Abstract
Wire-arc additive manufacturing (WAAM) based on cold metal transfer (CMT) is a promising repair technique for hydraulic turbine components made of 410NiMo martensitic stainless steel owing to its low heat input and high deposition efficiency. In this study, single-pass single-layer deposition experiments were carried out to clarify the influences of wire-feeding speed and welding speed on bead geometry. The optimal combination of process parameters, i.e., wire-feeding speed of 5 m/min and welding speed of 3 mm/s, was determined by the control-variable method. A back-propagation (BP) neural network was established to predict the geometric dimensions of single-pass beads, and the prediction error was as low as 1.46% under the verification condition. Using the optimised parameters, thin-wall samples were fabricated at interlayer temperatures of 150 °C and 350 °C. Macro-formability, microstructure, Vickers hardness and tensile performance were systematically characterised. The results showed that the thin-wall sample deposited at 150 °C possessed smoother surface morphology. Dominant lath martensite was observed at 150 °C, whereas cyclic thermal exposure at 350 °C triggered the precipitation of blocky ferrite and grain-boundary carbides. The average Vickers hardness decreased from 337.13 HV (150 °C) to 328.34 HV (350 °C), and lower hardness consistently appeared at fusion interfaces compared with inner weld zones. Benefiting from the cyclic low-temperature tempering effect, specimens fabricated at 350 °C exhibited distinctly higher tensile and yield strengths. This work provides fundamental experimental support for process optimisation of CMT-WAAM 410NiMo martensitic stainless steel for component-repair applications.
1. Introduction
Additive manufacturing (AM) enables near-net-shape component fabrication by layer-by-layer material deposition, which circumvents many limitations of conventional subtractive manufacturing [1,2]. As an important branch of metal AM, wire-arc additive manufacturing (WAAM) employs an electric arc to melt metallic wire feedstock, possessing distinctive advantages including high material utilisation, low equipment cost, and few restrictions on component dimensions [3,4]. Consequently, WAAM has attracted increasing interest in aerospace, shipbuilding and equipment remanufacturing fields [5,6].
Cold metal transfer (CMT) is a modified gas-metal-arc-welding (GMAW) variant characterised by controlled wire retraction during short-circuit metal transfer, which remarkably reduces heat input and spatter formation, making it favourable for depositing thin-wall metallic structures [7,8]. Martensitic stainless steel 410NiMo exhibits good mechanical strength and moderate cavitation-erosion resistance and is widely used for hydraulic turbine parts suffering from erosion-corrosion service conditions [9,10]. Repair of worn or cracked turbine components using WAAM is an economical alternative to replacing entire parts. Nevertheless, 410NiMo martensitic stainless steel is highly sensitive to thermal cycles during WAAM. Repeated heating and cooling give rise to complex solid-state phase transformations, residual stress, distortion, and anisotropic mechanical performance, which hinder reliable engineering applications [11,12,13].
Interlayer temperature is one of the most critical thermal variables in WAAM. It governs the cooling rate, residence time at elevated temperature and degree of cyclic tempering of previously deposited layers and further determines macro-formability, phase constitution and final mechanical performance [14,15]. Teixeira et al. [16] investigated coupled interlayer temperature and travel speed for low-alloy steel WAAM thin walls under natural and near-immersion active cooling, showing that cooling has little influence on geometry and microstructure and that high parameter combinations reduce production time under active cooling. Plazas et al. [17] revealed that Δt variation along the build height drives ferrite evolution and hardness reduction and yields thermal homogenization of carbon steel microstructure during GMAW-based WAAM. Li et al. [18] reported that, for WA-DED H13 steel thin walls, interlayer temperature modulates martensite, dislocations and precipitates, and dislocation strengthening primarily controls the mechanical properties, with the peak tensile strength obtained at an interlayer temperature of 400 °C. Existing studies have reported the influences of interlayer temperature on several martensitic stainless steels, whereas systematic investigations focusing on CMT-WAAM 410NiMo remain limited, especially regarding the correlation between interlayer temperature, cyclic thermal history and resultant microstructure–property relationships.
In WAAM repair practice, surface contaminants, including grease, oxide scale, and residual impurities on substrate surfaces, exert detrimental effects on deposited-bead integrity: surface contaminants can decompose within the high-temperature arc pool, introducing gas pores, inclusions, and local brittleness, which degrade both mechanical performance and service reliability of additively manufactured components [19,20]. Initial material conditions of the substrate, such as metallurgical state, prior damage history and heat-treatment status, also determine heat dissipation behaviour, dilution extent and resultant microstructure at the fusion interface [21,22]. Moreover, residual protective coatings (e.g., thermal-sprayed hard-facing layers and anti-corrosion coatings) on turbine components must be completely removed prior to WAAM deposition; incomplete coating removal will give rise to interfacial defects and elemental contamination of the martensitic stainless-steel deposit [23].
In the present work, single-pass single-layer bead experiments were performed to obtain feasible processing windows. A BP neural network was constructed for bead geometry prediction. Thin-wall samples were fabricated at interlayer temperatures of 150 °C and 350 °C. Macroscopic appearance, phase/microstructural features, Vickers hardness, and tensile behaviours were characterised. The underlying microstructure–property mechanisms induced by different interlayer thermal histories were discussed. This work aims to provide a fundamental experimental reference for WAAM repair of hydraulic-turbine-grade 410NiMo components.
2. Materials and Methods
2.1. Experimental Materials
ER410NiMo solid wire with a diameter of 1.2 mm was selected as the filler material. 1Cr18Ni9 stainless steel plates with dimensions of 400 mm × 200 mm × 10 mm and 150 mm × 100 mm × 8 mm served as substrates. Prior to deposition, substrate surfaces were ground and cleaned with anhydrous ethanol to remove oxides and contaminants. Nominal chemical compositions of the substrate and wire are summarised in Table 1.
Table 1.
Chemical compositions of substrate and ER410NiMo wire (wt.%).
Note that the as-received 1Cr18Ni9 substrate plates were free of any protective coatings. Prior to deposition, all substrate surfaces were ground and cleaned with anhydrous ethanol to remove surface oxides and organic contaminants to prevent impurity-induced deposition defects. After grinding, the arithmetic mean surface roughness Ra of the substrate was approximately 2.1 ± 0.3 μm, and the average initial Vickers hardness of the as-received substrate was 182 ± 7 HV. These initial surface and hardness conditions were kept consistent across all WAAM deposition trials in the present work.
2.2. Experimental Equipment and Procedures
2.2.1. CMT-WAAM Experimental Platform
The WAAM system consists of a Fronius TPS 4000 CMT welding source (Fronius International GmbH, Wels, Austria) and a KUKA KR 8 R1620 arc-HW six-axis industrial robot (KUKA AG, Augsburg, Germany). CMT achieves spatter-free droplet transfer through synchronous control of the current waveform and mechanical wire retraction. The protective gas mixture was 97.5% Ar + 2.5% O2.
2.2.2. Single-Pass Single-Layer Bead Deposition
Single-pass single-layer tests were implemented with varied wire-feeding speed (2–6 m/min) and travel speed (2–6 mm/s). Nozzle-to-work distance was kept at 15 mm with a torch angle of 90°. Bead width and bead height (reinforcement) were measured to evaluate formability. The reinforcement coefficient was defined as the ratio of bead height to bead width.
2.2.3. BP Neural Network for Bead-Geometry Prediction
Experimental data from single-pass single-layer tests (excluding discontinuous-bead invalid data) were imported into MATLAB R2024a. Wire-feeding speed and travel speed were set as input variables; bead width, bead height, and reinforcement coefficient were treated as outputs. The dataset was partitioned: 70% for training, 15% for validation, and 15% for testing. A two-layer feed-forward BP neural network with 10 hidden neurons was trained using the Levenberg–Marquardt algorithm. The coefficient of determination R2 was adopted to assess prediction accuracy.
2.2.4. Single-Pass Multi-Layer Thin-Wall Fabrication
Based on the optimised single-pass parameters (wire-feeding speed = 5 m/min, travel speed = 3 mm/s), thin-wall specimens were deposited under two controlled interlayer temperatures: 150 °C and 350 °C. A reciprocating “zig-zag” deposition path was applied to mitigate collapse at both ends of each layer. Main processing parameters are listed in Table 2. Infrared thermometry was used to monitor the surface temperature of the deposited layer; subsequent layer deposition started only when the surface temperature cooled down to the preset interlayer temperature.
Table 2.
Key parameters for single-pass multi-layer thin-wall WAAM.
2.2.5. Characterisation Procedures
Metallographic specimens were sectioned along the building direction from the stable middle region of as-deposited thin-wall samples. Specimens were mounted, ground step by step with abrasive papers (80#–1200#), polished with chromium-oxide polishing suspension, and etched with a copper–sulfate–hydrochloric acid reagent. Microstructural observation was performed using an optical microscope.
Vickers microhardness measurements were conducted on an HV-1000TPTA tester (Shanghai High Precision Instrument Co., Ltd., Shanghai, China) with an applied load of 0.2 kgf and a dwell time of 10 s. Indentations were arranged at 1 mm intervals across fusion boundaries and inner deposited zones, with five replicate points for each region. Arithmetic mean values calculated from these replicate indentation points were adopted for hardness analysis.
Uniaxial tensile tests were carried out on a WDW-100 universal testing machine (Jinan Chenda Testing Machine Manufacturing Co., Ltd., Jinan, China) at a constant cross-head speed of 2 mm/min, complying with GB/T 228-2002 [24]. Specimens were machined in both transverse and longitudinal directions relative to the building direction. Three transverse specimens and two longitudinal specimens were tested for each interlayer-temperature condition to ensure data reproducibility, and the average strength values are reported to represent the mechanical performance. Prior to testing, specimen surfaces were cleaned with anhydrous ethanol to remove grease and contaminants.
3. Results and Discussion
3.1. Analysis of Single-Pass Single-Layer Bead
3.1.1. Effect of Wire-Feeding Speed on Weld Surface Forming Quality
A set of single-pass, single-layer bead experiments was conducted at a constant welding speed of 3 mm/s, where the wire-feeding speed varied from 2 m/min to 6 m/min. The measured geometric parameters and surface morphologies of the deposited beads are summarized in Table 3. At a wire-feeding speed of 2 m/min, the deposited bead exhibited moderate forming quality with a distinct serpentine weld track. Its bead width and reinforcement height were 4.44 mm and 4.00 mm, respectively, corresponding to a reinforcement coefficient of 1.11. When the wire-feeding speed increased to 3 m/min, the bead width rose to 6.00 mm, and the reinforcement height reached 4.90 mm. The reinforcement coefficient was 1.22; the overall bead profile was acceptable, but the reinforcement coefficient remained relatively low.
Table 3.
Surface quality of weld beads at a constant welding speed of 3 mm/s with varying wire-feeding speeds.
As the wire-feeding speed increased to 4 m/min, the bead achieved sound forming quality, with a bead width of 6.84 mm and a reinforcement height of 3.80 mm, and the reinforcement coefficient was 1.80. A further increase in the wire-feeding speed to 5 m/min produced the best bead appearance within this experimental group. The bead width and reinforcement height reached 10.42 mm and 4.50 mm, respectively, and the reinforcement coefficient increased to 2.32. The bead morphology was continuous and uniform without obvious forming defects. When the wire-feeding speed was raised to 6 m/min, excessive heat input and surplus filler material generated an overly wide bead with a width of 11.54 mm. Although the reinforcement height slightly increased to 4.60 mm and the reinforcement coefficient reached 2.51, the excessively large bead width impaired the geometric suitability for the subsequent multi-layer thin-wall deposition.
Overall, both the bead width and reinforcement coefficient increased monotonically as the wire-feeding speed increased under a fixed welding speed. A low wire-feeding speed delivered insufficient feedstock and destabilized the molten pool, which induced serpentine weld beads. In contrast, an excessively high wire-feeding speed introduced excessive deposition volume and formed over-wide weld beads, which were unfavorable for the dimensional control of WAAM components. Within the investigated parameter window, the wire-feeding speed of 5 m/min yielded the most desirable bead formation.
3.1.2. Effect of Welding Speed on Weld Surface Forming Quality
Single-pass single-layer deposition experiments were performed at a fixed wire-feeding speed of 5 m/min, while the welding speed varied from 2 mm/s to 6 mm/s. The geometric dimensions and surface morphologies of the resultant weld beads are summarised in Table 4. At the welding speed of 2 mm/s, the molten pool retained heat for a longer duration, which promoted the lateral spreading of liquid metal. The bead width reached 12.90 mm, and the reinforcement height was 4.6 mm, yielding a reinforcement form factor of 2.80. When the welding speed increased to 3 mm/s, the bead width decreased to 10.42 mm, accompanied by a slight drop in the reinforcement form factor to 2.32, while the reinforcement height remained nearly unchanged at 4.5 mm. As the welding speed further rose to 4 mm/s, the bead width decreased continuously to 9.00 mm, and the reinforcement height stayed at 4.5 mm, which produced the minimum reinforcement form factor of 2.00 in this set of tests. A further increase in welding speed to 5 mm/s accelerated the cooling rate of the molten pool. The reinforcement height decreased markedly to 3.2 mm, and the bead width was 8.16 mm; the reinforcement form factor increased to 2.55. At the maximum welding speed of 6 mm/s, the bead width slightly increased to 8.30 mm, and the reinforcement height dropped to 3.1 mm, with the reinforcement form factor reaching 2.68.
Table 4.
Surface quality of weld beads at a constant wire-feeding speed of 5 m/min with varying welding speeds.
Overall, the bead width exhibited a decreasing trend with rising welding speed within the range of 2–5 mm/s. Higher welding speeds shortened the interaction time between the arc and the substrate, which reduced the total heat input per unit length and restrained the lateral spreading of the molten metal. The reinforcement height remained stable at low-to-moderate welding speeds (2–4 mm/s) and declined distinctly once the welding speed exceeded 4 mm/s. Among all tested conditions, the welding speed of 3 mm/s delivered a continuous, uniform bead profile with a reasonable reinforcement form factor, which matched the optimal parameter selected in the previous section.
3.1.3. BP-Neural-Network Prediction of Weld Surface Forming Quality
A back-propagation (BP) neural network model was constructed in MATLAB R2024a to predict the geometric features of single-pass single-layer weld beads, where wire-feeding speed and welding speed were set as input variables, and bead geometric parameters were defined as model outputs. The dataset was randomly partitioned into training, validation, and test subsets. Figure 1 presents the regression correlation plots between the network-predicted outputs and the experimental target values for each subset as well as the overall dataset. The correlation coefficient R reached 0.99993 for the training set, indicating an excellent fitting performance for the training samples. The validation set and test set yielded R values of 0.92438 and 0.98888, respectively. For all data points, the overall correlation coefficient R was 0.98493. Most scattered data points closely clustered around the ideal Y = T reference line, which demonstrated that the established BP neural network captured the inherent nonlinear relationship between process parameters and bead-forming characteristics. Although slight deviations were observed for several individual samples in the validation group, the model still achieved satisfactory prediction accuracy within the investigated processing window. Therefore, this BP network could be adopted to rapidly estimate the bead geometry and assist in the preliminary selection of CMT-WAAM process parameters.
Figure 1.
Regression plots of predicted outputs versus experimental targets of the BP neural network for single-pass single-layer weld bead-forming prediction. The symbol * denotes the multiplication operator in the fitted linear equation.
It is worth noting that back-propagation neural networks are inherently susceptible to overfitting, where the model memorizes noise in training data instead of learning general process rules. Several strategies were implemented in this study to suppress overfitting. First, the whole dataset was randomly split into independent training, validation, and test subsets. The validation set was used to monitor model performance during iteration, and the built-in early-stopping criterion of the Levenberg–Marquardt training algorithm terminated training once validation-set performance stopped improving. Second, a moderate network scale with only 10 hidden neurons was selected, avoiding excessive model capacity. High correlation coefficients obtained on both validation and test subsets, together with the low error from an external physical verification experiment, confirmed that obvious overfitting was absent under the current configuration. Nevertheless, the model exhibits clear parameter-window sensitivity: satisfactory prediction performance is guaranteed only within the experimental range of wire-feeding speed (2–6 m/min) and welding speed (2–6 mm/s). Direct extrapolation to parameters outside this data range is not recommended, as it may trigger unreliable outputs induced by potential overfitting or lack of training data.
The optimal process parameters were obtained using the trained BP neural network, and the verification experiment was carried out under the predicted optimal conditions, as listed in Table 5. The wire-feeding speed and welding speed were set to 3.5 m/min and 4 mm/s, respectively. The BP model predicted a bead width of 5.4789 mm, while the bead width measured in the confirmation experiment was 5.40 mm. The relative prediction error was calculated as 1.46%, which was sufficiently low for WAAM process prediction. The weld bead fabricated under this parameter combination exhibited a smooth and continuous surface without obvious forming defects. This verification result further confirmed the reliability of the established BP neural network, which could accurately predict the geometric dimensions of single-pass weld beads and provide reliable guidance for parameter optimization of the WAAM process.
Table 5.
Surface quality of the weld bead obtained under the optimal parameters predicted by the BP neural network.
3.2. Analysis of Single-Pass Multi-Layer Thin Walls
3.2.1. Effect of Interlayer Temperature on Thin-Wall Forming
Thin-walled components were fabricated by the single-track multi-layer WAAM process with interlayer temperatures controlled at 150 °C and 350 °C, and their forming characteristics were first evaluated by macroscopic observation, followed by subsequent characterizations of microstructure and mechanical properties. As illustrated in Figure 2, the thin wall deposited at an interlayer temperature of 150 °C exhibited fewer spatters and a relatively smooth weld bead surface. In contrast, the sample produced at 350 °C showed slight sagging at both ends of the weld beads and noticeable bead distortion, which indicated inferior forming quality. Since the wire-feeding speed was kept constant, the mass of deposited metal per unit time remained unchanged. The elevated interlayer temperature reduced the heat dissipation capacity of the deposited layer, which increased the surface temperature of the as-deposited wall during the deposition of the subsequent layer. Accordingly, the molten pool retained more heat and possessed a longer solidification time, which promoted the fluidity of molten metal and induced lateral spreading. This phenomenon decreased the average height of each deposited layer and increased the bead width. The overflow of molten metal toward both sides deteriorated the surface flatness of the thin wall and aggravated surface oxidation, resulting in a rough surface morphology. Severe lateral flow even caused blurred layer boundaries and local collapse of the deposited wall.
Figure 2.
Single-pass multi-layer thin-walled parts fabricated at different interlayer temperatures: (a) 150 °C; (b) 350 °C.
3.2.2. Effect of Interlayer Temperature on Microstructure of Single-Pass Multi-Layer Thin Walls
The microstructural evolution of thin-wall deposits under interlayer temperatures of 150 °C and 350 °C was characterized, as shown in Figure 3. For the sample fabricated at an interlayer temperature of 150 °C, a distinct fusion line was observed (Figure 3a). Continuous heat accumulation during layer-by-layer deposition deteriorated the heat dissipation condition, which raised the peak temperature of subsequent deposited layers. Region (a1) exhibited a relatively bright morphology under the same magnification, corresponding to coarse-grained lath martensite with sparse grain boundaries; this region experienced fewer repeated thermal cycles and showed weaker etching resistance. In contrast, region (a2) underwent repeated heating and cooling cycles from successive depositions, and a tempered microstructure was formed accordingly. When the interlayer temperature increased to 350 °C, remarkable differences in microstructure were identified near the fusion zone (Figure 3b). Multiple lath packets with different orientations were generated within a prior austenite grain, and each packet contained one or several sets of martensitic laths. Subjected to prolonged and repeated tempering cycles at higher interlayer temperatures, a small amount of ferrite precipitated as white blocky phases surrounding the lath martensite, accompanied by carbide precipitation along partial ferrite grain boundaries.
Figure 3.
Microstructures of single-pass multi-layer thin walls deposited at different interlayer temperatures: (a) low-magnification overview at an interlayer temperature of 150 °C, (a1) high-magnification micrograph of region (a1) marked in (a), (a2) high-magnification micrograph of region (a2) marked in (a); (b) low-magnification overview at an interlayer temperature of 350 °C, (b1) high-magnification micrograph of region (b1) marked in (b), (b2) high-magnification micrograph of region (b2) marked in (b).
3.2.3. Effect of Interlayer Temperature on Mechanical Properties of Single-Pass Multi-Layer Thin Walls
Figure 4 shows the Vickers hardness distributions in the weld zone and interface zone of WAAM thin walls deposited at interlayer temperatures of 150 °C and 350 °C. The specimens fabricated at 150 °C exhibited higher hardness values than those produced at 350 °C. The hardness of the sample with a 150 °C interlayer temperature ranged from 313 HV to 375 HV, with an average value of 337.13 HV, while the hardness of the sample at 350 °C varied between 309 HV and 359 HV, with an average of 328.34 HV. The elevated interlayer temperature increased cumulative heat input and impaired interlayer heat dissipation, which prolonged the holding time at high temperature and promoted grain coarsening, consequently reducing the hardness [25,26]. For both interlayer temperature conditions, the hardness measured at the fusion interface was consistently lower than that of the weld zone. The region adjacent to the fusion line underwent thermal cycling during deposition, and the distinct heat flux and cooling rate relative to the weld centre induced microstructural evolution such as grain growth and phase transformation, which degraded local hardness. Although the weld centre experienced the maximum heat input and a low temperature gradient with a reduced cooling rate, this cooling condition suppressed the epitaxial coalescent growth of grains during solidification and refined the microstructure in the weld zone, which accounted for the higher hardness of the weld region compared with the interface region.
Figure 4.
Vickers hardness distributions in the weld zone and interface zone of single-track multi-layer thin walls fabricated at different interlayer temperatures.
Figure 5 presents the tensile strength and yield strength of WAAM thin-wall samples tested along the transverse and longitudinal directions relative to the deposition direction under interlayer temperatures of 150 °C and 350 °C. The specimens deposited at 350 °C achieved substantially higher tensile and yield strengths than those fabricated at 150 °C for both sampling orientations. For the transverse direction, the average tensile strength and yield strength of the 350 °C group reached 973.3 MPa and 901.7 MPa, respectively, while the corresponding values for the 150 °C group were only 566.7 MPa and 335.0 MPa. In the longitudinal direction, the 350 °C samples exhibited an average tensile strength of 975.0 MPa and an average yield strength of 940.0 MPa, compared with 550.0 MPa and 322.5 MPa for the 150 °C counterparts. Such strength enhancement at a higher interlayer temperature originated from the repeated thermal cycling during layer-by-layer deposition, which induced a low-temperature tempering effect on the martensitic matrix. The cyclic thermal exposure modulated the substructure of lath martensite and raised dislocation density, contributing to the improved strength. In addition, the tensile properties showed limited anisotropy between the transverse and longitudinal directions at each fixed interlayer temperature [27,28].
Figure 5.
Tensile properties of single-track multi-layer thin walls deposited at different interlayer temperatures: (a) transverse direction; (b) longitudinal direction.
It is noteworthy that an apparent discrepancy is observed: the sample fabricated at 350 °C exhibits slightly lower average Vickers hardness yet distinctly higher yield and tensile strength compared with the 150 °C counterpart. This phenomenon can be rationalised by the different physical natures of hardness measurement and macroscopic tensile testing. Vickers microhardness is a local indentation-based property; the measured average hardness is affected by grain coarsening as well as the softening contribution from fusion-interface regions within the measured field of view. At 350 °C interlayer temperature, cyclic thermal exposure induces moderate grain coarsening, which partly reduces local indentation resistance and accounts for the slight drop in average hardness.
By contrast, uniaxial tensile performance reflects the bulk mechanical response of the whole tensile specimen rather than local micro-zones. Under the cyclic low-temperature tempering effect at 350 °C interlayer temperature, the as-built, brittle, as-quenched lath martensite undergoes sub-structure evolution: dislocation rearrangement, stable dislocation-cell formation, and fine carbide precipitation inside martensite laths strengthen the matrix. Although a small amount of blocky ferrite precipitates and fusion-zone softening still exist, these local soft regions do not dominate the overall bulk tensile behaviour. The strengthening effect induced by cyclic tempering of the martensitic matrix overwhelms the minor softening caused by grain coarsening and local ferrite formation, consequently producing higher yield and tensile strength for the 350 °C sample.
4. Conclusions
In this work, 410NiMo martensitic stainless-steel thin-wall components were fabricated by CMT-WAAM. Single-pass process optimisation, BP-neural-network prediction, and comparative experiments at interlayer temperatures of 150 °C and 350 °C were carried out. The main conclusions are summarised below:
(1) A sound single-pass bead was obtained at a wire-feeding speed of 5 m/min and welding speed of 3 mm/s. The established BP neural network predicted bead geometry with a verification relative error of 1.46%, which can assist rapid parameter selection for CMT-WAAM.
(2) Interlayer temperature strongly affected macro-formability. The 150 °C sample achieved a smoother surface, whereas 350 °C caused severe heat accumulation, prolonged molten-pool lifetime, and deteriorated surface quality due to enhanced lateral liquid-metal spreading.
(3) The as-deposited microstructure was dominated by lath martensite. Higher interlayer temperature (350 °C) promoted precipitation of blocky ferrite and grain-boundary carbides. For both groups, fusion interfaces exhibited lower hardness than inner weld zones; the average Vickers hardness decreased from 337.13 HV (150 °C) to 328.34 HV (350 °C) because of grain coarsening.
(4) Cyclic tempering under a 350 °C interlayer temperature improved tensile and yield strength. The mechanical performance of CMT-WAAM 410NiMo was highly sensitive to interlayer thermal history.
Future research perspectives can be drawn from the present work. First, the cavitation-erosion and corrosion resistance of CMT-WAAM 410NiMo deposits under actual hydraulic-turbine service conditions should be systematically evaluated, since the current study mainly focuses on forming, microstructure, and quasi-static mechanical properties. Second, multi-objective optimisation combining machine-learning prediction with experimental validation can be developed to simultaneously balance surface formability, microstructural homogeneity and mechanical performance under varied interlayer thermal histories. Third, further quantitative characterization, including precipitate evolution, residual stress distribution, and crystallographic texture, is required to gain deeper insight into microstructure–property relationships. Finally, practical repair trials on real damaged hydraulic turbine components are necessary to promote the engineering application of the CMT-WAAM repair technique.
Author Contributions
Conceptualization, X.L., Z.L., X.C. and S.Z.; methodology, Y.Z., J.D. and J.Z. (Jiansheng Zhang); formal analysis, J.D., Z.L., X.L. and Y.Z.; resources, X.C., S.Z. and J.Z. (Jie Zhou); writing—original draft preparation, X.L., Z.L., and J.Z. (Jiansheng Zhang); writing—review and editing, Y.Z., J.D., X.C., S.Z. and J.Z. (Jie Zhou). All authors have read and agreed to the published version of the manuscript.
Funding
This research was supported by the National Natural Science Foundation of China (No. 52475323), the New Chongqing Young Innovative Talents Project (No. CSTB2025YITP-QCRCX0033) and Research Projects for High-Level Talents of Sichuan Polytechnic University (No. XJ2026HT-01, XJ2026HT-07).
Data Availability Statement
The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding authors.
Conflicts of Interest
Authors Zuofa Liu and Jiansheng Zhang were employed by Chongqing Jiepin Technology Co., Ltd. while contributing to this manuscript. Their contributions to this work and manuscript were made independently without any requirement, guidance or input from their employer. They received no financial compensation from any source for the contributions they made to the scientific work and manuscript. The remaining authors declare no conflicts of interest.
References
- Ali, M.; Ullah, W.; Hussain, J.; Kalidasan, B.; Rajamony, R.K.; Mirza, S.; Singh, K.; Hussain, I. Additive manufacturing: A multidisciplinary review of techniques and applications. Resour. Chem. Mater. 2026, 100216, in press. [Google Scholar] [CrossRef] [Scilit]
- Das, B.; Sahoo, N.; Patel, P.; Ghosh, A.; Khan, M.A.; Bhushan, B.; Madan, R.; Shrivastava, P.; Msomi, V. Wire Arc Additive Manufacturing (WAAM): A comprehensive review of process, materials, modelling, artificial intelligence, and industrial applications. J. Alloys Compd. 2026, 1058, 186347. [Google Scholar] [CrossRef] [Scilit]
- Fattah, R.N.; Kusharjanta, B.; Akbar, H.I.; Triyono. A comprehensive review of materials and process parameters in Wire Arc Additive Manufacturing (WAAM): Current insights and future directions. Next Mater. 2026, 13, 103676. [Google Scholar] [CrossRef] [Scilit]
- Goka, S.; Manjaiah, M.; Davidson, M.J.; Moinuddin, S.Q. Review: State-of-art for wire arc additive manufacturing of metallic alloys—Insights into materials, methods, and future prospects. J. Mater. Sci. 2026, 61, 23409–23439. [Google Scholar] [CrossRef] [Scilit]
- He, F.; Yuan, L.; Yang, J.; Zhou, W.; Zhang, Y.; Pan, Z.; Li, H. Process innovations in wire arc additive manufacturing systems: Progress, challenges and future opportunities. Prog. Mater. Sci. 2027, 163, 101776. [Google Scholar] [CrossRef] [Scilit]
- Pant, H.; Arora, A.; Gopakumar, G.S.; Chadha, U.; Saeidi, A.; Patterson, A.E. Applications of wire arc additive manufacturing (WAAM) for aerospace component manufacturing. Int. J. Adv. Manuf. Technol. 2023, 127, 4995–5011. [Google Scholar] [CrossRef] [Scilit]
- Ain, M.Q.U.; Naik, D.K.; Rajendran, D.K.; Sekar, S. Comprehensive analysis of experimental studies in cold metal transfer welding. Discov. Appl. Sci. 2025, 7, 590. [Google Scholar] [CrossRef] [Scilit]
- Selvi, S.; Vishvaksenan, A.; Rajasekar, E. Cold metal transfer (CMT) technology—An overview. Def. Technol. 2018, 14, 28–44. [Google Scholar] [CrossRef] [Scilit]
- Abdian, K.; Eslami, A.; Ashrafizadeh, F.; Fadaeifard, F.; Hadizadeh, B. Effect of Heat Treatment on Microstructure, Mechanical Properties, and Corrosion Performance of 410NiMo Super Martensitic Stainless Steel Cladded on 21CrMoV5-11 by Submerged Arc Welding Process. Arab. J. Sci. Eng. 2024, 49, 1433–1446. [Google Scholar] [CrossRef] [Scilit]
- Constantineau, C.; Deschênes, P.A.; Dubois, R.; Brochu, M. Fatigue strength prediction of 410NiMo stainless steel with surrogate weld discontinuities. Int. J. Fatigue 2025, 197, 108955. [Google Scholar] [CrossRef] [Scilit]
- L’Hostis, J.; Thuinet, L.; Cadel, E.; Avettand-Fènoël, M.-N. Multiscale characterization of WAAMed martensitic stainless steel: Correlation between experimental AM thermal cycles, microstructural evolution and mechanical properties. Acta Mater. 2025, 291, 120972. [Google Scholar] [CrossRef] [Scilit]
- Mabruri, E.; Prifiharni, S.; Anwar, M.S.; Romijarso, T.B.; Adjiantoro, B. Mechanical properties optimization of the modified 410 martensitic stainless steel by heat treatment process. Mater. Today Proc. 2018, 5, 14918–14922. [Google Scholar] [CrossRef] [Scilit]
- Tenni, B.; Godin, S.; Thibault, D.; Brochu, M. Shielding Gas and Inclusion Content Effects on Impact Toughness and Tensile Properties of 410NiMo Steel Welds. Weld. J. 2021, 100, 52S–62S. [Google Scholar] [CrossRef] [Scilit]
- Li, M.; Zhang, W.; Zhou, Z.; Liang, J.; Sun, X.; Wang, W.; Mo, H.; Shang, X.; Chen, S.; Long, Y.; et al. Effect of the interlayer temperature on microstructure and mechanical behavior of the high-strength low-alloy steel manufactured by the wire arc additive manufacturing. Mater. Today Commun. 2025, 46, 112845. [Google Scholar] [CrossRef] [Scilit]
- Yang, S.; Yang, D.; Chang, G.; Su, Z.; Wang, L.; Huang, Y.; Li, X. Effect of interlayer temperature on the microstructure and mechanical properties of ultra-high-strength steel fabricated by ultrasonic impact-assisted wire arc additive manufacturing. Ultrasonics 2027, 169, 108286. [Google Scholar] [CrossRef] [Scilit]
- Teixeira, F.R.; Scotti, F.M.; Jorge, V.L.; Scotti, A. Combined effect of the interlayer temperature with travel speed on features of thin wall WAAM under two cooling approaches. Int. J. Adv. Manuf. Technol. 2023, 126, 273–289. [Google Scholar] [CrossRef] [Scilit]
- Gil Plazas, A.F.; Amaya Villabon, T.A.; Ramirez Vargas, D.A.; Rubiano Buitrago, J.D.; Herrera Quintero, L.K. Influence of interlayer thermal cycling on microstructural evolution in WAAM processed carbon steel. Weld. World 2026, 70, 471–489. [Google Scholar] [CrossRef] [Scilit]
- Li, C.; Suen, H.; Yang, Y.; Zhang, L.; Chen, Q.; Gao, T.; Yuan, B.; Cheng, L.; Lv, Z. Effect of Interlayer Temperature-Controlled Thermal Cycling on the Microstructure and Mechanical Properties of Wire Arc Directed Energy Deposition H13 Steel. Materials 2025, 19, 111, Correction in Materials 2026, 19, 2300. https://doi.org/10.3390/ma19112300. [Google Scholar] [CrossRef] [Scilit]
- Omiyale, B.O.; Ogedengbe, I.I.; Ogbeyemi, A.; Akinfolarin, J.F.; Adewole, K.A.; Zhang, W.C. Defects in Wire Arc Additive Manufacturing of Stainless Steel: A Brief Critical Review. Lasers Manuf. Mater. Process. 2025, 12, 1061–1105. [Google Scholar] [CrossRef] [Scilit]
- Yu, S.-P.; Tong, P.-G. Improving ultrasonic inspection reliability of as-built WAAM components with rough surfaces using solid composite couplants. Int. J. Adv. Manuf. Technol. 2026, 144, 1319–1329. [Google Scholar] [CrossRef] [Scilit]
- Jha, A.; Ramji, M.; Gopinath, M. Influence of substrate condition and thermal history on the microstructural evolution and mechanical performance of hybrid Inconel 718 repairs by laser directed energy deposition. J. Mater. Process. Technol. 2026, 355, 119444. [Google Scholar] [CrossRef] [Scilit]
- Martin, J.; Nominé, A.V.; Stef, J.; Nominé, A.; Zou, J.X.; Henrion, G.; Grosdidier, T. The influence of metallurgical state of substrate on the efficiency of plasma electrolytic oxidation (PEO) process on magnesium alloy. Mater. Des. 2019, 178, 107859. [Google Scholar] [CrossRef] [Scilit]
- Lakkannavar, V.; Yogesha, K.B.; Prasad, C.D.; Phanden, R.K.; G, S.; Prasad, S.C. Thermal spray coatings on high-temperature oxidation and corrosion applications—A comprehensive review. Results Surf. Interfaces 2024, 16, 100250. [Google Scholar] [CrossRef] [Scilit]
- GB/T 228-2002; Metallic Materials—Tensile Testing at Ambient Temperature. Standards Press of China: Beijing, China, 2002. (In Chinese)
- Wang, L.; Jiang, Y.; Hu, C.; Wan, X.; Li, G. Effect of heat input on microstructure evolution and fracture toughness of interlayer heat affected zone in ultra-high strength steel. J. Mater. Res. Technol. 2025, 39, 5189–5198. [Google Scholar] [CrossRef] [Scilit]
- He, B.; Wang, Y.; Wang, C.; Ren, Y.; Yang, G. Effect of gradient decrease heat-input combined with inter-layer cooling on microstructure and mechanical properties of WAAM-Ti-6Al-2Zr-1Mo-1V alloy. Mater. Today Commun. 2024, 39, 108628. [Google Scholar] [CrossRef] [Scilit]
- Gao, P.; Fan, J.; Cai, B.; Zhang, J.; Yang, D.; Peng, Y.; Wang, K. Effect of interlayer temperature on the microstructure and mechanical properties of new Co-Free maraging steel fabricated by arc-based directed energy deposition. Mater. Charact. 2025, 222, 114851. [Google Scholar] [CrossRef] [Scilit]
- Hu, M.; Chi, Q.; Ji, L.; Li, W.; Yan, S.; Cheng, F. Effect of Interlayer Temperature on Microstructure and Properties of High-Strength Low-Alloy Steel Manufactured Using Submerged-Arc Additive Manufacturing (SAAM). Materials 2024, 17, 5376. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.