of polishing traces. The hybrid nanocomposite groups containing both zinc oxide and samarium oxide nanoparticles exhibited distinct morphological features. The 1 wt.% hybrid group (Figure 1f) showed a relatively homogeneous surface with evenly distributed nanoscale features embedded within the polymer matrix. Polishing marks remained visible but were partially masked by the presence of the hybrid filler system. In contrast, the 2 wt.% hybrid group (Figure 1g) displayed more evident particle accumulation, with clustered regions appearing more frequently across the surface. These clusters were visually distinguishable from the surrounding matrix and appeared as raised features interrupting the otherwise continuous polymer surface.
Overall, FE-SEM analysis revealed clear differences in surface morphology as a function of nanoparticle type and concentration. Lower nanofiller concentrations were associated with more uniformly distributed nanoscale features, whereas higher concentrations resulted in increased particle visibility and localized clustering. These morphological variations provide a microstructural basis for comparison with the mechanical and surface property results reported in subsequent sections.
The Fourier transform infrared spectra of the unmodified control group and all nanoparticle-reinforced denture base resin groups are presented in (Figure 2). The spectra of all experimental formulations exhibited similar overall profiles across the scanned wavenumber range, indicating that the fundamental chemical structure of the polymer matrix was preserved following nanoparticle incorporation. The control group (Group I) displayed characteristic absorption bands consistent with the PMMA-based denture resin. Prominent peaks were observed in the region of approximately 2950–2850 cm−1, corresponding to aliphatic C–H stretching vibrations, along with a strong absorption band near 1720 cm−1 attributed to the ester carbonyl (C=O) stretching vibration. Additional absorption features were observed in the range of 1450–1380 cm−1, associated with C–H bending vibrations, and in the fingerprint region between approximately 1250 and 900 cm−1, corresponding to C–O–C stretching vibrations of the ester groups. The FTIR spectra of the nanoparticle-reinforced groups (Groups II–VII) exhibited absorption bands at positions comparable to those of the control group.
Figure 2. Fourier transform infrared (FTIR) spectra of the unmodified control denture base resin and nanoparticle-reinforced resins containing ZnO, Sm2O3, and hybrid ZnO–Sm2O3 at different concentrations.
No additional peaks or disappearance of characteristic PMMA absorption bands were observed in any of the experimental formulations containing zinc oxide, samarium oxide, or hybrid zinc oxide–samarium oxide nanoparticles at either 1 wt.% or 2 wt.% concentrations. The overall spectral patterns of all nanoparticle-containing groups remained closely aligned with that of the unmodified resin. Minor variations in peak intensity were observed among the experimental groups, particularly within the fingerprint region; however, the positions of the major absorption bands remained unchanged across all formulations. These observations indicate that the incorporation of nanoparticles did not result in detectable chemical modifications to the polymer backbone or the formation of new chemical bonds within the resin matrix. The FTIR results, therefore, confirm that the nanoparticle-reinforced materials maintained the same chemical identity as the control resin, with nanofillers incorporated as a secondary phase within the polymer matrix.
The impact strength values obtained for the control and nanoparticle-reinforced denture base resin groups are presented in Figure 3, with the corresponding numerical data summarized in Table 1. Statistical analysis using one-way ANOVA revealed highly significant differences among the experimental groups (p < 0.001). The unmodified control group (Group I) exhibited a mean impact strength of 8.578 ± 0.289 kJ/m2 and served as the baseline for comparison. As illustrated in Figure 3, all groups containing 1 wt.% nanofiller demonstrated higher impact strength values than the control group, indicating a consistent improvement in resistance to sudden impact loading at low filler concentrations. Group II (1 wt.% zinc oxide) recorded the highest mean impact strength (10.002 ± 0.336 kJ/m2), followed by Group IV (1 wt.% samarium oxide) and Group VI (1 wt.% hybrid zinc oxide–samarium oxide), with mean values of 9.694 ± 0.328 kJ/m2 and 9.496 ± 0.319 kJ/m2, respectively. This trend reflects the effectiveness of low nanofiller loading in enhancing energy absorption and stress transfer within the polymer matrix when nanoparticle dispersion is maintained. In contrast, Figure 3 also shows that increasing the nanofiller concentration to 2 wt.% resulted in lower impact strength values compared with the corresponding 1 wt.% formulations. Group III (2 wt.% zinc oxide) and Group VII (2 wt.% hybrid nanocomposite) exhibited mean impact strengths of 8.085 ± 0.478 kJ/m2 and 8.021 ± 0.270 kJ/m2, respectively, while the lowest impact strength was observed in Group V (2 wt.% samarium oxide), with a mean value of 7.453 ± 0.251 kJ/m2. The reduction in impact resistance at higher filler concentrations suggests the onset of nanoparticle agglomeration, which can act as stress concentration sites and limit effective energy dissipation during impact loading. Despite these reductions, statistically significant differences were observed among all experimental groups, confirming a strong concentration-dependent effect of nanoparticle incorporation on the impact behavior of three-dimensionally printed denture base resins.
Figure 3. Impact strength of control and nanoparticle-reinforced three-dimensionally printed denture base resin groups. Data are expressed as mean ± standard deviation.
Table 1. Descriptive statistics (mean ± standard deviation) and one-way ANOVA results for impact strength, transverse strength, and flexural strength of the control and nanoparticle-reinforced three-dimensionally printed denture base resin groups.
The transverse strength behavior of the control and nanoparticle-reinforced three-dimensionally printed denture base resin groups is illustrated in Figure 4, with the corresponding numerical data summarized in Table 1. One-way ANOVA revealed statistically significant differences among the tested groups (p = 0.015). The unmodified control group exhibited a mean transverse strength of 85.78 ± 2.89 MPa and served as the reference for comparison. As shown in Figure 4, all nanoparticle-reinforced formulations demonstrated transverse strength values exceeding that of the control material, confirming the reinforcing effect of inorganic nanofillers under static bending conditions. Among the experimental groups, the highest transverse strength was observed in Group II (1 wt.% zinc oxide), followed closely by Group VI (1 wt.% hybrid zinc oxide–samarium oxide) and Group IV (1 wt.% samarium oxide). This trend indicates that low nanofiller loading promotes efficient load transfer within the polymer matrix when nanoparticle dispersion is adequately maintained. In contrast, specimens containing 2 wt.% nanofiller exhibited comparatively lower transverse strength values than their corresponding 1 wt.% formulations, as evident in Figure 4. Group V (2 wt.% samarium oxide) and Group III (2 wt.% zinc oxide) showed moderate reductions, while Group VII (2 wt.% hybrid nanocomposite) displayed a transverse strength value approaching that of the control group. These findings suggest that excessive nanoparticle incorporation may reduce reinforcement efficiency, likely due to increased agglomeration and disruption of matrix continuity. Nevertheless, most nanoparticle-containing groups maintained transverse strength values above that of the unmodified resin, indicating an overall beneficial effect of nanoparticle reinforcement when applied at optimized concentrations.
Figure 4. Transverse strength of control and nanoparticle-reinforced three-dimensionally printed denture base resin groups. Data are presented as mean ± standard deviation.
The flexural strength behavior of the control and nanoparticle-reinforced three-dimensionally printed denture base resin groups is presented in Figure 5, with the corresponding numerical values summarized in Table 1. Statistical analysis revealed highly significant differences among the experimental groups (p < 0.001). The unmodified control group exhibited a mean flexural strength of 108.00 ± 3.63 MPa and served as the reference for comparison. As illustrated in Figure 5, incorporation of nanoparticles at low concentrations resulted in a clear enhancement of flexural strength relative to the control material. Among all formulations, Group VI (1 wt.% hybrid zinc oxide–samarium oxide) exhibited the highest flexural strength, indicating a favorable synergistic effect between the two oxide fillers under bending conditions. Groups IV (1 wt.% samarium oxide) and II (1 wt.% zinc oxide) also demonstrated increased flexural strength compared with the control, confirming the reinforcing potential of single-oxide systems at optimized filler loadings. In contrast, Figure 5 shows that increasing the nanofiller concentration to 2 wt.% led to a reduction in flexural strength across all filler types. Group III (2 wt.% zinc oxide) and Group VII (2 wt.% hybrid nanocomposite) exhibited moderate decreases relative to their corresponding 1 wt.% formulations, while the lowest flexural strength was observed in Group V (2 wt.% samarium oxide). This systematic decline at higher filler concentrations suggests reduced reinforcement efficiency, likely associated with nanoparticle agglomeration and disruption of matrix continuity under tensile–compressive stress gradients. Nevertheless, all tested groups maintained flexural strength values exceeding the minimum requirements specified for denture base polymers, indicating that the observed differences reflect optimization of material performance rather than structural inadequacy.
Figure 5. Flexural strength of control and nanoparticle-reinforced three-dimensionally printed denture base resin groups. Data are presented as mean ± standard deviation.
Intergroup comparisons of mechanical properties were further analyzed using Tukey’s post hoc test, and the results are summarized in Table 2. The post hoc analysis enabled pairwise comparisons between all experimental groups for impact strength, transverse strength, and flexural strength, allowing identification of statistically significant differences following the one-way ANOVA results. For impact strength, the Tukey test revealed statistically significant differences (p < 0.05) among the majority of group comparisons. The largest mean difference was observed between Group II (1 wt.% zinc oxide) and Group V (2 wt.% samarium oxide). Statistically significant differences were detected between Group II and all other groups. Comparisons involving the control group (Group I) also demonstrated statistically significant differences with all experimental groups. An exception was observed between Group III (2 wt.% zinc oxide) and Group VII (2 wt.% hybrid zinc oxide–samarium oxide), where no statistically significant difference was detected (p > 0.05). This indicates comparable impact strength values between these two groups based on the post hoc analysis.
Table 2. Pairwise intergroup comparison of mechanical tests among various groups using a post hoc (Tukey) test for impact strength, transverse strength, and flexural strength of the control and nanoparticle-reinforced three-dimensionally printed denture base resin groups.
Post hoc analysis of transverse strength data demonstrated statistically significant differences (p < 0.05) for most intergroup comparisons, as shown in Table 2. The greatest mean difference in transverse strength was observed between Group II (1 wt.% zinc oxide) and Group VII (2 wt.% hybrid nanocomposite). Comparisons between the control group (Group I) and the majority of nanoparticle-reinforced groups showed statistically significant differences. However, no statistically significant difference was observed between Group I and Group VII. Additionally, comparisons between Group IV (1 wt.% samarium oxide) and Group VI (1 wt.% hybrid nanocomposite), as well as between Group V (2 wt.% samarium oxide) and Group VII (2 wt.% hybrid nanocomposite), did not show statistically significant differences.
The Tukey post hoc test for flexural strength revealed multiple statistically significant pairwise differences among the experimental groups (p < 0.05), as summarized in Table 2. The largest mean difference was observed between Group II (1 wt.% zinc oxide) and Group V (2 wt.% samarium oxide). Statistically significant differences were detected between the control group (Group I) and Group IV (1 wt.% samarium oxide). In contrast, no statistically significant differences were observed between Group III (2 wt.% zinc oxide) and the control group or between Group V (2 wt.% samarium oxide) and Group VII (2 wt.% hybrid nanocomposite). These findings indicate overlapping flexural strength values among these specific group pairs according to the post hoc analysis.
The surface wettability behavior of the control and nanoparticle-reinforced three-dimensionally printed denture base resin groups is presented in Figure 6, with descriptive statistics and one-way ANOVA results summarized in Table 3. One-way ANOVA revealed statistically significant differences in water contact angle among the experimental groups (F = 29.501, p < 0.001). The unmodified control group (Group I) exhibited a mean contact angle of 73.72 ± 1.65°, which served as the baseline for comparison. As shown in Figure 6 and Table 3, incorporation of zinc oxide nanoparticles resulted in increased water contact angle values relative to the control material. Group II (1 wt.% zinc oxide) exhibited a mean contact angle of 77.21 ± 1.34°, while Group III (2 wt.% zinc oxide) showed the highest mean contact angle among all groups (79.44 ± 1.92°), indicating a concentration-dependent increase in surface hydrophobicity with increasing zinc oxide content. In contrast, specimens reinforced with samarium oxide nanoparticles demonstrated lower contact angle values compared with the control. Group IV (1 wt.% samarium oxide) exhibited a mean contact angle of 69.55 ± 3.76°, while Group V (2 wt.% samarium oxide) recorded the lowest mean contact angle (65.59 ± 3.45°), indicating a concentration-dependent increase in surface hydrophilicity with samarium oxide incorporation. The hybrid nanocomposite groups displayed intermediate wettability behavior. Group VI (1 wt.% hybrid zinc oxide–samarium oxide) exhibited a mean contact angle of 71.92 ± 2.41°, whereas Group VII (2 wt.% hybrid formulation) showed a value of 69.82 ± 2.18°. These values were lower than those of the zinc oxide-only groups and closer to the samarium oxide-reinforced specimens, reflecting the combined influence of both oxides on surface wettability. Overall, the results demonstrate that nanoparticle type and concentration exert a significant and opposing influence on surface wettability, as confirmed by the statistically significant ANOVA outcomes.
Figure 6. Water contact angle of control and nanoparticle-reinforced three-dimensionally printed denture base resin groups. Data are presented as mean ± standard deviation.
Table 3. Descriptive statistics (mean ± standard deviation) and one-way ANOVA results for water contact angle values of the control and nanoparticle-reinforced three-dimensionally printed denture base resin groups.
Pairwise intergroup comparisons of water contact angle values were performed using Tukey’s post hoc test, and the results are summarized in Table 4. The analysis identified statistically significant differences (p < 0.05) among several group comparisons, providing further resolution of the differences observed in the one-way ANOVA. Comparisons involving the control group (Group I) revealed statistically significant differences with Group II (1 wt.% zinc oxide) and Group III (2 wt.% zinc oxide), with mean differences of −4.489° and −6.717°, respectively. In contrast, no statistically significant differences were observed between the control group and Groups IV, VI, or VII. The comparison between Group I and Group V also did not reach statistical significance. Comparisons among zinc oxide-reinforced groups indicated no statistically significant difference between Group II (1 wt.% zinc oxide) and Group III (2 wt.% zinc oxide). However, Group II exhibited statistically significant differences when compared with Groups IV, V, VI, and VII. Similarly, Group III showed statistically significant differences with all samarium oxide-containing and hybrid nanocomposite groups. Within the samarium oxide-reinforced and hybrid nanocomposite groups, statistically significant differences were observed between Group IV (1 wt.% samarium oxide) and Group V (2 wt.% samarium oxide). No statistically significant differences were detected between Group IV and Group VI, or between Group IV and Group VII. Additionally, the comparison between Group V and Group VII did not reach statistical significance. No statistically significant difference was observed between Group VI and Group VII. Overall, the post hoc analysis demonstrated that surface wettability differences were strongly dependent on nanoparticle type and concentration, with multiple statistically significant pairwise differences identified among the experimental groups, as detailed in Table 4.
Table 4. Pairwise intergroup comparisons for water contact angle values of the control and nanoparticle-reinforced three-dimensionally printed denture base resin groups using Tukey’s post hoc test. Statistically significant differences were determined at p < 0.05.

4. Discussion

The present study demonstrated that the incorporation of zinc oxide and samarium oxide nanoparticles into a three-dimensionally printed denture base resin resulted in concentration-dependent changes in mechanical performance and surface wettability, while preserving the chemical identity of the resin matrix [1]. Most studies on denture base reinforcement have focused on commonly employed metal oxides, including ZnO, TiO2, ZrO2, and SiO2, which improve mechanical properties primarily through stress transfer mechanisms, crack arrest, and restriction of polymer chain mobility within the polymer matrix [31]. In contrast, the present work incorporates samarium oxide (Sm2O3), which differs from conventional metal oxides in electronic structure, refractive index, and surface chemistry, as well as reported electrochemical properties that may influence interactions with the photopolymerized resin matrix. These characteristics can affect not only mechanical reinforcement but also light–matter interactions during polymerization and the development of the filler–matrix interphase [32].
Fourier transform infrared spectroscopy confirmed that nanoparticle incorporation did not generate new absorption bands, indicating that reinforcement occurred predominantly through physical rather than chemical interactions. These findings are consistent with recent reports demonstrating that low, well-controlled nanoparticle loadings can enhance the performance of additively manufactured dental resins, whereas higher concentrations may lead to diminished or adverse effects due to dispersion-related limitations and interference with photopolymerization [1].
Field-emission scanning electron microscopy revealed distinct differences in surface micromorphology as a function of nanoparticle type and concentration. All specimens exhibited polishing marks consistent with the applied post-processing protocol; however, clear variations in nanoparticle distribution were observed among experimental groups. Specimens containing 1 wt.% nanofiller demonstrated relatively uniform nanoparticle dispersion within the polymer matrix, with limited surface protrusion and good interfacial integration. In contrast, specimens containing 2 wt.% nanofiller—particularly the hybrid ZnO–Sm2O3 formulation—exhibited visible nanoparticle clustering and localized agglomerates. These features indicate reduced homogeneity and less effective incorporation of nanofillers at higher concentrations. Similar dispersion-related challenges have been widely reported in polymer nanocomposites, where increased filler loading promotes particle–particle interactions that exceed matrix–particle interactions, leading to agglomeration [33]. The control group, which lacked particulate reinforcement, exhibited more pronounced polishing traces due to the absence of embedded nanofillers. These observations highlight the critical role of filler concentration in maintaining uniform dispersion in printed photopolymer systems.
FTIR analysis further revealed that the spectral profiles of nanoparticle-reinforced resins closely matched those of the unmodified control material, with no additional peaks or shifts indicative of chemical bonding or polymer degradation. This confirms that neither ZnO nor Sm2O3 nanoparticles chemically reacted with the resin matrix during formulation or photopolymerization. Taken together with the FE-SEM observations, these results indicate that reinforcement was achieved primarily through physical mechanisms, including nanoparticle embedding and microstructural modification, rather than chemical coupling. At low nanofiller concentrations, uniform dispersion was achieved without altering the polymer’s chemical structure. At higher concentrations, visible agglomeration may introduce localized variations in polymer–particle interactions, potentially influencing spectral intensity or peak definition without generating new chemical species [34]. The uniform dispersion observed at 1 wt.% likely enabled effective load transfer and crack deflection, leading to the measured improvements in mechanical strength. In contrast, the agglomerates observed at 2 wt.%—particularly in hybrid formulations—likely acted as stress concentrators, explaining the reduced toughness and flexural strength in these groups. These findings are consistent with established nanocomposite reinforcement mechanisms.
Mechanical testing revealed a clear concentration-dependent response across all measured properties. Impact strength was maximized in the 1 wt.% ZnO group and decreased in formulations containing higher samarium oxide content. This trend aligns with multiple studies reporting initial improvements in toughness at low nanoparticle loadings, followed by reductions at higher concentrations due to agglomeration and stress concentration effects [33,35]. Similar behavior has been reported for various metal oxide fillers incorporated into both heat-cured PMMA and photocurable resins, where optimal mechanical performance is typically achieved at loadings at or below approximately 1 wt.% [23]. All nanoparticle-reinforced groups exhibited increased transverse strength compared with the control, with the greatest improvement observed for the 1 wt.% ZnO formulation.
Flexural strength reached its maximum value in the 1 wt.% hybrid ZnO–Sm2O3 group, indicating a beneficial interaction between the two nanofiller types. Comparable enhancements in flexural behavior have been reported for low concentrations of ZnO, TiO2, and other ceramic fillers in additively manufactured dental resins, where improvements are attributed to enhanced load transfer and crack resistance when dispersion is adequate [23]. According to ISO 20795-1:2013, denture base polymers must achieve a minimum flexural strength of 65 MPa [36]. All formulations evaluated in the present study, including the unmodified control, exceeded this threshold (approximately 85–113 MPa), indicating compliance with ISO requirements and further enhancement through nanoparticle reinforcement. ADA Specification No. 12 establishes similar criteria (flexural strength ≥ 65 MPa), supporting the clinical relevance of the observed improvements.
The superior flexural performance of the 1 wt.% hybrid formulation suggests a synergistic effect arising from the combined presence of ZnO and Sm2O3 nanoparticles. While ZnO contributes stiffness and surface-related functionality, Sm2O3 may enhance hardness and resistance to localized deformation. Effective synergy likely depends on particle size distribution, homogeneous dispersion, and sufficient interparticle spacing to prevent agglomeration. Similar benefits of hybrid filler systems have been reported in PMMA-based composites incorporating combinations of metal oxides and functional nanoparticles [37]. Unlike more extensively studied oxides such as TiO2 or ZrO2, Sm2O3 has received limited investigation in dental photopolymers, and its incorporation in the present study highlights its potential as a complementary reinforcing phase with distinct optical and surface-related effects.
Surface wettability analysis revealed that ZnO-containing groups exhibited higher contact angles, indicating increased surface hydrophobicity, whereas Sm2O3-containing groups displayed lower contact angles, corresponding to increased hydrophilicity. Previous studies have shown that ZnO incorporation into PMMA can increase hydrophobicity and influence early salivary protein adsorption and microbial adhesion patterns [38,39]. However, the net clinical effect of such changes depends on the balance between surface energy, microbial species, and oral environmental conditions. The hydrophilic behavior observed for Sm2O3-containing formulations is consistent with reports describing the polar surface chemistry of lanthanide oxides, which can promote water spreading and surface film formation [40,41]. Clinically, increased wettability may improve denture comfort and mucosal adaptation, although it may also influence pellicle formation and long-term biofilm development. These findings emphasize the importance of evaluating wettability alongside microbial adhesion and biofilm assays when assessing the clinical relevance of nanoparticle-modified denture materials. It should be noted that contact angle measurements are sensitive to surface preparation and conditioning history, and thus the reported wettability trends should be interpreted within the context of the standardized measurement protocol applied in this study. Both microorganisms and material surfaces may exhibit hydrophilic or hydrophobic characteristics, and surface chemistry can significantly influence microbial retention. Adhesion forces are generally stronger on hydrophobic than on hydrophilic surfaces [42]. The contribution of surface hydrophobicity to fungal adhesion remains unclear. Early theories suggested that hydrophobic surfaces promote greater microbial adhesion; for example, Candida albicans has been reported to adhere more effectively to highly hydrophobic surfaces. However, Topaloğlu et al. reported no significant association between contact angle and C. albicans adhesion [43]. Staphylococcus aureus possesses a hydrophobic cell surface and demonstrates strong attraction to hydrophobic materials, as reported by Wang et al. [44] consistent with earlier findings showing stronger attachment of S. aureus to hydrophobic than to hydrophilic surfaces [42].
Despite the promising findings, this study has several limitations. First, the investigation focused primarily on short-term mechanical performance. Artificial aging methods, including prolonged water storage and thermocycling, are widely accepted for simulating long-term intraoral conditions for denture base materials. Aging processes may affect not only bulk mechanical properties but also filler–matrix interfacial interactions, potentially altering nanoparticle dispersion and stress transfer mechanisms over time. Thermocycling protocols—often consisting of approximately 5000 cycles between 5 and 55 °C with a 30 s dwell time—simulate thermal stresses associated with hot and cold food intake and have been shown to significantly influence water sorption and mechanical behavior of denture base resins [45]. Future studies should incorporate standardized aging procedures to better evaluate long-term performance.
Second, the DC and depth of cure were not assessed in the present study. These parameters are particularly important for light-polymerized and 3D-printed resins, as they directly influence mechanical properties, residual monomer release, and long-term stability. Nanoparticles may scatter or absorb incident light during photopolymerization, potentially reducing polymerization efficiency, especially in deeper layers [46]. Incomplete conversion has been reported to negatively affect mechanical performance and may accelerate aging-related degradation in printed resins [47]. Accordingly, future investigations should include FTIR- or Raman-based DC analysis to assess the influence of ZnO and Sm2O3 nanoparticles on polymerization behavior. Third, nanoparticle incorporation was limited to relatively low concentrations, and variations in particle size, surface treatment, or resin chemistry were not explored. In addition, color stability, dimensional accuracy, antimicrobial efficacy, and ion release behavior were not assessed.
Although the current results demonstrate that low-concentration incorporation of ZnO and Sm2O3 nanoparticles into DLP 3D-printed denture base materials can improve mechanical performance and surface characteristics, translation to direct clinical application remains prospective. Accordingly, the present findings should be interpreted as indicative of material performance trends under controlled in vitro conditions rather than as direct evidence of clinical efficacy. Confirmation through long-term aging, biological assessment, and validation under simulated intraoral conditions will be required prior to clinical application. While the present work focused on a DLP-based fabrication process, the concentration-dependent trends observed—namely improved properties at low filler loadings and degradation at higher concentrations due to aggregation—are fundamentally related to filler dispersion and polymer–particle interactions. These mechanisms are not specific to DLP and may also be expected in other vat photopolymerization systems, such as SLA, which use similar acrylate-based photopolymeric resins and curing wavelengths. However, differences in light delivery, exposure kinetics, and cure depth may influence the degree of reinforcement and should be considered in future comparative studies.
Future investigations should address long-term aging behavior, color stability, dimensional fidelity, and antimicrobial performance of nanoparticle-reinforced printed denture bases under clinically relevant conditions. In particular, the ZnO–Sm2O3 hybrid system warrants further study to clarify relationships between nanoparticle concentration, surface energy, roughness, ion release, and microbial adhesion. Advanced dispersion strategies or surface functionalization may also enable higher effective nanofiller loadings without compromising mechanical integrity [48,49]. Given the reported antimicrobial potential of ZnO in PMMA-based systems [50,51,52], future work integrating mechanical, biological, and esthetic performance metrics would further elucidate the clinical potential of these nanocomposite denture base materials. Although only a DLP-printed resin was evaluated, the observed trends—optimal low filler loadings and agglomeration-related property reductions at higher concentrations—are likely applicable to other vat-polymerized denture materials sharing similar acrylate chemistry. Comparable behavior has been reported for SLA-based systems incorporating oxide fillers, supporting the broader relevance of the present findings.

5. Conclusions

This study investigated the effects of zinc oxide and samarium oxide nanoparticles, incorporated individually and as hybrid systems, on the mechanical and surface properties of a three-dimensionally printed denture base resin. The findings demonstrated that nanoparticle incorporation resulted in concentration-dependent modifications in material performance while preserving the chemical structure of the polymer matrix, as confirmed by Fourier transform infrared spectroscopy. Morphological analysis revealed that low nanofiller concentrations promoted relatively uniform nanoparticle dispersion within the resin matrix, whereas higher concentrations were associated with increased particle clustering and reduced surface homogeneity. These microstructural differences were reflected in the mechanical performance of the printed resin, with formulations containing 1 wt.% nanofillers generally exhibiting superior impact, transverse, and flexural strength compared with those containing 2 wt.%. Among the tested formulations, the 1 wt.% zinc oxide group showed the highest impact and transverse strength values, while the maximum flexural strength was achieved using a 1 wt.% hybrid zinc oxide–samarium oxide formulation. Surface wettability was also influenced by nanoparticle type and concentration. Zinc oxide incorporation increased the water contact angle, indicating enhanced surface hydrophobicity, whereas samarium oxide reduced the contact angle, resulting in increased hydrophilicity. Hybrid formulations exhibited intermediate wettability behavior, demonstrating that surface characteristics of three-dimensionally printed denture base resins can be tailored through selective nanoparticle incorporation. Within the limitations of this in vitro study, the results suggest that controlled low-concentration incorporation of zinc oxide and samarium oxide nanoparticles—particularly in hybrid form—represents a promising strategy for improving the mechanical integrity and tailoring the surface properties of three-dimensionally printed denture base resins. However, the absence of artificial aging protocols and degree of conversion analysis limits direct extrapolation to long-term clinical performance. Further investigations incorporating thermocycling, water aging, polymerization efficiency assessment, and biological evaluation are required before definitive clinical recommendations can be made.

Author Contributions

Conceptualization, M.A.A., S.W.I. and M.H.M.A.; methodology, S.W.I., M.H.M.A. and M.A.A.; software, S.W.I. and M.H.M.A.; validation, M.A.A., S.S.A., M.S., S.W.I. and M.H.M.A.; formal analysis, S.S.A. and M.S.; investigation, M.A.A., S.W.I. and M.H.M.A.; resources, M.A.A. and S.W.I.; data curation, M.A.A., S.W.I., S.S.A. and M.H.M.A.; writing—original draft preparation, S.W.I., M.H.M.A. and M.A.A.; writing—review and editing, S.S.A., M.S., M.H.M.A. and S.W.I.; visualization, M.A.A., S.W.I. and M.H.M.A. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Institutional Review Board Statement

Not applicable.

Data Availability Statement

The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding authors.

Acknowledgments

The authors gratefully acknowledge the support provided by Mustansiriyah University, Baghdad, Iraq; Al Muthana University, Al Muthana, Iraq; and the University of Al-Ameed, Karbala, Iraq, during the conduct of this study.

Conflicts of Interest

The authors declare no conflicts of interest.

Abbreviations

3DThree-dimensional
AMAdditive manufacturing
DLPDigital light processing
SLAStereolithography
PMMAPolymethyl methacrylate
ZnOZinc-oxide
Sm2O3Samarium oxide
FE-SEMField-emission scanning electron microscopy
FTIRFourier-transform infrared spectroscopy
ANOVAAnalysis of variance
StdStandard deviation
DCDegree of conversion

References

  1. Majeed, H.F.; Hamad, T.I.; Bairam, L.R. Enhancing 3D-printed denture base resins: A review of material innovations. Sci. Prog. 2024, 107, 368504241263484. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  2. Beyer, M.; Scheller, L.; Burde, A.V.; Abazi, S.; Sommacal, A.; Seifert, L.; Sharma, N.; Thieringer, F.M. Comparative Evaluation of SLA and DLP 3D Printing in Dental Implant Guides: Impact on Fabrication Accuracy, Speed, and Resin Usage. Dent. J. 2025, 13, 471. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  3. Kessler, A.; Montenbruck, L.; Schwendicke, F.; Lüchtenborg, J.; Kaisarly, D. Narrative review of 3D-printed temporary and permanent dental resin restorations. Polym. Test. 2025, 151, 108953. [Google Scholar] [CrossRef] [Scilit]
  4. Szerszeń, M.; Cierech, M.; Wojnarowicz, J.; Górski, B.; Mierzwińska-Nastalska, E. Color Stability of Zinc Oxide Poly(methyl methacrylate) Nanocomposite—A New Biomaterial for Denture Bases. Polymers 2022, 14, 4982. [Google Scholar] [CrossRef] [Scilit]
  5. Gad, M.M.; Fouda, S.M. Factors affecting flexural strength of 3D-printed resins: A systematic review. J. Prosthodont. 2023, 32, 96–110. [Google Scholar] [CrossRef] [Scilit]
  6. Abd Elhamid Abo Salh, I.B.; Add El-Salam, E.B.; Ezzat, A.A.; Aboshama, M.; Elhagali, A.F. Antimicrobial Effect of Three Different Nanoparticles-Modified 3D-Printed Denture Resin: An In Vitro Study. J. Int. Soc. Prev. Community Dent. 2025, 15, 42–49. [Google Scholar] [CrossRef] [Scilit]
  7. Rao, U.M.; Singh, N.K.; Jyotsna, S.; Poojitha, Y.; Ssk Kinneresh, R.V.; Prasad Pallekonda, A.T. Titanium dioxide nanoparticles on flexural strength of conventional and injection moulded denture base materials. Bioinformation 2025, 21, 19–24. [Google Scholar] [CrossRef] [Scilit]
  8. Saini, R.S.; Bavabeedu, S.S.; Quadri, S.A.; Gurumurthy, V.; Kanji, M.A.; Okshah, A.; Binduhayyim, R.I.H.; Alarcón-Sánchez, M.A.; Mosaddad, S.A.; Heboyan, A. Mapping the research landscape of nanoparticles and their use in denture base resins: A bibliometric analysis. Discov. Nano 2024, 19, 95. [Google Scholar] [CrossRef] [Scilit]
  9. Pai, E.; Nayak, A.; Hallikerimath, R.B.; Ruttonji, Z.; Astagi, P.; Pokale, S. Comparison of titanium dioxide nanoparticles and silver nanoparticles for flexural strength once incorporated in heat-cure acrylic denture base resin: An in vitro Study. J. Indian Prosthodont. Soc. 2023, 23, 127–134. [Google Scholar] [CrossRef] [Scilit]
  10. Waghmare, A.; Nair, C.; Shukla, A.K.; Chaturvedi, M.; Bhagat, T.V.; Alsubaiy, E.F.; Suleman, G.; Khader, M.A.; Chaturvedi, S. Flexural strength and surface hardness of nanocomposite denture base resins. Heliyon 2024, 10, e40442. [Google Scholar] [CrossRef] [Scilit]
  11. Wang, H.; Huang, Q.; Zhai, Y. Influences of modified Sm2O3 on thermal stability, mechanical and neutron shielding properties of aminophenol trifunctional epoxy resin. Polymers 2022, 14, 638. [Google Scholar] [CrossRef] [Scilit]
  12. Bastami, H.; Taheri Nasaj, E.; Smet, P.F.; Poelman, D. The Effect of Sm2O3 on the Sintering and Grain Growth Behaviors of SnO2-Based Ceramics. Adv. Ceram. Prog. 2019, 5, 26–31. [Google Scholar]
  13. Kaurani, P.; Hindocha, A.; Porwal, A.; Tambe, A.; Price, C.; Goel, V.; Krasner, H.; Khubchandani, J.; Batra, K. Effect of Addition of Metal Oxide Nanoparticles on the Strength of Heat-Cured Denture Base Resins: Protocol for Systematic Review and Meta-Analysis of In Vitro Studies. JMIR Res. Protoc. 2024, 13, e59999. [Google Scholar] [CrossRef] [Scilit]
  14. Kaurani, P.; Hindocha, A.D.; Jayasinghe, R.M.; Pai, U.Y.; Batra, K.; Price, C. Effect of addition of titanium dioxide nanoparticles on the antimicrobial properties, surface roughness and surface hardness of polymethyl methacrylate: A Systematic Review. F1000Research 2023, 12, 577. [Google Scholar] [CrossRef] [Scilit]
  15. Shukur, B. Evaluation of the addition of tea tree oil on some mechanical properties of heat cured acrylic resin. J. Al-Rafidain Univ. Coll. Sci. 2018, 42, 301–316. [Google Scholar]
  16. Öztürk, Z.; Tosun, B. Comparison of 3D printed and conventional denture base materials in terms of durability and performance characteristics. Sci. Rep. 2025, 15, 18234. [Google Scholar] [CrossRef] [Scilit]
  17. AlGhamdi, M.A.; Fouda, S.M.; Al-Dulaijan, Y.A.; Khan, S.Q.; El Zayat, M.; Al Munif, R.; Albazroun, Z.; Amer, F.H.; Al Ammary, A.T.; Mahrous, A.A.; et al. Nanocomposite 3D printed resins containing titanium dioxide (TiO2) nanoparticles: An in vitro analysis of color, hardness, and surface roughness properties. Front. Dent. Med. 2025, 6, 1581461. [Google Scholar] [CrossRef] [Scilit]
  18. Ahmed Teama, E.M.; Amin Rashad, H.M.; Shakal, E.A.E.-S.M.; Hegazy, E.E. Clinical and microbial study of reinforced 3D-printed maxillary denture base resin: A randomized trial. BMC Oral Health 2025, 25, 1192. [Google Scholar] [CrossRef] [Scilit]
  19. Khan, M.M.; Matussin, S.N. Sm2O3 and Sm2O3-based nanostructures for photocatalysis, sensors, CO conversion, and biological applications. Catal. Sci. Technol. 2023, 13, 2274–2290. [Google Scholar]
  20. Abdelraouf, R.M.; Bayoumi, R.E.; Hamdy, T.M. Influence of incorporating 5% weight titanium oxide nanoparticles on flexural strength, micro-hardness, surface roughness and water sorption of dental self-cured acrylic resin. Polymers 2022, 14, 3767. [Google Scholar] [CrossRef] [Scilit]
  21. Kim, M.-C.; Byeon, D.-J.; Jeong, E.-J.; Go, H.-B.; Yang, S.-Y. Color stability, surface, and physicochemical properties of three-dimensional printed denture base resin reinforced with different nanofillers. Sci. Rep. 2024, 14, 1842. [Google Scholar] [CrossRef] [Scilit]
  22. Altarazi, A.; Haider, J.; Alhotan, A.; Silikas, N.; Devlin, H. Assessing the physical and mechanical properties of 3D printed acrylic material for denture base application. Dent. Mater. 2022, 38, 1841–1854. [Google Scholar] [CrossRef] [Scilit]
  23. Altarazi, A.; Haider, J.; Alhotan, A.; Silikas, N.; Devlin, H. 3D printed denture base material: The effect of incorporating TiO2 nanoparticles and artificial ageing on the physical and mechanical properties. Dent. Mater. 2023, 39, 1122–1136. [Google Scholar] [CrossRef] [Scilit]
  24. Hanno, K.I.; Metwally, N.A. The wettability of complete denture base materials constructed by conventional versus digital techniques: An in-vitro study. BMC Oral Health 2024, 24, 1081. [Google Scholar] [CrossRef] [Scilit]
  25. Reymus, M.; Lümkemann, N.; Stawarczyk, B. 3D-printed material for temporary restorations: Impact of print layer thickness and post-curing method on degree of conversion. Int. J. Comput. Dent. 2019, 22, 231–237. [Google Scholar]
  26. Alwan, S.A.; Alameer, S.S. The effect of the addition of silanized Nano titania fillers on some physical and mechanical properties of heat cured acrylic denture base materials. J. Baghdad Coll. Dent. 2015, 27, 86–91. [Google Scholar] [CrossRef] [Scilit]
  27. Omar, M.H.; Amin, M.H.; Younis, H.A. Comparison of using nano-ZnO and nano-Al2O3 to improve the properties of prepared polymethyl methacrylate denture base. Appl. Phys. A 2022, 128, 313. [Google Scholar] [CrossRef] [Scilit]
  28. Rafeeq, A.K.; Salman, I.A.; Ibrahim, S.W. Evaluation of Hardness, Impact, and Transverse Strength Tests of Heat-Cured Acrylic Denture Base Material Following the Addition of Watercress, Tea Tree, and Clove Oils: An In Vitro Study. Dent. Hypotheses 2025, 16, 23–26. [Google Scholar] [CrossRef] [Scilit]
  29. Ataei, K.; Ghaffari, T.; Moslehifard, E.; Dizaj, S.M. Physico-chemical and Mechanical Assessments of a New 3D Printed PMMA-Based Acrylic Denture Base Material. Open Dent. J. 2024, 18, e18742106278787. [Google Scholar] [CrossRef] [Scilit]
  30. Palencia, M. Surface free energy of solids by contact angle measurements. J. Sci. Technol. Appl. 2017, 2, 84–93. [Google Scholar] [CrossRef] [Scilit]
  31. Elkhouly, H.I.; Ali, E.M.; El-Sheikh, M.N.; Hassan, A.E.M. An investigated organic and inorganic reinforcement as an effective economical filler of poly (methyl methacrylate) nanocomposites. Sci. Rep. 2022, 12, 16416. [Google Scholar] [CrossRef] [Scilit]
  32. Al Mahmoud, Z.; Safaei, B.; Asmael, M.B.A.; Petrů, J.; Sahmani, S. Investigation for the Influence of Sm2O3 and CeO2 Nanoparticles on the Microstructure and Electrochemical Behavior of Epoxy and Prediction of Mechanical Characterizations of Adhesive Joining of CFPEEK via Machine Learning. J. Mater. Res. Technol. 2025, 38, 4917–4938. [Google Scholar]
  33. Ma, X.; Zare, Y.; Rhee, K.Y. A two-step methodology to study the influence of aggregation/agglomeration of nanoparticles on Young’s modulus of polymer nanocomposites. Nanoscale Res. Lett. 2017, 12, 621. [Google Scholar]
  34. Vu, M.-T.; Monsalve-Bravo, G.M.; Lin, R.; Li, M.; Bhatia, S.K.; Smart, S. Mitigating the agglomeration of nanofiller in a mixed matrix membrane by incorporating an interface agent. Membranes 2021, 11, 328. [Google Scholar] [CrossRef] [Scilit]
  35. Demir, E.C.; Benkaddour, A.; Aldrich, D.R.; McDermott, M.T.; Kim, C.I.; Ayranci, C. A predictive model towards understanding the effect of reinforcement agglomeration on the stiffness of nanocomposites. J. Compos. Mater. 2022, 56, 1591–1604. [Google Scholar] [CrossRef] [Scilit]
  36. ISO 20795-1:2013; Dentistry-Base Polymers-Part 1: Denture Base Polymers. International Organization for Standardization: Geneva, Switzerland, 2013.
  37. Ruan, S.; Zhao, Y.; Chen, R.; Ma, J.; Guan, Y.; Ma, J.; Ren, L. Effect of zinc oxide/graphene oxide nanocomposites on the cytotoxicity, antibacterial and mechanical properties of polymethyl methacrylate. BMC Oral Health 2024, 24, 1013. [Google Scholar] [CrossRef] [Scilit]
  38. Fardiaz, D.; Irnawati, D.; Nuryono, N. The effect of ZnO nanoparticles addition to PMMA on surface contact angle and adhesion of Candida albicans. Braz. Dent. Sci. 2024, 27, e4201. [Google Scholar] [CrossRef] [Scilit]
  39. Mlinarić, N.M.; Zore, A.; Veselinovic, V.; Trtić, N.; Dolić, O.; Štukelj, R.; Abram, A.; Učakar, A.; Adamović, T.; Vidrih, R.; et al. Antimicrobial Activity of Poly(methyl methacrylate) Doped with CuO and ZnO Nanoparticles. ACS Omega 2025, 10, 13060–13072. [Google Scholar]
  40. Huo, Z.; Lu, Y.; Zhang, H.; Zhong, G. Sm2O3 micron plates/B4C/HDPE composites containing high specific surface area fillers for neutron and gamma-ray complex radiation shielding. Compos. Sci. Technol. 2024, 251, 110567. [Google Scholar]
  41. Salman, I.A.S. Biosurfactant as a preventive agent on acrylic resin. Mustansiria Dent. J. 2018, 15, 83–89. [Google Scholar]
  42. Poker, B.d.C.; Oliveira, V.d.C.; Macedo, A.P.; Gonçalves, M.; Ramos, A.P.; Silva-Lovato, C.H. Evaluation of surface roughness, wettability and adhesion of multispecies biofilm on 3D-printed resins for the base and teeth of complete dentures. J. Appl. Oral Sci. 2024, 32, e20230326. [Google Scholar] [CrossRef] [Scilit]
  43. Topaloğlu, O.; Gürbüz, A.; Murat, S. Influence of Surface Properties on Candida albicans Adhesion to Denture Base Materials Fabricated by Different Techniques. Cumhur. Dent. J. 2025, 28, 427–434. [Google Scholar] [CrossRef] [Scilit]
  44. Wang, C.; van der Mei, H.C.; Busscher, H.J.; Ren, Y. Streptococcus mutans adhesion force sensing in multi-species oral biofilms. Npj Biofilms Microbiomes 2020, 6, 25. [Google Scholar] [CrossRef] [Scilit]
  45. Dimitrova, M.; Vlahova, A.; Hristov, I.; Kazakova, R.; Chuchulska, B.; Kazakov, S.; Forte, M.; Granberg, V.; Barile, G.; Capodiferro, S.; et al. Evaluation of water sorption and solubility of 3D-printed, CAD/CAM milled, and PMMA denture base materials subjected to artificial aging. J. Compos. Sci. 2023, 7, 339. [Google Scholar] [CrossRef] [Scilit]
  46. Fidalgo-Pereira, R.; Carvalho, Ó.; Catarino, S.O.; Henriques, B.; Torres, O.; Braem, A.; Souza, J.C.M. Effect of inorganic fillers on the light transmission through traditional or flowable resin-matrix composites for restorative dentistry. Clin. Oral. Investig. 2023, 27, 5679–5693. [Google Scholar] [CrossRef] [Scilit]
  47. Živković, N.; Vulović, S.; Lazarević, M.; Đukić, L.; Jakovljević, A.; Dinić, I.; Perić, M.; Lemić, A.M. Evaluation of biological properties of the light-cured, CAD/CAM milled, and 3D printed dental composites after artificial aging–an in vitro study. Dent. Mater. 2026; in press. [CrossRef] [Scilit]
  48. Kubiak, J.M.; Li, B.; Suazo, M.; Macfarlane, R.J. Polymer grafted nanoparticle composites with enhanced thermal and mechanical properties. ACS Appl. Mater. Interfaces 2022, 14, 21535–21543. [Google Scholar] [CrossRef] [Scilit]
  49. Shah, M.; Ullah, A.; Azher, K.; Ur Rehman, A.; Akturk, N.; Juan, W.; Tüfekci, C.S.; Salamci, M.U. The influence of nanoparticle dispersions on mechanical and thermal properties of polymer nanocomposites using SLA 3D printing. Crystals 2023, 13, 285. [Google Scholar] [CrossRef] [Scilit]
  50. Bakina, O.; Svarovskaya, N.; Ivanova, L.; Glazkova, E.; Rodkevich, N.; Evstigneev, V.; Evstigneev, M.; Mosunov, A.; Lerner, M. New PMMA-based hydroxyapatite/ZnFe2O4/ZnO composite with antibacterial performance and low toxicity. Biomimetics 2023, 8, 488. [Google Scholar] [CrossRef] [Scilit]
  51. Mazur, M.W.; Grudniak, A.; Szałaj, U.; Szerszeń, M.; Mizeracki, J.; Cierech, M.; Mierzwińska-Nastalska, E.; Kostrzewa-Janicka, J. Antifungal Activity of Newly Formed Polymethylmethacrylate (PMMA) Modification by Zinc Oxide and Zinc Oxide–Silver Hybrid Nanoparticles. Polymers 2024, 16, 3512. [Google Scholar] [CrossRef] [Scilit]
  52. Khlifi, K.; Atallah, M.S.; Cherif, I.; Karkouch, I.; Barhoumi, N.; Attia-Essaies, S. Synthesis of ZnO nanoparticles and study of their influence on the mechanical properties and antibacterial activity of PMMA/ZnO composite for orthotic devices. Surf. Interfaces 2023, 41, 103279. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.