Abstract
Pectin, a natural biopolymer, is a cost-effective, biocompatible, non-toxic, abundant, and flexible material, making it suitable for recording high-quality bioelectric signals from the dynamic surface of the human body. In this work, pectin-based flexible bioelectrodes were developed for the non-invasive monitoring of biopotentials. The bioelectrodes are composed of pectin, polyaniline emeraldine salt (PANI-ES), glycerol, and polydimethylsiloxane (PDMS) and therefore abbreviated as PPGP. The PPGP electrodes demonstrated a bulk electrical conductivity of (7.54 ± 0.81) × 10−3 S/cm, a very low impedance of 34 Ω, and a high charge storage capacity of 4.63 ± 2.70 mC/cm2. The surface morphology of the PPGP electrode plays a crucial role in enhancing biopotential signal detection by improving adhesion to skin contours. PPGP electrodes have been successfully used for high-fidelity electromyographic (EMG) bioelectric signal measurements. The developed PPGP bioelectrodes have the potential to advance next-generation human–machine interface (HMI) technologies and wearable healthcare systems, including prosthetic control, rehabilitation monitoring, and assistive communication devices.
1. Introduction
The development of flexible bioelectrodes for wearable bioelectric signal acquisition has gained significant interest in biomedical and healthcare technology [1,2]. Surface electromyography (sEMG) signal monitoring plays a crucial role in healthcare, supporting muscle and nerve health assessment and aiding in the diagnosis of conditions such as muscle weakness, spasms, and nerve damage [3,4]. Traditionally, biomedical electrodes for recording EMG have been manufactured using rigid metallic Ag/AgCl materials, which can cause skin irritation and discomfort for prolonged use [5]. There is a great interest in the development of flexible electrodes for bioelectric signal recording, including flexible electronics [6,7], electronic tattoos [8], and nanostructure-based physiological sensors [9] because these technologies enable seamless skin integration for high-fidelity monitoring [10]. However, previously developed physiological electrodes often relied on expensive materials, complex fabrication processes, and advanced equipment, necessitating a strictly controlled cleanroom environment. For example, earlier reported epidermal electrodes required photolithography and the use of costly gold as the electrode material [11]. Therefore, there is a growing need to develop low-cost physiological electrodes using natural organic biopolymers.
Pectin, a natural biopolymer, offers a cost-effective, biocompatible, non-toxic, and biodegradable alternative, making it ideal for recording high-quality bioelectric signals from the dynamic surface of the human body [12,13]. Owing to these properties, pectin-based bioelectrodes can seamlessly integrate with human tissue, minimizing the risk of adverse reactions and reducing environmental impact. However, despite these advantages, pectin faces several challenges, including poor electrical conductivity and limited flexibility, which hinder its effectiveness in electrophysiological monitoring. Recently, pectin was used in wearable pressure sensors, environmental monitoring, and glucose biosensors for healthcare applications [14,15]. The introduction of pectin nanostructures into flexible and electrophysiological sensors is still in its early stages of development. However, further research and development are required to fully realize the potential of pectin in this field and to systematically investigate its electrical performance for improved physiological sensing.
Pectin, a complex polysaccharide primarily composed of galacturonic acid chains, has low electrical conductivity [16]. Therefore, it cannot be used alone for electrophysiological recording. However, integrating conductive polymers into pectin nanostructures effectively enhances the electrical conductivity and mechanical strength of the resulting composites [17,18]. Such polymeric materials are gaining attention in healthcare applications due to their cost-effectiveness, ease of fabrication, and good electrical conductivity [19,20]. Other conductive nanofillers, including carbon nanotubes, graphene, and metallic nanoparticles, have been explored to minimize motion artifacts and electrical noise, and to enhance the stability and reliability of composite bioelectrode performance [5,21]. Liu et al. [22] developed a recyclable pectin-based conductive hydrogel with high strength, conductivity, and sensitivity, which was developed for wearable strain sensing, ECG monitoring, electronic skin applications, and implantable applications [23]. The low-esterified pectin hydrogels derived from food waste demonstrated high ionic conductivity, good electrochemical stability, and excellent long-term supercapacitor performance, making them promising sustainable electrolytes for energy storage. Kumar et al. [24] developed pectin-based polymer electrolytes incorporating sodium azide (NaN3) using a solution-casting method and investigated their ionic transport properties through electrochemical impedance spectroscopy. The optimized electrolyte from this study composed of 5 wt% NaN3 exhibited a maximum ionic conductivity of 2.3 × 10−3 S cm−1 at room temperature, which was attributed to enhanced charge carrier concentration and mobility. In comparison, the pectin/PANI-ES/glycerol/PDMS (named PPGP bioelectrodes) developed in the present study achieved a conductivity of (7.54 ± 0.81) × 10−3 S/cm, demonstrating the effectiveness of incorporating PANI-ES as a conductive filler for enhancing the electro0chemical properties of pectin-based composites intended for electrophysiological sensing applications.
Here, we report a simple solution-mixing method to fabricate flexible bioelectrodes composed of pectin/PANI-ES/glycerol/PDMS (named PPGP electrodes). The conductivity of the electrodes was systematically investigated using impedance spectroscopy to enhance signal transmission efficiency between biological tissues and electrodes. To demonstrate the applicability of flexible PPGP bioelectrodes for high-quality bioelectric signal monitoring, we successfully utilized them for sEMG signal recording from the human body. Human skin-attachable sensors and electrodes are capable of monitoring various bioelectric signals and hold the potential to drive innovation in essential technologies for future wearable smart textiles, prosthetic hand controllers for amputees, silent speech recognition for patients who have lost their voice due to mouth surgery or throat cancer, and control of home appliances and other electronic devices through next-generation human–machine interface (HMI) technology.
2. Methodology
2.1. Chemical
The experiments utilized several specific chemicals to fabricate flexible bioelectrodes, enabling the recording of bioelectric signals from the dynamic surfaces of the human body. PANI-ES, pectin derived from citrus peel, and glycerol were all obtained from Sigma Aldrich (St. Louis, MO, USA). Additionally, Sylcap 284-S (standard cure) silicone elastomer base along with its curing agent were procured from MicroLubrol (Clifton, NJ, USA). The chemicals were utilized directly as supplied, with no additional purification.
2.2. Synthesis of PPGP Composite
The PPGP composites were synthesized through a simple solution-mixing technique. Initially, 300 mg of pectin was dissolved in 15 mL of deionized (DI) water and stirred at 80 °C until a homogeneous solution was achieved. After cooling the pectin solution to room temperature, it was mixed with the Polyaniline in its Emeraldine Salt (PANI-ES) solution. The PANI-ES solution was prepared by dissolving 1.5 g of PANI-ES in 30 mL of DI water and then blending it with the pectin solution to form a uniform pectin/PANI-ES mixture. Glycerol, as a dispersing agent, was added to the pectin/PANI composite to improve the durability, stretchability, and interfacial adhesion force between the biopolymer composites. The supporting information (SI) [Figure S1] demonstrates the disc electrode and the presence of crevices and inadequate interfacial adhesion between pectin and PANI-ES in the absence of glycerol. Crack formation was observed in the pectin/PANI-ES composite after drying. Finally, the PDMS was incorporated to provide mechanical robustness, biocompatibility, and flexibility, making the bioelectrodes suitable for bioelectric signal monitoring. To prepare the PDMS mixture, 6 g of base was combined with 0.6 g of curing agent in a 10:1 ratio, and the mixture was thoroughly stirred to ensure uniformity and homogeneity. The as-prepared PDMS was incorporated into the pectin/PANI-ES/glycerol composite to formulate the final PPGP composite. The mixture was stirred for 30 min to achieve a homogeneous solution.
2.3. Fabrication of Flexible Bioelectrodes with PPGP Composites
The process flow for the fabrication of flexible bioelectrodes is shown in Figure 1. The chemical structures of the pectin, PANI-ES, glycerol, and PDMS are depicted in Figure 1a. The optimized bioelectrode composition comprised 64 wt% pectin, 9 wt% PANI-ES, 5 wt% glycerol, and 22 wt% PDMS, as it exhibited the highest conductivity among the investigated formulations. A detailed discussion on electrical conductivity investigation is presented in Section 5. Figure 1b presents a schematic of the flexible bioelectrode fabrication process. A 200 µL of the PPGP composite was pipetted and cast into a circular 3D-printed mold to fabricate flexible epidermal bioelectrodes. The material was then degassed for 5 min to remove any air bubbles formed during mixing, ensuring the PDMS elastomer was free of voids that could compromise its electrical and mechanical properties. Finally, thermal curing was applied to the electrodes by subjecting them to hot air at 55 °C for 3 h to accelerate the drying process.
Figure 1.
Schematic representation for the preparation of the PPGP circular bioelectrodes and its application for electrophysiological monitoring. (a) Chemical structures of pectin, PANI-ES, glycerol, PDMS. (b) Firstly, all materials, pectin, glycerol, PANI-ES, and PDMS, were simply processed in solution. Secondly, the mixture was drop-cast in a 3D-printed circular mold; finally, the thermal curing was applied at 55 °C. (c) Schematic representation of EMG recording setup.
3. Characterizations and Measurements
The surface morphologies and elemental composition of the electrodes were characterized by using field emission–scanning electron microscopy (FE-SEM) and energy dispersive X-ray spectroscopy (EDS) by TESCAN MAGNA and Tescan VEGA XMU. The structural characteristics of the samples were measured by X-ray diffraction (XRD) (X’Pert3 Powder (Malvern Panalytical B.V., Almelo, The Netherlands). The functional groups in the fabricated bioelectrodes were analyzed using ATR-FTIR spectroscopy with a SHIMADZU IRTracer-100 (Shimadzu Corporation, Kyoto, Japan). The mechanical properties of the electrodes were evaluated using an Instron 5582 universal testing machine (Instron, Norwood, MA, USA). A 3D-printed rectangular mold (5 cm × 0.6 cm × 0.2 cm) was fabricated to assess mechanical robustness. The Young’s modulus was determined by calculating the slope of the elastic region in the stress–strain curve. The EMG bioelectric signals were recorded using the high-quality data acquisition system “PowerLab 26T” with a built-in two-channel bio-amplifier.
3.1. Electrochemical Characterization
All electrochemical experiments were conducted using a Bio-Logic SP300 potentiostat/galvanostat (Bio-Logic, Seyssinet-Pariset, France) in a custom-built electrochemical cell. Electrochemical impedance spectroscopy (EIS) and cyclic voltammetry (CV) measurements were conducted under solid-state conditions using a symmetric two-electrode configuration to evaluate bulk resistance (R), electrical conductivity (σ), impedance (Z) at 1 kHz, charge storage capacity (CSC), and electrochemical stability. Disc-shaped bioelectrodes (1 cm diameter and 2 mm thickness) were prepared using a 3D-printed mold. Then flexible electrodes were sandwiched between two stainless steel electrodes in a Swagelok-type cell for electrochemical characterization. No liquid electrolyte was used during the measurements. The R, σ, and Z at 1 kHz were determined from the EIS measurements, whereas the CSC was obtained from the CV measurements. The R value of the electrodes was determined by identifying the point where the curve intersects the real axis. The electrical conductivity of the electrodes was determined using Equation (1).
where σ is the conductivity, t is the electrode thickness in centimeters, and A is the electrode area in square centimeters. The impedance Z at 1 kHz was plotted on a logarithmic scale, showing the relationship between real impedance and frequency. The CV curve in the potential range of −1 to 1 V at 50 mV scan rate was employed to analyze the electrochemical stability and charge storage capacity (CSC) of the bioelectrode. The CV curve (I vs. V) was transformed into an I vs. time plot to calculate the integral. Then the CSCs of the bioelectrodes were determined by calculating the area enclosed by the CV curve, which represents the charge stored during the reduction phase below the baseline. This value was then divided by the applied scan rate to obtain the CSC. No distinct redox peaks were detected during the CV scan, suggesting that the electrodes exhibit significant pseudocapacitive behavior.
3.2. Mechanical Testing
The mechanical characteristics of the PPGP samples were assessed using a quasi-static uniaxial tension test. The triplicate of the best-performing PPGP samples underwent tensile extension until the sample failed, resulting in breakage. Stress–strain data obtained during mechanical testing were systematically recorded and plotted. Young’s moduli of elasticity, elongation percentage, and maximum stress prior to breakage were calculated to evaluate flexibility, durability, and ductility. The Young’s modulus was determined from the linear region of the stress–strain curve where stress is directly proportional to strain. Each sample was subjected to a controlled tensile force at a constant rate of 5 mm/min until failure. The resulting data were plotted on a stress–strain graph to determine the modulus of elasticity. All samples had a rectangular geometry, measuring 50 mm in length, 10 mm in width. The linear region was identified by applying a linear trendline to various segments of the graph and selecting the segment with the best fit.
4. Results and Discussion
4.1. Structural and Spectroscopic Properties of the PPGP Bioelectrode
The XRD patterns of all materials were analyzed to examine any structural modifications that might occur during composite preparation, ensuring the electrodes retain optimal conductivity and durability. The structural properties of bioelectrodes are crucial for their performance in bioelectric signal detection. XRD analysis provides detailed information on the crystallinity, phases, and other structural parameters [25]. These properties directly influence the electrical characteristics and stability of bioelectrodes, which are essential for accurate and reliable bioelectric signal detection. The XRD spectra of pectin, PDMS, pectin/PDMS, pectin/glycerol/PDMS, and PPGP are shown in Figure 2a. The broad diffraction peak observed at 2θ around 21° indicates the characteristic amorphous nature of the pectin biopolymer, consistent with previous studies [26]. The molecular structure of pectin ranges from 1 to 5 nm [27]. The d-spacing value of pure pectin was observed at 0.42 nm, aligning well with previous reports. Pristine PDMS exhibits a diffraction peak at 2θ = ~11.54°, corresponding to the (101) reflection plane, which aligns with its known amorphous structure [28]. The d-spacing value for the synthesized PDMS polymer was observed at 0.77 nm. The presence of a PDMS peak at 2θ ≈ 11.34° in the pectin/PDMS composite confirms the successful integration of PDMS into the pectin biopolymer. The slight shift in the PDMS diffraction peak from 11.54° to 11.34°, corresponding to a d-spacing of 0.78 nm, suggests structural modifications in the composite and indicates successful integration. In contrast, the d-spacing for the pectin diffraction peak remained unchanged in the pectin/PDMS composite. The addition of glycerol to the pectin/PDMS composite does not alter the structural properties of the resulting pectin/glycerol/PDMS composite. The glycerol was added to the pectin/PDMS composite to enhance the structural flexibility.
Figure 2.
(a) XRD (b) FTIR spectra of the pectin, PDMS, pectin/PDMS, pectin/glycerol/PDMS, and PPGP electrodes.
Finally, PANI-ES was incorporated into the pectin/glycerol/PDMS composite as a conductive filler to synthesize the final PPGP composite electrodes. The PANI-ES-based composite exhibits a broad amorphous diffraction peak centered at 2θ = ~20.5°, characteristic of its non-crystalline structure [29]. A similar broad diffraction peak at 2θ = 20.5° in the PPGP composite confirms the successful incorporation of PANI-ES. Moreover, the addition of PANI-ES to the pectin/glycerol/PDMS composite increased the d-spacing from 0.42 nm to 0.43 nm while decreasing the 2θ value from 21° to 20.5° compared to pectin, suggesting that PANI-ES successfully cross-linked with pectin.
FTIR analysis was conducted to investigate composite formation and the chemical interactions between the composite, which are crucial for determining electrical conductivity. Strong bonding such as hydrogen bonding, π-π stacking, or covalent interactions promotes uniform dispersion of fillers, prevents agglomeration, and facilitates the formation of continuous conductive pathways. These interactions help reduce interfacial resistance, enhance charge transfer, and ensure network stability under mechanical stress. The FTIR spectra of the synthesized materials are shown in Figure 2b. The characteristic vibration band at wavenumber of 3273 cm−1 corresponds to -OH stretching, attributed to inter- and intramolecular hydrogen bonding of galacturonic acid of the pectin biopolymer [22]. The peak at 1407 cm−1 represents the vibrations of carboxylic anions (O=C–O−) in pectin, while the band at 1330 cm−1 corresponds to ring vibrations [30]. The CH stretching vibrations of pure pectin were observed at 2920 cm−1, corresponding to the stretching and bending of CH, CH2, and CH3 groups. The vibration band at 1739 cm−1 corresponds to the C=O stretching of the COOCH3 functional group in pure pectin [26]. The IR spectrum of PDMS exhibits symmetric Si-CH3 stretching at 2975 cm−1. The band at 1257 cm−1 corresponds to symmetric CH3 deformation in Si–CH3. Additionally, a strong band at 1020 cm−1 is associated with asymmetric Si–O–Si stretching, while the band at 790 cm−1 represents Si–C stretching in Si–CH3 [28]. A decrease in transmittance was observed in the pectin/PDMS composite, indicating a physical interaction between PDMS and the pectin biopolymer at the molecular level. A minor shift towards higher wavenumber was observed after incorporating glycerol in the pectin/PDMS composite. The shift of the symmetric Si-CH3 band from 1257 cm−1 to 1259 cm−1 suggests enhanced physical interactions and stronger hydrogen bonding between glycerol and the pectin/PDMS composite. Additionally, the decrease in peak intensity and broadening further validate these interactions.
Previous studies have reported the interaction between pectin and glycerol, indicated by a vibration peak at 1047 cm−1 [31]. In the current FTIR analysis, the broadening of this vibration peak in the pectin/glycerol/PDMS composite suggests a stronger interaction among pectin, glycerol, and PDMS. In the PPGP composite, the C–N= band at 1240 cm−1 appears due to the aromatic ring of PANI, and the C–H out-of-plane bending vibration in the benzene ring at 806 cm−1 was also present [32]. However, these peaks were suppressed by the high transmittance intensity of the Si–CH3 band at 1257 cm−1. The broad N–H stretching peak in the PPGP composite at 3444 cm−1 is associated with the PANI-ES [33], and confirms the successful incorporation of PANI-ES and the formation of the PPGP composite. A comparison of the FTIR spectra for pectin, PDMS, pectin/PDMS, pectin/glycerol/PDMS, and the PPGP composite shows no additional peaks, suggesting that no new substances were formed.
4.2. Morphological Properties of the PPGP Bioelectrode
Investigating the morphological properties of flexible electrodes for wearable application is crucial as it directly influences their performance in bioelectric signal monitoring applications. Surface features such as average roughness, porosity, and wrinkling patterns enhance electrode adhesion, flexibility, and interfacial stability, which are critical for improving electrical performance and ensuring consistent, high-quality signal acquisition. Understanding these morphological characteristics enables the design of electrodes that provide reliable monitoring of bioelectric signals, making them well-suited for applications like EMG recordings. Figure 3a presents a top-view SEM image of the PPGP electrode, fabricated via a simple solution-mixing method. The SEM and AFM images of pectin, PDMS, pectin/PDMS, and pectin/glycerol/PDMS, are shown in [Figure S2a–d]. Figure S2c shows the SEM image of pectin/PDMS, where the incorporation of PDMS into pectin leads to the formation of microwrinkle patterns on the surface. The detailed explanation is added in the SI. The incorporation of conductive fillers (PANI-ES) into the pectin/glycerol/PDMS composite enhanced the microwrinkle structure in the final PPGP electrode (Figure 3a). The microwrinkle surface morphology observed in the PPGP electrode, shown in the SEM image (Figure 3a), plays a crucial role in enhancing EMG detection performance. The wrinkling pattern on the electrode’s surface can facilitate better adhesion to the skin, ensuring a stable interface that is essential for the acquisition of high-fidelity bioelectric signals [34]. Moreover, the dynamic wrinkled surface morphology enables the electrodes to conform to skin contours [35]. This microwrinkle pattern significantly enhances the average surface roughness of PPGP flexible electrodes, exhibiting superior adaptability and electrophysiological sensing performance. The average surface roughness of the electrodes was examined using an AFM over a 3 × 3 μm area in non-contact mode. Figure S2e–h show the 3D AFM micrographs of the pectin, PDMS, pectin/PDMS, and pectin/glycerol/PDMS electrodes, with average surface roughness values of 7.42 nm 1.30 nm, 9.54 nm, and 23.39 nm, respectively. The introduction of the PANI-ES conductive filler to pectin/glycerol/PDMS significantly increased average surface roughness from 23.39 nm to 51.49 nm, as shown in Figure 3b. The SEM and AFM results align with the electrochemical performance of the flexible electrodes, as detailed in Section 5.4. This unique surface structure increases the effective surface area of the electrode, which is beneficial for improving the interaction between the electrode and biological tissues. AFM was utilized to quantify the local, sub-micron average surface roughness of the electrode as seen in S2. The local nanoscale surface roughness of the materials is shown in Table 1. The PPGP electrode appears to possess a complex hierarchical structure characterized by large macro-wrinkles. SEM images recorded at three different locations are shown in Figure S3, which confirms these features are uniformly distributed across the entire surface. The AFM scanning area was specifically selected to represent the intrinsic nanoscale texture of the material independent of the macro-scale folds.
Figure 3.
(a) SEM image and (b) 3D AFM micrograph of the PPGP bioelectrode.
Table 1.
Local nanoscale surface roughness of the electrodes.
4.3. Wettability and Adhesive Properties
The electrode’s surface wetting behavior was investigated using water contact angle measurement (WCA). The PPGP electrode exhibited an average WCA of ~71.2° (Figure 4a), affecting its wetting properties, which in turn influence skin adhesion and contact impedance. The electrophysiological sensors with a moderately hydrophilic surface (WCA < 90°) promote better electrode–skin interaction, reducing contact resistance and improving bioelectrical signal acquisition. Additionally, the hydrophilic nature allows for controlled sweat absorption and dispersion, minimizing motion artifacts and electrical noise, ensuring stable and reliable signal detection. Figure 4b illustrates the adhesive properties of the PPGP electrodes. The substantial surface wrinkles of the PPGP electrodes enable good adhesion to dynamic human skin.
Figure 4.
(a) Water contact angle (WCA) of the PPGP bioelectrode. The red line represents the fitted contour of the water droplet used for contact angle analysis. (b) Adhesivity of the PPGP electrodes to the inner wrist.
5. Systematic Investigation of Electrical Conductivity for Electrophysiological Sensing
The electrical conductivity of flexible epidermal electrodes plays a crucial role in electrophysiological sensing by facilitating efficient signal transmission between biological tissues and electrodes. The systematic investigation of the bulk electrical conductivity of the electrodes for electrophysiological sensing involved two key steps. In the first step, glycerol concentrations were varied in the pectin/PDMS composite to enhance the ion mobility and improve the overall conductivity of the bioelectrode. After determining the optimal glycerol percentage, the second step involved fixing the glycerol content and adjusting the PANI-ES percentage in the pectin/glycerol/PDMS composite. Investigating the use of PANI-ES as a conductive nanofiller in bioelectrode fabrication is expected to markedly enhance electrical conductivity.
5.1. Investigation of Glycerol Concentration in Pectin/PDMS Composite
Electrochemical impedance spectroscopy was utilized to evaluate the bulk electrical conductivity of the composition. Figure S4 shows the Nyquist plot, CV, and real impedance vs. frequency plot of pectin and PDMS. The conductivity of the pectin/PDMS composite was found to be in the order of 10−7 S/cm (Table S1). The initial conductivity of the pectin/PDMS composite is insufficient for recording high-quality bioelectric signals from the dynamic human body. Therefore, enhancing the conductivity was necessary. Incorporating glycerol into the composite materials enhances conductivity. Additionally, glycerol may improve the material’s overall performance by increasing ion mobility and promoting a more flexible, conductive network within the polymer matrix [36]. We varied the glycerol content to 1%, 3%, and 5% in the pectin/PDMS composite and their corresponding Nyquist plot, CV, and real impedance vs. frequency plots are shown in Figure S5. The bulk resistance (R), impedance (Z) at 1 kHz, electrical conductivity, and charge storage capacity (CSC) values of the glycerol-modified pectin/PDMS composite are shown in SI (Table S1). All experimental data are presented as mean ± standard deviation (n = 3). The conductivity of the glycerol-modified pectin/PDMS composite increased significantly from the order of 10−7 S/cm to the order of 2.22 × 10−4 S/cm, with notable improvements in other electrochemical parameters such as R, Z @ 1 kHz, and SCS, as detailed in Table S1. Nevertheless, the conductivity is still inadequate for capturing bioelectric signals using glycerol-modified pectin/PDMS electrodes. However, adding more than 5% glycerol caused the composite to become gel-like, preventing it from drying. Finally, we incorporated PANI-ES as a conductive filler into the pectin/glycerol/PDMS composite to further enhance the electrochemical performance of the flexible PPGP electrodes, as discussed in the next section.
5.2. Systematic Investigation of PANI-ES Concentration in Pectin/PDMS/Glycerol Composite
In this study, a systematic investigation was carried out by varying the PANI-ES concentration at 1, 3, 6, 9, and 12 wt% in the pectin/glycerol/PDMS composite to evaluate its influence on the electrical conductivity. Three independently fabricated electrodes were evaluated for each formulation, and the corresponding EIS spectra, Z at 1 kHz, and CV curves are shown in Figure S6. All electrochemical data are presented as mean ± standard deviation (n = 3). Figure S6a–e show the EIS spectra of the varying concentrations of PANI-ES between 1%, 3%, 6%, 9%, and 12% to investigate the electrical conductivity of the PPGP composite electrodes. At 1% PANI-ES, the conductivity was very low, indicating that this small amount of PANI-ES is insufficient to form effective conductive pathways. As the concentration increases to 3% and 6%, there is a noticeable improvement in conductivity, demonstrating that higher PANI-ES content enhances the composite’s electrical performance. The highest bulk electrical conductivity of (7.54 ± 0.81) × 10−3 S/cm, along with an R of 0.034 ± 0.00 kΩ, CSC of 4.63 ± 2.70 mC/cm2, and Z at 1 kHz of 0.48 ± 0.06 kΩ, was observed at 9% PANI-ES. This concentration was identified as most effective among the used concentrations for improving the electrochemical performance (Table 2). However, further increasing the PANI concentration to 12% resulted in a reduction in electrochemical performance. This suggests that the 9% concentration of PANI-ES exhibited superior performance. The excessive amount of PANI-ES negatively impacts the overall electrochemical performance. The conductivity of the PPGP composite decreases when the concentration of PANI-ES is increased due to the formation of insulating barriers within the composite. As the PANI-ES concentration reaches 12%, there is a tendency for PANI-ES particles to agglomerate within the composite [37]. These agglomerates disrupt the continuous conductive pathways, resulting in decreased conductivity to (3.05 ± 0.30) × 10−3 to (3.05 ± 0.30) × 10−3 S/cm. This is because the electrical conductivity is directly dependent on the agglomeration [38]. The presence of electron-donating substituents in the PANI chain increases steric hindrance between the molecular chains, thereby reducing intermolecular forces and minimizing the likelihood of agglomeration [39]. This phenomenon is especially evident when the distribution of polyaniline is uneven, leading to inefficient electron transport across the composite material and negatively impacting its electrochemical performance. The electrical conductivity trend was examined with an increasing PANI-ES percentage. Figure S6f–j represent the real impedance (Zreal) vs. frequency plots for pectin/glycerol/PDMS composites with varying PANI-ES concentrations (1%, 3%, 6%, 9%, and 12%). At the clinically relevant frequency of 1 kHz, the 9% PANI-ES composite exhibits the lowest impedance of 0.034 ± 0.003 kΩ. Figure 5 shows the relationship between the electrical conductivity of the pectin/glycerol/PDMS composite with varying percentages of PANI-ES. The conductivity error bars in the graph represent the variability in measurements obtained from three different electrodes for each PANI-ES percentage. Figure S6k–o presents the CV curves of pectin/glycerol/PDMS composites containing different PANI-ES concentrations (1%, 3%, 6%, 9%, and 12%). As the PANI content increases, the current response becomes more pronounced, reflecting enhanced charge storage capacity (CSC) and electrical conductivity. The 9% PANI-ES electrode exhibits superior electrochemical performance, consistent with the EIS results. Therefore, the systematic variation of PANI-ES content revealed that 9 wt% offers an effective trade-off between structural stability, electrical conductivity, and electrochemical behavior, making it suitable for bioelectric sensing applications.
Table 2.
Summary of the electrochemical properties of PPGP electrode compositions without and with PANI ((values represent mean ± standard deviation, where n = 3).
Figure 5.
Electrical conductivity error bar. Three samples were used to determine the error bars.
5.3. Electrochemical Performance
The electrochemical properties of electrodes were analyzed using EIS and CV techniques to evaluate their effectiveness for electrophysiological sensing applications. To confirm the reproducibility of the electrochemical performance, the best-performing electrodes were subjected to three independent trials. The Nyquist plots for the composite materials, shown in Figure 6a, reveal bulk resistance values of 1.29 ± 0.16 kΩ for pectin/PDMS, 0.36 ± 0.11 kΩ for pectin/glycerol/PDMS, and 0.034 ± 0.003 kΩ for PPGP electrodes. The EIS findings provided insight into the bulk resistance behavior of the electrodes, which is crucial for minimizing signal distortion during bioelectric signal monitoring. By systematically comparing these composite formulations, the study identified improvements in bulk electrical conductivity with the addition of glycerol as a plasticizer and PANI-ES as conductive filler. Glycerol helps disperse PANI-ES more evenly throughout the pectin/PDMS matrix. This prevents agglomeration of PANI-ES particles, ensuring a more effective conduction pathway. The conductivity (σ) results shown in Figure 6b reveal that the PPGP electrodes exhibited the highest σ of 7.54 ± 0.81 × 10−3 S/cm. Three samples were used to determine the error bars (Figure S7). The addition of glycerol and PANI-ES significantly enhanced both flexibility and electrical properties. The CSC and electrochemical stability of the bioelectrodes were evaluated using CV measurements, as shown in Figure 6c. The calculated CSC values for PP, PGP (Table S1), and PPGP electrodes were 99 ± 40 µC/cm2, 0.75 ± 0.31 µC/cm2, and 4.63 ± 2.70 mC/cm2, respectively. Notably, the PPGP electrodes exhibited the highest CSC at 4.63 ± 2.70 (Table 2) mC/cm2, significantly surpassing the CSC values of PP (99 ± 40 µC/cm2) and PGP (0.75 ± 0.31 µC/cm2). Figure 6d represents the impedance at 1 kHz spectra, which is a crucial metric for post-implantation evaluation at the electrode–tissue interface because it reflects the overall electrical behavior and the integrity of the interface between the implanted electrode and surrounding biological tissue. The comparative performance metrics of the current PPGP electrodes with literature benchmarks are shown in Table 3. The Z at 1 kHz for pectin/PDMS was 9.73 ± 3.55 kΩ, pectin/glycerol/PDMS was 6.68 ± 1.53 kΩ, and PPGP 0.034 ± 0.003 kΩ. At this frequency, which is within the range of bioelectric signals like EMG, impedance measurements provide insight into the quality of signal transmission and recording. High impedance at this frequency can indicate poor electrode–tissue contact, increased resistance, or signal loss due to factors such as inflammation, fibrosis, or degradation of the electrode material [40]. Lower impedance generally ensures efficient signal transduction, improved sensitivity, and reduced noise, which are essential for reliable bioelectric signal monitoring after implantation [41]. Thus, monitoring the impedance at 1 kHz helps assess the performance and biocompatibility of the electrode, ensuring its efficacy for electrophysiological sensing.
Figure 6.
Electrochemical characterization of the electrodes. (a) Nyquist plot. (b) Electrical conductivity error plot. Three samples were used to determine the error bars. (c) CV. (d) Real impedance vs. frequency plot of pectin/PDMS, pectin/glycerol/PDMS, PPGP.
Table 3.
Comparative performance metrics of the current PPGP electrodes with literature benchmarks.
5.4. Mechanical Characterization
Three identical samples, each measuring 50 mm in length and 10 mm in width, were fabricated from the best-identified composition of the PPGP electrode (9% PANI-ES, 64% pectin, 5% glycerol, 22% PDMS). The stress–strain curve of the best-performing PPGP electrode is presented in Figure 7, while the corresponding curves for three replicate PPGP electrodes are shown in Figure S8. These samples were clamped in the tensile testing apparatus and stretched until failure, typically by breakage. The applied force and extension values were recorded, from which stress–strain data were calculated and graphed. The stress and strain curve is used to determine Young’s modulus to quantify PPGP electrodes’ flexibility and stiffness. To highlight the mechanical performance of the prepared electrodes, their Young’s moduli are summarized and compared with the state-of-the-art literature values in Table 4. The PPGP electrode exhibits an average tensile strength of 0.183 ± 0.123 MPa on triplicate samples (Table S2).
Figure 7.
Stress–strain curve for PPGP electrode composed of 9% PANI-ES, 64% pectin, 5% glycerol, 22% PDMS.
Table 4.
Summary of the Young’s moduli of the fabricated electrodes and a comparative analysis with the literature.
6. Electrophysiological Sensing
The PPGP flexible bioelectrodes have been successfully applied for EMG signal measurements. The bioelectrodes used for EMG recordings are designed in a circular shape to match the intended application. However, to evaluate the PPGP electrodes’ mechanical properties, we fabricated them in a rectangular shape. This configuration allowed for a comprehensive demonstration of the electrodes’ durability and flexibility under various mechanical deformations. Figure 8a illustrates the bioelectrodes’ stretchability, bending, twisting, crumpling, and recovery, highlighting their robustness for bioelectronic applications. To evaluate the adhesion characteristics of the electrode, a simple peel test was conducted, demonstrating firm and stable attachment during deformation as illustrated in Figure 8b. The images show (left) the electrode firmly attached to the skin, (middle) the electrode during peeling, and (right) partial detachment, illustrating its stable adhesion and mechanical integrity.
Figure 8.
(a) PPGP electrode’s durability and flexibility under various mechanical deformations. (b) Representative photographs demonstrating the adhesion performance of the flexible bioelectrode during a manual peel test.
EMG Signal Recording
Electromyography (EMG) signals are generated by the electrical activity of muscle fibers when they are activated by motor neurons [47]. The developed PPGP electrodes were attached to the left human forearm to detect sEMG signals [48]. Before applying the electrodes with transparent scotch tape, the skin was cleansed with alcohol swabs. A blunted syringe was used to apply conductive gel onto the electrode surface to reduce skin–electrode impedance. During the EMG recording, the subject was seated upright with their arm resting on their thigh while performing fist opening and closing movements. A 2 kHz low-pass filter and a 1 Hz high-pass filter were applied to the recorded EMG signal. Sampling was performed at a frequency of 2 kHz. The EMG signal produced by first opening and closing was measured using both PPGP electrodes and commercial Ag/AgCl electrodes, as demonstrated in Figure 9. Signal-to-noise ratios (SNRs) of the EMG signals were determined using the following equation [49].
where Vs and Vn denote the voltage amplitude of signal and noise, respectively. The PPGP electrode demonstrated a significantly higher Signal-to-Noise Ratio (SNR) of 29.54 dB compared to the commercial Ag/AgCl electrode, which achieved an SNR of 16.48 dB. This superior SNR highlights the enhanced ability of the PPGP electrode to minimize noise and provide clearer bioelectric signal recordings, making it a promising candidate for advanced electrophysiological sensing applications. Detecting EMG signals from muscle movements is crucial for applications in human–machine interfaces. For instance, EMG signals from hand opening and closing, captured by PPGP electrodes, can be used as a real-time control interface for operating an anthropomorphic robotic hand.
Figure 9.
EMG signals generated by the opening and closing of the fist recorded by the commercial Ag/AgCl electrode and the developed PPGP electrode.
To evaluate the long-term stability of the developed bioelectrodes for EMG monitoring, the 9% PANI-ES/64% pectin/5% glycerol/22% PDMS electrodes were tested over a period of three weeks. As shown in Figure 10, the electrodes consistently recorded high-quality EMG signals, with average SNR values of ~36.35, ~33.13, and ~30.11 dB during weeks 1, 2, and 3, respectively. Although a slight decrease in SNR was observed over the three-week period, all values remained above 30 dB, indicating stable signal quality. The slight decrease in SNR over time may be attributed to minor changes in the electrode–skin interface during repeated use and storage [50]. Furthermore, the EMG waveforms retained their characteristic features throughout the evaluation period, demonstrating the long-term stability and reliability of the developed bioelectrodes.
Figure 10.
EMG recorded with the 9% PANI-ES, 64% pectin, 5% glycerol, 22% PDMS electrodes over a period of 3 weeks.
7. Conclusions
Flexible PPGP bioelectrodes composed of pectin, PANI-ES, glycerol, and PDMS were developed in this work. The optimal concentration of PANI-ES conductive nanofiller resulted in the formation of effective conductive pathways and reduced impedance. Moreover, the introduction of glycerol played a key role in dispersion and improving interfacial adhesion between the pectin biopolymers and PANI-ES nanofillers. The as-seen micro-wrinkle patterns on the surface of the PPGP bioelectrodes enhanced adhesion to skin contours. These combined features enabled the capture of high-fidelity bioelectric signals, making them more viable for application in EMG recording. While the current results demonstrate excellent electrical and mechanical performance, future investigations will prioritize comprehensive cytotoxicity testing to fully validate the biocompatibility of these electrodes for clinical use. Our skin-attachable PPGP flexible electrode holds promise for advancing biomedical skin patches, enabling a wide range of future healthcare applications. Additionally, it has the potential to drive innovation in key technologies, including future wearable smart textiles, prosthetic hand controllers for amputees, and the control of home appliances and other electronic devices through next-generation HMI technology.
Supplementary Materials
The following supporting information can be downloaded at: https://www.mdpi.com/article/10.3390/macromol6030064/s1, Figure S1: The circular disc electrode automatically generates crevices during room temperature drying process which indicate poor interfacial adhesion between pectin and PANI-ES; Figure S2: (a–d) SEM and (e–h) 3D AFM images of Pectin, PDMS, Pectin/PDMS, and Pectin/Glycerol/PDMS; Figure S3: SEM images of the PPGP electrode acquired from three randomly selected regions across the surface of the same sample; Figure S4: (a) Nyquist plot (b) cyclic voltammogram (c) real impedance vs. frequency plot of a pectin only. (d) Nyquist plot (e) cyclic voltammogram (f) real impedance vs. frequency plot of a PDMS only; Figure S5: Varying percentages of glycerol (0, 1, 3, and 5 %) in Pectin/PDMS. (a–d) Nyquist plot (e–h) Real impedance vs. frequency spectra to determine the real impedance at 1 kHz frequency (i–l) cyclic voltammogram; Figure S6: Varying percentages of PANI-ES (1, 3, 6, 9, and 12 %) in Pectin/PDMS/Glycerol composite. (a–e) Nyquist plot (f–j) Real impedance vs. frequency spectra to determine the real impedance at 1 kHz frequency (k–o) cyclic voltammogram; Figure S7: Nyquist plot of 3 different electrodes of (a) Pectin/PDMS and (b) Pectin/Glycerol/PDMS. Figure S8: Stress-strain curve of three different PPGP electrodes. Table S1: Electrode composition for glycerol-modified Pectin/PDMS electrodes; Table S2: Young’s Modulus of three different electrodes.
Author Contributions
Conceptualization, P.W.S., A.A.-O., H.A.-N. and M.H.A.-S.; methodology, P.W.S. and M.A.; software, P.W.S. and M.A.; validation, P.W.S., M.A., A.A.-O., H.A.-N. and M.A.; formal analysis, P.W.S.; investigation P.W.S., M.A., A.A.-O., H.A.-N. and M.H.A.-S.; resources, A.A.-O., H.A.-N. and M.H.A.-S.; data curation, P.W.S. and M.A.; writing—original draft preparation, P.W.S.; writing—review and editing, P.W.S., M.A., A.A.-O., H.A.-N. and M.H.A.-S.; visualization, P.W.S.; supervision, A.A.-O., H.A.-N. and M.H.A.-S.; project administration, A.A.-O., H.A.-N. and M.H.A.-S.; funding acquisition, A.A.-O. and H.A.-N. All authors have read and agreed to the published version of the manuscript.
Funding
This research was funded by American University of Sharjah through the PDFA program with award number PDFA24-E59.
Institutional Review Board Statement
The experiment complies with the guidelines stated in the Declaration of Helsinki and was approved by Institutional Review Board of the American University of Sharjah (protocol Code 25-026, approval date 8 January 2025).
Informed Consent Statement
All participants were undergraduate students from the American University of Sharjah, primarily seniors and juniors. The inclusion criteria of the participants include young healthy adults with no physiologic or neurological disorders. Participants sat in a cool, air-conditioned environment. A brief explanation about the experiment’s protocol was given to each participant, and they were asked to sign a written informed consent, knowing that they have the right to end the experiment at any time.
Data Availability Statement
The data supporting the findings of this study are available within the article and its Supplementary Materials.
Acknowledgments
The authors would like to thank the support provided by the American University of Sharjah through the PDFA program with award number PDFA24-E59. The authors sincerely acknowledge the Materials Research Center (MRC) for providing access to the SEM facilities and for their valuable support in analysis. The authors acknowledge the use of artificial intelligence (AI) tools (e.g., Grammarly, ChatGPT (GPT-5.6 Sol, OpenAI), OpenAI) solely for language polishing and improving grammar only. All intellectual and scientific content, including data analysis, interpretation, and conclusions, are entirely the authors’ own.
Conflicts of Interest
The authors declare no conflict of interest.
References
- Li, G.; Chen, N.; Xu, T.; Zhang, Y. Flexible Fe3 +-doped gelatin/poly(acrylate-co-acrylamide) conductive hydrogels for biopotential acquisition, salt recognition, and supercapacitors. Sens. Actuators Phys. 2025, 387, 116425. [Google Scholar] [CrossRef] [Scilit]
- Sayyad, P.W.; Park, S.-J.; Ha, T.-J. Recent advances in biosensors based on metal-oxide semiconductors system-integrated into bioelectronics. Biosens. Bioelectron. 2024, 259, 116407. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Hu, L.; Kim, B.J.; Ji, S.; Hong, J.; Katiyar, A.K.; Ahn, J.-H. Smart electronics based on 2D materials for wireless healthcare monitoring. Appl. Phys. Rev. 2022, 9, 041308. [Google Scholar] [CrossRef] [Scilit]
- Sayyad, P.W.; Al-Nashash, H.; Al-Othman, A.; Al-Sayah, M.H. Emerging Trends in System-Integrated Wearable Epidermal and Flexible Electrodes: Material Design and Applications in Physiological Monitoring. IEEE Trans. Compon. Packag. Manuf. Technol. 2025, 15, 905–937. [Google Scholar] [CrossRef] [Scilit]
- Li, Z.; Guo, W.; Huang, Y.; Zhu, K.; Yi, H.; Wu, H. On-skin graphene electrodes for large area electrophysiological monitoring and human-machine interfaces. Carbon 2020, 164, 164–170. [Google Scholar] [CrossRef] [Scilit]
- Li, W.; Xu, M.; Gao, J.; Zhang, X.; Huang, H.; Zhao, R.; Zhu, X.; Yang, Y.; Luo, L.; Chen, M.; et al. Large-Scale Ultra-Robust MoS2 Patterns Directly Synthesized on Polymer Substrate for Flexible Sensing Electronics. Adv. Mater. 2023, 35, 2207447. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Yang, H.; Li, G.; Wang, J.; Hou, Q.; Pan, H.; Quan, J.; Chen, Y.; Xu, J.; Liu, Y.; Liu, H. Paper-based microfluidic chip for sweat volume, ECG and EMG monitoring. Sens. Actuators Phys. 2024, 371, 115264. [Google Scholar] [CrossRef] [Scilit]
- Zhang, Y.; Deng, Z.; Hong, P.; Bao, Z.; Yin, X.; Zhu, P. Screen-printed ultra-thin and multifunctional e-tattoos towards epidermal sensors. Sens. Actuators Phys. 2025, 387, 116424. [Google Scholar] [CrossRef] [Scilit]
- Jeong, S.; Heo, S.; Kang, M.; Kim, H.-J. Mechanical durability enhancement of gold-nanosheet stretchable electrodes for wearable human bio-signal detection. Mater. Des. 2020, 196, 109178. [Google Scholar] [CrossRef] [Scilit]
- Sayyad, P.W.; Park, S.-J.; Ha, T.-J. Bioinspired nanoplatforms for human-machine interfaces: Recent progress in materials and device applications. Biotechnol. Adv. 2024, 70, 108297. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Ha, T.; Tran, J.; Liu, S.; Jang, H.; Jeong, H.; Mitbander, R.; Huh, H.; Qiu, Y.; Duong, J.; Wang, R.L.; et al. A Chest-Laminated Ultrathin and Stretchable E-Tattoo for the Measurement of Electrocardiogram, Seismocardiogram, and Cardiac Time Intervals. Adv. Sci. 2019, 6, 1900290. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Basarir, F.; Haj, Y.A.; Zou, F.; De, S.; Nguyen, A.; Frey, A.; Haider, I.; Sariola, V.; Vapaavuori, J. Edible and Biodegradable Wearable Capacitive Pressure Sensors: A Paradigm Shift toward Sustainable Electronics with Bio-Based Materials. Adv. Funct. Mater. 2024, 34, 2403268. [Google Scholar] [CrossRef] [Scilit]
- Kong, L.; Gao, Z.; Li, X.; Gao, G. An amylopectin-enabled skin-mounted hydrogel wearable sensor. J. Mater. Chem. B 2021, 9, 1082–1088. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Lersanansit, N.; Pungjunun, K.; Chailapakul, O.; Praphairaksit, N. Development of pectin-based gel electrolyte for wireless electrochemical determination of cadmium and lead using smartphone. Talanta 2024, 276, 126211. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Nemiwal, M.; Zhang, T.C.; Kumar, D. Pectin modified metal nanoparticles and their application in property modification of biosensors. Carbohydr. Polym. Technol. Appl. 2021, 2, 100164. [Google Scholar] [CrossRef] [Scilit]
- Groult, S.; Budtova, T. Thermal conductivity/structure correlations in thermal super-insulating pectin aerogels. Carbohydr. Polym. 2018, 196, 73–81. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Zhao, H.-B.; Chen, M.; Chen, H.-B. Thermally Insulating and Flame-Retardant Polyaniline/Pectin Aerogels. ACS Sustain. Chem. Eng. 2017, 5, 7012–7019. [Google Scholar] [CrossRef] [Scilit]
- Zhao, H.-B.; Yuan, L.; Fu, Z.-B.; Wang, C.-Y.; Yang, X.; Zhu, J.-Y.; Qu, J.; Chen, H.-B.; Schiraldi, D.A. Biomass-Based Mechanically Strong and Electrically Conductive Polymer Aerogels and Their Application for Supercapacitors. ACS Appl. Mater. Interfaces 2016, 8, 9917–9924. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Farea, M.A.; Mohammed, H.Y.; Sayyad, P.W.; Ingle, N.N.; Al-Gahouari, T.; Mahadik, M.M.; Bodkhe, G.A.; Shirsat, S.M.; Shirsat, M.D. Carbon monoxide sensor based on polypyrrole–graphene oxide composite: A cost-effective approach. Appl. Phys. A 2021, 127, 681. [Google Scholar] [CrossRef] [Scilit]
- Alex, M.; Al-Othman, A.; Al-Sayah, M.; Al-Nashash, H. Development and characterization of novel flexible cellulose electrodes for electrophysiological monitoring. RSC Adv. 2025, 15, 25698–25706. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Zhou, H.; Li, D.; He, X.; Hui, X.; Guo, H.; Hu, C.; Mu, X.; Wang, Z.L. Bionic Ultra-Sensitive Self-Powered Electromechanical Sensor for Muscle-Triggered Communication Application. Adv. Sci. 2021, 8, 2101020. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Liu, Y.; Liu, R.; Liu, H.; Li, D.; Fu, S.; Jin, K.; Cheng, Y.; Fu, Z.; Xing, F.; Tian, Y. Tough, high conductivity pectin polysaccharide-based hydrogel for strain sensing and real-time information transmission. Int. J. Biol. Macromol. 2024, 257, 128757. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Wilson, N.W.; Botte, G.G. Novel biopolymer pectin-based hydrogel electrolytes for sustainable energy storage. Mater. Adv. 2024, 5, 7312–7326. [Google Scholar] [CrossRef] [Scilit]
- Kumar, K.; Noor, I.S.M.; Pandey, S.P.; Bhattacharya, B.; Saxena, A. Electrical conductivity of pectin-based biopolymer electrolytes: Search for a theoretical framework. J. Solid State Electrochem. 2025, 29, 4209–4216. [Google Scholar] [CrossRef] [Scilit]
- Sayyad, P.W.; Hedau, B.; Kim, E.-H.; Kim, J.; Ha, T.-J. Moisture electric generators with Ti3C2Tx–gelatin nanocomposites driven by the hydrovoltaic effect for self-powered flexible humidity sensors. J. Mater. Chem. A 2026, 14, 5007–5017. [Google Scholar] [CrossRef] [Scilit]
- Perumal, P.; Christopher Selvin, P.; Selvasekarapandian, S. Characterization of biopolymer pectin with lithium chloride and its applications to electrochemical devices. Ionics 2018, 24, 3259–3270. [Google Scholar] [CrossRef] [Scilit]
- Siemianowski, O.; Rongpipi, S.; Del Mundo, J.T.; Freychet, G.; Zhernenkov, M.; Gomez, E.D.; Gomez, E.W.; Anderson, C.T. Flexible Pectin Nanopatterning Drives Cell Wall Organization in Plants. JACS Au 2024, 4, 177–188. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Atta, A.; Abdeltwab, E. Influence of Ion Irradiation on the Surface Properties of Silver-Coated Flexible PDMS Polymeric Films. Braz. J. Phys. 2021, 52, 3. [Google Scholar] [CrossRef] [Scilit]
- Srivastava, S.; Kumar, S.; Singh, V.N.; Singh, M.; Vijay, Y.K. Synthesis and characterization of TiO2 doped polyaniline composites for hydrogen gas sensing. Int. J. Hydrogen Energy 2011, 36, 6343–6355. [Google Scholar] [CrossRef] [Scilit]
- Kaczmarska, A.; Pieczywek, P.M.; Cybulska, J.; Zdunek, A. Effect of enzymatic modification on the structure and rheological properties of diluted alkali-soluble pectin fraction rich in RG-I. Sci. Rep. 2024, 14, 11454. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Costanza, V.; Bonanomi, L.; Moscato, G.; Wang, L.; Choi, Y.S.; Daraio, C. Effect of glycerol on the mechanical and temperature-sensing properties of pectin films. Appl. Phys. Lett. 2019, 115, 193702. [Google Scholar] [CrossRef] [Scilit]
- Yang, W.; Ji, Q.; Xiong, K.; Dong, Y.; Fu, Y.; Zhu, Y. Development of a Short Carbon Fiber@Polyaniline/Polydimethylsiloxane Flexible Composite Film with Excellent Microwave Absorption Properties at an Ultralow Filler Content. ACS Appl. Polym. Mater. 2023, 5, 10265–10275. [Google Scholar] [CrossRef] [Scilit]
- Hou, X.; Zhou, Y.; Liu, Y.; Wang, L.; Wang, J. Coaxial electrospun flexible PANI//PU fibers as highly sensitive pH wearable sensor. J. Mater. Sci. 2020, 55, 16033–16047. [Google Scholar] [CrossRef] [Scilit]
- Min, H.; Baik, S.; Kim, J.; Lee, J.; Bok, B.-G.; Song, J.H.; Kim, M.-S.; Pang, C. Tough Carbon Nanotube-Implanted Bioinspired Three-Dimensional Electrical Adhesive for Isotropically Stretchable Water-Repellent Bioelectronics. Adv. Funct. Mater. 2022, 32, 2107285. [Google Scholar] [CrossRef] [Scilit]
- Oh, J.; Nam, K.-W.; Kim, W.-J.; Kang, B.-H.; Park, S.-H. Flexible Dry Electrode Based on a Wrinkled Surface That Uses Carbon Nanotube/Polymer Composites for Recording Electroencephalograms. Materials 2024, 17, 668. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Jain, K.; Wang, Z.; Garma, L.D.; Engel, E.; Ciftci, G.C.; Fager, C.; Larsson, P.A.; Wågberg, L. 3D printable composites of modified cellulose fibers and conductive polymers and their use in wearable electronics. Appl. Mater. Today 2023, 30, 101703. [Google Scholar] [CrossRef] [Scilit]
- Umar, A.; Ahmed, F.; Ullah, N.; Ansari, S.A.; Hussain, S.; Ibrahim, A.A.; Qasem, H.; Kumar, S.A.; Alhamami, M.A.; Almehbad, N.; et al. Exploring the potential of reduced graphene oxide/polyaniline (rGO@PANI) nanocomposites for high-performance supercapacitor application. Electrochim. Acta 2024, 479, 143743. [Google Scholar] [CrossRef] [Scilit]
- Azimi, N.; Sharifzadeh, E. Improved aggregation/agglomeration-dependent percolation theory to predict nanoparticle-aided electrical conductivity in polymer nanocomposites: A combination of analytical strategy and artificial neural network. Comput. Mater. Sci. 2025, 246, 113424. [Google Scholar] [CrossRef] [Scilit]
- Gao, F.; Mu, J.; Bi, Z.; Wang, S.; Li, Z. Recent advances of polyaniline composites in anticorrosive coatings: A review. Prog. Org. Coat. 2021, 151, 106071. [Google Scholar] [CrossRef] [Scilit]
- Sankar, V.; Patrick, E.; Dieme, R.; Sanchez, J.C.; Prasad, A.; Nishida, T. Electrode impedance analysis of chronic tungsten microwire neural implants: Understanding abiotic vs. biotic contributions. Front. Neuroeng. 2014, 7, 13. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Chu, Y.; Sha, Z.; Brown, S.A.; He, S.; Wu, S.; Wang, C.H.; Peng, S. Recent advances in low-impedance conductive nanocomposites for wearable and implantable electronics. Adv. Nanocompos. 2024, 1, 275–289. [Google Scholar] [CrossRef] [Scilit]
- Alex, M.; Khan, K.R.B.; Al-Othman, A.; Al-Sayah, M.H.; Al Nashash, H. MXene-Based Flexible Electrodes for Electrophysiological Monitoring. Sensors 2024, 24, 3260. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Alatoom, A.; Al-Othman, A.; Al-Nashash, H.; Al-Sayah, M. Development and Characterization of Novel Composite and Flexible Electrode Based on Titanium Dioxide. IEEE Trans. Compon. Packag. Manuf. Technol. 2020, 10, 1079–1087. [Google Scholar] [CrossRef] [Scilit]
- Ali, A.A.; Al-Sayah, M.H.; Al-Othman, A.; Al-Nashash, H. Flexible PDMS Composite Electrodes with Boronic Acid-Modified Carbon Dots for Surface Electrophysiological Signal Recording. ACS Appl. Electron. Mater. 2024, 6, 576–586. [Google Scholar] [CrossRef] [Scilit]
- Almufleh, N.; Al-Othman, A.; Alani, Z.; Al-Sayah, M.H.; Al-Nashash, H. Highly Flexible Polyaniline-Based Implantable Electrode Materials for Neural Sensing/Stimulation Applications. Electron. Mater. 2021, 2, 413–427. [Google Scholar] [CrossRef] [Scilit]
- Oruç, S.; Boztepe, C.; Zengin, R. Development electrically conductive PAAm/Alg/CNC/rGO/PANI hydrogel composites and investigation their bioelectronic properties. Mater. Today Commun. 2023, 36, 106540. [Google Scholar] [CrossRef] [Scilit]
- Fayyaz Shahandashti, P.; Pourkheyrollah, H.; Jahanshahi, A.; Ghafoorifard, H. Highly conformable stretchable dry electrodes based on inexpensive flex substrate for long-term biopotential (EMG/ECG) monitoring. Sens. Actuators Phys. 2019, 295, 678–686. [Google Scholar] [CrossRef] [Scilit]
- Zhang, L.; Kumar, K.S.; He, H.; Cai, C.J.; He, X.; Gao, H.; Yue, S.; Li, C.; Seet, R.C.-S.; Ren, H.; et al. Fully organic compliant dry electrodes self-adhesive to skin for long-term motion-robust epidermal biopotential monitoring. Nat. Commun. 2020, 11, 4683. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Wu, B.; Mai, Z.; Ji, Z.; Du, B.; Huang, S.Y. Self-compounded, tough biohydrogels for robust self-adhesive biointerfaces. Mater. Today Phys. 2022, 29, 100905. [Google Scholar] [CrossRef] [Scilit]
- Wang, H.; Du, X.; Liu, N. An electron-ion dual-conductive electrode enables wearable monitoring of electromyography signals. Device 2025, 3, 100563. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.