Abstract
Thick-section 20Cr11W2VTaSi (SIMP) martensitic heat-resistant steel is used in high-temperature structural components, yet the effects of tungsten inert gas (TIG) heat input on residual stress and distortion remain insufficiently quantified. A sequentially coupled thermal–mechanical finite element model was developed for a 20 mm thick V-groove butt joint and validated against the measured fusion zone at 470 J/mm, with a mean absolute relative deviation of 12.4%. Heat input was varied from 350 to 700 J/mm. Peak temperature, fusion-zone width, penetration depth, and the cooling time from 800 to 500 °C (t8/5) increased with heat input, while peak von Mises stress changed only slightly (539.6–535.7 MPa). The high-stress region and path stresses, however, were redistributed. Maximum free-edge transverse shrinkage increased from 0.38 to 0.70 mm, whereas longitudinal displacement changed only from 0.30 to 0.35 mm. Post-weld heat treatment (PWHT) at 720 °C for 4 h reduced the 99th-percentile von Mises stress by 43–49%. The 470 J/mm joint satisfied the room- and elevated-temperature tensile and impact requirements of GB/T 38875-2020. These results support heat-input and PWHT selection for thick-section SIMP steel welds.
1. Introduction
SIMP (20Cr11W2VTaSi) martensitic heat-resistant steel is a silicon-containing ferritic/martensitic grade developed from conventional 9Cr–12Cr steels by adjusting the C, Cr, W, and Ta contents and adding Si. It was designed for high-temperature pressure-boundary components in accelerator-driven subcritical (ADS) systems and advanced nuclear reactors [1]. At 550–650 °C, it combines high creep rupture strength with resistance to irradiation swelling and liquid-metal corrosion, making it a candidate material for main-steam piping in ultra-supercritical units and internals of fourth-generation nuclear reactors [2,3].
The high alloy content and hardenability of SIMP steel, however, promote δ-ferrite retention and brittle Laves-phase precipitation in fusion-welded joints, which can degrade toughness and high-temperature performance. Studies of SIMP steel joining have therefore focused on transient liquid-phase (TLP) diffusion bonding, with attention to bonding temperature, pressure, and post-weld heat treatment (PWHT) [4,5,6]. Tungsten inert gas(TIG) welding of low-activation ferritic/martensitic steels is also sensitive to process parameters [7]. TLP bonding requires precise faying-surface preparation, long holding times, and specialized equipment. TIG welding, in contrast, provides a stable arc, adjustable heat input, flexible operation, and good bead formation, and is therefore well suited to the fabrication and repair of thick-walled nuclear components and complex structures [8,9].
Finite element analysis has been used to predict weld-pool geometry and temperature distributions during TIG welding of modified 9Cr–1Mo steel [10]. Residual stress and distortion arise from localized, non-uniform thermal cycles and can reduce load-bearing capacity, corrosion resistance, and dimensional accuracy [11,12]. Heat input is a principal adjustable parameter in TIG welding because it controls peak temperature, cooling rate, and weld-pool size, and thereby affects microstructure, residual stress, and distortion [13]. For nuclear martensitic heat-resistant steels, Yin et al. used ANSYS to simulate CLAM steel TIG welding in three dimensions. Both weld layers penetrated the plate; transverse stress was compressive at the arc-start and arc-stop ends and tensile in the middle, longitudinal stress was predominantly tensile, and angular distortion from the cover pass exceeded that from the root pass [14]. Zhu et al. combined experiments and FE analysis for a 5 mm thick CLAM steel butt joint and identified angular distortion as the dominant residual deformation [7]. Miao et al. calibrated a heat-source model for a T91 pipeline girth weld in SYSWELD and found the maximum residual stress in the outer heat-affected zone (HAZ), 5–10 mm from the weld center [15]. Deng and Murakawa modeled multi-pass pipe welds, and Zubairuddin et al. modeled modified 9Cr–1Mo plates. Both studies reported that martensitic transformation affects stress evolution and that thermal–mechanical models can reproduce measured temperature, stress, and distortion trends [12,16]. Asadi et al. modeled multi-pass TIG welding of SUS304 stainless-steel pipe and showed that heat input alters the residual-stress state on the inner and outer surfaces by changing the thermal field [13].
This study examines a 20 mm thick SIMP steel TIG butt joint using a sequentially coupled thermal–mechanical FE model developed in ABAQUS 2022. It quantifies the effects of heat input on the temperature field, residual-stress distribution, and welding distortion, and provides a basis for selecting heat input for thick-section SIMP steel.
2. Finite Element Model
2.1. Geometric Model and Mesh
The joint was a 20 mm thick SIMP steel TIG butt weld. Each plate measured 150 × 600 × 20 mm, giving a joint width of 300 mm after assembly. A 60° V-groove was used with a 1 mm root face and a 2.5 mm root gap. Figure 1 shows the assembly and dimensions of the joint.
Figure 1.
Assembly of the V-groove butt joint (dimensions in mm).
Because the joint geometry and loading are symmetric about the weld centerline, a half-model was built along this plane. The welded region was represented by a 100 mm length, giving a model of 100 × 150 × 20 mm. Modeling all 24 layers and 110 passes was impractical; following the principles of merging passes within a layer, merging adjacent layers with similar thermal histories, and retaining the cover layer [15], the half-model was simplified to 10 layers and 16 passes. The passes were deposited from the root to the cover in the simplified sequence. For each merged pass, the equivalent heat input was defined by energy conservation, as the heat input of the real passes that the simulated pass replaces, so that the energy deposited per unit length is preserved; no adjustment was made to bring the temperature or stress field closer to that of the 110-pass sequence. The single-pass reference welding parameters were kept fixed. For each merged pass, the heat-source semi-axes b and c were enlarged to match the cross-section of the merged bead. The heat-flux amplitude was scaled so that the energy deposited per unit length equaled the sum of the heat inputs of the actual passes it replaced, or k times the single-pass heat input for a merged pass representing k actual passes.
The mesh was generated in HyperMesh 2021. Elements measured 0.3–0.5 mm in the weld and HAZ and increased to about 5 mm away from the weld. DC3D8 elements were used for heat transfer, and the same mesh was converted to C3D8R elements for mechanical analysis. The model contained 175,934 nodes and 166,400 elements. Figure 2 shows the finite element mesh and the deposition order of the passes. The colors in the weld region distinguish the modeled passes, and the numbers 1–16 indicate their deposition order.
Figure 2.
Finite element mesh and deposition order of the passes.
2.2. Material Properties
The accuracy of the thermal and mechanical solutions depends strongly on high-temperature material properties. Published data for SIMP steel remain incomplete, so density, specific heat, thermal conductivity, Young’s modulus, yield strength, coefficient of thermal expansion, and Poisson’s ratio were calculated with JMatPro from the chemical composition in Table 1.
Table 1.
Chemical composition of the SIMP steel (wt.%).
Figure 3 shows the calculated temperature-dependent properties. To limit parameter fluctuations in the transformation interval and stabilize the FE solution, the thermophysical and mechanical property curves were piecewise smoothed and interpolated so that each property varied continuously above the solidus.
Figure 3.
Temperature-dependent properties of SIMP steel: (a) thermophysical properties and (b) mechanical properties.
2.3. Heat-Source Model
The heat-source model defines the spatial distribution of arc energy and therefore controls the predicted weld-pool shape and temperature field. For the 20 mm thick TIG weld, a Goldak double-ellipsoidal heat source [17] was used. The arc heat flux was divided into front and rear half-ellipsoids to represent its asymmetric distribution along the welding direction. The front and rear heat-flux densities are given by Equations (1) and (2), respectively.
Front half-ellipsoid heat flux:
Rear half-ellipsoid heat flux:
where af, ar, b, and c are the front semi-axis, rear semi-axis, half-width, and depth of the heat source; and ff and fr are the heat-fraction factors for the front and rear half-ellipsoids, with ff + fr = 2.
The effective arc power, Q, is
The heat input per unit length, E, is
In Equation (3), η is the arc thermal efficiency, taken as 0.65–0.75 for manual TIG welding [8]; U is the arc voltage; I is the welding current; and Q is the effective arc power. In Equation (4), E is the heat input, and v is the welding speed.
In ABAQUS, Equations (1) and (2) were implemented through a DFLUX user subroutine. At each increment, the subroutine calculated the local heat flux from the current source position and the integration-point coordinates and applied it to the corresponding element faces, thereby modeling the moving heat source. For a merged pass, the same subroutine was used with the enlarged source dimensions and the scaled flux amplitude described in Section 2.1, so that the energy deposited per unit length equals the equivalent line energy of that pass.
2.4. Boundary Conditions
During welding, the workpiece loses heat by convection and radiation, described by Equations (5) and (6). Convective loss depends on the temperature difference between the surface and the environment, whereas radiative loss increases with the fourth power of temperature and becomes important for cooling of the weld pool and near-weld region. Including both mechanisms avoids overestimating the peak temperature and high-temperature dwell time.
Convective heat transfer was described by Newton’s law of cooling:
Radiative heat transfer was described by the Stefan–Boltzmann law:
where hc is the convective heat-transfer coefficient, ε is the surface emissivity, σ is the Stefan–Boltzmann constant, T is the surface temperature, and T0 is the ambient temperature. To balance accuracy and computational cost, radiation was represented by an equivalent temperature-dependent convective coefficient [12].
In the mechanical analysis, only the minimum constraints required to suppress rigid-body motion were applied: three nodes at one end of the plate were fixed in Ux, Uy, and Uz, and Ux = 0 was imposed on the symmetry plane. No additional clamping was introduced, so the predicted distortion corresponds to free welding. The mechanical analysis was sequentially coupled to the thermal analysis: the nodal temperatures of the thermal solution were transferred to the same mesh, converted from DC3D8 to C3D8R elements, and applied as a predefined field at every mechanical increment, the mechanical dissipation being neglected because it is small compared with the arc power. The material was treated as an isotropic elasto-plastic von Mises solid with isotropic hardening and the temperature-dependent properties of Figure 3b, and the same constitutive description and the same minimum constraints were used in the PWHT analysis, which was continued from the as-welded state. Stresses and displacements were extracted as element-nodal values along paths on the transverse section at mid-length and on a longitudinal section along the weld centerline. The transverse paths were located at the top surface, 10 mm above the bottom surface, and at the bottom surface. Because the largest nodal values are located at a few nodes at the arc stop and at the groove root and are therefore mesh-dependent, the high-stress level is characterized additionally by the 99th-percentile von Mises stress over the nodes of the weld region, that is, by the value exceeded by 1% of those nodes.
2.5. Welding Parameters
Published process data for thick-section SIMP steel TIG welding under comparable conditions are limited. Process data for TIG welding of modified 9% Cr martensitic heat-resistant steel were therefore used as a reference [10]. With the welding power held at P = 1000 W and the thermal efficiency at η = 0.70, three heat inputs of 700, 470, and 350 J/mm were examined. Table 2 lists the process parameters.
Table 2.
Welding parameters for the three heat inputs.
3. Results and Discussion
3.1. Effects of Heat Input on Weld-Pool Geometry and Thermal Cycles
Figure 4 shows the weld-pool cross-sections for the three heat inputs. As the heat input decreased from 700 to 350 J/mm, the top-surface fusion-zone width decreased from about 13.9 to 11.6 mm, the fusion-zone width 10 mm above the bottom surface decreased from about 8.1 to 6.7 mm, and the root high-temperature zone decreased from about 4.6 to 2.1 mm. The top-surface width changed less than the mid-depth width and root fusion zone as heat input decreased, indicating that through-thickness penetration decreased faster than the surface bead width. The surface pool is heated directly by the arc and is therefore less sensitive to the heat-input change. In contrast, the root region depends on heat conduction and pool convection; as heat input decreases, the local energy density at the root falls below the fusion threshold first, so root fusion is more sensitive to heat input [11,13].
Figure 4.
Weld-pool profiles at (a) 700, (b) 470, and (c) 350 J/mm.
To quantify the thermal-cycle differences, six sampling nodes A–F were placed 1, 2, 6, 12, 20, and 30 mm from the weld centerline in the transverse section at mid-length. Figure 5 shows the locations of these nodes.
Figure 5.
Locations of sampling nodes A–F.
Figure 6 shows the temperature histories at the sampling nodes during pass w3 and reheating by the adjacent passes. All nodes heated rapidly and cooled more slowly. The closer a node was to the weld, the higher its heating rate and peak temperature. Lower heat input reduced the peak temperature at a given location, shortened the high-temperature dwell, shifted the cooling curves to shorter times, and increased the cooling rate. The combination of less energy per unit length and a shorter residence time of the heat source moved the near-weld cooling path toward lower temperatures and faster cooling [8,12].
Figure 6.
Thermal cycles at the sampling nodes in pass w3 and during reheating at heat inputs of (a) 700, (b) 470, and (c) 350 J/mm.
Table 3 lists the maximum temperature at each node during the full welding sequence. At 470 J/mm, the peak temperature was 1012 °C at 1 mm from the weld centerline, 810 °C at 2 mm, 427 °C at 6 mm, and 80 °C at 30 mm. The rapid lateral decay reflects strong heat conduction in the thick base metal; at greater distances, the temperature is controlled mainly by through-thickness conduction and surface heat loss. At 1 and 2 mm, the peak temperature increased to 1343 and 1083 °C at 700 J/mm and decreased to 935 and 726 °C at 350 J/mm. Beyond 12 mm, the differences among the three cases decreased substantially.
Table 3.
Peak temperatures at the sampling nodes (°C).
The cooling time from 800 to 500 °C, t8/5, was about 45 s at 700 J/mm and 12 s at 470 J/mm for nodes A and B. At 350 J/mm, t8/5 at node A decreased to about 9 s, while the peak temperature at node B was below 800 °C. The shorter t8/5 at lower heat input results from a narrower high-temperature zone, a steeper temperature gradient, faster outward heat conduction, and a shorter dwell time. Low heat input limits grain growth but increases hardenability and susceptibility to cold cracking [11,13].
3.2. Effects of Heat Input on Residual Stress
Figure 7 shows the von Mises residual-stress fields after welding for the three heat inputs. The peak stresses were 535.7, 537.7, and 539.6 MPa at 700, 470, and 350 J/mm, respectively, a difference of about 4 MPa; all were close to the room-temperature yield strength used in the model.
Figure 7.
Von Mises residual-stress fields at (a) 700 J/mm, (b) 470 J/mm, and (c) 350 J/mm.
High stresses were concentrated in the weld, fusion line, and near-weld HAZ and decayed rapidly into the base metal. Compared with the low heat-input cases, the high-stress band at 700 J/mm extended slightly farther in the plate-width and through-thickness directions, but the peak stress did not increase monotonically with heat input. A higher heat input enlarges the high-temperature plastic zone, but it also lowers the flow stress at high temperature and increases reheating by subsequent passes. The peak residual stress is therefore limited by plastic accommodation and overall self-equilibrium. In thick multi-pass V-groove joints, the residual-stress distribution also depends on the filling sequence and transverse restraint and cannot be explained by peak temperature alone [18,19,20].
The non-monotonic variation in the peak stress and of the near-weld tensile peaks described above, and the level of the stresses themselves, are affected by a mechanism that the present model does not contain. SIMP steel is a 10–12% Cr martensitic steel, so the weld metal and the coarse-grained heat-affected zone transform to martensite during cooling, and three transformation effects were omitted. (i) The austenite-to-martensite transformation is accompanied by a dilational strain of the order of one percent between the martensite-start and martensite-finish temperatures, which, for this class of steel, lie at 380–420 °C, that is, at a stage at which the surrounding metal has already cooled and responds essentially elastically; the expansion is therefore partly restrained, it generates compressive plastic strain in the weld metal, and it reduces the longitudinal tensile stress that a purely thermo-mechanical analysis predicts. (ii) The deviatoric stress that exists while the transformation proceeds produces transformation plasticity, which relaxes the stress in the transforming region further [21,22]. (iii) The latent heat released between the martensite-start and martensite-finish temperatures, and the change in the flow stress with the phase fractions modify the thermal and the mechanical response locally [23]. All three effects act in the same direction, so the as-welded tensile stresses computed here are upper estimates: the compressive longitudinal stress of 214 MPa computed at the weld-bead top surface (Figure 8a) would be amplified rather than reduced if the transformation were taken into account. The comparison between the three heat inputs is much less affected, because the three cases were analyzed with the same constitutive assumptions, the same material data, and the same pass sequence. The transformation was omitted because its input data are not available for 20Cr11W2VTaSi: the martensite-start temperature, the transformation strain, and the transformation-plasticity parameters all require dilatometric measurements on the steel and on its weld metal, and adopting the parameters measured on modified 9Cr–1Mo steels would introduce an uncertainty of the same order as the effect being modeled. A coupled transformation model of the type applied to modified 9Cr–1Mo welds [21] is therefore the next step of this work.
Figure 8.
Residual stresses at 470 J/mm: (a) longitudinal and (c) transverse stresses across the plate width; and (b) longitudinal and (d) transverse stresses along the weld, at three through-thickness positions.
Path stresses were extracted from the unclamped 470 J/mm model. Figure 8 shows the resulting longitudinal and transverse stress distributions at the three through-thickness positions.
Figure 8a shows pronounced through-thickness stratification of the longitudinal stress. At the top surface, the weld center was in compression at about 214 MPa; a local tensile peak of about 48 MPa appeared about 6 mm from the centerline, beyond which the stress returned to low-level compression. At 10 mm above the bottom surface, the near-weld tensile peak was about 310 MPa at a distance of about 4.5 mm from the centerline; the stress crossed zero at about 14 mm and remained compressive at about 15–42 MPa across the middle of the plate width. At the bottom surface, the near-weld peak was about 221 MPa at about 5.8 mm from the centerline; the stress changed from tension to compression at about 12 mm and reached about 17–19 MPa in compression farther away. Along the weld (Figure 8b), the path 10 mm above the bottom started at about 101 MPa in compression near the arc start, changed rapidly to about 48 MPa in tension, became slightly compressive in the middle, and reached a compressive peak of about 186 MPa near the arc stop at about 129 mm. The bottom path was tensile in the middle and reached about 311 MPa at about 117 mm. This through-thickness pattern of compression at the top, tension at the bottom, and transition at mid-depth is characteristic of self-equilibrium in thick multi-pass welded joints [19,20].
The through-thickness variation in transverse stress was larger (Figure 8c). At the top surface, the weld center was in compression at about 442 MPa; the stress crossed zero at about 27 mm from the centerline and became weakly tensile farther away. At 10 mm above the bottom, the near-weld stress was tensile at about 181 MPa and decreased monotonically to zero at the free edge. At the bottom surface, the weld center was in compression at about 165 MPa; the stress crossed zero at about 8 mm, reached about 95 MPa in tension near 13 mm, and then decreased. Along the weld (Figure 8d), the top surface was in high compression at about 444–553 MPa. At 10 mm above the bottom, the middle section was tensile at about 138 MPa and the ends were compressive. At the bottom surface, the middle section was compressive at about 81 MPa, and a tensile peak of about 132 MPa appeared at the end. Transverse stress is therefore controlled by bending self-equilibrium through the thickness, the V-groove geometry, and end restraint, and a single surface value cannot represent the whole section [20,24].
Figure 9 compares the path stresses 10 mm above the bottom surface for the three heat inputs.
Figure 9.
Residual stresses 10 mm above the bottom surface at the three heat inputs: (a) longitudinal and (c) transverse stresses across the plate width; and (b) longitudinal and (d) transverse stresses along the weld.
In Figure 9a, the near-weld longitudinal tensile peak at 10 mm above the bottom was highest at 470 J/mm, about 310 MPa, compared with about 128 and 125 MPa at 700 and 350 J/mm. Beyond 20 mm from the weld centerline, the stresses in all three cases decreased to between about 26 MPa in compression and 15 MPa in tension. Along the weld (Figure 9b), heat input had a limited effect on the longitudinal stress in the middle section: the stress was about 161 MPa in compression at 700 J/mm, about 225 MPa in compression at 350 J/mm, and only about 20 MPa in compression at 470 J/mm. These differences arose mainly from the accumulated thermal cycles of successive passes and end restraint rather than from peak temperature alone. In Figure 9c, the near-weld transverse tensile peak at 470 J/mm was about 181 MPa. At 700 and 350 J/mm, the weld center was initially compressive at about 85 and 68 MPa, respectively, and then became tensile, reaching about 55 and 93 MPa at about 7 mm from the centerline. Along the weld (Figure 9d), the middle section was tensile at about 138 MPa at 470 J/mm, whereas it was compressive at about 81 and 133 MPa at 700 and 350 J/mm, respectively; all three cases developed high compression near the arc stop.
These results show that when the heat input increased from 350 to 470 J/mm, the near-weld longitudinal and transverse tensile peaks at 10 mm above the bottom increased, but they decreased or became compressive when the heat input increased further to 700 J/mm. Residual stress therefore did not vary monotonically with heat input. This behavior reflects the simultaneous effects of heat input on peak temperature, high-temperature dwell, inter-pass reheating, and plastic-zone width. Lower heat input produces a steeper temperature gradient and a narrower plastic zone, whereas higher heat input expands the plastic zone and strengthens reheating of earlier passes by later passes. These effects act in opposite directions on the peak stress [19,20,24]. The omission of the transformation acts in the same direction in all three cases, so the non-monotonic variation in the near-weld tensile peaks with heat input, produced by the competition between the widening of the plastic zone and the stronger reheating of the earlier passes by the later ones, is retained by the model.
3.3. Effect of PWHT on Residual Stress
PWHT is an important means of improving the microstructure and properties of SIMP steel welded joints [4]. Stress relief during PWHT is controlled mainly by creep relaxation during holding and local plastic accommodation [25,26]. To assess the effect of PWHT on residual stress in the thick multi-pass joint, a numerical PWHT was performed using the minimum-displacement constraints described in Section 2.4. The thermal history followed the experimental schedule in simplified form. After welding, the joint was cooled to 80–90 °C, held for 1 h, heated at 200 °C/h to 300 °C, held for 2 h, and air-cooled to room temperature. It was then held at room temperature for 24 h, heated at 200 °C/h to 600 °C, held for 20 min, heated to 720 °C, held for 4 h, and air-cooled. Only the minimum constraints required to suppress rigid-body motion were retained. The analysis used the same thermal elastic–plastic constitutive model as the welding analysis, approximated the furnace by a uniform temperature, and did not include creep parameters for the 720 °C hold. The predicted stress relief may therefore be underestimated, and the residual stress after PWHT should be regarded as a conservative upper bound [25,26]. The holding temperature of 720 °C is below the Ac1 temperature of 10–12% Cr martensitic steels, about 810–830 °C, so neither re-austenitization nor a further martensitic transformation occurs during the heat treatment; at this stage, the omission of the transformation therefore acts only through the tempering of the martensite, which was also not modeled, and the comparison between the three heat inputs does not depend on it.
Figure 10 compares the path stresses before and after PWHT at 10 mm above the bottom for the three heat inputs; solid lines denote the condition before PWHT and dashed lines after PWHT. PWHT preserved the self-equilibrating nature of the residual stress but reduced the overall level of the high-stress region. Because residual stress in a thick joint varies strongly through the thickness and along the weld, a single peak value does not represent the overall high-stress level [19,20]. The 99th-percentile von Mises stress was therefore used to compare the high-stress level before and after PWHT. It decreased from 535.2–539.2 MPa to 272.5–308.5 MPa, a reduction of 43–49%. The maximum von Mises stress decreased from 535.7–539.6 MPa to 441.8–522.0 MPa. For longitudinal stress, the near-weld tensile peaks at 700, 470, and 350 J/mm changed from 128, 310, and 125 MPa to 300, 273, and 298 MPa, respectively, and the differences among the heat inputs narrowed. For transverse stress, the near-weld tensile peaks changed from 93, 181, and 55 MPa to 220, 160, and 144 MPa, and the differences again decreased.
Figure 10.
Residual-stress distributions before and after PWHT at 10 mm above the bottom surface: (a) longitudinal stress perpendicular to the weld; (b) longitudinal stress along the weld; (c) transverse stress perpendicular to the weld; and (d) transverse stress along the weld. Solid lines show the condition before PWHT and dashed lines after PWHT.
Stress redistribution along the weld was more pronounced. At 700 and 350 J/mm, the longitudinal compressive stress in the middle section changed to nearly zero or low-level tension after PWHT, whereas the transverse tensile peak at 470 J/mm decreased from 138 to 79 MPa. All three cases retained about 95–171 MPa in compression near the arc stop, indicating that end restraint cannot be fully relieved by a single holding schedule [25,26]. After PWHT, the maximum von Mises stress remained 441.8–522.0 MPa, well above the 99th-percentile value. The local high stresses remained mainly at the arc stop, groove root, and near-weld geometric transitions, where multiaxial constraint and stress concentration limit plastic and creep relaxation. The absence of creep parameters for the 720 °C hold further simplified local relaxation and probably reduced the predicted peak reduction [25,26].
3.4. Effect of Heat Input on Welding Distortion
Figure 11 compares the distortion at the three heat inputs: transverse shrinkage across the plate width (a) and along the weld (b), and longitudinal displacement across the plate width (c).
Figure 11.
Welding distortion at different heat inputs: (a) transverse shrinkage across the plate width; (b) transverse shrinkage along the weld; and (c) longitudinal displacement across the plate width.
Figure 11a shows that transverse shrinkage accumulated across the plate width and reached a maximum at the free edge. As the heat input increased from 350 to 470 and 700 J/mm, the maximum transverse shrinkage at the free edge increased from 0.38 to 0.60 and 0.70 mm, an overall increase of 84.2%. The increment between 470 and 700 J/mm was only 0.10 mm, smaller than the 0.22 mm increment between 350 and 470 J/mm, indicating that the shrinkage increment decreased as heat input increased. In Figure 11b, except for a transition zone of about 10 mm at the arc start, the transverse shrinkage became steady along the weld. The steady values were about 0.20, 0.32, and 0.37 mm at 350, 470, and 700 J/mm, respectively, and increased with heat input.
Longitudinal displacement was less sensitive to heat input than transverse shrinkage. In Figure 11c, the longitudinal displacement varied from about −0.12 mm to positive values across the plate width, with zero displacement at about 50 mm. The maximum longitudinal displacements near the free edge were about 0.30, 0.31, and 0.35 mm at 350, 470, and 700 J/mm, an increase of only about 16.7% from 350 to 700 J/mm. Transverse shrinkage was therefore the more sensitive distortion index for the thick V-groove joint, although longitudinal displacement also increased with heat input.
These trends reflect the welding thermal cycle and structural restraint. Higher heat input expands the compressive plastic zone and prolongs the high-temperature dwell, increasing irreversible transverse shrinkage after cooling [11,12]. Once the plastic zone reaches a certain extent, the elastic accommodation range across the plate width becomes stable, and the shrinkage increment decreases. A V-groove butt joint provides relatively weak transverse restraint, so free-edge displacement is sensitive to accumulated shrinkage in the weld region [21]. The 700 J/mm case had the largest transverse shrinkage and therefore the greatest demand for distortion control. The 350 J/mm case had the smallest distortion but smallest root-fusion margin. At 470 J/mm, the maximum free-edge transverse shrinkage and the steady transverse shrinkage were about 14.3% and 13.5% lower than at 700 J/mm, respectively, while the root still had adequate fusion. The dilational strain of the martensitic transformation has the opposite sign to the thermal contraction that drives the shrinkage, so a model that omits it tends to overestimate the transverse shrinkage; this effect is, again, common to the three heat inputs, and the comparison between them, in particular, the 14.3% lower free-edge shrinkage obtained at 470 J/mm, rather than at 700 J/mm, is expected to be preserved.
3.5. Comparison of the Heat Inputs
The three heat inputs produced different responses in temperature, residual stress, and distortion, and no single index ranked them consistently. Heat input changes peak temperature, high-temperature dwell, and plastic-zone width simultaneously, so these responses are not simply monotonic functions of heat input [11,13,19,20].
The 700 J/mm case produced the largest weld pool and the greatest root-penetration margin, but also the highest peak temperature, longest high-temperature dwell, widest HAZ, and largest free-edge transverse shrinkage (0.70 mm), placing the greatest demand on distortion control. The 350 J/mm case had a root high-temperature zone of only about 2.1 mm, the fastest cooling, and the smallest free-edge transverse shrinkage (0.38 mm). These conditions favor a narrow HAZ and low distortion, but they leave the smallest root-fusion margin and increase the risks of hardening and cold cracking. The 470 J/mm case had intermediate penetration, a free-edge transverse shrinkage of 0.60 mm, and near-weld longitudinal and transverse tensile peaks of about 310 and 181 MPa at 10 mm above the bottom. After PWHT, its 99th-percentile von Mises stress decreased to 272.5 MPa, a reduction of about 49%. Its maximum free-edge transverse shrinkage was 14.3% lower than that at 700 J/mm, and the root remained fused. On this basis, 470 J/mm was used for joint fabrication. The 700 J/mm condition provides a larger penetration margin, whereas 350 J/mm requires stricter preheat and interpass control.
3.6. Validation of the Heat-Source Model and Fusion-Zone Geometry
The heat-source model and weld-pool geometry were checked using a local validation test at 470 J/mm. A 20 mm thick SIMP steel V-groove butt specimen was prepared, a transverse section was extracted, and the measured fusion boundary was compared with the predicted pool profile. Figure 12 compares the predicted fusion-zone profile with the measured macrograph.
Figure 12.
Comparison of the predicted fusion-zone profile (left) with the measured macrograph (right) at 470 J/mm.
Fusion-zone widths were measured at the top surface, 10 mm above the bottom surface, and the root. The predicted widths were 11.7, 7.6, and 2.9 mm, and the measured widths were 12.4, 6.5, and 3.4 mm. The absolute deviations were 0.7, 1.1, and 0.5 mm, and the relative deviations were 5.6%, 16.9%, and 14.7%, with a mean absolute relative deviation of about 12.4%. The predicted top-surface width, root fusion shape, and penetration depth were generally consistent with the experiment. The local deviations are attributed to the steep temperature gradient near the fusion line; limited mesh resolution; uncertainty in extrapolated high-temperature properties and the resulting local heat-flux distribution; and the neglect of liquid-metal flow, latent heat of fusion, and metal vaporization in the weld pool [17]. The double-ellipsoidal source parameters and the equivalent 10-layer/16-pass model reproduced the fusion-zone profile at this heat input.
The comparison above validates the thermal part of the model, namely the heat-source parameters, the arc efficiency, and the resulting temperature field, and through the temperature field, the cooling times on which the predicted stresses and distortions depend; the mechanical part is not validated, because no residual-stress or distortion measurement was made on this joint. All three heat inputs were analyzed with one set of heat-source parameters, calibrated once at 470 J/mm without re-fitting, so that the differences reported in Section 3.2, Section 3.3, Section 3.4 and Section 3.5 reflect the energy input alone, and the stress and distortion results serve to rank the three heat inputs relative to each other.
3.7. Formation and Mechanical Properties of the V-Groove Joint
A 20 mm thick V-groove butt joint was fabricated at 470 J/mm. The groove had a 30° bevel on each side (60° included angle), a 1 mm root face, and a 2.5 mm root gap. Preheat and interpass temperatures were maintained at 200 °C. Welding followed the 470 J/mm condition in Table 2; arc voltage and current were 10–12 V and 95–105 A, respectively. Shielding used 99.999% Ar at the front and 99.99% Ar at the back. The groove was filled in 24 layers and 110 passes. PWHT followed the schedule in Section 3.3: 80–90 °C for 1 h, 300 °C for 2 h, air cooling to room temperature and holding for 24 h, heating to 600 °C for 20 min, and then 720 °C for 4 h, followed by air cooling.
The weld bead was continuous and blended smoothly into the base metal. Visual and radiographic examination in accordance with ASME BPVC Section V revealed no cracks or incomplete penetration. A transverse macrograph showed complete groove filling and a distinct weld/base-metal interface. Tensile specimens were taken transverse to the weld. Room-temperature tensile, impact, and side-bend tests followed AWS B4.0M, and elevated-temperature tensile tests followed ASTM E21; impact notches were located at the weld centerline or 2 mm from the fusion line.
Table 4 summarizes the tensile properties at room temperature, 450 °C, and 550 °C, together with the room-temperature impact and side-bend results. At room temperature, the 0.2% proof stress (Rp0.2), tensile strength (Rm), and elongation were 596.33 MPa, 802.63 MPa, and 18.07%, respectively. Rm exceeded the 800 MPa lower limit in GB/T 38875-2020 by only 2.63 MPa, so the tensile margin was small. At 450 and 550 °C, Rp0.2/Rm values were 421.33/512.31 MPa and 328.33/412.31 MPa, and the elongations were 19.67% and 23.00%, respectively. All tensile specimens failed in the weld metal. Weld-metal and HAZ impact energies were 183.9 and 77.9 J, respectively. Both met the requirements, but the HAZ toughness was lower than that of the weld metal [24].
Table 4.
Mechanical properties of the joint fabricated at 470 J/mm (mean values; n = number of specimens).
Of the four side-bend specimens, three showed no visible defects. One developed a 2–3 mm local surface crack in the bend region without through-thickness fracture and was qualified under AWS B4.0M. The macrograph, nondestructive examination, tensile, impact, and side-bend results met the applicable requirements. The joint fabricated at 470 J/mm therefore met the specified formation and mechanical-property criteria.
4. Conclusions
A sequentially coupled thermal–mechanical finite element model was used to analyze the temperature field, residual stress, distortion, and PWHT response of a 20 mm thick SIMP steel V-groove TIG joint. The 24-layer/110-pass welding procedure was represented by an equivalent 10-layer/16-pass sequence (Figure 2), and the fusion-zone geometry predicted with it was compared with the measured fusion zone of a joint fabricated at 470 J/mm. The main conclusions are as follows:
- (1)
- The 10-layer/16-pass merged-pass model reproduced the thermal field of multi-pass TIG welding of the 20 mm thick joint: at the three through-thickness positions, the predicted fusion boundary agreed with the measured profile, and the mean absolute relative deviation in fusion-zone width was about 12.4%, which supports the use of the calibrated heat-source parameters for predicting the fusion-zone geometry at the three heat inputs examined.
- (2)
- Increasing the heat input from 350 to 700 J/mm increased the peak temperature, fusion-zone width, penetration depth, and t8/5. The root high-temperature zone expanded from about 2.1 to 4.6 mm.
- (3)
- At 700, 470, and 350 J/mm, the peak as-welded von Mises stresses were 535.7, 537.7, and 539.6 MPa, respectively, a difference of about 4 MPa. Heat input therefore had a limited effect on the peak magnitude, but it changed the extent of the high-stress zone and the path stress distributions. Residual stress varied in a self-equilibrating manner through the thickness. At 470 J/mm, the near-weld longitudinal and transverse tensile peaks 10 mm above the bottom surface were about 310 and 181 MPa, respectively. Because the martensitic transformation was not modeled (Section 3.2), these as-welded tensile values are upper estimates.
- (4)
- After PWHT at 720 °C for 4 h, the 99th-percentile von Mises stresses for the three conditions decreased from 535.2–539.2 MPa to 272.5–308.5 MPa, a reduction of 43–49%. The differences in near-weld tensile stress among the heat inputs narrowed. High compressive stresses or local peaks remained at the arc stop and in some near-weld regions. Because creep was not included, the predicted post-PWHT stresses provide a conservative upper estimate. These post-PWHT values are predictions of the same model, so it is the relative effect of the heat treatment at the three heat inputs that the analysis establishes.
- (5)
- Among the extracted distortion indices, transverse shrinkage was more sensitive to heat input, and its increment decreased as heat input increased. The maximum free-edge transverse shrinkage increased from 0.38 mm at 350 J/mm to 0.60 and 0.70 mm at 470 and 700 J/mm, and the steady shrinkage along the weld increased from 0.20 to 0.32 and 0.37 mm. The maximum longitudinal displacement increased from about 0.30 to 0.35 mm and was less sensitive to heat input. The 700 J/mm case had the greatest distortion-control demand.
- (6)
- Under the conditions examined, 470 J/mm provided adequate root fusion with lower distortion than 700 J/mm, and it was used for joint fabrication and property testing. Its maximum free-edge transverse shrinkage was 14.3% lower than that at 700 J/mm, and the 99th-percentile von Mises stress decreased by 49% after PWHT at 720 °C for 4 h. The joint met the room- and elevated-temperature tensile and impact requirements of GB/T 38875-2020. Its side-bend specimens were qualified under AWS B4.0M, and none showed a through-thickness defect.
The model has several limitations. It used isotropic hardening, omitted the volumetric expansion and transformation plasticity associated with martensitic transformation, and did not include creep during PWHT [12,16,22,23]. The consequences of this omission for the predicted stresses and shrinkage are analyzed in Section 3.2, Section 3.3, Section 3.4 and Section 3.5. The residual-stress and distortion results are therefore intended for relative comparison under the same model conditions. Coupling transformation kinetics and creep relaxation with microstructural and mechanical testing, and measuring the residual stress and the distortion of dedicated joints with diffraction and contour methods, would improve the predictive capability of the model.
Author Contributions
Y.C., Conceptualization, Supervision, and Writing—Review and Editing; S.L., Methodology, Formal Analysis, and Writing—Original Draft. J.D.: Investigation and Validation. All authors have read and agreed to the published version of the manuscript.
Funding
This research was funded by the National Natural Science Foundation of China (No. 51809161).
Data Availability Statement
The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding author.
Conflicts of Interest
The authors declare no conflicts of interest.
References
- Yang, K.; Yan, W.; Wang, Z.G.; Shan, Y.Y.; Shi, Q.Q.; Shi, X.B.; Wang, W. Research progress of SIMP steel: A new high-temperature, irradiation-resistant and liquid-metal-corrosion-resistant structural material for nuclear applications. Acta Metall. Sin. 2016, 52, 1207–1221. (In Chinese) [Google Scholar]
- Klueh, R.L. Elevated-temperature ferritic and martensitic steels and their application to future nuclear reactors. Int. Mater. Rev. 2005, 50, 287–310. [Google Scholar] [CrossRef] [Scilit]
- Abe, F. Precipitate design for creep strengthening of 9% Cr tempered martensitic steel for ultra-supercritical power plants. Sci. Technol. Adv. Mater. 2008, 9, 013002. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Liu, Y.H.; Li, B.; Chen, S.J.; Ding, G.Z.; Li, S.H. Effect of post-weld heat treatment on microstructure and mechanical properties of SIMP steel TLP diffusion-bonded joints. Mater. Mech. Eng. 2021, 45, 77–80+86. (In Chinese) [Google Scholar]
- Hao, L.L.; Chen, S.J.; Ding, G.Z.; Li, B.; Li, S.H.; Zhao, P.F. Microstructure and properties of SIMP steel TLP diffusion-bonded joints under different three-stage process parameters. Mater. Mech. Eng. 2019, 43, 12–17+50. (In Chinese) [Google Scholar]
- Miao, X.; Chen, S.J.; Ding, G.Z.; Li, B.; Zhao, P.F. Effect of bonding pressure on microstructure and properties of SIMP steel TLP diffusion-bonded joints. Ordnance Mater. Sci. Eng. 2018, 41, 82–86. (In Chinese) [Google Scholar]
- Zhu, Q.; Lei, Y.; Wang, Y.; Liang, S.; Ye, Y.; Li, C. Microstructure and stress distribution on TIG welded joint of CLAM steel. J. Fusion Energy 2015, 34, 995–1001. [Google Scholar] [CrossRef] [Scilit]
- Kou, S. Welding Metallurgy, 2nd ed.; John Wiley & Sons: Hoboken, NJ, USA, 2003. [Google Scholar]
- Wu, C.S. Welding Thermal Process and Weld Pool Geometry; China Machine Press: Beijing, China, 2008. (In Chinese) [Google Scholar]
- Zubairuddin, M.; Albert, S.K.; Vasudevan, M.; Chaudhari, V.; Suri, V. Finite element simulation of weld bead geometry and temperature distribution during GTA welding of modified 9Cr-1Mo steel and experimental validation. J. Manuf. Sci. Prod. 2014, 14, 195–207. [Google Scholar] [CrossRef] [Scilit]
- Vu, T.D.; Tran, X.T.; Nguyen, M.N. Investigation on the effect of heat input and clamping positions on residual stress and distortion of the 316L steel butt-welded joint by numerical simulation. Weld. World 2024, 68, 1071–1087. [Google Scholar] [CrossRef] [Scilit]
- Zubairuddin, M.; Albert, S.K.; Mahadevan, S.; Vasudevan, M.; Chaudhari, V.; Suri, V.K. Experimental and finite element analysis of residual stress and distortion in GTA welding of modified 9Cr-1Mo steel. J. Mech. Sci. Technol. 2014, 28, 5095–5105. [Google Scholar] [CrossRef] [Scilit]
- Asadi, P.; Alimohammadi, S.; Kohantorabi, O.; Soleymani, A.; Fazli, A. Numerical investigation on the effect of welding speed and heat input on the residual stress of multi-pass TIG welded stainless steel pipe. Proc. Inst. Mech. Eng. Part B J. Eng. Manuf. 2021, 235, 1007–1021. [Google Scholar] [CrossRef] [Scilit]
- Yin, S.; Lei, Y.C.; Shao, Q.D.; Ju, X. Three-dimensional numerical simulation of welding residual stress and distortion in CLAM steel. Weld. Technol. 2010, 39, 12–15. (In Chinese) [Google Scholar]
- Miao, Z.Y.; Kong, F.Y.; Liu, H. Numerical simulation of residual stress in girth welded joints of T91 pipeline steel based on SYSWELD. Hot Work. Technol. 2016, 45, 156–160. (In Chinese) [Google Scholar]
- Deng, D.; Murakawa, H. Numerical simulation of temperature field and residual stress in multi-pass welds in stainless steel pipe and comparison with experimental measurements. Comput. Mater. Sci. 2006, 37, 269–277. [Google Scholar] [CrossRef] [Scilit]
- Goldak, J.; Chakravarti, A.; Bibby, M. A new finite element model for welding heat sources. Metall. Trans. B 1984, 15, 299–305. [Google Scholar] [CrossRef] [Scilit]
- He, X.J.; Song, Y.; Xiao, X.; Wang, J.J. Blind-hole measurement and numerical analysis of the effect of welding heat input on residual stress. J. Chongqing Jiaotong Univ. (Nat. Sci.) 2018, 37, 7–11. (In Chinese) [Google Scholar]
- Qiang, B.; Li, Y.D.; Yao, C.R.; Wang, X.; Gu, Y. Through-thickness distribution of residual stresses in Q345qD butt-welded steel plates. J. Mater. Process. Technol. 2018, 251, 54–64. [Google Scholar] [CrossRef] [Scilit]
- Taraphdar, P.K.; Kumar, R.; Giri, A.; Pandey, C.; Mahapatra, M.M.; Sridhar, K. Residual stress distribution in thick double-V butt welds with varying groove configuration, restraints and mechanical tensioning. J. Manuf. Process. 2021, 68, 1405–1417. [Google Scholar] [CrossRef] [Scilit]
- Deng, D.; Murakawa, H. Prediction of welding residual stress in multi-pass butt-welded modified 9Cr–1Mo steel pipe considering phase transformation effects. Comput. Mater. Sci. 2006, 37, 209–219. [Google Scholar] [CrossRef] [Scilit]
- Francis, J.A.; Bhadeshia, H.K.D.H.; Withers, P.J. Welding residual stresses in ferritic power plant steels. Mater. Sci. Technol. 2007, 23, 1009–1020. [Google Scholar] [CrossRef] [Scilit]
- Yaghi, A.H.; Hyde, T.H.; Becker, A.A.; Sun, W. Numerical simulation of P91 pipe welding including the effects of solid-state phase transformation on residual stresses. Proc. Inst. Mech. Eng. Part L J. Mater. Des. Appl. 2007, 221, 213–224. [Google Scholar] [CrossRef] [Scilit]
- Park, J.; An, G.; Ma, N.; Kim, S. Effect of transverse restraint on welding residual stress in V-groove butt welding. Metals 2022, 12, 654. [Google Scholar] [CrossRef] [Scilit]
- Cho, J.R.; Lee, B.Y.; Moon, Y.H.; Van Tyne, C.J. Investigation of residual stress and post weld heat treatment of multi-pass welds by finite element method and experiments. J. Mater. Process. Technol. 2004, 155–156, 1690–1695. [Google Scholar] [CrossRef] [Scilit]
- Dong, P.; Hong, J.K. Residual stress relief in post-weld heat treatment. In Proceedings of the ASME 2008 Pressure Vessels and Piping Conference, Chicago, IL, USA, 2008; ASME: New York, NY, USA, 2008; pp. 321–329. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.