Abstract
In spinal correction surgery, metallic rods are commonly bent intraoperatively by surgeons to conform to the patient-specific spinal curvature and are then fixed with pedicle screws. However, intraoperative rod contouring can introduce surface scratches and notches, which may reduce fatigue strength and act as initiation sites for fracture. In this study, spinal correction rods with a prescribed spinal contour were fabricated from a Co–28Cr–6Mo–0.11N alloy (hereafter referred to as the CCMN alloy) by electron beam powder bed fusion (PBF-EB) to reduce dependence on intraoperative bending. Their compressive response, cyclic compression behavior, and fracture characteristics were experimentally evaluated, and their deformation behavior was further examined by finite element analysis (FEA). The CCMN rods were subjected to one, two, or three cycles of combined aging and reverse transformation heat treatment, denoted RT, 2RT, and 3RT, respectively. Under a compressive load of 1000 N, the displacement decreased with an increasing number of reverse transformation cycles, and the 3RT specimen showed the highest apparent resistance to deformation. The loads required to produce a displacement of 5 mm were 812, 843, 865, and 896 N for the as-built, RT, 2RT, and 3RT rods, respectively; thus, the 3RT rod exhibited an increase of 84 N relative to the as-built rod. Although all specimens were fabricated using the same CAD geometry and adjusted to the same nominal dimensional profile, small specimen-specific geometric deviations could not be independently quantified. Therefore, the observed differences in load–displacement response cannot be attributed exclusively to heat-treatment-induced microstructural changes. Furthermore, increasing the maximum diameter of the middle region of the variable-diameter rod from 7 to 8 mm reduced the displacement under 1000 N from 3.3 to 2.7 mm. In a single-specimen cyclic compression screening test at 0–300 N, 1 Hz, and 1 × 106 cycles, no apparent macroscopic residual deformation or fracture was observed. This result represents runout under the specified loading condition and does not establish a fatigue limit. These results support the feasibility of using PBF-EB to fabricate CCMN rods with prescribed curved and variable-diameter geometries and demonstrate a stable mechanical response under the specific static and cyclic loading conditions examined in this study.
1. Introduction
In corrective surgery for spinal deformities such as scoliosis, rods and screws are widely used to correct and maintain spinal alignment. Recent enabling technologies, including preoperative planning, intraoperative navigation, and patient-specific implants, have been reported to improve the outcomes of spinal deformity surgery [1,2]. In conventional procedures, a straight rod is manually bent intraoperatively to fit the patient-specific spinal curvature, as shown in Figure 1. Although this bending operation enables flexible intraoperative adjustment, it can also introduce scratches, notches, local plastic deformation, and residual stresses on the rod surface. Rod contouring has been reported to reduce the fatigue strength of spinal constructs [3], and limitations in the accuracy and reproducibility of intraoperative rod bending have also been reported [4].
Figure 1.
Schematic illustration of intraoperative rod contouring during spinal correction surgery and possible surface damage introduced by manual bending.
To address these issues, the use of patient-specific rods based on preoperative planning has attracted considerable attention. Patient-specific rods can reduce intraoperative manual bending and may contribute to achieving and maintaining the target spinal alignment, and to reducing postoperative complications associated with mechanical problems [5,6]. In addition, four-dimensional anatomical reconstruction using pre-bent rods has been reported to be effective for thoracic adolescent idiopathic scoliosis [7]. Therefore, fabricating rods with high geometric fidelity based on preoperative design and reducing intraoperative bending are considered effective strategies for improving the reliability of spinal correction implants.
Material selection is also an important factor governing the mechanical performance of spinal correction rods. Comparative studies of conventional Co–Cr rods and Ti rods in adult spinal deformity surgery have shown that Co–Cr rods can provide advantages in mechanical stability, although their association with complications such as proximal junctional kyphosis has also been discussed [8,9]. Ti–6Al–4V alloys exhibit excellent biocompatibility; however, springback may complicate shape retention after rod bending [10,11]. Thus, the elastic modulus, strength, ductility, fatigue properties, and geometric design of the rod must be comprehensively considered for spinal correction applications.
Metal additive manufacturing is a fabrication method capable of directly producing complex and patient-specific geometries that are difficult to obtain by conventional processing, and its application to orthopedic implants is rapidly expanding [12,13,14]. Electron beam powder bed fusion (PBF-EB) has been applied to biomedical metallic materials such as Ti–6Al–4V and Co–Cr–Mo alloys [14,15]. Because PBF-EB enables the integrated fabrication of complex shapes, it is suitable not only for producing curved rods but also for introducing geometry-based mechanical functions, such as variable-diameter designs in which the middle-curved region is locally thickened to tailor flexural stiffness. Previous biomechanical testing of spinal constructs has shown that increasing rod diameter increases construct stiffness and load-carrying capacity [16]. Independent mechanical studies of spinal rods have further shown that rod-scale stiffness and correctional force are governed jointly by material, diameter, and contouring history. In particular, CoCr rods generally exhibit higher bending stiffness than Ti rods of comparable diameter, while manual contouring can reduce rod yield strength and bending stiffness [17,18,19]. These findings provide a mechanical rationale for combining material processing with local geometric design in the present PBF-EB rods.
Finite element analysis (FEA) has been used to identify stress-concentration regions, evaluate load-transfer paths, and optimize the geometry of spinal implants and rod–screw systems [20,21,22]. In addition, because the spine is subjected to large loads during daily activities, the static mechanical response of spinal rods and their durability under cyclic loading must be evaluated [23,24,25]. In metallic implants, the surface condition, internal defects, bending stress, and stress concentration are known to affect fatigue behavior [26,27,28,29,30,31,32,33].
The Co–28Cr–6Mo–0.11N alloy used in this study is a Co–Cr–Mo–N alloy whose microstructure and mechanical properties can be controlled by nitrogen addition and reverse transformation heat treatment. In Co–Cr–Mo–N alloys, grain refinement through reverse transformation based on the ε-to-γ phase transformation has been reported to achieve a balance between high strength and ductility [34,35,36,37]. In particular, repeated reverse transformation heat treatment of PBF-EB-fabricated Co–28Cr–6Mo–0.11N alloys has been shown to refine grains and improve mechanical properties [34,36].
Previous studies have therefore established three relevant bodies of knowledge: patient-specific or pre-bent spinal rods can reduce the need for intraoperative contouring [5,6,7]; rod-scale mechanical response depends strongly on material, diameter, and contouring history [16,17,18,19,38]; and reverse transformation treatment can modify the microstructure and tensile properties of PBF-EB-fabricated Co–Cr–Mo–N alloys [34,36,37]. The resulting engineering challenge is to determine how post-build material-state control and local cross-sectional design can be integrated within a directly fabricated curved CCMN rod, and how each contributes to the rod-scale mechanical response. Addressing this gap requires evaluation of the rod as a structural component rather than inference of rod behavior solely from coupon-level material properties.
In this study, CCMN alloy spinal correction rods with a prescribed spinal contour were fabricated by PBF-EB, and the effects of the number of reverse transformation heat-treatment cycles, the diameter of the middle region of the rod, and the material type on compressive deformation behavior were quantitatively evaluated. In addition, the deformation distribution of the curved rod and the effect of the variable-diameter design on deformation were examined by FEA. Furthermore, SEM observations of the fracture surface and cyclic compression testing at 0–300 N were performed for the 3RT-treated CCMN rod to evaluate the rod-scale mechanical response relevant to spinal correction applications.
2. Materials and Methods
2.1. Powders and Rod Materials
Gas-atomized powders with nominal compositions of Co–28Cr–6Mo–0.11N and Ti–6Al–4V were used in this study. Table 1 shows the chemical compositions of the powders. The CCMN alloy rods were used as the primary specimens, and Ti–6Al–4V alloy rods were used as comparison specimens.
Table 1.
Chemical compositions of the CCMN and Ti–6Al–4V powders (mass%).
2.2. Fabrication of Spinal Correction Rods with a Prescribed Spinal Contour by PBF-EB
Using the CCMN alloy powder, spinal correction rods with the prescribed contour shown in Figure 2 were fabricated by PBF-EB. An EBM system (Arcam A2X) was used for fabrication. The rods were designed with a curved geometry for spinal correction implants, and both ends were shaped to be fixed in dedicated fixtures. Ti–6Al–4V alloy rods with the same basic design were also fabricated for comparison. The appearances of the fabricated CCMN and Ti–6Al–4V alloy rods are shown in Figure 3.
Figure 2.
Geometric design of the spinal correction rod with a prescribed spinal contour. The cross marks (+) denote geometric reference points in the design drawing.
Figure 3.
Appearances of PBF-EB-fabricated spinal correction rods and diameter measurement. (a) As-built CCMN rod, (b) reverse-transformation-treated CCMN rod, (c) as-built Ti–6Al–4V rod, and (d) diameter measurement in the middle region of the rod.
The AsB, RT, 2RT, and 3RT rods were fabricated using the same CAD geometry. Following PBF-EB fabrication, shot peening was performed to remove loosely attached powder particles from the rod surfaces. Surface irregularities remained after shot peening, and the rod diameters were adjusted during polishing using the same dimensional criteria for all specimens. The diameter was approximately 5.5 mm over most of the rod length and increased to approximately 5.7 mm near the middle-curved region. Thus, the reported diameter range of 5.5–5.7 mm primarily represents the local diameter distribution along individual rods rather than systematic dimensional differences among the heat-treatment conditions.
In addition to rods with a nominal diameter of 5.5 mm, variable-diameter rods were fabricated for comparison. For the diameter-effect experiments described in Section 3.3, CCMN rods with maximum middle-region diameters of approximately 7 and 8 mm were evaluated. Figure 4 shows representative surface-polished Ti–6Al–4V rods with the corresponding variable-diameter geometries. In this design, the diameter at both ends was approximately 5.5 mm, whereas the maximum diameter in the middle region was increased to approximately 7 or 8 mm. The diameter decreased smoothly from the middle region toward both ends.
Figure 4.
PBF-EB-fabricated and surface-polished Ti–6Al–4V rods with a prescribed spinal contour. The maximum diameters in the middle region were approximately (a) 7 mm and (b) 8 mm, and the diameter gradually decreased to 5.5 mm at both ends.
2.3. Reverse Transformation Heat Treatment
The reverse transformation heat treatment of the PBF-EB-fabricated CCMN rods was performed using the dedicated heat-treatment fixture shown in Figure 5a to suppress rod deformation during heating. The heat-treatment schedule shown in Figure 5b consisted of aging at 1073 K for 43.2 ks, followed by reverse transformation treatment at 1273 K for 0.6 ks. This heat-treatment cycle was repeated once, twice, or three times, and the resulting specimens are referred to as RT, 2RT, and 3RT, respectively. The heat-treatment conditions were selected based on previous studies on grain refinement and mechanical-property improvement in Co–Cr–Mo–N alloys [34,36,37].
Figure 5.
Dedicated fixture for reverse transformation heat treatment and heat-treatment schedule: (a) the heat-treatment fixture and (b) the aging and reverse transformation cycle.
2.4. Compression and Cyclic Compression Tests
To evaluate the static compression and cyclic compression responses of the spinal correction rods, the dedicated fixture shown in Figure 6 was prepared. The rods were inserted into the upper and lower fixtures at the prescribed rod angles and were fixed with screws. The upper and lower fixtures were aligned with the loading axis, and compressive loading was applied vertically.
Figure 6.
Fixture used for static compression and cyclic compression testing.
Compression and cyclic compression tests were performed using an Instron 8801 testing machine. The test conditions are summarized in Table 2. In the compression tests, the maximum load was set to 1000 N, the maximum displacement was limited to 10 mm, and the load–displacement response within the prescribed displacement range was evaluated. The loads required to achieve displacements of 5 and 10 mm were also measured. The presence or absence of macroscopic residual deformation after unloading was examined by measuring the distance between gauge marks placed on both sides of the rod before and after testing.
Table 2.
Test conditions for mechanical property evaluation.
Figure 7 shows the rod before and after compression deformation at a maximum load of Pmax = 1000 N and a maximum displacement of Smax = 10 mm. In the cyclic compression test, a load range of 0–300 N was selected as a lower-load screening condition with reference to published biomechanical spinal loading data [24,25] and prior fatigue testing of contoured CoCr spinal constructs [39]. The test frequency was 1 Hz, and the total number of cycles was 1 × 106. After testing, the rods were examined for fracture and macroscopic residual deformation. This loading condition was intended as a proof-of-concept screening test and was not assumed to reproduce the complete in vivo rod–screw boundary condition. For fractographic evaluation, an additional 3RT-treated CCMN rod was compressed beyond the standard evaluation range until fracture, and the fracture surface was subsequently examined by SEM.
Figure 7.
Rod before and after compression deformation. Maximum load Pmax = 1000 N and maximum displacement Smax = 10 mm.
2.5. Finite Element Analysis
Finite element analysis (FEA) was performed with Abaqus/Standard 2020 to compare three curved CCMN rod geometries under identical idealized compressive loading conditions. The rod centerline was reconstructed from the original STL outline using 11 control points in the XY plane. All three models shared this centerline and the same end locations. Model D5.5 had a uniform circular diameter of 5.5 mm, whereas models D7 and D8 were progressively thickened toward the middle-curved region, reaching maximum diameters of 7 and 8 mm, respectively, and returning smoothly to 5.5 mm at the two ends. The material was assumed to be isotropic and linearly elastic (Young’s modulus, 210 GPa; Poisson’s ratio, 0.30). The models were discretized using eight-node, reduced-integration hexahedral elements (C3D8R) with a nominal mesh size of 0.50 mm. One end face was fully fixed. A reference point at the center of the opposite end face was kinematically coupled to that face and subjected to a compressive force of 300 N in the negative local y-direction; translations of the reference point in the local x and z directions were constrained. The loading fixtures, rod–fixture contact, and friction were not modeled explicitly; their effects were approximated through these idealized end constraints. The displacement field was evaluated using the displacement magnitude U, defined as [40]:
where ux, uy, and uz are the displacement components along the coordinate directions. In addition to displacement magnitude, the von Mises equivalent-stress field was examined. Global peak stresses and peak stresses within a designated middle-curved region near the centerline crest were evaluated separately. To assess mesh sensitivity, the D5.5 model was analyzed with nominal element sizes of 0.65, 0.50, and 0.35 mm under otherwise identical conditions; the middle-curved region was defined using three adjacent element sets. Mesh dependence was examined through changes in maximum displacement and curved-region maximum von Mises stress. The idealized loading and constraints are illustrated in Supplementary Figure S1; mesh-sensitivity contour plots are given in Supplementary Figure S2.
2.6. Fracture-Surface Observation by SEM
The fracture surface of the additional 3RT-treated CCMN rod described in Section 2.4 was examined by SEM. SEM imaging was performed at an accelerating voltage of 15 kV. The fracture-surface morphology and fracture mode were evaluated with reference to the nominal compressive and tensile sides of the curved rod.
3. Results and Discussion
3.1. Previous Findings on Reverse Transformation Heat Treatment
In this study, reverse transformation heat treatment was applied to the PBF-EB-fabricated CCMN rods, and their compressive deformation behavior was evaluated. The microstructural changes and basic tensile properties caused by the reverse transformation heat treatment have been reported previously [34]. In that previous study, EBSD observations and tensile tests were performed for as-built (AsB), solution-treated (ST), aged (AT), reverse-transformation-treated (RT), and three-cycle reverse-transformation-treated (3RT) PBF-EB-fabricated CCMN alloys, and grain refinement induced by reverse transformation heat treatment was demonstrated. For reference, the EBSD microstructures reported in Ref. [34] are shown in Figure 8.
Figure 8.
EBSD microstructures of PBF-EB-fabricated CCMN alloy specimens in the AsB, ST, AT, RT, and 3RT conditions, reproduced from Ref. [34]. The 3CT condition in the original figure corresponds to the 3RT condition used in the present study (Reprinted from Ref. [34], licensed under CC BY 4.0).
According to Ref. [34], the average grain sizes were 81, 92, 72, 30, and 19 µm for the AsB, ST, AT, RT, and 3RT specimens, respectively. Thus, the average grain size of the 3RT specimen decreased by approximately 77% relative to that of the AsB specimen. The 3RT specimen also exhibited a tensile strength of 1234 MPa and an elongation of 45%, demonstrating a combination of high strength and substantial ductility [34]. The improved balance between strength and ductility following reverse transformation heat treatment is considered to arise from ε ↔ γ phase transformation control and precipitation control in the Co–Cr–Mo–N alloy [34,36,37]. The engineering stress–strain curves reported in the same previous study are shown in Figure 9.
Figure 9.
Engineering stress–strain curves of PBF-EB-fabricated CCMN alloy specimens in the AsB, ST, AT, RT, and 3RT conditions, reproduced from Ref. [34]. The 3CT condition in the original figure corresponds to the 3RT condition used in the present study (Reprinted from Ref. [34], licensed under CC BY 4.0).
The previously reported tensile results indicate that the effect of repeated reverse transformation should be understood as coupled microstructural control rather than grain refinement alone. In Ref. [34], the three-cycle condition is denoted as 3CT; this corresponds to the 3RT condition used in the present manuscript. That condition exhibited a refined average grain size of 19 µm with a yield strength of 655 MPa, a tensile strength of 1234 MPa, and an elongation of 45%. The same study further showed that the γ/ε phase constitution affects the yield response, with a mixed γ + ε state providing a higher yield strength than that of a single γ state [34]. Together with the precipitation-control mechanism reported for this alloy system [36,37], these observations indicate that grain size, phase constitution, and precipitate state jointly govern the strength–ductility balance. This is relevant to a pre-curved rod because axial compression generates bending; thus, sufficient resistance to deformation must coexist with ductility to accommodate tensile and compressive strains across the rod section.
On the basis of these previous findings, the present study examined whether the microstructural and strength changes produced by repeated reverse transformation treatment were accompanied by changes in the rod-scale compressive load–displacement response.
From a material-selection perspective, the significance of repeated reverse transformation treatment is not limited to increasing strength. Ti–6Al–4V is widely used for spinal fixation because it combines useful ductility with a comparatively compliant mechanical response, although its lower rod-scale bending stiffness and springback can make shape retention more difficult than for CoCr-based rods [10,11,17,18,19]. In contrast, the reverse-transformation-treated CCMN alloy retains substantial tensile ductility while achieving a high-strength material state [34,36,37]. This strength–ductility balance is relevant to a pre-curved spinal rod, because resistance to structural deformation must be combined with sufficient ductility to accommodate bending-induced strain without promoting brittle failure.
3.2. Effect of Reverse Transformation Cycles on Compressive Deformation
Figure 10 shows the displacement of CCMN rods under a compressive load of 1000 N. For the AsB, RT, 2RT, and 3RT rods, the displacements under 1000 N were less than 10 mm, and no apparent macroscopic residual deformation was detected after unloading, as evaluated from the distance between gauge marks.
Figure 10.
Effect of the number of reverse transformation heat-treatment cycles on the displacement under a compressive load of 1000 N.
These observations suggest that the overall deformation was predominantly recoverable under the present loading conditions. However, the unloading load–displacement data are not available, and the unloading stiffness and hysteresis behavior therefore cannot be evaluated. Furthermore, the nonlinear load–displacement response of a curved rod may involve geometric nonlinearity, fixture constraints, and possible local plastic deformation. Consequently, the observed macroscopic recovery does not establish that the entire rod remained within the linear elastic regime, and the onset of local yielding cannot be determined from the present measurements.
The displacement of the AsB rod under a compressive load of 1000 N was 7.22 mm. The displacement decreased with increasing number of reverse transformation cycles, with the 3RT rod exhibiting the smallest displacement. These results indicate a systematic change in the apparent rod-scale deformation resistance associated with the heat-treatment condition.
Repeated reverse transformation treatment has previously been shown to refine the grain structure through ε ↔ γ phase transformation and associated microstructural control, resulting in improved tensile properties of PBF-EB-fabricated CCMN alloys [34,36,37]. These microstructural changes may enhance resistance to the onset of local plastic deformation during rod bending. However, improved tensile strength does not necessarily indicate increased elastic bending stiffness.
For predominantly recoverable bending deformation, the rod-scale load–displacement response is governed primarily by Young’s modulus, cross-sectional geometry, and boundary conditions. Lam et al. [41] reported a relatively small increase in Young’s modulus, from 191 to 198 GPa, after heat treatment of additively manufactured CoCrMo alloys. Nevertheless, these results cannot be directly applied to the present PBF-EB-fabricated and reverse-transformation-treated rods.
All rods subjected to different reverse transformation heat-treatment conditions were fabricated using the same CAD geometry and adjusted to the same nominal dimensional profile during polishing. The diameter range of approximately 5.5–5.7 mm primarily reflects local dimensional variations along the length of each rod. For a circular cross-section, the second moment of area is proportional to the fourth power of diameter, and the difference between 5.5 and 5.7 mm corresponds to an approximately 15.4% difference in local flexural rigidity at a constant Young’s modulus. However, this variation occurs primarily along individual rods and should not be directly interpreted as a difference between heat-treatment conditions. Although the same dimensional criteria were applied during polishing, small specimen-specific geometric deviations cannot be excluded because the exact post-processing dimensions of all tested specimens could not be independently verified. Therefore, the observed increase in apparent deformation resistance may involve contributions from material-state changes and possible geometric variations, whose individual contributions cannot be quantitatively separated from the available data.
Although heat-treatment-induced residual-stress relaxation may influence the onset of local yielding and the subsequent nonlinear deformation response, residual stress alone does not directly increase the intrinsic elastic modulus. Because Young’s modulus, specimen-specific geometry, and residual stresses were not independently quantified for each heat-treatment condition, their relative contributions cannot be determined from the present results. Therefore, the higher apparent deformation resistance of the 3RT-treated rods should be interpreted as an observed rod-scale response associated with the heat-treatment condition, rather than being attributed solely to grain refinement, elastic-modulus changes, or residual-stress relaxation.
Figure 11 shows the load required to produce a fixed displacement of 5 mm. The loads for the AsB, RT, 2RT, and 3RT rods were 812, 843, 865, and 896 N, respectively. The 3RT rod required a load that was 84 N higher than that required for the AsB rod, corresponding to an increase of approximately 10% in the apparent structural resistance to deformation. Together with the displacement results under 1000 N, these data demonstrate a systematic change in rod-scale load–displacement response with repeated reverse transformation treatment, while the specific contributions of elastic modulus, phase constitution, residual stress, and other heat-treatment-induced changes remain to be clarified. For the subsequent fracture-surface and cyclic-compression evaluations, the 3RT condition was selected because it exhibited the highest apparent deformation resistance among the heat-treatment conditions examined in the present rod tests, while previous work on the same alloy demonstrated a favorable strength–ductility balance after repeated reverse transformation treatment [34].
Figure 11.
Effect of the number of reverse transformation heat-treatment cycles on the load required to produce a displacement of 5 mm.
3.3. Effect of Middle-Region Diameter on Compressive Deformation
Figure 12 shows the compressive load–displacement curves of AsB CCMN rods with different middle-region diameters and a Ti–6Al–4V comparison rod. For the CCMN rods, the displacement of the rod with a maximum middle-region diameter of 8 mm was 2.7 mm under 1000 N. In contrast, the rod with a maximum middle-region diameter of 7 mm exhibited a displacement of 3.3 mm under 1000 N. Thus, increasing the middle-region diameter from 7 to 8 mm reduced the displacement under 1000 N by 0.6 mm, corresponding to an approximately 18% reduction in deformation.
Figure 12.
Compressive load–displacement curves of CCMN rods with different middle-region diameters and a Ti–6Al–4V comparison rod. The horizontal dashed line indicates the 1000 N load level.
For a circular cross-section, the second moment of area I is given by [42]
and the corresponding local flexural rigidity Db can therefore be expressed as
where E is Young’s modulus and d is the local rod diameter. Assuming the same elastic modulus for the 7 and 8 mm CCMN rods, the ratio of local flexural rigidities is
Thus, an approximately 14% increase in diameter theoretically produces an approximately 71% increase in local flexural rigidity. Experimentally, however, the whole-rod displacement under 1000 N decreased by approximately 18%, from 3.3 to 2.7 mm. The substantially smaller change in global deformation than the change in local flexural rigidity is mechanically reasonable because only the middle region was thickened, while the overall response also depends on the prescribed initial curvature, the unchanged end regions, fixture constraints, and the geometrically nonlinear deformation path of the entire rod. Consistent with this mechanical expectation, previous spinal-rod studies have shown increased stiffness and load-carrying capacity with increasing rod diameter [16], higher bending stiffness of CoCr than Ti rods at comparable diameters [17,18,19], and measurable variation in bending response even among rods with the same nominal diameter [38]. The present results therefore support variable-diameter design as an effective means of reducing deformation while retaining smaller end diameters for fixation.
The variable-diameter geometry can therefore be interpreted as local flexural-stiffness tailoring rather than simply as an increase in rod size. Monolithic spinal rods with spatially variable flexural stiffness have previously been proposed as a means of controlling the mechanical response of spinal instrumentation without introducing joints or multiple structural components [43]. In the present PBF-EB design, stiffness tailoring is achieved geometrically through a continuous change in cross-sectional diameter within a single rod. Because EI depends strongly on diameter, local thickening can alter the deformation distribution of the curved segment while retaining smaller end diameters for fixation. This design freedom is a specific structural advantage of additive manufacturing and is consistent with the displacement reduction observed experimentally and by FEA. Importantly, increasing rod stiffness should not be regarded as an unconditional design objective. Clinical studies have indicated that the high rigidity of CoCr-based constructs may be associated with proximal junctional complications [8,9]. The advantage of the present PBF-EB approach is therefore that the mechanically critical curved region can be selectively stiffened while maintaining smaller diameters elsewhere, rather than uniformly increasing the stiffness of the entire rod [43].
The Ti–6Al–4V rod with a diameter of 5.5 mm reached a displacement of 5 mm at a load of approximately 400 N. The Ti–6Al–4V rod exhibited greater deformation at lower loads than the CCMN rods. This result is consistent with previous reports that springback and shape retention can be problematic for Ti–6Al–4V spinal rods [10,11]. However, this comparison includes differences in both material and rod diameter. Therefore, additional tests using rods with matching geometries and diameters would be required to strictly isolate the intrinsic material effect. In addition, manual rod contouring has been reported to reduce yield strength and bending stiffness, with the magnitude of the change depending on rod material, diameter, and bend angle [17]. Conversely, notch-free pre-bent CoCr rods have exhibited higher ultimate load and cyclic bending performance than conventionally notched curved rods [18]. Thus, direct fabrication of the target curvature offers a mechanical advantage by avoiding the introduction of an additional contouring-related variable before testing.
3.4. Repeatability of Compression Behavior of 3RT-Treated CCMN Rods
Figure 13 shows the compressive load–displacement curves of multiple 3RT-treated CCMN rods. The curves for specimens a, b, c, and d showed relatively small scatter, indicating good repeatability under the present test configuration. At a displacement of 10 mm, the CCMN rods supported a load of approximately 950–1000 N.
Figure 13.
Comparison of compressive load–displacement curves for four 3RT-treated CCMN rods (specimens a–d) and a Ti–6Al–4V rod.
In contrast, the Ti–6Al–4V rod supported approximately 700 N at a displacement of 10 mm, whereas the 3RT-treated CCMN rods supported approximately 950–1000 N. Figure 13 therefore provides a comparison of the compressive responses of CCMN and Ti–6Al–4V rods with similar nominal diameters. The CCMN rods had a nominal diameter of approximately 5.5 mm over most of their length, with a local increase to approximately 5.7 mm near the middle-curved region, while the Ti–6Al–4V comparison rod had a nominal diameter of 5.5 mm.
Although the nominal diameters were comparable, the exact local diameter profiles were not verified to be identical. Furthermore, the CCMN rods were subjected to three reverse transformation heat-treatment cycles, whereas the Ti–6Al–4V rod was evaluated in the as-built condition. Therefore, the observed difference represents the combined effects of material state and possible geometric variations on the rod-scale compressive response. A comparison using specimens with precisely matched geometries and controlled material conditions would be required to isolate the intrinsic material contribution.
3.5. FEA of Deformation and Variable-Diameter Geometry
Figure 14 presents displacement-magnitude and von Mises equivalent-stress distributions for the D5.5, D7, and D8 models under a 300 N compressive load. The predicted global maximum displacements were 2.432, 1.405, and 1.026 mm, respectively. Relative to the uniform-diameter D5.5 model, the maximum displacement decreased by 42.2% in D7 and 57.8% in D8. The global maximum von Mises stress occurred near the constrained end, whereas the effect of local thickening was assessed separately within the middle-curved region.
Figure 14.
Finite element analysis of spinal correction rods with different diameter distributions under a compressive load of 300 N. (a–c) Uniform-diameter rod (D5.5, Ø5.5 mm); (d–f) variable-diameter rod with a maximum diameter of 7 mm in the middle-curved region (D7); and (g–i) variable-diameter rod with a maximum diameter of 8 mm in the middle-curved region (D8). The left column (a,d,g) shows displacement-magnitude distributions, the middle column (b,e,h) shows von Mises equivalent-stress distributions, and the right column (c,f,i) shows enlarged stress distributions in the middle-curved region. The orange dashed boxes indicate the locations of the enlarged regions. The maximum local von Mises stresses within the middle-curved region were 277.906, 164.387, and 123.952 MPa for D5.5, D7, and D8, respectively. Separate color scales are used for global and enlarged stress distributions.
Within the designated middle-curved region, the maximum von Mises stresses were 277.906 MPa for D5.5, 164.387 MPa for D7, and 123.952 MPa for D8. Relative to D5.5, the regional peak stress decreased by 40.8% in D7 and 55.4% in D8. The enlarged views in Figure 14c,f,i illustrate this stress attenuation. These regional stress values are more directly relevant to the locally thickened geometry than the global peak stress, which is influenced by the idealized end constraints.
Mesh sensitivity was evaluated separately for the D5.5 model using nominal element sizes of 0.65, 0.50, and 0.35 mm. Upon refinement from 0.50 to 0.35 mm, the global maximum displacement changed by 1.19%, and the maximum von Mises stress within the designated middle-curved region changed by 1.89%. The global peak stress changed by 2.55%, indicating greater sensitivity near the constrained end; complete mesh convergence of that peak was not established. These results support relative comparisons of displacement and curved-region stress using the nominal 0.50 mm mesh within the tested range. The geometry-comparison and mesh-sensitivity series were analyzed separately, and their absolute peak-stress values were not assumed to be identical. Supplementary Figure S2 shows the stress and displacement distributions for the mesh-sensitivity series. In compression experiments, the displacement under 1000 N decreased from 3.3 to 2.7 mm when the maximum middle-region diameter increased from 7 to 8 mm (Section 3.3). The experiments and FEA therefore show a qualitatively consistent reduction in deformation with local thickening. Their displacement values should not be compared quantitatively because the loads (1000 and 300 N, respectively) and boundary representations differ. The linearly elastic FEA was not intended to predict fatigue life or fracture initiation.
Figure 15 summarizes the geometrical relationship between axial shortening of the rod and lateral motion of the curved segment during compression. In this evaluation, a denotes the distance between the loading points, and b denotes the lateral offset of the curved region from the loading axis. When a decreased from 150 to 125 mm, b increased from 25 to 85 mm, corresponding to a 60 mm increase in lateral offset. For the initial configuration (a = 150 mm and b = 25 mm), the diagonal length c was 152.07 mm. This geometrical relation shows that axial shortening of a pre-curved rod is accompanied by substantial lateral motion of the curved segment. Because b is a geometrical measure rather than a directly measured stress position or local-curvature maximum, Figure 15 is used only to describe the deformation path of the curved rod. Accordingly, local diameter design should consider both the initial contour and the deformation path under compression. The observed coupling between axial shortening and lateral offset is consistent with large-displacement curved-beam mechanics, in which axial loading of an initially curved member produces coupled bending and lateral motion [44].
Figure 15.
Geometrical relationship between the distance between loading points, a, and the lateral offset of the curved region, b, during compression. The diagonal segment c in the schematic is the hypotenuse of the right triangle defined by a and b; its initial length is 152.07 mm for a = 150 mm and b = 25 mm. The solid red arrows indicate axial compression, and the outlined red arrows indicate the direction of increasing lateral offset.
3.6. Fracture-Surface Morphology and Fracture Behavior
Figure 16 shows a schematic representation of the bending stress state of the compression-tested rod together with SEM images of the 3RT-treated CCMN rod’s fracture surface after compression testing. Fracture occurred near the middle of the curved region. This location is consistent with a mechanically critical region of the curved rod under compression, where bending generates tensile and compressive stresses on opposite sides of the rod. Under the classical circular-beam approximation, the magnitude of the nominal surface bending stress, σb, can be expressed as [42]
where M is the local bending moment and c = d/2. Equation (5) shows that, for a given bending moment, the nominal surface bending stress scales with the inverse cube of diameter; therefore, local thickening strongly reduces the nominal bending-stress magnitude. The present rod, however, is initially curved and undergoes substantial geometrical deformation, so Equation (5) is used only to illustrate the diameter dependence of nominal bending stress and not to estimate the actual local fracture-initiation stress. A crack was observed in the central region of the fracture surface. This nominal tensile/compressive stress separation is consistent with prior analyses of contoured spinal rods, in which bending and contouring-induced residual stresses produce different local mechanical states on opposite sides of the rod [45].
Figure 16.
Fracture behavior of the 3RT-treated CCMN rod after compression testing: (a) schematic illustration of the bending stress state, (b) overall fracture surface, and (c,d) magnified SEM images of representative fracture regions.
When the fracture surface was examined by distinguishing the nominal compressive side from the nominal tensile side of the bent rod, the observed morphology was consistent with crack initiation and propagation from the tensile side followed by final fracture across the section. The outer side of the curved region showed fracture features along grain boundaries, whereas some regions also exhibited fracture features associated with plastic deformation. Because the present analysis is based on post-fracture morphology and a schematic bending-stress interpretation rather than a direct local stress measurement, the exact crack-initiation site should be regarded as a proposed interpretation rather than a definitively identified origin.
In Co–Cr–Mo and Ti–6Al–4V alloys, surface condition, processing history, residual stress, and microstructure have been reported to influence crack initiation and fracture-surface morphology [26,27,28,29,30,31,32,33,46,47]. The fracture surface observed in this study suggests crack initiation on the tensile side of the curved rod followed by directional fracture propagation. The fracture location and the region of relatively large displacement in the FEA model both occur in the middle-curved portion of the rod; however, displacement magnitude alone does not establish the local stress or strain that drove fracture. Further investigation using stress/strain-resolved analysis and direct defect characterization is required to clarify whether fracture initiation is governed by local bending stress, surface roughness, PBF-EB-derived internal defects, grain boundaries, or contact with the testing fixture. For additively manufactured Co–Cr–Mo specifically, notch geometry, internal defects, heat treatment, and shot peening have all been shown to alter fatigue response and fracture-surface characteristics [46,47]. These reports support interpreting the observed mixed fracture morphology as the result of multiple interacting microstructural and surface-related factors rather than a single unique fracture mechanism.
3.7. Cyclic Compression Behavior
Figure 17 shows the cyclic compression test results of the 3RT-treated CCMN rod. A compressive load of 0–300 N was applied at 1 Hz up to 1 × 106 cycles. Previous biomechanical studies have shown that spinal instrumentation is subjected to substantial cyclic loading [24,25]. In a posterior spinal construct study, contoured CoCr rods were tested under dynamic axial compression–bending at maximum loads of 250, 400, and 700 N, with runout defined at 2 × 106 cycles [39]. The present 300 N condition therefore represents a lower-load screening condition rather than a test to determine the fatigue limit of the rod. Related studies further show that fatigue performance of contoured spinal rods and additively manufactured Co–Cr–Mo is sensitive to contouring-induced residual stress, notch geometry, internal defects, heat treatment, and surface condition [45,46,47].
Figure 17.
Cyclic compression behavior of the 3RT-treated CCMN rod: (a) force–machine position curves at selected cycle numbers and (b) variation in compressive force with cycle number.
As shown in Figure 17a, the recorded machine position during cyclic loading remained within approximately 44.9–45.6 mm, corresponding to a positional excursion of about 0.7 mm over the plotted cycles. The close overlap of the force–position traces indicates that no large progressive change in the global cyclic response occurred during the test. Because the horizontal axis represents machine position rather than a directly measured local rod strain, these data should not be interpreted as a local strain or material fatigue parameter.
Figure 17b shows the variation in force with cycle number under the 0–300 N loading condition. Fluctuations were observed at high cycle counts. Such fluctuations may arise from changes in fixture contact, test-system compliance, or specimen response; the present measurements do not permit these contributions to be separated. Previous studies have shown that surface condition, microdefects, phase transformation, and heat treatment can influence the fatigue behavior of Co–Cr–Mo alloys [27,30,31,32,33,45,46,47].
Surface roughness is an important factor affecting the fatigue behavior of additively manufactured metallic components. In PBF-EB-fabricated rods, surface irregularities and partially attached powder particles may act as local stress concentrators under cyclic loading, promoting fatigue crack initiation. In the present study, shot peening was applied to remove loosely attached powder particles, although surface irregularities remained after treatment. Shot peening can introduce compressive residual stresses near the surface, potentially suppressing fatigue crack initiation and propagation. However, peening-induced surface indentations may also increase roughness and promote local stress concentration. Polat and Saklakoglu [47] reported that shot peening increased surface roughness while improving fatigue performance and shifting crack initiation farther from the surface in PBF-LB-fabricated Co–Cr–Mo specimens. These findings highlight the competing effects of surface topography and residual stresses on fatigue behavior. Because surface roughness and residual stresses were not quantitatively measured in the present study, their individual contributions to the observed cyclic compression response cannot be determined.
After 1 × 106 cycles, no apparent fracture or macroscopic residual deformation was observed. The 3RT-treated CCMN rod therefore survived the specified 0–300 N cyclic compression condition without macroscopic failure. However, the ability of the rod to withstand higher cyclic loads remains undetermined because cyclic compression tests above 300 N were not performed. Although the rod exhibited resistance to deformation under static compressive loading up to 1000 N, this result cannot be directly extrapolated to its fatigue performance under higher cyclic loads. Therefore, the present result should be interpreted as runout under a single preliminary screening condition rather than as evidence of a fatigue limit. Further cyclic tests at multiple maximum load levels, using geometrically matched specimens and clinically relevant boundary conditions, are required to determine the fatigue durability of the proposed CCMN rods [39]. Because only one specimen was tested at a single load level, statistical variability and the fatigue limit could not be determined.
Standardized evaluation of spinal fixation systems is addressed by ASTM F2193 [48], which covers individual spinal fixation components, and ASTM F1717 [49], which provides test methods for complete spinal implant constructs using a vertebrectomy model. In contrast, the present study employed a dedicated fixture to evaluate the mechanical response of individual curved rods without incorporating pedicle screws or a vertebrectomy model. Therefore, the present tests were intended as preliminary rod-level evaluations rather than standardized assessments of complete spinal fixation constructs. Further testing under standardized conditions would be necessary to evaluate the mechanical performance and fatigue durability of the proposed rods in a clinically relevant fixation configuration.
Although the static compression tests showed smaller deformation of the CCMN rods than the Ti–6Al–4V comparison rod under the tested conditions, this result does not necessarily indicate superior fatigue resistance. The cyclic response depends on the material properties, rod geometry, surface condition, residual stresses, and internal defects. In addition, differences in rod diameter and geometry may affect the local stress and strain distributions under cyclic loading. Therefore, a direct comparison of fatigue performance between CCMN and Ti–6Al–4V rods requires cyclic tests under identical loading conditions using geometrically matched specimens. Further testing at multiple load levels would also be necessary to evaluate their comparative fatigue durability.
3.8. Integrated Mechanical Interpretation
Mechanically, the present observations can be organized into three coupled levels. At the material level, PBF-EB followed by reverse transformation treatment defines the grain size, γ/ε phase constitution, strength–ductility balance, elastic response, and defect/residual-stress state. At the structural level, the prescribed initial curvature and local cross-sectional diameter determine flexural rigidity and the geometrically nonlinear deformation path of the rod. At the damage level, surface condition, internal defects, residual stresses, and local bending stresses influence where cyclic deformation may lead to crack initiation and propagation.
The measured static and cyclic responses therefore emerge from the interaction of material state, geometry, and surface/defect state rather than from any single material property. This coupled interpretation also highlights the relevance of PBF-EB: a monolithic component can be fabricated with a prescribed curved and variable-diameter geometry, while post-build heat treatment provides an independent route for controlling the material state.
Equations (2)–(4) quantify the strong structural sensitivity to local diameter: a modest increase in diameter produces a much larger increase in local flexural rigidity through the fourth-power dependence on d. Equation (5) likewise shows that, for a given bending moment, the nominal surface bending stress magnitude is inversely proportional to the cube of the diameter. When considered together with the FEA displacement magnitude defined in Equation (1), these relations provide a consistent mechanical basis for the observed deformation-suppression effect of local thickening. At the same time, the difference between the approximately 71% increase in local flexural rigidity predicted by Equation (4) and the approximately 18% reduction in whole-rod displacement emphasizes that the global response is governed by the complete curved geometry and boundary conditions rather than by local section properties alone.
4. Conclusions
Spinal correction rods made of CCMN alloy were fabricated by electron beam powder bed fusion (PBF-EB) according to a prescribed spinal contour. Their mechanical behavior was investigated through static and cyclic compression tests, finite element analysis (FEA), and scanning electron microscopy (SEM) of the fracture surfaces. Ti–6Al–4V rods were also evaluated for comparison. The main findings are summarized below:
- The PBF-EB process successfully produced rods with the intended curvature directly from the designed geometry. This capability may reduce the manual bending and adjustment required to obtain the desired rod shape during spinal surgery.
- The displacement of the CCMN rods under a load of 1000 N decreased as the number of reverse-transformation treatment cycles increased. At a displacement of 5 mm, the measured loads were 812 N for AsB, 843 N for RT, 865 N for 2RT, and 896 N for 3RT. These results show that the load–displacement response differed among the heat-treatment conditions. Previous studies have reported that reverse-transformation treatment can affect grain size, phase composition, and tensile properties. In the present study, the rods were fabricated from the same CAD data and polished to the same nominal dimensions. Nevertheless, Young’s modulus and residual stress were not measured separately for each condition, and slight dimensional differences among the finished specimens cannot be excluded. It is therefore difficult to determine how much of the observed difference in mechanical response arose from changes in the material state and how much was associated with specimen geometry.
- The FEA results showed a clear effect of the central-section diameter on rod deformation. Under a compressive load of 300 N, the maximum displacement decreased from 2.432 mm for the 5.5 mm rod to 1.405 mm for the 7 mm rod and 1.026 mm for the 8 mm rod. The corresponding maximum von Mises stresses in the central curved section were 277.906, 164.387, and 123.952 MPa. Thus, increasing the local diameter reduced both displacement and stress in the curved region of the numerical model. A similar tendency was found experimentally. At 1000 N, the measured displacement decreased from 3.3 mm for the 7 mm rod to 2.7 mm for the 8 mm rod. The experimental and numerical displacement values were not directly compared because the loading and boundary conditions were different.
- SEM observations showed that fracture occurred near the central curved section of the rod. The fracture-surface features suggested that the crack propagated from the side subjected to nominal tensile stress. However, the observations did not allow the exact crack-initiation site or the local stress at the onset of cracking to be determined.
- One CCMN rod subjected to 3RT treatment was tested under cyclic compression between 0 and 300 N at a frequency of 1 Hz. No visible fracture or macroscopic residual deformation was observed after 1 × 106 cycles. The specimen therefore reached runout under the selected test conditions, although this result alone is insufficient to establish a fatigue limit. Further fatigue tests involving multiple load levels and boundary conditions representative of spinal fixation are needed to assess the long-term mechanical reliability of these rods.
Supplementary Materials
The following supporting information can be downloaded at: https://www.mdpi.com/article/10.3390/alloys5040033/s1, Figure S1. Idealized boundary conditions used in Abaqus/Standard for the D5.5, D7, and D8 rod models. A 300 N compressive load was applied at a reference point kinematically coupled to one end face, with transverse translations restrained; the opposite end face was fully fixed. Fixture solids, rod–fixture contact, and friction were not explicitly modeled. Figure S2. Mesh-sensitivity study for the uniform-diameter D5.5 model under 300 N, with nominal hexahedral element sizes of 0.35, 0.50, and 0.65 mm. Each row displays the full-rod von Mises stress field, a middle-curved-region detail, and the displacement magnitude. The three meshes have consistent field patterns; the global peak stress remains more mesh-sensitive than the displacement and designated curved-region stress. These calculations represent a mesh-sensitivity series evaluated separately from the three-geometry comparison in Figure 14.
Author Contributions
Conceptualization, H.W.; methodology, H.W.; formal analysis, H.W., H.S., and Q.L.; investigation, H.W., H.S., and Q.L.; writing—original draft preparation, H.W.; writing—review and editing, H.W., Q.L., and A.C.; visualization, H.W., and H.S.; resources, Q.L., and A.C.; supervision, A.C. All authors have read and agreed to the published version of the manuscript.
Funding
This research received no external funding.
Data Availability Statement
The original contributions presented in this study are included in the article. Further inquiries can be directed to the corresponding authors.
Acknowledgments
During the preparation of this manuscript, the authors used ChatGPT (OpenAI, GPT-5.6 Sol) for English-language editing and manuscript organization. The authors reviewed and edited the output and take full responsibility for the content of this publication.
Conflicts of Interest
The authors declare no conflicts of interest.
References
- Kim, N.C.; Johnson, E.; DeWald, C.; Lee, N.; Wang, T.Y. Utility of Enabling Technologies in Spinal Deformity Surgery: Optimizing Surgical Planning and Intraoperative Execution to Maximize Patient Outcomes. J. Clin. Med. 2025, 14, 5377. [Google Scholar] [CrossRef] [Scilit]
- Lebovic, J.; Galetta, M.S.; Sardar, Z.M.; Goytan, M.; Daniels, A.H.; Miyanji, F.; Smith, J.S.; Burton, D.C.; Protopsaltis, T.S. Enabling technology in adult spinal deformity. Spine Deform. 2025, 13, 1547–1561. [Google Scholar] [CrossRef] [Scilit]
- Lindsey, C.; Deviren, V.; Xu, Z.; Yeh, R.-F.; Puttlitz, C.M. The Effects of Rod Contouring on Spinal Construct Fatigue Strength. Spine 2006, 31, 1680–1687. [Google Scholar] [CrossRef] [Scilit]
- Fakunle, O.; O’lAughlin, K.; Waldorff, E.; Zhang, C.; Magro, M.; Goodwin, R. How good are we at rod bending?—A review of the literature and a case series of experienced pediatric and adult scoliosis surgeons. J. Spine Surg. 2025, 11, 591–599. [Google Scholar] [CrossRef] [Scilit]
- Picton, B.; Stone, L.E.; Liang, J.; Solomon, S.S.; Brown, N.J.; Luzzi, S.; Osorio, J.A.; Pham, M.H. Patient-specific rods in adult spinal deformity: A systematic review. Spine Deform. 2024, 12, 577–585. [Google Scholar] [CrossRef] [Scilit]
- Faulks, C.R.; Biddau, D.T.; Munday, N.R.; McKenzie, D.P.; Malham, G.M. Patient-specific spinal rods in adult spinal deformity surgery reduce proximal junctional failure: A review of patient outcomes and surgical technique in a prospective observational cohort. J. Spine Surg. 2023, 9, 409–421. [Google Scholar] [CrossRef] [Scilit]
- Fukushima, A.; Ohnishi, T.; Kokabu, T.; Abe, Y.; Tachi, H.; Endo, T.; Ukeba, D.; Iwasaki, N.; Yamada, K.; Sudo, H. Four-dimensional anatomical spinal reconstruction using pre-bent rods in thoracic adolescent idiopathic scoliosis. Sci. Rep. 2025, 15, 378. [Google Scholar] [CrossRef] [Scilit]
- Shega, F.D.; Zhang, H.; Manini, D.R.; Tang, M.; Liu, S. Comparison of Effectiveness between Cobalt Chromium Rods versus Titanium Rods for Treatment of Patients with Spinal Deformity: A Systematic Review and Meta-Analysis. Adv. Orthop. 2020, 2020, 8475910. [Google Scholar] [CrossRef] [Scilit]
- Han, S.; Hyun, S.-J.; Kim, K.-J.; Jahng, T.-A.; Kim, H.-J. Comparative Study Between Cobalt Chrome and Titanium Alloy Rods for Multilevel Spinal Fusion: Proximal Junctional Kyphosis More Frequently Occurred in Patients Having Cobalt Chrome Rods. World Neurosurg. 2017, 103, 404–409. [Google Scholar] [CrossRef] [Scilit]
- Ayers, R.; Hayne, M.; Burger, E. Spine rod straightening as a possible cause for revision. J. Mater. Sci. Mater. Med. 2017, 28, 123. [Google Scholar] [CrossRef] [Scilit]
- Li, Q.; Min, X.; Bai, P.; Wang, W.; Tao, X.; Zhong, G.; Bai, S.; Zhao, J. Microstructure, mechanical properties and springback behaviour of Ti–6Al–4V alloy connection rod for spinal fixation device. Mater. Sci. Eng. C 2019, 94, 811–820. [Google Scholar] [CrossRef] [Scilit]
- Mobarak, M.H.; Abid, A.S.; Munna, M.S.; Dutta, M.; Rimon, M.I.H. Additive manufacturing in biomedical: Applications, challenges, and prospects. Hybrid. Adv. 2025, 10, 100467. [Google Scholar] [CrossRef] [Scilit]
- Joseph, A.; Uthirapathy, V. A Systematic Review of the Contribution of Additive Manufacturing toward Orthopedic Applications. ACS Omega 2024, 9, 44042–44075. [Google Scholar] [CrossRef] [Scilit]
- Joshua, R.J.N.; Raj, S.A.; Sultan, M.T.H.; Łukaszewicz, A.; Józwik, J.; Oksiuta, Z.; Dziedzic, K.; Tofil, A.; Shahar, F.S. Powder Bed Fusion 3D Printing in Precision Manufacturing for Biomedical Applications: A Comprehensive Review. Materials 2024, 17, 769. [Google Scholar] [CrossRef] [Scilit]
- Zhao, Y.; Aoyagi, K.; Yamanaka, K.; Chiba, A. Processing condition dependency of increased layer thickness on surface quality during electron beam powder bed fusion. J. Mater. Res. Technol. 2023, 26, 5264–5279. [Google Scholar] [CrossRef] [Scilit]
- Kovacı, H.; Yetim, A.F.; Çelik, A. Biomechanical analysis of spinal implants with different rod diameters under static and fatigue loads: An experimental study. Biomed. Tech. 2019, 64, 339–346. [Google Scholar] [CrossRef] [Scilit]
- Demura, S.; Murakami, H.; Hayashi, H.; Kato, S.; Yoshioka, K.; Yokogawa, N.; Ishii, T.; Igarashi, T.; Fang, X.; Tsuchiya, H. Influence of Rod Contouring on Rod Strength and Stiffness in Spine Surgery. Orthopedics 2015, 38, e520–e523. [Google Scholar] [CrossRef] [Scilit]
- Yamada, K.; Sudo, H.; Iwasaki, N.; Chiba, A. Mechanical Analysis of Notch-Free Pre-Bent Rods for Spinal Deformity Surgery. Spine 2020, 45, E312–E318. [Google Scholar] [CrossRef] [Scilit]
- Serhan, H.; Mhatre, D.; Newton, P.; Giorgio, P.; Sturm, P. Would CoCr Rods Provide Better Correctional Forces than Stainless Steel or Titanium for Rigid Scoliosis Curves? J. Spinal Disord. Tech. 2013, 26, E70–E74. [Google Scholar] [CrossRef] [Scilit]
- Weriono; Rusli, M.; Sahputra, R.E.; Dahlan, H. Finite element analysis of stress on thoracic and pedicle screw interface with various loading and bone quality. In AIP Conference Proceedings; AIP Publishing: Melville, NY, USA, 2022; Volume 2545, p. 020013. [Google Scholar] [CrossRef] [Scilit]
- Pan, A.; Ding, H.; Wang, J.; Zhang, Z.; Zhang, H.; Liu, Y.; Hai, Y. The application of finite element analysis to determine the optimal UIV of growing-rod treatment in early-onset scoliosis. Front. Bioeng. Biotechnol. 2022, 10, 978554. [Google Scholar] [CrossRef] [Scilit]
- Jayaswal, D.; Kodigudla, M.; Kelkar, A.; Goel, V.; Palepu, V. Validation of a patient-specific finite element analysis framework for identification of growing rod-failure regions in early onset scoliosis patients. Spine Deform. 2024, 12, 941–952. [Google Scholar] [CrossRef] [Scilit]
- Jost, B.; Cripton, P.A.; Lund, T.; Oxland, T.R.; Lippuner, K.; Jaeger, P.; Nolte, L.-P. Compressive strength of interbody cages in the lumbar spine: The effect of cage shape, posterior instrumentation and bone density. Eur. Spine J. 1998, 7, 132–141. [Google Scholar] [CrossRef] [Scilit]
- Dreischarf, M.; Shirazi-Adl, A.; Arjmand, N.; Rohlmann, A.; Schmidt, H. Estimation of loads on human lumbar spine: A review of in vivo and computational model studies. J. Biomech. 2016, 49, 833–845. [Google Scholar] [CrossRef] [Scilit]
- Rohlmann, A.; Pohl, D.; Bender, A.; Graichen, F.; Dymke, J.; Schmidt, H.; Bergmann, G. Activities of Everyday Life with High Spinal Loads. PLoS ONE 2014, 9, e98510. [Google Scholar] [CrossRef] [Scilit]
- Altenberger, I.; Nalla, R.K.; Sano, Y.; Wagner, L.; Ritchie, R.O. On the effect of deep-rolling and laser-peening on the stress-controlled low- and high-cycle fatigue behavior of Ti–6Al–4V at elevated temperatures up to 550 °C. Int. J. Fatigue 2012, 44, 292–302. [Google Scholar] [CrossRef] [Scilit]
- Sharma, A.; Oh, M.C.; Ahn, B. Recent Advances in Very High Cycle Fatigue Behavior of Metals and Alloys—A Review. Metals 2020, 10, 1200. [Google Scholar] [CrossRef] [Scilit]
- Kahlin, M.; Ansell, H.; Moverare, J.J. Fatigue behaviour of additive manufactured Ti–6Al–4V, with as-built surfaces, exposed to variable amplitude loading. Int. J. Fatigue 2017, 103, 353–362. [Google Scholar] [CrossRef] [Scilit]
- Chen, P.; Liu, H.; Niinomi, M.; Horita, Z.; Fujii, H.; Hanawa, T. Fatigue Property and Cytocompatibility of a Biomedical Co–Cr–Mo Alloy Subjected to a High Pressure Torsion and a Subsequent Short Time Annealing. Mater. Trans. 2020, 61, 361–367. [Google Scholar] [CrossRef] [Scilit]
- Khatibi, G.; Lederer, M.; Kotas, A.B.; Frotscher, M.; Krause, A.; Poehlmann, S. High-cycle fatigue behavior of thin-walled CoCr tubes. Int. J. Fatigue 2015, 80, 103–112. [Google Scholar] [CrossRef] [Scilit]
- Kajima, Y.; Takaichi, A.; Nakamoto, T.; Kimura, T.; Yogo, Y.; Ashida, M.; Doi, H.; Nomura, N.; Takahashi, H.; Hanawa, T.; et al. Fatigue strength of Co–Cr–Mo alloy clasps prepared by selective laser melting. J. Mech. Behav. Biomed. Mater. 2016, 59, 446–458. [Google Scholar] [CrossRef] [Scilit]
- Wei, D.; Koizumi, Y.; Takashima, T.; Nagasako, M.; Chiba, A. Fatigue improvement of electron beam melting-fabricated biomedical Co–Cr–Mo alloy by accessible heat treatment. Mater. Res. Lett. 2018, 6, 93–99. [Google Scholar] [CrossRef] [Scilit]
- Mitsunobu, T.; Koizumi, Y.; Lee, B.-S.; Yamanaka, K.; Matsumoto, H.; Li, Y.; Chiba, A. Role of strain-induced martensitic transformation on extrusion and intrusion formation during fatigue deformation of biomedical Co–Cr–Mo–N alloys. Acta Mater. 2014, 81, 377–385. [Google Scholar] [CrossRef] [Scilit]
- Wang, H.; Miyagi, T.; Chiba, A. Effect of Multiple Reverse Transformation Treatments on Grain Refinement and Mechanical Properties of Biomedical Co–Cr–Mo–N Alloys Fabricated by Electron Beam Melting. Materials 2023, 16, 6528. [Google Scholar] [CrossRef] [Scilit]
- Isik, M.; Niinomi, M.; Liu, H.; Cho, K.; Nakai, M.; Horita, Z.; Narushima, T.; Ueda, K. Optimization of Microstructure and Mechanical Properties of Co–Cr–Mo Alloys by High-Pressure Torsion and Subsequent Short Annealing. Mater. Trans. 2016, 57, 1887–1896. [Google Scholar] [CrossRef] [Scilit]
- Wang, H.; Miyagi, T.; Chiba, A. Improved Mechanical Properties of EBM Biomedical Co–28Cr–6Mo–0.11N Alloy by the Dispersed Precipitation Control of ε-HCP Phase Based on ε↔γ Phase Transformation. Metall. Mater. Trans. A 2023, 54, 3733–3741. [Google Scholar] [CrossRef] [Scilit]
- Kurosu, S.; Matsumoto, H.; Chiba, A. Grain refinement of biomedical Co–27Cr–5Mo–0.16N alloy by reverse transformation. Mater. Lett. 2010, 64, 49–52. [Google Scholar] [CrossRef] [Scilit]
- Upasani, V.V.; Kluck, D.G.; Farnsworth, C.L.; Shah, N.U.; Yaszay, B.; Caffrey, J.P.; Newton, P.O. Variation in Mechanical Properties of 5.5 mm Cobalt Chromium and Titanium Spinal Rods Across Suppliers. J. Orthop. Res. 2025, 43, 1493–1500. [Google Scholar] [CrossRef] [Scilit]
- Nguyen, T.Q.; Buckley, J.M.; Ames, C.; Deviren, V. The fatigue life of contoured cobalt chrome posterior spinal fusion rods. Proc. Inst. Mech. Eng. Part H J. Eng. Med. 2011, 225, 194–198. [Google Scholar] [CrossRef] [Scilit]
- Bathe, K.-J. Finite Element Procedures, 2nd ed.; K.J. Bathe: Watertown, MA, USA, 2014. [Google Scholar]
- Lam, T.-N.; Chen, K.-M.; Tsai, C.-H.; Tsai, P.-I.; Wu, M.-H.; Hsu, C.-C.; Jain, J.; Huang, E.-W. Effect of Porosity and Heat Treatment on Mechanical Properties of Additive Manufactured CoCrMo Alloys. Materials 2023, 16, 751. [Google Scholar] [CrossRef] [Scilit]
- Goodno, B.J.; Gere, J.M. Mechanics of Materials, 9th ed.; Cengage Learning: Boston, MA, USA, 2018. [Google Scholar]
- Facchinello, Y.; Brailovski, V.; Petit, Y.; Mac-Thiong, J.-M. Monolithic Superelastic Rods with Variable Flexural Stiffness for Spinal Fusion: Modeling of the Processing–Properties Relationship. Med. Eng. Phys. 2014, 36, 1455–1463. [Google Scholar] [CrossRef] [Scilit]
- González, C.; Llorca, J. Stiffness of a Curved Beam Subjected to Axial Load and Large Displacements. Int. J. Solids Struct. 2005, 42, 1537–1545. [Google Scholar] [CrossRef] [Scilit]
- Piovesan, A.; Berti, F.; Villa, T.; Pennati, G.; La Barbera, L. Computational and Experimental Fatigue Analysis of Contoured Spinal Rods. J. Biomech. Eng. 2019, 141, 044505. [Google Scholar] [CrossRef] [Scilit]
- Razavi, N.; Avanzini, A.; Cornacchia, G.; Giorleo, L.; Berto, F. Effect of Heat Treatment on Fatigue Behavior of As-Built Notched Co-Cr-Mo Parts Produced by Selective Laser Melting. Int. J. Fatigue 2021, 142, 105926. [Google Scholar] [CrossRef] [Scilit]
- Polat, E.; Saklakoglu, I.E. Effect of Shot Peening on Fatigue Behavior and Microstructure of Additively Manufactured Co-Cr-Mo Alloy. Fatigue Fract. Eng. Mater. Struct. 2024, 47, 240–253. [Google Scholar] [CrossRef] [Scilit]
- ASTM F2193-26; Standard Specifications and Test Methods for Components Used in the Surgical Fixation of the Spinal Skeletal System. ASTM International: West Conshohocken, PA, USA, 2026.
- ASTM F1717-21; Standard Test Methods for Spinal Implant Constructs in a Vertebrectomy Model. ASTM International: West Conshohocken, PA, USA, 2021.
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.