Abstract
This study measures the residual gas permeability of concrete in two directions after drying, heating, and sustained tensile or compressive loading of plain VeRCoRs specimens. Cylindrical slices were heated without mechanical loading to temperatures from 100 to 250 °C. Whole cylinders were tested after 180-day exposures at 20 or 40 °C with compressive stresses of up to 60% of compressive strength at 50% or 100% relative humidity. Dog-bone specimens were tested after thermal exposure alone or after 14 days at 30% of tensile strength at 20, 100, or 180 °C. All permeability measurements were made after exposure and cooling on dry material. The dried cylindrical reference slices had a mean intrinsic permeability of 2.93 × 10−17 m2 in both directions. Dried dog-bone slices had longitudinal and radial means of 7.17 × 10−17 and 4.23 × 10−17 m2, respectively. At 100 °C, the radial mean with tensile loading was about twice the corresponding unloaded mean. At 180 °C, the radial measurements under tensile loading showed substantial scatter. The largest radial permeability in the compression series was 42.6 × 10−17 m2, or 14.5 times the unloaded reference, after 180 days at 60% of compressive strength, 20 °C, and 50% relative humidity. The results quantify how exposure history and flow direction influence residual permeability and identify the limits of transferring dry-specimen results to structural leakage assessments.
1. Introduction
The long-term integrity and safety of reinforced concrete structures, particularly those in critical applications like nuclear power plants, necessitate a thorough understanding of their behavior under extreme conditions. These structures can be subjected to a complex interplay of thermal, hydraulic, and mechanical stresses, especially during severe accidents [1]. Such events, exemplified by a Loss of Coolant Accident (LOCA) in a nuclear power plant, can involve elevated temperatures reaching 180 °C and internal pressures up to 5 bars exerted on containment walls, sustained for extended periods, thus generating creep. These combined stresses can induce a cascade of changes within the concrete, beginning with alterations in the transport properties of water within the porous cementitious matrix. Moreover, drying shrinkage contributes to the development of microcracks, a process exacerbated by the high temperatures, which promote the release of bound water from hydration products and differential thermal expansion between cement paste and aggregates [2]. This can induce permeability anisotropy in concrete structures, dependent on the structural geometry. Furthermore, creep deformation, potentially thermally activated, may interact with these cracking mechanisms and ultimately govern the leakage rate of the structure. Therefore, a comprehensive investigation of the change in concrete permeability under these coupled thermo-hydro-mechanical conditions is essential for accurately predicting structural response and ensuring the safety and reliability of such critical infrastructure.
Burlion et al. [3] investigated the impact of drying-induced microcracks on concrete gas permeability in both longitudinal and transverse directions. Findings revealed that drying-induced permeability anisotropy can be significant. While initial microcracks preferentially align with the largest drying gradient (e.g., transversely), the resulting anisotropy is initially small. Subsequent crack growth, opening, and interconnection lead to a substantial permeability increase [4] and marked anisotropy, with longitudinal permeability potentially exceeding transverse permeability by a factor ranging from 5 to 20, indicating that cracks are running longitudinally through the entire specimen [3]. Wu et al. [5] explored the effects of drying and sample size, revealing that preconditioning significantly influences transport properties: “Cast” samples exhibited higher transport properties than “cut” samples, with the latter showing greater variability due to segregation, particularly in samples cut from the top portion.
Moreover, elevated temperatures, above 140 °C, induce the release of chemically bound water from concrete hydrates [6,7,8], altering the material’s porous network and mechanical behavior and potentially leading to a significant increase in gas permeability [9,10]. Furthermore, the differential thermal expansion and distinct stress–strain responses of aggregates and cement paste can generate microcracks at their interface [2]. Therefore, the estimation of concrete’s intrinsic permeability must consider the contribution of microcracks from these various sources. Upon coalescence of these microcracks, macrocracks can form, creating preferential flow paths that dominate fluid leakage [11,12,13,14]. Alkali-activated materials, e.g., metakaolin-based geopolymer mortar [15,16], initially exhibit lower permeability compared to Portland cement-based materials [17]. These materials demonstrated improvement in thermal stability and continued geopolymerization up to 200 °C. However, while increasing steadily between 100 °C and 200 °C, their permeability begins to rise exponentially beyond 200 °C [18].
Concrete permeability depends on stress level and crack development [13,19,20,21]. Short-term compression tests have reported a slight decrease in gas permeability up to 50–60% of compressive strength, a modest increase up to 80%, and a sharper increase above 80% [9]. Direct tension tests are less common because the material has a low tensile strength and a uniform tensile stress is difficult to maintain. Indirect splitting generates a localized crack [13,21]. Splitting studies report an increase in permeability of up to four orders of magnitude at 250 µm of crack opening displacement, with a marked increase beginning around 15 µm [11,22]. Gas flow through uncracked material is sensitive to saturation [22,23]. Once a connected macrocrack develops, flow through that crack can dominate transport [11,20,23,24].
A recent study has demonstrated that compressive creep with drying cycles can significantly impact concrete gas permeability. Creep loading to 60% of compressive strength yielded an increase in gas permeability by a factor of 10 during drying at 50% RH compared to an unloaded sample [25]. Creep behavior, which refers to the time-dependent deformation of concrete under sustained load, is significantly affected by temperature variations [26,27]. For instance, Yoon et al. [28] demonstrated that elevated temperatures exacerbate transient creep in high-strength concrete and observed a larger shrinkage strain, particularly in the range of 500–600 °C, as the compressive strength of concrete increased. While macroscopic deformations may be small, the process is driven by the dehydration of C–S–H gel and the decomposition of portlandite, which trigger internal mass movement and a reorganization of the pore network [29]. This microstructural sliding and the resulting redistribution of internal water facilitate the widening of interconnecting pathways [29]. Consequently, the connectivity of the capillary system is enhanced, which may lead to a significant increase in the material’s permeability to gases even at low strain levels. The relationship between temperature and gas permeability is underscored by findings from [9,10,30,31], which reported a significant increase in permeability with rising temperature, indicating a critical interplay between temperature effects and the material’s structural integrity. For instance, the permeability increase was found to be exponential, and it reached a factor of 15 at 250 °C with respect to the unloaded sample [31]. Moreover, the combined effects of drying and tensile or compressive creep can lead to significant changes in the mechanical properties of concrete [32], which in turn may affect its permeability characteristics. A study of concrete creep under various stress states (tension, compression, flexure) found that shrinkage significantly influences creep evaluation, complicated by low strain magnitudes, shrinkage strain variability, and tensile strength uncertainty. While basic creep and autogenous shrinkage superposition is plausible for undamaged concrete (e.g., flexural tests below 50% stress), microcracking under uniform loading (tension/compression) complicates interpretation due to strong shrinkage-damage interaction, potentially increasing shrinkage strains in loaded specimens [33]. A study on gas permeability of polypropylene-fiber-reinforced concrete under combined temperature (room temperature and from 40 to 280 °C at 40 °C increments) and cyclic loading (eight loading cycles from 0.03 to 0.5 stress ratios) has revealed that cyclic loading/unloading exacerbates damage to the matrix strength structure, leading to 1.24 to 1.57 times greater permeability loss compared to monotonic loading [34]. Finally, the study found that high temperatures affect both pore and strength structures, and above a stress ratio of 0.37, these combined damages synergistically diminish the concrete’s resistance to gas permeability.
Coupling between sustained stress, deformation, and permeability has also been examined in rock mechanics [35,36,37]. In concrete, drying and heating act on a hydrated cement paste that contains capillary pores and surrounds aggregates. Differential deformation of these phases can damage the paste–aggregate interfaces. Mineral fabrics and pre-existing discontinuities in rocks can govern fracture and flow through different mechanisms. Stress thresholds or permeability relationships derived for rocks therefore require separate verification before application to concrete.
The present work complements short-term loading and heating studies [9,10] and earlier work on compressive creep with drying [25] by comparing directional residual gas permeability across sustained tensile and compressive exposure histories for the same reference concrete. The program addresses three experimental issues. First, it checks the effect of specimen length and slice position, including the potential influence of casting segregation. Second, it uses separate tensile and compressive protocols to compare the responses within each loading mode against the relevant controls. Third, it measures longitudinal and radial flow wherever specimen preparation allows both directions to be tested. The 180-day compression series evaluates radial flow only.
Heat and moisture transport jointly govern the development of internal gradients during exposure. Surface temperature, moisture exchange, and specimen geometry control how quickly the interior responds and can produce spatially variable shrinkage and damage. Numerical studies of drying under variable climatic conditions illustrate the sensitivity of moisture redistribution to boundary histories and material properties [38]. The building-envelope application in [38] provides methodological context for selecting boundary conditions. The present study examines this issue through residual permeability measurements on concrete specimens.
This paper is organized as follows. Section 2 describes the concrete mixture, specimen preparation, loading conditions, and gas permeability measurement procedures. Section 3 presents and discusses the effects of specimen length and position, drying, temperature, and sustained tensile and compressive loading on concrete permeability, including its directional behavior. Finally, the main conclusions are presented.
2. Materials and Methods
2.1. Concrete Mixture
The concrete used in this study, designated “VeRCoRs,” is the reference concrete for the national “MaCEnA” project (tightness assessment of confinement vessels during an accident) and has been extensively documented in the literature [1,24,31,39,40]. EDF and their MaCEnA collaborators report that VeRCoRs concrete at 28 days has a tensile strength of approximately 3.85 MPa, a compressive strength of around 46 MPa, and a Young’s Modulus of roughly 35 GPa [1]. The concrete mixture proportions are provided in Table 1.
Table 1.
Mixture proportions of 1 m3 of MaCEnA’s concrete.
2.2. Specimens for the Assessment of Specimen Length and Positional Influence on Concrete Intrinsic Permeability
To investigate the impact of specimen length on intrinsic permeability, three cylindrical concrete samples, P1, P2 and P3 (110 mm diameter, 220 mm length), were prepared. They were cured in water at a temperature of 23 °C for 28 days. Prior to testing, the samples were dried at 80 °C until reaching constant mass. Initially, the intrinsic gas permeability in the longitudinal direction of each whole sample (before slicing) was measured. Subsequently, the samples were progressively sliced to obtain four length configurations: 220 mm, 110 mm (two slices), 55 mm (four slices), and 25 mm (eight slices) (see Figure 1). The longitudinal intrinsic permeability of each slice was then determined. To assess potential positional effects, the location of each slice within the original specimen was recorded.
Figure 1.
Concrete specimens and slices at nominal lengths of 220, 110, 55, and 25 mm.
2.3. Specimens and Experimental Setup
Table 2 and Table 3 summarize the treatment histories and specimen counts. Plain concrete specimens were water-cured at 23 °C for 28 days before exposure. The dog-bone geometry provides an 80 mm diameter, 120 mm long gauge section designed to promote a uniform axial stress in direct tension (see Figure 2). Sustained tensile loading was applied at 0.25 kN/s to 30% of tensile strength. For the heated tensile cases, the load was applied at 20 °C and maintained during heating and the prescribed exposure. Compressive loads were likewise applied before heating and maintained during the 180-day exposure at the specified temperature and relative humidity. Figure 3a shows the tensile setup, and Figure 3c summarizes the test sequence. RILEM TC 129-MHT provides test methods for the mechanical properties of concrete at high temperatures [41].
Table 2.
Specimen preparation and exposure histories for the drying, thermal, and sustained-tension series.
Table 3.
Specimens and exposure conditions for the 180-day compression series.
Figure 2.
Photos of the specimens: (a) 110 × 220 mm2 cylindrical specimens, (b) 80/120 × 610 mm2 dog-bone specimens.
Figure 3.
(a) Setup for sustained tensile loading and heating. (b) Slices used for permeability testing. (c) Loading, exposure, preparation, and measurement sequence.
The 30% and 60% compressive stress levels were selected to span a moderate sustained stress and a higher stress at which damage can become more important [9,25,42]. The 30% tensile stress allowed investigation of a sustained subcritical load while limiting the likelihood of premature fracture during heating. These uniaxial stress ratios define laboratory test conditions. Stress ratios in a reinforced or prestressed containment wall depend on restraint, pressure, thermal gradients, prestressing, and load history.
The compression series used a 180-day duration to capture longer-term exposure at 20–40 °C and to compare nominally saturated and drying environments. The 14-day tensile protocol examined shorter-duration sustained loading over a wider temperature range. These durations, together with differences in specimen geometry and environment, limit direct comparisons between loading modes. The experiment cannot establish a tension-to-compression difference at a common exposure age.
After exposure and unloading, where applicable, the dog-bone specimens were water-sawn into slices and oven-dried at 80 °C to constant mass. Longitudinal testing preceded wet drilling of a 16 mm axial bore, a second drying step at 80 °C to constant mass, and radial testing. The C1–C6 specimens were tested radially as whole 110 mm diameter, 220 mm long cylinders after wet drilling and drying to constant mass at 80 °C. The Th-C slices were initially dried at 80 °C before heating to the target temperature. Permeability was measured on dry specimens after cooling to ambient temperature.
The 80 °C treatment standardized the dry endpoint but may itself have generated shrinkage gradients and microcracking. In addition, the radial protocol included wet drilling and redrying. Because the program did not measure permeability immediately before and after each preparation step, the absolute residual values include any preparation effects, and the susceptibility to such effects may depend on earlier exposure. Comparisons are made within series using the corresponding preparation and exposure reference.
2.4. Gas Permeability Device
The experimental program required specimens of different diameters and heights (see Section 2.2 and Section 2.3). In addition, the permeability system employed in the current study, unlike commercial systems such as Cembureau [11], allows studying the intrinsic permeability in both longitudinal and radial directions. Classically, the permeability test is carried out by imposing a pressure gradient and measuring the flow rate. The permeability test is performed by injection of gas under a given pressure in the permeability chamber. The permeability is measured in two directions, longitudinal and radial, depending on the experimental setup. To measure the longitudinal permeability, the lateral surface of the specimen is sealed with three layers of aluminum foil of 0.1 mm thickness each, which impose the percolation path longitudinally. When measuring permeability in the longitudinal direction, in order to prevent measurement errors caused by gas pressure lifting the aluminum layers, a confinement system was employed for specimens exceeding 50 mm in length. This system consisted of a rubber layer and clamping collars, which secured the aluminum layers to the lateral surface of the concrete specimen. To measure radial permeability, a hole of 16 mm in the center of the specimen and along its height is drilled. Moreover, the lower and upper horizontal surfaces are sealed with three aluminum foil layers of 0.1 mm thickness each and rubber joints. After preparing the specimens for the permeability tests, gas is injected from the bottom part of the permeability chamber. It takes around 15 to 25 min, depending on the interconnected porosity, specimen length, presence of cracks (if any) and gas pressure, until steady state is reached.
A general view of the permeability device is displayed in Figure 4. It comprises (1) three mass flowmeters with nominal measurement capacities (25,000, 750, and 20 mln/min at 0 °C and 1 atm) equivalent to (31.25, 0.94, and 0.025 g/min), respectively; (2) a pressure regulator; (3) a nitrogen gas reservoir with pressure reducer; (4) a replaceable specimen holder within an impervious chamber (elaborated in Figure 5); and (5) a PC for data acquisition.
Figure 4.
Permeability device general view and components: (a) photo of the system; (b) drawing of the system.
Figure 5.
Technical displays of the chamber: (a) longitudinal permeability testing; (b) radial permeability testing. Photos of the chamber: (c) longitudinal permeability testing; (d) radial permeability testing.
All measurements characterize residual gas permeability at ambient temperature after cooling and drying. The applied inlet gas pressures ranged from 1.5 to 3.5 bar gauge. Absolute pressures were used in the calculations.
2.5. Permeability Calculation
At each constant inlet pressure, the nitrogen flow was monitored until it remained within 0.5% for at least 3 min. Under steady, laminar, approximately isothermal flow, integration of Darcy’s law for a compressible gas gives the longitudinal and radial apparent permeabilities in Equations (1) and (2), respectively [43,44]. The radial expression assumes axisymmetric flow from the central bore to the cylindrical exterior.
Use SI units in Equations (1) and (2). Qil and Qir are the longitudinal and radial nitrogen flow rates reported at 0 °C and 1 atm. Multiply readings in normal mL/min by 10−6/60 to obtain normal m3/s. Pi is the absolute inlet pressure, obtained by adding atmospheric pressure to the gauge reading. The outlet discharges to the atmosphere at Patm = 1.013 × 105 Pa, also used as the flowmeter reference pressure in the equations. The nitrogen dynamic viscosity used in the calculation was 1.75 × 10−5 Pa·s. L is specimen length, S is the cross-sectional area normal to longitudinal flow, and r1 and r2 are the bore and external radii, respectively. The bore radius was 8 mm.
The apparent gas permeability includes slip at pore walls. The Klinkenberg relation [45], Equation (3), represents this contribution as a term proportional to 1/Pm, where Pm = (Pi + Patm)/2 is the mean absolute pressure.
In Equation (3), ka is the apparent permeability, ki is the intrinsic permeability, and β is the Klinkenberg coefficient. Both permeability values are in m2. The coefficient β has the same pressure units as Pm.
For each specimen and measurement direction, calculate ka at several inlet pressures and regress ka against 1/Pm. The intercept is ki, and the slope divided by the intercept is β. With Pm in pascals, β is obtained in pascals. For example, the four reported P1 data pairs in Figure 6 give an intercept of 2.67 × 10−17 m2 and β = 1.31 × 105 Pa when the plotted reciprocal pressures are converted from bar−1 to Pa−1.
Figure 6.
Change in the apparent permeability versus the inverse of mean pressure for P1, P2 and P3.
2.6. Replication and Interpretation of Scatter
Table 2 and Table 3 identify parent specimens and the slices taken from them. The compression series used three independent cylinders per condition. The tensile series used two independent dog-bone specimens per condition, with three slices cut from each gauge section. Slices from the same parent specimen are subsamples. Repeated measurements at different gas pressures are used to estimate permeability for a test piece. They do not add independent replicates. The cylindrical thermal series used nine slices from three cylinders. The unloaded heated dog-bone series used three parent specimens per target temperature.
The comparisons are descriptive. Section 3.1.1 reports between-cylinder standard deviations calculated from the regressions in Figure 6. Section 3.2.1 reports the available slice-level standard deviations for the dried cylindrical reference. The plotted ranges or error bars and the reported spreads describe dispersion. Slice-level scatter cannot be used as between-specimen uncertainty without the parent-specimen identifiers. With few independently prepared specimens and incomplete specimen-level data for the full matrix, no formal significance tests or confidence intervals are reported.
3. Results and Discussion
This section presents and discusses the residual gas permeability of VeRCoRs concrete following drying, thermal exposure, and sustained tensile or compressive loading. The influence of specimen length and slice position is first examined, followed by the individual and combined effects of drying, temperature, and creep. Attention is given to longitudinal and radial permeability to assess directional differences and their relationship with microcrack development and connectivity.
3.1. Effect of Specimen Length on Concrete Intrinsic Permeability
3.1.1. Reference Permeability
Figure 6 shows the Klinkenberg regressions for the three whole cylinders P1, P2, and P3. Across these independent specimens, mean longitudinal intrinsic permeability was 2.72 × 10−17 m2 (sample standard deviation 0.09 × 10−17 m2, n = 3), and mean β was 1.39 × 105 Pa (sample standard deviation 0.09 × 105 Pa). Individual β values were 1.31, 1.36, and 1.49 × 105 Pa, respectively.
3.1.2. Influence of Slice Position on Its Intrinsic Permeability
Figure 7 and Figure 8 show that the spread of intrinsic permeability and Klinkenberg coefficients increases as slice length decreases. Table 4 gives the results for eight nominal 25 mm slices from P1, numbered from the top (P1.1) to the bottom (P1.8). The top and bottom permeability values were 6.31 and 1.92 × 10−17 m2, respectively. The lower slices generally exhibit lower permeability and higher Klinkenberg coefficients. This pattern is consistent with a possible effect of casting segregation or compaction [5]. Local aggregate content was not quantified for these slices.
Figure 7.
Intrinsic permeability of slices for various lengths.
Figure 8.
Klinkenberg coefficients of slices for various lengths.
Table 4.
Permeability of 8 slices of 25 mm length originating from the specimen P1.
3.2. Effect of Drying, Temperature and Tensile Creep on Concrete Permeability
3.2.1. Effect of Drying on Concrete Longitudinal and Radial Permeability
After drying at 80 °C and cooling, the nine S-C slices had the same rounded mean intrinsic permeability of 2.93 × 10−17 m2 in the longitudinal and radial directions. The respective slice-level standard deviations were 0.21 and 0.95 × 10−17 m2. The means were close to the longitudinal mean of 2.72 × 10−17 m2 for the whole reference cylinders in Section 3.1.1. The equal means indicate little average directional difference for these dried disks, with greater scatter in the radial direction.
The S-D dog-bone slices had longitudinal and radial mean intrinsic permeabilities of 7.17 and 4.23 × 10−17 m2, respectively. The directional difference is consistent with changes in flow-path connectivity caused by specimen geometry, exposed drying surfaces, or shrinkage gradients [3,5]. Longitudinal testing samples paths along the specimen axis. Radial testing samples paths between the axial bore and the external curved surface. A connected crack or network increases permeability most strongly when it links the boundaries used for a given flow test. Individual crack orientation cannot be inferred from the directional permeability values alone. No direct crack imaging was reported for these tests.
In the 180-day series, the unloaded C1 cylinders exposed at 40 °C and 50% relative humidity had a radial permeability approximately twice that of the dried cylindrical reference. Drying shrinkage can generate tensile stresses and microcracking when contraction is restrained by a wetter core or by aggregates [3,5]. The measured residual difference is consistent with that mechanism, including possible contributions from thermal and preparation histories.
3.2.2. Effect of High Temperatures Solely on Concrete Longitudinal and Radial Permeability Using Cylinders
Figure 9 shows the directional residual intrinsic permeability of Th-C slices after heating and cooling. The slices were initially dried at 80 °C, yielding a mean of 2.93 × 10−17 m2, and were then heated to target temperatures between 100 and 250 °C. Permeability increased with temperature in both directions. The pooled mean at 250 °C was approximately 4.25 × 10−16 m2. Thermal expansion mismatch and changes to the hydrated paste may contribute to greater connectivity of gas flow paths [2,6,8,9,10]. Water permeability after high-temperature exposure has also been investigated separately [46].
Figure 9.
Residual intrinsic permeability versus exposure temperature for nine Th-C slices from three cylinders. The directional error bars show the reported asymmetric spread.
The radial and longitudinal means followed broadly similar thermal trends in these cylindrical slices. The exposure temperatures are imposed boundary values. Surface heating and evaporation can produce temperature and moisture gradients even at the specified heating rate of 1 °C/min. The protocol did not quantify internal temperature or saturation profiles, so the fitted temperature response characterizes the applied test history.
The equation for the exponential fit in both directions is
where
- kT (m2) Intrinsic permeability after cooling from temperature T (°C).
- k0 (m2) Intrinsic permeability at temperature 80 °C, regarded as reference permeability.
- CT: VeRCoRs Concrete permeability parameter found equal to 0.0158 (°C)−1.
Concerning Klinkenberg’s coefficient, the average of the initial value at 80 °C is equal to 2.26 × 105 Pa (as presented in Figure 10), with a value in the longitudinal direction higher by a factor of 1.5 than the radial direction. As temperature increases, Klinkenberg’s coefficient decreases exponentially. An exponential fitting is proposed to relate the change in the Klinkenberg’s coefficient with respect to temperature:
where
- βT (Pa): The Klinkenberg’s coefficient after cooling from temperature T (°C).
- β0 (Pa): The Klinkenberg coefficient at T0 (80 °C).
- DT: VeRCoRs concrete Klinkenberg coefficient’s parameter is found equal to −0.008 (°C)−1.
Figure 10.
Residual Klinkenberg coefficient versus exposure temperature for nine Th-C slices from three cylinders. The directional error bars show the reported asymmetric spread.
Equations (4) and (5) summarize the residual, dry response of the VeRCoRs cylindrical slices after the thermal-only protocol over 80–250 °C, with the 80 °C preconditioning state as the reference. A calculation using Equation (4) could assign a temperature-history-dependent dry matrix permeability after cooling, subject to validation for the modeled geometry and boundary conditions. Equation (5) describes gas slip and is relevant when modeling pressure-dependent apparent permeability. Neither equation includes a time variable, saturation, sustained stress, or a structural crack contribution. The parameters should be calibrated independently before use for other concretes, specimen geometries, or exposure histories.
3.2.3. Effect of Temperature Combined with Tensile Stress on Concrete Longitudinal and Radial Permeability Using Dog-Bone Samples
Figure 11 presents directional intrinsic permeability for unloaded dog-bone specimens. The 80 °C dry reference gives 7.17 × 10−17 m2 longitudinally and 4.23 × 10−17 m2 radially. The 100, 180, and 220 °C points represent thermal exposure histories followed by the preparation described in Section 2.3.
Figure 11.
Directional residual intrinsic permeability of unloaded dog-bone specimens. The 80 °C point represents the dried reference. Error bars show the reported asymmetric spread.
At 180 °C, the mean longitudinal and radial values reached 1.99 × 10−16 and 1.58 × 10−16 m2, respectively, or approximately 2.8 and 3.7 times their corresponding dry reference values. The means increased with exposure temperature in both directions. The available directional data show scatter and do not establish a monotonic trend in anisotropy.
Figure 12 compares the directional intrinsic permeability of unloaded and tensile-loaded dog-bone specimens. The 80 °C category represents the drying condition. For the tensile-loaded group in that category, the sustained load was applied at 20 °C before drying at 80 °C.
Figure 12.
Directional residual intrinsic permeability after thermal exposure alone and after combined heating and sustained tension. The 80 °C category corresponds to final drying. Error bars show the reported spread, with substantial radial scatter in the tensile-loaded group at 180 °C.
The plotted means after tensile loading at 20 °C were close to the corresponding unloaded dry references. At 100 °C, the plotted radial mean was approximately twice the unloaded mean, whereas the longitudinal difference in Figure 12 was smaller. At 180 °C, the tensile-loaded longitudinal and radial means were similar to each other, and the radial group exhibited the largest plotted spread. A change in the connectivity of transverse flow paths could account for the radial response at 100 °C. The scatter at 180 °C, limited independent replication, and absence of direct crack observations prevent attribution of the changes to tensile creep alone.
3.3. Effect of Temperature Combined with Compressive Stress on Concrete Radial Permeability Using Cylinders
Table 5 reports the normalized radial permeability and Klinkenberg coefficient for C1–C6. The normalization uses the dried cylindrical reference values k0 = 2.93 × 10−17 m2 and β0 = 2.16 × 105 Pa. Each exposure group contained three independently prepared cylinders. The normalized means in Table 5 describe differences between exposure histories.
Table 5.
Normalized radial permeability and Klinkenberg coefficient after 180 days (three cylinders per condition). Values are means with the reported within-condition spreads.
The specimen C1, exposed at 40 °C and 50% relative humidity without mechanical loading, had a normalized radial permeability of 2.0. This comparison with the dried reference captures the combined influence of the 180-day warm drying exposure and any difference in susceptibility to the final preparation.
At 20 °C and 100% relative humidity, the normalized radial permeability was 0.8 for 30% of compressive strength (C2) and 3.1 for 60% (C5). Closure of existing pathways during moderate loading and increased crack connectivity at higher stress could contribute to the different residual responses [42,47]. The measurements were made after unloading, and transient changes in aperture while the load was applied were not measured.
At 30% of compressive strength and 50% relative humidity, the normalized radial permeability rose from 2.1 at 20 °C (C3) to 9.2 at 40 °C (C4). The matched unloaded group at 40 °C and 50% relative humidity (C1) gave 2.0. At 60% and 20 °C, the normalized mean was 3.1 at 100% relative humidity (C5) and 14.5 at 50% (C6). The latter corresponds to 42.6 × 10−17 m2. Sustained deformation can change the opening and connectivity of flow paths, while concurrent drying can generate shrinkage-induced damage and modify the creep response. Previous compression studies have also linked residual permeability to load-related damage [48]. The experiment includes selected matched contrasts but lacks a fully crossed set of unloaded, loaded, saturated-humidity, and drying controls for every temperature and stress level. The endpoint permeability data therefore cannot quantify the separate contributions of creep, drying, and temperature or identify a statistical interaction among them.
The normalized Klinkenberg coefficient for C6 was 0.18, corresponding to β ≈ 0.39 × 105 Pa. Lower β alongside higher intrinsic permeability is consistent with reduced gas slip in a network with wider conducting paths [49,50]. Variation in β alone cannot identify pore or crack size.
3.4. Implications for Reinforced Concrete Containment Assessment
The measurements characterize residual transport through the plain concrete matrix under laboratory conditions. In reinforced or prestressed walls, steel restrains shrinkage and redistributes tensile strain, influencing crack spacing, opening, and connectivity. Steel–concrete interfaces can form additional flow paths if debonding or cracking connects them to the pore network [19]. Multiaxial stress, thermal and moisture gradients through the wall thickness, construction joints, penetrations, and connected macrocracks can all influence measured leakage [1,14,20]. These effects were outside the specimen program.
For a structural assessment, the directional dry permeability data can inform a sensitivity range for matrix transport in regions with comparable exposure histories. A coupled heat, moisture, and mechanical analysis can estimate the local histories of temperature, saturation, and crack opening. A gas-flow analysis can then combine directional matrix transport with separately characterized flow through cracks, joints, and interfaces under the relevant pressure history. The calculated total leakage can be compared with the applicable acceptance criterion after verification against representative reinforced specimens and mock-up leakage measurements [1]. The 14.5-fold specimen ratio applies to C6 relative to the dry cylindrical reference. Its use as a multiplier for the total containment leak rate would omit the other flow paths and their response under load.
4. Conclusions
The study measured residual longitudinal and radial gas permeability of VeRCoRs concrete after drying, heating, or sustained loading. The compression series was assessed in the radial direction.
- Permeability varied with slice position, with generally lower values near the bottom of the cast cylinder. This pattern is consistent with possible casting segregation. The dried cylindrical reference slices had a rounded mean of 2.93 × 10−17 m2 in both directions, whereas the dried dog-bone slices had a longitudinal mean about 1.7 times their radial mean.
- Both directional means increased after thermal-only exposure. Direction-dependent connectivity of microcracks is a plausible explanation for the anisotropy of the dog-bone slices. Direct characterization of crack orientation and connectivity would be required to confirm that mechanism.
- At 100 °C, the radial mean for the tensile-loaded dog-bone specimens was about twice that for unloaded specimens. At 180 °C, radial scatter was substantial and the tensile-loaded radial and longitudinal means were similar. The data support descriptive comparisons of the exposure histories, with limited resolution of the contribution from tensile creep.
- After 180 days at 20 °C and 100% relative humidity, radial permeability ratios were 0.8 at 30% and 3.1 at 60% of compressive strength. At 60% of compressive strength, 20 °C, and 50% relative humidity, radial permeability reached 42.6 × 10−17 m2, or 14.5 times the dried reference. The tested conditions do not allow quantitative separation of the effects of sustained deformation, thermal exposure, and drying shrinkage.
Future experiments should track permeability during sustained loading, heating, cooling, and unloading and measure transport at controlled degrees of saturation. Internal temperature and moisture monitoring, specimen-level replication, and direct crack characterization would help distinguish the mechanisms. Transfer to containment leakage assessment requires validation under representative reinforcement, stress states, saturation histories, and structural details.
Author Contributions
Conceptualization, M.E.E.D., M.B., F.D. and C.E.H.; Methodology, M.E.E.D., M.B., F.D. and C.E.H.; Software, M.E.E.D. and C.E.H.; Validation, M.E.E.D., M.B. and C.E.H.; Formal analysis, M.E.E.D., M.B., F.D. and C.E.H.; Investigation, M.E.E.D., M.B. and C.E.H.; Resources, M.E.E.D., M.B., F.D. and C.E.H.; Data curation, M.E.E.D.; Writing—original draft, M.E.E.D.; Writing—review & editing, M.B., F.D. and C.E.H.; Visualization, M.E.E.D. and C.E.H.; Supervision, M.B. and F.D.; Project administration, M.B. and F.D.; Funding acquisition, M.B., F.D. and C.E.H. All authors have read and agreed to the published version of the manuscript.
Funding
This research was funded by the Agence Nationale de la Recherche through “MaCEnA” project. 3SR is part of the LabEx Tec 21 (Investissements d’Avenir—Grant agreement no. ANR-11-LABX-0030).
Data Availability Statement
The raw data supporting the conclusions of this article will be made available by the authors on request.
Conflicts of Interest
The authors declare no conflict of interest.
References
- Charpin, L.; Niepceron, J.; Corbin, M.; Masson, B.; Mathieu, J.P.; Haelewyn, J.; Hamon, F.; Åhs, M.; Aparicio, S.; Asali, M.; et al. Ageing and air leakage assessment of a nuclear reactor containment mock-up: VERCORS 2nd benchmark. Nucl. Eng. Des. 2021, 377, 111136. [Google Scholar] [CrossRef] [Scilit]
- Grondin, F.; Dumontet, H.; Hamida, A.B.; Boussa, H. Micromechanical contributions to the behaviour of cement-based materials: Two-scale modelling of cement paste and concrete in tension at high temperatures. Cem. Concr. Compos. 2010, 33, 424–435. [Google Scholar] [CrossRef] [Scilit]
- Burlion, N.; Skoczylas, F.; Dubois, T. Induced anisotropic permeability due to drying of concrete. Cem. Concr. Res. 2003, 33, 679–687. [Google Scholar] [CrossRef] [Scilit]
- Picandet, V.; Khelidj, A.; Bastian, G. Effect of axial compressive damage on gas permeability of ordinary and high-performance concrete. Cem. Concr. Res. 2001, 31, 1525–1532. [Google Scholar] [CrossRef] [Scilit]
- Wu, Z.; Wong, H.; Buenfeld, N. Influence of drying-induced microcracking and related size effects on mass transport properties of concrete. Cem. Concr. Res. 2015, 68, 35–48. [Google Scholar] [CrossRef] [Scilit]
- Baroghel-Bouny, V. Caractérisation des Pâtes de Ciment et des Bétons; Méthodes, Analyse, Interprétations; Edition du Laboratoire Central des Ponts et Chausées: Paris, France, 1994. [Google Scholar]
- Diederichs, U.; Jumppanen, U.M.; Penttala, V. Behaviour of High Strength Concrete at High Temperature; Report 92; Helsinki University of Technology: Espoo, Finland, 1989. [Google Scholar]
- Noumowé, A. Effet de Hautes Temperatures (20–600 °C) sur le Béton. Cas Particulier du Béton à Hautes Performance. Ph.D. Thesis, INSA, Lyon, France, 1995. [Google Scholar]
- Choinska, M.; Khelidj, A.; Chatzigeorgiou, G.; Pijaudier-Cabot, G. Effects and interactions of temperature and stress-level related damage on permeability of concrete. Cem. Concr. Res. 2007, 37, 79–88. [Google Scholar] [CrossRef] [Scilit]
- Zeiml, M.; Lackner, R.; Leithner, D.; Eberhardsteiner, J. Identification of residual gas-transport properties of concrete subjected to high temperatures. Cem. Concr. Res. 2008, 38, 699–716. [Google Scholar] [CrossRef] [Scilit]
- Picandet, V.; Khelidj, A.; Bellegou, H. Crack effects on gas and water permeability of concretes. Cem. Concr. Res. 2009, 39, 537–547. [Google Scholar] [CrossRef] [Scilit]
- Akhavan, A.; Shafaatian, S.; Rajabipour, F. Quantifying the effects of crack width, tortuosity, and roughness on water permeability of cracked mortars. Cem. Concr. Res. 2012, 42, 313–320. [Google Scholar] [CrossRef] [Scilit]
- Rastiello, G.; Boulay, C.; Dal Pont, S.; Tailhan, J.L.; Rossi, P. Real-time water permeability evolution of a localized crack in concrete under loading. Cem. Concr. Res. 2014, 56, 20–28. [Google Scholar] [CrossRef] [Scilit]
- Dandachy, M.E.E.; Briffaut, M.; Dufour, F.; Pont, S.D. Methods in a continuous framework to assess transfer properties of concrete structures. Results Eng. 2025, 26, 104736. [Google Scholar] [CrossRef] [Scilit]
- Hachem, A.A.K.; Barraj, F.; El-Mir, A.; Dandachy, M.E.E. Steel–Mortar and flexural Mortar–Mortar bond strengths of Metakaolin-Based geopolymer. Eng. Rep. 2025, 7, e70476. [Google Scholar] [CrossRef] [Scilit]
- Hawa, L.; El-Mir, A.; Khatib, J.; Nasr, D.; Assaad, J.; Elkordi, A.; Dandachy, M.E.E. Optimization of Metakaolin-Based geopolymer composite for repair application. J. Compos. Sci. 2025, 9, 527. [Google Scholar] [CrossRef] [Scilit]
- Hachem, A.K.A.; Khatib, M.J.; Dandachy, M.E.E. Assessment of interfacial mortar-mortar bond and pure shear strength of metakaolin-based geopolymer. Int. J. Build. Pathol. Adapt. 2024, 43, 732–748. [Google Scholar] [CrossRef] [Scilit]
- Dandachy, M.E.E.; Hassoun, L.; El-Mir, A.; Khatib, J.M. Effect of elevated temperatures on compressive strength, ultrasonic pulse velocity, and transfer properties of Metakaolin-Based geopolymer mortars. Buildings 2024, 14, 2126. [Google Scholar] [CrossRef] [Scilit]
- Hachem, Y.; Dandachy, M.E.E.; Khatib, J.M. Physical, Mechanical and Transfer Properties at the Steel-Concrete Interface: A Review. Buildings 2023, 13, 886. [Google Scholar] [CrossRef] [Scilit]
- Bouhjiti, D.E.M.; Dandachy, M.E.E.; Dufour, F.; Pont, S.D.; Briffaut, M.; Baroth, J.; Masson, B. New continuous strain-based description of concrete’s damage-permeability coupling. Int. J. Numer. Anal. Methods Geomech. 2018, 42, 1671–1697. [Google Scholar] [CrossRef] [Scilit]
- Dandachy, M.E.E.; Briffaut, M.; Dufour, F.; Pont, S.D. An original semi-discrete approach to assess gas conductivity of concrete structures. Int. J. Numer. Anal. Methods Geomech. 2016, 41, 940–956. [Google Scholar] [CrossRef] [Scilit]
- Rahal, S.; Sellier, A.; Casaux-Ginestet, G. Finite element modelling of permeability in brittle materials cracked in tension. Int. J. Solids Struct. 2017, 113–114, 85–99. [Google Scholar] [CrossRef] [Scilit]
- Sogbossi, H.; Verdier, J.; Multon, S. Impact of reinforcement-concrete interfaces and cracking on gas transfer in concrete. Constr. Build. Mater. 2017, 157, 521–533. [Google Scholar] [CrossRef] [Scilit]
- Dandachy, M.E.E.; Briffaut, M.; Dufour, F. Experimental investigation of the transfer properties of ribbed and round steel rebars concrete interfaces under shear loading and after unloading. Constr. Build. Mater. 2024, 451, 138746. [Google Scholar] [CrossRef] [Scilit]
- Cartier, R.; Verdier, J.; Cagnon, H.; Vidal, T. Gas permeability of concrete under compressive creep during drying–wetting cycles. Cem. Concr. Compos. 2025, 165, 106302. [Google Scholar] [CrossRef] [Scilit]
- Mindeguia, J.; Hager, I.; Pimienta, P.; Carré, H.; La Borderie, C. Parametrical study of transient thermal strain of ordinary and high performance concrete. Cem. Concr. Res. 2013, 48, 40–52. [Google Scholar] [CrossRef] [Scilit]
- Tao, J.; Liu, X.; Yuan, Y.; Taerwe, L. Transient strain of self-compacting concrete loaded in compression heated to 700 °C. Mater. Struct. 2012, 46, 191–201. [Google Scholar] [CrossRef] [Scilit]
- Yoon, M.; Kim, G.; Kim, Y.; Lee, T.; Choe, G.; Hwang, E.; Nam, J. Creep behavior of High-Strength concrete subjected to elevated temperatures. Materials 2017, 10, 781. [Google Scholar] [CrossRef] [Scilit]
- Hager, I. Behaviour of cement concrete at high temperature. Bull. Pol. Acad. Sci. Tech. Sci. 2013, 61, 145–154. [Google Scholar] [CrossRef] [Scilit]
- Gawin, D.; Alonso, C.; Andrade, C.; Majorana, C.; Pesavento, F. Effect of damage on permeability and hygro-thermal behaviour of HPCs at elevated temperatures: Part 1. Experimental results. Comput. Concr. An. Int. J. 2005, 2, 189–202. [Google Scholar] [CrossRef] [Scilit]
- Dandachy, M.E.E.; Briffaut, M.; Pont, S.D.; Dufour, F. Induced Anisotropic Gas Permeability of Concrete due to Coupled Effect of Drying and Temperature. Key Eng. Mater. 2016, 711, 871–878. [Google Scholar] [CrossRef] [Scilit]
- Forth, J. Predicting the tensile creep of concrete. Cem. Concr. Compos. 2015, 55, 70–80. [Google Scholar] [CrossRef] [Scilit]
- Ranaivomanana, N.; Multon, S.; Turatsinze, A. Tensile, compressive and flexural basic creep of concrete at different stress levels. Cem. Concr. Res. 2013, 52, 1–10. [Google Scholar] [CrossRef] [Scilit]
- Cen, P.; Wei, E.; Tian, K. Influence of multistage target temperature and cyclic Loading/Unloading on the permeability of polypropylene fiber concrete. Adv. Civ. Eng. 2022, 2022, 6756069. [Google Scholar] [CrossRef] [Scilit]
- Liu, Z.; Li, Y.; Fan, K.; Wang, S.; Gu, Y.; Xia, Z.; Yao, Q. Characteristics of Creep and Permeability Changes in Coal Samples from Underground Water Storage Structures Under High Stresses. Water 2025, 17, 538. [Google Scholar] [CrossRef] [Scilit]
- Li, T.; Peng, F.; Chen, C.; Ma, C.; Li, Y.; Wang, Y.; Li, Y. Investigating the creep damage and permeability evolution mechanism of Phyllite considering Non-Darcy’s flow. Rock Mech. Rock Eng. 2024, 57, 8483–8498. [Google Scholar] [CrossRef] [Scilit]
- Yang, S.; Hu, B. Creep and permeability evolution behavior of red sandstone containing a single fissure under a confining pressure of 30 MPa. Sci. Rep. 2020, 10, 1900. [Google Scholar] [CrossRef] [Scilit]
- Ksit, B.; Szymczak-Graczyk, A.; Orlik-Kożdoń, B.; Garbowski, T. Numerical and surrogate modeling of drying processes in building envelopes under variable climatic conditions. Energy 2025, 339, 139014. [Google Scholar] [CrossRef] [Scilit]
- Poyet, S.; Adia, J.; Michel-Ponnelle, S. Experimental characterisation of the isosteric desorption energy of VeRCoRs concrete: Comparison of the isotherms and hygrometric methods. Cem. Concr. Res. 2024, 184, 107627. [Google Scholar] [CrossRef] [Scilit]
- Ezzedine El Dandachy, M. Characterization and Modelling of Permeability of Damaged Concrete: Application to Reinforced Concrete Structures. Ph.D. Thesis, University of Grenoble Alpes, Saint-Martin-d’Hères, France, 2016. [Google Scholar]
- RILEM TC 129-MHT; Test Methods for Mechanical Properties of Concrete at High Temperatures, Part 1 Introduction, Part 2 Stress-Strain Relation, Part 3 Compressive Strength, Part 4 Tensile Strength, Part 5 Modulus of Elasticity, Part 6 Thermal Strain, Part 7 Transient Creep, Part 8 Steady-State Creep, Part 9 Shrinkage, Part 10 Restraint, Part 11 Relaxation. RILEM: Champs-sur-Marne, France, 2004.
- Hoseini, M.; Bindiganavile, V.; Banthia, N. The effect of mechanical stress on permeability of concrete: A review. Cem. Concr. Compos. 2009, 31, 213–220. [Google Scholar] [CrossRef] [Scilit]
- Darcy, H. Les Fontaines Publiques de la Ville de Dijon; Dalmont: Paris, France, 1856; 647p. [Google Scholar]
- Yang, S. Fundamentals of Petrophysics; Springer Geophysics; Springer: Berlin/Heidelberg, Germany, 2017. [Google Scholar] [CrossRef] [Scilit]
- Klinkenberg, L.J. The Permeability of Porous Media to Liquid and Gaz; American Petroleum Institute, Drilling and Production Practice: New York, NY, USA, 1941; pp. 200–213. [Google Scholar]
- Ladbut, N.; Pupitthayatorn, M.; Homwuttiwong, S. Water Permeability of Concrete after Exposed to High Temperatures. Eng. Access 2017, 3, 10–14. [Google Scholar] [CrossRef]
- Kermani, A. Permeability of stressed concrete. Build. Res. Inf. 1991, 19, 360–366. [Google Scholar] [CrossRef] [Scilit]
- Miah, M.J.; Kallel, H.; Carré, H.; Pimienta, P.; La Borderie, C. The effect of compressive loading on the residual gas permeability of concrete. Constr. Build. Mater. 2019, 217, 12–19. [Google Scholar] [CrossRef] [Scilit]
- Lion, M.; Skoczylas, F.; Lafhaj, Z.; Sersar, M. Experimental study on a mortar. Temperature effects on porosity and permeability. Residual properties or direct measurements under temperature. Cem. Concr. Res. 2005, 35, 1937–1942. [Google Scholar] [CrossRef] [Scilit]
- Tanikawa, W.; Shimamoto, T. Comparison of Klinkenberg-corrected gas permeability and water permeability in sedimentary rocks. Int. J. Rock Mech. Min. Sci. 2008, 46, 229–238. [Google Scholar] [CrossRef] [Scilit]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.