Abstract
Low-carbon structural materials must be evaluated for mechanical performance, post-damage repair, and environmental and economic consequences. This study examined the flexural behavior, CFRP rehabilitation performance, and environmental and economic impacts of fiber-reinforced alkali-activated concrete (AAC) beams using experimental testing and nonlinear numerical models. Five sets of 15 reinforced rectangular beams (150 × 250 × 1500 mm) were tested: regular concrete, plain AAC, steel-fiber-reinforced AAC, polypropylene-fiber-reinforced AAC, and hybrid steel–polypropylene-fiber-reinforced AAC. The alkali-activated binder was 50% fly ash and 50% ground granulated blast-furnace slag. The fiber-reinforced mixtures had a fiber volume of 0.75%. Each material property assessment included three specimens per combination. All beams were four-point bent to failure, repaired using externally bonded CFRP sheets, and retested. Experimental data verified a nonlinear finite-element model produced in ANSYS APDL, which was used to explore the impact of increasing fiber content from 0.75% to 1.25%. A comparative life-cycle environmental and economic study included material production, production-associated energy, and CFRP restoration. AAC with steel-fiber reinforcement demonstrated 15.4% higher compressive, flexural, and ultimate load capacities (106.96 kN) than conventional concrete. Flexural toughness was highest in hybrid-fiber reinforcement (2406.7 kN·mm), 58.3% greater than typical concrete. Polypropylene-fiber-reinforced AAC had the best strength-recovery ratio (89.57%) and steel-fiber-reinforced AAC had the highest load capacity (84.78 kN) for CFRP rehabilitation. The numerical model projected ultimate loads that differed by 0.56% and 6.02% from the experimental values. When fiber percentage was raised to 1.25%, the steel, polypropylene, and hybrid-fiber systems’ predicted capacities improved by 25.10, 21.19, and 30.04%, respectively. From an environmental and economic perspective, plain AAC has a 50% lower embodied carbon per unit ultimate load capacity than conventional concrete. The estimated material cost was reduced by 60.7% when using fly ash.
1. Introduction
The construction industry is facing growing pressure to reduce the reliance on ordinary Portland cement (OPC) as the production of OPC is energy- and natural resource-intensive and is a major contributor of global carbon dioxide emissions [1]. This challenge has driven the development of alternative cementitious systems capable of incorporating industrial by-products, while satisfying the mechanical and serviceability requirements of structural concrete. Among these alternatives, geopolymer concrete has been of great research interest because it can be produced by the alkaline activation of aluminosilicate-rich materials such as fly ash and ground granulated blast-furnace slag (GGBS). These precursors react with alkaline solutions to form hardening binding phases, with composition and performance depending on the chemistry of the precursor, the concentration of the alkaline activator, the ratio of silicate to hydroxide ions, the liquid-to-binder ratio and the curing regime [2,3]. The application of geopolymer technology can reduce the dependency on OPC and enable the beneficial utilization of industrial residues. Nevertheless, the assessment of the environmental advantages should be conducted at the mixture and regional level, as the manufacturing of the activators, thermal curing and transportation of the material can have a profound impact on the overall environmental footprint [4,5].
The fly ash and GGBS combination is a technically feasible binder system for structural geopolymer concrete. Low-calcium fly ash provides reactive silica and alumina and promotes the formation of sodium aluminosilicate hydrate gels. GGBS with high calcium content promotes the formation of calcium-containing reaction products, leading to faster setting and early strength development. These reaction products may be used to improve the pore structure and the compactness of the matrix. However, the performance of the material still depends on the proportions of precursors and activation conditions [6]. Nath and Sarker [7] reported that with increasing GGBS content in fly-ash geopolymer concrete, the setting time reduced and the early age strength improved under ambient curing. Hence, mixed fly ash-GGBS systems provide an attractive route for the production of structural geopolymer concrete without the sole dependence on extended heat curing.
Geopolymer concrete is a quasi-brittle material that has low tensile strain capacity, yet it has good compressive performance. If the matrix tensile strength is surpassed, cracks localize form quickly, resulting in a loss of stiffness and limited post-cracking strength. This limit is particularly relevant in reinforced beams where crack width, stiffness, energy dissipation and tensile cracking dictate deflection before the final state is attained. This response may be modified by discrete fibers bridging fractures and transmitting tensile loads across the divided crack surfaces. The improvement relies on the fiber stiffness, the tensile strength, the geometry, the aspect ratio, the volume fraction, the orientation, the dispersion and the interfacial bond with the geopolymer matrix [8]. However, the increase in the fiber content does not always lead to an improvement in the structural performance, as high doses may produce a reduction in the workability, fiber aggregation and the appearance of entrapped voids.
In geopolymer concrete, steel and polypropylene fibers have diverse roles [9]. Hooked-end steel fibers offer relatively high tensile strength and elastic modulus, and so may bridge macrocracks, limit crack opening and maintain tensile stress after matrix cracking occurs [10]. Their mechanical anchoring also leads to a higher resistance to fiber pull-out and favors the stress redistribution in the damaged zone. Polypropylene fibers are less rigid than the other fibers and typically contribute less directly to the peak load capacity [11]. However, their tiny dimensions, chemical stability and resistance to alkaline environments make them useful for the control of early microcracking and improvement in fracture dispersion. Such a hybrid steel–polypropylene system may therefore offer crack control at various scales, wherein polypropylene fibers would prevent the beginning and coalescence of tiny fractures and the steel fibers would become more active as the fissures enlarge [12].
Previous studies have shown feasibility of mono- and hybrid-fiber reinforcement in geopolymer composites at the material level. However, the reaction is very sensitive to the matrix composition and the fiber-matrix compatibility, as observed by Ranjbar and Zhang [8]. The addition of fibers can improve the tensile strength, flexural strength, fracture energy and residual capacity. Junior et al. [13] examined the performance of geopolymer composites with various mono and hybrid fibers and reported that steel-containing systems attained considerable residual flexural strength while some hybrid combinations had desirable deflection-hardening and toughness characteristics. The results indicate that the advantages of adding fibers cannot be evaluated merely on the basis of compressive strength, but the whole load–deflection behavior and the post-cracking resistance must be taken into consideration. It is crucial to move from the material characterization to the structural testing because the performance of a reinforced beam depends on the interaction between the concrete matrix, the longitudinal reinforcement, the stirrups, the fibers and the bond mechanisms. Dattatreya et al. [14] conducted a preliminary investigation on beams of steel-reinforced geopolymer concrete and observed a series of uncracked behavior, flexural cracking, yielding of reinforcement and failure similar to that commonly reported for conventional reinforced concrete members. Likewise, Yost et al. [15] demonstrated that alkali-activated fly-ash concrete is appropriate for structural application, but noted that differences in tensile strength, elastic modulus and reinforcing bond may influence cracking and serviceability predictions. These experiments demonstrated that conventional flexural principles could serve as a reasonable basis to evaluate the behavior of geopolymer beams, while the specific characteristics of the material are important for meaningful interpretation.
A number of recent studies have investigated the effect of mixture constituents and reinforcement variables on reinforced geopolymer members. Alex et al. [16] reported that fly-ash geopolymer beams with low calcium showed acceptable load capacity, crack propagation and moment resistance characteristics as compared to ordinary concrete specimens. The effect of the beam depth and longitudinal reinforcement ratio on the cracking moment, stiffness, deflection, ductility and ultimate strength of the beam was found to be significant. Öztürk and Arslan [17] conducted a study on ambient-cured GGBS-based geopolymer concrete beams. Their results confirmed the structural use of geopolymer concrete, but also showed that member-level response cannot be generalized from the measured compressive strength only. Research work on fiber-reinforced geopolymer beams are less common. Raj and Ramachandran [18] studied low-calcium fly-ash geopolymer beams reinforced with steel and hybrid steel–polypropylene fibers. Their results indicated that the fiber type and volume fraction influenced the first-cracking load, the ultimate resistance, the ductility, the energy absorption and the failure mode. The hybrid-fiber beams showed positive crack distribution and deformation behavior. The specimens, however, were purposely designed as shear-deficient members and the study was mainly on shear response. El-Sayed et al. [19] studied GGBS-based geopolymer ferrocement beams experimentally and numerically and found that cracking and flexural strength are governed by the reinforcement layout and matrix properties. However, the distributions of reinforcement, thickness and failure mechanics of ferrocement members are different from conventionally reinforced rectangular beams. The differences are therefore not clear on the flexural performance of plain, steel-fiber, polypropylene-fiber and hybrid-fiber geopolymer concrete beams with the same conventional steel reinforcement. While fiber reinforcement can increase the inherent cracking resistance, structural members may need repair after overloading, deterioration or changes in service demand.
Carbon-fiber-reinforced polymer (CFRP) sheets bonded externally are widely used for strengthening or repairing reinforced-concrete beams because of their high tensile strength, high stiffness-to-weight ratio, corrosion resistance and ease of installation. When bonded to the soffit of a flexural member, the CFRP sheet acts as supplementary tensile reinforcement, controls crack opening and can increase post-cracking stiffness and strength. However, the efficiency of strengthening depends on the particular substrate, surface treatment, adhesive characteristics, sheet sizes, fiber direction, bonded length and the anchorage configuration. The CFRP-concrete interface is generally the most critical part of the strengthening system. The high interfacial shear and normal stresses may cause the separation of plate-end or intermediate-crack-induced debonding before the CFRP reaches its tensile capacity. Alagusundaramoorthy et al. [20] have shown that the flexural resistance of reinforced-concrete beams could be substantially improved by the use of externally bonded CFRP sheets and fabrics. Later, Camata et al. [21] showed, through experimental and nonlinear finite-element analyses, that debonding and cover-splitting failures tend to propagate through the concrete adjacent to the adhesive layer rather than through the CFRP itself. Aram et al. [22] studied the mechanisms of premature debonding and emphasized the significance of interfacial stresses, crack location and strengthening geometry. According to Vahidpour et al. [23], addition of the externally bonded CFRP systems led to an increase in the flexural capacity and stiffness, but the strengthened members may show a decrease in ductility if the failure modes were brittle sheet rupture or debonding. Therefore, the performance of CFRP rehabilitation should be evaluated by both recovered strength and deformation-related indicators. However, the use of CFRP systems for geopolymer concrete has attracted relatively less attention. Junaid et al. [24] investigated geopolymer and fiber-reinforced geopolymer concrete beams internally reinforced with glass fiber-reinforced polymer bars. Selected specimens were preloaded to around 50% of their load capacity and subsequently reinforced by externally bonded CFRP sheets. The improved members showed better behavior in bending, which demonstrates the compatibility of internal GFRP reinforcement, geopolymer concrete and external CFRP strengthening. However, GFRP bars are linearly elastic to rupture and have a lower elastic modulus than conventional steel reinforcement. Their interaction with CFRP sheets is therefore different from that of steel reinforcement, which can yield and deform permanently before rehabilitation. Direct evidence of externally bonded CFRP strengthening of steel-reinforced fly-ash geopolymer concrete beams was given by Eisa et al. [25]. Different CFRP configurations increased first cracking, yielding and ultimate loads, and enhanced pre- and post-cracking stiffness. The study revealed that CFRP sheets can be used to improve the flexural and shear behavior of geopolymer members. However, it mainly focused on plain geopolymer concrete and the influence of CFRP configuration. The effect of internal steel, polypropylene and hybrid fibers on the efficiency of CFRP rehabilitation was not systematically evaluated. Furthermore, the rehabilitation of members with significant pre-cracking, yielding of reinforcement and irreversible loss of stiffness is not adequately represented by strengthening initially uncracked or lightly preloaded specimens. The performance of CFRP in geopolymer members is also dependent on the interfacial response. Al-Abdwais [26] studied the bond performance of geopolymer concrete and near-surface-mounted carbon-fiber-reinforced polymer (CFRP) laminates using experimental single-lap shear tests and finite-element modeling. The study showed that the bond length impacted the interfacial stress and bond-slip behavior and proved that geopolymer concrete could develop a good bond with CFRP composites. It is, however, not possible to fully replicate the combined effect of flexural cracking, reinforcement yielding, fiber pull-out, damage in the compression zone and gradual increase in CFRP stress in full beams by bond tests at prism level. Thus, the beam level tests are still necessary to determine whether the strengthening system can recover the stiffness and load capacity after severe structural damage.
Numerical modeling offers a complementary approach to investigate stress redistribution, and to extend an experimental program beyond the variables tested. Zinkaah et al. [27] developed a 3D finite-element model of FRP-reinforced geopolymer concrete beams and obtained reasonable predictions of flexural capacity and deformation. The accuracy of the simulation depends on the adopted constitutive representations of the concrete matrix, internal reinforcement, composite material and adhesive interface, as concluded by Naser et al. [28] in a review of modeling strategies for FRP-strengthened concrete members. Where global flexural response is the main concern, a smeared-crack or damage-based concrete formulation may suffice to reproduce cracking, stiffness reduction and ultimate behavior. For fiber-reinforced concrete, the mean contribution of the fibers randomly distributed in the concrete elements can be included through a smeared fiber approach into the constitutive response of the concrete elements. This approach is computationally efficient, but cannot explicitly reproduce individual fiber orientation, pull-out or localized fiber-matrix debonding and, as such, must be calibrated and validated against experimental results.
Although the research on reinforced geopolymer concrete beams is increasing, a full comparison of conventional concrete, plain geopolymer concrete, steel-fiber-reinforced geopolymer concrete, polypropylene-fiber-reinforced geopolymer concrete and hybrid steel–polypropylene-fiber geopolymer concrete is still lacking, especially when all beam specimens have the same dimensions and conventional steel-reinforcement details. Recent studies have investigated the structural behavior of geopolymer beams made from waste steel tire wires and polyamide fibers under varying curing conditions with a focus on flexural and shear behavior [29,30,31]. These investigations have contributed to understanding the impact of fiber properties, binder content and curing regimes on the structural response of geopolymer parts. However, due to variations in fiber type, mixture composition, beam configuration and experimental conditions, a direct comparison of the individual contributions of steel, polypropylene and hybrid steel–polypropylene fibers under consistent flexural testing conditions is difficult to establish. Hence, the relative contribution of various fiber systems to initial cracking resistance, post-cracking stiffness, ultimate load capacity, deformation capacity, and energy absorption is not well-defined.
Furthermore, although the potential of externally bonded carbon-fiber-reinforced polymer (CFRP) systems for strengthening concrete members has been demonstrated in previous studies, there is limited experimental evidence on the repair of severely damaged fiber-reinforced geopolymer concrete beams. In particular, the effect of the original geopolymer matrix and internal fiber structure on the recovery of load-bearing capacity, stiffness and deformation performance after significant pre-existing cracking has not been well explained. This information gap is especially significant when examining whether alternative fiber systems are relevant not only to the initial flexural performance of geopolymer beams but also their reaction following structural restoration. Thus, the present study aims to address these gaps by comparing the experimental performance of conventionally reinforced-concrete beams and geopolymer concrete beams with different fiber configurations before and after CFRP rehabilitation and their structural performance evaluation.
The present study addresses these gaps by an integrated experimental and numerical investigation of steel-reinforced rectangular beams produced with normal concrete, plain fly ash–GGBS geopolymer concrete, steel-fiber geopolymer concrete, polypropylene-fiber geopolymer concrete and hybrid steel–polypropylene-fiber geopolymer concrete. All the beams have the same diameters and the same internal reinforcement, so that the matrix and fiber systems may be assessed under the same circumstances. The flexural performance of the specimens is evaluated in terms of material strength, first-cracking load, load–deflection behavior, ultimate capacity, toughness and failure features. The damaged beams are repaired with externally bonded CFRP sheets after the first loading phase and reloaded for evaluating their residual stiffness, load capacity and strength-recovery efficiency. A nonlinear finite-element model is also built using ANSYS version 15.0.07 APDL and is verified against the original beam testing. Then, the validated model is applied to study the effect of increasing steel, polypropylene and hybrid-fiber contents from 0.75% to 1.25% on cracking resistance, load-carrying capacity, ultimate displacement and damage distribution. This integrated method of the inquiry enables the contributions of the geopolymer matrix, the internal fiber type and the exterior CFRP restoration to be distinguished, and offers a systematic foundation for the assessment of the structural performance and repairability of fibrous geopolymer concrete beams.
2. Experimental Work
2.1. Material
The materials used in the experimental program comprised ordinary Portland cement, fly ash, ground granulated blast-furnace slag (GGBS), sodium hydroxide, sodium silicate, natural fine aggregate, crushed coarse aggregate, superplasticizer, reinforcing steel, hooked-end steel fibers, polypropylene fibers, unidirectional CFRP fabric and epoxy resin. Their chemical compositions, physical characteristics, aggregate gradations and mechanical properties are summarized in the accompanying Table 1, Table 2 and Table 3.
Table 1.
Physical properties of the cementitious materials and aggregates.
Table 2.
Physical properties of ordinary Portland cement.
Table 3.
Oxide compositions of OPC, fly ash and GGBS.
The normal concrete reference mix was prepared using ordinary Portland cement Type I, supplied by Almas Cement Factory, Iraq. The properties of the cement tested were in accordance with Iraqi Standard Specification No. 5/1984 [32] as shown in Table 1, Table 2 and Table 3. The aluminosilicate precursors of the geopolymer binder were fly ash and GGBS, used in equal proportions. The fly ash was predominantly silica and alumina while GGBS provided a relatively calcium-rich fraction. The combination of these precursors aimed to balance repolymerization, setting behavior and strength development. All powdered materials were stored in sealed vessels under dry conditions prior to use.
Commercial sodium hydroxide flakes of purity of approximately 97% and an aqueous sodium silicate solution were used as the alkaline activator. A 14 M solution was prepared by dissolving sodium hydroxide flakes in potable water. The dissolution was strongly exothermic and was allowed to cool to room temperature before the solution was combined with sodium silicate. The activator was prepared 24 h before the concrete production in an effort to get a homogeneous and thermally stable solution. To ensure workability without excessive water addition, a polycarboxylate-based superplasticizer was added into the geopolymer mixtures at 2% of the total precursor mass.
The fine aggregate consisted of natural river sand, and the coarse aggregate was crushed stone. The coarse aggregate was washed prior to batching to remove dust and adhered contaminants that could weaken the aggregate–binder interface. Both aggregate fractions were air-dried to a surface-dry condition. Their physical properties and particle size distributions were experimentally determined and compared with the grading requirements of the Iraqi Standard Specification No. 45, as shown in Table 4 and Table 5.
Table 4.
Particle-size distribution of the fine aggregate.
Table 5.
Particle-size distribution of the coarse aggregate.
All beam specimens were reinforced with conventional deformed steel bars, whose measured properties are reported in Table 6. The longitudinal reinforcement consisted of two 10 mm diameter bottom bars and two 8 mm diameter top bars. The 8 mm bars had yield and ultimate tensile strengths of 462 and 609 MPa, respectively, with an elongation of 11.2%, whereas the corresponding values for the 10 mm bars were 546 MPa, 643 MPa, and 10.98%. Transverse reinforcement comprised 8 mm diameter stirrups spaced at 125 mm centers in the shear spans as shown in the reinforcement diagram in Figure 1. All beams had a rectangular cross-section of 150 × 250 mm and an overall length of 1500 mm. The clear concrete cover to the outer surface of the stirrups was 25 mm, giving an effective depth of 212 mm. The support span was 1400 mm, with symmetric two-point loading applied at locations 400 mm apart and 500 mm from the nearest support. The same reinforcement arrangement, cover, and loading geometry were used for all concrete types to facilitate comparison of their structural responses. As shown in Figure 2, Internal discontinuous reinforcement of steel fibers with hook ends and polypropylene fibers. The steel fibers were chosen because of their high stiffness, tensile strength and mechanical anchorage that enable bridging of emerging macrocracks, transfer of tensile stresses and enhancement of post-cracking resistance. Polypropylene fibers have been selected because of their chemical stability, low density, non-corrosive nature and resistance to degradation in alkaline environments. These fibers were mainly used to control the initiation of microcracks and to improve the crack distribution. The mono-fiber geopolymer mixtures contained either steel fibers at 0.75% by volume (58.8 kg/m3) or polypropylene fibers at 0.75% by volume (6.8 kg/m3). The hybrid mixture contained a total fiber volume fraction of 0.75%, shared equally between steel and polypropylene fibers. Each type contributed 0.375% by volume, corresponding to 29.4 kg/m3 of steel fibers and 3.4 kg/m3 of polypropylene fibers.
Table 6.
Properties of internal steel reinforcement and discrete fibers.
Figure 1.
Details of the standard beam dimensions.
Figure 2.
Hook-end steel fibers and polypropylene fibers.
The damaged beams were strengthened as external tensile reinforcement by the rehabilitation with SikaWrap® Hex-230 C unidirectional carbon-fiber fabric. The fabric was installed with the principal fibers parallel to the longitudinal axis of each beam. This orientation enabled the CFRP system to directly contribute to the flexural tensile resistance. Table 6 gives properties for both dry-fiber and cured-laminate conditions, as these values are not interchangeable: dry-fiber properties describe the carbon filaments themselves, laminate properties describe the combined carbon-fiber–epoxy system as used for structural calculations.
The CFRP fabric was impregnated with a two-component thixotropic epoxy resin Sikadur®-330 and bonded to the prepared concrete surface. Components A and B were blended in a mass ratio of 4:1 to achieve a uniform consistency. The epoxy system was chosen due to its compatibility with the CFRP fabric, satisfactory mechanical properties and strong adhesion to properly prepared concrete substrates. The CFRP fabric and epoxy propertise are shown in corresponding Table 7 contains the properties reported by the manufacturer.
Table 7.
Manufacturer-reported properties of the CFRP fabric and epoxy resin.
2.2. Mix Design for Conventional and Fibrous Geopolymer Concrete
The proportions of the mixtures were determined based on the standard geopolymer concrete design procedures described in earlier publications [36,37,38]. The experimental program comprised fifteen reinforced rectangular beam specimens, with three nominally identical specimens assigned to each of the five concrete groups: normal concrete (NC), plain geopolymer concrete (GPC), steel-fiber-reinforced geopolymer concrete (GPC-S), polypropylene-fiber-reinforced geopolymer concrete (GPC-P), and hybrid steel–polypropylene-fiber-reinforced geopolymer concrete (GPC-H). All specimens within each group had identical dimensions and reinforcement detailing. The reported experimental values represent the arithmetic averages of the measurements obtained from the three beam specimens in each group. This testing arrangement was adopted to improve the reliability of the comparisons between the investigated concrete systems.
The geopolymer binder was formulated utilizing fly ash and ground granulated blast-furnace slag (GGBS) as complimentary aluminosilicate precursors to provide an appropriate chemical composition for alkaline activation and formation of a cohesive binding matrix. The aggregate system was intended to provide an adequate granular skeleton. The alkaline activation was carried out by using sodium hydroxide and sodium silicate solutions. A polycarboxylate-based superplasticizer was also added to enhance the workability of the combination and to provide a homogeneous dispersion of constituents. The fiber-reinforced mixes were prepared using the same reference geopolymer matrix, without any deliberate alteration to the primary mix-design parameters, so that a systematic evaluation of the impact of individual and hybrid fiber inclusion was possible. Hooked-end steel fibers were chosen to improve crack bridging, post-cracking resistance and energy absorption, whereas polypropylene fibers were included mainly to reduce microcrack growth and to generate a more dispersed cracking pattern. The purpose of the hybrid structure was to integrate these complementing reinforcing mechanisms and to increase the overall cracking resistance of the geopolymer composite. The hybrid mixture contained a total fiber volume fraction of 0.75%, shared equally between steel and polypropylene fibers. Each fiber type therefore contributed 0.375% of the concrete volume, corresponding to steel and polypropylene-fiber contents of 29.4 and 3.4 kg/m3, respectively. The proportions of the constituents and the main characteristics of the mix design are described in Table 8. The experimental mix designations and the related fiber reinforcement configurations are shown in Table 9.
Table 8.
Constituent proportions and design parameters of the conventional and geopolymer concrete mixtures.
Table 9.
Identification and principal function of the investigated concrete mixtures.
2.3. Structural Beams Details and Studied Beams Variables
An experimental program of five reinforced rectangular beams was set up to study the impact of concrete matrix composition and fiber-reinforcement arrangement on flexural behavior. The tested specimens were conventional normal concrete (NC), plain geopolymer concrete (GPC), steel-fiber-reinforced geopolymer concrete (GPC-S), polypropylene-fiber-reinforced geopolymer concrete (GPC-P) and hybrid steel–polypropylene-fiber-reinforced geopolymer concrete (GPC-H). In an effort to guaranty the reliability of the comparative evaluation, all beams were built with the same geometrical configuration, internal reinforcement arrangements, concrete cover and boundary circumstances, the concrete matrix and fiber type being the main experimental variables. To preserve uniformity in the structural details of the specimen series, longitudinal tensile and compression reinforcement and closed transverse stirrups were provided in the reinforcement cage. All the beams were tested in symmetric four-point bending, which produces a constant-moment area and allows for the observation of flexural cracking and the subsequent development of failure. Pin and roller support were used to construct simply supported boundary conditions allowing longitudinal movement during loading. The structural reaction was monitored by recording the midspan displacements using a linear variable differential transformer (LVDT) and the strain development was measured using a strain gage attached to the longitudinal tensile reinforcement. The experimental setup allowed a consistent evaluation of the impacts of the concrete and fiber systems studied on load-carrying capacity, stiffness, deformation response and post-cracking behavior. Figure 1 shows the beam geometry, details of reinforcement and placement of loads.
2.4. Geopolymer Concrete Processing
The geopolymer concrete manufacturing process was carried out following a series of regulated steps that include the synthesis of alkaline activators, constituents batching, mixing, casting and curing, as shown in Figure 3. First, the sodium hydroxide pellets were dissolved in water to provide a 14 M alkaline solution. This concentration was chosen based on preliminary compressive-strength tests of the geopolymer mortar. Due to the exothermic dissolving process, the solution was allowed to cool down spontaneously to ambient temperature before mixing with the commercial sodium silicate solution with a SiO2/Na2O mass ratio of 2.4. The commercial sodium silicate solution was used as supplied. According to the product label, it contained 13.1–13.7% Na2O and 32–33% SiO2, with a specific gravity of 1.534–1.551. Assuming these are mass percentages and the remaining fraction is water, the estimated water content was 53.3–54.9% by mass. The activator obtained was homogenized well, kept in a tight container and conditioned for 24 h before combining. Then, the solid ingredients were weighted as per the preset mix proportions and the fly ash, GGBS, fine aggregate and coarse aggregate were first dry-mixed for 4–5 min for uniform distribution. The prepared alkaline activator, additional water, and commercial superplasticizer were then gradually added, and mixing continued for 4–5 min to obtain a homogeneous and cohesive mixture. The combined mass of the additional water and superplasticizer was 40 kg/m3, equivalent to 10% of the binder mass, comprising 32 kg/m3 of water and 8 kg/m3 of superplasticizer [39]. For the fiber-reinforced mixes, the corresponding fibers were added gradually during mixing to achieve uniform distribution within the geopolymer matrix and to reduce fiber aggregation. The fresh concrete obtained was then casted in the specified beam, cube, cylindrical and prismatic molds for the production of structural specimens and the preparation of samples for compressive, splitting tensile and flexural strength evaluations accordingly. The specimens were cast outside the laboratory at an ambient temperature of 37–40 °C and then stored within the laboratory at temperatures ranging from 25 to 30 °C. They were demolded 24 h after casting and covered with nylon sheets to prevent moisture loss until testing at 28 days. The curing technique for geopolymer concrete and conventional concrete reference specimens was same. Temperature data were taken both during casting and after demolding, and temperature was recorded continuously. The plain, steel-fiber-reinforced, polypropylene-fiber-reinforced and hybrid-fiber-reinforced geopolymer mixes were processed and cured in the same manner to ensure the consistency of the experimental conditions and to minimize the processing-related variability between the investigated specimens.
Figure 3.
Preparation, mixing, casting, and curing of geopolymer concrete.
2.5. External Strengthening Using CFRP Laminates
The previously evaluated reinforced-concrete beams were rehabilitated with an externally bonded wet-lay-up carbon-fiber-reinforced polymer (CFRP) system consisting of SikaWrap® Hex-230C unidirectional carbon-fiber fabric and Sikadur®-330 two-component epoxy resin, as shown in Figure 4. After the beams failed during loading at their ultimate capacities, the damaged specimens were realigned by applying an upward force at midspan with a hydraulic jack. The concrete soffit was mechanically prepared and cleaned to remove surface laitance, dust, loose concrete particles, and contaminants that could impair bonding. Particular attention was given to previously cracked regions to provide a suitable bonding surface. No crack injection was performed; epoxy was applied at the surface during CFRP installation rather than injected into the internal cracks. A single layer of CFRP fabric, 150 mm wide and 1000 mm long, was bonded longitudinally to the beam soffit as additional tensile reinforcement. The fabric covered the full soffit width, without end anchors or U-wraps. The two components of Sikadur®-330 epoxy were weighed and mixed at the manufacturer-specified mass ratio of 4:1 (A) until a homogeneous mixture was obtained. The adhesive was applied uniformly to the prepared soffit over the 1000 mm bonded length and to the contact face of the CFRP fabric. The fabric was then positioned and consolidated using a roller to promote resin impregnation, eliminate entrapped air, remove excess adhesive, and ensure close contact with the concrete substrate. Following installation, the rehabilitated specimens were stored in the laboratory for seven days to allow the epoxy to cure before retesting and evaluating their recovered load-carrying capacities.
Figure 4.
Wet-lay-up CFRP rehabilitation: fabric impregnation, bonding, and post-installation condition.
2.6. Life-Cycle Assessment and Economic Evaluation Methodology
A comparative life-cycle assessment (LCA) and economic evaluation were conducted to quantify the environmental and financial performance of the investigated reinforced-concrete beam systems. The assessment included the normal concrete reference beam (NC), plain geopolymer concrete (GPC), steel-fiber-reinforced geopolymer concrete (SF-GPC), polypropylene-fiber-reinforced geopolymer concrete (PP-GPC), and hybrid-fiber-reinforced geopolymer concrete (HB-GPC), in addition to their corresponding CFRP-rehabilitated configurations. The analysis was structured as a comparative cradle-to-gate plus rehabilitation assessment, in which the production of constituent materials, production-related energy, and CFRP rehabilitation were considered. The use phase, demolition, recycling, and final disposal were excluded because long-term service-life and end-of-life data were not available from the experimental program.
2.6.1. Functional Unit and Life-Cycle Inventory
In an effort to allow comparison of the tested concrete mixes, environmental and economic evaluations were carried out based on a consistent material inventory and a well-defined functional foundation. The functional main unit was considered to be one experimentally tested reinforced-concrete beam of nominal dimensions 150 mm × 250 mm × 1500 mm. All specimens were comparable in geometrical dimensions and basic reinforcing arrangement, giving a consistent foundation for comparison of the environmental and economic consequences of the varied concrete compositions. In addition to the beam-based evaluation, a performance-normalized indicator was used to tie the environmental effect and material cost to the experimentally obtained ultimate load capacity. The present supplemental indicator was represented as a global warming potential per unit of ultimate load (kg CO2-eq/kN) and material cost per unit of ultimate load (IQD/kN). It was created to enable comparisons between the material-associated environmental and economic impacts and the measured structural resistance of researched beams. However, such normalization is a comparative structural-performance indicator and not a service-life-equivalent functional unit, as the long-term durability, maintenance requirements and expected service life of the investigated alternatives were not established within the present experimental program. The concrete volume for the principal functional unit was calculated based on the nominal beam dimensions as follows:
where is the concrete volume of one beam , is the beam width , is the beam depth , and is the beam length .
For the investigated specimens:
The quantity of each constituent incorporated into one beam was obtained from:
where is the mass of constituent in one beam , and is the corresponding mixture quantity .
The material inventory was immediately created according to the selected experimental parameters shown in Table 8. Normal conventional concrete (NC) was made using 400 kg/m3 ordinary Portland cement (OPC) and geopolymer concrete (GPC) was made with a mixed aluminosilicate binder comprising 200 kg/m3 fly ash and 200 kg/m3 ground granulated blast-furnace slag (GGBS). The geopolymer matrix also included 650 kg/m3 fine aggregate, 1210 kg/m3 coarse aggregate, 120 kg/m3 sodium silicate solution and 60 kg/m3 sodium hydroxide solution. Emphasis was placed on the accounting of the polycarboxylate-based superplasticizer to maintain consistency between the experimental mix proportions and the environmental and economic inventory. The initial mix design called for a total of 40 kg/m3 of prepared superplasticizer solution, which was really 8 kg/m3 commercial superplasticizer and 32 kg/m3 carrier water. The exact quantity of superplasticizer used was 2% of the total geopolymer binder content (400 kg/m3). Therefore, the commercial admixture and carrier water were regarded as two different inventory components and assessed with their respective environmental emission factors and unit pricing. This separation avoided misallocation of the emission factor and market price of the commercial superplasticizer to the whole diluted solution.
The same reference geopolymer matrix was kept for the fiber-reinforced geopolymer mixes and the extra amounts of materials corresponding to steel fibers, polypropylene fibers and their hybrid combination were added according to the experimentally chosen proportions. So, the inventory included both environmental and economic contributions from the geopolymer matrix and the extra fiber-reinforcing elements.
This constituent-level inventory was the foundation for the calculation of material-related global warming potential and direct material procurement costs for each studied beam. All calculations were made on the basis of the same function and constituent-accounting technique to ensure consistency of the environmental and economic comparisons. The evaluation was limited to quantified material production inventory and expressly assessed CFRP restoration materials.
2.6.2. Iraqi-Market Economic Inputs
The economic evaluation was based on material prices representative of the Iraqi construction market. Local-market values were adopted for cement, aggregates, water, slag, chemical admixture, and fibers where suitable Iraqi data were available. For sodium hydroxide and sodium silicate, Iraq-specific import values were used as market proxies because these chemicals are predominantly supplied through imported sources. CFRP and epoxy costs were obtained from Iraqi-market supplier information. The baseline economic parameters adopted in the calculations are summarized in Table 10.
Table 10.
Adopted Iraqi-market material prices for the economic evaluation.
Because the local cost of fly ash can vary substantially depending on whether it is purchased commercially or obtained directly as an industrial by-product, the value in Table 10 was used as the baseline purchased-fly-ash scenario. A second sensitivity scenario was considered in which the purchase value of fly ash was substantially reduced, and only handling and processing costs were retained. This approach prevents the economic conclusions from being governed exclusively by one uncertain local-market parameter.
2.6.3. Environmental Impact Factors
Global warming potential (GWP), expressed in kg of carbon dioxide equivalent (kg CO2-eq), was chosen as the major environmental indicator to evaluate the impact of the component elements on climate change. The evaluation was performed on the basis of the cradle-to-gate emission factors attributed to the single ingredients. These parameters indicate the greenhouse-gas emissions associated with the manufacture of each material up to the factory gate as stated in the relevant LCA literature. The values used are shown in Table 11.
Table 11.
Adopted cradle-to-gate emission factors used in the LCA.
The emission factors shown in Table 11 were uniformly applied to the respective elements of all studied beam options to provide a similar foundation for comparative environmental assessment. But their interpretations have to be understood within the framework of the methodological assumptions on which the original LCA studies were based. In particular, the environmental loads associated with fly ash and GGBS are subject to the allocation methodologies used in the relevant source studies. Since these compounds are the by-products of industrial processes, the reported emission factors may vary depending on whether upstream production loads are attributed to the main manufacturing process, the by-product, or both. The comparatively low factors chosen for fly ash and GGBS should thus be read in accordance with their original allocation standards and not be understood as implying that these materials are devoid of environmental responsibilities.
Sodium silicate and sodium hydroxide environmental impacts were assessed separately as the manufacture of alkaline activators may be a significant part of the environmental effect of geopolymer concrete. Similarly, the emission factor associated with the superplasticizer was applied to the mass of the commercial admixture and not to the mass of the whole produced solution. So, the 40 kg/m3 of prepared superplasticizer solution described is understood to be 8 kg/m3 of commercial superplasticizer and 32 kg/m3 of carrier water. The emission factors were calculated based on these values. Such a difference is important to prevent an overestimation of the environmental impact of the admixture when applying its emission factor to the whole diluted solution. This interpretation has to be checked against the original experimental batching records.
The emission factors used give a consistent reference dataset for comparison and evaluation. However, the GWP numbers obtained still rely on the datasets, allocation assumptions and system limits chosen. The findings are thus taken as a comparative evaluation of the quantifiable environmental loads, and not as an externally validated environmental product statement. When assessing the environmental rankings of the mixes studied, the uncertainty of the emission factors of the main contributing elements should also be addressed.
2.6.4. Material-Related Global Warming Potential
The material-related GWP of each examined beam was calculated by multiplying the mass of each ingredient included in the beam with the relevant cradle-to-gate emission factor. Then, the overall material-related environmental effect was calculated by aggregating the individual contributions of all constituent materials as shown in Equation (4):
where () represents the material-related global warming potential of one beam (kg CO2-eq), () is the mass of constituent (i) incorporated into the beam (kg), () is the corresponding cradle-to-gate emission factor (kg CO2-eq/kg), and () represents the total number of constituent materials considered in the inventory.
The computation included regular Portland cement, fly ash, GGBS, fine and coarse aggregates, water, sodium silicate, sodium hydroxide, superplasticizer, steel fibers and polypropylene fibers, depending on the composition of each beam tested. For the fiber-reinforced geopolymer mixes, the extra environmental contributions from the included steel and polypropylene fibers were integrated based on their respective masses and emission factors. The environmental burdens connected to the quantitative production of the constituent materials are described by the ensuing material-specific GWPs. Impacts due to power consumption and CFRP restoration were examined independently in the following subsections and should be included to the overall environmental findings only when their respective inventory data are available and quantified in a consistent manner.
2.6.5. Energy-Related Environmental Impact
The electricity consumption during material preparation, concrete mixing, curing and CFRP restoration may be included in the total environmental effect of the evaluated structural systems. Where good statistics on energy use are available, the equivalent GWP may be calculated by multiplying the power used for each activity by the appropriate electrical-grid emission factor, as shown in Equation (5):
where () represents the electricity-related global warming potential (kg CO2-eq), is the electricity consumed during activity (j) (kWh), () is the electricity-grid emission factor (kg CO2-eq/kWh), and (r) denotes the number of activities included in the assessment.
The preparation and mixing of materials, curing and installation of CFRP may be included in the energy inventory, provided that the respective power consumption is monitored or reasonably calculated. For specimens cured under ambient conditions, the direct thermal curing-energy contribution is nil if no extra thermal energy is given. This assumption does not mean, however, that all additional power consumption connected to manufacturing is zero. If artificial thermal curing is used, it should be assessed in terms of the power consumption, and included in the evaluation with the relevant grid emission factor.
2.6.6. Environmental Assessment of CFRP Rehabilitation
The environmental burden associated with CFRP rehabilitation was evaluated separately because the CFRP strengthening system was installed only after the initial beam tests. The CFRP was externally bonded to the beam soffit over a strengthening length of 1000 mm.
The bonded CFRP area was determined from:
where is the CFRP width , is the bonded length , and is the number of CFRP layers.
The CFRP mass was determined using:
where is the CFRP areal mass .
The epoxy quantity was calculated as:
where is the epoxy consumption per unit bonded area .
The environmental impact associated with CFRP rehabilitation was subsequently calculated as:
where and are the corresponding production emission factors, and represents the energy required for surface preparation and installation.
The total GWP of each beam system was calculated as:
For specimens assessed before CFRP rehabilitation:
2.6.7. Economic Cost Calculation
The direct material cost of each beam was determined from:
where is the Iraqi-market price of constituent , based on the baseline values presented in Table 10.
The energy cost associated with mixing, curing, and other electrically powered operations was determined as:
where is the applicable electricity tariff .
2.6.8. CFRP Rehabilitation Cost
The total rehabilitation cost included CFRP fabric, epoxy adhesive, surface preparation, labor, equipment, and rehabilitation-related energy:
The CFRP material cost was determined as:
and the epoxy cost as:
where is the Iraqi-market price of CFRP per unit area and is the market price of epoxy resin per kilogram.
The total economic cost of each system was therefore determined from:
For the original beams prior to rehabilitation:
2.6.9. Performance-Normalized Environmental and Economic Indicators
Because the ultimate load capacities differed among the investigated beams, absolute GWP and total cost were normalized relative to structural performance.
The carbon-intensity index was determined from:
where is the experimentally determined ultimate load . A lower indicates a lower environmental burden per unit structural capacity.
Similarly, the cost-intensity index was calculated as:
where a lower indicates greater economic efficiency.
The corresponding carbon-efficiency index was expressed as:
while economic efficiency was evaluated as:
Higher values of and indicate improved structural performance relative to the associated environmental burden and financial expenditure, respectively.
2.6.10. CFRP Strength-Recovery Efficiency
The effectiveness of CFRP rehabilitation was quantified using the strength-recovery ratio:
where is the ultimate load after CFRP rehabilitation and is the original ultimate capacity of the corresponding beam before rehabilitation.
This parameter is particularly relevant to the present investigation because the CFRP-rehabilitated specimens recovered a substantial proportion of their original capacities.
The rehabilitation cost efficiency was further determined from:
where represents the rehabilitated load capacity obtained per unit CFRP-rehabilitation expenditure.
2.6.11. Sensitivity Analysis
A sensitivity analysis was undertaken because market prices, electricity conditions, and emission factors can vary substantially in the Iraqi context. The principal parameters considered were fly-ash price, GGBS price, NaOH and sodium-silicate prices, steel- and PP-fiber costs, electricity consumption, CFRP cost, and the relevant environmental factors. A ±20% variation around the baseline value was adopted:
where represents the baseline input and and are the corresponding lower and upper sensitivity limits.
The normalized sensitivity coefficient was calculated as:
where represents either total GWP or total cost.
For fly ash, two economic scenarios were considered: commercially purchased fly ash, represented by the value provided in Table 10, and a locally sourced industrial by-product scenario, in which the direct material purchase cost is substantially reduced and the expenditure is predominantly associated with processing. Reporting both scenarios provides a more realistic representation of the potential economic feasibility of geopolymer concrete under Iraqi supply-chain conditions.
3. Results and Discussion
3.1. Material Properties
Compressive strength was evaluated using 100 × 100 × 100 mm cubes following the British Standard, while splitting tensile strength was determined using cylinders measuring 100 mm in diameter and 200 mm in height according to ASTM C496 [40]. Flexural strength was evaluated using 100 × 100 × 400 mm prisms under symmetric four-point loading, with a support span of 300 mm and 150 mm between the loading points. Three specimens were tested for each test and for each concrete type at 28 days, and the reported strengths represent the average of the three sample results. All specimens followed the same ambient-curing procedure as the beam specimens and were tested immediately after removal of the nylon coverings. Fracture of the flexural specimens occurred between the loading points, and the testing machine recorded the total applied load in kN. Figure 5, Figure 6 and Figure 7 show the compressive, splitting tensile and flexural strengths of normal concrete (NC), geopolymer concrete (GPC), steel-fiber-reinforced geopolymer concrete (SF-GPC), polypropylene-fiber-reinforced geopolymer concrete (PP-GPC) and hybrid-fiber-reinforced geopolymer concrete (HB-GPC). The findings indicate that the addition of fibers had varying impacts based on the loading method and the fiber type. Steel fibers gave the largest increase in all three strength parameters examined. As indicated in Figure 5, the compressive strength rose from 34.62 MPa for NC to 37.60 MPa for GPC, which is an improvement of around 8.6%. The greatest compressive strength of 60.10 MPa was achieved by adding steel fibers, which is 73.6% higher than that of NC. The strength values of PP-GPC and HB-GPC were 40.86 MPa and 48.10 MPa, respectively, which were improved by 18.0% and 38.9%, respectively. The better performance of SF-GPC might be attributed to the steel fibers’ capacity to avoid the occurrence and propagation of internal microcracks, thereby enhancing the integrity of the concrete matrix under compression. However, the contribution of fibers to compressive strength is often less direct than to tensile and flexural behavior, as previously highlighted by Sathish Kumar et al. [41] and Wang et al. [42]. The findings of splitting tensile strength are shown in Figure 6. The strength of NC was 3.26 MPa and increased to 3.85 MPa for GPC. The maximum value was obtained for SF-GPC with 4.31 MPa, which is around 32.2% higher than NC. PP-GPC and HB-GPC showed 3.59 and 3.41 MPa, respectively, which are 10.1% and 4.6% higher. This improvement, especially in SF-GPC, largely comes down to the crack-spanning process where fibers bridging the growing tensile fractures transmit loads across the crack surfaces and retard crack propagation. The somewhat lower performance of HB-GPC in this test indicates that the hybrid fiber combination did not provide any appreciable tensile-strength improvement over steel fibers alone at the mixing proportions used. Sathish Kumar et al. [41] and Zhang et al. [43] observed similar effects of fiber bridging and impact of fiber type and volume percent on tensile behavior of geopolymer concrete. The flexural strength of the investigated mixes is shown in Figure 7 and follows a similar pattern. The flexural strength of NC and GPC were 7.59 MPa and 7.79 MPa, respectively. The greatest value was shown by SF-GPC with 13.28 MPa which is almost 74.8% higher than NC. The flexural strengths of PP-GPC and HB-GPC were 7.99 and 9.45 MPa, which were 5.3% and 24.4% higher than normal concrete. The significant improvement observed in SF-GPC is attributed to the high stiffness and tensile resistance of steel fibers which allow good stress transfer across flexural fractures and enhance resistance to crack opening. SF-GPC had a higher flexural strength than HB-GPC, but the improvement over NC shows a positive effect from the combination of multiple fiber types. This behavior is in agreement with the results obtained by Li et al. [44] showing that flexural performance may be improved by the steel–polypropylene fiber hybridization due to the complimentary crack-control mechanisms, and the geopolymer-specific findings published by Sathish Kumar et al. [41].
Figure 5.
Compressive strength for defernite concrete type.
Figure 6.
Split tensile strength for defernite concrete type.
Figure 7.
Flexural strength for defernite concrete type.
3.2. Structural Properties
3.2.1. Beam Flexural Behavior Under Statical Loads
The load–deflection response (Figure 8a) and the corresponding first-crack and ultimate loads (Figure 8b) of normal concrete (NC), geopolymer concrete (GPC), steel-fiber-reinforced geopolymer concrete (SF-GPC), polypropylene-fiber-reinforced geopolymer concrete (PP-GPC), and hybrid-fiber-reinforced geopolymer concrete (HB-GPC) are shown in Figure 8. From Figure 8b, it can be seen that the first-crack load of NC was 3.60 kN, which increased to 7.03 kN for GPC. The SF-GPC revealed the highest value of 10.52 kN, which is about 95.3% and 192.2% higher than NC, respectively. In contrast, the first fracture loads for PP-GPC and HB-GPC were 5.33 and 5.83 kN, respectively. SF-GPC had the greatest ultimate load capacity of 106.96 kN, followed by GPC (99.64 kN), HB-GPC (97.60 kN), NC (92.73 kN) and PP-GPC (94.44 kN). The results demonstrate that the addition of steel fiber was extremely effective in improving the crack initiation resistance and ultimate load capacity, with percentage increases of around 192.2% and 15.4%, respectively, in comparison with NC. The load–deflection curves in Figure 8 also reveal the differences in the post-cracking behavior. The NC response exhibits a gradual increase in load up to the maximum load, and then a sharp decrease in load at larger deflections. Conversely, the fiber-reinforced mixtures often sustain higher loads after the initial fracture, which shows a superior resistance to crack propagation and a better load transfer after breaking. The SF-GPC shows the steepest beginning load development and the highest peak load, which is in accordance with the effective bridging action and relatively high stiffness of steel fibers. However, HB-GPC shows a more stable load-bearing behavior over a greater range of deflections, which suggests superior deformation capacity and longer post-cracking resistance. The PP-GPC curve shows a comparatively lower ultimate load and a less important rise in peak resistance. This behavior is attributed to the lower elastic modulus of polypropylene fibers and their restricted capability to absorb high tensile loads soon after crack formation. This is in agreement with the results of Bhutta et al. [45] who studied the flexural behavior of steel- and polypropylene-fiber-reinforced geopolymer composites. Li et al. [44] reported that hybrid steel–polypropylene fiber systems can enhance post-peak ductility, toughness and load retention due to the complementary fiber-reinforcement mechanisms. Similar gains in initial crack load, ultimate capacity and post-cracking behavior have also been observed for hybrid-fiber-reinforced geopolymer concrete beams by Sathish Kumar et al. [41].
Figure 8.
Load–deflection curve and ultimate and first-crack load. (a) Load–deflection curve and (b) ultimate and first-crack load.
3.2.2. Toughness and Ductility of the Tested Beams
Figure 9 and Table 12 compare the toughness, defined here as energy absorbed up to peak load, of normal concrete (NC), geopolymer concrete (GPC), steel-fiber-reinforced geopolymer concrete (SF-GPC), polypropylene-fiber-reinforced geopolymer concrete (PP-GPC), and hybrid-fiber-reinforced geopolymer concrete (HB-GPC) beams. Table 12 also presents the displacement ductility indices and energy absorption at a common deflection of 15 mm. Toughness (energy absorbed up to peak load) was calculated as the area under the load–deflection curve from the start of loading to the deflection corresponding to the maximum recorded load. It was calculated numerically using the trapezoidal rule and expressed in kN·mm. This measure represents the energy absorbed by the beam up to its maximum load-carrying capacity and excludes the post-peak response. The findings show that the maximum toughness (energy absorbed up to peak load) was obtained in HB-GPC (2407.5 kN·mm), followed by GPC (1698.8 kN·mm), PP-GPC (1580.1 kN·mm), NC (1521.4 kN·mm) and SF-GPC (1318.2 kN·mm). Compared with NC, HB-GPC showed an increase of around 58.2%, and GPC and PP-GPC showed increases of 11.7% and 3.9%, respectively. SF-GPC, however, showed a reduction of around 13.4%, although it had the greatest ultimate load capacity of all the mixes studied. This result shows that the largest load resistance does not always mean the highest energy absorption, since toughness relies on the load resisted and the deformation attained during the test. HB-GPC exhibited an energy absorption up to peak load of 2407.5 kN·mm, exceeding SF-GPC and PP-GPC by approximately 82.6% and 52.4%, respectively. This observed improvement does not, by itself, establish synergy between the two fiber types. Steel fibers may facilitate stress transfer across cracks, while polypropylene fibers may contribute to controlling crack development and distribution. These complementary effects offer a possible explanation for the response of HB-GPC, but their individual contributions and interaction were not directly verified experimentally. Related hybrid-fiber behavior has been reported by Banthia and Trottier [46] and Li et al. [44]. The tangent-intersection technique was used to assess displacement ductility from the load–deflection curves [47]. The conventional approach defines ductility as the ratio of peak-load deflection () to equivalent yield deflection (), expressed mathematically by the following equation:
where δu is the midspan deflection at the maximum recorded load and δy is the equivalent yield deflection determined from the load–deflection curve. Accordingly, this index characterizes displacement ductility up to peak load and excludes post-peak deformation.
Figure 9.
Toughness (energy absorbed up to peak load) for defernite concrete type.
Table 12.
The ductility and toughness (energy absorption up to peak load and at a common deflection of 15 mm).
As presented in Table 12, the ductility indices were 1.19, 1.65, 2.84, 2.30, and 3.46 for N.C, GPC, S.F-GPC, P.P-GPC, and H.B-GPC, respectively. GPC exhibited a higher index than N.C, while all fiber-reinforced geopolymer beams exhibited higher indices than the GPC beam without fibers. H.B-GPC achieved the highest index, followed by S.F-GPC and P.P-GPC, indicating a greater relative deformation interval between equivalent yielding and peak load. Nevertheless, a higher index does not necessarily indicate a larger absolute deflection: S.F-GPC exhibited a lower peak-load deflection than GPC but a higher ductility index because of its smaller equivalent yield deflection.
To provide a consistent comparison despite differences in peak-load deflection, energy absorption was additionally evaluated at a common deflection of 15 mm, which preceded the peak load in all groups. Energy absorption was calculated as:
where is the applied load in kN and is the integration limit in mm, giving energy in kN·mm.
Integration was performed using the trapezoidal rule, with linear interpolation between adjacent recorded points where required. For energy absorption up to peak load, was the deflection corresponding to the maximum recorded load of each beam, and the post-peak response was excluded. For the common-deflection comparison, was fixed at 15 mm. The energies absorbed up to 15 mm were 271.6, 596.1, 1143.1, 804.3, and 821.4 kN·mm for N.C, GPC, S.F-GPC, P.P-GPC, and H.B-GPC, respectively. Although H.B-GPC exhibited the highest energy absorption up to peak load, S.F-GPC absorbed the most energy within the common deflection interval. This distinction demonstrates the influence of the integration limit on the comparison. The value for H.B-GPC at 15 mm should be interpreted cautiously because it relies on linear interpolation across the relatively large interval between recorded deflections of 9.316 and 32.24 mm.
3.2.3. Residual Strength of Beam After CFRP Repair
Figure 10 shows the load–deflection behavior of the concrete beams after rehabilitation with carbon-fiber-reinforced polymer (CFRP), while Table 13 compares their original and post-rehabilitation ultimate loads. The normal concrete (N.C) beam attained 82.33 kN after rehabilitation, corresponding to 88.78% of its original ultimate load of 92.73 kN. GPC reached 82.64 kN, with a capacity recovery of 82.94%. S.F-GPC attained 84.787 kN but exhibited the lowest recovery ratio, 79.27%, owing to its highest original ultimate capacity of 106.962 kN. P.P-GPC reached 81.01 kN, recovering 85.78% of its original capacity of 94.44 kN. H.B-GPC exhibited both the highest post-rehabilitation ultimate load, 87.66 kN, and the highest recovery ratio, 89.82%. However, these two measures are distinct: a higher recovery percentage does not necessarily imply a higher post-rehabilitation ultimate load, because the percentage is normalized by each beam’s original capacity. The load–deflection curves also reveal differences in post-rehabilitation response. N.C and GPC maintained relatively stable loads over portions of their deformation ranges, whereas S.F-GPC reached its peak at a comparatively small deflection. P.P-GPC exhibited a pronounced load reduction after the peak, while H.B-GPC maintained relatively high loads over the widest recorded deflection range, extending to approximately 55 mm. These observations indicate favorable load retention over an extended deformation range for the rehabilitated hybrid-fiber beam. This response reflects the combined behavior of the damaged beam and the rehabilitation system; the individual contribution of CFRP was not isolated experimentally. However, the post-rehabilitation response may be influenced by the bond between the CFRP and the concrete substrate, the extent of pre-existing damage, and potential failure modes such as interfacial debonding or CFRP rupture. These mechanisms have been observed in studies by Zhuang et al. [48] and Hamah-Ali and Abdul Qadir [49] using experimental studies on damaged and rehabilitated reinforced-concrete beams, and have been shown to affect the recovered capacity and deformation response depending on the initial damage state and the CFRP strengthening configuration [50]. Overall, the rehabilitated beams recovered 79.27–89.82% of their original load-carrying capacities. The favorable response of H.B-GPC may reflect complementary crack-bridging effects within the hybrid-fiber and CFRP rehabilitation system. The reported percentages represent post-rehabilitation capacity relative to the original capacity, rather than strength gains attributable solely to CFRP. Since no damaged control beam was retested without CFRP, its contribution could not be quantified separately.
Figure 10.
Load–deflection curve for repair beams.
Table 13.
Ultimate load capacity before and after CFRP rehabilitation.
To record the damage that occurred prior to being rehabilitated, Figure 11 illustrates the visible cracking that remained from the initial load test prior to reloading. NC displayed a large, primarily open crack close to midspan along with small amounts of fragmented concrete. GPC exhibited mainly vertical cracks with several branches growing upward from the bottom surface. SF-GPC had cracks at midspan with some fragmentation of the concrete, as well as spalling on the lower portion of the beam. PP-GPC displayed a series of closely spaced vertical and branching cracks while HB-GPC displayed one large crack at midspan with some branching. Maximum crack widths were about 25 mm for NC, 5 mm for GPC, 10 mm for PP-GPC, and 15 mm for HB-GPC. SF-GPC showed localized concrete spalling near the soffit, and it was estimated that the crack width would be between 4 and 8 mm when measured at a near distance from the spalled area. Photos show the remaining visible damage from the first test before the second test began.
Figure 11.
Visible cracking remaining from the initial loading tests before reloading.
4. Theoretical Program
The theoretical study was established to develop a nonlinear finite-element model for the reinforced geopolymer concrete beams and then apply the validated numerical framework to expand the experimental investigation using a parametric study design. The numerical evaluation utilized the ANSYS Parametric Design Language (APDL) where analyses aimed to replicate beams flexural response from experimental testing in their original, unstrengthened states and then progressed towards assessing the influence of different fiber-content configurations. The computer-based analysis uses the same logical order established in the numerical example description: finite element formulation, material behavior modeling, comparison versus experimental response and finally parametric numerical study. The finite-element model was developed to recreate the geometry of the experimentally tested beam configuration, along with its reinforcement arrangement, material properties, support conditions and applied loading. The nonlinear behavior of the concrete matrix and reinforcing steel is especially important, as the bars pass through a series of stages that range from initial elastic deformation to cracking, stiffness degradation, stress redistribution and ultimate failure. Experimental flexural testing had been utilized in order to study and analyze the structural performance of geopolymer concrete beams with different fiber systems, while numerical simulation provides a computational tool for investigating the effect of incorporated fibers on load-carrying capacity and deformation behavior.
4.1. Finite-Element Modeling
The experimental investigation was validated by numerical analysis as shown in Figure 12, where the beams were simulated using ANSYS APDL to ensure the accuracy of the results. The beams were modeled taking into account the effects of geometry and material nonlinearity during the analysis. In the preprocessing stage, the elements that would be used for the materials were selected, and even the real behaviors including loading and boundary conditions were input in order to emulate the same environment as an experimental test. Constitutive models were used to define the material behavior. Constitutive relations based on smeared and brittle cracking models were selected to predict the nonlinearity of concrete, which is considered a quasi-brittle material. Finite-element analysis using ANSYS APDL was performed on five beams for verification. The verification was accomplished against the experimental tests, with comparisons conducted using load–displacement correlations, ultimate load and displacement, and crack patterns [51,52,53]. In order to evaluate the sensitivity of the experimental beam models to mesh size, four different mesh sizes were evaluated for each experimental beam model (with element sizes ranging from 40 to 27 mm; see Table 14). For each experimental beam model, the change in Pu was found to be less than 6.4 percent when the results from the two finest meshes were compared. Therefore, the selected mesh of 2966 elements was determined to ensure mesh-independent results. All experimental beam models used a nonlinear solution procedure based on the full Newton–Raphson method, with force and displacement convergence criteria of 0.01 and 0.005 load sub-steps, respectively. Shear transfer coefficients were selected as 0.45 for open fractures and 0.90 for closed fractures [54,55,56,57,58]. All shear transfer coefficient values less than 0.2 produced problems with convergence.
Figure 12.
Finite-element modeling.
Table 14.
Mesh analysis for simulation of GPC-S Model.
A total of 2966 elements are included in the finite-element models. A convergence criterion was used based on the mesh and input results, whereby it could be observed that non-convergence happened below 0.2 of the open and close shear transfer coefficients.
4.1.1. Concrete, Steel Reinforcement and Fibers
Concrete is a semi-brittle material with tension–compression asymmetry. For the compression side, the concrete stress–strain curve is linearly elastic up to ~30% of σcu (maximum compressive strength). The stress continues to increase steadily until it reaches the peak stress after the yield point. Then, the ultimate compressive strength (σcu) is reached, and the stress starts to drop into the softening region until failure occurs at the maximum strain (εcu). As for tension, the curve is elastic and increases linearly until the value is value equal to the ultimate tensile strength. Following this, concrete cracks form up to 10 mm and the loss in strength eventually reach zero [59]. To define concrete properties in ANSYS, it is necessary to define the ultimate uniaxial compressive strength, ultimate uniaxial tensile strength (modulus of rupture), elastic modulus (E), Poisson’s ratio (μ) and a reduction factor of stiffness for the cracked tensile condition. For all cases, 10% of the compressive strength was assumed as the tensile strength of the concrete [59]. Constitutive models were used for normal concrete under uniaxial compression according to Kachlakev et al. [60], while for HSC, the Modified Stress–Strain Relation was used, according to Hsu and Hsu [61]. The concrete behavior is simulated using a plasticity-based damage model. In ANSYS, concrete is modeled using the SOLID65 element, which has eight nodes with three degrees of freedom at each node, and can simulate plastic deformation, cracking and crushing. In the case of steel- and PP-fiber-reinforced concrete, a smeared model was used to identify the model of this type of concrete, in which embedded fibers are present inside the Solid65 concrete element at varying orientation angles. In Solid65, a real constant enables users to define the volume ratio of fibers compared to the element volume (α) with orientation angles (horizontal and vertical). Most characterizations have values for the shear transfer coefficients (up to 1) where a smooth crack (complete loss of shear transfer) is indicated by a value of zero, and a rough crack (no loss of shear transfer), a unity value of (1.0) [62]. In the case of open cracks, a shear transfer coefficient 0.45 was used, and for closed cracks it was set to 0.9. The bilinear isotropic material was used to represent steel reinforcement based on the Von Mises failure criterion which behaves identically in tension and compression [63]. In this study, the reinforcing steel with Poisson’s ratio μ = 0.3 was also considered. Steel bearing plates were modeled with linear behavior. In order to avoid the stress concentrations in these regions, bearing plates were modeled in ANSYS. All the steel plates and reinforcements were modeled with Youngs modulus E = 200 GPa. Link180 was employed to model the longitudinal rebar and stirrups. Solid185 was also used in these beams to model the bearing plates of steel at loading and support points.
The concrete used in the study was modeled using SOLID65 elements, and the Willam–Warnke failure criterion. The Poisson’s ratio for all types of concrete mixtures was set at 0.2, while their elastic moduli are listed in Table 15 (and were calculated as approximately 4700√fc′ MPa). In addition, each mixture displayed a multilinear stress–strain behavior during compression tests, which is shown in Figure 13. All concrete mixtures were assumed to have a tensile strength that equaled 10 percent of their respective compressive strengths. Since SOLID65 does not allow for post-ultimate load fracture energy softening behavior, no tension–softening curve based on Gf was utilized. Additionally, crushing was turned off to assist with convergence. The reinforcement used in the study was modeled with LINK180 elements as a bilinear elastic–plastic material. Specifically, the Ø10 bars had fy = 420 MPa and fu = 550 MPa, while both the Ø8 bars and stirrups had fy = 400 MPa and fu = 530 MPa, with Es = 200 GPa, and a tangent modulus of 2 GPa. A perfect bond was assumed between the reinforcing bars and the concrete through common node connectivity. Fibers were modeled as smeared reinforcement within the SOLID65 elements at volume ratios identified in Table 15. These fibers were aligned along the longitudinal axis of the beam (θ = 0°, φ = 0°). The steel fibers had E = 200 GPa; the polypropylene fibers had E = 4 GPa; and the hybrid mixture was considered as having a single equivalent material with a volume-weighted modulus of 102 GPa. The assumed tensile strength of 0.10 fc′ is within six percent of the experimentally determined splitting strength of NC and GPC; however, it is larger than the experimental splitting strength of GPC-S (39%), GPC-P (14%), and GPC-H (41%) (Table 15). Since a SOLID65 element cracks when the maximum principal tensile stress equals this value, this assumption postpones the first predicted cracking of the fiber-reinforced beams and contributes to the higher-than-expected first-cracking loads.
Table 15.
Concrete properties and tensile-strength assumption.
Figure 13.
Plastic damage curve of ordinary concrete under uniaxial compression [19].
The fiber volume ratios of the hybrid models were varied while maintaining the same compressive strengths, elastic moduli and tensile strengths as the 0.75% mixtures. The volumes of steel and polypropylene fibers in the hybrid models were maintained as equal (0.50% + 0.50% at 1.00%; 0.625% + 0.625% at 1.25%).
4.1.2. Verification of Finite-Element Modeling
As shown in Figure 14, five-beam verification procedure had model inputs that were obtained from material testing and ACI 318 equations, and there was no adjustment of the beams’ response to these inputs. Thus, the comparison made here is a verification of the modeling approach used, not independent calibration. The model was found to accurately reproduce the ultimate load with error values ranging from 0.56% to 6.02%. Also, it was observed to overestimate the first-cracking load of the fibrous beams. In addition, the model was found to be more rigid than what was found during testing with initial stiffness being approximately 8–14% greater, and predicted peak displacement was within 2–6%. The results of five experimentally tested beams (the normal concrete beam denoted as N.C.; the plain geopolymer concrete beam, GPC; reinforced geopolymer concrete beam, GPC-S; polypropylene-fiber-reinforced geopolymer concrete beam, GPC-P; and hybrid-fiber-reinforced geopolymer concrete beam, GPC-H.) were chosen as reference samples for the finite element verification as shown in Table 16. The numerical models were created based on the exact same beam geometry, layout of reinforcement, material properties as well as support conditions and loading scheme used in the experimental program. Verification was undertaken with respect to the numerical predictions based on experimental load–deflection responses. The comparison demonstrated reasonable agreement between experimental and numerical responses, especially for the whole load-carrying behavior as well as the ultimate load capacity. The GPC, GPC-S, GPC-P and GPC-H beams predicted ultimate loads for FE models of 100.20 kN, 102.88 kN, 95.88 kN and 99.05 kN for experimental ultimate loads: 99.64 kN, 106.96 kN, 90.44 kN and 97.60 kN, respectively. The respective differences in the ultimate load are 0.56%, 3.82%, 6.02% and 1.49%. The small variations observed show that the adopted finite element formulation was able to reproduce the main load-carrying response of the experimentally tested geopolymer concrete beams. This was evaluated not only based on the ultimate load, but also by obtaining complete load–deflection curves for comparison with the experimental tests. The numerical results followed the experimental response within the same displacement range, with correlation coefficients of GPC: ∼0.955; S.F.-GPC: ∼0.964; GPC-P: ∼0.951; and GPC-H: ∼0.960 beams.
Figure 14.
Load–displacement curves clarifying the verification work.
Table 16.
Verification results.
4.1.3. Parametric Study
A numerical parametric study was also performed using the validated finite-element model developed in ANSYS APDL to explore the impact of fiber content on the structural behavior of geopolymer concrete beams. In this parametric study, the objective was to analyze the impact of higher fiber content compared with the experimentally explored configuration keeping beam geometry, reinforcement configuration, constraints and basic finite element formulation similar. Based on the types and sizes of fibers, three fiber-reinforced geopolymer concrete systems were selected as follows: steel-fiber geopolymer concrete (GPC-S), polypropylene-fiber geopolymer concrete (GPC-P) and hybrid-fiber geopolymer concrete (GPC-H), as listed in Table 17. The parametric models were structured based on the 0.75% fiber content mode, which is estimated from the experiment; two other numerical models were established by increasing another fiber content (1.00 and 1.25%) for each beam. Therefore, the steel-fibers series (GPC-S-0.75%, GPC-S-1.0%, and GPC-S-1.25%), GPC-polypropylene-fiber series (GPC-P-0.75%, GPC-P-1.0%, and GPC-P-1.25%), and hybrid model series (GPC-H) were developed, as listed in Table 18. The corresponding numerical matrix facilitated the independent assessment of fiber ratio effects, and comparisons were subsequently made between the beams. The parameter study investigated mainly changes in cracking load, ultimate load, ultimate displacement and load–deflection response due to increased fiber content. The numerical results were then compared within each fiber system to quantify how much of these improvements can be attributed to the increased fiber content and which of the different systems offered an advantageous combination of load-bearing capacity and response to deformation.
Table 17.
Parametric FE models.
Table 18.
Parametric FE results.
4.2. Results of the Parametric Study
For the fibrous concrete, the comparison between three numerical models GPC-S-0.75%, GPC-S-1.0%, and GPC-S-1.25% showed that increasing the steel-fiber content resulted in an improvement in the predicted load–displacement response. The ultimate load of GPC-S-0.75% was 102.88 kN, while this increased to 118.40 kN for GPC-S-1%, and for the contents of fibers which are equal to 1.25%, it is equal to 128.70 kN. Therefore, steel fiber (0.75% to 1.00% and also at 1.25%) increased the predicted ultimate load by 15.1% and 25.1%, respectively, compared to the reference beam. This additional fiber content also provided a significant enhancement to the predicted cracking resistance. The cracking load increased from 16.68 kN at 0.75% fiber content to 20.52 kN at 1.00%, and finally, a remarkable increase to 28.49 kN for 1.25%. The values represent increases of 23.0% and 70.7%, respectively, compared to the reference model. The larger increment of 1.25% also shows that steel fiber plays a more visible role under this higher ratio as it mainly slows down the transition from primary response to quasi-static cracked cases during loading. First-cracking load differences result from different methods used to determine when first cracking occurs. On one hand, experimentally, first cracking is identified by either the load at which the first visible hairline crack forms, or when the load–deflection curve first changes. Therefore, experimental first cracking represents the actual initiation of microcracks due to shrinkage and/or handling defects. On the other hand, in the finite-element analysis (FEA), SOLID65 utilizes a smeared-crack approach. This means that cracking is only flagged at an integration point when the maximum tensile stress exceeds the specified tensile strength (0.10 fc′) in a continuous homogeneous medium with a uniform distribution of fibers. Consequently, FEA predicts later and more idealized cracking. Thus, only ultimate load and overall performance can be verified. An increase of this nature was manifested in the displacement corresponding to the ultimate load. The ultimate displacement increased from 20.34 mm predicted for GPC-S-0.75%. The displacement measured depths of 26.70 mm and 30.65 mm for GPC-S-1.0% and GPC-S-1.25%, respectively. Consequently, supplementing the ultimate load with an increase in steel-fiber content also significantly improved the deformation capacity of the beam. The increasing trend of the cracking load, ultimate load and ultimate displacement with the increase in steel-fiber contents showed that higher steel-fiber contents have a better response in the investigated range.
4.2.1. Effect of Polypropylene-Fiber Content
The numerical models GPC- P-75%, GPC-P-1.0%, and GPC-P-1.25% were used to explore the effect of polypropylene-fiber content on flexural response. The load–deflection responses for this variable are shown in Figure 15. Results showed that increasing the polypropylene-fiber content induced a stepwise increase in the estimated load-carrying capacity. For GPC-P-0.75% the ultimate load was increased from 95.88 kN to 107.20 and 116.2 kN for ratios of 1.0% and 1.25% fiber contents, respectively. Similar increases of 11.8% and 21.2% were observed, respectively, relative to the model reference of 0.75%. The same trend was also observed for cracking load. As noted in Table 10, the predicted cracking load of the reference specimen GPC-P-0.75% was 15.22 kN, which increased to 18.85 kN at 1.0% and 24.95 kN at the maximum ratio of 1.25%. These values are increases of 23.9% and 63.9%, respectively, over the base model. The significant increase in cracking load at higher fiber content, predicted greater resistance to initiation of the nonlinear response achieved with the 1.25% configuration than for any model using unbounded polypropylene-fiber composites investigated in this study. Unlike the ultimate load and cracking load, there is less variation in ultimate displacement. The maximum displacement predicted increased from 31.68 mm for GPC-P-0.75% to 32.80 mm for GPC-P-1.0%, while the GPC-P-1.25% model reverted to 31.68 mm. Thus, additional polypropylene-fiber content did not yield a corresponding increase in displacement at ultimate load even though cracking and ultimate capacity both increased significantly. In general, the numerical results show that both load-carrying capacity and cracking resistance of the beams were mainly improved by increasing polypropylene-fiber content from 0.75% to 1.25%, while ultimate displacement was less affected across this range of investigated numbers.
Figure 15.
Effect of steel-fiber content on the FE load–deflection response.
4.2.2. Effect of Hybrid-Fiber Content
The flexural response of geopolymer concrete beams GPC-H-0.75%, GPC-H-1.0%, and GPC-H-1.25% was evaluated to study the effects of hybrid-fiber content. As illustrated in Figure 15, a higher ratio of hybrid fibers enhanced the predicted structural response moderately. The maximum load was 99.05 kN for the reference model with a value at 0.75% and increased to 120.30 and 128.80 kN corresponding to the 1.00% and 1.25% configurations. Such increases translate to 21.5% and 30.0% relative to GPC-H-0.75%, respectively. The relationship between the cracking load and hybrid-fiber content showed a similar trend, but with a steeper increase at higher hybrid-fiber contents. At 0.75%, the predicted value was 14.1 kN, while at 1.00% it increased to 22.58 kN and at 1.25% it finally reached a value of 26.26 kN. As a result, the cracking load increased in relation to the reference configuration by about 60.14% and 86.24% when compared with the ratio of 0.75%. This remarkable value demonstrates that hybrid-fiber system presents an increasing effectiveness in resisting the formation of first nonlinear response with increasing fiber content. The ultimate displacement also showed significant enhancement. The forecasted vertical displacement increased from 54.63 mm for GPC-H-0.75% to 62.5 mm for 1.00%, and 70.32 mm for 1.25%. These are equivalent to about 14.4% and 28.7% increases, respectively. As a result, the hybrid-fiber models experienced continuous growth both in load capacity and deformation capacity over the entire range of fiber content, which is unlike what was observed for the polypropylene-fiber series. The significant effect of hybrid-fiber content on predicted flexural response is shown in the joint increase in cracking load, ultimate load, and ultimate displacement.
4.2.3. Crack Pattern and Failure Mode
The crack patterns, failure mode and stress distribution of geopolymer concrete beams with different fiber contents and type are clearly represented in Figure 16. The largest flexural capacity of most models was achieved due to the formation of links by materials bridging cracks and increasing energy dissipation, sustained in cooperation between the surrounding concrete particles and absorbed energy (by tensile stiffening) through the equilibrium shift within this zone. The patterns of cracking show that the damage occurs predominantly in flexural (rather than as a simultaneous localized shear failure). In the steel-fiber series, as the fiber content increases from 0.75% to 1.0% and 1.25%, a more distributed damage pattern and larger stress field along the beam is generated again. The GPC-S-1.25% model shows the largest stress redistribution within this series, with the highly stressed area less focused in a single location. Such behavior is in agreement with the results of parametric analysis demonstrated earlier. The same trend is found for the polypropylene-fiber models; in this case, as the fiber content increases, the degrees of maximum stresses increase and the damage concentration changes to a different distribution in the central region. However, the shift in the deformation response is not as dramatic as that seen for steel- and hybrid-fiber systems. The combined-fiber models show the most pronounced evolution of a distributed stress field with fiber content. As shown in Figure 16, a fiber-proportional distribution of stress is extended throughout the beam at 1.25% hybrid fibers and damage occurs over less area than in localized regions, which signifies more efficient internal stress redistribution. The increasingly widespread stress field that occurs with increased fiber content results from the fibers delaying localization of damage due to their improved post-cracking stress-transfer capacity, allowing stresses to be transmitted across forming cracks.
Figure 16.
Crack pattern and stress distribution of simulated beams.
4.3. Life-Cycle Assessment and Economic Evaluation
Finally, large disparities in the analyzed concrete systems were found during environmental and economic evaluation. This demonstrates that advances in mechanical performance do not always correlate with a decrease in embodied carbon or material cost. The comparison was consequently carried out on three complimentary bases: per cubic meter of concrete, each test beam and per unit of ultimate load capacity. Moreover, a sensitivity analysis was carried out to study the effect of fly-ash procurement on the economic feasibility of geopolymer concrete in Iraqi market conditions. Finally, the additional environmental and financial implications of CFRP rehabilitation were evaluated.
4.3.1. Environmental and Economic Performance per Cubic Meter
The environmental and economic performance of the tested concrete mixes were evaluated by comparing the material production costs and the material-related global warming potential (GWP) per cubic meter. The results of Table 19 illustrate the trade-off between environmental performance and cost of materials associated with the replacement of ordinary Portland cement (OPC) with a fly ash-GGBS geopolymer binder, and the use of different fiber-reinforcing techniques. The normal concrete (NC) had the lowest cost of material production (57,474 IQD/m3) but the greatest GWP (302.98 kg CO2-eq/m3). In contrast, plain geopolymer concrete (GPC) had the lowest GWP among the investigated combinations at 165.31 kg CO2-eq/m3, which is a reduction of about 45.4% compared to NC. The reduction demonstrates the environmental benefit of a fly ash–GGBS geopolymer system compared to an OPC-based binder when the environmental burdens from the manufacturing of alkaline activators are included. However, this improvement was associated with significant increase in material cost (461.066 IQD/m3). The rise in cost was largely due to the acquisition of sodium silicate and sodium hydroxide and the rising price of fly ash. The addition of polypropylene fibers led to a GWP of 180.27 kg CO2-eq/m3 for PP-GPC, which is 40.5% lower than NC. The cost of material was 551,732 IQD/m3, which showed that the environmental advantage of the geopolymer binder was largely maintained despite the higher cost of the fiber reinforcement. In contrast, the hybrid-fiber geopolymer concrete (HB-GPC) showed a moderate environmental performance with a GWP of 246.29 kg CO2-eq/m3, which shows a reduction of 18.7% compared to NC. The material cost was 770,999 Iraqi dinars per cubic meter. Among the tested choices, the SF-GPC combination had the highest GWP (312.31 kg CO2-eq/m3), which was around 3.1% greater than the NC reference. It also had the greatest material cost (990,266 IQD/m3). This finding is attributed to the high environmental cost and material cost of steel fiber production, which partially offsets the benefits obtained from the replacement of OPC by the geopolymer binder. The differences in the material costs found were largely influenced by the price of the alkaline activators and the increased costs owing to the fiber reinforcing. The major cost factors in the geopolymer mixes were sodium silicate and sodium hydroxide. In particular, the use of steel fibers caused a large increase in the cost of materials. These findings are in line with the observations of Fernando et al. [64] who found that alkaline activators were the primary contributors to the environmental and economic impacts of fly-ash-based alkali-activated concrete. Similarly, Martínez and Miller [65] noted that the reduction in greenhouse-gas emissions that geopolymer technology may accomplish would have to be compensated for by increased manufacturing costs owing to the need for chemical activators. Tushar et al. [66] have shown that the quantities and manufacturing effects of the alkaline activators are the key factors affecting the environmental performance of geopolymer concrete. The impact of the selection of the precursor and activator on the GWP of the geopolymer combinations was also examined by Bajpai et al. [67]. However, the economic implications should be examined taking into account the local market prices employed in this study. The unit price for the fly ash in the cost estimates for the baseline purchased material scenario is 1400 IQD/kg. Thus, the presented geopolymer production costs should not be generalized for scenarios when fly ash is supplied directly from industrial sources at different prices. Any alternative sourcing scenarios would have to take into account the true expenses of processing, quality control, handling and shipping, rather than assuming that the usage of industrial by-products is free. Likewise, the environmental comparisons depend on the emission variables chosen and the allocation assumptions used. Thus, the quoted values are comparative estimations based on the material inventory and local economic inputs presented and not universal standards of environmental or economic performance.
Table 19.
Calculated material cost and GWP per cubic meter of concrete.
4.3.2. Beam-Level Environmental, Economic, and Structural Performance
Table 20 analyzes the environmental, economic and structural performance of the five concrete mixes in terms of cost, global warming potential (GWP), and ultimate load capacity of one experimental beam. Results showed that GPC had a maximum load of 99.64 kN, which was 7.5% higher than NC (92.73 kN), and GWP was reduced from 17.04 to 9.30 kg CO2-eq per beam, which was around a 45.4% reduction. This reveals the environmental benefit of the studied geopolymer combination with superior load-bearing ability compared to traditional concrete. SF-GPC showed a maximum ultimate load of 106.96 kN, a 15.3% improvement compared to NC. However, the GWP rose slightly to 17.57 kg CO2-eq per beam, which is about 3.1% more than the reference combination. This rise shows that the environmental cost associated with the steel-fiber manufacture partly compensates the advantages gained from the geopolymer binder.
Table 20.
Environmental, economic, and structural performance of one experimental beam.
However, the peak load of PP-GPC was 90.44 kN, which is 2.5% lower than NC, and its GWP was 10.14 kg CO2-eq per beam, which is around 40.5% lower than the reference. The HB-GPC had a maximum load of 97.60 kN (5.3% greater) and its GWP was 13.85 kg CO2-eq per beam (about 18.7% lower) than NC. The results indicated that the hybrid fiber addition provided a good compromise between structural capacity and environmental footprint, although the environmental footprint was still worse than plain GPC and PP-GPC. NC had the lowest manufacturing cost (3233 IQD, 2.47 USD) per beam, but the cost of GPC, SF-GPC, PP-GPC and HB-GPC was 25,935 IQD (19.80 USD), 55,702 IQD (42.52 USD), 31,035 IQD (23.69 USD) and 43,369 IQD (33.11 USD), respectively. Therefore, the geopolymer mixtures evaluated were more expensive than normal concrete. SF-GPC had the highest cost, reflecting the greater costs associated with the addition of steel-fibers and the geopolymer components. This economic–environmental trade-off is consistent with the meta-analysis of Martinez and Miller [65], reporting reduced average greenhouse-gas emissions but higher manufacturing costs for geopolymer concrete, largely owing to the production of alkaline activators. Likewise, Tushar et al. [66] found that sodium hydroxide and sodium silicate are the major contributors to the carbon footprint of geopolymer concrete. In addition, Asare, ref. [68] showed in their environmental evaluation of steel-fiber-reinforced concrete beams that the addition of fiber may influence embodied carbon, and the final outcome depends on the structural efficiency and material savings achieved.
4.3.3. Performance-Normalized Environmental and Economic Efficiency
Table 21 shows a comparison of the economic and environmental efficiencies of the investigated concrete combinations. The production cost and global warming potential (GWP) of concrete mixtures are related to their final load capacity. The reference mixture was NC, with a cost intensity of 34.86 IQD/kN and carbon intensity of 0.184 kg CO2-eq/kN. Results demonstrate that all geopolymer-based combinations have reduced carbon intensity but worse economic performance compared to NC. GPC had the lowest carbon intensity (0.093 kg CO2-eq/kN), which is a decrease of 49.5% compared to NC. PP-GPC had the greatest environmental performance of 0.112 kg CO2-eq/kN (39.1% decrease) followed by the HB-GPC at 0.142 kg CO2-eq/kN (22.8% reduction). SF-GPC achieved a carbon intensity of 0.164 kg CO2-eq/kN, a decrease of just 10.9%. Such differences demonstrate that the environmental advantages of geopolymer concrete are highly dependent on the mix composition and the manufacturing consequences of its constituent elements, especially alkaline activators and fiber reinforcing. However, the cost intensity data show that NC is still the cheapest solution. The values for GPC, PP-GPC, HB-GPC and SF-GPC are substantially higher at 260.29, 343.16, 444.35 and 520.78 IQD/kN, respectively. SF-GPC is characterized by a very high cost intensity, which is due to the higher material cost of incorporating steel fibers that cannot be offset by an acceptable improvement in load-bearing capability. This environmental–economic trade-off is consistent with the results of Martínez and Miller [65] who found that geopolymer concrete can achieve lower greenhouse-gas emissions than conventional concrete, but has higher production costs, mainly due to the cost and environmental burdens of alkaline activators. Nikravan et al. [69] demonstrated the influence of precursor selection, activator content, functional unit definition and life cycle system limits on the environmental performance of alkali-activated materials.
Table 21.
Performance-normalized environmental and economic indicators.
4.3.4. Influence of Fly-Ash Procurement on Economic Feasibility
Table 22 shows the production cost sensitivity of the concrete mixes examined for two fly-ash (FA) acquisition scenarios, i.e., bought FA and waste/by-product FA. Results demonstrate that the predicted production cost of the geopolymer-based mixes is substantially lower when the FA procurement assumption is changed. The amount of reduction varies depending on the composition of the mixtures. The manufacturing cost for conventional normal concrete (NC) is constant (57,474 IQD/m3) as no FA is added to its mix. The cost of GPC is reduced from 461,066 IQD/m3 to 181,066 IQD/m3, which is a 60.7% reduction compared to the original. Also, the cost of SF-GPC was reduced from 990,266 to 710,266 IQD/m3 (28.3%) and the cost of PP-GPC was reduced from 551,732 to 271,732 IQD/m3 (50.8%). Also, there is a large fall in HB-GPC from 770,999 to 490,999 IQD/m3, which is a 36.3% reduction. These savings are consistent with the economic advantage of substituting an industrial by-product for fly ash bought under the procurement assumptions applied. The percentage decrease difference is due to the difference in the amount and ratio of FA in the various blends. The alternate procurement scenario offers superior advantages for mixes with a higher relative dependency on bought FA. Even with these huge cost reductions, all geopolymer-based combinations are still more costly than NC, suggesting that the cost of acquisition of FA is only one facet determining the total economic viability of these materials. This is particularly critical since it has been observed that the production cost of alkaline activators such as NaOH and Na2SiO3 constitutes a substantial portion of the entire cost of geopolymer concrete. In a life-cycle research of fly-ash-based alkali-activated concrete, alkaline activators were the main contributors to cost and environmental impacts [64]. The larger expense for geopolymer concrete as compared to conventional concrete has also been associated by Martínez and Miller [65] to the production of the activator. Matsimbe et al. [70] also stressed the economic potential of using industrial by-products in geopolymer systems, noting that the cost-effectiveness of these materials depended on the availability of precursors, the necessity for activators, and the mixture design.
Table 22.
Sensitivity of material cost to fly-ash procurement scenario.
4.3.5. CFRP Rehabilitation Cost and Environmental Burden
The post-damage rehabilitation assessment considered one CFRP layer bonded along a 1000 mm strengthening length and a beam soffit width of 150 mm, giving:
Assuming an epoxy consumption of 1.0 kg/m2:
At 29,000 IQD/kg, the epoxy cost was:
The CFRP fabric cost was estimated at:
Hence, the direct rehabilitation material cost was approximately:
This value represents the CFRP and epoxy materials only and excludes labor, grinding, equipment use, and site overhead.
For the environmental calculation, the CFRP mass was estimated as:
The corresponding additional environmental burden was:
Thus, the CFRP rehabilitation stage introduced a relatively small absolute increase in embodied carbon compared with the initial beam production.
4.3.6. Environmental, Economic, and Structural Response After CFRP Rehabilitation
A comparative assessment of the structural, economic and environmental performance of the CFRP-rehabilitated beams is shown in Table 23 in terms of their repaired ultimate load, strength-recovery ratio, total rehabilitation cost, global warming potential (GWP) and post-repair carbon intensity [71]. The results indicated that the corrected load capacities of the five rehabilitation systems were relatively close, ranging from 81.01 to 84.78 kN, which demonstrated that the CFRP rehabilitation regained most of the original load-carrying capacity for different kinds of concrete. The load of SF-GPC + CFRP after repair was the highest at 84.78 kN, but its strength-recovery ratio was the lowest at 79.26%, due to its relatively high initial ultimate load. However, PP-GPC + CFRP recorded the highest recovery ratio of 89.57% and a repaired capacity of 81.01 kN. The recovery ratios for NC + CFRP and HB-GPC + CFRP were 88.79% and 85.66%, respectively, while that of GPC + CFRP was 82.94%. These findings highlight the necessity to distinguish between absolute repaired capacity and percentage strength recovery when measuring rehabilitation success. The GPC + CFRP combination showed the greatest environmental performance with the lowest overall GWP of 10.61 kg CO2-eq and the lowest post-repair carbon intensity of 0.128 kg CO2-eq/kN. These values correspond to a reduction of around 42.2% and 42.6% compared with NC + CFRP, respectively. PP-GPC + CFRP also showed strong environmental performance with a GWP of 11.46 kg CO2-eq and carbon intensity of 0.141 kg CO2-eq/kN, which showed a reduction of around 37.6% and 36.8% compared to the NC-based system. The HB-GPC + CFRP had an intermediate rank in performance with a GWP of 15.17 kg CO2-eq and a carbon intensity of 0.181 kg CO2-eq/kN. Conversely, SF-GPC + CFRP showed the highest GWP (18.88 kg CO2-eq) and carbon intensity (0.223 kg CO2-eq/kN), slightly higher than that of NC + CFRP (18.36 kg CO2-eq). The economic results have a clear hierarchy. The least overall cost was NC + CFRP (13,133 IQD) and the most expensive was SF-GPC + CFRP (65,602 IQD) followed by HB-GPC + CFRP (53,269 IQD), PP-GPC + CFRP (40,935 IQD) and GPC + CFRP (35,835 IQD). Therefore, GPC + CFRP had the best environmental performance, but the cost was around 2.73 times that of NC + CFRP, which meant a trade-off of economic expenditure for environmental efficiency. These results are consistent with published life-cycle assessments of structural strengthening systems, which suggest that environmental and economic rankings of rehabilitation alternatives may differ depending on impacts of material production, strengthening requirements, and structural performance achieved. For instance, Pedroso et al. [72] demonstrated that the preferred strengthening solution is contingent upon the relative weight assigned to environmental and economic criteria, and Stoiber et al. [73] pointed out the substantial environmental burden associated with CFRP materials during production and the necessity to evaluate its impact at the structural-system level.
Table 23.
Performance of CFRP-rehabilitated beams.
5. Conclusions
The experimental, numerical, and environmental investigations conducted in this study led to the following conclusions:
- Steel-fiber geopolymer concrete achieved the highest ultimate load of 106.96 kN, representing a 15.4% improvement over conventional concrete. Meanwhile, hybrid-fiber geopolymer concrete exhibited the highest toughness of 2406.73 kN·mm, approximately 58.3% higher than the reference beam.
- CFRP strengthening successfully recovered 79.26–89.57% of the original ultimate load capacity. The PP-GPC beam achieved the highest recovery ratio (89.57%), demonstrating the effectiveness of CFRP in rehabilitating damaged geopolymer concrete beams.
- The validated ANSYS APDL model showed satisfactory agreement with experimental results, with ultimate-load prediction errors ranging from 0.56% to 6.02%. The parametric analysis indicated that increasing fiber content to 1.25% improved the predicted ultimate capacity by 25.1%, 21.2%, and 30.0% for steel, polypropylene, and hybrid fibers, respectively.
- The GWP (material-related) of plain geopolymer concrete was around 165.31 kg CO2-eq/m3 which is 45.4% less than conventional concrete. When adjusted to the experimentally measured ultimate load, its carbon intensity was around 0.093 kg CO2-eq/kN, which represents a 49.5% reduction compared to the reference mixture. However, the environmental advantages were mainly due to the replacement of Portland cement with fly ash and GGBS, while the alkaline activators still contributed considerably to the overall environmental burden.
- The environmental response of the fiber-reinforced geopolymer mixtures was dependent on type and quantity of the fiber. Steel-fiber combination has a GWP of around 312.31 kg CO2-eq/m3, which is 3.1% more than the normal standard. Polypropylene and hybrid fiber mixtures decreased by 40.5% and 18.7%, respectively. The environmental advantages of geopolymer concrete are due to the combined effect of binder composition, alkaline activators and fiber-related production burdens.
- The economic research showed that the basic material cost of all the tested geopolymer mixes was higher than the conventional concrete at the recognized Iraqi market values. The economic benefit of the industrial by-product fly ash is dependent upon its actual delivery and processing purchase cost. So, the alternative procurement scenario has to be understood conditionally considering processing and shipping charges rather than as a blanket 60.7% cost savings.
Author Contributions
Conceptualization, A.F.A. and N.Y.E.; methodology, A.F.A. and N.Y.E.; investigation, A.F.A. and N.Y.E.; numerical analysis, D.T.H., S.H.S., and A.S.O.; software, D.T.H.; validation, D.T.H., S.H.S., and A.S.O.; formal analysis, Z.A.-K.; life-cycle assessment, Z.A.-K.; writing—original draft preparation, A.F.A. and N.Y.E.; writing—review and editing, Z.A.-K. All authors have read and agreed to the published version of the manuscript.
Funding
This research received no external funding.
Institutional Review Board Statement
Not applicable.
Informed Consent Statement
Not applicable.
Data Availability Statement
The data supporting the findings of this study are available within the article. Additional data can be obtained from the corresponding author upon reasonable request.
Conflicts of Interest
The authors declare no conflict of interest.
References
- Ezuldin, N.Y.; Raoof, S.M.; Alattar, A.A.; Hamada, H. Factors Affecting Durability Properties of GPC: A Review. Res. Eng. Struct. Mater. 2024, 11, 21–43. [Google Scholar] [CrossRef] [Scilit]
- Davidovits, J. Geopolymers: Inorganic Polymeric New Materials. J. Therm. Anal. Calorim. 1991, 37, 1633–1656. [Google Scholar]
- Ezuldin, N.Y.; Raoof, S.M.; Alattar, A.A.; Hamada, H. The Performance and Mechanical Properties of Geopolymer Concrete. In Proceedings of the AIP Conference Proceedings; AIP Publishing LLC: Melville, NY, USA, 2024; Volume 3249, p. 20025. [Google Scholar]
- Turner, L.K.; Collins, F.G. Carbon Dioxide Equivalent (CO2-e) Emissions: A Comparison between Geopolymer and OPC Cement Concrete. Constr. Build. Mater. 2013, 43, 125–130. [Google Scholar] [CrossRef] [Scilit]
- Habert, G.; De Lacaillerie, J.B.D.; Roussel, N. An Environmental Evaluation of Geopolymer Based Concrete Production: Reviewing Current Research Trends. J. Clean. Prod. 2011, 19, 1229–1238. [Google Scholar] [CrossRef] [Scilit]
- Abdullah, A.F.; Ezuldin, N.Y.; Ahmed, I.M.; Al-Khafaji, Z. Enhancing the Sustainability of Concrete Mixes Utilizing Supplementary Cementitious Materials in Renewable Energy Buildings. Eng. Technol. Appl. Sci. Res. 2025, 15, 28041–28049. [Google Scholar] [CrossRef] [Scilit]
- Nath, P.; Sarker, P.K. Effect of GGBFS on Setting, Workability and Early Strength Properties of Fly Ash Geopolymer Concrete Cured in Ambient Condition. Constr. Build. Mater. 2014, 66, 163–171. [Google Scholar] [CrossRef] [Scilit]
- Ranjbar, N.; Zhang, M. Fiber-Reinforced Geopolymer Composites: A Review. Cem. Concr. Compos. 2020, 107, 103498. [Google Scholar] [CrossRef] [Scilit]
- Mohamed, O.; Zuaiter, H. Fresh Properties, Strength, and Durability of Fiber-Reinforced Geopolymer and Conventional Concrete: A Review. Polymers 2024, 16, 141. [Google Scholar] [CrossRef] [Scilit]
- Okeh, C.A.O.; Begg, D.W.; Barnett, S.J.; Nanos, N. Behaviour of Hybrid Steel Fibre Reinforced Self Compacting Concrete Using Innovative Hooked-End Steel Fibres under Tensile Stress. Constr. Build. Mater. 2019, 202, 753–761. [Google Scholar] [CrossRef] [Scilit]
- Mohamed, A.M.; Tayeh, B.A. Polypropylene Fibers in Pavement Concrete: Mechanical, Durability, and Sustainability Review. J. Sustain. Res. 2026, 8, e260074. [Google Scholar] [CrossRef] [Scilit]
- Khan, M.I.; Abbas, Y.M. Synergistic Enhancement of High-Strength Concrete’s Mechanical Strength Through the Utilization of Steel, Synthetic, and Hybrid Fiber Systems. Int. J. Concr. Struct. Mater. 2025, 19, 18. [Google Scholar] [CrossRef] [Scilit]
- Junior, J.; Saha, A.K.; Sarker, P.K.; Pramanik, A. Workability and Flexural Properties of Fibre-Reinforced Geopolymer Using Different Mono and Hybrid Fibres. Materials 2021, 14, 4447. [Google Scholar] [CrossRef] [Scilit]
- Hasan, M.A.; Sheehan, T.; Ashour, A.; Elkezza, O. Flexural Behaviour of Geopolymer Concrete T-Beams Reinforced with GFRP Bars. In Proceedings of the Structures; Elsevier: Amsterdam, The Netherlands, 2023; Volume 49, pp. 345–364. [Google Scholar]
- Yost, J.R.; Radlińska, A.; Ernst, S.; Salera, M.; Martignetti, N.J. Structural Behavior of Alkali Activated Fly Ash Concrete. Part 2: Structural Testing and Experimental Findings. Mater. Struct. 2013, 46, 449–462. [Google Scholar] [CrossRef] [Scilit]
- Alex, A.G.; Gebrehiwet Tewele, T.; Kemal, Z.; Subramanian, R.B. Flexural Behavior of Low Calcium Fly Ash Based Geopolymer Reinforced Concrete Beam. Int. J. Concr. Struct. Mater. 2022, 16, 40. [Google Scholar] [CrossRef] [Scilit]
- Ozturk, M.; Arslan, G. Flexural Behavior of GBFS-Based Geopolymer-Reinforced Concrete Beams. Buildings 2023, 13, 141. [Google Scholar] [CrossRef] [Scilit]
- Raj, S.D.; Ramachandran, A. Performance of Hybrid Fibre Reinforced Geopolymer Concrete Beams. SN Appl. Sci. 2019, 1, 1725. [Google Scholar] [CrossRef] [Scilit]
- El-Sayed, T.A.; Deifalla, A.F.; Shaheen, Y.B.; Ahmed, H.H.; Youssef, A.K. Experimental and Numerical Studies on Flexural Behavior of GGBS-Based Geopolymer Ferrocement Beams. Civ. Eng. J. 2023, 9, 629–653. [Google Scholar] [CrossRef] [Scilit]
- Alagusundaramoorthy, P.; Harik, I.E.; Choo, C.C. Flexural Behavior of R/C Beams Strengthened with Carbon Fiber Reinforced Polymer Sheets or Fabric. J. Compos. Constr. 2003, 7, 292–301. [Google Scholar] [CrossRef] [Scilit]
- Camata, G.; Spacone, E.; Zarnic, R. Experimental and Nonlinear Finite Element Studies of RC Beams Strengthened with FRP Plates. Compos. Part B Eng. 2007, 38, 277–288. [Google Scholar] [CrossRef] [Scilit]
- Aram, M.R.; Czaderski, C.; Motavalli, M. Debonding Failure Modes of Flexural FRP-Strengthened RC Beams. Compos. Part B Eng. 2008, 39, 826–841. [Google Scholar] [CrossRef] [Scilit]
- Vahidpour, M.; Kheyroddin, A.; Kioumarsi, M. Experimental Investigation on Flexural Capacity of Reinforced Concrete Beams Strengthened with 3D-Fiberglass, CFRP and GFRP. Int. J. Concr. Struct. Mater. 2022, 16, 18. [Google Scholar] [CrossRef] [Scilit]
- Junaid, M.T.; Elbana, A.; Altoubat, S. Flexural Response of Geopolymer and Fiber Reinforced Geopolymer Concrete Beams Reinforced with GFRP Bars and Strengthened Using CFRP Sheets. In Proceedings of the Structures; Elsevier: Amsterdam, The Netherlands, 2020; Volume 24, pp. 666–677. [Google Scholar]
- Eisa, A.S.; Ahmed, M.H.; Demjan, I.; Katunský, D. Experimental Investigation on the Behavior of Fly-Ash Based Geopolymer Reinforced Concrete Beams Strengthened with CFRP. Heliyon 2023, 9, e17674. [Google Scholar] [CrossRef] [Scilit]
- Al-Abdwais, A.H. Experimental and Numerical Assessment of Bonding between Geopolymer Concrete and CFRP Sheet Using NSM Techniques. Civ. Environ. Eng. 2023, 19, 676–691. [Google Scholar] [CrossRef] [Scilit]
- Zinkaah, O.H.; Alridha, Z.; Alhawat, M. Numerical and Theoretical Analysis of FRP Reinforced Geopolymer Concrete Beams. Case Stud. Constr. Mater. 2022, 16, e01052. [Google Scholar] [CrossRef] [Scilit]
- Naser, M.Z.; Hawileh, R.A.; Abdalla, J. Modeling Strategies of Finite Element Simulation of Reinforced Concrete Beams Strengthened with FRP: A Review. J. Compos. Sci. 2021, 5, 19. [Google Scholar] [CrossRef] [Scilit]
- Özkılıç, Y.O.; Çelik, A.İ.; Aksoylu, C.; Karalar, M.; Mydin, M.A.O.; Althaqafi, E.; Yılmaz, F.; Umiye, O.A. Shear and Flexural Performance of Reinforced Geopolymer Concrete Beams Cured under Ambient and Oven Conditions with Environmentally Friendly Waste Steel Tire Wire Additives. Sci. Rep. 2025, 15, 22765. [Google Scholar] [CrossRef] [Scilit]
- ÇELİK, A.L.İ.; Tunc, U.; Karalar, M.; Güven, A.; Ozkilic, Y. Bending Behavior of Reinforced Geopolymer Concrete Beams with Varying Proportions of Slag and Polyamide Fibers in Oven and Ambient Curing. Adv. Concr. Constr. 2025, 20, 469–481. [Google Scholar]
- ÇELİK, A.L.İ.; Tunç, U.; Karalar, M.; Güven, A.; Ozkilic, Y. Investigation of Shear Behavior in Geopolymer Concrete Beams with Different Ratios of Slag and Polyamide Fibers under Oven and Ambient Curing Condition. Adv. Concr. Constr. 2026, 22, 53–73. [Google Scholar]
- IQS-5; Iraqi Standard Specification for the Portland Cement. COSQC: Baghdad, Iraq, 2019.
- ISO 527-2:2025; Plastics—Determination of Tensile Properties—Part 2: Test Conditions for Moulding and Extrusion Plastics. Available online: https://www.iso.org/standard/527-2 (accessed on 23 November 2026).
- Plastics-Determination of Flexural Properties INTERNATIONAL STANDARD ISO 178. 2019. Available online: www.iso.org (accessed on 23 November 2026).
- BS EN 1542:1999; Products and Systems for the Protection and Repair of Concrete Structures—Test Methods—Measurement of Bond Strength by Pull-Off, British. British Standards Institution: London, UK, 1999; p. 10.
- Mardan, G.A.; Abdul-Rahman, M.B.A.-D.; Abdullah, A.F.; Al-Khafaji, Z. Thermo-Mechanical Response of Reinforced Geopolymer Hollow Beams Containing Steel Fibers. Math. Model. Eng. Probl. 2025, 12, 2981–2992. [Google Scholar] [CrossRef] [Scilit]
- Arjan, F.A.; Al-Khafaji, Z.; Falah, M. Enhancing Fire Resistance of Geopolymer Concrete Through Steel Fiber Reinforcement: Microstructure and Mechanical Behavior at Elevated Temperatures. Mater. Mech. Eng. Technol. 2025, 4, 93. [Google Scholar] [CrossRef] [Scilit]
- Abdullah, A.F.; Abdul-Rahman, M.B.A.-D.; Al-Attar, A.A. Investigate the Mechanical Characteristics and Microstructure of Fibrous-Geopolymer Concrete Exposure to High Temperatures. J. Rehabil. Civ. Eng. 2025, 14, 2141. [Google Scholar] [CrossRef]
- Hadi, M.N.S.; Zhang, H.; Parkinson, S. Optimum Mix Design of Geopolymer Pastes and Concretes Cured in Ambient Condition Based on Compressive Strength, Setting Time and Workability. J. Build. Eng. 2019, 23, 301–313. [Google Scholar] [CrossRef] [Scilit]
- ASTM C496/C496M-11; Standard Test Method for Splitting Tensile Strength of Cylindrical Concrete Specimens. ASTM Int.: West Conshohocken, PA, USA, 2009; pp. 1–5. [Google Scholar] [CrossRef] [Scilit]
- Sathish Kumar, V.; Ganesan, N.; Indira, P. V Engineering Properties of Hybrid Fibre Reinforced Ternary Blend Geopolymer Concrete. J. Compos. Sci. 2021, 5, 203. [Google Scholar] [CrossRef] [Scilit]
- Wang, Y.; Aslani, F.; Valizadeh, A. An Investigation into the Mechanical Behaviour of Fibre-Reinforced Geopolymer Concrete Incorporating NiTi Shape Memory Alloy, Steel and Polypropylene Fibres. Constr. Build. Mater. 2020, 259, 119765. [Google Scholar] [CrossRef] [Scilit]
- Zhang, H.; Jia, T.C.; Sarker, P.K.; Chen, W.; Wang, Q.; Li, Z.; He, B.; Jiang, Z. Effect of Fibre Addition on the Static and Dynamic Compressive Properties of Ambient-Cured Geopolymer Concrete. J. Build. Eng. 2022, 58, 104991. [Google Scholar] [CrossRef] [Scilit]
- Li, B.; Chi, Y.; Xu, L.; Shi, Y.; Li, C. Experimental Investigation on the Flexural Behavior of Steel-Polypropylene Hybrid Fiber Reinforced Concrete. Constr. Build. Mater. 2018, 191, 80–94. [Google Scholar] [CrossRef] [Scilit]
- Bhutta, A.; Borges, P.H.R.; Zanotti, C.; Farooq, M.; Banthia, N. Flexural Behavior of Geopolymer Composites Reinforced with Steel and Polypropylene Macro Fibers. Cem. Concr. Compos. 2017, 80, 31–40. [Google Scholar] [CrossRef] [Scilit]
- Banthia, N.; Trottier, J.-F. Test Methods for Fexural Toughness Characterization of Fiber Reinforced Concrete: Some Concerns and a Proposition. Mater. J. 1995, 92, 48–57. [Google Scholar] [CrossRef] [Scilit]
- Ling, J.H.; Lim, Y.T.; Jusli, E. Methods to Determine Ductility of Structural Members: A Review. J. Civ. Eng. Forum 2023, 9, 181–194. [Google Scholar] [CrossRef] [Scilit]
- Zhuang, N.; Dong, H.; Chen, D.; Ma, Y. Experimental Study of Aged and Seriously Damaged RC Beams Strengthened Using CFRP Composites. Adv. Mater. Sci. Eng. 2018, 2018, 6260724. [Google Scholar] [CrossRef] [Scilit]
- Hamah-Ali, B.H.S.; Qadir, M.R.A. The Effect of Different Levels of Pre-Damage Loading on the Strength and Structural Behavior of CFRP Strengthened RC Beams: Experimental and Analytical Investigation. PLoS ONE 2021, 16, e0261290. [Google Scholar] [CrossRef] [Scilit]
- Jahami, A.; Issa, C.A. An Updated Review on the Effect of CFRP on Flexural Performance of Reinforced Concrete Beams. Int. J. Concr. Struct. Mater. 2024, 18, 14. [Google Scholar] [CrossRef] [Scilit]
- William, K.J.; Warnke, E.P. Constitutive Model for the Triaxial Behavior of Concrete. In Proceedings of the International Association for Bridge and Structural Engineering (IABSE); IABSE: Bergamo, Italy, 1975. [Google Scholar]
- Fluent, A. Ansys Fluent Theory Guide; ANSYS Inc.: Canonsburg, PA, USA, 2023. [Google Scholar]
- Luu, X.-B.; Kim, S.-K.; Kim, W. Investigation of Load–Displacement Characteristics and Crack Behavior of RC Beam Based on Nonlinear Finite Element Analysis Using Concrete Damage Plasticity. Appl. Sci. 2023, 13, 11798. [Google Scholar] [CrossRef] [Scilit]
- Albegmprli, H.M.; Cevik, A.; Gulsan, M.E.; Kurtoglu, A.E. Reliability Analysis of Reinforced Concrete Haunched Beams Shear Capacity Based on Stochastic Nonlinear FE Analysis. Comput. Concr. 2015, 15, 259–277. [Google Scholar] [CrossRef] [Scilit]
- Megahid, A.B.D.E.-R.; Rashwan, M.M.; Sayed, A.M. Static Behaviour of Reinforced High Strength Concrete Haunched Beams Strenghened by Using Epoxy Bonded External Steel Plates. JES J. Eng. Sci. 2010, 38, 1391–1428. [Google Scholar] [CrossRef] [Scilit]
- Galal, K.; Yang, Q. Experimental and Analytical Behavior of Haunched Thin-Walled RC Girders and Box Girders. Thin-Walled Struct. 2009, 47, 202–218. [Google Scholar] [CrossRef] [Scilit]
- Moaveni, S. Finite Element Analysis; Pearson Education, Limited: London, UK, 2014; ISBN 0273774336. [Google Scholar]
- Padmarajaiah, S.K.; Ramaswamy, A. A Finite Element Assessment of Flexural Strength of Prestressed Concrete Beams with Fiber Reinforcement. Cem. Concr. Compos. 2002, 24, 229–241. [Google Scholar] [CrossRef] [Scilit]
- Carreira, D.J.; Chu, K.-H. Stress-Strain Relationship for Plain Concrete in Compression. J. Proc. 1985, 82, 797–804. [Google Scholar] [CrossRef] [Scilit]
- Kachlakev, D.; Miller, T.R.; Yim, S.; Chansawat, K.; Potisuk, T. Finite Element Modeling of Concrete Structures Strengthened with FRP Laminates; Oregon Department of Transportation, Research Section: Salem, OR, USA, 2001. [Google Scholar]
- Hsu, L.S.; Hsu, C.-T. Complete Stress—Strain Behaviour of High-Strength Concrete under Compression. Mag. Concr. Res. 1994, 46, 301–312. [Google Scholar] [CrossRef] [Scilit]
- Luo, R.D. Values of Shear Transfer Coefficients of Concrete Element Solid65 in Ansys. J. Jiangsu Univ. 2008, 29, 169–172. [Google Scholar]
- Ali, T.; Yehia, S.; El-Didamouny, M. Analytical Study on Concrete Slabs with Decking Profiled Steel Sheet. Int. J. Adv. Res. Eng. Technol. 2020, 11, 939–950. [Google Scholar]
- Fernando, S.; Gunasekara, C.; Law, D.W.; Nasvi, M.C.M.; Setunge, S.; Dissanayake, R. Life Cycle Assessment and Cost Analysis of Fly Ash–Rice Husk Ash Blended Alkali-Activated Concrete. J. Environ. Manag. 2021, 295, 113140. [Google Scholar] [CrossRef] [Scilit]
- Martínez, A.; Miller, S.A. Life Cycle Assessment and Production Cost of Geopolymer Concrete: A Meta-Analysis. Resour. Conserv. Recycl. 2025, 215, 108018. [Google Scholar] [CrossRef] [Scilit]
- Tushar, Q.; Bhuiyan, M.A.; Abunada, Z.; Lemckert, C.; Giustozzi, F. Carbon Footprint and Uncertainties of Geopolymer Concrete Production: A Comprehensive Life Cycle Assessment (LCA). C 2025, 11, 55. [Google Scholar] [CrossRef] [Scilit]
- Bajpai, R.; Choudhary, K.; Srivastava, A.; Sangwan, K.S.; Singh, M. Environmental Impact Assessment of Fly Ash and Silica Fume Based Geopolymer Concrete. J. Clean. Prod. 2020, 254, 120147. [Google Scholar] [CrossRef] [Scilit]
- Asare, G.O.; Barnett, S.; Awinda, K.; Martinson, B. Life Cycle Assessment of Steel Fibre-Reinforced Concrete Beams. Cogent Eng. 2024, 11, 2374942. [Google Scholar] [CrossRef] [Scilit]
- Nikravan, M.; Firdous, R.; Stephan, D. Life Cycle Assessment of Alkali-Activated Materials: A Systematic Literature Review. Low-Carbon Mater. Green Constr. 2023, 1, 13. [Google Scholar] [CrossRef] [Scilit]
- Matsimbe, J.; Dinka, M.; Olukanni, D.; Musonda, I. Geopolymer: A Systematic Review of Methodologies. Materials 2022, 15, 6852. [Google Scholar] [CrossRef] [Scilit]
- Shi, C.; Wang, J.; Liu, Y.; Luo, W.; Mei, S.; Wang, Y.; Yu, J. Life-Cycle Study of Concrete Bridges Strengthened with Carbon-Fibre-Reinforced Polymer. In Proceedings of the Institution of Civil Engineers-Engineering Sustainability; Thomas Telford Ltd.: London, UK, 2021; Volume 174, pp. 289–303. [Google Scholar]
- Pedroso, P.F.; Correia, J.R.; Silvestre, J.D.; Firmo, J.P.; Garrido, M. Environmental and Economic LCA Comparison of Flexural Strengthening Solutions for a Reinforced Concrete Beam. Materials 2024, 17, 5879. [Google Scholar] [CrossRef] [Scilit]
- Stoiber, N.; Hammerl, M.; Kromoser, B. Cradle-to-Gate Life Cycle Assessment of CFRP Reinforcement for Concrete Structures: Calculation Basis and Exemplary Application. J. Clean. Prod. 2021, 280, 124300. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.