Skip to Content
MaterialsMaterials
  • Article
  • Open Access

27 November 2026

27 Pages

Fracture Damage Evolution of Stone Mastic Asphalt Mixtures Subjected to Salt Freeze–Thaw Cycles: A Multiscale Characterization Using SCB, AE, and DIC

,
,
,
and
College of Water Resources and Architecture Engineering, Tarim University, Alar 843300, China
*
Authors to whom correspondence should be addressed.
This article belongs to the Section Construction and Building Materials

Abstract

Salt freeze–thaw cycles can induce internal damage in SMA mixtures and weaken their fracture resistance, yet the relationship between internal damage evolution and localized deformation near the crack tip remains unclear. Semi-circular bending (SCB) tests were integrated with acoustic emission (AE) and digital image correlation (DIC) to clarify the fracture damage evolution of SMA mixtures subjected to different numbers of salt freeze–thaw cycles. For comparative analysis of AE responses, the loading process was divided into four operational intervals using 0.8Fmax as a reference on the pre-peak and post-peak branches. The SCB results showed that the fracture energy Gf, Mode I critical stress intensity factor KI, and flexibility index FI decreased by 72.0%, 57.5%, and 32.4%, respectively, after 20 cycles, while the crack path became increasingly localized. The SCB results are expressed as mean ± standard deviation based on three replicate specimens per conditioning level (n = 3). Welch’s one-way ANOVA showed significant overall differences among the five conditioning levels for Gf, KI, S, and FI (p < 0.05), and Games–Howell post hoc comparisons were used to examine pairwise differences. AE revealed that salt freeze–thaw cycling advanced the onset of internal damage and concentrated energy release near the peak load and after the peak load, while the relative proportions of tensile-type and shear-type AE events varied non-monotonically with the number of salt freeze–thaw cycles. DIC showed a substantial reduction in localized deformation, with the spatially averaged maximum horizontal strain Exx and mean normalized crack opening response decreasing by 71.71% and 69.45%, respectively, after 20 cycles, while crack opening remained concentrated near the L1 measurement location. The findings provide a reference for characterizing the multiscale fracture response of SMA mixtures under salt freeze–thaw conditions.

1. Introduction

Asphalt mixtures are widely used in pavement surface courses because of their high load-bearing capacity, construction adaptability, and favorable riding comfort. In recent years, the sustained growth in traffic loading in cold, arid, and saline regions such as southern Xinjiang has intensified pavement deterioration associated with the coupled effects of temperature fluctuations, water and salt ingress, and salt freeze–thaw cycling. Exposure to saline and humid environments can progressively degrade asphalt mixture performance, while salt immersion and freeze–thaw cycling can weaken adhesion at the asphalt–aggregate interface [1,2]. Chloride attack and repeated freeze–thaw cycles can further compromise the durability and moisture resistance of the mixtures [3,4]. SMA-13 mixtures are characterized by a coarse-aggregate skeleton formed through aggregate interlocking and an asphalt-mastic filling structure. The structural stability of the mixture is governed jointly by aggregate gradation, the interlocking condition of the coarse-aggregate skeleton, and the type of stabilizing agent [5,6]. To control asphalt-mastic draindown and preserve the integrity of the aggregate skeleton, fiber stabilizers are commonly incorporated into SMA mixtures. Basalt fibers can additionally enhance the mechanical performance of the asphalt mastic and improve the fracture resistance of the mixture [7,8].
The semi-circular bending (SCB) test requires relatively simple specimen preparation and provides a well-defined notch geometry. It has therefore been widely adopted to evaluate the low-temperature fracture performance of asphalt mixtures [9,10]. Based on the load–displacement response, the fracture resistance of asphalt mixtures can be characterized in terms of fracture energy, deformation capacity, and post-peak load decay. The flexibility index FI, which integrates fracture energy with post-peak load decay characteristics, has been used to quantify the cracking potential of asphalt mixtures [11]. Other fracture-related indices have also been proposed to quantitatively characterize the fracture response obtained from SCB testing [12]. For notched semi-circular specimens, the Mode I critical stress intensity factor provides a fracture mechanics-based parameter for evaluating resistance to crack propagation [13]. Karimi et al. [14] evaluated the long-term performance of asphalt mixtures subjected to moisture damage and freeze–thaw cycling using fracture parameters and demonstrated that macroscopic fracture responses can reflect environmentally induced changes in fracture resistance. Although the load–displacement response provides important information on the overall mechanical behavior and can indicate changes associated with microcrack development before the peak load and fracture progression after the peak load, it does not fully characterize the spatial distribution of localized deformation or the temporal evolution of internal damage activity. DIC and AE measurements can complement the SCB response by providing spatial and temporal information on the fracture process.
Acoustic emission (AE) enables the recording of transient elastic waves generated by microcrack initiation, propagation, and localized failure, thereby providing temporal information for characterizing damage evolution during loading [15,16]. Fu et al. [17] employed AE monitoring to investigate fracture damage in asphalt mixtures subjected to freeze–thaw cycling and aging, whereas Liang et al. [18] evaluated the fracture response of basalt fiber-reinforced asphalt mixtures after freeze–thaw conditioning. Qiu et al. [19] characterized the coupled fracture process of asphalt mixtures using AE parameters and waveform features, demonstrating that AE signals can capture crack activity at different stages of failure. Cumulative AE energy and ring counts can be used to compare the intensity of damage activity at different loading stages, whereas signal amplitude, rise time, and duration can be used to characterize the features of individual AE events. Differences in fracture behavior under different fiber-reinforcement conditions can also be evaluated based on AE responses [20]. In addition, two AE parameters, the rise time to peak amplitude ratio (RA) and average frequency (AF), are commonly used to distinguish cracking modes in asphalt mixtures. AF is calculated as the ratio of ring counts to event duration. AE events with low RA and high AF values are generally associated with tensile cracking, whereas those with high RA and low AF values are commonly associated with shear cracking [21,22]. However, because AE signals primarily describe the temporal evolution of internal damage activity, localized deformation concentrations and the corresponding surface crack paths cannot be independently resolved without reliable AE source localization.
Digital image correlation (DIC) enables displacement and strain fields to be obtained from sequential images, thereby facilitating analysis of crack opening, local deformation, and fracture response [23,24]. Yuan et al. [25] combined SCB testing with stereoscopic DIC to obtain the full-field deformation during the fracture process of asphalt concrete. Zieliński et al. [26] and Ren et al. [27] used SCB and DIC to evaluate the fracture performance of asphalt concrete and characterize crack evolution. Cao et al. [28] investigated the crack resistance and failure characteristics of asphalt concrete based on strain concentration zones and crack propagation paths. Previous studies have applied combined AE and DIC techniques to investigate the fracture behavior of asphalt materials, including cold-recycled asphalt mixtures containing 100% RAP [29], asphalt concrete [30], and fiber-reinforced asphalt concrete [31]. AE records the timing and intensity of damage-related activity, whereas DIC captures the spatial distribution of surface deformation and crack propagation. Their combined use enables the temporal evolution of damage activity to be examined in relation to the corresponding spatial development of surface deformation, providing complementary information that cannot be obtained from either technique alone. However, the fracture behavior of basalt-fiber-reinforced SMA-13 mixtures under repeated salt freeze–thaw conditioning remains insufficiently understood. In particular, how AE activity evolves with increasing numbers of conditioning cycles and relates to DIC measurements of localized strain and crack opening during SCB fracture has not been adequately investigated.
This study investigated an SMA-13 mixture with an engineering gradation typical of pavements in the cold, arid, and saline-alkali regions of southern Xinjiang. Semi-circular bending (SCB) fracture tests were performed on specimens subjected to different numbers of salt freeze–thaw cycles. During loading, acoustic emission (AE) monitoring was conducted simultaneously to record damage-related AE parameters, while digital image correlation (DIC) was used to capture the evolution of full-field surface displacement and strain. These synchronized measurements were used to establish the relationships among the number of salt freeze–thaw cycles, macroscopic fracture response, localized surface strain concentration, and internal damage activity. The characteristic stages of fracture damage evolution in SMA mixtures under salt freeze–thaw conditioning were identified, and the effect of salt freeze–thaw deterioration on internal crack propagation paths was clarified. The research workflow is shown in Figure 1. The findings help characterize the fracture behavior of the basalt-fiber-reinforced SMA-13 mixture examined under the salt freeze–thaw conditions used in this study. Their applicability to other mixture designs and field pavement conditions remains to be established through further testing across a wider range of salt concentrations and freeze–thaw cycles.
Figure 1. Schematic representation of the research workflow.

2. Materials and Methods

2.1. Raw Materials

2.1.1. SBS-Modified Asphalt Binder

An SBS-modified asphalt from a company in Karamay, Xinjiang, was used; its main technical performance indicators are shown in Table 1.
Table 1. Physical properties of the SBS-modified asphalt binder.

2.1.2. Aggregates and Mineral Filler

The coarse aggregate comprised basalt crushed stone in two size fractions, 5–10 mm and 10–16 mm. Basalt manufactured sand with a particle size of 0–3 mm was used as the fine aggregate, while limestone powder was used as the mineral filler. All aggregates and mineral filler were obtained from the same supplier in Alar, Xinjiang, China. Their basic technical properties are summarized in Table 2.
Table 2. Physical properties of the basalt aggregates and mineral filler.

2.1.3. Basalt Fibers

Basalt fibers were supplied by Xinjiang Woyu Textile New Materials Co., Ltd. (Alar, Xinjiang, China), and their basic properties are summarized in Table 3. Previous studies have shown that fiber length and dosage influence fiber dispersion and reinforcement efficiency in asphalt mixtures [32,33,34], with fiber length exerting a significant effect on mixture fracture resistance.
Table 3. Basic properties of the basalt fibers.
In preliminary mixture-design tests conducted by our research group, a hybrid basalt-fiber system consisting of 6 mm and 9 mm fibers at a mass ratio of 1:1 was adopted, and three total fiber dosages (0.2%, 0.3%, and 0.4% by mass of the asphalt mixture) were examined. Based on the preliminary mixture-design results, a total fiber dosage of 0.2% was selected for the present study. The 6 mm/9 mm hybrid configuration and the 1:1 blending ratio were retained as the adopted fiber arrangement, rather than treated as independently optimized parameters. These fiber parameters were kept constant in the subsequent salt freeze–thaw fracture tests.

2.1.4. Gradation of the SMA-13 Mixture

The SMA-13 gradation was designed according to the Technical Specifications for Construction of Highway Asphalt Pavements (JTG F40–2004). The aggregate gradation and target gradation curve are shown in Figure 2. Based on preliminary mixture-design tests, the optimum asphalt binder-to-aggregate ratio of the SMA-13 mixture was determined to be 5.8%.
Figure 2. Aggregate gradation and target gradation of the SMA-13 mixture: (a) Aggregate gradation curves; (b) target gradation curve.

2.2. Experimental Methods

2.2.1. Preparation of SCB Specimens

The basalt aggregate fractions were oven-dried and preheated to 100 °C, while the SBS-modified asphalt binder was heated to 175 °C. The aggregates were first dry-mixed with the pre-weighed 6 and 9 mm basalt fibers for 20 s to ensure uniform fiber dispersion. The SBS-modified asphalt binder was then added and mixed for 70 s, followed by the addition of the mineral filler and further mixing for 90 s until a homogeneous mixture was obtained. The mixing sequence is illustrated in Figure 3. Large cylindrical specimens with a diameter of 152.4 mm and a height of 95.3 mm were produced using the large Marshall compaction method. A compaction hammer with a mass of 10.21 kg was used, and 75 blows were applied to each face of the specimen. After cooling and demolding, the specimens were cut along the centerline to obtain semi-circular bending specimens for subsequent salt freeze–thaw conditioning and SCB testing. To ensure crack initiation at a predefined location, a notch 15 mm in length and 1 mm in width was introduced at the midpoint of the flat edge. The specimen preparation procedure and geometric dimensions are presented in Figure 4.
Figure 3. Preparation procedure of the SMA-13 mixture.
Figure 4. Preparation procedure and geometric dimensions of the SCB specimens.

2.2.2. Accelerated Laboratory Simulation of Salt Freeze–Thaw Cycling

Previous studies have investigated the effects of chloride salt erosion and combined salt freeze–thaw exposure on the performance of asphalt mixtures [3,35]. NaCl and anhydrous Na2SO4 were selected to establish a mixed chloride–sulfate exposure condition, reflecting the coexistence of chloride and sulfate salts in saline environments. The two salts were mixed at an equal mass ratio (1:1) to establish a defined and reproducible laboratory composition, yielding a solution with a nominal total salt mass fraction of 10%. This concentration was adopted as an accelerated exposure level to promote measurable deterioration within the test period. The selected salt composition was intended to investigate the combined effects of chloride and sulfate exposure rather than reproduce the exact salt proportions and concentration of a specific field environment. No separate pre-saturation treatment was applied before conditioning. During both freezing and thawing, the SCB specimens remained partially immersed in the salt solution to one-third of their height. The solution was renewed every 10 cycles, but its concentration was not monitored between replacements. Each salt freeze–thaw cycle consisted of freezing the SCB specimens at −15 °C for 10 h, followed by thawing at 25 °C for 14 h, resulting in a total cycle duration of 24 h. In accordance with previously reported salt freeze–thaw conditioning procedures [18,35], the specimens were subjected to 0, 5, 10, 15, or 20 cycles. After the prescribed number of cycles had been completed, the specimens were removed from the solution, and surface moisture was gently wiped off. The specimens were then conditioned at 25 ± 1 °C for 4 h before SCB fracture testing. The salt freeze–thaw conditioning tests were conducted using a laboratory water–temperature–salt multi-field coupled testing system previously developed by our research group, as shown in Figure 5.
Figure 5. Salt freeze–thaw conditioning system.

2.2.3. SCB Testing

(1)
Test Procedure
SCB fracture tests were performed using an LHMT-20 pavement material strength testing machine at 25 °C. Displacement-controlled loading was applied at a constant rate of 50 mm/min, which was selected as the test condition for this study and maintained for all specimens to ensure consistent loading conditions across the different salt freeze–thaw groups. Before formal loading, a small seating load was applied to ensure proper contact between the loading head and the specimen. The support span was 120 mm. The load was applied vertically along the specimen centerline, with the loading axis aligned with the notch at the midpoint of the flat edge. The load and load-point displacement were continuously recorded throughout the fracture process to obtain the complete load–displacement response. Three replicate specimens were tested for each conditioning group. The SCB fracture test setup is shown in Figure 6.
Figure 6. SCB fracture test setup.
(2)
Evaluation Indicators
Previous studies have demonstrated that energy-based parameters, fracture-mechanics parameters, and deformation-response indicators obtained from SCB tests can be used to evaluate the fracture behavior of asphalt mixtures from the perspectives of crack-propagation resistance, energy-dissipation capacity, and deformation characteristics [10,14]. Accordingly, fracture energy Gf, stiffness S, flexibility index FI, and Mode I critical stress intensity factor KI were selected as the evaluation indices for characterizing the evolution of the fracture performance of SMA-13 mixtures subjected to salt freeze–thaw cycling.
Fracture energy represents the energy consumed per unit fracture area during crack propagation and reflects the resistance of the mixture to crack growth. It was calculated using Equation (1).
G f = W f Area lig × 10 6
where Gf is the fracture energy (J/m2), Wf is the work of fracture, defined as the area under the load–displacement curve (J), and Arealig is the ligament area of the SCB specimen (mm2).
Stiffness S was used to characterize the mixture’s resistance to deformation up to the peak load. It was defined as the secant stiffness at the peak-load point and calculated as the ratio of the peak load to the corresponding displacement [10], as expressed in Equation (2).
S = F peak u peak × 10 3
where S is the stiffness (kN/m), and Fpeak and upeak denote the peak load (kN) and corresponding displacement (mm), respectively.
The flexibility index FI is used to evaluate deformation compatibility and fracture tolerance during post-peak crack propagation. Unlike single parameters such as peak load, FI incorporates both fracture energy and post-peak load-decay characteristics [12]. It was calculated using Equation (3).
FI = G f m × A
where FI is the flexibility index, Gf is the fracture energy (J/m2), m is the slope at the inflection point of the post-peak load–displacement curve, and A is the unit-conversion and scaling coefficient, which was set to 0.01. The absolute value of the post-peak slope was used because the load decreases with increasing displacement after the peak load. It therefore represents the magnitude of post-peak load decay, irrespective of the negative slope direction. The inflection point was identified on the post-peak branch by examining the change in curvature of the recorded load–displacement curve. The slope m was then determined numerically as the local tangent slope at the identified inflection point using the recorded load–displacement data in its vicinity. The same procedure for identifying the inflection point and determining the local slope was consistently applied to all specimens.
An apparent Mode I stress intensity factor (KI) was calculated using the stress intensity factor formulation for semi-circular specimens under three-point bending [13]. The calculation procedures are given in Equations (4) and (5).
K I = Y I σ 0 π a
σ 0 = F peak 2 rt
With the geometric correction factor determined using Equation (6):
Y I = 4.782 − 1.219 ( a r ) + 0.063 exp 7.045 ( a r )
where KI is the apparent Mode I stress intensity factor (kN·mm−3/2), YI is the Mode I geometric correction factor, r and t are the radius and thickness of the SCB specimen (mm), respectively, and a is the notch length (mm). Considering the viscoelastic and nonlinear behavior of asphalt mixtures at 25 °C under a loading rate of 50 mm/min, KI is treated as an apparent fracture parameter for comparing the fracture responses of specimens subjected to different salt freeze–thaw conditioning levels, rather than as an intrinsic critical fracture toughness.

2.2.4. AE Monitoring and Evaluation Parameters

(1)
AE Monitoring Procedure
Acoustic emission (AE) refers to the transient elastic waves generated by localized deformation, microcrack initiation, or crack propagation within a material. The resulting waves are detected by AE sensors mounted on the specimen surface and converted into electrical signals for acquisition, providing information on the temporal evolution of internal damage activity [17,19].
A multichannel AE monitoring system manufactured by Qingcheng Acoustic Emission Research Co., Ltd. (Guangzhou, Guangdong, China) was used to monitor the internal damage activity of the asphalt mixture during SCB loading. The system comprised an SWAE signal acquisition unit, an SAEU3H AE acquisition system, W800 AE transducers, and SAEPA 2 preamplifiers, as shown in Figure 7a–c.
Figure 7. AE monitoring system and characteristic waveform parameters: (a) AE acquisition system; (b) AE sensors; (c) pre-amplifier; (d) AE signal parameter definitions.
Four AE transducers were symmetrically mounted on both sides of the anticipated crack path on the specimen surface. Their spatial arrangement and coordinates are presented in Figure 8. The four AE transducers were used for signal acquisition only, and no AE source localization was performed in this study. Accordingly, the recorded AE signals were analyzed in terms of their temporal characteristics and cracking-mode features rather than the spatial locations of individual AE sources. Before testing, an acoustic couplant was uniformly applied to the contact interfaces between the transducers and the specimen to ensure adequate coupling, secure attachment, and stable signal transmission. The preamplifier gain was set to 40 dB, and the sampling frequency was set to 4 MHz. The W800 sensors had a nominal frequency range of 50–800 kHz and a resonant frequency of 600 kHz. The hit threshold and waveform acquisition threshold were both set to 37 dB, while the floating threshold was set to 0 dB. The hit definition parameters were set as follows: peak definition time (PDT), 150 μs; hit definition time (HDT), 300 μs; and hit lockout time (HLT), 300 μs. The analog high-pass and low-pass filter cutoffs were set to 20 and 100 kHz, respectively, and digital filtering was disabled. The waveform record length was 50,000 points, with a pre-trigger length of 512 points. Threshold triggering, independent-channel acquisition, and normal sampling mode were used. Before testing, channel sensitivity was checked using the pencil-lead break method, with three lead breaks performed to examine the responses of the sensor channels.
Figure 8. AE sensor arrangement.
(2)
AE Evaluation Parameters
AE waveforms and the corresponding outputs from the acquisition system were used to extract the characteristic parameters of ring counts, cumulative AE energy, peak amplitude, duration, rise time, and average frequency (AF). The definitions of these parameters are illustrated in Figure 7d. These parameters were used to characterize AE event activity, energy release, and the evolution of internal damage during loading.

2.2.5. DIC Measurement and Evaluation Parameters

(1)
DIC Measurement Procedure
Digital image correlation (DIC) is a non-contact, full-field optical measurement technique that determines surface displacement by correlating random speckle patterns recorded before and after deformation. The corresponding strain field can then be calculated from the displacement gradients [23,24]. DIC enables the localized deformation associated with crack initiation, propagation, and failure in asphalt mixtures to be characterized from surface displacement and strain fields and has therefore been widely applied in asphalt-mixture fracture studies [21,23].
A two-dimensional DIC system manufactured by Xintuo 3D Technology Co., Ltd. was used to monitor the surface deformation of the SCB specimens during loading. Before testing, a high-contrast random speckle pattern was applied to the specimen surface, and the positions of the camera, illumination source, and specimen were fixed. The system consisted of an ME2P-2621-15U3M camera and XTDIC Ver. 9.7.2 software. A 50 mm focal-length lens was used, and images were acquired at 300 ms intervals. Three replicate specimens were tested for each conditioning group in the SCB fracture tests; however, DIC monitoring was conducted on only one specimen per salt freeze–thaw conditioning group (n = 1).
The images (5120 × 5120 pixels) were calibrated using an 85 mm reference length, yielding a spatial scale of 0.0166 mm/pixel. Image correlation was performed using an 80 × 80-pixel subset with an 80-pixel step in both directions. The strain calculation window had a half-window size of 2 (5 × 5 points). Gaussian polynomial smoothing was applied to the strain fields, and normalized cross-correlation (NCC) was used for subset matching. The camera was aligned perpendicular to the specimen surface to minimize out-of-plane motion, which was not explicitly corrected. Measurement uncertainty was not independently quantified.
(2)
DIC Evaluation Parameters
The DIC analysis was performed by correlating the reference and deformed images to determine the displacement of corresponding speckle subsets, from which the surface strain field was calculated, as illustrated in Figure 9.
Figure 9. Reference image and target image: (a) reference image; (b) target image.
The reference and deformed images were first correlated to determine the positional changes in the corresponding subsets. The correlation function used for subset matching is given in Equation (7) [23].
C f , g P = ∑ x = − M M ∑ y = − M M f x , y − f m g x ′ , y ′ − g m ∑ x = − M M ∑ y = − M M f x , y − f m 2 ∑ x = − M M ∑ y = − M M g x ′ , y ′ − g m 2
where f(x,y) and g(x′,y′) represent the grayscale values of pixels within the corresponding subsets of the reference and deformed images, respectively. fm and gm denote the mean grayscale values of the corresponding subsets, M is the half-size of the correlation subset, and P represents the displacement parameters to be determined.
The displacement field was then obtained from the matched subsets, and the surface strain components were calculated from the corresponding displacement gradients using Equation (8) [23,24].
Exx = 1 2 2 ∂ u ∂ x + ∂ u ∂ x 2 + ∂ v ∂ x 2
where u and v are the displacement components in the x- and y-directions, respectively; ∂ u ∂ x and ∂ v ∂ x are used to calculate the surface strain components.
When the displacement field is continuous, Exx reflects the local strain derived from the displacement gradient. However, when a subset spans an open crack, the displacement discontinuity may produce an apparent strain concentration. Smaller subsets may capture sharper local strain variations, whereas larger subsets tend to smooth the displacement jump. Therefore, Exx near an open crack is interpreted as an indicator of localized deformation rather than continuous material strain across the crack.
To characterize localized deformation during crack propagation, four strain-monitoring locations were arranged above the prefabricated notch along the anticipated crack-propagation path. The spacing between adjacent locations was 15 mm, and the horizontal strain Exx was extracted at each location. In addition, four pairs of DIC measurement points, designated L1–L4, were arranged across the anticipated crack path at the corresponding elevations. The crack-opening displacement was quantified from the change in distance between each pair of points. The detailed arrangement of the strain-monitoring points and crack-opening point pairs is shown in Figure 10.
Figure 10. Arrangement of DIC strain-monitoring points and crack-opening point pairs.
The horizontal strain Exx was used to quantify the localized deformation response near the crack path. For the ith point pair spanning the crack, the incremental crack-opening displacement was calculated from the difference between the horizontal displacements of the right and left measurement points at the same elevation, as expressed in Equation (9).
Δ D i t = u R , i t − u L , i t
where ΔDi(t) denotes the incremental crack-opening displacement of the ith point pair at loading time t, and uR,i(t) and uL,i(t) represent the horizontal displacements of the measurement points on the right and left sides of the crack, respectively.
Because the initial spacing varied among the point pairs, the crack-opening response was normalized to facilitate comparison, as expressed in Equation (10).
L i t = Δ D i t D i , 0 × 100 %
where Li(t) is the normalized crack-opening response of the ith point pair at time t, Di,0 is the initial spacing between the corresponding measurement points, and i = 1, 2, 3, or 4.
At identical characteristic load levels, the Exx responses at C1–C4 and the normalized crack-opening responses at L1–L4 were jointly analyzed to evaluate localized strain concentration and crack-opening deformation in the crack region under different salt freeze–thaw conditioning levels.

3. Results and Discussion

3.1. SCB-Based Characterization of Fracture Behavior

3.1.1. Evolution of Crack Propagation Paths

The crack propagation paths of SCB specimens subjected to different numbers of salt freeze–thaw cycles are shown in Figure 11.
Figure 11. Crack-propagation paths of the SCB specimens: (a) 0 cycles; (b) 5 cycles; (c) 10 cycles; (d) 15 cycles; (e) 20 cycles.
As shown in Figure 11, the dominant crack in each specimen initiated near the prefabricated notch and propagated upward toward the upper region of the specimen, confirming that the notch effectively controlled the crack initiation location. Visual inspection of Figure 11 reveals differences in the surface crack trajectories among specimens subjected to different numbers of cycles involving salt exposure and repeated freezing and thawing. Compared with the crack path in the unconditioned specimen, the paths observed after 15 and 20 cycles appeared relatively confined to the region above the prefabricated notch. At 10 cycles, the crack trajectory exhibited more pronounced bending and deflection. This pattern suggests that crack path morphology did not vary monotonically with increasing cycles.
These observations are qualitative and do not establish a systematic reduction in crack tortuosity with increasing cycle number. The differences in crack-path morphology indicate that salt freeze–thaw conditioning modifies the surface crack propagation behavior of the SCB specimens. These observations are considered together with the SCB fracture parameters, AE responses, and DIC measurements to examine the relationship between crack-path morphology, fracture resistance, and localized deformation.

3.1.2. Evolution of SCB Fracture Properties

SCB fracture tests were performed on specimens subjected to different numbers of salt freeze–thaw cycles, and the corresponding load–displacement responses were recorded, as shown in Figure 12a. Fracture energy Gf, stiffness S, flexibility index FI, and Mode I critical stress intensity factor KI were calculated using Equations (1)–(6). The SCB results are expressed as mean ± standard deviation (SD) based on three replicate specimens (n = 3). For each fracture parameter at each conditioning level, the coefficient of variation (CV) was calculated as SD/mean × 100%. Error bars in Figure 12b,c represent ±SD. Welch’s one-way ANOVA followed by Games–Howell post hoc comparisons was used to evaluate differences in Gf, KI, S, and FI among the five conditioning levels. The overall analysis revealed statistically significant differences among the conditioning levels for all four parameters (p < 0.05). The pairwise comparisons were further used to identify the specific conditioning levels exhibiting statistically significant differences.
Figure 12. SCB fracture properties: (a) load–displacement responses; (b) Gf and KI; (c) S and FI.
As shown in Figure 12b, both Gf and KI decreased continuously with increasing numbers of salt freeze–thaw cycles, indicating a progressive reduction in the fracture resistance of the SMA-13 mixture. Relative to the unconditioned specimens, Gf and KI decreased by 72.0% and 57.5%, respectively, after 20 cycles. These reductions demonstrate that salt freeze–thaw conditioning substantially weakened the energy dissipation capacity and crack propagation resistance of the mixture. The decrease in Gf was particularly pronounced during the first five cycles and gradually slowed thereafter. This trend indicates that damage developed rapidly during the initial conditioning stage, followed by continued deterioration as damage accumulated. The observed deterioration may be related to repeated phase transitions of the salt solution during freeze–thaw cycling and the associated accumulation of internal damage, as discussed in previous studies [35,36].
As shown in Figure 12c, S increased by 30.6% from the unconditioned state to 20 cycles. Because S is determined by the peak load and its corresponding displacement, this increase was mainly attributed to the reduction in peak displacement. It therefore reflects changes in the load–displacement response near the peak load and does not directly indicate improved fracture resistance. The FI decreased by approximately 32.4% overall, although its evolution was non-monotonic. During the first five cycles, FI decreased by approximately 27.4% relative to the unconditioned state. It subsequently increased by approximately 11.9% from 5 to 10 cycles before decreasing again between 10 and 20 cycles. Because FI is jointly governed by fracture energy and the slope at the inflection point of the post-peak load–displacement branch [37], its non-monotonic evolution indicates that fracture energy deterioration and degradation of the post-peak load–displacement response did not occur synchronously. During the early conditioning stage, changes in the post-peak load–displacement response temporarily increased FI. With continued accumulation of salt freeze–thaw damage, however, both fracture energy and post-peak deformation capacity decreased, resulting in an overall decline in FI.
Overall, Gf, S, FI, and KI primarily characterize the macroscopic fracture properties of the mixture. These parameters cannot independently resolve localized crack deformation or the evolution of internal damage under salt freeze–thaw conditioning. Therefore, AE and DIC analyses are required to further elucidate the associated damage mechanisms.

3.2. AE-Based Characterization of Internal Damage Evolution

To facilitate consistent comparisons of AE responses among specimens subjected to different salt freeze–thaw cycles, the normalized load–displacement curves were divided into four operational loading stages, using 0.8Fmax as a reference level on the pre-peak and post-peak branches. Stage I extended from the beginning of loading to 0.8Fmax on the pre-peak branch; Stage II extended from this level to Fmax; Stage III extended from Fmax to 0.8Fmax on the post-peak branch; and Stage IV extended from this level to the end of the test. The 0.8Fmax threshold was adopted as a practical reference for segmenting the loading process, rather than as a physically verified damage-transition point. Accordingly, these stages represent operational loading intervals rather than independently verified damage stages. Ring counts, cumulative AE energy, peak amplitude, and RA–AF characteristics were analyzed within these intervals to characterize fracture damage evolution.

3.2.1. Damage Evolution Based on Cumulative AE Energy

Ring counts reflect AE activity, whereas cumulative AE energy characterizes the accumulation of energy associated with detected AE signals during loading. These parameters provide complementary information for evaluating damage evolution in asphalt mixtures [38]. Figure 13 presents the time histories of load, ring counts, and cumulative AE energy for specimens subjected to different numbers of salt freeze–thaw cycles. AE parameters provide indirect indicators of damage-related activity but do not directly identify the underlying damage mechanisms.
Figure 13. Time histories of load, ring counts, and cumulative AE energy: (a) 0 cycles; (b) 5 cycles; (c) 10 cycles; (d) 15 cycles; (e) 20 cycles.
As shown in Figure 13, during Stage I, the load increased continuously, whereas the ring counts and cumulative AE energy increased slowly in all specimens. The relatively low AE activity suggests that this stage was dominated by overall deformation, accompanied by limited activation of pre-existing defects and microcracks. As the number of salt freeze–thaw cycles increased, the onset of AE activity occurred earlier, and cumulative AE energy began to increase markedly at lower load levels. This earlier onset may reflect increased susceptibility of pre-existing defects to external loading after salt freeze–thaw conditioning, leading to detectable damage-related activity at earlier loading stages.
During Stage II, the load gradually approached its peak value; the ring counts increased markedly, and the growth rate of cumulative AE energy accelerated. The increase in ring counts and cumulative AE energy indicates intensified AE activity and may reflect progressive activation and interaction of microcracks as the load approached its peak value. In the unconditioned specimens, AE energy was concentrated mainly around the peak load, whereas specimens subjected to salt freeze–thaw cycles exhibited a pronounced AE response before the peak load was reached. This comparison shows that detectable AE activity occurred at lower pre-peak load levels in the conditioned specimens. The surface crack-path observations in Section 3.1.1 provide complementary qualitative evidence of changes in crack morphology under different conditioning levels.
During Stage III, on the post-peak branch, the ring counts and cumulative AE energy continued to increase rapidly, indicating concentrated AE energy release. Although the macroscopic load began to decrease, ring counts and cumulative AE energy continued to increase, indicating that detectable AE activity persisted beyond the peak load. Thus, the peak load marks the transition from increasing to decreasing macroscopic load-bearing capacity rather than the cessation of AE activity. The pronounced post-peak AE activity may be associated with the formation and propagation of the dominant crack. As the number of salt freeze–thaw cycles increased, post-peak AE activity became more pronounced and the duration of concentrated energy release became shorter, suggesting a more abrupt post-peak fracture response and a faster progression toward final failure in the conditioned specimens.
During Stage IV, the load continued to decrease, while cumulative AE energy continued to increase at a lower rate than that observed in Stage III. This behavior suggests that fracture-related processes persisted during the later post-peak stage, potentially involving further crack extension, interactions along fracture surfaces, and progressive degradation of the remaining load-bearing structure. The lower rate of cumulative AE energy increase indicates that AE energy accumulation gradually slowed, although detectable AE activity did not cease completely. As the number of salt freeze–thaw cycles increased, Stage IV became shorter and AE energy release became increasingly concentrated. This suggests that salt freeze–thaw conditioning shortened the late post-peak loading interval and concentrated the AE energy release over a shorter period.
Overall, salt freeze–thaw conditioning changed the AE response from energy release concentrated mainly around the peak load in the unconditioned specimens to earlier pre-peak activity followed by increasingly concentrated AE activity during the post-peak stage. This pattern indicates an earlier onset of detectable AE activity, a shorter Stage II loading interval, and a more temporally concentrated post-peak AE response.

3.2.2. Temporal Evolution of AE Event Peak Amplitude

The peak amplitude of an AE event reflects the instantaneous signal intensity of an individual damage event. Its temporal distribution can be used to identify the occurrence and stage-dependent development of abrupt damage events [39]. Unlike cumulative AE energy, which characterizes the overall accumulation of damage, peak amplitude primarily reflects the intensity of individual damage events. Figure 14 presents the temporal distribution of AE event peak amplitudes during SCB loading for specimens subjected to different numbers of salt freeze–thaw cycles.
Figure 14. Temporal distribution of AE event peak amplitudes during SCB loading: (a) 0 cycles; (b) 5 cycles; (c) 10 cycles; (d) 15 cycles; (e) 20 cycles.
As shown in Figure 14, the peak amplitudes during Stage I were generally low, and AE events were sparsely distributed. This response indicates that the initial loading stage was dominated by the adjustment of local defects and minor damage activity. With increasing salt freeze–thaw cycles, some high-amplitude events occurred earlier, indicating that localized abrupt damage had already developed at relatively low load levels in the conditioned specimens. However, high-amplitude events remained limited, and crack activity had not yet developed into continuous propagation.
During Stage II, as the load approached its peak value, the number of peak-amplitude events increased, and several high-amplitude events began to appear. This response indicates that crack activity evolved from localized initiation toward more sustained damage development. In the unconditioned specimens, high-amplitude events were concentrated mainly around the peak load, whereas the salt freeze–thaw-conditioned specimens exhibited a more pronounced amplitude response before the peak load was reached. This finding indicates that salt freeze–thaw conditioning advanced the occurrence of localized damage events and is consistent with the earlier increase in cumulative AE energy observed during Stage II.
During Stage III, the AE peak-amplitude response increased markedly, and high-amplitude events were concentrated around the peak load and within the post-peak interval. As the macroscopic load began to decrease, these intense transient damage events were associated with the rapid propagation of the dominant crack. Compared with the unconditioned specimens, the conditioned specimens exhibited a more concentrated distribution of high-amplitude events during the post-peak stage, indicating that salt freeze–thaw damage promoted localized rapid failure during load-bearing degradation.
During Stage IV, the load continued to decrease, while several AE events with measurable peak amplitudes remained detectable, indicating that internal damage continued to develop during the residual damage stage. The reduced number of high-amplitude events suggests that the intense AE activity associated with rapid crack propagation had diminished, although internal damage continued to develop. The remaining AE activity was mainly associated with further adjustment of the fracture region, interfacial friction, and failure of the residual load-bearing structure. As the number of salt freeze–thaw cycles increased, high-amplitude AE events became more concentrated during the post-peak stage, suggesting a more temporally localized distribution of intense damage events.
Overall, the AE peak-amplitude distribution changed from a concentration of high-amplitude events near the peak load in the unconditioned specimens to earlier pre-peak occurrence followed by a more concentrated distribution of high-amplitude events during the post-peak stage in specimens subjected to salt freeze–thaw cycles. This evolution indicates that salt freeze–thaw conditioning modified the temporal and intensity distributions of individual damage events, causing localized abrupt damage to occur earlier and develop more intensively during post-peak load degradation.

3.2.3. RA–AF Analysis of Cracking Modes

Previous studies have shown that RA–AF parameters can be used to distinguish cracking modes during asphalt mixture fracture. AE events in the low-RA/high-AF region are generally associated with tensile-type cracking, whereas events in the high-RA/low-AF region are commonly associated with shear-type cracking [39,40]. The RA parameter is defined as the ratio of rise time to peak amplitude, whereas AF is defined as the ratio of ring counts to event duration. To quantitatively evaluate changes in the relative proportions of tensile-type and shear-type AE events with increasing numbers of salt freeze–thaw cycles, the RA–AF method was adopted. For each salt freeze–thaw condition, RA and AF were independently normalized using the min–max method, with the minimum and maximum values calculated separately from the AE events in that condition, as expressed in Equations (11) and (12).
AF norm = AF − min ( AF ) max ( AF ) − min ( AF )
RA norm = RA − min ( RA ) max ( RA ) − min ( RA )
Based on the RA–AF crack-mode interpretation reported in previous studies [39,40,41], an operational threshold of RAnorm/AFnorm = 0.5 was adopted in this study to classify the normalized AE events. Events with RAnorm/AFnorm ≥ 0.5 were classified as shear-type events, whereas those with RAnorm/AFnorm < 0.5 were classified as tensile-type events. The corresponding classification boundary is AFnorm = 2RAnorm in the normalized coordinate system. Events with AFnorm = 0, for which the ratio is undefined, were excluded from the proportion analysis. The threshold was used as an operational criterion in this study rather than a universal physical boundary. Its sensitivity was examined using two additional thresholds of 0.4 and 0.6. The same valid AE hit population and group-specific normalization values were maintained for all three thresholds, allowing the effect of threshold selection on the classification results to be evaluated independently. The RA–AF distributions and the proportions of the two event types are presented in Figure 15.
Figure 15. RA–AF distributions and proportions of tensile- and shear-type AE events: (a) proportions of classified AE events; (b) RA–AF distributions after group-specific min–max normalization. The diagonal line in (b) represents the identity relation (RAnorm = AFnorm) and is included for visual reference only; it does not represent the operational classification.
As shown in Figure 15a, both tensile-type and shear-type AE events were detected under all salt freeze–thaw conditions, indicating the coexistence of the two types of cracking activity during SCB loading. Using the selected threshold of RAnorm/AFnorm = 0.5, the shear-type event proportions were 65.5%, 63.7%, 44.6%, 64.4%, and 69.1% after 0, 5, 10, 15, and 20 cycles, respectively. The corresponding tensile-type proportions were 34.5%, 36.3%, 55.4%, 35.6%, and 30.9%. The shear-type proportion reached its minimum at 10 cycles before increasing at 15 and 20 cycles, showing a non-monotonic change in the relative composition of AE events.
The results obtained using the alternative thresholds are summarized in Table 4. Although the calculated proportions differed among the three thresholds, the shear-type proportion remained lowest at 10 cycles and increased at 15 and 20 cycles. However, the dominant event type at 10 cycles depended on the selected threshold: shear-type events accounted for 54.2% at a threshold of 0.4, whereas tensile-type events accounted for 55.4% and 59.0% at thresholds of 0.5 and 0.6, respectively. Accordingly, the observed changes are interpreted as variations in the relative composition of AE event types rather than definitive evidence of a transition in the macroscopic cracking mode.
Table 4. Sensitivity of RA–AF event classification to alternative normalized thresholds.
The RA–AF analysis characterizes the relative composition of AE event types under the adopted classification criterion but cannot independently establish the macroscopic fracture mode. Therefore, the RA–AF results should be interpreted alongside the load–displacement response, AE energy evolution, and DIC-derived surface strain and crack-opening responses to provide a more comprehensive assessment of fracture damage evolution.

3.3. DIC-Based Evolution of Surface Deformation

3.3.1. Evolution of the Horizontal Strain Field

To investigate the influence of salt freeze–thaw cycling on surface deformation in the crack region of the SMA-13 mixture, DIC was used to obtain the horizontal strain field Exx during SCB loading. The Exx distributions at the characteristic load levels under different salt freeze–thaw conditioning levels are shown in Table 5. Because of the considerable differences in strain magnitudes among the conditioning and loading conditions, individual color scales were retained to preserve the visibility of local strain distribution features. Therefore, the contour plots are used primarily for qualitative examination of spatial strain patterns, while quantitative comparisons are based on the spatially averaged Exx values.
Table 5. Evolution of the surface horizontal strain field of SMA-13 specimens.
At the pre-peak 0.8Fmax level, a high-Exx region first developed near the tip of the prefabricated notch in all specimens, forming a localized strain-concentration zone. However, a continuous dominant strain band had not yet formed. As the load increased to Fmax, the high-strain region extended upward from the notch, and the localized strain-concentration zones gradually connected to form a relatively continuous dominant strain band. Moderate bending and deflection of the strain band were also observed in some specimens. At the 0.8Fmax level on the post-peak branch, the dominant strain band continued to develop along the path established near the peak load. When the load decreased to the 0.3Fmax level on the pre-peak and post-peak branches, its main location and propagation direction remained generally unchanged, with only limited local extension.
These observations indicate that a relatively stable crack-propagation path was established near the peak-load stage, whereas the post-peak stage was dominated by the continued development of the existing crack region. Although the pre-peak and post-peak 0.8Fmax levels corresponded to the same load ratio, their strain distributions differed markedly. Before the peak load, strain concentration remained mainly confined to the crack-tip region. After the peak load, a dominant strain band had already formed and continued to extend along the established path. This finding demonstrates that localized deformation continued after the peak load and that load reduction did not restore the damage state to its pre-peak condition [27].
The spatial morphology of the dominant strain band varied with the number of salt freeze–thaw cycles. The unconditioned specimens exhibited a relatively continuous high-strain path extending upward from the notch tip. After five cycles, the overall propagation pattern remained similar, although the continuity of the strain band decreased. After 10 cycles, the dominant strain band showed more pronounced bending and deflection, and the crack trajectory became more tortuous. After 15 and 20 cycles, the high-strain region became increasingly concentrated above the notch, while continuous extension away from the crack-tip region was restricted. This behavior may be attributed to the heterogeneous damage induced by salt freeze–thaw cycling, which promoted crack propagation through local weak zones [28].
Overall, salt freeze–thaw cycling affected both the spatial distribution of the high-strain region and the formation and propagation of the dominant strain band. With limited conditioning, the crack formed a relatively continuous strain band and retained a certain post-peak propagation capacity. With increasing conditioning severity, the strain band exhibited greater path deflection, stronger crack-tip localization, and more restricted extension. In all specimens, crack initiation remained controlled by the prefabricated notch, whereas salt freeze–thaw conditioning mainly affected the subsequent crack-propagation process.

3.3.2. Temporal Evolution of Horizontal Strain at Monitoring Locations

The time-dependent Exx responses at monitoring locations C1–C4 under different salt freeze–thaw conditioning levels are shown in Figure 16.
Figure 16. Evolution of horizontal strain Exx at monitoring locations C1–C4: (a) 0 cycles; (b) 5 cycles; (c) 10 cycles; (d) 15 cycles; (e) 20 cycles.
During the initial loading stage, the strain at all monitoring locations remained low. As the load increased, pronounced strain localization developed above the prefabricated notch and extended upward along the anticipated crack-propagation path. In the DIC-monitored specimen from the unconditioned group, C1, which was closest to the notch tip, exhibited a marked strain increase first, followed by the gradual development of deformation at C2–C4. The strain magnitude generally decreased with increasing distance from the crack tip, indicating that localized deformation was concentrated near the crack tip and exhibited a clear spatial gradient.
For the DIC-monitored specimens, the overall Exx response at C1–C4 was lower at higher salt freeze–thaw conditioning levels. After the peak load was reached, Exx continued to increase at some monitoring locations, indicating that the peak load represented the maximum macroscopic load-bearing capacity but did not mark the end of localized crack deformation. For each conditioning group, the spatial average of the maximum Exx values at C1–C4 throughout the loading process is reported in Table 6.
Table 6. Spatially averaged maximum horizontal strain Exx at monitoring locations C1–C4.
The spatially averaged maximum horizontal strain values decreased from 16.92% in the unconditioned group to 4.79% in the 20-cycle group, corresponding to a reduction of 71.71%. The decrease was relatively limited during the first five cycles but became more pronounced at higher conditioning levels. These measurements indicate a lower localized strain response in the DIC-monitored specimens subjected to more salt freeze–thaw cycles. However, because only one specimen per conditioning group was monitored by DIC, these observations are specimen-specific and do not provide an estimate of between-specimen variability.

3.3.3. Crack-Opening Response Before and After the Peak Load

To further characterize crack opening before and after the peak load, three characteristic load levels were selected: the pre-peak 0.8Fmax, peak load Fmax, and post-peak 0.8Fmax. The normalized crack-opening responses at L1–L4 under different salt freeze–thaw conditioning levels were compared, as shown in Figure 17.
Figure 17. Normalized crack-opening responses at L1–L4: (a) 0 cycles; (b) 5 cycles; (c) 10 cycles; (d) 15 cycles; (e) 20 cycles.
As the load increased from the pre-peak 0.8Fmax level to Fmax and then decreased to the post-peak 0.8Fmax level, the crack-opening response developed from limited localized deformation into pronounced crack opening and continued to increase during the post-peak stage. The unconditioned specimens exhibited the largest response at L1 at all three characteristic load levels, indicating that crack opening was dominated by the region near L1. Because L1 was located near the prefabricated notch tip, its large response confirms that crack-opening deformation was concentrated primarily in the crack-tip region. At the post-peak 0.8Fmax level, the normalized response at L1 reached 26.62%, substantially exceeding those at L2–L4.
The overall crack-opening response decreased with increasing salt freeze–thaw cycles. The spatially averaged normalized crack-opening response across L1–L4 at the post-peak stage decreased from 12.57% in the unconditioned specimen to 10.08%, 8.57%, 5.03%, and 3.84% after 5, 10, 15, and 20 cycles, respectively. The corresponding mean crack-opening displacements were 1.886, 1.512, 1.286, 0.755, and 0.576 mm, respectively. Although the overall crack-opening deformation decreased, L1 remained the dominant opening location under all conditioning levels, indicating that the controlling role of the crack-tip region was maintained.
At the post-peak 0.8Fmax level, the normalized response at L1 decreased from 26.62% in the unconditioned specimens to 9.14% after 20 cycles. The responses at L2–L4 also generally decreased, although some fluctuations occurred among the different measurement levels. This indicates that L1 remained the dominant crack-opening location, whereas the deformation responses at L2–L4 were adjusted as the crack propagated.
Under all conditioning levels, the response at L1 increased from the pre-peak 0.8Fmax level to Fmax and further to the post-peak 0.8Fmax level. This confirms that the dominant crack continued to open after the peak load. This result is consistent with the continued ring count activity, the evolution of AE event amplitude, and the increase in cumulative AE energy observed during the post-peak stage. AE characterized the continued temporal development of post-peak damage, whereas DIC revealed the spatial concentration of crack-opening deformation near the crack tip.
Overall, salt freeze–thaw cycling progressively reduced the crack-opening response of the specimens. The deformation changed from a pronounced crack-opening response in the unconditioned specimens to a lower-amplitude and more localized response after extensive conditioning. Nevertheless, L1 remained the dominant opening location, indicating that salt freeze–thaw cycling reduced the magnitude of crack deformation without changing the fundamental crack-tip-controlled deformation pattern.

4. Conclusions

The fracture damage evolution of an SMA-13 asphalt mixture containing 0.2% basalt fiber (by mixture mass, with 6 and 9 mm fibers blended at a 1:1 mass ratio) subjected to the laboratory salt freeze–thaw conditioning protocol adopted in this study was investigated using SCB testing, AE monitoring, and DIC. The main conclusions are as follows:
(1)
The fracture resistance of the SMA-13 mixture deteriorated with increasing salt freeze–thaw cycles, as evidenced by reductions in fracture energy Gf, Mode I critical stress intensity factor KI, and flexibility index FI. After 20 cycles, Gf and KI decreased by 72.0% and 57.5%, respectively, whereas stiffness S increased by 30.6% in association with reduced peak displacement. FI exhibited an initial decrease, a temporary recovery, and a subsequent decline. The most pronounced deterioration occurred during the first five cycles.
(2)
The fracture damage process was accompanied by distinct changes in AE activity and cumulative AE energy. With increasing salt freeze–thaw cycles, AE activity extended further into the pre-peak stage, while cumulative AE energy continued to increase during post-peak loading. RA–AF analysis showed that the proportion of shear-type AE events decreased from 65.5% at 0 cycles to 44.6% at 10 cycles, before increasing to 69.1% at 20 cycles. These findings indicate a non-monotonic variation in the relative proportions of tensile- and shear-type AE events under the laboratory conditioning conditions investigated.
(3)
DIC measurements from the single specimen subjected to synchronized AE and DIC monitoring in each conditioning group showed reductions in localized surface strain and crack-opening deformation with increasing salt freeze–thaw cycles. The spatially averaged maximum horizontal strain Exx across C1–C4 decreased from 16.92% to 4.79%, while the mean normalized crack-opening response across L1–L4 decreased from 12.57% to 3.84% at the post-peak 0.8 Fmax level. These values represent the measured responses of the monitored specimens rather than statistically representative group means.
(4)
SCB testing and synchronized AE and DIC monitoring provided complementary information on the fracture behavior of the investigated asphalt mixture. SCB testing quantified changes in macroscopic fracture resistance and post-peak mechanical response. AE monitoring captured the temporal evolution of damage-related activity and the relative proportions of tensile and shear-type AE events, whereas DIC characterized the spatial distribution of surface strain and crack opening deformation. Considered together at the conditioning group level, these measurements provided a multiscale description of fracture damage evolution under the laboratory salt freeze–thaw protocol used in this study. The four operational loading intervals provided a consistent framework for comparing AE responses during loading.
(5)
Several limitations should be noted. Water-only freeze–thaw and salt-immersion-only control groups were not included, preventing the separation of the individual and combined effects of salt exposure and freeze–thaw cycling. Although three replicate specimens were tested for SCB in each conditioning group, synchronized AE and DIC monitoring was conducted on only one specimen per group, limiting the assessment of between-specimen variability. AE source localization was not performed, and DIC measurements may be influenced by image quality and processing parameters, despite the use of consistent settings across groups. Furthermore, only one SMA-13 mixture and fiber formulation were investigated. Future studies should incorporate additional control groups, increase the number of specimens subjected to synchronized AE and DIC monitoring, and examine AE source localization, DIC parameter sensitivity, and different SMA mixtures and fiber formulations.

Author Contributions

Conceptualization, Q.Z. and H.J.; Methodology, Z.Z.; Software, Z.Z.; Validation, Z.Z.; Formal Analysis, K.R. and B.Y.; Investigation, Q.Z.; Resources, Q.Z.; Writing—Original Draft, Z.Z.; Supervision, K.R. and B.Y.; Project administration, Q.Z.; Funding acquisition, Q.Z. All authors have read and agreed to the published version of the manuscript.

Funding

This study was funded by the National Natural Science Foundation of China (grant no. 52068062), the Xinjiang Talent Development Fund (grant no. 2024TSYCCX0121), and the Graduate Research and Innovation Project of Tarim University (grant no. TDGRI2025098).

Institutional Review Board Statement

Not applicable.

Data Availability Statement

The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding authors.

Conflicts of Interest

The authors declare no conflicts of interest.

References

  1. Zhang, K.; Li, W.; Han, F. Performance deterioration mechanism and improvement techniques of asphalt mixture in salty and humid environment. Constr. Build. Mater. 2019, 208, 749–757. [Google Scholar] [CrossRef] [Scilit]
  2. Guo, Q.; Li, G.; Gao, Y.; Wang, K.; Dong, Z.; Liu, F.; Zhu, H. Experimental investigation on bonding property of asphalt-aggregate interface under the actions of salt immersion and freeze-thaw cycles. Constr. Build. Mater. 2019, 206, 591–599. [Google Scholar] [CrossRef] [Scilit]
  3. Wang, F.; Qin, X.; Pang, W.; Wang, W. Performance deterioration of asphalt mixture under chloride salt erosion. Materials 2021, 14, 3339. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  4. Wu, H.; Li, P.; Nian, T.; Zhang, G.; He, T.; Wei, X. Evaluation of asphalt and asphalt mixtures’ water stability method under multiple freeze-thaw cycles. Constr. Build. Mater. 2019, 228, 117089. [Google Scholar] [CrossRef] [Scilit]
  5. Devulapalli, L.; Sarang, G.; Kothandaraman, S. Characteristics of aggregate gradation, drain down and stabilizing agents in stone matrix asphalt mixtures: A state of art review. J. Traffic Transp. Eng. (Engl. Ed.) 2022, 9, 167–179. [Google Scholar] [CrossRef] [Scilit]
  6. Xue, J.; Jiang, Y.; Zheng, Y.; Xiong, S. Optimization design and verification of SMA-13 mixture gradation using mortar theory. Constr. Build. Mater. 2022, 335, 127478. [Google Scholar] [CrossRef] [Scilit]
  7. Qin, X.; Shen, A.; Guo, Y.; Li, Z.; Lv, Z. Characterization of asphalt mastics reinforced with basalt fibers. Constr. Build. Mater. 2018, 159, 508–516. [Google Scholar] [CrossRef] [Scilit]
  8. Guo, Q.; Chen, Z.; Liu, P.; Li, Y.; Hu, J.; Gao, Y.; Li, X. Influence of basalt fiber on Mode I and II fracture properties of asphalt mixture at medium and low temperatures. Theor. Appl. Fract. Mech. 2021, 112, 102884. [Google Scholar] [CrossRef] [Scilit]
  9. Li, X.J.; Marasteanu, M.O. Using semi-circular bending test to evaluate low temperature fracture resistance for asphalt concrete. Exp. Mech. 2010, 50, 867–876. [Google Scholar] [CrossRef] [Scilit]
  10. Saha, G.; Biligiri, K.P. Fracture properties of asphalt mixtures using semi-circular bending test: A state-of-the-art review and future research. Constr. Build. Mater. 2016, 105, 103–112. [Google Scholar] [CrossRef] [Scilit]
  11. Ozer, H.; Al-Qadi, I.L.; Lambros, J.; El-Khatib, A.; Singhvi, P.; Doll, B. Development of the fracture-based flexibility index for asphalt concrete cracking potential using modified semi-circle bending test parameters. Constr. Build. Mater. 2016, 115, 391–401. [Google Scholar] [CrossRef] [Scilit]
  12. Kaseer, F.; Yin, F.; Arámbula-Mercado, E.; Martin, A.E.; Daniel, J.S.; Salari, S. Development of an index to evaluate the cracking potential of asphalt mixtures using the semi-circular bending test. Constr. Build. Mater. 2018, 167, 286–298. [Google Scholar] [CrossRef] [Scilit]
  13. Lim, I.L.; Johnston, I.W.; Choi, S.K. Stress intensity factors for semi-circular specimens under three-point bending. Eng. Fract. Mech. 1993, 44, 363–382. [Google Scholar] [CrossRef] [Scilit]
  14. Karimi, M.M.; Dehaghi, E.A.; Behnood, A. A fracture-based approach to characterize long-term performance of asphalt mixes under moisture and freeze-thaw conditions. Eng. Fract. Mech. 2021, 241, 107418. [Google Scholar] [CrossRef] [Scilit]
  15. Qiu, X.; Xu, J.; Xiao, S.; Yang, Q. Acoustic emission parameters and waveforms characteristics of fracture failure process of asphalt mixtures. Constr. Build. Mater. 2019, 215, 135–147. [Google Scholar] [CrossRef] [Scilit]
  16. Qiu, X.; Xu, J.; Xu, W.; Yang, Q.; Wang, F.; Yuan, J. Diagnosis of damage evolution process for asphalt mixtures using pattern recognition with acoustic emission signals. Constr. Build. Mater. 2021, 280, 122536. [Google Scholar] [CrossRef] [Scilit]
  17. Fu, L.; Zhou, H.; Yuan, J.; An, W.; Chen, X. Damage fracture characterization of asphalt mixtures considering freeze-thaw cycling and aging effects based on acoustic emission monitoring. Materials 2021, 14, 5930. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  18. Liang, C.; Ma, J.; Zhou, P.; Ma, G.; Xu, X. Fracture damage properties of SBS-modified asphalt mixtures reinforced with basalt fiber after freeze-thaw cycles using the acoustic emission approach. Appl. Sci. 2020, 10, 3301. [Google Scholar] [CrossRef] [Scilit]
  19. Qiu, J.; Yang, Q.; Qiu, X.; Xiao, S.; He, L.; Hu, G. Use of acoustic emission for exploring characteristics and behaviors of mixed-mode fracture process of asphalt mixtures. Mater. Struct. 2022, 55, 199. [Google Scholar] [CrossRef] [Scilit]
  20. Fu, L.; Jiao, Y.; Chen, X. Reinforcement evaluation of different fibers on fracture resistance of asphalt mixture based on acoustic emission technique. Constr. Build. Mater. 2022, 314, 125606. [Google Scholar] [CrossRef] [Scilit]
  21. Jiao, Y.; Zhang, Y.; Zhang, M.; Fu, L.; Zhang, L. Investigation of fracture modes in pervious asphalt under splitting and compression based on acoustic emission monitoring. Eng. Fract. Mech. 2019, 211, 209–220. [Google Scholar] [CrossRef] [Scilit]
  22. Li, J.; Wang, L.; Zhang, X.; Miao, Y.; Guo, Y.; Wang, Y. Cracking process analysis and fracture pattern recognition of asphalt mixture based on acoustic emission characteristics. J. Mater. Civ. Eng. 2023, 35, 4023449. [Google Scholar] [CrossRef] [Scilit]
  23. Yoneyama, S. Basic principle of digital image correlation for in-plane displacement and strain measurement. Adv. Compos. Mater. 2016, 25, 105–123. [Google Scholar] [CrossRef] [Scilit]
  24. Mousa, M.A.; Yussof, M.M.; Hussein, T.S.; Assi, L.N.; Ghahari, S. A digital image correlation technique for laboratory structural tests and applications: A systematic literature review. Sensors 2023, 23, 9362. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  25. Yuan, F.; Cheng, L.; Shao, X.; Dong, Z.; Zhang, L.; Wu, G.; He, X. Full-field measurement and fracture and fatigue characterizations of asphalt concrete based on the SCB test and stereo-DIC. Eng. Fract. Mech. 2020, 235, 107127. [Google Scholar] [CrossRef] [Scilit]
  26. Zieliński, P.; Klimczak, M.; Tekieli, M.; Strzępek, M. An evaluation of the fracture properties of asphalt concrete mixes using the semi-circular bending method and digital image correlation. Materials 2025, 18, 967. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  27. Ren, H.; Qian, Z.; Huang, W.; Bo, W.; Chen, T.; Cao, H. Evaluation of fracture behavior in asphalt concrete through the combination of semi-circular bending test and digital image correlation technology. Constr. Build. Mater. 2024, 451, 138854. [Google Scholar] [CrossRef] [Scilit]
  28. Cao, G.; Qing, L.; Duan, J.; Chen, L.; Zeng, J.; Yan, E.; Liu, T. Investigations on the crack resistance characteristics of asphalt concrete based on digital image correlation method. Eng. Fract. Mech. 2024, 307, 110290. [Google Scholar] [CrossRef] [Scilit]
  29. Hu, G.; Yang, Q.; Qiu, X.; Zhang, D.; Zhang, W.; Xiao, S.; Xu, J. Use of DIC and AE for investigating fracture behaviors of cold recycled asphalt emulsion mixtures with 100% RAP. Constr. Build. Mater. 2022, 344, 128278. [Google Scholar] [CrossRef] [Scilit]
  30. Ye, Y.; Yang, Q.; Xiao, S.; Qiu, X.; Xiong, Y.; Yang, W. Fracture evolution characteristics of asphalt concrete using digital image correlation and acoustic emission techniques. Constr. Build. Mater. 2024, 447, 138100. [Google Scholar] [CrossRef] [Scilit]
  31. Jiao, Y.; Du, W.; Yang, H.; Shi, H. Low temperature failure behavior analysis of fiber reinforced asphalt concrete under indirect tension test using acoustic emission and digital image correlation. Case Stud. Constr. Mater. 2024, 20, e02720. [Google Scholar] [CrossRef] [Scilit]
  32. Guo, F.; Li, R.; Lu, S.; Bi, Y.; He, H. Evaluation of the effect of fiber type, length, and content on asphalt properties and asphalt mixture performance. Materials 2020, 13, 1556. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  33. Ji, X.; Yuan, Y.; Huang, Y.; Shao, J.; Li, S. Performance study of asphalt mixtures reinforced with gradated basalt fibers of mixed lengths. Materials 2024, 17, 4706. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  34. Zhang, Y.; Sang, T.; Kang, A.; Wang, B.; Wu, X.; Zhao, Y. Investigation of fiber length distribution on crack resistance mechanism of basalt fiber asphalt mixture based on digital image processing technology. Constr. Build. Mater. 2023, 401, 132753. [Google Scholar] [CrossRef] [Scilit]
  35. Feng, D.; Yi, J.; Wang, D.; Chen, L. Impact of salt and freeze-thaw cycles on performance of asphalt mixtures in coastal frozen region of China. Cold Reg. Sci. Technol. 2010, 62, 34–41. [Google Scholar] [CrossRef] [Scilit]
  36. Feng, B.; Wang, H.; Li, S.; Ji, K.; Li, L.; Xiong, R. The durability of asphalt mixture with the action of salt erosion: A review. Constr. Build. Mater. 2022, 315, 125749. [Google Scholar] [CrossRef] [Scilit]
  37. Radeef, H.; Hassan, N.; Mahmud, M.; Usman, K.; Ismail, C.; Al Saffar, Z.; Abbas, H. Influence of ageing and moisture damage on the Illinois flexibility index value of polymer modified asphalt mixture. Phys. Chem. Earth Parts A/B/C 2022, 128, 103248. [Google Scholar] [CrossRef] [Scilit]
  38. Song, W.; Yan, W.; Wu, H.; Sun, Y.; Chen, X.; Cheng, Z. Investigation of fracture behaviors of asphalt mixtures with different loading rates based on acoustic emission. Theor. Appl. Fract. Mech. 2025, 139, 105034. [Google Scholar] [CrossRef] [Scilit]
  39. Yang, K.; He, Z.; Li, D.; Xu, H.; Kong, L. Experimental study on basalt fiber crack resistance of asphalt concrete based on acoustic emission. Materials 2021, 14, 4096. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  40. Zhu, B.; Liu, H.; Li, W.; Wu, C.; Chai, C. Fracture behavior of permeable asphalt mixtures with steel slag under low temperature based on acoustic emission technique. Sensors 2020, 20, 5090. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  41. Lu, X.; Xu, G.; Hu, P.; Wang, S.; Chen, X. Cracking mode transition and anti-cracking mechanism of steel slag modified stone mastic asphalt mixtures: A multiscale SCB-AE-DIC-PFC investigation. Constr. Build. Mater. 2026, 542, 148115. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.