Abstract
This paper presents an experimental investigation into how different forming routes—multi-directional forging (AZ80-F), extrusion (AZ80-E), and multi-directional forging followed by extrusion (AZ80-FE)—affect the microstructure, monotonic mechanical properties, and low-cycle fatigue behavior of AZ80 magnesium alloy. As-cast AZ80 (AZ80-C) was also tested as a control group. The main contributions of this study are as follows: (1) SEM and EBSD data across all forming routes were comparatively analyzed to establish the influence of processing on grain size and microstructural type. (2) Monotonic test results revealed distinct tension–compression anisotropy and the effect of each forming process on tensile and compressive strengths. (3) Based on cyclic test data, the hysteresis behavior, evolution of maximum tensile and compressive stress, and plastic strain energy density were characterized and discussed. (4) A fatigue life prediction model with an explicit log–log multi-linear equation is proposed, which can readily predict the fatigue life of AZ80 magnesium alloy across strain amplitudes from 0.4% to 1.0%.
1. Introduction
Magnesium alloys [1,2] are among the lightest structural metals and, owing to their high specific strength, have become promising materials in aerospace engineering [3] and automotive engineering [4]. The merits of magnesium alloys [5,6]—low density, good heat dissipation, and excellent damping performance—can reduce vehicle weight and improve tire life [7,8]. Among these, AZ80 magnesium alloy is particularly attractive due to its excellent mechanical properties [9,10], high-temperature performance [11,12], and good wear resistance and processability [13,14]. For practical industrial applications [15,16,17], Wang et al. [18] manufactured integrated automotive wheel blanks from extruded AZ80 alloy, while Zhou et al. [19] successfully produced high-strength AZ80 components via air-based multidirectional forging without post-forging aging treatment.
Numerous studies have been conducted on AZ80 alloy, particularly regarding its material properties. Wang et al. [10] investigated the effect of lithium addition on AZ80 alloy: addition of 2 mass% Li improved ductility, impact toughness, and formability but reduced corrosion resistance. Yin et al. [20] found that ECAP and aging treatment significantly increased the static toughness of AZ80 alloy (by approximately 120%) due to increased dislocation density and nanoscale Al2Nd precipitation. Wang et al. [21] investigated the hot deformation characteristics and constitutive equation of AZ80 magnesium alloy through thermal simulation compression experiments. Based on the Arrhenius equation, they proposed a constitutive model, though they focused primarily on the monotonic stress–strain relationship.
Cai et al. [22] investigated the effect of thermomechanical treatment on the microstructure and properties of AZ80 alloy, finding that hardness increased with the degree of deformation, reaching a peak at 30% deformation. The heat treatment temperature also significantly influenced hardness, which was maximized at 170 °C. Liu et al. [23] examined the effects of strain rate and temperature on the high-temperature deformation behavior of AZ80 alloy; their results indicated that the peak stress decreased with increasing deformation temperature and decreasing strain rate. Chen et al. [24] studied the effect of neodymium (Nd) on the microstructure and mechanical properties of AZ80 alloy. They found that Nd reduced the size and refined the distribution of the β-Mg17Al12 phase while producing new phases such as Al11Nd3 and massive Al2Nd rare-earth phases. However, as the Nd content increased, the strength of as-cast AZ80 alloy first increased and then decreased, with the tensile strength and yield strength reaching their maximum at 0.9% Nd.
Zuraidawani et al. [25] reported that AZ80 samples aged for 2 h at 170 °C exhibited the highest hardness of 62.5 HV. Zhao et al. [26] comparatively analyzed the low-cycle fatigue performance of T5- and T6-aged extruded AZ80 wheel blanks, confirming that dense lamellar precipitates in T5 specimens suppress cyclic plastic deformation at fatigue crack tips, induce crack deflection, and prolong fatigue life within specific strain amplitude ranges. Salevati et al. [27] reported that a repeated upsetting process refined the grain size of SiC/AZ80 nanocomposites from 30.6 μm to the submicron level, improving shear strength by 35% while maintaining 85% fracture toughness. He et al. [28] identified residual twins and precipitated intermetallic phases as the primary fatigue crack initiation sites in extruded AZ80 alloy, with second-phase particles exerting a more dominant detrimental effect than twin boundaries. Liao et al. [8] increased the dynamic recrystallization ratio to 85% by adding LaMM (La-rich mischmetal) to AZ80 wheels via a single-pass radial forging process, achieving refinement of the average grain size from 45 μm to 12 μm and an increase in tensile strength to 380 MPa.
However, the studies described above focused on the microstructure and mechanical properties of AZ80 alloy under monotonic loading conditions. Recognizing the importance of fatigue behavior for structural safety, researchers have also investigated the fatigue response of AZ80 alloy. Xiong and Jiang [29] experimentally studied the cyclic performance of rolled AZ80 alloy. Their results demonstrated that material orientation significantly influences yield strength and fatigue life. The ND (normal direction) sample exhibited the lowest fatigue resistance at the same strain amplitude, while ND30 and ND60 (samples at 30° and 60° from ND, respectively) showed similar fatigue lives. For strain amplitudes greater than 0.4%, the fatigue lives of ND30 and ND60 exceeded that of the RD (rolling direction) sample, whereas the opposite trend was observed below 0.4%. Based on these results, they proposed a predictive model using the plastic strain energy density per loading cycle.
Subsequently, Wang et al. [30] investigated the fatigue behavior of extruded AZ80 alloy. Strain hardening was observed in samples tested at strain amplitudes from 0.4% to 1.0%, and the hysteresis loops became increasingly asymmetric with increasing strain amplitude. They also found that the modified Morrow model can predict the fatigue life of extruded AZ80 alloy. Later, Zhao et al. [7] investigated the fatigue behavior of AZ80 alloy using samples cut from prepared automotive wheels. They found that rim samples exhibited finer and more homogeneous dynamically recrystallized grains than disc samples and that the rim samples also exhibited superior fatigue properties. These studies have provided valuable data and references for understanding the fatigue behavior of AZ80 alloys. However, there is limited research on AZ80 alloys processed using composite-forming methods, such as a combination of forging and hot extrusion. The effects of these processes on the microstructure and macroscopic properties of AZ80 magnesium alloys, particularly their fatigue properties, require further investigation.
2. Experimental Procedures
2.1. Material
The chemical composition of the AZ80 alloy is summarized in Table 1. All test samples were cut from a billet or extruded billet of AZ80 alloy. To investigate the effect of the forming method on fatigue behavior, three forming methods (see Section 2.2) and five strain amplitudes (ranging from 0.4% to 1.0%) were considered.
Table 1.
Chemical composition of AZ80 magnesium alloy (wt.%).
2.2. Forming Methods
To investigate the influence of forming methods on the material properties and cyclic performance of AZ80 magnesium alloy, specimens fabricated by three different forming methods were tested: (1) hot multi-directional forging (AZ80-F); (2) hot extrusion only (AZ80-E); and (3) hot multi-directional forging followed by extrusion (AZ80-FE), as shown in Figure 1a. The forging procedures and mould are illustrated in Figure 1b and Figure 1c, respectively. Moreover, it is worth noting that all mechanical test samples (tensile, compressive, and fatigue samples) were taken in the longitudinal direction, which is aligned with the original AZ80 rod.
Figure 1.
Illustration of the procedures: (a) flowcharts of different procedures, (b) the order of multi-directional forging procedures, (c) illustration of the fabrication mould for multi-directional forging.
Figure 2 and Figure 3 present the microstructure and EBSD results of AZ80 alloy processed by the three different procedures (details regarding the preparation of the test samples are summarized in the Appendix A).
Figure 2.
Microstructure before test: (a) AZ80-F, (b) AZ80-E, (c) AZ80-FE, (d) AZ80-C.
Figure 3.
EBSD of AZ80 magnesium alloys: (a) AZ80–-F, (b) AZ80–E, (c) AZ80–FE.
(1) AZ80-F: The multi-directional-forged specimen exhibits a wide variation in grain size, with localized aggregation of bulk β-Mg17Al12 second-phase particles and numerous twin bands, as shown in Figure 2a. The EBSD IPF orientation map and quantitative grain size analysis indicate a bimodal grain distribution with a median grain size d50 = 20.05 μm. Dynamic recrystallization occurs only in localized areas, leaving a large number of coarse cast grains. The basal texture density (MRD) is only 1.5–2.0, representing the weakest texture among the three types of formed specimens, as shown in Figure 3a. The X/Y/Z triaxial alternating shear relies on twin-induced dynamic recrystallization to break up some coarse grains, but without subsequent axial compression leveling, the coarse second phase cannot be uniformly dispersed. The weak basal texture significantly increases the critical stress for twinning initiation, making it difficult to activate twinning during compression. Consequently, the ultimate compressive strength is much higher than the tensile strength, and the tension–compression asymmetry coefficient reaches 2.083 (see Section 3.1). At the same time, the coarse grains and agglomerated second phase act as stress concentration sites under cyclic loading, leading to early fatigue crack initiation. Ultimately, the fatigue performance is inferior to that of the extruded and forged-extruded composite specimens.
(2) AZ80-E: The microstructure exhibits a typical extrusion streamline structure, with the β phase continuously distributed in bands along the deformation direction, as shown in Figure 2b. Figure 3b shows that the EBSD grain size is refined to an average of 6.57 μm, but the IPF pattern reveals large areas of uniform orientation, and the basal texture MRD is as high as 4.0–5.5, forming a strong basal fiber texture. Uniaxial strain triggers dynamic recrystallization, achieving grain refinement; however, prolonged holding at 390 °C causes static recovery and local grain growth. Uniaxial deformation results in highly selective grain orientation, allowing tensile twinning to be initiated at low stress during the compression stage, leading to a significant difference between the tensile and compressive yield stresses and producing a highly asymmetric hysteresis curve throughout cycling. Although the banded second phase can improve plasticity, continuous damage accumulates at the streamline interface during cycling, resulting in a lower fatigue life than that of the forged-extruded composite specimen.
(3) AZ80-FE: The microstructure is uniform and dense, with no coarse grains or oriented second-phase flow lines in the metallographic structure, as shown in Figure 2c. Figure 3c shows the EBSD IPF image with randomly mixed grain orientations and a concentrated grain size distribution in the ultrafine range, with d50 of only 2.09 μm. The basal texture MRD is reduced to 1.5–2.0, indicating the optimal texture-weakening effect. Multi-directional forging pre-deformation introduces high-density dislocations and numerous twin boundaries into the matrix, providing sufficient nucleation sites for dynamic recrystallization during subsequent extrusion. Simultaneously, pre-forging breaks down the bulk β phase into nanoscale particles. During extrusion, the fine second-phase particles generate a grain boundary pinning effect, inhibiting grain boundary migration and basal texture strengthening. This simultaneously achieves triple micro-optimization: grain refinement, texture weakening, and second-phase dispersion. The ultrafine grain boundaries disperse cyclic stress concentrations, the weak texture reduces irreversible twin damage, and the dispersed second phase hinders crack propagation. Consequently, the material exhibits both optimal static tensile strength and low-cycle fatigue life. Benefiting from the pre-forging pretreatment, AZ80-FE achieves the highest recrystallized fraction. The pre-forging step introduces high-density dislocations and twin boundaries, which provide abundant nucleation sites for DRX. Meanwhile, the finely dispersed second-phase particles suppress the formation of large substructure regions. This high fraction of DRX grains, together with the weakened basal texture, is responsible for the improved fatigue performance of the composite-forming sample.
2.3. Test Methods
For materials from all three forming methods, both monotonic tension and compression tests were conducted to determine the material properties, and details regarding the preparation of the test samples are summarized in the Appendix A. Monotonic tensile and compressive tests were designed following GB/T 228.1-2010 [31,32], GB/T 145-2001 [33], and GB/T 7314-2017 [34,35]. The dimensions of the monotonic test specimens are shown in Figure 4a,b. Both the monotonic tensile and compressive tests were conducted using an electronic universal testing machine (TSE105D-100KN, Shenzhen Wance Testing Equipment Co., Ltd., Shenzhen, China), albeit with different grips. The low-cycle fatigue tests followed GB/T 15248-2008 [36]. To investigate the influence of forming methods on fatigue behavior, five different strain levels were designed. All low-cycle fatigue tests were conducted using a fatigue test system (HDT-MM-202310A, Shenzhen Wance Testing Equipment Co., Ltd., Shenzhen, China). The specimen dimensions and test setup are shown in Figure 4c. It is worth noting that, given the challenges associated with specimen preparation and testing, monotonic tensile and compressive tests were each performed in duplicate, whereas fatigue tests were conducted on a single specimen. For each test group, the average of all results was taken as the representative value, and half the difference between the maximum and minimum values was defined as the test error (used for plotting error bars). It is worth noting that, due to a lack of sufficient replication, this experimental study is preliminary in nature and requires further validation using a larger sample size. For all the tests, the force and strain were measured by the test machine (ISO 7500-1 class 0.5, Epsilon Technology Corp, Jackson, WY, USA) and strain gauge (ISO 9513 class 0.5, Epsilon Technology Corp, Jackson, WY, USA), respectively. The errors for both devices did not exceed ±0.5%.
Figure 4.
Shape and dimensions of test samples: (a) tensile test, (b) compressive test, (c) low-cycle test.
3. Results and Discussion
3.1. Monotonic Tension and Compression Behaviors
Figure 5 presents the engineering stress–strain curves of AZ80 magnesium alloys processed by different forming methods. Notably, the forming method significantly affects tension and compression behaviors. AZ80-C exhibits the lowest tensile strength, compressive strength, and elongation. Moreover, the tensile stress–strain curve can be divided into three stages: (1) a linearly increasing elastic stage, (2) a plastic stage with strain hardening, and (3) the final failure stage. In the compressive stress–strain curves, a more pronounced increase can be observed in the plastic stage. However, for the extruded or combined forged-and-extruded AZ80 alloy, the compressive yield stress is much lower than the corresponding tensile yield stress, indicating significant tension–compression anisotropy.
Figure 5.
Stress–strain curves: (a) tension, (b) compression.
Figure 6 summarizes the properties of the AZ80 magnesium alloys. The difference in elastic moduli among AZ80-F, AZ80-E, and AZ80-FE is less than 5%, indicating that the forming method has a limited influence on Young’s modulus. However, the forming method significantly affects the characteristic stresses. Compared with forged AZ80-F, AZ80-E and AZ80-FE increase the tensile and compressive yield stresses by (+174.05%, +77.58%) and (+185.79%, +14.47%), respectively. The increases in ultimate tensile and compressive stresses are (+120.28%, +34.86%) and (+127.83%, +48.06%), respectively. These results indicate that the forming method has a more pronounced influence on tensile properties than on compressive properties.
Figure 6.
Properties of AZ80 magnesium alloy: (a) tension, (b) compression (c) fatigue.
Moreover, Figure 6 shows that AZ80-FE exhibits the highest tensile yield and ultimate tensile strength, whereas AZ80-E exhibits the highest compressive yield strength. The tensile yield strength, ultimate tensile strength, and ultimate compressive strength of AZ80-E are very close to those of AZ80-FE. In addition, the forming method significantly changes the ratio of ultimate compressive strength to ultimate tensile strength of AZ80 magnesium alloy. The ratios for AZ80-F, AZ80-E, and AZ80-FE are 2.083, 1.275 (−38.79%), and 1.354 (−35.00%), respectively, indicating that AZ80 magnesium alloy exhibits more pronounced strain hardening under compressive loading than under tensile loading.
According to the EBSD orientation contrast map (Figure 3) and grain size statistics, the three forming processes control the grain size, basal texture intensity, and β-Mg17Al12 second-phase distribution through differentiated three-dimensional strain paths, ultimately yielding significant differences in the uniaxial tensile/compressive mechanical properties. In multi-directional-forged AZ80-F, following X/Y/Z triaxial shear deformation, the original as-cast coarse grains are partially refined through twin-induced dynamic recrystallization; however, without subsequent extrusion leveling, the grains exhibit a distinct bimodal structure, and the β phase shows local agglomeration. Although three-dimensional deformation effectively weakens the basal texture to 1.5–2.0 MRD, the coarse grains and the second phase cutting through the matrix result in limited grain refinement and precipitation strengthening, yielding a tensile yield strength of only 89.4 MPa.
Single-pass extrusion of AZ80-E involves unidirectional axial strain. After dynamic recrystallization, static recovery induced by heat treatment results in an average grain refinement to 6.57 μm. However, unidirectional deformation forms a strong basal fiber texture (4.0–5.5 MRD). The β phase is distributed in a banded pattern along the extrusion streamline. The fine grains and second-phase strengthening increase the tensile yield strength to 245.0 MPa. The strong basal texture facilitates tensile twinning initiation under compressive loading, which greatly reduces the compressive yield strength and lowers the tension–compression asymmetry coefficient to 1.275.
The forging–extrusion composite forming of AZ80-FE utilizes multi-directional forging pre-deformation to introduce high-density dislocations and twin boundaries, providing abundant nucleation sites for dynamic recrystallization during secondary extrusion. Simultaneously, pre-deformation breaks up bulk β phases. During extrusion, the nanoscale second-phase particles generate a grain boundary pinning effect, inhibiting grain growth and basal texture strengthening. This ultimately yields ultrafine, uniform grains with an average size of 2.09 μm, the lowest basal texture strength, and a fully dispersed nanoscale β phase. The synergistic effect of fine-grain strengthening and precipitation strengthening optimizes the tensile yield strength and ultimate tensile strength while maintaining a tension–compression asymmetry coefficient of 1.354.
From a deformation mechanism perspective, the weakly textured AZ80-F exhibits difficulty in activating twinning during compression, resulting in a compressive strength far exceeding the tensile strength and thus the strongest asymmetry. The moderately textured AZ80-E and AZ80-FE readily initiate compressive twinning, effectively reducing the tension–compression strength difference. These observations are consistent with the texture–twin coupling deformation theory of magnesium alloys.
3.2. Hysteretic Behaviors
3.2.1. Hysteresis Loops
To reveal the impact of forming on the hysteretic behavior of AZ80 magnesium alloy, low-cycle fatigue tests were also conducted on as-cast AZ80 (AZ80-C) as a control group. Figure 7, Figure 8, Figure 9 and Figure 10 present the evolution of stress–strain hysteresis loops (the 1st, 2nd, and stable loops) of AZ80 magnesium alloy processed by different forming methods. The first two hysteresis loops differ markedly, and due to cyclic hardening, the stable loop exhibits higher tensile and compressive stresses than the first two loops.
Figure 7.
Evolutionary changes in stress–strain hysteresis loops for AZ80-C at different strain amplitudes: (a) 0.4%; (b) 0.5%; (c) 0.6%; (d) 0.8%; (e) 1.0%; and (f) all stable loops.
Figure 8.
Evolutionary changes in stress–strain hysteresis loops for AZ80-F at different strain amplitudes: (a) 0.4%; (b) 0.5%; (c) 0.6%; (d) 0.8%; (e) 1.0%; and (f) all stable loops.
Figure 9.
Evolutionary changes in stress–strain hysteresis loops for AZ80-E at different strain amplitudes: (a) 0.4%; (b) 0.5%; (c) 0.6%; (d) 0.8%; (e) 1.0%; and (f) all stable loops.
Figure 10.
Evolutionary changes in stress–strain hysteresis loops for AZ80-FE at different strain amplitudes: (a) 0.4%; (b) 0.5%; (c) 0.6%; (d) 0.8%; (e) 1.0%; and (f) all stable loops.
The hysteresis loops of AZ80-C under all five strain amplitudes exhibit good symmetry: the loading half-cycle and the unloading half-cycle are approximately centrosymmetric about the origin (zero stress and zero strain). In other words, within the tested strain amplitude range, AZ80-C exhibits similar tensile and compressive behavior, indicating that dislocation slip is the dominant cyclic deformation mode in AZ80-C [37]. In contrast, the other three AZ80 alloys exhibit varying degrees of tension–compression asymmetry. At strain amplitudes not exceeding 0.5%, AZ80-F shows similar tensile and compressive behavior; however, as the strain amplitude increases, the tension and compression behaviors diverge, with larger strain amplitudes producing greater differences. Even at small strain amplitudes, the tensile and compressive behaviors of AZ80-E and AZ80-FE show marked differences, and the hysteresis loops exhibit significant asymmetry. Moreover, a yield plateau can be observed in the first compressive half-cycle of AZ80-E and AZ80-FE, which is not observed in the other two materials. This asymmetric hysteresis behavior is attributed to the partial twinning–detwinning process in magnesium alloys, which typically promotes crack nucleation and propagation during fatigue deformation [38].
Figure 11 illustrates the symmetry ratio (SR) of the AZ80 magnesium alloys, defined as the ratio of the maximum compressive stress to the maximum tensile stress of the stable loop. The closer this value is to 1, the more symmetric the hysteresis loop; conversely, the farther from 1, the more asymmetric the loop. Generally, when SR is between 0.95 and 1.05, the hysteresis loop can be considered approximately symmetric, whereas SR values below 0.8 or above 1.2 indicate strongly asymmetric hysteresis behavior. The SR values of AZ80-C range from 0.94 to 1.05, and when the strain amplitude is at least 0.5%, the SR increases with increasing strain amplitude, indicating that the AZ80-C hysteresis loops exhibit good symmetry. However, for the other specimens, the SR is greater than 1.05 or less than 0.95 in most cases, indicating asymmetric hysteresis loops—particularly for AZ80-E and AZ80-FE. Notably, the anomalous behavior of AZ80-F is presented in Figure 11: the SR value at a strain amplitude of 0.8% is significantly higher than those at 0.6% or 1.0%. As replicate fatigue tests were not conducted in this study, the authors plan to investigate this phenomenon further in future work.
Figure 11.
Symmetry ratios of AZ80 magnesium alloys at different strain levels.
The differences in grain size and basal texture across the different forming routes dictate the extent of twinning–detwinning activation under cyclic loading and thus govern the hysteresis loop symmetry. As-cast AZ80-C has no processing texture; the grain orientation is random, and cyclic plastic deformation relies solely on basal and prismatic dislocation slip without twinning involvement. Consequently, the steady-state hysteresis loop symmetry factor remains between 0.94 and 1.05, and the curve is approximately centrosymmetric.
Multi-directional-forged AZ80-F has the weakest basal texture. At low strain amplitudes (≤0.5%), cyclic loading struggles to reach the critical resolved shear stress for twinning, and dislocation slip dominates deformation, resulting in approximately symmetric hysteresis. When the strain amplitude exceeds 0.6%, large plastic deformation induces the formation of numerous twins; complete detwinning cannot be achieved during the tensile stage, leaving irreversible twins in the matrix. Hysteresis asymmetry increases significantly, with the symmetry factor abnormally rising to 1.33 at a strain amplitude of 0.8%.
Both the single-extrusion AZ80-E and the forging–extrusion composite AZ80-FE exhibit medium-to-high basal texture strength. Tensile twinning can be initiated under low stress during the compression half-cycle, while only partial detwinning occurs during the tensile half-cycle. Residual twin boundaries and dislocation pileups within twins persist throughout the cycle, resulting in significant hysteresis asymmetry across the entire strain range, with a yield plateau appearing in the compression segment. Compared with AZ80-E, AZ80-FE has finer grains and a more uniformly dispersed second phase. The finer grains can disperse stress concentrations at twin boundaries, mitigating irreversible twinning damage to some extent. The overall symmetry factor is higher than that of the single-extrusion specimen, demonstrating that grain refinement and texture weakening can synergistically improve the asymmetric characteristics of the cyclic hysteresis in magnesium alloys.
Notably, for AZ80-F at a strain amplitude of 0.8%, the SR abnormally increases to 1.33, and the maximum tensile stress is much lower than the corresponding maximum compressive stress. As shown in Figure 8f, the AZ80-F-0.8% specimen exhibits a lower degree of strain hardening in tension, and the maximum tensile stress is only slightly higher than that of the AZ80-F-0.4% specimen, whereas the maximum compressive stress is higher than that of the AZ80-F-1.0% specimen.
3.2.2. Cyclic Deformation Response
Figure 12 shows the evolution of the maximum tensile and compressive stresses of the AZ80 magnesium alloys. All AZ80 alloys processed by different methods exhibit pronounced cyclic hardening in both tensile and compressive stresses. The stress first increases with the number of loading cycles. After a certain number of cycles, the stress of some samples enters a stable stage and maintains a relatively constant value. Subsequently, as damage accumulates, the sample cracks, and the stress amplitude decreases rapidly until complete failure. This pronounced hardening is attributed to the activation of non-basal slip at high strain amplitudes [39,40]. The interaction between residual twins and basal/non-basal slip causes a large number of dislocations to accumulate at grain and twin interfaces, forming dislocation pileups, which enhances the material’s resistance to plastic deformation and leads to a higher cyclic hardening rate at high strain amplitudes [41].
Figure 12.
Stress amplitude of each hysteresis loop for AZ80 magnesium alloys at different strain levels: (a) AZ80-C; (b) AZ80-F; (c) AZ80-E; (d) AZ80-FE.
3.2.3. Plastic Strain Energy Density for Each Hysteresis Loop
Figure 13 presents the evolution of the plastic strain energy density (PSED, the area of the hysteresis loop) of AZ80 magnesium alloys processed by different methods. As shown in Figure 13a, the PSED of AZ80-C increases with increasing strain amplitude due to the increase in plastic strain. For the same specimen, PSED also increases with the number of loading cycles. For specimens tested at small strain amplitudes, the increase in plastic strain per loading cycle is not significant; therefore, the PSED changes very little. However, for specimens tested at large strain amplitudes, the plastic strain in each loading cycle is substantial, and under the influence of cyclic hardening, the hysteresis loop gradually expands with increasing loading cycles.
Figure 13.
Plastic strain energy density of each hysteresis loop for AZ80 magnesium alloys at different strain levels: (a) AZ80-C; (b) AZ80-F; (c) AZ80-E; (d) AZ80-FE.
For the other specimens, because processes such as forging or extrusion significantly affect the material’s microstructure and macroscopic mechanical behavior, the PSED is lower than that of AZ80-C under the same conditions. Furthermore, due to the influence of cyclic damage, the PSED of specimens tested at large strain amplitudes (e.g., 1.0%) reaches a peak before fatigue fracture and then decreases with increasing loading cycles. This phenomenon is particularly evident in the AZ80-E specimens (0.8% and 1.0%), which explains why AZ80-E exhibits a longer fatigue life, despite AZ80-E and AZ80-FE having similar strengths.
4. Prediction Models
4.1. Fatigue Life
Figure 14a summarizes the fatigue life versus strain amplitude data for AZ80 magnesium alloys processed by different methods. At the same strain amplitude, AZ80-E and AZ80-FE exhibit a longer fatigue life than the control group AZ80-C. Meanwhile, AZ80-C exhibits a longer fatigue life than AZ80-F, except at strain amplitudes of 0.4% and 0.6%. This indicates that the forming processes significantly affect the fatigue life of AZ80 magnesium alloy. In addition, Figure 14b compares the fatigue life data of AZ80 magnesium alloys from published studies with the test data obtained in this study. Although direct comparison is complicated by differences in processing conditions, the figure shows that the test results reported in the literature within the strain amplitude range of 0.4% to 1.0% mostly fall within the envelope of the present test results.
Figure 14.
Fatigue life of AZ80 magnesium alloy produced by different forming methods: (a) fatigue life vs. strain range; (b) comparison with the published data.
4.2. Fatigue Life Model and Prediction
The strain-based Smith–Watson–Topper (SWT) model [42] and the energy-based Jahed–Varvani (JV) model [43] are commonly used to predict the fatigue life of magnesium alloys, as shown in Equations (1) and (2). However, obtaining the fatigue life for a given strain amplitude (∆ε/2) or total strain energy density (∆E) is not straightforward, because both formulas are implicit equations with respect to fatigue life (Nf).
where Es is the Young’s modulus of the material, , , b, c, , , B, and C are parameters of the SWT and JV models, respectively.
To facilitate the determination of fatigue life, a log–log multi-linear explicit equation (Equation (3)) is proposed to describe the relationship between fatigue life and strain amplitude. The number of sub-linear segments depends on the test data.
where ai, ki, and are material parameters.
Figure 15 presents a comparison of the tested and predicted fatigue lives of AZ80 magnesium alloys processed by different methods. For all four types of AZ80 magnesium alloys, a single linear relationship cannot adequately describe the relationship between fatigue life and strain amplitude; therefore, a bilinear equation was adopted. The fitting results are summarized in Table 2. As shown in Figure 15, the proposed formula is in good agreement with the tested fatigue lives of all four types of AZ80 magnesium alloys, indicating that the proposed formula can be used to predict the fatigue life of AZ80 magnesium alloys.
Figure 15.
Comparisons of experimental and predicted fatigue life: (a) AZ80-C and AZ80-F; (b) AZ80-E and AZ80-FE.
Table 2.
Summary of the bilinear fitting parameters.
5. Conclusions
In this study, the authors experimentally investigated the effect of forming methods on the hysteresis behavior of AZ80 magnesium alloy. The main conclusions are as follows:
- (1)
- The four AZ80 magnesium alloys processed by different methods exhibit pronounced tension–compression anisotropy, with the ultimate compressive strength exceeding the corresponding ultimate tensile strength by more than 20%. Compared with the control material (as-cast AZ80), multi-directional forging (AZ80-F) has a marginal effect on the tensile yield strength, ultimate tensile strength, and fracture strain, but increases the compressive strength. In contrast, both extrusion (AZ80-E) and multi-directional forging followed by extrusion (AZ80-FE) significantly increase both the tensile and compressive strengths, with AZ80-FE exhibiting slightly higher strengths than AZ80-E.
- (2)
- Hot extrusion or hot multi-directional forging followed by extrusion offers a clear advantage: the finest and most uniform grains, the weakest basal texture, and the most uniformly dispersed nanoscale β phase, leading to better mechanical and fatigue performance than AZ80-F and AZ80-C.
- (3)
- The three types of AZ80 alloys processed by different methods show varying degrees of hysteresis asymmetry, particularly at large strain amplitudes, due to the partial twinning–detwinning mechanism. The symmetry ratio (SR) provides a reliable quantitative metric for evaluating this asymmetry.
- (4)
- A log–log multi-linear explicit equation is proposed to describe the relationship between fatigue life and strain amplitude. Comparison of the tested and predicted results shows that the proposed formula can accurately predict the fatigue life of AZ80 magnesium alloy across all forming methods, with R2 values exceeding 0.98 for three of the four materials. However, for AZ80-F, due to the large standard deviation (0.412), more fatigue tests are necessary to recalibrate the parameters.
Author Contributions
Methodology, C.-H.R.; validation, J.T.; formal analysis, H.X., C.-H.R. and L.S.; investigation, L.-C.F. and C.-H.R.; writing—original draft preparation, H.X. and L.S.; writing—review and editing, J.T.; visualization, C.-P.L.; supervision, C.-P.L.; project administration, L.-C.F.; funding acquisition, J.S. All authors have read and agreed to the published version of the manuscript.
Funding
This research was funded by the Jinhua Science and Technology Program of China (grant number 2026-1-082), the National Key R&D Program of China (grant number 2022YFB3709300), the Chongqing Vocational Education Teaching Reform Research Project (grant numbers Z2253101, Z2253102, Z211014, GZ222033), the Academician in Key Research and Development Plan of Sichuan Province (grant number 2024YFHZ0118), the Natural Science Foundation Commission of Chongqing (grant number 2024ZX039), the Chongqing Education Commission Scientific and Techno-logical Research Project (grant numbers KJQN202203414, KJQN202103409).
Data Availability Statement
The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding authors.
Conflicts of Interest
The authors declare no conflict of interest.
Appendix A
- (1)
- OM: The specimens used for metallographic examination shared exactly the same geometric specifications as those used for chemical composition analysis: rectangular blocks measuring 7 mm × 5 mm × 3 mm. An Axio Vert A1 inverted optical microscope (OM, Carl Zeiss AG, Oberkochen, Germany) was employed for image acquisition and microstructural characterization. Prior to observation, the specimens underwent a comprehensive, progressive wet-grinding process using silicon carbide (SiC) abrasive papers with grit sizes of 60#, 400#, 800#, 1200#, 2000#, and 4000#, proceeding from coarse to fine grinding. At each change of grit size, the specimen was rotated 90° relative to the previous grinding direction to ensure cross-grinding; the process continued until no grinding scratches were visible to the naked eye on the surface treated with 4000# paper, at which point the specimen was ready for polishing. Following wet grinding, mechanical fine polishing was performed using a specialized metallographic polishing cloth and a 0.25 μm diamond spray suspension, continuing until the specimen surface achieved a mirror-like finish free of visible scratches. After polishing, the specimen was thoroughly rinsed with anhydrous ethanol to remove residual polishing media and then dried with a stream of cold air. Finally, the specimens underwent chemical etching to reveal microstructural features—such as grains and secondary phases—through contrast differences. The etching reagent was prepared with the following volume fractions: 1% concentrated nitric acid, 20% glacial acetic acid, 20% deionized water, and 60% ethylene glycol; the immersion time was controlled within the range of 30 to 60 s. After the etched specimens were cleaned and dried, multi-scale micrographs of the microstructure were recorded using an optical microscope by switching between objective lens magnifications of 100×, 200×, and 500×.
- (2)
- SEM: In this study, a JEOL JSM-7800F field-emission scanning electron microscope (FESEM, JEOL Ltd., Akishima, Tokyo, Japan) equipped with an integrated energy-dispersive spectrometer (EDS, JEOL Ltd., Akishima, Tokyo, Japan) was utilized for comprehensive microstructural characterization. This system enabled the observation of surface morphologies and the quantitative analysis of the geometric dimensions and spatial distribution of intermetallic secondary phases. Additionally, the EDS module facilitated both point elemental analysis and full-area elemental mapping, allowing for the precise determination of the elemental composition and phase identity of various precipitated secondary phases. The system also enabled high-resolution observation of fracture surfaces from tensile-tested specimens; by analyzing fracture features, the dominant failure mechanism—whether ductile or brittle—was identified, thereby elucidating the underlying role of alloying elements in modulating the material’s plastic deformation behavior. Prior to FESEM characterization, specimen preparation followed the same protocol used for optical metallography, involving sequential water-based grinding followed by mechanical mirror polishing. After polishing, the observation surface was lightly etched using a solution of 4 vol% nitric acid in anhydrous ethanol. Following etching, specimens were rinsed with running water to remove residual etchant, rinsed again with anhydrous ethanol to remove water, thoroughly dried with a cold air stream, and sealed in bags for storage. Standardized operating parameters were maintained for all SEM observations: an accelerating voltage of 20 kV and a working distance of 10 mm between the electron beam and the specimen surface.
- (3)
- EBSD: Specimens dedicated to EBSD analysis were prepared as custom rectangular blocks measuring 7 mm in length, 5 mm in width, and 3 mm in thickness. These specimens underwent a comprehensive, progressive wet-grinding process using silicon carbide abrasive papers with grit sizes of 60#, 400#, 800#, 1200#, 2000#, and 4000#, proceeding from coarse to fine grinding. At each transition between grit sizes, the specimen was rotated 90° relative to the previous grinding direction to ensure cross-grinding, continuing until no grinding scratches were visible to the naked eye on the surface intended for observation. Following the mechanical grinding stages, chemical etching was omitted in favour of electropolishing using a specialized AC2 electrolyte solution; this step removed the surface layer of plastic deformation, thereby ensuring the clarity of diffraction patterns and a high rate of data indexing.
- (4)
- Mechanical tests (tension, compression, and fatigue): All specimen machining specifications and end-face pretreatment procedures adhered to national standards for low-cycle fatigue testing of metallic materials. The dimensions of the gauge section were consistent with the proportional specimens used in the aforementioned room-temperature tensile tests, and the gripping sections featured radiused transitions to prevent premature failure caused by stress concentrations at the grips. The final surface roughness of fatigue samples was 0.78 (average).
References
- Liu, W.; Yang, Y.; Duan, W.; Bao, J.; Yuan, M.; Zhao, Z.; Cui, J.; Zhang, Z. Scalable Dc Casting of Large-Size AZ80 Magnesium Alloy Slab under out-of-Phase Pulsed Magnetic Field: Experiment and Simulation. J. Mater. Res. Technol. 2024, 31, 1864–1870. [Google Scholar] [CrossRef] [Scilit]
- Žagar, S.; Soyama, H.; Markoli, B.; Naglič, I.; Šturm, R. Enhancing the Surface Strength of Magnesium Alloy AZ80 through Cavitation Peening. Mater. Des. 2025, 255, 114229. [Google Scholar] [CrossRef] [Scilit]
- Xia, L.; Zheng, J.; Wang, Q. Creep Deformation Mechanism and Microstructure Evolution of Mg-3Sm-0.5Zn-0.4Zr Alloy. Sci. Sin. Technol. 2024, 54, 1079–1090. [Google Scholar] [CrossRef] [Scilit]
- Koltygin, A.V.; Bazhenov, V.E.; Belova, E.A.; Nikitina, A.A. Development of a Magnesium Alloy with Good Casting Characteristics on the Basis of Mg-Al-Ca-Mn System, Having Mg–Al2Ca Structure. J. Magnes. Alloys 2013, 1, 224–229. [Google Scholar] [CrossRef] [Scilit]
- Yang, Y.; Xiong, X.; She, J.; Yuan, Y.; Tan, S.; Lu, Y.; Yao, W.; Chen, X.; Zhou, X.; Peng, X.; et al. Research advances of magnesium and magnesium alloys worldwide in 2025. J. Magn. Alloys 2026, 24, 102355. [Google Scholar] [CrossRef] [Scilit]
- Azqadan, E.; Arami, A.; Jahed, H. From Microstructure to Mechanical Properties: Image-Based Machine Learning Prediction for AZ80 Magnesium Alloy. J. Magnes. Alloys 2025, 13, 4231–4244. [Google Scholar] [CrossRef] [Scilit]
- Zhao, X.; Gao, P.; Zhang, Z.; Wang, Q.; Yan, F. Fatigue Characteristics of the Extruded AZ80 Automotive Wheel. Int. J. Fatigue 2020, 132, 105393. [Google Scholar] [CrossRef] [Scilit]
- Liao, Q.; Jiang, Y.; Le, Q.; Hu, W.; Zhou, X.; Li, D.; Li, Y. The Evolution of Microstructure and Texture of AZ80 and AZ80-Lamm Magnesium Alloy Wheel Hubs Processed by Single-Pass Radial Forging. J. Mater. Res. Technol. 2023, 22, 2473–2488. [Google Scholar] [CrossRef] [Scilit]
- Jiang, R.; Wang, R.; Ding, B.; Zhang, Z. Effects of T6 Treatment on the Microstructure and Mechanical Properties of Az80 Magnesium Alloy. J. Phys. Conf. Ser. 2024, 2730, 12040. [Google Scholar] [CrossRef] [Scilit]
- Wang, P.; Lin, C.; Huang, T.; Lin, H.; Lee, Y.; Yeh, M.T.; Wang, J.Y. Effects of 2 Mass% Li Addition on the AZ80 Mg Alloy. Mater. Trans. 2008, 49, 913–917. [Google Scholar] [CrossRef] [Scilit]
- Todkar, U.; Somasundaram, M.; NarendraKumar, U.; Muthuchamy, A.; Annamalai, A.R. Investigating the Impact of Heat Treatment on the Tribological Behaviour of AZ80 Magnesium Alloy at High Temperatures. Results Eng. 2024, 21, 101661. [Google Scholar] [CrossRef] [Scilit]
- Li, X.; Wang, Q.; Fang, Q.; Zhang, Z. Study on Cavity Evolution of AZ80 Magnesium Alloy during Rotary Extrusion. JOM 2022, 75, 470–477. [Google Scholar] [CrossRef] [Scilit]
- Jiang, J.; Wang, Y.; Qu, J.; Du, Z.; Luo, S. Preparation and Thixoforging of Semisolid Billet of AZ80 Magnesium Alloy. Trans. Nonferrous Met. Soc. China 2010, 20, 1731–1736. [Google Scholar] [CrossRef] [Scilit]
- Zhang, Z.; Le, Q.; Cui, J. Microstructures and Mechanical Properties of AZ80 Alloy Treated by Pulsed Ultrasonic Vibration. Trans. Nonferrous Met. Soc. China 2008, 18, s113–s116. [Google Scholar] [CrossRef] [Scilit]
- Azqadan, E.; Uramowski, J.; Roostaei, A.A.; Behravesh, S.B.; Javaid, A.; Williams, B.W.; Wells, M.A.; Jahed, H. The Effect of Cooling Rate and Degassing on Microstructure and Mechanical Properties of Cast AZ80 Magnesium Alloy. Mater. Sci. Eng. A 2022, 844, 143176. [Google Scholar] [CrossRef] [Scilit]
- Chen, F.; Jiang, S.; Chen, Z.; Liu, C. Effects of Heat Treatment on Microstructure and Tensile Mechanical Properties of Isothermal Die Forged AZ80–Ag Casing with Large Size. Trans. Nonferrous Met. Soc. China 2023, 33, 2340–2350. [Google Scholar] [CrossRef] [Scilit]
- Zhang, Z.; Yuan, L.; Zheng, M.; Wei, Q.; Shan, D.; Guo, B. Achievement of High Strength and Good Ductility in the Large-Size AZ80 Mg Alloy Using a Designed Multi-Directional Forging Process and Aging Treatment. J. Mater. Process. Technol. 2023, 311, 117828. [Google Scholar] [CrossRef] [Scilit]
- Wang, Q.; Zhang, Z.; Zhang, X.; Li, G. New Extrusion Process of Mg Alloy Automobile Wheels. Trans. Nonferrous Met. Soc. China 2010, 20, s599–s603. [Google Scholar] [CrossRef] [Scilit]
- Zhou, X.; Zhang, J.; Chen, X.; Zhang, X.; Li, M. Fabrication of High-Strength AZ80 Alloys via Multidirectional Forging in Air with No Need of Ageing Treatment. J. Alloys Compd. 2019, 787, 551–559. [Google Scholar] [CrossRef] [Scilit]
- Yin, D.; Chen, X.; Wang, J. Microstructure and Toughness of an AZ80 Mg Alloy Processed by Ecap and Ageing Treatment. Mater. Sci. Forum 2010, 667, 475–480. [Google Scholar] [CrossRef] [Scilit]
- Wang, Z.; Zhao, G.; Zhang, S.; Deng, Y. Constitutive Equation of AZ80 Magnesium Alloy at Thermal Deformation. Appl. Mech. Mater. 2011, 148–149, 762–765. [Google Scholar] [CrossRef] [Scilit]
- Cai, G.; Huang, X.; Deng, P. Effects of Thermomechanical Treatment Process on the Microstructure and Properties of AZ80 Magnesium Alloy. Adv. Mater. Res. 2011, 179–180, 354–358. [Google Scholar] [CrossRef] [Scilit]
- Liu, Y.; Zhou, J.; Zhan, C.; Tang, S.; Yang, Y. Tensile Deformation Behaviour of Magnesium Alloy AZ80 at High Temperatures. Mater. Res. Innov. 2014, 18, 148. [Google Scholar] [CrossRef] [Scilit]
- Chen, L.; Jiang, N.; Meng, L.; Fang, C.; Zhang, X. Effect of Re Element Nd on Microstructure and Mechanical Properties of AZ80 Magnesium Alloy. Spec. Cast. Nonferrous Alloys 2017, 37, 576–580. [Google Scholar]
- Daud, Z.C.; Azahar, S.H.; Derman, M.N.; Adzali, N.M.S.; Zaidi, N.H.A.; Adnan, S.A. The Effect of Aging Time on Microstructure and Hardness Value of AZ80 Mg Alloy. IOP Conf. Ser. Mater. Sci. Eng. 2020, 957, 012051. [Google Scholar] [CrossRef] [Scilit]
- Zhao, X.; Gao, P.; Chen, G.; Wei, J.; Zhu, Z.; Yan, F.; Zhang, Z.; Wang, Q. Effects of Aging Treatments on Low-Cycle Fatigue Behavior of Extruded AZ80 for Automobile Wheel Disks. Mater. Sci. Eng. A 2021, 799, 140366. [Google Scholar] [CrossRef] [Scilit]
- Salevati, M.A.; Imam, A.; Seifi, R.; Akbaripanah, F. The Effect of Repeated Upsetting Process on Microstructure, Shear Strength, and Fracture Toughness of Sic/AZ80 Nanocomposite. J. Mater. Eng. Perform. 2022, 31, 560–575. [Google Scholar] [CrossRef] [Scilit]
- He, Y.; Gao, M.; Zhao, X.; Ren, X.; Wu, Y.; Cheng, Y.; Dong, B.; Bai, S.; Zhang, Z.; Wu, S.; et al. Effect of Twinning and Precipitation on Low-Cycle Fatigue Damage Behaviour of Extruded AZ80 Magnesium Alloy. Mater. Sci. Eng. A 2023, 863, 144360. [Google Scholar] [CrossRef] [Scilit]
- Xiong, Y.; Jiang, Y. Cyclic Deformation and Fatigue of Rolled AZ80 Magnesium Alloy Along Different Material Orientations. Mater. Sci. Eng. A 2016, 677, 58–67. [Google Scholar] [CrossRef] [Scilit]
- Wang, C.; Luo, T.; Yang, Y. Low Cycle Fatigue Behavior of the Extruded AZ80 Magnesium Alloy under Different Strain Amplitudes and Strain Rates. J. Magnes. Alloys 2016, 4, 181–187. [Google Scholar] [CrossRef] [Scilit]
- Gungor, A.; Incesu, A.L.P.E.R. Effects of alloying elements and thermomechanical process on the mechanical and corrosion properties of biodegradable Mg alloys. J. Magnes. Alloys 2021, 9, 241–253. [Google Scholar] [CrossRef] [Scilit]
- GB/T 228.1-2010; Metallic Materials—Tensile Testing—Part 1: Method of Test at Room Temperature. Standards Press of China: Beijing, China, 2010.
- He, Y.-Y.; Bai, S.-W.; Fang, G. Coupled CA-FE simulation for dynamic recrystallization of magnesium alloy during hot extrusion. J. Magnes. Alloys 2022, 10, 769–785. [Google Scholar] [CrossRef] [Scilit]
- GB/T 145-2001; Center Holes. Standards Press of China: Beijing, China, 2001.
- GB/T 7314-2017; Metallic Materials―Compression Test Method at Room Temperature. Standards Press of China: Beijing, China, 2017.
- GB/T 15248-2008; The Test Method for Axial Loading Constant-Amplitude Low-Cycle Fatigue of Metallic Materials. Standards Press of China: Beijing, China, 2008.
- Xiong, Y.; Yu, Q.; Jiang, Y. An Experimental Study of Cyclic Plastic Deformation of Extruded ZK60 Magnesium Alloy under Uniaxial Loading at Room Temperature. Int. J. Plast. 2014, 53, 107–124. [Google Scholar] [CrossRef] [Scilit]
- Dong, S.; Yu, Q.; Jiang, Y.; Dong, J.; Wang, F.; Jin, L.; Ding, W. Characteristic Cyclic Plastic Deformation in ZK60 Magnesium Alloy. Int. J. Plast. 2017, 91, 25–47. [Google Scholar] [CrossRef] [Scilit]
- Li, H.; Lv, F.; Xiao, Z.; Liang, X.; Sang, F.; Li, P. Low-Cycle Fatigue Behavior of a Cast Mg–Y–Nd–Zr Alloy by T6 Heat Treatment. Mater. Sci. Eng. A 2016, 676, 377–384. [Google Scholar] [CrossRef] [Scilit]
- Morrow, B.M.; McCabe, R.J.; Cerreta, E.K.; Tomé, C.N. In-Situ Tem Observation of Twinning and Detwinning during Cyclic Loading in Mg. Metall. Mater. Trans. A 2014, 45, 36–40. [Google Scholar] [CrossRef] [Scilit]
- Yu, Q.; Zhang, J.; Jiang, Y.; Li, Q. An Experimental Study on Cyclic Deformation and Fatigue of Extruded ZK60 Magnesium Alloy. Int. J. Fatigue 2012, 36, 47–58. [Google Scholar] [CrossRef] [Scilit]
- Pahlevanpour, A.H.; Karparvarfard, S.M.; Shaha, S.K.; Behravesh, S.B.; Adibnazari, S.; Jahed, H. Anisotropy in the Quasi-Static and Cyclic Behavior of ZK60 Extrusion: Characterization and Fatigue Modeling. Mater. Des. 2018, 160, 936–948. [Google Scholar] [CrossRef] [Scilit]
- Karparvarfard, S.M.H.; Shaha, S.K.; Behravesh, S.B.; Jahed, H.; Williams, B.W. Fatigue Characteristics Modeling of Cast Cast-Forged ZK60 Magnesium Alloy. Int. J. Fatigue 2019, 118, 282–297. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.