Abstract
The fracturing process in fibre-reinforced brittle-matrix composites subjected to monotonic loading or low-cycle fatigue is strongly affected by the matrix damage mechanism together with the bridging action of the reinforcing fibres, including their plastic shake-down and hysteresis. The monotonic response is also considered, since it represents the envelope of the cyclic response and defines the critical (minimum reinforcement) condition against which the cyclic energy dissipation is assessed. The main features of the structural behaviour in both scenarios are associated with the fibre-reinforcement brittleness number (NP,f), which takes into account the influence of both structural size-scale and fibre volume fraction. In the case of monotonic loading, the brittleness number governs the post-cracking behaviour of the composite in terms of structural stability, which can range from ductile to catastrophic. On the other hand, when cyclic loading is considered, the brittleness number affects the cyclic energy dissipation, defined as the area enclosed by a single hysteretic loop in the load vs. deflection diagram. In the present work, numerical predictions are compared with experimental results, focusing on the evaluation of the hysteretic loops occurring in the structural behaviour of fibre-reinforced concrete beams. In this framework, a parametric study on beams of different depths shows, for the first time, that an optimum value of the reinforcement brittleness number, NP,opt ≈ 0.4, can be identified for the beam depths of 10 and 20 cm, which exhibit a clearly defined maximum of the energy dissipated in the first hysteretic loop, whereas no clear optimum is found for the smallest beam (5 cm), whose dissipated energy is almost insensitive to the brittleness number. This optimum lies below the critical value NPC ≈ 0.7 that governs the ductile-to-brittle transition under monotonic loading. On this basis, the interval NP,opt ≤ NP,f ≤ NPC is proposed as a preliminary criterion for selecting the fibre content of FRC members required to dissipate energy, e.g., under seismic actions. Since the brittleness number already accounts for the structural size, the same optimum value is found for both these beam depths, whereas the corresponding fibre volume fraction decreases with the beam depth.
1. Introduction: Scale Effects and Ductile-to-Brittle Transition in Fibre-Reinforced Concrete
The beneficial effect of adding reinforcing fibres to a concrete matrix is strongly dependent on the ability of the fibres to bridge the faces of cracks nucleating in the brittle matrix. In this context, many experimental studies have been devoted to investigating the enhancement of both the flexural and the shear capacity of fibre-reinforced concrete (FRC) structural elements [1,2,3,4]. The presence of fibres in concrete entails a strong improvement in the flexural capacity of the composite structure, together with a weaker beneficial effect on its shear capacity [5]. As a matter of fact, whilst the increase in flexural performance is related to the fibre bridging action, which is a function of the axial stiffness of the reinforcing layer (proportional to ℓ−1, where ℓ is the fibre characteristic size), the influence on shear capacity is mainly related to the fibre shear stiffness (proportional to ℓ−2).
An effective description of the complete flexural response of fibre-reinforced brittle-matrix composites under monotonic or cyclic loading is provided by the Updated Bridged Crack Model (UBCM) [6,7,8,9,10,11]. The model considers the bridging action of the reinforcing fibres (Figure 1a) and describes the fracturing process that occurs in the matrix, which is assumed to be linear elastic–perfectly brittle [12,13,14,15,16,17]. A suitable cohesive softening constitutive law that accounts for the fibre pull-out from the matrix is used to simulate the damage evolution [18,19].
Figure 1.
Fracturing process in fibre-reinforced brittle-matrix composites subjected to bending (a). Different post-cracking regimes depending on the fibre volume fraction (b).
The UBCM algorithm consists of three sets of equations (elastic, constitutive, and crack propagation equations), the solution of the structural problem being given by a system of (2n + 1) equations in (2n + 1) unknowns. In particular, n elastic equations are defined [6,8,15]:
where M denotes the bending moment due to the applied load, Fi are the bridging forces provided by the n fibre-reinforcements (Figure 1a), and λM and [λ] are the local compliances associated with the bending moment and with the bridging forces, respectively [6]. Then, n constitutive equations are introduced:
which describe the bridging action of the fibre distribution (Figure 1a) as a function of the n crack opening displacements, wi [8]. Finally, one crack propagation equation is imposed [6,8]:
where, in the framework of Linear Elastic Fracture Mechanics (LEFM), KIM is the stress-intensity factor due to the bending moment M, KIi is the stress-intensity factor due to the bridging action of the i-th fibre [8], and KIC is the fracture toughness of the brittle matrix. Hence, the crack length is the driving parameter of the structural problem.
On the other hand, the (2n + 1) unknowns involved in the structural problem are: n bridging forces, Fi, n crack opening displacements, wi, and the bending moment of crack propagation, MF.
It is noteworthy that, given a general loading history that can be split into distinct growing or decreasing phases, the case of low-cycle fatigue may be derived as an extension of the above-mentioned single phases [20]. In this way, when the unloading process is considered, the UBCM makes it possible to capture both elastic and plastic shake-down conditions of the reinforcing fibres. As extensively reported in [15,21], the plastic shake-down phenomenon is responsible for the hysteretic loops occurring in the structural response, together with the related energy dissipation.
From the numerical point of view, the fibres crossing the critical cross-section are represented by n bridging forces, evenly spaced along the ligament between the relative heights ζmin = a0/h (notch tip) and ζmax = 0.99, ζ being the distance from the bottom edge of the beam divided by h, with n = αVfbh/Afib, where Afib is the cross-sectional area of a single fibre and α is the orientation factor, i.e., the ratio between the actual and the theoretical number of fibres crossing the critical section [8,14]. Therefore, n is not a free parameter of the model, but follows from the fibre volume fraction and the cross-section geometry. The crack length control scheme is adopted: the crack depth, a, is increased step by step from the initial notch depth, a0, up to the complete disconnection of the cross-section (a → h). For each crack depth, the fibres are subdivided into three groups, i.e., fibres at which the crack is still closed (wi = 0), fibres undergoing pull-out (Fi = F(wi)), and fibres whose bridging action is exhausted (Fi = 0); Equations (1)–(3) are then solved iteratively, updating the three groups until all the constitutive conditions are satisfied, and the bending moment of crack propagation, MF, is obtained from Equation (3) [8]. The mid-span deflection is obtained by superposing the contribution of the localized rotation of the cracked cross-section (inelastic hinge) and the elastic deflection of the beam [8,15]. In the case of cyclic loading, the loading history is decomposed into a sequence of monotonic branches (loading, unloading, and reloading), each one starting from the configuration reached at the end of the previous branch [15,20]. Accordingly, Equation (1) is written in incremental form, {w} − {w0} = {λM}(M − M0) − [λ]({F} − {F0}), where the subscript 0 denotes the initial configuration of the current branch [15]. At the onset of unloading, the fibres respond rigidly, i.e., the crack opening at each fibre level remains unchanged, until the bridging force reaches the compressive value −FP, which triggers the reverse slippage of the fibre at constant force; upon reloading, the fibres respond rigidly again until the monotonic envelope is reached [15]. For the comparison with experimental tests, each loop is defined by the extreme values of load and deflection recorded in the experiments [15].
The main characteristics of the structural response in both scenarios—that is, under monotonically increasing or cyclic loading—are associated with the fibre-reinforcement brittleness number, NP,f. This dimensionless number depends on the following parameters: fibre volume fraction (Vf), element depth (h), fibre equivalent strength (σu), and matrix fracture toughness (KIC), as follows:
In Equation (4), σu is the equivalent strength of the fibre reinforcement. Although it nominally depends on several factors, such as fibre anchorage, orientation, and distribution (coefficients α and β), it is here considered as a parameter obtained directly from the behaviour of the structure by means of material identification, i.e., inverse analysis [8,14,15], as discussed in Section 4. Hence, σu should not be confused with the nominal tensile strength of the fibre material, fu. The composite post-cracking behaviour can range from ductile to brittle, depending on the brittleness number. This allows for the definition of a critical value of the reinforcement brittleness number, NPC, which represents the limit between stable and unstable post-elastic regimes (Figure 1b) [8,14,22,23,24,25,26].
The above-mentioned limit condition is reached when the first-cracking load (concrete matrix) is equal to the ultimate load (fibre slippage or flow). Thus, the bending moment of ultimate collapse, Mu, and that of first cracking, MF, can be defined as:
where Af is the reinforcement area, b is the thickness of the beam, and f is a nondimensional weight function according to LEFM [8]. Therefore, the non-integer power characterizing the beam depth, h, in Equation (4) derives from the dimension mismatch between the two generalized forces represented by strength and toughness: and .
The scaling problem is governed by the variation in beam depth, h, considering as constant the beam thickness, b, and the relative crack depth, a/h. The minimum area of fibre-reinforcement, Af,min, is given by the condition MF = Mu [7,8], preventing any potential losses in the structural load-bearing capacity and ensuring a stable post-elastic behaviour:
Then, the corresponding fibre volume fraction follows as
Therefore, the minimum fibre volume fraction, Vf,min, should not be regarded as a constant, since it varies with the structural size-scale, more precisely according to the power law h−1/2 (LEFM singularity).
By considering Equations (5), (6) and (8), the following relationship is obtained [7,8,14]:
where the right-hand side represents a nondimensional weight function, whereas the left-hand side is the fibre-reinforcement brittleness number NP,f [6,7,14].
On the other hand, the dimensionless number NP,f can also be obtained by applying Buckingham’s Π-theorem for physical similitude [27]. In particular, the following functional relationship, F, can describe the fracturing process in fibrous composites [14,27]:
in which the following quantities appear: the bending moment of crack propagation, MF, the corresponding localized rotation, φ, the fracture toughness, KIC, the matrix elastic modulus, E, the fibre volume fraction, Vf, the fibre equivalent strength, σu, the fibre distribution coefficients, α and β, the critical crack opening (i.e., the fibre embedment length), wc, the beam thickness, b, the beam depth, h, and the initial notch, a0.
F (MF, φ; KIC, E; Vf, σu, α, β, wc; b, h, a0) = 0,
Given the force [F] and the length [L] as the fundamental physical dimensions involved in the problem, if the fracture toughness, KIC, and the structural size, h, are assumed as dimensionally independent variables, the application of Buckingham’s Π-theorem [27] yields the following relationship among dimensionless groups:
in which only dimensionless quantities appear.
Then, for a given geometry, a further reduction can be obtained:
which shows that the structural response depends on the two dimensionless numbers and , the latter being the pull-out brittleness number, which describes the plastic rotation capacity of the structure [8].
Thus, Equation (9) can be associated with the ductile-to-brittle transition condition, which defines the minimum amount of fibres required for a beam to exhibit a stable load-bearing capacity:
where NPC is the critical value of the reinforcement brittleness number, which, for FRC, may vary between 0.7 and 1.3 depending on the initial notch depth [8].
It should be noted that the minimum reinforcement condition for FRC is not constant: as discussed above, it depends on the structural size, following the power law h−1/2. An alternative definition of the critical fibre volume fraction, based on the ductility index of FRC beams, has been proposed by Fantilli et al. [28,29].
The RILEM Recommendations for the design of FRC structures [30] include an interesting attempt to account for size-scale effects. The residual flexural stresses are adjusted by a coefficient that decreases with the increase in specimen size and are evaluated at a specific value of crack mouth opening displacement. In fact, this approach corresponds to the simple scaling law of strength [31], and it may be quantitatively assessed using the Multifractal Scaling Law for originally uncracked specimens [32,33].
According to Equation (13), the fibre volume fraction needed to satisfy the minimum reinforcement condition decreases with increasing beam size (Figure 2), in contrast with the provisions of current standards and technical documents [34,35]. In particular, following CNR-DT 204/2006 (Italy) [34], for structural use a minimum fibre dosage must be guaranteed, not less than 0.3% by volume (Figure 2). In addition, the Italian Circolare n. 7/2019 (NTC 2018) [36] takes the same 0.3% minimum, citing CNR-DT 204/2006. Finally, the 2021 Italian Ministry guidelines on FRC qualification [37] repeat it: besides minimum performance requirements, structural FRC must contain not less than 0.3% by volume of fibres. A close analogue is represented by ACI 318 (USA) [38]. Since the 2008 edition, ACI 318 has allowed SFRC to replace conventional shear reinforcement (stirrups) in beams, but such beams must contain at least 0.75% steel fibres by volume, i.e., 60 kg/m3. It is a single size-independent value, like the one by CNR-DT 204/2006, but it applies to minimum shear reinforcement instead of flexural minimum reinforcement. Therefore, the ACI 318 provision addresses a different structural mechanism and is not directly equivalent to the flexural minimum reinforcement condition of Equation (13): it is shown in Figure 2 only as an example of a size-independent prescription. Similarly, Annex L of the new Eurocode 2 (EN 1992-1-1:2023), which introduces European design provisions for steel-fibre-reinforced concrete structures [39,40], expresses the ductility requirement for SFRC as a minimum ratio, equal to 0.5, between the characteristic residual flexural strength and the characteristic tensile strength of concrete, again regardless of the structural size.
Figure 2.
Size-scale effect on the minimum fibre volume fraction in FRC beams: Comparison between the Italian standard Circolare n. 7/2019 (NTC 2018), the American standard ACI 318/2008, and the UBCM. The ACI 318 value refers to the size-independent replacement of the minimum shear reinforcement.
In this context, both the RILEM Recommendations [30] and the fib Model Code 2010 [41], recently superseded by the fib Model Code 2020 [42], show a significant lack of information: for hybrid-reinforced structures, they merely recognize that fibres allow a reduction in the minimum bar-reinforcement percentage needed to limit the crack width at the Serviceability Limit State. Conversely, no indication is given of the fibre volume fraction required to achieve a stable post-cracking behaviour at the Ultimate Limit State. In neither case is Vf,min quantitatively determined. Therefore, the size-dependence of the minimum fibre volume fraction, highlighted by the application of the UBCM under static loading [10,12,16,17], deserves consideration in future revisions of national and international codes of practice (Equation (13)).
On the other hand, when cyclic loading is considered, the brittleness number affects the residual crack opening [43] and the cyclic energy dissipation, which can be defined as the area enclosed by a single hysteretic loop.
Previous studies by the authors have established the role of NP,f in the post-cracking regimes and in the size effects of FRC beams under monotonic loading, including the definition of the critical value NPC [8,14], and have shown that the UBCM captures the plastic shake-down of the fibres and the hysteretic loops of FRC beams subjected to ultra-low-cycle fatigue [15,21]. However, the dependence of the hysteretic energy dissipation on the brittleness number, and therefore on structural size and fibre volume fraction, has not been investigated so far. The original contributions of the present work are as follows: (i) the hysteretic energy dissipated by FRC beams tested in four experimental campaigns available in the literature is evaluated and correlated with NP,f (Section 4); (ii) a parametric study on beams of different depths shows the existence of an optimum value of the brittleness number, NP,opt, at which the hysteretic energy dissipation is maximum, which has never been reported before (Section 5); (iii) NP,opt is compared with the critical value NPC governing the monotonic response, and the interval between the two values is discussed as a preliminary criterion for the selection of the fibre content. In this framework, the monotonic response is recalled not as an object of study in itself, but because it provides the envelope of the cyclic response and the reference condition, NPC, for the interpretation of the energy-based optimum.
2. Cyclic Loading: Plastic Shake-Down and Hysteresis
Let us consider, following the classical treatment of plastic shake-down reported in [44,45], a system of parallel elastic–plastic rods connected by a rigid cross member (Figure 3), simulating a distribution of internal reinforcements, and let us suppose that the system is loaded repeatedly with a pulsating force within the elastic limit, σP being the yield stress of the rods:
Figure 3.
System of parallel elastic–plastic rods connected by a rigid cross member.
For greater values of the maximum load F, the central rod yields, so that, on unloading, this rod is found to be compressed by the lateral ones, which are assumed to obey an elastic constitutive law, devoid of yielding. Under these hypotheses, a value FSD of the load is shown to exist, such that the central rod also yields in compression. When the external force is maximum, the equilibrium of the cross member gives
whereas, when the external force is zero, it gives
When the external force is maximum, the dilation of the central rod is
and hence
since the lateral rods are in elastic conditions.
On the other hand, when the external force is zero and at the onset of inverse plastic deformation, the dilation of the central rod is
Since it is also found that
by transitivity, it follows that
Thus, the reaction of the lateral rods at the maximum load is deduced as
The equilibrium of the rigid cross member yields
The hypothesis of inverse plastic deformation of the central rod gives
so that
Thus, it follows that
Since at maximum load the central rod has yielded, it follows that
Finally, the force of inverse plastic deformation is obtained
or
The inverse plastic deformation of the central rod occurs only for . Note that this threshold load FSD is exactly twice the load of first plastic deformation .
In summary:
- For 0 ≤ F ≤ F1, the system behaves elastically and its representative point in the plane F-δ (Figure 4) oscillates on the segment O1.Figure 4. Shake-down and hysteresis cycle (shaded area) of the rod system.
- For F1 < F ≤ FSD, the central rod yields only in tension and the representative point of the system oscillates on the corresponding segment O′1′ (shake-down).
- For F > FSD, the central rod yields both in tension (loading) and in compression (unloading) and the representative point of the system cyclically traverses the parallelogram SD-A-B-C. More precisely, at the first loading the point moves to A; on subsequent elastic unloading, the point moves to B, where the plastic flow in compression of the central rod starts. This flow ceases at C. From here the second loading cycle begins, which develops first elastically along the segment C-SD, and then plastically along the segment SD-A, and so forth. The energy dissipated in each hysteresis cycle is equal to the area of the parallelogram SD-A-B-C. The phenomenon of plastic dissipation just described is called alternating plastic deformation [45].
The same mechanism can be recognized at the level of a single fibre bridging a crack in a beam segment subjected to a cyclic bending moment, M (Figure 5a), when fibre slippage is described by the linear-softening law F(w) = FP(1 − w/wc). Let MP denote the bending moment at which fibre slippage starts, i.e., the counterpart of the load of first plastic deformation, F1, of the rod system. If the fibre behaved as a rigid-perfectly plastic element, the shake-down moment would be MSD = 2MP, in full analogy with FSD = 2F1. When slippage softening is taken into account, MSD is smaller than 2MP and approaches this limit only for large values of the fibre embedment length, wc (Figure 5b). Moreover, below the threshold value wSD, shake-down cannot occur: every load reversal beyond the onset of slippage produces reverse slippage of the fibre, i.e., alternating plastic deformation and hysteretic energy dissipation [21].
Figure 5.
Single fibre bridging a crack in a beam segment under cyclic bending: (a) scheme and linear-softening slippage law; (b) shake-down moment, MSD, vs. fibre embedment length, wc, for slippage and rigid–perfectly plastic behaviour.
3. Crack Opening and Closure in Fibre-Reinforced Concrete Subjected to Cyclic Loading
In the following, the hysteretic behaviour of an FRC beam is analysed by means of the UBCM. The analyses in this section are theoretical and are carried out in nondimensional form: according to Equation (12), the response depends only on NP,f and Nw, so that the results apply to any beam characterized by the same dimensionless numbers. The two values NP,f = 1.0 and NP,f = 0.4 are selected as representative of the hardening (NP,f > NPC) and softening (NP,f < NPC) regimes, respectively. The comparison with experimental results is presented in Section 4. In the first case, the fibre-reinforcement brittleness number is set equal to NP,f = 1.0, which produces a hardening post-elastic behaviour of the structural element [8]: if the process is controlled by loading (black curve in Figure 6), snap-through instabilities appear, subtending the local softening responses (red curve in Figure 6), which can be captured only by the crack length control [6,7,8,12,13,14,15]. Furthermore, the phenomenon of plastic shake-down resulting from slippage of the fibre-reinforcements may be identified. Accordingly, the dimensionless moment vs. rotation diagram of the beam cross-section illustrates a hysteretic loop, allowing the evaluation of the energy dissipation as the area enclosed by the hysteretic cycle.
Figure 6.
Nondimensional moment vs. rotation diagram for an FRC beam with NP,f = 1.0. Red curve: Crack length control scheme; Black curve: Loading control; Blue circle: Fibre slippage.
It is worth recalling that, until the fibre pull-out strength is reached, the fibre bridging action keeps the crack closed at each fibre level. Then, if the test is controlled by the load, snap-through phenomena cause the crack to propagate by jumping from one fibre to the next. Conversely, during the unloading stage, the fibres act as struts, keeping the crack open until they reach their reverse pull-out limit [46] (see the corresponding constitutive law in Figure 7). Then, the crack opening displacement begins to decrease. At the end of the unloading branch, the crack does not close completely: the crack faces come into contact at the crack mouth, whereas a residual opening persists along the inner part of the crack, where the fibres in reverse pull-out prevent complete closure, giving rise to the almond-shaped profile shown in Figure 8 [43]. A further decrease in the load is not permitted, otherwise an overlapping of the crack faces at the crack mouth would arise.
Figure 7.
Hysteretic behaviour at the single-fibre level (constitutive law): Slippage force vs. crack opening displacement.
Figure 8.
Almond-shaped residual crack opening in the FRC beam subjected to cyclic loading: numerical crack opening profile at the end of the unloading branch, i.e., at φ = φmin in Figure 6 (dimensionless moment −0.36, dimensionless rotation 1.27) [43].
As a second case study, the hysteretic behaviour of an FRC beam with NP,f = 0.4 is analysed by means of the UBCM (Figure 9). If the test is controlled by the beam deflection, a series of load drops appears in the softening post-peak regime (black curve in Figure 9), which subtend the local snap-back branches that can be captured only by the crack length control (red curve in Figure 9). Also in this case, the phenomenon of plastic shake-down due to fibre slippage can be observed, together with the related energy dissipation during hysteresis.
Figure 9.
Nondimensional moment vs. rotation diagram for an FRC beam with NP,f = 0.4. Red curve: crack length control scheme. Black curve: loading control. Blue circle: fibre slippage.
4. Low-Cycle Fatigue in Fibre-Reinforced Concrete
An extensive body of scientific literature is available on the flexural behaviour of FRC structures subjected to monotonically increasing loading, but only a small part of it is devoted to investigating the mechanical response of FRC under repeated loading, or low-cycle fatigue [47,48,49,50,51,52,53,54,55,56,57,58,59,60]. In the present section, the experimental results obtained by Boulekbache et al. [48] on the ultra-low-cycle fatigue behaviour of FRC beams are analysed by means of the UBCM. In that study, three types of matrix—ordinary concrete (OC), self-compacting concrete (SCC), and high-strength concrete (HSC)—were considered, characterized by an average cubic compressive strength of about 30 MPa, 60 MPa, and 80 MPa, respectively. Concerning the reinforcing fibres, two types of hooked-end steel fibres were adopted, with aspect ratios λf = 65 and 80, together with two fibre volume fractions, Vf = 0.50% and 1.00%. These dosages, selected in the original experimental campaign [48], correspond to about 39 and 78 kg/m3 of steel fibres and are representative of the range typically adopted for structural FRC, i.e., above the minimum value of 0.3% prescribed by the Italian provisions [34,36,37] and enclosing the value of 0.75% required by ACI 318 for shear [38]. In total, 12 four-point bending tests were conducted on notched specimens under cyclic loading (Figure 10), consisting of successive loading–unloading cycles at increasing deflection levels up to failure; the complete description of the test setup, loading protocol, and failure patterns is reported in [48]; only the six tests on the fibres with aspect ratio equal to 65 are analysed herein. The geometry of the specimens and the properties of the matrices and fibres are summarized in Table 1 [48]. The fibre bridging action is modelled by a constitutive law that is defined on the basis of single-fibre pull-out tests [19]. This law is defined by the critical crack opening, wc, which represents the slip (or crack opening) beyond which the fibre is completely pulled out of the matrix, its bridging effect being exhausted, and the maximum value of the bridging force, FP, beyond which the fibre pull-out starts. This constitutive law also holds in the compression regime, until the maximum fibre force is attained, which triggers the reverse pull-out of the fibre reinforcement (Figure 7).
Figure 10.
Four-point bending test geometry adopted in [48] (dimensions in mm).
Table 1.
Geometry of the specimens and mechanical properties of the matrices and fibres in the experimental campaign by Boulekbache et al. [48].
In Figure 11a–f, the comparison between experimental data (red curves) and numerical predictions (blue curves) is reported for fibre-reinforced ordinary concrete (FROC), fibre-reinforced self-compacting concrete (FRSCC), and fibre-reinforced high-strength concrete (FRHSC), respectively. In addition, a green circle indicates the first fracturing load predicted by the UBCM.
Figure 11.
Experimental (red) vs. numerical (blue) results. (a) FROC 65-0.5; (b) FROC 65-1; (c) FRSCC 65-0.5; (d) FRSCC 65-1; (e) FRHSC 65-0.5; (f) FRHSC 65-1. Green circle: first fracturing load predicted by the UBCM.
As reported in Table 2, the mechanical parameters characterizing the matrix (KIC) and the fibres (σu and wc) have been identified for each specimen by means of Pareto’s multi-objective optimization approach [8,11,12,14,15]. These parameters are not measured independently, but are obtained by material identification (inverse analysis) from the monotonic envelope of each experimental load–deflection curve, whereas the unloading and reloading branches are not used [8,14,15]. The matrix fracture toughness, KIC, is identified by the first-cracking load. The fibre bridging mechanism is represented by two parameters associated with the pull-out behaviour of the hooked-end steel fibres. The maximum pull-out force, expressed by the equivalent strength σu, defines the peak bridging resistance that can be transmitted across the crack, and it is identified by the maximum load shown by the structural response in the post-cracking regime. The equivalent embedded length, or critical pull-out displacement, wc, represents the crack opening at which the fibre bridging mechanism is fully exhausted, and it is identified by the slope of the post-cracking branch. Together, these quantities determine the energy dissipated during fibre pull-out and therefore control the post-cracking deformation capacity of the composite. The identified values of σu are 300, 233, 315, 287, 333, and 379 MPa for the specimens FROC 65-0.5, FROC 65-1, FRSCC 65-0.5, FRSCC 65-1, FRHSC 65-0.5, and FRHSC 65-1, respectively [15], and the corresponding values of NP,f are reported in Table 2. Accordingly, KIC should be regarded as an apparent (identified) toughness of the matrix: the differences between specimens with the same matrix (e.g., 15 and 17 MPa·mm1/2 for FROC, 17 and 21 MPa·mm1/2 for FRSCC) reflect the experimental scatter of the first-cracking load of individual specimens, which is directly governed by the tensile strength of the matrix, together with the pre-peak contribution of the fibres, which the model lumps into KIC. Since the identification is based on the envelope only, the hysteretic loops and the corresponding dissipated energy are not fitted, but predicted by the model. A good agreement between experimental data and numerical curves is obtained in terms of envelope, whereas the comparison in terms of dissipated energy is discussed below (Table 3 and Figure 12).
Table 2.
Mechanical parameters identified from the monotonic envelopes of the load–deflection curves in Figure 11.
Table 3.
Mean energy dissipated per hysteretic loop: experimental results vs. UBCM predictions for the campaigns by Güvensoy et al. [49], Bayramov et al. [50], Boulekbache et al. [48], and Naaman [61] (ARxx-yy: fibre aspect ratio xx and fibre volume fraction yy%).
Figure 12.
Mean energy dissipated per hysteretic loop vs. fibre-reinforcement brittleness number: experimental (red) vs. numerical (blue) results for the campaigns by Boulekbache et al. [48], Güvensoy et al. [49], Bayramov et al. [50], and Naaman [61].
Finally, considering the slope of the unloading branches of the P-δ diagrams, it is worth noting that the flexural stiffness predicted by the UBCM is slightly larger than the experimental one. This discrepancy derives from the assumption of a linear-elastic matrix with constant Young’s modulus, E, so that the progressive degradation of the matrix and of the fibre–matrix interface during the cycles is not described [15]. Since stiffer unloading and reloading branches produce narrower loops, this limitation leads to an underestimation of the dissipated energy, which is expected to grow with the number and amplitude of the cycles. A degradation law for E as a function of the number of cycles, e.g., based on the cyclic modulus reported in [48], would allow this effect to be captured.
To further assess the predictive capability of the UBCM in terms of hysteretic energy, the model has also been applied to the cyclic flexural tests by Güvensoy et al. [49] on a high-performance steel-fibre-reinforced cementitious composite (specimen M5: 70 × 70 × 280 mm, a0/h = 0.4, Vf = 7.8%, steel fibres with lf = 6 mm, df = 0.15 mm, and fu = 2250 MPa) and by Bayramov et al. [50] on notched beams (100 × 100 × 500 mm, span 400 mm, a0/h = 0.4) reinforced with hooked-end steel fibres with aspect ratios of 55, 65, and 80, and fibre volume fractions of 0.26%, 0.45%, and 0.64%. The identification procedure described above for the tests by Boulekbache et al. has been applied in the same way to the specimens by Güvensoy et al., Bayramov et al., and Naaman; the corresponding parameters are available from the corresponding author on request. The mean energy dissipated per hysteretic loop, obtained experimentally and numerically, is reported in Table 3 for these two campaigns, together with the results related to the campaign by Boulekbache et al. [48] and to the tests reported by Naaman [61] (unnotched 100 × 100 × 400 mm prisms, precracked before cycling and tested in third-point loading over a clear span of 300 mm, made of high-early-strength concrete with a 28-day compressive strength of 47.7 MPa and reinforced with 2% by volume of hooked-end steel fibres, i.e., an equal combination of fibres with lf = 30 mm and 50 mm and df = 0.5 mm; the specimens considered herein, nos. 16, 18, and 20 in [61], were tested under load control with load ranges of 10–90%, 10–70%, and 10–80% of the static flexural capacity, respectively), and is summarized in Figure 12 as a function of the fibre-reinforcement brittleness number. For both experimental and numerical curves, the energy dissipated in each loop is computed by numerical integration as the area enclosed, in the load–deflection plane, by each unloading branch and the subsequent reloading branch. The mean energy per loop is the arithmetic mean over all the complete loops of each test, i.e., eight loops for the tests by Boulekbache et al. (seven for specimen FRSCC 65-1), four for the specimen by Güvensoy et al., two or three for those by Bayramov et al., and four or five for those by Naaman, i.e., all the loops reported in [61]. For the specimens by Güvensoy et al. and Bayramov et al., the difference between experimental and numerical mean energy is within 20% in eight cases out of ten, the maximum deviations being found for the specimens AR80-0.45 and AR80-0.64 (underestimation of about 35%), i.e., for the longest fibres. On the other hand, the model systematically underestimates the energy dissipated by the specimens with NP,f > 1 (Table 3 and Figure 12), the largest deviations being found for specimen FRHSC 65-1 and for the specimens by Naaman. A possible interpretation is that the matrix damage accumulated during the cycles, the degradation of the fibre–matrix interface, and the consequent reduction in unloading stiffness, which widen the experimental loops, become more relevant as the fibre content increases. In any case, these discrepancies arise far from moderate values of NP,f, whereas the optimum condition discussed in Section 5 is found in the range of moderate values of NP,f, where the agreement between experimental and numerical results is better.
The key findings of Figure 12 can be summarized as follows. First, when the results of all the campaigns are collected as a function of NP,f, the experimental energy per loop spans more than two orders of magnitude, from about 20 N·mm to about 3700 N·mm, and the UBCM reproduces this trend, showing that the brittleness number, which combines fibre volume fraction, structural size, fibre strength, and matrix toughness, is an appropriate parameter to correlate the hysteretic dissipation of FRC beams. Second, the accuracy of the model is higher for NP,f < 1 (Güvensoy et al. and Bayramov et al.), whereas the energy is underestimated for larger values of NP,f, possibly for the reasons discussed above. Third, the experimental energies in Figure 12 increase with NP,f. This does not contradict the existence of an optimum value of the brittleness number discussed in Section 5, since the data in Figure 12 refer to specimens with different geometries, matrices, and fibres, and are averaged over all the loops of each test, performed at different amplitudes according to the loading protocol of each campaign. Conversely, the influence of NP,f on the energy dissipation can be isolated only by varying the brittleness number for a given geometry and loading history, as done in Section 5.
5. Scale-Dependent Energy Dissipation in Fibre-Reinforced Concrete
Further analyses have been carried out by means of the UBCM, considering three beam depths (h = 5, 10, and 20 cm) with a span-to-depth ratio equal to 4, together with nine different values of the brittleness number NP,f, ranging from 0.06 to 4.30. In all cases, the testing conditions are analogous to those of the experimental campaign by Boulekbache et al. [48], i.e., notched beams in four-point bending (Table 1 and Figure 10), subjected to a loading–unloading–reloading cycle. The combined effect of material and reinforcement parameters (fibre volume fraction, equivalent fibre strength, and matrix fracture toughness) is synthetically described by the brittleness number, NP,f (Equation (4)): the nine values of NP,f considered herein represent all the relevant variations of these parameters. Consequently, for a given NP,f, the corresponding fibre volume fraction scales as h−1/2. On the other hand, the pull-out brittleness number, Nw = Ewc/(KICh1/2) (Equation (12)), also varies with the beam depth, decreasing as h−1/2 for given material properties. This number governs the exhaustion of the fibre bridging action, i.e., the softening tail of the response and the rotation capacity of the cross-section [8,14], whereas the peak bridging resistance, and therefore the onset of the fibre slippage that triggers the hysteretic dissipation, is governed by NP,f. For each specimen size, the energy dissipated in the first hysteretic loop is evaluated as a function of the brittleness number. The first loop is considered in order to isolate the influence of NP,f from the effects of cumulative damage, which are not described by the model (Section 4), whereas the mean energy over several loops reported in Table 3 and Figure 12 refers to the experimental loading protocols. The numerical results are shown in Figure 13. For the beams with h = 10 and 20 cm, the dissipated energy exhibits a clear maximum at the same value, NP,f ≈ 0.4, which defines the optimum value of the reinforcement brittleness number, NP,opt ≈ 0.4, corresponding to the maximum dissipated energy. For the smallest beam (h = 5 cm), the dissipated energy is small and almost constant over the whole range of NP,f, so that no clearly defined peak can be recognized, and the small fluctuations of the curve do not identify a different optimum. Since the brittleness number already accounts for the structural size through the factor h1/2 (Equation (4)), the maxima of the two larger beams occur at the same value of NP,f, although their pull-out brittleness numbers differ by a factor of √2. This shows that, within the investigated range, the variation in Nw does not shift the position of the maximum, which is governed by NP,f: hence, NP,opt can be regarded as a dimensionless, size-independent quantity, whereas the corresponding optimum fibre volume fraction, Vf,opt, decreases with the beam depth as h−1/2. It is also worth noting that the increase in the absolute dissipated energy with h reflects the size of the beams, and that normalizing the energy by any size-dependent quantity, e.g., KIC2bh/E, would rescale each curve without changing the abscissa of its maximum; therefore, the position of NP,opt is not affected by such a normalization. In this sense, a remarkable analogy between the case of low-cycle fatigue and that of monotonically increasing load emerges. In the latter, the critical value of the reinforcement brittleness number, NPC, defines the minimum reinforcement condition, i.e., the scale-dependent fibre volume fraction required to achieve a stable post-peak response [8,14,16,17,22,23,24,25,26]. Similarly, the optimum value of the brittleness number, NP,opt, represents the condition at which, for a given structural size, the largest hysteretic energy is dissipated. In Figure 13, the dashed line marks the transition between softening and hardening post-cracking responses (NPC ≈ 0.7): the optimum value NP,opt ≈ 0.4 falls within the softening regime. Thus, an appropriate balance between the two dimensionless numbers, NPC and NP,opt, may be relevant to the design of FRC members required to dissipate energy, e.g., under seismic actions [62]. This suggests the range NP,opt ≤ NP,f ≤ NPC (shaded region in Figure 13), in which the hysteretic energy dissipation is high while the post-cracking response approaches the stable condition associated with the minimum reinforcement. Since most of this range belongs to the softening regime, its use requires that the structural stability be ensured. In members reinforced with fibres only, a stable post-cracking response requires NP,f ≥ NPC, so that the upper bound of the range, NP,f ≈ NPC, represents the recommended choice, which combines the minimum reinforcement condition with a dissipation still close to (about 80–90% of) its maximum value (Figure 13). Values of NP,f within the range are instead meaningful for hybrid-reinforced members, in which the conventional bars ensure the stable load-bearing capacity [12,16,17], and the fibre content can be selected to maximize the hysteretic dissipation. Since both bounds are expressed in terms of the brittleness number, the corresponding range of fibre volume fractions decreases with beam depth as h−1/2. It should be emphasized that this range is derived from the first-loop response of beams under prescribed cyclic flexural loading, whereas seismic actions possibly involve full load reversals, variable displacement amplitudes, progressive stiffness degradation, and flexure–shear interaction, which are not investigated herein.
Figure 13.
Energy dissipated in the first hysteretic loop vs. fibre-reinforcement brittleness number, NP,f, for three beam depths. Dashed line: transition from softening to hardening (NPC); dotted line: largest dissipation of energy (NP,opt).
6. Concluding Remarks
The mechanical response of fibre-reinforced concrete structures subjected to low-cycle fatigue in bending is strongly dependent on their size-scale. By means of a fracture mechanics model, the brittle matrix fracturing process, the bridging mechanisms due to fibre pull-out, as well as the plastic shake-down and hysteresis phenomena can be thoroughly described. The model parameters have been identified from the monotonic envelopes of the cyclic flexural tests by Boulekbache et al., in which three different matrices and two different fibre volume fractions were considered as variables, and the hysteretic loops have then been predicted; the model has been further assessed against the tests by Güvensoy et al., Bayramov et al., and Naaman. The hysteretic loops are satisfactorily reproduced, and the mean energy per loop is predicted within 20% in eight out of ten cases for NP,f < 1, whereas the energy dissipated by the specimens with NP,f > 1 is underestimated, possibly owing to cumulative damage and stiffness degradation. In addition, the dissipated energy can be correlated to the fibre-reinforcement brittleness number, NP,f, in which the effects of the fibre volume fraction and the structural size-scale are included. The main original result of the present work is the identification, by means of a parametric study on beams of different depths, of an optimum value of the brittleness number, NP,opt ≈ 0.4, which provides the maximum energy dissipated in the first hysteretic loop for the beam depths of 10 and 20 cm, both showing a clearly defined maximum at the same value of NP,f, whereas for the smallest beam (5 cm) the dissipated energy is almost constant and no clear optimum can be identified. Being a dimensionless number that includes the structural size, NP,opt is size-independent within the investigated range, despite the different pull-out brittleness numbers of the two larger beams, whereas the corresponding fibre volume fraction decreases with the beam depth as h−1/2. This optimum falls within the softening regime, i.e., below the critical value of the reinforcement brittleness number that defines the minimum reinforcement condition under monotonic loading. Since the latter condition implies a minimum fibre volume fraction that decreases with the beam size, whereas the current Italian provisions prescribe a constant minimum fibre content, an appropriate balance between the two dimensionless numbers should be sought when FRC members are required to dissipate energy: a fibre-reinforcement brittleness number comprised between the optimum and the critical values, NP,opt ≤ NP,f ≤ NPC, is suggested as a preliminary criterion, with NP,f ≈ NPC for members reinforced with fibres only, so as to ensure a stable post-cracking response.
Author Contributions
Conceptualization, F.A. and B.C.; methodology, F.A.; software, F.A.; validation, F.A.; formal analysis, F.A.; investigation, F.A.; writing—original draft preparation, F.A.; writing—review and editing, F.A. and B.C.; supervision, B.C. All authors have read and agreed to the published version of the manuscript.
Funding
This research received no external funding.
Data Availability Statement
The raw data supporting the conclusions of this article will be made available by the authors on request.
Conflicts of Interest
The authors declare no conflicts of interest.
References
- Barros, J.A.O.; Figueiras, J.A. Flexural Behavior of SFRC: Testing and Modeling. J. Mater. Civ. Eng. 1999, 11, 331–339. [Google Scholar] [CrossRef] [Scilit]
- Dinh, H.H.; Parra-Montesinos, G.J.; Wight, J.K. Shear Behavior of Steel Fiber-reinforced Concrete Beams without Stirrup Reinforcement. ACI Struct. J. 2010, 107, 597–606. [Google Scholar] [CrossRef] [Scilit]
- Minelli, F.; Conforti, A.; Cuenca, E.; Plizzari, G. Are Steel Fibres Able to Mitigate or Eliminate Size Effect in Shear? Mater. Struct. 2014, 47, 459–473. [Google Scholar] [CrossRef] [Scilit]
- Cucuzza, R.; Aloisio, A.; Accornero, F.; Marinelli, A.; Bassoli, E.; Marano, G.C. Size-scale Effects and Modelling Issues of Fibre-reinforced Concrete Beams. Constr. Build. Mater. 2023, 392, 131727. [Google Scholar] [CrossRef] [Scilit]
- Jiang, Z.; Zhu, Z.; Accornero, F. Tensile-to-Shear Crack Transition in the Compression Failure of Steel-Fibre-Reinforced Concrete: Insights from Acoustic Emission Monitoring. Buildings 2024, 14, 2039. [Google Scholar] [CrossRef] [Scilit]
- Carpinteri, A. A Fracture Mechanics Model for Reinforced Concrete Collapse. In Proceedings of the IABSE Colloquium on Advanced Mechanics of Reinforced Concrete, Delft, The Netherlands, 2–4 June 1981; pp. 17–30. [Google Scholar]
- Carpinteri, A. Stability of Fracturing Process in RC Beams. J. Struct. Eng. 1984, 110, 544–558. [Google Scholar] [CrossRef] [Scilit]
- Accornero, F.; Rubino, A.; Carpinteri, A. Post-cracking Regimes in the Flexural Behaviour of Fibre-reinforced Concrete Beams. Int. J. Solids Struct. 2022, 248, 111637. [Google Scholar] [CrossRef] [Scilit]
- Accornero, F.; Carpinteri, A.; Rubino, A. Fibre-reinforced and Hybrid-reinforced Concrete: An Updated Bridged Crack Model with Softening Pull-out Forces. In Proceedings of the 7th World Congress on Civil, Structural, and Environmental Engineering (CSEE’22), Lisbon, Portugal, 10–12 April 2022; Paper No. ICSECT 005. [Google Scholar] [CrossRef] [Scilit]
- Accornero, F.; Rubino, A.; Carpinteri, A. A Fracture Mechanics Approach to the Design of Fibre-reinforced and Hybrid-reinforced Concrete Beams. In Building for the Future: Durable, Sustainable, Resilient—Fib Symposium 2023; Ilki, A., Çavunt, D., Çavunt, Y.S., Eds.; Lecture Notes in Civil Engineering; Springer: Cham, Switzerland, 2023; Volume 349, pp. 1181–1189. [Google Scholar] [CrossRef] [Scilit]
- Rubino, A. A Fracture Mechanics Approach to the Design of Fibre-Reinforced and Hybrid-Reinforced Concrete Structures. Ph.D. Thesis, Politecnico di Torino, Turin, Italy, 2023. [Google Scholar]
- Accornero, F.; Rubino, A.; Carpinteri, A. A Fracture Mechanics Approach to the Design of Hybrid-reinforced Concrete Beams. Eng. Fract. Mech. 2022, 275, 108821. [Google Scholar] [CrossRef] [Scilit]
- Carpinteri, A.; Massabò, R. Bridged versus Cohesive Crack in the Flexural Behavior of Brittle-matrix Composites. Int. J. Fract. 1996, 81, 125–145. [Google Scholar] [CrossRef] [Scilit]
- Carpinteri, A.; Accornero, F.; Rubino, A. Scale Effects in the Post-cracking Behaviour of Fibre-reinforced Concrete Beams. Int. J. Fract. 2023, 240, 1–16. [Google Scholar] [CrossRef] [Scilit]
- Accornero, F.; Rubino, A.; Carpinteri, A. Ultra-low Cycle Fatigue (ULCF) in Fibre-reinforced Concrete Beams. Theor. Appl. Fract. Mech. 2022, 120, 103392. [Google Scholar] [CrossRef] [Scilit]
- Rubino, A.; Accornero, F.; Carpinteri, A. Flexural Behavior and Minimum Reinforcement Condition in Hybrid-reinforced Concrete Beams. Struct. Concr. 2023, 24, 4767–4778. [Google Scholar] [CrossRef] [Scilit]
- Rubino, A.; Accornero, F.; Carpinteri, A. Fracture Mechanics Approach to Minimum Reinforcement Design of Fibre-reinforced and Hybrid-reinforced Concrete Beams. Int. J. Damage Mech. 2025, 34, 900–919. [Google Scholar] [CrossRef] [Scilit]
- Abdallah, S.; Fan, M.; Rees, D.W.A. Bonding Mechanisms and Strength of Steel Fiber-reinforced Cementitious Composites: Overview. J. Mater. Civ. Eng. 2018, 30, 04018001. [Google Scholar] [CrossRef] [Scilit]
- Abdallah, S.; Rees, D.W.A. Analysis of Pull-out Behaviour of Straight and Hooked End Steel Fibres. Engineering 2019, 11, 332–341. [Google Scholar] [CrossRef]
- Carpinteri, A.; Carpinteri, A. Hysteretic Behavior of RC Beams. J. Struct. Eng. 1984, 110, 2073–2084. [Google Scholar] [CrossRef] [Scilit]
- Carpinteri, A.; Accornero, F. The Bridged Crack Model with Multiple Fibers: Local Instabilities, Scale Effects, Plastic Shake-down, and Hysteresis. Theor. Appl. Fract. Mech. 2019, 104, 102351. [Google Scholar] [CrossRef] [Scilit]
- Accornero, F.; Rubino, A.; Carpinteri, A. Ductile-to-brittle Transition in Fibre-reinforced Concrete Beams: Scale and Fibre Volume Fraction Effects. Mater. Des. Process. Commun. 2020, 2, e127. [Google Scholar] [CrossRef] [Scilit]
- Carpinteri, A.; Accornero, F. Ductile-to-brittle Transition in Fiber-reinforced Brittle-matrix Composites: Scale and Fiber Volume Fraction Effects. In Proceedings of the 10th International Conference on Fracture Mechanics of Concrete and Concrete Structures (FraMCoS-X), Bayonne, France, 24–26 June 2019. [Google Scholar] [CrossRef] [Scilit]
- Accornero, F.; Carpinteri, A. Ductile-to-brittle Transition in Fiber-reinforced Brittle-matrix Composites: Discontinuous Phenomena and Optimization of the Components. In Proceedings of the XXIV AIMETA Conference 2019; Lecture Notes in Mechanical Engineering; Springer: Cham, Switzerland, 2020; pp. 550–557. [Google Scholar] [CrossRef] [Scilit]
- Rubino, A.; Accornero, F.; Carpinteri, A. Post-cracking Structural Behaviour in FRC Beams: Scale Effects and Minimum Fibre Volume Fraction. In Proceedings of the fib Symposium 2021, Lisbon, Portugal, 14–16 June 2021; pp. 622–631. [Google Scholar]
- Accornero, F.; Rubino, A.; Marano, G.C.; Carpinteri, A. Smart Construction of Fibre-reinforced Concrete Structures: Size-scale Effects on Minimum Reinforcement and Plastic Rotation Capacity. Smart Constr. Sustain. Cities 2024, 2, 12, Correction in Smart Constr. Sustain. Cities 2025, 3, 8. [Google Scholar] [CrossRef] [Scilit]
- Carpinteri, A.; Accornero, F. Dimensional Analysis of Critical Phenomena: Self-weight Failure, Turbulence, Resonance, Fracture. Phys. Mesomech. 2021, 24, 459–463. [Google Scholar] [CrossRef] [Scilit]
- Fantilli, A.P.; Chiaia, B.; Gorino, A. Fiber Volume Fraction and Ductility Index of Concrete Beams. Cem. Concr. Compos. 2016, 65, 139–149. [Google Scholar] [CrossRef] [Scilit]
- Fantilli, A.P.; Chiaia, B.; Gorino, A. Unified Approach for Minimum Reinforcement of Concrete Beams. ACI Struct. J. 2016, 113, 1107–1116. [Google Scholar] [CrossRef] [Scilit]
- RILEM TC 162-TDF. Test and Design Methods for Steel Fibre Reinforced Concrete. σ-ε Design Method. Final Recommendation. Mater. Struct. 2003, 36, 560–567. [Google Scholar] [CrossRef] [Scilit]
- Carpinteri, A.; Accornero, F. Rotation versus Curvature Fractal Scaling in Bending Failure. Phys. Mesomech. 2019, 22, 46–51. [Google Scholar] [CrossRef] [Scilit]
- Carpinteri, A. Scaling Laws and Renormalization Groups for Strength and Toughness of Disordered Materials. Int. J. Solids Struct. 1994, 31, 291–302. [Google Scholar] [CrossRef] [Scilit]
- Carpinteri, A.; Chiaia, B.; Ferro, G. Size Effects on Nominal Tensile Strength of Concrete Structures: Multifractality of Material Ligaments and Dimensional Transition from Order to Disorder. Mater. Struct. 1995, 28, 311–317. [Google Scholar] [CrossRef] [Scilit]
- CNR-DT 204/2006; Istruzioni per la Progettazione, l’Esecuzione ed il Controllo di Strutture di Calcestruzzo Fibrorinforzato. National Research Council of Italy (CNR): Rome, Italy, 2007.
- International Federation for Structural Concrete (fib). Fibre-Reinforced Concrete: State-of-the-Art Report; fib Bulletin No. 105; International Federation for Structural Concrete (fib): Lausanne, Switzerland, 2022. [Google Scholar]
- Consiglio Superiore dei Lavori Pubblici. Istruzioni per l’Applicazione dell’«Aggiornamento delle “Norme Tecniche per le Costruzioni”» di cui al D.M. 17 gennaio 2018; Circolare n. 7 del 21 gennaio 2019; Consiglio Superiore dei Lavori Pubblici: Rome, Italy, 2019; Gazzetta Ufficiale n. 35 dell’11 febbraio 2019, Supplemento Ordinario n. 5.
- Consiglio Superiore dei Lavori Pubblici—Servizio Tecnico Centrale. Linea Guida per l’Identificazione, la Qualificazione, la Certificazione di Valutazione Tecnica ed il Controllo di Accettazione dei Calcestruzzi Fibrorinforzati FRC (Fiber Reinforced Concrete); Aggiornamento Novembre 2021: Rome, Italy, 2021.
- ACI Committee 318. Building Code Requirements for Structural Concrete (ACI 318-08) and Commentary; American Concrete Institute: Farmington Hills, MI, USA, 2008. [Google Scholar]
- EN 1992-1-1:2023; Eurocode 2—Design of Concrete Structures—Part 1-1: General Rules and Rules for Buildings, Bridges and Civil Engineering Structures. Annex L: Steel Fibre Reinforced Concrete Structures. European Committee for Standardization (CEN): Brussels, Belgium, 2023.
- de la Fuente, A.; Monserrat-López, A.; Tošić, N.; Serna, P. Design of Steel Fibre Reinforced Concrete Structures According to the Annex L of the Eurocode-2 2023. Hormigón Acero 2023, 74, 169–186. [Google Scholar] [CrossRef] [Scilit]
- International Federation for Structural Concrete (fib). Model Code 2010—Final Draft; fib Bulletin No. 65; International Federation for Structural Concrete (fib): Lausanne, Switzerland, 2012; Volume 1. [Google Scholar]
- fib. fib Model Code for Concrete Structures (2020); International Federation for Structural Concrete (fib): Lausanne, Switzerland, 2024. [Google Scholar]
- Carpinteri, A.; Accornero, F. Residual Crack Opening in Fiber-reinforced Structural Elements Subjected to Cyclic Loading. Strength Fract. Complex. 2020, 12, 63–74. [Google Scholar] [CrossRef] [Scilit]
- Carpinteri, A. Advanced Structural Mechanics; CRC Press: Boca Raton, FL, USA, 2017. [Google Scholar]
- König, J.A. Shakedown of Elastic-Plastic Structures; Elsevier: Amsterdam, The Netherlands, 1987. [Google Scholar]
- Matsumoto, T. Crack Bridging Law in Discontinuous Fiber Reinforced Composites under Cyclic Loading. J. Appl. Mech. JSCE 2007, 10, 923–933. [Google Scholar] [CrossRef] [Scilit]
- Lee, M.K.; Barr, B.I.G. An Overview of the Fatigue Behaviour of Plain and Fibre Reinforced Concrete. Cem. Concr. Compos. 2004, 26, 299–305. [Google Scholar] [CrossRef] [Scilit]
- Boulekbache, B.; Hamrat, M.; Chemrouk, M.; Amziane, S. Flexural Behavior of Steel Fibre-reinforced Concrete under Cyclic Loading. Constr. Build. Mater. 2016, 126, 253–262. [Google Scholar] [CrossRef] [Scilit]
- Güvensoy, G.; Bayramov, F.; Ilki, A.; Sengül, C.; Tasdemir, M.A.; Kocatürk, A.N.; Yerlikaya, M. Mechanical Behavior of High Performance Steel Fiber Reinforced Cementitious Composites under Cyclic Loading Condition. In Proceedings of the International Symposium on Ultra High Performance Concrete, Kassel, Germany, 13–15 September 2004. [Google Scholar]
- Bayramov, F.; Aydoner, T.; Ilki, A.; Tasdemir, C.; Tasdemir, M.A. An Optimum Design for Steel Fiber Reinforced Concretes under Cyclic Loading. In Proceedings of the 5th International Conference on Fracture Mechanics of Concrete and Concrete Structures (FraMCoS-5), Vail, CO, USA, 12–16 April 2004. [Google Scholar]
- Campione, G.; Miraglia, N.; Papia, M. Mechanical Properties of Steel Fibre Reinforced Lightweight Concrete with Pumice Stone or Expanded Clay Aggregates. Mater. Struct. 2001, 34, 201–210. [Google Scholar] [CrossRef] [Scilit]
- Fataar, H.; Combrinck, M.; Boshoff, W.P. An Experimental Study on the Fatigue Failure of Steel Fibre Reinforced Concrete at a Single Fibre Level. Constr. Build. Mater. 2021, 299, 123869. [Google Scholar] [CrossRef] [Scilit]
- Jun, P.; Mechtcherine, V. Behaviour of Strain-hardening Cement-based Composites (SHCC) under Monotonic and Cyclic Tensile Loading: Part 1—Experimental Investigations. Cem. Concr. Compos. 2010, 32, 801–809. [Google Scholar]
- Paschalis, S.A.; Lampropoulos, A.P. Ultra-high-performance Fiber-reinforced Concrete under Cyclic Loading. ACI Mater. J. 2016, 113, 419–427. [Google Scholar] [CrossRef] [Scilit]
- Schäfer, N.; Gudzulic, V.; Breitenbücher, R.; Meschke, G. Experimental and Numerical Investigation on High Performance SFRC: Cyclic Tensile Loading and Fatigue. Materials 2021, 14, 7593. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Banjara, N.K.; Ramanjaneyulu, K. Experimental Investigations and Numerical Simulations on the Flexural Fatigue Behavior of Plain and Fiber-reinforced Concrete. J. Mater. Civ. Eng. 2018, 30, 04018151. [Google Scholar] [CrossRef] [Scilit]
- Carlesso, D.M.; de la Fuente, A.; Cavalaro, S.H.P. Fatigue of Cracked High Performance Fiber Reinforced Concrete Subjected to Bending. Constr. Build. Mater. 2019, 220, 444–455. [Google Scholar] [CrossRef] [Scilit]
- Enfedaque, A.; Alberti, M.G.; Gálvez, J.C.; Proaño, J.S. Assessment of the Post-cracking Fatigue Behavior of Steel and Polyolefin Fiber-reinforced Concrete. Materials 2021, 14, 7087. [Google Scholar] [CrossRef] [Scilit] [PubMed]
- Germano, F.; Tiberti, G.; Plizzari, G. Post-peak Fatigue Performance of Steel Fiber Reinforced Concrete under Flexure. Mater. Struct. 2016, 49, 4229–4245. [Google Scholar] [CrossRef] [Scilit]
- Goel, S.; Singh, S.P.; Singh, P. Fatigue Analysis of Plain and Fiber-reinforced Self-consolidating Concrete. ACI Mater. J. 2012, 109, 573–582. [Google Scholar] [CrossRef] [Scilit]
- Naaman, A.E.; Hammoud, H. Fatigue Characteristics of High Performance Fiber-reinforced Concrete. Cem. Concr. Compos. 1998, 20, 353–363. [Google Scholar] [CrossRef] [Scilit]
- Parra-Montesinos, G.J. High-Performance Fiber-Reinforced Cement Composites: An Alternative for Seismic Design of Structures. ACI Struct. J. 2005, 102, 668–675. [Google Scholar] [CrossRef] [Scilit] [PubMed]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.