Highlights
What are the main findings?
- HF etching effectively removed partially fused powder from Ti6Al4V lattices.
- Plasma etching further refined surface quality with minimal material loss.
- DLC coatings resulted in more positive OCP values and enhanced osteoblast colonization.
What are the implications of the main findings?
- Multi-stage treatment improves LPBF Ti6Al4V lattice surface performance.
- Optimized processing preserves lattice integrity and mechanical properties.
- The approach supports advanced additively manufactured biomedical implants.
Abstract
Additively manufactured Ti6Al4V lattice structures are promising for biomedical applications, but partially melted powder particles and surface defects from Direct Metal Laser Sintering may adversely affect their properties. This study evaluated a three-stage post-processing strategy comprising wet chemical etching (in aqueous acid solution), plasma etching and diamond-like carbon (DLC) coating deposition. Hydrofluoric acid (HF) concentration and etching time were evaluated for powder removal, mass loss and mechanical properties, followed by assessment of surface and biological properties. The most favorable HF treatment was 1.4% HF for 7 min, effectively removing powder particles but causing 14.53% mass loss and a 14.69% reduction in load-bearing capacity at 0.2% strain. Plasma etching resulted in less than 0.2% mass loss and, when applied after chemical etching, removed surface defects and reduced roughness without changes in lattice geometry. DLC coatings exhibited an amorphous carbon structure with an ID/IG ratio of 1.18 ± 0.01. The highest open-circuit potential was obtained for DLC-coated samples (56 ± 34 mV), exceeding that of unmodified samples (22 ± 63 mV). All variants were non-cytotoxic according to ISO10993-5, while the highest surface colonization by Saos-2 cells was observed after deposition of a DLC coating through a comparative analysis of their growth on the solid region of 3D-printed samples. Overall, the sequential treatment enabled the functional properties of Ti6Al4V lattice structures to be tailored beyond the scope of conventional surface cleaning.
1. Introduction
Rapid advances in additive manufacturing technologies are expanding the possibilities for designing and manufacturing medical implants with complex geometries tailored to individual patient needs [1]. A particularly important group consists of lattice implants made from titanium alloys, which, thanks to their high biocompatibility, favorable mechanical properties and the ability to control porosity, promote osseointegration and provide suitable conditions for bone tissue regeneration [2,3]. Technologies such as Direct Metal Laser Sintering (DMLS) enable the production of lattice structures with complex three-dimensional architecture, which are difficult to achieve using conventional manufacturing methods [4].
Despite the numerous advantages of additive manufacturing techniques, the manufacturing process leads to the formation of characteristic surface imperfections [5]. The surfaces of printed components retain particles of unsintered or partially melted powder, material spatter and irregularities resulting from the layered nature of the process. In the case of medical implants, the presence of such impurities may adversely affect mechanical properties [6,7], corrosion resistance [8,9], safety during clinical use, and implant-tissue integration [10]. For this reason, a properly designed post-processing procedure is one of the key stages in the manufacture of implants using additive manufacturing methods, determining their surface, mechanical and biological properties [11,12].
Despite their generally high corrosion resistance, titanium alloys may still undergo degradation under physiological conditions. Local damage to the passive oxide layer, particularly in the presence of chloride ions, can promote localized electrochemical activity and accelerate material deterioration. Furthermore, Ti6Al4V components manufactured by additive processes often contain partially melted powder particles, surface irregularities, and process-induced defects, which may affect local electrochemical conditions and passivation behavior. In biomedical applications, where implants are subjected to mechanical loading, degradation may also result from tribocorrosion, i.e., the combined action of mechanical wear and electrochemical processes. Therefore, surface modification strategies aimed at reducing surface defects, improving surface homogeneity, and enhancing barrier properties may contribute to improved performance of Ti6Al4V implants [13,14,15].
Consequently, understanding and controlling surface degradation mechanisms is particularly important for additively manufactured lattice structures, whose high specific surface area and complex geometry may further influence interactions with the physiological environment.
A particular challenge is removing loosely attached particles from lattice structures, whose complex geometry significantly limits the effectiveness of conventional mechanical methods. Internal channels and porous areas are often inaccessible to grinding, polishing or abrasive blasting [16,17,18]. Consequently, there is growing interest in chemical and physicochemical methods, which allow for uniform treatment of the entire surface of the component, regardless of its complexity.
One of the most commonly used methods is chemical etching, which allows for the effective removal of powder particles and processing residues even from hard-to-reach internal spaces [1,19]. Depending on the process parameters, chemical etching can remove powder residues and modify surface roughness and topography, while also preparing the surface for subsequent treatment stages. This method is characterized by relatively simple technological implementation, but it also entails certain limitations. Etching leads to the partial removal of material, which may cause dimensional changes and affect the mechanical properties of thin-walled lattice structures. Furthermore, it requires the use of aggressive chemical reagents and the implementation of appropriate neutralization and waste disposal procedures.
Alternatives to chemical etching include electrochemical [19], ultrasonic, laser [20] and plasma [21,22] methods. Plasma treatment is a promising approach for surface finishing and modification, with limited effects on the overall geometry of the structure. However, plasma treatment alone may not provide sufficient removal of strongly adhered metallic powder particles and may therefore be more effective when used as a complementary treatment following chemical etching. Furthermore, plasma treatment can increase surface free energy and improve wettability, potentially promoting a more favorable cellular response.
Increasing attention is being paid to multi-stage post-processing strategies, which involve the sequential combination of various surface treatment methods [16,23]. Combining different techniques may produce synergistic effects, improving surface cleanliness and functional properties. Although multi-stage processes involve higher costs due to the need for additional manufacturing operations and enhanced quality control, in the case of medical implants, they are often justified by stringent requirements regarding product safety and quality.
This study evaluated a multi-stage surface engineering strategy for Ti6Al4V lattice structures comprising wet chemical etching, plasma etching and diamond-like carbon (DLC) coating deposition. This sequential approach was intended not only to remove residual powder particles but also to modify surface topography and electrochemical behavior and to improve the biological response of the structures.
Although chemical etching, plasma treatment, and DLC coating have each been individually investigated as surface modification methods for additively manufactured Ti6Al4V components, the effects of their sequential application to porous lattice structures remain insufficiently understood. Previous studies have primarily focused on the ability of individual treatments to remove partially melted powder particles, modify surface topography, or improve selected functional properties. However, the relationships between consecutive processing steps and their combined influence on the geometry, mechanical integrity, corrosion behavior, and biological performance of lattice structures have not been systematically examined. Therefore, the aim of the present study was not only to evaluate individual surface modification methods, but also to determine how successive treatment stages contribute to the final properties of the material. The scientific novelty of this work lies in identifying the complementary effects of chemical etching, plasma treatment, and DLC deposition and in establishing a multi-stage surface engineering approach for controlling the performance of additively manufactured Ti6Al4V lattice structures intended for biomedical applications.
The effectiveness of the proposed procedure was verified on the basis of observations of the surface topography using scanning electron microscopy (SEM), mass loss tests and an assessment of the effect of the treatment on the mechanical properties of the modified structures. Corrosion-related electrochemical behavior was assessed by measuring the open-circuit potential (OCP), while cytotoxicity was evaluated using an MTT assay and the cellular response was assessed by direct culture of Saos-2 osteoblast-like cells. The results provide insight into the effects of individual treatment stages and their combination on the surface and functional properties of Ti6Al4V lattice structures.
2. Materials and Methods
2.1. Preparation of Test Samples
The specimens were fabricated from Ti6Al4V alloy using the Direct Metal Laser Sintering (DMLS) method [24]. The starting material was commercial Ti6Al4V Grade 23 powder (LaserForm Ti Gr. 23 Type A, 3D Systems GmbH, Mörfelden-Walldorf, Germany) with particle sizes ranging from 10 to 50 µm.
Two types of specimens were prepared. Both types. were manufactured using a ProX 320A system (3D Systems, Rock Hill, SC, USA), equipped with a build platform measuring 275 × 275 mm. The main manufacturing parameters included a laser power of 500 W and a mean layer thickness of 60 µm. The declared printing accuracy was ±0.2%.
Cube-shaped specimens measuring 10 × 10 × 10 mm were used for most experiments. The specimens featured a stochastic lattice structure composed of elementary cells, as shown in Figure 1. The nominal diameter of the lattice struts (Dc) was 0.3 mm, while the nominal diameter of the structural nodes (Dn) was also 0.3 mm. The mean initial mass of these specimens was 2.590 g, with a standard deviation of 0.022 g.
Figure 1.
Geometry of the elementary cell of the stochastic lattice structure used during sample preparation using DMLS technology: (a) dimensioned geometric model of the structure (X, Y, Z = 0.8 mm, Dn = 0.3 mm, Dc = 0.3 mm), (b) SEM view of the actual structure after printing.
For surface roughness measurements, OCP and biological testing, similarly manufactured disc-shaped specimens with a diameter of 16 mm and a height of 5 mm were used. The outer rim and the bottom layer of these samples were solid, whilst the centrally located lattice region had a diameter of 10 mm and a height of 3 mm. The mean initial mass of this specimen type was 3.839 g, with a standard deviation of 0.070 g. The actual geometry of the fabricated samples is shown in Figure 2 as a reconstruction obtained using micro-CT.
Figure 2.
Micro-CT images of the tested samples: general view (a,c); cross-section (b,d).
After the printing process was completed, and before the samples were cut from the build plate, they underwent heat treatment to reduce the residual stresses generated during printing. The process was carried out in a vacuum furnace at a pressure of 5 × 10−5 mbar and a temperature of 920 ± 15 °C for 2 h.
When removing the supports, the bottom surface of each sample was marked, which enabled a consistent orientation to be maintained throughout all stages of the investigation, in accordance with the direction of material deposition during the printing process.
2.2. Modification Methods Used
The 3D-printed samples underwent post-processing to remove titanium powder residues remaining on their surfaces after manufacturing. An additional objective was to modify the surface in a manner that could improve the biological response, which was subsequently evaluated using osteoblast-like cells. The proposed multi-stage surface engineering strategy comprised three consecutive stages. In the first stage, chemical (wet) etching was carried out in a hydrofluoric acid (HF) solution, with the aim of initially removing loosely adhered powder particles whilst minimizing material loss. The second stage involved plasma etching, which was used to further remove residual surface contaminants and modify the surface microtopography, particularly following chemical etching. In the third stage, a DLC coating was deposited to modify the surface functional properties and provide an additional protective surface layer. In addition to the full, three-stage modification process, single- and two-stage variants were also carried out. These were used to assess the impact of individual treatment stages and to compare them with one another. However, the experimental design focused primarily on evaluating a predetermined, multi-stage surface treatment sequence. Consequently, this study did not consider all alternative process combinations—such as the direct deposition of DLC coatings onto samples that had undergone chemical or plasma etching. Figure 3 illustrates the sequence of surface treatment stages and the corresponding specimen group designations.
Figure 3.
Diagram of the individual modification processes, together with the designation system: S-0—unmodified sample after printing, S-CH—sample chemically etched in HF acid, S-P—plasma-etched sample, S-CH/P—sample etched in HF acid and by plasma, S-CH/P/DLC—sample modified in three stages in the following sequence: etching in HF acid–plasma etching–DLC layer synthesis.
2.2.1. Stage I—Wet Chemical Etching
Wet chemical etching was carried out in 70 mL of an aqueous solution of hydrofluoric acid (HF), prepared each time immediately prior to the modification process from a 40% stock solution (Chempur, Piekary Śląskie, Poland). Based on the results of our own research [25] and reports in the literature [26,27,28,29], three concentrations of the etching solution were selected: 1.0%, 1.4% and 2.0%. The etching process was carried out by agitating the solution using an ultrasonic cleaner (POLSONIC Soni2, Warsaw, Poland) operating at a frequency of 40 kHz at room temperature. The effectiveness of the chemical etching process for each solution concentration was assessed over a time period ranging from 3 to 30 min.
After etching, the samples were thoroughly rinsed in deionized water to remove any residual hydrofluoric acid from the surface and internal regions of the lattice structure. The samples were then washed with 99.8% methanol (POCH, Gliwice, Poland) and dried with a stream of compressed air.
2.2.2. Stage II—Plasma Etching
Plasma etching was carried out using the RF PACVD (radio frequency plasma-activated chemical vapor deposition) method. In this method, the samples are placed on a negatively polarized high-frequency electrode. During plasma etching, the RF generator output power and the negative self-polarization potential obtained at the electrode were controlled. The parameters of this process were determined on the basis of the authors’ previous experiments [30]. The etching process was carried out in argon at a pressure of 10–12 Pa and a gas flow rate of 4 sccm. The negative polarization potential of the electrode was −1700 V at a generator power of 1000 W. The process lasted 2 h. During the process, the temperature of the modified surfaces was measured using a pyrometer (Optris CT, TEST-THERM, Krakow, Poland). The temperature of the samples stabilized at 490 ± 5 °C.
2.2.3. Stage III—DLC Deposition
The RF PACVD method was also used in the third stage of modification to deposit DLC coatings. Methane (CH4) was used as a precursor gas during deposition. The pressure in the reactor chamber was 50 Pa, and the methane flow rate was maintained at a constant level of 60 sccm. The process was carried out at a negative electrode polarization potential of −1300 V and a generator power of 1800 W. The process duration was 3 min, starting from the moment the parameters stabilized. The temperature of the samples during the synthesis process was 500 ± 5 °C. Before DLC deposition, the specimens were subjected to ion etching. The deposition process was then initiated without interrupting the plasma discharge by gradually adjusting the process parameters.
2.3. Measurement of Sample Mass
Samples, both before and after post-processing, were washed, degreased and weighed, regardless of the modification procedure used. To this end, the samples were washed in an ultrasonic cleaner (POLSONIC Soni2, Warsaw, Poland) successively in deionized water and isopropyl alcohol, with each bath lasting 10 min. After completion of each stage, the samples were dried with a stream of compressed air.
The mass of the samples was determined using a moisture balance (RADWAG MA.60.3Y.WH, Radom, Poland). The samples were dried at 80 °C for 10 min, which ensured the removal of residual moisture and the attainment of a stable mass reading. The results of mass loss for individual modification processes (presented in Figure 3) were determined based on five independent series of samples. Evaluation of mass loss dynamics was conducted on a single series of samples.
2.4. Measurement of Mechanical Properties
Measurements of mechanical properties were carried out using an LFV −50 kN servo-hydraulic axial testing system (Walter + Bai AG, Löhningen, Switzerland). Compression tests were performed with the specimens maintained in the same spatial orientation as during the DMLS manufacturing process. The crosshead displacement rate was maintained at 1 mm/s. Deformation was determined on the basis of the displacement of the compression test head in accordance with the relationship Δh/h0. Due to the varying cross-sectional area of the specimens, resulting from their lattice geometry and progressive deformation during compression, stresses were not determined. To compare the mechanical properties, the structural behavior was analyzed: the force versus displacement curve generated by the testing system, which was subsequently converted into a force versus strain curve, and the conventional load-bearing capacity of the structure corresponding to a relative strain of 0.2% (F0.2), determined using the offset method.
To limit the influence of the selected quasi-linear region on the conventional load determined using the offset method, a sensitivity analysis of the calculation procedure was performed for each type of specimen. The influence of the starting point used for regression-based stiffness identification was evaluated in order to minimize the effects of initial specimen seating and clearance elimination during the early stage of compression testing. In addition, a moving linear regression window was employed to reduce the influence of local measurement fluctuations on the calculated apparent stiffness. For all analyzed cases, the highest stability of the obtained results was achieved using a regression window comprising 20 consecutive data points. Under these assumptions, a coefficient of determination of R2 ≥ 0.999 was obtained, while the maximum variation in the calculated conventional offset load did not exceed 5% relative to the minimum value.
The mechanical measurements were performed on three independent series of samples.
2.5. SEM Research
SEM analysis was used to visualize and evaluate the topography of the tested samples. For observations in SEI (secondary electron image) mode, an SM-6610LV scanning electron microscope (JEOL, Akishima, Japan) equipped with an X-Max 80 energy-dispersive X-ray spectrometer (EDS) (Oxford Instruments, Abingdon, UK) was used. SEM investigations were carried out in high vacuum using electron beam acceleration voltages of 20–30 kV. The conducted examination was based on three independent series of samples.
2.6. Micro-CT Research
Analysis of the internal structure and porosity of the samples was carried out using a high-resolution X-ray micro-computed tomography system, the SkyScan 1272 from Bruker (Kontich, Belgium). The scanning conditions are presented in Table 1. To determine the total porosity, the distribution of strut diameters and the pore distribution in the porous structures, three-dimensional reconstructions were carried out using the following software: NRecon 1.7.4.2, CTAn 1.17.7.2+ and Data Viewer 1.5.6.2 (Bruker, Kontich, Belgium). For each sample examined, the region of interest (ROI) encompassed the entire volume of the sample, ensuring that the comparison was based on the identical—and maximum possible—amount of material. This methodology precluded the possibility that differences in the tomographic results—arising from the comparison of different parts of a sample—could be misattributed to structural changes caused by physical or chemical processing.
Table 1.
High-resolution scanning conditions for the tested samples.
2.7. Raman Spectroscopy
Raman spectroscopy experiments were carried out using a Renishaw inVia spectrometer with a laser wavelength of 532 nm and a 50× objective lens. To determine the chemical structure of the DLC coatings produced, the experiments were conducted in the Raman shift range from approximately 900 to 2000 cm−1. The spectra obtained were analyzed using the 4-peak model described in the literature [31,32] with PEAKFIT 4.12 software. Raman measurements were performed at accessible locations distributed across different regions of the lattice structures on three independent samples, each processed in a separate plasma treatment run.
2.8. Surface Roughness
The surface roughness of the samples was examined using a Hommel Tester T1000Wave (Jenoptik Industrial Metrology Germany GmbH, Villingen-Schwenningen, Germany) contact profilometer fitted with a TKL 300L diamond measuring head with a radius of curvature of 5 µm and an angle of 90°. Due to the lattice nature of the samples, roughness measurements were carried out on the solid, disc-shaped sections of the samples. The results were compiled on the basis of measurements from 5 samples.
2.9. Corrosion-Related Electrochemical Behaviour
Corrosion-related electrochemical behavior was evaluated using an AUTOLAB PGSTAT 302N potentiostat (Metrohm Autolab B.V., Utrecht, The Netherlands) in a three-electrode configuration. The test specimen served as the working electrode, a saturated calomel electrode as the reference electrode, and a platinum electrode as the counter electrode. The tests were carried out in a 0.9% NaCl solution at a temperature of 37 °C; the solution was deoxygenated using argon with the aim of minimizing its influence on the electrochemical response of the samples under study. The OCP was monitored for 120 min to allow the potential to stabilize. The results were compiled on the basis of measurements from five samples.
The actual electrochemically active surface area of the investigated specimens was not determined. Due to the complex architecture of the lattice structures, the true surface area exposed to the electrolyte may differ substantially from the nominal geometric area derived from the CAD model. Furthermore, both the DMLS process and subsequent surface modification treatments, particularly chemical etching, alter the surface morphology and roughness, affecting the relationship between nominal and electrochemically active surface area. Therefore, the OCP measurements should be interpreted primarily as a comparative assessment of the relative electrochemical behavior of the investigated surface conditions rather than as a quantitative evaluation of corrosion kinetics. It should also be noted that OCP measurements provide information about the electrochemical state of the surface but do not directly determine corrosion rate or corrosion resistance.
2.10. Cytotoxicity Testing Using the MTT Assay
Prior to analysis, the samples were washed using an ultrasonic cleaner in deionized water for 20 min at 30 °C, and were then sterilized in an autoclave at 121 °C for 15 min. The samples were analyzed by extraction from 3 independent samples (n = 3), and 6 technical replicates were performed for each extract (n = 6). To prepare the extract, the samples were weighed and the medium was added at a sample-to-medium ratio of 0.2 g/mL (in accordance with standard PN-EN ISO 10993-12 [33]: Biological evaluation of medical devices—Part 12: Sample preparation and reference materials.). The extraction medium was Dulbecco’s Modified Eagle’s Medium (DMEM) High Glucose with L-Glutamine and Sodium Pyruvate (Capricorn Scientific, Ebsdorfergrund, Germany) supplemented with 10% Bovine Calf Serum (BCS) (Biowest, Nuaillé, France). The cytotoxicity assay was conducted on the NIH/3T3 mouse fibroblast line (ATCC CRL-1658, Manassas, VA, USA) at passage 6, which was cultured in complete medium (the same as extraction one with the addition of 1% penicillin–streptomycin–neomycin (P/S/N) (Sigma Aldrich, St. Louis, MO, USA)) for 24 h at 37 °C in a 5% CO2 atmosphere. The cells were seeded at the standard concentration of 1 × 105 cells/mL. After 24 h of cell exposure to the undiluted extracts, MTT dye (10 µL per well) was added; then, after a further 4 h, 200 µL of DMSO per well was added, and absorbance was measured at wavelengths of 570 and 660 nm using a Victor plate reader (PerkinElmer, Shelton, CT, USA). Cell viability was calculated relative to the negative control (in accordance with the equation provided below), which consisted of cells grown for the same duration and under the same conditions without exposure to any extract–cultured under standard conditions.
where A means absorbance.
The mean and standard deviation were calculated from 18 measurements (6 technical replicates for each of the 3 biological replicates).
2.11. Assessment of the Proliferative Capacity of Saos-2 Osteoblast-like Cells
The biological response to the post-processing strategies was evaluated using a direct cell-contact assay. Saos-2 osteoblast-like cells (Human Osteosarcoma Cell Line (ATCC HTB-85), Manassas, VA, USA) were cultured directly on the surfaces obtained after each of the applied post-processing procedures (S-CH, S-P, S-CH/P, S-CH/P/DLC). For the direct-contact cellular response studies, samples with a specific geometry were used–lattice in the central part of the sample and flat at the edges (Figure 2c,d). Cells were seeded in the central part by pipetting the cell suspension directly onto the lattice area. When replenishing the samples with culture medium, the medium was also added to the central part. As a result, the seeded cells were distributed across the entire surface of the sample. SEM observations of the lattice section allowed us to assess the presence and proliferative capacity of the cells; however, as this type of geometry does not provide a suitable basis for comparative observations, these were carried out on images taken at the periphery of the samples, on their solid sections.
Before seeding the cells, the samples were sterilized in an autoclave at 121 °C for 15 min. For each sample type and time point, three samples were prepared by random selection. Saos-2 cells were cultured in a dedicated culture medium (McCoy’s 5A Medium, Sigma Aldrich, St. Louis, MO, USA) supplemented with 15% FBS (Fetal Bovine Serum, Sigma Aldrich, St. Louis, MO, USA) and 1% Penicillin–Streptomycin–Neomycin (P/S/N) antibiotics (Sigma Aldrich, St. Louis, MO, USA) at 37 °C in a 5% CO2 atmosphere. The cells were seeded at a concentration of 1 × 105 cells/mL by first placing a 500 µL drop onto the surface of the test sample. After 2 min of incubation at room temperature, medium was added until the sample was fully submerged. The cells in contact with the surfaces being treated were cultured for 48 h and 96 h. The culture medium was replaced every 48 h. After the specified culture times, the samples were fixed in 2.5% glutaraldehyde (24 h at 4 °C), dehydrated and then dried in a critical-point freeze-dryer. The samples prepared in this way were coated with carbon (8 nm thick) and examined using a scanning electron microscope (three samples after each modification type for each time point). Based on the SEM images, comparisons were made of the degree of cell proliferation depending on the substrate on which they were grown.
3. Results
3.1. Stage One—Wet Chemical Etching
Wet chemical etching is the first stage in a multi-stage surface engineering of 3D-printed structures. In the present study, various concentrations of HF acid in deionized water were used, starting with the 2% concentration most frequently reported in the literature [26,27,28,29]. Due to the toxicity of HF and its negative impact on the environment, it was decided to reduce its concentration and investigate how this would affect the dynamics of the etching process; hence the selection of concentrations of 1.4% and 1%. At this stage of the research, the following were analyzed: mass loss, the effectiveness of removing loosely bound powder residues from the print (SEM imaging), and the decline in mechanical properties accompanying the etching processes.
3.1.1. Measurement of Mass Loss Following the Wet Chemical Etching Process
The experimental results for all concentrations tested are shown in Figure 4. As the etching time increased, a systematic decrease in mass was observed for all analyzed concentrations of hydrofluoric acid. For all tested variants, the greatest rate of mass loss was recorded in the initial stage of the process (up to approximately 6–9 min). Later in the process, the rate of mass loss gradually decreased, as indicated by the decreasing slope of the analyzed curves. The differences in mass loss between the HF concentrations increased with the duration of the process. After 3 min, the difference between the 1% and 2% solutions was approximately 7 percentage points, whilst after 30 min it had increased to over 20 percentage points. This indicates that the effect of acid concentration on the intensity of the etching process becomes increasingly pronounced as the treatment time increases. After 30 min of etching, the mass loss for the 1% solution was approximately 19%, whilst for the 1.4% and 2% solutions it reached approximately 33% and nearly 40%, respectively.
Figure 4.
Mass loss dynamics of samples during 3–30 min of wet chemical etching in 1%, 1.4% and 2% HF solutions.
3.1.2. SEM Analysis of Samples Following the Wet Chemical Etching Process
Analysis of SEM images of samples at specific time points during the wet chemical etching process made it possible to determine the effectiveness of this process for different concentrations of HF acid. This result is shown in Figure 5. In the case of 2% solutions, a satisfactory removal of loosely bound particles was achieved at around 6 min. The surface is almost entirely free of undesirable contaminants, whilst maintaining structural continuity. However, in a 2% acid solution, the process proceeds very rapidly, and any further extension of the time resulted in significant changes to the geometry of the specimen. After 9 min, the sample was already clearly etched. The cross-sectional area of the struts was significantly reduced, and some structural elements lost their continuity. In the 1.4% solution, the process was more controllable. The complete removal of loosely bound powder particles occurred between 6 and 9 min of etching, whilst maintaining the structural integrity. For the 1% solution, this effect was only achieved after more than 12 min of etching. However, SEM images revealed that even after 30 min of etching, areas of the sample remained uncleaned. As shown in Figure 4, 30 min of etching in a 1% acid solution produced a similar effect to 6 min of etching in a 2% solution. For both the 1.4% and 2% solutions, extending the etching time beyond 9 min resulted in degradation of the printed structures.
Figure 5.
The effect of wet chemical etching on the effectiveness of removing residues of incompletely sintered titanium powder from specimens, as a function of etching time and the concentration of the etching solution.
3.1.3. Strength Tests on Samples Following the Wet Chemical Etching Process
The observed gradual reduction in the thickness of the lattice elements and the appearance of an increasing number of material discontinuities, constrictions and pitting led to a decrease in the mass of the prints and a reduction in their mechanical properties. In the research cycle conducted, a conventional structural load-bearing capacity was used, corresponding to a relative deformation of 0.2% of the specimen during an axial compression test. This parameter depends on the decreasing cross-sectional areas of the samples’ lattice structures, which lead to their mass loss, and its changes are closely correlated with changes in the load-bearing capacity of the sample’s entire geometric structure. As shown in Figure 6, a gradual decrease in the F0.2 value was observed as the mass loss of the samples modified by the wet chemical etching method increased. These results are consistent with microscopic observations (Figure 5) indicating degradation of the printed structures during prolonged etching. For samples with a small mass loss (0–10%), the F0.2 values fell within the range of approximately 17–22 kN. As the mass loss increased to approximately 20–30%, the conventional force corresponding to 0.2% strain decreased to approximately 14–16 kN. The greatest mass loss resulted in a reduction in F0.2 of as much as over 50% compared with unmodified samples. As can be seen in Figure 6, despite a noticeable variation in results for samples with similar mass loss, the relationship between the analyzed parameters is close to linear. This variation is due to the specific nature of the samples obtained during the printing process. Defects and internal porosity arising during manufacture account for the lack of full reproducibility between individual samples. Chemical etching can reveal and exacerbate pre-existing defects, potentially contributing to the observed variability in mechanical performance.
Figure 6.
Effect of the weight loss of specimens, resulting from wet chemical etching in an HF solution, on the reduction in their mechanical properties.
3.1.4. Summary of the Results of Wet Chemical Etching
Based on the HF etching results, the treatment conditions offering the best compromise between powder removal, mass loss and mechanical performance were selected for further investigation. Samples etched in a 1.4% HF solution for 7 min were thus selected for further analysis. These parameters enabled the surface of the specimens to be cleaned of residues of powder not fully sintered during the printing process, whilst maintaining a mass loss of 14.53% and a reduction in the notional strength corresponding to 0.2% deformation of the sample during the compression test of 14.69%. The selected processing conditions corresponded to the shortest exposure time that enabled near-complete removal of visible powder residues while avoiding the substantially greater material loss and deterioration of mechanical properties observed at longer etching times. A sample modified in this way will be designated as S-CH in the following discussion. A representative example of the structure obtained after this etching treatment is shown in Figure 7.
Figure 7.
Results of the sample etching method applied, effect on a macroscale (left-hand column) and on a microscale (right-hand column), for samples following wet chemical etching (S-CH) (7 min, 1.4% HF), plasma etching (S-P) and a combination of wet chemical and plasma etching (S-CH/P), compared with the initial sample immediately after printing (S-0).
3.2. Stage Two—Plasma Etching
3.2.1. SEM Observations
Plasma etching was carried out on both samples that had undergone wet chemical etching and unmodified samples. Figure 7 compares the effects of the consecutive post-processing approach (S-CH and S-P, as well as a combination of both methods (S-CH/P), relative to an unmodified sample (S-0). The results can be considered at different scales. At the macroscopic scale (Figure 7, left column), the images show the removal of loosely bound powder residues. At the microscopic scale (Figure 7, right column), they reveal the surface microtopography resulting from each treatment.
At the microscale (Figure 7, right-hand column), we can observe the surface microtopography resulting from the different treatment methods. The effect of chemical etching (S-CH) at the macroscale is the removal of unwanted powders; however, the surface exhibits numerous sharp irregularities, and structural defects and internal porosity become apparent. Additional plasma etching (S-CH/P) eliminates these irregularities; the sample surface is smoothed, and fine irregularities and residues of under-etched structures from the HF etching process are removed. These observations indicate that plasma etching complements wet chemical etching by removing residual surface irregularities. The use of plasma etching alone (S-P), despite the lengthy process time, does not completely remove powders from the specimen surface. However, their shape does change. They transform from spherical to conical. Analysis of SEM images shows that only those cones that are firmly bonded to the substrate and pose no risk of detachment remain on the surface, whilst weaker structures have been removed during the plasma etching process. According to the authors, the resulting geometric structure is not prone to particle detachment from its surface and, during use, may offer an interesting alternative to wet chemical etching.
3.2.2. Mass Loss
An additional advantage of plasma etching is the minimal loss of sample mass. For the samples used in the study, this generally did not exceed 0.2%, compared with nearly 15% obtained with wet chemical etching (Table 2). Plasma etching therefore has a negligible effect on the sample’s geometry and, consequently, on changes to its mechanical properties. Plasma etching can be used as a complementary step following HF etching. The effects of this approach on specimen geometry are shown in Figure 8, using microtomography as an example. The greatest differences in geometric parameters are observed following wet chemical etching; the total porosity of the specimen increases from 27% to 55%. The average size of structural elements in openwork varies from 369 µm to 258 µm (a change of approximately 30%), which results in an increase in the space between them from 133 µm to 319 µm (a change of approximately 140%). Plasma etching, carried out following wet chemical etching, increases these dimensions slightly by 20–30 µm, whilst the total porosity increases by 3% compared with the previous treatment. This slight increase in porosity resulting from plasma etching occurs as a result of complementing the wet chemical etching process and removing surface defects and irregularities, as shown in Figure 7.
Table 2.
Comparison of the effect of surface treatment on mass loss for wet chemical etching (S-CH), plasma etching (S-P), a combination of chemical and plasma etching (S-CH/P), and a combination of wet chemical etching, plasma etching and a DLC coating (S-CH/P/DLC).
Figure 8.
Structural parameters of S-0, S-CH, S-CH/P: (a) lattice strut diameter distribution, (b) pore diameter distribution, (c) porosity.
3.2.3. Surface Topography in Microscale
When comparing sections of the sample surfaces between visible powder clusters, etched areas or holes, it can be observed that, at the microscale (Figure 7, right column), the smoothest surface is that of the sample immediately after printing. Each treatment applied, however, introduces a characteristic microtopographical effect. In chemical etching (S-CH), the α + β two-phase structure of the titanium alloy becomes apparent. Plasma etching (S-P) introduces a micro-indentation effect on the surface, likely also caused by the differing etching rates of the individual phases of the alloy. However, this effect is more subtle than in the case of HF etching (S-CH) or plasma etching following acid etching (S-CH/P).
3.3. Stage Three–Synthesis of the DLC Layer
The samples, which had been cleaned by wet and plasma etching (S-CH/P), were coated with a carbon layer using the RF PACVD process in the final stage. This process did not affect the surface topography; its sole purpose was to alter the chemical structure of the surface to improve its biocompatibility.
Raman Spectroscopy
The resulting layer was characterized using Raman spectroscopy. Raman spectroscopy confirmed the characteristic carbon bonding structure of the coatings, comprising a mixture of sp3-bonded carbon and sp2-bonded carbon, with the characteristic spectrum within the Raman shift range of 1000 to 2000 cm−1. The data were processed using PeakFit 4.12 to fit the spectra to a four-peak model comprising the following peaks: D1 (at 1180 cm−1); D2 (at 1350 cm−1); G1 (approximately1488 cm−1) and G2 (at 1590 cm−1), and to determine the ID/IG ratio, which in this case was equal to (ID1 + ID2)/(IG1 + IG2). An important aspect of the research conducted using Raman spectroscopy was the analysis of the uniformity of DLC coating coverage on metallic 3D printouts. To this end, spot analyses were carried out at various locations on selected samples from three different series following modification with DLC coatings. The spectra obtained in this way were compared with one another (Figure 9), and the parameters describing them enabled the determination of the ID/IG ratio (Table 3). Raman spectroscopy confirmed the presence of a DLC coating at the investigated measurement locations. Similar spectral characteristics obtained in different analyzed regions suggest comparable coating properties within the examined areas of the lattice structure. However, the present measurements do not directly verify coating uniformity throughout the entire three-dimensional lattice architecture. Based on the data collected, it can be determined that the coatings produced within the specified parameters had an ID/IG ratio of 1.18 ± 0.01.
Figure 9.
Raman spectra of DLC coatings for three different production batches.
Table 3.
Analysis of Raman spectra of DLC coatings for three different production batches.
3.4. Comparison of Sample Properties for All Modification Stages
3.4.1. Surface Roughness
In the roughness tests using contact profilometry, the Ra, Rz and Rmax parameters were determined. Due to the lattice nature of the samples, the tests were carried out on the solid region of the disc-shaped samples (Figure 2c). Although measurements were performed on the solid regions of the specimens, they provided an indirect indication of how the treatment affected surface topography. As shown in Figure 10, the highest roughness is observed on the initial sample (S-0), which reflects the initial state of the sample obtained after the printing process, with numerous powder residues not fully integrated into the printed surface. Surface roughness is reduced by wet chemical etching (S-CH). These results are consistent with those obtained from microscopic observations (Figure 7) and computed microtomography (Figure 8). Plasma etching (S-P) alone does not cause significant changes compared with the initial sample. Similarly, the synthesis of a carbon layer does not alter the surface roughness of a sample previously prepared by wet and plasma etching. In this case, a thin DLC coating is formed, which mirrors the topography of the substrate.
Figure 10.
Surface roughness parameters obtained by contact profilometry for samples after various stages of surface treatment, n = 5.
3.4.2. Chemical Composition of the Surface
The chemical composition was determined using the EDS technique (Figure 11). The test results for all samples show a significant proportion of the elements comprising the Ti6Al4V alloy from which the samples were made, namely Ti, Al and V. Differences are observed in the amount of oxygen, which forms the surface passive layer characteristic of titanium. The wet chemical etching process (S-CH) significantly roughens the surface, and the removal of material is accompanied by oxidation processes involving oxygen dissolved in the etching mixture. In the case of plasma etching, on the one hand, the process is carried out under low vacuum (10–12 Pa), so there may be residual oxygen in the vacuum chamber. On the other hand, oxygen may saturate free bonds on the surface during chamber aeration. Both processes are responsible for the presence of oxygen on such modified samples (S-P). The synergistic application of wet and plasma etching (S-CH/P) results in the amount of oxygen present on the sample surface being similar to the value for the reference surface (S-0). This effect can, in turn, be explained by the removal of loosely attached particles and smoothing of the surface and, consequently, a reduction in the chemically active surface area.
Figure 11.
Surface chemical composition obtained by EDS for samples after various stages of surface treatment, n = 3.
3.4.3. Corrosion-Related Electrochemical Behavior
The effect of surface modification on electrochemical behavior was assessed by measuring the open-circuit potential (OCP) (Table 4). Measurements were carried out on samples in which the lattice structure was confined to a cylindrical area 10 mm in diameter and 3 mm thick (Figure 2c,d). The effect of variations in the OCP depending on the surface modification carried out was investigated. A positive potential of 22 ± 63 mV was recorded for the specimen immediately after printing (S-0). All etching treatments reduce this potential, with the effect being most pronounced after wet chemical etching (S-CH), for which a negative OCP value of –165 ± 28 mV was recorded. This indicates a shift toward a more active electrochemical behavior compared with the unmodified sample. This effect may result from significant surface expansion and surface defects caused by the wet chemical etching process. The second stage of surface treatment, namely plasma etching (S-CH/P), raises the OCP value to –80 ± 25 mV. This can be explained by additional surface smoothing and the removal of irregularities. However, the greatest difference is observed after coating the sample with a DLC coating (S-CH/P/DLC), for which the OCP returns to a positive value of 56 ± 34 mV, achieving a better result than the S-0 sample.
Table 4.
Results of the OCP corrosion-related electrochemical behavior test for samples after various stages of surface treatment.
3.4.4. MTT Cytotoxicity Testing of Metallic 3D Printouts Made from Ti6Al4V Alloy Following Various Surface Treatment Processes
Loosely bound particles of the metallic powder used for printing may cause inflammatory reactions at the implantation site. The effectiveness of powder removal from implant surfaces is an important factor in assessing their suitability for biomedical applications. Treatment methods aimed at removing unbound powders (in particular chemical etching methods) may induce changes that compromise the biocompatibility of the Ti6Al4V alloy. With this in mind, a study was conducted to assess the cytotoxicity of metallic 3D-printed objects following various post-processing processes. The study was carried out in accordance with the PN-EN ISO 10993-5 standard [34].
The results of the cell viability assay using the MTT colourimetric test showed that after 24 h of contact with the extracts obtained from the individual samples, the cells retained high viability in every case, significantly above 70% (relative to the negative control designated as K−), which (in accordance with ISO 10993-5) means that they are not cytotoxic. The test results are presented graphically in Figure 12. The absence of any toxic effect of the extract on the cells may also indirectly confirm the effectiveness of the process used to clean the surfaces of the specimens and remove residues of the HF acid.
Figure 12.
Results of the viability assay for NIH/3T3 fibroblast cells after 24 h’ contact with 100% extracts prepared from samples following various post-processing processes: S-0—initial samples, S-CH—samples following wet chemical etching, S-CH/P—samples following wet chemical etching and plasma etching, S-CH/P/DLC—samples following wet chemical etching, plasma etching and DLC coating, K−–negative control—cells cultured under standard conditions without contact with the extract, and K+–positive control—cells deliberately treated with a toxic substance in the form of DMSO. The error bars represent the standard deviation, and the presented results are the mean calculated from 18 measurements for each type of modification.
3.4.5. Assessment of the Proliferative Capacity of Saos-2 Osteoblast-like Cells in Direct Contact with Metallic 3D Printouts Made of Ti6Al4V Alloy Following Various Surface Treatment Processes
A comparative analysis of SEM images showed that the cells adhere rapidly to the surfaces of the treated samples, proliferate and exhibit normal morphology. When comparing the number and morphology of cells growing on the surfaces of 3D-printed Ti6Al4V alloy samples (observation limited to the investigated fields of the solid peripheral regions of the specimens) treated by chemical etching, plasma etching and a combination of the two, no significant changes were observed after 48 h of culture. However, longer culture periods reveal that osteogenic cells occupy almost 100% of the surface area of the S-CH/P/DLC samples. The morphology and chemical composition of this surface make it highly conducive to proliferation. After 96 h of culture on the S-0 and S-P samples, the number of cells is lower, but the extracellular matrix (ECM) produced by them is extensive. In the case of chemically etched samples, where the surface morphology and roughness are altered, the cells produce a slightly less extensive ECM, but the number of cells is greater and their ECM overlaps to a significant extent, covering the surface.
4. Discussion
The results confirmed that effective post-processing of additively manufactured lattice structures made of Ti6Al4V alloy requires a compromise between the efficiency of removing loosely bound powder particles and the preservation of the geometric integrity and mechanical properties of the printed structures. The results indicate that, in the case of wet chemical etching, both the concentration of the HF solution and the etching time are critical parameters determining the final surface and the degree of material degradation, whilst additional plasma treatment can be a significant complement to the process of surface modification, influencing the surface structure and chemical composition. This, in turn, triggers a specific biological response when the material comes into contact with living tissue. Ultimately, there is a synergistic interaction between the individual stages of surface treatment, the main ones of which will be highlighted in the discussion below.
4.1. The Effect of HF Concentration on the Kinetics of the Etching Process
Analysis of mass loss showed that the wet chemical etching process was most intense during the initial stage of treatment, regardless of the HF concentration used. This phenomenon can be explained by the etchant having easier access to the most reactive areas of the surface, including loosely bound powder particles and irregularities formed during the DMLS process. As etching progressed, the rate of mass loss decreased, suggesting the gradual depletion of the areas most susceptible to dissolution, a restriction on the transport of reagents to deeper regions of the structure, and the simultaneous occurrence of dissolution processes and the re-formation of the titanium oxide passive layer. Similar relationships between etching time and the evolution of the Ti6Al4V surface morphology were described by Pankaj Chauhan et al. [35] and Melis Yurddaskal and Hülya Durmuş [36], highlighting the key role of etching time in shaping the topography and degree of surface degradation. In addition to the changes occurring on the material’s surface, the decrease in etching rate is also associated with changes in the composition of the etching solution. During the process, fluoride ions are gradually complexed into fluorotitanate complexes, and the concentration of Ti6Al4V alloy dissolution products increases; this may lead to a local reduction in the chemical activity of the solution and a restriction on the transport of reagents to the material’s surface [32]. However, these effects are likely to be of secondary importance compared to changes in the morphology and reactivity of the etched alloy surface itself [37,38].
SEM observations demonstrated a clear influence of HF concentration on the balance between efficiency of powder removal and the preservation of lattice geometry. The 2% solution enabled very rapid removal of powder residues; however, after just 9 min, it led to significant structural degradation, manifested as narrowings and localized discontinuities in the structural elements. This suggests that such conditions may be too aggressive for lattice-based structures with thin load-bearing elements. Conversely, the use of a 1% solution significantly reduced the rate of material degradation, but at the cost of insufficient efficiency, as areas that had not been etched were still observed even after 30 min. The most favorable compromise was achieved with a concentration of 1.4%, which enabled the complete removal of loose powder particles whilst minimizing mass loss and preserving structural integrity.
4.2. The Relationship Between Geometric Degradation and Mechanical Properties
A key finding of the study was the demonstration of an almost linear relationship between mass loss and the decrease in the F0.2 parameter. This means that material loss during etching directly translates into a reduction in the structure’s load-bearing capacity. The results of the Micro-CT investigations indicate that the reduction in the average diameter of the struts from 369 µm to 258 µm is the structural cause of the observed decrease in the F0.2 value, which proves that the deterioration in mechanical properties is primarily determined by the reduction in the cross-sectional area of the load-bearing struts. This mechanism is particularly significant in the case of lattice-based implants, where the load-bearing capacity of the structure depends on the diameter and continuity of the individual elements of the network.
The observed decline in mechanical properties was consistent with SEM results indicating the development of discontinuities, porosity and local narrowings. It is worth noting that when mass loss exceeded approximately 30% of the F0.2 value, the mechanical properties decreased by more than half compared with unmodified samples. These findings indicate that powder removal alone is insufficient as a criterion for process optimization; the preservation of mechanical integrity must also be considered. In biomedical applications, too, it is very important to maintain the implant’s adequate mechanical strength; therefore, it is essential to limit excessive etching.
The variation in strength results for similar mass loss further highlights the significant role of defects characteristic of the additive manufacturing process. Chemical etching may act selectively on areas of increased porosity or local microstructural inhomogeneities, revealing and exacerbating existing defects. This confirms that the post-processing stage is closely linked to the quality of the additive manufacturing process itself. Similar observations were reported by William W Hogg et al. [39] whilst investigating additively manufactured components made from Ti6Al4V alloy. They noted that even minor changes in the geometry of load-bearing components, the presence of pores and local discontinuities can lead to a significant deterioration in mechanical properties. Defects characteristic of DMLS technology constitute the primary sites of fracture initiation. In the present study, chemical etching likely revealed and magnified existing material inhomogeneities, which provides a good explanation for the observed variation in the results of the compression test.
The importance of processing history in determining the performance of additively manufactured metallic components has also been highlighted for manufacturing routes other than DMLS. For example, recent investigations of FFF-fabricated (Fused Filament Fabrication) and sintered 316L and 17-4PH steels demonstrated that stiffness degradation and failure mechanisms are strongly controlled by process-induced porosity, inter-filament discontinuities, and microstructural heterogeneity [40]. These findings indicate that the functional properties of additively manufactured metals cannot be considered independently of the defects generated during manufacturing. Although the characteristic defects associated with LPBF differ from those observed in FFF-sintered materials, both technologies produce microstructural and geometrical imperfections that influence the effectiveness of post-processing treatments. Therefore, the applicability of the surface modification strategy proposed in the present work to other additive manufacturing technologies would require consideration of the specific defect morphology and processing history associated with a given manufacturing route
4.3. The Role of Plasma Etching as a Complementary Process
Unlike wet chemical etching, plasma etching was characterized by a very small loss of the samples’ initial mass, not exceeding 0.2%. This means that this method had virtually no effect on the geometry of the specimens. At the same time, SEM observations showed that plasma etching alone did not lead to the complete removal of powder particles. However, the process altered their morphology and eliminated particles that were less firmly bound to the substrate.
The results indicate that plasma etching should not be regarded as a direct substitute for chemical etching, but rather as a complementary process. Particularly favorable results were obtained for samples subjected successively to chemical and plasma etching (S-CH/P). In this case, the plasma removed irregularities remaining after aggressive chemical treatment (HF etching), leading to surface smoothing without significant interference with the macrogeometry of the structure. Adel Ghezri et al. reached similar conclusions when applying the plasma electrolytic polishing (PEP) method to reduce the roughness of titanium alloy specimens. In this case, the electrolytic process, which generated a plasma field around the workpiece, led to effective surface smoothing with negligible mass loss. This is consistent with the results of the present study, where mass loss following plasma etching did not exceed 0.2%, whilst SEM observations indicated a marked smoothing of the microtopography. The resulting effect may be of particular significance for bone implants, where the balance between appropriate porosity and controlled surface topography influences the process of osseointegration [35,41]. It can therefore be concluded that plasma treatment acts as a finishing process, whilst the fundamental surface cleaning is carried out during the wet chemical etching stage.
4.4. The Effect of Surface Modification on Roughness and Chemical Composition
Profilometric studies confirmed that the greatest reduction in roughness was achieved by combining chemical and plasma etching. Plasma etching alone did not result in significant changes compared with the initial state, which is consistent with the slight loss of mass observed during this process. In contrast, the combination of both methods allowed for the simultaneous removal of powder residues and surface smoothing. It should be noted that the obtained roughness values reflect changes in the solid specimen regions and should not be interpreted as a direct quantitative representation of the surface characteristics of the internal lattice struts. Differences in local geometry and accessibility to the processing media may alter the processing conditions and dynamics within porous structures. Nevertheless, this approach is considered suitable for identifying general trends in the effects of the proposed post-processing treatments on surface roughness.
Although both chemical and plasma etching individually led to an increase in the oxygen content on the surface, their synergistic application resulted in a level of oxidation similar to that of the initial sample. This suggests that final plasma etching may remove the most developed and reactive surface areas formed during chemical etching, leading to the stabilization of the material’s surface state.
4.5. The Significance of the DLC Coating for Functional Properties
The DLC coating constitutes the final stage of the adopted post-processing sequence, complementing the geometric and physicochemical changes introduced during chemical and plasma etching and imparting to the surface the final functional properties relevant to biomedical applications. The synthesis of the DLC coating did not cause any significant changes to the surface topography, indicating that the deposited layer closely replicates the geometry of the substrate. Raman spectroscopy studies confirmed the formation of a typical amorphous carbon structure containing a mixture of sp2 and sp3 bonds, characteristic of DLC coatings. Slight deviations in the ID/IG ratio further attest to the high repeatability and uniformity of the deposition process. Although similar Raman spectra were obtained at different measurement locations, the internal regions of the lattice structures were not characterized by cross-sectional imaging, local coating-thickness measurements, or adhesion testing. Therefore, the available results confirm the presence of DLC characteristics in the analyzed regions but do not allow unequivocal assessment of coating uniformity throughout the entire lattice structure.
The return of the oxygen content to a level similar to that of the reference sample, observed following plasma etching, correlates well with the partial recovery of the OCP value, indicating that the surface stabilization achieved after the plasma stage prepares the substrate for the full protective effect provided by the DLC coating. It was precisely in the corrosion-related electrochemical behavior tests that a clear effect of this modification was observed. Chemical etching caused a marked deterioration in the OCP value, which can be attributed to an increase in specific surface area and the presence of numerous surface defects. DLC-coated samples exhibited a higher mean OCP value (56 ± 34 mV) than the untreated samples (22 ± 63 mV), indicating a favorable shift in the electrochemical state of the investigated surfaces. Due to the variability in the results and the inherent limitations of OCP measurements, these findings should be interpreted in a qualitative and comparative manner.
Of particular interest is the comparison of the electrochemical test results with the assessment of the cellular response. The unmodified sample was characterized by both a high degree of surface coverage by osteoblast-like cells and a positive OCP value (+22 mV). The application of individual surface treatment stages (plasma, chemical and a combination of both) led to a deterioration in one or both of these parameters. This behavior indicates a temporary trade-off between functional properties at the intermediate treatment stages, which is ultimately offset by the deposition of the DLC coating. The DLC-coated samples exhibited the highest mean OCP value (+56 mV) and the greatest cell coverage among the investigated surface conditions. These results indicate that the role of the DLC coating extends beyond that of a protective barrier—it constitutes a final stage that restores and simultaneously optimizes the functional properties of the surface following prior geometric and physicochemical modifications.
4.6. Biological Significance of the Modifications Obtained
It is known that cells do not merely respond to the chemical composition of the surface with which they come into contact. The surface’s topography generates mechanical forces that are transmitted via signals travelling from integrin adhesion sites, through actin filaments, to the cell nucleus. As a result, there are changes in the expression of hundreds of genes responsible for proliferation, differentiation, apoptosis and the synthesis of ECM. This process is referred to as mechanotransduction [42]. The effect of changes in surface topography on the number of Saos-2 cells proliferating on the surface was observed in the analyzed samples following various post-processing methods. On samples immediately after printing (S-0) and those treated with plasma alone (S-P), a smaller number of cells were observed that strongly extend their extracellular matrix. On samples subjected to chemical etching (S-CH), which alters the surface morphology and roughness, the number of cells is higher, but their matrix is less extensive. This confirms the relationships described in the literature. Surface morphology determines the first stage of cell growth–adhesion. It influences the quantity and spatial organization of adsorbed proteins, and thus also indirectly controls cell behavior [43]. First, serum proteins (fibronectin, vitronectin, laminin, collagen) adsorb onto the surface, and only then do cellular integrins bind to them. As the topography changes, so does the morphology of the cells themselves. On smooth surfaces, cells typically flatten considerably, develop numerous lamellipodia and increase their contact area, as observed for unmodified samples (S-0) and those treated with plasma alone (S-P). In contrast, on topographically more complex surfaces, they form numerous filopodia, anchor themselves at specific points, adopt a more three-dimensional shape and increase their mechanotransduction activity. These changes result from the reorganization of actin filaments and the activation of FAK (Focal Adhesion Kinase), RhoA/ROCK and YAP/TAZ [44]. This is evident in the SEM images (Figure 13) of samples following chemical etching in HF acid (S-CH), etching in acid supplemented with plasma etching (S-CH/P), and samples subjected to two-stage etching and coated with DLC (S-CH/P/DLC)—in these cases, numerous filopodia anchored at specific points strongly attach the cells to the sample surfaces.
Figure 13.
SEM images showing the morphology of cells adhering to the surfaces of modified samples. Condition after 96 h of culture.
An increase in surface roughness often leads to a decrease in the rate of proliferation. Boyan et al. demonstrated that, on rougher titanium surfaces, osteoblasts divide more slowly but commence maturation much earlier, increase their production of osteocalcin and alkaline phosphatase (ALP) activity, and synthesize more type I collagen [45]. This effect is not observed in samples that have undergone the full treatment cycle (S-CH/P/DLC)—in this case, cells are the most abundant of all the surfaces analyzed and, at the same time, have the greatest number of filopodia. This is a synergistic effect resulting from the influence of surface topography combined with its chemical activation through the application of a DLC coating, and may account for the surface’s high bioactivity. This is achieved by adopting a treatment sequence in which HF removes the layer of oxides and impurities and partially modifies the surface micro-roughness, whilst Ar plasma further cleans the surface of organic residues and increases the surface energy (which promotes the adsorption of proteins from the culture medium [46]), whilst the DLC coating provides a surface that may favorably influence the adsorption of adhesive proteins (e.g., fibronectin and vitronectin) [47], thereby facilitating the binding of cellular integrins [48]. These surface characteristics may favor cell adhesion and proliferation, potentially contributing to the higher surface coverage observed for Saos-2 cells on the DLC-coated samples. Greater roughness and strong cell adhesion to the substrate, confirmed by the abundant presence of filopodia, may have limited the cells’ ability to migrate across the surface. Consequently, the proliferating cells achieved high local confluence and formed clusters [49,50].
4.7. Practical Implications and Limitations of the Study
The results indicate that the most effective strategy for surface preparation of printed Ti6Al4V implants is to employ a multi-stage surface engineering process comprising wet chemical etching in 1.4% HF for 7 min, followed by plasma etching and final deposition of a DLC layer. This approach enables the effective removal of unbound powder particles, minimizes mechanical degradation of the structure, improves corrosion-related electrochemical behavior and yields a favorable biological response. In this way, the three-stage post-processing can serve as a tool for the targeted tuning of the functional properties of additively manufactured Ti6Al4V lattice-based implants, rather than merely a surface cleaning procedure.
It should be noted, however, that the research was conducted on a single alloy type, a single geometry of lattice-based structures, and specific DMLS process parameters. Future studies should investigate the effects of these treatments on lattice structures with different porosities and strut dimensions, as well as assess the long-term stability of their biological and electrochemical properties in vitro and in vivo.
It should also be noted that the design of the experiment does not enable the individual contribution of each processing stage to be fully isolated. Not all alternative process combinations were considered in the present study; for instance, specimens with DLC coating deposited immediately following chemical etching were not included. Consequently, while the results confirm the effectiveness of the investigated technological sequence, they do not permit definitive conclusions regarding the necessity of every individual processing stage. Future research should incorporate additional treatment variants, which would enable a quantitative assessment of the contribution of each surface modification step.
The mechanical characterization conducted in this study focused on assessing the effects of chemical etching, which directly affected the dimensions of the truss elements. The influence of subsequent steps—plasma treatment and DLC coating—on the mechanical properties of the structures was not directly investigated. Although these processes caused only minor mass changes and did not lead to visible geometric changes, the potential impact of thermal exposure and surface modification cannot be ruled out and should be further explored in future work.
5. Conclusions
This study demonstrated that multi-stage surface engineering can serve as a tool for the deliberate shaping of the functional properties of DMLS-fabricated Ti6Al4V lattice-based structures, going beyond the role of a conventional surface cleaning process. Etching in a 1.4% HF solution for 7 min provided the most favorable compromise between the effectiveness of powder residue removal and the preservation of structural integrity, enabling almost complete removal of loosely attached particles with limited mass loss and an acceptable reduction in strength. Plasma etching alone did not completely remove the powder particles; however, when applied following chemical etching, it exhibited a clear synergistic effect, leading to further homogenization of the surface without significantly affecting the geometry of the lattice-based structures. The application of the DLC coating allowed the previously formed surface topography to be preserved, while significantly improving its functional properties and indicating more favorable electrochemical behavior compared with unmodified samples. All the modification variants analyzed remained non-toxic; however, the full treatment sequence (HF etching + plasma etching + DLC) ensured the highest apparent cell coverage of osteoblast-like cells and the most extensive colonization observed by SEM. These findings suggest that DLC deposition may offset the changes in biological response observed after the intermediate treatment stages, resulting in greater cell coverage than on the unmodified samples. The proposed sequence of HF → plasma etching → DLC is not merely a surface treatment procedure, but an integrated approach enabling the deliberate tailoring of the functional properties of Ti6Al4V structures intended for biomedical applications.
Author Contributions
Conceptualization, J.G.; methodology, J.G., D.B., K.J., W.K., S.L., A.K.P. and A.N.; validation, J.G., D.B., K.J., W.K., J.K. and P.N.; formal analysis, J.G., D.B., K.J., W.K. and P.N.; investigation, J.G., D.B., K.J., W.K., S.L., A.K.P., A.N. and J.K.; resources, J.G.; data curation, J.G.; writing—original draft preparation, J.G., D.B., K.J., W.K. and A.K.P.; writing—review and editing, J.G., J.K. and P.N.; visualization, J.G., D.B., A.K.P. and W.K.; supervision, J.G. and P.N.; project administration, J.G.; funding acquisition, J.G. All authors have read and agreed to the published version of the manuscript.
Funding
Work funded by the Foundation for Polish Science under the 2nd Priority of the European Funds for Modern Economy 2021–2027 (FENG) Programme, Grant Agreement No. FENG.02.07-IP.05-0370/23, Project Title: Purification and bioactivation of titanium 3D printouts for biomedical applications.
Data Availability Statement
The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding author.
Acknowledgments
The authors acknowledge Medgal Ltd. for their support in preparing the samples used in the research described in this publication. The authors used the DeepL Write program (version 26.11.1.21905+2c27676d2cc38b00aef7dfeba6a717c036a181d7) to perform linguistic proofreading of the text. The authors have reviewed and edited the output and take full responsibility for the content of this publication. The micro-computed tomography (micro-CT) system used in this study was purchased with funding provided through statutory activity I42/501-4-42-1-1 at the Lodz University of Technology, Textile Institute, Poland. The acquisition of the equipment was additionally supported by the investment project “Innovative Textiles 2020+” (No. RPLD.01.01.00-10-0002/17-00), implemented under the Regional Operational Programme for Łódzkie Voivodeship 2014-2020.
Conflicts of Interest
The authors declare no conflicts of interest.
Abbreviations
The following abbreviations are used in this manuscript:
| DLC | Diamond-like carbon |
| HF | Hydrofluoric acid |
| DMLS | Direct Metal Laser Sintering |
| SEM | Scanning electron microscopy |
| EDS | Energy Dispersive X-ray Spectroscopy |
| OCP | Open-circuit potential |
| Dc | Diameter of the lattice struts |
| Dn | Diameter of the structural nodes |
| CT | Computed tomography |
| RFPACVD | Radio frequency plasma-activated chemical vapor deposition |
| CH4 | Methane |
| P/S/N | Penicillin–streptomycin–neomycin |
| BCS | Bovine Calf Serum |
| DMSO | Dimethyl sulfoxide |
| DMEM | Dulbecco’s Modified Eagle’s Medium |
| Saos-2 | Human Osteoblast-Like Osteosarcoma Cell Line |
| ECM | Extracellular matrix |
| PEP | Plasma electrolytic polishing |
| FAK | Focal Adhesion Kinase |
| FWHM | Full Width at Half Maximum |
| FFF | Fused Filament Fabrication |
References
- Madan, J.; Witherell, P.; Rosen, D.W. A Review of 3D-Printed Medical Implant Design. 3D Print. Med. 2026, 12, 3. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Ren, B.; Wan, Y.; Liu, C.; Wang, H.; Yu, M.; Zhang, X.; Huang, Y. Improved Osseointegration of a 3D-Printed Ti-6Al-4V Implant with a Hierarchical Micro/Nano Surface Topography: An In Vitro and In Vivo Study. Mater. Sci. Eng. C 2021, 118, 111505. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Li, Y.; Wang, F. Review of 3D-Printed Titanium-Based Implants: Materials and Post-Processing. ChemBioEng Rev. 2024, 11, e202400032. [Google Scholar] [CrossRef] [Scilit]
- Akula, S.B. Metallic Lattice Structures via Additive Manufacturing: Applications, Challenges and Opportunities in Aerospace and Defence. J. Manuf. Process. 2026, 157, 1308–1336. [Google Scholar] [CrossRef] [Scilit]
- Pourrahimi, S.; Hof, L. On the Post-Processing of Complex Additive-Manufactured Metallic Parts: A Review. Adv. Eng. Mater. 2024, 26, 2301511. [Google Scholar] [CrossRef] [Scilit]
- Heimbrook, A.; Gall, K. Effect of Surface Topography on the Fatigue Behaviour of Additively Manufactured Ti6Al4V and CoCr Alloys. Mater. Sci. Eng. A 2024, 909, 146821. [Google Scholar] [CrossRef] [Scilit]
- Mancisidor, A.M.; García-Blanco, M.B.; Quintana, I.; Arrazola, P.J.; Espinosa, E.; Cuesta, M.; Albizuri, J.; Garciandia, F. Effect of Post-Processing Treatment on the Fatigue Performance of Ti6Al4V Alloy Manufactured by Laser Powder Bed Fusion. J. Manuf. Mater. Process. 2023, 7, 119. [Google Scholar] [CrossRef] [Scilit]
- Soares, F.M.S.; Barbosa, D.M.; Corado, H.P.R.; Santana, A.I.C.; Elias, C.N. Surface Morphology, Roughness, and Corrosion Resistance of Dental Implants Produced by Additive Manufacturing. J. Mater. Res. Technol. 2022, 21, 3844–3855. [Google Scholar] [CrossRef] [Scilit]
- Melia, M.A.; Duran, J.G.; Koepke, J.R.; Saiz, D.J.; Jared, B.H.; Schindelholz, E.J. How Build Angle and Post-Processing Impact Roughness and Corrosion of Additively Manufactured 316L Stainless Steel. npj Mater. Degrad. 2020, 4, 21. [Google Scholar] [CrossRef] [Scilit]
- Tang, J.; Li, S.; Liu, Y.; Pei, G.; Yan, M. Significantly Enhanced Biocompatibility and Performance of 3D-Printed Porous 316L Stainless Steel via a Simple and Efficient Surface Polishing Approach. Mater. Des. 2025, 251, 113640. [Google Scholar] [CrossRef] [Scilit]
- McGee, O.M.; Geraghty, S.; Hughes, C.; Jamshidi, P.; Kenny, D.P.; Attallah, M.M.; Lally, C. An Investigation into Patient-Specific 3D-Printed Titanium Stents and the Use of Etching to Overcome Selective Laser Melting Design Constraints. J. Mech. Behav. Biomed. Mater. 2022, 134, 105388. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Mingear, J.; Zhang, B.; Elwany, A.; Hartl, D. Roughness Analysis of Powder-Bed Fused Nickel-Titanium Surfaces with Chemical Etching Enhancement by a Safe Aqueous Fluoride Solution. Shape Mem. Superelasticity 2023, 9, 504–519. [Google Scholar] [CrossRef]
- Bocchetta, P.; Chen, L.-Y.; Tardelli, J.D.C.; dos Reis, A.C.; Almeraya-Calderón, F.; Leo, P. Passive Layers and Corrosion Resistance of Biomedical Ti-6Al-4V and β-Ti Alloys. Coatings 2021, 11, 487. [Google Scholar] [CrossRef] [Scilit]
- Yi, G.; Liu, X.; Zheng, C.; Zhang, H.; Xu, C.; Cui, Y.-W.; Liu, S. Characteristics of Passive Films Formed on As-Cast Ti-6Al-4V in Hank’s Solution Before and After Transpassivation. Front. Mater. 2021, 7, 640081. [Google Scholar] [CrossRef] [Scilit]
- Licausi, M.P.; Igual Muñoz, A.; Amigó Borrás, V. Tribocorrosion Mechanisms of Ti6Al4V Biomedical Alloys in Artificial Saliva With Different pHs. J. Phys. D Appl. Phys. 2013, 46, 404003. [Google Scholar] [CrossRef] [Scilit]
- An, L.; Wang, D.; Zhu, D. Combined Electrochemical and Mechanical Polishing of Interior Channels in Parts Made by Additive Manufacturing. Addit. Manuf. 2022, 51, 102638. [Google Scholar] [CrossRef] [Scilit]
- Hunter, L.W.; Brackett, D.; Brierley, N.; Yang, J. Assessment of Trapped Powder Removal and Inspection Strategies for Powder-Bed Fusion Techniques. Int. J. Adv. Manuf. Technol. 2020, 106, 4521–4532. [Google Scholar] [CrossRef] [Scilit]
- Surmeneva, M.A.; Khrapov, D.; Prosolov, K.; Kozadayeva, M.; Koptyug, A.; Volkova, A.; Paveleva, A.; Surmenev, R.A. The Influence of Chemical Etching on the Porous Structure and Mechanical Properties of Ti6Al4V Functionally Graded Porous Scaffolds Fabricated by EBM. Mater. Chem. Phys. 2022, 275, 125217. [Google Scholar] [CrossRef] [Scilit]
- Chang, S.; Liu, A.; Ong, C.Y.A.; Zhang, L.; Huang, X.; Tan, Y.H.; Zhao, L.; Li, L.; Ding, J. Highly Effective Smoothing of 3D-Printed Metal Structures via Overpotential Electrochemical Polishing. Mater. Res. Lett. 2019, 7, 359–366. [Google Scholar] [CrossRef] [Scilit]
- Xie, D.; Lv, F.; Shen, L.; Tian, Z.; Jiang, R.; Zhao, J. Effect of Higher Laser Power Remelting on Porosity and Mechanical Performance of Parts Built by Laser Powder Bed Fusion. Int. J. Adv. Manuf. Technol. 2023, 125, 4779–4791. [Google Scholar] [CrossRef] [Scilit]
- Bolli, E.; Kaciulis, S.; Lanzutti, A. Surface Characteristics and Tribological Behaviour of 3D-Printed 316L Steel after Plasma-Assisted Low-Temperature Carburising. Surf. Coat. Technol. 2024, 477, 130295. [Google Scholar] [CrossRef] [Scilit]
- Tillmann, W.; Dias, N.F.L.; Stangier, D.; Schaak, C.; Höges, S. Coatability of Diamond-Like Carbon on 316L Stainless Steel Printed by Binder Jetting. Addit. Manuf. 2021, 44, 102064. [Google Scholar] [CrossRef] [Scilit]
- Akbay, Ö.C.; Bahçe, E.; Uysal, A.; Gezer, I. Production and Cleaning of Lattice Structures Used in the Space and Aerospace Industry with Metal Additive Manufacturing Methods. J. Mater. Eng. Perform. 2022, 31, 6310–6321. [Google Scholar] [CrossRef] [Scilit]
- Brezinová, J.; Hudák, R.; Guzanová, A.; Draganovská, D.; Ižaríková, G.; Koncz, J. Direct Metal Laser Sintering of Ti6Al4V for Biomedical Applications: Microstructure, Corrosion Properties, and Mechanical Treatment of Implants. Metals 2016, 6, 171. [Google Scholar] [CrossRef] [Scilit]
- Jastrzębski, K.; Szafarz, K.; Puszkarz, A.K. Chemical Post-Processing of SLM Ti6Al4V Structures Using HF with Propylene Glycol: Surface, Structural and Biological Evaluation of an Exploratory Post-Processing Strategy. Materials 2026, 19, 3924. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Pham, M.H.; Landin, M.A.; Tiainen, H.; Reseland, J.E.; Ellingsen, J.E.; Haugen, H.J. The Effect of Hydrofluoric Acid Treatment of Titanium and Titanium Dioxide Surfaces on Primary Human Osteoblasts. Clin. Oral Implants Res. 2014, 25, 385–394. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Hung, K.-Y.; Lin, Y.-C.; Feng, H.-P. The Effects of Acid Etching on the Nanomorphological Surface Characteristics and Activation Energy of Titanium Medical Materials. Materials 2017, 10, 1164. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Sotgiua, G.; Orsini, M.; Porcelli, F.; De Santis, S.; Petrucci, E. Wettability of Micro- and Nanostructured Surfaces of Titanium-Based Electrodes: Influence of Chemical and Electrochemical Etching. Chem. Eng. Trans. 2021, 86, 1417–1422. [Google Scholar] [CrossRef] [Scilit]
- Huang, B.-H.; Lu, Y.-J.; Lan, W.-C.; Ruslin, M.; Lin, H.-Y.; Ou, K.-L.; Saito, T.; Tsai, H.-Y.; Lee, C.-H.; Cho, Y.-C.; et al. Surface Properties and Biocompatibility of Anodised Titanium with a Potential Pretreatment for Biomedical Applications. Metals 2021, 11, 1090. [Google Scholar] [CrossRef] [Scilit]
- Bociaga, D.; Grabarczyk, J.; Niedzielski, P.; Januszewicz, B.; Bogdański, M.; Kotela, I.; Borowska-Skarzyńska, U. The Effect of Post-Processing in the Form of Ion Etching with Ar and O Applied to Metallic 3D Prints Produced Using the DMP Method on Their Cleaning Efficiency and Biological Response. J. Biomed. Mater. Res. B Appl. Biomater. 2026, 114, e70068. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Tai, F.C.; Lee, S.C.; Chen, J.; Wei, C.; Chang, S.H. Multipeak Fitting Analysis of Raman Spectra on DLC Films. J. Raman Spectrosc. 2009, 40, 1055–1059. [Google Scholar] [CrossRef] [Scilit]
- Kaczorowski, W.; Świątek, H.; Łuczak, K.; Głuszek, M.; Cłapa, M. Impact of Plasma Pre-Treatment on the Tribological Properties of DLC Coatings on PDMS Substrates. Materials 2021, 14, 433. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- ISO 10993-12:2021; Biological Evaluation of Medical Devices—Part 12: Sample Preparation and Reference Materials. International Organization for Standardization (ISO): Geneva, Switzerland, 2021.
- ISO 10993-5:2009; Biological Evaluation of Medical Devices—Part 5: Tests for In Vitro Cytotoxicity. International Organization for Standardization (ISO): Geneva, Switzerland, 2009.
- Chauhan, P.; Koul, V.; Bhatnagar, N. Critical Role of Etching Parameters in the Evolution of Nano-Micro SLA Surface on Ti6Al4V Alloy Dental Implants. Materials 2021, 14, 6344. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Yurddaskal, M.; Durmuş, H. The Effects of Acid Concentration, Etching Temperature and Time on the Surface Morphologies of Ti6Al4V. Eur. J. Tech. 2020, 10, 386–394. [Google Scholar] [CrossRef] [Scilit]
- Amrutha, M.S.; Fasmin, F.; Ramanathan, S. Effect of HF Concentration on Anodic Dissolution of Titanium. J. Electrochem. Soc. 2017, 164, H1–H10. [Google Scholar] [CrossRef] [Scilit]
- Mizuhata, M.; Yamamoto, S.; Maki, H. Removal of Surface Scale from Titanium Metal by Etching with HF–HNO3 Mixed Acid. Mater. Trans. 2017, 58, 1280–1289. [Google Scholar] [CrossRef] [Scilit]
- Hogg, W.W.; Jamal, M.; Zuckschwerdt, N.W.; Hess, C.M.; Bose, S.; Bandyopadhyay, A. Corrosion-Fatigue of Additively Manufactured Ti6Al4V. J. Mech. Behav. Biomed. Mater. 2025, 175, 107289. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Iandiorio, C.; Ceci, A.; Marotta, E.; Salvini, P.; Costanza, G.; Tata, M.E. Microstructure-Driven Damage Mechanics and Failure of FFF-Sintered 316L and 17-4PH Steels. Eng. Fail. Anal. 2026, 197, 111364. [Google Scholar] [CrossRef] [Scilit]
- Liang, C.-Y.; Jiang, X.-J.; Ji, R.-L.; Li, B.-E.; Zou, X.-R.; Wang, H.-S.; Hao, J.-Z.; Yang, T. Preparation and Surface Modification of 3D-Printed Ti–6Al–4V Porous Implants. Rare Met. 2021, 40, 1164–1172. [Google Scholar] [CrossRef] [Scilit]
- Ermis, M.; Antmen, E.; Hasirci, V. Micro- and Nanofabrication Methods to Control Cell-Substrate Interactions and Cell Behaviour: A Review from the Tissue Engineering Perspective. Bioact. Mater. 2018, 3, 355–369. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Anselme, K.; Bigerelle, M. The Role of Materials’ Surface Topography on Mammalian Cell Response. Int. Mater. Rev. 2011, 56, 243–266. [Google Scholar] [CrossRef] [Scilit]
- Nguyen, A.T.; Sathe, S.R.; Yim, E.K.F. From Nano to Micro: Topographical Scale and Its Impact on Cell Adhesion, Morphology and Contact Guidance. J. Phys. Condens. Matter 2016, 28, 183001. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Boyan, B.D.; Lohmann, C.H.; Dean, D.D.; Sylvia, V.L.; Cochran, D.L.; Schwartz, Z. Mechanisms Involved in Osteoblast Response to Implant Surface Morphology. Annu. Rev. Mater. Res. 2001, 31, 357–371. [Google Scholar] [CrossRef] [Scilit]
- Rupp, F.; Scheideler, L.; Olshanska, N.; de Wild, M.; Wieland, M.; Geis-Gerstorfer, J. Enhancing Surface Free Energy and Hydrophilicity through Chemical Modification of Microstructured Titanium Implant Surfaces. J. Biomed. Mater. Res. A 2006, 76, 323–334. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Narayan, R. (Ed.) Diamond-Based Materials for Biomedical Applications; Elsevier: Amsterdam, The Netherlands, 2013. [Google Scholar]
- Keselowsky, B.G.; Collard, D.M.; García, A.J. Surface Chemistry Modulates Fibronectin Conformation and Directs Integrin Binding and Specificity to Control Cell Adhesion. J. Biomed. Mater. Res. A 2003, 66, 247–259. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Palecek, S.; Loftus, J.C.; Ginsberg, M.H.; Lauffenburger, D.A.; Horwitz, A.F. Integrin-Ligand Binding Properties Govern Cell Migration Speed through Cell-Substrate Adhesiveness. Nature 1997, 385, 537–540. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Huttenlocher, A.; Horwitz, A.R. Integrins in Cell Migration. Cold Spring Harb. Perspect. Biol. 2011, 3, a005074. [Google Scholar] [CrossRef] [Scilit] [PubMed]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.