Full-Cell Performance Benchmarking and Digitalization-Ready Testing Protocols for Direct Formic Acid Fuel Cells

,
,
and
1
Dr. Franjo Tuđman Defense and Security University, Zrinsko-Frankopanska 207a, 21000 Split, Croatia
2
Faculty of Electrical Engineering, Mechanical Engineering and Naval Architecture, University of Split, Ruđera Boškovića 32, 21000 Split, Croatia
*
Authors to whom correspondence should be addressed.
This article belongs to the Section B: Energy and Environment

Abstract

Direct formic acid fuel cells (DFAFCs) offer a liquid-fuel alternative to hydrogen-fed proton-exchange membrane fuel cells, but inconsistent designs and operating conditions hinder performance comparisons. This review critically compares selected experimentally tested single-cell DFAFCs using Pt-, Pd-, Pt–Pd-, and non-noble-metal catalyst systems in terms of peak power density, catalyst loading, durability, and operating conditions. Reported peak power densities range from 20 to 550 mW cm−2. Pd–Ni2P/C achieved 550 mW cm−2, while PtBiPbNiCo reached 321.2 mW cm−2. Iron(II) tetrasulfophthalocyanine (FeTSPc)-promoted Pt increased peak power density from 76.3 to 126.6 mW cm−2 and suppressed CO-forming pathways. A Co–nitrogen-doped carbon nanotubes (NCNT) cathode achieved 160.7 mW cm−2, exceeding the corresponding Pt/C reference. However, inconsistent durability tests and cell configurations prevent reliable cross-study rankings and assessments of commercial readiness. A baseline protocol is proposed that specifies operation at 60 °C with 3 M formic acid, controlled oxidant supply, defined membrane-electrode assembly geometry, liquid-compatible anode diffusion layers, and at least 100 h of durability testing. The protocol is designed to generate interoperable, machine-readable datasets, which are prerequisites for digital twins, predictive degradation assessment, and real-time energy management of DFAFC-based hybrid transport power systems. Standardized full-cell testing can distinguish catalyst improvements from configuration effects and support reproducible DFAFC development.

1. Introduction

Proton exchange membrane fuel cells (PEMFCs) have received significant attention as green energy policies have gained prominence [1]. Beyond production costs, their reliance on hydrogen as a fuel is the primary barrier to widespread commercial implementation. Although hydrogen has exceptionally high gravimetric energy density, its low volumetric energy density poses a major challenge for practical storage and transportation.
To overcome the limitations of hydrogen-based PEMFC systems, formic acid has been extensively investigated as a promising alternative liquid fuel because of its high volumetric energy density compared with hydrogen. Its direct use in PEMFC architectures offers a viable pathway to address transport and handling bottlenecks [2,3]. In low-temperature fuel cells, formic acid (FA) offers several advantages over other liquid fuels. As a simple C1 molecule, FA can be produced sustainably from biomass or through the electrochemical reduction in CO2, aligning with environmental and resource sustainability targets [4,5]. FA is also advantageous for practical operation because it is a nonflammable organic acid that remains stable in liquid form at room temperature, has a pungent warning odor, and is biocompatible (approved as a food additive by the FDA) [6]. Crucially, FA has a high energy density and a significantly lower fuel crossover rate through Nafion membranes than methanol [7], which directly translates into enhanced cathode performance and minimized voltage losses during operation [8,9].
Although the absolute energy density of formic acid (1725 Wh/kg or 2100 Wh/L) is lower than that of methanol (6100 Wh/kg or 4900 Wh/L), operational DFAFCs frequently outperform direct methanol fuel cells (DMFCs). This performance advantage stems directly from a threefold reduction in fuel crossover through the Nafion membrane to the cathode side. The lower crossover is caused by electrostatic repulsion between the formate (HCOO−) species and the fixed sulfonate groups (-SO3−) within the proton exchange membrane (PEM) [10]. Additionally, the apparent diffusion coefficient of formic acid through the Nafion membrane is three times lower than that of methanol, significantly enhancing fuel utilization and voltage efficiency in DFAFCs [11]. Combined with the inherently higher electrooxidation kinetics of FA at the anode relative to methanol, these properties make formic acid a superior liquid fuel candidate for next-generation PEMFC systems [12]. Compared with hydrogen, formic acid has an energy density equivalent to that of commercial hydrogen systems, such as the 70 MPa storage tanks used in the Toyota Mirai vehicle [13]. Furthermore, the theoretical open-circuit potential of the DFAFC is 1.45 V [14], significantly higher than the theoretical open-circuit potential of 1.23 V for PEMFCs and 1.21 V for DMFCs, as well as the 1.13 to 1.25 V range reported for direct alcohol fuel cells (DAFCs).
Against this background, the development of modern polymer-electrolyte DFAFCs gained momentum in the early 2000s. Ref. [15] reported a pioneering device-level demonstration, followed by their investigation of anode catalysts in 2003 [16]. Subsequently, ref. [17] demonstrated higher-power operation using ambient air, including at room temperature. These early studies helped establish DFAFCs as candidates for portable power generation and provided a foundation for subsequent catalyst development and cell engineering.
The working principle of DFAFCs is based on the electrochemical oxidation of formic acid at the anode, which can proceed via three distinct reaction pathways. A schematic overview of the DFAFC working principle is shown in Figure 1, and this principle is explained further below.
Figure 1. Schematic overview of the reaction pathway inside a direct formic acid fuel cell.
The first and preferred pathway is direct dehydrogenation, in which formic acid is converted directly into carbon dioxide, two protons, and two electrons. This route enables efficient energy conversion while minimizing catalyst poisoning. The second pathway is dehydration, which yields water and undesirable carbon monoxide (CO). CO generation is highly detrimental because CO strongly adsorbs to and poisons active catalyst sites, thereby reducing overall cell performance. The third pathway, discovered more recently and often categorized as a branch of the direct reaction pathway, involves the generation of HCOO−, adding further complexity to the interfacial reaction mechanism [18].
Because CO generation remains the primary threat to DFAFC durability, contemporary research focuses heavily on suppressing the indirect pathway or developing CO-resistant catalyst formulations suitable for long-term operation. Although several reviews have summarized recent progress in catalysts for formic acid oxidation from an electrochemical perspective, they often rely primarily on half-cell measurements and do not systematically compare full-cell DFAFC performance under comparable operating conditions.
In contrast, the present review focuses exclusively on experimentally tested full single-cell DFAFCs. It compares polarization curves, peak power densities, and catalyst loadings, alongside key operating parameters such as catalyst composition, temperature, fuel concentration, and mass flow rates at the anode and cathode. The substantial performance variability reported across the literature indicates that cross-study comparisons are hindered by nonstandardized experimental configurations rather than by intrinsic catalyst limitations. Accordingly, this review has two objectives: first, to identify realistic device-level performance boundaries and catalyst-development priorities for DFAFCs; and second, to establish a practical, digitalization-ready standardization framework centered on controllable operational parameters to ensure uniform and reproducible testing and provide a consistent data basis for future digital twins, predictive optimization, and real-time energy management in low-carbon transport applications. This approach provides an application-oriented perspective on DFAFC catalysts, identifies realistic performance limits, and outlines the remaining challenges to commercialization. Several reviews have examined DFAFC catalysts from complementary perspectives. Li et al. [2] focus on electrode engineering from the nanomaterial to the device scale, covering nanowire-array catalysts, electrode fabrication routes, and the mass-transport and interfacial losses that arise during scale-up to membrane electrode assemblies. Cheng et al. [19] survey catalyst materials for formic acid-powered PEM fuel cells, including high-entropy and non-precious systems, with an emphasis on anode degradation mechanisms. Bhaskaran et al. [18] combine discussion of the dual-pathway oxidation mechanism with nanoparticle design and cell-architecture considerations, including flow fields and stack aspects. Fang and Chen [5] concentrate on the fundamental formic acid oxidation mechanism and nanostructured electrocatalysts, drawing predominantly on half-cell electrochemical measurements and theoretical calculations. Jiang et al. [4] review formic acid electrocatalysis on Pt and Pd surfaces based on single-crystal studies and early nanoparticle work published up to 2014. None of these reviews compiles reported full single-cell polarization and power-density data under explicitly compared operating conditions, and none proposes a standardized full-cell testing protocol. These two elements constitute the gap addressed by the present work, as summarized in Table 1.
Table 1. Summary of the scope and core findings of existing DFAFC reviews, their limitations, and how they compare with the framework of this work.
The literature search for this review focused on catalysts evaluated in complete single-cell direct formic acid fuel cells. Publications were identified through publisher platforms, including Elsevier and MDPI, as well as other relevant sources, using keywords such as “direct formic acid fuel cell,” “DFAFC,” “formic acid oxidation,” “catalyst,” and combinations of these terms. Both recent publications and earlier foundational studies were considered to capture developments in catalyst design, full-cell performance, and testing procedures.
The quantitative benchmarking focused on experimental studies reporting complete single-cell DFAFC performance, including polarization curves and/or power-density measurements. Both anode and cathode catalyst modifications were considered, and their respective roles were identified in the comparison. Studies reporting exclusively half-cell electrochemical measurements, theoretical calculations, or numerical simulations were excluded from the quantitative full-cell benchmark, although reaction mechanisms and catalyst-development strategies were considered a main pillar of catalyst development. Publications concerning hydrogen-fed PEMFCs, direct methanol fuel cells, and other related systems were used only for contextual discussion and to identify potentially transferable approaches, rather than as direct evidence of DFAFC performance.
The extracted information from the included full-cell studies comprised catalyst composition, peak power density, anode and cathode catalyst loadings, operating temperature, fuel concentration, reactant flow rates, and durability measurements, where available. Parameters that were not reported were identified as such and were not used as automatic exclusion criteria. Reported performance was interpreted alongside the corresponding operating conditions and cell configurations; consequently, the comparison characterizes reported device-level performance rather than establishing an intrinsic ranking of catalyst activity. Differences in testing conditions and reporting practices informed the proposed experimental standardization framework. The extracted variables also provided the basis for discussing data-reporting requirements for future DFAFC modeling, digital-twin development, and energy management in hybrid transport systems.

2. Catalysts for Direct Formic Acid Fuel Cells

Catalysts are among the key determinants of DFAFC performance, and three principal types are currently under active investigation for formic acid oxidation. This section of the review considers three major catalyst groups and one additional subgroup. The first group comprises platinum-based catalysts, the second consists of palladium-based catalysts, and the third includes catalysts based on non-noble metals. Finally, a subgroup of bimetallic Platinum-Palladium catalysts is analyzed to provide a more comprehensive assessment of catalyst performance based on catalyst composition in DFAFCs. Techniques for catalyst preparation and implementation are also described as crucial aspects of catalyst development. The primary focus is on full-cell DFAFC catalyst power density and durability as functions of different catalyst compositions, loads, testing temperatures, and flow rates, where available. At the end of this chapter, an overview of all catalyst performances and other influential parameters is presented, with catalyst performance as the main parameter. In terms of Table 1, this section addresses the absence of a compiled full-cell performance matrix by reviewing the single-cell polarization and power-density evidence for each catalyst family.
There are two main methods for improving catalyst activity: incorporation of the support material (the most common method) and catalyst alloying to enhance electro-oxidation kinetics [2,20]. Although catalysts are the most widely researched topic related to DFAFCs, designing a highly efficient FAO catalyst remains a significant challenge. This challenge arises because the FAO reaction mechanism remains controversial and is not fully understood. Adsorbed CO (COads) is generally accepted as the primary intermediate that causes degradation of electrocatalytic performance. Accordingly, further research into the FAO mechanism is essential, and the challenge of improving electrocatalyst stability during FAO must be addressed before DFAFC commercialization.
Catalyst cost is another critical factor in the implementation of DFAFCs and PEMFCs in general. The main goal is to reduce noble metal loading without compromising performance.
The cost aspect remains largely neglected. However, promising examples of cost reduction in hydrogen PEMFCs demonstrate significant progress in reducing Pt catalyst loading through the use of different materials and catalysts.

2.1. Platinum-Based Catalysts

Platinum-based catalysts are the most well-known and widely used catalysts in proton-exchange membrane fuel cells (PEMFCs), particularly hydrogen-powered PEMFCs, in which Pt remains the preferred catalyst at both the anode and cathode [21]. On the anode, Pt catalyzes the electro-oxidation of formic acid via a dual-pathway mechanism (dehydrogenation and dehydration) or, as recently proposed, a triple-pathway mechanism that adds the HCOO− pathway to the dual-pathway mechanism as an additional reaction [22]. The direct pathway (dehydrogenation) generates hydrogen and carbon dioxide and is preferred for Pt-based catalysts. The second, indirect pathway (dehydration) produces CO, which severely degrades the performance of Pt-based catalysts. CO poisoning results from the strong binding of CO to Pt. Because CO adsorbs strongly on Pt atoms, it is difficult to remove at low potential, blocking active sites for hydrogen adsorption and subsequent oxidation. Another relevant factor is that the strength of CO adsorption on Pt-based catalysts is inversely proportional to temperature. However, practical exploitation of this effect is hindered by the relatively low operating temperature of DFAFCs.
At low temperatures, trace amounts of CO can have considerable detrimental effects on fuel cell performance [23]. The importance of CO concentration is underscored by International Organization for Standardization (ISO) standards, which require the CO concentration in H2 for fuel cell vehicles to be less than 0.2 ppm [24], reflecting the negative impact of CO on the catalyst. To put this into perspective, the literature indicates that exposure to 100 ppm CO can reduce the steady-state current density of a conventional pure Pt anode by up to 75%, from 400 mA/cm2 to just 100 mA/cm2 at 0.7 V [25]. One strategy for reducing overall CO coverage and weakening CO adsorption on Pt-based catalysts is to develop single-atom Pt site catalysts. This approach modifies the geometry and electronic properties of the catalysts, thereby reducing CO adsorption and improving catalyst performance [26].
The first notable catalyst reviewed in this paper is Pt-FeTSPc [27]. The authors demonstrated an innovative approach using iron (II) tetrasulfophthalocyanine (FeTSPc) as an environmentally friendly material to improve the FAO by inhibiting self-poisoning and enhancing intrinsic catalytic activity. This, in turn, results in a higher electro-oxidation current in the fuel cell. The approach involved modifying the existing Pt-based anode by pumping a 4 µg/mL FeTSPc solution through the anode channels for 2 h, followed by rinsing with 0.5 M H2SO4 and water.
The single-cell test was conducted at 60 °C without back pressure. The anode was fed with 6 M FA using a peristaltic pump at a flow rate of 1 mL/min. The cathode was supplied with 100 mL/min of dry pure oxygen. Catalyst loadings were 0.5 mg/cm2 for the anode and 1.5 mg/cm2 for the cathode. The MEA was prepared according to [28], and its geometry is illustrated in Figure S1 (Supplement Materials).
This article demonstrates that FeTSPc effectively promotes FA electro-oxidation, showing that performance can be enhanced using environmentally friendly materials that are inexpensive, easy to synthesize, stable, and water-soluble. In addition, the catalyst concentration is low compared with standard catalyst loadings for DFAFCs, further supporting its commercial viability.
Figure S2 presents the cyclic voltammograms of Pt electrodes modified with FeTSPc. Bare carbon modified with FeTSPc showed no catalytic activity toward the FAO reaction, indicating that FeTSPc acts not as a catalyst but as a promoter of Pt catalytic activity. Notably, the FeTSPc concentration was 0.1 mg/mL for the Pt electrode immersed in the FeTSPc solution.
Two peaks are visible in the anodic forward scan of the pristine Pt catalyst, confirming a dual-pathway mechanism. The first peak (Peak A), observed at 0.397 V with a current density of 2.62 mA/cm2, corresponds to the direct oxidation of FA via active intermediates. The second peak (Peak B), observed at 0.74 V with a current density of 5.58 mA/cm2, is due to the oxidation of adsorbed carbon monoxide [27].
For the Pt electrode modified with adsorbed FeTSPc, cyclic voltammetry reveals a FAO peak (Peak 1) at 0.404 V with a current density of 21.95 mA/cm2, representing an 8.38-fold increase in performance compared with pristine Pt. Furthermore, the onset potential of the modified catalyst decreased from −0.01 to −0.13 V. This suggests a novel approach to modulating the reaction pathways of active intermediates.
Although a small “shoulder” indicated some residual poisoning, it is hypothesized that this behavior can be mitigated through prolonged Pt treatment and higher FeTSPc concentrations. To test this hypothesis, the electrode was evaluated in a mixture containing 0.1 mg/mL FeTSPc, with the addition of 1 M HCOOH and 0.5 M H2SO4. The CV results are shown by the dashed line. This measurement revealed a single peak at 0.405 V with a current density of 25.25 mA/cm2 (Peak 2), representing a 9.64-fold improvement over the pristine Pt catalyst. The resulting bell-shaped curve in the forward scan is a novel observation in CV measurements of DFAFC catalysts and demonstrates that FeTSPc treatment of Pt efficiently inhibits poison species and enhances catalyst activity for FAO by suppressing CO formation.
In addition to suppressing CO poisoning, the catalytic activity of the Pt electrode was enhanced, as measured by double-potential-step chronoamperometry. This is demonstrated by the modified Pt electrode’s higher activity than that of bare Pt in the absence of intermediate poisoning, indicating a reduction in the required activation energy. These results are illustrated in Figure S3, which shows current density–time profiles for HCOOH oxidation in 0.01 M HCOOH + 0.5 M H2SO4, with the oxidation potential varying from 0 to 0.9 V, for Pt with adsorbed FeTSPc (left) and pristine Pt (right).
The resulting polarization curves for the pristine Pt and treated Pt catalysts, obtained using a single-cell experimental setup, are shown in Figure S4. Notably, the measured cell potential was not compensated for series resistance (iR-compensation).
As a result, FeTSPc-treated Pt achieved a peak power density of 126.6 mW/cm2, whereas pristine Pt achieved a peak power density of 76.3 mW/cm2. A comprehensive overview of the pure and treated catalysts is presented in Table S1. The data were extracted directly from Figure S4, so minor measurement errors may be present.
The novel FeTSPc-treated Pt catalyst shows promise for reducing catalyst loading and mitigating CO poisoning. To gain a broader perspective on its long-term viability, prolonged performance-degradation tests should be conducted. These tests were beyond the scope of this paper and remain a subject for potential future research.
A well-defined, high-performance PtBiPbNiCo high-entropy alloy (HEA) catalyst with a hexagonal nanoparticle (HP) morphology was developed in [29]. This catalyst consists of a PtBiPb medium-entropy core and a PtBiNiCo high-entropy shell. It was prepared by wet-chemical synthesis using lead(II) acetylacetonate, bismuth subcarbonate, platinum(II) acetylacetonate, basic nickel(II) carbonate, and basic cobalt(II) carbonate as metal precursors. Oleylamine and 1-octadecene served as solvents, and L-ascorbic acid was used as the reducing agent. Experimental results demonstrate that this HEA catalyst can achieve a power density of 321.2 mW/cm2 when used for FAO, representing one of the highest power densities for DFAFCs to date. Furthermore, theoretical and experimental analyses show that this catalyst’s core and shell compositions promote the direct dehydrogenation pathway, thereby greatly inhibiting CO production and significantly reducing CO poisoning.
This article demonstrates that HEAs offer a promising catalyst-design pathway for FAO, with high power density and the ability to inhibit CO production and poisoning, even at this early stage of research. Their potential lies in elemental diversity and structural tunability, which could open a new area in which HEA catalysts have electronic and structural properties that differ drastically from those of conventional alloys. The most widely used industrial techniques for preparing HEAs are magnetron sputtering, mechanical alloying, and high-temperature metallurgy, which yield commercial, mass-produced materials. With advances in nanotechnology and nanoscience, various methods have been developed to produce HEA nanoparticles. For this HEA HP production, a wet-chemical synthesis process was used [30].
Merging several components into a stable solid solution remains a complex process, and successfully achieving this through structural control is a notable merit of the article. This novel catalyst achieved a high power density of 321.2 mW/cm2 and improved CO resistance. Its decay was 55.1% over 30 h, compared with 97.6% for the Pd/C catalyst over the same period. Figure 2 shows the catalyst performance decay, a comparison of polarization curves, and the mass activity of HEA HPs/C compared with that of other catalysts.
Figure 2. Polarization curve of HEA HPs/C and commercial Pd/C (upper left); performance decay curves of HEA HPs/C and commercial Pd/C at 0.4 V (upper right); and comparison of the mass activity of HEA HPs/C with that of different FAO reaction catalysts (bottom). Reproduced with permission from [29], © 2022 John Wiley and Sons.
The testing conditions were 80 °C, with 0.5 M H2SO4 and 0.5 M HCOOH on the anode side and 100% RH oxygen on the cathode side, at 100 kPa back pressure; the flow rates were unknown. The main data are extracted and presented in Table S2.
The PtBiPbNiCo catalyst has shown outstanding performance, with a maximum power density that significantly surpasses those of competing catalysts. However, a full assessment of this catalyst is limited by the lack of detailed information on its preparation, which is necessary to evaluate the complexity of its synthesis and compare it fairly with alternative catalysts. Furthermore, although CO poisoning was reduced, it was not eliminated. The durability test should also be extended to enable a better evaluation of the catalyst’s long-term stability and commercial viability.
In [3], the in situ growth of ultrathin PtCu alloy nanowire arrays directly on carbon-paper gas diffusion layers (GDLs) was investigated for DFAFC applications. The goal was to prepare and grow PtCu nanowire (NW) arrays as a catalyst under surfactant-free, room-temperature conditions. Precise regulation of the ions during the formation and crystallization of Pt and Cu enabled the synthesis of alloy nanowires with a median diameter of 4 nm. These PtCu NW gas diffusion electrodes (GDEs) were prepared using a template- and surfactant-free formic acid reduction method at room temperature, adapted from [31]. Initially, the GDL was immersed in an aqueous solution containing HCOOH and H2PtCl6 for 6 h, after which CuCl2 solution was added and the reaction continued for a further 90 h at room temperature. The resulting electrode was washed with isopropyl alcohol and deionized water and dried at 40 °C.
This approach demonstrates that a GDE can be prepared in a one-step process using a metal precursor and a gas diffusion layer (GDL). It enables the direct integration of the GDE with the membrane by hot pressing, unlike conventional wet-chemical methods, in which the catalyst is prepared separately and then dispersed as a catalyst ink. Growth required around 96 h. Figure 3 illustrates the growth process of PtCu NW crystals on the GDL, together with the polarization and power curves obtained for different PtCu configurations.
Figure 3. Schematic illustration of PtCu NW arrays on the GDL surface used to fabricate a PtCu NW GDE (top), and (a) polarization (bottom left) and (b) power density (bottom right) curves for different PtCu catalyst configurations at a testing temperature of 75 °C [3]. Creative Commons CC BY-NC-ND 4.0.
Different amounts of Pt and Cu precursors were used to synthesize anodes with different PtCu ratios while maintaining a constant total metal loading. The electrodes were designated as follows: Pt NW GDE (2.0 mgPt/cm2), Pt5Cu1 (1.88 mgPt/cm2 + 0.12 mgCu/cm2), Pt3Cu1 (1.8 mgPt/cm2 + 0.2 mgCu/cm2), and Pt1Cu1 (1.5 mgPt/cm2 + 0.5 mgCu/cm2). A commercial GDE with a Pt loading of 2 mg/cm2 was used as the cathode.
After the catalyst layer was grown on the GDL, Nafion DE 1021 in an IPA solution at a volume ratio of 1:2 was applied to the GDE (Nafion loading at 1.2 mg/cm2) and dried under an infrared lamp for 2 h. The active area of the MEA was 4 cm2. The MEA was fabricated by hot-pressing the anode and cathode GDEs onto Nafion 212 at 135 °C under a pressure of 4.9 MPa for 2 min. Two Teflon gaskets, each with a thickness of 254 µm, were used to seal the anode and cathode compartments.
The DFAFC performance was evaluated using 3 M HCOOH at a flow rate of 1 mL/min at the anode and dry air at a flow rate of 300 mL/min at the cathode, without backpressure, at a temperature of 75 °C.
The PtCu combination has been shown to promote the direct FAO pathway by optimizing the electrode structure and leveraging the third-body effect. Specifically, Cu atoms prevent the formation of large Pt clusters and promote better dispersion of Pt within the structure, with the primary goal of achieving single-atom Pt sites. This is important because the indirect FAO pathway requires at least two adjacent Pt atoms to be in contact with a formic acid molecule. The polarization and power density curves at the bottom of Figure 3 reveal significant variations in catalyst performance according to the concentrations of Pt and Cu, with Pt3Cu1 achieving the highest power density. A detailed comparison of these catalyst compositions is presented in Table S3.
This paper presents a comprehensive overview of a novel in situ growth method that enables the direct growth of catalysts on the GDL. This method offers two main advantages: precise control of catalyst composition and uniform catalyst distribution across the GDL. These advantages result in a 2.4-fold increase in power density for Pt3Cu1 compared with pristine Pt. However, this approach has three main challenges. First, catalyst growth on the GDL requires more than 96 h. Second, catalyst growth is limited to the GDL and is not performed directly on the PEM, limiting the potential for direct catalyst incorporation into the PEM. Lastly, the catalyst is coated with Nafion ionomer at the end of the process, which can cover active sites and consequently reduce the catalyst’s active area. The effect of active-site blockage is significantly increased by the Nafion coating, which has a thickness of 1.2 mg/cm2. This is an unusually high Nafion loading on the catalyst, particularly when the ionomer is coated on top of the catalyst (on the side exposed to formic acid). Based on these conclusions, a starting point for further improving overall performance would be to evaluate different Nafion loadings on the GDE. Optimizing this parameter could drastically increase the power output of the GDE.
In [32], the results for PtRu and PtAu catalysts are presented. Figure 4A shows polarization curves for 6 M HCOOH at the anode and oxygen at the cathode at a testing temperature of 30 °C. The long-term performance of the PtRu and PtAu catalysts is shown on the right. The catalysts were synthesized using the borohydride reduction method to achieve a 1:1 atomic ratio of Pt to Ru and Au.
Figure 4. Single-cell performance of PtAu- and PtRu-based catalysts with 6 M HCOOH and oxygen at 30 °C (A), and changes in cell voltage for PtAu- and PtRu-based MEA during a 500 h lifetime test at 100 mA/cm2 and 60 °C (B). Data were approximately digitized from the published experimental plots and replotted independently. Lines connect the extracted points.
An overview of the performance of the PtAu and PtRu catalysts is shown in Table S4.
Finally, Bi-modified commercial 40 wt% Pt/C was investigated in half-cell, single-cell, and stack tests in [33]; the latter two configurations are particularly relevant to this review. Commercial 40 wt% Pt/C was surface-modified by irreversible adsorption of Bi3+ from a 5 mM Bi3+ solution in 0.5 M H2SO4 for 48 h, followed by washing and NaBH4 reduction for 30 min. Both the single cell and the 35-cell DFAFC stack were operated at 60 °C. The single cell had an active area of 5 cm2, with anode and cathode catalyst loadings of 1.2 mg BiPt cm−2 and 3 mg Pt cm−2, respectively. TGP-H-060 and SGL 10BC were used as gas-diffusion-layer materials. The anode was supplied with 6 M HCOOH at 5 mL min−1, while the cathode received humidified air at 500 mL min−1. The stack used the same catalyst loadings, an active area of 50 cm2 per cell, and reactant flow rates ten times those used in the single-cell tests. The single cell achieved a maximum power density of 191 mW cm−2, whereas the 35-cell stack delivered a peak power output of 300 W.
The summary of all Pt-based catalysts mentioned in this chapter is shown in Table 2.
Table 2. Overview of all researched Pt-based catalysts.
Pristine Pt offers limited promise for DFAFCs compared with Pd. However, this review has shown that Pt can remain an interesting catalyst when modified or alloyed. All Pt-based catalysts considered, except PtRu, showed increased maximum power density.
HEAs represent a promising alternative to classic catalyst design approaches. To the best of our knowledge, PtBiPbNiCo achieves the highest power density reported to date for Pt-based catalysts (321.2 mW/cm2), with reduced catalyst degradation. However, this catalyst has not yet demonstrated adequate long-term stability, which remains a challenge for future research. From a durability perspective, the most promising catalyst combination reviewed here is Pt treated with FeTSPc, as it successfully inhibits CO generation. Aside from the previously mentioned complete direct pathway of FAO, this catalyst offers the additional benefit of relative ease of production compared with PtBiPbNiCo. The main limitation of Pt with FeTSPc, and a focus for future work, is the lack of long-term stability testing, which should confirm the complete inhibition of CO generation. The in situ growth of the PtCu catalyst on the GDL represents a novel application of the catalyst, in which catalyst growth together with the addition of a non-noble metal offers an interesting approach. The paper quantified the influence of different Pt and Cu compositions on peak power density. This parameter should be further addressed when testing novel DFAFC catalysts in general. Finally, adding a Nafion coat after catalyst growth is complete is identified as a drawback; however, this catalyst yielded significant results even with a Nafion loading of 1.2 mg/cm2. For this type of catalyst application, the Nafion loading could potentially be drastically reduced to increase the active area and, consequently, catalyst performance, particularly because different Nafion loadings would have different effects on the influence of Cu on Pt. PtRu and PtAu have shown low degradation during DFAFC operation, but adding another noble metal to Pt drastically increases the catalyst price. The peak power density does not justify this price increase, as these combinations are not competitive with the high-end catalysts reviewed in this paper. Bi-modified 40 wt% Pt/C demonstrated promise for DFAFC scale-up, enabling a 35-cell stack to achieve a peak power output of 300 W. This result supports its potential for further development of practical DFAFC systems.

2.2. Palladium-Based Catalysts

Palladium-based catalysts are considered among the most effective catalysts for FAO, alongside Pt. Palladium is preferred for FAO in DFAFCs because it promotes the direct reaction pathway, resulting in better long-term activity than Pt [34]. The indirect pathway is remarkably difficult to detect on Pd electrodes, primarily because of the high surface coverage by HCOO−. This dense formate layer blocks the ensemble active sites required for the dehydration reaction and prevents CO species from adsorbing, while simultaneously driving the reaction through dehydrogenation. Thus, Pd is a preferred catalyst despite its high binding affinity for CO. The possibility of further enhancing the site-blocking effect also provides an alternative strategy to that used with Pt for designing highly efficient FAO catalysts [35]. Although these mechanisms inhibit poisoning, CO is still considered the primary cause of catalytic decay. This indicates that COads can be generated and adsorbed on the catalyst’s active areas through pathways other than the standard dehydration of formic acid.
As demonstrated in [36,37], the reaction of CO2, the final product of FAO, has been proposed to undergo reduction to generate COads. Further studies have shown that COads accumulation is promoted at lower potentials, particularly at the open-circuit potential (OCP), which can significantly contribute to the decay in Pd catalyst activity. Because the poisoning process is reversible, bonded COads can be oxidized back to CO2 and removed by applying a higher potential [38,39,40]. Alternatively, the catalyst can be regenerated by water flushing; however, frequent regeneration cycles limit the practical and commercial viability of DFAFC systems. Attenuated total reflection-IR spectroscopy has shown that alloying can mitigate COads through the ensemble effect. For example, in intermetallic PdBi(O-PdBi), the ordered atomic arrangement could effectively hinder the formation of 3-fold hollow COads (COT) and facilitate its removal. Both COT and bridged COads (COB) were observed on pure Pd, which possesses continuous sites [41]. This results in enhanced CO tolerance on the catalyst. In [42], hydrazine treatment of presynthesized Pd nanocubes was used to prepare a series of PdHx with different hydride contents to investigate their FAO performance. Density functional theory calculations showed that the hydride degree modulates the relative stability of carboxyl (COOH*) and HCOO− intermediates, thereby affecting the selectivity of the different FAO reaction pathways. PdHx with the highest hydride content exhibited the highest selectivity toward the direct pathway, consistent with its high activity and stability.
Studies have demonstrated that unsupported Pd (Pd black)-based DFAFCs exhibit unusually high power density at ambient temperatures. To further improve performance, the authors of [43] synthesized finely deposited Pd particles on carbon supports (Vulcan XC-72) and studied the performance of 20 and 40 wt% Pd/C. Carbon-supported Pd and Pd–Au catalysts were prepared by chemically reducing metal chloride precursors in the presence of acid-pretreated Vulcan XC-72 carbon. The support was treated with concentrated HCl for 12 h and washed with ultrapure water. The precursor quantities were then adjusted to obtain the desired metal loadings of 20 or 40 wt%.
The experimental setup used an MEA with an active area of 5 cm2. The catalyst was applied directly to the Nafion 112 membrane using a painting technique. The total catalyst loading on the anode was 6 mg/cm2, including 2.4 mg/cm2 of Pd black, and the cathode loading was 8 mg/cm2 of unsupported Pt black. The anode catalyst was tested in two configurations: one with carbon-supported Pd and the other without it. Teflon-coated carbon cloth was used as the diffusion layer/gas diffusion layer for both the anode and cathode. The single-cell fixture consisted of machined graphite flow fields with direct liquid feeds and gold-plated copper current collectors. Carbon-supported catalysts were prepared using a metal chloride reduction process taken from [44] and additionally described here.
Cell conditioning was performed at 60 °C in H2/Air fuel cell operating mode for 2 h at a cell potential of 0.6 V. The H2 flow rate was set to 200 mL/min, and the gas was humidified at 70 °C before entering the fuel cell, with a back pressure of 20 psi. Finally, fuel cell operation and polarization measurements were conducted using different concentrations of formic acid. The anode flow rate was 1 mL/min, while dry air was supplied to the cathode at a flow rate of 390 mL/min without back pressure. For the potentiostatic test at 0.39 V, 3 M HCOOH was fed to the anode at the same flow rate as previously mentioned. For the polarization curve measurement, dry air was supplied to the cathode at the same flow rate and without back pressure. The measured results are shown in Figure 5. The polarization curves for different wt% of Pd and Pd black are shown on the left, and the corresponding power density curves for different wt% and Pd black are shown on the right.
Figure 5. Polarization curves (A) and power curves (B) for different Pd/C concentrations and Pd black; polarization plots of currents normalized by the total weight of the Pd metals at the anode (C); and power density as a function of formic acid feed concentration from 3 M to 20 M at 0.39 V cell potential (D), at an operating temperature of 30 °C. Data were approximately digitized from the published experimental plots and independently replotted. Lines connect the extracted points.
The peak power densities were 146 mW/cm2 for 20 wt% Pd/C, 171 mW/cm2 for 40 wt% Pd/C, and 243 mW/cm2 for Pd black. Additionally, polarization curves were measured for the specific weight of Pd, as shown in the lower-left part of Figure 5. The power density as a function of the formic acid feed concentration at a potential of 0.39 V is plotted in the lower-right part of the same figure.
The data from this study are summarized in Table S5.
Pd black has shown promising results, but the evaluation reveals a critical architectural mismatch: the same GDL is used at the anode and cathode. While a Teflon-coated GDL effectively mitigates water flooding at the cathode, it can substantially impair performance when liquid fuels such as formic acid are used because Teflon introduces an adverse capillary barrier that severely restricts reactant mass transport to the catalyst active sites. Consequently, maximizing the potential of unsupported catalysts like Pd black requires an asymmetric electrode design that favors a more hydrophilic anode GDL to ensure uniform fuel infiltration and lower concentration overpotentials. Following the approach of [43], the authors in [45] expanded the investigation by employing two additional catalysts and measuring their performance. The first was a Pd black catalyst, and the second was a 20 wt% PdAu (50 atoms of Pd to 1 atom of Au ratio) catalyst on VulcanXC-72 carbon made in house. Catalyst preparation followed the same process as in the previous paper. The only difference from the previous work in the fuel concentrations and flow rates at the anode and cathode was that the formic acid concentration was 5 M for constant-voltage tests, compared with the previously used concentration of 3 M. Additionally, transmission electron microscopy imaging of the Pd catalysts was performed.
The 20 wt% Pd on carbon consists of Pd nanoparticles with an average size of 3–10 nm, although a few reach 30 nm. Some nanoparticles are significantly agglomerated, whereas others remain isolated. The nanoparticles in PdAu on carbon and 40 wt% Pd on carbon are similar in size, but those in PdAu on carbon appear to be less agglomerated than the pure Pd nanoparticles on carbon. The Pd nanoparticles in 40 wt% Pd on carbon are even more agglomerated than those in 20 wt% Pd on carbon. High surface area Pd black (Sigma–Aldrich) has a filamentous structure with a high degree of void space, whereas low surface area Pd black from Alfa Aesar consists of large chunks with rough surfaces and Pd particles exceeding 100 nm in size. Additionally, chronoamperometric activity tests were conducted over time for the catalysts, considering total catalyst weight, Pd weight, and electrochemically active catalyst surface area. The most significant results are those for time-dependent catalyst activity, shown in Table 3.
Table 3. Chronoamperometric activity of a Pd catalyst in air-exposed 5 M HCOOH/0.1 M H2 SO4 at 0.3 V vs. RHE derived from [45].
Polarization and power density curves were also measured for each evaluated catalyst, and the results are shown in the bottom part of Figure 6.
Figure 6. Polarization (A) and power density curves (B) for DFAFCs with various Pd anode catalysts, operated with dry air at 30 °C and 5 M HCOOH. Data were approximately digitized from the published experimental plots and replotted independently. Lines show shape-preserving interpolation between estimated data points.
Since the 20 wt% and 40 wt% Pd/C catalysts were described in a previous study, they have been excluded from Table S6, which provides an overview of the maximum power densities of the additional catalysts investigated in this paper.
HS area Pd black (Sigma-Aldrich) has shown slightly higher performance than Pd black, although the difference is almost negligible. If varying the catalyst composition and dimensions is the main goal, a further route to achieving higher current densities is to use a different anode diffusion layer. This could potentially boost performance and demonstrate that simple Pd catalysts can achieve even higher current densities than 254 mW/cm2.
The [46] article incorporated nickel phosphide (Ni2P) nanoparticles to produce the novel Pd-Ni2P/C catalyst, which demonstrated very high catalytic activity. Ni2P/C particles were synthesized by solid-phase reaction. Pd was deposited onto Ni2P/C using a microwave-assisted ethylene glycol reduction method, as described in the article’s supporting material. Anti-poisoning tests were conducted, and Pd- Ni2P/C (30 wt% Ni2P/C) showed the highest negative maximal potential, indicating that this catalyst had the best anti-poisoning ability. The activities of catalysts containing different weight percentages of Ni2P/C are shown in Figure S5 as cyclic voltammograms. The test solution contained 0.5 M H2SO4 and 0.5 M HCOOH.
As shown in Figure S5, pristine Ni2P has almost no catalytic activity, yet it significantly influences Pd performance. The cyclic voltammograms show that Pd-Ni2P/C-30% exhibits the highest catalytic activity, particularly at the catalyst’s peak potential. This is probably attributable to reduced passivation of the Pd sites. Additionally, Ni2P was found to be an effective hydrogen evolution catalyst [47], which could potentially enhance the kinetics of the FAO reaction.
To demonstrate the potential of the Pd-Ni2P/C catalyst, it was incorporated into the anode of a custom-built fuel cell. The polarization and power-density curves of several catalysts were compared. The discharge curves at a potential of 0.35 V are also presented together in Figure 7.
Figure 7. Steady-state polarization curves (A), power density curves (B), and discharge curves at 0.35 V (C) for Pd-Ni2P/C-30%, PdNi/C, PdP/C, and Pd/C-C as anode catalysts in a DFAFC, with 3 M HCOOH at the anode and O2 at the cathode, at 30 °C [46]. The figures were used with permission from Wiley.
The flow rates for the experiment were 200 mL/min at the anode and 500 mL/min at the cathode.
Pd-Ni2P/C-30% has exhibited significantly higher catalytic activity, as evidenced by the lowest Tafel slope, the highest current density in the ohmic resistance region of the chart, and a peak power density of 550 mW/cm2. This performance is approximately twice as high as that of PdNi/C, three times higher than that of PdP/C, and 3.5 times higher than that of the state-of-the-art Pd/C catalyst. These results represent a significant advancement in catalytic activity and the overall development of the field of DFAFCs.
Table S7 provides an overview of catalyst performance in this study.
To date, among the Pd-based catalysts, Pd-Ni2P/C-30% is the most promising, exhibiting the highest power density and promising durability for implementation in commercial DFAFCs. The results for Pd-based catalysts thoroughly reviewed in this study are presented in Table 4, whereas results for other Pd-based catalysts available in the literature are presented in Table 5.
Table 4. Summary of different Pd-based catalysts listed in Tables S5–S7.
Table 5. Summary of different Pd-based catalysts in the literature.
An alternative route to durable, low-loading Pd anodes was demonstrated in [48], where the Au-stabilized nanoporous PdCuAu ternary alloy has been developed. The catalyst was prepared on a nanoporous gold substrate obtained by dealloying 100 nm thick Au50Ag50 leaves in concentrated nitric acid, after which Cu (~6 µg/cm2) and Pd (~10 µg/cm2) layers were sequentially electrodeposited and thermally treated at 270 °C for 30 min in an Ar–H2 atmosphere, forming a ~2 nm PdCuAu alloy shell on the gold ligaments. The design combines two complementary stabilization mechanisms: Cu provides surface-adsorbed hydroxyl groups at low potentials that remove adsorbed CO through a bifunctional mechanism, while Au suppresses the dissolution of both Pd and Cu and shifts the d-band center of Pd away from the Fermi level, lowering the calculated CO adsorption energy.
The practical relevance of this architecture was confirmed in single-cell DFAFC tests. Membrane electrode assemblies were fabricated with Nafion 115 and a commercial Pt/C cathode (2 mg Pt/cm2), with the nanoporous film anodes attached directly to the membrane; the cell was operated at 80 °C with 3 M formic acid supplied to the anode at 1.0 mL/min and oxygen to the cathode at 200 mL/min. The PdCuAu anode achieved a peak power density of 93.2 mW/cm2 at a Pd loading of only 0.01 mg/cm2, compared with 70.9 mW/cm2 for the Pd-only nanoporous reference, 47.5 mW/cm2 for PdCu (which degraded through Cu leaching), and 60.3 mW/cm2 for a commercial Pd/C anode loaded with 1.2 mg/cm2 under identical conditions. Although the absolute power density is moderate relative to the high-loading Pd systems in Table 5, the Pd mass efficiency is roughly two orders of magnitude higher than that of the Pd/C reference (about one order of magnitude when the ~0.1 mg/cm2 of Au in the substrate is included), which directly demonstrates that the reduced-loading target proposed in Section 2.5 is experimentally attainable.
Pd has significant potential as a catalyst in DFAFCs, delivering high power density even when combined only with carbon black. By promoting HCOO− intermediates, Pd favors the direct dehydrogenation pathway, thereby mitigating immediate poisoning and enhancing durability. However, CO poisoning remains the main cause of Pd catalyst deactivation; CO is produced through CO2 reduction, particularly at the open circuit potential (OCP) and lower operating potentials. Research suggests that ordered atomic arrangements can address this issue. Another challenge is the high Pd catalyst loading of 4 to 8 mg/cm2, compared with the typical loading of only 0.5 to 3 mg/cm2 for Pt-based catalysts in DFAFC systems. Although the price per gram of raw palladium has historically been competitive with that of platinum, the 3- to 8-fold higher mass loading required per unit area for Pd effectively eliminates this material-cost advantage, resulting in a substantially higher net financial investment for the final device [57]. To the best of our knowledge, the Pd-Ni2P/C-30% catalyst has demonstrated the highest power density among the catalysts researched to date (550 mW/cm2). The Ni2P ratio critically affects catalyst performance. It is important not only to combine different additives with a catalyst but also to study different ratios of the catalyst and additives in the composition to ensure optimal catalyst activity. This raises the question of whether optimizing the ratios of different catalysts could improve their performance. Although this catalyst is more durable than regular Pd/C, a four-hour durability test showed that it remains susceptible to CO poisoning over the long term. In general, durability tests for other Pd-based catalysts have been shorter or nonexistent, a critical deficit that future research should address by standardizing testing to better understand catalyst durability and power decline. This assessment is crucial for evaluating the commercial viability of novel electrocatalysts. Because these materials can be regenerated via water flushing or periodic potential stepping, catalysts with low degradation rates offer a viable strategy for mitigating poisoning in specialized DFAFC applications. This could ultimately provide higher energy density than battery systems and extend operational autonomy in electric systems where conventional internal combustion engines are unfeasible. Finally, systematic analysis reveals that conventional hardware, such as the anode diffusion layer, is incompatible with the liquid nature of formic acid. To fully unlock the electrochemical potential of Pd-based FAO, future testing protocols should mandate catalyst benchmarking using hardware specifically optimized for liquid-phase mass transport.

2.3. Non-Noble Metal Catalysts

The oxygen reduction reaction (ORR) is one of the most demanding electrocatalytic reactions in terms of material selection. Although the acidic environment of a PEMFC favors the reaction, it also creates a high oxidizing potential, resulting in extremely aggressive conditions that most metals cannot withstand without significant degradation. This is the main reason for using platinum-based catalysts supported on materials with high electrical conductivity. However, platinum also degrades during long-term PEMFC operation. To address these challenges, Pd-based catalysts can be improved, particularly through catalyst nanostructuring and alloying [58,59]. Catalyst stability is an even greater concern when non-noble-metal catalysts are used. Consequently, because of their competitive electrocatalytic activity toward the oxygen reduction reaction and their inefficiency toward hydrogen oxidation, non-noble-metal catalysts are currently considered exclusively for the cathode side in DFAFCs [60].
The first non-platinum catalyst, cobalt phthalocyanine, was developed by Jasinski in 1964, who reported its oxygen reduction activity in alkaline media [61]. This pioneering work laid the foundation for the development of numerous non-noble metal catalysts. In recent years, interest in non-noble metal catalysts has increased because they offer a sustainable and cost-effective alternative to noble metal catalysts in organic synthesis and electrochemistry [62]. Among the most promising platinum metal-free (PMF) catalysts with the potential to replace Pt in the cathode catalyst layer (CCL) are the so-called M-N-C (metal-nitrogen-carbon) catalysts, a type of single-atom catalyst. Within this class, first-row transition metals, especially Fe, have gained significant interest [63,64]. The Fe2+ ion coordinated by four nitrogen atoms within the graphenic carbon structure is considered the most attractive non-precious Fe-N-C catalyst for acidic conditions [65]. Furthermore, nitrogen doping is considered indispensable for achieving high catalytic activity under acidic conditions [66]. M-N-C catalysts are considered most catalytically active when the metal atom is coordinated to four nitrogen atoms within a carbon matrix. In addition to the structure of these active sites, long-range order is a second key parameter because it plays a crucial role in electrical conduction and diffusion. Fe-N-C catalysts supported on reduced graphene oxide have been found to benefit from the interlayer distance between the graphene oxide sheets, which improves oxygen diffusivity compared with purely graphitic structures [67]. Because iron exhibits the highest catalytic activity among all non-noble metals, it is the most widely used metal in M-N-C catalysts. Nickel, copper, cobalt, chrome, manganese, and vanadium are also employed.
Experimental testing of DFAFCs using non-precious catalysts is scarce; however, relevant studies can be found, such as in [68]. For this reason, this review compares the use of non-noble metal catalysts in DFAFCs and DMFCs. The cathode reaction in DFAFCs is comparable to that in DMFCs, which have been more extensively researched; therefore, improvements to DMFC cathodes could potentially be applicable to the DFAFC cathode catalyst layer [69].
The paper discussed for non-noble metal catalysts is [68]. In this study, nitrogen-doped carbon nanotubes (NCNT) were used in Fe-NCNT and Co-NCNT cathode catalysts. The results showed that higher power density than that of the well-known Pt/C catalyst, which had a peak power density of 128.9 mW/cm2, could be achieved with Co-NCNT, which had a peak power density of 160.7 mW/cm2. Fe-NCNT had a peak power density of 94.9 mW/cm2. Previous studies in this field focused mainly on DAFCs. These studies examined cathode catalysts derived from aminobenzimidazole and aminoantipyrine [70], nicarbazin [71], four different carbonaceous supports, among which Fe-N-MPC performed best, and Fe-N with mesoporous silica nanoparticles as the carbon support [72], as well as Fe- or Co-supported N-doped carbon aerogels [73]. A summary of these catalysts is presented in Table S8.
Fe, Co-NCNT, and transition metal-N-doped carbon nanotube (TM-NCNT) catalysts were synthesized by simple pyrolysis from a low-cost precursor, following a previously conducted study [74]. To compare the performance of Fe-NCNT and Co-NCNT catalysts with that of a commercial Pt/C catalyst, a formic acid tolerance test was conducted in a single-cell DFAFC with a Pt/C cathode catalyst.
For single-cell fabrication, MEAs were prepared with a commercial Pd/C anode catalyst, while Fe-NCNT and Co-NCNT were used as cathode catalysts. The catalyst layers were applied by ultrasonic spraying [75]. A schematic of the catalyst application process is shown in Figure S6.
The anode was prepared by coating plain carbon cloth with a commercial Pd/C catalyst ink (5 wt% Nafion, isopropyl alcohol, and water). The cathode catalyst ink was sprayed onto carbon paper, with loadings of 4.6 and 3.3 mg/cm2 for Fe-NCNT and Co-NCNT, respectively. A commercial Pt/C cathode electrode with a Pt concentration of 2 mg/cm2 was used as the reference MEA, with an ionomer content of 50 wt% of the catalyst loading on both sides.
To fabricate the MEA, the anode and cathode electrodes with diffusion layers were hot-pressed with a Nafion 212 membrane between them at 140 °C and 5 MPa for 3 min. The active area of the MEA was 4.84 cm2. Silicone gaskets with a thickness of 20 µm were used to prevent potential leakage on the anode side. Gaskets with thicknesses ranging from 150 to 350 µm were used on the cathode side, depending on the electrode thickness. A FC-05-02-H2R fuel cell (ElectroChem, Inc. in Woburn, Massachusetts, MA 01801, USA) was used for full-cell testing. Before performance testing, the cells were pretreated with humidified hydrogen supplied to the anode and dry oxygen supplied to the cathode. For DFAFC pretreatment, the MEAs were operated at 60 °C with a 5 M formic acid solution at the anode and dry oxygen flowing at 500 mL/min at the cathode to prevent flooding of the cathode channels. For DFAFC performance testing, formic acid concentrations of 3, 5, 7 and 10 M were used at the anode, with a flow rate of 5 mL/min, and oxygen flow rates of 300, 500, 700 mL/min were used at the cathode. Tests were conducted at two temperatures, 30 and 60 °C. Fresh water was fed to the anode between each test to wash the anode surface and eliminate catalyst poisoning by the formic acid solution. The washing process was stopped once the cell voltage dropped to 0.1 V. The authors stated that the anode performance could be recovered to its initial level through this regeneration process [40,76].
The detailed polarization and power curves for Co-NCNT at 30 °C are presented in Figure 8, while those at 60 °C are presented in Figure 9.
Figure 8. Polarization curves at different fuel concentrations and flow rates: (A) 300 mL/min, (B) 500 mL/min, and (C) 700 mL/min at 30 °C [68]. Reproduced with permission from Wiley.
Figure 9. Polarization curves for different fuel concentrations at flow rates of (A) 300 mL/min, (B) 500 mL/min, and (C) 700 mL/min at 60 °C [68]. The figures were used with permission from Wiley.
Table S9 provides a numerical overview of the peak power densities reported for these results.
The Fe-NCNT cathode catalyst yielded lower results, with the highest overall power density for the DFAFC reaching 71.5 mW/cm2 when dry oxygen was supplied at a flow rate of 500 mL/min. In contrast, the surveyed literature indicates that Co-based counterparts can achieve significantly higher power densities, highlighting a promising development pathway for platinum group metal-free (PGM-free) cathodes. A key advantage of Co over Fe is its high resistance to Fenton degradation, which prevents the radical-induced chemical decomposition of the proton exchange membrane typically triggered by iron ions. The peak power density of 160.7 mW/cm2 is significant and demonstrates the strong potential of the Co-NCNT catalyst to reduce system costs by replacing noble metal catalysts at the cathode while simultaneously enhancing peak power density. Furthermore, by outperforming conventional Pt/C cathode catalysts, this highly active catalyst mitigates the sluggish kinetics and overpotentials associated with the oxygen reduction reaction. Crucially, although non-noble PGM-free architectures generally struggle to match conventional Pt/C performance in standard hydrogen-fed PEMFCs because of severe mass transport and durability barriers, the surveyed data demonstrate that these architectures can outperform Pt/C in the unique operating environment of DFAFCs. Consequently, improved cathode oxygen reduction reaction efficiency shifts the cell’s performance limitation, opening new pathways to further improve anode catalysts in general. Lastly, DFAFCs offer distinct thermodynamic and kinetic advantages over DMFCs. Although methanol has a higher theoretical energy density, DFAFCs can operate at significantly higher fuel concentrations because formic acid has lower crossover and faster reaction kinetics than methanol.

2.4. Combination of Platinum and Palladium Catalysts

The incorporation of diverse materials has proven to be a leading strategy for enhancing both the performance and efficiency of the ORR. Pt and Pd are widely recognized as the two most effective catalysts for formic acid oxidation [17,77], and combining them can yield enhanced catalytic properties compared with single-metal catalysts. In recent years, an increasing number of publications have reported catalysts incorporating Pt, Pd, and additional materials. Because platinum- and palladium-based catalysts are among the most extensively researched [74,75], their synergy with other materials may overcome dehydration-related issues. Additionally, Pd-based catalysts are known for their excellent direct FAO activity and greater resistance to CO poisoning than Pt. Pd tends to selectively break the O-H bond in the FA molecule across the entire potential range, promoting the almost exclusive direct oxidation of FA and the generation of H2 and CO2. Consequently, the CO concentration during initial-activity tests is nearly zero, in contrast to Pt. Pt, on the other hand, tends to exhibit combined FAO behavior: it breaks C-O and/or C-H bonds at low overpotential and O-H bonds at high overpotential [78]. Consequently, CO forms and poisons the Pt catalyst surface.
Bimetallic Pd-Pt alloys effectively reduce reaction intermediates and increase overall catalytic performance and stability, primarily because of the high surface-to-volume ratio of Pd-Pt nanoparticles. However, long-term testing has shown that catalytic activity degrades, even with the combination of Pd and Pt. Pt-Pd catalysts are generally prepared using three methods: spontaneous deposition [79], forced (electrolytic) deposition [80], and a combination of both. This chapter focuses on spontaneous deposition because it is more common and is stated to offer better results for catalysts than forced or combined deposition methods.
In [81], a Pt-Pd catalyst (1:1 weight ratio) was prepared using the spontaneous deposition method, following the procedure described in [82]. Formic acid was supplied to the anode side at a flow rate of 1 mL/min, while humidified air was supplied to the cathode at 200 mL/min. All experiments were conducted at room temperature and repeated at least three times to ensure reproducibility. A schematic overview of the experimental setup is shown in Figure S7.
The anode and cathode catalyst loadings were 4 mg/cm2 and 7 mg/cm2, respectively. To determine the optimal calcination atmosphere, initial tests were conducted under air and nitrogen atmospheres. The results are shown in panel (A) of Figure 10. The air atmosphere yields a slightly higher OCP of 0.812 V than the nitrogen atmosphere. This advantage over the nitrogen atmosphere is evident but decreases as the load increases. It is suggested that crystalline PdO phases are present on the Pt-Pd surface because Pd reacts with oxygen at high temperatures, forming this pattern [83]. Furthermore, certain by-products present in the air may have inhibited overall catalytic activity at higher current densities [81]. The results regarding the effect of anode catalyst loading are presented in panel (C) of Figure 10.
Figure 10. Effects of the calcination atmosphere on fuel cell performance at 500 °C (A), of calcination temperature on DFAFC performance (B), and the effect of anode-side catalyst loading, with the cathode catalyst loading held constant at 7 mg/cm2, at an operating temperature of 25 °C (C). Data were approximately digitized from the published experimental plots and independently replotted. Lines connect the extracted points.
The anode catalyst was subsequently prepared at 300, 400, and 500 °C under a nitrogen atmosphere, which was selected based on the results shown in (B) of Figure 10. The best performance was achieved at a calcination temperature of 400 °C, as shown in the upper-right chart in Figure 10.
The best test results were obtained with the catalyst calcined at 400 °C, which exhibited a peak power density of 58.8 mW/cm2. The poorest performance was observed for the catalyst calcined at 300 °C, with a power density of approximately 53 mW/cm2. These findings demonstrate that calcination significantly influences catalyst morphology, as previously reported in [84] for Pt-Ru/C catalysts calcined at temperatures of 300 and 400 °C. Calcination temperature drives changes in the catalyst’s active surface area, consequently affecting fuel cell performance. Although thermal treatment removes impurities from the catalyst, a temperature of 300 °C was not sufficient to remove all impurities adequately compared with temperatures of 400 and 500 °C. Increasing catalyst loading improved fuel cell performance, but only to a certain extent. The difference between catalyst loadings of 3 and 4 mg/cm2 was relatively negligible, especially when cost is considered. Furthermore, as shown in Table S10, the optimal trade-off between price and performance was achieved with catalyst loadings of 3 mg/cm2 for the anode and 5 mg/cm2 for the cathode.
This effect can be explained by the kinetic and mass-transfer limitations associated with catalyst loading. An excessively thick catalyst layer inhibits effective proton transport to the PEM. Furthermore, a thicker catalyst layer can increase the mass transport resistance for the reactants.
The results exhibit trends similar to those observed in DMFCs, demonstrating that advances in DMFCs can be applied to DFAFCs. This could substantially accelerate DFAFC development. Another parameter evaluated in [85] was the influence of the Pd-to-Pt ratio on catalyst performance. The authors investigated the effects of different ratios of the two catalysts and presented a nanostructured catalyst based on Pd0.64Pt0.36 nanoparticles immobilized on MWCNT-supported carbon cloth. Two catalysts were prepared: Pd0.64Pt0.36 (64/36% Pd/Pt metal ratio) and Pd0.5Pt0.5 (50/50% Pd/Pt metal ratio), using electrochemical synthesis under potentiodynamic conditions via linear sweep voltammetry. Pd and Pt nanoparticles were formed from platinum tetrachloride (PtCl4) and Pd(OAc)2 precursors, which had previously been deposited within the MWCNT network on the carbon cloth. This resulted in an evenly distributed catalyst across the entire MWCNT area. Diffuse Reflectance Infrared Fourier Transform Spectroscopy measurements clearly indicated increased resistance to CO poisoning compared with pure Pd and Pt catalysts. This system exhibited a high electrochemically active surface area of 56.94 m2/g and active site availability above 80%, explaining its high activity and stability toward FA electrooxidation.
The catalysts were evaluated at a load of 50 mA/cm2, a temperature of 60 °C, and an air flow rate of 200 mL/min. A 14 h long-term stability study demonstrated excellent catalyst durability. The DFAFC with the Pd0.64Pt0.36 catalyst exhibited a power density of 64 mW/cm2 at 250 mA/cm2 and 60 °C, with a stabilized air flow on the cathode side. To reduce fuel cell costs, tests were conducted with a low catalyst loading of 0.6 mg/cm2 of PdxPt1−x, which is significantly lower than typical DFAFC catalyst loadings.
The tested DFAFC was a single cell with stainless steel end plates, graphite bipolar plates with serpentine-shaped flow field channels covering an active area of 5 cm2, and a pretreated Nafion 115 membrane. Pretreatment of the Nafion membrane consisted of soaking it in 3% H2O2 for 1 h at 80 °C, then in deionized water for 2 h at 80 °C, and finally in 0.5 M H2SO4 for 1 h at 80 °C. After each step, the membrane was thoroughly rinsed with deionized water to remove any residues.
The graphite plates, electrodes, and MEA were compressed between holders at a pressure of 10 bar to ensure good electrical and ionic conductivity.
The test setup for the single-cell DFAFC is shown in Figure S8.
After assembly, the DFAFC was heated to 60 °C and supplied with water at a flow rate of 1.5 mL/min to the anode and oxygen at a flow rate of 50 mL/min to the cathode. The water was then replaced with a 3 M HCOOH solution, and an activity test was performed. After the test, the HCOOH solution was replaced with water, and the cell was regenerated by flowing water through it until the cell voltage dropped below 100 mV and stabilized. An anode activity test was also performed, followed by catalyst regeneration. The stability test was then conducted for 14 h, with air supplied to the cathode at a flow rate of 200 mL/min and formic acid supplied to the anode at a current density of 50 mA/cm2. The test was then continued by periodically increasing the current density to determine the maximum power output of the cell for each catalyst.
The polarization curves for Pd0.5Pt0.5 and Pd0.64Pt0.36 are shown in Figure S9.
The polarization curves in Figure S8 show that adjusting the Pd/Pt catalyst ratio significantly improved DFAFC performance, as is also evident in all articles in this review that optimize catalyst compositions.
The data from this study, together with the results obtained for different Pd-Pt ratios, are summarized in Table 6.
Table 6. Summary of the concentrations and performances of different Pd-Pt catalysts from [85].
Varying the composition of Pd–Pt catalysts produces distinct results, highlighting the potential for improvement through precise compositional control. Although catalyst loading was significantly reduced, the overall performance and longevity remain unsatisfactory, particularly because both constituents are expensive noble metals. Further research into ternary configurations incorporating macrocyclic additives such as FeTSPc offers a viable pathway to accelerate direct dehydrogenation kinetics, reduce noble metal loading, and ultimately lower the cost of Pt/Pd-based DFAFCs. Continued research in this direction could determine whether adding a third material or additive such as FeTSPc improves catalyst performance and reduces loading, potentially benefiting commercial viability.

2.5. Summary of DFAFC Catalyst Performance and Proposal for Standardizing the Testing Procedure

This section addresses the second gap identified in Table 1: the absence of a standardized testing protocol for DFAFC single cells. To clarify the data gathered from the available papers, Table 7 and Table 8 summarize the main parameters described in each paper included in the literature overview, together with data from other review papers with a similar focus.
Table 7. Characteristics of all catalysts described in detail in this paper.
Table 8. Main parameters for standardizing DFAFC catalyst benchmarking.
To accelerate the development of DFAFC catalysts and enable meaningful cross-study comparisons, testing parameters that can be readily controlled in typical laboratory single-cell setups must be standardized. Because such standardization is largely neglected in the DFAFC field, the recommendations below deliberately focus on low-complexity conditions as a starting point for FAO catalyst testing. They do not require specialized hardware or complex control systems; instead, they rely on simple choices of operating temperature, fuel composition, cell area, and commercially available components. This practical approach to standardizing DFAFC catalyst testing emphasizes three key aspects: (1) operating parameters and performance metrics, (2) cell geometry and component design, and (3) catalyst durability assessment. By implementing this minimal protocol, research groups can benchmark DFAFC catalyst performance on a common footing while retaining flexibility for advanced system-level optimization.
As shown in Table 7 and Table 8, catalyst performance varies significantly across the literature. The most promising catalysts for the FAO reaction at the anode include Pd-Ni2P/C-30% [46], PtBiPbNiCo [29], and Pd-Ni/C [46], all of which substantially outperform conventional benchmark catalysts. However, meaningful comparisons between these systems are hindered by inconsistencies in testing conditions. Therefore, standardizing key experimental parameters is essential to minimize external influences and isolate intrinsic catalyst performance.
Operating temperatures vary significantly among the reported DFAFC systems. For example, Pd-Ni2P/C and Pd-Ni/C are evaluated at 30 °C, whereas PtBiPbNiCo is tested at 80 °C. Because temperature strongly influences catalyst utilization and reaction kinetics, it should be standardized at a highly reproducible and easily maintained value above ambient temperature, such as 60 °C. This value lies between the 30 °C used for the highest-power Pd systems [43,45,46] and the 80 °C used for PtBiPbNiCo [29]: raising the temperature accelerates both FAO and ORR kinetics, whereas temperatures approaching 80 °C increase formic acid evaporation, crossover and water-management variability and are harder to control reproducibly in simple laboratory cells. Fuel concentrations and compositions are also inconsistent, ranging from mixtures such as 0.5 M H2SO4 + 0.5 M HCOOH to as high as 10 M HCOOH. This discrepancy complicates direct comparisons, particularly because PtBiPbNiCo exhibits exceptionally high power density despite unusually low fuel concentration. A reference formic acid concentration of 3 M could be used for catalyst comparisons because it provides a less aggressive environment for catalyst degradation, especially before the catalysts’ resistance to CO inhibition or adsorption is fully achieved and understood, while remaining practical to handle. Within the 0.5–10 M span of the benchmarked literature, 3 M lies in the concentration window where parametric single-cell studies report near-maximal performance before crossover losses begin to dominate at higher concentrations [11,12,14]. Additives such as H2SO4 could be introduced, but only after the initial benchmarking of the catalyst. Finally, cathode reactants span a wide range of gas mixtures. These should be standardized into two categories: fully humidified pure oxygen as the primary baseline, which minimizes cathode limitations and isolates anode catalyst performance, and fully humidified ambient air as an application-oriented secondary condition. Full humidification removes relative humidity as an uncontrolled variable, while the measured humidity and oxidant flow rate are reported for every test; this also mitigates the cathode flooding associated with fuel crossover and water accumulation during cell operation.
Geometry also strongly influences DFAFC performance and should be considered explicitly. For single-cell benchmarking, a reference active area of 4 cm2 should be adopted, with the active area explicitly reported in all cases, to ensure that geometric effects on mass transport and water management are comparable across studies. Membrane thickness also varies, often to reduce fuel crossover at the expense of performance. While this is a valid system-level strategy, the present research focuses primarily on catalyst performance; therefore, the influence of differences in proton conductivity should be minimized. From the perspective of the catalyst-coated membrane, DFAFCs differ from hydrogen-powered PEMFCs in their fuel type: formic acid is a liquid that dissociates directly on the catalyst into the gaseous phase. To improve the utilization of the hydrogen in formic acid, special diffusion layers should be considered, along with micro diffusion layers if necessary. The anode diffusion layer should be hydrophilic and provide efficient gas extraction, ensuring sustained contact between the catalyst active area and formic acid. This challenge is closely analogous to that encountered in PEM electrolyzers, suggesting that diffusion layer designs from electrolyzer technology could be adapted for DFAFCs, provided that the specific physicochemical properties of formic acid are considered. In addition, bipolar plate channel geometry should be standardized for formic acid as the working fluid. This aspect has been neglected with respect to both the fluid properties and potential enhancements to formic acid distribution across the membrane active area.
Catalyst longevity is currently defined inconsistently because there is no standard definition of a “short” or “long” catalyst duration or of what constitutes a significant performance drop. This field is still in its infancy, and measurements differ significantly. Some tests last only 1 h [45], whereas others extend to 500 h [32]. Some studies do not even present durability charts yet still claim reduced or eliminated CO poisoning. This methodological inconsistency must be addressed to clarify whether the absolute inhibition of CO poisoning is thermodynamically and kinetically achievable under realistic cell loads. The 100 h durability threshold falls within the 1–500 h span of reported tests [32,45]. This duration is long enough to move beyond temporary surface phenomena that can be reversed by water flushing or potential stepping and to expose the onset of persistent degradation modes, such as catalyst agglomeration, active-phase dissolution, and carbon-support corrosion. At the same time, it remains feasible (approximately four days) for routine laboratory throughput.
The final major discrepancy lies in catalyst loading. Although this is not directly a problem for standardizing test conditions, most DFAFC studies employ noble metal loadings that are an order of magnitude higher than those used in hydrogen PEMFCs. For DFAFC technology to become competitive, catalyst loading should be reduced. Accordingly, standardized testing protocols should encourage evaluation at lower catalyst loadings while promoting strategies to increase electrochemically active surface area to compensate for reduced material usage. That such loadings are attainable in practice is demonstrated by the nanoporous PdCuAu film anode [48], which delivered 93.2 mW/cm2 at only 0.01 mg Pd/cm2, outperforming a Pd/C anode with a 120-fold higher loading under identical conditions. Table 8 provides a consolidated overview of the minimal DFAFC single-cell test protocol and proposed standardization parameters.
To support implementation of the proposed parameters, Figure 11 presents the testing-protocol flowchart, and Table 9 provides the corresponding minimum-reporting checklist covering all requirements from cell assembly to data reporting.
Figure 11. Standardized testing procedure for catalysts in DFAFCs.

3. Digitalization-Ready DFAFC Benchmarking for Transport Energy Systems

This section addresses the third gap identified in Table 1, the missing digitalization and data-reporting perspective. The value of standardized DFAFC testing extends beyond conventional comparisons of catalyst activity. Logistics and transport are major energy consumers, and digital twins are increasingly used in these sectors to monitor, simulate, and optimize energy use [88]. In fuel-cell hybrid electric vehicles, the energy-management strategy determines the power split among the fuel cell, the battery, and auxiliary loads, thereby directly governing fuel consumption, efficiency, and component lifetime [89]. For PEMFCs, data-driven digital twins have already been demonstrated for degradation tracking and remaining useful life (RUL) prediction. In these applications, the digital model is continuously updated with measured operating data [90,91]. Such tools combine physical models with operational data to estimate non-measurable states, predict degradation, identify abnormal behavior, and optimize operation in real time.
For DFAFC-based systems, the usefulness of this approach depends directly on the availability of consistent full-cell datasets. However, the DFAFC studies reviewed in Section 2 report polarization and durability data for widely varying MEA designs, temperatures, fuel concentrations, oxidants, flow rates, active areas, and test durations (Table 2, Table 3, Table 4, Table 5, Table 6 and Table 7). This heterogeneity prevents the aggregation of published datasets and limits the calibration and validation of physics-based or machine-learning models. It may also cause differences in polarization curves to be attributed to catalyst chemistry, even when they arise from mass transport, thermal conditions, cell geometry, water management, or oxidant supply. The minimum input variables required for a DFAFC digital twin therefore include cell voltage, current density, power density, fuel concentration, anode flow rate, cathode oxidant type, flow rate and humidity, cell and inlet temperatures, back pressure, active area, membrane type and thickness, catalyst composition and loading, operating time, and clearly defined durability-test conditions.
The standardization framework proposed in Section 2.5 (Table 8) can therefore be interpreted as the first data architecture for DFAFC digitalization. A reference operating point of 60 °C with 3 M HCOOH and a clearly reported active area provides a common baseline for interlaboratory comparison. Complementary off-design measurements obtained by varying fuel concentration, temperature, current density, and reactant flow rates in a controlled manner would enable the development of reduced-order electrochemical models, degradation models, surrogate models, and machine-learning predictors capable of estimating power availability and efficiency during dynamic operation. To make such data reusable across laboratories, Table 9 extends the protocol with a minimum data-reporting schema that follows the FAIR principles of findable, accessible, interoperable, and reusable research data [92].
Table 9. Minimum data-reporting checklist for digitalization-ready DFAFC single-cell testing.
In future hybrid-electric transport applications, including light-duty vehicles, automated logistics platforms, and marine auxiliary power systems, such models could support predictive energy management. They could keep DFAFC output within an efficient operating window, limit operation under conditions associated with accelerated catalyst deactivation (e.g., prolonged operation that promotes CO accumulation on Pd surfaces), schedule regeneration steps such as water flushing or potential pulsing, and coordinate fuel-cell output with battery charging and transient power demand. The resulting pathway is summarized in Figure 12.
Figure 12. Conceptual pathway from standardized DFAFC single-cell testing to digital-twin-assisted energy management of hybrid-electric transport systems. Steps 1–2 correspond to the scope of the present review; steps 3–6 represent future digitalization stages enabled by the proposed framework.
It should be emphasized that the contribution of the present review is not the implementation of a DFAFC digital twin, but the definition of the comparable experimental conditions and reporting variables that are needed for its future development and validation.

4. Conclusions

This review demonstrates that Pt-based catalysts remain highly competitive alternatives to the widely preferred Pd-based catalysts in the field of DFAFCs, despite generally producing lower peak power densities. Among the surveyed Pt-based catalysts, PtBiPbNiCo HEA achieved the highest reported peak power density (321.2 mW/cm2), which was the second highest among all catalysts evaluated in this review. From a durability perspective, modifying Pt with FeTSPc successfully suppresses the indirect dehydration pathway and subsequent CO generation while maintaining competitive power output.
Direct growth of the PtCu catalyst on the GDL offers an interesting alternative to the standard ink-spraying technique, providing highly precise spatial control over catalyst deposition on the GDL. Alloying Pt with other noble metals, such as Ru or Au, significantly improves catalyst longevity. However, the comparatively modest power densities warrant further assessment of the performance–cost trade-off. Reported Pt catalyst loadings of 0.5–3 mg/cm2 were lower than those of Pd-based systems, at 4 to 8 mg/cm2, suggesting a potential precious-metal cost advantage that requires techno-economic verification.
Among palladium-based catalysts, Pd/C has been reported to achieve peak power densities of up to 243 mW/cm2. Although Pd favors the direct dehydrogenation pathway, it remains susceptible to poisoning and activity loss.
The highest peak power density among the surveyed DFAFCs was 550 mW/cm2, achieved using Pd-Ni2P/C-30%. However, degradation during its four-hour durability test demonstrates that high initial power density does not establish long-term operational stability. Partial regeneration through in situ water flushing or potential stepping may support the use of these cells in specialized, high-autonomy electronic applications, subject to verification of sustained performance and regeneration requirements.
Platinum group metal-free (PGM-free) cathode catalysts also show promise. A DFAFC employing Co-NCNT achieved a peak power density of 160.7 mW/cm2, exceeding the peak power density obtained with the commercial Pt/C comparator under the conditions of the cited study. Combining these cathodes with improved anode catalysts warrants investigation as a strategy to reduce precious-metal dependence while maintaining or improving performance.
The surveyed peak power densities were obtained under different operating temperatures, fuel concentrations, oxidant compositions, flow rates, catalyst loadings, membrane thicknesses, active areas, electrode architectures, and durability conditions. Consequently, the reported values define the performance envelope found in the available literature but do not establish an intrinsic ranking of catalyst activity from full-cell measurements. Moreover, the limited availability of long-duration experiments, transient measurements, stack-level demonstrations, cost analyses, and lifecycle assessments prevents definitive conclusions regarding commercial readiness.
To improve cross-study comparability and support future digitalization, this review proposes a practical, low-complexity framework for DFAFC single-cell testing, summarized in Table 8. To minimize external environmental variations and isolate intrinsic catalyst behavior, future investigations should adopt a uniform operating temperature of 60 °C and use a baseline fuel concentration of 3 M HCOOH. This concentration offers a practical, less aggressive testing environment before advanced CO-resistance parameters are evaluated. For single-cell benchmarking, a reference active area of 4 cm2 should be adopted, and membrane thickness should be explicitly reported to ensure comparable mass transport profiles. Studies should also report the catalyst and ionomer loadings of both electrodes, as well as the membrane type, oxidant composition and flow rate, relative humidity, operating pressure, MEA preparation procedure, and flow-field geometry. In addition to polarization and peak-power measurements, studies should report performance at defined current densities, catalyst-mass-normalized power, and time-dependent voltage or power degradation. A minimum 100 h durability experiment at a fixed current density is recommended as a baseline, followed by polarization measurements before and after durability testing and, where possible, characterization of catalyst regeneration after poisoning. The proposed framework should therefore be regarded as a baseline for generating comparable experimental evidence, rather than as a validated commercial qualification standard.
Potential transportation applications include hybrid systems in which a DFAFC supplies average power demand while a battery or supercapacitor accommodates transient loads and recovers braking energy. Potential early applications include auxiliary power units, range extenders, material-handling vehicles, and specialized low-power mobility systems. Application in primary vehicle propulsion would require substantial improvements in durability, transient response, catalyst utilization, stack scalability, cold-start capability, and balance-of-plant integration. The proposed framework could also provide a basis for validated digital models and, ultimately, digital twins, as discussed in Future Directions. DFAFCs release CO2 at the point of use and are therefore not zero-emission devices. Their contribution to transportation decarbonization therefore depends on the formic acid production pathway and should ultimately be evaluated using lifecycle or well-to-wheel emissions.

5. Future Directions

Future work should first focus on implementing and evaluating the proposed standardization framework, with consistent control and reporting of the relevant testing parameters. The framework presented in this review could provide an accessible starting point for this process. A second priority is to develop a standardized fuel-cell setup for catalyst comparison that is specifically optimized for liquid fuels, particularly formic acid, while accounting for its distinct properties relative to other liquid fuels used in proton-exchange membrane fuel cells. This setup should also facilitate efficient CO2 removal to prevent local fuel starvation and reduce mass-transport limitations that could distort the assessment of catalyst performance. The potential cost reduction associated with non-noble-metal cathode catalysts, together with the differences in reported anode catalyst loadings between Pt- and Pd-based systems, warrants an in-depth techno-economic analysis. This analysis should support meaningful comparisons between DFAFCs and competing technologies and should be accompanied by a systematic assessment of the relationship between catalyst loading and performance, including the influence of the electrochemically accessible catalyst surface area. Approaches from different types of PEMFCs could potentially be adopted. For example, adding Fe-N1C3 to an ultralow Pt loading achieved results comparable to those of regularly used Pt/C. This modification achieved 97% activity retention after 100,000 cycles over a potential range from 0.6 to 0.95 V, without a noticeable current drop at 0.6 V for 200 h. These test results show a specific power density of 1.08 W/cm2 [93]. This approach could potentially be implemented in DFAFCs to reduce noble metal loading and, consequently, the overall cost of DFAFC systems. Regarding catalyst optimization, future studies should systematically investigate catalyst-to-additive ratios within individual catalyst systems and compare the resulting performance under standardized conditions. This would help clarify the influence of composition on performance and identify suitable ratios for further development. These investigations should be complemented by extended durability and regeneration testing to determine whether improvements in initial performance translate into sustained operation. Future work should also use standardized DFAFC testing to build datasets for digital models and, ultimately, digital twins. These datasets should combine operating conditions, catalyst and ionomer loadings, MEA preparation details, polarization behavior, and time-resolved degradation and regeneration data. They would support physics-based models of anode two-phase flow, formic acid transport and poisoning, as well as data-driven or hybrid models for state-of-health estimation, fault detection, and predictive maintenance. Meaningful digital-twin development will require validation against transient duty cycles, including start–stop operation, load ramps, idle periods, and repeated OCP exposure, in addition to steady-state measurements.

Supplementary Materials

The following supporting information can be downloaded at https://www.mdpi.com/article/10.3390/en19235735/s1.

Author Contributions

Conceptualization, J.P. and Ž.P.; methodology, J.P., Ž.P. and G.R.; investigation, J.P., Ž.P., L.M. and G.R.; data curation, J.P. and Ž.P.; writing—original draft preparation, J.P. and G.R.; writing—review and editing, Ž.P., L.M. and G.R.; visualization, J.P., Ž.P., L.M. and G.R.; supervision, Ž.P., L.M. and G.R.; funding acquisition, Ž.P. All authors have read and agreed to the published version of the manuscript.

Funding

The authors gratefully acknowledge the support provided by the project STIM-REI 2.0 PK.1.1.10.0005, funded by the European Union through the European Regional Development Fund under the Operational Programme Competitiveness and Cohesion 2014–2020 (KK.01.1.1.01). The authors also acknowledge support from the project “Overcoming the Technological Hurdles in the Incorporation of Biopolymers as Ion Exchange Membranes in Fuel Cell Applications” and ATASYS IP-UNIST-06.

Data Availability Statement

No new experimental data were generated in this study. The data discussed in this review are available in the cited references and in the Supplementary Materials.

Conflicts of Interest

The authors declare no conflicts of interest.

Abbreviations

CCLCathode Catalyst Layer
DFAFCDirect Formic Acid Fuel Cell
DMFCDirect Methanol Fuel Cell
FAFormic Acid
FAOFormic Acid Oxidation
GDEGas Diffusion Electrode
GDLGas Diffusion Layer
HEAHigh-Entropy Alloy
HPHexagonal Nanoparticle
ISOInternational Organization for Standardization
MEAMembrane Electrode Assembly
MPLMicro Porous Layer
MWCNTsMulti-Walled Carbon Nano Tubes
NCNTsNitrogen Doped Carbon Nanotubes
NWNanowire
PEMProton Exchange Membrane
PEMFCProton Exchange Membrane Fuel Cell
PMFPlatinum metal-free
OCPOpen Circuit Potential
ORROxygen Reduction Reaction
TMsTransition Metals
AuGold
BiBismuth
CCarbon
COCarbon Monoxide
CO2Carbon Dioxide
CuCopper
FeTSPcTetrasulfophthalocyanine
H2Hydrogen
H2OWater
H2SO4Sulfuric acid
HCOO−Formate
HCOOHFormic Acid
Ni2PNickel Phosphide
PdPalladium
PbLead
PtPlatinum
PtCl4Platinum Tetrachloride
RuRuthenium

References

  1. Kiani, M.; Zhao, Y.; Zhang, R. Proton Exchange Membrane Fuel Cells: Recent Developments and Future Perspectives. Chem. Commun. 2025, 61, 9392–9411. [Google Scholar] [CrossRef] [Scilit]
  2. Li, Y.; Yao, M.S.; He, Y.; Du, S. Recent Advances of Electrocatalysts and Electrodes for Direct Formic Acid Fuel Cells: From Nano to Meter Scale Challenges. Nanomicro Lett. 2025, 17, 148. [Google Scholar] [CrossRef] [Scilit]
  3. Li, Y.; Yan, Y.; He, Y.; Du, S. Catalyst Electrodes with PtCu Nanowire Arrays In Situ Grown on Gas Diffusion Layers for Direct Formic Acid Fuel Cells. ACS Appl. Mater. Interfaces 2022, 14, 11457–11464. [Google Scholar] [CrossRef] [Scilit]
  4. Jiang, K.; Zhang, H.X.; Zou, S.; Cai, W. Bin Electrocatalysis of Formic Acid on Palladium and Platinum Surfaces: From Fundamental Mechanisms to Fuel Cell Applications. Phys. Chem. Chem. Phys. 2014, 16, 20360–20376. [Google Scholar] [CrossRef] [Scilit]
  5. Fang, Z.; Chen, W. Recent Advances in Formic Acid Electro-Oxidation: From the Fundamental Mechanism to Electrocatalysts. Nanoscale Adv. 2021, 3, 94–105. [Google Scholar] [CrossRef] [Scilit]
  6. Johnson, W.; Heldreth, B.; Bergfeld, W.F.; Belsito, D.V.; Hill, R.A.; Klaassen, C.D.; Liebler, D.C.; Marks, J.G.; Shank, R.C.; Slaga, T.J.; et al. Safety Assessment of Formic Acid and Sodium Formate as Used in Cosmetics. Int. J. Toxicol. 2016, 35, 41S–54S. [Google Scholar] [CrossRef] [Scilit]
  7. Uwitonze, N.; Chen, Y.-X. The Study of Pt and Pd Based Anode Catalysis for Formic Acid Fuel Cell. Chem. Sci. J. 2017, 8, 1–12. [Google Scholar] [CrossRef]
  8. Duarah, P.; Haldar, D.; Yadav, V.S.K.; Purkait, M.K. Progress in the Electrochemical Reduction of CO2 to Formic Acid: A Review on Current Trends and Future Prospects. J. Environ. Chem. Eng. 2021, 9, 106394. [Google Scholar] [CrossRef] [Scilit]
  9. Nitopi, S.; Bertheussen, E.; Scott, S.B.; Liu, X.; Engstfeld, A.K.; Horch, S.; Seger, B.; Stephens, I.E.L.; Chan, K.; Hahn, C.; et al. Progress and Perspectives of Electrochemical CO2 Reduction on Copper in Aqueous Electrolyte. Chem. Rev. 2019, 119, 7610–7672. [Google Scholar] [CrossRef] [Scilit]
  10. Nogalska, A.; Navarro, A.B.; Garcia-Valls, R. Mea Preparation for Direct Formate/Formic Acid Fuel Cell—Comparison of Palladium Black and Palladium Supported on Activated Carbon Performance on Power Generation in Passive Fuel Cell. Membranes 2020, 10, 355. [Google Scholar] [CrossRef] [Scilit]
  11. Wang, X.; Hu, J.M.; Hsing, I.M. Electrochemical Investigation of Formic Acid Electro-Oxidation and Its Crossover through a Nafion ® Membrane. J. Electroanal. Chem. 2004, 562, 73–80. [Google Scholar] [CrossRef] [Scilit]
  12. Ha, S.; Dunbar, Z.; Masel, R.I. Characterization of a High Performing Passive Direct Formic Acid Fuel Cell. J. Power Sources 2006, 158, 129–136. [Google Scholar] [CrossRef] [Scilit]
  13. Eppinger, J.; Huang, K.W. Formic Acid as a Hydrogen Energy Carrier. ACS Energy Lett. 2017, 2, 188–195. [Google Scholar] [CrossRef] [Scilit]
  14. Lue, S.J.; Liu, N.Y.; Kumar, S.R.; Tseng, K.C.Y.; Wang, B.Y.; Leung, C.H. Experimental and One-Dimensional Mathematical Modeling of Different Operating Parameters in Direct Formic Acid Fuel Cells. Energies 2017, 10, 1972. [Google Scholar] [CrossRef] [Scilit]
  15. Rice, C.; Ha, S.; Masel, R.I.; Waszczuk, P.; Wieckowski, A.; Barnard, T. Direct Formic Acid Fuel Cells. J. Power Sources 2002, 111, 83–89. [Google Scholar] [CrossRef] [Scilit]
  16. Rice, C.; Ha, S.; Masel, R.I.; Wieckowski, A. Catalysts for Direct Formic Acid Fuel Cells. J. Power Sources 2003, 115, 229–235. [Google Scholar] [CrossRef] [Scilit]
  17. Zhu, Y.; Ha, S.Y.; Masel, R.I. High Power Density Direct Formic Acid Fuel Cells. J. Power Sources 2004, 130, 8–14. [Google Scholar] [CrossRef] [Scilit]
  18. Bhaskaran, R.; Abraham, B.G.; Chetty, R. Recent Advances in Electrocatalysts, Mechanism, and Cell Architecture for Direct Formic Acid Fuel Cells. Wiley Interdiscip. Rev. Energy Environ. 2022, 11, e419. [Google Scholar] [CrossRef] [Scilit]
  19. Cheng, H.; Wang, J.; Wu, C.; Liu, Z. Electrocatalysts for Formic Acid-Powered PEM Fuel Cells: Challenges and Prospects. Energy Mater. Adv. 2023, 4, 67. [Google Scholar] [CrossRef] [Scilit]
  20. Zhan, C.; Sun, H.; Yan, W.; Xia, J.; Meng, X.-M.; Li, T.; Bu, L.; Kong, Q.; Lin, H.; Liu, W.; et al. A Biphasic Strategy to Synergistically Accelerate Activation and CO Spillover in Formic Acid Oxidation Catalysis. Nano Lett. 2024, 24, 8134–8142. [Google Scholar] [CrossRef] [Scilit]
  21. Sapkota, P.; Lim, S.; Aguey-Zinsou, K.F. Platinum-Tin as a Superior Catalyst for Proton Exchange Membrane Fuel Cells. RSC Sustain. 2023, 1, 368–377. [Google Scholar] [CrossRef] [Scilit]
  22. Chen, Y.X.; Heinen, M.; Jusys, Z.; Behm, R.J. Kinetics and Mechanism of the Electrooxidation of Formic Acid-Spectroelectrochemical Studies in a Flow Cell. Angew. Chem. Int. Ed. 2006, 45, 981–985. [Google Scholar] [CrossRef] [Scilit]
  23. Li, Q.; He, R.; Gao, J.-A.; Jensen, J.O.; Bjerrum, N.J. The CO Poisoning Effect in PEMFCs Operational at Temperatures up to 200 °C. J. Electrochem. Soc. 2003, 150, A1599. [Google Scholar] [CrossRef] [Scilit]
  24. Beurey, C.; Gozlan, B.; Carré, M.; Bacquart, T.; Morris, A.; Moore, N.; Arrhenius, K.; Meuzelaar, H.; Persijn, S.; Rojo, A.; et al. Review and Survey of Methods for Analysis of Impurities in Hydrogen for Fuel Cell Vehicles According to ISO 14687:2019. Front. Energy Res. 2021, 8, 615149. [Google Scholar] [CrossRef] [Scilit]
  25. Divisek, J.; Oetjen, H.-F.; Peinecke, V.; Schmidt, V.M.; Stimming, U. Components for PEM Fuel Cell Systems Using Hydrogen and CO Containing Fuels; Elsevier: Amsterdam, The Netherlands, 1998. [Google Scholar]
  26. Duchesne, P.N.; Li, Z.Y.; Deming, C.P.; Fung, V.; Zhao, X.; Yuan, J.; Regier, T.; Aldalbahi, A.; Almarhoon, Z.; Chen, S.; et al. Golden Single-Atomic-Site Platinum Electrocatalysts. Nat. Mater. 2018, 17, 1033–1039. [Google Scholar] [CrossRef] [Scilit]
  27. Zhou, X.; Xing, W.; Liu, C.; Lu, T. Platinum-Macrocycle Co-Catalyst for Electro-Oxidation of Formic Acid. Electrochem. Commun. 2007, 9, 1469–1473. [Google Scholar] [CrossRef] [Scilit]
  28. Zhou, X.; Li, S.; Su, Y.; Liu, C.; Huang, M.; Lu, T.; Xing, W. Preparation and Simulation of an Additional Catalyst Layer for Direct Methanol Fuel Cell. J. Electroanal. Chem. 2006, 588, 129–139. [Google Scholar] [CrossRef] [Scilit]
  29. Zhan, C.; Bu, L.; Sun, H.; Huang, X.; Zhu, Z.; Yang, T.; Ma, H.; Li, L.; Wang, Y.; Geng, H.; et al. Medium/High-Entropy Amalgamated Core/Shell Nanoplate Achieves Efficient Formic Acid Catalysis for Direct Formic Acid Fuel Cell. Angew. Chem. Int. Ed. 2023, 62, e202213783. [Google Scholar] [CrossRef] [Scilit]
  30. Sun, Y.; Dai, S. High-Entropy Materials for Catalysis: A New Frontier; Springer Nature: London, UK, 2021; Volume 7. [Google Scholar]
  31. Du, S. A Facile Route for Polymer Electrolyte Membrane Fuel Cell Electrodes with in Situ Grown Pt Nanowires. J. Power Sources 2010, 195, 289–292. [Google Scholar] [CrossRef] [Scilit]
  32. Choi, J.H.; Jeong, K.J.; Dong, Y.; Han, J.; Lim, T.H.; Lee, J.S.; Sung, Y.E. Electro-Oxidation of Methanol and Formic Acid on PtRu and PtAu for Direct Liquid Fuel Cells. J. Power Sources 2006, 163, 71–75. [Google Scholar] [CrossRef] [Scilit]
  33. Choi, M.; Ahn, C.-Y.; Lee, H.; Kim, J.K.; Oh, S.-H.; Hwang, W.; Yang, S.; Kim, J.; Kim, O.-H.; Choi, I.; et al. Bi-Modified Pt Supported on Carbon Black as electro-Oxidation Catalyst for 300 W Formic Acid Fuel Cell Stack. Appl. Catal. B 2019, 253, 187–195. [Google Scholar] [CrossRef] [Scilit]
  34. Russell, A.E. Electrocatalysis: Theory and Experiment at the Interface. Phys. Chem. Chem. Phys. 2008, 10, 3607–3608. [Google Scholar] [CrossRef] [Scilit]
  35. Chen, X. Adsorption and Catalysis on Pt and Pd Monolayer-Modified Pt Single Crystal Electrodes. Ph.D. Thesis, Leiden University, Leiden, The Netherlands, 2019. [Google Scholar]
  36. Obradović, M.D.; Gojković, S.L. HCOOH Oxidation on Thin Pd Layers on Au: Self-Poisoning by the Subsequent Reaction of the Reaction Product. Electrochim. Acta 2013, 88, 384–389. [Google Scholar] [CrossRef] [Scilit]
  37. Wang, J.Y.; Zhang, H.X.; Jiang, K.; Cai, W. Bin From HCOOH to CO at Pd Electrodes: A Surface-Enhanced Infrared Spectroscopy Study. J. Am. Chem. Soc. 2011, 133, 14876–14879. [Google Scholar] [CrossRef] [Scilit]
  38. Zhu, Y.; Khan, Z.; Masel, R.I. The Behavior of Palladium Catalysts in Direct Formic Acid Fuel Cells. J. Power Sources 2005, 139, 15–20. [Google Scholar] [CrossRef] [Scilit]
  39. Zhang, H.X.; Wang, S.H.; Jiang, K.; André, T.; Cai, W. Bin In Situ Spectroscopic Investigation of CO Accumulation and Poisoning on Pd Black Surfaces in Concentrated HCOOH. J. Power Sources 2012, 199, 165–169. [Google Scholar] [CrossRef] [Scilit]
  40. Zhou, Y.; Liu, J.; Ye, J.; Zou, Z.; Ye, J.; Gu, J.; Yu, T.; Yang, A. Poisoning and Regeneration of Pd Catalyst in Direct Formic Acid Fuel Cell. Electrochim. Acta 2010, 55, 5024–5027. [Google Scholar] [CrossRef] [Scilit]
  41. Shen, T.; Chen, S.; Zeng, R.; Gong, M.; Zhao, T.; Lu, Y.; Liu, X.; Xiao, D.; Yang, Y.; Hu, J.; et al. Tailoring the Antipoisoning Performance of Pd for Formic Acid Electrooxidation via an Ordered PdBi Intermetallic. ACS Catal. 2020, 10, 9977–9985. [Google Scholar] [CrossRef] [Scilit]
  42. Shi, Y.; Schimmenti, R.; Zhu, S.; Venkatraman, K.; Chen, R.; Chi, M.; Shao, M.; Mavrikakis, M.; Xia, Y. Solution-Phase Synthesis of PdH0.706Nanocubes with Enhanced Stability and Activity toward Formic Acid Oxidation. J. Am. Chem. Soc. 2022, 144, 2556–2568. [Google Scholar] [CrossRef] [Scilit]
  43. Ha, S.; Larsen, R.; Masel, R.I. Performance Characterization of Pd/C Nanocatalyst for Direct Formic Acid Fuel Cells. J. Power Sources 2005, 144, 28–34. [Google Scholar] [CrossRef] [Scilit]
  44. Biella, S.; Porta, F.; Prati, L.; Rossi, M. Surfactant-Protected Gold Particles: New Challenge for Gold-on-Carbon Catalysts; Springer: Berlin/Heidelberg, Germany, 2003. [Google Scholar]
  45. Larsen, R.; Ha, S.; Zakzeski, J.; Masel, R.I. Unusually Active Palladium-Based Catalysts for the Electrooxidation of Formic Acid. J. Power Sources 2006, 157, 78–84. [Google Scholar] [CrossRef] [Scilit]
  46. Chang, J.; Feng, L.; Liu, C.; Xing, W.; Hu, X. An Effective Pd-Ni2P/C Anode Catalyst for Direct Formic Acid Fuel Cells. Angew. Chem. Int. Ed. 2014, 53, 122–126. [Google Scholar] [CrossRef] [Scilit]
  47. Popczun, E.J.; McKone, J.R.; Read, C.G.; Biacchi, A.J.; Wiltrout, A.M.; Lewis, N.S.; Schaak, R.E. Nanostructured Nickel Phosphide as an Electrocatalyst for the Hydrogen Evolution Reaction. J. Am. Chem. Soc. 2013, 135, 9267–9270. [Google Scholar] [CrossRef] [Scilit]
  48. Xie, J.; Huang, D.; Yin, H.; Liu, F.; Ding, Y. Au-Stabilized Nanoporous PdCuAu Alloys Exhibiting Outstanding Catalytic Activity and Durability for the Formic Acid Oxidation Reaction. ACS Appl. Mater. Interfaces 2022, 14, 35466–35476. [Google Scholar] [CrossRef] [Scilit]
  49. Jiang, K.; Chang, J.; Wang, H.; Brimaud, S.; Xing, W.; Behm, R.J.; Cai, W. Bin Small Addition of Boron in Palladium Catalyst, Big Improvement in Fuel Cell’s Performance: What May Interfacial Spectroelectrochemistry Tell? ACS Appl. Mater. Interfaces 2016, 8, 7133–7138. [Google Scholar] [CrossRef] [Scilit]
  50. Feng, L.; Chang, J.; Jiang, K.; Xue, H.; Liu, C.; Cai, W.-B.; Xing, W.; Zhang, J. Nanostructured Palladium Catalyst Poisoning Depressed by Cobalt Phosphide in the Electro-Oxidation of Formic Acid for Fuel Cells. Nano Energy 2016, 30, 355–361. [Google Scholar] [CrossRef] [Scilit]
  51. Kang, Y.S.; Choi, D.; Cho, J.; Park, H.Y.; Lee, K.S.; Ahn, M.; Jang, I.; Park, T.; Ham, H.C.; Yoo, S.J. Highly Active and Durable Ordered Intermetallic PdFe Electrocatalyst for Formic Acid Electrooxidation Reaction. ACS Appl. Energy Mater. 2020, 3, 4226–4237. [Google Scholar] [CrossRef] [Scilit]
  52. Huang, S.; Li, J.; Chen, Y.; Yan, L.; Zhang, P.; Zhang, X.; Zhao, C. Boosting the Anti-Poisoning Ability of Palladium towards Electrocatalytic Formic Acid Oxidation via Polyphosphide Chemistry. J. Colloid Interface Sci. 2022, 615, 366–374. [Google Scholar] [CrossRef] [Scilit]
  53. Yang, S.; Chung, Y.; Lee, K.-S.; Kwon, Y. Enhancements in Catalytic Activity and Duration of PdFe Bimetallic Catalysts and Their Use in Direct Formic Acid Fuel Cells. J. Ind. Eng. Chem. 2020, 90, 351–357. [Google Scholar] [CrossRef] [Scilit]
  54. Yang, S.; Yang, J.; Chung, Y.; Kwon, Y. Pd–Bi Bimetallic Catalysts Including Polyvinylpyrrolidone Surfactant Inducing Excellent Formic Acid Oxidation Reaction and Direct Formic Acid Fuel Cell Performance. Int. J. Hydrogen Energy 2017, 42, 17211–17220. [Google Scholar] [CrossRef] [Scilit]
  55. Ding, J.; Liu, Z.; Liu, X.; Liu, B.; Liu, J.; Deng, Y.; Han, X.; Hu, W.; Zhong, C. Tunable Periodically Ordered Mesoporosity in Palladium Membranes Enables Exceptional Enhancement of Intrinsic Electrocatalytic Activity for Formic Acid Oxidation. Angew. Chem. Int. Ed. 2020, 59, 5092–5101. [Google Scholar] [CrossRef] [Scilit]
  56. Cheng, H.; Zhou, J.; Xie, H.; Zhang, S.; Zhang, J.; Sun, S.; Luo, P.; Lin, M.; Wang, S.; Pan, Z.; et al. Hydrogen Intercalation-Induced Crystallization of Ternary PdNiP Alloy Nanoparticles For Direct Formic Acid Fuel Cells. Adv. Energy Mater. 2023, 13, 2203893. [Google Scholar] [CrossRef] [Scilit]
  57. Che Ramli, Z.A.; Pasupuleti, J.; Tengku Saharuddin, T.S.; Yusoff, Y.N.; Isahak, W.N.R.W.; Baharudin, L.; Tak Yaw, C.; Koh, S.P.; Tiong Kiong, S. Electrocatalytic Activities of Platinum and Palladium Catalysts for Enhancement of Direct Formic Acid Fuel Cells: An Updated Progress. Alex. Eng. J. 2023, 76, 701–733. [Google Scholar] [CrossRef] [Scilit]
  58. Mølmen, L.; Eiler, K.; Fast, L.; Leisner, P.; Pellicer, E. Recent Advances in Catalyst Materials for Proton Exchange Membrane Fuel Cells. APL Mater. 2021, 9, 040702. [Google Scholar] [CrossRef] [Scilit]
  59. Muthuvel, M.; Jin, X.; Botte, G.G. Fuel Cells–Exploratory Fuel Cells | Direct Carbon Fuel Cells. In Encyclopedia of Electrochemical Power Sources, 2nd ed.; Garche, J., Ed.; Elsevier: Oxford, UK, 2009; pp. 834–848. ISBN 978-0-323-95822-6. [Google Scholar]
  60. Tao, J.; Wang, X.; Xu, M.; Liu, C.; Ge, J.; Xing, W. Non-Noble Metals as Activity Sites for ORR Catalysts in Proton Exchange Membrane Fuel Cells (PEMFCs). Ind. Chem. Mater. 2023, 1, 388–409. [Google Scholar] [CrossRef] [Scilit]
  61. Jasinski, R. A New Fuel Cell Cathode Catalyst. Nature 1964, 201, 1212–1213. [Google Scholar] [CrossRef] [Scilit]
  62. Baruah, M.J.; Dutta, R.; Zaki, M.E.A.; Bania, K.K. Heterogeneous Iron-Based Catalysts for Organic Transformation Reactions: A Brief Overview. Molecules 2024, 29, 3177. [Google Scholar] [CrossRef] [Scilit]
  63. Wang, X.X.; Swihart, M.T.; Wu, G. Achievements, Challenges and Perspectives on Cathode Catalysts in Proton Exchange Membrane Fuel Cells for Transportation. Nat. Catal. 2019, 2, 578–589. [Google Scholar] [CrossRef] [Scilit]
  64. Jaouen, F.; Jones, D.; Coutard, N.; Artero, V.; Strasser, P.; Kucernak, A. Toward Platinum Group Metal-Free Catalysts for Hydrogen/Air Proton-Exchange Membrane Fuel Cells. Johns. Matthey Technol. Rev. 2018, 62, 231–255. [Google Scholar] [CrossRef] [Scilit]
  65. Li, J.; Sougrati, M.T.; Zitolo, A.; Ablett, J.M.; Oğuz, I.C.; Mineva, T.; Matanovic, I.; Atanassov, P.; Huang, Y.; Zenyuk, I.; et al. Identification of Durable and Non-Durable FeNx Sites in Fe–N–C Materials for Proton Exchange Membrane Fuel Cells. Nat. Catal. 2021, 4, 10–19. [Google Scholar] [CrossRef] [Scilit]
  66. Varnell, J.A.; Tse, E.C.M.; Schulz, C.E.; Fister, T.T.; Haasch, R.T.; Timoshenko, J.; Frenkel, A.I.; Gewirth, A.A. Identification of Carbon-Encapsulated Iron Nanoparticles as Active Species in Non-Precious Metal Oxygen Reduction Catalysts. Nat. Commun. 2016, 7, 12582. [Google Scholar] [CrossRef] [Scilit]
  67. Chen, S.; Zhang, N.; Narváez Villarrubia, C.W.; Huang, X.; Xie, L.; Wang, X.; Kong, X.; Xu, H.; Wu, G.; Zeng, J.; et al. Single Fe Atoms Anchored by Short-Range Ordered Nanographene Boost Oxygen Reduction Reaction in Acidic Media. Nano Energy 2019, 66, 104164. [Google Scholar] [CrossRef] [Scilit]
  68. Abd Lah Halim, F.; Tsujiguchi, T.; Osaka, Y.; Kodama, A. Performance of Direct Formic Acid Fuel Cell Using Transition Metal-Nitrogen-Doped Carbon Nanotubes as Cathode Catalysts. Int. J. Energy Res. 2019, 43, 8070–8084. [Google Scholar] [CrossRef] [Scilit]
  69. Blair, S.L.; Law, W.L. Electrocatalysis in Other Direct Liquid Fuel Cells; Wiley: Weinheim, Germany; John Wiley: Hoboken, NJ, USA, 2009; ISBN 9783527323777. [Google Scholar]
  70. Sebastián, D.; Serov, A.; Artyushkova, K.; Atanassov, P.; Aricò, A.S.; Baglio, V. Performance, Methanol Tolerance and Stability of Fe-Aminobenzimidazole Derived Catalyst for Direct Methanol Fuel Cells. J. Power Sources 2016, 319, 235–246. [Google Scholar] [CrossRef] [Scilit]
  71. Sebastián, D.; Serov, A.; Matanovic, I.; Artyushkova, K.; Atanassov, P.; Aricò, A.S.; Baglio, V. Insights on the Extraordinary Tolerance to Alcohols of Fe-N-C Cathode Catalysts in Highly Performing Direct Alcohol Fuel Cells; Elsevier: Amsterdam, The Netherlands, 2017. [Google Scholar]
  72. Osmieri, L.; Escudero-Cid, R.; Armandi, M.; Monteverde Videla, A.H.A.; García Fierro, J.L.; Ocón, P.; Specchia, S. Fe-N/C Catalysts for Oxygen Reduction Reaction Supported on Different Carbonaceous Materials. Performance in Acidic and Alkaline Direct Alcohol Fuel Cells. Appl. Catal. B 2017, 205, 637–653. [Google Scholar] [CrossRef] [Scilit]
  73. Wei, Y.; Shengzhou, C.; Weiming, L. Oxygen Reduction on Non-Noble Metal Electrocatalysts Supported on N-Doped Carbon Aerogel Composites. Int. J. Hydrogen Energy 2012, 37, 942–945. [Google Scholar] [CrossRef] [Scilit]
  74. Ratso, S.; Kruusenberg, I.; Sarapuu, A.; Kook, M.; Rauwel, P.; Saar, R.; Aruväli, J.; Tammeveski, K. Electrocatalysis of Oxygen Reduction on Iron- and Cobalt-Containing Nitrogen-Doped Carbon Nanotubes in Acid Media. Electrochim. Acta 2016, 218, 303–310. [Google Scholar] [CrossRef] [Scilit]
  75. Zainoodin, A.M.; Tsujiguchi, T.; Masdar, M.S.; Kamarudin, S.K.; Osaka, Y.; Kodama, A. Performance of a Direct Formic Acid Fuel Cell Fabricated by Ultrasonic Spraying. Int. J. Hydrogen Energy 2018, 43, 6413–6420. [Google Scholar] [CrossRef] [Scilit]
  76. Tsujiguchi, T.; Matsuoka, F.; Hokari, Y.; Osaka, Y.; Kodama, A. Overpotential Analysis of the Direct Formic Acid Fuel Cell. Electrochim. Acta 2016, 197, 32–38. [Google Scholar] [CrossRef] [Scilit]
  77. Jiang, K.; Cai, W. Bin Carbon Supported Pd-Pt-Cu Nanocatalysts for Formic Acid Electrooxidation: Synthetic Screening and Componential Functions. Appl. Catal. B 2014, 147, 185–192. [Google Scholar] [CrossRef] [Scilit]
  78. Meng, H.; Zeng, D.; Xie, F. Recent Development of Pd-Based Electrocatalysts for Proton Exchange Membrane Fuel Cells. Catalysts 2015, 5, 1221–1274. [Google Scholar] [CrossRef] [Scilit]
  79. Waszczuk, P.; Barnard, T.M.; Rice, C.; Masel, R.I.; Wieckowski, A. A Nanoparticle Catalyst with Superior Activity for Electrooxidation of Formic Acid; Elsevier: Amsterdam, The Netherlands, 2002. [Google Scholar]
  80. Jayashree, R.S.; Spendelow, J.S.; Yeom, J.; Rastogi, C.; Shannon, M.A.; Kenis, P.J.A. Characterization and Application of Electrodeposited Pt, Pt/Pd, and Pd Catalyst Structures for Direct Formic Acid Micro Fuel Cells. Electrochim. Acta 2005, 50, 4674–4682. [Google Scholar] [CrossRef] [Scilit]
  81. Kim, K.H.; Yu, J.-K.; Lee, H.S.; Choi, J.H.; Noh, S.Y.; Yoon, S.K.; Lee, C.-S.; Hwang, T.-S.; Rhee, Y.W. Preparation of Pt-Pd Catalysts for Direct Formic Acid Fuel Cell and Their Characteristics. Korean J. Chem. Eng. 2007, 24, 518–521. [Google Scholar] [CrossRef] [Scilit]
  82. Attard, G.A.; Bannister, A. The Electrochemical Behaviour of Irreversibly Adsorbed Palladium on Pt(111) in Acid Media; Elsevier Sequoia S.A: Amsterdam, The Netherlands, 1991; Volume 300. [Google Scholar]
  83. Morlang, A.; Neuhausen, U.; Klementiev, K.V.; Schütze, F.W.; Miehe, G.; Fuess, H.; Lox, E.S. Bimetallic Pt/Pd Diesel Oxidation Catalysts: Structural Characterisation and Catalytic Behaviour. Appl. Catal. B 2005, 60, 191–199. [Google Scholar] [CrossRef] [Scilit]
  84. Kim, T.; Takahashi, M.; Nagai, M.; Kobayashi, K. Preparation and Characterization of Carbon Supported Pt and PtRu Alloy Catalysts Reduced by Alcohol for Polymer Electrolyte Fuel Cell. Proc. Electrochim. Acta 2004, 50, 817–821. [Google Scholar] [CrossRef] [Scilit]
  85. Juchniewicz, K.; Pieta, I.S.; Mierzwa, B.; Pisarek, M.; Kadam, R.G.; Mozgova, O.; Holdynski, M.; Malolepszy, A.; Borodzinski, A.; Pieta, P. Codeposited Bimetallic Pt-Pd Catalyst Supported on MWCNTs/Carbon Cloth as an Efficient DFAFC Anode Material. ACS Sustain. Chem. Eng. 2025, 13, 9609–9620. [Google Scholar] [CrossRef] [Scilit]
  86. Muthukumar, V.; Chetty, R. Electrodeposited Pt–Pd Dendrite on Carbon Support as Anode for Direct Formic Acid Fuel Cells. Ionics 2018, 24, 3937–3947. [Google Scholar] [CrossRef] [Scilit]
  87. Hong, P.; Luo, F.; Liao, S.; Zeng, J. Effects of Pt/C, Pd/C and PdPt/C Anode Catalysts on the Performance and Stability of Air Breathing Direct Formic Acid Fuel Cells. Int. J. Hydrogen Energy 2011, 36, 8518–8524. [Google Scholar] [CrossRef] [Scilit]
  88. Kajba, M.; Jereb, B.; Cvahte Ojsteršek, T. Exploring Digital Twins in the Transport and Energy Fields: A Bibliometrics and Literature Review Approach. Energies 2023, 16, 3922. [Google Scholar] [CrossRef] [Scilit]
  89. Yu, P.; Li, M.; Wang, Y.; Chen, Z. Fuel Cell Hybrid Electric Vehicles: A Review of Topologies and Energy Management Strategies. World Electr. Veh. J. 2022, 13, 172. [Google Scholar] [CrossRef] [Scilit]
  90. Meraghni, S.; Terrissa, L.S.; Yue, M.; Ma, J.; Jemei, S.; Zerhouni, N. A Data-Driven Digital-Twin Prognostics Method for Proton Exchange Membrane Fuel Cell Remaining Useful Life Prediction. Int. J. Hydrogen Energy 2021, 46, 2555–2564. [Google Scholar] [CrossRef] [Scilit]
  91. Tang, A.; Yang, Y.; Yu, Q.; Zhang, Z.; Yang, L. A Review of Life Prediction Methods for PEMFCs in Electric Vehicles. Sustainability 2022, 14, 9842. [Google Scholar] [CrossRef] [Scilit]
  92. Wilkinson, M.D.; Dumontier, M.; Aalbersberg, I.J.; Appleton, G.; Axton, M.; Baak, A.; Blomberg, N.; Boiten, J.W.; da Silva Santos, L.B.; Bourne, P.E.; et al. Comment: The FAIR Guiding Principles for Scientific Data Management and Stewardship. Sci. Data 2016, 3, 160018. [Google Scholar] [CrossRef] [Scilit]
  93. Xiao, F.; Wang, Q.; Xu, G.L.; Qin, X.; Hwang, I.; Sun, C.J.; Liu, M.; Hua, W.; Wu, H.w.; Zhu, S.; et al. Atomically Dispersed Pt and Fe Sites and Pt–Fe Nanoparticles for Durable Proton Exchange Membrane Fuel Cells. Nat. Catal. 2022, 5, 503–512. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.