Abstract
BO33−, PO43−, and SO42− anionic groups were used to study their effects on the structure and luminescence of Sm3+-doped ZnO. ZnO, ZnO:Sm3+, ZnO, Zn4B6O13:Sm3+, and Zn2P2O7:Sm3+ phosphors were successfully synthesized via combustion synthesis. While BO33− and PO43− ions led to the formation of new crystalline phases, the sulfate precursor decomposed during synthesis, yielding ZnO with only minor surface sulfur traces. The XRD results revealed the formation of wurtzite crystal structures in the ZnO, ZnO:Sm3+, and ZnO-SO4:Sm3+ samples, while a complete change of structure was observed after the incorporation of borate (BO33−) and phosphate (PO43−) ions into ZnO:Sm3+ to Zn4B6O13:Sm3+ and Zn2P2O7:Sm3+, respectively. The structures for borate and phosphate ions were confirmed as cubic (Zn4B6O13) and monoclinic (Zn2P2O7) crystal structures, respectively. The morphological studies of ZnO:Sm3+ and ZnO-SO4:Sm3+ were characterized by aggregated particles with different shapes and sizes. Zn4B6O13 and Zn2P2O7 samples were characterized by having cubic and rough surfaces, respectively. The oxidation state of the Sm ions was confirmed by XPS analysis. The photoluminescence studies revealed a broad-band emission for the ZnO:Sm3+ and ZnO-SO4:Sm3+ materials and characteristic Sm3+ emissions (from the 4G5/2 level to lower states 6HJ (J = 5/2, 7/2, 9/2, and 11/2)) for the Zn4B6O13 and Zn2P2O7 samples. Enhanced emissions were observed after the incorporation of anionic group systems. The most intense PL emission was observed from the Zn4B6O13 phosphor material. The CIE calculations revealed that the best color purity results were from Zn4B6O13, which lay in the orange region with 98% color purity.
1. Introduction
Solid-state lighting in the form of LEDs has been favored in comparison to incandescent and fluorescent lamps, and this is because of interesting characteristics, such as a higher brightness, low power consumption, high efficiency, and being environmentally friendly [1,2,3,4]. The production of light by these materials depends on selective phosphor materials emitting light in the visible region by a UV excitation source [4]. Recently, w-LEDs have been made by two methods, which include coating a blue-emitting InGaN chip with a yellow-emitting YAG:Ce3+ phosphor material [5] and combining near-UV LEDs with tri-color emitting phosphor materials. White light produced by such methods usually has some drawbacks due to the lack of a red ingredient, which leads to a low color rendering index (CRI) and high correlated color temperature (CCT) [5]. These drawbacks can be overcome by improving the red components in the selected host materials with relevant dopant ions excited by an NUV LED chip [6,7,8].
ZnO is a semiconducting material and a widely studied phosphor due to its wide utility in solar cells [9], gas sensors [10], LEDs [11], and applications in optoelectronics [12]. It has a wide direct band gap of 3.37 eV and a large binding energy of 60 meV. These characteristics make it an ideal material for incorporating dopants into the ZnO matrix. Rare earth dopants, which have partially filled 4f electrons, can be easily incorporated into ZnO to tune its optical properties. These rare earths, when incorporated into ZnO, allow parity-forbidden 4f-4f transitions and defect emissions to take place [13]. Sm3+() is a rare earth ion that is widely known as a dopant due to its strong orange-red luminescence in the visible region and has applications in high-density optical storage systems, undersea communication systems, solid-state lasers, etc. [14].
The generation of white light by combining a blue LED with a yellow phosphor, such as Y3Al5O12:Ce3+, suffers from a low color rendering index and high correlated color temperature. Attempts to solve this involve exciting the RGB phosphor by a near-UV semiconductor chip for generating white light. However, this approach is not widely used because of the ineffective absorption of n-UV by red phosphors such as Y2O2S:Eu3+ from the semiconductor chip [15]. Therefore, there is a need to develop a red phosphor that has effective n-UV absorption abilities with enhanced emission intensities.
Amongst other red-emitting phosphors, Sm3+ serves as a better choice due to its low cost [16]. In the Sm3+ configuration, the 4f electrons are shielded by the outer 5s and 5p orbitals, which retain the atomic character of Sm3+. Thus, its characteristic transitions are not affected much by the host material. This results in a strong emission from Sm3+ ions due to transitions such as 4G5/2 → 6HJ (J = 5/2, 7/2, 9/2, and 11/2) of the energy level [17,18]. Most Sm3+-doped phosphors tend to show effective absorption characteristics in the wavelength 380–420 nm [19,20]. Gupta et al. [21] investigated perovskite-type YAlO3:xSm3+ with varying concentrations of Sm3+ for application in n-UV-energized WLEDs. Kumari et al. [22] co-doped Sm3+ and Eu3+ ions in Sr9Y2W4O24 red-emitting phosphors for effective energy transfer from Sm3+ to Eu3+. Their findings revealed that n-UV light may effectively excite the Sr9Y2W4O24:Sm3+/Eu3+ co-doped phosphor material. In recent years, it has been demonstrated by different research groups that partial replacement of anionic groups in ZnO can greatly increase light emission from the dopant ions. B. Avula et al.’s [23] and M.L.A Letswalo et al.’s [24] research works demonstrated considerable improvement in red photoluminescence (PL) from Eu3+ in host lattices such as calcium molybdate, double molybdate, and calcium titanium oxide. The substitution of anionic groups like SO42−, PO43−, SiO32−, and BO33− has produced striking improvements in red PL. The mechanism of such improvement is, however, not yet clearly understood. In order to fill this gap, a study was carried out to examine the manner in which the substitution of these anionic groups increases PL intensity. Furthermore, earlier studies [23,24] discovered that partial replacement of these anions can affect the color purity of the emitted red light in phosphor materials.
In this study, ZnO, ZnO:Sm3+, Zn4B6O13:Sm3+, Zn2P2O7:Sm3+, ZnO-SO4, and ZnO-SO4:Sm3+ phosphors were synthesized via urea-assisted combustion. ZnO-SO4:Sm3+ retained the wurtzite structure of ZnO when synthesized in the presence of ammonium sulfate, which acts as a combustion modifier rather than a dopant. After annealing at 1000 °C, the products remained as ZnO, as confirmed by XRD analysis. The influence of the anions as a tuning parameter was investigated for their luminescence, optical, and structural properties to see which phosphor material produced the best luminescence of all anionic group-doped materials. This work was inspired by the work of Balakrishna and co-workers, who substituted different anions into the CaMoO4 host material, which, when doped with Sm3+ ion, produced a 30 times more intense red emission when excited by an NUV LED chip [23]. Furthermore, doping with BO33− and PO42− ions by combustion synthesis may influence the crystal structure formation of the material, and different types of borate and phosphate structures may be formed, respectively. In the case of BO33−, some of the possible borate structures that may form include ZnB4O7, ZnB2O4, Zn4B6O13, or Zn3(BO3)2 [25,26]. Similar behavior of structural change when introducing the borate (BO33−) unit into a different host material was observed by Tamboli et al. [27]. In their work, the crystal structure was changed from the monoclinic phase of Ba2Mg(PO4)2 to the rhombohedral phase of Ba2Mg(BO3)2 when they introduced the BO33− ions into Ba2Mg(PO4)2 material. For PO42− doping, possible formations of phosphate may include Zn2P2O7, Zn3P2O8, or ZnP2O6 [28,29,30]. In this work, a notable phase change was observed when introducing BO33− and PO42− ions, significantly influencing the material’s structural and optical properties. In contrast, the ZnO initially doped with SO42− anion maintains the same phase as the host, consistent with the findings reported by Letswalo et al. [24] using the solid-state reaction method. The structural variation induced by the introduction of BO33− and PO42− anions are analyzed by XRD and Rietveld refinement.
2. Results and Discussion
2.1. X-Ray Diffraction—Phase Identification
Figure 1 shows the XRD patterns of ZnO, ZnO:Sm3+, Zn4B6O13:Sm3+, Zn2P2O7:Sm3+, and ZnO-SO4:Sm3+ phosphors synthesized via urea-assisted combustion. ZnO-SO4:Sm3+ retained the wurtzite structure of ZnO when synthesized in the presence of ammonium sulfate, which acts as a combustion modifier rather than a dopant. After annealing at 1000 °C, the products remained as ZnO, as confirmed by XRD analysis. The XRD peaks of the undoped ZnO host material (Figure 1a) correspond to those of a hexagonal crystal structure and are well matched with the standard background ZnO structure (PDF file number 04-022-5463) with a space group of P63mc [31]. These diffraction peaks were found around 2θ angles of 32°, 35°, 37°, 48°, 57°, 63°, 67°, 68°, 70°, 73°, 77°, 82°, and 87°, which are well indexed as (100), (002), (101), (102), (110), (103), (200), (112), (201), (004), (202), (104), and (203) crystal planes of the material, respectively, and whose lattice parameters are a = b = 3.25 Å and c = 5.21 Å [31]. However, when adding the other two anions (PO42− and BO33−) into ZnO (Figure 1d,e), the crystal structure was altered completely from a hexagonal wurtzite crystal structure to monoclinic zinc pyrophosphate (Zn2P2O7) and cubic zinc metaborate (Zn4B6O13) crystal structures for PO42− and BO33−, respectively. This behavior was not observed in the work of Balakrishna et al. [23], where they added the anions into a different host material. The diffraction peaks of the Zn4B6O13 phosphor material are well matched with its reference background structure (PDF file number 01-080-7675) with a space group of I-43m, with cubic lattice parameters of a = b = c = 7.48 Å [32]. These diffraction peaks were found around at 2θ angles of 17°, 26°, 30°, 35°, 38°, 42°, 46°, 50°, 55°, 58°, 62°, 65°, 70°, 72°, 75°, 77°, 80°, 82°, 85°, and 90° and are well indexed as (110), (200), (211), (220), (310), (222), (321), (400), (300), (332), (422), (431), (521), (440), (433), (442), (532), (620), (541), and (631) crystal planes of the material, respectively. The addition of the dopant Sm3+ into the Zn4B6O13 phosphor material did not change its cubic crystal structure; there were no additional peaks observed. In a similar manner, the addition of the phosphate (PO42−) group into the ZnO matrix resulted in a change of crystal structure to a monoclinic zinc pyrophosphate crystal structure. The diffraction pattern of Zn2P2O7 is well matched with the background reference crystal structure (PDF file number 04-009-2628) with a space group of C2/c and with monoclinic lattice parameters of a = 6.61 Å, b = 8.29 Å, and c = 4.51 Å [28]. These diffraction peaks were found at 2θ angles of 17°, 20°, 21°, 25°, 27°, 29°, 35°, 40°, 44°, 48°, 53°, 59°, 63°, and 70°, which are well indexed as (310), (01), (311), (510), (600), (222), (330), (14), (910), (42), (442), (25), (52), and (843) crystal planes of the material, respectively. The crystal structures of ZnO, Zn4B6O13, and Zn2P2O7 materials are displayed in Figure 2.
Figure 1.
XRD patterns of (a) ZnO, (b) ZnO:Sm3+, (c) ZnO-SO4:Sm3+, (d) Zn4B6O13:Sm3+, and (e) Zn2P2O7:Sm3+ and (f) enlarged XRD pattern of ZnO, ZnO-SO4, ZnO:Sm3+, and ZnO-SO4:Sm3+.
Figure 2.
Crystal structure for ZnO, Zn4B6O13, and Zn2P2O7 materials.
It appears that the addition of the dopant Sm3+ to the Zn2P2O7 has no significant effect on the diffraction patterns; the monoclinic crystal structure was preserved. Figure 1f presents the magnified 2θ region (31–37°) of the ZnO-based materials. It is evident that the incorporation of ammonium sulfate, intended to introduce SO42− ions into the ZnO lattice, did not result in any significant structural modification and was not successful. This is likely because sulfate species decompose at temperatures below the synthesis temperature (600 °C), leading to volatilization of sulfur as gaseous oxides such as SO3. Consequently, ZnO remains the dominant crystalline phase. The slight and negligible peak shift observed may be attributed to minor surface adsorption or residual impurities rather than actual lattice substitution, as shown in Figure 1f [24,33]. The Sm3+ ion on the other side causes a 2θ shift to the left. The shift to the lower angle suggests that the Sm3+ ion with a larger ionic radius (1.09 Å) substitutes the smaller-sized Zn2+ (0.74 Å) [34]; this will cause an increase in the interplanar d-spacing [22]. In order to retain Bragg’s law 2dsinθ = n, where n remains constant, the angle θ should shift to lower angles [21].
The average crystallite sizes were estimated from the XRD patterns using the Debye–Scherrer equation:
where D is the average crystallite size and k is the shape factor, while β is the full width at half maximum (FWHM) and θ is the diffraction angle for the diffraction peak [35]. Table 1 below presents the estimated crystallite sizes. The materials with a ZnO hexagonal crystal structure show similar crystallite sizes; however, for the ZnO-SO4:Sm3+ sample, the crystallite size is lower by as much as 10 nm. The smaller crystallite size agrees with the XRD peak broadening of the ZnO-SO4:Sm3+ compared to other ZnO samples. All numerical values are presented with estimated uncertainties derived from the instrumental resolution and data fitting precision. The crystallite size error (±0.8–1.0 nm) was determined from multiple peak broadening fits using the Scherrer equation. Lattice parameters and cell volumes have uncertainties of ±0.001–0.005 Å and ±0.1–1.5 Å3, respectively. To obtain a clear indication of the changes that occur in the structure when introducing the dopant ions, the structural refinements were performed using the Rietveld refinement (RR) method in the Expo-2014 program (Figure 3). The agreement factors and the cell parameters derived from refinement are tabulated in Table 2. After the introduction of Sm3+ ions into the crystal structure, the ZnO-SO4:Sm3+ retained the hexagonal phase of the host material, and the cell volumes were very close. Substituting BO33− and PO42− ions completely formed new phases. This behavior was not observed when substituting with sulfate precursors, mainly because the sulfate decomposes below the synthesis temperature (600–1000 °C), resulting in the evolution of sulfur trioxide (SO3) gas rather than retention of SO42− ions in the ZnO lattice. The goodness of fit (χ2) plays a significant role in the process of Rietveld refinement and is described as follows [36]:
where Rwp is the weighted profile factor and Rexp is the expected profile factor. Based on the findings of the RR analysis, the calculated χ2 values for the prepared phosphors exhibit a range of values, suggesting the presence of favorable characteristics. Any minor discrepancies observed are likely attributed to internal strain, as the relevant peaks are more accurately described by a Gaussian function. The RR analysis indicates that the crystallographic characteristics, volumes, and refinement factors of the solid samples are highly comparable. The fitting graphs correspond well with the experimental outcomes, verifying the hexagonal structure of ZnO, ZnO:Sm3+, and ZnO-SO4:Sm3+, cubic structure of Zn4B6O13:Sm3+, and monoclinic framework of Zn2P2O7:Sm3+ phosphors, which closely align with the crystal structure information of the respective standard JCPDS cards.
Table 1.
Estimated crystallite sizes of ZnO, ZnO:Sm3+, Zn4B6O13:Sm3+, Zn2P2O7:Sm3+, and ZnO-SO4:Sm3+ samples and their respective lattice parameters.
Figure 3.
Rietveld analysis of ZnO, ZnO:Sm3+, ZnO-SO4:Sm3+, Zn4B6O13:Sm3+, and Zn2P2O7:Sm3+ phosphors.
Table 2.
Crystallographic data from Rietveld refinement of ZnO, ZnO:Sm3+, ZnO-SO4:Sm3+, Zn4B6O13:Sm3+, and Zn2P2O7:Sm3+ phosphors.
2.2. Morphological Study
Figure 4 and Figure 5 show the SEM images and EDS spectra, respectively, of the ZnO:Sm3+, Zn4B6O13:Sm3+, Zn2P2O7:Sm3+, and ZnO-SO4:Sm3+ samples. Figure 4a shows Sm3+ (1mol%)-doped ZnO phosphors with a cluster type of spherical particles with different sizes and shapes. A sponge-like morphology made up of fused micro-grains with pore sizes centered at (0.651 μm) and an average grain diameter of (0.721 μm) is revealed by the SEM image. Figure 6a,b shows the particle sizes and pore sizes distributions of the ZnO:Sm3+ material. A high specific surface area is suggested by the open porous network, which is consistent with quick nucleation and aggregation during synthesis [37]. Due to structural change, a completely different type of morphology was observed for the Zn4B6O13:Sm3+ material (Figure 4b). This phosphor is characterized by clustered cubic types of particles with sharp edges and smooth surfaces. Under the synthesis conditions used, SEM (Figure 4b) shows well-defined faceted microcrystals with a dominant cubic/rectangular habit and an average particle size of 1.981 μm, indicating robust crystal growth and high crystallinity. The typical size distribution of this material is presented in Figure 6c. This type of morphology is typical of Zn4B6O13:Sm3+ and is in good agreement with the XRD results. The EDS spectra of ZnO:Sm3+ and Zn4B6O13:Sm3+ are represented in Figure 5a,b, respectively. The morphological structures of the Zn2P2O7:Sm3+ and ZnO-SO4:Sm3+ phosphor materials are represented in Figure 4c,d, respectively. Zn2P2O7:Sm3+ materials are characterized by rough surfaces with scattered particles of irregular shapes and sizes across the surface. These materials have some pores on the surface, which may be because of escaping gases during the synthesis process. Similarly, ZnO-SO4:Sm3+ (Figure 4d) phosphor has aggregated particles throughout the surface with different shapes and sizes. The pores observed in these materials are due to escaping gases during fabrication. The microstructure of Zn2P2O7:Sm3+ (Figure 4c) is primarily smooth and compact, with sparse granular features approximately 0.767 μm on average, suggesting a denser morphology that can reduce surface-related non-radiative recombination. The sparse granular distribution of Zn2P2O7:Sm3+ is represented in Figure 6d. The EDS spectra for Zn2P2O7:Sm3+ and ZnO-SO4:Sm3+ phosphors shown in Figure 5c,d, respectively, confirm the presence of all the individual elements in the respective phosphor material. For the ZnO-SO4:Sm3+ material, the EDS spectrum reveals a very low sulfur content (≈0.5 wt%). This low S content can be attributed to the synthesis conditions. Although ammonium sulfate was introduced as a precursor to supply sulfate ions intended to act as dopants, the high processing temperature likely caused thermal decomposition of sulfate species, resulting in the release of volatile gases such as SO2 or SO3 [38,39]. The EDS spectra of all materials reveal the presence of carbon in the samples, which did not form part of the precursors. The presence of carbon is due to the carbon coating that was used during analysis, and the unexpected detection of Na in all samples may be due to surface contamination.
Figure 4.
SEM images of (a) ZnO:Sm3+, (b) Zn4B6O13:Sm3+, (c) Zn2P2O7:Sm3+, and (d) ZnO-SO4:Sm3+.
Figure 5.
EDS spectra of (a) ZnO:Sm3+, (b) Zn4B6O13:Sm3+, (c) Zn2P2O7:Sm3+, and (d) ZnO-SO4:Sm3+.
Figure 6.
Average particle size of (a) ZnO:Sm3+, (b) average pore size of ZnO:Sm3+, and average particle size of (c) Zn4B6O13:Sm3+ and (d) Zn2P2O7:Sm3+.
2.3. FTIR Measurements
The FTIR spectra of ZnO:Sm3+, Zn4B6O13:Sm3+, Zn2P2O7:Sm3+, and ZnO-SO4:Sm3+ phosphors are depicted in Figure 7. The spectra are recorded in the wavenumber range from 400 to 4000 cm−1 measured at room temperature. The Zn-O bonds are revealed by the presence of a broad transmission band found between 450 and 650 cm−1 observed in the ZnO crystal structure materials [40,41]. The transmission bands around 3000–3700 cm−1 and around 1700 cm−1 observed in all samples are attributed to the O-H stretching modes of water moisture that settled on the sample surface during the fabrication process [14,42].
Figure 7.
FTIR spectra of ZnO, ZnO:Sm3+, Zn4B6O13:Sm3+, Zn2P2O7:Sm3+, and ZnO-SO4:Sm3+ phosphor materials.
More transmission bands are observed for Zn4B6O13:Sm3+and Zn2P2O7:Sm3+ samples, which resulted in a different crystal structure from that of ZnO. For the Zn2P2O7:Sm3+ sample, characteristic transmission bands of symmetric and asymmetric PO3 functional groups are observed in the region around 1000–1200 cm−1 [43]. The symmetric modes of PO3 groups appear as a shoulder situated at 1078 cm−1 [44]. Similarly, the Zn4B6O13:Sm3+ FTIR spectrum shows three characteristic transmission bands at 600–700 cm−1, 800–950 cm−1, and 1200–1500 cm−1, which are attributed to B-O-B bending modes of BO3 and BO4 units, B-O stretching of the BO4 tetrahedral unit, and asymmetric stretching relaxations of the B-O bonds of the BO3 trigonal unit, respectively [45,46,47]. The transmission bands between 450 and 500 cm−1 are also attributed to BO4 units [42]. The FTIR analysis of ZnO-SO4:Sm3+ confirms the absence of characteristic sulfate ion vibrations (1100–1300 cm−1), indicating that sulfate species were not incorporated into the ZnO lattice. This observation is consistent with the XRD results [48], which show that ZnO remains the dominant crystalline phase. This suggests that during high-temperature combustion synthesis, the sulfate precursor decomposed and volatilized—likely as SO3 or SO2 gases. This finding corroborates that the detected 0.5 wt% sulfur in the EDS spectrum most likely originates from surface contamination or residual surface species.
2.4. UV–Visible and Band Gap Measurements
The UV–visible reflectance spectra of undoped ZnO, ZnO:Sm3+, Zn4B6O13:Sm3+, Zn2P2O7:Sm3+, and ZnO-SO4:Sm3+ phosphor materials are presented in Figure 8a. The spectra are recorded in the spectral wavelength range from 200 to 800 nm. It is observed that all prepared materials show high and low reflectance intensities in the visible and UV regions, respectively. Similar reflectance behavior is observed for all materials with a wurtzite crystal structure, both in the visible and UV regions of the DSR spectra, and this is due to the similarity of their crystal structure. From these ZnO materials, the undoped ZnO has the highest reflectance intensity while the ZnO-SO4:Sm3+ has the lowest in the visible region. This is likely due to the sulfate volatilizing as SO3 during high-temperature synthesis, resulting in the crystal structure remaining intact but being influenced by residual sulfur contamination. The effect of Sm3+ doping is clearly observed in the DRS spectra of the ZnO:Sm3+ and ZnO-SO4:Sm3+ phosphor materials. The absorption band situated at 478 nm in these samples is due to the Sm3+ transitions. On the other hand, the other two substituted anionic groups, BO33− and PO42−, which resulted in different crystal structures, also show different behavior in the DSR spectra as compared to the ZnO materials. The reflectance of these materials (Zn4B6O13:Sm3+and Zn2P2O7:Sm3+) lies deep in the UV region of the DSR spectra. The observed absorption bands for Sm3+-doped samples in the region 300 to 500 nm are attributed to the 4f5→ 4f5 intra-configurational transitions from the ground state (6H5/2) to various excited states 3H7/2 (345 nm), 4F9/2 (363 nm), 4D5/2 (376 nm), 6F7/2 (403 nm), 4I13/2 (365 nm), and 4I11/2 (478 nm) of the Sm3+ ion [16,49,50]. The presence of these bands shows that the atomic nature of Sm3+ is not affected much by the host material; only weak interactions are present between the host and the dopant ions [49]. This implies that there is an effective shielding of the forbidden 4f5 electrons by the filled 5s and 5p shells of Sm3+ ions.
Figure 8.
(a) UV-Vis spectra of ZnO, ZnO:Sm3+, Zn4B6O13:Sm3+, Zn2P2O7:Sm3+, and ZnO-SO4:Sm3+ phosphors material with 1mol% of Sm3+ ion, (b) optical gap of ZnO, ZnO:Sm3+, ZnO-SO4:Sm3+,Zn4B6O13:Sm3+, and Zn2P2O7:Sm3+ phosphors, and (c) enlarged figure showing the optical gap of the Zn4B6O13:Sm3+ and Zn2P2O7:Sm3+ phosphors.
The optical energies of ZnO, ZnO:Sm3+, Zn4B6O13:Sm3+, Zn2P2O7:Sm3+, and ZnO-SO4:Sm3+ phosphors were estimated from Kubelka–Munk (M-K) function theory by using data from Figure 8a [51]. The method adopted from the Tauc equation can be represented in the following form [51]:
Figure 8b,c show the plots of [ as a function of photon energy hν for direct transitions. Extrapolations of the best linear parts of the curve to the x-intercept at zero absorption give the band gap energy values [52,53,54]. The estimated band gap values are presented in Table 3.
Table 3.
Band gap energies of ZnO, ZnO:Sm3+, Zn4B6O13:Sm3+, Zn2P2O7:Sm3+, and ZnO-SO4:Sm3+ materials estimated from the Kubelka–Munk plot.
The band gaps for the pure ZnO, ZnO:Sm3+, Zn4B6O13:Sm3+, Zn2P2O7:Sm3+, and ZnO-SO4:Sm3+ phosphor materials appear to remain unchanged for the ZnO:Sm3+ sample, and this band gap becomes smaller for other samples when anionic groups are introduced, as tabulated in Table 3. Accordingly, by introducing various anionic groups, the band gap values are Zn4B6O13:Sm3+ (3.145 eV), Zn2P2O7:Sm3+ (2.830 eV), and ZnO-SO4:Sm3+ (3.165 eV) for the respective anions. The variation profile of band gap values clearly indicates that Zn4B6O13:Sm3+, Zn2P2O7:Sm3+, and ZnO-SO4:Sm3+ show lower band gap values compared to ZnO and ZnO:Sm3+ materials, with the Zn2P2O7:Sm3+ material having the smallest band gap value. The smaller decrease in the band gap of the ZnO-SO4:Sm3+ sample, which retained the hexagonal structure, is mainly due to the volatilization of the sulfate during synthesis, as observed from the DSR spectra. Numerical values are presented with estimated uncertainties derived from the instrumental resolution and data fitting precision of the optical band gap values, which carry a ±0.01–0.02 eV experimental error based on Tauc plot fitting.
2.5. XPS Analysis
The XPS of ZnO, Zn4B6O13, and Zn4B6O13:Sm3+ were performed in order to assess the elemental states of the present elements in these materials. Figure 9 presents the XPS survey of ZnO, Zn4B6O13, and Zn4B6O13:Sm3+ phosphors recorded from a binding energy of 1400 to 0 eV. The composition of our samples is confirmed in Figure 9, as we can observe that the ZnO host sample contains core-level peaks from Zn 2p and O 1s, Zn4B6O13 shows core-level peaks from Zn 2p, O1s, and B 1s only, and Zn4B6O13:Sm3+ contains peaks from Zn 2p, O1s, B 1s, and Sm 3d [55,56]. This is in good correspondence with our EDS findings. Figure 10 shows high-resolution XPS spectra of Sm 3d, O 1s, B 1s, and Zn 2p bands from the prepared phosphors. From Figure 10a we observe two well-separated peaks of Sm 3d located at 1110.27 and 1082.95 eV, corresponding to Sm 3d3/2 and Sm 3d5/2, respectively [57]. The binding energy difference of these two peaks is 27.32 eV, which confirms the +3-oxidation state of the Sm ion in the Zn4B6O13:Sm3+ sample [51,53,58]. The high-resolution spectra of O 1s and B 1s are represented in Figure 10b,c, respectively, for Zn4B6O13 and Sm-activated Zn4B6O13 samples. The binding energy curve of B 1s located at 191.02 eV is attributed to photoelectrons originating from B atoms bounded to oxygen (B-O) in the Zn4B6O13 matrix [56]. The Zn 2p XPS spectra, Figure 10d, reveal the Zn 2p1/2 and Zn 2p3/2 peaks located at a binding energy of 1045.01 eV and 1022.14 eV, respectively. These two peaks are characteristic of ZnO, and the binding energy difference of 22.87 eV also confirms the formation of ZnO material [55]. The peak located at a binding energy of 284 eV is attributed to carbon (C1s), which is due to the instrument; the C1s peak is normally used as the reference peak in determining the binding energies of other elements [59].
Figure 9.
XPS survey of ZnO, Zn4B6O13, and Zn4B6O13:Sm3+ phosphors.
Figure 10.
High-resolution XPS spectra of (a) Sm 3d, (b) O 1s, (c) B 1s, and (d) Zn 2p.
2.6. Photoluminescence Studies
The PL excitation spectra of ZnO:Sm3+, Zn4B6O13:Sm3+, Zn2P2O7:Sm3+, and ZnO-SO4:Sm3+ materials while monitoring at an emission wavelength of 600 nm are presented in Figure 11. The borate and phosphate materials show some intense excitation peaks as compared to other phosphor materials. The excitation band observed in the region between 200 and 275 nm can be associated with the charge transfer of Sm3+→ O2− [14]. The intense excitation peaks are due to transitions from the ground state of Sm3+ (6H5/2) to various excited states such as 3H7/2, 4F9/2, 4D5/2, 4F7/2,4I13/2 and 4I11/2 located at 345 nm, 361 nm, 376 nm, 403 nm, 470 nm, and 486 nm wavelengths, respectively [60]. From these excitation peaks, the most intense peak observed at 403 nm is used as an excitation wavelength for the PL emission scan of these materials. The highest intensity for this transition is observed in the Zn4B6O13:Sm3+ sample.
Figure 11.
PL excitation spectra of ZnO:Sm3+, Zn4B6O13:Sm3+, Zn2P2O7:Sm3+, and ZnO-SO4:Sm3+ phosphor materials with 1 mol% of Sm3+ ion monitored under 600 nm wavelength.
The PL emission scan for the prepared materials was carried out using an excitation wavelength of 403 nm (Sm3+ ion), and the spectra are displayed in Figure 12. In the wavelength region 400–800 nm, the characteristic Sm3+ emissions are only observed from the Zn4B6O13:Sm3+ and Zn2P2O7:Sm3+ samples, while the other materials show negligible emissions (see insert of Figure 12). The absence of characteristic Sm3+ emissions from ZnO:Sm3+ and ZnO-SO4:Sm3+ may be due to the host influences on the Sm3+ luminescence properties. The absence of characteristic Sm3+ emissions from ZnO:Sm3+ may be attributed to the strong influence of the ZnO host lattice defects on the luminescence properties of Sm3+ ions. In the ZnO-SO4:Sm3+, the low emission intensity could result from partial decomposition or volatilization of the sulfate species as SO3 during high-temperature synthesis, which alters the local chemical environment of Sm3+. Additionally, ZnO may induce non-radiative relaxation processes or inefficient energy transfer between the host and the Sm3+ activator, leading to luminescence quenching. Figure 13 shows a schematic representation of Sm3+ energy levels within the Zn4B6O13:Sm3+ and Zn2P2O7:Sm3+ phosphors. Firstly, when excited with 403 nm, the 6H5/2 level of Sm3+ transitions to a higher energy state, followed by non-radiative relaxations to the metastable level 4G5/2. Finally, the 4G5/2 level depopulation to the ground state results in different Sm3+ emissions [61]. The four characteristic Sm3+ emissions observed from Zn4B6O13:Sm3+ and Zn2P2O7:Sm3+ samples located at 563 nm, 605 nm, 656 nm, and 720 nm correspond to 4G5/2 → 6H5/2, 4G5/2 → 6H7/2, 4G5/2 → 6H9/2, and 4G5/2 → 6H11/2 transitions, respectively [14,60]. The highest intensity is observed from the Zn4B6O13:Sm3+ material. This high intensity may be attributed to the high crystallinity of the borate material. Of these Zn4B6O13:Sm3+ emissions, the most intense is from the 4G5/2 → 6H9/2 transition. The Zn2P2O7:Sm3+ sample, which has the second highest Sm3+ emission intensity, has the most intense peak located at 605, which is assigned to a 4G5/2 → 6H7/2 transition. From these Sm3+ emission bands, the emissions at 656 nm and 720 nm are attributed to the electric dipole (ED) contributions [14,49], while the other two emission bands at 605 nm and 563 nm are attributed to both electric and magnetic dipole (MD) contributions [14,49]. From the combinations of dipole contributions at these sites, the magnetic dipole contribution at 6H5/2 is most dominant, while the electric dipole contribution at 6H7/2 is most prominent [42].
Figure 12.
PL emission spectra of ZnO:Sm3+, Zn4B6O13:Sm3+, Zn2P2O7:Sm3+, and ZnO-SO4:Sm3+ phosphors material with 1 mol% of Sm3+ ion monitored under 403 nm excitation wavelength.
Figure 13.
Partial energy level diagram of Sm3+ in Zn4B6O13:Sm3+ and Zn2P2O7:Sm3+ phosphors.
The intensity ratio, which is the ratio of the electric dipole to the magnetic dipole, R = , quantifies the symmetry position of the Sm3+ ion in the local surroundings of the host material. This ratio is a measure of distortion and is often called the asymmetric ratio (which is a measure of distortion) [5]. The measured intensity ratio for Zn4B6O13:Sm3+, R = , is greater than 1, implying that Sm3+ ions occupies the asymmetric sites (absence of symmetry) in the crystal lattice at a fixed concentration of 1 mol% [5,49], leading to a higher 4G5/2 →6H9/2 emission for the ED contribution. In the case of the Zn2P2O7:Sm3+ phosphor material, R is slightly greater than 1 (R = 1.31). The high R value (1.95) for Zn4B6O13:Sm3+ compared to the Zn2P2O7:Sm3+ material implies that there is a greater asymmetrical property in the crystal field for the borate sample as compared to phosphate sample. The calculated R value of 1.95 for Zn4B6O13:Sm3+ is much closer to the calculated value of 2.05 by Zhang et al. on a different host material [20]. The effect of different host materials on Sm3+ ion emissions can be clearly seen from the PL peak shift. The Zn4B6O13 host material causes red shift, which implies that there is an energy transfer from the host material to the Sm3+ ions, and this can be confirmed by high-intensity emissions of the activator ion Sm3+ in the Zn4B6O13:Sm3+ sample.
2.7. CIE Chromaticity Coordinates and CCT Values
The Commission International de I’Eclairage (CIE) chromaticity coordinates for the ZnO:Sm3+, Zn4B6O13:Sm3+, Zn2P2O7:Sm3+, and ZnO-SO4:Sm3+ phosphor materials are depicted in Figure 14. The CIE color chromaticity coordinates of the ZnO:Sm3+, Zn4B6O13:Sm3+, Zn2P2O7:Sm3+, and ZnO-SO4:Sm3+ phosphor materials are given as (0.430, 0.400), (0.600, 0.400), (0.520, 0.400), and (0.420, 0.360) coordinates, respectively. The ZnO-SO4:Sm3+ sample shows minimal changes compared to the ZnO:Sm3+, suggesting that the shift in CIE coordinates likely arises from the residual sulfur contamination during the synthesis process. Using the CIE coordinate values, the color purities (CPs) of the phosphor materials are evaluated using equation [54]:
where (, are the CIE color coordinates of the dominant wavelength (edge of color gamut, extrapolating the line from the neutral white light coordinate point to intersect the CIE coordinate), (x, y) are the color chromaticity coordinates, and (, are the standard color coordinates of neutral white light, taken as (0.333, 0.333) [5,61]. The evaluated color purity for each phosphor material is given in Table 4.
Figure 14.
CIE chromaticity diagram of ZnO:Sm3+, Zn4B6O13:Sm3+, Zn2P2O7:Sm3+, and ZnO-SO4:Sm3+ phosphors.
Table 4.
CIE coordinates, color purity, and calculated correlated color temperature of ZnO:Sm3+, Zn4B6O13:Sm3+, Zn2P2O7:Sm3+, and ZnO-SO4:Sm3+ materials.
From the CIE diagram, it is observed that the Zn4B6O13:Sm3+ and Zn2P2O7:Sm3+ materials’ color emissions lie deep in the red-orange color. The color purity of these materials has been evaluated as 98% for Zn4B6O13:Sm3+ and 71% for Zn2P2O7:Sm3+, producing orange emissions. The strong orange emissions produced by Zn4B6O13:Sm3+ result from the Sm3+ concentration of 1 mol%; this suggests that by varying the concentration of the dopant, red emissions might be produced. Red emissions of the commercially available Y2O3:Eu3+ phosphor have the CIE coordinates of (0.622, 0.350), which are close to the results for Zn4B6O13:Sm3+ materials (0.600, 0.400) [62]. The Zn4B6O13:Sm3+ resulted in an orange emission of high quality. The ZnO:Sm3+ and ZnO-SO4:Sm3+ phosphor materials were evaluated to produce yellow emissions of 46% and 27% purity, respectively.
The additions of borate ions effectively resulted in orange luminescence of a high quality. In general, the chromaticity CIE coordinates (x, y) as well as chromaticity epicenter (xe, ye) = (0.3320, 0.1858) values were used to determine the correlated color temperature (CCT) values for the prepared phosphor materials by use of the McCamy empirical formula [63]:
CCT = 437n3 + 3601n2 + 6861n + 5517, where n = (x − 0.3320)/(y − 0.1858)
The values obtained from this formula, together with their corresponding emission colors, are also shown in Table 4. The CCT values for the ZnO-doped materials were found to vary from 1713 K to 3090 K. These values correspond to typical temperatures of yellow to orange light emissions under near-UV excitation of light. The CCT value of the Zn4B6O13:Sm3+ material is regarded as a warm-orange-emitting phosphor candidate in W-LED applications.
2.8. Lifetime Decay Time Measurements
Figure 15 shows the decay curves for Zn4B6O13:Sm3+ and Zn2P2O7:Sm3+ phosphor materials. The excitation wavelength used was 403 nm for both samples, and the emission wavelengths were 656 nm and 600 nm for Zn4B6O13:Sm3+ and Zn2P2O7:Sm3+, respectively. These were the most intense emissions; hence they were chosen. The two decay curves were well fitted by a bi-exponential curve of the form [5]
where and I are the luminescent intensities at t = 0 and t. Further, and are the fast and slow lifetimes, respectively. Fitting constants and are evaluated at time t, where = 0.6993244 ms, = 0.0051049 ms, = 217.58, and = 10.65 for Zn4B6O13:Sm3+ and = 0.1806959 ms, = 0.0161197 ms, = 620.81, and = 69.81 for Zn2P2O7:Sm3+. The equation used to find the average decay time of the 4G5/2 level for each phosphor material is given by the equation [5]
Figure 15.
Lifetime decay curves for zinc metaborate and zinc pyrophosphate phosphor materials and their respective fit results.
The average decay time for Zn4B6O13:Sm3+ and Zn2P2O7:Sm3+ phosphor materials was found to be 0.6991 ms and 0.1079 ms, respectively. The bi-exponential function indicates that the PL mechanism is linked to the trap states due to impurities or structural imperfections as dopants are introduced [64]. The significant difference in lifetimes may be due to the Zn2P2O7 favoring the non-radiative transitions due to the trap states’ recombination rather than the radiative transitions [64]. Furthermore, the overall decay time of Zn4B6O13 is in agreement with previous studies [65]. The shorter wavelength in the phosphate material arises from the high number of non-radiative transitions.
3. Materials and Methods
ZnO, ZnO:Sm3+, Zn4B6O13:Sm3+, Zn2P2O7:Sm3+ and ZnO-SO4:Sm3+ phosphors were prepared by urea-assisted combustion synthesis with a fixed concentration of Sm3+ at 1 mol%. ZnO-SO4:Sm3+ retained the wurtzite structure of ZnO when synthesized in the presence of ammonium sulfate, which acts as a combustion modifier rather than a dopant; the resulting product remains ZnO, as confirmed by XRD. The precursor materials for this method are in the form of nitrates (oxidizers), with the use of urea as a fuel (reducers). The high-purity raw materials were all sourced from SRL (RSA, Johannesburg, South Africa). In the preparation method, zinc nitrate hexahydrate Zn(NO3)2·(6H2O) (99%), urea (CH4N2O) (96%), and samarium (III) nitrate hexahydrate Sm(NO3)3·(6H2O) (99.9%) were weighed and added into different beakers at relevant masses to allow addition of anions. To the relevant masses, boric acid (H3BO3) (99.5%), di-ammonium hydrogen orthophosphate (N2H9PO4) (99%), and ammonium sulfate (H8N2SO4) (99.5%) were added to their respective beakers. De-ionized water (50 mL) was added to each beaker, and then the beakers were placed over a magnetic stirrer for 30 min at 500 rpm. The phosphate mixture showed a milky solution, and the other mixtures were clear. After stirring, the mixture was then placed in a pre-heated muffle furnace maintained at 600 °C for about 10 min, and a porous-like ash was produced. The ash was then ground with a mortar and pestle to produce greater homogeneity in the sample. The samples were then annealed at different temperatures for 5 h (undoped ZnO, ZnO:Sm3+, and ZnO-SO4:Sm3+ at 1000 °C, Zn2P2O7:Sm3+ at 600 °C, and Zn4B6O13:Sm3+ at 900 °C), after which they were ground again and then made ready for characterization.
The balanced chemical equations for the products are as follows:
Zn(NO3)2·(6H2O) + NH2CONH2 + (NH4)2HPO4 → Zn2P2O7 + gases
Zn(NO3)2·(6H2O) + NH2CONH2 + (NH4)2SO4 → ZnO + SO3(g) + N2(g) + CO2(g) + H2O(g)
Zn(NO3)2·(6H2O) + NH2CONH2 + H3BO3 → Zn4B6O13 + gases
It was observed in this synthesis process that the crystal structures of both phosphate and borate compounds changed, leading to different luminescent characteristics. Figure 16 shows a flow diagram of a typical combustion synthesis method.
Figure 16.
Flow diagram of combustion synthesis method.
4. Conclusions
This study successfully synthesized Sm3+-doped ZnO, Zn4B6O13:Sm3+, and Zn2P2O7:Sm3+ phosphors via combustion synthesis. While BO33− and PO43− formed new crystalline phases, the sulfate precursor decomposed, resulting in a ZnO lattice with minor surface sulfur traces (ZnO-SO4:Sm3+). Regarding XRD results, the formation of a hexagonal wurtzite crystal structure was observed for ZnO, ZnO:Sm3+, and ZnO-SO4:Sm3+ phosphor materials. However, incorporation of borate and phosphate ions resulted in the formation of cubic and monoclinic crystal structures, respectively. The cubic and monoclinic structures were observed for zinc metaborate (Zn4B6O13:Sm3+) and zinc pyrophosphate (Zn2P2O7:Sm3+), respectively. The PL emission scan monitored at an excitation wavelength of 403 nm revealed a characteristic emission of Sm3+ ions from the excited state 4G5/2 level to lower state 6HJ (J = 5/2, 7/2, 9/2, and 11/2) levels. A higher emission performance was observed for the Zn4B6O13:Sm3+ sample, followed by Zn2P2O7:Sm3+. An intense emission was observed for a peak at 654 nm. The lifetime measurement confirmed a higher decay time for Zn4B6O13:Sm3+ as compared to the Zn2P2O7:Sm3+ material. For color purity studies, the best color purity of 98% in the orange region was observed for Zn4B6O13:Sm3+ as the best color purity amongst all the prepared Sm3+-doped materials. This material can be regarded as a promising candidate for orange LED applications.
Author Contributions
E.T.M.: writing—original draft, conceptualization, methodology, and software, M.L.A.L.: software, validation, conceptualization, funding, and writing—review and editing; B.M.S.: resource, conceptualization, validation, and Writing—review and editing. All authors have read and agreed to the published version of the manuscript.
Funding
This research received no external funding.
Institutional Review Board Statement
Not applicable.
Informed Consent Statement
Not applicable.
Data Availability Statement
The raw data supporting the conclusions of this article will be made available by the authors on request.
Acknowledgments
The authors would like to thank L. Reddy for fruitful discussions.
Conflicts of Interest
The authors declare no conflicts of interest.
Abbreviations
The following abbreviations are used in this manuscript:
| UV | Ultraviolet |
| NUV | Near Ultraviolet |
| LED | Light-Emitting Diode |
| PL | Photoluminescence |
| w-LEDs | White Light-Emitting Diodes |
| ASFAC | Ammonium Sulfate Fuel-Assisted Combustion |
References
- Nakamura, S.; Senoh, M.; Nagahama, S.I.; Iwasa, N.; Yamada, T.; Matsushita, T.; Sugimoto, Y.S.Y.; Kiyoku, H.K.H. High-power, long-lifetime InGaN multi-quantum-well-structure laser diodes. Jpn. J. Appl. Phys. 1997, 36, L1059. [Google Scholar] [CrossRef] [Scilit]
- Ye, S.; Xiao, F.; Pan, Y.X.; Ma, Y.Y.; Zhang, Q.Y. Phosphors in phosphor-converted white light-emitting diodes: Recent advances in materials, techniques and properties. Mater. Sci. Eng. R Rep. 2010, 71, 1–34. [Google Scholar] [CrossRef] [Scilit]
- Liu, H.; Guo, S.; Hao, Y.; Wang, H.; Xu, B. Luminescent properties of Eu3+ and Sm3+ activated M2SiO4 (M = Ba, Sr and Ca) red-emitting phosphors for WLEDs. J. Lumin. 2012, 132, 2908–2912. [Google Scholar] [CrossRef] [Scilit]
- Pamuluri, H.; Rathaiah, M.; Linganna, K.; Jayasankar, C.K.; Lavin, V.; Venkatramu, V. Role of Dy3+→ Sm3+ energy transfer in the tuning of warm to cold white light emission in Dy3+/Sm3+ co-doped Lu3Ga5O12 nano-garnets. New J. Chem. 2018, 42, 1260–1270. [Google Scholar] [CrossRef] [Scilit]
- Zou, C.; Sun, N.; Zhang, W.; Li, W.; Huang, Y.; Fan, J. Effect of charge compensators on the luminescence enhancement of Ca2ZnSi2O7: Sm3+ phosphors. J. Mater. Sci. Mater. Electron. 2019, 30, 17412–17423. [Google Scholar] [CrossRef] [Scilit]
- Sheu, J.K.; Chang, S.J.; Kuo, C.H.; Su, Y.K.; Wu, L.W.; Lin, Y.C.; Lai, W.C.; Tsai, J.M.; Chi, G.C.; Wu, R.K. White-light emission from near UV InGaN-GaN LED chip precoated with blue/green/red phosphors. IEEE Photonics Technol. Lett. 2003, 15, 18–20. [Google Scholar] [CrossRef] [Scilit]
- Zhang, X.; Mo, F.; Zhou, L.; Gong, M. Properties–structure relationship research on LiCaPO4: Eu2+ as blue phosphor for NUV LED application. J. Alloys Compd. 2013, 575, 314–318. [Google Scholar] [CrossRef] [Scilit]
- Zhang, S.; Zhang, P.; Liu, X.; Yang, Z.; Huang, Y.; Seo, H.J. A red-emitting phosphor of Li5La3Ti2O12: Eu3+ with garnet-like structure and near-UV/blue light excitation. J. Lumin. 2018, 203, 152–159. [Google Scholar] [CrossRef] [Scilit]
- Tarwal, N.L.; Patil, P.S. Superhydrophobic and transparent ZnO thin films synthesized by spray pyrolysis technique. Appl. Surf. Sci. 2010, 256, 7451–7456. [Google Scholar] [CrossRef] [Scilit]
- Abbasi, M.A.; Khan, Y.; Hussain, S.; Nur, O.; Willander, M. Anions effect on the low temperature growth of ZnO nanostructures. Vacuum 2012, 86, 1998–2001. [Google Scholar] [CrossRef] [Scilit]
- Tarwal, N.L.; Jadhav, P.R.; Vanalakar, S.A.; Kalagi, S.S.; Pawar, R.C.; Shaikh, J.S.; Mali, S.S.; Dalavi, D.S.; Shinde, P.S.; Patil, P.S. Photoluminescence of zinc oxide nanopowder synthesized by a combustion method. Powder Technol. 2011, 208, 185–188. [Google Scholar] [CrossRef] [Scilit]
- Liu, Z.; Tang, Y.; Liao, N.; Yang, P. Study on interfacial interaction between Si and ZnO. Ceram. Int. 2019, 45, 21894–21899. [Google Scholar] [CrossRef] [Scilit]
- Othmen, W.B.H.; Ali, M.B.; Bouslama, W.; Elhouichet, H. Solar driven photocatalytic properties of Sm3+ doped ZnO nanocrystals. Ceram. Int. 2020, 46, 18878–18887. [Google Scholar] [CrossRef] [Scilit]
- Arunkmar, S.; Marimuthu, K. Concentration effect of Sm3+ ions in B2O3–PbO–PbF2–Bi2O3–ZnO glasses–structural and luminescence investigations. J. Alloys Compd. 2013, 565, 104–114. [Google Scholar] [CrossRef] [Scilit]
- Singh, V.; Kumari, S.; Haidari, M.M.; Bhat, A.A.; Rao, A.S.; Joo, J.B. Photoluminescence Behavior of Sm3+-Doped YPO4 Phosphors for Solid-State Lighting. Luminescence 2025, 40, 70190. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Nair, G.B.; Dhoble, S.J. Orange light-emitting Ca3Mg3 (PO4)4: Sm3+ phosphors. Luminescence 2017, 32, 125–128. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Zhang, Y.; Pang, R.; Li, C.; Zang, C.; Su, Q. Reddish orange long lasting phosphorescence of Sm3+ in Sr2ZnSi2O7: Sm3+ phosphors. J. Rare Earths 2010, 28, 705–708. [Google Scholar] [CrossRef] [Scilit]
- Ning, Q.; Quan, B.; Shi, Y. Effect of alkali metal ions on the spectra of CaZn2(PO4)2: Sm3+ phosphor analyzed by JO theory. J. Lumin. 2019, 206, 498–508. [Google Scholar] [CrossRef] [Scilit]
- Ye, H.; Zhang, W.; Cheng, X.; Hu, Z.; Sheng, X.; Feng, Z.; Qiu, L.; Xiong, G.; Xie, W. Enhancing the luminescence and thermal stability of Sm3+ single-doped phosphors through partial cation substitution strategy. Ceram. Int. 2025, 51, 3224–3233. [Google Scholar] [CrossRef] [Scilit]
- Zhang, N.N.; Yang, Y.G.; Yan, X.Y.; Wang, M.Q.; Zhang, Y.Y.; Zhang, H.D.; Zhang, R.; Qiu, C.C.; Chen, F.D.; Wang, J.Y. Preparation and photoluminescence properties of novel orange-red La3Ga5SiO14: Sm3+ phosphors. Ceram. Int. 2023, 49, 16080–16088. [Google Scholar] [CrossRef] [Scilit]
- Gupta, I.; Kumar, P.; Singh, S.; Bhagwan, S.; Kumar, V.; Singh, D. Phase recognition, structural measurements and photoluminescence studies of reddish-orange-emissive YAlO3: Sm3+ perovskite nanophosphors for NUV energized WLEDs. J. Mol. Struct. 2022, 1267, 133567. [Google Scholar] [CrossRef] [Scilit]
- Kumari, S.; Rao, A.S.; Sinha, R.K. Investigations on photoluminescence and energy transfer studies of Sm3+ and Eu3+ ions doped Sr9Y2W4O24 red emitting phosphors with high color purity for w-LEDs. J. Mol. Struct. 2024, 1295, 136507. [Google Scholar] [CrossRef] [Scilit]
- Balakrishna, A.; Swart, H.C.; Ramaraghavulu, R.; Bedyal, A.K.; Kroon, R.E.; Ntwaeaborwa, O.M. Structural evolution induced by substitution of designated molybdate sites (MoO4−2) with different anionic groups (BO3−3, PO4−3 and SO4−2) in CaMoO4: Sm3+ phosphors-A study on color tunable luminescent properties. J. Alloys Compd. 2017, 727, 224–237. [Google Scholar] [CrossRef] [Scilit]
- Letswalo, M.L.A.; Reddy, L.; Balakrishna, A.; Swart, H.C.; Ntwaeaborwa, O.M. The role of sulfate ions on distinctive defect emissions in ZnO: Ce3+ nanophosphors-A study on the application in color display systems. J. Lumin. 2021, 240, 118462. [Google Scholar] [CrossRef] [Scilit]
- Lian, W.L.; Liang, P.; Liu, Z.H. Controllable hydrothermal synthesis and morphology evolution of Zn4B6O13: Tb/Eu phosphors with tunable luminescent properties. Adv. Powder Technol. 2020, 31, 1633–1642. [Google Scholar] [CrossRef] [Scilit]
- Kucuk, N.; Kaynar, Ü.H.; Akca, S.; Alajlani, Y.; Yin, L.; Wang, Y.; Guinea, J.G.; Bulcar, K.; Dogan, T.; Karabulut, Y.Ü.K.S.E.L.; et al. Enhancing the blue luminescence behaviour of the Li co-doped novel phosphor ZnB2O4: Tm3+. J. Alloys Compd. 2020, 838, 155587. [Google Scholar] [CrossRef] [Scilit]
- Tamboli, S.; Nair, G.B.; Kroon, R.E.; Dhoble, S.J.; Swart, H.C. Color tuning of the Ba1.96Mg(PO4)2: 0.04Eu2+ phosphor induced by the chemical unit co-substitution of the (BO3)3− anion group. J. Alloys Compd. 2021, 864, 158124. [Google Scholar] [CrossRef] [Scilit]
- Calvo, C. The crystal structure and phase transitions of β-Zn2P2O7. Can. J. Chem. 1965, 43, 1147–1153. [Google Scholar] [CrossRef] [Scilit]
- Maslyk, M.; Bach, S.; Li, W.; Shylin, S.I.; Panthöfer, M.; Barton, B.; Ksenofontov, V.; Xu, K.; Meermann, B.; Kolb, U.; et al. Understanding the stability and recrystallization behavior of amorphous zinc phosphate. J. Phys. Chem. C 2021, 125, 2636–2647. [Google Scholar] [CrossRef] [Scilit]
- Soriano-Romero, O.; Carmona-Téllez, S.; Alarcón-Flores, G.; Lozada-Morales, R.; Caldiño, U.; Juárez-Rayón, I.; Meza-Rocha, A.N. Tunable rare-earth-free white light emission in zinc phosphate glasses activated with Agmn+ clusters and Mn2+ ions. Ceram. Int. 2022, 48, 33108–33114. [Google Scholar] [CrossRef] [Scilit]
- Garcia-Martinez, O.; Rojas, R.M.; Vila, E.; De Vidales, J.M. Microstructural characterization of nanocrystals of ZnO and CuO obtained from basic salts. Solid State Ion. 1993, 63, 442–449. [Google Scholar] [CrossRef] [Scilit]
- Smith, P.; Garcia-Blanco, S.T.; Rivoir, L. The crystal structure of anhydrous zinc metaborate Zn4O(BO2)6. Z. Für Krist. 1964, 119, 375–383. [Google Scholar] [CrossRef] [Scilit]
- Deyneko, D.V.; Titkov, V.V.; Fedyunin, F.D.; Spassky, D.A.; Volkov, S.N.; Borovikova, E.Y.; Lazoryak, B.I.; Aksenov, S.M. «Ellestadite»-type anionic [PO4]3−→[SO4]2− substitutions in β-Ca3(PO4)2 type compounds: A new route to design the inorganic phosphors. Ceram. Int. 2022, 48, 24012–24020. [Google Scholar] [CrossRef] [Scilit]
- Wongrerkdee, S.; Wongrerkdee, S.; Boonruang, C.; Sujinnapram, S. Enhanced photocatalytic degradation of methylene blue using Ti-doped ZnO nanoparticles synthesized by rapid combustion. Toxics 2022, 11, 33. [Google Scholar] [CrossRef] [Scilit]
- Pant, B.; Park, M.; Kim, H.Y.; Park, S.J. Ag-ZnO photocatalyst anchored on carbon nanofibers: Synthesis, characterization, and photocatalytic activities. Synth. Met. 2016, 220, 533–537. [Google Scholar] [CrossRef] [Scilit]
- Kummara, S.K.; Reddy, L. Tailored Optical, Magnetic and Photoluminescence properties of Fe/Cr-doped ZnO nanoparticles synthesized via solution combustion method. Nano-Struct. Nano-Objects 2024, 39, 101263. [Google Scholar] [CrossRef] [Scilit]
- Liu, T.; Li, X.; Curnow, O.J.; Choi, J.; Yip, A.C. A two-step ionothermal synthesis of MFI zeolite framework and its potential applications in adsorption and catalysis. Microporous Mesoporous Mater. 2025, 398, 113834. [Google Scholar] [CrossRef] [Scilit]
- Shan, Y.Q.; Xu, Z.X.; Duan, P.G.; Fan, H.L.; Hu, X.; Luque, R. Nitrogen-and sulfur-doped carbon obtained from direct hydrothermal carbonization of cellulose and ammonium sulfate for supercapacitor applications. ACS Sustain. Chem. Eng. 2020, 8, 15809–15814. [Google Scholar] [CrossRef] [Scilit]
- Jiao, K.; Ma, S.; Chen, X.; Liu, J.; Qiao, L. Experimental research on the volatilization and condensation of ammonium bisulfate as SCR byproduct. Pol. J. Chem. Technol. 2022, 24, 30–38. [Google Scholar] [CrossRef] [Scilit]
- Reddy Yadav, L.S.; Raghavendra, M.; Sudheer Kumar, K.H.; Dhananjaya, N.; Nagaraju, G. Biosynthesised ZnO: Dy3+ nanoparticles: Biodiesel properties and reusable catalyst for N-formylation of aromatic amines with formic acid. Eur. Phys. J. Plus 2018, 133, 153. [Google Scholar] [CrossRef] [Scilit]
- Zheng, Y.; Chen, C.; Zhan, Y.; Lin, X.; Zheng, Q.; Wei, K.; Zhu, J.; Zhu, Y. Luminescence and photocatalytic activity of ZnO nanocrystals: Correlation between structure and property. Inorg. Chem. 2007, 46, 6675–6682. [Google Scholar] [CrossRef] [Scilit]
- Kumar, S.; Babu, S.; Rajeswara Reddy, B.; Ratnakaram, Y.C. Study of structural and spectroscopic behavior of Sm3+ ions in lead–zinc borate glasses containing alkali metal ions. Indian J. Phys. 2017, 91, 677–687. [Google Scholar] [CrossRef] [Scilit]
- Petrova, M.A.; Shitova, V.I.; Mikirticheva, G.A.; Popova, V.F.; Malshikov, A.E. New data on Zn2P2O7 phase transformations. J. Solid-State Chem. 1995, 119, 219–223. [Google Scholar] [CrossRef] [Scilit]
- Lim, K.S.; Vijaya, N.; Kesavulu, C.R.; Jayasankar, C.K. Structural and luminescence properties of Sm3+ ions in zinc fluorophosphate glasses. Opt. Mater. 2013, 35, 1557–1563. [Google Scholar] [CrossRef] [Scilit]
- Ganguli, M.; Rao, K.J. Studies on the effect of Li2SO4 on the structure of lithium borate glasses. J. Phys. Chem. B 1999, 103, 920–930. [Google Scholar] [CrossRef] [Scilit]
- Thomas, S.; Rasool, S.N.; Rathaiah, M.; Venkatramu, V.; Joseph, C.; Unnikrishnan, N.V. Spectroscopic and dielectric studies of Sm3+ ions in lithium zinc borate glasses. J. Non-Cryst. Solids 2013, 376, 106–116. [Google Scholar] [CrossRef] [Scilit]
- Alemi, A.; Mohseni, N.; Dolatyari, M.; Bakhtiari, A. New Method for Synthesis of Zinc Metaborate Zn4B6O13 Crystals via Sol-Gel Process and Investigation of DFT Calculations. Int. J. Bio-Inorg. Hybd. Nanomat 2012, 1, 79–86. [Google Scholar]
- Sabilladin, A.; Saviola, A.J.; Wijaya, K.; Hutama, A.S.; Pradipta, M.F.; Saputri, W.D.; Ismail, H.; Budhijanto, B.; Oh, W.C.; Ravindran, B. Optimizing nitrobenzene synthesis catalyzed by sulfated silica (SO4/SiO2) through response surface methodological approach. Korean J. Mater. Res. 2024, 34, 341–354. [Google Scholar] [CrossRef] [Scilit]
- Sailaja, B.; Stella, R.J.; Rao, G.T.; Raja, B.J.; Manjari, V.P.; Ravikumar, R.V.S.S.N. Physical, structural and spectroscopic investigations of Sm3+ doped ZnO mixed alkali borate glass. J. Mol. Struct. 2015, 1096, 129–135. [Google Scholar] [CrossRef] [Scilit]
- Shih, H.R.; Chang, Y.S. Structure and photoluminescence properties of Sm3+ ion-doped YInGe2O7 phosphor. Materials 2017, 10, 779. [Google Scholar] [CrossRef] [Scilit]
- Morales, A.E.; Mora, E.S.; Pal, U. Use of diffuse reflectance spectroscopy for optical characterization of un-supported nanostructures. Rev. Mex. Física 2007, 53, 18–22. [Google Scholar]
- Som, S.; Chowdhury, M.; Sharma, S.K. Band gap and trapping parameters of color tunable Yb3+/Er3+ codoped Y2O3 upconversion phosphor synthesized by combustion route. J. Mater. Sci. 2014, 49, 858–867. [Google Scholar] [CrossRef] [Scilit]
- Divya, J.; Shivaramu, N.J.; Roos, W.D.; Purcell, W.; Swart, H.C. Synthesis, surface and photoluminescence properties of Sm3+ doped α-Bi2O3. J. Alloys Compd. 2021, 854, 157221. [Google Scholar] [CrossRef] [Scilit]
- Singh, S.; Prasher, S. The etching and structural studies of gamma irradiated induced effects in CR-39 plastic track recorder. Nucl. Instrum. Methods Phys. Res. Sect. B Beam Interact. Mater. At. 2004, 222, 518–524. [Google Scholar] [CrossRef] [Scilit]
- Dovom-Niasar, S.J.; Seifi, A.; Bahramian, A.R.; Abzal, A. A mechanistic study of the fire performance of the silica and zinc borate nanoparticles-incorporated intumescent coatings based on epoxy resin. J. Vinyl Addit. Technol. 2023, 29, 849–863. [Google Scholar] [CrossRef] [Scilit]
- Bedyal, A.K.; Kumar, V.; Prakash, R.; Ntwaeaborwa, O.M.; Swart, H.C. A near-UV-converted LiMgBO3: Dy3+ nanophosphor: Surface and spectral investigations. Appl. Surf. Sci. 2015, 329, 40–46. [Google Scholar] [CrossRef] [Scilit]
- Kumar, I.; Gathania, A.K. Photoluminescence and quenching study of the Sm3+-doped LiBaPO4 phosphor. J. Mater. Sci. Mater. Electron. 2022, 33, 328–341. [Google Scholar] [CrossRef] [Scilit]
- Pandey, P.K.; Dixit, P.; Chauhan, V.; Pandey, P.C. Luminescence properties and energy transfer studies in thermally stable Bi2O3: Sm3+, Eu3+ phosphor. J. Alloys Compd. 2023, 952, 169911. [Google Scholar] [CrossRef] [Scilit]
- Katta, V.S.; Chappidi, V.R.; Kumar, A.; Asthana, S.; Raavi, S.S.K. Enriched visible light absorption by Au-embedded Sm3+ doped TiO2 compact photoanode for enhanced dye-sensitized solar cell performance. Phys. B Condens. Matter 2023, 652, 414621. [Google Scholar] [CrossRef] [Scilit]
- Yang, L.; Yu, X.; Yang, S.; Zhou, C.; Zhou, P.; Gao, W.; Ye, P. Preparation and luminescence properties of LED conversion novel phosphors SrZnO2: Sm3+. Mater. Lett. 2008, 62, 907–910. [Google Scholar] [CrossRef] [Scilit]
- Halappa, P.; Rajashekar, H.M.; Shivakumara, C. Synthesis and structural characterization of orange red light emitting Sm3+ activated BiOCl phosphor for WLEDs applications. J. Alloys Compd. 2019, 785, 169–177. [Google Scholar] [CrossRef] [Scilit]
- Zhang, L.; Xie, Y.; Geng, X.; Deng, B.; Geng, H.; Yu, R. Double perovskite Ca2MgTeO6: Eu3+ red-emitting phosphors with high thermal stability for near UV/blue excited white LEDs. J. Lumin. 2020, 225, 117365. [Google Scholar] [CrossRef] [Scilit]
- McCamy, C.S. Correlated color temperature as an explicit function of chromaticity coordinates. Color Res. Appl. 1992, 17, 142–144. [Google Scholar] [CrossRef] [Scilit]
- Singh, M.K.; Mehata, M.S. Temperature-dependent photoluminescence and decay times of different phases of grown TiO2 nanoparticles: Carrier dynamics and trap states. Ceram. Int. 2021, 47, 32534–32544. [Google Scholar] [CrossRef] [Scilit]
- Deng, B.; Zhou, C.S.; Liu, H.; Chen, J. Structure and photoluminescence properties of Sm3+ ion-doped LiSrBiTeO6 phosphor. IOP Conf. Ser. Earth Environ. Sci. 2018, 186, 012069. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.