Skip to Content
MoleculesMolecules
  • Article
  • Open Access

6 October 2026

24 Pages

Gd3+-Driven Microstructure Regulation of Tm3+, Yb3+: GdxBi2−xWO6 for High-Sensitivity Temperature Sensing and Magnetism

,
,
,
,
,
and
1
School of Physics and Electronic Engineering, Xinjiang Normal University, Urumqi 830054, China
2
Xinjiang Key Laboratory for Luminescence Minerals and Optical Functional Materials, Xinjiang Normal University, Urumqi 830054, China
*
Author to whom correspondence should be addressed.
This article belongs to the Section Inorganic Chemistry

Abstract

Tm3+, Yb3+: GdxBi2−xWO6 series upconversion luminescent materials were synthesized via a solid-state method. Calculations and XRD analysis reveal that Gd3+ in the lattice exhibits both substitutional and interstitial doping. Compared with the NaYF4 matrix, the Bi2WO6 material doped with Gd3+ has a lower Debye temperature (392.45 K), and the maximum phonon energy is low; thus, the probability of nonradiative transitions decreases. SEM images and EDS results reveal that the powder particle size ranges from 0.5 to 3 μm and that the elements are evenly distributed on the surface. The diffuse reflectance absorption spectra indicate that moderate Tm3+, Yb3+ and Gd3+ doping shifts the absorption band of the material towards longer wavelengths and decreases the band gaps. Under 980 nm laser excitation and a Gd3+ doping concentration of x = 0.2, the emission intensities of Tm3+ at 476 nm, 683 nm, 703 nm, and 804 nm increase by 1.8, 1.24, 1.35, and 81.9 times, respectively. Calculations reveal that these emissions in the range of 450 to 850 nm originate from three-photon or two-photon absorption. Gd3+ codoping can prolong the lifetime of the Tm3+ energy levels. When this sample was excited at 980 nm (518 mW), the temperature was characterized by FIR703nm/476nm from 298 K to 573 K, and the obtained maximum relative sensitivity was 3.4907 K−1 (298 K). The minimum temperature resolution was 0.0083 K (298 K). Compared with that of the undoped Gd3+ sample, the temperature sensitivity of the Gd3+-codoped sample increased by 92.35 times. Under an external magnetic field of 20 kOe and a temperature of 300 K, the magnetization of the sample doped with Gd3+ increased fourfold to 0.08174 emu/g. This material has potential applications in temperature sensing and magnetic resonance imaging.

1. Introduction

Rare-earth upconversion nanomaterials with adjustable particle sizes, good photostability, and low background fluorescence interference have broad applications in noncontact environmental temperature measurements [1,2]. Several reports have investigated the upconversion luminescence and temperature measurement properties of different matrix materials codoped with Tm3+ and Yb3+. For example, Zhou [3] prepared Y2O3: Yb3+, Tm3+ via fusion and used the three Stark-split bands of Tm3+ to achieve temperature sensing at low and high temperatures with the same material. An [4] prepared a series of Tm3+, Yb3+: LuAG materials using the floating zone method with a CO2 laser and investigated the optical temperature sensing properties in the range of 298–1023 K. The maximum absolute and relative sensitivities for optical temperature sensing were obtained at 1023 K and 555 K, respectively. Additionally, Krishna [5] used a hydrothermal method to dope Tm3+ and Yb3+ into Ca3(PO4)2. The Judd–Ofelt intensity parameters were calculated and found to follow the order Ω2 > Ω4 > Ω6, and the maximum absolute sensor sensitivity was 0.00363 K−1 at 623 K when 1G4 and 3F2,3 levels were considered nonthermally coupled.
As reported in the literature [6], Gd3+ doping can regulate the luminescent properties of certain luminescent materials by adjusting their energy band structure and changing their lattice symmetry. Zhang [7] prepared a series of AWO4 (A = Sr, Ca) materials doped with Gd3+, Yb3+, and Er3+ via a high-temperature solid phase method, and Gd3+ doping effectively improved the luminescence and thermometry sensitivity. Furthermore, Xiao [8] synthesized CaF2: Gd3+, Yb3+ and Ho3+ using a hydrothermal method and reported that the introduction of Gd3+ reduced the clustering of Ho3+ and Yb3+ and increased their upconversion luminescence efficiency. Yunfeng Bai [9] investigated the effect of Gd3+ doping on the luminescence of Lu3Al5O12: 1% Ce3+ powders and reported that as the concentration of Gd3+ increased, the 5d orbital splitting of Ce3+ increased, which led to broadening of the Ce3+ emission peak and a redshift in the Ce3+ emission. Moreover, Ilya E. Kolesniko [10] prepared NaYF4: Eu3+ and Gd3+ samples via a hydrothermal method using citric acid as a stabilizer and reported that when Gd3+ with a relatively large radius replaced Y3+, the positive charge density on the crystal surface decreased, and the luminescence increased. S. G. Revankard [11] analysed the upconversion luminescence of materials codoped with Gd3+ and a series of Ln3+ (Eu3+, Tb3+, and Dy3+). As the energy gap between the Pj state and the ground state of Gd3+ is too large for the energy to dissipate into the surrounding lattice, energy is transferred to Ln3+, increasing the luminescence intensity of Ln3+. In summary, Gd3+ doping may alter the lattice symmetry and substrate band gap, thus affecting the luminescence and fluorescence temperature measurement properties of the material.
Because Gd has paramagnetic properties, when it is close to the proton in resonance, it can effectively change the magnetic field of the proton and shorten the T1 and T2 relaxation times. In nuclear magnetic resonance imaging, Gd3+ can greatly increase imaging contrast and resolution. Jiaxi Ru [12] designed and synthesized a novel Gd(III) complex-based magnetic resonance imaging (MRI) contrast agent, GdL, which exhibited a high relaxivity (7.8 m/Ms), good water solubility (>100 mg mL−1), excellent thermodynamic stability, and high biosafety and biocompatibility. These results suggest that GdL is an excellent T1-weighted MRI contrast agent with potential applicability in clinical diagnosis. Additionally, Rugmani Meenambal [13] prepared multifunctional Gd3+, Dy3+ and Yb3+: β-Ca3(PO4)2 via a facile synthetic technique. The materials also displayed paramagnetic behaviour and exhibited high longitudinal (r1 = 48.71 m/Ms) and transverse relaxivity (r2 = 61.79 m/Ms), indicating their potential as T1 and T2 contrast agents in MRI. Furthermore, Alireza Shariati [14] developed and tested a new class of dual contrast agents based on polydopamine nanoparticles (PDA-NPs) that are functionalized and targeted with hyaluronic acid (HA). These nanoparticles (NPs) are chelated with Gd3+ to provide suitable contrast. The stability of the PDA/HA/Gd3+ material was evaluated by ICP–OES, zeta potentials, and DLS over 3 days, and the results suggested that the Gd-HA NPs were stable. If paramagnetic Gd3+ is doped into near-infrared-excited upconversion luminescent materials, high-precision imaging and accurate fluorescence temperature measurements can be achieved.
However, relatively few reports have investigated the doping mode of Gd3+ ions entering the lattice and their effects on material structural stiffness (Young’s modulus and Debye temperature), upconversion luminescence, temperature sensing, and magnetic properties. Bi2WO6 is a promising upconversion host because of its low phonon energy and stable physicochemical properties. However, its 2.7 eV band gap limits absorption to below 450 nm; thus, its upconversion luminescence has been explored primarily for photocatalysis. To broaden its spectral absorption and applications and to investigate its upconversion luminescence and temperature-sensing properties, on the basis of previous research on the fluorescence temperature measurement of Tm3+, Yb3+: Bi2WO6 [15], density functional theory was used to estimate the effects of different doping modes of Gd3+ on the lattice structure, band gap, and density of states of the material. The changes in Young’s modulus and Debye temperature of the material before and after Gd3+ doping were calculated. The effects of Gd3+ doping on the microstructure, upconversion luminescence, fluorescence thermometry, and magnetic properties of synthesized materials were analysed.

2. Results and Discussion

2.1. Structural Calculations

The Bi2WO6 host is part of the layered perovskite group called Bi2WnO3n+3 (n = 1). This structure includes layers that are positively charged (Bi2O2)2+ and layers arranged in octahedrons (WO4)2−. Defects in the (Bi2O2)2+ layer can interfere with the regular patterns and electronic properties of the crystal structure.
In the calculation, if the doping concentration of Tm3+ is 1% and the ion concentration is too low, the constructed supercell will be very large, and the result will be difficult to determine. To obtain effective calculation results, the Tm3+ doping concentration was set to 10%, and the calculated lattice structure and bond length around the doped Bi2WO6, Tm3+, Yb3+: Bi2WO6 and Tm3+, Yb3+, Gd3+: Bi2WO6 are shown in Figure 1.
Figure 1. The crystal structure and bond angle of the material before and after doping (2 × 1 × 2 supercell): (a) Bi2WO6; (b)10% Tm3+, 6% Yb3+ substitution for Bi3+ sites; (c) 10% Tm3+, 6% Yb3+, 10% Gd3+ substitution for Bi3+ sites; (d) Tm3+ and Yb3+ substitution for Bi3+ sites and Gd3+ interstitial doping.
To accurately describe the electronic structure of the system, Hubbard U was considered in the DFT calculations [16]. A value of U = 6.0 eV was introduced to the f-orbital of Tm, Gd and Yb. The formation energy of the supercells with different doping types was calculated using Equation (1).
E f = E dop − E perfect + ∑ n i E i
where Edop and Eperfect are the total energies of the doped model and pristine supercells, respectively. ni and Ei are the number and energy of the dopant species, respectively.
Table 1 shows the lattice parameters and formation energy calculated by VASP. When the small-radius ions Tm3+ (0.088 nm) and Yb3+ (0.0868 nm) undergo substitutional doping, the calculated unit cell volume decreases. When Tm3+, Yb3+, and Gd3+ (0.0938 nm) completely replace the large-radius Bi3+ (0.103 nm) ion lattice, the bond length around Tm3+/Yb3+/Gd3+ decreases, and the volume of the unit cell decreases further. When Tm3+/Yb3+ undergoes substitutional doping and Gd3+ undergoes interstitial doping, the calculated unit cell volume increases. The calculations reveal that the formation energies associated with Gd3+ substitutional doping and Gd3+ interstitial doping are −44.124 eV and −24.526, respectively. The negative values indicate that in both cases, the system energy decreases, suggesting good thermodynamic stability. Gd3+ substitutional doping results in a lower formation energy, leading to more stable compounds. The lower the formation energy is, the more stable the formed compound is.
Table 1. Lattice parameters and defect formation energy of samples calculated by VASP.
Tm3+, Yb3+ and Gd3+ codoping result in Bi3+ in the matrix being replaced at multiple lattice sites, which can result in the formation of multiple structures. Considering the periodicity and symmetry of the crystal cell, the static energy of each structure was obtained by optimizing the atomic position. The structure with the lowest static energy was selected, and the energy band and density of states before and after Tm3+, Yb3+ and Gd3+ doping of Bi2WO6 were optimized. The band structures of the Bi2WO6 matrix, Tm3+/Yb3+/Gd3+-substituted doped samples, and Tm3+/Yb3+-substituted doped and Gd3+ gap-doped samples are shown in Figure 2a, Figure 2b, and Figure 2c, respectively. The corresponding electronic density of states maps are shown in Figure 2d–f. The energy band structure reveals that the calculated band gap of Bi2WO6 is 2.08 eV, which is lower than the experimental value of 2.69 eV. The reason is that the generalized gradient approximation functional cannot completely offset the Coulomb interaction between the electron and the material, resulting in excessive delocalization of the electron cloud, overestimation of the valence band top and underestimation of the conduction band bottom, resulting in a slightly smaller calculated band gap.
Figure 2. First-principles calculations of the band structure: (a) Bi2WO6; (b) 10% Tm3+, 6% Yb3+ and 10% Gd3+ substitutional doping; (c) 10% Tm3+ and 6% Yb3+ substitutional doping and 10% Gd3+ interstitial doping; (d–f) the corresponding electronic density of states.
Compared with the Bi2WO6 matrix, when Tm3+/Yb3+/Gd3+ doping is performed to replace Bi3+, the calculated valence band top of the material shifts slightly downwards, and the band gap widens to 2.26 eV, as shown in Figure 2b. Owing to the weak hybridization between the 4f semi-full stable orbitals of Gd3+ and the O-2p valence band orbitals of the host lattice, the energy at the top of the valence band is slightly reduced. When Tm3+/Yb3+ doping is used to replace Bi3+ and Gd3+ is interstitially doped, impurity energy bands are calculated to appear between the band gaps. Both the conduction band and the valence band move synchronously towards lower energy, with a band gap of 2.14 eV, as shown in Figure 2c. Compared with Bi3+ (with an electronegativity of 1.2), Gd3+ ions have a higher electronegativity (1.9) and a higher effective ion potential in the trivalent state, resulting in a stronger ability to attract electrons. When the more electronegative Gd3+ is doped into the lattice, it strongly attracts the electron cloud of the surrounding O2−, reduces the overall average electrostatic potential of the system, and drives the conduction band and valence band to move downwards towards lower energies. When the doping concentration of the Gd3+ gap reaches the threshold, the 4f orbitals of adjacent Gd3+ overlap and broaden to form localized impurity bands that fill the band gap, providing intermediate energy bands for carrier transitions. Compared with the sample with Gd3+ substitutional doping (with a band gap of 2.26 eV), the sample with Gd3+ interstitial doping has a smaller band gap of 2.14 eV, which is beneficial for the matrix to absorb more low-energy photons.

2.2. Structural Stiffness

Typically, Young’s modulus E and Debye temperature θD are used to describe the structural stiffness of crystals [17]. Crystals with higher structural stiffness have weaker phonon energy, which limits electron–phonon coupling and leads to a lower probability of nonradiative relaxation [18]. The energy cutoff for plane-wave basis expansion was 400 eV, and the geometric structure relaxation convergence criterion was −0.02 eV/Å.
The elastic constants of the Bi2WO6 and Gd3+-doped Bi2WO6 matrices calculated using VASP are shown in Table 2. The stability was determined by measuring the elastic coefficients Cij of the cubic crystalline phase Bi2WO6 as follows: C11 > 0, C44 > 0, C55 > 0, C66 > 0, C11C22 > C122, and C11C22C33+2C12C13C23-C11C232-C22C132-C33C122 > 0. The calculated elastic coefficients Cij of Gd3+-doped Bi2WO6 are shown in Table 2.
Table 2. Calculation results of the elastic coefficients Cij.
The Voigt and Reuss equations describe the upper and lower limits of the real crystal constants, respectively. The crystal moduli are taken as the Voigt–Reuss–Hill approximations, which are the arithmetic averages given by Voigt and Reuss. The calculation formulas are as follows:
G = ( G V + G R ) / 2
B = ( B V + B R ) / 2
Here, GV, which represents the shear modulus under the Voigt approximation, and BV, which represents the bulk modulus, can be expressed by the elastic coefficient Cij of the Bi2WO6 crystal as follows:
G V = 1 15 [ C 11 + C 22 + C 33 + 3 ( C 44 + C 55 + C 66 ) − ( C 12 + C 13 + C 23 ) ]
B V = 1 9 C 11 + C 22 + C 33 + 2 ( C 12 + C 13 + C 23 )
Here, the shear modulus GR and bulk modulus BR under the Reuss approximation have the following relationships with the elastic compliance coefficients Cij of the crystal:
G R = 15 { 4 [ C 11 ( C 22 + C 33 + C 23 ) + C 22 ( C 33 + C 13 ) + C 33 C 12 − C 12 ( C 23 + C 12 ) − C 13 ( C 12 + C 13 ) − C 23 ( C 13 + C 23 ) ] / Δ + 3 [ ( 1 / C 44 ) + ( 1 / C 55 ) + ( 1 / C 66 ) ] } − 1
B R = Δ [ C 11 ( C 22 + C 33 − 2 C 23 ) + C 22 ( C 33 − 2 C 13 ) − 2 C 33 C 12 + C 12 ( 2 C 23 − C 12 ) ] + C 33 ( 2 C 12 − C 13 ) + C 23 ( 2 C 13 − C 23 ) ] − 1
Here, Δ is formulated as follows:
Δ = C 13 ( C 12 C 23 − C 13 C 22 ) + C 23 ( C 12 C 13 − C 23 C 11 ) + C 33 ( C 11 C 22 − C 12 2 )
Young’s modulus E represents the structural stiffness of the material and is calculated as follows:
E = 9 G B / ( G + 3 B )
The compressional longitudinal wave velocity (VP) and transverse wave velocity (VS) are calculated as follows:
V p = ( 4 3 G + B ) / ρ 1 / 2
V S = ( G / ρ ) 1 / 2
Here, ρ is the mass density of the matrix material.
The mean sound velocity Vm is calculated as follows:
V m = 2 3 V s 3 + 1 3 V p 3 − 1 3
The Debye temperature θD can be obtained from the average sound speed and Debye approximation as follows:
θ D = h k B ( 3 n 4 π V ) 1 3 V m
where h is the Planck constant, kB is the Boltzmann constant, n is the number of atoms in the primitive cell, V is the primitive cell volume, and Vm is the average phonon velocity.
The calculations show that Young’s modulus of the Bi2WO6 crystal is 184.210 GPa. When the same calculation method is used, Young’s modulus of the Bi2WO6 crystal doped with Gd3+ is 183.579 GPa, which is slightly smaller, as shown in Table 3.
Table 3. Calculation parameters and Young’s modulus E of the Bi2WO6 host and Gd0.2Bi1.8WO6.
Generally, the lower Young’s modulus is for a material, the weaker the interatomic forces, and materials with lower Young’s moduli undergo greater elastic deformation. After appropriate doping with Gd3+ ions, the matrix material is more prone to lattice distortion; this distortion reduces the lattice symmetry, which is beneficial for enhancing the luminescence.
Recent studies on perovskites have further revealed the correlation between structural rigidity and thermal stability, indicating that when the Debye temperature (quantifiable lattice vibration hardness) exceeds 200 K, nonradiative transitions can be effectively suppressed, resulting in stable luminescence [19]. In this work, through first-principles calculations, the Debye temperatures of the Bi2WO6 matrix and Gd3+-doped material were calculated to be 391.94 K and 392.45 K, respectively. These values are much higher than the above threshold, indicating excellent luminescence stability.
As shown in Table 4, according to the calculation results, compared with the NaYF4 host material, the Bi2WO6 host material and Gd3+-doped Bi2WO6 material have lower Debye temperatures. The lower the Debye temperature of the host is, the lower the upper limit of the lattice vibration frequency. Crossing the same electronic energy gap requires an increase in the number of phonons, which reduces the probability of nonradiative transitions. Importantly, Bi2WO6 also has a lower phonon energy, which is beneficial for improving the upconversion luminescence performance of the material.
Table 4. Debye temperatures and phonon energies of typical host materials.

2.3. Microstructural Characterization

The XRD patterns of the prepared y% Tm3+, 6% Yb3+: GdxBi2−xWO6 (x = 0, 0.06, 0.1, 0.2, 0.3; y = 0.5, 1, 3, 6) phosphors calcined at 800 °C for 3 h are shown in Figure 3. The diffraction peaks of all the prepared samples are essentially consistent with those of the Bi2WO6 standard card (PDF#39-0256). However, as the doping concentration of Tm3+ and Yb3+ ions increases, the diffraction peak shifts towards larger angles, as shown in Figure 3b. When smaller-radius Tm3+(0.088 nm)/Yb3+(0.0868 nm) ions replace Bi3+(0.103 nm), the cell volume decreases, the interplanar spacing d decreases, and the diffraction angle increases, resulting in the diffraction peaks shifting towards larger angles.
Figure 3. XRD patterns of the y% Tm3+/6% Yb3+: GdxBi2−xWO6 phosphors: (a) y = 0.5, 1, 3, 6; (b)The movement of the main diffraction peak (131) for (a); (c) x = 0, 0.06, 0.1, 0.2, 0.3; (d) The movement of the main diffraction peak (131) for (c).
As the doping amount of low-concentration Gd3+ increases, the diffraction peak of the sample gradually shifts towards a smaller angle. When the amount of doped Gd3+ ions is x = 0.3, the diffraction peak (131) begins to reverse shift, as shown in Figure 3d. Although the formation energy of the sample with Gd3+ substitutional doping is lower, as shown in Table 1, when small-radius Gd3+ ions are doped into the lattice gap, the surrounding atoms spread, resulting in lattice expansion and a continuous increase in the interplanar spacing d. This is the core reason for the shift in the peak position towards small angles after Gd3+ doping. This finding also indicates that low-concentration doped Gd3+ ions are likely to enter the lattice gap. When the interstitial sites tend to saturate, excess Gd3+ ions are likely to replace the existing larger-radius Bi3+ ion sites in the lattice, resulting in cell shrinkage and a decrease in the interplanar spacing d. In addition, under high-concentration Gd3+ doping, the accumulated tensile strain of the lattice in the early stage reaches a critical value, and the lattice releases strain through local atomic rearrangement. The originally stretched interplanar spacing gradually decreases, resulting in a reverse shift in the diffraction peaks.
The JADE calculation results based on the XRD patterns are shown in Table 5, where a, b, and c are the cell parameters and V is the unit cell volume.
Table 5. Cell parameters of samples obtained by JADE.
According to Scherrer’s formula [23], the grain size and the full width at half maximum (FWHM) of a diffraction peak are related as follows:
D hkl = K λ β c o s   θ
where Dhkl is the grain size, K is Scherrer’s constant, λ is the wavelength of incident X-rays, β is the FWHM, and θ is the Bragg angle. K depends on the grain shape and size distribution, the diffraction line index, and the actual definition (FWHM or integration range). Assuming a constant K, the grain size of the samples with different Gd3+ doping concentrations was estimated as Dhkl.
Compared with the original Bi2WO6 matrix, doping with appropriate amounts of Tm3+ and Yb3+ ions can lead to a decrease in the unit cell volume. As the concentration of Gd3+ ions gradually increases, the calculated unit cell volume first increases but then decreases. This finding indicates that when Gd3+ ions are doped into the lattice, interstitial doping is the main mode at low concentrations, whereas substitutional doping is the main mode after a certain concentration is reached. The VASP estimation results (Table 1) are consistent with the XRD experimental results (Figure 3) and JADE analysis results (Table 5) in terms of the trend of the unit cell volume change.

2.4. Morphological Analysis

The scanning electron microscopy (SEM) image of the 1% Tm3+, 6% Yb3+: Gd0.2Bi1.8WO6 powder sample prepared by the high-temperature solid-phase method and calcined at 800 °C for 3 h is shown in Figure 4a. The SEM image reveals that the particle size is in the range of 0.5–3 μm, the particles have an inhomogeneous nearly spherical shape, the powder has undergone some agglomeration, and smaller particles are attached to the surface of larger particles. The SEM maps in Figure 4b–h show that Bi, W, O, Tm, Yb, and Gd are relatively uniformly distributed on the surface of the powder particles.
Figure 4. (a) SEM image of the 1% Tm3+, 6% Yb3+: Gd0.2Bi1.8WO6 sample; (b–h) SEM mapping of each element.
The energy-dispersive X-ray spectroscopy (EDS) spectrum of the 1% Tm3+, 6% Yb3+: Gd0.2Bi1.8WO6 sample is shown in Figure 5. On the basis of the contents of Bi, W, O, Tm, Yb, and Gd, each element is uniformly distributed in the powder particles.
Figure 5. EDS energy spectrum of the 1% Tm3+, 6% Yb3+: Gd0.2Bi1.8WO6 sample.
The UV–VIS diffuse reflection spectra of three samples, namely, the Bi2WO6 matrix, 1% Tm3+, 6% Yb3+: Bi2WO6 sample, and 1% Tm3+, 6% Yb3+: Gd0.2Bi1.8WO6 sample, are shown in Figure 6a. The samples containing Tm3+ have one weak absorption peak at 683 nm. To calculate the band gap (Eg) of the three samples, the following formula was used [24]:
[ F ( R ) hv ] 1 / n = A ( hv   - E g )
F ( R ) = ( 1 - R ) 2 / 2 R
where F(R) is the absorption coefficient α and R is the reflection coefficient (direct semiconductor: n = 1/2; indirect semiconductor: n = 2). A is the absorption constant, Eg is the luminescence band gap, ν is the photon frequency, and h is the Planck constant.
Figure 6. (a) Diffuse reflection spectra; (b) band gaps of Bi2WO6 and 1% Tm3+, 6% Yb3+: GdxBi2−xWO6 (x = 0, 0.2).
The results in Figure 6a reveal that with Tm3+/Yb3+/Gd3+ doping, the diffuse reflectance spectra shift towards longer wavelengths, indicating that the material can absorb lower-energy long-wave photons. In addition, after codoping with Gd3+, the absorption peaks of Tm3+ around 683 nm and 779 nm became more pronounced. Figure 6b shows the band gap Eg before and after Tm3+/Yb3+/Gd3+ doping, which are 2.69 eV, 2.3 eV, and 2.24 eV, respectively. Compared with the Bi2WO6 matrix, the band gaps of the samples are reduced with codoping Tm3+/Yb3+/Gd3+, especially Gd3+ codoping. These results indicate that the impurity energy bands reduce the recombination probability of the electron–hole pairs, increase the probability of radiative transitions, and significantly increase the luminescence intensity.
The band gap obtained here deviates somewhat from the calculation results shown in Figure 2. The main reason for this is that the VAPS calculations did not consider the actual probabilities of different Bi3+ sites and interstitial sites being occupied after doping. This may change the symmetry of the computational structure, and irreducible high-symmetry points may be offset relative to undoped points.

2.5. Upconversion Luminescence Properties

The spectra of y% Tm3+, 6% Yb3+: GdxBi2−xWO6 (x = 0, 0.1, 0.2, 0.3; y = 0.5, 1, 3, 6) under 980 nm laser excitation are shown in Figure 7. At room temperature, under 980 nm excitation, all samples exhibited characteristic peaks of Tm3+, such as those at 476 nm (1G4→3H6), 650 nm (1G4→3F4), 683 nm (3F2→3H6), 703 nm (3F3→3H6), 779 nm (3H4(1)→3H6) and 804 nm (3H4(2)→3H6).
Figure 7. Emission spectra of the y% Tm3+, 6% Yb3+: GdxBi2−xWO6 samples under 980 nm laser excitation: (a) y = 0.5, 1, 3, 6; (b) x = 0, 0.1, 0.2, 0.3.
When the doping concentrations of Yb3+/Tm3+ ions are 6% and 1%, respectively, and the doping amount of Gd3+ is x = 0.2, the synthesized Tm3+, Yb3+: Gd0.2Bi1.8WO6 sample exhibits the strongest luminescence, as shown in Figure 7a,b. Compared with that of the sample without Gd3+doping, when the Gd3+ doping amount is x = 0.2, the emission intensities of Tm3+ at 476 nm, 683 nm, 703 nm, and 804 nm increase by 1.8, 1.24, 1.35, and 81.9 times, respectively, as shown in Figure 7b. Many factors affect the luminescence of synthetic materials. The main reasons that Gd3+ doping increases the luminescence of Tm3+ materials are as follows.
Gd3+ and Bi3+ have the same valence, and substitution does not introduce intrinsic charge defects (such as vacancies), but size mismatches during ion doping may lead to lattice dislocations or oxygen vacancies to alleviate strain. Dislocations typically reduce luminescence (as nonradiative recombination centres), whereas moderate oxygen vacancies can increase luminescence. If Gd3+ doping occurs in the lattice interstitial state, the Bi–O bond within the lattice will be weakened or even broken, resulting in a small amount of oxygen atoms leaving the lattice and forming new oxygen vacancies. The newly added oxygen vacancies can serve as electron capture centres, introducing intermediate energy levels in the band gap, reducing the energy required for electron transitions, increasing the number of particles in the excited state, and increasing the probability of radiative transitions. The above results are consistent with the relevant content reported in the literature [25,26].
The introduction of an appropriate amount of Gd3+ can disperse the luminescent centre, namely, Tm3+, thereby avoiding the nonradiative dissipation caused by cross-energy transfer due to Tm3+ ion aggregation and allowing more energy to be released in the form of radiative luminescence. In addition, if Gd3+ with a smaller radius replaces Bi3+ with a larger radius, the adjacent M–O (M = Gd/Bi) bond length decreases, the local lattice shrinks, and compressive strain increases. At this point, owing to the increased probability of valence electron orbital overlap, the band gap of the material decreases. During the same excitation process, more electrons are excited, thereby promoting the upconversion process. Gd3+ doping does not change the main crystal structure of bismuth tungstate but does reduce the band gap, causing a redshift in the absorption edge of the material, which can then capture more long-wavelength photons and provide more energy for the upconversion luminescence process, thereby increasing the luminescence.
In the layered structure of perovskite, doped Gd3+ can adapt to irregular sites, especially at high doping concentrations, resulting in the formation of local disorder, increasing the probability of nonradiative recombination, increasing the number of defect states, and decreasing the luminescence.
On the basis of the energy level positions of Tm3+ in GdxBi2−xWO6 (3H4: 5800 cm−1, 3F4: 2900 cm−1), the energy mismatch during this process (3H4 +3H6→3F4+ 3F4 (CR1)) is close to zero, making it highly resonant and allowing it to be assisted by a single phonon [27]. Gd3+ doping tunes this rate by altering the lattice constant and Tm3+–Tm3+ distance. As the ion concentration increases, the CR1 energy transfer efficiency increases, resulting in reduced luminescence. In accordance with the literature [28], in the Tm3+-doped system, 1G4 + 3H6 → 3H4 + 3H5 (CR2) and 1G4 + 3H6→3H5 + 3H4 (CR3) are identified as the primary cross-relaxation pathways for the 1G4 energy level. Moreover, the reduced matrix elements (Uλ)2 of these two processes are relatively large, ensuring a high energy transfer rate. These channels have also been reported in Gd2O2S: Tm3+ [29]. At excessively high concentrations of Gd3+ ions, the ion spacing rapidly decreases, and the cross-energy transfer (3H4+3H6→3F4+3F4, 1G4+3H6→3H5+3H4, 1G4+3H6→3H4+3H5) between ions and the probability of nonradiative transitions increase; thus, the luminescence decreases.
The upconversion luminescence spectra of the 1% Tm3+, 6% Yb3+: Gd0.2Bi1.8WO6 sample measured under 980 nm laser excitation at powers ranging from 10 mW to 518 mW are shown in Figure 8a. All the intensities I of the 476 nm, 683 nm, 703 nm, and 804 nm emission peaks of Tm3+ in the sample gradually increase with increasing power P. According to the literature [30], the number of absorbed photons n can be determined on the basis of I ∝ P   n   . The value of n is influenced by the competition between the nonradiative relaxation probability and the radiative transition probability of intermediate ions.
Figure 8. The 1% Tm3+, 6% Yb3+: Gd0.2Bi1.8WO6 sample: (a) Relationship between the luminescence intensity and the excitation power; (b) Linear fitting of LgI and LgP.
The logarithmic relationships between the luminescence intensities I at 476 nm, 683 nm, 703 nm, 779 nm and 804 nm and the power P were fitted (178–518 mW), as shown in Figure 8b. The numbers of absorbed photons n corresponding to these emission peaks of Tm3+ are calculated to be 2.51, 1.89 1.97, 1.73 and 1.67, indicating that the peaks at 683, 703, 779 and 804 nm originate from two-photon absorption and that the peak at 476 nm originates from three-photon absorption.
When the excitation pump power increases, the probability of Yb3+ ions being excited increases, the probability of energy transfer from Yb3+ ions to Tm3+ ions increases, the probability of radiative transitions of Tm3+ ions increases, and the luminescence of the sample increases. When the excitation power increases to 518 mW, the thermal effect caused by the high power increases the probability of cross-relaxation between ions and the nonradiative relaxation probability, saturation effects occur, and the luminescence intensity I and power P have a nonlinear relationship. Thus, the number of absorbed photons n cannot be determined. Therefore, the best power of 518 mW was selected for this experiment.
The energy transfer and energy level transition of Yb3+ and Tm3+ under 980 nm laser excitation are shown in Figure 9. The Tm3+ ions in the ground state 3H6 absorb some of the energy and transition to 3H5. Yb3+ has a large absorption cross-section at 980 nm, so Yb3+ absorbs photons under 980 nm excitation and transitions to the excited state 2F5/2. Because the 2F5/2 energy level of Yb3+ and the 3H5 energy level of Tm3+ do not exactly match, an energy transfer process from Yb3+ to Tm3+ occurs with the assistance of phonons. ET1, ET2 and ET3 in the figure represent the transfer of energy from Yb3+ to Tm3+ [15]. Tm3+ ions at 3H5 undergo nonradiative relaxation to 3F4, and Tm3+ ions accept energy from Yb3+ and transition from 3F4 to 3F2,3. Some Tm3+ ions in the excited state level 3F2,3 transition to the ground state 3H6 and emit red light at 683 and 703 nm. Some Tm3+ ions at the 3F2,3 level undergo nonradiative relaxation to the splitting energy level 3H4(1)(2) state. Here, 3H4 is a multienergy level that is split into upper and lower energy levels, denoted 3H4(1) and 3H4(2). When Tm3+ ions transition from 3H4(1)(2) to 3H6, they produce near-infrared light with wavelengths of 779 nm and 804 nm. With the help of phonons, the Yb3+ ions in the excited state of 2F5/2 transfer energy to the Tm3+ ions at the 3H4 level, and the Tm3+ ions are excited from 3H4 to 1G4. Some Tm3+ ions at the 1G4 energy level transition to the ground state 3H6 and emit blue light at 476 nm, and a small number of Tm3+ ions at the 1G4 energy level transition to the 3F4 energy level and emit red light at 650 nm [15].
Figure 9. Energy transfer and energy level transition of Yb3+ and Tm3+ under 980 nm laser excitation.
The energy level decay curves of 3F3→3H6 and 3H4(2)→3H6 under 980 nm excitation for the 1% Tm3+, 6% Yb3+: GdxBi2−xWO6 (x = 0, 0.2) samples are shown in Figure 10. By fitting the energy level decay curve with a double exponential function, the energy level lifetime τ is calculated as follows:
I ( t ) = A 1 e − t / τ 1 + A 2 e − t / τ 2
τ = A 1 τ 1 2 + A 2 τ 2 2 A 1 τ 1 + A 1 τ 2
where I(t) is the luminescence intensity and A1 and A2 are coefficients. τ1 and τ2 are the radiative transition lifetime and radiation-free relaxation lifetime, respectively. τ is the energy level lifetime.
Figure 10. Energy level decay curves and fitting curves of the 1% Tm3+, 6% Yb3+: GdxBi2−xWO6 samples: (a) x = 0, λex = 703 nm; (b) x = 0.2, λex = 703 nm; (c) x = 0, λex = 804 nm; (d) x = 0.2, λex = 804 nm.
The lifetimes of the 3F3 and 3H4(2) energy levels of the sample before and after Gd3+ doping are shown in Table 6. After the material was doped with Gd3+, the lifetimes of the 3F3 and 3H4(2) energy levels for Tm3+ in the synthesized material increased to varying degrees. The analysis results in Figure 6 show that moderate codoping with Gd3+ shifted the absorption band of the material towards longer wavelengths. These results are consistent with the predicted trend shown in Figure 2b,c, indicating that Gd3+ doping narrows the matrix band gap, which is beneficial for the matrix to absorb more low-energy photons and promote energy upconversion. Therefore, Gd3+ codoping can optimize the energy transfer from Yb3+ to Tm3+ through energy exchange interactions, thereby extending the lifetime of the Tm3+ energy levels.
Table 6. Energy level lifetimes of the 1% Tm3+, 6% Yb3+: GdxBi2−xWO6 (x = 0, 0.2) samples.

2.6. Temperature Sensing Characteristics

The upconversion emission spectra of the 1% Tm3+, 6% Yb3+: Gd0.2Bi1.8WO6 sample in the range of 450–750 nm under 980 nm laser excitation (518 mW) and variable temperature conditions (298–573 K) are shown in Figure 11a. The upconversion emission spectra from 750–850 nm at 298 to –573 K under the same excitation conditions is shown in Figure 11b.
Figure 11. Emission spectra of the 1% Tm3+, 6% Yb3+: Gd0.2Bi1.8WO6 sample at 298~573 K: (a) 450–750 nm, (b) 750–850 nm.
The intensities of the 804 nm, 650 nm and 476 nm emission peaks monotonically decrease as the temperature increases from 298 K to 573 K, whereas those of the 703 nm and 683 nm emission peaks first increase but then decrease with increasing temperature. Owing to the temperature sensitivity of the thermal coupling energy levels 3F2,3 and 3H4, with the assistance of phonons, the number of particles thermally excited at the 3F2,3 energy levels begins to increase, which leads to an increase in the probability of radiative transitions from the 3F2,3 energy levels and increases the emission intensities at 683 nm and 703 nm, corresponding to the thermal coupling energy levels. Moreover, the probability of the particles in the 3F2,3 energy level relaxing to the 3H4 energy level decreases. Therefore, the probabilities of emissions from the 3H4 transition to 3H6 and from the 3F2,3 excited state to 1G4 decrease, and the luminescence intensities at 804 nm, 779 nm, 650 nm and 476 nm decrease.
The relationship between the fluorescence intensity ratio (FIR) and temperature based on the thermal coupling energy levels of luminescent materials follows the Boltzmann distribution function [30]:
FIR = I 1 I 2 = A exp ( − Δ E   k B T )
where I1 and I2 denote the fluorescence intensities of the two peaks from the thermal coupling energy levels; FIR is the ratio of the intensities of the two peaks; and A is a constant related to the energy level simplicity, spontaneous radiation rate, and phonon energy of Tm3+. ∆E is the energy level spacing between the upper thermal coupling energy levels, and kB is the Boltzmann constant.
The thermal coupling energy levels 3F3 and 3H4 transition to the 3H6 energy level, emitting light at 703 nm and 804 nm, respectively. The fluorescence intensity ratio at 703 nm and 804 nm varies with temperature T as follows:
FIR = I 703 nm I 804 nm = 0.3396 exp ( − 1807.4475 / T )
The relationship between FIR703nm and 804nm and temperature was fitted, as shown in Figure 12a.
Figure 12. (a) Fluorescence intensity ratio of the 703 nm and 804 nm peaks versus temperature. (b) Sa and Sr.
In Figure 12a, R2 indicates the degree of agreement between the theoretical fit and the experimental data, and the theoretical values are in perfect agreement with the experimental values when R2 = 1.
In accordance with the literature [31], the absolute thermometry sensitivity Sa can be expressed as follows:
S a = | d F I R d T |
The relative thermometry sensitivity Sr can be expressed as follows:
S r = | 1 F I R d F I R d T |
The relationships of the absolute thermometry sensitivity Sa and relative thermometry sensitivity Sr with temperature were calculated for the 1% Tm3+, 6% Yb3+: Gd0.2Bi1.8WO6 sample at temperatures ranging from 298 to 573 K, as shown in Figure 12b. The obtained Sr of the material decreases with increasing temperature. At 298 K, the maximum Sa and Sr values are 0.000084 K−1 (573 K) and 0.0153 K−1 (298 K), respectively.
The fluorescence intensity ratio for the nonthermal coupling energy levels can be used to measure the temperature; according to reference [32], a polynomial function can be used to establish a quantitative relationship between FIR and temperature, and the equation is as follows:
F I R = A + B T + C T 2 + D T 3
where FIR is the intensity ratio of the two luminescence peaks; T denotes the absolute temperature; and A, B, C and D are undetermined coefficients.
The FIR values of the 703 nm and 476 nm peaks (nonthermal coupling energy level pairs 3F3/1G4→3H6) versus temperature for this sample are shown in Figure 13a. The fitted FIR versus T relationship is as follows:
FIR = I 703 nm I 476 nm = - 24023.486 + 199.514 T − 0.547 T   2 + 4.966 × 10 − 4 T   3
Figure 13. (a) Fluorescence intensity ratio of the 703 nm and 476 nm peaks versus temperature; (b) Sa and Sr.
On the basis of FIR703nm/476nm, Sa and Sr were calculated from 298 to 573 K, as shown in Figure 13b. The maximum Sa is 61.3556 K−1 (573 K), and the maximum Sr is 3.4907 K−1 (298 K).
The temperature sensing properties of rare earth ions and Gd3+-codoped upconversion materials with different matrix materials are shown in Table 7. Under 980 nm excitation, the 1% Tm3+, 6% Yb3+: Gd0.2Bi1.8WO6 sample prepared in this work exhibits better properties compared with the materials reported in the literature [7,8,33,34,35] in terms of the maximum Sr. Compared with that of the undoped Gd3+ sample [15], the maximum Sr of the Gd3+-codoped sample was 92.35 times larger.
Table 7. Temperature measurement sensitivity of rare-earth ions in different matrix materials.
The temperature resolution δT refers to the smallest change in temperature that a temperature-sensing material can sense [36] and is calculated as follows:
δ T = 1 S r δ Δ Δ
δ Δ Δ = ( δ I I 1 ) 2 + ( δ I I 2 ) 2
where δ Δ / Δ represents the relative uncertainty in the fluorescence intensity ratio, Sr is the relative thermometry sensitivity, Δ is the fluorescence intensity ratio, δI is the uncertainty in the fluorescence intensity, and I1 and I2 are the intensities of the two fluorescence peaks.
The δ T of this sample based on the FIR703nm/804nm or FIR703nm/476nm value was calculated according to Equations (25) and (26), as shown in Figure 14. The corresponding minimum δ T values are 0.0474 K at 423 K and 0.0083 K at 298 K, respectively.
Figure 14. Temperature resolution δ T at different temperatures for 1% Tm3+, 6% Yb3+: Gd0.2Bi1.8WO6.
The CIE colour coordinates and colour temperatures of this powder at different temperatures are shown in Figure 15. As the temperature increases (298–573 K), the chromaticity coordinates of the material shift from the blue region to the red region.
Figure 15. The CIE coordinates of the 1% Tm3+, 6% Yb3+: Gd0.2Bi1.8WO6 phosphor at different temperatures.
Thermochromic photos of this phosphor in a dark environment are shown in Figure 16. When the sample is irradiated with a 980 nm (518 mW) laser, as the temperature increases (298–473 K), the luminescence colour of the sample changes from blue to red. According to spectrum 11 (a), at room temperature, the blue light intensity emitted by the sample at 476 nm is not significantly different from the red light intensity at 683 nm and 703 nm. When the temperature rises from room temperature to 473 K, the red light emitted by the sample rapidly increases at 683 nm and 703 nm, but the blue light rapidly weakens, causing the composite light color to shift towards red light. When the temperature exceeds 473 K, the red light also begins to weaken, so the corresponding color of the light begins to shift in the opposite direction. When the temperature gradually decreases from 573 K, the luminescence colour of the sample changes from red to blue, which indicates that the phosphor synthesized in this work has potential application value in thermochromism and laser anticounterfeiting. After four cycles of heating and cooling, the luminescence of the sample switched between blue and red light, and the luminescence was relatively stable.
Figure 16. (a) Thermochromic photos of 1% Tm3+, 6% Yb3+: Gd0.2Bi1.8WO6 phosphor under different temperature at 980 nm excitation; (b) luminescence color change of under the temperature cycles.

2.7. Magnetic Properties of the Materials

Considering that Gd3+ has seven unpaired 4f electrons and strong paramagnetic properties, it can significantly shorten the relaxation time of surrounding water molecules at magnetic resonance T1 and generate T1-weighted signals, and its chelates can serve as good magnetic resonance contrast agents. If both fluorescence temperature measurements and magnetic resonance imaging can be achieved with synthetic materials, their application value will increase. Therefore, the magnetic properties of synthetic materials at different temperatures were analysed.
As shown in Figure 17, when the applied magnetic field increased from −20 to 20 kOe, the magnetization strength of 1% Tm3+, 6% Yb3+, x% Gd: Bi2WO6 (x = 0, 10) powder under an external magnetic field significantly increased. Compared with that of the Tm3+, Yb3+: Bi2WO6 powder, the magnetization of the sample doped with Gd3+ (x = 0.2) increased fourfold and reached 0.08174 emu/g (20 kOe, 300 K).
Figure 17. Magnetization intensity of the 1% Tm3+, 6% Yb3+: GdxBi2−xWO6 (x = 0, 0.2) powder under different external magnetic fields at 300 K.
Table 8 presents a comparison of the magnetic properties of different matrix materials doped with Gd3+. The 1% Tm3+, 6% Yb3+: Gd0.2Bi1.8WO6 powder particles synthesized in this work exhibit typical paramagnetic properties.
Table 8. Magnetization of the different host materials.
The temperature-dependent magnetic properties of the 1% Tm3+, 6% Yb3+: Gd0.2Bi1.8WO6 powder under an external magnetic field of 1 kOe are shown in Figure 18. At 1 kOe, as the temperature increases from 5 K to 300 K, the magnetization intensity of this powder samples decreases exponentially. The data were fit to obtain the relationship between the magnetization M and temperature T of the powder sample as follows:
M   = 0.253 exp ( − T / 12.556 ) + 0.009
Figure 18. Magnetism (5~300 K) of the 1% Tm3+, 6% Yb3+: Gd0.2Bi1.8WO6 powder samples under an external magnetic field of 1 kOe.
In Figure 18, R2 = 0.96 represents the degree of agreement between the theoretical fit and the experimental value. Through the above M–T function relationship, this material can provide information regarding magnetization intensity under external magnetic fields while enabling temperature measurements, thereby permitting the dual calibration of temperature and magnetism. Under an external magnetic field of 1 kOe and temperatures of 5 K and 300 K, the magnetization strengths of the 1% Tm3+, 6% Yb3+: Gd0.2Bi1.8WO6 samples were 0.19724 and 0.00447 emu/g, respectively. The above results indicate that the powder synthesized in this work has potential applications in fluorescence thermometry and magnetic resonance imaging.

3. Materials and Methods

3.1. Theoretical Calculation

All density functional theory (DFT) calculations were conducted with the Vienna ab-Initio Simulation Package (VASP) [40,41]. The generalized gradient approximation (GGA) using the Perdew–Burke–Ernzerhof (PBE) functional was employed to account for exchange correlations. The ionic cores and valence electrons were described using the projected augmented wave (PAW) method. A plane-wave basis set with an energy cutoff of 450 eV was adopted for the calculations. On the basis of a 2 × 1 × 2 supercell with 144 atoms, Bi2WO6 models with different concentrations of doped Tm, Yb, and Gd were constructed. Additionally, 2 × 2 × 2 gamma-centre grids were used for structure relaxation. During structure optimization, the conjugate gradient method was used, and the convergence criteria for energy and force were set to 1 × 10−5 eV and 2 × 10−2 eV Å−1, respectively.

3.2. Experimental Methods

The raw materials Bi2O3 (99.9%), WO3 (99.9%), Tm2O3 (99.9%), Yb2O3 (99.9%), and Gd2O3 (99.9%) (from Aladdin, Shanghai, China) were weighed using an AL104 electronic balance and mixed in accordance with the chemical ratios of y% Tm3+, 6% Yb3+: GdxBi2−xWO6 (x = 0, 0.06, 0.1, 0.2, 0.3; y = 0.5, 1, 3, 6). The ion doping concentration is expressed as a mole percentage concentration. The powder was then ground for 25 min and calcined in a muffle furnace (SX-12-16) at 800 °C for 3 h in air to obtain various Tm3+, Yb3+, Gd3+: Bi2WO6 samples, and the above doping concentrations were determined on the basis of the amounts of the materials.
Physical phase analysis of the samples was performed using a X-ray diffractometer (XRD-6100, Shimadzu, Kyoto, Japan). Scanning electron microscope (ZEISS SUPRA55 VP, Carl Zeiss, Jena, Germany) was used to observe the microscopic morphology, size and dispersion of the samples. The elemental and powder contents on the surface were analysed using a EDS X-ray energy spectrometer (X-Flash SDD 5010, Bruker, Karlsruhe, Germany). Fluorescence detection was performed using an full-featured steady-state/transient fluorescence spectrometer (Edinburgh VFLS920, Edinburgh Instruments, Livingston, UK), which was used to measure the upconversion emission spectra of the samples at different pump powers, and the excitation source was infrared light from a 980 nm laser (MDL-III-980-2W, Edinburgh Instruments, UK). Diffuse reflectance spectra were obtained with a UV–visible diffuse reflection spectrometer (UV-3900 plus, Shimadzu, Japan). To detect the upconversion luminescence of the samples at different temperatures, the samples were heated in the high-temperature accessory heater of the spectrometer to temperatures ranging from 298 K to 573 K. The magnetic properties of the synthesized powders were measured using an high precision magnetic measurement system (MPMS XL-7 SQUID, San Diego, CA, USA). The magnetic changes in the synthesized powder were measured at a temperature of 300 K under an external magnetic field ranging from −20 to 20 kOe. The temperature-dependent magnetic properties of the synthesized powders were measured in the temperature range of 5–300 K under an external magnetic field of 1 kOe. To avoid laser-induced thermal effects, the samples were excited with a low excitation power. The instruments were calibrated before use.

4. Conclusions

y% Tm3+, 6% Yb3+: GdxBi2−xWO6 (x = 0, 0.06, 0.1, 0.2, 0.3; y = 0.5, 1, 3, 6) upconversion luminescent materials were prepared via a high-temperature solid-phase method and calcined at 800 °C for 3 h. Young’s modulus and the Debye temperature of the Bi2WO6 matrix material doped with Gd3+ were calculated to be 183.579 GPa and 392.45 K, respectively. Compared with the NaYF4 matrix, the Bi2WO6 material doped with Gd3+ had lower Debye temperatures, which resulted in a lower probability of nonradiative transitions. The XRD results revealed that the doping of low-concentration small-radius ions Tm3+ and Yb3+ does not affect the orthorhombic crystal structure of the Bi2WO6 matrix, and its diffraction peaks shift towards larger angles with increasing doping concentrations. However, as the amount of doped Gd3+ increases, diffraction peaks of Gd2WO6 appear, and the main diffraction peak of the lattice (131) shifts to a smaller angle, indicating that in addition to Gd3+ replacing Bi3+, excessive Gd3+ ions enter the main lattice gap, thereby expanding the lattice. SEM images revealed that the samples were composed of 0.5~3 μm heterogeneous particles, and EDS analysis revealed that the elements were evenly distributed in the powder. Under 980 nm excitation, the emission intensity of the 1% Tm3+, 6% Yb3+: Gd0.2Bi1.8WO6 sample was the strongest among all the samples, and the intensity of the Tm3+ peak at 804 nm increased by 81.9 times. Moderate Tm3+, Yb3+ and Gd3+ doping can cause the absorption band of the synthesized material to shift towards longer wavelengths, and the band gaps decrease. When the sample was excited at 980 nm (178–518 mW), the logarithm of its light intensity and power exhibited a linear relationship. Tm3+ was emitted from three-photon absorption at 476 nm (n = 2.51) and from two-photon absorption at 683, 703, 779, and 804 nm (n = 1.89 1.97, 1.73 and 1.67, respectively). Under 980 nm excitation (518 mW), from 298 K to 573 K, on the basis of the fluorescence intensity ratio of 703 nm/804 nm or 703 nm/476 nm for the 1% Tm3+, 6% Yb3+: Gd0.2Bi1.8WO6 sample, the maximum relative sensitivities reach 0.0153 K−1 at 298 K and 3.4907 K−1 at 298 K, with minimum temperature resolutions of 0.0474 K at 423 K and 0.0083 K at 298 K. Under excitation at 980 nm, as the temperature increased from 298 K to 473 K, the luminescence colour of this powder changed from blue to purple, then to orange, and finally to red. Under an external magnetic field of 20 kOe and a temperature of 300 K, the magnetization of the sample was 0.08174 emu/g. Compared with that of the undoped Gd3+ sample, the temperature sensitivity of the Gd3+-codoped sample increased by 92.35 times. This material enables noncontact, high-sensitivity micro/nanoscale temperature sensing and real-time magnetic feedback, with potential applications in temperature sensing and magnetic resonance imaging.

Author Contributions

X.F.: Investigation, methodology, data curation, writing—original draft preparation; L.W.: formal analysis, investigation, methodology, resources, data curation, software, supervision, writing—review and editing, project administration, funding acquisition; J.S.: validation, visualization, data curation; M.J.: methodology, software; M.M., Y.Z. and Y.B.: Conceptualization. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by the National Natural Science Foundation of China (12164048) and the Natural Science Foundation of Xinjiang Uygur Autonomous Region (2023D01A41).

Data Availability Statement

The data that supports the findings of this study are available on request from the corresponding author.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Zheng, Y.; Meana, Y.; Mazza, M.M.A.; Baker, J.D.; Minnett, P.J.; Raymo, F.M. Fluorescence switching for temperature sensing in water. J. Am. Chem. Soc. 2022, 144, 4759–4763. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  2. He, H.; Jiang, Q.; Wan, Y.; Mia, H.; Qu, X.; Zhou, M.; He, X.; Li, X.; Hong, M.; Yu, Z.; et al. Biological skin-inspired damage warning and self-healing thermoelectric aerogel fiber via coaxial wet spinning for wearable temperature sensing. J. Mater. Sci. Technol. 2026, 250, 57–271. [Google Scholar] [CrossRef] [Scilit]
  3. Zhou, H.; Zhu, K.; Wang, J.; Qiu, J.; Yue, L.; Wang, L.-G.; Ye, L. Effects of Yb3+ concentration on up-conversion luminescence and temperature sensing characteristics of Tm3+/Yb3+:Y2O3 phosphors. J. Alloys Compd. 2022, 918, 165674. [Google Scholar] [CrossRef] [Scilit]
  4. Zhou, H.; An, N.; Zhu, K.; Qiu, J.; Yue, L.; Wang, L.-G.; Ye, L. Optical temperature sensing properties of Tm3+/Yb3+ co-doped LuAG polycrystalline phosphor based on up-conversion luminescence. J. Lumin. 2021, 229, 117656. [Google Scholar] [CrossRef] [Scilit]
  5. Krishna, K.; Upadhyay, M.M.; Kesarwani, V.; Kumar, K. Blue frequency upconversion emission and optical thermometry of Ca3(PO4)2: Tm3+/Yb3+. Optik 2023, 273, 170477. [Google Scholar] [CrossRef] [Scilit]
  6. Sun, Y.; Wang, Y.; Hu, C.; Zhou, X.; Hao, J.; Li, W.; Li, H. Energy transfer from Pr3+ to Gd3+ and upconversion photoluminescence properties of Y7O6F9: Pr3+, Gd3+. Materials 2022, 15, 7680. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  7. Zhang, Y.; Guo, Y.; Zheng, X.; Wang, P.; Liu, H. Bright upconversion luminescence performance of Yb3+/Tm3+/Gd3+/Er3+ doped AWO4 (A=Sr or Ca) phosphor for optical temperature sensor. Phys. B Condens. Matter 2023, 649, 414467. [Google Scholar] [CrossRef] [Scilit]
  8. Xiao, X.; Sun, Q.; Hu, T.; Song, Y.; Zhou, X.; Zheng, K.; Sheng, Y.; Shi, Z.; Zou, H. Multifunctional CaF2: Yb3+, Ho3+, Gd3+ nanocrystals: Insight into crystal growth and properties of upconversion luminescence, magnetic, and temperature sensing properties. Inorg. Chem. 2022, 61, 14934–14946. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  9. Park, K.; Kim, H.; Kim, D.; Gwon, S. Influence of lattice distortions on the emission wavelengths of Y3+–and Gd3+–substituted Lu3Al5O12: Ce3+ phosphors. Ceram. Int. 2023, 49, 15176–15182. [Google Scholar]
  10. Kolesnikov, I.E.; Vidyakina, A.A.; Vasileva, M.S.; Nosov, V.G.; Bogachev, N.A.; Sosnovsky, V.B.; Skripkin, M.Y.; Tumkin, I.I.; Lähderanta, E.; Mereshchenko, A.S. The effect of Eu3+ and Gd3+ co-doping on the morphology and luminescence of NaYF4: Eu3+, Gd3+ phosphors. New J. Chem. 2021, 45, 10599–10607. [Google Scholar]
  11. Revankar, S.G.; Gedekar, K.A.; Belsare, P.D.; Moharil, S. Study of luminescence of Gd3+ in some aluminoborates and energy transfer from Gd3+to Ln3+ (Ln = Eu, Tb or Dy). Optik 2022, 266, 169610. [Google Scholar] [CrossRef] [Scilit]
  12. Ru, J.; Xu, W.; Kou, M.; Dong, H.; Tang, X.; Chen, Y.; Kang, L.; Dai, L.; Liang, C. A novel Gd3+ DTPA-bisamide complex with high relaxivity as an MRI contrast agent. J. Mater. Chem. B 2023, 11, 7182–7189. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  13. Meenambal, R.; Kannan, S. Cosubstitution of lanthanides (Gd3+/Dy3+/Yb3+) in β-Ca3(PO4)2 for upconversion luminescence, CT/MRI multimodal imaging. ACS Biomater. Sci. Eng. 2018, 4, 47–56. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  14. Shariati, A.; Ebrahimi, T.; Babadinia, P.; Shariati, F.S.; Cohan, R.A. Synthesis and characterization of Gd3+-loaded hyaluronic acid-polydopamine nanoparticles as a dual contrast agent for CT and MRI scans. Sci. Rep. 2023, 13, 4520. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  15. Xiakeer, A.; Wang, L.; Maimaiti, M.; Feng, X.; Jiang, M. Luminescence and temperature sensing properties of Li+, Na+ or K+, Tm3+, and Yb3+ codoped Bi2WO6 phosphors. Rev. Adv. Mater. Sci. 2023, 62, 20230104. [Google Scholar] [CrossRef] [Scilit]
  16. Neufeld, O.; Toroker, M.C. Platinum-doped α-Fe2O3 for enhanced water splitting efficiency: A DFT+U study. J. Phys. Chem. C 2015, 119, 5836–5847. [Google Scholar]
  17. Denault, K.A.; Brgoch, J.; Kloß, S.D.; Gaultois, M.W.; Siewenie, J.; Page, K.; Seshadri, R. Average and local structure, debye temperature, and structural rigidity in some oxide compounds related to phosphor hosts. ACS Appl. Mater. Interfaces 2015, 7, 7264–7272. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  18. Zhou, Y.; Li, C.; Wang, Y. Crystal-field engineering control of an ultraviolet-visible-responsive near-infrared-emitting phosphor and its applications in plant growth, night vision, and NIR spectroscopy detection. Adv. Opt. Mater. 2022, 10, 2102246. [Google Scholar] [CrossRef] [Scilit]
  19. Yang, Z.; Cui, J.; Gu, L.; Wang, T.; Song, J. Leveraging structural rigidity for thermal robust scintillation in rare-earth halide perovskites. Adv. Powder Mater. 2026, 5, 100371. [Google Scholar] [CrossRef] [Scilit]
  20. Li, K.; Dai, M.; Fu, Z.; Wang, Z.; Xu, H.; Wang, R. A latest-generation fluoride with excellent structural stiffness for ultra-efficient photoluminescence and specific four-peak emission temperature sensing. Inorg. Chem. Front. 2024, 11, 172–185. [Google Scholar] [CrossRef] [Scilit]
  21. Luo, X.; Akimoto, K. Upconversion properties in hexagonal-phase NaYF4:Er3+/NaYF4 nanocrystals by off-resonant excitation. Appl. Surf. Sci. 2013, 273, 257–260. [Google Scholar] [CrossRef] [Scilit]
  22. Phuruangrat, A.; Buapoon, S.; Bunluesak, T.; Suebsom, P.; Wannapop, S.; Thongtem, T.; Thongtem, S. Hydrothermal preparation of Au-doped Bi2WO6 nanoplates for enhanced visible-light-driven photocatalytic degradation of rhodamine B. Solid State Sci. 2022, 128, 106881. [Google Scholar] [CrossRef] [Scilit]
  23. Uvarov, V.; Popov, I. Metrological characterization of X-ray diffraction methods at different acquisition geometries for determination of crystallite size in nano-scale materials. Mater. Charact. 2013, 85, 111–123. [Google Scholar] [CrossRef] [Scilit]
  24. Zhang, Y.; Zhang, N.; Wang, P.; Zheng, X.; Guo, Y.; Liu, H. Enhancement of up-conversion luminescence efficiency and temperature sensing properties in BaWO4: Ho3+/Yb3+ phosphor via Gd3+ incorporation. Mater. Today Commun. 2022, 33, 104589. [Google Scholar] [CrossRef] [Scilit]
  25. Tian, N.; Zhang, Y.; Huang, H.; He, Y.; Guo, Y. Influences of Gd substitution on the crystal structure and visible-light-driven photocatalytic performance of Bi2WO6. J. Phys. Chem. C 2014, 118, 15640–15648. [Google Scholar] [CrossRef] [Scilit]
  26. Mathankumar, G.; Bharathi, P.; Krishna Mohan, M.; Harish, S.; Navaneethan, M.; Archana, J.; Suresh, P.; Mani, G.; Dhivya, P.; Ponnusamy, S.; et al. Synthesis and functional properties of nanostructured Gd-doped WO3/TiO2 composites for sensing applications. Mater. Sci. Semicond. Process. 2020, 105, 104732. [Google Scholar] [CrossRef] [Scilit]
  27. Veselský, K.; Santos Magalhaes, E.; Nasser, K.; Ojha, N.; Petit, L.; Šulc, J.; Jelínková, H. Structural, thermal and spectroscopic properties of Tm3+ doped TeO2-Bi2O3-ZnO glasses. J. Alloys Compd. 2026, 1050, 185662. [Google Scholar] [CrossRef] [Scilit]
  28. Chen, X.; Salamo, G.J.; Li, S.; Wang, J.; Guo, Y.; Gao, Y.; He, L.; Ma, H.; Tao, J.; Sun, P.; et al. Two-photon, three-photon, and four-photon excellent near-infrared quantum cutting luminescence of Tm3+ ion activator emerged in Tm3+:YNbO4 powder phosphor one material simultaneously. Physica B 2015, 479, 159–164. [Google Scholar] [CrossRef] [Scilit]
  29. Yu, D.C.; Martín-Rodríguez, R.; Zhang, Q.-Y.; Meijerink, A.; Rabouw, F.T. Multi-photon quantum cutting in Gd2O2S:Tm3+ to enhance the photo-response of solar cells. Light Sci. Appl. 2015, 4, e344. [Google Scholar] [CrossRef] [Scilit]
  30. Jiang, M.; Wang, L.; Maimaiti, M.; Feng, X.; Zhang, Y.; Shi, J. Effects of Li+, Na+, and K+ doping on the microstructure, fluorescence thermometry, and thermochromism of Ho3+, Yb3+: Bi2WO6 materials. J. Mater. Chem. C 2025, 13, 15555–15571. [Google Scholar]
  31. Liu, L.; Liu, H.; Zou, W.; Ding, S. Er3+ doping YbTaO4 phosphors: Upconversion luminescence and temperature sensing characteristics. Ceram. Int. 2023, 49, 28500–28505. [Google Scholar] [CrossRef] [Scilit]
  32. Lu, Y.; Lin, D.; Li, Y.; Zou, H.; Lu, H.; Zhu, J.; Liu, S.; Li, J.; Zhang, Q. Thermal enhancement of upconversion luminescence in Sc2Mo3O12: Nd/Yb/Er crystals for optical temperature sensing. Ceram. Int. 2023, 49, 29370–29374. [Google Scholar] [CrossRef] [Scilit]
  33. Upadhyay, M.M.; Kumar, K. Gd3+ ion induced UV up-conversion emission and temperature sensing in Tm3+/Yb3+: Y2O3 phosphor. J. Rare Earths 2023, 41, 1295–1301. [Google Scholar]
  34. Yu, X.; Li, X.; Jiang, Y.; Song, Z.; Zhang, Z.; Xue, X.; Jiang, Z.; Fan, J.; Zhao, P. Effects of K+ and Gd3+ concentration on up-conversion luminescence and optical thermometric properties in NaYF4:Yb/Ho microcrystals. J. Alloys Compd. 2022, 896, 162793. [Google Scholar] [CrossRef] [Scilit]
  35. Zhang, J.; Riesen, H. Mechanochemical preparation of nanocrystalline NaYF4: Gd3+/Yb3+/Tm3+: An efficient upconversion phosphor. Chem. Phys. Lett. 2015, 641, 1–4. [Google Scholar] [CrossRef] [Scilit]
  36. Qiu, L.; Wang, P.; Wei, X.; Chi, F.; Chen, Y.; Yin, M. Investigation of a phosphor mixture of LiAl5O8: Cr3+ and LuPO4: Tb3+ as a dual-mode temperature sensor with high sensitivity. J. Alloys Compd. 2021, 879, 160461. [Google Scholar] [CrossRef] [Scilit]
  37. Liu, Z.; Wang, Q.; Yao, S.; Yang, L.; Yu, S.; Feng, X.; Li, F. Synthesis and characterization of Tb3+/Gd3+ dual-doped multifunctional hydroxyapatite nanoparticles. Ceram. Int. 2014, 40, 2613–2617. [Google Scholar] [CrossRef] [Scilit]
  38. Atabaev, T.S.; Hong, N.H. Enhanced optical properties of ZrO2: Eu3+ powders codoped with gadolinium ions. J. Sol.-Gel Sci. Technol. 2017, 82, 15–19. [Google Scholar] [CrossRef] [Scilit]
  39. Kumar, A.; Prakash Tiwari, S.; Kumar, K.; da Silva, J.C.E. Magnetic tuning in upconversion emission enhanced through Ag+ ions co-doped in GdF3: Ho3+/Yb3+ phosphor and a real-time temperature sensing demonstration. J. Alloys Compd. 2019, 776, 207–214. [Google Scholar] [CrossRef] [Scilit]
  40. Kresse, G.; Furthmüller, J. Efficiency of ab-initio total energy calculations for metals and semiconductors using a plane-wave basis set. Comput. Mater. Sci. 1996, 6, 15–50. [Google Scholar] [CrossRef] [Scilit]
  41. Kresse, G.; Furthmüller, J. Efficient iterative schemes for ab initio total-energy calculations using a plane-wave basis set. Phys. Rev. B 1996, 54, 11169. [Google Scholar] [CrossRef] [Scilit] [PubMed]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.