Nano-yarns Reinforced Silk Fibroin Composites Scaffold for Bone Tissue Engineering

,
,
,
,
,
and
1
Biomaterials and Tissue Engineering Lab, College of Chemistry, Chemical Engineering & Bioengineering, Donghua University, Shanghai 201620, China
2
Petrochemical Research Chair, Department of Chemistry, College of Science King Saud University, Riyadh 11451, Saudi Arabia
3
Department of Chemistry, Faculty of Science, Tanta University, Tanta 31527, Egypt
4
State Key Laboratory of Bioreactor Engineering, East China University of Science and Technology, Shanghai 200237, China

Abstract

In this paper, novel nano-yarn reinforced scaffolds were fabricated and further biomineralized by submerging in 10×Simulated Body Fluid (SBF). The compressive strength of P(LLA-CL)/Silk Fibroin (SF) nano-yarns reinforced scaffold was 1.72±0.50 MPa and its porosity is 82.8%. Fourier Transform Infrared Spectrum (FTIR) and X-ray Diffraction (XRD) data confirmed the mineral phase was made of Hydroxyapatite (HA). MC3T3-E1 cell proliferation and differentiation on the scaffolds were evaluated. In vitro biological evaluation showed that HA coated scaffolds provided higher cell proliferation efficiency (t-test, P < 0.05) than uncoated scaffolds.

1. Introduction

Tissue engineering is considered as a promising alternative therapy to bone defects. The basic strategy of tissue engineering is to fabricate a scaffold to mimic the nature Extracellular Matrix (ECM) [1]. Bone ECM is a kind of hierarchically structured organic–inorganic composite, which consists of collagen fibrils embedded with nanoscopic Hydroxyapatite (HA) crystals [2]. From the bionic aspect, nanofiber is the nearest approach to morphology of bone ECM. Apart from that, a successful scaffold for bone tissue engineering should be i) three dimensional (3D), ii) have interconnected porous network, [3] iii) possess sufficient strength, iv) be biocompatible and osteoconductive [4].
Liquid-electrospinning first reported by Teo [5] is a new way to fabricate continuous nano-yarns. Nano-yarns are a new type of yarns that consists of nanofibers. On the basis of summarizing forefathers, we added several improvements on its roller to obtain a layer-by-layer 3D nanoyarn structure. We anticipated that modified 3D assembly nanoyarns would mimic the macrostructure of bone with nanofiber components. A certain level of mechanical strength is necessary for the growth of a new bone [6]. However one drawback of nanoyarns is that their cotton-like structure is too soft to counteract the effects of stress in the hard tissue. As we know, fiber reinforce is an effective method to increase the strength of materials. In this study, we introduce nanoyarns into nature protein matrix to give the fiber reinforced scaffolds to solve this problem.
Osteoconduction is an essential element for bone tissue regeneration, an osteoconductive scaffold, such as a scaffold with apatite surface, can promote the formation of a new bone [3,7]. By soaking the scaffolds in the Simulated Body Fluid (SBF), apatite calcium phosphates would deposit the scaffolds ranging from a few days to 2 weeks [8]. To speed up the process, we adopted a 10×SBF to increase the mineral content deposited on the scaffolds.
Silk Fibroin (SF) has favorable physical characteristics, due to its β-sheet (crystalline)-rich structure and excellent biocompatibility [9]. Poly(l-lactide-co-e-caprolactone) (P(LLA-CL)) has both good biocompatibility and slower degradation rate [1]. In this study, P(LLA-CL) and P(LLA-CL)/SF nanoyarns were fabricated by modified liquid-electrospinning, they were then combined with SF to give the fiber reinforced novel scaffold by freeze-drying. These scaffolds were then biomineralized by submersion in 10×SBF. Scanning Electron Microscope (SEM), Fourier Transforms Infrared Spectrum (FTIR) and X-ray Diffraction (XRD) were used to test the chemical properties of the bioceramic phase. Morphology, proliferation of MC3T3-E1 pre-osteoblasts on these scaffolds were investigated in vitro.

2. Experimental

2.1. Materials

A copolymer of P(LLA-CL) (75:25), which has a composition of 75 mol% L-lactide, was supplied by Nara University (Japan). Cocoons of Bombyx mori silkworm were kindly supplied by Jiaxing Silk Co., Ltd. (China). The silk fibroin was prepared as an earlier published procedure [10].

2.2. 3D Composite Scaffolds Fabrication

SF (8 wt%) and P(LLA-CL) (8 wt%) were dissolved respectively in 1, 1, 1, 3, 3, 3, -hexafluoro-2 (HFIP, Daikin Industries Ltd, Japan). After SF and P(LLA-CL) completely dissolved, the two solutions were mixed together in different proportions (v/v) of 0:100 and 50:50 whilst being constantly stirred overnight.
These prepared solutions were used for nanoyarn fabrication by the methods showed in Fig. 1. Step 1 – Nanoyarns fabrication with a modified liquid-electrospinning method. In brief, electrospinning was carried out above the water cycling system consisted of two receptacles up and down, a pump used to recirculate the water from the down one to the up one (a hole of diameter 8 mm was drilled in the up one) and a seven-pin plug-like roller rotating in the down flowing water at a lower speed to collect nanoyarns. Irregular nano-yarns were intertwined layer-by-layer across the roller. Pure P(LLA-CL) nanoyarns and P(LLA-CL)/SF nanoyarns were fabricated and respectively submerged in excess water pre-frozen at −80 °C then lyophilized for 24 h in a freeze-dryer (Christ, Alpha 1-2LD, Germany) to keep their original structure. Step 2 is the fiber reinforced scaffold fabrication. The two kinds of nanoyarns were added into Teflon molds containing SF solutions (6 wt%) and pre-frozen in a fridge at −80 °C before transferring to the freeze drier. Samples were freeze-dried for 24 h. Finally, the resulting composites were exposed to 75% ethanol vapor for 6h to transfer the water soluble SF into water insoluble SF.
Figure 1. “Two steps method” of the fabrication of the 3D composite scaffolds: Step 1. Nanoyarns fabrication by modified liquid-electrospinning; Step 2. Fiber reinforced scaffold fabrication. Moving scaffold from the roller after freeze-drying.

2.3. Scaffold Biomineralization

The scaffolds were biomineralized by submersion in 10×Simulated Body Fluid (SBF) as previously reported by Beskardes et al [11]. The 10×SBF was prepared by sequentially dissolving reagent grade substances in the following order: NaCl (1000 mM), KCl (5 mM), CaCl2·2H2O (25 mM), MgCl2·6H2O (5 mM) and NaH2PO4·H2O (3.62 mM) in deionized (DI) water. Before the scaffolds biomineralization, NaHCO3 (10 mM equivalent) was added during stirring. The 10×SBF solution was capped in 100 ml glass bottles for using. The scaffolds were respectively immersed in the SBF for 20 h at room temperature and then rinsed with amounts of DI water to remove the salt residues.

2.4. Characterization

Phase identification of the bioceramic coating layer was done by the examination of X-ray Diffraction (XRD) analysis conducted using a D/Max-2550 PC X-ray diffractometer (Rigaku, Japan) with Cu Ka radiation. Fourier Transform Infrared Spectroscopy (FTIR) (Avatar 380 FTIR, Thermo Electron, Waltham, MA) was used to determine the chemical structure of the scaffolds after soaking in 10×SBF solution in the range 4000∼600 cm−1 wavenumbers.
The morphology of modified liquid-electrospun nano-yarns reinforced composite scaffolds. The ceramic phase on composite scaffolds was observed by TM-1000 (Hitachi, Japan) Scanning Electron Microscope (SEM) at an accelerated voltage of 10 KV. The Ca/P ratios of the coatings were evaluated by an Energy-dispersive X-ray spectroscopy (EDX) system attached to the SEM system.
Porosity of 3D composite scaffolds was measured by liquid displacement method [12]. Hexane was used as the displacement liquid because it is a non-solvent for silk and P(LLA-CL) hence will not cause silk swelling or shrinkage. Firstly, the scaffold was immersed in a known volume (V1) of hexane in a cylinder for 5 min. The total volume of hexane and hexane-impregnated scaffold was recorded (V2). The volume difference (V2 −V1) is the volume of the composite scaffold. Secondly, the hexane-impregnated scaffold was removed from the cylinder scaffold and the residual hexane volume was recorded (V3). The porosity of the scaffold (ε) was obtained by:
ε(%) = (V1 − V3)/(V2 − V3)

2.5. Mechanical Properties

The compression modulus of the scaffolds was evaluated at room temperature on an electronic universal material testing machine with a 100N load cell (WDW3020, Changchun, China). The scaffolds were cut into 18 mm in diameter and 10 mm in height prior to testing. The cross-head speed was set at 1 mm/min. The compressive stress and strain were determined (six samples per group). The compressive modulus was calculated from the slope of the initial linear portion of the compression test.

2.6. Cell Culture on Scaffolds

Mouse pre-osteoblastic cells (MC3T3-E1) (Type Culture Collection of the Chinese Academy of Sciences, Shanghai, China) were cultured in Alpha Minimum Essential Medium containing 10% fetal bovine serum and 1% streptomycin/penicillin and maintained at 37 °C in a CO2 incubator. The media were changed every other day.
The scaffolds were cut 1 mm in height, 14 mm in diameter and placed into 24-well plates. The samples were sterilized in 75% ethanol for 2 h, then washed with PBS and soaked in a cell culture medium overnight. MC3T3-E1 were seeded at a density of 1.0×104 cells per well on different scaffolds. After 24h, the media were supplemented with 10 mM β-glycerol phosphate and 50 mg/ml L-ascorbic acid (Sigma, St. Louis, MO). Cells were cultured for a period of 21 days. Cell viability was measured by cell proliferation assay (MTS Assay) on days 3, 7, 14, and 21 separately. The plate was read at the absorbance of 570 nm using an enzyme-labeled instrument (MK3, Thermo, USA).
Cell morphology and the interaction between cells and scaffolds were studied by SEM on the 14th day. After the culture media was removed, the scaffolds were gently washed with PBS and cells were fixed with 4% (v/v) paraformaldehyde solution for 30 min at 4 °C. Then the scaffolds were dehydrated at the gradient ethanol with concentrations of 30, 50, 70, 90, and 100% (v/v) respectively before being dried. After the scaffolds were completely dried, they were coated with a gold-palladium layer prior to SEM analysis.

3. Results and Discussion

3.1. Scaffold Preparation

6 wt% SF water solution was pre-frozen at −80 °C and then lyophilized for 24 h in a freeze-dryer to make SF sponge, which was named as SF. P(LLA-CL) nanoyarns fabricated by modified liquid-electrospinning was added into 6% SF solutions, pre-frozen in a fridge at −80 °C and then lyophilized to give a P(LLA-CL) nanoyarns reinforced scaffold named as PLCL-R-SF. P(LLA-CL)/SF. Nanoyarns reinforced scaffolds were fabricated with the same method, which is named as PLCL/SF-R-SF. The three different scaffolds were exposed to 75% ethanol vapor before biomineralization. After being biomineralized by submersion in 10×SBF, they were marked as SF-HA, PLCL-R-SF-HA and PLCL/SF-R-SF-HA respectively.

3.2. Morphology, Porosity and Mechanical Properties

Fig. 2 shows cross section SEM image of SF (a), PLCL-R-SF (b) and PLCL/SF-R-SF (c). It could be seen that both P(LLA-CL) nanoyarns and P(LLA-CL)/SF nanoyarns well-distributed in the SF sponge structure and the pores were interconnected. Pore size was decreased by adding fiber reinforcements.
Figure 2. SEM images of SF (a), PLCL-R-SF (b) and PLCL/SF-R-SF (c) the scale bar equals 100 µm. (d), (e) and (f) are high magnification of (a), (b) and (c). Scale bar indicates 25 µm.
Table 1 shows the porosity variation for different scaffolds, highest porosity of 86.28% was observed in pure SF, which reduced to 84.97 and 82.82% in case of combining P(LLA-CL) nanoyarns reinforcement and P(LLA-CL)/SF nanoyarns reinforcement.
Table 1. Porosity and mechanical properties of the scaffolds. Data shown are mean ±SD, n = 6.
Table 1 shows the mechanical properties for different scaffolds. The profiles of the stress-strain curve of different scaffolds are displayed in Fig. 3. It can be seen that nanoyarns reinforced scaffold give higher compressive modulus than non-reinforced SF scaffold. The compressive modulus of the non-reinforced SF scaffold was only 0.98±0.23 MPa while it increased to 1.170±0.16 MPa for PLCL-R-SF scaffold and it reached to 1.72±0.50 MPa for PLCL/SF-R-SF scaffolds. It could be seen that the compressive modulus of PLCL/SF-R-SF were nearly twice as much as that of pure SF with little decrease of porosity. Nanoyarns as reinforcement were effective to prepare porous scaffold with certain strength. This result was in agreement with previous reports [13]. As PLCL/SF nanofibers have stranger tensile modulus than PLCL nanofibers [14], so that the PLCL/SF nanoyarns reinforced scaffold (PLCL/SF-R-SF) has higher compressive modulus than PLCL nanoyarns reinforced scaffold (PLCL-R-SF).
Figure 3. Stress-strain curve of SF, PLCL-R-SF and PLCL/SF-R-SF.

3.3. Characterization of Biomineralized Composites

Apatite formation is a complex process that involves nucleation and growth of the apatite [15]. In this study, a 10×SBF solution was used for apatite deposition. After soaking the scaffolds of SF, PLCL-R-SF and PLCL/SF-R-SF in 10×SBF separately for 20h, we got the apatite deposited scaffolds. Fig. 4 shows the SEM micrographs of the apatite deposited scaffolds, SF-HA (Fig. 4 (a)), PLCL-R-SF-HA (Fig. 4 (b)) and PLCL/SF-R-SF-HA (Fig. 4 (c)). Crystalline particles had significantly increased to cover all the surface of the scaffolds respectively after 20 hours of soaking. Fig. 4(d) showes the spherical HA covered on the surface of scaffold at high magnification. The EDS analysis (Fig. 5) showes that the apatite deposited on the SF-HA scaffolds has a Ca/P ratio of about 1.56, which is similar to the ratio of 1.67 seen in stoichiometric hydroxyapatite, indicating that the particles consists of calcium and phosphorus.
Figure 4. SEM micrographs of SF-HA (a), PLCL-R-SF-HA (b), PLCL/SF-R-SF-HA (c), High magnification of graph a (d).
Figure 5. EDS analysis of apatite particles on SF-HA.
Fig. 6 shows the FTIR spectra of apatite deposited scaffolds (SF-HA, PLCL-R-SF-HA, PLCL/SF-R-SF-HA) and commercial HA. FTIR spectra of the commercial HA (Fig. 6-(1)) displays characteristic absorption bands at 962 (ν1), 472 (ν2), 1038 (ν3), 564 and 602 (ν4) cm−1, which was assigned to PO4 [16]. FTIR spectra of the apatite deposited scaffolds in Fig. 6-(2), Fig. 6-(3) and Fig. 6-(4) have displayed characteristic absorption bands at 603, 562, 563 cm−1 (P–O bending) corresponding to the group in commercial HA, that means apatite were deposited on the scaffolds. Fig. 7 shows that the XRD pattern of apatite deposited scaffolds (SF-HA, PLCL-R-SF-HA, PLCL/SF-R-HA) and commercial HA. It also can be seen that the apatite crystals peek at 26° and 32° appeared in the scaffolds, which are typical “apatitic CaP” [17,18].
Figure 6. FTIR of apatite deposited scaffolds and commercial HA.
Figure 7. XRD profiles of SF-HA, PLCL-R-SF-HA and PLCL/SF-R-SF-HA compared with commercial HA.

3.4. Adhesion and Proliferation Behavior of MC3T3-E1 Cells

Fig. 8 shows the MTT assay of MC3T3-E1 cells proliferation on the non-biomineralized and biomineralized scaffolds. For the biomineralized scaffolds, we can see that the cell number leveled off on the SF-HA, PLCL-R-SF-HA and PLCL/SF-R-SF-HA from days 3 to 7. Previous studies showed that HA surface at a nanometer level could decrease osteoblast-like cells on early period of proliferation [19]. Biomineralized PLCL-R-SF-HA and PLCL/SF-R-SF-HA scaffolds had a significant improvement in the cell number on day 21 (p < 0.05) compared to non-mineralized PLCL-R-SF and PLCL/SF-R-SF, suggesting that the apatite surface contributes to cell proliferation on later period. For the non-biomineralized scaffolds, SF, PLCL-R-SF and PLCL/SF-R-SF, there was no significant difference in cell number from days 3 to 21. After 21 days of cultivation, cell number of MC3T3-E1 cultivated on PLCL-R-SF-HA and PLCL/SF-R-SF-HA scaffolds is higher than on SF-HA scaffold. That means nanoyarns in the scaffold enhanced the cell proliferation. The nanoyarn reinforced composite may provide favorable conditions for cell anchorage and growth. Comparing the block structure of SF, nanoyarn has a crude surface and greater capability of cell seizing. Only the cells adhered to the scaffolds can proliferate effectively.
Figure 8. MC3T3-E1 cells proliferation on the non-mineralized and mineralized SF, PLCL-R-SF and PLCL/SF-R-SF.Data represented as mean±standard deviation with n = 3(∗p < 0.05).
Fig. 9 shows the SEM micrographs of MC3T3-E1 cells proliferation on biomineralized and non-biomineralized scaffolds. It can be seen the cells adhere to nanoyarns regions more than to SF blocks regions (Fig. 9 (b,e–g)), that means the electrospun nanoyarns are more appropriate for cell proliferation and migration. Cells still keep a cuboidal cellular morphology on the pure SF scaffold (Fig. 9 (c)) compare with biomineralized SF (Fig. 9 (d)).
Figure 9. SEM micrographs of MC3T3-E1 cells proliferation on PLCL-R-SF. (a) At low magnification of ×300 and (b) At high magnification of ×1000; (c) On SF, (d) SF-HA, (e) PLCL-R-SF, (f) PLCL-R-SF-HA, (g) PLCL/SF-R-SF, (h) PLCL/SF-R-SF-HA.

4. Conclusion

In this study modified liquid-electrospun was used to fabricate novel P(LLA-CL) and P(LLA-CL)/SF nanoyarns, which was then dipped in SF solution and further freeze-dried to give the nanoyarns reinforcement scaffolds. Those scaffolds were further biomineralized. FTIR and XRD analyses illustrated that the apatite were deposited on the scaffolds. Biomineralization had enhanced the MC3T3-E1 cells proliferation on the scaffolds after 21 days of culturing. On reinforcement scaffolds, cells adhered to nanoyarns regions prior to SF blocks. We speculate that electrospun nanoyarns are more appropriate for cell proliferation and migration. All these results suggest that novel composites have potential as bone tissue engineering scaffolds.

Acknowledgments

This research was Supported by Open Funding Project of the State Key Laboratory of Bioreactor Engineering, China, National High Technology Research and Development Program (863 Program, 2008AA03Z305), Science and Technology Commission of Shanghai Municipality Program (11nm0506200), National Nature Science Foundation of China (31070871) and The National Plan for Science and Technology Project (10- NAN1013-02).

References

  1. Mo, X.M.; Xu, C.Y.; Kotaki, M.; Ramakrishna, S. Electrospun P(LLA-CL) nanofiber: a biomimetic extracellular matrix for smooth muscle cell and endothelial cell proliferation. Biomaterials 2004, 25, 1883–1890. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  2. Olszta, M.J.; Cheng, X.; Jee, S.S.; et al. Bone structure and formation: A new perspective. Mater. Sci. Eng. R 2007, 58, 77–116. [Google Scholar] [CrossRef] [Scilit]
  3. Tang, Y.W.; Eng, M.; Wong, C.; et al. Three-Dimensional Tissue Scaffolds from Interbonded Poly(e-Caprolactone) Fibrous Matrices with Controlled Porosity. Tissue Eng. Part C 2011, 17, 209–218. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  4. Rockwood, D.N.; Gil, E.S.; Park, S.H.; et al. Ingrowth of human mesenchymal stem cells into porous silk particle reinforced silk composite scaffolds: An in vitro study. Acta Biomater. 2011, 7, 144–150. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  5. Teo, W.E.; Gopa, R.; Ramaseshan, R.; et al. A dynamic liquid support system for continuous electrospun yarn fabrication. Polymer 2007, 48, 3400–3405. [Google Scholar] [CrossRef] [Scilit]
  6. Turner, C.H.; Robling, A.G. Designing exercise regimens to increase bone strength. Exerc. Sport Sci. Rev. 2003, 31, 45–50. Available online: http://www.scopus.com/authid/detail.url?origin=resultslist&authorId=6701795966. [PubMed]
  7. Shi, X.D.; Jiang, J.; Sun, L.; et al. Hydrolysis and biomineralization of porous PLA microspheres and their influence on cell growth. Colloids Surf. B Biointerfaces 2011, 85, 73–80. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  8. Mavis, B.; Demirtas, T.T.; et al. Synthesis, characterization and osteoblastic activity of polycaprolactone nanofibers coated with biomimetic calcium phosphate. Acta Biomaterialia 2009, 5, 3098–3111. [Google Scholar]
  9. Li, M.Z.; Tao, W.; Lu, S.Z.; et al. Porous 3-D scaffolds from regenerated Antheraea pernyi silk fibroin. Polym. Adv. Tevhnologies 2008, 19, 207–212. [Google Scholar] [CrossRef] [Scilit]
  10. Nazarov, R.; Jin, H.J.; Kaplan, D.L. Porous 3-D Scaffolds from Regenerated Silk Fibroin. Biomacromolecules 2004, 5, 718–726. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  11. Beskardes, I.G.; et al. Biomimetic Apatite-coated PCL Scaffolds: Effect of Surface Nanotopography on Cellular Functions. J. Bioact. Compat. Polym. 2009, 24, 507. [Google Scholar] [CrossRef] [Scilit]
  12. Zhang, R.Y.; Ma, P.X. Poly(alpha-hydroxyl acids) hydroxyapatite porous composites for bone-tissue engineering. I. Preparation and morphology. J. Biomed. Mater. Res. 1999, 44, 446–455. [Google Scholar] [CrossRef]
  13. Wang, J.; Sun, Q.Z.; Gao, J.; et al. Preparation and Properties on Silk Fibers Reinforced Hydroxyapatite/Chitosan Composites. Adv. Mater. Res. 2010, 105, 557–560. [Google Scholar] [CrossRef] [Scilit]
  14. Zhang, K.H.; Wang, H.S.; Huang, C.; Su, Y.; Mo, X.M.; Ikada, Y. Fabrication of silk fibroin blended P(LLA-CL) nanofibrous scaffolds for tissue engineering. J. Biomed. Mater. Res. A 2010, 93(3), 984–993. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  15. Tanahashi, M.; Matsuda, T. Surface functional group dependence on apatite formation on selfassembled monolayers in a simulated body fluid. J. Biomed. Mater. Res. 1997, 34, 305–315. [Google Scholar] [CrossRef] [Scilit]
  16. Yang, F.; Wolke, J.G.C.; Jansen, J.A. Biomimetic calcium phosphate coating on electrospun poly(ε-caprolactone) scaffolds for bone tissue engineering. Chem. Eng. J. 2008, 137, 154161. [Google Scholar] [CrossRef] [Scilit]
  17. Takeuchi, A.; Ohtsuki, C.; Miyazaki, T.; et al. Deposition of bone-like apatite on silk fiber in a solution that mimics extracellular fluid. J. Mater. Sci. Mater. Med. 2003, 14, 569–74. [Google Scholar]
  18. Kawai, T.; Ohtsuki, C.; Kamitakahara, M.; et al. Coating of an apatite layer on polyamide films containing sulfonic groups by a biomimetic process. Biomaterials 2004, 25, 4529–4534. [Google Scholar] [CrossRef] [Scilit] [PubMed]
  19. Wei, K.; Li, Y.; Kim, K.O. Fabrication of nano-hydroxyapatite on electrospun silk fibroin nanofiber and their effects in osteoblastic behavior. J. Biomed. Mater. Res. 2011, 97, 272–280. [Google Scholar] [CrossRef] [Scilit] [PubMed]

Article Metrics

Citations

Article Access Statistics

Multiple requests from the same IP address are counted as one view.